Oxygen absorbent resin composition and oxygen absorbent film containing the same
The oxygen-absorbing resin composition, using a transition metal catalyst and acid compound, addresses deactivation issues by controlling oxygen absorption through humidity and UV, ensuring stable and efficient oxygen absorption.
Patent Information
- Application Number
- JP2024111638
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2038-05-14
AI Technical Summary
Existing oxygen-absorbing resin materials for packaging start an oxidation reaction immediately when exposed to the atmosphere, leading to deactivation during handling and storage, and their oxygen absorption capacity is not maintained over time.
An oxygen-absorbing resin composition containing a transition metal catalyst and an acid compound with specific functional groups, allowing controlled oxygen absorption by adjusting environmental conditions such as humidity and UV irradiation.
The resin composition maintains oxygen absorption capacity effectively for extended periods by suppressing deactivation and enabling controlled oxygen absorption, even in ambient conditions, with enhanced stability and cost-effectiveness.
Smart Images

Figure 2024138446000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an oxygen-absorbing resin composition in which the oxygen-absorbing reaction can be controlled by controlling the temperature, humidity, etc., and an oxygen-absorbing film containing the same. [Background technology]
[0002] Various oxygen-absorbing resin materials have been proposed for use as packaging materials for beverages, foods, and medicines (for example, Patent Document 1). Furthermore, an oxygen-absorbing adhesive resin composition using such an oxygen-absorbing resin material has been proposed (Patent Document 2). However, when such oxygen-absorbing packaging materials using oxygen-absorbing resins are exposed to the atmosphere, they immediately start an oxidation reaction, which makes them difficult to handle during film production and bag making processes, and there are problems with the film being deactivated depending on the exposure time. For example, when oxygen-absorbing packaging materials using oxygen-absorbing resins are stored for a long period of time, they may not be able to exhibit the desired oxygen absorption ability when used. For example, in Patent Document 3, the incorporation of an antioxidant into an oxygen-absorbing resin layer is considered in order to suppress deactivation during handling and improve oxygen absorption capacity, and an appropriate amount of antioxidant increases the amount of oxygen absorbed by the packaging material and suppresses discoloration of the packaging material. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 4978884 [Patent Document 2] Patent No. 5671802 [Patent Document 3] Patent No. 5862988 [Patent Document 4] Patent No. 4863042 Summary of the Invention [Problem to be solved by the invention]
[0004] As described above, attention has been focused on the oxygen absorbing ability of the oxygen absorbing resin, and methods for controlling the oxygen absorbing reaction itself have also been investigated. For example, Patent Document 4 considers a method of irradiating a laminate containing an oxygen-absorbing resin with ultraviolet light in a specific wavelength range to induce an oxygen absorption reaction. However, this method requires special processes such as irradiation equipment, and therefore has problems such as high manufacturing costs and poor productivity. The present invention aims to provide an oxygen-absorbing resin composition that is suppressed from being deactivated during handling, can be stably used even in the atmosphere, and can easily control the oxygen absorption reaction, and an oxygen-absorbing film containing the same. [Means for solving the problem]
[0005] The present inventors focused on developing an oxygen absorbing resin having an oxygen absorption trigger, which does not start the oxygen absorbing reaction until the oxygen absorbing ability is required, and an oxygen absorbing film containing the same, and which can easily start the oxygen absorbing reaction at any timing. As a result of intensive research, the present inventors discovered that the oxygen absorbing ability of the oxygen absorbing resin can be controlled in conjunction with the control of external environmental conditions such as humidity by adding a transition metal catalyst and an acid compound such as a specific organic acid or inorganic acid to the oxygen absorbing resin, and thus completed the present invention. That is, the present invention is configured as follows: [1] to [7]. [1] An oxygen-absorbing resin composition comprising an oxygen-absorbing resin, a transition metal catalyst, and an acid compound having, in the same molecule, two or more functional groups selected from a carboxyl group and a hydroxyl group. [2] The oxygen-absorbing resin composition according to [1] above, wherein at least one of the acid dissociation constants (pKa) of a diluted aqueous solution of the acid compound at 25° C. is lower than 3.7. [3] The oxygen-absorbing resin composition according to [1] or [2], wherein the acid compound is one or more selected from the group consisting of oxalic acid, citric acid, glycolic acid and phosphoric acid. [4] The oxygen absorbing resin is 4-methyl-△ 3-Tetrahydrophthalic acid, 4-methyl-△ 3 -Tetrahydrophthalic anhydride, cis-3-methyl-△ 4 -Tetrahydrophthalic acid, cis-3-methyl-△ 4 The oxygen-absorbing resin composition according to any one of the above [1] to [3], which contains an oxygen-absorbing polyester resin having a structural unit derived from tetrahydrophthalic anhydride or a derivative thereof. [5] The oxygen-absorbing resin composition according to any one of the above [1] to [4], wherein the transition metal catalyst is a transition metal salt composed of a transition metal selected from manganese, iron, cobalt, nickel, and copper and an organic acid. [6] An oxygen-absorbing adhesive comprising an isocyanate-based curing agent and the oxygen-absorbing resin composition according to any one of [1] to [5] above. [7] An oxygen absorbing film having a laminated structure including a film substrate and an oxygen absorbing layer, An oxygen absorbing film, wherein the oxygen absorbing layer comprises the oxygen absorbing resin composition according to any one of [1] to [5] above or the oxygen absorbing adhesive according to [6] above. Effect of the Invention
[0006] The present invention can provide an oxygen absorbing resin provided with an oxygen absorption trigger function that can control the oxygen absorbing reaction in a simple manner and at low production costs, and an oxygen absorbing film containing the same. [Brief description of the drawings]
[0007] [Figure 1] 1 is a graph showing an oxygen absorption trigger obtained from the oxygen-absorbing resin composition of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <Oxygen-absorbing resin composition> The oxygen absorbing resin composition according to the present invention contains at least an oxygen absorbing resin, a transition metal catalyst, and an acid compound having two or more functional groups selected from a carboxyl group and a hydroxyl group in the same molecule. In the oxygen absorbing film of the present invention, by introducing both a transition metal catalyst and a specific acid compound, it is possible to control the transition metal catalyst activity and the oxygen absorbing ability of the oxygen absorbing resin itself, and as a result, it is possible to impart a humidity-dependent oxygen absorption reaction. When the oxygen absorbing ability inherent to the oxygen absorbing resin composition is taken as 100%, and the time when the oxygen absorbing ability is 100% is taken as day 0, the oxygen absorbing resin composition of the present invention is characterized in that, when placed in an environment at an ambient temperature (22°C) and a relative humidity (RH) of 75% RH or less, more preferably 60% RH or less, and even more preferably 50% RH or less, it can maintain the oxygen absorbing ability of 75% or more, more preferably 80% or more, and even more preferably 90% or more without absorbing oxygen for at least about one day, more preferably 3 days, and even more preferably 7 days. The oxygen absorption trigger function in this specification means that the oxygen absorbing resin composition is capable of absorbing oxygen by increasing the oxygen absorption reaction rate and exerting 40% or more, more preferably 50% or more, and even more preferably 60% or more of the oxygen absorbing capacity within 3 days, more preferably within 1 day, only when the oxygen absorbing resin composition is placed in an environment with a relative humidity (RH) of 80% RH or more at an ambient temperature (22°C), more preferably 85% RH or more, and even more preferably 90% RH or more. Here, in this specification, the oxygen absorption amount when a resin composition (standard composition) containing only the corresponding oxygen absorbing resin and a transition metal catalyst is placed in an environment with a humidity of 90% RH for 7 days is defined as the 100% oxygen absorption capacity inherent to the oxygen absorbing resin composition. The oxygen absorption amount can be measured, for example, by the method described in the following examples.
[0009] It is believed that the oxygen absorbing resin composition of the present invention, by containing the specific acid compound, can suppress the catalytic activity of the transition metal catalyst and / or the autoxidation reaction of the oxygen absorbing resin composition in an environment of 40°C or less and a relative humidity of 75%RH or less. Therefore, for example, when the acid compound is not contained, oxygen absorption starts immediately regardless of the surrounding temperature and humidity. In addition, it is believed that as the humidity of the surrounding environment increases, the activity of the transition metal catalyst is no longer suppressed and the autoxidation reaction of the oxygen absorbing resin composition becomes more active, and the oxygen absorption rate increases with an increase in the humidity of the surrounding environment, and the oxygen absorption rate increases with an increase in the temperature of the surrounding environment. By combining the oxygen absorption reaction described above, the autoxidation reaction can be controlled. As shown in Figure 1, the oxygen absorption reaction can be started quickly by first managing the mixture under low humidity and then shifting it to a high humidity environment at any time.
[0010] In addition, when the oxygen-absorbing resin composition of the present invention contains the above-mentioned acid compound, it is preferable that the composition is irradiated with ultraviolet light having a wavelength in the ultraviolet light wavelength range of 200 to 400 nm at an ultraviolet light irradiation dose of at least 300 mJ / cm. 2 When irradiated under the above conditions, the oxygen absorption reaction rate is increased, and oxygen absorption can be achieved with 40% or more of the oxygen absorption capacity, more preferably 50% or more, and even more preferably 60% or more within 3 days, more preferably within 1 day, even in an environment with an ambient temperature (22°C) and a relative humidity (RH) of 75% or less. That is, the oxygen absorption trigger function in this specification means, in addition to the above definition, a function of irradiating ultraviolet rays having a wavelength of 200 to 400 nm at an ultraviolet irradiation dose of at least 300 mJ / cm even when the oxygen absorbing resin composition is placed in an environment with an ambient temperature (22°C) and a relative humidity (RH) of 75% or less. 2 It also means that when irradiated under the above conditions, the oxygen absorption reaction rate increases and the oxygen absorption capacity is exerted to absorb 40% or more, more preferably 50% or more, and even more preferably 60% or more of the oxygen absorption capacity within 3 days, more preferably within 1 day. The oxygen-absorbing resin composition of the present invention can be used as an adhesive by further containing a curing agent as described below, but it can also be used in paint applications other than as an adhesive, and can be applied as a coating film for various films and the like. Each component will be described in detail below.
[0011] ≪Transition metal catalyst≫ The oxygen absorbing resin composition of the present invention contains a transition metal catalyst whose main purpose is to promote the oxygen absorbing reaction. Examples of such transition metal catalysts include inorganic salts, organic salts, or complex salts of transition metals such as iron, cobalt, nickel, copper, silver, tin, titanium, zirconium, vanadium, chromium, and manganese, and particularly preferably manganese, iron, cobalt, nickel, and copper. More specifically, examples of the transition metal catalyst include transition metal salts composed of a transition metal selected from manganese, iron, cobalt, nickel, and copper and an organic acid. In particular, from the viewpoint of promoting the oxygen absorbing reaction of the oxygen absorbing resin and increasing the oxygen absorbing ability, the transition metal catalyst is preferably an organic acid salt of manganese, iron, or cobalt, and particularly preferably an organic acid salt of cobalt. The content of the transition metal catalyst in the oxygen absorbing resin composition is 1 ppm to 1000 ppm, preferably 10 ppm to 500 ppm, and more preferably 20 ppm to 300 ppm, in terms of metal. If the transition metal catalyst is not blended in the oxygen absorbing resin composition, the oxygen absorption trigger function cannot be imparted. Therefore, the transition metal catalyst must be contained in an amount of at least 1 ppm in terms of metal. In addition, if the content of the transition metal catalyst in the oxygen absorbing resin composition is more than 1000 ppm, a large amount of acid compound must be added accordingly, and in some cases, there is a risk that the effect of the oxygen absorption trigger is not sufficient.
[0012] ≪Acid compound≫ The oxygen absorbing resin composition of the present invention contains an acid compound having two or more functional groups selected from a carboxyl group and a hydroxyl group in the same molecule, the main purpose of which is to suppress the oxygen absorbing reaction in a low humidity environment. Preferably, at least one of the acid dissociation constants (pKa) of a diluted aqueous solution of the acid compound at 25°C is lower than 3.7, more preferably lower than 3.0, and even more preferably lower than 2.0. If the acid dissociation constant is 3.7 or more, the effect of suppressing the catalytic activity of the transition metal catalyst is weakened, so that the desired effect of suppressing the oxygen absorbing reaction may not be obtained. In addition, the acid compound of the present invention may be an organic acid such as oxalic acid, citric acid, or phthalic acid, or a polycarboxylic acid or glycolic acid, or an inorganic acid such as phosphoric acid, but oxalic acid is particularly preferred because it has a low acid dissociation constant and exhibits a strong interaction with the transition metal catalyst. As an example of comparing acid dissociation constants, for example, an organic acid having an ionic strength of 0.10 mol / dm -3 The acid dissociation constant measured in a dilute aqueous solution of 0.20 mol / dm2 can be used. In the case of inorganic acids such as phosphoric acid, the acid dissociation constant can be measured in a dilute aqueous solution of 0.20 mol / dm2 using potassium chloride as a supporting electrolyte at 25°C. -3 The acid dissociation constants measured in a diluted aqueous solution of 100 mg / kg can be used for comparison.
[0013] The content of the acid compound in the oxygen absorbing resin composition is, in terms of volume concentration, 10 ppm to 20000 ppm, more preferably 20 ppm to 1000 ppm, and further preferably 50 ppm to 1000 ppm. If the amount of the acid compound added is insufficient relative to the amount of the transition metal catalyst, it may not function sufficiently as an oxygen absorption trigger, and if added in excess, the oxygen absorption reaction may simply be inhibited and the trigger effect may not be obtained.
[0014] <Oxygen absorbing resin> The oxygen-absorbing resin of the present invention preferably contains an oxygen-absorbing polyester resin (A) mainly composed of an unsaturated polyester resin. The oxygen-absorbing polyester resin (A) may contain a saturated polyester resin (B) to the extent that the oxygen absorption reaction is not inhibited.
[0015] The oxygen-absorbing polyester resin (A) is a polyester resin containing a functional group or a bond group reactive with oxygen in the structure. Examples of the functional group or bond group reactive with oxygen include a carbon-carbon double bond group, an aldehyde group, and a phenolic hydroxyl group. In particular, a polyester resin having a carbon-carbon double bond group is preferred, and a polyester resin having an unsaturated alicyclic structure is more preferred. In the reaction between the unsaturated alicyclic structure and oxygen, the amount of low molecular weight decomposition components, which are by-products in the autoxidation reaction of the resin, is suppressed, which is preferable. Examples of polyester resins having an unsaturated alicyclic structure include polyesters using tetrahydrophthalic acid or a derivative thereof, or tetrahydrophthalic anhydride or a derivative thereof as a raw material. As tetrahydrophthalic acid or a derivative thereof or tetrahydrophthalic anhydride or a derivative thereof, 4-methyl-△ 3 -Tetrahydrophthalic acid or 4-methyl-△ 3 -Tetrahydrophthalic anhydride, cis-3-methyl-△ 4 -Tetrahydrophthalic acid or cis-3-methyl-△ 4 The tetrahydrophthalic acid or its derivatives or tetrahydrophthalic anhydride or its derivatives are highly reactive with oxygen and can be suitably used as a raw material for oxygen absorbing resins. In addition, these tetrahydrophthalic acids or their derivatives or tetrahydrophthalic anhydride or its derivatives are obtained by reacting a C5 fraction of naphtha, which is mainly composed of isoprene and trans-piperylene, with maleic anhydride to produce 4-methyl-△ 4 It can be obtained by structural isomerization of an isomer mixture containing .-tetrahydrophthalic anhydride and is produced industrially. When tetrahydrophthalic acid or a derivative thereof, or tetrahydrophthalic anhydride or a derivative thereof is used as a raw material to polymerize the oxygen-absorbing polyester resin (A), the dicarboxylic acid and dicarboxylic anhydride may be esterified to, for example, a methyl ester.
[0016] The oxygen-absorbing polyester resin (A) can be produced by reacting tetrahydrophthalic acid or a derivative thereof, or tetrahydrophthalic anhydride or a derivative thereof with a diol component. Examples of the diol component include ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, polypropylene glycol, trimethylene glycol, 1,3-butanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, 2-phenylpropanediol, 2-(4-hydroxyphenyl)ethyl alcohol, α,α-dihydroxy-1,3-diisopropylbenzene, o-xylene glycol, m-xylene glycol, p-xylene glycol, α,α-dihydroxy-1,4-diisopropylbenzene, hydroquinone, 4,4-dihydroxydiphenyl, naphthalenediol, and derivatives thereof. Preferably, the resin is an aliphatic diol, such as diethylene glycol, triethylene glycol, or 1,4-butanediol, and more preferably, 1,4-butanediol. When 1,4-butanediol is used, the resin has high oxygen absorption performance, and the amount of decomposition products generated during the oxidation process is small. These may be used alone or in combination of two or more.
[0017] The oxygen-absorbing polyester resin (A) may contain, in addition to tetrahydrophthalic acid or a derivative thereof, or tetrahydrophthalic anhydride or a derivative thereof, other acid components and their derivatives, such as aromatic dicarboxylic acids, aliphatic dicarboxylic acids, and aliphatic hydroxycarboxylic acids, as raw materials. Examples of aromatic dicarboxylic acids and derivatives thereof include phthalic acid, phthalic anhydride, benzene dicarboxylic acids such as isophthalic acid and terephthalic acid, naphthalenedicarboxylic acids such as 2,6-naphthalenedicarboxylic acid, anthracene dicarboxylic acid, sulfoisophthalic acid, sodium sulfoisophthalate, and derivatives thereof. Among these, phthalic acid, phthalic anhydride, isophthalic acid, and terephthalic acid are preferred. Examples of the aliphatic dicarboxylic acid and its derivatives include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, 3,3-dimethylpentanedioic acid, and derivatives thereof. Among these, adipic acid and succinic acid are preferred, and succinic acid is particularly preferred. Further, hexahydrophthalic acid and dimer acid having an alicyclic structure and their derivatives are also included. Examples of the aliphatic hydroxycarboxylic acid and its derivatives include glycolic acid, lactic acid, hydroxypivalic acid, hydroxycaproic acid, hydroxyhexanoic acid, and derivatives thereof. These acid components may be esterified, for example, as dimethyl terephthalate or bis-2-hydroxydiethyl terephthalate. They may also be acid anhydrides, such as phthalic anhydride or succinic anhydride. These may be used alone or in combination of two or more. By copolymerizing the other acid components, the glass transition temperature of the resulting polyester can be easily controlled, and the oxygen absorption performance can be improved. Furthermore, the solubility in organic solvents can be improved by controlling the crystallinity of the polyester resin. In addition, since tetrahydrophthalic acid or a derivative thereof, or tetrahydrophthalic anhydride or a derivative thereof is likely to undergo a radical crosslinking reaction due to heat during polymerization, when the composition ratio of tetrahydrophthalic acid or a derivative thereof, or tetrahydrophthalic anhydride or a derivative thereof contained in the polyester is reduced by the other acid component, gelation during polymerization is suppressed and a high molecular weight resin can be stably obtained.
[0018] The oxygen-absorbing polyester resin (A) may further contain structural units derived from polyhydric alcohols, polybasic carboxylic acids, or derivatives thereof, etc. By controlling the branched structure through the introduction of polyhydric alcohols and polybasic carboxylic acids, it is possible to adjust the melt viscosity characteristics and the solution viscosity characteristics of the polyester dissolved in a solvent. Examples of polyhydric alcohols and derivatives thereof include 1,2,3-propanetriol, sorbitol, 1,3,5-pentanetriol, 1,5,8-heptanetriol, trimethylolpropane, pentaerythritol, 3,5-dihydroxybenzyl alcohol, glycerin, and derivatives thereof. Examples of polyvalent carboxylic acids and derivatives thereof include 1,2,3-propanetricarboxylic acid, meso-butane-1,2,3,4-tetracarboxylic acid, citric acid, trimellitic acid, pyromellitic acid, and derivatives thereof. When a component having three or more functional groups, such as a polyhydric alcohol or a polycarboxylic acid, is copolymerized, the amount is preferably 5 mol % or less based on the total acid components.
[0019] Polyesters obtainable by copolymerizing a tetrahydrophthalic acid derivative or a tetrahydrophthalic anhydride derivative, 1,4-butanediol, and, as an optional component, succinic acid or succinic anhydride, are preferred as the oxygen-absorbing polyester resin (A). In this case, the structural unit derived from tetrahydrophthalic acid or its derivative, or tetrahydrophthalic anhydride or its derivative contained in the oxygen-absorbing polyester resin (A) is 70 to 95 mol %, preferably 75 to 95 mol %, more preferably 80 to 95 mol %, based on the total acid components. The structural unit derived from succinic acid or succinic anhydride is 0 to 15 mol %, preferably 0 to 12.5 mol %, more preferably 0 to 10 mol %, based on the total acid components. By setting the composition ratio in this way, an oxygen-absorbing resin having excellent oxygen absorption performance and adhesiveness, and excellent solubility in organic solvents can be obtained.
[0020] The glass transition temperature of the oxygen-absorbing polyester resin (A) is −20° C. to 10° C., preferably −15° C. to 6° C., and more preferably −12° C. to 2° C. By setting the glass transition temperature within this range, sufficient oxygen absorbing performance can be obtained. In order to obtain sufficient oxygen absorption performance, the acid value of the oxygen-absorbing polyester resin (A) is preferably 5 mgKOH / g or less, more preferably 1 mgKOH / g or less. If the acid value of the polyester exceeds 5 mgKOH / g, a rapid autoxidation reaction is hindered, and stable oxygen absorption performance may not be obtained. The acid value of the oxygen-absorbing polyester resin (A) is measured according to JIS K 0070. The oxygen-absorbing polyester resin (A) may be used alone or in combination of two or more kinds.
[0021] The saturated polyester resin (B) is a polyester resin that does not substantially contain a carbon-carbon double bond group, and can be obtained, for example, by polycondensation of a dicarboxylic acid component, a diol component, and a hydroxycarboxylic acid component. The saturated polyester resin (B) is preferably a polyester having an iodine value of 3 g / 100 g or less, particularly 1 g / 100 g or less. The iodine value is measured according to JIS K 0070. If the iodine value of the saturated polyester resin (B) exceeds 3 g / 100 g, it is not preferable because low molecular weight decomposition components are easily generated during the oxygen absorption reaction of the oxygen absorbing resin composition. Examples of the dicarboxylic acid component include the aliphatic dicarboxylic acids and aromatic dicarboxylic acids described above as components of the oxygen-absorbing polyester resin (A), hexahydrophthalic acid, dimer acid, and derivatives thereof, etc. These can be used alone or in combination of two or more kinds. The diol component includes the diols described above as the components of the oxygen-absorbing polyester resin (A), which may be used alone or in combination of two or more kinds. Examples of the hydroxycarboxylic acid component include the aliphatic hydroxycarboxylic acids described as components of the oxygen-absorbing polyester resin (A). When the terminal functional group of the saturated polyester resin (B) is a hydroxyl group, the curing proceeds together with the oxygen-absorbing polyester resin (A) by a curing agent such as an isocyanate curing agent, and the cohesive strength increases when used as an adhesive as described below, which is preferable. It is also preferable to modify the saturated polyester resin (B) with an alkyl group at the terminal with a monoalcohol such as n-butanol or 2-ethylhexanol, a fatty acid, or the like. The glass transition temperature of the saturated polyester resin (B) is −10° C. or lower, preferably −70° C. to −15° C., and more preferably −60° C. to −20° C. By setting the glass transition temperature within this range, it is possible to effectively relieve internal stress caused by the oxidative curing reaction accompanying oxygen absorption.
[0022] A suitable embodiment of the oxygen-absorbing resin composition is a composition containing an oxygen-absorbing polyester resin (A) having a glass transition temperature of -20°C to 10°C and a saturated polyester resin (B) having a glass transition temperature of -10°C or lower. The oxygen-absorbing polyester resin (A) and the saturated polyester resin (B) used in the present invention can be obtained by any polyester polycondensation method known to those skilled in the art, such as interfacial polycondensation, solution polycondensation, melt polycondensation, and solid-phase polycondensation. When synthesizing the oxygen-absorbing polyester resin (A) and saturated polyester resin (B) used in the present invention, a polymerization catalyst is not necessarily required, but it is possible to use ordinary polyester polymerization catalysts such as titanium-based, germanium-based, antimony-based, tin-based, aluminum-based, etc. It is also possible to use known polymerization catalysts such as nitrogen-containing basic compounds, boric acid and boric acid esters, and organic sulfonic acid compounds. Furthermore, various additives such as a coloring inhibitor such as a phosphorus compound and an antioxidant can be added during polymerization. By adding an antioxidant, oxygen absorption during polymerization and subsequent processing can be suppressed, and therefore the performance degradation and gelation of the oxygen absorbing resin can be suppressed. The number average molecular weight of the oxygen-absorbing polyester resin (A) used in the present invention is preferably 500 to 100,000, more preferably 2,000 to 10,000. The weight average molecular weight is preferably 5,000 to 200,000, more preferably 10,000 to 100,000, and even more preferably 20,000 to 70,000. If the molecular weight is lower than the above range, the cohesive force, i.e., creep resistance, of the resin decreases, and if it is higher, it is not preferable because the solubility in organic solvents decreases and the coatability decreases due to an increase in solution viscosity. The number average molecular weight of the saturated polyester resin (B) is preferably 500 to 100,000, more preferably 500 to 10,000. The weight average molecular weight is preferably 1,000 to 100,000, more preferably 1,000 to 70,000, and even more preferably 1,000 to 50,000. If the molecular weight is lower than the above range, the cohesive strength is significantly reduced, and if it is higher, it is not preferable because the compatibility with the oxygen-absorbing polyester resin (A) is reduced and the coating property is reduced due to the increase in solution viscosity. When the molecular weights of the oxygen-absorbing polyester resin (A) and the saturated polyester resin (B) are each within the above range, an oxygen-absorbing adhesive having excellent cohesive strength, adhesiveness, and solubility in organic solvents and suitable viscosity characteristics as an adhesive solution as described below can be obtained.
[0023] <Oxygen absorbing adhesive> The oxygen-absorbing resin of the present invention can be used as an oxygen-absorbing adhesive by further including a curing agent. Examples of adhesives include acrylic adhesives, urethane adhesives, epoxy adhesives, ethylene-vinyl acetate adhesives, vinyl chloride adhesives, silicone adhesives, rubber adhesives, etc., to which oxygen-absorbing function has been imparted. In particular, when used as an adhesive for dry lamination, urethane adhesives are preferred, and two-liquid curing urethane adhesives that combine an oxygen-absorbing polyester base agent and an isocyanate curing agent are more preferred.
[0024] The ratio A / B of the oxygen-absorbing polyester resin (A) to the saturated polyester resin (B) in the oxygen-absorbing adhesive or in the oxygen-absorbing adhesive layer of the oxygen-absorbing film described below is preferably 0.6 to 9, more preferably 1 to 9, and even more preferably 2 to 9. By setting the ratio A / B in this range, it is possible to achieve excellent oxygen-absorbing performance while maintaining high laminate strength before and after oxygen absorption.
[0025] The oxygen absorbing adhesive is preferably cured by blending an isocyanate-based curing agent such as an aliphatic and / or alicyclic isocyanate-based curing agent, and the oxygen absorbing adhesive layer of the oxygen absorbing film of the present invention described later preferably contains an oxygen absorbing adhesive cured by blending an isocyanate-based curing agent such as an aliphatic and / or alicyclic isocyanate-based curing agent with a base material consisting of an oxygen absorbing polyester resin (A) and a saturated polyester resin (B). When an isocyanate-based curing agent is blended, the adhesive strength and cohesive force are increased, and curing is possible at a low temperature around room temperature. Examples of the aliphatic isocyanate-based curing agent include xylylene diisocyanate (XDI), hexamethylene diisocyanate (HDI), lysine diisocyanate, lysine methyl ester diisocyanate, trimethylhexamethylene diisocyanate, n-pentane-1,4-diisocyanate, etc. Examples of alicyclic isocyanate-based curing agents include isophorone diisocyanate (IPDI), cyclohexane-1,4-diisocyanate, methylcyclohexyl diisocyanate, and dicyclohexylmethane-4,4'-diisocyanate. Among these, XDI and HDI are preferred as aliphatic isocyanate-based curing agents, and IPDI is preferred as an alicyclic isocyanate-based curing agent. XDI is particularly preferred. By using XDI, the oxygen absorbing adhesive of the present invention or the oxygen absorbing adhesive layer of the oxygen absorbing film described below exhibits the most excellent oxygen absorbing performance. It is also preferred to use a combination of IPDI and XDI, IPDI and HDI, etc. Aromatic isocyanate-based curing agents can also be used, but aromatic isocyanate-based curing agents are not preferred because they may reduce oxygen absorbing performance, although they improve the adhesiveness and cohesive force of the resin. The reason for this is thought to be that the aromatic urethane moiety formed when the aromatic isocyanate curing agent reacts with the hydroxyl group at the end of the polyester base resin works in the same way as aromatic amines, which act as antioxidants, to deactivate / stabilize radicals.
[0026] These isocyanate-based curing agents are preferably used in the form of polyisocyanate compounds with increased molecular weight, such as adducts, isocyanurates, or biuret forms. These isocyanate-based curing agents may be used alone or in combination of two or more kinds. The isocyanate-based curing agent component is preferably added in an amount of 3 phr to 30 phr, more preferably 3 phr to 20 phr, and even more preferably 3 phr to 15 phr, based on the solid weight of the oxygen-absorbing resin as the main component. If the amount added is too small, the adhesiveness and cohesive strength become insufficient, and if the amount added is too large, the amount of the oxygen-absorbing component contained in the unit weight of the resin composition becomes small, resulting in insufficient oxygen-absorbing performance. In addition, if the mobility of the resin is significantly reduced by curing, the oxygen-absorbing reaction becomes difficult to proceed, and the oxygen-absorbing performance decreases.
[0027] One embodiment of the oxygen-absorbing adhesive of the present invention has a single glass transition temperature of -2°C or lower. In this case, it is possible to effectively relieve the internal stress caused by the oxidative curing reaction accompanying oxygen absorption and ensure sufficient transparency. The single glass transition temperature is more preferably -50°C to -2°C, and even more preferably -20°C to -2°C.
[0028] The oxygen absorbing adhesive preferably contains a solvent such as an organic solvent. Examples of the solvent include ethyl acetate, acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, xylene, isopropanol, etc. In particular, ethyl acetate is generally used as a solvent for adhesives for dry lamination of flexible packaging because it is relatively less likely to cause odor problems due to residual solvents, and in consideration of industrial applications, it is preferable to use a single solvent of ethyl acetate that does not contain toluene, xylene, etc. as the solvent of the present invention. Various additives such as silane coupling agents, antioxidants, ultraviolet absorbers, hydrolysis inhibitors, anti-fungal agents, curing catalysts, thickeners, plasticizers, pigments, fillers, polyester resins, and epoxy resins may be added to the oxygen-absorbing adhesive of the present invention or the oxygen-absorbing adhesive layer of the oxygen-absorbing film described below, as necessary, within the scope of the object of the present invention.
[0029] <Oxygen absorbing film> The oxygen absorbing film of the present invention is an oxygen absorbing film of a laminated structure including a film substrate and an oxygen absorbing layer, and the oxygen absorbing layer includes the above-mentioned oxygen absorbing resin composition or oxygen absorbing adhesive. The oxygen absorbing adhesive of the present invention can be used, for example, as an oxygen absorbing adhesive layer constituting the oxygen absorbing layer of an oxygen absorbing film, for the purpose of laminating a plurality of film substrates in the same manner as with a normal adhesive for dry lamination. In particular, it can be suitably used for laminating a film substrate having oxygen barrier properties with a sealant film having heat sealability and oxygen gas permeability. In this case, the laminated structure is an oxygen barrier substrate layer / oxygen absorbing adhesive layer / sealant layer from the outer layer side, and the oxygen permeating in from the outside is blocked by the oxygen barrier substrate, so that the decrease in oxygen absorbing performance due to oxygen outside the container is suppressed, and the oxygen absorbing adhesive can quickly absorb oxygen inside the container through the oxygen permeable sealant film, which is preferable. The oxygen barrier film substrate and the sealant film may each be a single layer or a laminate. As the oxygen barrier film substrate, a biaxially oriented PET film, a biaxially oriented polyamide film, or a biaxially oriented polypropylene film having a barrier coating layer mainly composed of a gas barrier organic material such as a vapor-deposited thin film of a metal oxide or metal such as silica or alumina as a barrier layer, a polyvinyl alcohol resin, an ethylene-vinyl alcohol copolymer, a polyacrylic acid resin, or a vinylidene chloride resin, etc., can be suitably used. In addition, an ethylene-vinyl alcohol copolymer film, a polymetaxylylene adipamide film, a polyvinylidene chloride film, or a metal foil such as an aluminum foil is also preferred. These oxygen barrier film substrates can be used by laminating the same type of substrate or two or more different types of substrates, and it is also preferred to use a biaxially oriented PET film, a biaxially oriented polyamide film, a biaxially oriented polypropylene film, cellophane, paper, etc.
[0030] Suitable materials for the sealant film include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, linear very low-density polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, cyclic olefin polymers, cyclic olefin copolymers, or random or block copolymers of α-olefins such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers and their ion-crosslinked products (ionomers), ethylene-methyl methacrylate copolymers, and other ethylene-vinyl compound copolymers, heat-sealable polyesters such as PET, A-PET, PETG, and PBT, and amorphous nylon, etc. Two or more of these materials can be blended and used, or the same or different materials can be laminated and used.
[0031] When laminating a plurality of film substrates using the oxygen-absorbing adhesive of the present invention, a known dry laminator can be used. The dry laminator can carry out a series of lamination steps, including coating the oxygen-absorbing adhesive onto a barrier film substrate, volatilizing the solvent in a drying oven, and bonding with a sealant film using nip rolls heated to 50 to 120°C. The coating amount of the oxygen-absorbing adhesive is 0.1 to 30 g / m2 in terms of solid content. 2 , preferably 1 to 15 g / m 2 and more preferably 2 to 10 g / m 2 It is also preferable to age (cure) the oxygen-absorbing laminated film laminated with the oxygen-absorbing adhesive at a temperature near room temperature, for example, 10 to 60°C, in order to promote the curing reaction. The curing is mainly due to a crosslinking reaction caused by an isocyanate-based curing agent, and is preferable because the adhesive strength and cohesive force are improved by the curing. It is preferable to perform the aging in the absence of oxygen or under oxygen blocking conditions, for example, by sealing the oxygen-absorbing laminated film in an oxygen-impermeable bag. In this way, it is possible to suppress the decrease in oxygen absorption performance caused by oxygen in the air during aging. The oxygen-absorbing resin composition of the present invention can also be used as a solvent-free adhesive without being dissolved in a solvent. In this case, an oxygen-absorbing laminated film can be obtained using a known non-solvent laminator.
[0032] The oxygen absorbing film and the oxygen absorbing resin composition of the present invention can be irradiated with light as necessary. A commonly used ultraviolet ray irradiator or an electron beam irradiator can be used as the light irradiator. Examples of the form of light irradiation include a laminate film, a bag-shaped container, a lid material, and a packaging bag filled with contents.
[0033] The oxygen-absorbing film of the present invention can be suitably used as a lid material for various types of bag-shaped containers and cup / tray containers, such as flat pouches sealed on three or four sides, pouches with gussets, standing pouches, pillow packaging bags, etc. An oxygen-absorbing container that uses an oxygen-absorbing film in at least a portion thereof effectively blocks oxygen that permeates from the outside of the container and absorbs oxygen remaining in the container, and is therefore useful as a container that can maintain the oxygen concentration in the container at a low level for a long period of time, prevent quality deterioration of the contents due to oxygen, and improve shelf life. In particular, examples of contents that are susceptible to deterioration in the presence of oxygen include, but are not limited to, food such as coffee beans, tea leaves, snacks, rice crackers, fresh and semi-fresh confectioneries, fruits, nuts, vegetables, fish and meat products, paste products, dried fish, smoked foods, tsukudani (food boiled in soy sauce), raw rice, cooked rice, baby foods, jams, mayonnaise, ketchup, edible oils, dressings, sauces, dairy products, etc.; beverages such as beer, wine, fruit juice, green tea, coffee, etc.; and other products such as medicines, cosmetics, and electronic components. EXAMPLES
[0034] The present invention will now be described in more detail with reference to examples. Each value was measured by the following method. (1) Number average molecular weight (Mn), weight average molecular weight (Mw) and molecular weight distribution index (Mw / Mn) The measurement was performed using gel permeation chromatography (GPC, Tosoh Corporation; HLC-8320 type GPC) in terms of polystyrene. Chloroform was used as the solvent. (2) Oxygen absorption A laminated film test piece cut to 2 cm x 15 cm was placed in a container with an internal volume of 85 cm 3 The mixture was placed in an oxygen-impermeable steel foil laminated cup, heat-sealed with an aluminum foil laminated film lid, and stored in an atmosphere at 22°C. After storage for the number of days shown in Table 1, the oxygen concentration in the cup was measured using a micro gas chromatograph (Shimadzu Corporation; GC-2014AT) and the concentration of oxygen in the cup was measured at 1 cm 2 The amount of oxygen absorbed per unit was calculated. Regarding the humidity dependency of the oxygen absorption reaction, the oxygen absorption amount (0.038cc / cm) after storage for 7 days at 22°C-90%RH (relative humidity) in Comparative Example 1 was 2) was used as a control. In the present Examples 1 to 6, samples in which the oxygen absorption amount of the sample after storage for the number of days listed in Table 1 was 50% or more of the control at 22°C-90% RH and 50% or less of the control at 22°C-50% RH were evaluated as having good humidity dependency (◯). In the comparative examples 1 to 3, samples in which the oxygen absorption amount after storage for 7 days at 22°C-50% RH exceeded 50% of the oxygen absorption amount after storage for 7 days at 22°C-90% RH in the respective comparative examples were evaluated as not having humidity dependency (×). Regarding the trigger function of the oxygen absorption reaction, the amount of oxygen absorbed 3 days after the humidity change was 0.038 cc / cm 2 ) was judged to have a good trigger function (◯), and one with a trigger function of less than 50% was judged to have no trigger function (×).
[0035] Example 1 As the acid component, methyl tetrahydrophthalic anhydride isomer mixture (Hitachi Chemical; HN-2200) was used in a molar ratio of 0.9, as other acid components, succinic anhydride in a molar ratio of 0.1, as a diol component, 1,4-butanediol in a molar ratio of 1.3, and as a polymerization catalyst, 300 ppm of isopropyl titanate was charged, and the mixture was reacted for about 6 hours at 150°C to 200°C in a nitrogen atmosphere while removing the water generated. Subsequently, polymerization was carried out for about 3 hours at 200°C to 220°C under a reduced pressure of 0.1 kPa, to obtain an oxygen-absorbing polyester resin (A). At this time, Mn was 4800, Mw was 57200, and Tg was -5.0°C. The obtained oxygen-absorbing polyester resin (A) was mixed with a saturated polyester resin (B1) (Polysizer W4010, manufactured by DIC Corporation, Mn: 3600, Mw: 9500) having a Tg of -26°C so that the solid content weight ratio A / B1 was 2.3. An HDI / IPDI curing agent (KL-75, manufactured by DIC Graphics Corporation) was mixed with the solid content of the mixture as an isocyanate curing agent so that the solid content was 7 phr (parts per hundred resin). Further, cobalt neodecanoate was added as a catalyst so that the metal content relative to the solid content was 80 ppm, and 240 ppm of oxalic acid was added as an acid compound. The mixture was dissolved in ethyl acetate, and the oxygen-absorbing adhesive (a) solution with a solid content concentration of 20 wt% was applied to the barrier coating surface of a transparent vapor-deposited PET film (GL-AE, manufactured by Toppan Printing Co., Ltd., film thickness 13 μm) using a #15 bar coater. After evaporating the solvent with hot air from a hair dryer, the adhesive-coated surface of the laminated film and the corona treatment of a 40 μm LDPE film (discharge amount 25 W min / m 2 ) faces facing each other and passed through a heated roll at 50°C to obtain an oxygen-absorbing laminate film consisting of a transparent vapor-deposited PET film (film thickness 13 μm) / oxygen-absorbing adhesive (a) (film thickness 4 μm) / LDPE (film thickness 40 μm). The obtained oxygen-absorbing laminate film was cured at 35° C. in a nitrogen atmosphere for 5 days, and then the amount of oxygen absorbed was evaluated.
[0036] Example 2 Evaluation was carried out in the same manner as in Example 1, except that the acid compound in Example 1 was changed to citric acid. The results are shown in Table 1.
[0037] Example 3 Evaluation was performed in the same manner as in Example 1, except that the acid compound was changed to citric acid, the concentration was changed to 960 ppm, and the time period was changed to 9 days. The results are shown in Table 1.
[0038] Example 4 Evaluation was carried out in the same manner as in Example 1, except that the acid compound was changed to glycolic acid and the time period was changed to 1 day. The results are shown in Table 1.
[0039] Example 5 Evaluation was carried out in the same manner as in Example 1, except that the acid compound was changed to phosphoric acid and the aging period was changed to 8 days. The results are shown in Table 1.
[0040] Example 6 Evaluation was carried out in the same manner as in Example 1, except that the catalyst was iron heptanoate and the aging period was 14 days. The results are shown in Table 1.
[0041] Comparative Example 1 The evaluation was carried out in the same manner as in Example 1, except that no acid compound was added. The results are shown in Table 1.
[0042] Comparative Example 2 Evaluation was carried out in the same manner as in Example 1, except that the acid compound in Example 1 was changed to acetic acid. The results are shown in Table 1.
[0043] Comparative Example 3 Evaluation was carried out in the same manner as in Example 1, except that the acid compound in Example 1 was changed to dodecylbenzenesulfonic acid. The results are shown in Table 1.
[0044] [Table 1]
[0045] The results in Table 1 show that the inclusion of an acid compound in the present invention causes the amount of oxygen absorbed to change depending on humidity.
[0046] Example 7 The oxygen-absorbing laminate film obtained in Example 1 was left to stand for one day under 22°C and 50% RH (in the atmosphere), and then the amount of oxygen absorbed after storing for three days under conditions of 22°C and 90% RH was evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0047] Example 8 The oxygen-absorbing laminate film obtained in Example 1 was left to stand for 4 days under 22°C and 50% RH (in the atmosphere), and then the amount of oxygen absorbed after storing for 3 days under conditions of 22°C and 90% RH was evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0048] Example 9 The oxygen-absorbing laminate film obtained in Example 1 was left to stand for 7 days under 22°C and 50% RH (in the atmosphere), and then the amount of oxygen absorbed after storing for 3 days under conditions of 22°C and 90% RH was evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0049] [Table 2]
[0050] From the results in Table 1, the oxygen absorbing capacity of the oxygen absorbing adhesive of Example 1 when left for 7 days at 22°C and 50% RH (in the atmosphere) was 0.004 cc / cm 2 In light of this, the results in Table 2 demonstrate that the oxygen absorbing adhesive of the present invention is capable of changing the amount of oxygen absorbed in response to changes in humidity.
[0051] Example 10 The LDPE surface of the oxygen-absorbing laminate film obtained in Example 1 was irradiated with ultraviolet light (metal halide light source ultraviolet irradiation device (peak wavelength 370 nm)) at a dose of 300 mJ / cm 2 After irradiation with 100 uL, the evaluation was carried out in the same manner as in Example 1. The results are shown in Table 3.
[0052] Example 11 The LDPE surface of the oxygen-absorbing laminate film obtained in Example 1 was irradiated with ultraviolet light at a dose of 600 mJ / cm. 2 After irradiation with 100 uL, the evaluation was carried out in the same manner as in Example 1. The results are shown in Table 3.
[0053] [Table 3] From the results in Table 3, it was found that the oxygen absorbing laminate film of the present invention can control (improve) its oxygen absorbing ability by ultraviolet irradiation, even when it is left for 7 days in an environment of 22°C and 50% RH. (From the results in Table 1, it was found that the oxygen absorbing laminate film of the present invention has an oxygen absorption amount of 0.004 cc / cm even when it is left for 7 days in an environment of 22°C and 50% RH without ultraviolet irradiation.) 2 The effect of ultraviolet light exposure is clear, as the effect was only about 100%.
[0054] Example 12 Using a film similar to the sample used in Example 1 in Table 1, the change in oxygen absorption capacity over time was measured when the film was transferred from low humidity conditions (22°C-0% RH) to high humidity conditions (22°C-90% RH). The results showed an oxygen absorption reaction that was dependent on humidity, as shown in Figure 1. The results in Figure 1 clearly demonstrate that the oxygen-absorbing resin composition of the present invention exhibits an oxygen absorption trigger.
Claims
1. The oxygen absorbing resin includes a transition metal catalyst and an acid compound, The oxygen-absorbing resin composition, wherein the acid compound is one or more selected from the group consisting of oxalic acid, citric acid, and glycolic acid.
2. The oxygen-absorbing resin composition according to claim 1 , wherein the oxygen-absorbing resin has a carbon-carbon double bond.
3. An oxygen-absorbing adhesive comprising an isocyanate-based curing agent and the oxygen-absorbing resin composition according to claim 1 or 2.
4. An oxygen absorbing film having a laminated structure including a film substrate and an oxygen absorbing layer, An oxygen absorbing film, wherein the oxygen absorbing layer comprises the oxygen absorbing resin composition according to claim 1 or 2 or the oxygen absorbing adhesive according to claim 3.
5. Oxygen absorbing resin, A method for controlling the oxygen absorption reaction of the oxygen absorbing resin by adding a transition metal catalyst and an acid compound, comprising: The method, wherein the acid compound is one or more selected from the group consisting of oxalic acid, citric acid, and glycolic acid.
Citation Information
Patent Citations
Oxygen absorbing resin composition
JP2001106866A
Resin composition having gas barrier property
JP2002069319A
Composition for controlling exposure to oxygen
JP2009536973A
Polyester resin composition
JP2016044185A
Oxygen-absorbing property added laminate adhesive resin composition
JP2017105910A