Modified ethylene-based polymer composition and production method of the same, olefin-based polymer composition containing the same, and laminate using the same

By integrating an acrylic polymer with specific ethylenically unsaturated compounds, the ethylene polymer composition addresses fish eyes and transparency issues, resulting in a modified ethylene polymer with enhanced adhesion and appearance.

JP2024137909APending Publication Date: 2024-10-07MCPP INNOVATION LLC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024046507
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-22
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing modified ethylene polymer compositions suffer from the occurrence of fish eyes and lack transparency, despite improvements in adhesive properties and mechanical properties.

Method used

Incorporating an acrylic polymer with methyl (meth)acrylate and alkyl (meth)acrylate units into the ethylene polymer composition, along with specific ethylenically unsaturated compounds, to enhance transparency and reduce fish eyes.

Benefits of technology

The modified ethylene polymer composition achieves excellent adhesion, reduced fish eyes, and improved transparency, making it suitable for applications requiring strong adhesive strength and good appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137909000001
    Figure 2024137909000001
Patent Text Reader

Abstract

To provide a modified ethylene-based polymer composition which brings about an excellent reduction effect of fish eye generation and which has excellent transparency while maintaining excellent adhesiveness.SOLUTION: A modified ethylene-based polymer composition contains a modified ethylene-based polymer and an acrylic polymer, wherein the modified ethylene-based polymer is a polymer formed by modifying an ethylene-based polymer with an ethylenically unsaturated compound, the acrylic polymer contains a methyl (meth-)acrylate unit and a 2-18C alkyl (meth-)acrylate unit as constitutional units, and a content of the acrylic polymer in the modified ethylene-based polymer composition is 0.01-4 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a modified ethylene polymer composition and a production method thereof. The present invention also relates to an olefin polymer composition containing the modified ethylene polymer composition, and a laminate using the modified ethylene polymer composition. [Background technology]

[0002] Modified ethylene polymer compositions modified with ethylenically unsaturated compounds, which have excellent adhesive properties, moldability, mechanical properties, and barrier properties against oxygen gas, carbon dioxide gas, etc., have been used in various packaging and container materials, etc.

[0003] In the modified ethylene polymer composition, the amount of the ethylenically unsaturated compound added can be increased by increasing the amount of the ethylenically unsaturated compound used or the amount of the radical generator used, but a large amount of fish eyes are generated due to gelation of the modified ethylene polymer composition, etc.

[0004] In response to this, for example, Patent Document 1 discloses that the occurrence of fisheyes can be reduced by using specific polymers or compounds that constitute the modified ethylene polymer composition. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-036221 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the modified ethylene polymer composition disclosed in Patent Document 1 has room for improvement in terms of reducing the occurrence of fisheyes, and higher transparency is required.

[0007] Therefore, an object of the present invention is to provide a modified ethylene polymer composition which exhibits a good effect of reducing the occurrence of fisheyes while maintaining excellent adhesion and has excellent transparency, and a method for producing the same. Another object of the present invention is to provide an olefin polymer composition containing the modified ethylene polymer composition, and a laminate using the modified ethylene polymer composition. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted extensive research and found that the above-mentioned problems can be solved by allowing a modified ethylene-based polymer composition to contain an acrylic polymer and employing a specific structural unit for the acrylic polymer, thereby completing the present invention. That is, the gist of the present invention is as follows.

[0009] A first aspect of the present invention is a modified ethylene-based polymer composition comprising a modified ethylene-based polymer and an acrylic polymer, the modified ethylene-based polymer being a polymer obtained by modifying an ethylene-based polymer with an ethylenically unsaturated compound, the acrylic polymer comprising, as constituent units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms, and the content of the acrylic polymer in the modified ethylene-based polymer composition is 0.01 to 4 mass%.

[0010] A second aspect of the present invention is the modified ethylene polymer composition of the first aspect, wherein the acrylic polymer is a copolymer containing a methyl methacrylate unit as the methyl (meth)acrylate unit and containing a butyl methacrylate unit and a butyl acrylate unit as the alkyl (meth)acrylate unit having 2 to 18 carbon atoms.

[0011] A third aspect of the present invention is the modified ethylene polymer composition of the first or second aspect, wherein the ethylenically unsaturated compound is a polar ethylenically unsaturated compound having a carboxyl group, a hydroxyl group or an amino group, an anhydride of a polar ethylenically unsaturated compound having a carboxyl group, or an aromatic vinyl compound.

[0012] A fourth aspect of the present invention relates to the modified ethylene polymer composition of the third aspect, wherein the ethylenically unsaturated compound is the polar ethylenically unsaturated compound having a carboxyl group or an anhydride thereof, and the polar ethylenically unsaturated compound having a carboxyl group or an anhydride thereof is an unsaturated dicarboxylic acid or an anhydride thereof.

[0013] A fifth aspect of the present invention relates to the modified ethylene polymer composition according to any one of the first to fourth aspects, wherein the content of the ethylenically unsaturated compound is 0.05 to 10% by mass.

[0014] A sixth aspect of the present invention relates to a modified ethylene polymer composition according to any one of the first to fifth aspects, which has a melt flow rate of 0.05 to 50 g / 10 min as measured at a temperature of 190° C. and a load of 21.2 N in accordance with JIS K 7210:2014, and a density of 0.85 to 0.97 g / cm as measured by an underwater displacement method in accordance with JIS K 7112:1999. 3 It is.

[0015] A seventh aspect of the present invention is a method for producing an olefin polymer composition, comprising mixing the modified ethylene polymer composition according to any one of the first to sixth aspects with an olefin polymer, wherein the mixing ratio of the modified ethylene polymer composition to the olefin polymer is 1:99 to 99:1 (mass ratio).

[0016] An eighth aspect of the present invention is a laminate in which a layer made of the modified ethylene polymer composition according to any one of the first to sixth aspects is bonded to a layer serving as an adherend.

[0017] A ninth aspect of the present invention relates to the laminate of the eighth aspect, wherein the layer that is the adherend is at least one layer selected from the group consisting of thermoplastic resins, metal foils, paper, wood, and fibers.

[0018] A tenth aspect of the present invention is a method for producing a laminate, comprising forming a layer made of the olefin polymer composition obtained by the production method of the seventh aspect, and bonding the layer made of the olefin polymer composition to a layer serving as an adherend.

[0019] An eleventh aspect of the present invention relates to the method for producing a laminate according to the tenth aspect, wherein the layer that is the adherend is at least one layer selected from the group consisting of thermoplastic resins, metal foils, paper, wood, and fibers.

[0020] A twelfth aspect of the present invention is a method for producing a modified ethylene polymer composition, comprising a step of melt-kneading an ethylene polymer, an ethylenically unsaturated compound, an acrylic polymer, and a radical generator, wherein the acrylic polymer contains, as constituent units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms, and the blending amount of the acrylic polymer is 0.01 to 4 parts by mass per 100 parts by mass of the ethylene polymer. Effect of the Invention

[0021] According to the present invention, a modified ethylene polymer composition having excellent transparency and exhibiting a favorable effect of reducing the occurrence of fisheyes while maintaining excellent adhesion can be obtained. Therefore, the modified ethylene polymer composition, the olefin polymer composition containing the same, and the laminate using the same can achieve both excellent adhesion and good appearance, and are very useful. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The following describes in detail the embodiments of the present invention, but the following embodiments are examples (representative examples) of the present invention and the present invention is not limited thereto. The present invention can be carried out in any modified form without departing from the gist of the present invention. In this specification, when "~" is used with a numerical value or a physical property value enclosed therein, the values ​​before and after the "~" are included in the expression. In this specification, "(meth)acrylate" means at least one of acrylate and methacrylate. In addition, "(meth)acrylate" may be written as "(meth)acrylic acid". In addition, in this specification, "mass %" and "weight %", and "parts by mass" and "parts by weight" have the same meaning.

[0023] Modified ethylene polymer composition The modified ethylene-based polymer composition according to the present embodiment includes a modified ethylene-based polymer and an acrylic polymer. The modified ethylene-based polymer composition is mainly composed of the modified ethylene-based polymer. That is, in the modified ethylene-based polymer composition according to the present embodiment, the content of the modified ethylene-based polymer, expressed as mass%, is the highest. The modified ethylene polymer is an ethylene polymer modified with an ethylenically unsaturated compound. The acrylic polymer contains, as constituent units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms. The content of the acrylic polymer in the modified ethylene polymer composition is 0.01 to 4% by mass.

[0024] <Modified ethylene polymer> The modified ethylene polymer in this embodiment is an ethylene polymer modified with an ethylenically unsaturated compound.

[0025] The ethylene polymer before modification may be either an ethylene homopolymer or a copolymer containing ethylene units as a constituent unit.

[0026] When the ethylene polymer is a copolymer, examples of the constituent units other than the ethylene unit include α-olefins having 3 or more carbon atoms, vinyl acetate, (meth)acrylic acid, and (meth)acrylic acid esters. Examples of α-olefins having 3 or more carbon atoms include propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, 4,4-dimethyl-1-pentene, 1-hexene, 4-methyl-1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-octadecene, and the number of carbon atoms of the α-olefin is preferably 3 to 20. The ethylene and other structural units of the ethylene-based polymer may be structural units derived from biomass produced using plants as raw materials. Examples of the biomass ethylene-based polymer include biomass branched low-density polyethylene and biomass linear high-density polyethylene, which contain structural units derived from biomass such as ethylene and other structural units.

[0027] When the ethylene polymer is a homopolymer of ethylene, examples thereof include branched low density polyethylene and linear high density polyethylene.

[0028] When the ethylene polymer is a copolymer, examples thereof include linear low / medium density ethylene-α-olefin copolymers, ethylene resins, and ethylene rubbers.

[0029] Examples of linear low / medium density ethylene-α-olefin copolymers include ethylene-propylene copolymers, ethylene-1-butene copolymers, ethylene-propylene-1-butene copolymers, ethylene-4-methyl-pentene copolymers, ethylene-1-heptene copolymers, ethylene-1-hexene copolymers, and ethylene-1-octene copolymers.

[0030] Examples of ethylene-based resins include ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, ethylene-methyl (meth)acrylate copolymers, ethylene-ethyl (meth)acrylate copolymers, and ethylene-(meth)acrylic acid-methyl (meth)acrylate copolymers.

[0031] Examples of ethylene-based rubbers include ethylene-propylene copolymers, ethylene-1-butene copolymers, and ethylene-propylene-non-conjugated diene copolymers and ethylene-1-butene-non-conjugated diene copolymers obtained by further copolymerizing these copolymers with non-conjugated dienes such as 1,4-hexadiene, dicyclopentadiene, and 5-ethylidene-2-norbornene.

[0032] Among them, the ethylene-based polymer is more preferably a branched low-density ethylene homopolymer or a linear low-density ethylene-α-olefin copolymer. The ethylene-based polymer may be used alone or in combination of two or more kinds.

[0033] The density of the ethylene polymer, as measured by the underwater displacement method in accordance with JIS K 7112:1999, is 0.85 to 0.97 g / cm 3 is preferable, and 0.86 to 0.965 g / cm 3 From the viewpoint of adhesiveness to an adherend when the modified ethylene polymer composition is prepared, the density is more preferably 0.85 g / cm. 3 More than 0.86 g / cm is preferable. 3 More preferably, 0.97 g / cm 3 Less than 0.965 g / cm is preferred. 3 The following is more preferred:

[0034] The melt flow rate (MFR) of the ethylene polymer is preferably 0.1 to 200 g / 10 min, and more preferably 0.5 to 100 g / 10 min, as measured at a temperature of 190° C. and a load of 21.2 N in accordance with JIS K 7210: 2014. From the viewpoint of moldability of the modified ethylene polymer composition, the MFR is preferably 0.1 g / 10 min or more, and more preferably 0.5 g / 10 min or more, and is preferably 200 g / 10 min or less, and more preferably 100 g / 10 min or less.

[0035] The ethylene polymer has a density of 0.85 to 0.97 g / cm 3Furthermore, the MFR is preferably 0.1 to 200 g / 10 min, and the more preferred ranges of the density and MFR are as described above.

[0036] The modified ethylene polymer in this embodiment is a polymer obtained by modifying the above-mentioned ethylene polymer with an ethylenically unsaturated compound.

[0037] The above-mentioned ethylenically unsaturated compound is not particularly limited as long as it is a compound having an ethylenically unsaturated bond.As the ethylenically unsaturated compound, for example, the polar ethylenically unsaturated compound having a carboxyl group, a hydroxyl group or an amino group, the anhydride of the polar ethylenically unsaturated compound having a carboxyl group, etc. may be used as the ethylenically unsaturated compound. The ethylenically unsaturated compounds may be used alone or in combination of two or more.

[0038] Examples of polar ethylenically unsaturated compounds having a carboxyl group or their anhydrides include unsaturated carboxylic acids such as (meth)acrylic acid, crotonic acid, isocrotonic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, and tetrahydrophthalic acid, or their anhydrides. The above-mentioned unsaturated carboxylic acid is a concept that includes those having two or more carboxylic acids, such as unsaturated dicarboxylic acids.

[0039] Examples of the ethylenically unsaturated compound containing a hydroxyl group include p-hydroxystyrene, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, and 2-hydroxybutyl acrylate.

[0040] As the ethylenically unsaturated compound containing an amino group, for example, a primary, secondary or tertiary amino group-containing monomer can be used. More specifically, for example, monomethylaminoethyl acrylate, dimethylaminoethyl acrylate, diethylaminoethyl acrylate, monomethylaminoethyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, dimethylaminopropyl acrylamide, dimethylaminopropyl methacrylamide, allylamine, etc. can be mentioned.

[0041] Examples of the aromatic vinyl compound include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, dimethylstyrene, and chlorostyrene.

[0042] Among these, the ethylenically unsaturated compound is preferably a polar ethylenically unsaturated compound having a carboxyl group or an anhydride thereof, more preferably an unsaturated dicarboxylic acid or an anhydride thereof, from the viewpoint of adhesiveness of the modified ethylene polymer composition. Examples of the unsaturated dicarboxylic acid include maleic acid, fumaric acid, itaconic acid, citraconic acid, and tetrahydrophthalic acid. As mentioned above, from the viewpoint of adhesion, the ethylenically unsaturated compound is preferably maleic acid or maleic anhydride, and particularly preferably maleic anhydride.

[0043] In the present embodiment, the content of the ethylenically unsaturated compound in the modified ethylene polymer composition is preferably 0.05 to 10% by mass, more preferably 0.1 to 5% by mass. From the viewpoint of sufficiently modifying the ethylene polymer and obtaining better adhesiveness as the modified ethylene polymer composition, the content is preferably 0.05% by mass or more, more preferably 0.1% by mass or more. From the viewpoint of further suppressing the occurrence of fisheyes, the content is preferably 10% by mass or less, more preferably 5% by mass or less.

[0044] The density of the modified ethylene polymer in the present embodiment, in which the ethylene polymer is modified with an ethylenically unsaturated compound, measured by an underwater displacement method in accordance with JIS K 7112:1999, is 0.85 to 0.97 g / cm 3 is preferable, and 0.86 to 0.965 g / cm 3 From the viewpoint of adhesiveness to an adherend when the modified ethylene polymer composition is prepared, the density is more preferably 0.85 g / cm. 3 More than 0.86 g / cm is preferable. 3 More preferably, 0.97 g / cm 3 Less than 0.965 g / cm is preferred. 3 The following is more preferred:

[0045] The melt flow rate (MFR) of the modified ethylene polymer in this embodiment, measured in accordance with JIS K 7210: 2014 at a temperature of 190°C and a load of 21.2 N, is preferably 0.1 to 200 g / 10 min, and more preferably 0.5 to 100 g / 10 min. From the viewpoint of moldability of the modified ethylene polymer composition, the MFR is preferably 0.1 g / 10 min or more, and more preferably 0.5 g / 10 min or more, and is preferably 200 g / 10 min or less, and more preferably 100 g / 10 min or less.

[0046] The modified ethylene polymer in the present embodiment has a density of 0.85 to 0.97 g / cm 3 Furthermore, the MFR is preferably 0.1 to 200 g / 10 min, and the more preferred ranges of the density and MFR are as described above.

[0047] <Acrylic Polymer> The acrylic polymer in this embodiment contains, as structural units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms. This improves the apparent fluidity of the modified ethylene polymer composition and suppresses the occurrence of fish eyes. Furthermore, the acrylic polymer has excellent compatibility with the modified ethylene polymer, and the transparency of the modified ethylene polymer composition is also improved.

[0048] The acrylic polymer in this embodiment is a component contained as a polymer processing aid that improves the moldability of the resulting modified ethylene polymer composition. Conventional polymer processing aids are generally materials containing fluorine atoms, such as polymers of fluorinated olefins and copolymers of vinylidene fluoride and fluorinated olefins.

[0049] In contrast, in the modified ethylene polymer composition according to the present embodiment, a specific acrylic polymer is used instead of the above-mentioned conventional polymer processing aid, and thus the composition can achieve the effects of the present invention, such as a favorable effect of reducing the occurrence of fisheyes and excellent transparency while maintaining excellent adhesion. Incidentally, a conventional polymer processing aid containing a fluorine atom may be used together with the acrylic polymer of the present embodiment, so long as the effects of the present invention are not impaired.

[0050] Specifically, the acrylic polymer in this embodiment contains a methyl (meth)acrylate unit as a structural unit, and thus has excellent releasability from metal, that is, excellent lubricity. In particular, from the viewpoint of effectively accumulating at the interface between the modified ethylene polymer and the metal and exhibiting lubricity, the acrylic polymer preferably contains a methyl methacrylate unit. The methyl (meth)acrylate unit may contain both a methyl methacrylate unit and a methyl acrylate unit.

[0051] The acrylic polymer in the present embodiment contains an alkyl (meth)acrylate unit having 2 to 18 carbon atoms as a constituent unit, and thus has excellent compatibility with the modified ethylene polymer.

[0052] The alkyl (meth)acrylate unit may have 2 to 18 carbon atoms, and preferably has 2 to 12 carbon atoms. From the viewpoint of compatibility with the modified ethylene polymer, the carbon number is 2 or more, and more preferably 3 or more. Furthermore, from the viewpoint of suppressing a decrease in the polymerization rate and achieving suitable polymerizability, i.e., good productivity, the carbon number is 18 or less, and preferably 12 or less. The alkyl (meth)acrylate unit having 2 to 18 carbon atoms may contain only one type, or two or more types.

[0053] From the viewpoint of compatibility with the modified ethylene polymer, the alkyl (meth)acrylate unit having 2 to 18 carbon atoms preferably contains a butyl (meth)acrylate unit, more preferably a butyl methacrylate unit and a butyl acrylate unit, and more preferably contains two or more units selected from the group consisting of an n-butyl methacrylate unit, an n-butyl acrylate unit, and an iso-butyl methacrylate unit.

[0054] From the viewpoint of compatibility with the modified ethylene polymer, the acrylic polymer in the present embodiment is preferably a copolymer containing methyl methacrylate units as methyl (meth)acrylate units and containing butyl methacrylate units and butyl acrylate units as alkyl (meth)acrylate units having 2 to 18 carbon atoms.

[0055] The acrylic polymer in the present embodiment may contain, as a structural unit, a structural unit other than the methyl (meth)acrylate unit and the alkyl (meth)acrylate unit having 2 to 18 carbon atoms, as long as the effects of the present invention are not impaired. Examples of other structural units include aromatic alkenyl compounds such as styrene, α-methylstyrene, chlorostyrene, and vinyltoluene, vinyl cyanide compounds such as acrylonitrile and methacrylonitrile, vinyl esters such as vinyl acetate, and dicarboxylic acid anhydrides such as maleic anhydride. When other structural units are contained, the total unit amount of the other structural units relative to all the structural units is preferably from 0 to 30 mol %, more preferably from 0 to 25 mol %, and even more preferably from 0 to 20 mol %.

[0056] The weight average molecular weight (Mw) of the acrylic polymer in this embodiment is preferably 10,000 to 500,000. From the viewpoint of obtaining a suitable lubrication effect and obtaining high transparency of the modified ethylene polymer composition, and from the viewpoint of obtaining good adhesion, the weight average molecular weight is preferably 10,000 or more. From the viewpoint of obtaining a suitable lubrication effect and obtaining high transparency of the modified ethylene polymer composition, the weight average molecular weight is preferably 500,000 or less. The weight average molecular weight (Mw) in this specification is a value measured using gel permeation chromatography (GPC) under the following conditions. (conditions) 0.05 g of an acrylic polymer is dissolved in 10 ml of tetrahydrofuran, and the molecular weight is determined as polymethyl methacrylate equivalent molecular weight using a column (K-806L, manufactured by Showa Denko K.K.) in gel permeation chromatography (LC-10A system, manufactured by Shimadzu Corporation).

[0057] The content of the acrylic polymer in this embodiment is preferably 0.01 to 4 parts by mass, more preferably 0.05 to 2 parts by mass, per 100 parts by mass of the ethylene polymer. The content may be 0.01 to 10 parts by mass, may be 0.05 to 5 parts by mass, and more preferably 0.1 to 2.5 parts by mass. Here, from the viewpoint of obtaining a suitable lubrication effect and more preferably suppressing the occurrence of fisheyes in the modified ethylene polymer composition, the content is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more. From the viewpoint of ensuring higher transparency and adhesiveness of the modified ethylene polymer composition, the content may be 10 parts by mass or less, may be 5 parts by mass or less, preferably 4 parts by mass or less, and more preferably 2.5 parts by mass or less.

[0058] The content of the acrylic polymer in the modified ethylene polymer composition in this embodiment is preferably 0.01 to 4 mass%, more preferably 0.05 to 2 mass%. The content may be 0.01 to 10 mass%, may be 0.05 to 5 mass%, and more preferably 0.1 to 2.5 mass%. Here, from the viewpoint of obtaining a suitable lubrication effect and more preferably suppressing the occurrence of fisheyes in the modified ethylene polymer composition, the content is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, and even more preferably 0.1 mass% or more. From the viewpoint of ensuring higher transparency and adhesiveness of the modified ethylene polymer composition, the content may be 10 mass% or less, may be 5 mass% or less, preferably 4 mass% or less, and more preferably 2.5 mass% or less.

[0059] The acrylic polymer in the present embodiment may be a manufactured one or a commercially available one. Examples of commercially available acrylic polymers include "Metablen (registered trademark) L type" manufactured by Mitsubishi Chemical Corporation, "PLASTISTRENGTH (registered trademark) L series" manufactured by ARKEMA, "Kane Ace (registered trademark) PA series" manufactured by Kaneka Corporation, and "PARALOID K series" manufactured by Dow Chemical Company.

[0060] <Physical properties / applications> The melt flow rate (MFR) of the modified ethylene polymer composition according to the present embodiment, measured according to JIS K 7210:2014 at a temperature of 190°C and a load of 21.2N, is preferably 0.05 to 50g / 10min, more preferably 0.1 to 30g / 10min, and even more preferably 0.5 to 10g / 10min. Here, from the viewpoint of reducing the energy load during production and the processability of the molded product, the MFR is preferably 0.05g / 10min or more, more preferably 0.1g / 10min or more, and even more preferably 0.5g / 10min or more. From the same viewpoint, the MFR is preferably 50g / 10min or less, more preferably 30g / 10min or less, and even more preferably 10g / 10min or less.

[0061] The density of the modified ethylene polymer composition according to this embodiment, measured by the underwater displacement method in accordance with JIS K 7112:1999, is 0.85 to 0.97 g / cm 3 is preferable, and 0.87 to 0.95 g / cm 3 More preferably, 0.89 to 0.93 g / cm 3 From the viewpoint of rigidity and heat resistance, the density is more preferably 0.85 g / cm. 3 More than 0.87 g / cm is preferable. 3 More preferably, 0.89 g / cm 3 More preferably, the density is 0.97 g / cm. 3 Less than 0.95 g / cm is preferred. 3 Less than 0.93 g / cm is more preferable. 3 The following is even more preferred:

[0062] The modified ethylene polymer composition according to the present embodiment has a melt flow rate (MFR) of 0.05 to 50 g / 10 min and a density of 0.85 to 0.97 g / cm 3 More preferred ranges of MFR and density are as described above.

[0063] The modified ethylene polymer composition according to this embodiment has an effect of reducing the occurrence of fisheyes and has a good appearance. As a guideline, when the composition is made into a film having a thickness of 50 μm, the amount of fisheyes having a major axis of 0.1 mm or more and less than 0.5 mm (FE amount) is preferably 210 pieces / g or less, more preferably 205 pieces / g or less, and even more preferably 200 pieces / g or less. The smaller the amount, the better. In addition, when the film is formed, the amount of FE having a major axis of 0.5 mm or more is preferably less than 20 pieces / g, more preferably 18 pieces / g or less, and even more preferably 15 pieces / g or less, and the smaller the better. Furthermore, when the film is formed, it is more preferable that the amount of FEs having a major axis of 0.1 mm or more and less than 0.5 mm is 210 pieces / g or less, and the amount of FEs having a major axis of 0.5 mm or more is less than 20 pieces / g, and the more preferable ranges of each of the FE amounts are as described above. Here, the FE amount is a value determined by using a surface defect inspection device within an area of ​​200 mm×120 mm, and the detailed conditions can be those described in the examples described later.

[0064] The modified ethylene polymer composition according to the present embodiment can be said to have excellent transparency and good compatibility with the acrylic polymer. As a guideline, the internal haze value when made into a film having a thickness of 50 μm is preferably 4.0% or less, more preferably 2.5% or less, and even more preferably 2.0% or less. Here, the internal haze is an index for evaluating the compatibility and dispersibility of the acrylic polymer, which is a polymer processing aid, in the modified ethylene polymer composition, and it can be said that the smaller the internal haze value, the more compatible the polymer processing aid is and the better the appearance is. The internal haze value is a value determined using a haze meter, and the detailed conditions can be those described in the examples below.

[0065] The modified ethylene polymer composition according to the present embodiment may be used as it is as an adhesive composition, or another polymer composition obtained by further kneading the modified ethylene polymer composition with other optional components may be used as an adhesive composition. Another example of the polymer composition is an olefin-based polymer composition using an olefin-based polymer as the other optional component, the details of which will be described later.

[0066] The modified ethylene polymer composition according to the present embodiment can be used as an adhesive composition in the production of a laminate to form one layer of the laminate. The modified ethylene polymer composition according to the present embodiment can also be used as an adhesive composition in the production of a laminate to form one layer of the laminate by further kneading another polymer composition obtained by kneading the modified ethylene polymer composition according to the present embodiment with other optional components.

[0067] <Other ingredients> The modified ethylene polymer composition according to the present embodiment may contain any other components, as necessary, in addition to the modified ethylene polymer and the acrylic polymer, within a range that does not impair the effects of the present invention.

[0068] Examples of other components include thermoplastic resins other than the polymer in the present embodiment, tackifiers, light stabilizers, UV absorbers, nucleating agents, lubricants, antioxidants, antiblocking agents, plasticizers, release agents, flame retardants, colorants, dispersants, bulking agents, and the like, and any of these may be used that are conventionally known. These may be used alone or in combination of two or more. In addition, some or all of the other ingredients may be produced from plant-derived raw materials.

[0069] Examples of thermoplastic resins include polyolefins and olefin-based elastomers, polyphenylene ethers, polycarbonates, polyamides such as nylon 66 and nylon 11, polyesters and polyester-based elastomers such as polyethylene terephthalate and polybutylene terephthalate, polystyrene and styrene copolymers or hydrogenated products thereof and styrene-based elastomers, cyclic polyolefins, and acrylics / methacrylics such as polymethyl methacrylate.

[0070] The amount of the thermoplastic resin used in the present embodiment varies depending on the type of resin used, but is, for example, preferably 0 to 49 parts by mass, more preferably 0 to 20 parts by mass, relative to 100 parts by weight of the ethylene polymer. From the viewpoints of ensuring higher transparency and adhesiveness of the modified ethylene polymer composition, the amount used is preferably 49 parts by mass or less, more preferably 20 parts by mass or less.

[0071] Examples of the tackifier include amorphous resins that are solid at room temperature, such as petroleum resins, rosin resins, terpene resins, and hydrogenated products thereof.

[0072] Among the above, examples of the petroleum resin include aliphatic petroleum resin, aromatic petroleum resin, or copolymers thereof, and hydrogenated products thereof. Examples of the petroleum resin skeleton include C5 resin, C9 resin, C5 / C9 copolymer resin, cyclopentadiene resin, polymer of vinyl-substituted aromatic compound, copolymer of olefin / vinyl-substituted aromatic compound, copolymer of cyclopentadiene compound / vinyl-substituted aromatic compound, etc. In addition, as mentioned above, hydrogenated products of these can also be used as tackifiers.

[0073] Among the above, the rosin resin is a natural resin containing abietic acid as a main component, and examples thereof include natural rosin, polymerized rosin derived from natural rosin, stabilized rosin obtained by disproportionating natural rosin or polymerized rosin, unsaturated acid modified rosin obtained by adding unsaturated carboxylic acids to natural rosin or polymerized rosin, natural rosin ester, modified rosin ester, polymerized rosin ester, etc. Furthermore, examples of the above hydrogenated products include stabilized rosin obtained by hydrogenating natural rosin or polymerized rosin.

[0074] Among the above, examples of the terpene resin include aromatic terpene resins such as polyterpene resins, terpene phenol resins, and aromatic modified terpene resins. As described above, hydrogenated products of these resins can also be used as tackifiers.

[0075] The amount of the tackifier used in the present embodiment varies depending on the type of resin used, but is preferably 1 to 40 parts by mass, and more preferably 5 to 30 parts by mass, relative to 100 parts by weight of the ethylene polymer. From the viewpoint of ensuring adhesiveness, the amount is preferably 1 part by mass or more, and more preferably 5 parts by mass or more. Also, from the viewpoint of productivity of the modified ethylene resin, that is, suppressing blocking during pelletization, the amount is preferably 40 parts by mass or less, and more preferably 30 parts by mass or less.

[0076] Examples of antioxidants include phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants. Among these, phenol-based antioxidants are preferred, and a combination of a phenol-based antioxidant with a phosphorus-based antioxidant or a sulfur-based antioxidant is also preferred.

[0077] Examples of phenol-based antioxidants include 2,4-dimethyl-6-t-butylphenol, 2,6-di-t-butylphenol, 2,6-di-t-butyl-p-cresol, 2,6-di-t-butyl-4-ethylphenol, 2,4,6-tri-t-butylphenol, 2,5-di-t-butylhydroquinone, butylated hydroxyanisole, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, and butyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate. phenyl)propionate and other monophenols, 4,4'-dihydroxydiphenyl, 2,2'-methylenebis(4-methyl-6-t-butylphenol), 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 4,4'-methylenebis(2,6-di-t-butylphenol), 4,4'-butylidenebis(3-methyl-6-t-butylphenol), 2,6-bis(2'-hydroxy-3'-t-butyl-5'-methylbenzyl)-4-methylphenol and other bisphenols, 1,1,3- Tris(2'-methyl-4'-hydroxy-5'-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3',5'-di-t-butyl-4'-hydroxybenzyl)benzene, tris(3,5-di-t-butyl-4-hydroxyphenyl)isocyanurate, tris[β-(3,5-di-t-butyl-4-hydroxyphenyl)propionyloxyethyl]isocyanurate, tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate] Polyphenols of tri- or higher order such as methane, thiobisphenols such as 2,2'-thiobis(4-methyl-6-t-butylphenol), 4,4'-thiobis(2-methyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), naphthylamines such as aldol-α-naphthylamine, phenyl-α-naphthylamine, phenyl-β-naphthylamine, diphenylamines such as p-isopropoxydiphenylamine, N,N'-diphenyl-p-phenylenediamine, N,Examples of the phenylenediamine-based compounds include N'-di-β-naphthyl-p-phenylenediamine, N-cyclohexyl-N'-phenyl-p-phenylenediamine, and N-isopropyl-N'-phenyl-p-phenylenediamine. Among these, monophenol-based compounds, bisphenol-based compounds, tri- or higher polyphenol-based compounds, and thiobisphenol-based compounds are preferred.

[0078] The phosphorus-based antioxidant preferably has a basic skeleton of a phosphite ester in which three alkoxy groups are bonded to a phosphorus atom, and at least one of the alkoxy groups is a bulky group having three or more carbon atoms. Examples include phenyldiisoalkyl (C1-C10) phosphite, diphenylisoalkyl (C1-C10) phosphite, and tris-(2,4-di-t-butylphenyl) phosphite.

[0079] Examples of sulfur-based antioxidants include dilauryl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, pentaerythritol-tetrakis-(β-lauryl-thiopropionate), 2-mercapto-5-methylbenzimidazole, and the like.

[0080] The amount of the antioxidant used in the present embodiment varies depending on the type of antioxidant used, but is, for example, preferably 0.001 to 2 parts by mass, more preferably 0.005 to 1 part by mass, and even more preferably 0.007 to 0.8 parts by mass, relative to 100 parts by weight of the ethylene polymer. Here, from the viewpoint of obtaining a better fisheye reduction effect, the amount used is preferably 0.001 parts by mass or more, more preferably 0.005 parts by mass or more, and even more preferably 0.007 parts by mass or more. Also, from the viewpoint of suppressing the antioxidant from bleeding out from the modified ethylene polymer composition, the amount used is preferably 2 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.8 parts by mass or less.

[0081] Examples of the filler include calcium carbonate, talc, and silica.

[0082] <Manufacturing method> The method for producing the modified ethylene polymer composition according to the present embodiment includes a step of melt-kneading an ethylene polymer, an ethylenically unsaturated compound, an acrylic polymer, and a radical generator.

[0083] Here, the ethylene-based polymer, the ethylenically unsaturated compound, and the acrylic polymer can be the ethylene-based polymer, the ethylenically unsaturated compound, and the acrylic polymer described in the above-mentioned <Modified ethylene-based polymer>, respectively, and preferred embodiments are also the same. In addition to the above, the optional components described in the above <Other Components> may be melt-kneaded together.

[0084] The radical generator in this embodiment is preferably, for example, an organic peroxide. Specifically, for example, dialkyl peroxides such as di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, 1,4-bis(t-butylperoxyisopropyl)benzene, 1,1-bis(t-butylperoxy)cyclohexane, n-butyl-4,4-bis(t-butylperoxy)valerate, 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, 2,2-bis(t-butylperoxy)butane, and 1,1-bis(t-butylperoxy)cyclododecane, t-butylperoxyacetate, t-butylperoxy-2-ethylhexanoate, t-butylperoxypivalate, t-butylperoxylaurate, t-butylperoxybenzoate, t-butylperoxyphenyl per ... peroxy esters such as di-t-butylperoxyisopropyl carbonate, t-butylperoxymaleic acid, di-t-butylperoxyisophthalate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(toluylperoxy)hexane, diacyl peroxides such as 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, benzoyl peroxide, hydroperoxides such as t-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, p-mentha hydroperoxide, 2,5-dimethyl-2,5-di(hydroperoxy)hexane, ketone peroxides such as methyl ethyl ketone peroxide, cyclohexanone peroxide, etc. These may be used alone or in combination of two or more.

[0085] Among these, radical generators having a 1-minute half-life temperature of 140°C or higher are preferred, and for example, dialkyl peroxides such as di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, and peroxy esters such as t-butyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexyne-3, are particularly preferred.

[0086] The melt-kneading in the manufacturing method according to the present embodiment is usually performed by uniformly mixing each component and then melt-kneading. Here, the ethylenically unsaturated compound and the radical generator may be added during the melt-kneading. In addition, the ethylenically unsaturated compound and the radical generator may be added in a state of being dissolved in an organic solvent or the like.

[0087] As the mixing device, for example, a tumbler blender, a ribbon blender, a V-type blender, a Henschel mixer, or the like can be used. The mixing time is usually 0.1 to 30 minutes, preferably 0.5 to 5 minutes.

[0088] As a kneading device for carrying out the melt kneading, for example, a mixing roll, a kneader, a Banbury mixer, a Brabender Plastograph, a single-screw or twin-screw extruder, or the like is used.

[0089] The temperature for melt kneading is usually 120 to 300° C., preferably 150 to 280° C., and the kneading time is usually 0.1 to 30 minutes, preferably 0.5 to 10 minutes.

[0090] The amount of the ethylenically unsaturated compound in this embodiment is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the ethylene polymer. From the viewpoint of sufficiently modifying the ethylene polymer and obtaining better adhesiveness as a modified ethylene polymer composition, the amount is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more. From the viewpoint of further suppressing the occurrence of fisheyes, the amount is preferably 10 parts by mass or less, more preferably 5 parts by mass or less.

[0091] The amount of the radical generator in this embodiment is preferably 0.01 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, and even more preferably 0.01 to 1 part by mass, relative to 100 parts by mass of the ethylene-based polymer. From the viewpoint of obtaining a sufficient graft amount, the amount is preferably 0.01 parts by mass or more. From the viewpoint of suppressing side reactions such as crosslinking of the ethylene-based polymer, the amount is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 1 part by mass or less.

[0092] The blending amount of the acrylic polymer in this embodiment is preferably 0.01 to 4 parts by mass, more preferably 0.05 to 2 parts by mass, per 100 parts by mass of the ethylene polymer. The blending amount may be 0.01 to 10 parts by mass, may be 0.05 to 5 parts by mass, and more preferably 0.1 to 2.5 parts by mass. Here, from the viewpoint of obtaining a suitable lubrication effect and more preferably suppressing the occurrence of fisheyes in the modified ethylene polymer composition, the blending amount is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more. From the viewpoint of ensuring higher transparency and adhesiveness of the modified ethylene polymer composition, the blending amount may be 10 parts by mass or less, may be 5 parts by mass or less, preferably 4 parts by mass or less, and more preferably 2.5 parts by mass or less.

[0093] Olefin Polymer Composition The olefin polymer composition according to the present embodiment contains a modified ethylene polymer composition and an olefin polymer. Here, the modified ethylene polymer composition may be one described in the above "Modified ethylene polymer composition", and preferred embodiments are also the same.

[0094] Use of the olefin polymer composition according to the present embodiment as an adhesive composition is preferable from the viewpoint of stabilizing the modification amount in the polymer composition and the effect of reducing the occurrence of fisheyes, as well as from the viewpoint of productivity, as compared with the use of the modified ethylene polymer composition as it is as an adhesive composition.

[0095] The olefin-based polymer in this embodiment may be a homopolymer or a copolymer. As the homopolymer, for example, a homopolymer of ethylene or a homopolymer of an α-olefin having 3 to 20 carbon atoms is preferable, and a homopolymer of ethylene or a homopolymer of propylene is more preferable. The olefin-based polymer in this embodiment may be a biomass polyolefin containing structural units derived from biomass produced using plants as raw materials.

[0096] As the copolymer, a copolymer obtained from two or more monomers selected from the group consisting of ethylene and an α-olefin having 3 to 20 carbon atoms, a copolymer of ethylene and vinyl acetate, (meth)acrylic acid, a (meth)acrylic acid ester, or the like is preferred, and a copolymer obtained from two or more monomers selected from ethylene and an α-olefin having 3 to 10 carbon atoms, or a copolymer obtained from two or more monomers selected from the group consisting of ethylene and vinyl acetate and a (meth)acrylic acid ester is more preferred.

[0097] Examples of α-olefins having 3 to 20 carbon atoms include propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 4-methyl-1-hexene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-octadecene. Among these, α-olefins having 3 to 10 carbon atoms are more preferred.

[0098] The olefin polymer in the present embodiment is preferably a homopolymer of ethylene, a homopolymer of propylene, a copolymer obtained from two or more monomers selected from ethylene and an α-olefin having 3 to 10 carbon atoms, or a copolymer obtained from ethylene and two or more monomers selected from the group consisting of vinyl acetate and a (meth)acrylic acid ester, and even more preferably a homopolymer of ethylene, or a copolymer of two or more monomers selected from ethylene, propylene, 1-butene, 1-hexene, and 1-octene.

[0099] In the olefin polymer composition according to this embodiment, the mass ratio of the modified ethylene polymer composition to the olefin polymer (modified ethylene polymer composition:olefin polymer) is preferably 1:99 to 99:1, more preferably 2:98 to 98:2. That is, the content of the olefin polymer relative to the total content of the modified ethylene polymer composition and the olefin polymer is preferably 1 to 99 mass%, more preferably 2 to 98 mass%. The content of the modified ethylene polymer composition relative to the total content is preferably 1 to 99 mass%, more preferably 2 to 98 mass%.

[0100] From the viewpoint of obtaining good adhesion, the content of the olefin polymer is preferably 99% by mass or less, more preferably 98% by mass or less, and the content of the modified ethylene polymer composition is preferably 1% by mass or more, more preferably 2% by mass or more. From the viewpoint of the effect of reducing the occurrence of fisheyes and productivity, the content of the olefin polymer is preferably 1% by mass or more, more preferably 2% by mass or more, and the content of the modified ethylene polymer composition is preferably 99% by mass or less, more preferably 98% by mass or less.

[0101] The method for producing the olefin polymer composition according to the present embodiment is not particularly limited and may be a method known in the art, provided that the modified ethylene polymer composition described in the above "Modified ethylene polymer composition" is mixed with an olefin polymer. That is, the method for producing an olefin polymer composition according to the present embodiment includes mixing the modified ethylene polymer composition with an olefin polymer, wherein the mixing ratio of the modified ethylene polymer composition to the olefin polymer is preferably 1:99 to 99:1 (mass ratio).

[0102] The mixing ratio (mass ratio) is preferably 1:99 to 99:1, and more preferably 2:98 to 98:2. That is, the mixing ratio of the olefin polymer to the total of the modified ethylene polymer composition and the olefin polymer is preferably 1 to 99 mass%, and more preferably 2 to 98 mass%. The mixing ratio of the modified ethylene polymer composition to the total is preferably 1 to 99 mass%, and more preferably 2 to 98 mass%.

[0103] From the viewpoint of obtaining good adhesion, the mixing ratio of the olefin polymer is preferably 99% by mass or less, more preferably 98% by mass or less, and the mixing ratio of the modified ethylene polymer composition is preferably 1% by mass or more, more preferably 2% by mass or more. From the viewpoint of the effect of reducing the occurrence of fisheyes and productivity, the mixing ratio of the olefin polymer is preferably 1% by mass or more, more preferably 2% by mass or more, and the mixing ratio of the modified ethylene polymer composition is preferably 99% by mass or less, more preferably 98% by mass or less.

[0104] In the method for producing the olefin polymer composition according to the present embodiment, for example, a method of mechanically blending the modified ethylene polymer composition, the olefin polymer, and other components added as necessary using an extruder, kneader, or the like, or a method of dissolving and mixing them in an appropriate good solvent and then removing the solvent, or the like, can be used.

[0105] The mechanical blending method includes, for example, a melt kneading method. The temperature for melt kneading is usually 120 to 300° C., preferably 150 to 280° C., and the kneading time is usually 0.1 to 30 minutes, preferably 0.5 to 10 minutes.

[0106] <Laminate> One aspect of the laminate according to this embodiment is one in which a layer made of a modified ethylene polymer composition and a layer serving as an adherend are bonded and laminated. Another aspect of the laminate according to this embodiment is one in which a layer made of an olefin polymer composition and a layer serving as an adherend are bonded and laminated.

[0107] The modified ethylene polymer composition may be one described in the above section "Modified ethylene polymer composition", and the preferred embodiments are the same. The olefin polymer composition may be one described in the above section "Olefin polymer composition", and the preferred embodiments are the same.

[0108] The layer that is the adherend in this embodiment may be at least one layer selected from the group consisting of thermoplastic resin, metal foil, paper, wood, and fiber.

[0109] The modified ethylene polymer composition and the olefin polymer composition in the present embodiment both exhibit better adhesion than conventional polymer compositions and can therefore be suitably used as an adhesive composition layer, and are also excellent in adhesion to the above-mentioned thermoplastic resins, metal foils, paper, wood, and fibers.

[0110] Examples of the thermoplastic resin in this embodiment include polyamide-based resins, polyester-based resins, saponified ethylene-vinyl acetate copolymers, polycarbonate-based resins, polystyrene-based resins, acrylic resins, polyolefin-based resins, and ethylene-vinyl alcohol copolymers. Examples of polyamide resins include nylon 6, nylon 11, nylon 12, nylon 6-6, nylon 6-10, and nylon 6-12.

[0111] Examples of the metal foil include aluminum, copper, and stainless steel foils. Examples of wood include veneer, plywood, and wood fiberboard. Examples of the fibers include woven fabrics and nonwoven fabrics.

[0112] Among the above, laminates having layers made of saponified ethylene-vinyl acetate copolymer, polyamide resin, polyester resin or metal foil have excellent gas barrier properties and are suitably used as food storage containers, packaging materials and the like.

[0113] The laminate according to the present embodiment may be in the form of a film, plate, tube, foil, or woven fabric, as well as a bottle, a container, or an injection-molded product. In particular, from the viewpoint of more suitably utilizing the effect of reducing fisheyes, the laminate is preferably in the form of a film or plate, and more preferably in the form of a film. When the laminate is in the form of a film, the thickness is preferably 2 mm or less, and more preferably 1 mm or less.

[0114] The method for producing the laminate according to the present embodiment is not particularly limited as long as it includes a step of forming a phase made of the olefin polymer composition described above in "Olefin Polymer Composition" and a step of bonding a layer made of the olefin polymer composition to a layer serving as an adherend.

[0115] Examples of the method for producing the laminate according to the present embodiment include a method for laminating another layer onto a previously molded film or sheet by a lamination method such as extrusion lamination, dry lamination, sandwich lamination, etc. Other examples include a multi-layer inflation method in which a multi-layer die is used to bond resin molten in an extruder at the tip of the die to form a laminate, a co-extrusion molding method such as a multi-layer T-die co-extrusion molding method, a multi-layer blow molding method, an injection molding method, and other conventional molding methods.

[0116] When the layer to be adherend is a layer of a saponified ethylene-vinyl acetate copolymer, a polyamide-based resin, or a polyester-based resin, and is to be laminated with an adhesive composition layer made of the modified ethylene-based polymer composition or the olefin-based polymer composition in this embodiment, the method for producing the laminate is preferably coextrusion molding.

[0117] When a laminate is to be prepared by combining a metal foil or the like with an adhesive composition layer comprising the above-mentioned modified ethylene polymer composition or olefin polymer composition, the laminate is preferably produced by a lamination method.

[0118] Specific examples of the layer structure of the laminate according to this embodiment include a gas barrier layer / modified ethylene polymer composition layer, a gas barrier layer / modified ethylene polymer composition layer / polyolefin layer, a polyolefin layer / modified ethylene polymer composition layer / gas barrier layer / modified ethylene polymer composition / polyolefin layer, etc. Here, the gas barrier layer is a layer made of a saponified ethylene-vinyl acetate copolymer, a metal foil, etc. Furthermore, the modified ethylene polymer composition layer in the above layer structure can be replaced with the olefin polymer composition of the present embodiment.

[0119] The laminate according to this embodiment has excellent adhesion due to the layer made of the modified ethylene polymer composition or the olefin polymer composition, and has excellent surface smoothness with reduced occurrence of fisheyes.

[0120] Furthermore, laminates using polyamide resins, polyester resins, saponified ethylene-vinyl acetate copolymers, and metal foils as constituent layers as adherend layers have good gas barrier properties, and therefore, by forming a laminate together with the olefin polymer composition of the present embodiment or an olefin polymer composition, the laminate has good processability, water resistance, chemical resistance, flexibility, and other properties.

[0121] Furthermore, laminates using polycarbonate resins, polystyrene resins, metal foils, and wood as constituent layers as adherend layers have excellent rigidity, while laminates using paper, wood, and fiber as constituent layers have excellent mechanical strength. EXAMPLES

[0122] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. Note that the values ​​of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​of the examples.

[0123] "raw materials" In the following examples, the following raw materials were used:

[0124] <Component (A): Ethylene-based polymer> (A)-1 Linear ethylene-1-butene copolymer [density: 0.92 g / cm 3, MFR (190℃, load 21.2N): 30.0g / 10min, melting point: 123℃] (A)-2 Linear ethylene-1-butene copolymer [density: 0.92 g / cm 3 , MFR (190℃, load 21.2N): 2.1g / 10min, melting point: 123℃]

[0125] <Component (B): Polymer processing aid> (B)-1 Polymer processing aid (B)-1 Acrylic polymer [copolymer consisting of methyl methacrylate units, butyl methacrylate units, and butyl acrylate units, weight average molecular weight: approximately 250,000 g / mol, glass transition temperature: approximately 25°C] (B')-2 Vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer [3M: Dynamer(registered trademark) FX5911] (B')-3 Vinylidene fluoride-hexafluoropropylene copolymer + antiblocking agent mixture [3M: Dynamer(registered trademark) FX9613]

[0126] <Component (C): Ethylenically unsaturated compound> (C)-1 Maleic anhydride [NOF Corporation]

[0127] <Component (D): Radical generator) (D)-1 2,5-Dimethyl-2,5-bis(t-butylperoxy)hexane [Perhexa 25B (registered trademark), manufactured by NOF Corporation]

[0128] <Ingredient (E): Antioxidant> (E)-1 Phenol-based antioxidant [BASF: IRGANOX (registered trademark) 1010]

[0129] <Component (F): Olefin-based polymer> (F)-1 Linear ethylene-1-butene copolymer [Saudi Petrochemical Company, QAMAR (trademark) FD18N, MFR: 2.0 g / 10 min, density: 0.92 g / cm 3 ]

[0130] Examples 1-1 to 1-6, Comparative Examples 1-1 to 1-6, and Reference Example 1-1 The components described in the above "Raw Materials" were mixed for 1 minute using a super mixer in the amounts shown in Table 1. The resulting mixture was melt-kneaded using a twin-screw extruder (manufactured by Japan Steel Works, Ltd.: TEX25αIII, diameter 25 mm, L / D 43) under conditions of a kneading temperature of 240°C, a screw rotation speed of 300 rpm, and a discharge rate of 20 kg / hour, and extruded through a die into a strand shape and cut to obtain modified ethylene polymer compositions. When the obtained modified ethylene polymer composition was subjected to each evaluation, the modified ethylene polymer composition was used within 30 minutes to 1 hour after the start of strand cut granulation. In addition, blank spaces in Table 1 indicate that no compound was added.

[0131] Examples 2-1a to 2-6a and Comparative Examples 2-1a to 2-6a A mixture of 10 parts by mass of each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-6 and Comparative Examples 1-1 to 1-6 and 90 parts by mass of an olefin polymer was melt-kneaded at a kneading temperature of 210°C using a single-screw extruder (PSM50-32(1V), manufactured by IKG, D=50 mmφ, L / D=32), and the mixture was extruded through a die in the form of a strand and cut to obtain each modified olefin polymer.

[0132] Examples 2-1b to 2-6b and Comparative Examples 2-1b to 2-6b A mixture of 15 parts by mass of each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-6 and Comparative Examples 1-1 to 1-6 and 85 parts by mass of an olefin polymer was melt-kneaded at a kneading temperature of 210°C using a single-screw extruder (PSM50-32(1V), manufactured by IKG, D=50 mmφ, L / D=32) to obtain each modified olefin polymer.

[0133] Measurement and evaluation methods <Component (C); Content of ethylenically unsaturated compound> The content of ethylenically unsaturated compounds, that is, the graft ratio, was determined using an infrared spectrometer. Specifically, the amount of ethylenically unsaturated compounds in the modified ethylene polymer was determined in advance as a standard sample by nuclear magnetic resonance measurement, and a calibration curve was prepared from the quantitative values. Next, pellets of each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-6, Comparative Examples 1-1 to 1-6, and Reference Example 1-1 were press-molded into a film having a thickness of 100 μm at 200° C. Using this as a sample, the absorption characteristic of the ethylenically unsaturated compound in the sample, i.e., the absorption at 1900 to 1600 cm, was measured with an FT-IR device (JASCO FT / IR610, manufactured by JASCO Corporation). -1 The carbonyl characteristic absorption observed in the (C=O stretching vibration band) was measured, and the carbonyl content was calculated using the calibration curve prepared above. In addition, in the modification with an ethylenically unsaturated compound, not all of the ethylenically unsaturated compound, i.e. 100%, is subjected to the reaction, and the ethylenically unsaturated compound that has not reacted with the ethylenic polymer may remain in the modified ethylenic polymer composition. However, the content of the ethylenically unsaturated compound (graft ratio) in this specification means the value measured by the above method. The results are shown in Table 1.

[0134] <Melt Flow Rate (MFR)> The melt flow rate (MFR) of each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-6, Comparative Examples 1-1 to 1-6, and Reference Example 1-1 was measured at a temperature of 190° C., a load of 21.2 N, and for 10 minutes in accordance with JIS K 7210: 2014. The results are shown in Table 1.

[0135] <density> For each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-6, Comparative Examples 1-1 to 1-6 and Reference Example 1-1, the density was measured by the underwater displacement method in accordance with JIS K 7112: 1999. The results are shown in Table 1.

[0136] <HAZE (interior)> For each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-6, Comparative Examples 1-1 to 1-6, and Reference Example 1-1, three single-layer films each having a layer thickness of 50 μm were obtained in the same manner as in the evaluation of the above-mentioned fisheye (FE). The internal haze of the obtained monolayer film was measured using a haze meter (NDH2000, manufactured by Nippon Denshoku Industries Co., Ltd.), and the average value of the measurement results for three sheets each was recorded as the internal haze value. In this evaluation, if the internal haze value is 2.5% or less, the compatibility as a polymer processing aid is evaluated as good. The results are shown in Table 1.

[0137] <Fisheye (FE)> For each of the modified ethylene polymer compositions obtained in Examples 1-1 to 1-6, Comparative Examples 1-1 to 1-6, and Reference Example 1-1, a monolayer film molding machine having a T-die with a width of 300 mm (GSI Creos Corporation) was used to obtain a monolayer film having a layer thickness of 50 μm under conditions of a T-die temperature of 200° C., a molding speed of 5 m / min, and a cast roll temperature of 30° C. The obtained monolayer film was cut to a length of 200 mm and a width of 120 mm, which was used as the inspection area. Then, using a compact digital surface defect inspection device (GX-70LT, manufactured by Mamiya-OP Co., Ltd.), the number of FEs with a major axis of 0.1 mm or more and less than 0.5 mm, and the number of FEs with a major axis of 0.5 mm or more were counted. The number of FEs counted was divided by the weight of the monolayer film in the inspection area to determine the amount of fisheyes (FEs) per unit mass (pieces / g). In this evaluation, if the amount of FE with a major axis of 0.1 mm or more and less than 0.5 mm is 210 pieces / g or less, the appearance is evaluated as good. In addition, the amount of FE with a major axis of 0.5 mm or more is more preferably 18 pieces / g or less. The results are shown in Table 1. In Table 1, "-" indicates that the measurement was not performed.

[0138] <Adhesive strength> A multilayer film molding machine (manufactured by Labtech Engineering Co.) with a 350 mm wide three-type five-layer feedblock type T-die was used to produce a five-layer film consisting of an ethylene-based polymer layer / adhesive resin layer / ethylene-vinyl alcohol copolymer (EVOH) layer / adhesive resin layer / ethylene-based polymer layer. Here, the adhesive resin layers were made of the olefin polymer compositions obtained in Examples 2-1a to 2-6a and Comparative Examples 2-1a to 2-6a, and Examples 2-1b to 2-6b and Comparative Examples 2-1b to 2-6b. The ethylene polymer layers were made of Novatec (registered trademark) SF8402 (manufactured by Japan Polyethylene Corporation). The ethylene-vinyl alcohol copolymer layer was made of Soarnol (registered trademark) DC3203RB (manufactured by Mitsubishi Chemical Corporation). The specific conditions were a T-die temperature of 240°C, a molding speed of 5 m / min, and a cast roll temperature of 80°C. The thicknesses of the individual layers were 30 μm / 10 μm / 20 μm / 10 μm / 30 μm, respectively, resulting in a five-layer film laminate with a total thickness of 100 μm.

[0139] The five-layer film obtained above was cut into 15 mm-wide strips parallel to the molding direction to prepare test pieces. A T-peel test was performed on each test piece at a constant temperature of 23°C and a speed of 300 mm / min to measure the adhesive strength at the interface between the adhesive resin layer and the EVOH layer. Generally, an interlayer strength of 2N / 15mm or more is considered to be sufficient for practical use, so in this evaluation, adhesion is evaluated as good if the adhesive strength at the interface between the adhesive resin layer and the EVOH layer is 2N / 15mm or more. The results are shown in Table 1. In Table 1, "-" indicates that the measurement was not performed.

[0140] [Table 1]

[0141] From the results in Table 1, it was found that the modified ethylene polymer composition according to this embodiment exhibits a good effect of reducing the occurrence of fisheyes and is also excellent in transparency. In addition, it was found that the olefin polymer composition containing the modified ethylene polymer composition according to this embodiment can maintain good adhesion at the same level as when a conventional copolymer of vinylidene fluoride and fluorinated olefin is used as a polymer processing aid.

Claims

1. The modified ethylene polymer and the acrylic polymer are included. The modified ethylene polymer is an ethylene polymer modified with an ethylenically unsaturated compound, The acrylic polymer contains, as structural units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms, The modified ethylene-based polymer composition has a content of the acrylic polymer of 0.01 to 4% by mass.

2. The modified ethylene polymer composition according to claim 1, wherein the acrylic polymer is a copolymer containing a methyl methacrylate unit as the methyl (meth)acrylate unit and containing a butyl methacrylate unit and a butyl acrylate unit as the alkyl (meth)acrylate unit having 2 to 18 carbon atoms.

3. The modified ethylene polymer composition according to claim 1, wherein the ethylenically unsaturated compound is a polar ethylenically unsaturated compound having a carboxyl group, a hydroxyl group or an amino group, an anhydride of a polar ethylenically unsaturated compound having a carboxyl group, or an aromatic vinyl compound.

4. the ethylenically unsaturated compound is the polar ethylenically unsaturated compound having a carboxyl group or an anhydride thereof, The modified ethylene polymer composition according to claim 3, wherein the polar ethylenically unsaturated compound having a carboxyl group or an anhydride thereof is an unsaturated dicarboxylic acid or an anhydride thereof.

5. The modified ethylene-based polymer composition according to claim 1, wherein the content of the ethylenically unsaturated compound in the modified ethylene-based polymer composition is 0.05 to 10% by mass.

6. The melt flow rate measured in accordance with JIS K 7210:2014 under conditions of a temperature of 190°C and a load of 21.2N is 0.05 to 50 g / 10 min, and Density measured by underwater displacement method according to JIS K 7112:1999 is 0.85 to 0.97 g / cm 3 The modified ethylene polymer composition according to claim 1,

7. A method for producing an olefin polymer composition, comprising the steps of: The method includes mixing the modified ethylene polymer composition according to any one of claims 1 to 6 with an olefin polymer, The modified ethylene polymer composition and the olefin polymer are mixed in a mixing ratio of 1:99 to 99:1 (mass ratio).

8. A laminate comprising a layer made of the modified ethylene polymer composition according to any one of claims 1 to 6 and a layer serving as an adherend bonded to the layer.

9. 9. The laminate according to claim 8, wherein the layer that is the adherend is at least one layer selected from the group consisting of thermoplastic resins, metal foils, paper, wood, and fibers.

10. A method for producing a laminate, comprising the steps of: forming a layer made of an olefin polymer composition obtained by the production method according to claim 7; and and bonding a layer made of the olefin polymer composition to a layer serving as an adherend.

11. The method for producing a laminate according to claim 10, wherein the layer that is the adherend is at least one layer selected from the group consisting of a thermoplastic resin, a metal foil, paper, wood, and a fiber.

12. A method for producing a modified ethylene polymer composition, comprising the steps of: The method includes a step of melt-kneading an ethylene-based polymer, an ethylenically unsaturated compound, an acrylic polymer, and a radical generator, The acrylic polymer contains, as structural units, a methyl (meth)acrylate unit and an alkyl (meth)acrylate unit having 2 to 18 carbon atoms, The amount of the acrylic polymer blended is 0.01 to 4 parts by mass per 100 parts by mass of the ethylene polymer.

Citation Information

Patent Citations

  • Modified ethylene-based polymer composition and laminated product given by using the same

    JP2005036221A