Pretreatment liquid for solvent inkjet ink, and solvent inkjet ink set

The use of a (meth)acrylic resin with a high glass transition point and an aminoethyl group in a pretreatment liquid, combined with an epoxy resin in the solvent ink, addresses the issues of alcohol abrasion resistance and image bleeding on non-absorbent substrates, creating a durable and scratch-resistant coating.

JP2024138811AInactive Publication Date: 2024-10-09RISO KAGAKU CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023049508
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional solvent inkjet inks face issues with alcohol abrasion resistance and image bleeding on non-absorbent substrates, particularly when cleaned with alcohol-containing cloths, and there is a challenge in forming a strong coating film that can withstand alcohol scrubbing and prevent ink spreading.

Method used

A pretreatment liquid containing a (meth)acrylic resin with a glass transition point of 70°C or higher and an aminoethyl group, combined with an epoxy resin in the solvent ink, is applied to the substrate using an inkjet method to enhance adhesion and form a strong, scratch-resistant coating that suppresses ink bleeding and improves alcohol resistance.

Benefits of technology

The combination of the pretreatment liquid and solvent ink significantly enhances alcohol abrasion resistance and prevents image bleeding, forming a durable coating film that maintains image integrity even on non-absorbent substrates like polyvinyl chloride sheets and polypropylene synthetic paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138811000001
    Figure 2024138811000001
  • Figure 2024138811000002
    Figure 2024138811000002
  • Figure 2024138811000003
    Figure 2024138811000003
Patent Text Reader

Abstract

To provide a pretreatment liquid which improves alcohol scratch resistance of a printed matter and suppression of bleeding of an image.SOLUTION: A pretreatment liquid is used in a method for imparting solvent inkjet ink onto a base material by an inkjet method and can be imparted by the inkjet method, and contains an organic solvent, and a (meth)acrylic resin having a glass transition point (Tg) of 70°C or higher and having an aminoethyl group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] An embodiment of the present invention relates to a pretreatment liquid for a solvent inkjet ink and a solvent inkjet ink set. [Background technology]

[0002] Inkjet recording is a method of ejecting highly fluid inkjet ink as droplets from a fine nozzle to record an image on a substrate placed opposite the nozzle. This method has been rapidly spreading in recent years because it allows low-noise, high-speed printing. Inks used in this type of inkjet recording method include aqueous inks that contain water as the main solvent, ultraviolet-curable inks (UV inks) that contain a high content of polymerizable monomers as the main component, and hot-melt inks (solid inks) that contain a high content of wax as the main component, as well as so-called non-aqueous inks that contain a non-aqueous solvent as the main solvent. Non-aqueous inks can be classified into solvent inks (solvent-based inks) whose main solvent is a volatile organic solvent, and oil-based inks (oil-based inks) whose main solvent is a low-volatility or non-volatile organic solvent. Solvent inks dry on the substrate mainly due to the evaporation of the organic solvent, whereas oil-based inks dry mainly due to penetration into the substrate.

[0003] Inkjet recording methods can print on various substrates without contact, and the fields of application are expanding. For example, by directly inkjet printing on non-absorbent substrates such as polyvinyl chloride sheets and synthetic polypropylene paper, it is possible to efficiently provide printed matter. In addition, such durable printed matter is used for outdoor applications and applications where it is touched by people, and therefore the printed matter is required to have abrasion resistance. In addition, the printed matter may be cleaned by wiping off dirt, so the abrasion resistance of the printed matter becomes even more important.

[0004] For non-absorbent substrates, the image can be fixed to the substrate by applying the solvent ink and then drying and removing the solvent. Since the solvent ink contains a binder resin and the binder resin is dissolved in the solvent, the binder resin and the pigment are applied uniformly to the substrate, and the image can be fixed more firmly to the substrate.

[0005] Patent Document 1 proposes using, as a dispersant for a solvent-based inkjet ink composition, a dispersant whose main chain is polyethyleneimine and whose side chain has at least an oxyalkylenecarbonyl group, and whose weight average molecular weight (Mw), acid value, amine value, and weight average molecular weight (Mw) / number average molecular weight (Mn) satisfy predetermined ranges. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2015-71681 A Summary of the Invention [Problem to be solved by the invention]

[0007] When a printed matter printed with solvent ink is rubbed with a cloth containing alcohol for cleaning or the like, the image dissolves in the alcohol, causing the printed matter to fade. Patent Document 1 discloses that a low-viscosity pigment dispersion can be produced by using a specific dispersant, and that the low viscosity makes it possible to increase the ratio of binder resin in the ink, which contributes to the resistance of the ink coating, thereby improving the alcohol resistance of the ink coating.

[0008] As a further consideration, a method of applying a solvent ink to a substrate by an inkjet method can form a delicate image, but there is a phenomenon in which the image bleeds when the solvent ink spreads when it lands on the substrate. With conventional techniques, it is difficult to achieve both alcohol abrasion resistance and suppression of solvent ink bleed.

[0009] An object of the present invention is to provide a pretreatment liquid and a solvent inkjet ink set that improve the alcohol abrasion resistance of printed matter and the suppression of bleeding in images. [Means for solving the problem]

[0010] One embodiment of the present invention relates to a pretreatment liquid for solvent inkjet ink, which is used in a method of applying a solvent inkjet ink to a substrate by the inkjet method and can be applied by the inkjet method, and which contains an organic solvent and a (meth)acrylic resin having a glass transition point (Tg) of 70°C or higher and having an aminoethyl group.

[0011] Another embodiment relates to a solvent inkjet ink set comprising a solvent inkjet ink and a pretreatment liquid, the solvent inkjet ink comprising an organic solvent, an epoxy resin, and a pigment, and the pretreatment liquid being the pretreatment liquid for a solvent inkjet ink described above.

[0012] Yet another embodiment relates to a method for producing a printed matter, comprising applying the above-described pretreatment liquid for a solvent inkjet ink to a substrate by an inkjet method, and applying a solvent inkjet ink to the substrate to which the pretreatment liquid has been applied by an inkjet method. Effect of the Invention

[0013] According to one embodiment of the present invention, it is possible to provide a pretreatment liquid and a solvent inkjet ink set that improve the alcohol abrasion resistance of printed matter and the suppression of bleeding of images. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described below using embodiments. The examples in the following embodiments are not intended to limit the present invention.

[0015] <Pretreatment solution> A pretreatment liquid for a solvent inkjet ink according to one embodiment is used in a method for applying a solvent inkjet ink to a substrate by an inkjet method, and is a pretreatment liquid that can be applied by the inkjet method, and contains an organic solvent and a (meth)acrylic resin having a glass transition point (Tg) of 70° C. or higher and having an aminoethyl group.

[0016] In the following description, the solvent inkjet ink is also simply referred to as "solvent ink" or "ink." The pretreatment liquid for the solvent inkjet ink is also simply referred to as "pretreatment liquid." A (meth)acrylic resin having a glass transition point (Tg) of 70° C. or higher and containing an aminoethyl group is also referred to as "(meth)acrylic resin A." In this specification, the (meth)acrylic resin means at least one of an acrylic resin and a methacrylic resin.

[0017] According to one embodiment, it is possible to provide a pretreatment liquid that improves the alcohol rub resistance of printed matter and suppresses bleeding of images.

[0018] The (meth)acrylic resin A having an aminoethyl group has an amino group which is a basic group. The basic group can bond with an acidic hydroxyl group on the surface of the pigment contained in the solvent ink. In addition, the (meth)acrylic resin A has excellent adhesion to the substrate. In particular, since the (meth)acrylic resin has compatibility with polyvinyl chloride resin, polypropylene resin, etc., the (meth)acrylic resin A shows excellent adhesion to non-absorbent substrates such as polyvinyl chloride sheets and polypropylene synthetic paper even when the substrate does not have an ink receiving layer. Due to these actions, the (meth)acrylic resin A becomes a primer that connects the substrate and the solvent ink on the substrate surface. Due to this effect, the pretreatment liquid according to one embodiment can suppress the bleeding of the solvent ink on various substrate surfaces including non-absorbent substrates. In addition, since the aminoethyl group of the (meth)acrylic resin A has an amino group which is a polar group and an ethylene group which is a hydrophobic group, it is considered that the adhesion of the coating film is improved even on non-absorbent substrates without an ink receiving layer while suppressing the bleeding of the solvent ink on the substrate surface.

[0019] In addition, the (meth)acrylic resin A has a glass transition point (Tg) of 70° C. or higher, and is therefore capable of forming a coating film having high abrasion resistance and durability. Therefore, the pretreatment liquid according to one embodiment is capable of forming a strong coating film on the surface of the substrate, and is capable of forming a coating film that exhibits abrasion resistance even against alcohol. In addition, due to the action of the (meth)acrylic resin A and the pigment described above, the pretreatment liquid according to one embodiment can also fix the pigment on the substrate surface. Due to these actions, the pretreatment liquid according to one embodiment can increase the alcohol abrasion resistance of an image formed by a solvent ink on the substrate surface, even if the substrate is a non-absorbent substrate.

[0020] Furthermore, since the pretreatment liquid contains (meth)acrylic resin A, the alcohol abrasion resistance of the coating film after the solvent ink is applied can be improved by controlling the amount of the pretreatment liquid applied to the substrate. In the case of a solvent ink, the amount of binder resin that can be added to the ink may be limited from the viewpoint of inkjet ejection suitability. Due to this limitation, it is known that it is difficult to form a coating film that can be sufficiently imparted with alcohol abrasion resistance by the solvent ink. By using the solvent ink in combination with the pretreatment liquid according to one embodiment, a strong coating film can be formed by the (meth)acrylic resin A on the substrate surface, and this coating film and the image by the solvent ink can be integrated to form a coating film having alcohol abrasion resistance. Even when the solvent ink contains a binder resin, a strong coating film is formed by the pretreatment liquid on the substrate surface, so that the content of the binder resin contained in the solvent ink can be reduced to prevent a decrease in the inkjet ejection performance of the solvent ink.

[0021] The pretreatment liquid contains a (meth)acrylic resin A having a glass transition point (Tg) of 70° C. or higher and having an aminoethyl group. The (meth)acrylic resin A is preferably an aminoethylated (meth)acrylic resin obtained by reacting a (meth)acrylic copolymer having a carboxy group with ethyleneimine to perform aminoethylation. This aminoethylated (meth)acrylic resin is preferably a (meth)acrylic resin having a primary amino group on the polyethyleneimine chain, which is a resin having a main chain and a polyethyleneimine chain grafted thereon. In this case, the polyethyleneimine chain may be a straight chain or a branched chain, but is preferably a straight chain polyethyleneimine chain. Due to the high reactivity derived from the primary amino group, the solvent ink is bonded to the acidic hydroxyl group on the pigment surface of the solvent ink on the substrate surface, and the solvent ink bleeding can be suppressed. In addition, since the (meth)acrylic resin has a skeleton, it has high adhesion to the substrate, forms a strong coating film on the substrate surface, and can enhance the alcohol abrasion resistance of the printed matter. It is also possible to obtain high adhesion to non-absorbent substrates such as polyvinyl chloride sheets and synthetic polypropylene paper.

[0022] The (meth)acrylic resin A preferably has a glass transition point (Tg) of 70° C. or higher, more preferably 80° C. or higher, and even more preferably 100° C. or higher. This allows a strong coating film to be formed on the substrate surface, and the alcohol abrasion resistance of the image formed by the solvent ink can be improved. The glass transition point (Tg) of the (meth)acrylic resin A is not particularly limited, but may be 200° C. or lower, 180° C. or lower, or 150° C. or lower, from the viewpoint of adhesion of the coating film to the substrate. For example, the glass transition point (Tg) of the (meth)acrylic resin A may be 70 to 150° C., 80 to 180° C., or 100 to 200° C.

[0023] In this specification, the glass transition point of a resin is a value measured by differential scanning calorimetry (DSC). For example, a high-sensitivity differential scanning calorimeter DSC8231 manufactured by Rigaku Corporation can be used as the glass transition point measuring device.

[0024] The (meth)acrylic resin A preferably has an amine value of 0.5 mmol / g-solid or more, and more preferably 0.7 mmol / g-solid or more, so that the pigment contained in the solvent ink and the (meth)acrylic resin A interact in appropriate amounts on the substrate surface, and bleeding of the solvent ink can be further suppressed.

[0025] In this specification, the amine value of a resin is the number of milligrams of potassium hydroxide equivalent to the amount of hydrochloric acid required to neutralize all basic components contained in 1 g of nonvolatile matter.

[0026] The (meth)acrylic resin A may be a synthesized resin or a commercially available product. An example of a commercially available product is "Polyment NK-380" manufactured by Nippon Shokubai Co., Ltd.

[0027] From the viewpoint of adjusting the amount applied to the substrate, the (meth)acrylic resin A is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 6% by mass or more, based on the total mass of the pretreatment liquid. From the viewpoint of adjusting the viscosity when applied to the substrate, the (meth)acrylic resin A is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and even more preferably 20% by mass or less, based on the total mass of the pretreatment liquid. Within these ranges, it is also possible to eject the pretreatment liquid by inkjet. For example, the (meth)acrylic resin A may be 1 to 50% by mass, 3 to 40% by mass, 6 to 30% by mass, or 6 to 20% by mass, based on the total mass of the pretreatment liquid.

[0028] The pretreatment liquid contains an organic solvent. The organic solvent is not particularly limited, but is preferably one that exhibits affinity with an organic solvent that can be used in solvent ink, and is more preferably an organic solvent that can be used in solvent ink. Such an organic solvent is preferably an organic solvent with a low boiling point and high polarity. The organic solvent of the pretreatment liquid is preferably an organic solvent that can dissolve the (meth)acrylic resin A. This allows the (meth)acrylic resin A to be applied more uniformly to the substrate by applying the pretreatment liquid.

[0029] From the viewpoint of drying property, the organic solvent of the pretreatment liquid preferably has a boiling point of 250° C. or less, and more preferably 200° C. or less. From the viewpoint of suppressing odors during printing work, the organic solvent of the pretreatment liquid preferably has a boiling point of 100° C. or more, and more preferably 150° C. or more. For example, the organic solvent of the pretreatment liquid preferably has a boiling point of 150° C. to 200° C. Furthermore, the pretreatment liquid preferably contains organic solvents having a boiling point of 150° C. to 200° C. in an amount of 70 mass % or more of the total mass of the organic solvents.

[0030] The organic solvent is preferably a glycol ether-based solvent. The glycol ether-based solvent can enhance compatibility with the (meth)acrylic resin A, and the solvent can be easily removed after the coating film is formed. In addition, the glycol ether-based solvent has high affinity with the organic solvent, pigment, and resin contained in the solvent ink, and therefore can promote the interaction between the pretreatment liquid and the solvent ink on the substrate surface after the pretreatment liquid is applied.

[0031] The glycol ether solvent is preferably an alkylene glycol monoalkyl ether acetate, an alkylene glycol monoalkyl ether, etc. Examples of the alkylene glycol monoalkyl ether include ethylene glycol monomethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol isopropyl methyl ether, diethylene glycol dimethyl ether, dipropylene glycol dimethyl ether, ethylene glycol monobutyl ether, propylene glycol monobutyl ether, propylene glycol monopropyl ether, diethylene glycol monoethyl ether, dipropylene glycol monomethyl ether, and triethylene glycol monomethyl ether.

[0032] Examples of the alkylene glycol monoalkyl ether acetate include ethylene glycol monobutyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.

[0033] Examples of glycol ether solvents include alkylene glycol diacetates such as ethylene glycol monomethyl ether acetate, propylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, dipropylene glycol monobutyl ether acetate, 3-methoxybutyl acetate, and ethylene glycol diacetate; and alkylene glycol dialkyl ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol methylpropyl ether, diethylene glycol dibutyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0034] As the organic solvent, lactone-based solvents, nitrogen-containing solvents, acetate-based solvents, ketone-based solvents, alcohol-based solvents, etc. may be used. Examples of lactone-based solvents include γ-butyrolactone and γ-valerolactone. Examples of nitrogen-containing solvents include N-methyl-2-pyrrolidone. Examples of acetate-based solvents include cyclohexyl acetate. Examples of ketone-based solvents include acetone, methyl ethyl ketone, cyclohexanone, methylcyclohexanone, isophorone, etc. Examples of alcohol-based solvents include those having 8 or less carbon atoms, preferably 4 or less carbon atoms, specifically methanol, ethanol, etc. Examples of fatty acid-based solvents include those having 8 or less carbon atoms, preferably 4 or less carbon atoms, specifically methyl acetate, ethyl acetate, methyl propionate, etc.

[0035] The organic solvent may be used alone or in combination of two or more. As described above, the organic solvent preferably contains an alkylene glycol-based solvent, and preferably contains at least one selected from alkylene glycol monoalkyl ether acetate and alkylene glycol monoalkyl ether. The organic solvent is contained in an amount of preferably 50 to 95 mass %, more preferably 60 to 90 mass %, and further preferably 70 to 80 mass %, based on the total mass of the pretreatment liquid.

[0036] The pretreatment liquid is preferably a solvent composition. The pretreatment liquid preferably does not contain water, and may contain, for example, 5% by mass or less, 1% by mass or less, or 0.1% by mass or less of water relative to the total mass of the pretreatment liquid.

[0037] The pretreatment liquid preferably contains a surfactant. For example, from the viewpoint of improving the wettability of the pretreatment liquid even on a hydrophobic substrate surface, increasing the drying speed, and uniformly applying the pretreatment liquid, the pretreatment liquid preferably contains a surfactant. As the surfactant, a nonionic surfactant is preferable, and examples thereof include a silicone-based surfactant, a fluorine-based surfactant, and an acetylene glycol-based surfactant.

[0038] Examples of silicone surfactants include polyester-modified silicone, polyether-modified silicone, etc. Examples of commercially available silicone surfactants include "BYK-307", "BYK-313", "BYK-330", "BYK-333", "BYK-342", "BYK-370", "BYK-377", "BYK-378", "BYK-3550", "BYK-3565", "BYK-3750", "BYK-3761", "BYK-3762", "BYK-3764", and "BYK-SILCLEAN 3700" manufactured by BYK-Chemie Japan Co., Ltd., and "Silface SAG005" and "Silface SAG008" manufactured by Nissin Chemical Industry Co., Ltd. (all trade names).

[0039] Examples of commercially available fluorosurfactants include "BYK-340" manufactured by BYK Japan K.K., and "Surflon S-211," "Surflon S-131," "Surflon S-132," "Surflon S-141," "Surflon S-144," and "Surflon S-145" manufactured by AGC Inc. (all trade names).

[0040] Examples of commercially available acetylene glycol surfactants include "Surfynol 82", "Surfynol 104", "Surfynol 465", "Surfynol 485", and "Surfynol TG" manufactured by Evonik Industries, Ltd., and "Olfyn STG" and "Olfyn E1004" manufactured by Nissin Chemical Industry Co., Ltd. (all trade names).

[0041] The surfactant may be used alone or in combination of two or more kinds. The surfactant content is preferably 0.05 to 2 mass %, more preferably 0.1 to 1 mass %, based on the total mass of the pretreatment liquid.

[0042] The pretreatment liquid may contain various additives depending on the application, etc. Examples of the additives include UV absorbers, light stabilizers, antioxidants, plasticizers, etc.

[0043] The method for preparing the pretreatment liquid is not limited, but the pretreatment liquid can be obtained by mixing the raw materials all at once or in portions, stirring the resulting mixture, and optionally removing foreign matter with a filter, etc. In order to dissolve the (meth)acrylic resin A in the organic solvent, it is preferable to stir the mixture while heating it.

[0044] The viscosity of the pretreatment liquid varies depending on the nozzle diameter of the ejection head of the inkjet recording system, the ejection environment, and the like, but in general, the viscosity is preferably 5 to 35 mPa·s at 23° C., more preferably 5 to 30 mPa·s, and even more preferably 8 to 25 mPa·s. In this specification, the viscosity of the pretreatment liquid is a value measured at 23° C. As a viscosity measuring device, for example, a "Rheometer MCR302" manufactured by Anton Paar Japan Ltd. can be used.

[0045] The pretreatment liquid according to the present embodiment is preferably used for non-permeable substrates because it is used in combination with a solvent ink. Examples of non-permeable substrates include glass, ceramics, metals, and plastics. Examples of glass include plate glass such as borosilicate glass, quartz glass, and soda lime glass. Examples of ceramics include molded bodies such as alumina, zirconia, steatite, and silicon nitride. Examples of metals include metal plates such as aluminum, iron, copper, tin, chromium, cadmium, stainless steel, and tinplate, which may be plated, painted, or coated. Examples of plastics include sheets and films of acrylic resin, polycarbonate resin, polyester resin, polyethylene resin, polypropylene resin, polyvinyl chloride resin, polyvinylidene chloride resin, polyvinyl acetal resin, polystyrene resin, ABS resin, and polyamide resin. Examples of synthetic paper made from these resins include synthetic paper.

[0046] The substrate may be an absorbent substrate capable of absorbing the applied ink, such as a substrate having an ink-receiving layer, but a non-absorbent substrate is preferred. The pretreatment liquid of the present embodiment can be combined with a solvent ink to form a printed matter having excellent alcohol abrasion resistance and image quality even on a non-absorbent substrate having no ink-receiving layer. Examples of non-absorbent substrates include synthetic paper having no ink-receiving layer (e.g., synthetic paper made of polypropylene, etc.), plastic sheets such as polyvinyl chloride sheets having no ink-receiving layer, metal plates, glass plates, etc.

[0047] It is preferable that the pretreatment liquid is applied to the substrate by an inkjet method. This allows the inkjet printing device to be shared in the method of applying the solvent inkjet ink to the substrate, and simplifies the process. In addition, since the inkjet method allows images to be formed on demand, printing can be performed by matching the application area of ​​the pretreatment liquid and the ink. Therefore, if the application amount of the pretreatment liquid is adjusted to an appropriate amount according to the application area of ​​the ink, the amount of the pretreatment liquid used can be reduced.

[0048] The pretreatment liquid contains a (meth)acrylic resin A and an organic solvent, and preferably contains the (meth)acrylic resin A dissolved in the organic solvent, so that the viscosity of the pretreatment liquid can be reduced and the inkjet ejection performance of the pretreatment liquid is also good.

[0049] <Solvent Inkjet Ink Set> According to one embodiment, it is possible to provide a solvent inkjet ink set including a solvent inkjet ink and a pretreatment liquid, the solvent inkjet ink including an organic solvent, an epoxy resin, and a pigment, and the pretreatment liquid including an organic solvent and a (meth)acrylic resin having a glass transition point (Tg) of 70° C. or higher and having an aminoethyl group.

[0050] The details of the pretreatment liquid are as described above. The details of the solvent inkjet ink will be described below.

[0051] <Solvent ink> The solvent ink contains an organic solvent, an epoxy resin, and a pigment. It is preferable that the solvent ink contains a pigment dispersant in addition to the pigment.

[0052] The ink may contain a pigment. Depending on the intended use of the printed matter, it is also possible to use coloring materials other than pigments, such as acid dyes. Examples of the pigments that can be used include organic pigments such as azo pigments, phthalocyanine pigments, polycyclic pigments, and dye lake pigments, and inorganic pigments such as carbon black and metal oxides. Examples of the azo pigments include soluble azo lake pigments, insoluble azo pigments, and condensed azo pigments. Examples of the phthalocyanine pigments include metal phthalocyanine pigments and metal-free phthalocyanine pigments. Examples of the polycyclic pigments include quinacridone pigments, perylene pigments, perinone pigments, isoindoline pigments, isoindolinone pigments, dioxazine pigments, thioindigo pigments, anthraquinone pigments, quinophthalone pigments, metal complex pigments, and diketopyrrolopyrrole (DPP). Examples of the carbon black include furnace carbon black, lamp black, acetylene black, and channel black. Examples of the metal oxides include titanium oxide and zinc oxide. These pigments may be used alone or in combination of two or more kinds.

[0053] From the viewpoints of color development and ejection stability, the average particle size of the pigment particles in the ink is preferably 50 to 500 nm, and more preferably 50 to 200 nm, as the volume-based average value in the particle size distribution measured by dynamic light scattering.

[0054] From the viewpoints of the type of pigment, color development, ejection stability, and the like, the content of the pigment is preferably 0.1 to 20 mass % relative to the total mass of the ink, more preferably 0.1 to 15 mass %, even more preferably 0.5 to 10 mass %, and even more preferably 1 to 5 mass %.

[0055] The pigment dispersion form may be a so-called capsule pigment in which the pigment is coated with an oil-insoluble resin, or a dispersion in which colored resin particles are dispersed with a pigment dispersant, but a dispersion in which the pigment dispersant is directly adsorbed onto the pigment surface and dispersed is preferred.

[0056] In order to stably disperse the pigment in the ink, a pigment dispersant can be used together with the pigment. The pigment dispersant is not particularly limited as long as it can stably disperse the pigment in an organic solvent, but for example, hydroxyl group-containing carboxylic acid ester, salt of long-chain polyaminoamide and high molecular weight acid ester, salt of high molecular weight polycarboxylic acid, salt of long-chain polyaminoamide and polar acid ester, high molecular weight unsaturated acid ester, copolymer of vinylpyrrolidone and long-chain alkene, modified polyurethane, modified polyacrylate, polyether ester type anionic surfactant, polyoxyethylene alkyl phosphate ester, polyester polyamine, etc. are preferably used.

[0057] Examples of commercially available pigment dispersants include Solsperse 11200, Solsperse 13940, Solsperse 20000, Solsperse 24000, Solsperse 32000, Solsperse 33000, Solsperse 32500, Solsperse 32600, Solsperse 33500, Solsperse 34750, Solsperse 35000, Solsperse 35100, Solsperse 36000, Solsperse 37500, Solsperse 39000, Solsperse 41000, Solsperse 56000, Solsperse 71000, and Solsperse 73000, Solsperse 74000, Solsperse 75000, Solsperse 75500, Solsperse 85000, Solsperse 86000, Solsperse 87000, Solsperse 88000, Solsperse J180, Solsperse J200; BYK Japan Co., Ltd.'s DISPERBYK-162, DISPERBYK-163, DISPERBYK-168, DISPERBYK-2050, DISPERBYK-2055, DISPERBYK-2150, DISPERBYK-2155, ANTI-TERRA-U / U 100; and Kusumoto Chemicals Co., Ltd.'s Disparlon KS-873N4.

[0058] The pigment dispersant may be used alone or in combination of two or more. The pigment dispersant is preferably contained in a mass ratio of 0.2 to 1.0 per 1 pigment. The content of the pigment dispersant relative to the total mass of the ink is preferably 0.5 to 15 mass%, and more preferably 1 to 5 mass%.

[0059] The ink preferably contains an epoxy resin. The epoxy resin functions as a binder resin, forms a coating film on the surface of the substrate, and can improve the alcohol abrasion resistance. The epoxy resin preferably has an epoxy equivalent of 450 to 2200 g / eq. The epoxy resin can form a stronger coating film on the substrate surface by forming a crosslinking reaction with the aminoethyl group of the (meth)acrylic resin A contained in the pretreatment liquid as the base point. As a result, the coating film of the solvent ink and the coating film of the pretreatment liquid are integrated on the substrate surface to form a stronger coating film, and the alcohol abrasion resistance of the printed matter can be further improved.

[0060] Epoxy resins usually have two or more epoxy groups. Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, biphenol type epoxy resins, alicyclic epoxy resins, aliphatic chain epoxy resins, glycidyl ester type epoxy resins, glycidyl ethers of condensates of phenolic compounds (phenol, cresol, alkylphenol, catechol, bisphenol F, bisphenol A, bisphenol S, etc.) and aldehyde compounds (formaldehyde, salicylaldehyde, etc.), glycidyl ethers of bifunctional phenols, glycidyl ethers of bifunctional alcohols, glycidyl ethers of trifunctional or higher polyphenols, and hydrogenated or halides thereof. The epoxy resins may be used alone or in combination of two or more.

[0061] From the viewpoint of alcohol abrasion resistance of the printed image, the epoxy equivalent of the epoxy resin is preferably 2200 g / eq or less, more preferably 1400 g / eq or less, and even more preferably 550 g / eq or less. If the epoxy equivalent exceeds 2200 g / eq, the epoxy resin has fewer epoxy groups, which tends to reduce the reactivity with the (meth)acrylic resin A of the pretreatment liquid. Therefore, the epoxy equivalent is set to 2200 g / eq or less, and the (meth)acrylic resin A of the pretreatment liquid and the epoxy resin of the solvent ink are appropriately reacted on the substrate surface, thereby further increasing the strength of the coating film after the solvent ink is applied and further improving the alcohol abrasion resistance.

[0062] If the epoxy equivalent is less than 450 g / eq, the epoxy resin has more epoxy groups, and therefore the (meth)acrylic resin A of the pretreatment liquid and the epoxy resin of the solvent ink tend to react preferentially on the substrate surface. As a result, there is a phenomenon in which the reaction between the (meth)acrylic resin A of the pretreatment liquid and the pigment of the solvent ink is less likely to occur. Therefore, by setting the epoxy equivalent to 450 g / eq or more and appropriately reacting the (meth)acrylic resin A of the pretreatment liquid with the pigment of the solvent ink, the bleeding of the solvent ink on the substrate surface can be further suppressed, the fixation of the pigment can be improved, and the alcohol abrasion resistance can be further enhanced. The epoxy equivalent of the epoxy resin is preferably 450 to 2200 g / eq, more preferably 450 to 1400 g / eq, and even more preferably 450 to 550 g / eq.

[0063] The epoxy equivalent is the number of grams of epoxy resin that contains 1 gram equivalent of epoxy groups. The epoxy equivalent of an epoxy resin can be measured according to JIS K7236:2001 "Determination of the epoxy equivalent of epoxy resins".

[0064] The number average molecular weight of the epoxy resin is preferably 500 or more, and more preferably 900 or more. On the other hand, from the viewpoint of reducing the viscosity of the pretreatment liquid, the number average molecular weight of the epoxy resin is preferably less than 4000, and more preferably less than 3000. The number average molecular weight of the epoxy resin is, for example, preferably 500 or more and less than 4000, and more preferably 900 or more and less than 3000.

[0065] The number average molecular weight of epoxy resin is the number average molecular weight determined by the GPC method using standard polystyrene conversion. The number average molecular weight of epoxy resin can be measured according to JIS K7252-1:2016 "Plastics - Determination of average molecular weight and molecular weight distribution of polymers by size exclusion chromatography - Part 1: General rules."

[0066] Examples of commercially available epoxy resins include "jER819", "jER1001", "jER1002", "jER1003", "jER1055", "jER1004", "jER1004AF", "jER1007", "jER1003F", "jER1004F", "jER1005F", "jER1004FS", "jER1006FS", "jER1007FS", "jER1009", "jER819", "jER825", "jER827", "jER828", "jER828EL", "jER828US", "jER828XA", "jER834", "jER801N", "jER802", "jER811", "jER813", "jER816A", "jER1010", "jER1009F", and "jER828F" manufactured by Mitsubishi Chemical Corporation. "ER1001B80", "jER1001X70", "jER1001X75", "jER1001T75", "jER806", "jER806H", "jER807", "jER4005P", "jER4007P", "jER4010P" manufactured by DIC Corporation; "EPICLON1050", "EPICLON1055", "EPICLON2050", "EPICLON3050", "EPICLON4050", "EPICLON7050", "EPICLON1050-70X", "EPICLON1050-75X", "EPICLON1055-75X", "EPICLON1051-75M", "EPICLON840", "EPICLON840-S", "EPICLON850", "EPICLON850-S", "EPICLON EXA-850CRP”, “EPICLON850-LC”, “EPICLON860”, “EPICLON HM-091”, “EPICLON HM-101”, “EPICLON830”, “EPICLON830-S”, “EPICLON835”, “EPICLON EXA-830CRP”, “EPICLON EXA-830LVP”, “EPICLON EXA-835LV”, “EPICLON855”, “EPICLON D-591”, “EPICLON D-595”, “EPICLON860-90X”, “EPICLON1051-75M”, “EPICLON HM-091-40AX”, “EPICLON5300-70”, “EPICLON HP-820”;ADEKA Corporation "ADEKA RESIN EP-4005", "ADEKA RESIN EP-7001", "ADEKA RESIN EP-5100-75X", "ADEKA RESIN EP-4100", "ADEKA RESIN EP4100-G", "ADEKA RESIN EP-4100TX", "ADEKA RESIN EP-4400", "ADEKA RESIN EP-4520S", "ADEKA RESIN EP-4530", "ADEKA RESIN EP-4901", "ADEKA RESIN EP-4000", "ADEKA RESIN EP-4005", "ADEKA RESIN EPU-6", "ADEKA RESIN EPU-7N", "ADEKA RESIN EPU-11F", "ADEKA RESIN EPU-1395", "ADEKA RESIN EPU-73B", "ADEKA RESIN EPU-17", "ADEKA RESIN EPU-17T-6", "ADEKA RESIN EP-49-10N", Toray Fine Chemicals Co., Ltd.'s "FLEP-50", "FLEP-60", "FLEP-125X" and the like (all trade names).

[0067] The epoxy resin may be used alone or in combination of two or more. From the viewpoint of alcohol abrasion resistance, the epoxy resin is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 5% by mass or more, based on the total mass of the ink. On the other hand, from the viewpoint of suppressing an increase in viscosity and improving inkjet dischargeability and ink storage stability, the epoxy resin is preferably 20% by mass or less, more preferably 10% by mass or less, based on the total mass of the ink. For example, the epoxy resin is preferably 0.1 to 20% by mass, more preferably 1 to 10% by mass, and even more preferably 5 to 10% by mass, based on the total mass of the ink.

[0068] The ink may contain other binder resins in addition to the epoxy resin. However, the content of the epoxy resin is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, based on the total mass of the binder resins in the ink. The total amount of the binder resins including the epoxy resin and other binder resins is preferably 0.1 to 20% by mass, more preferably 1 to 10% by mass, and even more preferably 5 to 10% by mass, based on the total mass of the ink.

[0069] Examples of the binder resin include (meth)acrylic resin, styrene-(meth)acrylic copolymer resin, vinyl chloride-vinyl acetate copolymer resin, fluororesin, phenol resin, rosin resin, urethane resin, and polyester resin.

[0070] The organic solvent is not particularly limited, and any organic solvent that can be used in a solvent inkjet ink can be used. Examples include ketone-based solvents, alcohol-based solvents, glycol ether-based solvents, and acetate-based solvents. From the viewpoint of suppressing odor during printing work, it is preferable to use an organic solvent having a boiling point of 100°C or more, and more preferably to use an organic solvent having a boiling point of 150°C or more. In addition, from the viewpoint of drying property, it is preferable to use an organic solvent having a boiling point of 250°C or less, and more preferably to use an organic solvent having a boiling point of 200°C or less. It is preferable that the organic solvent having a boiling point of 150°C or more and 200°C or less accounts for 70% by mass or more of the total mass of the organic solvents. The details of the organic solvent are as explained in the pretreatment liquid above. For example, the organic solvent of the solvent ink may be one or a combination of two or more of the organic solvents explained in the pretreatment liquid above.

[0071] In the ink set, the organic solvent of the pretreatment liquid and the organic solvent of the solvent ink may be the same or may be partially or entirely different. It is preferable that the organic solvent of the pretreatment liquid and the organic solvent of the solvent ink are combined so as to be miscible with each other on the surface of the substrate.

[0072] The organic solvent is contained in an amount of preferably 60 to 95% by mass, more preferably 70 to 90% by mass, and even more preferably 80 to 90% by mass, based on the total mass of the ink.

[0073] The ink preferably contains a surfactant. For example, from the viewpoint of improving the wettability of the ink even on a hydrophobic substrate surface and increasing the drying speed to form a good image, the ink preferably contains a surfactant. Examples of the surfactant include silicone-based surfactants, fluorine-based surfactants, and acetylene glycol-based surfactants. The surfactant is preferably a nonionic surfactant. Details of the surfactant are as described above in the pretreatment liquid. For example, the surfactant of the ink may be one or a combination of two or more of the surfactants described above in the pretreatment liquid.

[0074] From the viewpoints of continuous ejection property during printing and gloss of printed images, it is preferable that the ink contains a silicone-based surfactant.

[0075] The surfactant may be used alone or in combination of two or more kinds. The surfactant content is preferably 0.05 to 2 mass %, more preferably 0.1 to 1 mass %, based on the total mass of the ink.

[0076] The ink may contain various additives depending on the application, etc. Examples of the additives include UV absorbers, light stabilizers, antioxidants, plasticizers, etc.

[0077] The method for producing the ink is not particularly limited, but in one method, the ink can be produced by mixing and stirring each component all at once or in portions. Specifically, the ink can be produced by dispersing all the components in a dispersing machine such as a beads mill, either all at once or in portions, and dispersing the components, and, if desired, passing the mixture through a filtering machine such as a membrane filter.

[0078] The suitable range of viscosity of the solvent ink varies depending on the nozzle diameter of the ejection head of the inkjet recording system, the ejection environment, etc., but in general, it is preferably 3 to 30 mPa·s, more preferably 3 to 15 mPa·s, and even more preferably 5 to 13 mPa·s at 23° C. In this specification, the viscosity of the solvent ink is a value measured using the same procedure as the viscosity of the pretreatment liquid described above.

[0079] <Manufacturing method of printed matter> Hereinafter, the method for producing a printed matter will be described using several embodiments. According to one embodiment, it is possible to provide a method for producing a printed matter, which includes applying a pretreatment liquid to a substrate by an inkjet method, and applying a solvent inkjet ink to the substrate to which the pretreatment liquid has been applied by an inkjet method. The pretreatment liquid contains an organic solvent and a (meth)acrylic resin having a glass transition point (Tg) of 70° C. or higher and an aminoethyl group. The solvent inkjet ink contains an organic solvent, an epoxy resin, and a pigment. Details of the pretreatment liquid and the solvent inkjet ink are as described above. Details of the substrate are as described above. The substrate is preferably a non-permeable substrate, and is preferably a non-absorbent substrate having no ink receiving layer.

[0080] The inkjet method is a printing method that can easily and freely form an image on demand without contacting a substrate. The inkjet method is not particularly limited, and may be any of a piezo type, an electrostatic type, a thermal type, etc. When an inkjet printing device is used, it is preferable to eject droplets of the pretreatment liquid or ink from an inkjet head based on a digital signal and to adhere the ejected droplets to the cloth. The inkjet printing device may be a serial head type or a line head type.

[0081] The area to which the pretreatment liquid is applied may be an area having the same shape as the image formed by the solvent ink, a wider area including the shape of the image formed by the solvent ink, or the entire surface of the substrate. The amount of the pretreatment liquid applied to the substrate is 5 to 200 g / m 2 is preferable, and 10 to 100 g / m 2 is preferable, and 15 to 80 g / m 2 The amount of the solvent ink applied to the substrate is not particularly limited, but is, for example, 10 to 400 g / m 2 is preferable, and 15 to 250 g / m 2 is more preferred.

[0082] After applying the pretreatment liquid to the substrate and before applying the solvent ink, a step of heat treating the substrate may be further provided. This heat treatment can remove the organic solvent in the pretreatment liquid and fix the (meth)acrylic resin A in the pretreatment liquid to the substrate.

[0083] After the solvent ink is applied to the substrate, a step of heat-treating the substrate may be further provided. This heat treatment can remove the organic solvent of the solvent ink and fix the epoxy resin of the solvent ink to the substrate. In addition, the reactivity of the (meth)acrylic resin A of the pretreatment liquid with the epoxy resin can be increased on the surface of the substrate, thereby further increasing the strength of the coating film.

[0084] The heat treatment temperature after the application of the pretreatment liquid and after the application of the solvent ink can be appropriately selected depending on the material of the substrate. The heat treatment temperature is preferably 100° C. or higher, and more preferably 150° C. or higher, for example. From the viewpoint of reducing damage to the substrate, the heat treatment temperature is preferably 200° C. or lower. The heating device is not particularly limited, and for example, a heat press, a roll heater, a hot air device, an infrared lamp heater, etc. can be used. The heat treatment time can be appropriately set depending on the heating method, etc., and is preferably 1 second to 10 minutes, and may be 5 seconds to 5 minutes, for example.

[0085] The step of applying the pretreatment liquid and the step of applying the solvent ink may be performed by separate printing apparatuses, or may be performed by using a single printing apparatus.

[0086] The present disclosure includes the following embodiments. <1> The pretreatment liquid is used in a method of applying a solvent inkjet ink to a substrate by the inkjet method and can be applied by the inkjet method, the pretreatment liquid for solvent inkjet ink comprising an organic solvent and a (meth)acrylic resin having a glass transition point (Tg) of 70°C or higher and having an aminoethyl group.

[0087] <2> A solvent inkjet ink and a pretreatment liquid, the solvent inkjet ink including an organic solvent, an epoxy resin, and a pigment, the pretreatment liquid including <1> 2. A solvent inkjet ink set comprising the pretreatment liquid for the solvent inkjet ink according to claim 1. <3> The epoxy resin of the solvent inkjet ink has an epoxy equivalent of 450 to 2200 g / eq. <2> 2. A solvent inkjet ink set according to claim 1 .

[0088] <4> the above <1> 2. A method for producing a printed matter, comprising: applying the pretreatment liquid for a solvent inkjet ink according to claim 1 to a substrate by an inkjet method; and applying a solvent inkjet ink to the substrate to which the pretreatment liquid has been applied by an inkjet method. <5> The substrate is a non-absorbent substrate; <4> A method for producing a printed matter according to claim 1. EXAMPLES

[0089] The present invention will be described in detail below with reference to examples. The present invention is not limited to the following examples. In the tables, "-" for the content of a component indicates that the component is not added.

[0090] <Preparation of pretreatment solution> The formulation of the pretreatment liquid is shown in Table 1. The resin content shown in the table is the total amount including the solvent. First, the solvent of aminoethylated acrylic resin (1) "Polyment NK-380" (trade name, glass transition point 100°C, amine value 0.7-1.3 mmol / g-solid) manufactured by Nippon Shokubai Co., Ltd. was removed under reduced pressure and replaced with triethylene glycol monomethyl ether to prepare a resin solution with a concentration of 30% by mass. The solvent of aminoethylated acrylic resin (2) "Polyment NK-350" (trade name, glass transition point 40°C, amine value 0.6-1.0 mmol / g-solid) manufactured by Nippon Shokubai Co., Ltd. was removed under reduced pressure and replaced with triethylene glycol monomethyl ether to prepare a resin solution with a concentration of 30% by mass.

[0091] Pretreatment liquids 1 to 3 were prepared by mixing the resin, organic solvent, and surfactant according to the recipe shown in the table, and stirring the mixture with a mix rotor at 100 rpm for 30 minutes to obtain the pretreatment liquids.

[0092] In preparing pretreatment liquid 4, a mixed liquid containing an organic solvent and a surfactant was prepared according to the recipe shown in the table, and the mixed liquid was heated to 80°C using a hot stirrer. A resin powder of styrene acrylic resin (1) "Hi-Loss RS-1191" (product name, glass transition point 128°C) manufactured by Seiko PMC Corporation was weighed and added to the mixed liquid, and the mixed liquid was heated and stirred for 1 hour using a hot stirrer. After visually confirming that the resin powder had dissolved in the mixed liquid, the mixed liquid was cooled to room temperature to obtain a pretreatment liquid.

[0093] [Table 1]

[0094] In formulating the pretreatment liquid, the surfactant used was the silicone surfactant "BYK-3565" (product name, active ingredient 100 mass%) manufactured by BYK Japan Co., Ltd. The organic solvent used in formulating the pretreatment liquid is available from Tokyo Chemical Industry Co., Ltd., etc.

[0095] <Ink Preparation> The ink formulations are shown in Tables 2 and 3. The raw materials were mixed according to the formulations shown in the tables, φ0.5 mm zirconia beads were added, and the mixture was dispersed for 2 hours in a rocking mill (manufactured by Seiwa Giken Co., Ltd.). The zirconia beads were removed, and coarse particles were removed with a membrane filter to obtain ink.

[0096] [Table 2]

[0097] [Table 3]

[0098] The components used in the ink formulation are as follows: (Pigment) Carbon black: "#950" (product name) manufactured by Mitsubishi Chemical Corporation. (Pigment dispersant) "Solsperse 86000": Made by Lubrizol Corporation, 100% active ingredient. (Pigment dispersant) "Solsperse 75000": Made by Lubrizol Corporation, 100% active ingredient.

[0099] (binder resin) Epoxy resin (1): "jER1001" manufactured by Mitsubishi Chemical Corporation (epoxy equivalent: 450-500 g / eq). Epoxy resin (2): "jER819" manufactured by Mitsubishi Chemical Corporation (epoxy equivalent 180-220g / eq). Epoxy resin (3): "jER1007" manufactured by Mitsubishi Chemical Corporation (epoxy equivalent 1750~2200g / eq). Epoxy resin (4): "jER1009" manufactured by Mitsubishi Chemical Corporation (epoxy equivalent 2400~3300g / eq).

[0100] In the ink formulation, the surfactant used was a silicone surfactant "BYK-3565" (product name, active ingredient 100% by mass) manufactured by BYK Japan Co., Ltd. The organic solvents used in the ink formulation are available from Tokyo Chemical Industry Co., Ltd., etc.

[0101] <Creating printed matter> The substrates and printing equipment used in producing the printed matter are as follows. Base material: Polypropylene synthetic paper, "New Yupo FGS80" (product name) manufactured by Yupo Corporation. Printing device: Shuttle type inkjet printer, Mastermind's "MMP845H" (product name).

[0102] The prints were made according to the following procedure. (1) The pretreatment liquid was loaded into a shuttle-type inkjet printer, and the amount of the pretreatment liquid applied was 12 g / m. 2 The pretreatment liquid was then discharged onto synthetic polypropylene paper. (2) The synthetic polypropylene paper onto which the pretreatment liquid had been discharged was left to stand in a thermostatic chamber set at 120° C. for 1 minute and dried. (3) The ink was loaded into a shuttle-type inkjet printer, and the ink application amount was set to 20 g / m 2 The ink was discharged onto synthetic polypropylene paper that had been pretreated with the pretreatment liquid, and a solid image and a 10 pt fine print image were printed. (4) The printed synthetic polypropylene paper was dried by placing it in a thermostatic chamber set at 120° C. for 2 minutes. The printing was performed so that the areas to which the pretreatment liquid was applied and the ink were substantially aligned.

[0103] <Evaluation of printed matter> The obtained prints were subjected to the following evaluations, and the results are shown in Table 4.

[0104] "Alcohol abrasion resistance" A cotton swab was immersed in ethanol diluted to 60% with ion-exchanged water for at least 5 seconds, and then the cotton swab was used to rub the solid image of the printed matter under a load of 100 g, and the number of times until a specified area lost color was counted. The alcohol rub resistance was evaluated based on the number of rubs according to the following criteria.

[0105] AA: No color fading after 5 rubs. A: There is no discoloration after rubbing three times, but discoloration occurs in less than 30% of the area of ​​the rubbed part after rubbing five times. B: Discoloration occurred in 30% or less of the rubbed area after rubbing three times. C: Discoloration occurred in less than 50% of the rubbed area after rubbing three times. D: Discoloration occurred over more than 50% of the rubbed area after rubbing 3 or fewer times.

[0106] "Suppression of image bleeding" The solid image and the fine print image on the printed matter were visually observed, and the suppression of bleeding of the image was evaluated according to the following criteria.

[0107] A: No bleeding is observed in both solid images and fine print images. B: No bleeding is observed in the solid image, but bleeding is observed in the fine print image. C: Bleeding of fine print images is observed, and the edges of solid images are distorted.

[0108] [Table 4-1]

[0109] [Table 4-2]

[0110] [Table 4-3]

[0111] [Table 4-4]

[0112] As shown in the table, in each Example, the prints had excellent resistance to alcohol abrasion, and bleeding of the images was prevented.

[0113] In Comparative Example 1, the ink was applied directly to the printed matter without using a pretreatment liquid, so that the effect of alcohol abrasion resistance and suppression of image bleeding was not obtained. In Comparative Example 2, the aminoethylated acrylic resin contained in the pretreatment liquid had a low Tg, so that sufficient alcohol abrasion resistance was not obtained. In Comparative Example 3, the resin contained in the pretreatment liquid was a styrene acrylic resin, so that image bleeding occurred.

[0114] Each of the Examples had better image bleeding suppression performance than Comparative Examples 1 and 3. This is believed to be because the aminoethylated acrylic resin contained in the pretreatment liquids 1 and 2 bonded to the pigment in the ink, thereby suppressing image bleeding. Furthermore, each of the Examples had better alcohol rub resistance than Comparative Examples 1 to 3. In addition to the high Tg of the aminoethylated acrylic resin contained in the pretreatment liquid, it is believed that the alcohol rub resistance was improved by the bond formation between the aminoethyl group and the pigment.

[0115] In the comparison between Examples 1 and 2, and between Examples 3 and 4, the results are equivalent in terms of alcohol abrasion resistance and suppression of image bleeding, regardless of the difference in the ink. As a result of the amount of aminoethyl groups in the pretreatment liquid and the amount of epoxy groups in the ink being sufficient, strong bonds can be formed between the aminoethyl groups and the pigment, and between the (meth)acrylic resin A and the epoxy resin, and it is considered that the alcohol abrasion resistance and the suppression of image bleeding are equivalent regardless of the difference in the ink. In addition, it was confirmed from Example 13 that good results can be obtained even when the ink does not contain a binder resin.

[0116] In Examples 5 and 9, the same pretreatment liquid was used, but Example 5, which used Ink 3, had better alcohol abrasion resistance and image bleeding suppression performance. This is thought to be due to the fact that in Example 9, the epoxy resin contained in Ink 5 contained too many epoxy groups, which caused the aminoethylated acrylic resin to preferentially bond with the epoxy resin in the ink, and the pigment and the aminoethylated acrylic resin were not sufficiently bonded. It is thought that the same results were caused by the same factors in Examples 7 and 11.

[0117] In Examples 6 and 10, the same pretreatment liquid was used, but Example 6, which used Ink 4, had better ethanol abrasion resistance. This is thought to be due to the fact that in Example 10, the amount of epoxy groups in the epoxy resin contained in Ink 6 was too small, so that a strong coating film could not be formed to obtain sufficient alcohol abrasion resistance. It is thought that the same factors also caused the same results in Examples 8 and 12.

Claims

1. The pretreatment liquid is used in a method for applying a solvent inkjet ink to a substrate by the inkjet method and can be applied by the inkjet method, the pretreatment liquid for solvent inkjet ink comprising an organic solvent and a (meth)acrylic resin having a glass transition point (Tg) of 70° C. or higher and having an aminoethyl group.

2. A solvent inkjet ink set comprising: a solvent inkjet ink; and a pretreatment liquid, the solvent inkjet ink comprising an organic solvent, an epoxy resin, and a pigment, the pretreatment liquid being the pretreatment liquid for the solvent inkjet ink according to claim 1.

3. 3. The solvent inkjet ink set according to claim 2, wherein the epoxy resin of the solvent inkjet ink has an epoxy equivalent of 450 to 2200 g / eq.

4. 13. A method for producing a printed matter, comprising: applying the pretreatment liquid for a solvent ink-jet ink according to claim 1 to a substrate by an ink-jet method; and applying a solvent ink-jet ink to the substrate to which the pretreatment liquid has been applied by an ink-jet method.

5. The method for producing a printed matter according to claim 4 , wherein the substrate is a non-absorbent substrate.

Citation Information

Patent Citations

  • Solvent-based inkjet ink

    JP2015071681A