Crosslinked thermoplastic elastomer composition
A crosslinked thermoplastic elastomer composition with a hydrogenated block copolymer, hydrocarbon rubber softener, and polypropylene resin addresses the flexibility and abrasion resistance imbalance, producing molded articles with enhanced properties for automotive applications.
Patent Information
- Application Number
- JP2024042071
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-07
AI Technical Summary
Existing thermoplastic elastomer compositions used in automotive applications lack the balance of flexibility and abrasion resistance required for severe conditions, particularly when substituting for vulcanized rubber.
A crosslinked thermoplastic elastomer composition comprising a hydrogenated block copolymer with specific molecular weight, a hydrocarbon rubber softener, and polypropylene resin, with a defined ratio and crosslinking agent, enhancing flexibility and wear resistance.
The composition achieves improved flexibility and abrasion resistance, enabling the production of molded articles with excellent moldability, suitable for automotive sealing materials and joining members.
Smart Images

Figure 2024137827000002 
Figure 2024137827000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a crosslinked thermoplastic elastomer composition. More specifically, the present invention relates to a crosslinked thermoplastic elastomer composition having excellent flexibility and abrasion resistance, and also to a molded article obtained by molding the crosslinked thermoplastic elastomer composition, a joining member, and an automotive composite member using the joining member. [Background technology]
[0002] Thermoplastic elastomer compositions obtained by dynamic heat treatment of polypropylene resins and styrene-butadiene block copolymers exhibit the properties of rubber-like soft materials, but do not require a vulcanization process and have moldability similar to that of thermoplastic resins. For this reason, such thermoplastic elastomer compositions have attracted attention from the viewpoints of streamlining the manufacturing process by replacing vulcanized rubber, recyclability, etc., and are widely used in the fields of automobile parts, home appliances, medical device parts, electric wires, miscellaneous goods, etc. In particular, thermoplastic elastomer compositions have been widely used in applications such as automobile sealants and building material sealants.
[0003] In this context, various inventions have been made relating to thermoplastic elastomers, particularly for use as automotive sealing materials. For example, Patent Document 1 discloses a peroxide cross-linked product containing a styrene copolymer rubber, a thermoplastic olefin resin, and a non-aromatic process oil, as a technology for obtaining a molded product having excellent flexibility and abrasion resistance for use as an automotive weather strip.
[0004] As an example of a thermoplastic elastomer used in a joining member as an automobile sealing material, Patent Document 2 discloses a composition containing a styrene copolymer rubber of a specific molecular weight, a hydrocarbon rubber softener, a polypropylene resin, and a crosslinking agent. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 11-20479 [Patent Document 2] JP 2020-125442 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, while thermoplastic elastomers are widely used in this way, molded articles obtained by molding thermoplastic elastomer compositions that have been widely used in the past have had a problem in terms of achieving both of the contradictory properties of greater flexibility and excellent abrasion resistance when used in applications such as automobile sealants and building sealants, particularly in recent years as replacements for vulcanized rubber. That is, although abrasion resistance is generally a property that is improved as the material becomes harder, in recent years, there has been a strong demand for materials that are both more flexible and abrasion resistant.
[0007] According to detailed studies by the present inventors, even the thermoplastic elastomer compositions described in Patent Documents 1 and 2 have not yet been used to replace vulcanized rubber in demanding applications where extremely good flexibility and abrasion resistance are required. Although the compositions have good abrasion resistance and fusibility and moldability for use as joining members, their Duro A hardness (based on JIS K6253) is at most 60, which means that their flexibility is insufficient.
[0008] The present invention has an object to solve the above-mentioned problems of the prior art, that is, to provide a thermoplastic elastomer composition which is more flexible and has excellent abrasion resistance, and a molded article thereof. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems, and have found that a crosslinked thermoplastic elastomer composition containing a styrene-isoprene-butadiene-based hydrogenated block copolymer having a specific weight average molecular weight and a crosslinking site, a hydrocarbon-based rubber softener, and a polypropylene-based resin in specific ratios is more flexible and has excellent abrasion resistance, thereby completing the present invention. That is, the gist of the present invention is as follows.
[0010] [1] A crosslinked thermoplastic elastomer composition comprising the following components (A), (B), and (C), containing 100 to 300 parts by mass of component (B) and 10 to 100 parts by mass of component (C) per 100 parts by mass of component (A), and having crosslinking sites in at least a portion of component (A): Component (A): A hydrogenated block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one copolymer block containing butadiene and isoprene, wherein the weight average molecular weight of the hydrogenated block copolymer is less than 350,000. Component (B): Hydrocarbon-based rubber softener. Component (C): Polypropylene resin.
[0011] [2] The crosslinked thermoplastic elastomer composition according to [1], wherein the weight ratio of the contents of the components (B) and (C) (content of component (B) / content of component (C)) is 1.6 or more. [3] The crosslinked thermoplastic elastomer composition according to [1] or [2], having a durometer hardness A (JIS K6253, after 15 seconds) of less than 60. [4] The crosslinked thermoplastic elastomer composition according to any one of [1] to [3], further comprising, as component (E), one or more lubricants selected from fatty acid amides and silicone oils. [5] The crosslinked thermoplastic elastomer composition according to [4], wherein the content of the component (E) is 1 to 20 parts by mass per 100 parts by mass of the total amount of the components (A), (B), and (C).
[0012] [6] A molded article obtained by molding the crosslinked thermoplastic elastomer composition according to any one of [1] to [5]. [7] The molded article according to [6], which is an automobile molded article. [8] The molded article according to [7], which is a joining member for automobiles. [9] The molded article according to [8] is a sealing member for an automobile, and the sealing member for an automobile is included in a composite member for an automobile.
[10] The composite component for an automobile according to [9], which is a seal component for an automobile door.
[0013]
[11] A method for producing a crosslinked thermoplastic elastomer composition, comprising melt-kneading a mixture at 80 to 300°C containing the following components (A), (B) a hydrocarbon-based rubber softener, (C) a polypropylene-based resin, and (D) a crosslinking agent, in such proportions that the component (B) is 100 to 300 parts by mass per 100 parts by mass of the component (A), the component (C) is 10 to 100 parts by mass of the component (C), and the component (D) is 0.1 to 10 parts by mass per 100 parts by mass of the total amount of the components (A), (B), and (C). Component (A): A hydrogenated block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one copolymer block containing butadiene and isoprene, wherein the weight average molecular weight of the hydrogenated block copolymer is less than 350,000. Effect of the Invention
[0014] The thermoplastic elastomer composition of the present invention has excellent flexibility and good abrasion resistance. In addition, by using the thermoplastic elastomer composition of the present invention, a molded article such as a joining member for a composite molded article having excellent flexibility and abrasion resistance can be obtained with good molding processability. Furthermore, due to its excellent flexibility, abrasion resistance and moldability, the joining member made of the thermoplastic elastomer composition of the present invention is useful as a sealing material for automobiles, sealing materials for building materials, etc. In particular, the joining member made of the thermoplastic elastomer composition of the present invention is useful as a joining member used in composite molded articles for automobiles, such as sealing members for automobile doors. [Brief description of the drawings]
[0015] [Figure 1] 1 is a perspective view showing a portion of an example of an automobile door seal member using a crosslinked thermoplastic elastomer composition according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described in detail below. The present invention is not limited to the following description, and can be modified in any manner without departing from the gist of the present invention. In this specification, when a numerical value or physical property value is enclosed before and after "~", the values before and after are included.
[0017] [Crosslinked Thermoplastic Elastomer Composition] The thermoplastic elastomer composition of the present invention is a crosslinked thermoplastic elastomer composition (hereinafter, sometimes referred to as "crosslinked thermoplastic elastomer composition") comprising at least the following components (A) to (C) in a predetermined ratio:
[0018] [Component (A)] Component (A) is a hydrogenated product of a block copolymer (hereinafter, sometimes referred to as a "hydrogenated block copolymer") having at least two polymer blocks (hereinafter, sometimes referred to as "block P") mainly composed of a vinyl aromatic compound and at least one copolymer block containing butadiene and isoprene (hereinafter, sometimes referred to as a "block Q"). Here, "polymer mainly composed of vinyl aromatic compound" means a polymer of a monomer mainly composed of vinyl aromatic compound. "Polymer containing butadiene" means a polymer of a monomer containing butadiene. "Mainly composed of vinyl aromatic compound" means a polymer containing 50 mol % or more of vinyl aromatic compound.
[0019] The vinyl aromatic compound as the monomer constituting the block P is not limited, but is preferably styrene and / or a styrene derivative such as α-methylstyrene. Of these, it is preferable that the main component is styrene. The block P may contain a monomer other than the vinyl aromatic compound as a raw material.
[0020] The monomers constituting the block Q are monomers having a butadiene skeleton, and are a monomer group containing at least butadiene and isoprene. This monomer group may contain one or more monomers having a butadiene skeleton other than butadiene and isoprene, but a monomer group mainly containing butadiene and isoprene is preferred. The phrase "mainly composed of butadiene and isoprene" means that the total content of butadiene and isoprene is 50 mol % or more.
[0021] The block copolymer can be hydrogenated by a general hydrogenation reaction, and examples of the hydrogenation catalyst used include general hydrogenation catalysts such as alkyl lithium catalysts, Ni, Co-based Ziegler catalysts, and Ti-based metallocene catalysts. When the hydrogenation reaction of the block copolymer is carried out using these hydrogenation catalysts, most of the block Q in the block copolymer is hydrogenated, but the block P is hardly hydrogenated at all.
[0022] The weight average molecular weight of the component (A) is less than 350,000, preferably 340,000 or less, more preferably 330,000 or less, and even more preferably 320,000 or less from the viewpoint of abrasion resistance. On the other hand, the lower limit of the weight average molecular weight of the component (A) is 50,000 or more, preferably 60,000 or more, and more preferably 70,000 or more. If the weight average molecular weight of the component (A) is within the above range, it is possible to obtain good abrasion resistance while having sufficient fusion strength. The weight average molecular weight of the component (A) is a value calculated in terms of polystyrene measured by gel permeation chromatography (hereinafter sometimes abbreviated as "GPC").
[0023] The weight percentage of block P in the hydrogenated block copolymer of component (A) is not limited, but is preferably 5% by mass or more, more preferably 10% by mass or more, and is preferably 55% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less. By having the weight percentage of block P in the above range, the rate of crosslinking reaction tends to be good.
[0024] The chemical structure of the block copolymer of component (A) may be any of linear, branched, radial, etc., but is preferably a structure represented by the following formula (1) or (2), and more preferably a structure represented by the following formula (1) from the viewpoint of improving mechanical strength. P-(QP)m (1) (PQ)n (2) In the formula, P represents a block P, and Q represents a block Q. m represents an integer of 1 to 5. n represents an integer of 2 to 5.
[0025] In the formula (1) or (2), larger values of m and n are preferred from the viewpoint of lowering the order-disorder transition temperature of the rubber-like polymer, but smaller values are preferred from the viewpoints of ease of production and cost.
[0026] As the block copolymer of component (A), a block copolymer represented by formula (1) is preferred over a block copolymer represented by formula (2) because of its excellent rubber elasticity, a block copolymer represented by formula (1) in which m is 3 or less is more preferred, and a hydrogenated block copolymer represented by formula (1) in which m is 2 or less is even more preferred.
[0027] Specific examples of hydrogenated block copolymers for component (A) include hydrogenated block copolymers of styrene-isoprene-butadiene-styrene, hydrogenated block copolymers of styrene (-isoprene-butadiene-styrene)2, and hydrogenated block copolymers of (styrene-isoprene-butadiene)2. These are suitable in that they easily obtain the fluidity required for fusion with olefin-based rubber, which is the adherend, in applications as joining materials.
[0028] The method for producing the hydrogenated block copolymer of component (A) in the present invention is not particularly limited, and may be any method as long as the above-mentioned structure and physical properties can be obtained. For example, the block copolymer can be obtained by block polymerization using a lithium catalyst or the like according to the method described in JP-A-7-97493. The hydrogenation (hydrogenation) of the block copolymer can be carried out in an inert solvent in the presence of a hydrogenation catalyst, for example, according to the method described in JP-A-59-133203.
[0029] Commercially available hydrogenated block copolymers of component (A) include "TAIPOL-6151" and "TAIPOL-6159" manufactured by Taiwan Synthetic Rubber Corporation (TSRC), "G1651" and "G1633" manufactured by Kraton Polymer Japan Co., Ltd., and "Septon 4055" and "Septon 4033" manufactured by Kuraray Co., Ltd.
[0030] The hydrogenated block copolymer of component (A) may be used alone or in combination of two or more types having different physical properties such as composition and weight average molecular weight. In order to easily control the overall balance of properties, it is preferable to use a combination of two or more types such that the weight average molecular weight of component (A) falls within the above-mentioned preferred range.
[0031] [Component (B)] The crosslinked thermoplastic elastomer composition of the present invention contains a hydrocarbon rubber softener, which is component (B), from the viewpoint of improving moldability.
[0032] The content of the component (B) is usually 100 parts by mass or more, preferably 102 parts by mass or more, and more preferably 104 parts by mass or more, per 100 parts by mass of the component (A), from the viewpoints of moldability and flexibility. On the other hand, the upper limit of the content of the component (B) is usually 300 parts by mass or less, preferably 280 parts by mass or less, and more preferably 250 parts by mass or less, per 100 parts by mass of the component (A), from the viewpoints of suppressing bleeding.
[0033] The component (B) may be a mineral oil-based rubber softener, a synthetic resin-based rubber softener, etc. Specific examples of these include a paraffin-based rubber softener made of paraffin oil in which 50% or more of the total carbon atoms are paraffin-based hydrocarbons, a naphthene-based rubber softener made of naphthene oil in which 30 to 45% of the total carbon atoms are naphthene-based hydrocarbons, an aromatic rubber softener made of aromatic oil in which 35% or more of the total carbon atoms are aromatic hydrocarbons, and a mineral oil-based rubber softener made of a mixture of aromatic hydrocarbons, naphthene-based hydrocarbons, and paraffin-based hydrocarbons. Of these, it is preferable to use a paraffin-based rubber softener.
[0034] The kinematic viscosity of the component (B) at 40° C. is not particularly limited, but is preferably 20 cSt or more, more preferably 50 cSt or more, and preferably 800 cSt or less, more preferably 600 cSt or less. The flash point (measured by the Cleveland Opening Method (COC Method)) of the hydrocarbon-based rubber softener is preferably 200° C. or more, more preferably 250° C. or more.
[0035] The component (B) can be obtained as a commercially available product. Examples of the commercially available product include the "Nippon Oil Polybutene (registered trademark) HV" series manufactured by JX Nippon Oil & Energy Corporation and the "Diana (registered trademark) Process Oil PW" series manufactured by Idemitsu Kosan Co., Ltd., and the relevant product can be appropriately selected and used from these. The component (B) may be used alone or as a mixture of two or more kinds in any combination and ratio.
[0036] [Component (C)] The crosslinked thermoplastic elastomer composition of the present invention contains a polypropylene resin as component (C) from the viewpoint of improving moldability. The lower limit of the content of the component (C) is usually 10 parts by mass or more, preferably 20 parts by mass or more, more preferably 30 parts by mass or more, based on 100 parts by mass of the component (A), from the viewpoint of moldability. On the other hand, the upper limit of the content of the component (C) is usually 100 parts by mass or less, preferably 90 parts by mass or less, more preferably 80 parts by mass or less, based on 100 parts by mass of the component (A), from the viewpoint of obtaining a hardness with sufficient flexibility as a molded product.
[0037] The polypropylene resin of component (C) is not particularly limited and may be a crystalline polypropylene resin or a non-crystalline polypropylene resin, and only one of these may be used or two or more of them may be combined.
[0038] The crystalline polypropylene resin is not particularly limited, but it is more preferable to use a crystalline polypropylene resin (hereinafter, sometimes referred to as "component (C1)") having a melting peak temperature of 100° C. or more and less than 165° C. A melting peak temperature of 100° C. or more is preferable from the viewpoint of heat resistance, and a melting peak temperature of less than 165° C. is preferable from the viewpoint of compatibility with component (A).
[0039] The non-crystalline polypropylene resin is not particularly limited, but it is more preferable to use a non-crystalline propylene polymer (hereinafter, sometimes referred to as "component (C2)") having a melting peak temperature of 45° C. or more and less than 100° C. This melting peak temperature is preferably 45° C. or more, preferably 55° C. or more, from the viewpoint of heat resistance, and is preferably 100° C. or less, preferably 90° C. or less, from the viewpoint of improved fusion property.
[0040] When this component (C2) is used, the content of component (C2) in component (C) is preferably 50 mass% or less, for example, 5 to 50 mass%. By including component (C2) in component (C), the fusibility is improved, but if the content is too high, the heat resistance may decrease.
[0041] The melting peak temperatures of the components (C1) and (C2) can be measured by the following method in accordance with JIS K7121. The melting behavior of the polypropylene resin is measured by carrying out the following steps (1) to (3) in order using a differential scanning calorimeter (DSC6220 manufactured by SSI NanoTechnology Inc.). In each step, a melting curve is obtained by plotting time on the horizontal axis and heat of fusion on the vertical axis, and the peak top of the peak observed in step (3) is taken as the melting peak temperature. Step (1): 5 mg of a sample is heated from room temperature to between 40° C. and 200° C. at a rate of 100° C. / min, and after the temperature increase is complete, the sample is held for 3 minutes. Step (2): The temperature is lowered from 200° C. to 40° C. at a rate of 10° C. / min, and after the temperature drop is complete, the temperature is held at this temperature for 3 minutes. Step (3): The temperature is increased from 40° C. to 200° C. at a rate of 10° C. / min.
[0042] The component (C1) may be one of crystalline propylene homopolymer, crystalline propylene-ethylene copolymer, and crystalline propylene random copolymer, or two or more of them may be used in any combination and ratio. When a crystalline propylene random copolymer is used as the component (C1), the content of propylene units in the crystalline propylene random copolymer is preferably 60-99% by mass, more preferably 80-98% by mass, based on the total amount of monomer units constituting the component (C1). When the content of propylene units in the component (C1) is within the above range, it is preferable because the melting peak temperature is easily within the above range. The content of each structural unit of component (C1) can be determined by infrared spectroscopy. The same applies to component (C2).
[0043] The crystalline propylene-based random copolymer that can be used as component (C1) is a copolymer having a propylene unit and a structural unit other than the propylene unit. Specific examples of the structural unit other than the propylene unit include an ethylene unit and an α-olefin unit other than the propylene unit. Examples of the structural units other than the propylene unit that may be contained in component (C1) include ethylene unit, 1-butene unit, 1-pentene unit, 1-hexene unit, 1-heptene unit, 1-octene unit, 1-nonene unit, 1-decene unit, 1-undecene unit, 1-dodecene unit, 1-tridecene unit, 1-tetradecene unit, 1-pentadecene unit, 1-hexadecene unit, 1-heptadecene unit, 1-octadecene unit, 1-nonadecene unit, 1-eicosene unit, 3-methyl-1-butene unit, 3-methyl-1-pentene unit, 4-methyl-1-pentene unit, 2-ethyl-1-hexene unit, and 2,2,4-trimethyl-1-pentene unit. Component (C1) may contain only one of these units, or may contain two or more units. Preferred examples of the structural unit other than the propylene unit contained in the component (C1) include an ethylene unit and a 1-butene unit.
[0044] When a non-crystalline propylene polymer is used as the component (C2), the content of the propylene unit is preferably 50% by mass to 93% by mass, more preferably 80% by mass to 92% by mass, and even more preferably 85% by mass to 91% by mass, based on the total amount of the monomer units constituting the component (C2). When the content of the propylene unit in the component (C2) is within the above range, it is preferable because the melting peak temperature is likely to fall within the above range.
[0045] The non-crystalline propylene polymer of component (C2) is typically a non-crystalline propylene-ethylene copolymer, but may have a structural unit other than propylene units or ethylene units, for example, an α-olefin unit other than propylene. In this case, examples of the α-olefin units that may be contained in component (C2) include 1-butene unit, 1-pentene unit, 1-hexene unit, 1-heptene unit, 1-octene unit, 1-nonene unit, 1-decene unit, 1-undecene unit, 1-dodecene unit, 1-tridecene unit, 1-tetradecene unit, 1-pentadecene unit, 1-hexadecene unit, 1-heptadecene unit, 1-octadecene unit, 1-nonadecene unit, 1-eicosene unit, 3-methyl-1-butene unit, 3-methyl-1-pentene unit, 4-methyl-1-pentene unit, 2-ethyl-1-hexene unit, and 2,2,4-trimethyl-1-pentene unit. Component (C2) may contain only one of these non-propylene structural units, or may contain two or more of them. A preferred example of the structural unit other than the propylene unit or ethylene unit contained in the component (C2) is the 1-butene unit.
[0046] The propylene polymers of the components (C1) and (C2) can be produced by known polymerization methods using known olefin polymerization catalysts. For example, a polymerization method using a Ziegler-Natta catalyst can be used. The polymerization method can be a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, or the like, or two or more of these methods can be combined.
[0047] The above-mentioned components (C1) and (C2) can also be obtained as commercial products. Commercially available products corresponding to the crystalline propylene-based polymer (C1) include Prim Polypro (registered trademark) from Prime Polymer Co., Ltd., Sumitomo Noblen (registered trademark) from Sumitomo Chemical Co., Ltd., polypropylene block copolymer from SunAllomer Co., Ltd., Novatec (registered trademark) PP from Japan Polypropylene Co., Ltd., Moplen (registered trademark) from LyondellBasell Co., Ltd., ExxonMobil PP from ExxonMobil Co., Ltd., Formolene (registered trademark) from Formosa Plastics Co., Ltd., Borealis PP from Borealis Co., Ltd., SEETEC PP from LG Chemical Co., Ltd., ASI POLYPROPYLENE from A. Schulman Co., Ltd., INEOS PP from INEOS Olefins & Polymers Co., Ltd., Braskem PP from Braskem Co., Ltd., Samsung Total from SAMSUNG TOTAL PETROCHEMICALS Co., Ltd., Sabic (registered trademark) PP from Sabic Co., Ltd., TOTAL PETROCHEMICALS Polypropylene from TOTAL PETROCHEMICALS Co., Ltd., and YUPLENE (registered trademark) from SK Co., Ltd., and the like. These may be appropriately selected and used in combination. In addition, examples of commercially available products corresponding to the amorphous propylene-based polymer (C2) include "Prime TPO (registered trademark)" manufactured by Prime Polymer, "VERSIFY (registered trademark)" manufactured by Dow Chemical Company, and "Vistamaxx (registered trademark)" manufactured by ExxonMobil Chemical Company. Examples of propylene-ethylene-1-butene copolymers include "TAFMER (registered trademark) PN" manufactured by Mitsui Chemicals, Inc. Any of these may be appropriately selected and used.
[0048] The component (C1) and the component (C2) may each be used alone or in combination of two or more types having different compositions or physical properties.
[0049] [Ratio of component (B) to component (C)] The weight ratio of the contents of the components (B) and (C), i.e., [content of component (B)] / [content of component (C)], is preferably 1.6 or more, and more preferably 2.0 or more, from the viewpoint of flexibility. On the other hand, the upper limit of the weight ratio of the contents of the components (B) and (C) is preferably 5.0 or less, and more preferably 4.0 or less, from the viewpoint of suppressing bleeding.
[0050] [Component (D)] The crosslinked thermoplastic elastomer composition according to the present invention is prepared by subjecting a composition containing predetermined amounts of the above-mentioned components (A), (B), (C) and other components to dynamic heat treatment in the presence of a crosslinking agent (hereinafter sometimes referred to as "component (D)"), or by subjecting a predetermined amount of component (D) to component (A) and subjecting it to dynamic heat treatment in the presence of component (D). Crosslinked sites are formed in at least a portion of the component (A), specifically, at least a portion of the molecule of the component (A), at least a portion between the molecule of the component (A) and the molecule of another component (A), or at least a portion between the component (A) and the component (C). The formation of these crosslinked sites allows the crosslinked thermoplastic elastomer composition according to the present invention to be a crosslinked body with good rubber elasticity.
[0051] As the component (D), organic peroxides, phenolic resins, other crosslinking assistants, etc. These crosslinking agents may be used alone or in combination of two or more.
[0052] As the organic peroxide, either an aromatic organic peroxide or an aliphatic organic peroxide can be used. Specific examples of the peroxides include dialkyl peroxides such as di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, 1,3-bis(t-butylperoxyisopropyl)benzene, and 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane; peroxy esters such as t-butyl peroxybenzoate, t-butylperoxyisopropyl carbonate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, and 2,5-dimethyl-2,5-di(benzoylperoxy)-3-hexyne; and hydroperoxides such as acetyl peroxide, lauroyl peroxide, benzoyl peroxide, p-chlorobenzoyl peroxide, and 2,4-dichlorobenzoyl peroxide. Among these, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane is preferred. These organic peroxides may be used alone or in combination of two or more.
[0053] The phenol resin includes alkylphenol formaldehyde, brominated alkylphenol formaldehyde, etc. These phenol resins may be used alone or in combination of two or more kinds.
[0054] Examples of crosslinking assistants other than the organic peroxides and phenolic resins include assistants for peroxides such as sulfur, p-quinone dioxime, p-dinitrosobenzene, 1,3-diphenylguanidine, etc.; crosslinking assistants for phenolic resins such as stannous chloride anhydride, stannous chloride dihydrate, ferric chloride, etc.; polyfunctional vinyl compounds such as divinylbenzene, triallyl cyanurate, triallyl isocyanurate, diallyl phthalate, etc.; polyfunctional (meth)acrylate compounds such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, allyl (meth)acrylate, etc. These may be used alone or in combination of two or more.
[0055] The amount of the component (D) used is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, more preferably 1.0 parts by mass or more, and even more preferably 1.5 parts by mass or more, based on 100 parts by mass of the total amount of the components (A), (B), and (C), from the viewpoint of sufficiently proceeding with the crosslinking reaction. The upper limit of the amount of the component (D) used is preferably 10 parts by mass or less, more preferably 9.0 parts by mass or less, and more preferably 8.0 parts by mass or less, based on 100 parts by mass of the total amount of the components (A), (B), and (C), from the viewpoint of controlling the crosslinking reaction.
[0056] [Component (E)] In producing the crosslinked thermoplastic elastomer composition of the present invention, in addition to the above components (A) to (D), at least one lubricant selected from fatty acid amides and silicone oils may be contained as component (E).
[0057] The fatty acid amide used as the lubricant of the component (E) is usually a fatty acid amide having 12 or more carbon atoms, and specifically includes, for example, saturated fatty acid amides such as lauric acid amide, palmitic acid amide, stearic acid amide, and behenic acid amide, unsaturated fatty acid amides such as oleic acid amide, erucic acid amide, brassidic acid amide, and elaidic acid amide, fatty acid bisamides such as methylene bisstearic acid amide, ethylene bisstearic acid amide, and ethylene bisoleic acid amide, and branched fatty acid amides such as isobehenic acid amide and isostearic acid amide. Of these, only one kind may be used, or two or more kinds may be used in any combination and ratio. Among these fatty acid amides, oleic acid amide and erucic acid amide are particularly preferred from the viewpoint of sliding properties.
[0058] The silicone oil used as the lubricant of the component (E) includes organosiloxanes that have been used as slip agents in the past, specifically, dimethylpolysiloxane, methylphenylpolysiloxane, methylhydrogenpolysiloxane, and other polysiloxanes, and modified polysiloxanes obtained by modifying these polysiloxanes with epoxy, alkyl, methacryl, carbinol, amino, mercapto, carboxyl, alcohol, phenol, fluorine, aralkyl, diol, alkyl aralkyl polyether, epoxy polyether, or polyether. Of these, only one type may be used, or two or more types may be used in any combination and ratio. Among these organosiloxanes, dimethylpolysiloxane and its alkyl and methacryl modified polysiloxanes are particularly preferred from the viewpoint of sliding properties.
[0059] The viscosity of the polysiloxane at 25°C is usually 0.5 cSt or more and 1,000,000 cSt or less, preferably 1 cSt or more and 500,000 cSt or less, more preferably 1.5 cSt or more and 300,000 cSt or less, and even more preferably 20,000 to 100,000 cSt. When the viscosity of the polysiloxane is within this range, it is possible to improve the abrasion resistance while suppressing bleeding. Among these, only one type of polysiloxane having the same viscosity may be used, or two or more types having different viscosities may be used in any combination and ratio. In this case, the ratio of the combination may be any ratio, but from the viewpoint of wear resistance, it is preferable to add a greater amount of silicone oil than the amount of fatty acid amide, and from the viewpoint of bleeding suppression, it is more preferable to add a greater amount of silicone oil with a viscosity of 100 cSt or more than the amount of silicone oil with a viscosity of less than 100 cSt at 25°C.
[0060] The component (E) is preferably used in combination of two or more kinds, including the fatty acid amide and silicone oil. For example, three or four kinds of components (E) may be used in combination. By using a plurality of kinds of components (E) in combination, the bleeding speed of the lubricant can be controlled, and it is possible to suppress problems caused by bleeding while ensuring both the effect of the lubricant in the short term (slidability) and the effect of the lubricant in the long term (slidability).
[0061] When the component (E) is used as a lubricant, the component (E) is used in an amount of 1 to 20 parts by mass, preferably 2 to 15 parts by mass, per 100 parts by mass of the total amount of the components (A), (B), and (C). By satisfying this range, it is possible to suppress a decrease in adhesion and obtain sufficient abrasion resistance. As described below, in the present invention, the amount of lubricant used can be reduced due to the effect of component (A) in improving the sliding properties, and as described above, by adding a small amount of 20 parts by mass or less per 100 parts by mass of component (A) in total, it is possible to obtain excellent wear resistance while suppressing a decrease in adhesion.
[0062] [Component (G)] In the production of the crosslinked thermoplastic elastomer composition of the present invention, in addition to the above-mentioned components (A) to (D), a component (G) may be used which is a block copolymer or a hydrogenated product thereof having a polymer block R mainly composed of a vinyl aromatic compound other than the above-mentioned and a copolymer block S of a vinyl aromatic compound and at least one of an olefin and a conjugated diene. The polymer block R constitutes a hard segment, and the copolymer block S constitutes a soft segment.
[0063] Examples of the vinyl aromatic compound of the polymer block R include styrene compounds such as styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, and 1,3-dimethylstyrene, and polycyclic aromatic compounds such as vinylnaphthalene and vinylanthracene. Among these, styrene compounds are preferred, and styrene is particularly preferred.
[0064] The vinyl aromatic compound used in the copolymer block S may be the same as the vinyl aromatic compound used in the polymer block R. Conjugated dienes used in the copolymer block S include, for example, butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene. Of these, butadiene, isoprene, or a mixture of butadiene and isoprene is preferred, with butadiene being particularly preferred. Moreover, the polymer block R is preferably a random copolymer block in order to impart flexibility to the resulting thermoplastic elastomer composition.
[0065] Component (G) is a hydrogenated block copolymer obtained by hydrogenating the carbon-carbon double bonds derived from the conjugated diene of the block copolymer, and may be either completely hydrogenated (fully hydrogenated) or partially hydrogenated (selectively hydrogenated). The content of the polymer block R in the block copolymer of component (G) is usually 3% by mass or more and 70% by mass or less. If the content of the polymer block R is equal to or more than the above lower limit, the thermoplastic elastomer composition tends to have excellent mechanical strength and heat resistance. The lower limit of the content of the polymer block R is preferably 4% by mass or more, more preferably 5% by mass or more. On the other hand, the upper limit of the content of the polymer block R is preferably 50% by mass or less, more preferably 40% by mass or less. If the content of the polymer block R is equal to or less than the above upper limit, flexibility can be maintained and bleeding of the hydrocarbon rubber softener can be suppressed.
[0066] The proportion of the constituent units derived from vinyl aromatic compounds in the hydrogenated copolymer of component (G) is usually 50% by mass or more and 90% by mass or less. From the viewpoint of improving the abrasion resistance of the thermoplastic elastomer composition, the lower limit of the proportion of the constituent units derived from vinyl aromatic compounds is preferably 55% by mass or more, and the upper limit is preferably 85% by mass or less. Therefore, the proportion of the constituent units derived from vinyl aromatic compounds in the copolymer block S, in combination with the constituent units derived from vinyl aromatic compounds in the polymer block R, is preferably such that the proportion of the constituent units derived from vinyl aromatic compounds in component (G) falls within the above range.
[0067] The weight average molecular weight of the block copolymer of component (G) measured by the GPC method in terms of polystyrene is preferably 50,000 or more, more preferably 75,000 or more, as a lower limit from the viewpoint of improving the mechanical strength of the thermoplastic elastomer composition, and is preferably 1,000,000 or less, more preferably 500,000 or less, as an upper limit from the viewpoint of moldability.
[0068] The component (G) used in the thermoplastic elastomer composition of the present invention preferably has a glass transition temperature of 0°C or higher. From the viewpoint of abrasion resistance, the glass transition temperature of component (G) is more preferably 10°C or higher, and the upper limit is preferably 40°C or lower, more preferably 30°C or lower. By making the glass transition temperature of component (G) 0°C or higher, it is possible to obtain good abrasion resistance while maintaining flexibility. In addition, by making the glass transition temperature of component (G) 40°C or lower, it is possible to exhibit the characteristic of cold resistance (flexibility at low temperatures).
[0069] The glass transition temperature of the component (G) can be measured under the following measurement conditions and by the following measurement method with reference to JIS K6394. I) Measurement conditions: Measurement equipment: TA Instruments dynamic viscoelasticity measuring device "RSA-III" Measurement mode: Tensile Atmosphere: Nitrogen ·Temperature: -20~100℃ Heating rate: 2℃ / min Soak time: 30 seconds Frequency: 1Hz II) Measurement method: Component (G) is press-molded at 200° C. into a flat plate of 1 mm thickness, which is then cut into a strip of 4 mm width, which is then fixed to the above-mentioned measuring device and measured under the above-mentioned measuring conditions.
[0070] The block copolymer of component (G) can be produced by any known method. For example, a method of block polymerization in an inert solvent using a lithium catalyst or the like (see JP-B-40-23798, etc.) can be mentioned. In addition, the hydrogenation treatment of the block copolymer can be carried out in an inert solvent in the presence of a hydrogenation catalyst (see JP-B-42-8704, JP-B-43-6636, JP-A-59-133203, JP-A-60-79005, etc.). In addition, the hydrogenated copolymer of component (G) can be a commercially available product. Examples of commercially available hydrogenated copolymers include "Tuftec (registered trademark) SOE-SS" (manufactured by Asahi Kasei Corporation) and "Kraton A series" (manufactured by Kraton Polymers).
[0071] The hydrogenated copolymer of a vinyl aromatic compound and a conjugated diene of component (G) may be used alone as one type, or as two or more types in any combination and in any ratio.
[0072] [Other ingredients] In producing the crosslinked thermoplastic elastomer composition of the present invention, other components can be used as raw materials, as necessary, in addition to the above-mentioned components (A) to (G), within the scope that does not impair the effects of the present invention.
[0073] Examples of the other components include resins such as thermoplastic resins and elastomers other than component (A), component (C), and component (G), antioxidants, fillers, heat stabilizers, light stabilizers, ultraviolet absorbers, neutralizing agents, lubricants other than component (E), antifogging agents, antiblocking agents, slip agents, dispersants, colorants, flame retardants, antistatic agents, conductivity imparting agents, metal deactivators, molecular weight regulators, antibacterial agents, antifungal agents, fluorescent whitening agents, etc. Any of these may be used alone or in combination.
[0074] Examples of thermoplastic resins other than the above-mentioned components (A), (C), and (G) include polyphenylene ether resins; polyamide resins such as nylon 6 and nylon 66; polyester resins such as polyethylene terephthalate and polybutylene terephthalate; polyoxymethylene resins such as polyoxymethylene homopolymers and polyoxymethylene copolymers; polymethyl methacrylate resins, and polyolefin resins (excluding those corresponding to component (C)). Examples of the elastomers other than the components (A), (C) and (G) include styrene-based elastomers (excluding those corresponding to the component (A)); polyester-based elastomers; and polybutadiene.
[0075] Examples of lubricants other than the component (E) include fatty acids, fatty acid esters, metal soaps, silicone masterbatches, silicone gums, liquid siloxane waxes, and polyolefin waxes.
[0076] Examples of the antioxidant (hereinafter sometimes referred to as "component (F)") include phenol-based antioxidants, phosphite-based antioxidants, and thioether-based antioxidants. When an antioxidant is used, the antioxidant is usually used in the range of 0.01 to 3.0 parts by mass, preferably 0.15 to 0.6 parts by mass, per 100 parts by mass of the total of component (A). When the content of the antioxidant is within the above range, good thermal stability is obtained.
[0077] Examples of the filler include glass fiber, hollow glass spheres, carbon fiber, talc, calcium carbonate, mica, potassium titanate fiber, silica, metal soap, titanium dioxide, and carbon black. When a filler is used, the filler is usually used in an amount of 0.3 to 100 parts by mass per 100 parts by mass of the total of component (A).
[0078] [Method of producing crosslinked thermoplastic elastomer composition] The crosslinked thermoplastic elastomer composition of the present invention can be obtained by subjecting a composition containing predetermined amounts of component (A), component (B), component (C), and, if necessary, component (G) and other components, etc., to dynamic heat treatment in the presence of component (D) to crosslink the composition. The crosslinked thermoplastic elastomer composition of the present invention can also be obtained by blending component (A) with component (D) in predetermined amounts in advance, crosslinking the blend by dynamic heat treatment, and then blending component (B), component (C), and, if necessary, component (G) and other components in predetermined amounts, respectively.
[0079] In the present invention, "dynamic heat treatment" means kneading in a molten or semi-molten state in the presence of a crosslinking agent. The dynamic heat treatment is preferably performed by melt kneading. As a mixing and kneading device for melt kneading, for example, a non-open type Banbury mixer, a mixing roll, a kneader, or a twin-screw extruder is used. Among these, it is preferable to use a twin-screw extruder. In a preferred embodiment of the production method using a twin-screw extruder, each component is supplied to a raw material supply port (hopper) of a twin-screw extruder having multiple raw material supply ports, and dynamic heat treatment is performed. The temperature when the dynamic heat treatment is carried out is usually 80 to 300° C., and preferably 100 to 250° C. The time for which the dynamic heat treatment is carried out is usually 0.1 to 30 minutes.
[0080] When the crosslinked thermoplastic elastomer composition of the present invention is produced by subjecting a composition containing the components (A) to (D) to be crosslinked or a composition containing the components (A) and (D) to dynamic heat treatment in a twin-screw extruder, it is preferable to extrude the composition while maintaining the relationship of the following formula (I) between the barrel radius (R (mm)), the screw rotation speed (N (rpm)), and the discharge rate (W (kg / hour)) of the twin-screw extruder, and it is more preferable to extrude the composition while maintaining the relationship of the following formula (II). 2.6 <NW / R 3 <22.6 (I) 3.0 <NW / R 3 <20.0 (II)
[0081] It is preferable that the above relationship between the barrel radius (R (mm)), screw rotation speed (N (rpm)), and discharge rate (W (kg / hour)) of the twin-screw extruder is larger than the lower limit value in order to efficiently produce a crosslinked thermoplastic elastomer composition. On the other hand, it is preferable that the above relationship is smaller than the upper limit value in order to suppress heat generation due to shear and to prevent the generation of foreign matter that causes a defective appearance.
[0082] [Physical properties of crosslinked thermoplastic elastomer composition] From the viewpoint of moldability, the crosslinked thermoplastic elastomer composition of the present invention preferably has a melt flow rate (MFR) of 1 g / 10 min or more, more preferably 1.3 g / 10 min or more, and even more preferably 1.5 g / 10 min or more, as measured by a method conforming to JIS K7210 at a measurement temperature of 230° C. and a measurement load of 21.2 N. From the viewpoint of moldability, the melt flow rate (MFR) of the crosslinked thermoplastic elastomer composition of the present invention is preferably 80 g / 10 min or less, more preferably 75 g / 10 min or less, and even more preferably 70 g / 10 min or less.
[0083] From the viewpoint of flexibility, the crosslinked thermoplastic elastomer composition of the present invention has a Duro A hardness measured after 15 seconds according to the measuring method of JIS K6253 of preferably less than 60, more preferably not more than 55. Also, from the viewpoint of abrasion resistance, it is preferably 30 or more, more preferably 35 or more.
[0084] From the viewpoint of abrasion resistance, the crosslinked thermoplastic elastomer composition of the present invention has an abrasion loss of preferably 130 mg or less, more preferably 100 mg or less, as measured by a Gakushin trial friction tester in accordance with the measurement method of JIS L 849, after 10,000 reciprocations under a load of 500 g. The lower limit of the abrasion loss is not particularly specified, since the lower the better.
[0085] [Molding] The crosslinked thermoplastic elastomer composition of the present invention can be molded into a molded article by a molding method generally used for crosslinked thermoplastic elastomer compositions, such as injection molding, extrusion molding, blow molding, and compression molding. Among these, the crosslinked thermoplastic elastomer composition of the present invention is preferably molded by injection molding. After these moldings, the composition can also be molded into a molded article by secondary processing such as lamination molding and thermoforming. The molded articles obtained by the above molding method include various types, such as molded articles for automobiles used as automobile parts, molded articles for civil engineering works used as civil engineering parts and building material parts, and molded articles for building materials.
[0086] [Jointing material] The molded article of this crosslinked thermoplastic elastomer composition can be used as a joining member. For example, the above-mentioned molded article for automobiles, molded article for civil engineering, molded article for building materials, etc. can be used as a joining member. An example of the molded article for automobiles used as a joining member can be a sealing material for automobiles, etc., and an example of the molded article for civil engineering and molded article for building materials used as a joining member can be a sealing material for building materials, etc. Moreover, the automotive sealant or building sealant can be combined with other components to form a composite member. This joining member can be produced by the above-mentioned molding method, particularly injection molding, specifically by melt-kneading the crosslinked thermoplastic elastomer composition of the present invention and injection-molding the kneaded mixture.
[0087] An example of a composite member using the above-mentioned automotive molded article as one of its constituent members is an automotive composite molded article, and a specific example of such a composite member is an automotive door seal member that includes an automotive seal material as the automotive molded article and is combined with a plurality of other parts and members. An example of this automobile door seal member is the automobile door seal member 3 shown in Fig. 1. This is formed by fusion-bonding crosslinked rubber members 1A and 1B together at a corner portion made of the automobile seal material 2 according to the present invention.
[0088] Such an automobile door seal member 3 can be produced, for example, by inserting the joining ends of prefabricated crosslinked rubber members 1A, 1B into an injection molding die, and then injecting the thermoplastic elastomer composition of the present invention into this die to form an automobile seal material 2 for the corner portion, while fusing and integrating it with the end faces of the crosslinked rubber members 1A, 1B.
[0089] The crosslinked rubber members 1A and 1B as the adherend are preferably olefin-based rubber. Specific examples of olefin-based rubber include sulfur vulcanized rubber and its foam, and olefin-based thermoplastic elastomer. From the viewpoint of obtaining good flexibility, rubber elasticity, and compression set properties as a seal member for automobile doors, sulfur vulcanized rubber is preferable, and sulfur vulcanized rubber foam is particularly preferable.
[0090] A weatherstrip product can be given as a specific example of the automobile door sealing material 2. Examples of the weatherstrip product include an opening trim weatherstrip, a door glass run, a door weatherstrip, an outer weatherstrip, and a luggage weatherstrip.
[0091] [Application] The molded article made of the crosslinked thermoplastic elastomer composition of the present invention can be used as the automobile parts, civil engineering parts, and building material parts. In addition to the sealing material, the automobile parts can include components constituting the surface and weather strip, ceiling materials, interior sheets, bumper moldings, side moldings, air spoilers, air duct hoses, etc. In addition to the sealing material, the automobile parts, civil engineering parts, and building material parts can include water-stopping materials, joint materials, window frames, etc. Applications of the automobile parts, civil engineering parts, and building material parts can include sports goods such as the grip parts of golf clubs and the grip parts of tennis rackets; industrial parts such as hose tubes and gaskets; home appliance parts such as hoses and packings; medical parts such as medical containers, gaskets, and packings; food parts such as containers and packings; medical equipment parts; electric wires; and miscellaneous goods.
[0092] [mechanism] The crosslinked thermoplastic elastomer composition of the present invention exhibits the effects of being excellent in flexibility and abrasion resistance, and also having good moldability. Although the details of why the crosslinked thermoplastic elastomer composition of the present invention exhibits such effects are not clear, it is presumed to be as follows. 1) The small amount of double bonds between carbon atoms present in component (A) act as crosslinking points with the crosslinking agent or crosslinking aid of component (D) added during dynamic crosslinking, forming gentle bonds between molecular chains while also involving the surrounding resins of components (A) and (C). This makes it difficult for the molecular chains to separate, improving abrasion resistance. 2) By kneading component (A) together with the crosslinking agent and crosslinking aid of component (D), the rubber components are uniformly dispersed with extremely fine dispersion diameters during kneading, which makes it easier for the crosslinking reaction to proceed uniformly, thereby further improving abrasion resistance. 3) The uniform dispersion and crosslinking of the rubber component in component (A) results in good abrasion resistance, which in turn reduces surface tension (adhesion to the adherend) and allows the amount of lubricant such as silicone oil, which may cause defects due to bleeding, to be kept within a practical upper limit. This means that abrasion resistance can be maintained even with a component ratio that provides greater flexibility. 4) Component (A), which is the rubber component, has a polymer block mainly composed of vinyl aromatic compound units, and since this polymer block is crosslinked, it can contain a larger amount of rubber softener than olefin-based rubber or non-crosslinked styrene-based rubber, and a more flexible compounding ratio can be achieved. EXAMPLES
[0093] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the invention. The values of various production conditions and evaluation results in the following examples are meant as preferred upper or lower limit values in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values and the values of the following examples or values of the examples.
[0094] 〔raw materials〕 The raw materials used in the following examples and comparative examples are as follows. [Component (A)] {Hydrogenated block copolymer (A)} <a-1> Styrene-isoprene-butadiene-styrene hydrogenated block copolymer (having the structure of the above formula (1)), styrene (block P) content: 30% by mass, weight average molecular weight: 288,000, "Septon 4055" manufactured by Kuraray Co., Ltd. <a-2> Styrene-isoprene-butadiene-styrene hydrogenated block copolymer (having the structure of the above formula (1)), styrene (block P) content: 30% by mass, weight average molecular weight: 83,800, "Septon 4033" manufactured by Kuraray Co., Ltd.
[0095] <a-3>(For comparison purposes) Styrene-isoprene-butadiene-styrene hydrogenated block copolymer (having the structure of the above formula (1)), styrene (block P) content: 30% by mass, weight average molecular weight: 381,000, "Septon 4077" manufactured by Kuraray Co., Ltd. <a-4>(For comparison purposes) Styrene-butadiene-styrene hydrogenated block copolymer (having the structure of the above formula (1), where block Q is a butadiene homopolymer), styrene (block P) content: 32% by mass, weight average molecular weight: 260,000), "TAIPOL-6151" manufactured by Taiwan Synthetic Rubber Corporation (TSRC)
[0096] [Component (B)] <b-1> Paraffin-based rubber softener (kinematic viscosity at 40°C: 95.5 cSt, pour point: -15°C, flash point: 272°C), Idemitsu Kosan's "Diana (registered trademark) Process Oil PW90"
[0097] [Component (C)] <c-1> Propylene-ethylene random copolymer (MFR (JIS K7210): 30 g / 10 min (230°C, 21.2 N), melting peak temperature: 155°C, propylene unit content: 98% by mass), Japan Polypropylene Corporation "Novatec (registered trademark) PP MG03BD" <c-2> Propylene homopolymer (MFR (JIS K7210): 10g / 10min (230°C, 21.2N), melting peak temperature: 160°C, propylene unit content: 100% by mass), "Novatec (registered trademark) PP MA3" manufactured by Japan Polypropylene Corporation <c-3> Propylene-ethylene random copolymer (MFR (JIS K7210): 8 g / 10 min (230°C, 21.2 N), melting peak temperature: 75°C, propylene unit content: 91% by weight), ExxonMobil Chemical Corporation "Vistamaxx (registered trademark) 3980FL"
[0098] [Component (D)] <d-1> A mixture of 40 parts by mass of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane and 60 parts by mass of calcium carbonate, "Trigonox 101-40C" manufactured by Nouryon Chemical Industries, Ltd. <d-2> A mixture of 55 parts by mass of divinylbenzene and 45 parts by mass of ethylvinylbenzene, "Divinylbenzene" manufactured by Wako Pure Chemical Industries, Ltd.
[0099] [Component (E)] <e-1> Oleic acid amide, Nippon Kasei's "Diamid O-200" <e-2> Silicone oil, Shin-Etsu Chemical's "KF96-10CS" <e-3> Silicone oil, Shin-Etsu Chemical's "KF96-100CS" <e-4> Silicone oil, Shin-Etsu Chemical's "KF96-1000CS"
[0100] [Component (F)] <f-1> Antioxidant: BASF Japan's "Irganox (registered trademark) 1076"
[0101] [Component (G)] {Hydrogenated block copolymer (G)} <g-1> Hydrogenated block copolymer consisting of polymer block R of vinyl aromatic compound constituting the hard segment and copolymer block S of vinyl aromatic compound and conjugated diene constituting the soft segment: "Tuftec (registered trademark) SOES1605" manufactured by Asahi Kasei Corporation Hydrogenation: Fully hydrogenated Glass transition temperature: 16℃ Polymer block R: styrene Copolymer block S: styrene and butadiene Styrene unit content: 67% by mass ·Weight average molecular weight: 203,000
[0102] <g-2> A hydrogenated block copolymer consisting of a polymer block R of a vinyl aromatic compound constituting the hard segment and a copolymer block S of a vinyl aromatic compound and a conjugated diene constituting the soft segment, manufactured by Asahi Kasei Corporation, "Tuftec (registered trademark) SOES1609" Hydrogenation: Selective hydrogenation Glass transition temperature: 17℃ Polymer block R: styrene Copolymer block S: styrene and butadiene ·Weight average molecular weight; 203,000
[0103] [Evaluation method] The crosslinked thermoplastic elastomer compositions in the following Examples and Comparative Examples were evaluated as follows. For the measurement of (2) below, a sheet (120 mm wide, 80 mm long, 2 mm thick) was used which was obtained by injection molding using an in-line screw type injection molding machine ("IS130" manufactured by Toshiba Machine Co., Ltd.) under conditions of an injection pressure of 50 MPa, a cylinder temperature of 220°C, and a mold temperature of 40°C. For the measurements of (3) and (4), each crosslinked thermoplastic elastomer composition was used and injection molded using an in-line screw type injection molding machine ("SE-180" manufactured by Sumitomo Machine Co., Ltd.) under conditions of an injection pressure of 50 MPa, a cylinder temperature of 220°C, and a mold temperature of 40°C to obtain a sheet (100 mm wide, 345 mm long, 2 mm thick), which was then cut to a size of 30 mm wide and 125 mm long.
[0104] (1) Melt flow rate (MFR) The measurement was performed in accordance with the JIS K7210 standard at a measurement temperature of 230°C and a measurement load of 21.2 N. The higher the melt flow rate value, the better the injection moldability is evaluated to be.
[0105] (2) Duro A hardness According to JIS K6253 (JIS-A), the value was measured 15 seconds after pressing the needle against the test piece. The lower the Duro A hardness value, the better the flexibility of the crosslinked thermoplastic elastomer composition is evaluated to be. In particular, for use as a seal material for automobile doors, a value of less than 60 is preferable.
[0106] (3) Abrasion resistance / wear loss The weight loss was measured after 10,000 strokes under a load of 500g using a Gakushin trial friction tester conforming to JIS L849. The measured values were evaluated according to the following criteria. ◎: Wear loss of 100mg or less 〇: Wear loss 100~130mg ×: Wear loss of 130 mg or more ××: Measurement not possible due to breakage occurring before the specified condition (10,000 times) is achieved
[0107] (4) Abrasion resistance / appearance after abrasion test The appearance of the test piece was visually evaluated after 10,000 strokes under a load of 500g using a Gakushin trial friction tester conforming to JIS L849. The evaluation was made on the following five-point scale. 5: Wear is observed on the surface of the test piece, but is barely noticeable. 4: Wear is observed on the surface of the test piece, but is not very noticeable. 3: Wear is visible on the surface of the test piece and is noticeable. 2: Wear is visible on the surface of the test piece and is very noticeable 1: Significant wear is observed on the surface of the test piece, and is very noticeable The criteria for judgment were as follows: ◎: Rating 5 〇: Rating 4~3 ×: Rating 2 ××: Rating 1
[0108] [Examples / Comparative Examples] <Example 1> A mixture was obtained by blending 100 parts by mass of (A-1), 143 parts by mass of (B-1), 43 parts by mass of (C-1), 1.7 parts by mass of (D-1) (of which, the amount excluding calcium carbonate is 0.7 parts by mass), 1.7 parts by mass of (D-2) (of which, the amount excluding ethylvinylbenzene is 0.9 parts by mass), 0.6 parts by mass of (E-1), 1.4 parts by mass of (E-2), 8.6 parts by mass of (E-3), 8.6 parts by mass of (E-4), and 0.3 parts by mass of (F-1) in a Henschel mixer for 1 minute. This mixture was fed into the feed section of a co-rotating twin-screw extruder ("TEX30" manufactured by Japan Steel Works, Ltd., L / D=46, number of cylinder blocks: 12) using a gravimetric feeder, and melt-kneaded by increasing the temperature from the upstream section to the downstream section in the range of 110 to 220°C at a total discharge rate of 25 kg / h, and pelletized to produce a crosslinked thermoplastic elastomer composition. The obtained crosslinked thermoplastic elastomer composition was evaluated as described above in (1) to (4). The obtained results are shown in Table 1.
[0109] <Examples 2 to 8 and Comparative Examples 1 to 3> Pellets of a crosslinked thermoplastic elastomer composition were obtained in the same manner as in Example 1, except that the blending composition was changed as shown in Table 1. The obtained crosslinked thermoplastic elastomer composition was evaluated in the same manner as in Example 1. The results are shown in Table 1. In Table 1, for (D-1), the actual amount is not shown, but rather the amount of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane in (D-1) alone (40% of the actual amount), and for (D-2), the actual amount is not shown, but rather the amount of divinylbenzene in (D-2) alone (55% of the actual amount).
[0110] [Table 1]
[0111] [Evaluation Results] As shown in Table 1, Examples 1 to 8, which correspond to the crosslinked thermoplastic elastomer composition of the present invention, are flexible (evaluated as Duro hardness A) yet are excellent in the evaluation of "abrasion resistance", and also satisfy the fluidity of 1 to 100 g / 10 min (230°C, 21.2 N) suitable for injection molding in terms of moldability. On the other hand, Comparative Example 1 is an example in which the component (D) of the present invention was not used and crosslinking by dynamic heat treatment was not performed, Comparative Example 2 is an example in which the (A-1) of the present invention was not used but instead (a-4) was used, and Comparative Example 3 is an example in which (a-3) was used instead of (A-1) of the present invention, and all of these examples were evaluated as having poor abrasion resistance. [Industrial Applicability]
[0112] The crosslinked thermoplastic elastomer composition of the present invention has the above-mentioned effects, and therefore can be used in a wide range of fields, such as automobile parts such as skins, weather strips, ceiling materials, interior sheets, bumper moldings, side moldings, air spoilers, air duct hoses, and sealants; civil engineering and building material parts such as water-stopping materials, joint materials, window frames, and sealants; sporting goods such as the grips of golf clubs and the grips of tennis rackets; industrial parts such as hose tubes and gaskets; home appliance parts such as hoses and packings; medical parts such as medical containers, gaskets, and packings; food parts such as containers and packings; medical equipment parts; electric wires; and miscellaneous goods. The crosslinked thermoplastic elastomer composition of the present invention is suitable as an automobile sealant and a building material sealant among the above-mentioned, and is suitable as an automobile sealant, particularly an automobile door sealant. [Explanation of symbols]
[0113] 1A, 1B Cross-linked rubber material 2. Automotive sealing materials 3. Automobile door seal materials
Claims
1. A crosslinked thermoplastic elastomer composition comprising the following components (A), (B), and (C), containing 100 to 300 parts by mass of component (B) and 10 to 100 parts by mass of component (C) relative to 100 parts by mass of component (A), and having a crosslinking site in at least a portion of component (A). Component (A): A hydrogenated block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one copolymer block containing butadiene and isoprene, the weight average molecular weight of the hydrogenated block copolymer being less than 350,000. Component (B): A hydrocarbon-based rubber softener. Component (C): Polypropylene resin.
2. The crosslinked thermoplastic elastomer composition according to claim 1, wherein the weight ratio of the contents of the components (B) and (C) (content of component (B) / content of component (C)) is 1.6 or more.
3. 3. The crosslinked thermoplastic elastomer composition according to claim 1, having a durometer hardness A (JIS K6253, after 15 seconds) of less than 60.
4. The crosslinked thermoplastic elastomer composition according to claim 1 or 2, further comprising, as component (E), one or more lubricants selected from fatty acid amides and silicone oils.
5. The crosslinked thermoplastic elastomer composition according to claim 4, wherein the content of the component (E) is 1 to 20 parts by mass per 100 parts by mass of the total amount of the components (A), (B), and (C).
6. A molded article obtained by molding the crosslinked thermoplastic elastomer composition according to claim 1 or 2.
7. The molded article according to claim 6, which is an automobile molded article.
8. The molded article according to claim 7, which is a joining member for an automobile.
9. 9. The molded article according to claim 8, which is a sealing member for an automobile, and a composite member for an automobile having this sealing member for an automobile.
10. 10. The automotive composite member according to claim 9, which is an automotive door seal member.
11. A method for producing a crosslinked thermoplastic elastomer composition, comprising melt-kneading a mixture at 80 to 300°C containing the following components (A), (B) a hydrocarbon-based rubber softener, (C) a polypropylene-based resin, and (D) a crosslinking agent, in such proportions that, relative to 100 parts by mass of component (A), 100 to 300 parts by mass of component (B), 10 to 100 parts by mass of component (C), and 0.1 to 10 parts by mass of component (D) relative to 100 parts by mass of the total amount of (A), (B), and (C). Component (A): A hydrogenated block copolymer having at least two polymer blocks mainly composed of a vinyl aromatic compound and at least one copolymer block containing butadiene and isoprene, the weight average molecular weight of the hydrogenated block copolymer being less than 350,000.
Citation Information
Patent Citations
Automobile weatherstrip
JP1999020479A
Thermoplastic elastomer composition, and joining member and method for manufacturing the same
JP2020125442A
Cited By