Manufacturing method of flame-resistant fiber and manufacturing method of carbon fiber
By optimizing heat treatment conditions in an oxidizing atmosphere and subsequent carbonization, the method addresses low yields in carbon fiber production, achieving high-quality carbon fibers with enhanced stability and mechanical properties.
Patent Information
- Application Number
- JP2023049176
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing methods for producing carbon fibers from acrylic fibers result in low yields due to decomposition products during the pre-carbonization step, as flame-retardant treatments may remain and cause yield loss, or incomplete cyclization reactions lead to unstable structures.
A method involving controlled heat treatment in an oxidizing atmosphere with specific conditions, including fiber density, heat input, and oxidizing gas concentration, followed by carbonization and optional graphitization, to enhance the yield of carbon fibers.
The method reduces decomposition products and enhances the yield of carbon fibers by promoting stable cyclization and dehydrogenation reactions, resulting in high-quality carbon fibers with improved mechanical properties.
Smart Images

Figure 2024138615000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an oxidation-resistant fiber and a method for producing a carbon fiber. [Background technology]
[0002] Acrylic fibers made of acrylonitrile copolymers are used as precursors for carbon fibers. The so-called PAN-based carbon fibers obtained from acrylic fibers as precursors have excellent mechanical properties and good productivity, and are therefore widely produced industrially. However, when acrylic fibers are converted into carbon fibers, heating causes a weight loss due to a decomposition reaction of the acrylonitrile copolymer, and the yield of carbon fiber obtained from the acrylic fibers is reduced to less than half, which has a significant impact on costs, so it is necessary to increase the yield.
[0003] For example, Patent Document 1 proposes obtaining a flame-retardant fiber by performing heat treatment in two stages, and describes a method in which an acrylic fiber material is flame-retardant treated in the presence of one or more compounds (flame-retardant treatment agents) selected from organic compounds other than amine compounds, fluorine compounds, siloxanes, nitrates, and nitrites, and then oxidized at 0 to 400°C in an oxidizing atmosphere. Patent Document 2 describes a method in which acrylic fibers are heat-treated in an inert atmosphere with an oxygen concentration of 0.01 to 3% by volume, and then heat-treated in an active atmosphere. It also describes that heat treatment in the active atmosphere at 220 to 320°C for about 3 to 10 minutes is sufficient. Patent Document 3 describes a method in which the pre-heat-treated fiber is subjected to low-temperature heat treatment in a non-oxidizing or weakly oxidizing atmosphere at a temperature of 300 to 500° C. for 0.3 minutes or more. The non-oxidizing atmosphere refers to helium, argon, etc., and mixtures thereof, and the weakly acidic atmosphere refers to an atmosphere in which non-oxidizing gas is mixed with 10% or less oxygen. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-3043 A [Patent Document 2] Japanese Patent Application Publication No. 7-292526 [Patent Document 3] Japanese Patent Application Publication No. 51-75124 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the method of Patent Document 1, the flame-retardant treatment agent used in the first heat treatment may remain in the flame-retardant fiber, and the remaining material will be decomposed in the pre-carbonization step, which will cause a low yield of carbon fiber. In the method of Patent Document 2, only the cyclization reaction proceeds in the first heat treatment with a low oxygen concentration, and there is almost no stable cyclization structure at this stage. In the second heat treatment, an oxidation-dehydrogenation reaction occurs rapidly on the surface side. For this reason, it is difficult to make the acrylic fiber have a thermally stable structure sufficiently inside. In the method of Patent Document 3, a reaction equivalent to the pre-carbonization step occurs simultaneously, and some parts decompose before the cyclization reaction, oxidation, or dehydrogenation reaction, resulting in a low yield of carbon fiber.
[0006] An object of the present invention is to provide a method for producing a flame-retardant fiber, which reduces the amount of decomposition products of the flame-retardant fiber in the pre-carbonization step compared to conventional methods, and enables carbon fiber to be obtained from polyacrylonitrile-based fiber in a high yield. [Means for solving the problem]
[0007] The present invention has the following aspects. [1] Polyacrylonitrile fibers in an oxidizing atmosphere until the fiber density reaches 1.35 g / cm 3 ~1.50g / cm 3 A method for producing a flame-retardant fiber, comprising a flame-retardant process. [2] In the flame retardant treatment, the fiber density is 1.22 g / cm 3The method for producing a flame-resistant fiber according to [1], further comprising heating the fiber so that the integrated heat value applied to the fiber from the time when the fiber becomes flame-resistant is within a range of 300 J·h / g to 1200 J·h / g. [3] The method for producing the flame-resistant fiber according to [1] or [2], comprising a flame-resistant step in which the oxidizing gas concentration in the oxidizing atmosphere is 1 volume % to 15 volume %. [4] The method for producing a flame-resistant fiber according to [3], wherein the heating temperature in the flame-resistant treatment is 230°C to 300°C. [5] The method for producing a flame-retardant fiber according to [3] or [4], wherein the heating time in the flame-retardant treatment is 1 minute to 80 minutes. [6] The method for producing a flame-resistant fiber according to any one of [1] to [5], wherein in the flame-resistant step, the flame-resistant fiber is obtained by heating the fiber in an air atmosphere at 230 to 245°C for 40 to 75 minutes, and then heating the fiber in an atmosphere having an oxidizing gas concentration of 1% by volume to 15% by volume for 1 to 40 minutes at 250°C to 300°C. [7] A method for producing carbon fibers, comprising heating a flame-resistant fiber produced by the method according to any one of [1] to [6] in an inert atmosphere at 1200°C to 3000°C to obtain carbon fibers. Effect of the Invention
[0008] According to the present invention, there is provided a method for producing a flame-retardant fiber, which reduces decomposition products of the flame-retardant fiber in the pre-carbonization step compared to conventional methods, and enables carbon fiber to be obtained in a high yield from polyacrylonitrile-based fiber. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Preferred embodiments of the present invention will now be described.
[0010] The method for producing the flame-resistant fiber of the present invention comprises the steps of: preparing a polyacrylonitrile fiber in an oxidizing atmosphere; 3 ~1.50g / cm 3 This includes a flame-proofing process in which the material is heated until it becomes flame-proof. When producing carbon fiber from acrylic fiber, the acrylic fiber is first heated to 200-300°C in an oxidizing atmosphere to form a flame-resistant fiber (flame-resistant process), and then heated at a higher temperature to form carbon fiber (carbonization process). In the carbonization process, heat treatment is generally performed in an inert gas at 1000-2000°C by a known technique. In addition, it is considered preferable to heat the fiber in an inert atmosphere furnace with an increasing temperature gradient of 400-700°C before the carbonization process (pre-carbonization process). In some cases, the carbon fiber thus obtained is further heated in a high-temperature inert gas to form graphite fiber. The reactions in the flame-proofing process for acrylic fibers are a cyclization reaction of the nitrile groups bonded to the polymer chains that make up the acrylic fibers, and a further reaction in which the structure is oxidized or dehydrogenated to change into a thermally stable molecular chain in which naphthyridine rings and acridone rings are combined. That is, in the flame-proofing reaction at 200 to 300°C, the acrylic fiber changes to a thermally stable structure due to the diffusion of oxygen from the surface. If the time of this flame-proofing reaction is extended, the structure changes to a thermally stable structure up to the center of the acrylic fiber. However, because the flame-proofing is carried out for 30 to 60 minutes for productivity reasons, the structure does not completely change to a thermally stable structure up to the inside of the acrylic fiber, although this depends on the diameter of the acrylic fiber. If the flameproofing time is extended, the acrylic fiber can have a thermally stable structure even inside, but extending the flameproofing time is not desirable from the viewpoint of productivity. Also, extending the flameproofing time too long in an oxidizing atmosphere is not desirable because it reduces the strength of the carbon fiber. In the flameproofing reaction, a cyclization reaction and an oxidation / dehydrogenation reaction occur simultaneously due to the diffusion of oxygen. Both reactions are exothermic. If the number of filaments is large, they may break during flameproofing due to heat accumulation.
[0011] (Precursor fiber) The precursor fiber used in one embodiment of the present invention may be an acrylic fiber spun by a known technique, specifically, an acrylic fiber obtained by spinning an acrylonitrile copolymer. An acrylonitrile copolymer is a polymer obtained by polymerizing acrylonitrile as a main monomer. The acrylonitrile copolymer may be a homopolymer obtained only from acrylonitrile, or an acrylonitrile copolymer using other monomers in addition to acrylonitrile as a main component. The content of acrylonitrile units in the acrylonitrile copolymer is preferably 96.0% by mass or more and 98.5% by mass or less in terms of preventing thermal fusion of fibers in the baking process, heat resistance of the copolymer, stability of the spinning dope, and quality when made into carbon fiber. When the acrylonitrile units are 96.0% by mass or more, the excellent quality and performance of the carbon fiber can be maintained without inviting thermal fusion of the fibers in the baking process when converted into carbon fiber, which is preferable. In addition, the heat resistance of the copolymer itself is not reduced, and adhesion between single fibers can be avoided in the process of drying the fibers or stretching with a heated roller or pressurized steam when spinning the precursor fiber. On the other hand, when the acrylonitrile units are 98.5% by mass or less, the solubility in the solvent is not reduced, the stability of the spinning dope can be maintained, and the precipitation and coagulation of the copolymer is not increased, which is preferable because it enables stable production of the precursor fiber.
[0012] In the case of using a copolymer, the monomer other than acrylonitrile can be appropriately selected from vinyl monomers copolymerizable with acrylonitrile. It is preferable to select from monomers such as acrylic acid, methacrylic acid, itaconic acid, or alkali metal salts or ammonium salts thereof, acrylamide, etc., which have the effect of promoting the flame retardancy reaction, because the flame retardancy can be promoted. As the vinyl monomer copolymerizable with acrylonitrile, a carboxyl group-containing vinyl monomer such as acrylic acid, methacrylic acid, itaconic acid, etc. is more preferable. The content of the carboxyl group-containing vinyl monomer unit in the acrylonitrile copolymer is preferably 0.5% by mass or more and 2.0% by mass or less. These vinyl monomers may be used alone or in combination of two or more kinds.
[0013] In spinning, the acrylonitrile polymer is dissolved in a solvent to prepare a spinning solution. The solvent can be appropriately selected from known solvents such as organic solvents such as dimethylacetamide, dimethylsulfoxide, and dimethylformamide, or aqueous solutions of inorganic compounds such as zinc chloride and sodium thiocyanate. Among these, dimethylacetamide, dimethylsulfoxide, and dimethylformamide, which have a fast coagulation rate, are preferred from the viewpoint of improving productivity, and dimethylacetamide is more preferred. In order to obtain a dense coagulated yarn, it is preferable to prepare the spinning dope so that the polymer concentration in the spinning dope is at a certain level or higher. Specifically, it is preferable to prepare the spinning dope so that the polymer concentration in the spinning dope is at least 17% by mass, and more preferably at least 19% by mass. Since the spinning dope needs to have appropriate viscosity and fluidity, it is preferable that the polymer concentration does not exceed 25% by mass.
[0014] The spinning method can be appropriately selected from known spinning methods such as a wet spinning method in which the above-mentioned spinning dope is directly spun into a coagulation bath, a dry spinning method in which the dope is coagulated in air, and a dry-wet spinning method in which the dope is spun once into air and then coagulated in a bath. In order to obtain carbon fibers having higher performance, the wet spinning method or the dry-wet spinning method is preferred. The spinning shaping by the wet spinning method or the dry-wet spinning method can be carried out by spinning the spinning dope into a coagulation bath from a nozzle having a circular cross-sectional hole. As the coagulation bath, it is preferable to use an aqueous solution containing the solvent used in the spinning dope from the viewpoint of ease of solvent recovery. The spinning method can be appropriately selected from known spinning methods such as a wet spinning method in which the above-mentioned spinning dope is directly spun into a coagulation bath, a dry spinning method in which the dope is coagulated in air, and a dry-wet spinning method in which the dope is spun once into air and then coagulated in a bath. In order to obtain carbon fibers having higher performance, the wet spinning method or the dry-wet spinning method is preferred.
[0015] The spinning shaping by the wet spinning method or the dry-wet spinning method can be carried out by spinning the spinning dope into a coagulation bath from a nozzle having a circular cross-sectional hole. As the coagulation bath, it is preferable to use an aqueous solution containing the solvent used in the spinning dope from the viewpoint of ease of solvent recovery. When an aqueous solution containing a solvent is used as the coagulation bath, the solvent concentration in the aqueous solution is preferably 50% by mass or more and 85% by mass or less, and the temperature of the coagulation bath is preferably 10° C. or more and 60° C. or less, for reasons such as that a dense structure without voids can be formed to obtain high-performance carbon fiber, and that stretchability can be ensured, resulting in excellent productivity. The polymer or copolymer is dissolved in a solvent, and the resulting spinning solution is discharged into a coagulation bath to form a coagulation fiber. The resulting coagulated fiber can then be stretched in a coagulation bath or a stretching bath. Alternatively, the fiber may be partially stretched in the air and then stretched in a bath. The fiber may be washed with water before, after or simultaneously with the stretching to obtain a precursor fiber in a water-swollen state.
[0016] The bath drawing is usually carried out in a water bath at 50°C to 98°C in one or more divided stages, and the coagulated yarn is drawn so that the total drawing ratio of the air drawing and the bath drawing is 2 to 10 times, which is preferable from the viewpoint of the properties of the obtained carbon fiber. To apply an oil to the coagulated yarn (water-swollen precursor fiber) stretched in a bath, it is preferable to use an oil treatment liquid for carbon fiber precursor acrylic fibers (hereinafter also referred to simply as "oil treatment liquid") in which an oil composition containing an oil is dispersed in water. The average particle size of the dispersed oil composition is preferably 0.01 μm or more and 0.3 μm or less. If the average particle size of the dispersed oil composition is within the above range, the oil can be applied more uniformly to the surface of the precursor fiber.
[0017] The precursor fibers in a water-swollen state to which the oil agent has been applied are dried and densified in the subsequent drying step. The drying and densifying process must be carried out at a temperature higher than the glass transition temperature of the fiber to be dried and densified, but the glass transition temperature differs between the fiber to be dried and densified in a wet state and in a dry state. For example, the drying and densifying process is preferably carried out by a method using a heating roller at a temperature of 100° C. to 200° C. In this case, the number of heating rollers may be one or more.
[0018] The densely dried fibers are preferably subjected to a pressurized steam drawing treatment, which can further increase the denseness and the degree of orientation of the resulting precursor fibers. The pressurized steam drawing treatment is a method of drawing fibers in a pressurized steam atmosphere. The pressurized steam drawing treatment enables drawing at a high ratio, which allows for faster and more stable spinning and also contributes to improving the denseness and orientation of the resulting fibers. In the pressurized steam stretching treatment, it is preferable to control the temperature of the heating roller immediately before the pressurized steam stretching device to 120°C or higher and 190°C or lower, and the fluctuation rate of the steam pressure in the pressurized steam stretching to 0.5% or lower. By controlling the temperature of the heating roller and the fluctuation rate of the steam pressure in this way, it is possible to suppress the fluctuation of the draw ratio in a small section and the resulting fluctuation of the total fiber bundle fineness in a small section. If the temperature of the heating roller is less than 120°C, the temperature of the fiber to be subjected to the pressurized steam stretching treatment does not rise sufficiently, and the stretchability is likely to decrease.
[0019] The precursor fibers obtained by drying and densifying, or the precursor fibers obtained by drying and densifying and then subjecting them to pressurized steam stretching, are preferably subjected to an entanglement treatment, in which the precursor fibers are introduced into a grooved guide or a grooved roll, the width of which is kept constant, and the fibers are passed through an entanglement device having a flat rectangular cross section that blows air in an untwisted state, thereby providing entanglement. The materials for the groove guide, grooved roll, and intertwining device are not particularly limited, but in consideration of durability and cost, stainless steel, titanium, ceramic, etc. are preferable. Furthermore, in order to reduce the performance degradation caused by the friction between the grooved roll and the precursor fiber, those that have been plated are preferable. The entangled precursor fibers are wound onto a bobbin by a winder, or fed into a can and stored.
[0020] The carbon fiber precursor acrylic fiber is then subjected to a baking process, where it is flame-retarded, carbonized, and, if necessary, graphitized and surface-treated to become carbon fiber.
[0021] In the flame-retardant process, the carbon fiber precursor acrylic fiber is heat-treated in an oxidizing atmosphere to convert it into a flame-retardant fiber. The fiber density of the flame-resistant fiber obtained here is preferably 1.35 g / cm 3 More than 1.50g / cm 3 Less than or equal to 1.40 g / cm 3 More than 1.50g / cm 3 More preferably, 1.45 g / cm 3 More than 1.50g / cm 3 It is recommended to heat it until the density is 1.35g / cm 3 If the density is 1.50 g / cm or more, the generation of decomposition gas during the next carbonization step can be suppressed. 3 If it is less than this, the flameproofing step does not become too long, which is economical.
[0022] In addition, the density of the fiber during flame retardation is 1.22 g / cm 3 From the point when this temperature rises, the integrated value of the heat applied to the fiber during heat treatment in an oxidizing atmosphere is preferably within the range of 300 J·h / g to 1200 J·h / g. By adjusting the integrated value of the heat applied in the latter half of the flame-stabilizing process to fall within this range, it is easy to increase the yield of the obtained carbon fiber. The integrated value of the heat was calculated by the following formula using the flame-stabilizing temperature T (K), the residence time in the flame-stabilizing furnace t (h), and the heat capacity of the polyacrylonitrile precursor fiber, 1.507 J / g °C. Integrated value of heat (J·h / g) = T×t×1.507 When the flame-proofing step has a plurality of temperature conditions, the amount of heat can be calculated from the residence time at each temperature and integrated. Flame-resistant density is 1.22g / cm 3The point at which this occurs can be calculated by creating a master curve that predicts the flame-stabilization temperature, flame-stabilization time, and the fiber density that will be achieved at that time.
[0023] In part or all of the flame-proofing step, the oxidizing gas concentration is preferably 1 vol % to 15 vol %, more preferably 1 vol % to 10 vol %, and further preferably 1 vol % to 5 vol %. In part or all of the flame-resistant treatment process, if the oxidizing gas concentration is 1% by volume or more, reactions equivalent to the pre-carbonization process, such as decomposition before the cyclization reaction, oxidation, or dehydrogenation reaction, can be sufficiently suppressed, making it easier to increase the yield of carbon fiber, and if it is 15% by volume or less, the formation of oxidized structures is suppressed, making it easier to increase the yield of carbon fiber.
[0024] The heating temperature in the flame-proofing step is preferably 230° C. to 300° C., more preferably 250° C. to 300° C., and even more preferably 270° C. to 300° C. If the flame-proofing temperature is 230° C. or higher, the cyclization reaction and dehydrogenation reaction can be efficiently promoted to increase the density, and if the temperature is 300° C. or lower, there are fewer problems with yarn breakage and it is easy to obtain high-quality fibers.
[0025] In addition, the heating time in the flame-proofing step is preferably 1 to 80 minutes, more preferably 5 to 80 minutes, and even more preferably 220 to 80 minutes. If the flame-proofing time is 1 minute or more, there is little trouble with yarn breakage, and if it is 80 minutes or less, high-quality fibers are likely to be obtained.
[0026] To summarize the above-mentioned flame-resistant conditions, in the flame-resistant step, it is preferable from the viewpoint of the yield of carbon fiber to obtain a flame-resistant fiber by performing a heat treatment at 230 to 245°C for 40 to 75 minutes in an air atmosphere, and then performing a heat treatment at 250 to 300°C for 1 to 40 minutes in an atmosphere having an oxidizing gas concentration of 1% by volume to 15% by volume.
[0027] The apparatus for performing the flame-resistant treatment is not particularly limited, but a conventionally known hot air circulating oven or a method of contacting with a heated solid surface can be adopted. Usually, in a flame-resistant oven (hot air circulating oven), the carbon fiber precursor acrylic fiber that has entered the flame-resistant oven is once taken out of the flame-resistant oven, and then folded back by a folding roll disposed outside the flame-resistant oven and repeatedly passed through the flame-resistant oven. In addition, in the method of contacting with a heated solid surface, a method of intermittent contact is adopted. One or more of these flame-proofing treatment devices may be used, and devices using different treatment methods may be combined.
[0028] The flame-retardant fiber is then subjected to a carbonization process. In the carbonization step, the flame-resistant fiber is carbonized in an inert atmosphere to obtain carbon fiber. Carbonization is carried out in an inert atmosphere with a maximum temperature of 1000°C or higher. The gas forming the inert atmosphere may be any inert gas such as nitrogen, argon, or helium, but it is preferable to use nitrogen from an economical standpoint. In particular, it is preferable to obtain carbon fiber by heating the flame-resistant fiber in an inert atmosphere at 1200°C to 3000°C. In the early stages of the carbonization process, i.e., when the treatment temperature is between 300° C. and 400° C., scission and crosslinking reactions occur in the polyacrylonitrile copolymer, which is a component of the fiber. In this temperature range, it is preferable to slowly increase the temperature of the fiber at a heating rate of 300° C. / min or less in order to improve the mechanical properties of the final carbon fiber. At a processing temperature of 400°C or higher and 900°C or lower, the polyacrylonitrile copolymer undergoes thermal decomposition, gradually forming a carbon structure. In the stage of forming this carbon structure, the ordered orientation of the carbon structure is promoted, so it is preferable to treat the carbon structure while stretching it under tension. Therefore, in order to control the temperature gradient and stretching (tension) at 900°C or lower, it is more preferable to set up a pre-process (pre-carbonization process) separate from the final carbonization process. At a treatment temperature of 900° C. or higher, the remaining nitrogen atoms are eliminated, and the carbonaceous structure develops, causing the fiber to shrink as a whole. Even in heat treatment at such high temperatures, it is preferable to treat the fiber under tension in order to achieve good mechanical properties in the final carbon fiber. The carbon fibers thus obtained may be subjected to a graphitization treatment, if necessary, which increases the elasticity of the carbon fibers. As for the conditions for graphitization, it is preferable to perform the process in an inert atmosphere with a maximum temperature of 2000°C or higher, while elongating at an elongation rate in the range of 3% to 15%. When the elongation rate is 3% or higher, highly elastic carbon fibers (graphitized fibers) having sufficient mechanical properties can be obtained. This is because, when attempting to obtain carbon fibers having a predetermined elastic modulus, the lower the elongation rate, the higher the processing temperature required. On the other hand, when the elongation rate is 15% or lower, the difference in the effect of promoting the growth of the carbon structure due to elongation is small between the surface layer and the interior, forming uniform carbon fibers, and high-quality carbon fibers can be obtained.
[0029] After the above-mentioned calcination step, the carbon fiber is preferably subjected to a surface treatment suitable for the final use. Although there is no limitation on the method of surface treatment, a method of electrolytic oxidation in an electrolyte solution is preferred. Electrolytic oxidation is a method of modifying the surface by generating oxygen on the surface of the carbon fiber to introduce oxygen-containing functional groups onto the surface. As the electrolyte, acids such as sulfuric acid, hydrochloric acid, and nitric acid, and salts thereof can be used. As conditions for the electrolytic oxidation, the temperature of the electrolytic solution is preferably not more than room temperature, the electrolyte concentration is from 1% by mass to 15% by mass, and the quantity of electricity is preferably not more than 100 coulombs / g. The carbon fiber precursor acrylic fiber obtained by the above-mentioned method has excellent bundling properties because the oil agent of the present invention is attached to the fiber. Furthermore, since the fusion between the single fibers is prevented in the baking process and the generation of silicon compounds and the diffusion of silicone components and non-silicone components can be suppressed, the operability and process passability are significantly improved and industrial productivity can be maintained. Therefore, carbon fibers with excellent mechanical properties can be obtained with good productivity. Furthermore, the carbon fiber obtained by baking this carbon fiber precursor acrylic fiber has excellent mechanical properties and high quality, and is suitable as a reinforcing fiber for use in fiber-reinforced resin composite materials used in various structural materials. EXAMPLES
[0030] The following examples will be described. <Measurement of fiber density> The fiber density was measured according to the fiber density test method specified in JIS-R-7603. The measurement was performed five times, and the average value was used for evaluation.
[0031] <Carbon fiber yield> The carbon fiber precursor acrylic fiber bundle and 1 m of the carbon fiber bundle were collected and dried at 120° C. for 2 hours. Next, the bone dry mass C (g) of the carbon fiber precursor acrylic fiber bundle and the bone dry mass D (g) of the carbon fiber bundle were measured, and the yield was calculated by the formula Yield (%) = (D / C) × 100.
[0032] <Example 1> <Production of carbon fiber precursor acrylic fiber> An acrylonitrile copolymer (composition ratio: acrylonitrile / acrylamide / methacrylic acid = 96.5 / 2.7 / 0.8 (mass ratio)) was dispersed in dimethylacetamide at a ratio of 21 mass%, heated and dissolved to prepare a spinning dope, which was extruded from a spinning nozzle with a hole size (diameter) of 45 μm and 50,000 holes into a coagulation bath at 38 ° C filled with a 67 mass % dimethylacetamide aqueous solution to form a coagulated yarn. The coagulated yarn was desolvated in a water washing tank and stretched three times to form a precursor fiber in a water-swollen state. The precursor fibers in a water-swollen state were then introduced into an oil treatment tank filled with an aminosilicone-based oil treatment liquid, and oil was applied to them. The precursor fibers to which the oil was applied were then dried and densified using a roller with a surface temperature of 150°C, and then stretched 5 times in water vapor at a pressure of 0.3 MPa to obtain carbon fiber precursor acrylic fibers. The resulting bundle of carbon fiber precursor acrylic fibers had a filament count of 50,000, a single fiber fineness of 1.3 dtex, and a fiber density of 1.18 g / cm. 3 It was. <Carbon fiber manufacturing> The obtained carbon fiber precursor acrylic fiber was made flame-resistant by passing it through a flame-resistant furnace at 240°C in an atmosphere of 21% by volume oxygen concentration for 80 minutes to obtain a flame-resistant fiber. The flame-resistant fiber was then passed through a carbonization furnace having a temperature gradient in the range of 400°C to 1250°C in a nitrogen atmosphere for 3 minutes to be calcined to obtain a carbon fiber.
[0033] <Examples 2 to 36, Comparative Examples 1 and 2> Carbon fibers were obtained in the same manner as in Example 1, except that the oxygen concentration, temperature, and time in the flame-proofing furnace were changed as shown in Table 1. The integrated heat amount and yield are also shown in Table 1.
[0034] [Table 1] [Industrial Applicability]
[0035] The method for producing carbon fibers according to the present invention can provide carbon fibers at a high yield, which was not possible with conventional techniques.
Claims
1. Polyacrylonitrile fibers are subjected to oxidation in an atmosphere until the fiber density reaches 1.35 g / cm 3 ~1.50g / cm 3 A method for producing a flame-retardant fiber, comprising a flame-retardant process.
2. In the flame retardant treatment, the fiber density is 1.22 g / cm 3 2. The method for producing an oxidation-resistant fiber according to claim 1, wherein the fiber is heated so that an integrated value of the amount of heat applied to the fiber from the time when the fiber reaches the temperature is within a range of 300 J·h / g to 1200 J·h / g.
3. The method for producing an oxidation-resistant fiber according to claim 1, further comprising a oxidation step in which the oxidizing gas concentration in the oxidizing atmosphere is 1% by volume to 15% by volume.
4. The method for producing an oxidation-resistant fiber according to claim 3, wherein the heating temperature in the oxidation step is 230°C to 300°C.
5. The method for producing an oxidation-resistant fiber according to claim 3, wherein the heating time in the oxidation-resistant step is from 1 minute to 80 minutes.
6. 2. The method for producing a flame-resistant fiber according to claim 1, wherein in the flame-resistant step, the fiber is heated in an air atmosphere at 230° C. to 245° C. for 40 minutes to 75 minutes, and then heated in an atmosphere having an oxidizing gas concentration of 1% by volume to 15% by volume for 1 minute to 40 minutes at 250° C. to 300° C. to obtain a flame-resistant fiber.
7. A method for producing carbon fibers, comprising heating the flame-resistant fiber produced by the method according to any one of claims 1 to 6 at 1200°C to 3000°C in an inert atmosphere to obtain carbon fibers.
Citation Information
Patent Citations
Polyacrylonitrile-based copolymer, polyacrylonitrile-based precursor fiber for carbon fiber, carbon fiber bundles, process for producing flameproofed fiber bundles, and process for producing carbon fiber bundles
WO2013015210A1
Carbon fiber bundle and method for manufacturing same
WO2016068034A1
Tansoseninoseizohoho
JP1976075124A
Production of acrylic carbon fiber
JP1995292526A
Flameproof fiber material, carbon fiber material, graphite fiber material and method for producing the same
JP2004003043A
Cited By
Heat-treated flame-resistant fibers, graphite fibers, and methods for producing same
WO2026211648A1
Heat-treated flame-resistant fiber for brake material production, graphite fiber for brake material production, and methods for producing same
WO2026211650A1