Underfill material, electronic component device and method for producing electronic component device
The underfill material composition addresses stress and thermal expansion issues in semiconductor devices by combining epoxy resin, curing agent, and inorganic filler, improving crack resistance and reliability.
Patent Information
- Application Number
- JP2024120328
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2036-10-14
AI Technical Summary
Semiconductor technology advancements have led to larger and thinner semiconductors and wiring boards, causing stress concentration in solder resist due to high elastic modulus underfill materials, which can result in cracks during reflow, and reducing inorganic filler content exacerbates thermal expansion issues.
An underfill material composition comprising epoxy resin, curing agent, and inorganic filler, with specific thermal expansion and storage modulus properties, optionally including flexibilizing agents and other additives, to mitigate stress and thermal expansion.
The underfill material effectively suppresses solder resist cracks during reflow and enhances temperature cycle resistance, ensuring high reliability of electronic component devices.
Smart Images

Figure 2024138099000001 
Figure 2024138099000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an underfill material, an electronic component device, and a method for manufacturing an electronic component device. [Background technology]
[0002] Conventionally, in the field of element encapsulation of electronic component devices such as transistors, ICs (Integrated Circuits), and LSIs (Large Scale Integration), the mainstream method is to encapsulate using an encapsulating material containing a resin from the viewpoints of productivity, cost, etc. Epoxy resin compositions are widely used as encapsulating materials because epoxy resins have a good balance of various properties such as workability, moldability, electrical properties, moisture resistance, heat resistance, mechanical properties, and adhesion to insert products.
[0003] 2. Description of the Related Art Underfill materials are widely used as sealing materials in electronic component devices with bare chips mounted thereon, such as chip on board (COB), chip on glass (COG), and tape carrier package (TCP). In addition, in electronic component devices (flip chips) in which electronic components such as semiconductor elements are directly bump-connected to a wiring board made of ceramic, glass epoxy resin, glass imide resin, polyimide film, etc., epoxy resin compositions are used as underfill materials that fill the gaps between the bump-connected electronic components and the wiring board. Underfill materials play an important role in protecting electronic components from temperature, humidity, and external mechanical forces.
[0004] Here, in order to provide an encapsulating epoxy resin composition excellent in moisture-resistant adhesive strength and low stress, and an electronic component device having an element encapsulated therewith and having high reliability (moisture resistance, thermal shock resistance), an encapsulating epoxy resin composition containing (A) a liquid epoxy resin, (B) a curing agent containing a liquid aromatic amine, (C) rubber particles, and (D) an inorganic filler, as well as an electronic component device having an element encapsulated with this encapsulating epoxy resin composition have been disclosed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-270976 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, semiconductor technology has progressed remarkably, and semiconductors and wiring boards are becoming larger and thinner. Therefore, in the flip chip method using bump connections, if the elastic modulus of the cured underfill material at the reflow temperature is high, the cured underfill material cannot keep up with the expansion of the bumps, and stress is likely to concentrate on the solder resist formed on the wiring board. The concentration of stress on the solder resist may cause cracks in the solder resist on the wiring board due to the expansion of the bumps during reflow. The elastic modulus of the cured underfill material can be lowered by reducing the amount of inorganic filler contained in the underfill material. However, reducing the amount of inorganic filler too much increases the thermal expansion coefficient, which may cause problems due to expansion and contraction of the cured underfill material during temperature cycle testing.
[0007] As described above, with the progress of semiconductor technology, underfill materials are required to solve various problems. The present invention has been made in consideration of the above circumstances, and has an object to provide an underfill material that suppresses the occurrence of cracks in solder resist during reflow and has excellent temperature cycle resistance characteristics, as well as a highly reliable electronic component device encapsulated therewith and a method for manufacturing the same. [Means for solving the problem]
[0008] As a result of extensive investigations into solving the above problems, the inventors have found that the above object can be achieved by forming an underfill material composition containing (A) an epoxy resin, (B) a curing agent, and (C) an inorganic filler, and by setting the thermal expansion coefficient below the glass transition temperature of the cured product to 30 ppm / °C or less as measured by TMA (thermomechanical analysis) and the storage modulus at 240°C to 0.10 GPa or less as measured by DMA (dynamic viscoelastic analysis), thereby completing the present invention.
[0009] The present invention relates to the following: <1> (A) an epoxy resin, (B) a curing agent, and (C) an inorganic filler; An underfill material that, when cured, has a thermal expansion coefficient below the glass transition temperature of 30 ppm / ℃ or less as measured by TMA (thermomechanical analysis), and a storage modulus at 240℃ of 0.10 GPa or less as measured by DMA (dynamic mechanical analysis). <2> The glass transition temperature of the cured product, as measured by TMA (thermomechanical analysis), is 60°C to 150°C. <1> The underfill material according to claim 1. <3> When cured, the storage modulus at 25°C measured by DMA (dynamic mechanical analysis) is 5 GPa to 10 GPa. <1> or <2> The underfill material according to claim 1. <4> Further containing (D) a flexibilizing agent, <1> ~ <3> 13. The underfill material according to claim 12 . <5> Further containing (E) a surfactant, <1> ~ <4> 13. The underfill material according to claim 12 . <6> Further containing (F) an ion trapping agent, <1> ~ <5> 13. The underfill material according to claim 12 . <7> Further containing (G) a curing accelerator, <1> ~ <6> 13. The underfill material according to claim 12 . <8> Further containing (H) a coupling agent, <1> ~ <7> 13. The underfill material according to claim 12 . <9> Further containing (I) an antioxidant, <1> ~ <8> 13. The underfill material according to claim 12 . <10> Further, (J) an organic solvent is contained, and the content of the organic solvent is 10 mass% or less. <1> ~ <9> 13. The underfill material according to claim 12 . <11> The (B) curing agent is an aromatic amine compound. <1> ~ <10> 13. The underfill material according to claim 12 . <12> A wiring board; an electronic component disposed on the wiring board and electrically connected to the wiring board via a connection portion; At least the connection portion between the wiring board and the electronic component is sealed. <1> ~ <11> A cured product of the underfill material according to any one of claims 1 to 5, An electronic component device comprising: <13> The connection does not contain lead; <12> The electronic component device according to claim 1 . <14> The connection portion comprises copper. <12> or <13> The electronic component device according to claim 1 . <15> A method for manufacturing an electronic component device in which an electronic component and a wiring board are electrically connected via a connection portion, comprising the steps of: At least one of a surface of the electronic component facing the wiring board and a surface of the wiring board facing the electronic component, <1> ~ <11> A supplying step of supplying the underfill material according to any one of claims 1 to 5; a connecting step of connecting the electronic component and the wiring board via the connecting portion and curing the underfill material. <16> A method for manufacturing an electronic component device in which an electronic component and a wiring board are electrically connected via a connection portion, comprising the steps of: In the gap between the connected electronic component and the wiring board <1> ~ <11> A filling step of filling the underfill material according to any one of the above items. and a curing step of curing the underfill material. Effect of the Invention
[0010] According to the present invention, there are provided an underfill material which suppresses the occurrence of cracks in the solder resist during reflow and has excellent temperature cycle resistance characteristics, as well as a highly reliable electronic component device encapsulated therewith and a method for manufacturing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In this specification, the term "process" refers not only to an independent process, but also to a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Furthermore, in this specification, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. In this specification, the content of each component in a composition means, when multiple substances corresponding to each component are present in the composition, the total content of those multiple substances present in the composition, unless otherwise specified. In this specification, the particle size of each component in a composition means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified, when multiple types of particles corresponding to each component are present in the composition. In this specification, the terms "layer" and "film" include cases where the layer or film is formed over the entire area when the area in which the layer or film is present is observed, as well as cases where the layer or film is formed over only a portion of the area.
[0012] <Underfill material> The underfill material disclosed herein comprises (A) an epoxy resin, (B) a curing agent, and (C) an inorganic filler, and when cured, has a thermal expansion coefficient below the glass transition temperature of 30 ppm / °C or less as measured by TMA (thermomechanical analysis), and a storage modulus at 240°C of 0.10 GPa or less as measured by DMA (dynamic mechanical analysis).
[0013] Each component constituting the underfill material of the present disclosure will be described below.
[0014] ((A) Epoxy resin) The epoxy resin of component (A) used in the present disclosure is not particularly limited as long as it has one or more epoxy groups in one molecule, and any epoxy resin commonly used in underfill materials can be used. The type of epoxy resin used in the present disclosure is not particularly limited. Examples of epoxy resins include glycidyl ether type epoxy resins obtained by reacting bisphenol A, bisphenol F, bisphenol AD, bisphenol S, hydrogenated bisphenol A, naphthalene diol, alkyl diol, etc. with epichlorohydrin, novolac type epoxy resins obtained by epoxidizing novolac resins obtained by condensing or co-condensing phenols, such as orthocresol novolac type epoxy resins, with aldehydes, glycidyl ester type epoxy resins obtained by reacting polybasic acids, such as phthalic acid and dimer acid, with epichlorohydrin, glycidyl amine type epoxy resins obtained by reacting amine compounds, such as aminophenol, diaminodiphenylmethane, isocyanuric acid, with epichlorohydrin, linear aliphatic epoxy resins obtained by oxidizing olefin bonds with peracids, such as peracetic acid, alicyclic epoxy resins, etc., which may be used alone or in combination of two or more. Among these, liquid bisphenol type epoxy resins, which are a type of glycidyl ether type epoxy resins, are preferred from the viewpoint of fluidity, and liquid glycidyl amine type epoxy resins are preferred from the viewpoints of heat resistance, adhesiveness and fluidity.
[0015] The above-mentioned two types of epoxy resins may be used either alone or in combination, but in order to exhibit their performance, their blending ratio in total is preferably 20 mass % or more, more preferably 30 mass % or more, and even more preferably 50 mass % or more, based on the total amount of the epoxy resin. In addition, the underfill material of the present disclosure can also be used in combination with a solid epoxy resin as long as the effects of the present disclosure are achieved. From the viewpoint of the fluidity of the underfill material, the amount of the solid epoxy resin used in combination is preferably 20 mass % or less based on the total amount of the epoxy resin.
[0016] In order to ensure that the thermal expansion coefficient below the glass transition temperature, as measured by TMA (thermomechanical analysis), of the cured underfill material is 30 ppm / °C or less, the proportion of epoxy resin containing an aromatic ring in the molecule in the total amount of epoxy resin is preferably 65 mass % or more, and more preferably 70 mass % or more. In order to ensure that the storage modulus of the cured underfill material at 240°C measured by DMA (dynamic mechanical analysis) is 0.10 GPa or less, the proportion of tri- or higher functional epoxy resins in the total amount of epoxy resins is preferably 80 mass % or less, more preferably 70 mass % or less, and even more preferably 60 mass % or less.
[0017] Liquid epoxy resin means an epoxy resin that is liquid at room temperature (25°C). Specifically, it means that the viscosity measured with an E-type viscometer at 25°C is 1000 Pa s or less. Specifically, the above viscosity is measured using an EHD-type E-type viscometer (cone angle 3°, cone diameter 28 mm), with a measurement temperature of 25°C, sample volume of 0.7 ml, and the rotation speed set according to the expected viscosity of the sample with reference to the following, and the value measured one minute after the start of measurement is the measured value. (1) When the expected viscosity is 100 Pa·s to 1000 Pa·s: Rotation speed 0.5 rpm (2) When the expected viscosity is less than 100 Pa·s: Rotation speed: 5 rpm In addition, a solid epoxy resin means an epoxy resin that is solid at room temperature (25°C).
[0018] The purity of the epoxy resin, especially the amount of hydrolyzable chlorine, is preferably low because it is related to the corrosion of aluminum wiring on elements such as ICs, and in order to obtain an underfill material with excellent moisture resistance, the amount of hydrolyzable chlorine in the epoxy resin is preferably 500 ppm or less. Here, the amount of hydrolyzable chlorine is measured by dissolving 1 g of a sample epoxy resin in 30 ml of dioxane, adding 5 ml of 1N-KOH methanol solution, refluxing for 30 minutes, and then measuring the value obtained by potentiometric titration.
[0019] From the viewpoint of viscosity adjustment, the epoxy equivalent of the epoxy resin is preferably 90 g / eq to 450 g / eq, more preferably 90 g / eq to 350 g / eq, and even more preferably 90 g / eq to 250 g / eq. The epoxy equivalent of an epoxy resin is measured by dissolving a weighed amount of the epoxy resin in a solvent such as methyl ethyl ketone, adding acetic acid and a tetraethylammonium bromide acetate solution, and then subjecting the solution to potentiometric titration with a perchloric acid acetate standard solution. An indicator may be used in this titration.
[0020] The content of the epoxy resin is not particularly limited, and for example, in terms of the proportion of the solid content of the underfill material, it is preferably 10% by mass to 50% by mass, more preferably 15% by mass to 45% by mass, and even more preferably 20% by mass to 40% by mass. In this disclosure, the "solid content" of the underfill material means the remaining components after removing volatile components such as organic solvents from the underfill material.
[0021] ((B) Hardener) The curing agent of component (B) used in the present disclosure is not particularly limited. As the curing agent, examples of amines having an aromatic ring (aromatic amine compounds) include diethyltoluenediamine, 1,3,5-triethyl-2,6-diaminobenzene, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and 3,5,3',5'-tetramethyl-4,4'-diaminodiphenylmethane. These aromatic amine compounds are commercially available, such as Epicure-W, Epicure-Z (product names manufactured by Mitsubishi Chemical Corporation), Kayahard AA, Kayahard AB, Kayahard AS (product names manufactured by Nippon Kayaku Co., Ltd.), Tohtoamine HM-205 (product name manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.), Adeka Hardener EH-101 (product name manufactured by ADEKA Corporation), Epomic Q-640, Epomic Q-643 (product names manufactured by Mitsui Chemicals, Inc.), and DETDA80 (product name manufactured by Lonza), and these may be used alone or in combination of two or more types.
[0022] When an aromatic amine compound is used as a curing agent, from the viewpoint of storage stability of the underfill material, for example, 3,3'-diethyl-4,4'-diaminodiphenylmethane and diethyltoluenediamine are preferable. Examples of diethyltoluenediamine include 3,5-diethyltoluene-2,4-diamine and 3,5-diethyltoluene-2,6-diamine. When an aromatic amine compound is used as a curing agent, the curing agent is preferably one containing 50 mass% or more of 3,3'-diethyl-4,4'-diaminodiphenylmethane or 3,5-diethyltoluene-2,4-diamine.
[0023] Examples of the acid anhydride as the curing agent include phthalic anhydride, maleic anhydride, methyl himic anhydride, himic anhydride, succinic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, chlorendic anhydride, methyl tetrahydrophthalic anhydride, 3-methylhexahydrophthalic anhydride, 4-methylhexahydrophthalic anhydride, trialkyl tetrahydrophthalic anhydride maleic anhydride, benzophenone tetracarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, hydrogenated methyl nadic anhydride, trialkyl tetrahydrophthalic anhydride obtained by Diels-Alder reaction from maleic anhydride and a diene compound, dodecenyl succinic anhydride, and other various acid anhydrides. These may be used alone or in combination of two or more.
[0024] When an acid anhydride is used as the curing agent, from the viewpoint of reducing the viscosity of the underfill material, for example, tetrahydrophthalic anhydride and hexahydrophthalic anhydride are preferable. When an acid anhydride is used as the curing agent, the curing agent preferably contains 50 mass% or more of tetrahydrophthalic anhydride or hexahydrophthalic anhydride.
[0025] In addition, in addition to the aromatic amine compound and the acid anhydride, the underfill material can also contain a curing agent that is commonly used in underfill materials, such as a phenolic curing agent, as long as the effects of the present disclosure are achieved. As the curing agent, an aromatic amine compound is preferable because the cured product is unlikely to be hydrolyzed and therefore has good moisture resistance reliability.
[0026] The equivalent ratio of the epoxy resin equivalent number to the curing agent equivalent number contained in the underfill material (curing agent equivalent number / epoxy resin equivalent number) is preferably 0.7 to 1.3, more preferably 0.8 to 1.2, and even more preferably 0.9 to 1.1. If the ratio is 0.7 or more, the curing agent is not insufficient, the epoxy resin not involved in the reaction is reduced, and the reliability tends not to deteriorate. On the other hand, if the ratio is 1.3 or less, the excess curing agent is reduced, so the glass transition temperature does not become too high, and the elastic modulus of the cured product at high temperatures does not become too high, so that warping at room temperature and high temperatures tends not to occur.
[0027] ((C) Inorganic filler) Examples of the inorganic filler of component (C) used in the present disclosure include powders such as spherical silica, crystalline silica, and the like, calcium carbonate, clay, alumina, silicon nitride, silicon carbide, boron nitride, calcium silicate, potassium titanate, aluminum nitride, beryllia, zirconia, zircon, fosterite, steatite, spinel, mullite, and titania, as well as beads obtained by spheronizing these, and glass fibers. Further, examples of inorganic fillers having a flame retardant effect include aluminum hydroxide, magnesium hydroxide, zinc borate, zinc molybdate, etc. These inorganic fillers may be used alone or in combination of two or more. Among them, spherical silica is more preferable from the viewpoint of the flowability and permeability of the underfill material into fine gaps.
[0028] The average particle size of the inorganic filler, particularly in the case of spherical silica, is preferably in the range of 0.05 μm to 20 μm, more preferably in the range of 0.2 μm to 10 μm. If the average particle size is 0.05 μm or more, the dispersibility in the liquid resin is improved, the viscosity is unlikely to increase, and the flow characteristics of the underfill material tend to be improved. If the average particle size is 20 μm or less, sedimentation tends to be unlikely to occur, and the permeability and flowability of the underfill material into fine gaps are improved, making it difficult to cause voids and unfilled underfill material. Here, the average particle size is the particle size that corresponds to 50% volume when a cumulative frequency distribution curve of particle sizes is calculated assuming the total volume of the particles to be 100%, and can be measured using a particle size distribution measuring device using a laser diffraction scattering method, etc.
[0029] The content of the inorganic filler, as a percentage of the solid content of the underfill material, is preferably in the range of 20% by mass to 90% by mass, more preferably 30% by mass to 85% by mass, and even more preferably 40% by mass to 80% by mass. If the content is 20% by mass or more, the thermal expansion coefficient is less likely to decrease and the temperature cycle resistance of the cured product of the underfill material tends to be more excellent, and if it is 90% by mass or less, the viscosity of the underfill material is less likely to increase and the fluidity, permeability, and dispensability tend not to decrease.
[0030] ((D) Flexibilizer) The underfill material of the present disclosure may contain various flexibilizing agents from the standpoint of improving thermal shock resistance, reducing stress on electronic components such as semiconductor elements, and the like. The flexibilizer is not particularly limited, but is preferably rubber particles. Examples of the rubber particles include rubber particles of silicone rubber and rubber particles of synthetic rubber other than silicone rubber (hereinafter, sometimes simply referred to as "synthetic rubber"). Examples of synthetic rubber particles include rubber particles of styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), butadiene rubber (BR), urethane rubber (UR), acrylic rubber (AR), etc. Among them, rubber particles of acrylic rubber are preferred from the viewpoint of heat resistance and moisture resistance, and core-shell type acrylic polymer, i.e., core-shell type acrylic rubber particles, are more preferred.
[0031] Examples of silicone rubber particles include silicone rubber particles crosslinked with polyorganosiloxanes such as linear polydimethylsiloxane, polymethylphenylsiloxane, and polydiphenylsiloxane, silicone rubber particles whose surfaces are coated with silicone resin, core-shell polymer particles having a core of solid silicone particles obtained by emulsion polymerization and a shell of a polymer such as acrylic resin, and spherical silicone particles whose surfaces are modified with epoxy groups. These silicone rubber particles can be used in either an amorphous or spherical shape. In order to keep the viscosity, which is related to the moldability of the underfill material, low, it is preferable to use spherical particles. These silicone rubber particles are commercially available from Dow Corning Toray Co., Ltd., Shin-Etsu Chemical Co., Ltd., and other companies.
[0032] The average particle size of these flexibilizers is preferably small in order to modify the underfill material uniformly, and is preferably in the range of 0.05 μm to 10 μm, and more preferably in the range of 0.1 μm to 5 μm. If the average particle size is 0.05 μm or more, the dispersibility in the underfill material tends to be excellent, and if it is 10 μm or less, the stress tends to be reduced, and further, the permeability and fluidity of the underfill material into fine gaps are improved, making it less likely that voids and unfilled underfill material will occur.
[0033] The content of the flexibilizer is preferably set in the range of 1% by mass to 30% by mass, and more preferably 2% by mass to 20% by mass, based on the total epoxy resin. If the content of the flexibilizer is 1% by mass or more, the effect of reducing stress tends to be improved, and if it is 30% by mass or less, the viscosity of the underfill material is less likely to increase, and moldability (flow characteristics, etc.) tends to be excellent.
[0034] ((E) Surfactant) The underfill material of the present disclosure may contain various surfactants from the viewpoints of reducing the occurrence of voids during molding and improving adhesive strength by improving wettability to various adherends. The surfactant is not particularly limited, but a nonionic surfactant is preferred, and examples thereof include polyoxyalkylene alkyl ether surfactants such as polyoxyethylene alkyl ether surfactants, sorbitan fatty acid ester surfactants, polyoxyethylene sorbitan fatty acid ester surfactants, polyoxyethylene sorbitol fatty acid ester surfactants, glycerin fatty acid ester surfactants, polyoxyethylene fatty acid ester surfactants, polyoxyethylene alkylamine surfactants, alkyl alkanolamide surfactants, polyether modified silicone surfactants, aralkyl modified silicone surfactants, polyester modified silicone surfactants, and polyacrylic surfactants, which may be used alone or in combination of two or more. These surfactants are commercially available from BYK Japan Co., Ltd., Kao Corporation, etc.
[0035] In addition, a silicone-modified epoxy resin can be added as a surfactant. The silicone-modified epoxy resin can be obtained as a reaction product between an organosiloxane having a functional group reactive with an epoxy group and an epoxy resin. The silicone-modified epoxy resin is preferably liquid at room temperature (25°C). Examples of organosiloxane having a functional group reactive with an epoxy group include dimethylsiloxane, diphenylsiloxane, and methylphenylsiloxane having one or more amino groups, carboxy groups, hydroxyl groups, phenolic hydroxyl groups, mercapto groups, etc. in one molecule. The weight-average molecular weight of the organosiloxane is preferably in the range of 500 to 5000. If the weight-average molecular weight of the organosiloxane is 500 or more, the compatibility with epoxy resins and the like is not too improved, and the effect as an additive tends to be easily exhibited. When the weight-average molecular weight of the organosiloxane is 5,000 or less, it is unlikely to be incompatible with epoxy resins, etc., and therefore the silicone-modified epoxy resin is unlikely to separate or exude from the underfill material when the underfill material is cured, and problems such as impairing adhesion or appearance tend not to occur. The weight average molecular weight of the organosiloxane is determined by converting the molecular weight distribution measured by GPC (gel permeation chromatography) using a calibration curve of standard polystyrene.
[0036] There are no particular limitations on the epoxy resin used to obtain the silicone modified epoxy resin, so long as it is compatible with the resin system of the underfill material, and any epoxy resin commonly used in underfill materials can be used. Examples of the epoxy resin include glycidyl ether type epoxy resins obtained by reacting bisphenol A, bisphenol F, bisphenol AD, bisphenol S, naphthalenediol, hydrogenated bisphenol A, or the like, with epichlorohydrin; novolac type epoxy resins obtained by epoxidizing a novolac resin obtained by condensing or co-condensing a phenol, such as orthocresol novolac type epoxy resin, with an aldehyde; glycidyl ester type epoxy resins obtained by reacting a polybasic acid, such as phthalic acid or dimer acid, with epichlorohydrin; glycidyl amine type epoxy resins obtained by reacting an amine compound, such as diaminodiphenylmethane or isocyanuric acid, with epichlorohydrin; linear aliphatic epoxy resins obtained by oxidizing an olefin bond with a peracid, such as peracetic acid; and alicyclic epoxy resins. These may be used alone or in combination of two or more kinds, but those that are liquid at room temperature (25° C.) are preferred.
[0037] The content of the surfactant is preferably 0.01% by mass to 1.5% by mass, and more preferably 0.05% by mass to 1% by mass, based on the total epoxy resin. If the content of the surfactant is 0.01% by mass or more, a sufficient effect of addition tends to be easily obtained, and if it is 1.5% by mass or less, the surfactant is less likely to bleed out from the surface of the cured product when the underfill material is cured, and the adhesive strength tends not to decrease.
[0038] ((F) Ion trapping agent) In the underfill material of the present disclosure, an ion trap agent can be blended as necessary from the viewpoints of improving migration resistance, moisture resistance, and high-temperature storage characteristics, as long as the filling property and fluidity during application to an electronic component device are not impaired. There are no particular restrictions on the ion trap agent, and conventionally known ones can be used. Hydrotalcite represented by the following compositional formula (I) or hydrated bismuth oxide represented by the following compositional formula (II) is preferable.
[0039] Mg 1-X Al X (OH)2(CO3) X / 2 ·mH2O (I) (In compositional formula (I), 0 < X ≦ 0.5, and m represents a positive number.) BiO a (OH) b (NO3) c (II) (In compositional formula (II), a, b, and c are each 0.9 ≦ a ≦ 1.1, 0.6 ≦ b ≦ 0.8, and 0.2 ≦ c ≦ 0.4, respectively.)
[0040] The content of the ion trap agent is preferably 0.1% by mass to 3.0% by mass, more preferably 0.3% by mass to 1.5% by mass, based on the total amount of the epoxy resin. The average particle size of the ion trap agent is preferably 0.1 μm to 3.0 μm, and the maximum particle size is preferably 10 μm or less. Note that the compound represented by the above compositional formula (I) is available as a commercial product under the trade name DHT-4A manufactured by Kyowa Chemical Industry Co., Ltd. Also, the compound represented by the above compositional formula (II) is available as a commercial product under the trade name IXE-500 (manufactured by Toagosei Co., Ltd.). Also, if necessary, other anion exchangers can be blended as the ion trap agent. There are no particular restrictions on the anion exchanger, and conventionally known ones can be used. Examples of the ion trap agent include hydrated oxides such as magnesium, aluminum, titanium, zirconium, and antimony, and these can be used alone or in combination of two or more.
[0041] ((G) Curing accelerator) The underfill material of the present disclosure may contain various curing accelerators from the viewpoint of accelerating the curing reaction between the epoxy resin and the curing agent. The curing accelerator is not particularly limited as long as it accelerates the reaction between the epoxy resin and the curing agent, and conventionally known accelerators can be used. Examples of the curing accelerator include cycloamidine compounds such as 1,8-diaza-bicyclo(5.4.0)undecene-7, 1,5-diaza-bicyclo(4.3.0)nonene, and 5,6-dibutylamino-1,8-diaza-bicyclo(5.4.0)undecene-7, tertiary amine compounds such as triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol, 2-methylimidazole, and 2-ethyl-4-methylimidazoline. imidazole compounds such as 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4-diamino-6-(2'-methylimidazolyl-(1'))-ethyl-s-triazine, and 2-heptadecylimidazole; tributylphosphine and other triaryl compounds; and organic phosphines such as dialkylarylphosphines such as alkyl phosphine and dimethylphenylphosphine, alkyldiarylphosphines such as methyldiphenylphosphine, triarylphosphines such as triphenylphosphine and alkyl-substituted triphenylphosphine; compounds having intramolecular polarization obtained by adding compounds having a π bond such as maleic anhydride, 1,4-benzoquinone, 2,5-toluquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, 2,3-dimethoxy-5-methyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, and phenyl-1,4-benzoquinone to these compounds, diazophenylmethane, and phenol resins, and derivatives thereof; and phenylboron salts such as 2-ethyl-4-methylimidazole tetraphenylborate and N-methylmorpholine tetraphenylborate. These may be used alone or in combination of two or more.Furthermore, examples of the latent curing accelerator include core-shell particles in which a core is a compound having an amino group that is solid at room temperature (25° C.) and a shell is coated with an epoxy compound that is solid at room temperature (25° C.). Commercially available products that can be used include Amicure (trade name, manufactured by Ajinomoto Co., Inc.) and Novacure (trade name, manufactured by Asahi Kasei Co., Ltd.), which is imparted with latency by dispersing microencapsulated amine in bisphenol A type epoxy resin and bisphenol F type epoxy resin.
[0042] Among these, imidazole derivatives are preferred from the viewpoint of the balance between the curing acceleration effect and reliability, and imidazole derivatives having a phenyl group and a hydroxyl group as substituents, such as 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and Novacure (trade name, manufactured by Asahi Kasei Corporation), which is obtained by dispersing microencapsulated amine in bisphenol A type epoxy resin and bisphenol F type epoxy resin to impart latency, are more preferred, and 2-phenyl-4,5-dihydroxymethylimidazole and 2-phenyl-4-methyl-5-hydroxymethylimidazole are even more preferred.
[0043] The content of the curing accelerator is not particularly limited as long as it is an amount that achieves the curing acceleration effect, but is preferably in the range of 0.2% by mass to 5% by mass, and more preferably in the range of 0.5% by mass to 3% by mass, relative to the mass of the total epoxy resin. If the content of the curing accelerator is 0.2% by mass or more, the effect of adding the curing accelerator is fully exerted, and as a result, it becomes possible to suppress the generation of voids when curing the underfill material, and the warpage reduction effect tends to be sufficient, and if it is 5% by mass or less, the storage stability tends to be excellent.
[0044] ((H) Coupling Agent) The underfill material of the present disclosure may contain a coupling agent for the purpose of strengthening adhesion at the interface between the epoxy resin and the inorganic filler, or between the epoxy resin and the constituent members of the electronic component device. There is no particular limitation on the coupling agent, and any conventionally known one may be used. Examples of the coupling agent include silane compounds having at least one selected from the group consisting of primary amino groups, secondary amino groups, and tertiary amino groups, various silane-based compounds such as epoxy silane, mercaptosilane, alkyl silane, ureidosilane, and vinyl silane, titanium-based compounds, aluminum chelates, and zirconium-based compounds. Examples of these include vinyltrichlorosilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, vinyltriacetoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-anilinopropyltrimethoxysilane, γ-anilinopropyltriethoxysilane, γ-(N,N-dimethyl)aminopropyl aryltrimethoxysilane, γ-(N,N-diethyl)aminopropyltrimethoxysilane, γ-(N,N-dibutyl)aminopropyltrimethoxysilane, γ-(N-methyl)anilinopropyltrimethoxysilane, γ-(N-ethyl)anilinopropyltrimethoxysilane, γ-(N,N-dimethyl)aminopropyltriethoxysilane, γ-(N,N-diethyl)aminopropyltriethoxysilane, γ-(N,N-dibutyl)aminopropyltriethoxysilane, γ-(N-methyl)anilinopropyltriethoxysilane, γ-(N-ethyl)anilinopropyltriethoxysilane, γ-(N,N-dimethyl)aminopropylmethyldimethoxysilane, γ-(N,N-diethyl)aminopropylmethyldimethoxysilane, γ-(N,Silane coupling agents such as N-dibutyl)aminopropylmethyldimethoxysilane, γ-(N-methyl)anilinopropylmethyldimethoxysilane, γ-(N-ethyl)anilinopropylmethyldimethoxysilane, N-(trimethoxysilylpropyl)ethylenediamine, N-(dimethoxymethylsilylisopropyl)ethylenediamine, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, γ-chloropropyltrimethoxysilane, hexamethyldisilane, vinyltrimethoxysilane, and γ-mercaptopropylmethyldimethoxysilane; isopropyl triisostearoyl titanate, isopropyl tris(dioctylpyrophosphate)titanate, isopropyl tri(N-aminoethyl-aminoethyl)titanate, and tetraoctylbis(di tridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl phosphite) titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, bis(dioctyl pyrophosphate)ethylene titanate, isopropyl trioctanoyl titanate, isopropyl dimethacryl isostearoyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, isopropyl isostearoyl diacryl titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumyl phenyl titanate, tetraisopropyl bis(dioctyl phosphite) titanate, and other titanate-based coupling agents, which may be used alone or in combination of two or more.
[0045] The content of the coupling agent is preferably 0.1% by mass to 10% by mass, and more preferably 1% by mass to 5% by mass, based on the total epoxy resin.
[0046] ((I) Antioxidants) The underfill material of the present disclosure may contain an antioxidant. As the antioxidant, any known antioxidant may be used. As phenolic compound-based antioxidants, there are compounds having at least one alkyl group at the ortho position of the phenol nucleus, such as 2,6-di-t-butyl-4-methylphenol, n-octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis-(4-methyl-6-t-butylphenol), 3,9-bis[2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]u, and the like. , 4,4'-butylidenebis-(6-t-butyl-3-methylphenol), 4,4'-thiobis(6-t-butyl-3-methylphenol), tetrakis[methylene-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]methane, 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionamide], isooctyl-3-(3,5-di-t-butyl 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 4,6-bis(dodecylthiomethyl)-o-cresol, bis[3,5-di-t-butyl-4-hydroxybenzyl(ethoxy)phosphinate]calcium, 2,4-1-bis[(octylthio)methyl]-o-cresol, 1,6-hexanediol-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 6-[3-(3-t-butyl-4 -hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenz[d,f][1,3,2]dioxaphosphepine, 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenylacrylate, 2-[1-(2-hydroxy-3,5-di-t-pentylphenyl)ethyl]-4,6-di-t-pentylphenylacrylate, 2,2'-methylenebis-(4-ethyl-6-t-butylphenol), 2,6-di-t-butyl-4-ethylphenol, 1,1,Examples of such compounds include 3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, triethylene glycol-bis[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionate], tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 2,5,7,8-tetramethyl-2-(4',8',12'-trimethyltridecyl)chroman-6-ol, and 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine. The organic sulfur compound antioxidants include dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, pentaerythrityl tetrakis (3-lauryl thiopropionate), ditridecyl-3,3'-thiodipropionate, 2-mercaptobenzimidazole, 4,4'-thiobis (6-t-butyl-3-methyl phenol), 2,2-thio-diethylenebis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 4,6-bis(dodecylthiomethyl)-o-cresol, 2,4-1-bis[(octylthio)methyl]-o-cresol, 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, and the like. Examples of the amine compound antioxidants include N,N'-diallyl-p-phenylenediamine, N,N'-di-sec-butyl-p-phenylenediamine, octylated diphenylamine, and 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine. Among the amine compound-based antioxidants, dicyclohexylamine is commercially available under the trade name D-CHA-T manufactured by New Japan Chemical Co., Ltd., and its derivatives include dicyclohexylamine ammonium nitrite, N,N-di(3-methyl-cyclohexyl)amine, N,N-di(2-methoxy-cyclohexyl)amine, and N,N-di(4-bromo-cyclohexyl)amine. Phosphorus compound antioxidants include trisnonylphenyl phosphite, triphenyl phosphite, bis[3,5-di-t-butyl-4-hydroxybenzyl (ethoxy)phosphinate]calcium, tris(2,4-di-t-butylphenyl)phosphite, 2-[[2,4,8,10-tetrakis(1,1-dimethylether)dibenzo[d,f][1,3,2]dioxaphosphepin-6-yl]oxy]-N,N-bis[2-{[2,4,8 ,10-tetrakis(1,1 dimethylethyl)dibenzo[d,f][1,3,2]dioxaphosphepin-6-yl]oxy}-ethyl]ethanamine, 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenz[d,f][1,3,2]dioxaphosphepin, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, and the like. The antioxidant may be used alone or in combination of two or more. Specific examples of the antioxidant include compounds that contain at least one of a phosphorus atom, a sulfur atom, and an amine in the same molecule in addition to a phenolic hydroxyl group, but these compounds may be listed multiple times.
[0047] The content of the antioxidant is preferably 0.1% by mass to 10% by mass, and more preferably 0.5% by mass to 5% by mass, based on the total epoxy resin.
[0048] ((J) Organic Solvent) The underfill material of the present disclosure may be blended with an organic solvent as necessary to reduce viscosity. In particular, when a solid epoxy resin and hardener are used, it is preferable to blend an organic solvent in order to obtain a liquid underfill material. The organic solvent is not particularly limited, and examples thereof include alcohol-based solvents such as methyl alcohol, ethyl alcohol, propyl alcohol, and butyl alcohol, ketone-based solvents such as acetone and methyl ethyl ketone, glycol ether-based solvents such as ethylene glycol ethyl ether, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, dipropylene glycol methyl ether, propylene glycol ethyl ether, and propylene glycol methyl ether acetate, lactone-based solvents such as γ-butyrolactone, δ-valerolactone, and ε-caprolactone, amide-based solvents such as dimethylacetamide and dimethylformamide, and aromatic solvents such as toluene and xylene, which may be used alone or in combination of two or more. Among these, organic solvents having a boiling point of 170° C. or higher are preferred from the viewpoint of avoiding bubble formation due to sudden volatilization when curing the underfill material.
[0049] The amount of organic solvent added is not particularly limited as long as it does not form bubbles when the underfill material is cured, but it is preferably 10 mass % or less, and more preferably 5 mass % or less, of the total underfill material.
[0050] (Other additives) The underfill material of the present disclosure may contain other additives, such as dyes, colorants such as carbon black, diluents, leveling agents, and defoamers, as needed.
[0051] (Physical properties of underfill material) The viscosity of the underfill material is not particularly limited. From the viewpoint of high fluidity, the viscosity is preferably 1 Pa·s to 100 Pa·s, and more preferably 3 Pa·s to 70 Pa·s at 25°C. The viscosity of the underfill material is measured at 25°C using an E-type viscometer (cone angle 3°, rotation speed 10 rpm).
[0052] Furthermore, as an index of ease of filling narrow gaps of several tens to several hundreds of microns with underfill material at around 100°C to 120°C, the viscosity at 110°C is preferably 0.3 Pa·s or less, and more preferably 0.2 Pa·s or less. The viscosity of the underfill material at 110°C is measured using a rheometer AR2000 (manufactured by TA Instruments, aluminum cone 40 mm, shear rate 32.5 / sec).
[0053] The underfill material preferably has a thixotropy index [(viscosity at 1.5 rpm) / (viscosity at 10 rpm)], which is the ratio of the viscosity at a rotation speed of 1.5 rpm to the viscosity at a rotation speed of 10 rpm measured at 25° C. using an E-type viscometer, of 0.3 to 1.1, more preferably 0.4 to 1.0. When the thixotropy index is within the above range, the fillet formability is further improved. The viscosity and thixotropy index of the underfill material can be set within a desired range by appropriately selecting the composition of the epoxy resin, the content of the inorganic filler, etc.
[0054] (Physical properties of the cured product) In this disclosure, the cured underfill material used for measuring the glass transition temperature and thermal expansion coefficient by TMA and the storage modulus by DMA was obtained by heating the underfill material at 150°C for 2 hours.
[0055] When the underfill material is cured, the thermal expansion coefficient below the glass transition temperature measured by TMA (thermomechanical analysis) is 30 ppm / °C or less, preferably 28 ppm / °C or less, and more preferably 26 ppm / °C or less. If the thermal expansion coefficient below the glass transition temperature is 30 ppm / °C or less, the occurrence of bump cracks during reflow is suppressed and temperature cycle resistance characteristics are improved. The thermal expansion coefficient below the glass transition temperature measured by TMA (thermomechanical analysis) may be 15 ppm / °C or more. The storage modulus of the underfill material at 240°C measured by DMA (dynamic viscoelasticity measurement) when cured is 0.10 GPa or less, preferably 0.09 GPa or less, more preferably 0.08 GPa or less, and even more preferably 0.07 GPa or less. If the storage modulus at 240°C is 0.10 GPa or less, the occurrence of cracks in the solder resist during reflow is suppressed, and the temperature cycle resistance characteristic is improved. The storage modulus at 240°C measured by DMA (dynamic viscoelasticity measurement) may be 0.02 GPa or more. The glass transition temperature of the cured underfill material measured by TMA (thermo-mechanical analysis) is preferably 60°C to 150°C, more preferably 70°C to 140°C, and even more preferably 70°C to 130°C. If the glass transition temperature is 60°C or higher, the bumps tend to be more protected at high temperatures and less likely to break. If the glass transition temperature is 150°C or lower, warping at room temperature (25°C) tends to be less likely to occur. The storage modulus of the underfill material at 25°C, measured by DMA (dynamic mechanical analysis), when cured, is preferably 5 GPa to 10 GPa, more preferably 5.5 GPa to 9.5 GPa, and even more preferably 6 GPa to 9 GPa. If the storage modulus at 25°C is 5 GPa or more, the bumps tend to be more protected at high temperatures and less likely to break. If the modulus at 25°C is 10 GPa or less, warping at room temperature (25°C) tends to be less likely to occur.
[0056] The TMA can be measured, for example, using a TA4000SA manufactured by TA Instruments Co., Ltd. The measurement conditions can be a temperature rise rate of 5° C. / min. DMA can be measured, for example, using Q800 manufactured by TA Instruments Co., Ltd. The measurement conditions can be a frequency of 1 Hz and a temperature rise rate of 3° C. / min.
[0057] (Manufacturing of underfill materials) The underfill material of the present disclosure can be produced by any method that can uniformly disperse and mix the above various components. In a typical method, the components are weighed out in a predetermined blend ratio, mixed and kneaded using a mixing machine, mixing roll, planetary mixer, etc., and degassed as necessary to obtain the underfill material.
[0058] <Electronic component equipment> The electronic component device of the present disclosure includes a wiring board, an electronic component disposed on the wiring board and electrically connected to the wiring board via a connection portion, and a cured product of the underfill material of the present disclosure that seals at least the connection portion between the wiring board and the electronic component. The electronic component device of the present disclosure can be obtained by sealing at least the connection portion between the electronic component and the wiring board with the underfill material of the present disclosure. By sealing the electronic component with the underfill material, the electronic component device of the present disclosure has excellent reliability, such as temperature cycle resistance. The connection portion in the electronic component device preferably contains copper in order to ensure high electrical conductivity.
[0059] Examples of electronic component devices include electronic component devices obtained by mounting electronic components such as active elements such as semiconductor chips, transistors, diodes, and thyristors, and passive elements such as capacitors, resistors, resistor arrays, coils, and switches on a wiring substrate such as a lead frame, a pre-wired tape carrier, a rigid wiring board, a flexible wiring board, glass, or a silicon wafer, and sealing necessary parts with the underfill material of the present disclosure. In particular, a semiconductor device in which a semiconductor element is flip-chip bonded to wiring formed on a rigid wiring board, a flexible wiring board, or glass by bump connection is preferably sealed with the underfill material of the present disclosure. Specific examples of flip-chip bonded semiconductor devices include semiconductor devices such as flip-chip BGA (Ball Grid Array), LGA (Land Grid Array), and COF (Chip On Film).
[0060] The underfill material of the present disclosure is suitable as an underfill material for flip chips with excellent reliability. The field of flip chips in which the underfill material of the present disclosure is particularly suitable is the field of flip chip semiconductor components in which the bumps connecting the wiring board and the semiconductor element are made of lead-free solder such as Sn-Ag-Cu solder, rather than the conventional lead-containing solder. The connection part in the electronic component device may be a lead-free structure. The underfill material of the present disclosure can maintain good reliability even for flip chips bump-connected using lead-free solder, which is physically brittle compared to conventional lead solder. Furthermore, the underfill material of the present disclosure is suitable for semiconductor elements having a long side of 2 mm or more, and shows good fluidity and filling properties even for flip chip connections in which the distance between the bump connection surface of the wiring board and the semiconductor element constituting the electronic component device is 200 μm or less, and can provide a semiconductor device with excellent reliability such as moisture resistance and thermal shock resistance. In addition, with the increase in speed of semiconductor elements in recent years, low-dielectric constant interlayer insulating films may be formed on the semiconductor elements, and these low-dielectric constant insulators have weak mechanical strength and are prone to failure due to external stress. This tendency becomes more pronounced as the semiconductor element becomes larger, and there is a demand for reducing stress by the underfill material. The underfill material of the present disclosure can provide excellent reliability even for flip chip semiconductor devices mounted with semiconductor elements having a long side of 2 mm or more and an interlayer insulating film with a dielectric constant of 3.0 or less.
[0061] <Electronic component device manufacturing method> Methods for sealing electronic component devices using the underfill material of the present disclosure include a dispensing method, a casting method, a printing method, and the like. The underfill material of the present disclosure is suitable for use in the manufacture of electronic component devices in which an electronic component and a wiring board are electrically connected via a connection portion. For example, a first method for manufacturing an electronic component device according to the present disclosure includes a supplying step of supplying the underfill material according to the present disclosure to at least one of a surface of an electronic component facing a wiring board and a surface of a wiring board facing the electronic component, and a connecting step of connecting the electronic component and the wiring board via a connecting portion and curing the underfill material. In the first method for manufacturing an electronic component device, the underfill material according to the present disclosure can be used as an underfill material for a pre-supply system. The second method for manufacturing an electronic component device according to the present disclosure includes a filling step of filling the gap between the connected electronic component and the wiring board with the underfill material according to the present disclosure, and a curing step of curing the underfill material. In the second method for manufacturing an electronic component device, the underfill material according to the present disclosure can be used as a post-supply underfill material. EXAMPLES
[0062] Next, the present invention will be described more specifically based on examples, but the present invention is not limited to these examples.
[0063] The methods for evaluating the characteristics and reliability of the underfill material in the examples are summarized below.
[0064] The semiconductor element used for the evaluation was 25 mm long, 25 mm wide, and 725 μm thick, with bumps of 30 μm high copper + 15 μm high lead-free solder, a bump pitch of 150 μm, and 25,921 bumps in total. The wiring board used was E-705 (trade name, manufactured by Hitachi Chemical Co., Ltd.) with a length of 55 mm, width of 55 mm, and thickness of 1 mm. The solder resist was AUS703 (trade name, manufactured by Taiyo Ink Mfg. Co., Ltd.) with a thickness of 15 μm.
[0065] The electronic component device was fabricated by filling the gap between the semiconductor element and the wiring board, which were electrically connected via bumps, with underfill material using a dispense method, and curing it for 2 hours at 150°C. The curing conditions for each test piece were also the same.
[0066] (1) Glass transition temperature The cured underfill material was subjected to TMA (thermo-mechanical analysis) using a TA4000SA made by TA Instruments, and the intersection of the tangent lines before and after the inflection point of the obtained chart was taken as the glass transition temperature. The heating rate was 5° C. / min. (2) Thermal expansion coefficient The cured underfill material was subjected to TMA (thermo-mechanical analysis) using a TA4000SA made by TA Instruments, and the thermal expansion coefficient was determined by dividing the slope connecting the two points of 10°C and 30°C on the obtained chart by the length of the test piece. The heating rate was 5°C / min. (3) Storage modulus The cured underfill material was subjected to DMA (dynamic viscoelasticity measurement) using a TA Instruments Q800, and the storage modulus at 240° C. was obtained from the measurement results. The frequency was 1 Hz, and the heating rate was 3° C. / min. (4) Solder resist cracks Electronic component devices that had been subjected to a thermal history of at least one minute at a temperature of 240°C or higher three times were cut so that the bumps could be observed, and the presence or absence of solder resist cracks was observed using a scanning electron microscope (device name SU1510) manufactured by Hitachi High-Technologies Corporation. (5) Temperature cycle After a temperature cycle test of -55°C / 10 minutes and 125°C / 10 minutes was performed, the electronic component devices were observed using an ultrasonic microscope (IS-350) manufactured by Insight Corporation to check for peeling of the cured underfill material. In Table 2, ">1000" indicates that no peeling occurred at the end of 1000 cycles. Furthermore, "<500" indicates that peeling occurred at the end of 500 cycles.
[0067] (Examples 1 to 5 and Comparative Examples 1 and 2) As the epoxy resins of component (A), liquid diepoxy resin (epoxy resin 1) obtained by epoxidizing bisphenol F and having an epoxy equivalent of 160 g / eq, trifunctional liquid epoxy resin (epoxy resin 2) obtained by epoxidizing aminophenol and having an epoxy equivalent of 95 g / eq, diepoxy resin (epoxy resin 3) obtained by epoxidizing naphthalenediol and having an epoxy equivalent of 140 g / eq, and liquid diepoxy resin (epoxy resin 4) obtained by epoxidizing alkyldiol and having an epoxy equivalent of 128 g / eq were used. As the curing agent for component (B), 3,5-diethyltoluene-2,4-diamine with an active hydrogen equivalent of 45 g / eq was used. As the inorganic filler of component (C), spherical silica having an average particle size of 1 μm was used. As a flexibilizing agent for component (D), spherical silicone particles having an average particle size of 2 μm, in which the surface of dimethyl-type solid silicone rubber particles was modified with epoxy groups, were used. As the surfactant of component (E), a silicone-modified epoxy resin, which is a reaction product of an organosiloxane having a weight-average molecular weight of 1000 and a functional group reactive with an epoxy group, and a bisphenol F type epoxy resin, was used. As the ion trapping agent of component (F), a bismuth-based ion trapping agent (product name IXE-500, manufactured by Toagosei Co., Ltd.) was used. 2-Phenyl-4-methyl-5-hydroxymethylimidazole was used as the curing accelerator for component (G). As the coupling agent for component (H), γ-glycidoxypropyltrimethoxysilane was used. As the antioxidant for component (I), 3,9-bis[2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane was used. γ-Butyrolactone was used as the organic solvent for component (J). Carbon black (product name MA-100, manufactured by Mitsubishi Chemical Corporation) was used as a colorant. The above components were mixed in the compositions shown in Table 1 below, and kneaded and dispersed using a triple roll and a pressure-reducing mill to prepare the underfill materials of Examples 1 to 5 and Comparative Examples 1 and 2.
[0068] [Table 1]
[0069] The amount of each component in Table 1 is expressed in parts by mass. In addition, the "equivalent ratio" in Table 1 represents "equivalent number of curing agent (equivalent number of active hydrogen) / equivalent number of epoxy resin (equivalent number of epoxy group)."
[0070] The various evaluation results are summarized in Table 2 below.
[0071] [Table 2]
[0072] In Examples 1 to 5, the glass transition temperature measured by TMA was 60°C to 150°C, the thermal expansion coefficient was 30 ppm / °C or less, the storage modulus measured by DMA was 5 GPa to 10 GPa at 25°C, and the storage modulus measured by DMA was 0.10 GPa or less at 240°C. Comparative Example 1, which had a storage modulus of 0.40 GPa at 240°C, had excellent temperature cycle resistance, but cracks occurred in the solder resist. This is thought to be because when the storage modulus at high temperatures is high, the hardened underfill material cannot absorb the expansion of the solder at the reflow temperature, and stress is applied to the solder resist. In Comparative Example 2, which had a thermal expansion coefficient of 36 ppm / °C, no cracks appeared in the solder resist, but peeling was observed after 500 temperature cycles. This is thought to be because a large thermal expansion coefficient results in large expansion and contraction of the cured underfill material due to temperature cycles, causing peeling between the chip interface and the underfill material during contraction.
Claims
1. (A) an epoxy resin, (B) a curing agent, and (C) an inorganic filler; An underfill material that, when cured, has a thermal expansion coefficient below the glass transition temperature of 30 ppm / °C or less as measured by TMA (thermomechanical analysis), and a storage modulus at 240°C of 0.10 GPa or less as measured by DMA (dynamic mechanical analysis).
2. 2. The underfill material according to claim 1, wherein the cured product has a glass transition temperature of 60° C. to 150° C. as measured by TMA (thermomechanical analysis).
3. 3. The underfill material according to claim 1, wherein the cured product has a storage modulus of 5 GPa to 10 GPa at 25° C. as measured by DMA (dynamic mechanical analysis).
4. The underfill material according to any one of claims 1 to 3, further comprising (D) a flexibilizing agent.
5. The underfill material according to any one of claims 1 to 4, further comprising (E) a surfactant.
6. The underfill material according to any one of claims 1 to 5, further comprising (F) an ion trapping agent.
7. The underfill material according to any one of claims 1 to 6, further comprising (G) a curing accelerator.
8. The underfill material according to any one of claims 1 to 7, further comprising (H) a coupling agent.
9. The underfill material according to any one of claims 1 to 8, further comprising (I) an antioxidant.
10. The underfill material according to any one of claims 1 to 9, further comprising (J) an organic solvent, the content of the organic solvent being 10 mass % or less.
11. The underfill material according to any one of claims 1 to 10, wherein the (B) curing agent is an aromatic amine compound.
12. A wiring board; an electronic component disposed on the wiring board and electrically connected to the wiring board via a connection portion; A cured product of the underfill material according to any one of claims 1 to 11 that seals at least a connection portion between the wiring board and the electronic component; An electronic component device comprising:
13. The electronic component device of claim 12 , wherein the connection portion is lead-free.
14. The electronic component device according to claim 12 or 13, wherein the connection portion contains copper.
15. A method for manufacturing an electronic component device in which an electronic component and a wiring board are electrically connected via a connection portion, comprising the steps of: a supplying step of supplying the underfill material according to any one of claims 1 to 11 to at least one of a surface of the electronic component facing the wiring board and a surface of the wiring board facing the electronic component; a connecting step of connecting the electronic component and the wiring board via the connecting portion and curing the underfill material.
16. A method for manufacturing an electronic component device in which an electronic component and a wiring board are electrically connected via a connection portion, comprising the steps of: a filling step of filling a gap between the connected electronic component and the wiring board with the underfill material according to any one of claims 1 to 11; and a curing step of curing the underfill material.
Citation Information
Patent Citations
Liquid epoxy resin composition and electronic component device
JP2004210901A
Underfill agent and semiconductor device using the same
JP2010254955A
Semiconductor device
JP2010262973A
Highly flexible resin and curable resin composition
JP2010285627A
Epoxy resin composition, cured article and electronic component
JP2014034680A