Polystyrene resin foam and exhibition panel

A polystyrene resin foam with a butadiene content of 0.4 to 4.0% and Mz of 300,000 to 650,000 addresses ripples, providing excellent bending strength and surface quality for display panels.

JP2024138145AActive Publication Date: 2024-10-07SEKISUI PLASTICS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024122446
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-07
Estimated Expiration
2041-04-16

AI Technical Summary

Technical Problem

Polystyrene resin foams often develop surface undulations called 'ripples' which impair the surface quality and beauty of display panels, and existing technologies do not address this issue effectively.

Method used

A polystyrene resin foam with a specific composition containing a butadiene component of 0.4 to 4.0% by mass and a Z average molecular weight (Mz) of 300,000 to 650,000, along with a molecular weight distribution of 1.6 to 2.2, is used to create a foam layer with excellent bending strength and reduced warpage.

Benefits of technology

The solution results in a polystyrene resin foam with enhanced bending strength, minimal warpage, and improved surface properties, ensuring clear and beautiful printing on display panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138145000001_ABST
    Figure 2024138145000001_ABST
Patent Text Reader

Abstract

To provide a polystyrene resin foam and an exhibition panel which have excellent flexural strength, little warpage, and excellent surface properties.SOLUTION: A polystyrene resin foam 1 has a plate-like or sheet-like shape and includes a foam layer being an extruded foam containing a polystyrene resin. The polystyrene resin contains a butadiene component. The content of the butadiene component is 0.4-4.0 mass% based on the total mass of the foam layer. The polystyrene resin has a Z-average molecular weight (Mz) of 300,000-650,000.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polystyrene-based resin foam and an exhibition panel. [Background technology]

[0002] Conventionally, plate-shaped polystyrene resin foams have been known as exhibition panels for attaching printed matter such as photographs, posters, advertisements, etc. For exhibition panels, it is required that the printed matter be sufficiently bonded to the polystyrene resin foam and not peeled off or lifted off.

[0003] As such an exhibition panel, for example, Patent Document 1 proposes a polystyrene resin foam having a surface layer and having recesses of a specific size at a specific density on the surface of the surface layer. According to the invention of Patent Document 1, the adhesiveness of paper (paper lamination property) by the glue is good, and it is intended to make the adhered paper difficult to peel off. Patent Document 2 proposes a sheet-like polystyrene resin foam in which the arithmetic mean roughness of the sheet surface is within a specific range, and the shape of the air bubbles present within a specific depth range from the surface satisfies a specific relational expression. According to the invention of Patent Document 2, it is intended to improve the surface smoothness and enable not only ultraviolet-curable ink but also water-based ink to be directly printed on the surface.

[0004] In addition, polystyrene-based resin foams are required to not adhere to a mold during molding and to have excellent thermal stability. For example, Patent Document 3 proposes, as such a polystyrene-based resin foam, a styrene-based resin composition for foam molding, which contains a specific amount of a conjugated diene polymer per 100 parts by mass of a styrene-based resin and has a total content of a styrene dimer and a styrene trimer of not more than a specific concentration. According to the invention of Patent Document 3, it is intended to achieve excellent thermal stability during molding, extremely low molecular weight reduction, and excellent strength. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2003-220639 A [Patent Document 2] JP 2011-98509 A [Patent Document 3] JP 2004-315692 A Summary of the Invention [Problem to be solved by the invention]

[0006] By the way, the surface of polystyrene foamed resin may have a wavy shape called "ripples." If a polystyrene foamed resin with ripples is used, the ripples on the surface of an exhibition panel to which a printed matter is attached become conspicuous, and the beauty of the surface (surface quality) is impaired. In the techniques of Patent Documents 1 to 3, no consideration is given to reducing ripples.

[0007] SUMMARY OF THE PRESENT EMBODIMENTS The present invention has an object to provide a polystyrene-based resin foam and an exhibition panel that have excellent bending strength, little warping, and excellent surface properties. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention has the following aspects. It is in a plate or sheet shape, The foam layer is an extruded foam containing a polystyrene-based resin, The polystyrene resin contains a butadiene component, The content of the butadiene component is 0.4 to 4.0% by mass based on the total mass of the foamed layer, The polystyrene resin foam has a Z-average molecular weight (Mz) of 300,000 to 650,000. The present invention also has the following aspects. [1] It is in plate or sheet form, A foam layer containing a polystyrene resin is provided. The polystyrene resin contains a butadiene component, The content of the butadiene component is 0.4 to 4.0% by mass based on the total mass of the foamed layer, The polystyrene resin foam has a Z-average molecular weight (Mz) of 300,000 to 650,000. [2] The polystyrene-based resin contains a styrene-butadiene copolymer; The polystyrene-based resin foam according to [1], wherein the content of the styrene-butadiene copolymer is 10 to 65 mass % based on the total mass of the polystyrene-based resin. [3] The polystyrene-based resin foam according to [1] or [2], wherein the molecular weight distribution (Mz / Mw) obtained by dividing the Z-average molecular weight (Mz) of the polystyrene-based resin by the mass-average molecular weight (Mw) of the polystyrene-based resin is 1.6 to 2.2. [4] The polystyrene-based resin foam according to any one of [1] to [3], wherein the polystyrene-based resin is a polystyrene-based resin derived from recycled products.

[0009] [5] An exhibition panel comprising the polystyrene resin foam according to any one of [1] to [4], and a skin material provided on either or both surfaces of the polystyrene resin foam. Effect of the Invention

[0010] The polystyrene-based resin foam and the display panel of the present invention have excellent bending strength, are less prone to warping, and have an excellent surface property. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view of a polystyrene-based resin foam according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing an example of a production apparatus for a polystyrene-based resin foam according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic diagram showing another example of an apparatus for producing a polystyrene-based resin foam according to an embodiment of the present invention. [Figure 4] FIG. 2 is a perspective view illustrating an example of ripples formed on the surface of a polystyrene-based resin foam. [Diagram 5] 1 is a photograph of the surface of a polystyrene-based resin foam of Example 5. [Figure 6] 1 is a photograph of the surface of a polystyrene-based resin foam of Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In this specification, the symbol "to" indicates a range that includes both ends of the symbol as the lower limit and upper limit. A preferred embodiment of the present invention will be described below by taking a plate-shaped polystyrene resin foam as an example. The polystyrene resin foam may be composed of a single foamed layer, or may have two or more foamed layers. The polystyrene resin foam may have a non-foamed resin layer provided on one side of the polystyrene resin foam, or may have non-foamed resin layers provided on both sides of the polystyrene resin foam. The non-foamed resin layer may be composed of a single non-foamed layer, or may have two or more non-foamed layers.

[0013] [Polystyrene resin foam] The polystyrene resin foam of the present invention (hereinafter, also simply referred to as "foam") is a plate- or sheet-like foam having a foam layer containing a polystyrene resin. One embodiment of the foam will be described with reference to the drawings.

[0014] 1 is a foamed plate made up of a first foamed layer 2a and a second foamed layer 2b. The first foamed layer 2a and the second foamed layer 2b are joined at a joint 3.

[0015] Thickness T of foam 1 1 can be determined taking into consideration the application. For example, the thickness T 1 The thickness T is preferably 3.0 to 15.0 mm, more preferably 4.0 to 12.0 mm, and further preferably 5.0 to 10.0 mm. 1 When the thickness T is equal to or greater than the lower limit, the bending strength can be further increased and warping can be suppressed. 1 When is equal to or less than the above upper limit, the foam 1 can be made lightweight and easy to produce. Thickness T 1 can be measured, for example, using a microgauge.

[0016] Thickness T of the first foam layer 2a 2a can be determined taking into consideration the application. For example, the thickness T 2a The thickness T is preferably 1.5 to 7.5 mm, more preferably 2.0 to 6.0 mm, and further preferably 2.5 to 5.0 mm. 2a When the thickness T is equal to or greater than the lower limit, the flexural strength of the foam 1 can be further increased, and warping can be suppressed. 2a When is equal to or less than the above upper limit, the foam 1 can be made lightweight and easy to produce. Thickness T 2a is the thickness T 1 It can be calculated in the same way.

[0017] Thickness T of the second foam layer 2b 2b is the thickness T 2a The thickness T 2b is the thickness T 2a It may be the same as or different from. Thickness T 2b is the thickness T 2a It can be calculated in the same way.

[0018] <Foam layer> The foam 1 has a first foam layer 2a and a second foam layer 2b. The first foam layer 2a and the second foam layer 2b are joined by fusion at a joint 3. The first foam layer 2a is a layer (foamed resin layer) formed by foaming a foamable resin composition containing a polystyrene-based resin, and air bubbles are formed in the resin. The resin contained in the foamable resin composition is a polystyrene-based resin. The second foam layer 2b is similar to the first foam layer 2a. Hereinafter, the physical properties of the first foamed layer 2a will be described as the foamed layer of the foam 1. The physical properties of the second foamed layer 2b are similar to those of the first foamed layer 2a, and therefore the description thereof will be omitted.

[0019] The apparent density of the first foamed layer 2a is, for example, 0.04 to 0.15 g / cm 3is preferable, and 0.05 to 0.12 g / cm 3 More preferably, 0.06 to 0.10 g / cm 3 It is more preferable that the apparent density of the first foamed layer 2a is equal to or higher than the above lower limit, the bending strength of the foam 1 can be further increased. If the apparent density of the first foamed layer 2a is equal to or lower than the above upper limit, the foam 1 can be made lightweight and easy to manufacture. The apparent density of the first foamed layer 2a is determined by measurement in accordance with JIS K7222:2005 "Foamed plastics and rubber - Determination of apparent density". Specifically, the mass and apparent volume of a test piece of the first foamed layer 2a cut without changing the original cell structure are measured, and the mass and apparent volume are calculated according to the following formula (1). Apparent density (g / cm 3 ) of the first foam layer 2a 3 ) = mass of test piece (g) / apparent volume of test piece (cm 3 ) · · · (1)

[0020] The basis weight of the first foam layer 2a is, for example, 50 to 600 g / m 2 is preferable, and 90 to 500 g / m 2 More preferably, 150 to 400 g / m 2 It is more preferable that the first foamed layer 2a has a basis weight of not less than the above lower limit, thereby further increasing the bending strength of the foam 1. The first foamed layer 2a has a basis weight of not more than the above upper limit, thereby making the foam 1 lightweight and easy to manufacture. The basis weight of the first foamed layer 2a can be measured by the following method.

[0021] Excluding 20 mm from both ends of the width direction (TD direction) of the first foamed layer 2a, ten pieces of 10 cm x 10 cm are cut out at equal intervals in the width direction, and the mass (g) of each piece is measured to the nearest 0.001 g. The average value of the mass (g) of each piece is calculated by dividing the mass (g) by the mass (g) of the first foamed layer 2a by 1 m. 2 The value converted into the mass per unit area was used as the basis weight (g / m) of the first foamed layer 2a. 2 )

[0022] The expansion ratio of the first foamed layer 2a is, for example, preferably 1.5 to 20 times, more preferably 2 to 15 times, and further preferably 3 to 10 times. When the expansion ratio of the first foamed layer 2a is equal to or higher than the above lower limit, the impact resistance of the foam 1 can be further improved. When the expansion ratio of the first foamed layer 2a is equal to or lower than the above upper limit, the surface properties of the foam 1 can be further improved. The expansion ratio of the first foamed layer 2a is calculated by dividing 1 by the apparent density (g / cm 3 )"

[0023] The average bubble diameter of the first foamed layer 2a is, for example, preferably 80 to 450 μm, more preferably 150 to 400 μm, and even more preferably 200 to 350 μm. When the average bubble diameter of the first foamed layer 2a is equal to or more than the above lower limit, the impact resistance of the foam 1 can be further improved. When the average bubble diameter of the first foamed layer 2a is equal to or less than the above upper limit, the surface properties of the foam 1 can be further improved. The average cell diameter of the first foamed layer 2a can be measured in accordance with the method described in ASTM D2842-69.

[0024] The closed cell ratio of the first foamed layer 2a is preferably 70% or more, more preferably 80% or more, even more preferably 90% or more, and may be 100%. The closed cell ratio of the first foamed layer 2a can be measured in accordance with the method described in JIS K7138:2006 "Rigid foamed plastics - Determination of open cell ratio and closed cell ratio".

[0025] <Polystyrene resin> The first foam layer 2a contains a polystyrene resin. Examples of polystyrene-based resins include homopolymers of styrene-based monomers such as styrene, α-methylstyrene, vinyltoluene, chlorostyrene, ethylstyrene, i-propylstyrene, dimethylstyrene, and bromostyrene, or copolymers thereof; copolymers of styrene-based monomers and vinyl monomers polymerizable therewith, with a styrene-based monomer as the main component; copolymers of styrene-based monomers and rubber components such as butadiene, homopolymers of styrene-based monomers or copolymers thereof, or mixtures or polymers of copolymers of styrene-based monomers and vinyl monomers and diene-based rubber-like polymers, which are so-called high impact polystyrenes; and the like.

[0026] Examples of vinyl monomers polymerizable with styrene-based monomers include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and cetyl (meth)acrylate, and bifunctional monomers such as (meth)acrylonitrile, dimethyl maleate, dimethyl fumarate, diethyl fumarate, ethyl fumarate, divinylbenzene, and alkylene glycol dimethacrylate. These vinyl monomers may be used alone or in combination of two or more. Here, "(meth)acrylate" refers to either or both of "acrylate" and "methacrylate", and "(meth)acrylonitrile" refers to either or both of "acrylonitrile" and "methacrylonitrile".

[0027] Examples of diene rubber polymers include polybutadiene, styrene-butadiene copolymers, and ethylene-propylene-non-conjugated diene three-dimensional copolymers. These polystyrene resins may be used alone or in combination of two or more. In this specification, the polystyrene resin refers to a resin containing 50 mol % or more of units derived from a styrene monomer.

[0028] When the polystyrene resin contains a styrene-butadiene copolymer, the content of the styrene-butadiene copolymer is preferably 10 to 65 mass%, more preferably 15 to 55 mass%, and even more preferably 20 to 45 mass%, based on the total mass of the polystyrene resin. When the content of the styrene-butadiene copolymer is equal to or more than the above lower limit, the surface properties of the foam 1 can be further improved. When the content of the styrene-butadiene copolymer is equal to or less than the above upper limit, the bending strength of the foam 1 can be further increased, and warping can be suppressed.

[0029] The polystyrene resin may be a polystyrene resin not derived from a recycled product, such as general-purpose polystyrene resin (GPPS), a commercially available polystyrene resin, a polystyrene resin newly prepared by a method such as suspension polymerization, etc. From the viewpoint of further reducing the environmental load, the polystyrene resin is preferably a polystyrene resin derived from a recycled product. Examples of polystyrene resins derived from recycled products include those obtained by recovering used polystyrene resin foam molded products, such as fish boxes, cushioning materials for home appliances, food packaging trays, etc., and regenerating them by a limonene dissolution method or a heat volume reduction method. Examples of polystyrene resins derived from recycled products include those obtained by crushing scraps generated after punching food packaging trays, etc., from a polystyrene resin foam sheet, melt-kneading them, and repelletizing them. Examples of polystyrene-based resins derived from recycled products that can be used include those obtained by recycling molded bodies such as used foamed containers, as well as non-foamed polystyrene-based resins separated and recovered from home appliances (e.g., televisions, refrigerators, washing machines, air conditioners, etc.), office equipment (e.g., copiers, facsimiles, printers, etc.), etc.

[0030] The Z-average molecular weight (Mz) of the polystyrene resin is 300,000 to 650,000, preferably 300,000 to 550,000, and more preferably 350,000 to 450,000. When the Mz of the polystyrene resin is equal to or more than the above lower limit, the bending strength of the foam 1 can be further increased. When the Mz of the polystyrene resin is equal to or less than the above upper limit, the surface properties of the foam 1 can be further increased. The Mz of the polystyrene resin can be determined by the measurement method described in the Examples.

[0031] The mass average molecular weight (Mw) of the polystyrene resin is preferably 190,000 to 260,000, more preferably 200,000 to 250,000, and even more preferably 210,000 to 250,000. When the Mw of the polystyrene resin is equal to or greater than the above lower limit, the flexural strength of the foam 1 can be further increased. When the Mw of the polystyrene resin is equal to or less than the above upper limit, the surface properties of the foam 1 can be further increased. The Mw of the polystyrene resin is determined by the same measurement method as that for the Mz of the polystyrene resin.

[0032] The number average molecular weight (Mn) of the polystyrene resin is preferably 75,000 to 110,000, more preferably 85,000 to 110,000, and even more preferably 95,000 to 105,000. When the Mn of the polystyrene resin is equal to or more than the above lower limit, the bending strength of the foam 1 can be further increased. When the Mn of the polystyrene resin is equal to or less than the above upper limit, the surface properties of the foam 1 can be further increased. The Mn of the polystyrene resin is determined by the same measurement method as that for the Mz of the polystyrene resin.

[0033] The molecular weight distribution (Mz / Mw) obtained by dividing the Mz of the polystyrene resin by the Mw of the polystyrene resin is preferably 1.6 to 2.2, more preferably 1.7 to 2.1, and even more preferably 1.8 to 2.0. When the Mz / Mw of the polystyrene resin is equal to or greater than the lower limit, the bending strength of the foam 1 can be further increased. When the Mz / Mw of the polystyrene resin is equal to or less than the upper limit, the occurrence of die swell (a phenomenon in which a resin composition expands during extrusion molding, causing the cross-sectional area of ​​the extrudate to be larger than the cross-sectional area of ​​the die nozzle) can be suppressed, and surface properties can be further improved.

[0034] The value (Mw / Mn) obtained by dividing the Mw of the polystyrene resin by the Mn of the polystyrene resin is preferably 2.2 to 3.0, more preferably 2.3 to 2.8, and even more preferably 2.4 to 2.6. When the Mw / Mn of the polystyrene resin is equal to or more than the above lower limit, the flexural strength of the foam 1 can be further increased. When the Mw / Mn of the polystyrene resin is equal to or less than the above upper limit, the surface properties can be further improved.

[0035] The melt flow rate (MFR) of the polystyrene resin is preferably 1.0 to 10.0 g / 10 min, more preferably 2.5 to 9.0 g / 10 min, further preferably 3.5 to 8.5 g / 10 min, and particularly preferably 4.0 to 7.9 g / 10 min. When the MFR of the polystyrene resin is equal to or higher than the lower limit, the surface properties of the foam 1 can be further improved. When the MFR of the polystyrene resin is equal to or lower than the upper limit, the bending strength can be further improved. In this specification, the MFR of a polystyrene resin refers to a value measured by the following method.

[0036] <Melt flow rate (MFR) measurement method> (Pretreatment) The foam 1 is heat pressed at 180° C. for 5 minutes and degassed. The degassed foam is cut into small pieces to prepare a sample for MFR measurement. (Measurement conditions) The MFR is measured using a "Melt Flow Index Tester 120-SAS" manufactured by Yasuda Seiki Seisakusho Co., Ltd., in accordance with "b) Method for measuring the time it takes for the piston to move a specified distance" of Method B described in JIS K7210:1999 "Test methods for melt mass flow rate (MFR) and melt volume flow rate (MVR) of plastics - thermoplastics". The measurement conditions are as follows: sample approximately 3 to 8 g, preheating time 5 minutes, test temperature 200°C, test load 49.03 N, piston movement distance (interval): 25 mm. The sample is tested three times, and the average is the MFR (g / 10 min) value.

[0037] In this specification, the styrene component means a styrene monomer obtained when the foam layer is heated and decomposed. In this specification, the butadiene component means butadiene monomer and 4-vinyl-1-cyclohexene monomer obtained when the foam layer is heated and decomposed. The butadiene component is derived from a styrene-butadiene copolymer contained in a polystyrene-based resin.

[0038] The content of the butadiene component in the polystyrene resin is 0.4 to 4.0 mass%, preferably 0.6 to 3.5 mass%, more preferably 1.0 to 3.0 mass%, and even more preferably 1.5 to 2.5 mass%, based on the total mass of the foam layer. When the content of the butadiene component is equal to or more than the lower limit, the surface properties of the foam 1 can be further improved. When the content of the butadiene component is equal to or less than the upper limit, the bending strength of the foam 1 can be further improved, and warping can be suppressed. The butadiene content in the polystyrene resin is determined by the following method.

[0039] <Method for measuring butadiene content> The first foamed layer 2a is cut into a slice using a slicer or a razor from the foam 1, and about 0.1 to 0.5 mg of the sample is precisely weighed. The sample is wrapped in a ferromagnetic metal body "Pyrofoil" manufactured by Japan Analytical Industry Co., Ltd., which has a Curie point of 590°C, to prepare a test specimen. The test specimen is prepared so that the ferromagnetic metal body is pressed against the sample, and the test specimen is heated using a Curie point pyrolyzer "JPS-700" manufactured by Japan Analytical Industry Co., Ltd., to decompose the sample.

[0040] The butadiene monomer and 4-vinyl-1-cyclohexene monomer produced by decomposition are measured using an Agilent Technologies GC7820A gas chromatograph (detector = FID) to determine the total peak area of ​​butadiene monomer and 4-vinyl-1-cyclohexene monomer. The total of butadiene monomer and 4-vinyl-1-cyclohexene monomer is regarded as the butadiene component. The proportion of butadiene component contained in the sample is calculated from a calibration curve prepared in advance. The standard sample used to prepare the calibration curve is St / BD=85 / 15 (CAT#07073) resin manufactured by POLYSCIENCES.INC. The measurement conditions for gas chromatography (GC) are as follows:

[0041] (Pyrolysis conditions) Heating: 590℃ for 5 seconds. Oven temperature: 300℃ Needle temperature: 300℃. (GC measurement conditions) Apparatus: Gas chromatograph "GC7820A" manufactured by Agilent Technologies, Inc. Column: Agilent Technologies "DB-5" (film thickness 0.25 μm x inner diameter 0.25 mm x length 30 m).

[0042] (GC oven heating conditions) Initial temperature: 50°C (hold for 0.5 minutes). -First stage heating rate: 10℃ / min (up to 200℃, holding time 0 minutes). - Second stage heating rate: 20℃ / min (up to 320℃). Final temperature: 320°C (hold for 0.5 minutes). Carrier gas: He gas. ·He flow rate: 63.736mL / min. Inlet pressure: 100kPa. ·Column inlet pressure: 100kPa. ·Inlet temperature: 300℃. ·Detector temperature: 300℃. Split ratio: 1 / 50

[0043] The content of the styrene component in the polystyrene resin is preferably 95 to 99.6 mass%, more preferably 94 to 99.6 mass%, and even more preferably 95 to 99 mass%, based on the total mass of the foam layer. When the content of the styrene component is equal to or more than the lower limit, the bending strength of the foam 1 can be further increased and warping can be suppressed. When the content of the styrene component is equal to or less than the upper limit, the surface properties of the foam 1 can be further improved. The content of the styrene component in the polystyrene-based resin is determined by the following method.

[0044] <Method for measuring styrene component content> As in the method for measuring the butadiene content, the sample is precisely weighed to prepare a test specimen. As in the method for measuring the butadiene content, the test specimen is heated to decompose the sample. The styrene monomer generated by decomposition is measured using an Agilent Technologies GC7820A gas chromatograph (detector = FID) to determine the peak area of ​​the styrene monomer. The percentage of styrene contained in the sample is calculated from the peak area of ​​the styrene monomer using a calibration curve that was prepared in advance. Suspension polymerization PS microparticles manufactured by Sekisui Plastics Co., Ltd. are used as the standard sample for creating the calibration curve. The measurement conditions for the gas chromatograph (GC) are the same as those for the method for measuring the content of butadiene components.

[0045] The foamable resin composition contains a foaming agent. Examples of the blowing agent include hydrocarbons such as propane, butane, and pentane; halogenated hydrocarbons such as tetrafluoroethane, chlorodifluoroethane, and difluoroethane; and among these, hydrocarbons are preferred, and butane is preferred. As butane, normal butane or isobutane may be used alone, or normal butane and isobutane may be used in any ratio. These blowing agents may be used alone or in combination of two or more.

[0046] The content of the foaming agent in the foamable resin composition is, for example, preferably 0.1 to 10 parts by mass, more preferably 1 to 7 parts by mass, and even more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the polystyrene resin.

[0047] The foamable resin composition may contain components other than the polystyrene resin and the foaming agent (hereinafter, also referred to as "optional components"). Examples of the optional components include a cell regulator, a stabilizer, an ultraviolet absorber, an antioxidant, a colorant, a deodorant, a lubricant, a flame retardant, and an antistatic agent. The type of optional component is determined taking into consideration the physical properties required for the foam 1, etc. The optional components may be used alone or in combination of two or more.

[0048] Examples of the cell regulator include mixtures of inorganic powders such as talc and silica. These cell regulators increase the closed cell ratio of the foam 1, making it easier to form the foam layer 5. Examples of the stabilizer include calcium zinc-based heat stabilizers, tin-based heat stabilizers, and lead-based heat stabilizers. Examples of the ultraviolet ray absorbent include cesium oxide-based ultraviolet ray absorbents and titanium oxide-based ultraviolet ray absorbents. Examples of the antioxidant include cerium oxide, cerium oxide / zirconia solid solution, cerium hydroxide, carbon, carbon nanotubes, titanium oxide, and fullerene. Examples of colorants include titanium oxide, carbon black, titanium yellow, iron oxide, ultramarine, cobalt blue, calcined pigments, metallic pigments, mica, pearl pigments, zinc oxide, precipitated silica, and cadmium red. Examples of deodorants include silica, zeolite, zirconium phosphate, and calcined hydrotalcite.

[0049] The content of the optional component in the foamable resin composition is, for example, preferably 0.05 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.3 to 5.0 parts by mass, relative to 100 parts by mass of the polystyrene resin. When the content of the optional component is equal to or more than the lower limit, the effects derived from the optional component can be exhibited. When the content of the optional component is equal to or less than the upper limit, clogging of the die or the like can be more effectively prevented, and the appearance of the foam 1 can be more improved.

[0050] The polystyrene-based resin foam of the present invention is not limited to the present embodiment shown in FIG. 1, and various changes and modifications are possible. For example, the foam 1 is formed by fusion-bonding a first foam layer 2a and a second foam layer 2b, but the polystyrene-based resin foam may be formed of a single foam layer, or may be formed of three or more foam layers. By using two or more foam layers, the thickness of the polystyrene foam increases and the strength of the foam board increases, making it suitable for use as an exhibition panel to which posters can be attached.

[0051] The foam 1 is composed of only a foam layer and does not have a non-foamed resin layer, but a non-foamed resin layer may be provided on one or both sides of the foam layer. When the foam has a non-foamed resin layer, the bending strength can be further increased. The resin constituting the non-foamed resin layer is not particularly limited, and may be the same resin as the resin constituting the first foamed layer 2a. The resin constituting the non-foamed resin layer may be the same as or different from the resin constituting the first foamed layer 2a.

[0052] The thickness of the non-foamed resin layer is, for example, preferably 10 to 300 μm, more preferably 20 to 200 μm. When the thickness of the non-foamed resin layer is equal to or more than the above lower limit, the flexural strength of the foam can be further increased. When the thickness of the non-foamed resin layer is equal to or less than the above upper limit, the weight of the foam can be reduced.

[0053] When the foam has a non-foamed resin layer, the non-foamed resin layer may be laminated directly onto the surface of the foam by heat fusion or the like, or may be laminated via an adhesive. The adhesive may be an oil-based adhesive using an organic solvent as the main solvent, an aqueous adhesive using water as the main solvent, or a heat-fusible adhesive (hot melt adhesive) using a heat-melting resin. As the aqueous adhesive, for example, emulsion-based aqueous adhesives such as starch, modified starch, casein, carboxymethyl cellulose, hydroxycellulose, soy protein, polyvinyl acetate, ethylene-vinyl acetate-acrylic copolymer, ethylene-vinyl acetate copolymer, and acrylic-modified vinyl acetate copolymer can be applied. As the hot melt adhesive, for example, synthetic rubber-based hot melt adhesives, polyolefin-based hot melt adhesives, polyester-based hot melt adhesives, etc. can be mentioned.

[0054] The foam 1 of the present embodiment has a butadiene component content of 0.4 to 4.0 mass % relative to the total mass of the foam layer, and the Mz of the polystyrene resin is 300,000 to 650,000, and therefore has excellent bending strength, little warping, and excellent surface properties.

[0055] [Method of manufacturing polystyrene foam] The method for producing the foam 1 includes the steps of melting a polystyrene resin, kneading the molten polystyrene resin with a foaming agent to obtain a molten mixture, and extruding and foaming the molten mixture to obtain a foam layer. As a suitable method for producing the foam 1, a known method for producing a foam can be adopted, and for example, the following production method can be mentioned. An example of a method for producing the foam 1 will be described below using a foam production apparatus 100 shown in FIG.

[0056] The foam manufacturing apparatus 100 in Fig. 2 is an apparatus for obtaining a foam by extrusion molding. The manufacturing apparatus 100 includes an extruder 10, a foaming agent supply source 18, a circular die 20 attached to the tip of the extruder 10, a guide roller 24 that sends the tubular foam 2 extruded and foamed from the discharge port of the circular die 20 to a pinch roll 30, and the pinch roll 30 that presses the tubular foam 2 into a plate shape.

[0057] The extruder 10 is a so-called single-type extruder. The extruder 10 includes a hopper 14. A foaming agent supply source 18 is connected to the extruder 10.

[0058] The extruder 10 of the production apparatus 100 may be an extruder other than a single extruder. For example, the extruder 10 may be a so-called tandem extruder (FIG. 3). The tandem extruder includes a first extrusion section 11 and a second extrusion section 12 connected to the first extrusion section 11 by a pipe 16. The first extrusion section 11 includes a hopper 14. A foaming agent supply source 18 is connected to the first extrusion section 11. A circular die 20 is connected to the second extrusion section 12. Provided downstream of the circular die 20 are a guide roller 24 that sends the cylindrical foam 2 extruded and foamed from the discharge port of the circular die 20 to the pinch roll 30, and the pinch roll 30 that presses the cylindrical foam 2 into a plate shape. Moreover, the extruder 10 of the production apparatus 100 may be a single screw extruder or a multi-screw extruder such as a twin screw extruder.

[0059] The raw material constituting the foam layer is fed from a hopper 14 into the extruder 10. The raw material fed from the hopper 14 includes the resin constituting the foam layer and any optional components that are blended as necessary. In the extruder 10, the raw materials are mixed while being heated to a given temperature to form a resin melt, and a foaming agent is supplied to the extruder 10 from a foaming agent supply source 18, and the foaming agent is mixed with the resin melt to form a foamable resin composition. The heating temperature is appropriately determined in consideration of the type of resin, etc., so long as the resin melts and the optional components are not denatured.

[0060] The heating temperature may be any temperature at which styrene softens, and is, for example, preferably 100 to 180° C., more preferably 110 to 170° C., and even more preferably 120 to 160° C. When the heating temperature is equal to or higher than the lower limit, the cylindrical foam 2 is sufficiently softened, and the first foamed layer 2a and the second foamed layer 2b can be neatly fusion-bonded. When the heating temperature is equal to or lower than the upper limit, the outer surface of the cylindrical foam 2 can be prevented from being excessively softened, and the surface properties can be further improved.

[0061] The foamable resin composition is heated and extruded from the discharge opening of a circular die 20 attached to the tip of the extruder 10, and is foamed at the same time. At this time, the discharge opening of the circular die 20 is annular, and a cylindrical foam 2 is formed. The cylindrical foam 2 is cooled by air 26 sent from an air ring device (not shown) provided downstream of the circular die 20, and is sent to a pinch roll 30 by a guide roller 24.

[0062] Before the inside of the cylindrical foam 2 cools completely, the cylindrical foam 2 is pressed from above and below with a pair of pinch rolls 30 to be heat-sealed, thereby forming a foam 1 in which two foam layers are fused together.

[0063] The pressure when the cylindrical foam 2 is squeezed by the pinch roll 30 is preferably 0.1 to 1.1 MPa, more preferably 0.2 to 1.0 MPa, and even more preferably 0.3 to 0.9 MPa. When the pressure when the cylindrical foam 2 is squeezed by the pinch roll 30 is equal to or higher than the above lower limit, the first foamed layer 2a and the second foamed layer 2b can be sufficiently bonded. When the pressure when the cylindrical foam 2 is squeezed by the pinch roll 30 is equal to or lower than the above upper limit, the first foamed layer 2a and the second foamed layer 2b are not excessively crushed, and the surface properties can be further improved.

[0064] The foam 1 may then be cut to a desired size and its surface may be printed. The foam 1 may also be provided with a non-foamed resin layer.

[0065] Examples of methods for providing a non-foamed resin layer on a foamed body include the following methods (1) to (4). (1) A method in which the resin that will become the non-foamed resin layer is fed into an extruder, and the molten resin for forming the non-foamed resin layer is extruded onto a foam from a T-die attached to the tip of the extruder. (2) A method in which a co-extrusion device equipped with two extruders is used, and foaming-extrusion of a foam is performed with one extruder, while a resin for forming a non-foamed resin layer is co-extruded from the other extruder. (3) A method of laminating a resin film that will become a non-foamed resin layer on the surface of a foam by heat and pressure bonding. (4) A method in which a resin film that will become a non-foamed resin layer is adhered to the surface of a foam using an adhesive. When a polystyrene resin is used as the non-foamed resin layer, the above methods (1) to (3) for forming the non-foamed resin layer on the surface of the foam without using an adhesive are preferred.

[0066] In the method for producing a foam according to the present embodiment, the residual stress of the foam layer can be reduced by heating both sides of the foam layer and stacking multiple sheets of the foam layer under pressure. This reduces the warping of the foam and improves the surface properties. In addition, because the foam is less warped, it is possible to suppress paper lifting after lamination. In particular, the effect of the present invention is remarkable in that warping and dimensional changes can be suppressed in high temperature environments such as during transportation and storage in summer.

[0067] An example of ripples formed on the surface of a polystyrene-based resin foam will be described with reference to FIG. As shown in FIG. 4, ripples are formed on the surface of the foam 4 over the entire area indicated by A. 4, X indicates the width direction (TD direction) of the resin, and Y indicates the extrusion direction (MD direction) of the resin. The TD direction is a direction perpendicular to the MD direction.

[0068] In the region indicated by A, ripples are formed along the TD direction. Unlike surface irregularities, the ripples are considered to be caused by a phenomenon called die swelling, in which the foamable resin composition expands during extrusion molding and the cross-sectional area of ​​the extrudate becomes larger than the cross-sectional area of ​​the die nozzle. When die swelling occurs, the shrinkage variation when the foamable resin composition cools increases. It is considered that the ripples are formed due to this shrinkage variation. As shown in FIG. 4, the ripples tend to be formed along the TD direction. However, the ripples may also be formed along the MD direction. The ripples may also be formed along directions other than the TD and MD directions, and may also be formed on a part of the surface of the foam.

[0069] In order to suppress the formation of ripples, it is considered effective to suppress the occurrence of die swell. The foam of the present invention has a butadiene content of 0.4 to 4.0% by mass relative to the total mass of the foam layer, and the polystyrene resin has an Mz of 300,000 to 650,000, so that the occurrence of die swelling can be suppressed. Therefore, the foam of the present invention has excellent surface properties.

[0070] [Exhibition panel] The display panel of the present invention is prepared by cutting the foam 1 of the present invention produced by the above-mentioned manufacturing method to the desired dimensions as necessary to form a panel body, and providing a skin material on both or one of the surfaces of the panel body. If a skin material is provided on the surface of the foam 1, the bending strength can be further increased, and the surface properties can be further improved. Examples of the skin material include fine paper, glassine paper, parchment paper, craft paper, synthetic paper, release paper, tack paper, etc. One type of skin material may be used alone, or two or more types may be used in combination.

[0071] The method for providing the surface material on the surface of the foam 1 is not particularly limited. For example, the surface material may be provided using the above-mentioned adhesive, or may be provided using a thumb tack or adhesive tape. In order to make the appearance of the display panel beautiful, it is preferable that the skin material be provided using the above-mentioned adhesive.

[0072] The display panel may further include a printed layer on the surface of the covering material. The method for providing the printed layer is not particularly limited, but it is preferable to use inkjet printing. Both UV inks and water-based inks can be used as inks for inkjet printing. These inks can be appropriately selected from various inks for inkjet printing that are commercially available. In addition, it is preferable that the inkjet printer is equipped with a UV light source for irradiating ultraviolet rays immediately after printing, a heater or dryer for drying, and the like, depending on the curing characteristics of the ink used.

[0073] As described above, the exhibition panel of the present invention uses foam 1, which has little warping and excellent surface properties, as the panel body, and therefore can be used as an exhibition panel on which extremely clear and beautiful printing can be performed. EXAMPLES

[0074] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the following description.

[0075] First, the polystyrene resins shown in Table 1 were prepared as the polystyrene resin foam.

[0076] [Table 1]

[0077] The raw materials shown in Table 1 are as follows: HIPS: Product name "E-641N", high impact polystyrene, manufactured by Toyo Styrene Co., Ltd. · GPPS: Product name "G0002", general-purpose polystyrene, manufactured by PS Japan Co., Ltd. · GPPS: Product name "HRM48N", general-purpose polystyrene, manufactured by Toyo Styrene Co., Ltd. · GPPS: Product name "HRM10N", general-purpose polystyrene, manufactured by Toyo Styrene Co., Ltd. HIPS, GPPS mixture: PS1, a mixture of high impact polystyrene and general-purpose polystyrene, repelletized waste material of the foam obtained in Example 4. HIPS, GPPS mixture: PS2, a mixture of high impact polystyrene and general-purpose polystyrene, a repellet product of the waste material of the foam obtained in Example 5.

[0078] [Example 1] <Production of polystyrene-based resin foam> An extruder having an inner diameter of 115 mm and an extruder having an inner diameter of 150 mm connected thereto was prepared. A blended raw material obtained by adding 0.5 parts by mass of talc (manufactured by Kihara Chemical Industries, Ltd.) and 1.2 parts by mass of talc master batch (manufactured by Toyo Styrene Co., Ltd., product name "DSM1401A") to 100 parts by mass of polystyrene resin (manufactured by PS Japan Co., Ltd., product name "G0002" 90 parts by mass and manufactured by Toyo Styrene Co., Ltd., product name "E-641N" 10 parts by mass) was put into the extruder. The blended raw material was melted at a maximum temperature of 230°C in the extruder, kneaded, and then 4.0 parts by mass of butane (isobutane / normal butane mass ratio: 68% / 32%) was added as a foaming agent and mixed with the resin to obtain a foamable resin composition (molten resin). The molten resin was cooled to a resin temperature (148°C) suitable for foaming. The molten resin was then extruded into the atmosphere through a circular die with a 160mm diameter and 1.0mm slit clearance, which was attached to the tip of the extruder, to foam the resin. Cooled air (40°C) was blown onto the outer surface of the extruded cylindrical foam, and the foam was cooled while being pressed from above and below with a crocodile-jaw roll to fuse the two layers together. After cooling, the foam was cut into a thickness of 5 mm, length of 935 mm, width of 630 mm, and basis weight of 320 g / m. 2 Thus, a plate-shaped polystyrene resin foam (foam plate) was obtained.

[0079] [Examples 2 to 16, Comparative Examples 1 to 3] A foam board was obtained in the same manner as in Example 1, except that the polystyrene resin was blended as shown in Tables 2 and 3. In the tables, "-" indicates that the component was not blended.

[0080] The butadiene component content and styrene component content of the foam board of each example were measured according to the above <Method of measuring butadiene component content> and <Method of measuring styrene component content>. The thickness, apparent density, molecular weight and MFR of each foam board were measured by the following methods. The results are shown in Tables 2 and 3.

[0081] <Thickness measurement> The thickness of the resulting foamed board was measured using a thickness measuring device SM-114 (manufactured by TECLOCK).

[0082] <Measurement of apparent density> The apparent density (g / cm 3 ) is calculated by measuring its mass and apparent volume and dividing it by mass (g) / apparent volume (cm 3 ) was calculated.

[0083] <Molecular weight measurement> The method for measuring the Z-average molecular weight Mz of the polystyrene resin in the foamed board obtained in each example is described below. The mass average molecular weight Mw of the polystyrene resin and the number average molecular weight Mn of the polystyrene resin were measured in the same manner as the Z-average molecular weight Mz of the polystyrene resin.

[0084] The foamed board obtained in each example was cut with a slicer or a razor to be collected as a sample. The sample was pretreated to obtain a filtrate under the following measurement conditions, and the Z-average molecular weight Mz of the polystyrene resin was measured.

[0085] <Measurement conditions> (Pretreatment) 6 mg of the collected sample was dissolved in 6 mL of tetrahydrofuran (THF) (immersion time: 6±1 hr (complete dissolution)) to obtain a sample solution. The sample solution was filtered using a non-aqueous 0.45 μm syringe filter manufactured by Shimadzu GLC Co., Ltd. to obtain a filtrate.

[0086] The filtrate obtained in the above pretreatment was used to measure the Z-average molecular weight Mz of the polystyrene resin with the following measuring device under the following measuring conditions. (Measuring Equipment) GPC device: Tosoh Corporation, HLC-8320GPC (with built-in RI detector and UV detector). Guard column: TOSOH TSK guard column SuperMP(HZ)-H (4.6mmI.D. x 2cm) x 1. Column (reference): TOSOH TSKgel Super HZ1000 (6.0mm I.D. x 15cm) x 1. Column (sample): Two TSKgel SuperMultipore HZ-H (4.6 mm I.D. × 15 cm) columns in series. (Measurement conditions) Column temperature: 40 °C. Detector temperature: 40 °C. Pump injection section temperature: 40 °C. Solvent: THF. Flow rate (reference): 0.2 mL / min. Flow rate (sample): 0.2 mL / min. Run time: 21 min. Data integration time: 6 - 25 min. Data interval: 200 msec. Injection volume: 20 μL. Detector: RI.

[0087] (Standard polystyrene sample for calibration curve) As the standard polystyrene samples for the calibration curve, those with weight-average molecular weights Mw of 5,620,000, 3,120,000, 1,250,000, 442,000, 151,000, 53,500, 17,000, 7,660, 2,900, and 1,320 from the product names "STANDARD SM-105" and "STANDARD SH-75" manufactured by Showa Denko K.K. were used. The above standard polystyrene for the calibration curve was grouped into A (5,620,000, 1,250,000, 151,000, 17,000, 2,900) and B (3,120,000, 442,000, 53,500, 7,660, 1,320). After weighing A (2 mg, 3 mg, 4 mg, 4 mg, 4 mg), it was dissolved in 30 mL of THF. After weighing B (3 mg, 4 mg, 4 mg, 4 mg, 4 mg), it was dissolved in 30 mL of THF. The standard polystyrene calibration curve was obtained by creating a calibration curve (linear equation) from the retention times obtained after injecting 20 μL of each of the prepared A and B solutions for measurement. The Z-average molecular weight Mz was calculated using this calibration curve.

[0088] (Measurement of MFR) (Pretreatment) The foamed plate obtained in each example was defoamed by hot pressing at 180° C. for 5 minutes. The defoamed foamed plate was cut into small pieces to prepare samples for MFR measurement. (Measurement conditions) The MFR was measured using a "Melt Flow Index Tester 120-SAS" manufactured by Yasuda Seiki Seisakusho Co., Ltd., in accordance with "b) Method for measuring the time it takes for the piston to move a specified distance" in Method B described in JIS K7210:1999 "Test methods for melt mass flow rate (MFR) and melt volume flow rate (MVR) of plastics-thermoplastics". The measurement conditions were as follows: sample approximately 3 to 8 g, preheating time 5 minutes, test temperature 200°C, test load 49.03 N, piston movement distance (interval): 25 mm. The test was performed three times for each sample, and the average was taken as the MFR (g / 10 min).

[0089] The foamed boards obtained in each example were evaluated for bending strength, warpage, and surface properties, and an overall evaluation was performed using the following evaluation methods. The results are shown in Tables 2 to 3.

[0090] <Bending strength evaluation> The bending strength was measured using a Tensilon universal testing machine "RTC-1310A" manufactured by Orientec Co., Ltd. The test pieces were cut to a size of 50 mm wide x 150 mm long x thickness (thickness of each example) in the extrusion direction (MD direction) and the direction perpendicular to the extrusion direction (TD direction). The number of test pieces was three for each direction. The measurement conditions were a test speed of 50 mm / min, a radius of the tip of the pressure wedge and the fulcrum of 3.2R, and a distance between the fulcrums of 100 mm. Three-point bending measurement was performed for each test piece, and the maximum point load was taken as the bending strength (N) of the foam board. Next, the average value (N) of the bending strength (N) in the MD direction and the bending strength (N) in the TD direction was used to make a judgment based on the following evaluation criteria. Evaluation Criteria A: The average bending strength is 13N or more...The bending strength is extremely high and excellent. B: The average bending strength is 12 N or more and less than 13 N...The bending strength is sufficiently high and good. C: The average bending strength is 10 N or more but less than 12 N...The bending strength is low, but acceptable. D: The average bending strength is less than 10 N...The bending strength is extremely low and poor.

[0091] <Evaluation of the amount of warpage> The foam plate was left to stand for 24 hours in an environment of 23° C. and a relative humidity of 50% RH, and the amount of warping was measured by the following measurement method. Two opposing vertical sides (long sides) of a rectangular foam board in plan view, 935 mm vertical (MD, long side) and 630 mm horizontal (TD, short side), were placed against a horizontal surface to measure the maximum lifting distance from the horizontal surface (distance (mm) from the horizontal surface to the bottom surface of the foam board), and this measurement was taken as the amount of warping (mm) in the TD direction (short side). Next, two opposing horizontal sides (short sides) of the foam board were placed against a horizontal surface to measure the maximum lifting distance from the horizontal surface (distance (mm) from the horizontal surface to the bottom surface of the foam board), and this measurement was taken as the amount of warping (mm) in the MD direction (long side). Next, the warpage (mm) in the TD direction (short side) and the average warpage (mm) in the MD direction (long side) were used to make a judgment based on the following evaluation criteria. Evaluation Criteria A: The average amount of warping is less than 5 mm...The amount of warping is extremely small and excellent. B: The average amount of warping is 5 mm or more and less than 7 mm...The amount of warping is sufficiently small and good. C: The average amount of warping is 7 mm or more and less than 10 mm...The amount of warping is small and acceptable. D: The average amount of warping is 10 mm or more. The amount of warping is large and poor.

[0092] <Evaluation of surface properties> The surface of the obtained foamed board was visually observed and the surface properties were evaluated based on the following evaluation criteria. Evaluation Criteria A: No ripples are observed. B: Ripples are barely noticeable. C: Ripples slightly mar the appearance, but are acceptable. D: Ripples clearly mar the appearance and it is poor.

[0093] <Overall rating> From the results of the above <Evaluation of bending strength>, <Evaluation of warpage> and <Evaluation of surface properties>, a comprehensive evaluation was made according to the following evaluation criteria. Evaluation Criteria S: All ratings are "A". A: All ratings are either "A" or "B", with one "B" rating. B: No "C" or "D" grades, two or more "B" grades, or no "D" grades and one "C" grade. C: No "D" grades and two or more "C" grades. D: One or more "D" ratings.

[0094] [Table 2]

[0095] [Table 3]

[0096] As shown in Tables 2 and 3, Examples 1 to 16 in which the present invention was applied were given an overall evaluation of "S" to "C." In contrast, Comparative Example 1, in which the butadiene component content is outside the range of the present invention, was rated as "D" for surface properties and as a comprehensive evaluation of "D." Comparative Example 2, in which the butadiene component content is outside the range of the present invention, was rated as "D" for warpage and as a comprehensive evaluation of "D." Comparative Example 3, which does not contain a butadiene component and in which the butadiene component content is outside the range of the present invention, was rated as "D" for surface properties and as a comprehensive evaluation of "D."

[0097] FIG. 5 shows a photograph of the surface of the foam board of Example 5. As shown in FIG. 5, no ripples were observed on the surface of the foamed board of Example 5, indicating that the foamed board had excellent surface properties.

[0098] FIG. 6 shows a photograph of the surface of the foam board of Comparative Example 3. As shown in FIG. 6, ripples were clearly observed on the surface of the foamed board of Comparative Example 3, impairing the appearance.

[0099] These results demonstrate that the polystyrene-based resin foam of the present invention has excellent bending strength, little warping, and excellent surface properties. [Explanation of symbols]

[0100] 1. Polystyrene resin foam (foam board) 2a First foam layer 2b Second foam layer 3 Joint

Claims

1. It is in a plate or sheet shape, The foam layer is an extruded foam containing a polystyrene-based resin, The polystyrene resin contains a butadiene component, The content of the butadiene component is 0.4 to 4.0% by mass based on the total mass of the foamed layer, The polystyrene-based resin foam has a Z-average molecular weight (Mz) of 300,000 to 650,000.

2. The polystyrene-based resin foam according to claim 1 , wherein the polystyrene-based resin is a polystyrene-based resin derived from recycled products.

3. 3. An exhibition panel comprising the polystyrene-based resin foam according to claim 1 or 2, and a skin material provided on either or both of its surfaces.

Citation Information

Patent Citations

  • Method for producing foaming particles from recovered styrene-based resin material, foamed particles containing recovered material and foamed molded material

    JP2003213030A

  • Extruded foam of polystyrenic resin

    JP2008214533A

  • Polystyrene resin foam and method for producing the same

    JP2010174193A

  • Cushioning material

    JP2013203985A

  • Heat-resistant styrenic resin composition, extruded sheet, and molding

    JP2014169391A