Semiconductor device and method for manufacturing semiconductor device
The semiconductor device employs a silicon carbide layer with strategically designed n-type impurity concentration gradients to minimize gate-drain capacitance and on-resistance, ensuring high-speed operation and improved reliability by avoiding reactor contamination and crystallinity issues.
Patent Information
- Application Number
- JP2023049514
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing semiconductor devices, particularly trench-gate MOSFETs, face challenges in achieving high-speed operation due to increased gate-drain capacitance when the n-type impurity concentration in the drift region is too high, which can reduce operating speed.
The semiconductor device incorporates a silicon carbide layer with specific regions of varying n-type impurity concentrations, including a second region with a lower n-type impurity concentration closer to the gate electrode to reduce gate-drain capacitance, and a current diffusion layer to enhance carrier spreading, thereby reducing on-resistance and maintaining high-speed operation.
The solution effectively reduces gate-drain capacitance and on-resistance, enabling faster operation of the MOSFET while preventing reactor contamination and crystallinity deterioration, thus enhancing device performance and reliability.
Smart Images

Figure 2024138816000001_ABST
Abstract
Description
[Technical field]
[0001] FIELD An embodiment of the present invention relates to a semiconductor device and a method for manufacturing a semiconductor device. [Background technology]
[0002] Silicon carbide (SiC) is a material used in semiconductor devices. Compared to silicon, silicon carbide has excellent physical properties, such as a band gap approximately three times larger, a breakdown electric field strength approximately ten times larger, and a thermal conductivity approximately three times larger. By utilizing these characteristics, it is possible to realize, for example, MOSFETs (Metal Oxide Semiconductor Field Effect Transistors) that have high breakdown voltage, low loss, and can operate at high temperatures.
[0003] Trench-gate MOSFETs, in which the gate electrode is formed inside a trench, achieve low on-resistance. The trench-gate type increases the channel area per unit area, reducing the on-resistance.
[0004] It is expected that the operation speed of trench-gate MOSFETs will be increased and the transistor characteristics will be improved. In order to achieve the increase in the speed of trench-gate MOSFETs, for example, it is conceivable to reduce the gate-drain capacitance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-4010 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a semiconductor device and a method for manufacturing the same that can realize high-speed operation. [Means for solving the problem]
[0007] A semiconductor device according to an embodiment includes a first electrode, a second electrode, and a silicon carbide layer provided between the first electrode and the second electrode, the first silicon carbide region including a first region, a second region provided between the first region and the first electrode and having a first conductivity type impurity concentration higher than a first conductivity type impurity concentration of the first region, and a third region provided between the second region and the first electrode, a second silicon carbide region of a second conductivity type provided between the first silicon carbide region and the first electrode, a third silicon carbide region of the first conductivity type provided between the second silicon carbide region and the first electrode, and a fourth silicon carbide region of the second conductivity type provided between the first region and the second region. a gate electrode provided in the silicon carbide layer and facing the first silicon carbide region, the second silicon carbide region, the third silicon carbide region, and the fourth silicon carbide region, and a gate insulating layer provided between the first silicon carbide region and the gate electrode, between the second silicon carbide region and the gate electrode, between the third silicon carbide region and the gate electrode, and between the fourth silicon carbide region and the gate electrode, wherein the second region has a first portion and a second portion, the second portion is provided between the first portion and the gate insulating layer and between the fourth silicon carbide region and the third region, and a first conductivity type impurity concentration of the second portion is lower than a first conductivity type impurity concentration of the first portion. [Brief description of the drawings]
[0008] [Figure 1] 1 is a schematic diagram of a semiconductor device according to an embodiment; [Diagram 2] 1 is a schematic diagram of a semiconductor device according to an embodiment; [Diagram 3] 3A to 3C are explanatory diagrams of a manufacturing method of a semiconductor device according to an embodiment. [Figure 4] 3A to 3C are explanatory diagrams of a manufacturing method of a semiconductor device according to an embodiment. [Diagram 5] 3A to 3C are explanatory diagrams of a manufacturing method of a semiconductor device according to an embodiment. [Figure 6] 3A to 3C are explanatory diagrams of a manufacturing method of a semiconductor device according to an embodiment. [Figure 7] 3A to 3C are explanatory diagrams of a manufacturing method of a semiconductor device according to an embodiment. [Figure 8] 3A to 3C are explanatory diagrams of a manufacturing method of a semiconductor device according to an embodiment. [Figure 9] 3A to 3C are explanatory diagrams of a manufacturing method of a semiconductor device according to an embodiment. [Figure 10] 3A to 3C are explanatory diagrams of a manufacturing method of a semiconductor device according to an embodiment. [Figure 11] 3A to 3C are explanatory diagrams of a manufacturing method of a semiconductor device according to an embodiment. [Figure 12] FIG. 13 is a schematic diagram of a semiconductor device according to a modified example of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description, the same reference numerals will be used to designate the same or similar components, and the description of components that have already been described may be omitted as appropriate.
[0010] In the following description, n + , n, n - And, p + , p, p - The notation indicates the relative level of impurity concentration in each conductivity type. + has a relatively higher n-type impurity concentration than n, - indicates that the n-type impurity concentration is relatively lower than that of n. + has a relatively higher p-type impurity concentration than p, - indicates that the p-type impurity concentration is relatively lower than that of p. + shape, n - Simply put, n-type and p-type + shape, p - The shape is sometimes simply described as p-shape.
[0011] The impurity concentration can be measured by, for example, Secondary Ion Mass Spectrometry (SIMS). The relative level of the impurity concentration can also be determined from the level of the carrier concentration obtained by, for example, Scanning Capacitance Microscopy (SCM). The distances such as the width and depth of the impurity region can be obtained by, for example, SIMS. The distances such as the width and depth of the impurity region can also be obtained from, for example, an image of an SCM or an image of a Scanning Electron Microscope (SEM).
[0012] Furthermore, the thickness of materials constituting a semiconductor device, the distance between materials, and the like can be measured on images obtained by, for example, SIMS, SEM, or a Transmission Electron Microscope (TEM).
[0013] In this specification, the "p-type impurity concentration" of a p-type silicon carbide region means a net p-type impurity concentration obtained by subtracting the n-type impurity concentration of the region from the p-type impurity concentration of the region. Also, the "n-type impurity concentration" of an n-type silicon carbide region means a net n-type impurity concentration obtained by subtracting the p-type impurity concentration of the region from the n-type impurity concentration of the region.
[0014] Furthermore, unless otherwise specified in the specification, the impurity concentration in a particular region means the maximum impurity concentration in that region.
[0015] The semiconductor device according to the embodiment includes a first electrode, a second electrode, and a silicon carbide layer provided between the first electrode and the second electrode, the first silicon carbide region including a first region, a second region provided between the first region and the first electrode and having a first conductivity type impurity concentration higher than a first conductivity type impurity concentration of the first region, and a third region provided between the second region and the first electrode, a second silicon carbide region of a second conductivity type provided between the first silicon carbide region and the first electrode, and a third region provided between the second region and the first electrode. the gate insulating layer is provided between the first portion and the gate insulating layer, and between the fourth silicon carbide region and the third region, and a first conductivity type impurity concentration of the second portion is lower than a first conductivity type impurity concentration of the first portion.
[0016] Fig. 1 and Fig. 2 are schematic diagrams of a semiconductor device according to an embodiment. Fig. 1 is a schematic cross-sectional view of a portion of the semiconductor device according to an embodiment. Fig. 2 is a top view of the semiconductor device according to an embodiment. Fig. 2 shows the surface of a silicon carbide layer. Fig. 1 is a cross-section taken along line AA' in Fig. 2.
[0017] The semiconductor device of the embodiment is a vertical MOSFET 100 using silicon carbide. The MOSFET 100 is a trench-gate MOSFET in which a gate electrode is formed in a trench.
[0018] In the following, an example will be described in which the first conductivity type is n-type and the second conductivity type is p-type. The MOSFET 100 is an n-channel MOSFET that uses electrons as carriers.
[0019] The MOSFET 100 includes a silicon carbide layer 10, a source electrode 12, a drain electrode 14, a gate insulating layer 16, a gate electrode 18, and an interlayer insulating layer 20. The source electrode 12 is an example of a first electrode. The drain electrode 14 is an example of a second electrode.
[0020] At least a portion of the silicon carbide layer 10 is provided between the source electrode 12 and the drain electrode 14. The silicon carbide layer 10 is single crystal SiC. The silicon carbide layer 10 is, for example, 4H—SiC. The silicon carbide layer 10 has a thickness of, for example, 5 μm or more and 150 μm or less.
[0021] Silicon carbide layer 10 has a first surface ("F1" in FIG. 1) and a second surface ("F2" in FIG. 1). Hereinafter, the first surface F1 may be referred to as the front surface, and the second surface F2 may be referred to as the back surface. Note that, hereinafter, "depth" refers to the depth based on the first surface F1.
[0022] Hereinafter, the first direction and the second direction are parallel to the first face F1. The second direction is perpendicular to the first direction. The third direction is perpendicular to the first face F1. The third direction is perpendicular to the first direction and the second direction.
[0023] The first face F1 is the face of the silicon carbide layer 10 on the source electrode 12 side. The second face F2 is the face of the silicon carbide layer 10 on the drain electrode 14 side.
[0024] The first face F1 is, for example, a face inclined from 0 to 8 degrees with respect to the (0001) face. The second face F2 is, for example, a face inclined from 0 to 8 degrees with respect to the (000-1) face. The (0001) face is called a silicon face. The (000-1) face is called a carbon face.
[0025] The silicon carbide layer 10 is + a drain region 22 of n-type, a drift region 24 of p-type, a body region 26 of p-type, + Shaped source region 28, p + The field relief region 30 includes a trench 40 .
[0026] The drift region 24 is an example of a first silicon carbide region. The body region 26 is an example of a second silicon carbide region. The source region 28 is an example of a third silicon carbide region. The electric field relaxation region 30 is an example of a fourth silicon carbide region.
[0027] n + The drain region 22 is provided on the back surface side of the silicon carbide layer 10. The drain region 22 contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the drain region 22 is, for example, 1×10 18 cm -3 More than 1×10 21 cm -3 The following is the result.
[0028] The n-type drift region 24 is provided between the drain region 22 and the source electrode 12. The drift region 24 is provided between the drain region 22 and the first face F1. The drift region 24 is provided on the drain region 22. The drift region 24 contacts the drain region 22, for example.
[0029] The drift region 24 is - A first region 24a of n-type, a second region 24b of n-type, and - The third region 24c has a shape similar to that of the first region 24a.
[0030] n - The first region 24a having a shape similar to that of the first region 24a is provided between the drain region 22 and the source electrode 12. The first region 24a is provided between the drain region 22 and the first face F1. The first region 24a contacts the drain region 22.
[0031] The first region 24a is, for example, an epitaxially grown layer formed on the drain region 22 by using an epitaxial growth method.
[0032] The first region 24a contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the first region 24a is lower than the n-type impurity concentration of the drain region 22. The n-type impurity concentration of the first region 24a is, for example, 5×10 14cm -3 5×10 or more 16 cm -3 The following is the result.
[0033] The thickness of the first region 24a in the third direction is, for example, not less than 3 μm and not more than 150 μm.
[0034] The second region 24b is provided between the first region 24a and the source electrode 12. The second region 24b is provided between the first region 24a and the first face F1. The second region 24b contacts the first region 24a.
[0035] The second region 24b is, for example, an epitaxially grown layer formed on the first region 24a by using an epitaxial growth method.
[0036] The second region 24b contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the second region 24b is higher than the n-type impurity concentration of the first region 24a. The n-type impurity concentration of the second region 24b is, for example, 1×10 16 cm -3 More than 1×10 18 cm -3 The following is the result.
[0037] The thickness of the second region 24b in the third direction is thinner than the thickness of the first region 24a in the third direction. The thickness of the second region 24b in the third direction is, for example, not less than 0.1 μm and not more than 0.5 μm.
[0038] The second region 24b includes a first portion 24bx and a second portion 24by. The second portion 24by is provided between the first portion 24bx and the gate insulating layer 16 in the second direction. The second portion 24by is provided between the first portion 24bx and the trench 40 in the second direction. In addition, the second portion 24by is p + The second region 24c is provided between the first region 24a and the second region 24b.
[0039] The first portion 24bx is located between the first region 24a and the third region 24c in the third direction. The first portion 24bx, for example, contacts the first region 24a and the third region 24c.
[0040] The n-type impurity concentration of the second portion 24by is lower than the n-type impurity concentration of the first portion 24bx. The n-type impurity concentration of the second portion 24by is, for example, half or less of the n-type impurity concentration of the first portion 24bx.
[0041] The n-type impurity concentration of the second portion 24by increases, for example, from the electric field buffer region 30 toward the third region 24c.
[0042] The second portion 24by includes aluminum. The first portion 24bx includes or does not include aluminum. The concentration of aluminum included in the second portion 24by is higher than the concentration of aluminum included in the first portion 24bx, for example.
[0043] The concentration of aluminum contained in the second portion 24by decreases, for example, from the electric field buffer region 30 toward the third region 24c.
[0044] The third region 24c is provided between the second region 24b and the source electrode 12. The third region 24c is provided between the second region 24b and the first face F1. The third region 24c contacts the second region 24b.
[0045] The third region 24c is, for example, an epitaxially grown layer formed on the second region 24b by using an epitaxial growth method.
[0046] The third region 24c contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the third region 24c is, for example, lower than the n-type impurity concentration of the second region 24b. The n-type impurity concentration of the third region 24c is, for example, 1×10 15 cm -3 More than 1×10 18 cm -3 The following is the result.
[0047] The thickness of the third region 24c in the third direction is smaller than the thickness of the first region 24a in the third direction. The thickness of the third region 24c in the third direction is, for example, not less than 0.1 μm and not more than 0.5 μm.
[0048] The p-type body region 26 is provided between the drift region 24 and the source electrode 12. The body region 26 is provided between the drift region 24 and the first face F1. The body region 26 extends in a first direction, for example, as shown in FIG. 2. The body region 26 functions as a channel region of the MOSFET 100.
[0049] The body region 26 contains, for example, aluminum (Al) as a p-type impurity. The p-type impurity concentration of the body region 26 is, for example, 5×10 16 cm -3 5×10 or more 18 cm -3 The following is the result.
[0050] The depth of the body region 26 is, for example, not less than 0.5 μm and not more than 2 μm.
[0051] n + A source region 28 having a shape similar to that of the first face F1 is provided between the body region 26 and the source electrode 12. The source region 28 is provided between the body region 26 and the first face F1. The source region 28 extends in a first direction, for example, as shown in FIG.
[0052] The source region 28 contains, for example, phosphorus (P) as an n-type impurity. The n-type impurity concentration of the source region 28 is higher than the n-type impurity concentration of the drift region 24. The n-type impurity concentration of the source region 28 is, for example, 1×10 19 cm -3 5×10 or more 21 cm -3 The following is the result.
[0053] The depth of the source region 28 is shallower than the depth of the body region 26. The depth of the source region 28 is, for example, not less than 0.1 μm and not more than 0.5 μm.
[0054] p + A field relief region 30 having a shape similar to that of the drift region 24 is provided in the drift region 24. The field relief region 30 is sandwiched between one portion of the drift region 24 and another portion of the drift region 24 in the second direction.
[0055] The electric field relaxation region 30 is provided between the first region 24a and the second region 24b. The electric field relaxation region 30 is provided between the drift region 24 and the trench 40. The electric field relaxation region 30 is provided at the bottom of the trench 40.
[0056] The width of the electric field relief region 30 in the second direction is, for example, larger than the width of the trench 40 in the second direction.
[0057] The electric field relaxation region 30 has a function of relaxing the electric field applied to the gate insulating layer 16 at the bottom of the trench 40 when the MOSFET 100 is in an off state.
[0058] The electric field buffer region 30 contains, for example, aluminum (Al) as a p-type impurity. The p-type impurity concentration of the electric field buffer region 30 is, for example, higher than the p-type impurity concentration of the body region 26. The p-type impurity concentration of the electric field buffer region 30 is, for example, 5×10 17 cm -3 5×10 or more 19 cm -3 The following is the result.
[0059] The trench 40 is provided on the first face F1 side of the silicon carbide layer 10. The trench 40 is a recessed portion provided in the silicon carbide layer 10. The depth of the trench 40 is, for example, not less than 1 μm and not more than 3 μm. Note that in the MOSFET 100, a plurality of trenches 40 (not shown) are repeatedly arranged in the second direction.
[0060] The gate electrode 18 is provided in the silicon carbide layer 10. The gate electrode 18 is provided in the trench 40. The gate electrode 18 faces the drift region 24, the body region 26, the source region 28, and the electric field relief region 30.
[0061] 2, the gate electrode 18 extends, for example, in a first direction. In the MOSFET 100, a plurality of gate electrodes 18 (not shown) are repeatedly arranged in a second direction.
[0062] The gate electrode 18 is, for example, polycrystalline silicon containing p-type or n-type impurities.
[0063] The gate insulating layer 16 is provided in the silicon carbide layer 10. The gate insulating layer 16 is provided in the trench 40. The gate insulating layer 16 is provided between the gate electrode 18 and the drift region 24, between the gate electrode 18 and the body region 26, between the gate electrode 18 and the source region 28, and between the gate electrode 18 and the electric field relaxation region 30.
[0064] The gate insulating layer 16 contacts the drift region 24. The gate insulating layer 16 contacts the second region 24b and the third region 24c. The gate insulating layer 16 contacts the body region 26, the source region 28, and the electric field reduction region 30.
[0065] The gate insulating layer 16 is, for example, silicon oxide.
[0066] The interlayer insulating layer 20 is provided between the gate electrode 18 and the source electrode 12. The interlayer insulating layer 20 electrically separates the gate electrode 18 from the source electrode 12. The interlayer insulating layer 20 is, for example, silicon oxide.
[0067] The source electrode 12 is provided on the first face F1 side of the silicon carbide layer 10. The source electrode 12 is in contact with the source region . The source electrode 12 is in contact with the body region .
[0068] The drain electrode 14 is provided on the second face F2 side of the silicon carbide layer 10. The drain electrode 14 is in contact with the drain region 22.
[0069] Next, an example of a method for manufacturing the semiconductor device of the embodiment will be described. The example of the method for manufacturing the semiconductor device of the embodiment includes forming a second silicon carbide layer of a first conductivity type having a higher first conductivity type impurity concentration than the first conductivity type impurity concentration of the first silicon carbide layer by epitaxial growth on a first silicon carbide layer of a first conductivity type, ion-implanting a second conductivity type impurity into the first silicon carbide layer under conditions that the surface of the second silicon carbide layer does not become the second conductivity type, forming a first region of the second conductivity type in the first silicon carbide layer, and epitaxially growing the second silicon carbide layer on the second silicon carbide layer. A third silicon carbide layer of a first conductivity type is formed using a Sharper growth method, a second conductivity type impurity is ion-implanted into the third silicon carbide layer, a second region of the second conductivity type is formed in the third silicon carbide layer, a first conductivity type impurity is ion-implanted into the second region, a third region of the first conductivity type is formed in the second region, a trench is formed penetrating the third region and the second region to reach the first region, a gate insulating layer is formed in the trench, and a gate electrode is formed on the gate insulating layer.
[0070] Figures 3, 4, 5, 6, 7, 8, 9, 10, and 11 are explanatory diagrams of a method for manufacturing a semiconductor device according to an embodiment. Figures 3 to 11 are schematic cross-sectional views during the manufacturing method of a semiconductor device according to an embodiment. Figures 3 to 11 show cross sections corresponding to Figure 1.
[0071] First n + On the substrate layer 51 having a shape of n - A first silicon carbide layer 52 having a shape similar to that of the first region 24a of the drift region 24 is formed (FIG. 3). The substrate layer 51 is, for example, a silicon carbide wafer. The first silicon carbide layer 52 is formed on the substrate layer 51 by, for example, an epitaxial growth method. The first silicon carbide layer 52 is an epitaxially grown layer. The first silicon carbide layer 52 will eventually become the first region 24a of the drift region 24.
[0072] Next, an n-type second silicon carbide layer 53 is formed on the first silicon carbide layer 52 (FIG. 4). The second silicon carbide layer 53 is formed on the first silicon carbide layer 52 by epitaxial growth. The second silicon carbide layer 53 is an epitaxially grown layer. The n-type impurity concentration of the second silicon carbide layer 53 is higher than the n-type impurity concentration of the first silicon carbide layer 52.
[0073] For example, the first silicon carbide layer 52 and the second silicon carbide layer 53 are successively formed in a reaction chamber of an epitaxial growth apparatus.
[0074] The second silicon carbide layer 53 eventually becomes the second region 24b of the drift region 24.
[0075] Next, a first mask material 54 is formed on the second silicon carbide layer 53. The first mask material 54 is formed, for example, by depositing a film using a chemical vapor deposition method (CVD method), and patterning the film using a photolithography method and a reactive ion etching method (RIE method). The first mask material 54 is, for example, silicon oxide.
[0076] Next, using the first mask material 54 as a mask, aluminum (Al) is ion-implanted into the first silicon carbide layer 52 to form p + A first SiC region 55 of the mold is formed (FIG. 5). The first SiC region 55 is an example of a first region.
[0077] When aluminum ions are implanted, the ions are implanted under conditions that do not cause the surface of second silicon carbide layer 53 to become p-type. By appropriately setting the dose and acceleration energy of the aluminum ion implantation, the surface of second silicon carbide layer 53 is prevented from changing from n-type to p-type.
[0078] It should be noted that aluminum is also contained in second silicon carbide layer 53 on first SiC region 55 due to the aluminum ion implantation. The concentration of aluminum contained in second silicon carbide layer 53 decreases toward the surface of second silicon carbide layer 53.
[0079] The first SiC region 55 ultimately becomes the electric field relief region 30 .
[0080] Next, the first mask material 54 is removed (FIG. 6). The first mask material 54 is removed by using, for example, a wet etching method.
[0081] Next, on the second silicon carbide layer 53, - A third silicon carbide layer 56 having a n-type impurity concentration is formed on the second silicon carbide layer 53 (FIG. 7). The third silicon carbide layer 56 is formed on the second silicon carbide layer 53 by epitaxial growth. The third silicon carbide layer 56 is an epitaxially grown layer. The n-type impurity concentration of the third silicon carbide layer 56 is, for example, lower than the n-type impurity concentration of the second silicon carbide layer 53.
[0082] A hydrogen etching process is performed before forming the third silicon carbide layer 56. The hydrogen etching process is performed in a reaction furnace of an epitaxial growth apparatus in which the third silicon carbide layer 56 is formed.
[0083] The hydrogen etching process is performed in an atmosphere containing hydrogen. The temperature of the hydrogen etching process is, for example, 1500° C. or more and 1650° C. or less. The hydrogen etching process is a process for cleaning the surface of the second silicon carbide layer 53. By the hydrogen etching process, for example, a native oxide film on the surface of the second silicon carbide layer 53 is removed.
[0084] Following the hydrogen etching treatment, a third silicon carbide layer 56 is formed on the second silicon carbide layer 53. The heat treatment temperature when forming the third silicon carbide layer 56 is, for example, 1500° C. or higher and 1650° C. or lower.
[0085] The third silicon carbide layer 56 will eventually become the third region 24c of the drift region 24, the body region 26, and the source region 28.
[0086] It should be noted that activation annealing for activating aluminum ion-implanted in first SiC region 55 is not performed before forming third silicon carbide layer 56. The activation of aluminum ion-implanted in first SiC region 55 is substituted by a hydrogen etching treatment or a heat treatment accompanying the formation of third silicon carbide layer 56. In other words, the activation annealing step is omitted.
[0087] Next, aluminum (Al) is ion-implanted into the third silicon carbide layer 56 to form a p-type second SiC region 57 in the third silicon carbide layer 56 (FIG. 8). The second SiC region 57 is an example of a second region. The second SiC region 57 will eventually become the p-type body region 26.
[0088] Next, a second mask material 58 is formed on the second SiC region 57. The second mask material 58 is formed by, for example, depositing a film using a CVD method, and patterning the film using a photolithography method and an RIE method. The second mask material 58 is, for example, silicon oxide.
[0089] Next, using the second mask material 58 as a mask, phosphorus (P) is ion-implanted into the second SiC region 57 to form n-type ions in the second SiC region 57. + A third SiC region 59 of a mold is formed (FIG. 9). The third SiC region 59 is an example of a third region. The third SiC region 59 will eventually become the source region 28.
[0090] Next, the second mask material 58 is removed. Next, a third mask material 60 is formed on the second SiC region 57 and the third SiC region 59. The third mask material 60 is formed, for example, by depositing a film using a CVD method, and patterning the film using a photolithography method and an RIE method. The third mask material 60 is, for example, silicon oxide.
[0091] Next, using the third mask material 60 as a mask, a trench 40 is formed that penetrates the third SiC region 59 and the second SiC region 57 and reaches the first SiC region 55 (FIG. 10). The trench 40 is formed by using, for example, the RIE method.
[0092] Next, the third mask material 60 is removed. Next, using a known process technology, the gate insulating layer 16 is formed in the trench 40, and the gate electrode 18 is formed on the gate insulating layer 16 (FIG. 11).
[0093] Thereafter, the source electrode 12 and the drain electrode 14 are formed using known process techniques.
[0094] By the above manufacturing method, the MOSFET 100 shown in FIGS. 1 and 2 is formed.
[0095] Next, the functions and effects of the semiconductor device and the method for manufacturing the semiconductor device according to the embodiment will be described.
[0096] Trench-gate MOSFETs, in which the gate electrode is formed inside a trench, achieve low on-resistance. The trench-gate type increases the channel area per unit area, reducing the on-resistance.
[0097] The MOSFET 100 of the embodiment is a trench gate type MOSFET. + A second region 24b having an n-type impurity concentration higher than the n-type impurity concentration of the first region 24a is provided between the p-type body region 26 and the electric field relaxation region 30 and between the p-type body region 26 and the first region 24a of the drift region 24.
[0098] In the MOSFET 100, the second region 24b having a high n-type impurity concentration functions as a current spreading layer, thereby further reducing the on-resistance. That is, when the MOSFET 100 is turned on, carriers flow from the source region 28 to the drift region 24 through a channel region formed in the body region 26 near the side surface of the trench 40. The carriers that flow into the drift region 24 are diffused laterally (the second direction in FIG. 1) along the low-resistance second region 24b. Therefore, the path through which the carriers flow is widened in the drift region 24, and the on-resistance of the MOSFET 100 is reduced.
[0099] On the other hand, if the n-type impurity concentration in the drift region 24 facing the gate electrode 18 becomes too high, the gate-drain capacitance increases, and the operating speed of the MOSFET 100 may decrease.
[0100] In the MOSFET 100 of the embodiment, the second region 24b functioning as a current spreading layer includes a first portion 24bx and a second portion 24by that is closer to the gate electrode 18 than the first portion 24bx. The n-type impurity concentration of the second portion 24by is lower than the n-type impurity concentration of the first portion 24bx. The n-type impurity concentration of the drift region 24 facing the gate electrode 18 is partially lowered, thereby reducing the gate-drain capacitance of the MOSFET 100. This prevents a decrease in the operating speed of the MOSFET 100, and enables the MOSFET 100 to operate at a higher speed.
[0101] From the viewpoint of reducing the gate-drain capacitance, the n-type impurity concentration of the second portion 24by is preferably equal to or less than half the n-type impurity concentration of the first portion 24bx, more preferably equal to or less than one-fifth, and even more preferably equal to or less than one-tenth.
[0102] For example, when a silicon carbide layer is formed by epitaxial growth on a p-type silicon carbide layer having a high concentration of aluminum on its surface, the reactor of the epitaxial growth apparatus is contaminated with aluminum. The aluminum contamination occurs when the surface of the p-type silicon carbide layer is etched during a hydrogen etching process performed prior to the formation of the silicon carbide layer.
[0103] If the reactor of an epitaxial growth apparatus is contaminated with aluminum, particularly when forming a low-concentration n-type silicon carbide layer, the aluminum, which is a p-type impurity, becomes mixed in, making it difficult to control the n-type impurity concentration.
[0104] Furthermore, when a silicon carbide layer is formed by epitaxial growth on a silicon carbide layer having a p-type region formed on its surface by high-dose aluminum ion implantation, the crystallinity of the silicon carbide layer deteriorates, presumably because of the high density of defects caused by the ion implantation in the p-type region.
[0105] Deterioration of the crystallinity of the silicon carbide layer may cause deterioration of the characteristics of the MOSFET, such as an increase in junction leakage.
[0106] In the method for manufacturing a semiconductor device according to the embodiment, + In order to form the electric field relaxation region 30 having a shape like a silicon carbide layer, p + A first SiC region 55 having a p-type impurity is formed. Before performing aluminum ion implantation to form the first SiC region 55, the surface of the first silicon carbide layer 52 is covered with a second silicon carbide layer 53 having a higher n-type impurity concentration than the first silicon carbide layer 52. Then, ion implantation is performed under conditions that the surface of the second silicon carbide layer 53 does not become p-type. Thereafter, a third silicon carbide layer 56 is formed on the second silicon carbide layer 53 by epitaxial growth.
[0107] In the method for manufacturing a semiconductor device according to the embodiment, the surface of the second silicon carbide layer 53 is n-type, which prevents the reactor of the epitaxial growth apparatus from being contaminated with aluminum, thereby facilitating control of the n-type impurity concentration of the silicon carbide layer by the epitaxial growth apparatus.
[0108] Furthermore, in the method for manufacturing a semiconductor device according to the embodiment, the surface of the second silicon carbide layer 53 is n-type, and no p-type region formed by high-dose aluminum ion implantation is present. This suppresses deterioration of the crystallinity of the third silicon carbide layer 56 formed on the second silicon carbide layer 53. This suppresses deterioration of the characteristics of the MOSFET 100.
[0109] Furthermore, in the method for manufacturing a semiconductor device according to the embodiment, before the third silicon carbide layer 56 is formed, + It is possible to omit the activation annealing step of the first SiC region 55 of the mold.
[0110] Consider a case where a silicon carbide layer is formed by epitaxial growth on a silicon carbide layer having a p-type region formed by high-dose aluminum ion implantation, without performing the activation annealing process. In this case, for example, when the temperature is raised during the hydrogen etching process, the wafer may deform, and may fly off the wafer holder in the epitaxial growth apparatus. The wafer deformation is considered to be due to ion implantation damage to the p-type region exposed on the wafer surface.
[0111] In the method for manufacturing a semiconductor device according to the embodiment, the surface of the second silicon carbide layer 53 is n-type, and the p-type region formed by high-dose aluminum ion implantation is not exposed on the surface. Therefore, deformation of the wafer and occurrence of wafer flying during the temperature rise in the hydrogen etching process are suppressed. + It is possible to omit the activation annealing step of the first SiC region 55 of the mold.
[0112] (Modification) The semiconductor device of the modified embodiment differs from the semiconductor device of the embodiment in that the first conductivity type impurity concentration in the third region is higher than the first conductivity type impurity concentration in the second region. Also, the manufacturing method of the semiconductor device of the modified embodiment differs from the manufacturing method of the semiconductor device of the embodiment in that the first conductivity type impurity concentration in the third silicon carbide layer is higher than the first conductivity type impurity concentration in the second silicon carbide layer.
[0113] Fig. 12 is a schematic diagram of a semiconductor device according to a modified example of the embodiment, Fig. 12 is a schematic cross-sectional view of a part of a semiconductor device according to a modified example of the embodiment, Fig. 12 is a diagram corresponding to Fig. 1 of the embodiment.
[0114] The semiconductor device according to the modified embodiment is a vertical MOSFET 101 using silicon carbide. The MOSFET 101 is a trench-gate MOSFET in which a gate electrode is formed in a trench.
[0115] The drift region 24 of the MOSFET 101 is - A first region 24a of n-type, a second region 24b of n-type, and + The third region 24c has a shape similar to that of the first region 24a.
[0116] The third region 24c contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the third region 24c is, for example, higher than the n-type impurity concentration of the second region 24b. The n-type impurity concentration of the third region 24c is, for example, 2×10 16 cm -3 More than 2×10 18 cm -3 The following is the result.
[0117] The MOSFET 101 can be manufactured by the same manufacturing method as the MOSFET 100 of the embodiment. However, the n-type impurity concentration of the third silicon carbide layer 56 is set higher than the n-type impurity concentration of the second silicon carbide layer 53.
[0118] In the MOSFET 101 according to the modified example of the embodiment, the third region 24c having a high concentration of n-type impurities also functions as a current spreading layer, thereby further reducing the on-resistance.
[0119] It is also possible to make the n-type impurity concentration of the third region 24c equal to the n-type impurity concentration of the second region 24b.
[0120] As described above, the semiconductor device and the manufacturing method of the semiconductor device according to the embodiment and the modification can reduce the gate-drain capacitance, thereby realizing high-speed operation of the MOSFET. Furthermore, the manufacturing method of the semiconductor device according to the embodiment and the modification can suppress contamination of the reactor of the epitaxial growth apparatus, suppress deterioration of the characteristics of the MOSFET, and omit the activation annealing step.
[0121] In the embodiment, the case of 4H-SiC as the crystal structure of SiC has been described as an example, but the present invention can also be applied to devices using SiC with other crystal structures such as 6H-SiC, 3C-SiC, etc. Also, it is possible to apply a plane other than the (0001) plane to the surface of silicon carbide layer 10.
[0122] In the embodiment, the first conductivity type is n-type and the second conductivity type is p-type, but it is also possible for the first conductivity type to be p-type and the second conductivity type to be n-type.
[0123] In the embodiment, aluminum (Al) is exemplified as the p-type impurity, but boron (B) can also be used. In addition, nitrogen (N) and phosphorus (P) are exemplified as the n-type impurity, but arsenic (As), antimony (Sb), etc. can also be used.
[0124] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. For example, components of one embodiment may be replaced or changed with components of another embodiment. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0125] 10 Silicon carbide layer 12 source electrode (first electrode) 14 Drain electrode (second electrode) 16 Gate insulating layer 18 gate electrode, 24 Drift region (first silicon carbide region) 24a First Area 24b The second area 24bx Part 1 24by 2nd part 24c The third area 26 Body region (second silicon carbide region) 28 source region (third silicon carbide region) 30 Electric field relaxation region (fourth silicon carbide region) 40 Trench 52 First silicon carbide layer 53 Second silicon carbide layer 55 First SiC region (first region) 56 Third silicon carbide layer 57 Second SiC region (Second region) 59 The third SiC region 100 MOSFET (semiconductor device) F1 First Side F2 Second Face
Claims
1. A first electrode; A second electrode; and A silicon carbide layer provided between the first electrode and the second electrode, a first silicon carbide region of a first conductivity type including: a first region; a second region provided between the first region and the first electrode, the second region having a first conductivity type impurity concentration higher than a first conductivity type impurity concentration of the first region; and a third region provided between the second region and the first electrode; a second silicon carbide region of a second conductivity type provided between the first silicon carbide region and the first electrode; a third silicon carbide region of the first conductivity type provided between the second silicon carbide region and the first electrode; a fourth silicon carbide region of a second conductivity type provided between the first region and the second region; A silicon carbide layer comprising: a gate electrode provided in the silicon carbide layer and facing the first silicon carbide region, the second silicon carbide region, the third silicon carbide region, and the fourth silicon carbide region; gate insulating layers provided between the first silicon carbide region and the gate electrode, between the second silicon carbide region and the gate electrode, between the third silicon carbide region and the gate electrode, and between the fourth silicon carbide region and the gate electrode; Equipped with the second region has a first portion and a second portion; the second portion is provided between the first portion and the gate insulating layer and between the fourth silicon carbide region and the third region; a first conductivity type impurity concentration of the second portion is lower than a first conductivity type impurity concentration of the first portion.
2. 2. The semiconductor device according to claim 1, wherein a concentration of the first conductivity type impurity in said third region is lower than a concentration of the first conductivity type impurity in said second region.
3. 2. The semiconductor device according to claim 1, wherein said first conductivity type is n-type, said second conductivity type is p-type, and a concentration of aluminum contained in said second portion is higher than a concentration of aluminum contained in said first portion.
4. 4. The semiconductor device according to claim 3, wherein a concentration of aluminum contained in said second portion decreases from said fourth silicon carbide region toward said third region.
5. forming a second silicon carbide layer of a first conductivity type, the second silicon carbide layer having a first conductivity type impurity concentration higher than a first conductivity type impurity concentration of the first silicon carbide layer, on the first silicon carbide layer of a first conductivity type by epitaxial growth; ion-implanting a second conductivity type impurity into the first silicon carbide layer under conditions that a surface of the second silicon carbide layer does not become the second conductivity type, thereby forming a first region of the second conductivity type in the first silicon carbide layer; forming a third silicon carbide layer of a first conductivity type on the second silicon carbide layer by epitaxial growth; ion-implanting a second conductivity type impurity into the third silicon carbide layer to form a second region of the second conductivity type in the third silicon carbide layer; ion-implanting a first conductivity type impurity into the second region to form a third region of the first conductivity type in the second region; forming a trench passing through the third region and the second region and reaching the first region; forming a gate insulating layer in the trench; A method for manufacturing a semiconductor device, comprising the steps of: forming a gate electrode on the gate insulating layer.
6. 6. The method for manufacturing a semiconductor device according to claim 5, wherein a concentration of the first conductivity type impurity in said third silicon carbide layer is lower than a concentration of the first conductivity type impurity in said second silicon carbide layer.
Citation Information
Patent Citations
Semiconductor device
JP2015141919A
Silicon carbide semiconductor device
JP2017050516A
Semiconductor device and method of manufacturing the same
JP2018026562A
Semiconductor device and manufacturing method for the same
JP2019004010A