Water-containing glass-based articles with high indentation cracking threshold
Glass-based articles with a hydrogen-containing layer formed by exposing a substrate to water vapor exhibit high resistance to indentation cracking, addressing the need for improved damage resistance in thinner electronic device materials.
Patent Information
- Application Number
- JP2024112308
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-05-08
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2038-11-16
AI Technical Summary
The increasing demand for smaller and thinner materials in portable electronic devices, such as smartphone displays and enclosures, necessitates the development of materials with higher damage resistance to withstand indentation cracking.
Glass-based articles with a hydrogen-containing layer extending from the surface, where the hydrogen concentration decreases with depth, and a layer depth greater than 5 μm, exhibiting a Vickers crack initiation threshold of 1 kgf (approximately 9.8 N) or more, are formed by exposing a glass substrate to a water vapor environment.
The glass-based articles demonstrate high resistance to indentation cracking, maintaining structural integrity under significant loads without conventional strengthening methods, enhancing damage resistance.
Smart Images

Figure 2024138482000001_ABST
Abstract
Description
Related Applications
[0001] This application claims the benefit of priority to U.S. Provisional Application No. 62 / 587,872, filed November 17, 2017, and Dutch Provisional Application No. 2020896, filed May 8, 2018, the contents of which are relied upon and incorporated by reference in their entireties herein.
[0002] This application is also a divisional application of Patent Application No. 2020-526391, filed on November 16, 2018. [Technical field]
[0003] The present disclosure relates to glass-based articles containing hydrogen, glass compositions utilized to form the glass-based articles, and methods of forming the glass-based articles. [Background technology]
[0004] Portable electronic devices, such as smartphones, tablets and wearable devices (such as watches and fitness trackers), continue to become smaller and more complex. Accordingly, the materials traditionally used for at least one outer surface of such portable electronic devices also continue to become more complex. For example, as portable electronic devices become smaller and thinner to meet consumer demand, the display covers and housings used in these portable electronic devices also become smaller and thinner, resulting in higher performance requirements for the materials used to form these parts. Summary of the Invention [Problem to be solved by the invention]
[0005] Therefore, there is a need for materials that exhibit higher performance, such as damage resistance, for use in portable electronic devices. [Means for solving the problem]
[0006] In embodiment (1), a glass-based article is provided. The glass-based article includes SiO2, Al2O3, and P2O5; and a hydrogen-containing layer extending from a surface of the glass-based article to a depth of the layer. The hydrogen concentration of the hydrogen-containing layer decreases from a maximum hydrogen concentration toward the depth of the layer, and the depth of the layer is greater than 5 μm.
[0007] In an embodiment (2), there is provided the glass-based article according to embodiment (1), wherein the glass-based article has a Vickers crack initiation threshold of 1 kgf (about 9.8 N) or more.
[0008] In an embodiment (3), there is provided the glass-based article according to embodiment (1) or (2), having a depth of layer of 10 μm or more.
[0009] In an embodiment (4), there is provided the glass-based article of any one of embodiments (1) to (3), wherein the maximum hydrogen concentration is located at a surface of the glass-based article.
[0010] In an embodiment (5), there is provided the glass-based article of any one of embodiments (1) to (4), further comprising at least one of Li2O, Na2O, K2O, Cs2O, and Rb2O.
[0011] In an embodiment (6), there is provided the glass-based article of any one of embodiments (1) to (5), further comprising KO.
[0012] In an embodiment (7), there is provided the glass-based article of any one of embodiments (1) to (6), wherein the center of the glass-based article comprises: -45 mol% to -75 mol% SiO2; -3 mol% to -20 mol% Al2O3; -6 mol% to -15 mol% P2O5; and -6 mol% to 25 mol% KO.
[0013] In an embodiment (8), there is provided the glass-based article of any one of embodiments (1) to (6), wherein the center of the glass-based article comprises: -45 mol% to -75 mol% SiO2; -3 mol% to -20 mol% Al2O3; -4 mol% to -15 mol% P2O5; and -11 mol% to -25 mol% KO.
[0014] In an embodiment (9), there is provided the glass-based article of any one of embodiments (1) to (6), wherein the center of the glass-based article comprises: -55 mol% to -69 mol% SiO2; -5 mol% to -15 mol% Al2O3; -6 mol% to -10 mol% P2O5; and -10 mol% to -20 mol% KO.
[0015] In an embodiment (10), there is provided the glass-based article of any one of embodiments (7) to (9), wherein the center of the glass-based article comprises: 0 mol% to 10 mol% CsO; and 0 mol% to 10 mol% RbO.
[0016] In an embodiment (11), there is provided the glass-based article of any one of embodiments (1) to (10), wherein the glass-based article is substantially free of at least one of lithium and sodium.
[0017] In an embodiment (12), there is provided the glass-based article of any one of embodiments (1) to (11), further comprising a compressive stress layer extending from a surface of the glass-based article to a compressed depth within the glass-based article.
[0018] In an embodiment (13), there is provided the glass-based article of embodiment (12), wherein the compressive stress layer comprises a compressive stress of at least about 100 MPa and a compression depth of at least about 75 μm.
[0019] In an embodiment (14), a consumer electronics product is provided. The consumer electronics product includes a housing having a front, a back, and a side; electrical components at least partially within the housing, the electrical components including at least a controller, a memory, and a display, the display being disposed at or adjacent to the front of the housing; and a cover substrate disposed over the display. At least a portion of at least one of the housing or the cover substrate comprises the glass-based article of any one of embodiments (1) to (13).
[0020] In an embodiment (15), a glass is provided, the glass comprising: 45 mol% to 75 mol% SiO2; 3 mol% to 20 mol% Al2O3; 6 mol% to 15 mol% P2O5; and 6 mol% to 25 mol% K2O.
[0021] In an embodiment (16), there is provided the glass of embodiment (15), comprising: 55 mol% to 69 mol% SiO2; 5 mol% to 15 mol% Al2O3; 6 mol% to 10 mol% P2O5; and 10 mol% to 20 mol% KO.
[0022] In an embodiment (17), there is provided the glass of embodiment (15) or (16), further comprising: 0 mol % to 10 mol % CsO; and 0 mol % to 10 mol % RbO.
[0023] In an embodiment (18), there is provided the glass of any one of embodiments (15) to (17), wherein the glass is substantially free of lithium.
[0024] In an embodiment (19), there is provided the glass of any one of embodiments (15) to (18), wherein the glass is substantially free of sodium.
[0025] In an embodiment (20), there is provided the glass of any one of embodiments (15) through (19), comprising: from 58 mol% to 63 mol% SiO; from 7 mol% to 14 mol% AlO; from 7 mol% to 10 mol% PO; and from 15 mol% to 20 mol% KO.
[0026] In an embodiment (21), there is provided the glass of any one of embodiments (15) to (20), wherein the glass has a Vickers crack initiation threshold of 5 kgf (about 49 N) or greater.
[0027] In an embodiment (22), there is provided the glass of any one of embodiments (15) to (21), further comprising at least one of Li2O, Na2O, Cs2O, and Rb2O.
[0028] In an embodiment (23), a glass is provided, the glass comprising: 45 mol% to 75 mol% SiO2; 3 mol% to 20 mol% Al2O3; 4 mol% to 15 mol% P2O5; and 11 mol% to 25 mol% K2O.
[0029] In an embodiment (24), there is provided the glass of embodiment (23), comprising: from 55 mol% to 69 mol% SiO; from 5 mol% to 15 mol% AlO; from 5 mol% to 10 mol% PO; and from 11 mol% to 20 mol% KO.
[0030] In embodiment (25), there is provided the glass of embodiment (23) or (24), further comprising: equal to or greater than 0 mol % and equal to or less than 10 mol % CsO; and equal to or greater than 0 mol % and equal to or less than 10 mol % RbO.
[0031] In an embodiment (26), there is provided the glass of any one of embodiments (23) to (25), wherein the glass is substantially free of lithium.
[0032] In an embodiment (27), there is provided the glass of any one of embodiments (23) to (26), wherein the glass is substantially free of sodium.
[0033] In embodiment (28), there is provided the glass of any one of embodiments (23) through (27), comprising: from 58 mol% to 63 mol% SiO; from 7 mol% to 14 mol% AlO; from 7 mol% to 10 mol% PO; and from 15 mol% to 20 mol% KO.
[0034] In an embodiment (29), there is provided the glass of any one of embodiments (23) through (28), wherein the glass has a Vickers crack initiation threshold of 5 kgf (about 49 N) or greater.
[0035] In an embodiment (30), there is provided the glass of any one of embodiments (23) to (29), further comprising at least one of Li2O, Na2O, Cs2O, and Rb2O.
[0036] In an embodiment (31), a method is provided. The method includes exposing a glass-based substrate to an environment having a relative humidity of 75% or more to form a glass-based article having a hydrogen-containing layer extending from a surface of the glass-based article to a depth of the layer. The glass-based substrate includes SiO2, Al2O3, and PO5. The hydrogen concentration of the hydrogen-containing layer decreases from a maximum hydrogen concentration toward the depth of the layer, and the depth of the layer is greater than 5 μm.
[0037] In an embodiment (32), there is provided the method of embodiment (31), wherein the glass-based substrate has a composition including 55 mol% to 69 mol% SiO2; 5 mol% to 15 mol% Al2O3; 6 mol% to 10 mol% P2O5; and 10 mol% to 20 mol% KO.
[0038] In an embodiment (33), there is provided the method of embodiment (31), wherein the glass-based substrate has a composition including 45 mol% to 75 mol% SiO2; 3 mol% to 20 mol% Al2O3; 4 mol% to 15 mol% P2O5; and 11 mol% to 25 mol% KO.
[0039] In an embodiment (34), there is provided the method of embodiment (31), wherein the glass-based substrate has a composition including 45 mol% to 75 mol% SiO2; 3 mol% to 20 mol% Al2O3; 6 mol% to 15 mol% P2O5; and 6 mol% to 25 mol% KO.
[0040] In an embodiment (35), there is provided the method of any one of embodiments (31) to (34), wherein the glass-based substrate further comprises: 0 mol% to 10 mol% CsO; and 0 mol% to 10 mol% RbO.
[0041] In an embodiment (36), there is provided the method of any one of embodiments (31) to (35), further comprising at least one of Li2O, Na2O, Cs2O, and Rb2O.
[0042] In an embodiment (37), there is provided the method of any one of embodiments (31) to (36), wherein the glass-based article is substantially free of at least one of lithium and sodium.
[0043] In an embodiment (38), there is provided the method according to any one of embodiments (31) to (37), wherein the exposing is performed at a temperature of 70° C. or higher.
[0044] In an embodiment (39), there is provided the method of any one of embodiments (31) to (38), wherein the glass-based article has a Vickers crack initiation threshold of 1 kgf (about 9.8 N) or greater.
[0045] These and other aspects, advantages and salient features will become apparent from the following detailed description, the accompanying drawings and the appended claims. [Brief description of the drawings]
[0046] [Figure 1] FIG. 1 is a cross-sectional view of a glass-based article according to one embodiment. [Figure 2A] FIG. 1 is a plan view of an exemplary electronic device incorporating any of the glass-based articles disclosed herein. [Figure 2B] FIG. 2B is a perspective view of the example electronic device of FIG. 2A. [Diagram 3] FIG. 1 shows SIMS measurements of hydrogen concentration as a function of depth below the generated surface for glass-based articles formed from glass-based substrates having the composition of Example 1. [Figure 4] FIG. 2 is a photograph showing a Vickers indentation at 5 kgf (about 49 N) in a glass-based substrate having the composition of Example 1 before exposure to a water-containing environment. [Diagram 5] FIG. 2 is a photograph showing a Vickers indentation at 10 kgf (approximately 98 N) on a glass-based substrate having the composition of Example 1 before exposure to a water-containing environment. [Figure 6] FIG. 2 is a photograph of a Vickers indentation at 5 kgf (about 49 N) in a glass-based article formed by exposing a glass-based substrate having the composition of Example 1 to a water-containing environment. [Figure 7] FIG. 2 is a photograph of a Vickers indentation at 10 kgf (approximately 98 N) in a glass-based article formed by exposing a glass-based substrate having the composition of Example 1 to a water-containing environment. [Figure 8] FIG. 2 is a photograph of a Vickers indentation at 20 kgf (approximately 196 N) in a glass-based article formed by exposing a glass-based substrate having the composition of Example 1 to a water-containing environment. [Figure 9] FIG. 2 illustrates a plot of hydroxyl (βOH) concentration of a 0.5 mm thick glass article as a function of depth from the surface after exposure to a water-containing environment, according to one embodiment. [Figure 10] FIG. 2 illustrates a plot of hydroxyl (βOH) concentration of a 1.0 mm thick glass article as a function of depth from the surface after exposure to a water-containing environment, according to one embodiment. [Figure 11] FIG. 2 is a side view of the ring-on-ring test apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0047] In the following description, like reference characters indicate like or corresponding parts throughout the figures from several defined positions shown in the figures. It is also understood that, unless otherwise stated, terms such as "upper", "lower", "external", "internal" and the like are words of convenience and should not be construed as limiting terms. Unless otherwise stated, ranges of values include both the upper and lower limits of the range, as well as any subranges therebetween, when recited. As used herein, the indefinite articles "a", "an" and the corresponding definite article "the" mean "at least one" or "one or more", unless otherwise stated. It is also understood that the various features disclosed in the specification and drawings can be used in any combination.
[0048] As used herein, the term "glass-based" is used in its broadest sense and includes any body made in whole or in part of glass, including glass-ceramics (containing crystalline phases and residual amorphous glass phases). Unless otherwise noted, all compositions of glasses described herein are expressed in terms of mole percent (mol%) and components are provided on an oxide basis. Unless otherwise noted, all temperatures are expressed in degrees Celsius (°C).
[0049] It should be noted that the terms "substantially" and "about" may be utilized herein to express the inherent degree of uncertainty that may result from any quantitative comparison, value, measurement, or other representation. These terms are also utilized herein to express the extent to which a quantitative representation may vary from the stated standard without resulting in a change in the basic functionality of the subject matter at issue. For example, a glass that is "substantially free of K2O" is a glass in which K2O is not actively added or batched into the glass, but may be present as a contaminant in very small amounts, e.g., less than about 0.01 mole %. As used herein, when the term "about" is used to modify a value, the exact value is also disclosed. For example, the term "greater than about 10 mole %" also discloses "10 mole % or greater."
[0050] Reference will now be made in detail to various embodiments, examples of which are illustrated in the accompanying examples and drawings.
[0051] The glass-based articles disclosed herein include a hydrogen-containing layer extending from the surface to a layer depth of the article. The hydrogen-containing layer includes a hydrogen concentration that decreases from a maximum hydrogen concentration of the glass-based article toward the layer depth. In some embodiments, the maximum hydrogen concentration may be located at the surface of the glass-based article. The glass-based articles exhibit a Vickers indentation crack threshold (e.g., 1 kgf (about 9.8 N) or greater) without the use of conventional strengthening methods (e.g., ion exchange of a pair of alkali metal ions or thermal strengthening). A high Vickers indentation crack threshold exhibited by the glass-based article indicates high damage tolerance.
[0052] The glass-based article may be formed by exposing a glass-based substrate to an environment containing water vapor, which allows hydrogen species to permeate the glass-based substrate and form a glass-based article having a hydrogen-containing layer. As used herein, hydrogen species include molecular water, hydroxyl, hydrogen ions, and hydronium. The composition of the glass-based substrate may be selected to promote interdiffusion of hydrogen species into the glass. As used herein, the term "glass-based substrate" refers to the precursor prior to exposure to a water vapor-containing environment to form a glass-based article including a hydrogen-containing layer. Similarly, the term "glass-based article" refers to the article after exposure including a hydrogen-containing layer.
[0053] A representative cross-section of a glass-based article 100 according to some embodiments is shown in Figure 1. The glass-based article 100 has a thickness t extending between a first surface 110 and a second surface 112. A first hydrogen-containing layer 120 extends from the first surface 110 to a first layer depth, where the first layer depth has a depth d1 measured from the first surface 110 into the glass-based article 100. A second hydrogen-containing layer 122 extends from the second surface 112 to a second layer depth, where the second layer depth has a depth d2 measured from the second surface 112 into the glass-based article 100. A region 130 that does not include added hydrogen species exists between the first layer depth and the second layer depth.
[0054] The hydrogen-containing layer of the glass-based article may have a depth of layer (DOL) of greater than 5 μm. In some embodiments, the depth of layer is greater than 10 μm, e.g., greater than 15 μm, greater than 20 μm, greater than 25 μm, greater than 30 μm, greater than 35 μm, greater than 40 μm, greater than 45 μm, greater than 50 μm, greater than 55 μm, greater than 60 μm, greater than 65 μm, greater than 70 μm, greater than 75 μm, greater than 80 μm, greater than 85 μm, greater than 90 μm, greater than 95 μm, greater than 100 μm, greater than 105 μm, greater than 110 μm. or greater than 115 μm, or greater than 120 μm, or greater than 125 μm, or greater than 130 μm, or greater than 135 μm, or greater than 140 μm, or greater than 145 μm, or greater than 150 μm, or greater than 155 μm, or greater than 160 μm, or greater than 165 μm, or greater than 170 μm, or greater than 175 μm, or greater than 180 μm, or greater than 185 μm, or greater than 190 μm, or greater than 195 μm, or greater than 200 μm. In some embodiments, the layer depth is greater than 5 μm and less than or equal to 205 μm, e.g., from 10 μm to 200 μm, from 15 μm to 200 μm, from 20 μm to 195 μm, from 25 μm to 190 μm, from 30 μm to 185 μm, from 35 μm to 180 μm, from 40 μm to 175 μm, from 45 μm to 170 μm, from 50 μm to 165 μm, from 55 μm to 160 μm, from 60 μm to 70 μm, from 75 μm to 80 μm, from 85 μm to 90 μm, from 90 μm to 100 μm, from 95 μm to 100 μm, from 95 μm to 110 μm, from 95 μm to 120 μm, from 95 μm to 130 μm, from 95 μm to 140 μm, from 95 μm to 150 μm, from 95 μm to 160 μm, from 95 μm to 170 μm, from 95 μm to 180 μm, from 95 μm to 100 μm, from 95 μm to 110 μm, from 95 μm to 120 μm, from 95 μm to 140 μm, from 95 μm to 150 μm, from 95 μm to 160 μm, from 95 μm to 170 μm, from 95 μm to 180 μm, from 95 μm to 190 μm, from 95 μm to 100 μm, from 95 μm to 100 μm, from 95 μm The depth of layer may be from 0 to 155 μm, from 65 to 150 μm, from 70 to 145 μm, from 75 to 140 μm, from 80 to 135 μm, from 85 to 130 μm, from 90 to 125 μm, from 95 to 120 μm, from 100 to 115 μm, from 105 to 110 μm, or any subrange formed by any of these endpoints. Generally, the glass-based article exhibits a depth of layer that is greater than the depth of layer that may be produced by exposure to the ambient environment.
[0055] The hydrogen-containing layer of the glass-based article may have a depth of layer (DOL) greater than 0.005t, where t is the thickness of the glass-based article. In some embodiments, the depth of layer may be 0.010t or greater, e.g., 0.015t or greater, 0.020t or greater, 0.025t or greater, 0.030t or greater, 0.035t or greater, 0.040t or greater, 0.045t or greater, 0.050t or greater, 0.055t or greater, 0.060t or greater, 0.065t or greater, 0.070t or greater, 0.075t or greater, 0.080t or greater, 0.085t or greater, 0.090t or greater, 0.095t or greater, 0.10t or greater, 0.15t or greater, 0.20t or greater, or greater than 0.20t. In some embodiments, the DOL is greater than 0.005t and less than or equal to 0.205t, e.g., from 0.010t to 0.200t, from 0.015t to 0.195t, from 0.020t to 0.190t, from 0.025t to 0.185t, from 0.030t to 0.180t, from 0.035t to 0.175t, from 0.040t to 0.170t, from 0.045t to 0.165t, from 0.050t to 0.160t, from 0.055t The range may be up to and including 0.155t, from 0.060t to 0.150t, from 0.065t to 0.145t, from 0.070t to 0.140t, from 0.075t to 0.135t, from 0.080t to 0.130t, from 0.085t to 0.125t, from 0.090t to 0.120t, from 0.095t to 0.115t, from 0.100t to 0.110t, or any subrange formed by any of these endpoints.
[0056] Depth of layer and hydrogen concentration are measured by secondary ion mass spectrometry (SIMS) techniques known in the art. SIMS techniques can measure hydrogen concentration at a given depth, but cannot distinguish between hydrogen species present in the glass-based article. Thus, all hydrogen species contribute to the hydrogen concentration measured by SIMS. As used herein, depth of layer (DOL) refers to the first depth below the surface of the glass-based article, where the hydrogen concentration is equal to the hydrogen concentration at the center of the glass-based article. This definition takes into account the hydrogen concentration of the glass-based substrate before treatment, so depth of layer refers to the depth of hydrogen added by the treatment process. In practical terms, the hydrogen concentration at the center of the glass-based article can be approximated by the hydrogen concentration at a depth from the surface of the glass-based article where the hydrogen concentration is substantially constant, since the hydrogen concentration is expected to remain unchanged between such depth and the center of the glass-based article. This approximation allows the DOL to be determined without measuring the hydrogen concentration throughout the entire depth of the glass-based article.
[0057] In some embodiments, the entire thickness of the glass-based article may be part of the hydrogen-containing layer. Such a glass-based article may be produced when the treatment of the glass-based substrate continues for a sufficient time under sufficient conditions for hydrogen species to diffuse from each exposed surface to the center of the glass-based article. In some embodiments where the surfaces of the glass-based article are exposed to the same treatment conditions, the minimum hydrogen concentration may be located at half the thickness of the glass-based article, so that the hydrogen-containing layer contacts the center of the glass-based article. In such embodiments, the DOL may be located at half the thickness of the glass-based article. In some embodiments, the glass-based article may not include regions that do not contain added hydrogen species. In some embodiments, the glass-based article may be treated in a wet environment such that the concentration of added hydrogen species is equilibrated throughout the glass-based article, and the hydrogen concentration does not change with depth below the surface of the glass-based article. Because the hydrogen concentration at the center of the glass-based article is equivalent to the hydrogen concentration at all other depths, the glass-based article according to such embodiments does not exhibit a DOL as defined herein.
[0058] The glass-based article is highly resistant to Vickers indentation cracking. High Vickers indentation cracking resistance gives the glass-based article high damage resistance. Without wishing to be bound by a particular theory, the water content of the glass-based article can reduce the local viscosity of the hydrogen-containing layer, causing local flow instead of cracking. The Vickers indentation cracking threshold of the glass-based article is achieved without the use of traditional strengthening techniques, such as exchanging larger alkali metal ions in the glass for smaller alkali metal ions, thermal strengthening, or stacking glass layers using thermal expansion coefficient mismatch. Glass-based articles are generally 1 kgf (about 9.8 N) or more, for example, 2 kgf (about 19.6 N) or more, 3 kgf (about 29.4 N) or more, 4 kgf (about 39.2 N) or more, 5 kgf (about 49 N) or more, 6 kgf (about 58.8 N) or more, 7 kgf (about 68.6 N) or more, 8 kgf (about 78.4 N) or more, 9 kgf (about 88.2 N) or more, 10 kgf (about 98 N) or more, 11 kgf (about 107.8 N) or more, 12 kgf (about 117.6 N) or more, 13 kgf (about 127.4 N) or more, 14 kgf (about 137.2 N) or more, 15 kgf (about 147 N) or more, 16 kgf (about 156.8 N) or more, 17 kgf (about 166.6N) or more, 18kgf (about 176.4N) or more, 19kgf (about 186.2N) or more, 20kgf (about 196N) or more, 21kgf (about 205.8N) or more, 22kgf (about 215.6N) or more, 23kgf (about 225.4N) or more, 24kgf (about 235.2N) or more, 25kgf (about 245N) or more, 26kgf (about 254.8N) or more, 27kgf (about 264.6N) or more, 28kgf (about 274.4N) or more, 29kgf (about 284.2N) or more, 30kgf (about 294N) or more, or greater than 30kgf (about 294N).In some embodiments, the glass-based article has a compressibility of 1 kgf (about 9.8 N) or more and 30 kgf (about 294 N) or less, such as 2 kgf (about 19.6 N) or more and 29 kgf (about 284.2 N) or less, 3 kgf (about 29.4 N) or more and 28 kgf (about 274.4 N) or less, 4 kgf (about 39.2 N) or more and 27 kgf (about 264.6 N) or less, 5 kgf (about 49 N) or more and 26 kgf (about 254.8 N) or less, 6 kgf (about 58.8 N) or more and 25 kgf (about 245 N) or less, 7 kgf (about 68.6 N) or more and 24 kgf (about 235.2 N) or less, 8 kgf (about 78.4 N) or more and 23 kgf (about 225.4 N) or less, 9 kgf (about 100 N) or more and 10 ... In one embodiment, the Vickers indentation crack threshold is from 10 kgf (about 88.2 N) to 22 kgf (about 215.6 N), from 10 kgf (about 98 N) to 21 kgf (about 205.8 N), from 11 kgf (about 107.8 N) to 20 kgf (about 196 N), from 12 kgf (about 117.6 N) to 19 kgf (about 186.2 N), from 13 kgf (about 127.4 N) to 18 kgf (about 176.4 N), from 14 kgf (about 137.2 N) to 17 kgf (about 166.6 N), from 15 kgf (about 147 N) to 16 kgf (about 156.8 N), or any subrange formed by any of these endpoints.
[0059] The Vickers crack initiation threshold (or indentation failure threshold) was measured with a Vickers indenter. The Vickers crack initiation threshold is a measure of the indentation damage resistance of glass. A square-based pyramidal diamond indenter with an angle between the faces of 136°, called a Vickers indenter, was used in this test. The Vickers indenter was the same as that used in standard microhardness testing (described in ASTM-E384-11). A minimum of five specimens were selected to represent the glass type and / or sample of interest. For each specimen, multiple sets of five indentations were introduced into the specimen surface. Each set of five indentations was introduced at a given load, with each individual indentation spaced a minimum of 5 mm apart and not closer than 5 mm to the edge of the specimen. For test loads of 2 kg or greater, an indenter loading / unloading rate of 50 kg / min was used. For test loads less than 2 kg, a rate of 5 kg / min was used. A dwell (i.e., hold) time of 10 seconds at the target load was utilized. The machine maintained load control throughout the dwell period. After at least 12 hours, the indentations were inspected under reflected light at 500X magnification using a compound microscope. The presence or absence of a central / radial crack (a crack extending from the indentation along a plane perpendicular to the major plane of the article) or specimen failure was then recorded for each indentation. Note that because this test was focused on the formation of a central / radial crack or specimen failure, the formation of a transverse crack (a crack extending along a plane parallel to the major plane of the article) was not considered an indication of threshold behavior. The threshold for a specimen is defined as the midpoint of the lowest consecutive indentation load that collectively exceeds 50% of the individual indentations that meet the threshold. For example, if within an individual specimen, two out of five (40%) indentations induced by a load of 5 kg exceed the threshold and three out of five (60%) indentations induced by a load of 6 kg exceed the threshold, then the threshold for the specimen is defined as greater than 5 kg. The range of midpoint values (lowest to highest) for all specimens may also be reported for each sample. The environment before, during and after the test was controlled at 23±2°C and 50±5% RH to minimize variation in the fatigue (stress corrosion) behavior of the specimens.
[0060] Without wishing to be bound by any particular theory, the hydrogen-containing layer of the glass-based article may be the result of interdiffusion of hydrogen species of ions contained in the composition of the glass-based substrate. + and / or H + Monovalent hydrogen-containing species such as HO can replace alkali metal ions in glass-based substrate compositions to form glass-based articles. The size of the alkali metal ion that the hydrogen-containing species replaces contributes to the diffusivity of the hydrogen-containing species in the glass-based substrate, as larger alkali metal ions create larger interstitial spaces that facilitate interdiffusion mechanisms. For example, hydronium ions (HO + The ionic radius of ruthenium ions is close to that of potassium and much larger than that of lithium. The diffusion coefficient of hydrogen-containing species in glass-based substrates was observed to be significantly higher by two orders of magnitude when the glass-based substrate contained potassium than when it contained lithium. This observed behavior may also indicate that hydronium ions are the predominant monovalent hydrogen-containing species diffusing into the glass-based substrate. The ionic radii of alkali metal ions and hydronium ions are reported in Table I below. As shown in Table I, the ionic radii of rubidium and cesium are significantly larger than the hydronium ion, which may result in higher hydrogen diffusion coefficients than observed for potassium.
[0061] [Table 1]
[0062] In some embodiments, the replacement of alkali metal ions of a glass-based substrate with hydrogen-containing ions can produce a compressive stress layer that extends from the surface of the glass-based article to a compressive depth within the glass-based article. As used herein, depth of compression (DOC) refers to the depth at which the stress of the glass-based article changes from compressive to tensile. Thus, the glass-based article also includes a tensile stress region with a maximum central tension (CT) such that the forces within the glass-based article are balanced. Without wishing to be bound by theory, the compressive stress region may be the result of replacement with hydrogen-containing ions that have a larger ionic radius than the ions they replace.
[0063] In some embodiments, the compressive stress layer can include a compressive stress of 100 MPa or more, such as 105 MPa or more, 110 MPa or more, 115 MPa or more, 120 MPa or more, 125 MPa or more, 130 MPa or more, 135 MPa or more, or greater than 135 MPa. In some embodiments, the compressive stress layer can include a compressive stress of 100 MPa or more to 150 MPa or less, such as 105 MPa or more to 145 MPa or less, 110 MPa or more to 140 MPa or less, 115 MPa or more to 135 MPa or less, 120 MPa or more to 130 MPa or less, 125 MPa, or any subrange formed from any of these endpoints.
[0064] In some embodiments, the DOC of the compressive stress layer can be 75 μm or more, such as 80 μm or more, 85 μm or more, 90 μm or more, 95 μm or more, 100 μm or more, or greater than 100 μm. In some embodiments, the DOC of the compressive stress layer can be 75 μm or more and 115 μm or less, such as 80 μm or more and 110 μm or less, 85 μm or more and 105 μm or less, 90 μm or more and 100 μm or less, 95 μm, or any subrange that can be formed from any of these endpoints.
[0065] In some embodiments, the glass-based article can have a DOC of 0.05t or greater, where t is the thickness of the glass-based article, e.g., 0.06t or greater, 0.07t or greater, 0.08t or greater, 0.09t or greater, 0.10t or greater, 0.11t or greater, 0.12t or greater, or greater than 0.12t. In some embodiments, the glass-based article can have a DOC of 0.05t or greater and 0.20t or less, e.g., 0.06t or greater and 0.19t or less, 0.07t or greater and 0.18t or less, 0.08t or greater and 0.17t or less, 0.09t or greater and 0.16t or less, 0.10t or greater and 0.15t or less, 0.11t or greater and 0.14t or less, 0.12t or greater and 0.13t or less, or any subrange formed from any of these endpoints.
[0066] In some embodiments, the CT of the glass-based article can be 10 MPa or more, such as 11 MPa or more, 12 MPa or more, 13 MPa or more, 14 MPa or more, 15 MPa or more, 16 MPa or more, 17 MPa or more, 18 MPa or more, 19 MPa or more, 20 MPa or more, 22 MPa or more, 24 MPa or more, 26 MPa or more, 28 MPa or more, 30 MPa or more, 32 MPa or more, or more than 32 MPa. In some embodiments, the CT of the glass-based article can be 10 MPa or more to 35 MPa or less, such as 11 MPa or more to 34 MPa or less, 12 MPa or more to 33 MPa or less, 13 MPa or more to 32 MPa or less, 14 MPa or more to 32 MPa or less, 15 MPa or more to 31 MPa or less, 16 MPa or more to 30 MPa or less, 17 MPa or more to 28 MPa or less, 18 MPa or more to 26 MPa or less, 19 MPa or more to 24 MPa or less, 20 MPa or more to 22 MPa or less, or any subrange formed from any of these endpoints.
[0067] Compressive stress (including surface CS) is measured with a surface stress meter using commercially available equipment such as the FSM-6000 (FSM) manufactured by Orihara Seisakusho Co., Ltd. (Japan). Surface stress measurements rely on accurate measurement of the stress optical coefficient (SOC), which is related to the birefringence of the glass. SOC is also measured according to procedure C (glass disk method) as described in ASTM standard C770-16, entitled "Standard Test Method for Measurement of the Stress-Optical Coefficient of Glass," the contents of which are incorporated herein by reference in their entirety. DOC is measured with the FSM. Maximum central tension (CT) values are measured using the Scattered Light Polariscope (SCALP) technique known in the art.
[0068] The glass-based article may be formed from a glass-based substrate having any suitable composition. The composition of the glass-based substrate may be specifically selected to promote the diffusion of hydrogen-containing species, so that a glass-based article including a hydrogen-containing layer may be efficiently formed. In some embodiments, the glass-based substrate may have a composition including SiO2, Al2O3, and P2O5. In some embodiments, the glass-based substrate may further include at least one of an alkali metal oxide, such as Li2O, Na2O, KO, Rb2O, and Cs2O. In some embodiments, the glass-based substrate may be substantially free or free of at least one of lithium and sodium. In some embodiments, after diffusion of the hydrogen-containing species into the glass-based substrate, the glass-based article may have a bulk composition that is approximately the same as the composition of the glass-based substrate. In some embodiments, the hydrogen species may not diffuse to the center of the glass-based article. In other words, the center of the glass-based article is the area least affected by the water vapor treatment. Thus, the center of the glass-based article may have a composition that is substantially the same or the same as the composition of the glass-based substrate before treatment in a water-containing environment.
[0069] The glass-based substrate may contain any suitable amount of SiO2. SiO2 is the largest component, and therefore SiO2 is the main component of the glass network formed from the glass composition. If the concentration of SiO2 in the glass composition is too high, the formability of the glass composition may decrease. This is because a higher concentration of SiO2 makes it more difficult to melt the glass, which also negatively affects the formability of the glass. In some embodiments, the glass-based substrate may include SiO2 in an amount of 45 mol% or more and 75 mol% or less, for example, 46 mol% or more and 74 mol% or less, 47 mol% or more and 73 mol% or less, 48 mol% or more and 72 mol% or less, 49 mol% or more and 71 mol% or less, 50 mol% or more and 70 mol% or less, 51 mol% or more and 69 mol% or less, 52 mol% or more and 68 mol% or less, 53 mol% or more and 67 mol% or less, 54 mol% or more and 66 mol% or less, 55 mol% or more and 65 mol% or less, 56 mol% or more and 64 mol% or less, 57 mol% or more and 63 mol% or less, 58 mol% or more and 62 mol% or less, 59 mol% or more and 61 mol% or less, 60 mol%, or any subrange formed by any of these endpoints. In some embodiments, the glass-based substrate may include SiO2 in an amount of 55 mol% or more and 69 mol% or less, for example, 58 mol% or more and 63 mol% or less, or any subrange formed by any of these endpoints.
[0070] The glass-based substrate may include any suitable amount of Al2O3. Al2O3 may function as a glass network former similar to SiO2. Al2O3 increases the viscosity of the glass composition due to its tetrahedral coordination in the glass melt formed from the glass composition, and if the amount of Al2O3 is too high, the formability of the glass composition decreases. However, when the concentration of Al2O3 is balanced with the concentration of SiO2 and the concentration of alkali metal oxides in the glass composition, Al2O3 can lower the liquidus temperature of the glass melt, thereby increasing the liquidus viscosity and improving the compatibility of the glass composition with certain forming processes, such as melt forming processes. The inclusion of Al2O3 in the glass-based substrate prevents phase separation and reduces the number of non-bridging oxygens (NBOs) in the glass. In addition, Al2O3 can improve the effect of ion exchange. In some embodiments, the glass-based substrate may include Al2O3 in an amount of 3 mol% or more and 20 mol% or less, such as 4 mol% or more and 19 mol% or less, 5 mol% or more and 18 mol% or less, 6 mol% or more and 17 mol% or less, 7 mol% or more and 16 mol% or less, 8 mol% or more and 15 mol% or less, 9 mol% or more and 14 mol% or less, 10 mol% or more and 13 mol% or less, 11 mol% or more and 12 mol% or less, or any subrange formed by any of these endpoints. In some embodiments, the glass-based substrate may include Al2O3 in an amount of 5 mol% or more and 15 mol% or less, such as 7 mol% or more and 14 mol% or less, or any subrange formed by any of these endpoints.
[0071] The glass-based substrate may include any amount of P2O5 sufficient to provide a desired hydrogen diffusion coefficient. The inclusion of phosphorus in the glass-based substrate promotes faster interdiffusion, regardless of the pair of ions exchanged. Thus, phosphorus-containing glass-based substrates allow for efficient formation of glass-based articles including hydrogen-containing layers. The inclusion of P2O5 also allows for the manufacture of glass-based articles with deep layers (e.g., greater than about 10 μm) with relatively short processing times. In some embodiments, the glass-based substrate may include P2O5 in an amount of 4 mol% or more and 15 mol% or less, such as 5 mol% or more and 14 mol% or less, 6 mol% or more and 13 mol% or less, 7 mol% or more and 12 mol% or less, 8 mol% or more and 11 mol% or less, 9 mol% or more and 10 mol% or less, or any subrange formed by any of these endpoints. In some embodiments, the glass-based substrate can include P2O5 in an amount of 5 mol% or more and 15 mol% or less, such as 6 mol% or more and 15 mol% or less, 5 mol% or more and 10 mol% or less, 6 mol% or more and 10 mol% or less, 7 mol% or more and 10 mol% or less, or any subrange formed by any of these endpoints.
[0072] The glass-based substrate may include any suitable amount of alkali metal oxide. The alkali metal oxide promotes ion exchange. The alkali metal oxides in the glass composition (e.g., Li2O, Na2O, and K2O, as well as other alkali metal oxides including Cs2O and Rb2O) may be collectively referred to as "R2O", and R2O may be expressed in mole percent. In some embodiments, the glass-based substrate may be substantially free or free of at least one of lithium and sodium. In an embodiment, the glass composition includes R2O in an amount of 6 mol% or more, such as 7 mol% or more, 8 mol% or more, 9 mol% or more, 10 mol% or more, 11 mol% or more, 12 mol% or more, 13 mol% or more, 14 mol% or more, 15 mol% or more, 16 mol% or more, 17 mol% or more, 18 mol% or more, 19 mol% or more, 20 mol% or more, 21 mol% or more, 22 mol% or more, 23 mol% or more, or 24 mol% or more. In one or more embodiments, the glass composition includes RO in an amount of 25 mol% or less, e.g., 24 mol% or less, 23 mol% or less, 22 mol% or less, 21 mol% or less, 20 mol% or less, 19 mol% or less, 18 mol% or less, 17 mol% or less, 16 mol% or less, 15 mol% or less, 14 mol% or less, 13 mol% or less, 12 mol% or less, 11 mol% or less, 10 mol% or less, 9 mol% or less, 8 mol% or less, or 7 mol% or less. It should be understood that any of the above ranges may be combined with any other range in an embodiment. In some embodiments, the glass composition comprises RO in an amount of from 6.0 mol% to 25.0 mol%, e.g., from 7.0 mol% to 24.0 mol%, from 8.0 mol% to 23.0 mol%, from 9.0 mol% to 22.0 mol%, from 10.0 mol% to 21.0 mol%, from 11.0 mol% to 20.0 mol%, from 12.0 mol% to 19.0 mol%, from 13.0 mol% to 18.0 mol%, from 14.0 mol% to 17.0 mol%, or from 15.0 mol% to 16.0 mol%, and all ranges and subranges between the aforesaid values.
[0073] In some embodiments, the alkali metal oxide can be KO. The inclusion of KO allows for efficient exchange of hydrogen species into the glass substrate when exposed to a water-containing environment. In embodiments, the glass-based substrate can include KO in an amount of 6 mol% to 25 mol%, such as 7 mol% to 24 mol%, 8 mol% to 23 mol%, 9 mol% to 22 mol%, 10 mol% to 21 mol%, 11 mol% to 20 mol%, 12 mol% to 19 mol%, 13 mol% to 18 mol%, 14 mol% to 17 mol%, 15 mol% to 16 mol%, or any subrange formed from any of these endpoints. In some embodiments, the glass-based substrate can include KO in an amount of 10 mol% or more and 25 mol% or less, such as 10 mol% or more and 20 mol% or less, 11 mol% or more and 25 mol% or less, 11 mol% or more and 20 mol% or less, 15 mol% or more and 20 mol% or less, or any subrange formed from any of these endpoints.
[0074] The glass-based substrate may include RbO in any suitable amount. In some embodiments, the glass-based substrate may include RbO in an amount of 0 mol% or more and 10 mol% or less, such as 1 mol% or more and 9 mol% or less, 2 mol% or more and 8 mol% or less, 3 mol% or more and 7 mol% or less, 4 mol% or more and 6 mol% or less, 5 mol%, or any subrange formed from any of these endpoints.
[0075] The glass-based substrate may include CsO in any suitable amount. In some embodiments, the glass-based substrate may include CsO in an amount of 0 mol% or more and 10 mol% or less, such as 1 mol% or more and 9 mol% or less, 2 mol% or more and 8 mol% or less, 3 mol% or more and 7 mol% or less, 4 mol% or more and 6 mol% or less, 5 mol%, or any subrange formed from any of these endpoints.
[0076] In some embodiments, the glass-based substrate may have a composition including 45 mol% to 75 mol% SiO, 3 mol% to 20 mol% AlO, 6 mol% to 15 mol% PO, and 6 mol% to 25 mol% KO.
[0077] In some embodiments, the glass-based substrate may have a composition including 45 mol% to 75 mol% SiO, 3 mol% to 20 mol% AlO, 4 mol% to 15 mol% PO, and 11 mol% to 25 mol% KO.
[0078] In some embodiments, the glass-based substrate may have a composition including 55 mol% to 69 mol% SiO, 5 mol% to 15 mol% AlO, 6 mol% to 10 mol% PO, and 10 mol% to 20 mol% KO.
[0079] In some embodiments, the glass-based substrate may have a composition including 55 mol% to 69 mol% SiO, 5 mol% to 15 mol% AlO, 5 mol% to 10 mol% PO, and 11 mol% to 20 mol% KO.
[0080] In some embodiments, the glass-based substrate may have a composition including 58 mol% to 63 mol% SiO, 7 mol% to 14 mol% AlO, 7 mol% to 10 mol% PO, and 15 mol% to 20 mol% KO.
[0081] In some embodiments, the glass-based substrate may exhibit a Vickers crack initiation threshold of 5 kgf (about 49 N) or more, e.g., 6 kgf (about 58.8 N) or more, 7 kgf (about 68.6 N) or more, 8 kgf (about 78.4 N) or more, 9 kgf (about 88.2 N) or more, 10 kgf (about 98 N) or more, or greater than 10 kgf (about 98 N).
[0082] The glass-based substrate may have any suitable shape. In some embodiments, the glass-based substrate may have a thickness of 2 mm or less, such as 1 mm or less, 900 μm or less, 800 μm or less, 700 μm or less, 600 μm or less, 500 μm or less, 400 μm or less, 300 μm or less, or less than 300 μm. In some embodiments, the glass-based substrate may be in a plate or sheet shape. In some other embodiments, the glass-based substrate may have a 2.5D or 3D shape. As used herein, a "2.5D shape" refers to a sheet-shaped article in which at least one major surface is at least partially non-planar and the second major surface is substantially planar. As used herein, a "3D shape" refers to an article having first and second opposing major surfaces that are at least partially non-planar.
[0083] Glass-based articles can be produced from glass-based substrates by exposure to water vapor under any suitable conditions. Exposure can be performed in any suitable apparatus, such as an oven with relative humidity control. In some embodiments, the glass-based substrate can be exposed to an environment having a relative humidity of 75% or more, such as 80% or more, 85% or more, 90% or more, 95% or more, 99% or more, or more than 99%. In some embodiments, the glass-based substrate can be exposed to an environment having a relative humidity of 100%.
[0084] In some embodiments, the glass-based substrate may be exposed to an environment at a temperature of 70°C or higher, e.g., 75°C or higher, 80°C or higher, 85°C or higher, 90°C or higher, 95°C or higher, 100°C or higher, 105°C or higher, 110°C or higher, 115°C or higher, 120°C or higher, 125°C or higher, 130°C or higher, 135°C or higher, 140°C or higher, 145°C or higher, 150°C or higher, 155°C or higher, 160°C or higher, 160°C or higher, 165°C or higher, 170°C or higher, 175°C or higher, 180°C or higher, 185°C or higher, 190°C or higher, 195°C or higher, 200°C or higher, or greater than 200°C. In some embodiments, the glass-based substrate may be exposed to an environment at a temperature of 70° C. or more and 210° C. or less, e.g., 75° C. or more and 205° C. or less, 80° C. or more and 200° C. or less, 85° C. or more and 195° C. or less, 90° C. or more and 190° C. or less, 95° C. or more and 185° C. or less, 100° C. or more and 180° C. or less, 105° C. or more and 175° C. or less, 110° C. or more and 170° C. or less, 115° C. or more and 165° C. or less, 120° C. or more and 160° C. or less, 125° C. or more and 155° C. or less, 130° C. or more and 150° C. or less, 135° C. or more and 145° C. or less, 140° C., or any subrange formed from these endpoints.
[0085] In some embodiments, the glass-based substrate can be exposed to the water vapor-containing environment for a time sufficient to provide a desired degree of diffusion of hydrogen-containing species and a desired layer depth. In some embodiments, the glass-based substrate can be exposed to the water vapor-containing environment for 1 day or more, such as 2 days or more, 3 days or more, 4 days or more, 5 days or more, 6 days or more, 7 days or more, 8 days or more, 9 days or more, 10 days or more, 15 days or more, 20 days or more, 25 days or more, 30 days or more, 35 days or more, 40 days or more, 45 days or more, 50 days or more, 55 days or more, 60 days or more, 65 days or more, or more than 65 days. In some embodiments, the glass-based substrate can be exposed to the water vapor-containing environment for a period of 1 to 70 days, such as 2 to 65 days, 3 to 60 days, 4 to 55 days, 5 to 45 days, 6 to 40 days, 7 to 35 days, 8 to 30 days, 9 to 25 days, 10 to 20 days, 15 days, or any subrange formed from any of these endpoints. The exposure conditions can be modified to reduce the time required to achieve a desired amount of diffusion of hydrogen-containing species into the glass-based substrate. For example, the temperature and / or relative humidity can be increased to reduce the time required to achieve a desired degree of diffusion and depth of layer of hydrogen-containing species into the glass-based substrate.
[0086] The glass-based articles disclosed herein may be incorporated into another article, such as an article with a display (or display article) (e.g., consumer electronics including mobile phones, tablets, computers, navigation systems, wearable devices (e.g., watches), etc.), a building article, a transportation article (e.g., automobiles, trains, aircraft, watercraft, etc.), a specialized appliance article, or any article that requires some degree of transparency, scratch resistance, abrasion resistance, or combinations thereof. An exemplary article incorporating any of the glass-based articles disclosed herein is shown in Figures 2A and 2B. Specifically, Figures 2A and 2B show a consumer electronic device 200 including a housing 202 having a front surface 204, a back surface 206, and a side surface 208; electrical components (not shown) at least partially within or entirely within the housing, and including at least a controller, memory, and a display 210 disposed at or adjacent to the front surface of the housing; and a cover substrate 212 disposed at or over the front surface of the housing to cover the display. In some embodiments, at least a portion of one of the cover substrate 212 and the housing 202 may include any of the glass-based articles disclosed herein.
[0087] Exemplary embodiments Glass compositions particularly suitable for forming glass-based articles as described herein were formed into glass-based substrates. The compositions of Examples 1-6 are set forth in Table II below. Density was determined using the buoyancy method of ASTM C693-93(2013). The coefficient of linear thermal expansion (CTE) over the temperature range of 25°C to 300°C was 10 -7 The viscosity is expressed in units of 1 / °C and was determined using a push rod dilatometer in accordance with ASTM E228-11. The strain point and annealing point were determined using the beam bending viscosity method of ASTM C598-93(2013). The softening point was determined using the parallel plate viscosity method of ASTM C1351M-96(2012). The temperatures at which the viscosity of the glass was 200P, 35,000P and 200,000P were determined for the resulting compositions in accordance with ASTM C965-96(2012), entitled "Standard Practice for Measuring the Viscosity of Glasses Above Their Softening Points."
[0088] [Table 2]
[0089] A glass-based substrate comprising the composition of Example 1 and having a thickness of 1 mm was exposed to an environment of 85% relative humidity for 65 days to form a glass-based article comprising a hydrogen-containing layer of the type described herein.
[0090] The hydrogen-containing layer depth was measured by SIMS before and after exposure. The results of the SIMS hydrogen concentration measurements are shown in Figure 3, where the hydrogen concentration curve 301 for the untreated glass-based substrate has a layer depth of about 5 μm and the hydrogen concentration curve 302 for the glass-based article has a layer depth of about 30 μm. The exposed glass-based article was measured to a depth of about 25 μm and the layer depth was determined by extrapolating the curve 303. The hydrogen diffusion coefficient (D) was calculated based on the measurements using the general formula DOL = √(D x time).
[0091] The Vickers indentation crack threshold was measured before and after exposure to the water vapor-containing environment. The Vickers indentation results of the glass-based substrate before exposure are shown in Figures 4 and 5 after indentation with 5 kgf (about 49 N) and 10 kgf (about 98 N), respectively. As shown in Figures 4 and 5, the glass-based substrate had a Vickers crack initiation threshold higher than 5 kgf (about 49 N) but lower than 10 kgf (about 98 N). The Vickers indentation results of the exposed glass-based article are shown in Figures 6, 7, and 8 after indentation with 5 kgf (about 49 N), 10 kgf (about 98 N), and 20 kgf (about 196 N), respectively. As shown in Figures 6, 7, and 8, the Vickers indentation crack threshold of the glass-based article was greater than 20 kgf (about 196 N).
[0092] Glass-based substrates containing the compositions of Comparative Examples 1-3 and having a thickness of 1 mm were also prepared and exposed to an environment of 85% relative humidity for 30 days. The compositions of Comparative Examples 1-3 are reported in Table III below. The Vickers indentation crack threshold was measured before and after exposure to the water vapor-containing environment, and the hydrogen-containing layer depth was measured by SIMS after exposure. The hydrogen diffusion coefficient was calculated based on the measured values.
[0093] [Table 3]
[0094] As shown in Table III, the glass composition of Example 1 exhibited a hydrogen diffusion coefficient two orders of magnitude higher than the glass composition of Comparative Example 3, which also contained potassium but no phosphorus. These results indicate that the presence of phosphorus in the glass composition significantly increases the hydrogen diffusion coefficient. Similarly, the glass composition of Comparative Example 3 exhibited a hydrogen diffusion coefficient two orders of magnitude higher than Comparative Examples 1 and 2, which contained lithium and sodium, respectively. The difference in hydrogen diffusion coefficient between the potassium-containing glass composition and the lithium- and sodium-containing glass compositions indicates that the alkali metal ions with larger ionic radii allow for faster hydrogen diffusion.
[0095] Glass-based substrates comprising the glass composition of Example 6 were produced at thicknesses of 0.5 mm and 1.0 mm. The glass-based substrates were exposed to a 100% relative humidity environment at a temperature of 200° C. for 7 days to produce glass-based articles of the type described herein. The glass-based articles exhibited compressive stress regions extending from the surface to the compression depth. The 0.5 mm glass-based article had a maximum measured compressive stress of 124 MPa, and the 1.0 mm glass-based article had a maximum measured compressive stress of 137 MPa. The 0.5 mm glass-based article had a maximum measured central tension of 32 MPa, and the 1.0 mm glass-based article had a maximum measured central tension of 15 MPa. The 0.5 mm glass-based article had a compression depth of 101 μm, and the 1.0 mm glass-based article had a compression depth of 99 μm.
[0096] After exposure to a 100% relative humidity environment at 200° C. for 7 days, samples were cut from the center of 0.5 mm and 1.0 mm thick glass-based articles formed from glass-based substrates containing the glass composition of Example 6. The samples were then polished to a width of 0.5 mm and subjected to Fourier transform infrared spectroscopy (FTIR) analysis. The FTIR analysis was performed under the following conditions: CaF / InSb, 64 scans, 16 cm -1 The scan was performed with a resolution of 10 μm, an aperture of 10 μm, and a step of 10 μm. The scan started at the surface of the sample and continued to approximately the midpoint of the thickness. The spectrum was generated for "dry" silica, with a hydroxyl (βOH) concentration of 3900 cm -1 (max) and 3550cm -1 The plots report the concentration of the total hydroxyl content, since it was not possible to distinguish between bound and molecular hydroxyls due to the multicomponent nature of the glass-based articles. The measured hydroxyl concentration profiles for samples with thicknesses of 0.5 mm and 1.0 mm are shown in Figures 9 and 10, respectively. As shown in Figures 9 and 10, the depth into the sample where the measured hydroxyl content becomes substantially constant and equivalent to the hydroxyl content at the center of the article, which indicates the background hydroxyl content of the precursor glass-based substrate, was approximately 200 μm as measured by FTIR. The appearance of the buried hydroxyl concentration peak in Figures 9 and 10 is an artifact of the measurement method.
[0097] Square samples having the composition of Example 1 were prepared with a thickness of 1 mm and a side of 50 mm. Five of these samples were then treated at 200° C. for 121 hours in a 100% relative humidity environment. The compressive stress (CS) and depth of compression (DOC) of the treated samples were then measured by FSM, with a CS of 167 MPa and a DOC of 73 μm. The five steam-treated samples and three control samples that were not exposed to steam treatment were then subjected to an abrasive ring-on-ring (AROR) test. The strength and peak load of each tested sample are shown in Table IV. As shown in Table IV, the steam-treated samples showed significantly increased peak load and strength compared to the untreated control samples.
[0098] [Table 4]
[0099] The AROR test is a surface strength measurement for examining flat glass specimens, and ASTM C1499-09 (2013), entitled "Standard Test Method for Equibiaxial Bending Strength of Advanced Ceramics at Ambient Temperature", is the basis for the AROR test method used herein. The contents of ASTM C1499-09 are incorporated herein by reference in their entirety. The glass specimens are polished prior to ring-on-ring testing using 90 grit silicon carbide (SiC) particles delivered to the glass sample using the method and apparatus described in Appendix A2 entitled "Polishing Procedure" in ASTM C158-02 (2012), entitled "Standard Test Method for Strength of Glass in Bending (Measurement of Modulus of Rupture)". The contents of ASTM C158-02 and particularly Appendix 2 are incorporated herein by reference in their entirety.
[0100] The surfaces of the glass-based article samples were abraded prior to ring-on-ring testing as described in ASTM C158-02, Appendix 2, to normalize and / or control the surface defect condition of the samples using the apparatus shown in Figure A2.1 of ASTM C158-02. The abrasive is sandblasted onto the surface of the glass-based article at an air pressure of 5 psi (approximately 34 kPa). After the air flow is established, the abrasive is sandblasted at a pressure of 1 cm. 3 of abrasive is added to the funnel and the sample is sandblasted.
[0101] In the AROR test, a glass-based article having at least one wear surface is placed between two concentric rings of different sizes to measure equibiaxial bending strength (i.e., the maximum stress the material can withstand when subjected to bending between two concentric rings), as shown in Figure 11. In the AROR configuration 400, a polished glass-based article 410 is supported by a support ring 420 having a diameter D2. A force F is applied to the surface of the glass-based article by a load ring 430 having a diameter D1 via a load cell (not shown).
[0102] The ratio of the diameters of the load ring to the support ring, D1 / D2, can range from 0.2 to 0.5. In some embodiments, D1 / D2 is 0.5. The load ring 430 and the support ring 420 are desirably aligned concentrically to within 0.5% of the support ring diameter D2. The load cell used for testing is desirably accurate to within ±1% at any load within the selected range. Testing is performed at a temperature of 23±2° C. and a relative humidity of 40±10%.
[0103] In the fixture design, the radius r of the protruding surface of the loading ring 430 is in the range of h / 2≦r≦3h / 2, where h is the thickness of the glass-based article 410. The loading ring 430 and the support ring 420 are made of hardened steel with a hardness of HRc>40. The AROR fixture is commercially available.
[0104] The intended failure mechanism of the AROR test is to observe the failure of the glass-based article 410 originating at surface 430a within the loading ring 430. Failures occurring outside of this region, i.e., between the loading ring 430 and the support ring 420, are excluded from the data analysis. However, due to the thinness and high strength of the glass-based article 410, large deflections exceeding ½ of the specimen thickness h are sometimes observed. Thus, it is not uncommon to see a high percentage of failures originating below the loading ring 430. Without knowing the stress development both inside and below the ring (collected with strain gauge analysis) and the origin of failure for each specimen, the stress cannot be calculated accurately. Therefore, the AROR test focuses on the peak load at failure as the response to be measured.
[0105] Although exemplary embodiments have been described for purposes of illustration, the foregoing description should not be deemed to be limiting on the scope of the disclosure or the appended claims. Thus, various modifications, adaptations and alternatives may occur to those skilled in the art without departing from the spirit and scope of the disclosure or the appended claims.
[0106] Preferred embodiments of the present invention will be described below in detail.
[0107] EMBODIMENT 1 1. A glass-based article comprising: SiO2, Al2O3 and P2O5; and A hydrogen-containing layer extending from a surface of the glass-based article to a layer depth. Including, The hydrogen concentration of the hydrogen-containing layer decreases from a maximum hydrogen concentration toward the layer depth; and The glass-based article, wherein the depth of layer is greater than 5 μm.
[0108] EMBODIMENT 2 2. The glass-based article of embodiment 1, wherein the glass-based article has a Vickers crack initiation threshold of at least 1 kgf (about 9.8 N).
[0109] EMBODIMENT 3 3. The glass-based article of claim 1 or 2, wherein the depth of layer is at least about 10 μm.
[0110] EMBODIMENT 4 4. The glass-based article of any one of claims 1 to 3, wherein the maximum hydrogen concentration is located at a surface of the glass-based article.
[0111] EMBODIMENT 5 5. The glass-based article of any one of the preceding claims, further comprising at least one of Li2O, Na2O, K2O, Cs2O, and Rb2O.
[0112] EMBODIMENT 6 6. The glass-based article of any one of claims 1 to 5, further comprising K2O.
[0113] EMBODIMENT 7 The center of the glass-based article is 45 mol% or more and 75 mol% or less of SiO2; 3 mol% to 20 mol% Al2O3; 6 mol% to 15 mol% P2O5; and 6 mol% to 25 mol% K2O 7. The glass-based article of any one of claims 1 to 6, comprising:
[0114] EMBODIMENT 8 The center of the glass-based article is 45 mol% or more and 75 mol% or less of SiO2; 3 mol% to 20 mol% Al2O3; 4 mol% to 15 mol% P2O5; and 11 mol% to 25 mol% K2O 7. The glass-based article of any one of claims 1 to 6, comprising:
[0115] EMBODIMENT 9 The center of the glass-based article is SiO2 between 55 mol% and 69 mol%; 5 mol% to 15 mol% Al2O3; 6 mol% to 10 mol% P2O5; and 10 mol% to 20 mol% K2O 7. The glass-based article of any one of claims 1 to 6, comprising:
[0116] EMBODIMENT 10 The center of the glass-based article is 0 mol% to 10 mol% CsO; and 0 mol% to 10 mol% RbO 10. The glass-based article of any one of claims 7 to 9, comprising:
[0117] EMBODIMENT 11 11. The glass-based article of any one of the preceding claims, wherein the glass-based article is substantially free of at least one of lithium and sodium.
[0118] EMBODIMENT 12 12. The glass-based article of any one of claims 1 to 11, further comprising a compressive stress layer extending from a surface of the glass-based article to a compressive depth within the glass-based article.
[0119] EMBODIMENT 13 13. The glass-based article of embodiment 12, wherein the compressive stress layer comprises a compressive stress of 100 MPa or more, and the compression depth is 75 μm or more.
[0120] EMBODIMENT 14 A household electronic product, comprising: The housing, including the front, back and sides; electrical components at least partially within said housing, the electrical components including at least a controller, a memory, and a display, the display being disposed on or adjacent to a front surface of said housing; and A cover substrate disposed over the display wherein at least a portion of at least one of the housing or cover substrates comprises the glass-based article of any one of claims 1 to 13.
[0121] EMBODIMENT 15 A glass, 45 mol% or more and 75 mol% or less of SiO2; 3 mol% to 20 mol% Al2O3; 6 mol% to 15 mol% P2O5; and 6 mol% to 25 mol% K2O Including glass.
[0122] EMBODIMENT 16 SiO2 between 55 mol% and 69 mol%; 5 mol% to 15 mol% Al2O3; 6 mol% to 10 mol% P2O5; and 10 mol% to 20 mol% K2O 16. The glass of embodiment 15, comprising:
[0123] EMBODIMENT 17 0 mol% to 10 mol% CsO; and 0 mol% to 10 mol% RbO 17. The glass of embodiment 15 or 16, further comprising:
[0124] EMBODIMENT 18 18. The glass of any one of claims 15 to 17, wherein the glass is substantially free of lithium.
[0125] EMBODIMENT 19 19. The glass of any one of claims 15 to 18, wherein the glass is substantially free of sodium.
[0126] EMBODIMENT 20 SiO2 between 58 mol% and 63 mol%; 7 mol% or more and 14 mol% or less of Al2O3; 7 mol% to 10 mol% P2O5; and 15 mol% to 20 mol% K2O 20. The glass of any one of embodiments 15 to 19, comprising:
[0127] EMBODIMENT 21 21. The glass of any one of claims 15 to 20, wherein the glass has a Vickers crack initiation threshold of 5 kgf (about 49 N) or greater.
[0128] EMBODIMENT 22 22. The glass of any one of embodiments 15 to 17, 20 and 21, further comprising at least one of Li2O, Na2O, Cs2O and Rb2O.
[0129] EMBODIMENT 23 A glass, 45 mol% or more and 75 mol% or less of SiO2; 3 mol% to 20 mol% Al2O3; 4 mol% to 15 mol% P2O5; and 11 mol% to 25 mol% K2O Including glass.
[0130] EMBODIMENT 24 SiO2 between 55 mol% and 69 mol%; 5 mol% to 15 mol% Al2O3; 5 mol% to 10 mol% P2O5; and 11 mol% to 20 mol% K2O 24. The glass of embodiment 23, comprising:
[0131] EMBODIMENT 25 0 mol% to 10 mol% CsO; and 0 mol% to 10 mol% RbO 25. The glass of embodiment 23 or 24, further comprising:
[0132] EMBODIMENT 26 26. The glass of any one of claims 23 to 25, wherein the glass is substantially free of lithium.
[0133] EMBODIMENT 27 27. The glass of any one of claims 23 to 26, wherein the glass is substantially free of sodium.
[0134] EMBODIMENT 28 SiO2 between 58 mol% and 63 mol%; 7 mol% or more and 14 mol% or less of Al2O3; 7 mol% to 10 mol% P2O5; and 15 mol% to 20 mol% K2O 28. The glass of any one of embodiments 23 to 27, comprising:
[0135] EMBODIMENT 29 29. The glass of any one of claims 23 to 28, wherein the glass has a Vickers crack initiation threshold of 5 kgf (about 49 N) or greater.
[0136] EMBODIMENT 30 30. The glass of any one of embodiments 23 to 25, 28, and 29, further comprising at least one of Li2O, Na2O, Cs2O, and Rb2O.
[0137] EMBODIMENT 31 1. A method comprising: exposing the glass-based substrate to an environment having a relative humidity of 75% or greater to form a glass-based article having a hydrogen-containing layer extending from a surface of the glass-based article to a depth of the layer. Including, The glass-based substrate contains SiO2, Al2O3, and P2O5, The hydrogen concentration of the hydrogen-containing layer decreases from a maximum hydrogen concentration toward the layer depth; and The method, wherein the depth of layer is 5 μm or more.
[0138] EMBODIMENT 32 The glass-based substrate is SiO2 between 55 mol% and 69 mol%; 5 mol% to 15 mol% Al2O3; 6 mol% to 10 mol% P2O5; and 10 mol% to 20 mol% K2O 32. The method of embodiment 31, having a composition comprising:
[0139] EMBODIMENT 33 The glass-based substrate is 45 mol% or more and 75 mol% or less of SiO2; 3 mol% to 20 mol% Al2O3; 4 mol% to 15 mol% P2O5; and 11 mol% to 25 mol% K2O 32. The method of embodiment 31, having a composition comprising:
[0140] EMBODIMENT 34 The glass-based substrate is 45 mol% or more and 75 mol% or less of SiO2; 3 mol% to 20 mol% Al2O3; 6 mol% to 15 mol% P2O5; and 6 mol% to 25 mol% K2O 32. The method of embodiment 31, having a composition comprising:
[0141] EMBODIMENT 35 The glass-based substrate is 0 mol% to 10 mol% CsO; and 0 mol% to 10 mol% RbO 35. The method of any one of embodiments 31 to 34, further comprising:
[0142] EMBODIMENT 36 36. The method of any one of embodiments 31 to 35, further comprising at least one of Li2O, Na2O, Cs2O, and Rb2O.
[0143] EMBODIMENT 37 37. The method of any one of claims 31 to 36, wherein the glass-based article is substantially free of at least one of lithium and sodium.
[0144] EMBODIMENT 38 The method of any one of embodiments 31 to 37, wherein said exposing is performed at a temperature of 70° C. or higher.
[0145] EMBODIMENT 39 39. The method of any one of claims 31 to 38, wherein the glass-based article has a Vickers crack initiation threshold of 1 kgf (about 9.8 N) or greater.
Claims
1. A glass article strengthened by a water treatment, 11 mol% or more and 25 mol% or less of K 2 O The glass article comprises: A surface of the glass article, a hydrogen-containing layer extending from the surface of the glass article to a layer depth into the glass article; and a compressive stress layer of hydrogen species extending from the surface of the glass article to a compression depth into the glass article; Including, the depth of layer is a first depth below the surface where the hydrogen concentration matches the hydrogen concentration at a center of the glass article, and the compression depth is the depth at which stress in the glass article changes from compressive to tensile; The depth of the layer is greater than 5 μm from the surface, The compressive stress layer has a compressive stress of at least 100 MPa. Glass articles.
2. 10. The glass article of claim 1, wherein the hydrogen species comprises one or more of molecular water, hydroxyl, hydrogen ions, and hydronium.
3. 10. The glass article of claim 1, wherein the surface is a first surface of the glass article, the glass article further having a second surface and a thickness between the first surface and the second surface, and the depth of layer is greater than 0.005 times the thickness of the glass article.
4. 10. The glass article of claim 1 , wherein the surface is a first surface of the glass article, the glass article further having a second surface and a thickness between the first surface and the second surface, and the glass article has a 3D shape such that the first surface and the second surface are at least partially non-planar.
5. Electrical components, including displays; and A cover for covering the display; 13. A device comprising: at least a portion of the cover comprising the glass article of claim 1.
Citation Information
Patent Citations
Methods for enhancing strength and durability of a glass article
US20120277085A1
Dealkalization of glass surfaces
US3653864A
Degradable glass suitable for containers
US3811853A
Hydraulic cements prepared from glass powders
US4440576A