Thermosetting resin, cured product of the same and thermosetting composition

A linear copolymer-based thermosetting resin with specific aromatic compound units addresses the balance of dielectric properties, glass transition temperature, and melt viscosity, improving processability and moldability.

JP2024138812AActive Publication Date: 2024-10-09DKS CO LTD

Patent Information

Application Number
JP2023049509
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Conventional thermosetting resins face challenges in achieving a balance between dielectric properties, glass transition temperature, and low melt viscosity, leading to poor processability.

Method used

A thermosetting resin comprising a linear copolymer with repeating units of monovinyl monocyclic aromatic, divinyl aromatic, and monovinyl polycyclic aromatic compounds, specifically formulated to include 20-80 mol% monovinyl polycyclic aromatic compound, with a structure derived from a polymerization initiator, ensuring a linear structure without branching.

Benefits of technology

The resin achieves both excellent dielectric properties and glass transition temperature while maintaining low melt viscosity, enhancing processability and moldability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138812000001
    Figure 2024138812000001
  • Figure 2024138812000002
    Figure 2024138812000002
  • Figure 2024138812000003
    Figure 2024138812000003
Patent Text Reader

Abstract

To provide a thermosetting resin which can achieve both dielectric characteristics and a glass transition temperature, while maintaining low melting viscosity.SOLUTION: A thermosetting resin is a linear copolymer having a repeating unit corresponding to a monovinyl monocyclic aromatic compound, a repeating unit corresponding to a divinyl aromatic compound, and a repeating unit corresponding to a monovinyl polycyclic aromatic compound.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] FIELD OF THEINVENTION The present invention relates to a thermosetting resin and a cured product thereof, and also to a thermosetting composition containing the thermosetting resin. [Background technology]

[0002] In recent years, electronic devices have become smaller and more powerful, and the performance requirements for the materials used in them are increasing accordingly. For example, there is a demand for printed circuit board materials with low dielectric tangents that can be used for high-frequency communications.

[0003] For example, Patent Documents 1 and 2 disclose linear vinyl copolymers having repeating units corresponding to monovinyl aromatic compounds and repeating units corresponding to divinyl aromatic compounds as thermosetting resins that can produce cured products with excellent dielectric properties. These documents list styrene and vinylnaphthalene as monovinyl aromatic compounds. However, they do not disclose that the use of three components, a monovinyl monocyclic aromatic compound, a divinyl aromatic compound, and a monovinyl polycyclic aromatic compound, as constituent monomers can achieve both dielectric properties and glass transition temperature while maintaining a low melt viscosity.

[0004] On the other hand, Patent Document 3 discloses a copolymer of vinylnaphthalene, styrene and divinylbiphenyl as a high refractive index crosslinked resin for optical materials. However, since the copolymer is polymerized using a mixed solution of these monomers, the obtained copolymer has a branched chain. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2022-052522 [Patent Document 2] Patent No. 7017662 [Patent Document 3] Japanese Patent Application Publication No. 08-092322 Summary of the Invention [Problem to be solved by the invention]

[0006] Conventional thermosetting resins are not necessarily satisfactory in terms of dielectric properties, and even those with excellent dielectric properties have problems such as a low glass transition temperature and high melt viscosity, resulting in poor processability.

[0007] In view of the above, an object of an embodiment of the present invention is to provide a thermosetting resin that can achieve both dielectric properties and glass transition temperature while maintaining a low melt viscosity. [Means for solving the problem]

[0008] The present invention includes the embodiments set forth below. [1] A thermosetting resin that is a linear copolymer having a repeat unit corresponding to a monovinyl monocyclic aromatic compound, a repeat unit corresponding to a divinyl aromatic compound, and a repeat unit corresponding to a monovinyl polycyclic aromatic compound. [2] The thermosetting resin according to [1], wherein the content of the repeating unit corresponding to the monovinyl polycyclic aromatic compound is 20 to 80 mol % in 100 mol % of all repeating units. [3] The linear copolymer has a terminal end having the general formula (1): R 1 -N=NR 2 In the general formula (1), R 1 and R 2 each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group. [4] The thermosetting resin according to any one of [1] to [3], wherein the total content of the repeating units corresponding to the monovinyl monocyclic aromatic compound, the repeating units corresponding to the divinyl aromatic compound, and the repeating units corresponding to the monovinyl polycyclic aromatic compound is 80 mol % or more, based on 100 mol % of all repeating units. [5] The thermosetting resin according to any one of [1] to [4], wherein the monovinyl polycyclic aromatic compound has 3 or less rings. [6] A cured product obtained by curing the thermosetting resin according to any one of [1] to [5]. [7] A thermosetting composition comprising the thermosetting resin according to any one of [1] to [5]. [8] The thermosetting composition according to [7], which is a printed circuit board material. Effect of the Invention

[0009] According to an embodiment of the present invention, a thermosetting resin that can achieve both dielectric properties and glass transition temperature and has a low melt viscosity can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The thermosetting resin according to this embodiment is a copolymer having (A) a repeating unit corresponding to a monovinyl monocyclic aromatic compound, (B) a repeating unit corresponding to a divinyl aromatic compound, and (C) a repeating unit corresponding to a monovinyl polycyclic aromatic compound.

[0011] The repeating unit corresponding to the monovinyl monocyclic aromatic compound of (A) (hereinafter also referred to as "monovinyl monocyclic aromatic compound unit") is a structural unit of the copolymer, and is a structural unit having a structure formed by addition polymerization of a monovinyl monocyclic aromatic compound as a monomer. The repeating unit is not necessarily limited to one obtained by polymerization using the monovinyl monocyclic aromatic compound, as long as it has a structure corresponding to the monovinyl monocyclic aromatic compound, and may be one that is further reacted after polymerization to form a structure corresponding to the monovinyl monocyclic aromatic compound.

[0012] Monovinyl monocyclic aromatic compounds are compounds having one vinyl group and one aromatic ring, and are preferably monovinyl monocyclic aromatic hydrocarbons.Specific examples of monovinyl monocyclic aromatic compounds include styrene, alkylstyrenes (e.g., o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene), dialkylstyrenes (e.g., 3,5-dimethylstyrene, 2,5-dimethylstyrene, 2,5-diethylstyrene), and other styrene-based compounds, and these can be used alone or in combination of two or more.

[0013] In one embodiment, the monovinyl monocyclic aromatic compound unit preferably contains a repeating unit represented by the following general formula (2): The repeating unit of formula (2) has a structure in which the vinyl group of a styrene-based compound becomes a single bond through addition polymerization. [ka]

[0014] In formula (2), R 3 represents an aliphatic hydrocarbon group having 1 to 20 carbon atoms, and k represents an integer of 0 to 3. When k is 2 or more, R 3 may be the same or different. 3 is preferably an alkyl group having a carbon number of 1 to 3. k is preferably an integer of 0 to 2.

[0015] When the repeating unit represented by the above formula (2) is contained, the amount of the repeating unit represented by the formula (2) in 100 mol % of the monovinyl monocyclic aromatic compound units is preferably 70 mol % or more, more preferably 80 mol % or more, and even more preferably 90 mol % or more, and may be 100 mol %.

[0016] In one embodiment, the monovinyl monocyclic aromatic compound preferably contains styrene. In this case, the amount of repeating units corresponding to styrene (hereinafter also referred to as "styrene units") in 100 mol% of the monovinyl monocyclic aromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.

[0017] The repeating unit corresponding to the divinylaromatic compound of (B) (hereinafter also referred to as "divinylaromatic compound unit") is a structural unit of the copolymer, and is a structural unit having a structure with one vinyl group formed by addition polymerization of a divinylaromatic compound as a monomer. The repeating unit is not necessarily limited to one obtained by polymerization using the divinylaromatic compound, as long as it has a structure corresponding to the divinylaromatic compound, and may be one that is further reacted after polymerization to form a structure corresponding to the divinylaromatic compound.

[0018] The divinylaromatic compound unit may be a repeating unit having a structure in which one vinyl group of the divinylaromatic compound is converted into a single bond by addition polymerization, as represented by the following general formula (3). [ka]

[0019] In formula (3), R 4 represents a divalent aromatic hydrocarbon group having 6 to 30 carbon atoms. 4 is a divalent aromatic hydrocarbon group having 6 to 30 carbon atoms (more preferably 6 to 20 carbon atoms) selected from the group consisting of a phenylene group which may have a substituent, a biphenyldiyl group which may have a substituent, a naphthylene group which may have a substituent, and a terphenyldiyl group which may have a substituent. 4 When R has a substituent such as an alkyl group, the number of carbon atoms in the substituent is included in the number of carbon atoms in the substituent. 4 The total number of carbon atoms.

[0020] The divinyl aromatic compound forming such a repeating unit may be any aromatic compound having two vinyl groups, such as divinylbenzene (including each positional isomer or a mixture thereof), divinylnaphthalene (including each positional isomer or a mixture thereof), and divinylbiphenyl (including each positional isomer or a mixture thereof), and any one of these may be used alone or in combination of two or more.

[0021] In one embodiment, the divinylaromatic compound preferably contains at least one (B1) selected from the group consisting of divinylbenzene, divinylnaphthalene, and divinylbiphenyl. In this case, the amount of repeating units corresponding to the at least one (B1) in 100 mol% of the divinylaromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.

[0022] In one embodiment, the divinylaromatic compound preferably contains divinylbenzene (m-isomer, p-isomer, or a mixture of positional isomers thereof). In this case, the amount of repeating units corresponding to divinylbenzene (hereinafter also referred to as "divinylbenzene units") in 100 mol% of the divinylaromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.

[0023] The repeating unit corresponding to the monovinyl polycyclic aromatic compound of (C) (hereinafter also referred to as "monovinyl polycyclic aromatic compound unit") is a structural unit of the copolymer, and is a structural unit having a structure formed by addition polymerization of a monovinyl polycyclic aromatic compound as a monomer. The repeating unit is not necessarily limited to one obtained by polymerization using the monovinyl polycyclic aromatic compound, as long as it has a structure corresponding to the monovinyl polycyclic aromatic compound, and may be one that is further reacted after polymerization to form a structure corresponding to the monovinyl polycyclic aromatic compound.

[0024] The monovinyl polycyclic aromatic compound is a compound having one vinyl group and a plurality of aromatic rings, and is preferably a monovinyl polycyclic aromatic hydrocarbon. The monovinyl polycyclic aromatic compound may be a condensed polycyclic compound, a non-condensed polycyclic compound, or a combination of both.

[0025] Examples of monovinyl condensed polycyclic aromatic compounds include vinylnaphthalenes (e.g., 1-vinylnaphthalene, 2-vinylnaphthalene), vinylanthracenes (e.g., 1-vinylanthracene, 2-vinylanthracene, 9-vinylanthracene), vinylphenanthrenes (e.g., 9-vinylphenanthrene, 3-vinylphenanthrene), vinylpyrenes (e.g., 1-vinylpyrene, 4-vinylpyrene), and nuclear-substituted compounds thereof (e.g., nuclear alkyl-substituted monovinyl condensed polycyclic aromatic compounds such as alkylvinylnaphthalenes), and any one of these may be used alone or in combination of two or more.

[0026] Examples of monovinyl non-condensed polycyclic aromatic compounds include vinyl biphenyls (e.g., 4-vinyl biphenyl, 3-vinyl biphenyl), vinyl terphenyls (e.g., 4-vinyl-o-terphenyl), and nuclear-substituted products thereof (e.g., nuclear alkyl-substituted monovinyl non-condensed polycyclic aromatic compounds such as alkyl vinyl biphenyls), and any one of these may be used alone or in combination of two or more.

[0027] Among these, the monovinyl polycyclic aromatic compound is preferably one having 3 or less rings. Specifically, the monovinyl polycyclic aromatic compound preferably contains at least one (C1) selected from the group consisting of vinylnaphthalene, vinylanthracene, vinylphenanthrene, vinylbiphenyl, vinylterphenyl, and their nuclear alkyl-substituted derivatives. In this case, the amount of repeating units corresponding to the at least one (C1) in 100 mol% of monovinyl polycyclic aromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.

[0028] In one embodiment, the monovinyl polycyclic aromatic compound preferably contains vinylnaphthalene and / or its nuclear alkyl-substituted derivative, more preferably contains vinylnaphthalene. In detail, the monovinyl polycyclic aromatic compound unit preferably contains a repeating unit represented by the following general formula (4), more preferably contains a repeating unit corresponding to vinylnaphthalene (hereinafter also referred to as "vinylnaphthalene unit"). In this case, the amount of the repeating unit represented by formula (4) (preferably vinylnaphthalene unit) in 100 mol% of the monovinyl polycyclic aromatic compound unit is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%. [ka]

[0029] In formula (4), R 5 represents a naphthyl group which may have one or more alkyl groups as a substituent, and R 5 The number of carbon atoms is preferably 10 to 20, more preferably 10 to 15, and further preferably 10 to 13.

[0030] The thermosetting resin according to the present embodiment is a linear copolymer having the above three repeating units. The linear structure causes molecular chain entanglement, improving moldability. Here, linear refers to a structure in which the repeating units constituting the copolymer are linked together in a one-dimensional chain shape and bonded to each other, and refers to a structure without a cross-linked structure.

[0031] In the thermosetting resin, the monovinyl monocyclic aromatic compound units, the divinylaromatic compound units and the monovinyl polycyclic aromatic compound units may be arranged in a regular order or in a random order. The thermosetting resin is preferably a random copolymer in which the monovinyl monocyclic aromatic compound units, the divinylaromatic compound units and the monovinyl polycyclic aromatic compound units are arranged in a random order.

[0032] In addition to the monovinyl monocyclic aromatic compound unit, the divinyl aromatic compound unit, and the monovinyl polycyclic aromatic compound unit, the thermosetting resin may contain repeating units corresponding to other monomers, such as trivinyl aromatic compounds, trivinyl aliphatic compounds, divinyl aliphatic compounds, and monovinyl aliphatic compounds, to the extent that the effect of the other monomers is not impaired.

[0033] In the thermosetting resin, the content of the monovinyl monocyclic aromatic compound unit is not particularly limited, but is preferably 10 to 75 mol% out of 100 mol% of all repeating units constituting the copolymer. By being 10 mol% or more, the effect of reducing the melt viscosity is excellent. The content of the monovinyl monocyclic aromatic compound unit is more preferably 15 to 60 mol%, further preferably 20 to 55 mol%, and further preferably 22 to 50 mol%. In this specification, the total repeating units of 100 mol% does not include the structure derived from the polymerization initiator present at the end of the copolymer.

[0034] In the thermosetting resin, the content of the divinyl aromatic compound unit is not particularly limited, but is preferably 3 to 40 mol% in 100 mol% of all repeating units constituting the copolymer. By having a content of 3 mol% or more, it is possible to improve the thermosetting property to obtain a good cured product, and also to improve the glass transition temperature. The content of the divinyl aromatic compound unit is more preferably 5 to 30 mol%, further preferably 10 to 25 mol%, and further preferably 12 to 22 mol%.

[0035] In the thermosetting resin, the content of the monovinyl polycyclic aromatic compound unit is not particularly limited, but is preferably 20 to 80 mol % in 100 mol % of all repeating units constituting the copolymer. When it is 20 mol % or more, the effect of improving the dielectric properties and the glass transition temperature is excellent. When it is 80 mol % or less, the effect of reducing the melt viscosity is excellent. The content of the monovinyl polycyclic aromatic compound unit is more preferably 30 to 70 mol %, further preferably 35 to 65 mol %, and further preferably 35 to 62 mol %.

[0036] The total content of the monovinyl monocyclic aromatic compound units, the divinyl aromatic compound units and the monovinyl polycyclic aromatic compound units is preferably 80 mol % or more, more preferably 90 mol % or more, and may be 100 mol %, based on 100 mol % of all repeating units constituting the copolymer.

[0037] In one embodiment, the thermosetting resin is preferably a copolymer having a repeating unit represented by the above formula (2) (preferably a styrene unit), a repeating unit represented by the above formula (3) (preferably a divinylbenzene unit), and a repeating unit represented by the above formula (4) (preferably a vinylnaphthalene unit). In this case, the thermosetting resin preferably contains each repeating unit as follows, with the total repeating units constituting the copolymer being 100 mol %. In this case, the thermosetting resin may contain, together with these repeating units, the repeating units (A), (B), or (C) other than the repeating units. Repeating units represented by formula (2) (preferably styrene units): 10 to 75 mol %, preferably 15 to 60 mol %, more preferably 20 to 55 mol %, and even more preferably 22 to 50 mol %. Repeating units represented by formula (3) (preferably divinylbenzene units): 3 to 40 mol %, preferably 5 to 30 mol %, more preferably 10 to 25 mol %, and even more preferably 12 to 22 mol %. Repeating units represented by formula (4) (preferably vinylnaphthalene units): 20 to 80 mol %, preferably 30 to 70 mol %, more preferably 35 to 65 mol %, and even more preferably 35 to 62 mol %.

[0038] The thermosetting resin may have at least one of a structure derived from a polymerization initiator represented by the following general formula (1) or a structure derived from a polymerization initiator represented by the following general formula (5) at the end of a linear copolymer. The polymerization initiator represented by formula (1) is an azo initiator having no cyano group, unlike azobisisobutyronitrile (AIBN), which is a general-purpose azo initiator. The polymerization initiator represented by formula (5) is an organic peroxide such as dialkyl peroxide. By using the polymerization initiator represented by formula (1) among these, better dielectric properties can be imparted. R 1 -N=NR 2 (1) R 6 -OOR 7 (5)

[0039] In formula (1) and formula (5), R 1 , R 2 , R 6 and R 7 each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group, and does not contain a heteroatom. The number of carbon atoms in the saturated hydrocarbon group is not particularly limited, but is preferably 1 to 23, and more preferably 4 to 13. The number of carbon atoms in the aromatic hydrocarbon group is not particularly limited, but is preferably 6 to 23, and more preferably 6 to 13.

[0040] The saturated hydrocarbon group may be a branched or straight-chain saturated aliphatic hydrocarbon group (alkyl group) or a saturated alicyclic hydrocarbon group. Specific examples of the saturated hydrocarbon group include alkyl groups such as tert-butyl group, tert-pentyl group, tert-hexyl group, and 1,1,3,3-tetramethylbutyl group, and saturated alicyclic hydrocarbon groups such as cyclohexyl group.

[0041] Specific examples of the aromatic hydrocarbon group include aryl groups such as a phenyl group, a tolyl group, and a naphthyl group, a cumyl group, a benzyl group, and a phenethyl group. base Examples of aralkyl groups include the following.

[0042] In one embodiment, R 1 , R 2 , R 6 and R 7 may each independently be a group represented by the following general formula (6): [ka]

[0043] In formula (6), R 8 , R 9 and R 10 each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group. More preferably, R 8 represents a monovalent saturated hydrocarbon group having 1 to 20 carbon atoms (more preferably 1 to 10 carbon atoms) or a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms (more preferably 6 to 10 carbon atoms); R 9 and R 10 R represents a methyl group. 8 , R 9 and R 10 (Preferably R 8 The saturated hydrocarbon group for R may be branched or linear, and examples thereof include alkyl groups such as methyl, ethyl, propyl, butyl, heptyl, isopropyl, tert-butyl, and 2,2-dimethylpropyl, and saturated alicyclic hydrocarbon groups such as cyclohexyl. 8 , R 9 and R 10 (Preferably R 8 ) Aromatic hydrocarbons include a phenyl group, a tolyl group, a naphthyl group, and the like.

[0044] When a vinyl copolymer is synthesized by radical polymerization using these polymerization initiators, both ends of the obtained vinyl copolymer usually have a structure derived from the polymerization initiator.1 - and / or R 2 - at both ends of the copolymer. 1 -But it's okay, both are R 2 - is also acceptable, and one end is R 1 - and the other end is R 2 On the other hand, when polymerization is performed using the polymerization initiator of the above formula (5), R 6 O- and / or R 7 A copolymer having O- at both ends is obtained. In other words, both ends of the copolymer are R 6 O- is also acceptable, both are R 7 O- is also acceptable, and one end is R 6 O- and the other end is R 7 O- is also acceptable.

[0045] The weight average molecular weight Mw of the thermosetting resin is not particularly limited, and may be, for example, 1,000 to 100,000, 2,000 to 50,000, or 3,000 to 20,000. By having a weight average molecular weight Mw of 1,000 or more, it is possible to reduce the concentration of terminal groups derived from the polymerization initiator, thereby improving the dielectric properties, and also to improve the glass transition temperature. In addition, by having a weight average molecular weight Mw of 100,000 or less, it is possible to reduce the melt viscosity. Here, the weight average molecular weight Mw is a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).

[0046] The method for producing the thermosetting resin is not particularly limited. As a method for synthesizing a linear copolymer, in a preferred embodiment of the production method, a vinylbenzylphosphonium salt, a monovinyl monocyclic aromatic compound, and a monovinyl polycyclic aromatic compound are copolymerized using at least one of the polymerization initiator represented by the above formula (1) or the polymerization initiator represented by the formula (5), and the copolymer obtained is reacted with formaldehyde. However, the production method is not limited to this method.

[0047] As the vinylbenzyl phosphonium salt, it is preferable to use vinylbenzyl phosphonium halide.As the phosphonium group in the vinylbenzyl phosphonium salt, for example, quaternary phosphonium groups such as trialkyl phosphonium, triaryl phosphonium, and triaryl alkyl phosphonium can be mentioned.In addition, as the halogen that forms a salt with the phosphonium group, for example, chlorine, bromine, etc. can be mentioned.

[0048] The vinylbenzylphosphonium salt can be copolymerized with a monovinyl monocyclic aromatic compound and a monovinyl polycyclic aromatic compound by a known vinyl polymerization method. By using the radical polymerization initiator represented by the above formula (1) and / or formula (5) as a polymerization initiator, a copolymer having a repeating unit derived from a vinylbenzylphosphonium salt, a repeating unit derived from a monovinyl monocyclic aromatic compound, and a repeating unit derived from a monovinyl polycyclic aromatic compound can be obtained. During polymerization, a chain transfer agent may be added to adjust the molecular weight of the copolymer.

[0049] The method for reacting the obtained copolymer with formaldehyde can be the well-known Wittig reaction, in which the copolymer is treated with a base and then reacted with formaldehyde, whereby the phosphonium group is removed and a vinyl group is introduced.

[0050] In this production method, since the vinylbenzyl phosphonium salt is monovinyl in the copolymerization step, a linear copolymer without branches can be obtained, and since a vinyl group is introduced into the repeating unit derived from the vinylbenzyl phosphonium salt after copolymerization, a linear copolymer without branches can be obtained while having a repeating unit corresponding to the divinyl aromatic compound.

[0051] The thermosetting composition according to the present embodiment contains the thermosetting resin. The content of the thermosetting resin in the thermosetting composition is not particularly limited as long as the composition has the property of being cured by heat. For example, the content may be 1 to 99% by mass or 10 to 95% by mass relative to 100% by mass of the solid content of the thermosetting composition (the amount excluding the organic solvent when the organic solvent described below is contained, and the amount of the entire composition when the organic solvent is not contained).

[0052] In addition to the above-mentioned thermosetting resin, the thermosetting composition may contain various components such as other thermosetting resins (thermosetting crosslinking agents), thermoplastic resins, fillers, flame retardants, curing accelerators, polymerization initiators, defoamers, heat stabilizers, antistatic agents, ultraviolet absorbers, colorants such as dyes and pigments, lubricants, and dispersants.

[0053] The thermosetting composition may contain an organic solvent to adjust its viscosity, and the thermosetting composition may be a solution containing the thermosetting resin. The organic solvent used may be one capable of dissolving the thermosetting resin, and examples of the organic solvent include ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, esters such as ethyl acetate, propyl acetate, and butyl acetate, amides such as dimethylacetamide and dimethylformamide, and aromatic hydrocarbons such as toluene and xylene, and any one or more of these may be used in combination.

[0054] The thermosetting resin or thermosetting composition of the present embodiment has a vinyl group in the molecular chain of the copolymer, and therefore can be crosslinked by polymerization, and a cured product can be obtained by thermal curing. The cured product has a low dielectric tangent and dielectric constant and excellent dielectric properties, and can be used for electronic materials such as printed circuit board materials and semiconductor sealing materials. That is, the thermosetting composition according to one embodiment is a thermosetting composition for electronic materials.

[0055] Examples of the printed circuit board material include rigid printed circuit board materials such as single-sided boards, double-sided boards, multilayer boards, and build-up boards, and film- or sheet-shaped flexible printed circuit board materials. In addition, because of its excellent dielectric properties, it is suitably used as a high-frequency board material for use in high-frequency communication devices. EXAMPLES

[0056] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0057] <Measurement and evaluation method> [Molar ratio of styrene / divinylbenzene / vinylnaphthalene] The products and compositions obtained in Examples 1 to 9, 11 to 13, and Comparative Examples 1, 4, 5, and 8 were dissolved in deuterated chloroform and analyzed by a nuclear magnetic resonance spectrometer (JEOL). 1 H-NMR measurement was carried out to determine the molar ratios of the repeating units corresponding to styrene, the repeating units corresponding to divinylbenzene, and the repeating units relative to vinylnaphthalene, and the content of the repeating units corresponding to styrene (styrene ratio), the content of the repeating units corresponding to divinylbenzene (divinylbenzene ratio), and the content of the repeating units corresponding to vinylnaphthalene (vinylnaphthalene ratio) relative to 100 mol% of all repeating units were calculated.

[0058] [Molar ratio of styrene / divinylbenzene / vinylnaphthalene / vinylcyclohexane] The products obtained in Example 10 and Comparative Examples 2 and 6 were dissolved in deuterated chloroform and analyzed by a nuclear magnetic resonance spectrometer (JEOL). 1H-NMR measurement was carried out to determine the molar ratios of repeating units corresponding to styrene, repeating units corresponding to divinylbenzene, repeating units relative to vinylnaphthalene, and repeating units relative to vinylcyclohexane, and the content of repeating units corresponding to styrene relative to 100 mol% of all repeating units (styrene ratio), the content of repeating units corresponding to divinylbenzene (divinylbenzene ratio), the content of repeating units corresponding to vinylnaphthalene (vinylnaphthalene ratio), and the content of repeating units corresponding to vinylcyclohexane (vinylcyclohexane ratio) were calculated.

[0059] [Molar ratio of styrene / divinylbenzene / isobornyl acrylate] The products obtained in Comparative Examples 3 and 7 were dissolved in deuterated chloroform and analyzed by a nuclear magnetic resonance spectrometer (JEOL). 1 H-NMR measurement was carried out to determine the molar ratios of the repeating units corresponding to styrene, the repeating units corresponding to divinylbenzene, and the repeating units corresponding to isobornyl acrylate, and the content of the repeating units corresponding to styrene (styrene ratio), the content of the repeating units corresponding to divinylbenzene (divinylbenzene ratio), and the content of the repeating units corresponding to isobornyl acrylate (isobornyl acrylate ratio) relative to 100 mol% of all repeating units were calculated.

[0060] [Weight average molecular weight] The products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 8 were dissolved in tetrahydrofuran, and the weight average molecular weight Mw in terms of polystyrene was measured by gel permeation chromatography (GPC) (Prominence, Shimadzu Corporation) connected to four columns (Shodex GPC columns KF-601, KF-602, KF-603, KF-604, Showa Denko Corporation) filled with polystyrene gel. A differential refractive index detector (Shodex RI-504, Showa Denko Corporation) was used, with the column oven temperature at 40°C, the THF flow rate at 0.6 mL / min, the sample concentration at 0.1 mass%, and the sample injection amount at 10 μL.

[0061] [Dielectric constant, dielectric loss tangent] The products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 8 were used as samples. Using a single-action compression molding machine for testing (manufactured by Yasuda Seiki Seisakusho), 1.5 g of sample was pressed for 15 minutes at a pressure of 10 MPa and a temperature of 220°C to produce a flat plate of 30 mm x 30 mm x 1 mm thickness. The obtained flat plate was cut to produce a test piece of 2 mm width, 1 mm thickness, and 30 mm length. The dielectric constant and dielectric loss tangent of the test piece at 10 GHz were measured using a cavity resonator method dielectric constant measuring device (manufactured by KEYSIGHT), and evaluated according to the following criteria.

[0062] Those with a dielectric constant of less than 2.4 were rated as "A" (excellent), those between 2.4 and 2.5 were rated as "B" (good), those between 2.5 and 2.6 were rated as "C" (fair), those between 2.6 and 2.7 were rated as "D" (poor), and those above 2.7 were rated as "E" (poor).

[0063] Those with a dielectric tangent of less than 0.001 were rated as "A" (excellent), those between 0.001 and 0.002 were rated as "B" (good), those between 0.002 and 0.003 were rated as "C" (fair), those between 0.003 and 0.004 were rated as "D" (poor), and those 0.004 or greater were rated as "E" (poor).

[0064] [Glass transition temperature Tg] The flat plate prepared according to the above [dielectric constant, dielectric tangent] was cut to prepare a test piece with a width of 5 mm, a thickness of 1 mm, and a length of 25 mm. The glass transition temperature of this test piece was measured using a dynamic viscoelasticity measuring device: Rheogel-E4000 (manufactured by UBM Co., Ltd.). The maximum value of the loss tangent (tan δ) measured for the test piece under the conditions of a tensile sine wave, dynamic strain of 5 μm, frequency of 1 Hz, and temperature rise rate of 3 ° C. / min was obtained as the glass transition temperature. Glass transition temperatures of 170 ° C. or higher were rated as "A" (excellent), those of 160 ° C. or higher and lower than 170 ° C. were rated as "B" (good), those of 150 ° C. or higher and lower than 160 ° C. were rated as "C" (average), and those of less than 150 ° C. were rated as "D" (poor).

[0065] [Melt viscosity (minimum melt viscosity)] The products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 8 were used as samples. 0.4 g of sample was pressed for 1 minute at a pressure of 10 MPa using a manual hydraulic pump: P-1B (manufactured by Riken) to produce pellets with a diameter of 20 mm and a thickness of 1 mm. The obtained pellets were used as samples and heated from 50°C to 200°C at a heating rate of 5°C / min using a rheometer: MCR 302 (manufactured by Anton Paar). The minimum value of the complex viscosity was taken as the minimum melt viscosity, and a minimum melt viscosity of less than 50,000 poise was rated as "○" (low viscosity), and a minimum melt viscosity of 50,000 poise or more was rated as "×" (high viscosity).

[0066] (Synthesis Example 1) Compound 1: Synthesis of vinylbenzyltriphenylphosphonium chloride Vinylbenzyl chloride (trade name: CMS-14, manufactured by AGC Seimi Chemical Co., Ltd.) 1.5 mol (228.9 g), triphenylphosphine 1.8 mol (472.1 g), and dimethylformamide 622.4 g were charged into a 2.0 L reactor and reacted at 70° C. for 3 hours under nitrogen conditions to precipitate a white solid. The solid was thoroughly washed with acetone and then dried under reduced pressure at 92° C. to recover 490 g of compound 1.

[0067] (Synthesis Example 2) Synthesis of Copolymer A 11.1 g of styrene, 12.4 g of compound 1, 12.0 g of 2-vinylnaphthalene, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene as a chain transfer agent, 1.35 g of 2,2'-azobis(2,4,4-trimethylpentane) (product name: VR-110, Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator, and 82.7 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer A as a dimethylformamide solution.

[0068] (Synthesis Example 3) Synthesis of Copolymer B 8.2 g of styrene, 13.8 g of compound 1, 10.0 g of 2-vinylnaphthalene, 3.3 g of 2,4-diphenyl-4-methyl-1-pentene, 1.21 g of 2,2'-azobis(2,4,4-trimethylpentane), and 74.6 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer B as a dimethylformamide solution.

[0069] (Synthesis Example 4) Synthesis of Copolymer C 13.3 g of styrene, 8.9 g of compound 1, 13.0 g of 2-vinylnaphthalene, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 1.34 g of 2,2'-azobis(2,4,4-trimethylpentane), and 82.3 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer C as a dimethylformamide solution.

[0070] (Synthesis Example 5) Synthesis of Copolymer D 13.5 g of styrene, 12.4 g of compound 1, 9.0 g of 2-vinylnaphthalene, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.33 g of 2,2'-azobis(2,4,4-trimethylpentane), and 81.4 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer D as a dimethylformamide solution.

[0071] (Synthesis Example 6) Synthesis of Copolymer E 5.8 g of styrene, 11.7 g of compound 1, 17.0 g of 2-vinylnaphthalene, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.31 g of 2,2'-azobis(2,4,4-trimethylpentane), and 80.5 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer E as a dimethylformamide solution.

[0072] (Synthesis Example 7) Synthesis of Copolymer F 11.9 g of styrene, 8.9 g of compound 1, 14.5 g of 2-vinylnaphthalene, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 1.34 g of 2,2'-azobis(2,4,4-trimethylpentane), and 82.2 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer F as a dimethylformamide solution.

[0073] (Synthesis Example 8) Synthesis of Copolymer G 9.5 g of styrene, 14.2 g of compound 1, 9.0 g of 2-vinylnaphthalene, 3.4 g of 2,4-diphenyl-4-methyl-1-pentene, 1.24 g of 2,2'-azobis(2,4,4-trimethylpentane), and 76.1 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer G as a dimethylformamide solution.

[0074] (Synthesis Example 9) Synthesis of Copolymer H 4.1 g of styrene, 13.8 g of compound 1, 15.0 g of 2-vinylnaphthalene, 3.4 g of 2,4-diphenyl-4-methyl-1-pentene, 1.25 g of 2,2'-azobis(2,4,4-trimethylpentane), and 76.7 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer H as a dimethylformamide solution.

[0075] (Synthesis Example 10) Synthesis of Copolymer I 16.4 g of styrene, 9.2 g of compound 1, 10.0 g of 2-vinylnaphthalene, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 1.35 g of 2,2'-azobis(2,4,4-trimethylpentane), and 83.0 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer I as a dimethylformamide solution.

[0076] (Synthesis Example 11) Synthesis of Copolymer J 5.6 g of styrene, 11.4 g of compound 1, 5.0 g of 2-vinylnaphthalene, 7.2 g of vinylcyclohexane, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 1.34 g of 2,2'-azobis(2,4,4-trimethylpentane), and 82.0 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer J as a dimethylformamide solution.

[0077] (Synthesis Example 12) Synthesis of Copolymer K 10.1 g of styrene, 11.4 g of compound 1, 11.0 g of 2-vinylnaphthalene, 3.4 g of 2,4-diphenyl-4-methyl-1-pentene, 0.71 g of di-tert-butyl peroxide (product name: Perbutyl D, manufactured by NOF Corp.) as a polymerization initiator, and 75.8 g of dimethylformamide were placed in a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions to obtain copolymer K as a dimethylformamide solution.

[0078] (Synthesis Example 13) Synthesis of Copolymer L 11.1 g of styrene, 12.4 g of compound 1, 12.0 g of 2-vinylnaphthalene, 2.5 g of 2,4-diphenyl-4-methyl-1-pentene, 1.35 g of 2,2'-azobis(2,4,4-trimethylpentane), and 82.7 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer L as a dimethylformamide solution.

[0079] (Synthesis Example 14) Synthesis of Copolymer M 10.1 g of styrene, 11.4 g of compound 1, 11.0 g of 2-vinylnaphthalene, 6.8 g of 2,4-diphenyl-4-methyl-1-pentene, 2.47 g of 2,2'-azobis(2,4,4-trimethylpentane), and 75.8 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 1.5 hours under nitrogen conditions to obtain copolymer M as a dimethylformamide solution.

[0080] (Comparative Synthesis Example 1) Synthesis of Copolymer N 22.0 g of styrene, 15.5 g of compound 1, 3.9 g of 2,4-diphenyl-4-methyl-1-pentene, 0.82 g of di-tert-butyl peroxide, and 87.4 g of dimethylformamide were charged into a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions to obtain copolymer N as a dimethylformamide solution.

[0081] (Comparative Synthesis Example 2) Synthesis of Copolymer O 9.9 g of styrene, 11.1 g of compound 1, 14.0 g of vinylcyclohexane, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 0.53 g of di-tert-butyl peroxide, and 81.4 g of dimethylformamide were charged into a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions to obtain copolymer O as a dimethylformamide solution.

[0082] (Comparative Synthesis Example 3) Synthesis of Copolymer P 9.2 g of styrene, 10.7 g of compound 1, 15.0 g of isobornyl acrylate, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 0.77 g of di-tert-butyl peroxide, and 81.4 g of dimethylformamide were placed in a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions to obtain copolymer P as a dimethylformamide solution.

[0083] (Comparative Synthesis Example 4) Synthesis of Copolymer Q 10.7 g of compound 1, 22.0 g of 2-vinylnaphthalene, 3.4 g of 2,4-diphenyl-4-methyl-1-pentene, 1.24 g of 2,2'-azobis(2,4,4-trimethylpentane), and 76.3 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer Q as a dimethylformamide solution.

[0084] (Comparative Synthesis Example 5) Synthesis of Copolymer R 9.9 g of styrene, 11.1 g of compound 1, 14.0 g of vinylcyclohexane, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.33 g of 2,2'-azobis(2,4,4-trimethylpentane), and 81.7 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer R as a dimethylformamide solution.

[0085] (Comparative Synthesis Example 6) Synthesis of Copolymer S 9.2 g of styrene, 10.7 g of compound 1, 15.0 g of isobornyl acrylate, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.33 g of 2,2'-azobis(2,4,4-trimethylpentane), and 81.4 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer S as a dimethylformamide solution.

[0086] (Comparative Synthesis Example 7) Synthesis of Copolymer T 17.0g of styrene, 16.9g of compound 1, 3.5g of 2,4-diphenyl-4-methyl-1-pentene, 1.29g of 2,2'-azobis(2,4,4-trimethylpentane), and 79.2g of dimethylformamide were charged into a 500mL reactor and reacted at 120°C for 2 hours under nitrogen conditions to obtain a dimethylformamide solution. 117.9g of this dimethylformamide solution, 117.9g of toluene, 32.9g of 37% by mass formalin, and 40.6g of 28% by mass aqueous potassium hydroxide solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After dehydrating and concentrating the organic layer, 23.3g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solid was removed by filtration and then dried under reduced pressure at 60° C. to recover 13.0 g of copolymer T. Copolymer T had Mw of 6400, a styrene ratio of 79.5 mol %, and a divinylbenzene ratio of 20.5 mol %.

[0087] (Comparative Synthesis Example 8) Synthesis of Polymer U 35.0 g of 2-vinylnaphthalene, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.33 g of 2,2'-azobis(2,4,4-trimethylpentane), and 81.7 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 4 hours under nitrogen conditions. This reaction solution was reprecipitated in a large excess of methanol, and the supernatant was decanted. The remaining solid was dried under reduced pressure at 92°C to recover 33.2 g of polymer U.

[0088] Example 1 123.2g of the dimethylformamide solution of copolymer A obtained in Synthesis Example 2, 123.2g of toluene, 29.1g of 37% by mass formalin, and 35.9g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 17.0g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 1 was recovered by drying under reduced pressure at 60°C, resulting in 15.6g of product 1. The Mw of product 1 was 7200, the styrene ratio was 43.7 mol%, the divinylbenzene ratio was 15.7 mol%, and the 2-vinylnaphthalene ratio was 40.6 mol%.

[0089] Example 2 111.0 g of the dimethylformamide solution of copolymer B obtained in Synthesis Example 3, 111.0 g of toluene, 32.3 g of 37% by mass formalin, and 39.9 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 18.9 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 2 was dried under reduced pressure at 60°C to recover 13.1 g. The Mw of product 2 was 7100, the styrene ratio was 38.9 mol%, the divinylbenzene ratio was 20.8 mol%, and the 2-vinylnaphthalene ratio was 40.3 mol%.

[0090] Example 3 122.5g of the dimethylformamide solution of copolymer C obtained in Synthesis Example 4, 122.5g of toluene, 21.0g of 37% by mass formalin, and 25.9g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 12.3g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 3 was recovered in 17.2g by drying under reduced pressure at 60°C. The Mw of product 3 was 7500, the styrene ratio was 48.1 mol%, the divinylbenzene ratio was 11.0 mol%, and the 2-vinylnaphthalene ratio was 40.9 mol%.

[0091] Example 4 121.3 g of the dimethylformamide solution of copolymer D obtained in Synthesis Example 5, 121.3 g of toluene, 29.1 g of 37% by mass formalin, and 35.9 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 17.0 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 4 was recovered in 15.5 g by drying under reduced pressure at 60°C. The Mw of product 4 was 7000, the styrene ratio was 54.2 mol%, the divinylbenzene ratio was 15.5 mol%, and the 2-vinylnaphthalene ratio was 30.3 mol%.

[0092] Example 5 119.9g of the dimethylformamide solution of copolymer E obtained in Synthesis Example 6, 119.9g of toluene, 27.4g of 37% by mass formalin, and 33.9g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 16.1g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. The solid matter was removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solid was removed by filtration, and 15.4g of product 5 was recovered by drying under reduced pressure at 60°C. The Mw of product 5 was 7300, the styrene ratio was 22.7 mol%, the divinylbenzene ratio was 15.8 mol%, and the 2-vinylnaphthalene ratio was 61.5 mol%.

[0093] Example 6 122.5g of the dimethylformamide solution of copolymer F obtained in Synthesis Example 7, 122.5g of toluene, 20.8g of 37% by mass formalin, and 25.7g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 12.2g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. The solid matter was removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solid was removed by filtration, and 17.1g of product 6 was recovered by drying under reduced pressure at 60°C. The Mw of product 6 was 7400, the styrene ratio was 44.6 mol%, the divinylbenzene ratio was 10.1 mol%, and the 2-vinylnaphthalene ratio was 45.3 mol%.

[0094] Example 7 113.4g of the dimethylformamide solution of copolymer G obtained in Synthesis Example 8, 113.4g of toluene, 33.2g of 37% by mass formalin, and 41.0g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 19.5g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 13.2g of product 7. The Mw of product 7 was 6800, the styrene ratio was 44.5 mol%, the divinylbenzene ratio was 20.0 mol%, and the 2-vinylnaphthalene ratio was 35.5 mol%.

[0095] Example 8 114.2g of the dimethylformamide solution of copolymer H obtained in Synthesis Example 9, 114.2g of toluene, 32.3g of 37% by mass formalin, and 39.9g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 18.9g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 13.6g of product 8. The Mw of product 8 was 7200, the styrene ratio was 18.7 mol%, the divinylbenzene ratio was 20.3 mol%, and the 2-vinylnaphthalene ratio was 61.0 mol%.

[0096] Example 9 123.6 g of the dimethylformamide solution of copolymer I obtained in Synthesis Example 10, 123.6 g of toluene, 21.5 g of 37 mass% formalin, and 26.6 g of 28 mass% potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 12.6 g of anhydrous magnesium chloride was charged and stirred at 65 ° C. for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 9 was recovered in 17.0 g by drying under reduced pressure at 60 ° C. The Mw of product 9 was 7400, the styrene ratio was 58.7 mol%, the divinylbenzene ratio was 10.7 mol%, and the 2-vinylnaphthalene ratio was 30.6 mol%.

[0097] Example 10 122.1 g of the dimethylformamide solution of copolymer J obtained in Synthesis Example 11, 122.1 g of toluene, 26.6 g of 37 mass% formalin, and 32.9 g of 28 mass% potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 15.6 g of anhydrous magnesium chloride was charged and stirred at 65 ° C. for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60 ° C. to recover 11.5 g of product 10. The Mw of product 10 was 7600, the styrene ratio was 25.0 mol%, the divinylbenzene ratio was 16.1 mol%, the 2-vinylnaphthalene ratio was 40.8 mol%, and the vinylcyclohexane ratio was 18.1 mol%.

[0098] Example 11 114.9g of the dimethylformamide solution of copolymer K obtained in Synthesis Example 12, 114.9g of toluene, 26.6g of 37% by mass formalin, and 32.9g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 15.6g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. The solid matter was removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solid was removed by filtration, and 14.5g of product 11 was recovered by drying under reduced pressure at 60°C. The Mw of product 11 was 7000, the styrene ratio was 44.1 mol%, the divinylbenzene ratio was 15.5 mol%, and the 2-vinylnaphthalene ratio was 40.4 mol%.

[0099] Example 12 122.0 g of the dimethylformamide solution of copolymer L obtained in Synthesis Example 13, 122.0 g of toluene, 29.1 g of 37% by mass formalin, and 35.9 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 17.0 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 15.5 g of product 12. The Mw of product 12 was 9900, the styrene ratio was 43.2 mol%, the divinylbenzene ratio was 16.0 mol%, and the 2-vinylnaphthalene ratio was 40.8 mol%.

[0100] (Example 13) 117.5g of the dimethylformamide solution of copolymer M obtained in Synthesis Example 14, 117.5g of toluene, 26.6g of 37% by mass formalin, and 32.9g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 15.6g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 14.0g of product 13. The Mw of product 13 was 2800, the styrene ratio was 44.4 mol%, the divinylbenzene ratio was 15.4 mol%, and the 2-vinylnaphthalene ratio was 40.2 mol%.

[0101] Comparative Example 1 129.7 g of the dimethylformamide solution of copolymer N obtained in Comparative Synthesis Example 1, 129.7 g of toluene, 36.2 g of 37% by mass formalin, and 44.7 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 21.3 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and 15.6 g of product 14 was recovered by drying under reduced pressure at 60°C. The Mw of product 14 was 5600, the styrene ratio was 83.2 mol%, and the divinylbenzene ratio was 16.8 mol%.

[0102] Comparative Example 2 121.0 g of the dimethylformamide solution of copolymer O obtained in Comparative Synthesis Example 2, 121.0 g of toluene, 26.1 g of 37% by mass formalin, and 32.2 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 15.3 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 15.8 g of product 15. The Mw of product 15 was 7100, the styrene ratio was 45.2 mol%, the divinylbenzene ratio was 16.4 mol%, and the vinylcyclohexane ratio was 38.4 mol%.

[0103] Comparative Example 3 120.7 g of the dimethylformamide solution of copolymer P obtained in Comparative Synthesis Example 3, 120.7 g of toluene, 25.2 g of 37% by mass formalin, and 31.1 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 14.8 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 16 was recovered in 16.0 g by drying under reduced pressure at 60°C. The Mw of product 16 was 7000, the styrene ratio was 43.4 mol%, the divinylbenzene ratio was 15.6 mol%, and the isobornyl acrylate ratio was 41.0 mol%.

[0104] Comparative Example 4 49.2g of styrene, 20.0g of vinylnaphthalene, 9.3g of 2,4-diphenyl-4-methyl-1-pentene, 3.39g of 2,2'-azobis(2,4,4-trimethylpentane), and 208.1g of dimethylformamide were charged into a 500mL reactor and reacted at 120°C for 3 hours under nitrogen conditions. This reaction solution was reprecipitated in a large excess of methanol, and the supernatant was decanted. The remaining solid was dried under reduced pressure at 80°C to recover 51.9g of product 17. The Mw of product 17 was 6500, the styrene ratio was 58.9 mol%, and the 2-vinylnaphthalene ratio was 41.1 mol%.

[0105] Comparative Example 5 113.6 g of the dimethylformamide solution of copolymer Q obtained in Comparative Synthesis Example 4, 113.6 g of toluene, 25.1 g of 37% by mass formalin, and 31.0 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 14.7 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. The solid matter was removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solid was removed by filtration, and 14.9 g of product 18 was recovered by drying under reduced pressure at 60°C. The Mw of product 18 was 7500, the divinylbenzene ratio was 15.2 mol%, and the 2-vinylnaphthalene ratio was 84.8 mol%.

[0106] Comparative Example 6 121.7 g of the dimethylformamide solution of copolymer R obtained in Comparative Synthesis Example 5, 121.7 g of toluene, 26.1 g of 37% by mass formalin, and 32.2 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 15.3 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 15.8 g of product 19. The Mw of product 19 was 7200, the styrene ratio was 46.4 mol%, the divinylbenzene ratio was 16.6 mol%, and the vinylcyclohexane ratio was 37.0 mol%.

[0107] Comparative Example 7 121.2 g of the dimethylformamide solution of copolymer S obtained in Comparative Synthesis Example 6, 121.2 g of toluene, 25.2 g of 37 mass% formalin, and 31.1 g of 28 mass% potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 14.8 g of anhydrous magnesium chloride was charged and stirred at 65 ° C. for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 20 was recovered in 16.0 g by drying under reduced pressure at 60 ° C. The Mw of product 20 was 7300, the styrene ratio was 44.5 mol%, the divinylbenzene ratio was 15.3 mol%, and the isobornyl acrylate ratio was 40.2 mol%.

[0108] Comparative Example 8 4.3 g of Copolymer T obtained in Comparative Synthesis Example 7 and 4.0 g of Polymer U obtained in Comparative Synthesis Example 8 were mixed and dissolved in toluene to obtain a homogeneous solution. This solution was dried under reduced pressure at 60°C to recover 8.0 g of Composition 1. Composition 1 had an Mw of 7700, a styrene ratio of 47.7 mol%, a divinylbenzene ratio of 12.3 mol%, and a 2-vinylnaphthalene ratio of 40.0 mol%.

[0109] The dielectric constant, dielectric tangent, glass transition temperature, and melt viscosity were evaluated for the products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 8. The results are shown in Tables 1 to 5 below.

[0110] [Table 1]

[0111] [Table 2]

[0112] [Table 3]

[0113] [Table 4]

[0114] [Table 5]

[0115] Example 11 and Comparative Examples 1 to 3 are examples in which a peroxide-type polymerization initiator was used. In Comparative Example 1, since there was no vinylnaphthalene unit, the dielectric constant and dielectric loss tangent were poor. In Comparative Example 2, vinylcyclohexane was added as a monomer to Comparative Example 1 for copolymerization, but the dielectric constant and dielectric loss tangent did not improve and the glass transition temperature decreased. In Comparative Example 3, isobornyl acrylate was added as a monomer to Comparative Example 1 for copolymerization, and although the glass transition temperature was improved, both the dielectric constant and dielectric loss tangent deteriorated due to the presence of an ester group.

[0116] In contrast, in Example 11, the dielectric constant and dielectric loss tangent were improved and the glass transition temperature was improved by incorporating vinyl naphthalene units compared to Comparative Example 1, and it was possible to achieve both dielectric properties and glass transition temperature. In Example 11, the minimum melt viscosity was also low.

[0117] Examples 1 to 10, 12 to 13 and Comparative Examples 4 to 8 are examples in which the azo-based initiator of the above formula (1) was used. In Comparative Example 4, the divinylbenzene unit was not present, and thermal curing did not proceed. Therefore, test pieces for evaluating the dielectric constant, dielectric tangent, and glass transition temperature could not be prepared, and these items could not be evaluated. In addition, since thermal curing did not proceed, the melt viscosity continued to decrease monotonically, and the minimum melt viscosity could not be observed.

[0118] In Comparative Example 5, the dielectric properties and glass transition temperature were excellent, but the minimum melt viscosity was high and the processability was poor due to the absence of styrene units. In Comparative Example 6, in which styrene, divinylbenzene, and vinylcyclohexane were copolymerized, the dielectric constant and dielectric loss tangent were improved compared to Comparative Example 2 due to the difference in the polymerization initiator, but the glass transition temperature was poor due to the absence of vinylnaphthalene units. In Comparative Example 7, in which isobornyl acrylate was copolymerized with styrene and divinylbenzene, the glass transition temperature was excellent, but the dielectric constant and dielectric loss tangent were poor due to the presence of ester groups.

[0119] Comparative Example 8 was a mixture of Copolymer T and Polymer U, and contained styrene units, divinylbenzene units, and vinylnaphthalene units as a composition. However, it had a poor glass transition temperature, a high minimum melt viscosity, and poor processability.

[0120] In contrast, in Examples 1 to 10, 12 to 13, styrene, divinylbenzene, and vinylnaphthalene were copolymerized, and thus the dielectric constant and dielectric loss tangent were excellent, and the glass transition temperature was maintained or improved compared to Comparative Example 1, and both the dielectric properties and the glass transition temperature were achieved. The minimum melt viscosity was also low. Furthermore, in Examples 1 to 10, 12 to 13, due to the difference in the polymerization initiator, the dielectric constant and dielectric loss tangent were superior to those of Example 11.

[0121] Furthermore, the products of Examples 1 to 13 were excellent in moldability, being capable of being molded into sheets sufficient to stand on their own without the use of a thermoplastic resin or a crosslinking agent.

[0122] In addition, the various numerical ranges described in the specification can be arbitrarily combined with their upper and lower limits, and all such combinations are considered to be preferred numerical ranges described in the specification. In addition, a numerical range described as "X to Y" means from X to Y.

[0123] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.

Claims

1. A thermosetting resin that is a linear copolymer having a repeating unit corresponding to a monovinyl monocyclic aromatic compound, a repeating unit corresponding to a divinyl aromatic compound, and a repeating unit corresponding to a monovinyl polycyclic aromatic compound.

2. 2. The thermosetting resin according to claim 1, wherein the content of the repeating unit corresponding to the monovinyl polycyclic aromatic compound is 20 to 80 mol % in 100 mol % of all repeating units.

3. The linear copolymer has a terminal end having the general formula (1): R 1 -N=N-R 2 In the general formula (1), R 1 and R 2 The thermosetting resin according to claim 1 , wherein each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group.

4. 2. The thermosetting resin according to claim 1, wherein the total content of the repeating units corresponding to the monovinyl monocyclic aromatic compound, the repeating units corresponding to the divinyl aromatic compound, and the repeating units corresponding to the monovinyl polycyclic aromatic compound is 80 mol % or more in 100 mol % of all repeating units.

5. The thermosetting resin according to claim 1 , wherein the monovinyl polycyclic aromatic compound has 3 or less rings.

6. A cured product obtained by curing the thermosetting resin according to any one of claims 1 to 5.

7. A thermosetting composition comprising the thermosetting resin according to any one of claims 1 to 5.

8. The thermosetting composition of claim 7 which is a printed circuit board material.

Citation Information

Patent Citations

  • Curable resin composition

    JP2004131638A

  • Curable resin composition

    JP2006274169A

  • Curable resin composition, cured product and optical article

    JP2013133375A

  • Thermosetting resins and their cured products

    JP7017662B1

  • Thermosetting resin and cured object obtained therefrom

    WO2022065269A1

Cited By

  • Resin composition and method for producing the same

    JP2024173576A

  • Resin composition and method for producing same