Adhesive composition, film, and laminate
A polyester-based adhesive composition with specific structural units addresses the limitations of conventional adhesives by achieving low dielectric properties and flexibility, enhancing signal transmission in FPCs.
Patent Information
- Application Number
- JP2024042989
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-07
AI Technical Summary
Existing adhesives for flexible printed circuit boards (FPCs) fail to meet the requirements of low dielectric constant, low dielectric loss tangent, and high flexibility, with conventional styrene-based elastomers having poor solubility and handling issues, and polyester resins not adequately addressing dielectric properties after curing.
A polyester-based adhesive composition containing specific structural units derived from polystyrene with carboxylic acid methyl ester groups and hydrogenated polybutadiene with hydroxyl groups, combined with (meth)acrylate, organic peroxide, and organic solvent, to achieve low dielectric properties and excellent adhesion.
The adhesive composition exhibits a low dielectric constant and loss tangent, maintaining flexibility and adhesion after curing, suitable for bonding electronic components in FPCs, reducing transmission loss in high-frequency signals.
Smart Images

Figure 2024137840000001 
Figure 2024137840000002 
Figure 2024137840000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an adhesive composition having low dielectric properties, good adhesion to substrates, and excellent flexibility. More specifically, the present invention relates to an adhesive composition suitable for bonding electronic components, particularly for the production of products related to flexible printed circuit boards (hereinafter also referred to as "FPC"). [Background technology]
[0002] As electronic devices become smaller and lighter, the adhesive applications for electronic components are becoming more diverse, and the demand for adhesives to create metal and plastic laminates is increasing. FPC-related products that use adhesives include, for example, flexible copper-clad laminates (hereinafter also referred to as "FCCL") made by laminating copper foil to polyimide film, polyethylene naphthalate film, liquid crystal polymer (LCP) film, etc., FPCs with electronic circuits formed on FCCL, FPCs with reinforced plates made by laminating FPCs and reinforced plates, and multilayer boards made by stacking and bonding FCCL and FPC.
[0003] Adhesives for making FCCLs and FPCs are required to have various properties such as dielectric properties (low dielectric constant, low dielectric tangent) and flex resistance in addition to adhesive properties. In particular, for FPCs involving high-speed signal transmission, dielectric properties are important for reducing the transmission loss of electrical signals in the high-frequency range. Traditionally, styrene-based elastomers have been widely used as adhesive materials with the desired dielectric properties, but because conventional styrene-based elastomers have low solubility and problems with handling, there has been a demand for adhesives that are soluble at higher concentrations and with lower viscosity and have good handling properties.
[0004] For example, Patent Document 1 proposes an adhesive composition that has a sufficiently low relative dielectric constant and dielectric tangent, and a high elongation rate even with a high elastic modulus, and an adhesive sheet using the same, which is an adhesive composition that contains a modified polyphenylene ether resin, a styrene-based elastomer, and a silane coupling agent. However, there is room for improvement, for example, in that the concentration of the adhesive component needs to be reduced to 20% in consideration of handling properties, and because polyphenylene ether resin has a high melting point (softening point) and is hard at room temperature, when the blending ratio is set to fully satisfy the desired dielectric properties, the elastic modulus tends to increase and the elongation rate and flex resistance tend to decrease.
[0005] On the other hand, polyester has excellent heat resistance, chemical resistance, durability, and mechanical strength, and is therefore used in a wide range of applications, including films, PET bottles, fibers, toner, electrical components, adhesives, and pressure sensitive adhesives. In addition, polyester has high polarity due to its polymer structure, and is known to exhibit excellent adhesion to polar polymers such as polyester, polyvinyl chloride, polyimide, and epoxy resin, as well as metal materials such as copper and aluminum. Taking advantage of this property, its use as an adhesive for producing FCCLs and FPCs is being considered.
[0006] For example, Patent Document 2 discloses an adhesive composition containing a polyester resin having a specific glass transition temperature and dielectric loss tangent, which contains a structural unit derived from polyvalent carboxylic acids and a structural unit derived from polyhydric alcohols, as a polyester resin having a lower dielectric constant and a lower dielectric loss tangent than conventional polyester resins, and which is excellent in initial adhesion after curing and long-term durability in a humid and hot environment. Patent Document 3 also discloses an adhesive containing a polyester that exhibits desired dielectric properties by lowering the ester group concentration and decreasing the polarity of the polymer, as a polyester, film, and adhesive composition having excellent solvent solubility, heat resistance, and adhesion, and having low relative dielectric constant and dielectric loss tangent. However, in both of the disclosed techniques, although the dielectric properties before curing are evaluated, the dielectric properties of the film after curing, which are a problem during mounting, are not taken into consideration. In fact, there is no adhesive using a polyester resin that satisfies the recent required level of dielectric properties (relative dielectric constant after curing: 3.0 or less and dielectric loss tangent after curing: 0.0035 or less). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent Publication No. 2022-026390 [Patent Document 2] JP 2022-051543 A [Patent Document 3] JP 2022-068240 A Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a polyester-based resin which forms an adhesive composition which has higher solubility, lower dielectric constant and lower dielectric tangent than those of the prior art, and which has excellent adhesion to copper foil and polyimide film and further excellent flexibility, as well as an adhesive composition, a film and a laminate which use the same. [Means for solving the problem]
[0009] However, in view of the above circumstances, the present inventors conducted extensive research and found that a polyester resin containing a specific structural unit can solve the above problems, thereby completing the present invention.
[0010] That is, the present invention provides: <1> An adhesive composition comprising the following (1): (1) A polyester resin having a structural unit derived from polystyrene with carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene with hydroxyl groups at both ends. <2> An adhesive composition comprising the following (1) and (2): (1) A polyester resin having a structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends, (2) (Meth)acrylate having an isocyanate group <3> An adhesive composition comprising all of the following (1) to (3): (1) A polyester resin having a structural unit derived from polystyrene with carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene with hydroxyl groups at both ends. (2) (Meth)acrylate having an isocyanate group (3)Organic peroxide <4> An adhesive composition comprising all of the following (1) to (4): (1) A polyester resin having a structural unit derived from polystyrene with carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene with hydroxyl groups at both ends. (2) (Meth)acrylate having an isocyanate group (3)Organic peroxide (4) Organic Solvent <5> An adhesive composition comprising all of the following (1) to (5): (1) A polyester resin having a structural unit derived from polystyrene with carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene with hydroxyl groups at both ends. (2) (Meth)acrylate having an isocyanate group (3)Organic peroxide (4) Organic Solvent (5) Polyphenylene ether resin having terminal double bonds <6> An adhesive composition comprising the following (6): (6) A polyester resin having double bonds at both ends, which is a reaction product of a polyester resin having a structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends with a (meth)acrylate having an isocyanate group. <7> An adhesive composition comprising the following (6) and (7): (6) A polyester resin having double bonds at both ends, which is a reaction product of a polyester resin having a structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends with a (meth)acrylate having an isocyanate group. (7)Organic peroxide <8> An adhesive composition comprising all of the following (6) to (8): (6) A polyester resin having double bonds at both ends, which is a reaction product of a polyester resin having a structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends with a (meth)acrylate having an isocyanate group. (7)Organic peroxide (8) Organic Solvents <9> An adhesive composition comprising all of the following (6) to (9): (6) A polyester resin having double bonds at both ends, which is a reaction product of a polyester resin having a structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends with a (meth)acrylate having an isocyanate group. (7)Organic peroxide (8) Organic Solvents (9) Polyphenylene ether resin having terminal double bonds <10> The composition is characterized in that the ratio of the structural unit derived from polystyrene having carboxylate methyl ester groups at both ends to the structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends is 10 to 60:90 to 40 (mass ratio). <1> ~ <9> The adhesive composition according to <11> The above <1> ~ <9> A film obtained by curing the adhesive composition according to claim 1. <12> The above <1> ~ <9> A laminate comprising a film obtained by curing the adhesive composition according to claim 1. It is. Effect of the Invention
[0011] The polyester resin contained in the adhesive composition of the present invention has a low dielectric constant and a low dielectric tangent, particularly a low dielectric tangent, and forms a film that has excellent adhesion and flexibility after curing. In particular, such an adhesive composition is effective as an adhesive for producing a laminate consisting of a metal foil and a plastic film, for example, for bonding electronic materials, and particularly as an adhesive used in the production of FPCs such as FCCL, coverlays, and bonding sheets. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Polyester resin> The adhesive composition of the present invention contains at least a polyester resin having structural units derived from polystyrene having carboxylate methyl ester groups at both ends and structural units derived from hydrogenated polybutadiene having hydroxyl groups at both ends.
[0013] [Polystyrene with carboxylate methyl ester groups at both ends] The polystyrene having methyl carboxylate groups at both ends can be obtained by radical polymerization of a styrene monomer and / or a monomer containing a styrene derivative in an organic solvent using an initiator capable of introducing a methyl carboxylate group. An example of an initiator capable of introducing a methyl carboxylate group is dimethyl 2,2'-azobis(2-methylpropionate). When the dimethyl 2,2'-azobis(2-methylpropionate) is used as the initiator, dimethyl tetramethylsuccinate is generated from a part of it. Since dimethyl tetramethylsuccinate has a methyl ester, it is involved in an ester exchange reaction and inhibits polyester resin polymerization. Therefore, it is preferable to remove as much dimethyl tetramethylsuccinate as possible, which is contained as an impurity in the polystyrene having methyl carboxylate groups at both ends. The content of dimethyl tetramethylsuccinate contained as an impurity in the polystyrene having methyl carboxylate groups at both ends is preferably 2,000 ppm or less, more preferably 1,000 ppm or less, and particularly preferably 500 ppm or less.
[0014] In the present invention, the styrene derivative refers to a styrene derivative having only one vinyl group and having no reactive groups other than the vinyl group. Examples of the styrene derivative include α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, p-methoxystyrene, and p-phenylstyrene. The proportion of the styrene monomer and / or styrene derivative is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 100% by mass, of the raw material monomer component of the polystyrene having methyl carboxylate groups at both ends. In addition, from the viewpoint of versatility and handling, styrene monomer is preferred.
[0015] As long as the effect of the present invention is not hindered, other monomers having only one vinyl group or allyl group other than styrene monomers and the styrene derivatives can be used as the raw material monomers of the polystyrene having methyl carboxylate groups at both ends. In particular, when using a monomer having a reactive group or ester bond other than the vinyl group or allyl group, such as a carboxyl group, a hydroxyl group, or an amino group, as the other monomer, it is necessary to pay attention to the fact that the reactive group or ester bond causes a branched structure in the polyester resin. The proportion of the monomer having a reactive group or ester bond is usually preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 1% by mass or less of the raw material monomer components of the polystyrene having methyl carboxylate groups at both ends. Examples of other monomers include acrylic polymerizable monomers such as methyl acrylate, ethyl acrylate, and n-propyl acrylate.
[0016] The weight average molecular weight (hereinafter sometimes abbreviated as Mw) of the polystyrene having methyl carboxylate groups at both ends is preferably 1,000 or more and 20,000 or less. Since the π electrons of the phenyl group constituting the polystyrene contribute to the adhesion with the copper foil, if the Mw is 1,000 or more, the ratio of the structural unit derived from the polystyrene having methyl carboxylate groups at both ends in the polyester resin increases, and the adhesion is improved. In addition, if the Mw is 20,000 or less, the properties of the polystyrene part are not too strong, and the flexibility due to the structural unit derived from the hydrogenated polybutadiene having hydroxyl groups at both ends is not impaired, and the adhesion can be maintained. The Mw of the polystyrene having methyl carboxylate groups at both ends is more preferably 1,500 or more and 10,000 or less. In the present invention, the weight average molecular weight (Mw) and the number average molecular weight (hereinafter sometimes abbreviated as Mn) refer to the values measured by gel permeation chromatography (GPC) of the soluble matter in tetrahydrofuran (hereinafter sometimes abbreviated as THF). The molecular weight measurement conditions are as follows. Equipment: Tosoh Corporation HLC-8320 Column: TSKGEL SUPERMULTIPORE HZ-H +TSKGEL SUPERMULTIPORE HZ-M Measurement temperature: 40℃ Sample concentration: 1.0g / L (THF solution) Solvent: THF Solution injection volume: 100μL Detector: Refractive index detector Molecular weight calibration curve: Created using standard polystyrene
[0017] [Hydrogenated polybutadiene with hydroxyl groups at both ends] The hydrogenated polybutadiene having hydroxyl groups at both ends is a hydrogenated product of polybutadiene having hydroxyl groups at both ends, and the polybutadiene having hydroxyl groups at both ends is a compound having a polymer chain derived from butadiene and hydroxyl groups at both ends of the polymer chain. The polymer chain derived from butadiene can act as an elastomer, and by having such a polymer chain, it is possible to impart adhesion and flexibility to the polyester resin. The hydrogenated polybutadiene having hydroxyl groups at both ends preferably has an average of 1.8 to 2.5 hydroxyl groups in the molecule. By having 1.8 or more hydroxyl groups in the molecule, the polymerization of the polyester resin can be increased in molecular weight without stopping, and by having 2.5 or less, gelation of the polyester resin due to crosslinking is suppressed, and the molecular weight can be increased, making it easier to obtain the excellent effects of the present invention.
[0018] Commercially available hydrogenated polybutadiene having hydroxyl groups at both ends can be used as is. Examples of commercially available hydrogenated polybutadiene having hydroxyl groups at both ends include NISSO-PB (registered trademark) GI-1000, GI-2000, and GI-3000 (all trade names, manufactured by Nippon Soda Co., Ltd.), Krasol (registered trademark) HLBH-P2000, and HLBH-P3000 (all trade names, manufactured by Cray Valley). These may be used alone or in combination of two or more types depending on the amount of hydroxyl groups in the molecule.
[0019] From the viewpoint of the balance between viscosity and adhesive strength, the Mn of the hydrogenated polybutadiene having hydroxyl groups at both ends is preferably from 500 to 100,000, more preferably from 700 to 50,000, and most preferably from 900 to 10,000.
[0020] The hydrogenated polybutadiene having hydroxyl groups at both ends is most preferably GI-3000 (Mn 3,920) in consideration of the number average molecular weight, weight average molecular weight and amount of hydroxyl groups in the molecule of the hydrogenated polybutadiene.
[0021] [Ratio of polystyrene with carboxylate methyl ester groups at both ends and hydrogenated polybutadiene with hydroxyl groups at both ends] The ratio of polystyrene having carboxylate methyl ester groups at both ends and hydrogenated polybutadiene having hydroxyl groups at both ends constituting the polyester resin is preferably 10-60:40-90 (mass%), taking into consideration the amount of polyester resin having hydroxyl groups at both ends produced and the weight average molecular weight, which will be described later. By setting it within the above range, an adhesive composition having an excellent balance between the improvement of film strength and adhesion due to the structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and the flexibility due to the structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends is obtained. Preferably, polystyrene having carboxylate methyl ester groups at both ends: hydrogenated polybutadiene having hydroxyl groups at both ends is 15-55:45-85 (mass%), more preferably 20-50:50-80 (mass%).
[0022] [Polyester resin with hydroxyl groups at both ends] The polyester resin used in the adhesive composition of the present invention forms a film by a crosslinking reaction via terminal hydroxyl groups. Specifically, a polyester resin having hydroxyl groups at both ends is cured using a (meth)acrylate having an isocyanate group or a polyisocyanate curing agent described below. Therefore, in order to obtain a film that satisfies the desired effect, it is preferable that the polyester resin used in the present invention contains a large amount of polyester resin having hydroxyl groups at both ends in addition to the design that takes into consideration both the adhesion and balance described above. The polyester resin having hydroxyl groups at both ends is sufficiently produced even with the above ratio, but it can usually be increased by increasing the number of moles of hydrogenated polybutadiene having hydroxyl groups at both ends relative to the number of moles of polystyrene having carboxylate methyl ester groups at both ends.
[0023] [Polyol other than hydrogenated polybutadiene with hydroxyl groups at both ends] In preparing the polyester resin, a polyol capable of reacting with the polystyrene having carboxylate methyl ester groups at both ends (hereinafter also referred to as "other polyol") may be used in combination with the hydrogenated polybutadiene having hydroxyl groups at both ends.
[0024] From the viewpoint of flexibility, the ratio of hydrogenated polybutadiene having hydroxyl groups at both ends is preferably 70% by mass or more, more preferably 80% by mass or more, based on the total amount of polyols (total of hydrogenated polybutadiene having hydroxyl groups at both ends and other polyols). The polyol may be composed only of hydrogenated polybutadiene having hydroxyl groups at both ends. The content of other polyols is preferably 0 to 30% by mass, more preferably 0 to 10% by mass, based on the total amount of polyols.
[0025] Examples of the other polyols include dimer diols, bisphenol skeleton-containing monomers, aliphatic polyhydric alcohols, alicyclic polyhydric alcohols, aromatic polyhydric alcohols, polyester resin polyols, polyether polyols, polyacrylate polyols, polycarbonate polyols, polysiloxane polyols, polyisoprene polyols, polyolefin polyols, etc. The other polyols may be used alone or in combination of two or more.
[0026] In the present invention, the compound constituting the polyester resin preferably contains dimer diols as other polyols. Examples of dimer diols include dimer diols which are reduction products of dimer acids (mainly those having 36 to 44 carbon atoms) derived from oleic acid, linoleic acid, linolenic acid, erucic acid, etc., and hydrogenated products thereof. Among them, hydrogenated products are preferred from the viewpoint of suppressing gelation during the production of the polyester resin.
[0027] When dimer diols are contained as other polyols, the content of the dimer diols relative to the total amount of polyols is preferably 1 to 20% by weight. The content of the dimer diols relative to the total amount of polyester resin is preferably 0.5 to 10% by weight. When the dimer diols are contained in an amount of 0.5% or more, the adhesion tends to improve, and when the dimer diols are contained in an amount of 10% by weight or less, the dielectric tangent value becomes preferable.
[0028] [Other raw materials that make up polyester resin] Polyester resin may contain polyvalent carboxylic acids. Examples of polyvalent carboxylic acids constituting polyester resin include dimer acids and condensed polycyclic aromatic compounds. Examples of dimer acids include dimer acids (mainly those having 36 to 44 carbon atoms) derived from oleic acid, linoleic acid, linolenic acid, erucic acid, etc., and hydrogenated products thereof. Among them, hydrogenated products are preferred from the viewpoint of suppressing gelation during the production of polyester resin. As the condensed polycyclic aromatic compound, examples of the condensed polycyclic aromatic compound of polyvalent carboxylic acids include naphthalenedicarboxylic acid, dimethyl naphthalenedicarboxylate, anthracene dicarboxylic acid, etc., among which naphthalenedicarboxylic acids are preferred from the viewpoint of price and availability, and dimethyl naphthalenedicarboxylate is more preferred from the viewpoint of reactivity. These can be used alone or in combination of two or more kinds. When polyvalent carboxylic acids are contained, the content of the polyvalent carboxylic acids is preferably 0.5 to 10 mass%. When the polyvalent carboxylic acid is contained at 0.5% by mass, the adhesion tends to improve, and when it is contained at 10% by mass or less, the dielectric tangent value becomes preferable.
[0029] [General raw material compounds that make up polyester resins] The polyester resin preferably has an ester group concentration of 500 eq / g or less. The low ester group concentration reduces the polarity of the polymer, thereby exhibiting low dielectric properties. The ester group concentration is preferably 400 eq / g or less, more preferably 300 eq / g or less.
[0030] [Calculation method for ester group concentration] The reciprocal of the weight-average molecular weight of the units formed from each acid component and each glycol component is 2×10 6 For example, in the case of a polyester resin consisting of polystyrene (Mw 5,040) with carboxylate methyl ester groups at both ends and GI-3000 (Mw 5,380), taking into account the methanol (molecular weight 32) that is eliminated, the weight-average molecular weight of the product unit is Mw = (5,040 + 5,380 - 32 × 2) = 10,356, so the ester group concentration is 193 eq / 106 g. Here, the product unit consisting of glycol (chemical formula 1) and polystyrene with methyl ester groups at both ends (chemical formula 2) means (chemical formula 3).
[0031] [ka]
[0032] [ka]
[0033] [ka]
[0034] [Production of polyester resin] Since polycondensation by ester exchange reaction between functional groups at the polymer terminals generally has low reactivity, it is preferable to use an organic solvent that can act as a compatibilizer for both polystyrene having carboxylate methyl ester groups at both ends and hydrogenated polybutadiene having hydroxyl groups at both ends in order to promote the reaction between them. Furthermore, a catalyst that promotes the ester exchange reaction can also be used in combination. Polycondensation can be carried out by distilling off the by-product methanol from the system while keeping the organic solvent that can act as a compatibilizer in the system. Thereafter, volatile components including the organic solvent are distilled off under reduced pressure to obtain a polyester resin having hydroxyl groups at both ends with a high molecular weight.
[0035] The organic solvent is preferably one or a mixture of two or more selected from aromatic organic solvents such as toluene, xylene, solvent naphtha, and Solvesso (registered trademark). From the viewpoint of the solubility of polystyrene having methyl carboxylate groups at both ends and hydrogenated polybutadiene having hydroxyl groups at both ends and the transesterification reaction temperature, xylene is particularly preferred. The amount of the organic solvent used may be an amount that can adjust the viscosity to promote the reaction. The amount of the organic solvent used is preferably 10 to 50 parts by mass relative to 100 parts by mass of the solute. By using an organic solvent in an amount of 10 parts by mass or more, the effect of compatibilization is sufficiently exhibited, and by using an organic solvent in an amount of 50 parts by mass or less, the transesterification reaction is promoted.
[0036] Examples of catalysts that can be used to promote the transesterification reaction include titanium compounds such as tetra-n-butyl titanate, tetraisopropyl titanate, and titanium oxyacetylcetonate, antimony compounds such as antimony trioxide and tributoxyantimony, germanium compounds such as germanium oxide and tetra-n-butoxygermanium, and acetates of magnesium, iron, zinc, manganese, cobalt, aluminum, etc. These catalysts can be used alone or in combination of two or more.
[0037] The temperature in a typical transesterification reaction between polystyrene having carboxylate methyl ester groups at both ends and hydrogenated polybutadiene having hydroxyl groups at both ends and other raw material compounds is 140 to 220°C, and the reaction time is 4 to 8 hours.The temperature in a typical polycondensation reaction is 160 to 240°C, and the reaction time is 4 to 20 hours.
[0038] [Crystallization of polyester resin] In the present invention, the polyester resin is preferably non-crystalline from the viewpoint of solubility in organic solvents and solution stability. A non-crystalline resin refers to a resin that has a glass transition temperature but does not have a melting point, and the presence or absence of crystallinity can be confirmed by the presence or absence of an endothermic peak due to crystal melting using a differential scanning calorimeter used for measuring the glass transition temperature described below.
[0039] [Glass transition temperature (Tg) of polyester resin] The Tg of the polyester resin used in the present invention is preferably −50 to 0° C., more preferably −40 to −15° C., and particularly preferably −35 to −25° C. The polyester resin of the present invention does not lose flexibility even after curing because it contains polybutadiene having hydroxyl groups at both ends.
[0040] The method for measuring Tg is as follows: Tg is determined by measurement using a differential scanning calorimeter. Equipment: Discovery DSC25 manufactured by TA Instruments Japan Co., Ltd. Sample amount: 10 mg of resin Measurement method: In a nitrogen atmosphere, the sample was heated to 150°C (first heating), maintained at that temperature for 10 minutes, then cooled to -100°C at a rate of 10°C / min, maintained at that temperature for 10 minutes, and then heated at a rate of 10°C / min (second heating). Glass transition temperature: In the DSC curve obtained by the second heating, the intersection point (intersection 1) of a straight line extending the baseline on the low temperature side toward the high temperature side and a tangent line showing the maximum slope from the rising part of the peak to the peak apex, and the intersection point (intersection 2) of a straight line extending the baseline on the high temperature side toward the low temperature side and a tangent line showing the maximum slope from the rising part of the peak to the peak apex, are taken as the glass transition temperature. The temperature midway between the temperatures indicated by intersection 1 and intersection 2 is taken as the glass transition temperature.
[0041] [Dielectric properties of polyester resin] (Dielectric constant (Dk)) The relative dielectric constant of the polyester resin used in the present invention at a frequency of 10 GHz under an environment of a temperature of 23° C. and a relative humidity of 50% RH is preferably 2.8 or less, more preferably 2.6 or less, particularly preferably 2.5 or less, and even more preferably 2.4 or less. By setting the relative dielectric constant within the above range, the transmission speed when used as a substrate can be maintained and transmission loss can be suppressed. (Dielectric loss tangent (Df)) The polyester resin used in the present invention has a dielectric loss tangent of 0.0040 or less, preferably 0.0030 or less, and more preferably 0.0025 or less at a frequency of 10 GHz under an environment of a temperature of 23° C. and a relative humidity of 50% RH. By setting the dielectric loss tangent to the above range, the transmission loss when used in a substrate can be suppressed.
[0042] Polyester resins have terminal hydroxyl groups that increase the dielectric tangent, but because the concentration of ester groups is extremely low, the dielectric tangent before curing is also kept low.
[0043] The dielectric constant and dielectric loss tangent can be determined by the cavity resonator perturbation method using a network analyzer (Agilent Technologies E8361A) and a cylindrical cavity resonator (Kanto Electronics Application Development CP531). If the polyester resin is highly adhesive and it is difficult to prepare a measurement sample on its own, it is measured while inserted into a PTFE tube, and the dielectric properties of the polyester resin alone are calculated by subtracting the weight of the PTFE tube.
[0044] Thus, in the present invention, a polyester resin having a very small dielectric tangent can be obtained compared to conventional polyester resins. Since the polyester resin has a very small dielectric tangent, it is very useful as a raw material for adhesives used for bonding electronic materials and components, because it can suppress transmission loss in the high frequency range.
[0045] [Weight average molecular weight (Mw) of polyester resin] The Mw of the polyester resin used in the present invention is preferably 10,000 to 400,000, more preferably 20,000 to 300,000, and particularly preferably 50,000 to 250,000. When the Mw is higher than 10,000, the adhesion is good, and problems such as the polyester resin of the adhesive layer flowing and seeping out during press processing in producing flexible laminates such as FCCL and FPC can be prevented. Furthermore, when the Mw is lower than 400,000, the solution viscosity during coating can be kept within an appropriate range, and a uniform coating film can be obtained.
[0046] <(Meth)acrylate having an isocyanate group> The adhesive composition of the present invention preferably contains a (meth)acrylate having an isocyanate group. By containing a (meth)acrylate having an isocyanate group, it is possible to harden the resin by crosslinking with a radical polymerization initiator such as an organic peroxide after or simultaneously with the introduction of a terminal double bond into the polyester resin via a terminal hydroxyl group.
[0047] The reaction for introducing a double bond into the terminal hydroxyl group of the polyester resin can be carried out, for example, by applying an adhesive composition containing a (meth)acrylate having an isocyanate group to a substrate and then heating the composition to a temperature of 40 to 150°C.
[0048] Another embodiment of the adhesive composition of the present invention is an adhesive composition containing a polyester resin having a double bond introduced at both ends by reacting a polyester resin with a (meth)acrylate having an isocyanate group in advance. The adhesive composition is obtained as a solution by, for example, dissolving a polyester resin in an organic solvent that can be included in the adhesive composition described below, and then adding a (meth)acrylate having an isocyanate group at 30 to 120°C and reacting it. In order to promote the reaction between the polyester resin and the (meth)acrylate having an isocyanate group, a catalyst can be used in combination. In addition, a polymerization inhibitor can be used in combination to suppress the polymerization reaction of the double bond.
[0049] Examples of catalysts for promoting the reaction between polyester resins and (meth)acrylates having an isocyanate group include titanium compounds such as tetra-n-butyl titanate, tetraisopropyl titanate, and titanium oxyacetylcetonate; antimony compounds such as antimony trioxide and tributoxyantimony; germanium compounds such as germanium oxide and tetra-n-butoxygermanium; bismuth catalysts such as bismuth tris(2-ethylhexanoate); and acetates of magnesium, iron, zinc, manganese, cobalt, and aluminum. These catalysts can be used alone or in combination of two or more. Among these, bismuth catalysts capable of suppressing the decomposition of polyester resins are particularly preferred. The amount of catalyst added is preferably in the range of 0.01 to 0.1% by mass based on the total amount of (meth)acrylates having an isocyanate group.
[0050] Examples of polymerization inhibitors for suppressing the polymerization reaction of double bonds include hydroquinone, p-methoxyphenol, 2,6-di-tert-butyl-p-cresol (hereinafter also referred to as BHT), pyrogallol, β-naphthol, etc. The amount of the polymerization inhibitor added is preferably within a range of 0.01 to 1% by mass based on the total amount of the (meth)acrylate having an isocyanate group.
[0051] In either case, the introduction of a double bond at the end of the polyester resin can be confirmed by IR measurement of the adhesive layer in the case of a polyester resin and a (meth)acrylate having an isocyanate group, or by IR measurement of the adhesive composition in the case of a polyester resin having a double bond introduced at both ends by reacting a polyester resin with a (meth)acrylate having an isocyanate group in advance. -1 This can be confirmed by the decrease or disappearance of the absorption bands attributable to the isocyanate in the vicinity. In the latter case, the amount introduced can be confirmed by measuring the hydroxyl value before and after the reaction. If the measured hydroxyl value after the reaction is decreased, it means that a double bond has been introduced into the terminal hydroxyl group of the polyester resin.
[0052] [Hydroxyl value] The acid value and hydroxyl value in the present invention are values measured in accordance with the standard of JIS K0070. The acid value used to calculate the hydroxyl value is also a value measured in accordance with the standard of JIS K0070.
[0053] Examples of the (meth)acrylate having an isocyanate group include methacryloyl isocyanate, 3-isopropenyl-α,α-dimethylbenzyl isocyanate, and 2-isocyanateethyl methacrylate.
[0054] As the (meth)acrylate having an isocyanate group, commercially available products can be used, such as the Karenz (registered trademark, omitted in the following paragraph) series (manufactured by Resonac Co., Ltd.). Examples include Karenz MOI, Karenz AOI, Karenz MOI-EG, Karenz BEI, Karenz MOI-BP, Karenz MOI-BM, Karenz MOI-EM, etc. In the present invention, Karenz AOI or Karenz MOI is preferred from the viewpoints of reactivity, low dielectric properties, etc.
[0055] The amount of the (meth)acrylate having an isocyanate group added is usually 0.1 to 10 parts by mass, and preferably 0.3 to 6 parts by mass, based on 100 parts by mass of the polyester resin from the viewpoints of dielectric properties and crosslinkability.
[0056] <Organic peroxide> The adhesive composition of the present invention may further contain an organic peroxide. The organic peroxide is not particularly limited as long as it is chemically stable in storage even when mixed with the adhesive composition and promotes crosslinking by polymerization reaction of the double bond introduced to the polyester resin terminal at an appropriate temperature during use. For example, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxide)hexane, 2,5-dimethyl-2,5-di(t-butylperoxide)hexyne-3, α,α'-di(t-butylperoxy)diisopropylbenzene, etc. can be mentioned. One or more kinds of organic peroxides can be mixed and used. The content of the organic peroxide is usually 0.1 to 10 parts by mass, preferably 1 to 5 parts by mass, based on 100 parts by mass of the total of the polyester resin and the modified polyphenylene ether resin described later.
[0057] <Organic solvent> In addition, the adhesive composition of the present invention may further contain an organic solvent that the polyester resin is soluble in. By containing the organic solvent, the viscosity of the adhesive composition when applied to a substrate can be adjusted to an appropriate range, making it easy to handle when forming a coating film.
[0058] The organic solvent is preferably an aromatic organic solvent such as xylene used in producing a polyester resin, but may also be an alicyclic hydrocarbon organic solvent such as methylcyclohexane or ethylcyclohexane; a ketone organic solvent such as methyl ethyl ketone, methyl isobutyl ketone, or cyclohexanone; an alcohol organic solvent such as methyl alcohol, ethyl alcohol, isopropyl alcohol, or isobutyl alcohol; an ester organic solvent such as ethyl acetate or normal butyl acetate; an acetate organic solvent such as cellosolve acetate or methoxy acetate; or a mixture of two or more of these organic solvents. The amount of the organic solvent used is not particularly limited, and may be an amount that can be adjusted to an optimal viscosity when the adhesive composition of the present invention is applied. The amount of the organic solvent used is preferably 10 to 150 parts by mass relative to 100 parts by mass of the solute.
[0059] <Co-crosslinked component> The adhesive composition of the present invention may further contain a co-crosslinking component capable of co-crosslinking with a polyester resin having a terminal double bond introduced therein. By co-crosslinking, the adhesion is somewhat lowered compared to the case where the co-crosslinking is not performed, but the durability (tensile strength) can be improved, so that an adhesive layer having a good balance between adhesion and durability can be obtained. Examples of the co-crosslinking component include triallyl isocyanurate, monoalkyl diallyl isocyanurate, diallyl isocyanurate containing a phosphorus-based substituent, and modified polyphenylene ether resin having a terminal double bond. Among them, modified polyphenylene ether resin having a terminal double bond is preferred.
[0060] [Modified polyphenylene ether resin] From the viewpoint of reactivity with a polyester resin having a terminal double bond introduced therein and the dielectric properties of the adhesive, it is preferable that the modified polyphenylene ether resin has at least one type of ethylenically unsaturated bond (e.g., a (meth)acryloyl group, a vinylbenzyl group) at both ends.
[0061] An example of a modified polyphenylene ether resin is a modified polyphenylene ether resin having vinylbenzyl groups at both ends, which can be obtained, for example, by subjecting a difunctional phenol compound and a monofunctional phenol compound to oxidative coupling to obtain a difunctional phenylene ether oligomer, and then converting the terminal phenolic hydroxyl groups of the difunctional phenylene ether oligomer to vinylbenzyl etherification.
[0062] The Mw of the modified polyphenylene ether resin is preferably 1,000 to 4,000 from the viewpoints of compatibility with polyester-based resins and conformability to unevenness when the substrate and the wiring pattern side of a wiring-equipped resin substrate having a wiring pattern are thermally cured (pressed) via an adhesive layer.
[0063] Specific examples of modified polyphenylene ether resins that can be used include OPE-2St (modified polyphenylene ether resin having vinylbenzyl groups at both ends), OPE-2EA (modified polyphenylene ether resin having acryloyl groups at both ends, both manufactured by Mitsubishi Gas Chemical Company), and NORYL (registered trademark) SA9000 (modified polyphenylene ether resin having methacryloyl groups at both ends, manufactured by SABIC).
[0064] The content of the modified polyphenylene ether resin in the adhesive composition is 3 to 60 parts by mass, preferably 5 to 50 parts by mass, based on 100 parts by mass of the total of the polyester resin and the modified polyphenylene ether resin of the present invention. By making the content of the modified polyphenylene ether resin 60 parts by mass or less, it is possible to improve the bending resistance. Furthermore, by making the content of the modified polyphenylene ether resin 3 parts by mass or more, it is possible to improve the heat resistance. The polyphenylene ether resin may be used alone or in combination of two or more kinds.
[0065] In addition to the components listed above, the adhesive composition of the present invention may contain a conjugated diene polymer, a styrene elastomer, a modified styrene elastomer, or the like depending on the desired effect or purpose.
[0066] [Conjugated diene polymer] Examples of the conjugated diene polymer include a polymer obtained by polymerizing a conjugated diene hydrocarbon, or a copolymer obtained by copolymerizing a conjugated diene hydrocarbon with a monoolefin unsaturated compound, which may be contained in the adhesive composition. Specific examples of the conjugated diene polymer include butadiene polymer, isoprene polymer, and chloroprene polymer.
[0067] [Styrene-based elastomers, modified styrene-based elastomers] The adhesive composition may also contain a styrene-based elastomer or a modified styrene-based elastomer. Specific examples of the styrene-based elastomer include styrene-butadiene block copolymer, styrene-ethylene propylene block copolymer, styrene-butadiene-styrene block copolymer, styrene-isoprene-styrene block copolymer, styrene-ethylenebutylene-styrene block copolymer, and styrene-ethylenepropylene-styrene block copolymer, and specific examples of the modified styrene-based elastomer include those obtained by modifying these block copolymers with an unsaturated carboxylic acid. These various styrene-based elastomers may contain only one type, or may contain two or more types. Among the copolymers, styrene-ethylenebutylene-styrene block copolymer and styrene-ethylenepropylene-styrene block copolymer are preferred from the viewpoints of adhesiveness and electrical properties.
[0068] [Other ingredients] The adhesive composition of the present invention may contain other components other than those listed above in order to further improve its functionality. Examples of other components include inorganic fillers, coupling agents such as silane coupling agents, ultraviolet inhibitors, antioxidants, plasticizers, fluxes, flame retardants, colorants, dispersants, emulsifiers, elasticity reducing agents, diluents, defoamers, ion trapping agents, leveling agents, and catalysts. The content of other components is preferably 70% by mass or less, more preferably 0.05 to 60% by mass, particularly preferably 0.1 to 50% by mass, and even more preferably 0.2 to 40% by mass, based on the total amount of the adhesive composition of the present invention.
[0069] <Film> The film can be obtained by curing the adhesive composition or the adhesive layer. Here, the adhesive layer refers to a layer made of a coating and dried product of the adhesive composition formed on a substrate film or metal foil, and refers to a state in which at least the organic solvent has almost completely evaporated and the fluidity has been lost (generally referred to as "B stage" in this technical field). In addition, curing refers to polymerizing the terminal double bonds in the adhesive or adhesive layer to crosslink them. In the present invention, the adhesive layer also refers to a layer that is partially cured as necessary in the production process (a layer that is cured in a later process). The film has the effects of low dielectric properties, excellent adhesion, and excellent flexibility.
[0070] <Film properties> [Glass transition temperature (Tg)] The Tg of the film is preferably −50 to 0° C., more preferably −40 to −10° C., and particularly preferably −30 to −20° C. The polyester resin of the present invention does not lose flexibility even after curing because it contains polybutadiene having hydroxyl groups at both ends.
[0071] [Gel fraction] The degree of crosslinking can be confirmed by the gel fraction of the film. In the present invention, the gel fraction is calculated as a percentage of the mass of insoluble components obtained by immersing the film in tetrahydrofuran at 23°C for 24 hours to the mass of the film before immersion. From the viewpoint of heat resistance and long-term durability under a humid and hot environment, the gel fraction is preferably 40% or more, more preferably 50% or more, particularly preferably 60% or more, and even more preferably 70% or more.
[0072] [Dielectric properties] The dielectric properties of a film depend on the magnitude of the dipole moment in the adhesive component that constitutes the film, and it is known that the presence of polar groups with large dipole moments such as hydroxyl groups enhances the dielectric properties. In the case of a crosslinking system of carboxyl groups and epoxy groups in a conventional adhesive composition (carboxyl group-containing polyester resin + epoxy crosslinking agent), the carboxyl group, which has a small adverse effect on the dielectric tangent, reacts with the epoxy group to generate hydroxyl groups before and after curing, so that the dielectric tangent generally increases with curing. On the other hand, in the adhesive composition of the present invention, since the terminal hydroxyl group of the polyester resin is a primary hydroxyl group, not only can a double bond be easily introduced by the (meth)acrylate having an isocyanate group, but also the amount of hydroxyl groups remaining in the film can be reduced as much as possible, which is effective in maintaining or improving the low dielectric properties of the film. As a result, the film of the present invention has low dielectric properties and low dielectric tangent.
[0073] In particular, the film of the present invention has excellent electrical properties at high frequencies. Specifically, the film of the present invention, which is a preferred embodiment in which a polyester resin having hydroxyl groups at both ends is reacted with a (meth)acrylate having an isocyanate group and then crosslinked with an organic peroxide, has a relative dielectric constant (ε) of 3 or less in a frequency range of 1 to 80 GHz. In a more preferred embodiment of the film of the present invention, the dielectric loss tangent (tan δ) in a frequency range of 1 to 80 GHz is 0.0035 or less, in a further preferred embodiment, it is 0.0030 or less, and in a particularly preferred embodiment, it is 0.0025 or less. By having the relative dielectric constant (ε) and dielectric loss tangent (tan δ) in a frequency range of 1 to 80 GHz in the film of the present invention within the above ranges, it is possible to reduce electrical signal loss in a high frequency range of 3 GHz or more.
[0074] [Adhesion] The adhesive layer of the present invention has sufficient adhesion to both the roughened and glossy surfaces of the copper foil forming the wiring of the FPC. The film of the present invention can be adhered to a copper foil surface with a small degree of roughness. Therefore, the film of the present invention is not easily affected by the roughness, and therefore transmission loss (transmission loss due to the skin effect) can be reduced. In addition, the film of the present invention has sufficient adhesion to polyimide films and LCP films used as substrate materials for FPCs.
[0075] The adhesion can be evaluated by measuring the 180° peel strength (N / cm) using the method described below, and the higher the peel strength value, the better the adhesion to the substrate. The peel strength can be evaluated by cutting a laminate having an adhesive layer with substrates bonded to both sides into a 1 cm wide test piece after curing under a pressure of 0.04 MPa (curing for 2 hours at 130°C, curing for 1 hour at 170°C, or curing for 1 hour at 160°C, curing for 1 hour at 170°C), fixing the test piece to a plastic plate using double-sided tape, and performing a 180° peel test (pulling speed 20 mm / min) using a Tensilon tester (A&D RTC-1150A) in an environment at a temperature of 25°C. Specifically, in a preferred embodiment of the adhesive composition, which can be crosslinked with an organic peroxide after reacting a polyester resin having hydroxyl groups at both ends with a (meth)acrylate having an isocyanate group, the 180° peel strength from a roughened copper foil surface, the 180° peel strength from a roughened copper surface and a polyimide film, and the 180° peel strength from a roughened copper surface and a liquid crystal polymer film are 6 N / cm or more, and in a more preferred embodiment, 7 N / cm or more, and in a particularly preferred embodiment, 8 N / cm or more.
[0076] <Laminate with Adhesive Layer> The laminate having an adhesive layer comprises an adhesive layer made of an adhesive composition, and a substrate film in contact with at least one surface of the adhesive layer.
[0077] In a laminate having an adhesive layer, the thickness of the adhesive layer is preferably 5 to 100 μm, more preferably 10 to 70 μm, and even more preferably 10 to 50 μm. The thicknesses of the base film and the adhesive layer are selected depending on the application, but there is a tendency for the base film to be thinner in order to improve electrical properties.
[0078] Examples of the laminate having an adhesive layer include a coverlay film, a bonding sheet, and a resin-coated copper foil. A coverlay film is a laminate in which it is difficult to peel the adhesive layer from the base film. On the other hand, a bonding sheet is a laminate in which an easily peelable release film is used as the base film, and the release film is peeled off when used for bonding. The bonding sheet may have an adhesive layer between two release films. When the laminate having an adhesive layer is a coverlay film, a release film used for the bonding sheet may be laminated on the surface of the adhesive layer as necessary for storage, etc.
[0079] Examples of the substrate film used in the coverlay film include polyimide film, polyether ether ketone film, polyphenylene sulfide film, aramid film, polyethylene naphthalate film, liquid crystal polymer film, polyethylene terephthalate film, polyethylene film, polypropylene film, TPX film, and fluorine-based resin film, etc. Among these, from the viewpoints of adhesiveness and electrical properties, polyimide film, polyethylene naphthalate film, and liquid crystal polymer film are preferred, and polyimide film and liquid crystal polymer film are more preferred.
[0080] Such substrate films are commercially available, and examples of polyimide films include Kapton (registered trademark, manufactured by Toray-DuPont Co., Ltd.), Xenomax (registered trademark, manufactured by Toyobo Co., Ltd.), Upilex S (registered trademark, manufactured by Ube Industries, Ltd.), and Apical (registered trademark, manufactured by Kaneka Corporation). Examples of polyethylene naphthalate films include Teonex (registered trademark, manufactured by Teijin DuPont Films Co., Ltd.). Examples of liquid crystal polymer films include Copolymen (registered trademark, manufactured by Ningbo JUJIA New Materials Technology Co., Ltd.), Vecstar (registered trademark, manufactured by Kuraray Co., Ltd.), Viac (registered trademark, manufactured by Ise Murata Manufacturing Co., Ltd.), and Pericule LCP (Chiyoda Integre Co., Ltd.). The substrate film can also be made by forming the corresponding resin into a film of a desired thickness.
[0081] Examples of the base film (release film) used in the bonding sheet include polyethylene terephthalate film, polyethylene film, polypropylene film, silicone release-treated paper, polyolefin resin-coated paper, polymethylpentene (TPX) film, fluorine-based resin film, etc. There are no particular limitations as long as it is peelable, but release-treated polyethylene terephthalate film is preferred in terms of availability, cost, and processability during coating and lamination.
[0082] Such release films are also commercially available, and examples that can be used include Lumirror (registered trademark, manufactured by Toray Advanced Film Co., Ltd.), Toyobo Ester (registered trademark) Film (manufactured by Toyobo Co., Ltd.), Aflex (registered trademark, manufactured by AGC Inc.), and Opulent (registered trademark, manufactured by Mitsui Chemicals Tocello Co., Ltd.).
[0083] As a method for producing a laminate having an adhesive layer, for example, the above-mentioned adhesive composition can be applied to the surface of a base film and then dried to produce a laminate having an adhesive layer formed thereon.
[0084] The introduction reaction of the terminal double bond may be carried out, for example, during drying of the adhesive layer. The drying conditions are appropriately designed according to the type and amount of the organic solvent used in the coating liquid, the thickness of the coating liquid, and the difference in the drying device, and are not particularly limited. Drying is carried out, for example, at a temperature of 40 to 150°C for 30 minutes to 3 hours under atmospheric pressure. A drying temperature of 40°C or higher makes it easier to prevent deterioration of electrical properties due to remaining organic solvents, and a drying temperature of 150°C or lower makes it easier to obtain an adhesive layer. Specifically, the drying is carried out by passing the laminate coated with the adhesive composition through a furnace in which hot air drying, far-infrared heating, high-frequency induction heating, etc. are performed.
[0085] <Flexible copper clad laminate> The flexible copper clad laminate has at least one laminated structure in which a base film and a copper foil are bonded together via an adhesive layer. The adhesive layer has excellent adhesion to the copper foil, so that the flexible copper clad laminate of the present invention has excellent shape stability.
[0086] A method for producing a flexible copper clad laminate includes, for example, a method in which a copper foil is placed in surface contact with the adhesive layer of a laminate having an adhesive layer, thermal lamination is performed at 80°C to 150°C, and the adhesive layer is further cured by a curing treatment. The curing treatment conditions can be, for example, 100°C to 200°C, 30 minutes to 6 hours, and 0.01 to 50 MPa. The copper foil is not particularly limited, and it is preferable to use an electrolytic copper foil, a rolled copper foil, or the like.
[0087] It is also possible to manufacture a flexible copper-clad laminate without using a laminate with an adhesive layer. For example, the adhesive composition is applied to the bonded surface of a copper foil and dried in the same manner as for a laminate with an adhesive layer. The remaining substrate film is then placed on the dried adhesive layer, and the adhesive layer is cured by the above-mentioned thermal lamination and curing treatment.
[0088] <Application> The adhesive composition of the present invention has a low dielectric constant and a low dielectric tangent, particularly a low dielectric tangent, and the film obtained using the adhesive composition also has a low dielectric constant and a low dielectric tangent, a high gel fraction, excellent flexibility, and a low elastic modulus, and is effective for bonding substrates made of various materials such as resins and metals, and is particularly suitable as an adhesive for producing a laminate of a metal foil and a plastic film, for example, an adhesive used for bonding electronic material members. Examples of the "electronic material member" in the present invention include flexible printed circuit boards, coverlays, and bonding sheets. Examples of materials produced by bonding electronic material members include flexible laminates such as flexible copper-clad laminates and flexible printed circuit boards. Flexible laminates are, for example, laminates in which "flexible flexible substrate / adhesive layer / conductive metal layer made of copper, aluminum, or an alloy thereof" are laminated in sequence, and the adhesive composition of the present invention can be used as the adhesive constituting the adhesive layer. In addition to the various layers described above, the flexible laminate may further include other insulating layers, other adhesive layers, and other conductive metal layers. EXAMPLES
[0089] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. Unless otherwise specified, all numerical values indicated by "parts" and "%" below are based on mass.
[0090] <Synthesis example of polystyrene (PS) with carboxylate methyl ester groups at both ends> (PS-1) A reaction vessel equipped with a thermometer, a stirrer, a reflux tower, a dropping funnel, and a nitrogen inlet tube was charged with 50 parts by mass of xylene as an organic solvent, and 100 parts by mass of styrene monomer (St) and 19 parts by mass of dimethyl 2,2'-azobis(2-methylpropionate) as an initiator were dropped into the reaction vessel under reflux of xylene over a period of 5.5 hours to carry out radical polymerization.
[0091] After the dropwise addition was completed, the mixture was kept under reflux for 30 minutes, and then the reflux tower was changed to a distillation system. After normal pressure distillation up to 170°C, the initiator decomposition product dimethyl tetramethylsuccinate was distilled under reduced pressure until it was 1,000 ppm or less. The reaction product was then taken out to obtain polystyrene with methyl carboxylate groups at both ends (PS-1).
[0092] (PS-2)~(PS-4) Polystyrenes with carboxylate methyl ester groups at both ends (PS-2) to (PS-4) were synthesized in the same manner as polystyrene with carboxylate methyl ester groups at both ends (PS-1), except that the type of organic solvent and the amount of initiator used in the synthesis were changed as shown in Table 1.
[0093] (PS-5) A pressurizable reaction vessel equipped with a thermometer, a stirrer, a reflux tower, a dropping pump, and a nitrogen inlet tube was charged with 30 parts by mass of cyclohexane as an organic solvent, and the temperature was raised under pressure with stirring until it reached 120°C, after which 100 parts by mass of styrene monomer (St) and 30 parts of dimethyl 2,2'-azobis(2-methylpropionate) as an initiator were dropped over 5.5 hours to carry out radical polymerization. Thereafter, a polystyrene having methyl carboxylate groups at both ends (PS-5) was obtained in the same manner as (PS-1), except that the distillation temperature was changed to 195°C.
[0094] [Table 1]
[0095] <Synthesis of polyester resin (A-1)> In a reaction vessel equipped with a reflux tower equipped with a thermometer, a stirrer, a fractionator filled with toluene in advance, and a nitrogen inlet tube, 25 parts by mass of xylene as an organic solvent, polystyrene (PS-1) with methyl carboxylate groups at both ends, and NISSO-PB (registered trademark) GI-3000 (manufactured by Nippon Soda Co., Ltd.) as a hydrogenated polybutadiene with hydroxyl groups at both ends were charged in the amounts shown in Table 2, and the inside of the reaction vessel was replaced with nitrogen, and the temperature was raised while stirring. When the temperature inside the reaction vessel reached 140°C, tetraisopropyl titanate (trade name: Orgatix (registered trademark) TA-10, manufactured by Matsumoto Fine Chemical Co., Ltd.) was added as a catalyst, and the temperature inside the reaction vessel was further increased from 160°C to 170°C, and the by-product (methanol) was distilled out of the system under xylene reflux, and the transesterification reaction was carried out at normal pressure for 10 hours. The fractionator was then removed and replaced with a distillation system to remove the xylene. After the internal temperature reached 175°C, the pressure inside the reactor was reduced to further increase the molecular weight, and a polyester resin (A-1) was obtained after 20 hours of reduced pressure reaction.
[0096] <Synthesis of polyester resins (A-2) to (A-9)> Polyester resins (A-2) to (A-9) were synthesized in the same manner as (A-1), except that the raw material types and amounts were changed as shown in Table 2-1.
[0097] <Preparation of Organic Solvent Varnishes (B-1) to (B-9) of Polyester Resin> The obtained polyester resins (A-1) to (A-9) were each dissolved in an organic solvent prepared with the ratio of methyl ethyl ketone (MEK) and methylcyclohexane (MCH) shown in Table 2-1 so as to obtain the mass % of the polyester resin shown in Table 2-1, to obtain organic solvent varnishes (B-1) to (B-9) of the polyester resins (A-1) to (A-9).
[0098] [Table 2-1]
[0099] PS: Polystyrene with carboxylate methyl ester groups at both ends GI-3000: Hydrogenated polybutadiene with hydroxyl groups at both ends (product name: GI-3000, manufactured by Nippon Soda Co., Ltd.) Pripol 2033: Dimer diol (product name: Pripol (registered trademark) 2033, manufactured by Croda) TA: Tetraisopropyl titanate (product name: TA-10, manufactured by Matsumoto Fine Chemical Co., Ltd.)
[0100] <Synthesis of organic solvent varnish (B-10) of polyester resin with double bonds at both ends> In a reaction vessel equipped with a reflux tower equipped with a thermometer, a stirrer, a fractionator filled with toluene in advance, and a nitrogen inlet tube, as shown in Table 2-2, polyester resin organic solvent varnish (B-7), a mixture of bismuth tris(2-ethylhexanoate) and 2-ethylhexanoic acid as a catalyst (trade name: Neostan (registered trademark) U-600, manufactured by Nitto Kasei Co., Ltd.), and 2,6-di-tert-butyl-p-cresol (hereinafter sometimes abbreviated as BHT) as a polymerization inhibitor were charged into the reaction vessel, and the inside of the reaction vessel was replaced with nitrogen, and the temperature was raised while stirring. When the temperature inside the reaction vessel reached 80°C, 2-methacryloyloxyethyl isocyanate (trade name: Karenz (registered trademark) MOI, manufactured by Resonac Co., Ltd.) was added as a (meth)acrylate having an isocyanate group over a period of 3 hours. After that, the reaction was continued for another 2 hours, and the IR measurement showed that the 2230 cm -1 It was confirmed that the absorption peak of the isocyanate group of the above disappeared. After that, the reaction vessel was cooled to obtain an organic solvent varnish (B-10) of a polyester resin having double bonds at both ends.
[0101] <Synthesis of organic solvent varnish (B-11, 12) of polyester resin with double bonds at both ends> Except for changing the raw material types and amounts as shown in Table 2-2, organic solvent varnishes of polyester resins with double bonds at both ends (B-11, 12) were synthesized in the same manner as (B-10).
[0102] [Table 2-2]
[0103] U-600: A mixture of bismuth tris(2-ethylhexanoate) and 2-ethylhexanoic acid (product name: Neostan (registered trademark) U-600, manufactured by Nitto Kasei Co., Ltd.) MOI: 2-methacryloyloxyethyl isocyanate (product name: Karenz (registered trademark) MOI, manufactured by Resonac Co., Ltd.) AOI: 2-methacryloyloxyethyl isocyanate (product name: Karenz (registered trademark) AOI, manufactured by Resonac Co., Ltd.)
[0104] The physical properties of the polyester resins (A-1) to (A-12) are shown in Tables 3-1 and 3-2. The physical properties of the polyester resins and the polyester resins having double bonds at both ends were evaluated as follows.
[0105] <Evaluation of physical properties of polyester resin> [Preparation of polyester resin film for evaluation of Dk, Df, and glass transition temperature] The polyester resin organic solvent varnishes (B-1) to (B-12) were applied to a release film so that the thickness after drying would be 25 μm, and the resin film obtained by drying (drying at 100°C for 20 minutes) was then covered with a release film.
[0106] [Measurement of Dk and Df] The release film was peeled off from the resin film, and the Dk and Df at 10 GHz were measured. The measurements were performed in an environment of 25°C and 50% RH using a cavity resonator perturbation method with a network analyzer (Agilent Technologies E8361A) and a cylindrical cavity resonator (Kanto Electronics Application Development CP531). [Acid value and hydroxyl value measurement] The acid value and hydroxyl value were measured in accordance with the standard of JIS K0070.
[0107] [Measurement of glass transition temperature (Tg)] The release film was peeled off from the prepared resin film, and the glass transition temperature was measured using a differential scanning calorimeter (DSC25 manufactured by TA Instruments) at a measurement temperature of −100 to 150° C. and a measurement speed of 10° C. / min.
[0108] The weight average molecular weight (Mw) of the THF soluble portion was measured by gel permeation chromatography (GPC) under the following conditions. Equipment: Tosoh Corporation HLC-8320 Column: TSKGEL SUPERMULTIPORE HZ-H +TSKGEL SUPERMULTIPORE HZ-M Measurement temperature: 40℃ Sample concentration: 1.0g / L (THF solution) Solvent: THF Solution injection volume: 100μL Detector: Refractive index detector Molecular weight calibration curve: Created using standard polystyrene
[0109] [Table 3-1]
[0110] The ester group concentration in Table 3-1 is calculated by multiplying the weight average molecular weight of the unit formed from each acid component and each glycol component by 2×10 6 It is double.
[0111] [Table 3-2]
[0112] <Production Example of Adhesive Composition (C-1)> Into a flask equipped with a thermometer, a stirrer, a reflux tower, and a nitrogen inlet tube, 200 parts by mass of the polyester resin organic solvent varnish (B-1) obtained above (100 parts by mass as polyester resin), 4 parts by mass of 2-methacryloyloxyethyl isocyanate (product name: Karenz (registered trademark) MOI, manufactured by Resonac Co., Ltd.) as a (meth)acrylate having an isocyanate group, and 3 parts by mass of 1,3-di(t-butylperoxyisopropyl)benzene (product name: Perbutyl (registered trademark) P, manufactured by NOF Corporation) as an organic peroxide were added and mixed uniformly to obtain an adhesive composition (C-1).
[0113] <Synthesis Examples of Adhesive Compositions (C-2 to C-9)> Adhesive compositions (C-2) to (C-9) were obtained in the same manner as (C-1), except that the organic solvent varnish, organic peroxide, and co-crosslinking component of the polyester resin used were changed as shown in Table 4-1.
[0114] [Table 4-1]
[0115] MOI: 2-methacryloyloxyethyl isocyanate (product name: Karenz (registered trademark) MOI, manufactured by Resonac Co., Ltd.) PBP: 1,3-di(t-butylperoxyisopropyl)benzene (product name: Perbutyl (registered trademark) P, manufactured by NOF Corporation) PCD: Dicumyl peroxide (product name: Percumyl (registered trademark) D, manufactured by NOF Corporation) TAIC: Triallyl isocyanurate (product name: TAIC (registered trademark), manufactured by Shinryo Corporation) SA9000: Modified polyphenylene ether resin having terminal double bonds (product name: NORYL (registered trademark) SA9000, manufactured by SABIC)
[0116] <Production Example of Adhesive Composition (C-10)> To a flask equipped with a thermometer, a stirrer, a reflux tower, and a nitrogen inlet tube, 200 parts by mass of the organic solvent varnish (B-10) of the polyester resin having double bonds at both ends obtained above (100 parts by mass as polyester resin) and 3 parts by mass of 1,3-di(t-butylperoxyisopropyl)benzene (product name: Perbutyl (registered trademark) P, manufactured by NOF Corporation) as an organic peroxide were added and mixed uniformly to obtain an adhesive composition (C-10).
[0117] <Production Examples of Adhesive Compositions (C-11, 12)> Adhesive compositions (C-11, 12) were obtained in the same manner as (C-10) except that the organic solvent varnish, organic peroxide, and co-crosslinking component of the polyester resin used were changed as shown in Table 4-2.
[0118] [Table 4-2]
[0119] <Film evaluation> [Preparation of film for evaluation of Dk, Df, and glass transition temperature] The adhesive compositions (C-1) to (C-9) were applied to a release film so that the thickness after curing would be 25 μm, and then the film was pretreated (dried at 60°C for 2 hours, then dried at 100°C for 20 minutes) to obtain a B-stage film, which was then covered with a release film and cured (cured at 130°C for 2 hours, then cured at 170°C for 1 hour) to produce a film.
[0120] The adhesive compositions (C-10) to (C-12) were applied to a release film so that the thickness after curing would be 25 μm, and then the B-stage film obtained by pre-treating (drying at 130°C for 10 minutes) was covered with a release film and cured (curing at 160°C for 1 hour, followed by curing at 170°C for 1 hour) to produce a film.
[0121] [Measurement of Dk and Df] The release film was peeled off from the prepared film, and the film was subjected to measurement of Dk and Df at 10 GHz. The measurement of Dk and Df was performed in the same manner as for the resin film.
[0122] [Measurement of glass transition temperature] The release film was peeled off from the prepared film, and the glass transition temperature was measured in the same manner as for the resin film.
[0123] [Creating films for evaluating gel fraction, tensile strength, tensile elongation, and elastic modulus] Adhesive compositions (C-1) to (C-9) were each applied to four release films so that the thickness after curing would be 25 μm, and then pre-treated (dried at 60°C for 2 hours, then dried at 100°C for 20 minutes). The films were then superimposed on each other to achieve the required thickness (100 μm), and then covered with release films and cured (cured at 130°C for 2 hours, then cured at 170°C for 1 hour).
[0124] Adhesive compositions (C-10) to (C-12) were each applied to four sheets of release film so that the thickness after curing would be 25 μm, and then pre-treated (dried at 130°C for 10 minutes). The films were then overlapped to the required thickness (100 μm), covered with release film, and cured (cured at 160°C for 1 hour, then cured at 170°C for 1 hour).
[0125] [Gel fraction] The 100 μm thick film obtained above was cut into a size of 3 cm × 3 cm, and immersed in tetrahydrofuran at 23° C. for 24 hours, and the weight percentage of the remaining insoluble film components relative to the weight of the film before immersion was taken as the gel fraction.
[0126] [Tensile strength, tensile elongation, elastic modulus] The 100 μm thick film obtained above was cut into a dumbbell shape No. 1 as specified in JIS K6251, and the tensile strength, tensile elongation, and elastic modulus were evaluated by a tensile test (tensile speed 50 mm / min) using a Tensilon testing machine (A&D RTG-1210).
[0127] [Preparation of laminate for copper foil adhesion evaluation] The adhesive compositions (C-1) to (C-9) were applied to a release film so that the thickness after curing would be 25 μm, and then pre-treated (dried at 60°C for 2 hours, then dried at 100°C for 20 minutes). The coating was then transferred to the roughened surface of a low-roughness copper foil for high frequencies, and the copper foil was covered with the roughened surface. A laminate was obtained by curing the coating under a pressure of 0.04 MPa (cured at 130°C for 2 hours, then cured at 170°C for 1 hour). [Film thickness] 25μm [Copper foil] Electrolytic copper foil CF-T9DA-SV-18 (manufactured by Fukuda Metal Foil Powder Co., Ltd., thickness 18 μm, roughness of roughened surface Rz 0.7 μm)
[0128] The adhesive compositions (C-10) to (C-12) were applied to a release film so that the thickness after curing would be 25 μm, and then the coating was pretreated (dried at 130°C for 10 minutes), transferred to the roughened surface of a low-roughness copper foil for high frequencies, covered with the roughened surface of the copper foil, and cured under a pressure of 0.04 MPa (cured at 160°C for 1 hour, then cured at 170°C for 1 hour) to obtain a laminate. [Film thickness] 25μm [Copper foil] Electrolytic copper foil CF-T9DA-SV-18 (manufactured by Fukuda Metal Foil Powder Co., Ltd., thickness 18 μm, roughness of roughened surface Rz 0.7 μm)
[0129] [Preparation of polyimide film / copper foil adhesion evaluation laminate] The adhesive compositions (C-1) to (C-9) were applied to a release film so that the thickness after curing would be 25 μm, and then pre-treated (dried at 60°C for 2 hours, then dried at 100°C for 20 minutes). The coating was then transferred to the roughened surface of a low-roughness copper foil for high frequencies, and the coating was covered with a polyimide (hereinafter sometimes abbreviated as PI) film. A laminate was obtained by curing the coating under a pressure of 0.04 MPa (cured at 130°C for 2 hours, then cured at 170°C for 1 hour). [Polyimide film] Kapton (registered trademark) EN (manufactured by Toray DuPont Co., Ltd., thickness 25 μm)
[0130] The adhesive compositions (C-10) to (C-12) were applied to a release film so that the thickness after curing would be 25 μm, and then the coating was pretreated (dried at 130°C for 10 minutes). The coating was then transferred to the roughened surface of a low-roughness copper foil for high frequencies, covered with a polyimide (hereinafter sometimes abbreviated as PI) film, and cured under a pressure of 0.04 MPa (cured at 160°C for 1 hour, then cured at 170°C for 1 hour) to obtain a laminate. [Polyimide film] Kapton (registered trademark) EN (manufactured by Toray DuPont Co., Ltd., thickness 50 μm)
[0131] [Preparation of LCP film / copper foil laminate for evaluation of adhesion] Laminates were obtained in the same manner as for the adhesive compositions (C-5) and (C-12), except that the polyimide film was changed to an LCP film. [LCP film] Copolymen (registered trademark) (Ningbo JUJIA New Material Technology Co., Ltd.)
[0132] [Adhesion] Each of the laminates obtained above for evaluating adhesion was cut into 1 cm width to prepare test pieces. The test pieces were fixed to a plastic plate using double-sided tape and evaluated in a 180° peel test (tensile speed 20 mm / min) using a Tensilon tester (A&D RTC-1150A) in an environment at 25°C.
[0133] <Evaluation Results> The evaluation results are summarized in Table 5. The LCP / copper foil adhesion was 7.5 (N / cm) for Example 5 and 8.0 (N / cm) for Example 12.
[0134] [Table 5]
[0135] PI / copper foil adhesion: Polyimide film / copper foil adhesion
[0136] Tables 3-1, 3-2 and 5 show that the polyester resins (A-1 to 12) satisfying the requirements of the present invention have low dielectric constants and low dielectric tangents, particularly low dielectric tangents, and that the films obtained using them also have low dielectric constants and low dielectric tangents, excellent adhesion to various substrates, high gel fractions, excellent flexibility and low elastic modulus.
Claims
1. An adhesive composition comprising the following (1): (1) A polyester resin having a structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends.
2. An adhesive composition comprising the following (1) and (2): (1) A polyester resin having a structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends, (2) (Meth)acrylate having an isocyanate group
3. An adhesive composition comprising all of the following (1) to (3): (1) A polyester resin having a structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends. (2) (Meth)acrylate having an isocyanate group (3) Organic peroxide
4. An adhesive composition comprising all of the following (1) to (4): (1) A polyester resin having a structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends. (2) (Meth)acrylate having an isocyanate group (3) Organic peroxide (4) Organic Solvent
5. An adhesive composition comprising all of the following (1) to (5): (1) A polyester resin having a structural unit derived from polystyrene having carboxylate methyl ester groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends. (2) (Meth)acrylate having an isocyanate group (3) Organic peroxide (4) Organic Solvent (5) Polyphenylene ether resin having terminal double bonds
6. An adhesive composition comprising the following (6): (6) A polyester resin having double bonds at both ends, which is a reaction product of a polyester resin having a structural unit derived from polystyrene having methyl carboxylate groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends with a (meth)acrylate having an isocyanate group.
7. An adhesive composition comprising the following (6) and (7): (6) A polyester resin having double bonds at both ends, which is a reaction product of a polyester resin having a structural unit derived from polystyrene having methyl carboxylate groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends with a (meth)acrylate having an isocyanate group. (7) Organic peroxide
8. An adhesive composition comprising all of the following (6) to (8): (6) A polyester resin having double bonds at both ends, which is a reaction product of a polyester resin having a structural unit derived from polystyrene having methyl carboxylate groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends with a (meth)acrylate having an isocyanate group. (7) Organic peroxide (8) Organic solvent
9. An adhesive composition comprising all of the following (6) to (9): (6) A polyester resin having double bonds at both ends, which is a reaction product of a polyester resin having a structural unit derived from polystyrene having methyl carboxylate groups at both ends and a structural unit derived from hydrogenated polybutadiene having hydroxyl groups at both ends with a (meth)acrylate having an isocyanate group. (7) Organic peroxide (8) Organic solvent (9) Polyphenylene ether resin having terminal double bonds
10. The adhesive composition according to any one of claims 1 to 9, characterized in that the structural units derived from polystyrene having carboxylate methyl ester groups at both ends:the structural units derived from hydrogenated polybutadiene having hydroxyl groups at both ends = 10 to 60:90 to 40 (mass ratio).
11. A film obtained by curing the adhesive composition according to any one of claims 1 to 9.
12. A laminate comprising a film obtained by curing the adhesive composition according to any one of claims 1 to 9.
Citation Information
Patent Citations
Resin composition and adhesive sheet using the same
JP2022026390A
Polyester-based resin, adhesive composition and adhesive
JP2022051543A
Polyester, film and adhesive composition, as well as adhesive sheet, laminate and printed wiring board
JP2022068240A