Resin film for terminal and selection method of the same, and power storage device

A terminal resin film with tailored tan δ profiles and optional hydrogen sulfide adsorbing substance addresses the heat resistance issue in all-solid-state batteries, ensuring robust sealing and insulation across varying temperatures and environments.

JP2024138137AActive Publication Date: 2024-10-07TOPPAN HOLDINGS INC
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024122261
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-07
Estimated Expiration
2039-12-27

AI Technical Summary

Technical Problem

The sealing of all-solid-state batteries is challenging due to the insufficient heat resistance of conventional resin films for terminals, leading to potential quality issues.

Method used

A terminal resin film with a single-layer or multi-layer structure, featuring specific loss tangent tan δ profiles with secondary dispersion peak γ between -130°C to -50°C and main dispersion peak α between 30°C to 130°C, optionally containing a hydrogen sulfide adsorbing substance, to ensure high seal strength at both high and room temperatures.

Benefits of technology

The resin film achieves both high seal strength at elevated temperatures and initial seal strength at room temperature, maintaining adhesion and insulation properties even after exposure to hydrogen sulfide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138137000001_ABST
    Figure 2024138137000001_ABST
Patent Text Reader

Abstract

To provide a resin film for a terminal which can achieve both seal strength under high temperature and initial seal strength at a sufficiently high level.SOLUTION: A resin film for a terminal is arranged so as to cover an outer peripheral surface of a part of a terminal electrically connected to a power storage device body in a power storage device including the power storage device body, and the terminal, and has a single layer structure or a multilayer structure, and includes a resin layer which has at least one sub-dispersion peak γ within a range of -130°C to -74°C of a profile of a loss tangent tanδ obtained by dynamic viscoelasticity measurement under a condition of 1.0 Hz, and contains a polyester-based resin or an amide-modified polyolefin-based resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a terminal resin film arranged to cover a part of an outer peripheral surface of a terminal in an electricity storage device including an electricity storage device main body and a terminal electrically connected to the electricity storage device main body, and a selection method thereof.The present disclosure also relates to an electricity storage device using the terminal resin film. [Background technology]

[0002] Known examples of power storage devices include secondary batteries such as lithium ion batteries, nickel metal hydride batteries, and lead storage batteries, as well as electrochemical capacitors such as electric double layer capacitors. Due to the miniaturization of portable devices or the limitations of installation space, there is a demand for further miniaturization of power storage devices, and lithium ion batteries with high energy density have attracted attention. Metal cans have traditionally been used as exterior materials for lithium ion batteries, but multilayer films that are lightweight, have high heat dissipation properties, and can be produced at low cost have come to be used.

[0003] A lithium ion battery using the above multilayer film as an exterior material is called a laminated lithium ion battery. The exterior material covers the battery contents (positive electrode, separator, negative electrode, electrolyte, etc.) and prevents moisture from penetrating into the battery. A laminated lithium ion battery is manufactured, for example, by forming a recess in a part of the exterior material by cold forming, accommodating the battery contents in the recess, folding back the remaining part of the exterior material, and heat sealing the edges (see, for example, Patent Document 1).

[0004] Laminated lithium-ion batteries include a current extraction terminal (sometimes called a "tab lead"). In order to improve the adhesion between the current extraction terminal and the exterior material, a resin film for terminals (sometimes called a "tab sealant") may be disposed so as to cover part of the outer periphery of the current extraction terminal (see, for example, Patent Documents 2 to 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-101765 A [Patent Document 2] JP 2008-4316 A [Patent Document 3] JP 2010-218766 A [Patent Document 4] JP 2009-259739 A Summary of the Invention [Problem to be solved by the invention]

[0006] Meanwhile, research and development is being conducted on a power storage device called an all-solid-state battery as a next-generation battery of lithium-ion batteries. An all-solid-state battery is characterized by using a solid electrolyte as the electrolyte, rather than an organic electrolyte. While a lithium-ion battery cannot be used at temperatures higher than the boiling point of the electrolyte (about 80°C), an all-solid-state battery can be used at temperatures exceeding 100°C, and the conductivity of lithium ions can be increased by operating it under high temperature conditions (for example, 100 to 150°C).

[0007] However, when using such a laminated body as an exterior material to manufacture a laminate-type all-solid-state battery, the heat resistance of the terminal resin film may be insufficient, which may result in insufficient sealing of the package of the all-solid-state battery.

[0008] The present disclosure provides a resin film for a terminal that can achieve sufficiently high levels of both seal strength at high temperatures and initial seal strength, and a method for selecting the same. The present disclosure also provides an electricity storage device using the resin film for a terminal. [Means for solving the problem]

[0009] A resin film for a terminal according to one aspect of the present disclosure is disposed so as to cover a part of the outer circumferential surface of a terminal in an electricity storage device including a main body of the electricity storage device and a terminal electrically connected to the main body of the electricity storage device. The resin film for a terminal has a single-layer structure or a multilayer structure, and includes a resin layer having at least one minor dispersion peak γ in the range of −130° C. to −50° C. in a profile of loss tangent tan δ obtained by dynamic viscoelasticity measurement under a condition of 1.0 Hz.

[0010] The sub-dispersion peak γ is an index of molecular motion of the resin material constituting the resin layer, specifically, a parameter reflecting the local twisting motion of the main chain in the crystalline and amorphous parts of the resin material and the thermal motion of the entire side chain. According to the study by the inventors, a resin layer that satisfies the above requirements for the sub-dispersion peak γ contains a resin material that starts molecular motion at a relatively high temperature, and can exhibit excellent seal strength at high temperatures. Note that the lower the temperature at which the sub-dispersion peak γ appears, the more flexible the resin layer is, and the higher the temperature at which the sub-dispersion peak γ appears, the more heat-resistant the resin layer is.

[0011] The resin layer preferably has at least one main dispersion peak α in the range of 30°C to 130°C of the tan δ profile. The main dispersion peak α is a parameter that reflects the micro-Brownian motion of molecular chains of the amorphous part in the vicinity of the glass transition temperature (Tg) of the resin material contained in the resin layer. According to the study by the present inventors, a resin layer that satisfies the above requirements regarding the main dispersion peak α contains a resin material that starts molecular motion at a relatively low temperature (for example, room temperature) and is excellent in flexibility. Therefore, the resin layer can exhibit even better seal strength (initial seal strength) in a room temperature environment. Note that the lower the temperature at which the main dispersion peak α appears, the more flexible the resin layer is, and the higher the temperature at which the main dispersion peak α appears, the more heat-resistant the resin layer is.

[0012] The resin layer preferably contains a plasticizer. By adjusting the content of the plasticizer in the resin layer, the temperature at which the minor dispersion peak γ and the major dispersion peak α appear can be controlled. For example, by increasing the content of the plasticizer, the minor dispersion peak γ and the major dispersion peak α can be shifted to a lower temperature side.

[0013] The terminal resin film preferably contains a hydrogen sulfide adsorbent. The hydrogen sulfide adsorbent may be contained in the resin layer, or in the case where the terminal resin film has a multi-layer structure, it may be contained in another layer. In the all-solid-state battery, for example, a sulfide-based electrolyte, an oxide-based electrolyte, or an organic polymer electrolyte is used as the electrolyte. When a sulfide-based electrolyte is used, hydrogen sulfide is generated when moisture is mixed into the cell, and there is a concern that the adhesion between the outer surface of the terminal and the terminal resin film may decrease. When the terminal resin film contains a hydrogen sulfide adsorbent, it is possible to maintain excellent seal strength at room temperature and high temperature even after exposure to hydrogen sulfide.

[0014] One aspect of the present disclosure relates to a method for selecting a terminal resin film to be arranged so as to cover a part of an outer circumferential surface of a terminal in an energy storage device including an energy storage device main body and a terminal electrically connected to the energy storage device main body, the selection method including the following steps. (A) A process of performing dynamic viscoelasticity measurement on the resin film for terminals to be evaluated at 1.0 Hz (B) A step of determining whether or not at least one sub-dispersion peak γ exists in the range of −130° C. to −50° C. in the profile of tan δ obtained by the dynamic viscoelasticity measurement. Effect of the Invention

[0015] According to the present disclosure, there are provided a resin film for a terminal capable of achieving a sufficiently high level of both seal strength at high temperatures and initial seal strength, and a method for selecting the same. Also, according to the present disclosure, there is provided an electricity storage device using the resin film for a terminal. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a perspective view showing an example of an all-solid-state battery. [Diagram 2] FIG. 2 is a cross-sectional view that typically illustrates one example of an exterior material for an electricity storage device. [Diagram 3]3(a) to 3(c) are cross-sectional views that typically show the configuration of a sealant layer provided in an exterior packaging material for an electricity storage device. [Figure 4] FIG. 4 is a cross-sectional view taken along line IV-IV shown in FIG. 1, and is a cross-sectional view that typically illustrates the configuration of a tab (a resin film for terminal and a metal terminal) of an all-solid-state battery. [Diagram 5] 5(a) to 5(c) are cross-sectional views that typically show examples of the configuration of the resin film for terminal. [Figure 6] FIG. 2 is a plan view illustrating the evaluation samples prepared in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present disclosure will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. In addition, the dimensional ratios of the drawings are not limited to the illustrated ratios.

[0018] <Electricity storage device> Fig. 1 is a perspective view showing a schematic configuration of a power storage device according to the present embodiment. In Fig. 1, an all-solid-state battery is illustrated as an example of a power storage device 100, and the following description will be given. Note that the power storage device having the configuration shown in Fig. 1 may be called a battery pack or a battery cell.

[0019] The energy storage device 100 is an all-solid-state battery, and includes an energy storage device body 50, an exterior material 10, a pair of metal terminals 30, and a terminal resin film 40 (tab sealant). The energy storage device body 50 is a battery body that performs charging and discharging. The exterior material 10 covers the surface of the energy storage device body 50, and is disposed so as to be in contact with a part of the terminal resin film 40.

[0020] [Exterior material] 2 is a cross-sectional view showing an example of a cut surface of the exterior material 10. The exterior material 10 has a multilayer structure including, from the outside to the inside (the electricity storage device main body 50 side), a base material layer 11, a first adhesive layer 12, a barrier layer 13, a corrosion prevention treatment layer 14, a second adhesive layer 17, and a sealant layer 16, in this order.

[0021] (Sealant layer) The sealant layer 16 is a layer that imparts heat-sealing sealability to the exterior material 10, and is a layer that is placed on the inside and heat-sealed (thermally fused) when the electricity storage device is assembled.

[0022] For example, thermoplastic resins such as polyolefin, polyamide, polyester, polycarbonate, polyphenylene ether, polyacetal, polystyrene, polyvinyl chloride, and polyvinyl acetate can be used as the sealant layer 16, and polyolefin, polyamide, and polyester are preferred from the viewpoints of heat resistance and sealing suitability. When directly laminating to the barrier layer without using an adhesive, it is preferred to use a material in which at least one layer in contact with the barrier layer is modified with an acid, glycidyl, or the like.

[0023] Examples of polyolefin resins include low-, medium- and high-density polyethylenes, ethylene-α-olefin copolymers, polypropylene, and propylene-α-olefin copolymers. When the polyolefin resin is a copolymer, it may be a block copolymer or a random copolymer.

[0024] Examples of polyester resins include polyethylene terephthalate (PET) and polybutylene terephthalate (PBT). These polyester resins may be used alone or in combination of two or more. In addition, copolymers of any acid and glycol may be used.

[0025] In order to impart sealing properties, heat resistance, and other functionalities, for example, antioxidants, slip agents, flame retardants, antiblocking agents, light stabilizers, dehydrating agents, tackifiers, crystal nucleating agents, plasticizers, etc. may be added.

[0026] The peak melting temperature of the sealant layer varies depending on the application, but in the case of an exterior material for an all-solid-state battery, it is preferably 160 to 280° C. because this improves heat resistance.

[0027] The sealant layer 16 preferably has at least one sub-dispersion peak γ in the range of −130° C. to −50° C. in the profile of the loss tangent tanδ obtained by dynamic viscoelasticity measurement under the condition of 1.0 Hz. When the sealant layer 16 satisfies this condition, the exterior material 10 can achieve both the seal strength at high temperatures and the initial seal strength (seal strength at room temperature) at a sufficiently high level. The temperature range in which the sub-dispersion peak γ exists is more preferably −120° C. to −60° C., and even more preferably −110° C. to −70° C., from the viewpoint of the seal strength at room temperature and at high temperatures. If the temperature in which the sub-dispersion peak γ exists is less than −130° C., the heat resistance of the sealant layer 16 may be poor, and the seal strength at high temperatures may be insufficient. On the other hand, if the temperature in which the sub-dispersion peak γ exists exceeds −50° C., the flexibility of the sealant layer 16 may be poor, and the seal strength at room temperature may be insufficient.

[0028] The above-mentioned tan δ can be calculated as the loss tangent tan δ from the loss modulus E″ and the storage modulus E′, for example, by immersing the exterior material in an aqueous sodium hydroxide solution to dissolve the barrier layer (metal foil) and extracting a film consisting of only the sealant layer, and measuring the extracted film under the following conditions using a dynamic viscoelasticity device (manufactured by SII, product name: DMS6100) in accordance with a method in accordance with JIS K7244-4. Peeling mode: Pulling Heating rate: 2℃ / min Temperature range: -150~150℃ Frequency: 1.0Hz

[0029] The sealant layer 16 preferably has at least one main dispersion peak α in the range of 30°C to 130°C of the above tan δ profile. When the sealant layer 16 satisfies this condition, the exterior material 10 exhibits even better initial seal strength (seal strength at room temperature). The temperature range in which the main dispersion peak α exists is preferably 40°C to 110°C, more preferably 50°C to 100°C, from the viewpoint of seal strength at room temperature. If the temperature in which the main dispersion peak α exists is less than 30°C, the heat resistance of the sealant layer 16 tends to be poor and the seal strength at high temperatures tends to be insufficient. On the other hand, if the temperature in which the main dispersion peak α exists exceeds 130°C, the flexibility of the sealant layer 16 tends to be poor and the seal strength at room temperature tends to be insufficient.

[0030] The temperature at which the minor dispersion peak γ and the major dispersion peak α of the sealant layer 16 appear can be controlled, for example, by the structure of the base resin material contained in the sealant layer 16, the stretching ratio of the sealant layer 16, or the amount of additives (e.g., plasticizers) blended. The sealant layer 16 contains additives as necessary. Examples of additives include plasticizers, antioxidants, slip agents, flame retardants, AB agents, light stabilizers, dehydrating agents, and tackifiers.

[0031] Examples of the base resin material contained in the sealant layer 16 include polyester-based, polyolefin-based, and polyamide-based resins.

[0032] The polyester resin can be obtained by copolymerizing an acid component and a glycol component. Examples of the acid component include phthalic acid, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, cyclohexanedicarboxylic acid, adipic acid, and sebacic acid. Examples of the glycol component include ethylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, diethylene glycol, polytetramethylene glycol, cyclohexanedimethanol, and propanediol. According to the study by the present inventors, the temperature at which the secondary dispersion peak γ exists in the general PET (copolymer of terephthalic acid and ethylene glycol) is outside the range of −130° C. to −50° C., and the seal strength at room temperature is insufficient. When a plasticizer is not blended in the sealant layer 16, it is preferable that the sealant layer 16 contains a polyester resin in which one acid component and two or more glycol components are copolymerized.

[0033] Examples of polyolefin resins include polyethylene and polypropylene resins. Generally used polyolefin resins have poor heat resistance, so it is preferable to use polyethylene or polypropylene modified with amide or the like.

[0034] Examples of polyamide resins include nylon 6 and nylon 6,6.

[0035] From the viewpoint of adjusting the temperature at which the minor dispersion peak γ and the major dispersion peak α of the sealant layer 16 appear, the sealant layer 16 preferably contains a plasticizer. As the plasticizer, for example, an ester-based compound can be used. Specific examples include glycol diesters, adipic acid esters, phthalic acid esters, diacetyl monoacyl glycerol derivatives, and esters having an ether skeleton. Although it depends on the base resin material of the sealant layer 16, the content of the plasticizer in the sealant layer 16 is preferably 30 mass% or less based on the mass of the sealant layer 16. When an excessive amount of plasticizer is blended in the sealant layer 16, the temperature at which the minor dispersion peak γ and the major dispersion peak α appear is excessively lowered, and the cohesive force tends to decrease.

[0036] The sealant layer 16 may have a single layer structure or a multi-layer structure of two or more layers (see Figs. 3(a) to 3(c)). When the sealant layer has a single layer structure, its thickness is preferably 10 to 300 µm, and more preferably 20 to 100 µm. When the thickness of the sealant layer 16 is 10 µm or more, it is easy to ensure sealing properties and insulation properties, while when the thickness is 300 µm or less, it is possible to ensure the cell volume.

[0037] FIG. 3(b) is a cross-sectional view that shows a two-layer structure of the sealant layer 16. The sealant layer 16 shown in the figure has a first resin layer 16a and a second resin layer 16b formed on the inner surface of the first resin layer 16a. The first resin layer 16a may be made of a different material from the second resin layer 16b, for example, and may have a different thickness from the second resin layer 16b. The thicknesses of the first resin layer 16a and the second resin layer 16b are, for example, 5 to 300 μm, and may be 20 to 200 μm. As shown in FIG. 3(c), the sealant layer 16 may have a three-layer structure and further include a third resin layer 16c.

[0038] When the electrolyte of the all-solid-state battery is a sulfide-based electrolyte, the sealant layer 16 preferably contains a hydrogen sulfide adsorbent. By containing the hydrogen sulfide adsorbent, the sealant layer 16 can maintain excellent seal strength at room temperature and at high temperatures even after exposure to hydrogen sulfide. As the hydrogen sulfide adsorbent, a material having the ability to absorb or adsorb hydrogen sulfide can be used. Specific examples thereof include zinc oxide, amorphous metal silicate, hydroxide of zirconium and lanthanoid elements, tetravalent metal phosphate, potassium permanganate, sodium permanganate, aluminum oxide, iron hydroxide, silver sulfate, silver acetate, isocyanate compounds, aluminum silicate, potassium aluminum sulfate, zeolite, activated carbon, amine compounds, and ionomers.

[0039] The content of the hydrogen sulfide adsorption substance in the sealant layer 16 is preferably 1 to 50 mass %, more preferably 2 to 25 mass %, and even more preferably 5 to 15 mass %, based on the mass of the sealant layer 16. When the content of the hydrogen sulfide adsorption substance in the sealant layer 16 is 1 mass % or more, the hydrogen sulfide adsorption effect is exhibited, while when the content is 50 mass % or less, the sealant layer 16 can achieve both adhesion and sealant suitability. When the sealant layer 16 has a multi-layer structure, all or a part of the layers may contain the hydrogen sulfide adsorption substance. Note that a layer other than the sealant layer 16 (for example, the second adhesive layer 17) in the exterior packaging material 10 may contain a sulfide-based electrolyte, but from the viewpoint of the content of the hydrogen sulfide adsorption substance, it is preferable that at least the sealant layer 16 contains the hydrogen sulfide adsorption substance.

[0040] (base material layer) The base layer 11 provides heat resistance in the sealing process when manufacturing the electricity storage device and plays a role in suppressing the occurrence of pinholes that may occur during molding and distribution. In particular, in the case of an exterior material for a large-scale electricity storage device, the base layer 11 can also provide scratch resistance, chemical resistance, insulation, and the like.

[0041] The base layer 11 is preferably a layer made of a resin film formed of an insulating resin. Examples of the resin film include stretched or unstretched films such as polyester film, polyamide film, polypropylene film, and polyphenylene sulfide film. The base layer 11 may be a single layer film made of any of these resin films, or a laminate film made of two or more of these resin films.

[0042] Among these, polyester film and polyamide film are preferable as the base layer 11 because of their excellent moldability, and polyamide film is more preferable. These films are preferably biaxially stretched films. Examples of polyester resins constituting the polyester film include polyethylene terephthalate. Examples of polyamide resins constituting the polyamide film include nylon 6, nylon 6,6, a copolymer of nylon 6 and nylon 6,6, nylon 6,10, polymetaxylylene adipamide (MXD6), nylon 11, nylon 12, etc. Among these, nylon 6 (ONy) is preferable because of its excellent heat resistance, puncture strength, and impact strength.

[0043] Examples of the stretching method for the biaxially stretched film include a sequential biaxial stretching method, a tubular biaxial stretching method, a simultaneous biaxial stretching method, etc. From the viewpoint of obtaining better deep drawing formability, the biaxially stretched film is preferably one stretched by a tubular biaxial stretching method.

[0044] The thickness of the substrate layer 11 is preferably 6 to 40 μm, and more preferably 10 to 30 μm. When the thickness of the substrate layer 11 is 6 μm or more, the pinhole resistance and insulating properties of the packaging material 10 tend to be improved. When the thickness of the substrate layer 11 exceeds 40 μm, the total thickness of the packaging material 10 tends to be large.

[0045] (First adhesive layer) The first adhesive layer 12 is a layer that bonds the base layer 11 and the barrier layer 13. Specific examples of materials constituting the first adhesive layer 12 include polyurethane resins in which a bifunctional or higher isocyanate compound is reacted with a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol. The above-mentioned various polyols can be used alone or in combination of two or more types depending on the functions and performance required for the exterior material. In addition, the above-mentioned polyurethane resins may be mixed with various other additives and stabilizers depending on the performance required for the adhesive.

[0046] The thickness of the first adhesive layer 12 is not particularly limited, but from the viewpoint of obtaining desired adhesive strength, conformability, processability, and the like, the thickness is, for example, preferably 1 to 10 μm, and more preferably 3 to 7 μm.

[0047] (Barrier layer) The barrier layer 13 has water vapor barrier properties that prevent moisture from penetrating into the inside of the electricity storage device. The barrier layer 13 also has extensibility for deep drawing. As the barrier layer 13, various metal foils such as aluminum, stainless steel, and copper, metal vapor deposition films, inorganic oxide vapor deposition films, carbon-containing inorganic oxide vapor deposition films, films provided with these vapor deposition films, and the like can be used. In terms of mass (specific gravity), moisture resistance, processability, and cost, metal foils are preferred, and aluminum foil is more preferred.

[0048] As the aluminum foil, a soft aluminum foil that has been annealed can be preferably used from the viewpoint of imparting desired ductility during molding, but it is more preferable to use an aluminum foil containing iron for the purpose of imparting further pinhole resistance and ductility during molding. The content of iron in the aluminum foil is preferably 0.1 to 9.0 mass%, more preferably 0.5 to 2.0 mass%, in 100 mass% of the aluminum foil. By having an iron content of 0.1 mass% or more, an exterior material 10 having better pinhole resistance and ductility can be obtained. By having an iron content of 9.0 mass% or less, an exterior material 10 having better flexibility can be obtained. Although untreated aluminum foil may be used, it is preferable to use an aluminum foil that has been degreased. When the aluminum foil is degreased, the degreased treatment may be performed on only one side of the aluminum foil, or on both sides.

[0049] The thickness of the barrier layer 13 is not particularly limited, but taking into consideration the barrier properties, pinhole resistance, and processability, it is preferably 9 to 200 μm, and more preferably 15 to 100 μm.

[0050] (Corrosion prevention treatment layer) The corrosion prevention treatment layer 14 is a layer provided to prevent corrosion of the barrier layer 13. The corrosion prevention treatment layer 14 is formed, for example, by degreasing treatment, hydrothermal conversion treatment, anodizing treatment, chemical conversion treatment, or a combination of these treatments.

[0051] The degreasing treatment may be acid degreasing or alkaline degreasing. The acid degreasing may be a method using an inorganic acid such as sulfuric acid, nitric acid, hydrochloric acid, or hydrofluoric acid alone or a mixture thereof. In addition, by using an acid degreasing agent obtained by dissolving a fluorine-containing compound such as monosodium ammonium difluoride in the inorganic acid as the acid degreasing, not only can the aluminum be degreased, but also a passive aluminum fluoride can be formed, which is effective in terms of hydrofluoric acid resistance, particularly when an aluminum foil is used for the barrier layer 13. The alkaline degreasing may be a method using sodium hydroxide or the like.

[0052] An example of the hydrothermal modification treatment is boehmite treatment in which an aluminum foil is immersed in boiling water containing triethanolamine. An example of the anodization treatment is alumite treatment.

[0053] The chemical conversion treatment may be of the immersion type or the coating type. Examples of the immersion type chemical conversion treatment include chromate treatment, zirconium treatment, titanium treatment, vanadium treatment, molybdenum treatment, calcium phosphate treatment, strontium hydroxide treatment, cerium treatment, ruthenium treatment, and various chemical conversion treatments consisting of a mixture of these. On the other hand, examples of the coating type chemical conversion treatment include a method in which a coating agent having corrosion prevention properties is applied onto the barrier layer 13.

[0054] When forming at least a part of the corrosion prevention layer by any of these corrosion prevention treatments, namely hydrothermal conversion treatment, anodizing treatment, and chemical conversion treatment, it is preferable to perform the above-mentioned degreasing treatment in advance. Note that, when using a degreased metal foil, such as a metal foil that has been subjected to an annealing process, as the barrier layer 13, there is no need to perform a degreasing treatment again in forming the corrosion prevention layer 14.

[0055] The coating agent used in the spray-type chemical conversion treatment preferably contains trivalent chromium. The coating agent may also contain at least one polymer selected from the group consisting of cationic polymers and anionic polymers, which will be described later.

[0056] Among the above treatments, particularly in hydrothermal conversion treatment and anodization treatment, the aluminum foil surface is dissolved by a treatment agent to form an aluminum compound (boehmite, alumite) with excellent corrosion resistance. Therefore, since a bicontinuous structure is formed from the barrier layer 13 using the aluminum foil to the corrosion prevention treatment layer 14, the above treatment is included in the definition of chemical conversion treatment. On the other hand, as described later, it is also possible to form the corrosion prevention treatment layer 14 by a pure coating method alone, which is not included in the definition of chemical conversion treatment. As an example of this method, a method using a sol of a rare earth element oxide such as cerium oxide with an average particle size of 100 nm or less can be mentioned, which has an aluminum corrosion prevention effect (inhibitor effect) and is also environmentally friendly. By using this method, it is possible to impart a corrosion prevention effect to metal foil such as aluminum foil even with a general coating method.

[0057] Examples of the rare earth oxide sol include sols using various solvents such as water-based, alcohol-based, hydrocarbon-based, ketone-based, ester-based, and ether-based solvents. Among these, water-based sols are preferred. In order to stabilize the dispersion of the rare earth oxide sol, inorganic acids such as nitric acid, hydrochloric acid, and phosphoric acid or their salts, and organic acids such as acetic acid, malic acid, ascorbic acid, and lactic acid are usually used as dispersion stabilizers. Among these dispersion stabilizers, phosphoric acid is particularly expected to (1) stabilize the dispersion of the sol, (2) improve adhesion to the barrier layer 13 by utilizing the aluminum chelating ability of phosphoric acid, and (3) improve the cohesive force of the corrosion prevention treatment layer 14 (oxide layer) by easily causing dehydration condensation of phosphoric acid even at low temperatures.

[0058] The corrosion prevention treatment layer 14 formed by the rare earth element oxide sol is an aggregate of inorganic particles, and therefore the layer itself may lose its cohesive strength even after the dry curing process. Therefore, in this case, the corrosion prevention treatment layer is preferably compounded with the following anionic polymer or cationic polymer to supplement the cohesive strength.

[0059] The corrosion prevention treatment layer is not limited to the above-mentioned layers. For example, it may be formed using a treatment agent in which phosphoric acid and a chromium compound are mixed with a resin binder (such as aminophenol), as in the case of coating-type chromate, which is a known technology. By using this treatment agent, a layer having both corrosion prevention function and adhesion can be obtained. In addition, although it is necessary to consider the stability of the coating liquid, a coating agent in which a rare earth element oxide sol and a polycationic polymer or a polyanionic polymer are previously mixed into a one-component solution can be used to obtain a layer having both corrosion prevention function and adhesion.

[0060] The mass per unit area of ​​the corrosion prevention treatment layer is 0.005 to 0.200 g / m2, whether it is a multi-layer structure or a single-layer structure. 2 is preferable, and 0.010 to 0.100 g / m 2 It is more preferable that the mass per unit area is 0.005 g / m 2 If the mass per unit area is 0.200 g / m or more, it is easy to impart a corrosion prevention function to the barrier layer 13. 2 Even if the thickness exceeds 100 mm, the corrosion prevention function does not change much. On the other hand, when a rare earth oxide sol is used, if the coating is thick, the heat curing during drying may be insufficient, which may result in a decrease in cohesive force. The thickness of the corrosion prevention treatment layer 14 can be calculated from its specific gravity.

[0061] From the viewpoint of adhesion between the sealant layer and the barrier layer, the corrosion prevention treatment layer may be, for example, an embodiment that contains cerium oxide, 1 to 100 parts by mass of phosphoric acid or a phosphate relative to 100 parts by mass of the cerium oxide, and a cationic polymer, or an embodiment that is formed by subjecting the barrier layer 13 to a chemical conversion treatment, or an embodiment that is formed by subjecting the barrier layer to a chemical conversion treatment and contains a cationic polymer.

[0062] (Second adhesive layer) The second adhesive layer 17 is a layer that bonds the barrier layer 13, on which the corrosion prevention treatment layer 14 is formed, to the sealant layer 16. For the second adhesive layer 17, a general adhesive for bonding the barrier layer 13 and the sealant layer 16 can be used.

[0063] When the corrosion prevention treatment layer 14 has a layer containing at least one type of polymer selected from the group consisting of the above-mentioned cationic polymers and anionic polymers, the second adhesive layer 17 is preferably a layer containing a compound (hereinafter also referred to as a "reactive compound") that is reactive with the above-mentioned polymer contained in the corrosion prevention treatment layer 14.

[0064] For example, when the corrosion prevention treatment layer 14 contains a cationic polymer, the second adhesive layer 17 contains a compound reactive with the cationic polymer. When the corrosion prevention treatment layer 14 contains an anionic polymer, the second adhesive layer 17 contains a compound reactive with the anionic polymer. When the corrosion prevention treatment layer 14 contains a cationic polymer and an anionic polymer, the second adhesive layer 17 contains a compound reactive with the cationic polymer and a compound reactive with the anionic polymer. However, the second adhesive layer 17 does not necessarily have to contain the above two types of compounds, and may contain a compound reactive with both the cationic polymer and the anionic polymer. Here, "reactive" means to form a covalent bond with the cationic polymer or the anionic polymer. The second adhesive layer 17 may further contain an acid-modified polyolefin resin.

[0065] The compound reactive with the cationic polymer may be at least one compound selected from the group consisting of a polyfunctional isocyanate compound, a glycidyl compound, a compound having a carboxy group, and a compound having an oxazoline group.

[0066] Examples of the polyfunctional isocyanate compound, glycidyl compound, compound having a carboxy group, and compound having an oxazoline group include the polyfunctional isocyanate compound, glycidyl compound, compound having a carboxy group, and compound having an oxazoline group, which are exemplified above as crosslinking agents for forming a crosslinked structure from a cationic polymer. Among these, the polyfunctional isocyanate compound is preferred in terms of high reactivity with the cationic polymer and ease of forming a crosslinked structure.

[0067] The compound reactive with anionic polymers includes at least one compound selected from the group consisting of glycidyl compounds and compounds having oxazoline groups.These glycidyl compounds and compounds having oxazoline groups include the glycidyl compounds and compounds having oxazoline groups exemplified above as crosslinking agents for forming cationic polymers into crosslinked structures.Among these, glycidyl compounds are preferred because of their high reactivity with anionic polymers.

[0068] When the second adhesive layer 17 contains an acid-modified polyolefin resin, it is preferable that the reactive compound also has a reactivity with the acidic group in the acid-modified polyolefin resin (i.e., forms a covalent bond with the acidic group). This further enhances the adhesion to the corrosion prevention treatment layer 14. In addition, the acid-modified polyolefin resin has a crosslinked structure, further improving the solvent resistance of the exterior material 10.

[0069] The content of the reactive compound is preferably from an equivalent amount to 10 times the equivalent amount of the acidic group in the acid-modified polyolefin resin. If it is an equivalent amount or more, the reactive compound reacts sufficiently with the acidic group in the acid-modified polyolefin resin. On the other hand, if it exceeds 10 times the equivalent amount, the crosslinking reaction with the acid-modified polyolefin resin is sufficiently saturated, so that there is a concern of the presence of unreacted substances and a decrease in various performances. Therefore, for example, the content of the reactive compound is preferably 5 to 20 parts by mass (solid content ratio) per 100 parts by mass of the acid-modified polyolefin resin.

[0070] The acid-modified polyolefin resin is a polyolefin resin to which an acidic group has been introduced. Examples of the acidic group include a carboxyl group, a sulfonic acid group, and an acid anhydride group, and maleic anhydride groups and (meth)acrylic acid groups are particularly preferred. For example, the acid-modified polyolefin resin may be the same as the modified polyolefin resin used in the sealant layer 16.

[0071] The second adhesive layer 17 may contain various additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, and a tackifier.

[0072] Examples of adhesives that form the second adhesive layer 17 include polyurethane resins in which a difunctional or higher isocyanate compound is reacted with a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol, and epoxy resins in which an amine compound or the like is reacted with a base material having an epoxy group, and these are preferred from the standpoint of heat resistance.

[0073] The thickness of the second adhesive layer 17 is not particularly limited, but from the viewpoint of obtaining the desired adhesive strength, processability, and the like, it is preferably 1 to 10 μm, and more preferably 2 to 7 μm.

[0074] [Metal terminal] Fig. 4 is a cross-sectional view of the terminal resin film and the metal terminal shown in Fig. 1 in the direction of line IV-IV. Of the pair of metal terminals 30, 30, one metal terminal 30 is electrically connected to the positive electrode of the electricity storage device main body 50, and the other metal terminal 30 is electrically connected to the negative electrode of the electricity storage device main body 50. The pair of metal terminals 30, 30 extend from the electricity storage device main body 50 to the outside of the exterior material 10. The shape of the pair of metal terminals 30, 30 may be, for example, a flat plate shape.

[0075] Metals can be used as the material of the metal terminal 30. The metal to be used as the material of the metal terminal 30 may be determined in consideration of the structure of the power storage device main body 50 and the materials of its components. For example, when the power storage device 100 is an all-solid-state battery, aluminum is preferably used as the material of the metal terminal 30 connected to the positive electrode of the power storage device main body 50. Copper having a nickel plating layer formed on the surface, or nickel, is preferably used as the material of the metal terminal 30 connected to the negative electrode of the power storage device main body 50.

[0076] The thickness of the metal terminal 30 depends on the size and capacity of the all-solid-state battery. In the case of a small all-solid-state battery, the thickness of the metal terminal 30 may be, for example, 50 μm or more. In the case of a large all-solid-state battery for power storage, vehicle mounting, etc., the thickness of the metal terminal 30 may be appropriately set within the range of, for example, 100 to 500 μm.

[0077] [Resin film for terminals] 4, the terminal resin film 40 is disposed so as to cover a portion of the outer circumferential surface of the metal terminal 30. By disposing the terminal resin film 40 between the metal terminal 30 and the exterior material 10, it is possible to achieve an even higher level of sealing and insulating properties of the electricity storage device 100. The terminal resin film 40 has heat resistance equal to or greater than that of the sealant layer 16 and the base material layer 11 described above.

[0078] The resin film 40 for terminals includes a resin layer 40a having at least one sub-dispersion peak γ in the range of −130° C. to −50° C. in the profile of loss tangent tanδ obtained by dynamic viscoelasticity measurement under the condition of 1.0 Hz. The resin film 40 for terminals has a single-layer structure or a multi-layer structure. When the resin film 40 for terminals has a single-layer structure, the resin film 40 for terminals is made of the resin layer 40a (see FIG. 5(a)). When the resin film 40 for terminals has a multi-layer structure, the resin film 40 for terminals may include at least one resin layer (resin layer 40a) that satisfies the above conditions (see FIGS. 5(b) and 5(c)). When the resin film 40 for terminals has a multi-layer structure, it is preferable that all layers are made of the same resin material from the viewpoint of adhesion between adjacent layers.

[0079] By providing the resin film 40 for terminal with the resin layer 40a, the resin film 40 for terminal can achieve both a sufficiently high level of sealing strength at high temperatures and an initial sealing strength (sealing strength at room temperature). The temperature range in which the minor dispersion peak γ exists is preferably -120°C to -60°C, more preferably -110°C to -70°C, from the viewpoint of sealing strength at room temperature and at high temperatures. If the temperature in which the minor dispersion peak γ exists is less than -130°C, the heat resistance of the resin layer 40a may be poor, and the sealing strength at high temperatures may be insufficient. On the other hand, if the temperature in which the minor dispersion peak γ exists exceeds -50°C, the flexibility of the resin layer 40a may be poor, and the sealing strength at room temperature may be insufficient.

[0080] The above tan δ can be calculated, for example, as the loss tangent tan δ from the loss modulus E'' and the storage modulus E' by measuring the terminal resin film 40 under the following conditions using a dynamic viscoelasticity device (manufactured by SII, product name: DMS6100) in accordance with a method conforming to JIS K7244-4. Peeling mode: Pulling Heating rate: 2℃ / min Temperature range: -150~150℃ Frequency: 1.0Hz

[0081] The resin layer 40a preferably has at least one main dispersion peak α in the range of 30°C to 130°C of the tan δ profile. When the resin layer 40a satisfies this condition, the terminal resin film 40 exhibits even better initial seal strength (seal strength at room temperature). The temperature range in which the main dispersion peak α exists is preferably 40°C to 110°C, more preferably 50°C to 100°C, from the viewpoint of seal strength at room temperature. If the temperature in which the main dispersion peak α exists is less than 30°C, the heat resistance of the resin layer 40a tends to be poor and the seal strength at high temperatures tends to be insufficient. On the other hand, if the temperature in which the main dispersion peak α exists exceeds 130°C, the flexibility of the resin layer 40a tends to be poor and the seal strength at room temperature tends to be insufficient.

[0082] The temperature at which the minor dispersion peak γ and the major dispersion peak α of the resin layer 40a appear can be controlled, for example, by the structure of the base resin material contained in the resin layer 40a, the stretching ratio of the resin layer 40a, or the amount of additives (e.g., plasticizers). The resin layer 40a contains additives as necessary. Examples of additives include plasticizers, antioxidants, slip agents, flame retardants, AB agents, light stabilizers, dehydrating agents, and tackifiers.

[0083] Examples of the base resin material contained in the terminal resin film 40 include polyester-based, polyolefin-based, and polyamide-based resins.

[0084] The polyester resin can be obtained by copolymerizing an acid component and a glycol component. Examples of the acid component include phthalic acid, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, cyclohexanedicarboxylic acid, adipic acid, and sebacic acid. Examples of the glycol component include ethylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, diethylene glycol, polytetramethylene glycol, cyclohexanedimethanol, and propanediol. According to the study by the present inventors, the temperature at which the secondary dispersion peak γ exists for a typical PET (a copolymer of terephthalic acid and ethylene glycol) is outside the range of −130° C. to −50° C., and the seal strength at room temperature is insufficient. When a plasticizer is not blended in the resin layer 40a, the resin layer 40a preferably contains a polyester resin in which one type of acid component is copolymerized with two or more types of glycol components.

[0085] Examples of polyolefin resins include polyethylene and polypropylene resins. Since commonly used polyolefin resins have poor heat resistance, it is preferable to use polyethylene or polypropylene modified with amide or the like. From the viewpoint of adhesion between the metal terminal 30 and the terminal resin film 40, it is preferable to use, as the base resin material of the terminal resin film 40, polyolefin modified with an acid such as carboxylic acid or maleic anhydride or modified with amide.

[0086] Examples of polyamide resins include nylon 6 and nylon 6,6.

[0087] From the viewpoint of adjusting the temperature at which the minor dispersion peak γ and the major dispersion peak α of the resin layer 40a appear, the resin layer 40a preferably contains a plasticizer. As the plasticizer, for example, an ester-based compound can be used. Specific examples include glycol diester, adipic acid ester, phthalic acid ester, diacetyl monoacyl glycerol derivative, and ester having an ether skeleton. Although it depends on the base resin material of the resin layer 40a, the content of the plasticizer in the resin layer 40a is preferably 30 mass% or less based on the mass of the resin layer 40a. When an excessive amount of plasticizer is blended in the resin layer 40a, the temperature at which the minor dispersion peak γ and the major dispersion peak α appear is excessively lowered, and the cohesive force tends to decrease.

[0088] When the resin film 40 for a terminal has a multi-layer structure, the resin layer 40a may be disposed on the side in contact with the metal terminal 30, or on the side in contact with the exterior material 10. When the resin film 40 for a terminal is made up of three or more layers, the resin layer 40a may be disposed between the resin layer 40b and the resin layer 40c (see FIG. 5(c)).

[0089] From the viewpoints of embeddability and insulating properties, the thickness of the resin film 40 for terminal is preferably 15 μm or more, more preferably 30 to 300 μm, and further preferably 50 to 200 μm.

[0090] When the electrolyte of the all-solid-state battery is a sulfide-based electrolyte, the terminal resin film 40 preferably contains a hydrogen sulfide adsorbent. By containing a hydrogen sulfide adsorbent in the terminal resin film 40, excellent seal strength can be maintained at room temperature and at high temperatures even after exposure to hydrogen sulfide. Examples of hydrogen sulfide adsorbents include those mentioned above.

[0091] The content of the hydrogen sulfide adsorbent in the resin film for terminal 40 is preferably 1 to 50 mass %, more preferably 2 to 25 mass %, and even more preferably 5 to 15 mass %, based on the mass of the resin film for terminal 40. When the content of the hydrogen sulfide adsorbent in the resin film for terminal 40 is 1 mass % or more, the hydrogen sulfide absorption or adsorption effect is exhibited, while when the content is 50 mass % or less, the resin film for terminal 40 can achieve both adhesion and sealant suitability. When the resin film for terminal 40 has a multi-layer structure, from the viewpoint of adhesion to the metal terminal 30, it is preferable that the layer in contact with the metal terminal 30 does not contain a hydrogen sulfide adsorbent. That is, it is preferable that the layer in contact with the exterior material 10 (for example, the resin layer 40a in FIG. 5(b) or the resin layers 40a, 40c in FIG. 5(c)) contains a hydrogen sulfide adsorbent, and when the resin film for terminal 40 is composed of three or more layers, it is preferable that an intermediate layer (for example, the resin layer 40a in FIG. 5(c)) contains a hydrogen sulfide adsorbent.

[0092] Although the embodiment of the present disclosure has been described above in detail, the present invention is not limited to the above embodiment, and various modifications and changes are possible within the scope of the gist of the present disclosure described in the claims. For example, in the above embodiment, the corrosion prevention treatment layer 14 is provided only on one surface (the second adhesive layer 17 side) of the barrier layer 13, but the corrosion prevention treatment layer 14 may also be provided on the other surface (the first adhesive layer 12 side) of the barrier layer 13. In addition, for example, when the sealant layer 16 is attached to the barrier layer 13 by thermal lamination, the second adhesive layer 17 may not be provided. When the base layer 11 is provided by coating or painting, the first adhesive layer 12 may not be provided. In the above embodiment, an electric solid battery is exemplified as an electric storage device to which the exterior material 10 is applied, but the exterior material 10 may be applied to other electric storage devices (for example, lithium ion batteries).

[0093] A method for selecting a resin film for terminals may be carried out based on the contents of the above embodiment. That is, this selection method is for selecting a resin film for terminals to be arranged so as to cover a part of the outer circumferential surface of a terminal in an electricity storage device including an electricity storage device main body and a terminal electrically connected to the electricity storage device main body, and may include (A) a step of performing dynamic viscoelasticity measurement under a condition of 1.0 Hz on the resin film for terminals to be evaluated, and (B) a step of judging whether or not at least one sub-dispersion peak γ exists in the range of −130° C. to −50° C. in the profile of tan δ obtained by the dynamic viscoelasticity measurement. The matters described in the above embodiment may be appropriately applied to this selection method. EXAMPLES

[0094] The present disclosure will be described more specifically below based on examples, but the present disclosure is not limited to the following examples.

[0095] [Materials used] In order to produce the resin films for terminals according to the examples and comparative examples, the following materials were prepared. [Base resin material] Polyester resin 1: A copolymer of terephthalic acid as the acid component and ethylene glycol as the glycol component. Polyester resin 2: A copolymer of terephthalic acid as the acid component and ethylene glycol and butanediol as the glycol component. Polyester resin 3: A copolymer of terephthalic acid and isophthalic acid as the acid component and ethylene glycol, butanediol and neopentyl glycol as the glycol component. Polyester resin 4: A copolymer of terephthalic acid as the acid component and ethylene glycol and 1,4-cyclohexanedimethanol as the glycol component. Polyester resin 5: A copolymer of terephthalic acid and isophthalic acid as the acid component and butanediol and hexanediol as the glycol component. Polyester resin 6: A copolymer of terephthalic acid and isophthalic acid as the acid component and butanediol and hexanediol as the glycol component (the proportion of butanediol is increased more than that of polyester resin 5) Polyester resin 7: A copolymer of naphthalenedicarboxylic acid as the acid component and 1,4-cyclohexanedimethanol as the glycol component. Polyester resin 8: A copolymer of terephthalic acid and isophthalic acid as the acid component and ethylene glycol and hexanediol as the glycol component. Polyolefin resin 1: Amide-modified polyethylene Polyolefin resin 2: Random polypropylene [Plasticizer] Glycol diester: 10 parts by weight per 100 parts by weight of the base resin material was mixed as required. [Hydrogen sulfide absorber] Zinc oxide: 3 parts by mass was mixed in with 100 parts by mass of the base resin material as required.

[0096] Example 1 A resin film for terminals (single layer, thickness: 100 μm) made of the following resin composition was produced by an inflation method. Polyester resin 1:100 parts by weight Plasticizer: 10 parts by weight Hydrogen sulfide adsorption material: 3 parts by weight

[0097] Example 2 A resin film for terminals (single layer, thickness: 100 μm) was produced in the same manner as in Example 1, except that polyester resin 2 was used instead of polyester resin 1.

[0098] Example 3 A resin film for terminals (single layer, thickness: 100 μm) was produced in the same manner as in Example 1, except that no hydrogen sulfide adsorbing substance was used.

[0099] Example 4 A resin film for terminals (single layer, thickness: 100 μm) made of polyester resin 3 was produced by an inflation method.

[0100] Example 5 A resin film for terminals (single layer, thickness: 100 μm) was produced in the same manner as in Example 4, except that a plasticizer (10 parts by mass) and a hydrogen sulfide adsorbing material (3 parts by mass) were blended into the polyester resin 3.

[0101] Example 6 A resin film for terminal (single layer, thickness: 100 μm) consisting of a polyester resin 4 and a hydrogen sulfide adsorbing material (3 parts by mass) was produced by an inflation method.

[0102] Example 7 A resin film for terminal (single layer, thickness: 100 μm) consisting of a polyester resin 5 and a hydrogen sulfide adsorbing material (3 parts by mass) was produced by an inflation method.

[0103] Example 8 A resin film for terminals (single layer, thickness: 100 μm) consisting of a polyester resin 6 and a hydrogen sulfide adsorbing material (3 parts by mass) was produced by an inflation method.

[0104] Example 9 A resin film for terminals (single layer, thickness: 100 μm) consisting of polyolefin resin 1 and hydrogen sulfide adsorbing material (3 parts by mass) was produced by an inflation method.

[0105] Example 10 A two-layered resin film for terminals (50 μm / 50 μm) was produced by the inflation method. Exterior layer: 1 part polyester resin and 3 parts hydrogen sulfide adsorbent -Layer on metal terminal side: Polyester resin 7

[0106] Example 11 A three-layered resin film for terminals (25 μm / 50 μm / 25 μm) was produced by the inflation method. Exterior layer: polyester resin 2, plasticizer (10 parts by weight), and hydrogen sulfide adsorbent (3 parts by weight) Middle layer: polyester resin 1, plasticizer (10 parts by weight), and hydrogen sulfide adsorbent (3 parts by weight) Layer on metal terminal side: polyester resin 2 and plasticizer (10 parts by weight)

[0107] Example 12 A three-layered resin film for terminals (25 μm / 50 μm / 25 μm) was produced by the inflation method. Exterior layer: 1 part polyester resin and 10 parts plasticizer Middle layer: polyester resin 8 and hydrogen sulfide adsorbent (3 parts by weight) -Layer on metal terminal side: Polyester resin 1 and plasticizer (10 parts by weight)

[0108] (Example 13) A two-layered resin film for terminals (50 μm / 50 μm) was produced by the inflation method. Exterior layer: polyester resin 1, plasticizer (10 parts by weight), and hydrogen sulfide adsorbent (3 parts by weight) -Layer on metal terminal side: Polyester resin 8

[0109] Example 14 A three-layered resin film for terminals (25 μm / 50 μm / 25 μm) was produced by the inflation method. Exterior layer: Polyester resin 7 Middle layer: polyester resin 1, plasticizer (10 parts by weight), and hydrogen sulfide adsorbent (3 parts by weight) -Layer on metal terminal side: Polyester resin 7

[0110] Comparative Example 1 A resin film for terminal (single layer, thickness: 100 μm) consisting of polyester resin 7 and hydrogen sulfide adsorbing material (3 parts by mass) was produced by an inflation method.

[0111] Comparative Example 2 A resin film for terminals (single layer, thickness: 100 μm) consisting of polyester resin 1 and hydrogen sulfide adsorbing material (3 parts by mass) was produced by an inflation method.

[0112] Comparative Example 3 A resin film for terminal (single layer, thickness: 100 μm) consisting of a polyester resin 8 and a hydrogen sulfide adsorbing material (3 parts by mass) was produced by an inflation method.

[0113] Comparative Example 4 A resin film for terminals (single layer, thickness: 100 μm) made of polyolefin resin 2 was produced by an inflation method.

[0114] Comparative Example 5 A three-layered resin film for terminals (25 μm / 50 μm / 25 μm) was produced by the inflation method. Exterior layer: Polyester resin 7 Middle layer: polyester resin 8 and hydrogen sulfide adsorbent (3 parts by weight) -Layer on metal terminal side: Polyester resin 7

[0115] <Evaluation> The resin films for terminals obtained in the examples and comparative examples were subjected to the following evaluation tests.

[0116] [Loss tangent of resin film for terminals tanδ] The resin film for terminals was cut to 10 mm (TD) x 30 mm (MD) to obtain a test piece. The test piece was held with a chuck distance of 20 mm. Measurements were performed under the following conditions using a dynamic viscoelasticity device (manufactured by SII, product name: DMS6100) in accordance with the method in accordance with JIS K7244-4, and the loss tangent tanδ was calculated from the loss modulus E'' and storage modulus E'. In addition, the temperature of the minor dispersion peak γ and the temperature of the major dispersion peak α were determined from the obtained tanδ profile. The results are shown in Tables 1 to 3. Peeling mode: Pulling Heating rate: 2℃ / min Temperature range: -150~150℃ Frequency: 1.0Hz

[0117] [Initial seal strength] A chemically treated aluminum plate (50mm x 50mm) was prepared. On the other hand, a resin film for terminals was cut to 50mm (TD) x 100mm (MD) to obtain a test piece. This test piece was folded in half, and an aluminum plate was placed between the two. One side of the laminate (test piece / aluminum plate / test piece) was heat sealed with a 10mm wide seal bar at 165°C, 0.6MPa, and 10 seconds. The heat sealed portion was then cut to a width of 15mm to obtain a measurement sample (see Figure 6). The seal strength was measured at room temperature (23°C) with a peel speed of 50mm / min. Based on the results, evaluation was performed according to the following criteria. The results are shown in Tables 1 to 3. A: Burst strength is 25N / 15mm or more B: Burst strength is 20N / 15mm or more and less than 25N / 15mm C: Burst strength is 15N / 15mm or more and less than 20N / 15mm D: Burst strength is less than 15N / 15mm

[0118] [High temperature seal strength] A chemically treated aluminum plate (50mm x 50mm) was prepared. On the other hand, a resin film for terminals was cut to 50mm (TD) x 100mm (MD) to obtain a test piece. This test piece was folded in half, and an aluminum plate was placed between them. One side of the laminate (test piece / aluminum plate / test piece) was heat sealed with a 10mm wide seal bar at 165°C, 0.6MPa, and 10 seconds. Thereafter, the heat sealed portion was cut to a width of 15mm, and left to stand in a 150°C environment for 5 minutes, after which the seal strength was measured in a 150°C environment at a peel speed of 50mm / min. Based on the results, evaluation was performed according to the following criteria. The results are shown in Tables 1 to 3. A: Burst strength is 15N / 15mm or more B: Burst strength is 10N / 15mm or more and less than 15N / 15mm C: Burst strength is 5N / 15mm or more and less than 10N / 15mm D: Burst strength is less than 5N / 15mm

[0119] [Seal strength after exposure to hydrogen sulfide (at room temperature)] A chemically treated aluminum plate (50mm x 50mm) was prepared. On the other hand, a resin film for terminals was cut to 50mm (TD) x 100mm (MD) to obtain a test piece. This test piece was folded in half, and an aluminum plate was placed between them. One side of the laminate (test piece / aluminum plate / test piece) was heat sealed with a 10mm wide seal bar at 165°C, 0.6MPa, and 10 seconds. Thereafter, the heat sealed portion was cut to a width of 15mm, and left to stand for 72 hours in a room temperature environment with a hydrogen sulfide concentration of 20ppm, after which the seal strength was measured in a room temperature environment at a peel speed of 50mm / min. Based on the results, the following criteria were used for evaluation. The results are shown in Tables 1 to 3. A: Burst strength is 25N / 15mm or more B: Burst strength is 20N / 15mm or more and less than 25N / 15mm C: Burst strength is 15N / 15mm or more and less than 20N / 15mm D: Burst strength is less than 15N / 15mm

[0120] [Seal strength after exposure to hydrogen sulfide (150℃ environment)] A chemically treated aluminum plate (50mm x 50mm) was prepared. On the other hand, a resin film for terminals was cut to 50mm (TD) x 100mm (MD) to obtain a test piece. This test piece was folded in half, and an aluminum plate was placed between them. One side of the laminate (test piece / aluminum plate / test piece) was heat sealed with a 10mm wide seal bar at 165°C, 0.6MPa, and 10 seconds. Thereafter, the heat sealed portion was cut to a width of 15mm and left to stand for 72 hours in a room temperature environment with a hydrogen sulfide concentration of 20ppm. After that, it was left to stand for 5 minutes in a 150°C environment, and then the seal strength was measured in a 150°C environment at a peel speed of 50mm / min. Based on the results, it was evaluated according to the following criteria. The results are shown in Tables 1 to 3. A: Burst strength is 15N / 15mm or more B: Burst strength is 10N / 15mm or more and less than 15N / 15mm C: Burst strength is 5N / 15mm or more and less than 10N / 15mm D: Burst strength is less than 5N / 15mm

[0121] [Table 1]

[0122] [Table 2]

[0123] [Table 3]

[0124] In Tables 1 to 3, it can be said that the overall quality is excellent if there is no D in the evaluation results. Examples 1 to 14 were rated A to C for seal strength. In contrast, some of Comparative Examples 1 to 5 were rated D for seal strength. Specifically, Comparative Example 1 was rated D for seal strength at room temperature (initial and after hydrogen sulfide exposure). This is presumably because the temperature of the minor dispersion peak γ was higher than the range of -130°C to -50°C and the temperature of the major dispersion peak α was also higher than the range of 30°C to 130°C. Comparative Example 2 was also rated D for seal strength at room temperature (initial and after hydrogen sulfide exposure). This is presumably because the temperature of the minor dispersion peak γ was higher than the range of -130°C to -50°C. Comparative Example 3 was rated D for seal strength in a 150°C environment both before and after hydrogen sulfide exposure. This is presumably because the temperature of the minor dispersion peak γ was lower than the range of -130°C to -50°C. The seal strength of Comparative Example 4 in a 150° C. environment both before and after exposure to hydrogen sulfide was evaluated as D. This is presumably because the temperature of the minor dispersion peak γ was lower than the range of −130° C. to −50° C. and the temperature of the major dispersion peak α was lower than the range of 30° C. to 130° C. Comparative Example 5 received all evaluations of D for seal strength. [Explanation of symbols]

[0125] DESCRIPTION OF SYMBOLS 10... exterior material for electricity storage device, 11... base material layer, 12... first adhesive layer, 13... barrier layer, 14... corrosion prevention treatment layer, 16... sealant layer, 16a... first resin layer, 16b... second resin layer, 16c... third resin layer, 17... second adhesive layer, 30... metal terminal, 40... resin film for terminal, 40a... resin layer, 50... electricity storage device main body, 100... electricity storage device

Claims

1. A resin film for a terminal is disposed so as to cover an outer peripheral surface of a part of a terminal in an electricity storage device including an electricity storage device main body and a terminal electrically connected to the electricity storage device main body, The resin film for terminals has a single-layer structure or a multi-layer structure, A resin layer having at least one sub-dispersion peak γ in the range of −130° C. to −74° C. of a profile of loss tangent tanδ obtained by dynamic viscoelasticity measurement under a condition of 1.0 Hz; The resin film for a terminal, wherein the resin layer contains a polyester-based resin or an amide-modified polyolefin-based resin.

2. 2. The resin film for a terminal according to claim 1, wherein the resin layer has at least one main dispersion peak α in the range of 30° C. to 130° C. of the tan δ profile.

3. The resin film for a terminal according to claim 1 , wherein the resin layer contains a plasticizer.

4. The resin film for a terminal according to any one of claims 1 to 3, which contains a hydrogen sulfide adsorbing substance.

5. A method for selecting a terminal resin film to be disposed so as to cover an outer peripheral surface of a part of a terminal in an electric storage device including an electric storage device main body and a terminal electrically connected to the electric storage device main body, comprising: The resin film for terminal to be evaluated has a resin layer, The resin layer contains a polyester-based resin or an amide-modified polyolefin-based resin, (A) performing dynamic viscoelasticity measurement on the resin layer of the resin film for terminal to be evaluated under a condition of 1.0 Hz; (B) determining whether or not at least one minor dispersion peak γ exists in the range of −130° C. to −74° C. in the profile of tan δ obtained by the dynamic viscoelasticity measurement; A method for selecting a resin film for a terminal, comprising:

6. A power storage device main body; A terminal extending from the power storage device body; an exterior material that holds the terminals and houses the electricity storage device main body; The resin film for terminal according to any one of claims 1 to 4, which is disposed between the terminal and the exterior material; A power storage device comprising:

7. The exterior material has a laminated structure including at least a base layer, a barrier layer, and a sealant layer in this order, 7. The power storage device according to claim 6, wherein the sealant layer has at least one sub-dispersion peak γ in a range of −130° C. to −50° C. in a profile of loss tangent tan δ obtained by dynamic viscoelasticity measurement under a condition of 1.0 Hz.

8. The electricity storage device according to claim 7 , wherein the sealant layer has at least one main dispersion peak α in a range of 30° C. to 130° C. of the tan δ profile.

9. The electricity storage device according to claim 7 or 8, wherein the sealant layer contains a plasticizer.

10. The electricity storage device according to any one of claims 7 to 9, wherein the sealant layer contains a hydrogen sulfide adsorbing substance.

11. The adhesive layer is disposed between the barrier layer and the sealant layer. The electricity storage device according to any one of claims 7 to 10, wherein the adhesive layer contains a hydrogen sulfide adsorbing substance.

12. The power storage device according to any one of claims 7 to 11, further comprising a corrosion prevention treatment layer provided on at least one surface of the barrier layer.

Citation Information

Patent Citations

  • Metallic terminal film and metallic terminal bonded with same

    JP2010097853A

  • Tab lead

    JP2016129105A

  • All-solid type lithium ion secondary battery

    JP2016143520A

  • Adhesive film for metal terminal

    JP2016184546A

  • Laminate for sulfide-based gas adsorption

    JP2017001187A