Method of recovering active metal of lithium secondary battery

The method addresses the low purity and efficiency of existing lithium secondary battery recycling by using an acidic leaching, solid-liquid separation, and electrodialysis to achieve high-purity lithium precursor recovery.

JP2024137930APending Publication Date: 2024-10-07SK INNOVATION CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
JP2024047328
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-22
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing methods for recovering active metals from lithium secondary batteries suffer from low purity and efficiency, particularly due to the presence of impurities such as iron, phosphorus, and aluminum.

Method used

A method involving an acidic leaching process followed by solid-liquid separation, water washing, and the use of a lithium hydroxide solution to remove impurities, combined with electrodialysis to convert lithium sulfate, chloride, or nitrate into lithium hydroxide, enhancing purity and yield.

Benefits of technology

The method achieves a highly pure lithium precursor recovery by effectively removing impurities and increasing the concentration of lithium, thereby improving the efficiency and environmental friendliness of the recycling process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137930000001_ABST
    Figure 2024137930000001_ABST
Patent Text Reader

Abstract

To provide a method of recovering a lithium precursor with decreased amounts of impurities and increased purity and recovery rates.SOLUTION: In a method of recovering an active metal of a lithium secondary battery, an acidic leaching liquid is added to a material to be recovered which contains a lithium metal oxide to form a mixture including a first active metal solution and a leached residue. Solid-liquid separation is performed for separating the first active metal solution from the leached residue to form a second active metal solution. A lithium hydroxide aqueous solution containing an iron salt is added to the second active metal solution to form a third active metal solution from which impurities are removed or decreased. A lithium precursor is recovered from the third active metal solution. Thereby, there is provided a method of recovering a lithium precursor with decreased amounts of impurities and increased purity and recovery rates.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The disclosure of the present application relates to a method for recovering active metals from a lithium secondary battery, and more particularly to a method for recovering active metals from a positive electrode active material of a lithium secondary battery. [Background technology]

[0002] Secondary batteries are widely used as power sources for portable electronic communication devices such as camcorders, mobile phones, and notebook computers, and for vehicles such as hybrid cars, electric cars, etc. As a secondary battery, lithium secondary batteries have high operating voltage and high energy density per unit weight, and are advantageous in terms of charging speed and weight reduction.

[0003] The positive electrode active material of the lithium secondary battery may be a lithium metal oxide, which may further contain a valuable metal such as iron, nickel, cobalt, or manganese.

[0004] Due to the use of the aforementioned high-cost valuable metals in the positive electrode active material and the growing interest in environmental protection, research into methods for recycling the positive electrode active material is being conducted. Summary of the Invention [Problem to be solved by the invention]

[0005] One objective of the present disclosure is to provide a method for recovering active metals of lithium secondary batteries with improved purity and efficiency. [Means for solving the problem]

[0006] In the method for recovering active metals of a lithium secondary battery according to the embodiment of the present disclosure, an acidic leachate may be added to a material to be recovered that includes lithium metal oxide to form a mixture that includes a first active metal solution and a leach residue. The first active metal solution may be separated from the leach residue into a solid-liquid separation to form a second active metal solution. An aqueous lithium hydroxide solution that includes an iron salt may be added to the second active metal solution to form a third active metal solution in which impurities have been removed or reduced. A lithium precursor may be recovered from the third active metal solution.

[0007] In some embodiments, the leach residue can be washed with water to produce a wash solution, which can be provided to the mixture or the second active metal solution.

[0008] In some embodiments, the water wash is repeated in multiple cycles, and the wash solution produced from an earlier cycle in the cycles can be fed to the second active metal solution and the wash solution produced from a later cycle in the cycles can be fed to the mixture.

[0009] In some embodiments, the lithium metal oxide may include a lithium iron phosphate based active material, the first active metal solution may include lithium sulfate, lithium chloride, or lithium nitrate, and the leach residue may include an iron phosphate based material.

[0010] In some embodiments, the material to be recovered can be obtained by crushing used lithium secondary batteries.

[0011] In some embodiments, the impurities can include iron (Fe), phosphorus (P), and aluminum (Al).

[0012] In some embodiments, the iron salt comprises iron sulfate, iron chloride, or iron nitrate, and residual phosphorus may precipitate from the second active metal solution in the form of iron phosphate.

[0013] In some embodiments, the aqueous lithium hydroxide solution may be free of salts of alkali metals or alkaline earth metals other than lithium.

[0014] In some embodiments, recovering the lithium precursor may include converting lithium sulfate, lithium chloride, or lithium nitrate to lithium hydroxide by electrodialysis.

[0015] In some embodiments, a portion of the lithium hydroxide produced by the electrodialysis can be recycled to forming the third active metal solution.

[0016] In some embodiments, the acidic leachate comprises sulfuric acid, hydrochloric acid, or nitric acid, and the sulfuric acid, hydrochloric acid, or nitric acid produced by the electrodialysis can be recycled to the step of forming the mixture.

[0017] In some embodiments, the acidic leach solution may include at least one oxidizing agent selected from the group consisting of hydrogen peroxide, oxygen, ozone, and lithium persulfate.

[0018] In some embodiments, the lithium hydroxide aqueous solution can be added at 0.1 to 0.5 wt % based on the total weight of the second active metal solution. Effect of the Invention

[0019] According to the above-described exemplary embodiment, the precipitate residue is repeatedly washed with water to increase the concentration of lithium contained in the second active metal solution, and the lithium precursor can be recovered at a high concentration.

[0020] In some embodiments, the second active metal solution can be added with an aqueous lithium hydroxide solution containing an iron salt to precipitate remaining impurities, and the impurities can be removed by solid-liquid separation, whereby the third active metal solution can be easily converted to lithium hydroxide by electrodialysis, and a high-purity lithium precursor can be recovered. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a schematic flow chart illustrating a method for recovering active metals from a lithium secondary battery according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] According to an exemplary embodiment of the present disclosure, there is provided a method for recovering lithium precursors in high purity and high yield from the positive electrodes of spent lithium secondary batteries by a wet-based process.

[0023] As used herein, the term "precursor" is used to refer collectively to a compound containing a specific metal to provide the specific metal contained in the electrode active material.

[0024] FIG. 1 is a schematic flow chart illustrating a method for recovering active metals from a lithium secondary battery according to an exemplary embodiment.

[0025] As shown in FIG. 1, an acidic leachate may be added to a material to be recovered that contains lithium metal oxide to form a mixture that contains a first active metal solution and a leach residue (eg, step S10).

[0026] According to some embodiments, the material to be recovered can be obtained by crushing waste lithium secondary batteries. For example, the lithium metal oxide can be obtained from the positive electrode active material of waste lithium secondary batteries or used lithium secondary batteries.

[0027] The lithium secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, and the positive electrode and the negative electrode may include a positive electrode active material layer and a negative electrode active material layer coated on a positive electrode current collector and a negative electrode current collector, respectively.

[0028] For example, the positive electrode active material contained in the positive electrode active material layer can include a lithium metal oxide containing lithium and a transition metal.

[0029] In some embodiments, the lithium metal oxide can include a compound having a structure represented by Formula 1:

[0030] [Chemical formula 1] Life (1-x) M x PO4

[0031] In Chemical Formula 1, M includes at least one selected from the group consisting of Ni, Co, Mn, Mg, Y, Zn, Ru, Ti, Nb, Mo, Cr, Cu, Zr, W, Ir, and V, and 0≦x≦1 may be satisfied.

[0032] In some embodiments, the lithium metal oxide can include a lithium iron phosphate based active material, for example, an LFP based lithium oxide that includes iron (Fe) and phosphorus (P).

[0033] For example, the positive electrode can be separated from the used lithium secondary battery to recover the used positive electrode. The used positive electrode includes a positive electrode current collector (e.g., aluminum (Al)) and a positive electrode active material layer as described above, and the positive electrode active material layer can include a conductive material and a binder in addition to the positive electrode active material.

[0034] The conductive material may include, for example, a carbon-based material such as graphite, carbon black, graphene, carbon nanotubes, etc. The binder may include, for example, a resin material such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, etc.

[0035] According to some embodiments, the material to be recovered can be obtained by pulverizing the waste positive electrodes, and thus the material to be recovered can include lithium metal oxide, for example, a lithium iron phosphate-based active material (e.g., LiFePO4).

[0036] The material to be recovered may include a component derived from the positive electrode current collector, the binder, or the conductive material. In one embodiment, the material to be recovered may be substantially composed of the lithium metal oxide particles.

[0037] In some embodiments, the material to be recovered may be subjected to a heat treatment prior to reaction with the acidic leachate, which may remove or reduce impurities, such as the conductive material and binder, contained in the material to be recovered, thereby increasing the purity of the lithium metal oxide.

[0038] The temperature of the heat treatment may be, for example, about 100° C. to 500° C. or about 350° C. to 450° C. Within the above range, the impurities can be removed and decomposition and damage of the lithium metal oxide can be prevented.

[0039] An acidic leach solution may be added to the material to be recovered, including the lithium metal oxide prepared according to some of the embodiments described above, to form a mixture including a first active metal solution and a leach residue.

[0040] For example, after separating the positive electrode from the waste lithium secondary battery, an acid leachate can be poured into the separated positive electrode, in which case the positive electrode active material layer can be peeled off from the positive electrode current collector, and the lithium metal oxide can be dissolved in the acid leachate.

[0041] In some embodiments, the acidic leach solution may include at least one oxidizing agent selected from the group consisting of hydrogen peroxide, oxygen, ozone, and lithium persulfate.

[0042] For example, the oxidizing agent can oxidize the iron (Fe) contained in the lithium metal oxide, such as the lithium iron phosphate active material (e.g., LiFePO4), from divalent to trivalent, and precipitate it in the form of iron phosphate (e.g., FePO4). For example, the acidic leaching solution may contain hydrogen peroxide, which can prevent the inclusion of cations.

[0043] In some embodiments, the equivalent ratio of the lithium metal oxide to the oxidizing agent may be 1:0.4 to 1:4, for example, the equivalent ratio may mean using 0.4 moles to 4 moles of the oxidizing agent for each mole of the lithium metal oxide.

[0044] For example, the equivalent ratio of the lithium metal oxide to the oxidizing agent may be 1:0.5 to 1:3.5, 1:1 to 1:3.0, or 1:1.5 to 1:2.5, within the above ranges, the amount of iron oxidized from divalent to trivalent and the amount of FePO4 precipitated are increased, and the concentration of iron impurities can be reduced.

[0045] In some embodiments, the acidic leach solution can include sulfuric acid, hydrochloric acid, or nitric acid, which can provide a first active metal solution in which lithium contained in the lithium metal oxide, e.g., lithium iron phosphate-based active material (e.g., LiFePO4), is selectively leached.

[0046] For example, depending on the type of acid contained in the acid leach solution, the first active metal solution may contain lithium sulfate (Li2SO4), lithium chloride (LiCl), or lithium nitrate (LiNO3).

[0047] In some embodiments, the equivalent ratio of the lithium metal oxide to the acid may be from 0.8:1 to 2.2:1, for example, the equivalent ratio may mean using 0.8 moles to 2.2 moles of the lithium metal oxide for each mole of the acid.

[0048] For example, the equivalent ratio of the lithium metal oxide to the acid may be 0.9:1 to 2.1:1, 1.0:1 to 2.0:1, or 1.1:1 to 2.1:1.

[0049] For example, the equivalent ratio of the lithium metal oxide to the monovalent acid (eg, hydrochloric acid and nitric acid) may be 0.8:1 to 1.2:1, 0.9:1 to 1.1:1, or 1.0:1 to 1.2:1.

[0050] For example, the equivalent ratio of the lithium metal oxide to the diacid (sulfuric acid) may be 1.8:1 to 2.2:1, 1.9:1 to 2.1:1, or 2.0:1 to 2.2:1.

[0051] Within this range, the amount of lithium selectively leached increases, the concentration of lithium contained in the first active metal solution increases, and a high-purity lithium precursor can be recovered.

[0052] In some embodiments, the leach residue may include an iron phosphate-based material. For example, the leach residue may include a precipitate formed when trivalent iron precipitates in the form of iron phosphate (e.g., FePO4). The leach residue may also include a portion of the unrecovered lithium that is not included in the first active metal solution.

[0053] In some embodiments, the mixture can be formed at a pressure of 0.1 atm to 5 atm, a temperature of 50° C. to 90° C., and a rotation speed of 100 rpm to 500 rpm for 1 hour to 4 hours.

[0054] For example, in step S10, the pressure may be 0.3 atm to 4 atm, 0.5 atm to 3 atm, or 0.8 atm to 2 atm, the temperature may be 60° C. to 85° C. or 70° C. to 80° C., the rotation speed may be 150 rpm to 400 rpm or 200 rpm to 300 rpm, and the operation time may be 1.5 to 3 hours or 2 hours to 2.5 hours. Within the above pressure, temperature, rotation speed, and operation time ranges, the amount of lithium contained in the first active metal solution and recovered can be further increased.

[0055] For example, in step S20, the first active metal solution can be separated from the leaching residue into a solid-liquid separation to form a second active metal solution.

[0056] According to an exemplary embodiment, the leach residue may be washed with water to produce a wash solution, and the wash solution may be provided to the mixture or the second active metal solution.

[0057] In some embodiments, the water wash is repeated in multiple cycles, and the wash solution produced from an earlier cycle in the cycles can be fed to the second active metal solution and the wash solution produced from a later cycle in the cycles can be fed to the mixture.

[0058] Thereby, the lithium contained in the leaching residue is recovered as the second active metal solution, and the second active metal solution can be concentrated so as to contain a high concentration of lithium.

[0059] For example, in step S30, a lithium hydroxide aqueous solution containing an iron salt may be added to the second active metal solution to form a third active metal solution in which impurities are removed or reduced.

[0060] In some embodiments, the impurities may include iron (Fe), phosphorus (P) and aluminum (Al). For example, the impurities may be derived from the positive electrode active material layer and positive electrode current collector of a waste lithium secondary battery or a used lithium secondary battery.

[0061] In some embodiments, the iron salt comprises iron sulfate, iron chloride, or iron nitrate, and residual phosphorus may precipitate from the second active metal solution in the form of iron phosphate. For example, the iron sulfate may be iron(III) sulfate (Fe2(SO4)3).

[0062] For example, phosphorus remaining in the second active metal solution reacts with the iron salt to precipitate in the form of iron phosphate (e.g., FePO4), which can be removed by subsequent solid-liquid separation. Iron and aluminum remaining in the second active metal solution also form precipitates, which can be removed by solid-liquid separation.

[0063] In some embodiments, the iron salt can be added in an amount necessary to make the molar ratio of iron (Fe) and phosphorus (P) in the second active metal solution 1:1, which can more effectively precipitate FePO4 and reduce the concentration of residual phosphorus, thereby further increasing the purity and yield of the recovered lithium precursor.

[0064] In some embodiments, the aqueous lithium hydroxide solution may be free of salts of alkali metals or alkaline earth metals other than lithium.

[0065] For example, an aqueous solution of lithium hydroxide can act as a neutralizing agent or base, and lithium ions (Li + ), it is possible to prevent other ions (e.g., ions of alkali metals or alkaline earth metals) from remaining as impurities. This makes it easier to obtain lithium hydroxide by electrodialysis, and allows the recovery of a high-purity lithium precursor.

[0066] For example, when an aqueous solution of sodium hydroxide, an aqueous solution of potassium hydroxide, and / or aqueous ammonia is used instead of an aqueous solution of lithium hydroxide, impurities such as sodium and potassium may remain, resulting in a low purity of the recovered lithium precursor.

[0067] In some embodiments, the lithium hydroxide aqueous solution may be added in an amount of 0.1 wt% to 0.5 wt% based on the total weight of the second active metal solution. For example, the amount of the lithium hydroxide aqueous solution added may be 0.1 wt% to 0.45 wt%, 0.1 wt% to 0.4 wt%, 0.15 wt% to 0.5 wt%, 0.1 wt% to 0.3 wt%, or 0.15 wt% to 0.3 wt% based on the total weight of the second active metal solution.

[0068] Within this range, the lithium hydroxide aqueous solution acts as a neutralizing agent to more effectively precipitate phosphorus remaining in the second active metal solution, thereby reducing the concentration of impurities remaining in the third active metal solution after solid-liquid separation and increasing the purity of the recovered lithium precursor.

[0069] For example, in step S40, a lithium precursor can be recovered from the third active metal solution.

[0070] The third active metal solution contains lithium sulfate, lithium chloride or lithium nitrate and does not contain an alkali metal ion other than lithium (e.g., Na + , K + ) may be absent or may be contained in a trace amount. The lithium precursor may be lithium hydroxide.

[0071] In some embodiments, lithium sulfate, lithium chloride, or lithium nitrate can be converted to lithium hydroxide by electrodialysis to recover the lithium precursor.

[0072] For example, the electrodialysis can be carried out by a bipolar electrodialysis device including a positive electrode and a negative electrode facing each other with an ion exchange membrane therebetween.

[0073] For example, a hydrolysis reaction can be carried out in the bipolar electrodialysis device according to the following formulas 1 to 3. This produces lithium ions (Li + ) (e.g., moving to the negative electrode) and sulfate ions (SO4 2- ), chloride ion (Cl- ) or nitrate ion (NO3 - ) (e.g., to the positive electrode) can be separated by an ion exchange membrane to produce lithium hydroxide and acid. The lithium hydroxide can be collected as the lithium precursor.

[0074] [Formula 1] Li2SO4+2H2O→2LiOH+H2SO4

[0075] [Formula 2] LiCl+H2O→LiOH+HCl

[0076] [Formula 3] LiNO3+H2O→LiOH+HNO3

[0077] In some embodiments, a portion of the lithium hydroxide produced by the electrodialysis can be recycled to the step of forming the third active metal solution (S30), thereby reducing the amount of aqueous lithium hydroxide solution used and further improving the environmental friendliness and productivity of the process.

[0078] In some embodiments, the sulfuric acid, hydrochloric acid, or nitric acid produced by the electrodialysis can be recycled to the step of forming the mixture (S10).

[0079] As shown in the above formulas 1 to 3, sulfate ions (SO4 2- ), chloride ion (Cl - ) or nitrate ion (NO3 - ) can react with water to produce sulfuric acid, hydrochloric acid, or nitric acid. The produced sulfuric acid, hydrochloric acid, or nitric acid can be used as the acid contained in the acid leachate added in step S10.

[0080] This reduces the amount of acid leaching solution used in step S10, improving process efficiency and significantly reducing environmental pollution.

[0081] Examples and comparative examples of the present disclosure are described below. However, the following examples are merely embodiments of the present disclosure and are not intended to limit the present disclosure.

[0082] Examples and Comparative Examples An acidic leaching solution containing 32 g of sulfuric acid and 40 g of hydrogen peroxide was added to 100 g of scrap metal lithium iron phosphate active material, and the mixture was reacted for 2 hours under conditions of 1 atm, 80°C and 250 rpm to obtain a mixture containing a first active metal solution and leaching residue (primary leaching).

[0083] Thereafter, a second active metal solution was obtained from the mixture using a solid-liquid separator, and the separated leaching residue was washed with water (first water washing) to obtain a washing liquid, which was then added to the second active metal solution.

[0084] The leaching residue after washing was washed again with water (secondary water washing) to obtain a washing liquid, which was added to a mixture (secondary leaching) containing the first active metal solution and the leaching residue obtained by a similar method, and then the solution obtained by solid-liquid separation was added to the second active metal solution.

[0085] Thereafter, a base aqueous solution (neutralizing agent) and iron sulfate (Fe2(SO4)3) as shown in Table 1 below were added to the second active metal solution, and the formed precipitate was separated using a solid-liquid separator to obtain a third active metal solution.

[0086] [Table 1] 1) Fe2(SO4)3 margin: The amount of iron sulfate (Fe2(SO4)3) required to make the molar ratio of iron (Fe) and phosphorus (P) in the second active metal solution 1:1. 2) Amount of the second active metal solution added relative to the total weight (wt%)

[0087] Experimental Example 1. Metal concentration of lithium iron phosphate active material before the first leaching The concentrations of metals contained in the lithium iron phosphate active material before the addition of the acid leaching solution are shown in Table 2 below.

[0088] [Table 2]

[0089] 2. Metal concentrations after primary and secondary leaching (1) The percentage of the concentrations of Li, Fe, and P contained in the second active metal solution (before the addition of the cleaning solution) relative to the concentrations of Li, Fe, and P contained in the lithium iron phosphate active material before the addition of the acid leaching solution (the leaching rates of Li, Fe, and P) are shown in Table 3 below.

[0090] [Table 3]

[0091] From Table 3 it can be seen that lithium was selectively leached.

[0092] (2) The concentrations of metals contained in the second active metal solution (before the addition of the washing solution) (a), the washing solution obtained by the first water washing (b), the washing solution obtained by the second water washing (c), and the second active metal solution to which the solution obtained by solid-liquid separation after the second leaching (d) was added are shown in Table 4 below.

[0093] [Table 4]

[0094] From Table 4, it can be seen that the lithium remaining in the leaching residue separated after the first leaching is recovered from the washing solution obtained by the first water washing, and more lithium is recovered by additional washing and second leaching, thereby obtaining a second active metal solution containing a high concentration of lithium.

[0095] 3. Metal concentration of the third active metal solution The concentrations (unit: ppm by weight) of the metals contained in the third active metal solutions according to the examples and comparative examples are shown in Table 5 below.

[0096] [Table 5]

[0097] As shown in Tables 1 and 5, the third active metal solutions according to the examples had lower concentrations of impurities such as iron, phosphorus and sodium than the third active metal solutions according to the comparative examples.

[0098] The third active metal solution of Comparative Example 1, which used an aqueous lithium hydroxide solution but did not use iron sulfate, had a high phosphorus concentration, while the third active metal solutions of Comparative Examples 2 and 3, which used an aqueous sodium hydroxide solution as a neutralizing agent, had a high sodium concentration.

[0099] In addition, the third active metal solution according to Example 2, in which the amount of lithium hydroxide aqueous solution added was high, had a lower iron concentration than the third active metal solution according to Example 1.

[0100] From these, it can be seen that the active metal recovery method of the illustrative embodiment prevents the inclusion of impurities and enables the recovery of a lithium precursor with high purity and high yield.

Claims

1. adding an acidic leach solution to a material to be recovered, the material including lithium metal oxide, to form a mixture including a first active metal solution and a leach residue; separating the first active metal solution from the leaching residue to form a second active metal solution; adding an aqueous lithium hydroxide solution containing an iron salt to the second active metal solution to form a third active metal solution in which impurities have been removed or reduced; and recovering a lithium precursor from the third active metal solution.

2. washing the leach residue with water to produce a wash liquor; The method for recovering active metals from a lithium secondary battery according to claim 1 , further comprising the step of: supplying the cleaning solution to the mixture or the second active metal solution.

3. The water washing is repeated in multiple cycles, the cleaning solution produced from an earlier cycle in the cycle is fed to the second active metal solution; The method for recovering active metals from a lithium secondary battery according to claim 2 , wherein the cleaning solution produced from a later cycle among the cycles is supplied to the mixture.

4. The lithium metal oxide includes a lithium iron phosphate-based active material, 2. The method for recovering active metals of a lithium secondary battery according to claim 1, wherein the first active metal solution contains lithium sulfate, lithium chloride or lithium nitrate, and the leaching residue contains an iron phosphate-based material.

5. 2. The method for recovering active metals from lithium secondary batteries according to claim 1, wherein the material to be recovered is obtained by pulverizing used lithium secondary batteries.

6. 2. The method for recovering active metals from a lithium secondary battery according to claim 1, wherein the impurities include iron (Fe), phosphorus (P) and aluminum (Al).

7. 2. The method for recovering active metals of a lithium secondary battery according to claim 1, wherein the iron salt comprises iron sulfate, iron chloride or iron nitrate, and residual phosphorus is precipitated from the second active metal solution in the form of iron phosphate.

8. 2. The method for recovering active metals from a lithium secondary battery according to claim 1, wherein the lithium hydroxide aqueous solution does not contain salts of alkali metals or alkaline earth metals other than lithium.

9. 2. The method for recovering active metals of a lithium secondary battery according to claim 1, wherein the step of recovering the lithium precursor comprises converting lithium sulfate, lithium chloride or lithium nitrate into lithium hydroxide by electrodialysis.

10. 10. The method for recovering active metals of a lithium secondary battery according to claim 9, further comprising recycling a portion of the lithium hydroxide produced by the electrodialysis to the step of forming the third active metal solution.

11. 10. The method for recovering active metals of a lithium secondary battery according to claim 9, wherein the acidic leaching solution contains sulfuric acid, hydrochloric acid or nitric acid, and further comprises a step of recycling the sulfuric acid, hydrochloric acid or nitric acid produced by the electrodialysis to the step of forming the mixture.

12. 2. The method for recovering active metals from a lithium secondary battery according to claim 1, wherein the acidic leaching solution contains at least one oxidizing agent selected from the group consisting of hydrogen peroxide, oxygen, ozone, and lithium persulfate.

13. 2. The method for recovering active metals from a lithium secondary battery according to claim 1, wherein the lithium hydroxide aqueous solution is added in an amount of 0.1 to 0.5 wt % based on the total weight of the second active metal solution.

Citation Information

Cited By

  • A method for producing lithium iron phosphate from waste lithium iron phosphate material.

    JP2026109503A

  • A method for producing lithium iron phosphate from waste lithium iron phosphate material.

    JP7951370B2