Rubber composition for sliding seal and sliding seal
A rubber composition for sliding seals, combining ethylene/α-olefin/nonconjugated polyene copolymer, carbon black, and modified silicone oil, addresses the issue of friction maintenance in ethylene-based seals by enhancing sliding performance and reducing lubricant bleeding.
Patent Information
- Application Number
- JP2023049671
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional sliding seals made from ethylene-based copolymers like EPDM face issues with maintaining low friction properties over time, particularly due to the bleeding of lubricants which leads to increased friction and poor sliding performance.
A rubber composition comprising a specific ethylene/α-olefin/nonconjugated polyene copolymer, carbon black, and a modified silicone oil with unsaturated carbon-carbon bonds, formulated to maintain low friction properties through a balanced molecular structure and crosslinking process.
The composition forms a sliding seal that maintains excellent low friction properties, ensuring effective sliding performance and resistance to wear, while minimizing lubricant bleeding.
Smart Images

Figure 2024138939000001 
Figure 2024138939000002 
Figure 2024138939000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for a sliding seal and a sliding seal. [Background technology]
[0002] Ethylene-based copolymers such as ethylene-α-olefin-non-conjugated diene copolymers (EPDM) have no unsaturated bonds in the main chain and therefore have superior weather resistance, heat resistance, and ozone resistance compared to general-purpose diene-based rubbers. They are widely used in rubber products such as automotive industrial parts, industrial rubber products, electrical insulation materials, civil engineering and building materials, and rubber-coated fabrics.
[0003] For example, it is known that a rubber molded article for sealing is obtained by using EPDM (see Patent Document 1). Seal packings, which are rubber molded articles for sealing, are used in various applications such as automobiles, industrial machinery, and electronic components. In particular, rubber products with excellent abrasion resistance are required for seal parts used in dynamic environments, and it is widely known that carbon black is blended to enhance reinforcing properties (see Patent Documents 2 and 3).
[0004] In addition, additives that reduce the coefficient of friction are often added to improve wear resistance, and in particular, silicone oil, silicone polymers, and various other organic and inorganic lubricants are used. Silicone oil can greatly improve the sliding properties of the contact body when added, but it is prone to bleeding out onto the surface, and when the contact body moves up and down several or several dozen times, the silicone content on the surface is transferred to and taken away by the contact body surface, resulting in an increase in the dynamic friction coefficient and the risk of causing problems with poor sliding of the contact body. Other lubricants are also prone to bleeding out, causing problems with poor sliding and poor appearance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2000 / 59962 [Patent Document 2] JP 2000-191863 A [Patent Document 3] JP 2012-031342 A Summary of the Invention [Problem to be solved by the invention]
[0006] Conventionally known sliding seals containing EPDM or the like have the problem that they are unable to maintain low friction when used for long periods of time. An object of the present invention is to provide a rubber composition for a sliding seal capable of forming a sliding seal excellent in maintaining low friction, and a sliding seal containing said composition. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that the above problems can be solved by a composition containing a specific ethylene-α-olefin-non-conjugated polyene copolymer, carbon black, and a specific modified silicone oil, and have completed the present invention. Examples of aspects of the present invention are shown below.
[0008] [1] (A) 100 parts by mass of an ethylene-α-olefin-non-conjugated polyene copolymer having a structural unit derived from ethylene (a1), a structural unit derived from an α-olefin (a2) having 3 to 20 carbon atoms, and a structural unit derived from a non-conjugated polyene (a3); (B) 10 to 300 parts by mass of carbon black, and (C) 0.1 to 40 parts by mass of modified silicone oil containing unsaturated carbon-carbon bonds and the copolymer (A) satisfies the following requirements (i) to (v): (i) the molar ratio of ethylene / α-olefin is 40 / 60 to 99.9 / 0.1; (ii) the mass fraction of the structural units derived from the non-conjugated polyene (a3) is 0.07% by mass to 10% by mass in 100% by mass of the copolymer (A); (iii) the weight average molecular weight (Mw) of the copolymer (A), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) (mass fraction (mass %) of (a3)), and the molecular weight of the non-conjugated polyene (a3) (the molecular weight of (a3)) satisfy the following formula (1); 4.5≦Mw×(a3) mass fraction / 100 / (a3) molecular weight≦80 … (1) (iv) Complex viscosity η at frequency ω = 0.1 rad / s obtained by linear viscoelastic measurement (190 °C) using a rheometer * ( ω =0.1) (Pa sec) and the complex viscosity η at frequency ω = 100 rad / s * ( ω =100) (Pa sec) * ( ω =0.1) / η * ( ω =100) ), the intrinsic viscosity [η], and the mass fraction of the structural unit derived from the non-conjugated polyene (a3) (mass fraction of (a3)) satisfy the following formula (2); P / ([η] 2.9 ) ≦ (a3) mass fraction × 6 … (2) (v) Number of long chain branches (LCB) per 1000 carbon atoms obtained using 3D-GPC 1000C ) and the natural logarithm of the weight average molecular weight (Mw) [Ln(Mw)] satisfy the following formula (3). LCB 1000C ≦1-0.07×Ln(Mw) ‥ Equation (3)
[0009] [2] The rubber composition for a sliding seal according to item [1], further comprising 0.1 to 20 parts by mass of an organic peroxide-based crosslinking agent (D). [3] The rubber composition for sliding seals according to item [1] or [2], wherein the modified silicone oil (C) is a methacrylic-modified silicone oil. [4] The modified silicone oil (C) has a kinetic viscosity at 25°C of 30 to 500 mm 2 The rubber composition for a sliding seal according to any one of items [1] to [3], wherein R 1 is 0.01 to 0.15;
[0010] [5] The rubber composition for sliding seals according to any one of items [1] to [4], wherein the non-conjugated polyene (a3) contains, in the molecule, two or more partial structures selected from the group consisting of the following general formulae (I) and (II):
[0011] [ka]
[0012] [6] The rubber composition for a sliding seal according to any one of items [1] to [5], wherein the non-conjugated polyene (a3) contains 5-vinyl-2-norbornene (VNB). [7] The rubber composition for a sliding seal according to any one of items [1] to [6], wherein the α-olefin (a2) is propylene.
[0013] [8] The rubber composition for a sliding seal according to any one of items [1] to [7], further comprising 1 to 100 parts by mass of a softener (E). [9] The rubber composition for a sliding seal according to any one of items [1] to [8], further comprising 0.1 to 20 parts by mass of an antioxidant (F).
[0014]
[10] A crosslinked body of the rubber composition for a sliding seal according to any one of items [1] to [9].
[11] A sliding seal comprising the crosslinked body according to item
[10] . Effect of the Invention
[0015] According to the present invention, it is possible to provide a rubber composition for a sliding seal capable of forming a sliding seal excellent in maintaining low friction, and a sliding seal including said composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described in detail below. [Rubber composition for sliding seals] The rubber composition for sliding seals of the present invention (hereinafter sometimes referred to as "rubber composition of the present invention" or "composition of the present invention") contains an ethylene-α-olefin-non-conjugated polyene copolymer (A) having a structural unit derived from ethylene (a1), a structural unit derived from an α-olefin (a2) having 3 to 20 carbon atoms, and a structural unit derived from a non-conjugated polyene (a3), carbon black (B), and a modified silicone oil (C) containing an unsaturated carbon-carbon bond, and may contain an organic peroxide crosslinking agent (D), a softener (E), an antioxidant (F), and other components, as necessary.
[0017] <Ethylene-α-olefin-non-conjugated polyene copolymer (A)> The copolymer (A) used in the present invention has a structural unit derived from ethylene (a1), a structural unit derived from an α-olefin (a2) having 3 to 20 carbon atoms, and a structural unit derived from a non-conjugated polyene (a3).
[0018] Examples of the α-olefin (a2) include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-eicosene. Among these, α-olefins having 3 to 8 carbon atoms such as propylene, 1-butene, 1-hexene, and 1-octene are preferred, and propylene is particularly preferred. Such α-olefins are preferred because the raw material cost is relatively low, the resulting copolymer (A) exhibits excellent mechanical properties, and a molded product having rubber elasticity can be obtained.
[0019] The α-olefin (a2) may be used alone or in combination of two or more kinds. That is, the copolymer (A) contains structural units derived from at least one α-olefin (a2) having 3 to 20 carbon atoms, and may contain structural units derived from two or more α-olefins (a2) having 3 to 20 carbon atoms.
[0020] The non-conjugated polyene (a3) is not particularly limited as long as it is a compound having two or more non-conjugated unsaturated bonds, and examples thereof include compounds having a total of two or more partial structures selected from the group consisting of the following general formulas (I) and (II) in the molecule.
[0021] [ka]
[0022] Examples of the non-conjugated polyene (a3) include 5-vinyl-2-norbornene (VNB), norbornadiene, 1,4-hexadiene, and dicyclopentadiene. Among these, it is preferable that the non-conjugated polyene (a3) contains VNB, and it is more preferable that the non-conjugated polyene (a3) is VNB, because it is highly available, has good reactivity with peroxide during crosslinking reaction after polymerization, and tends to improve the heat resistance of the polymer composition. The non-conjugated polyene (a3) may be used alone or in combination of two or more kinds.
[0023] The copolymer (A) may have, in addition to the structural units derived from the above (a1), (a2), and (a3), a structural unit derived from a non-conjugated polyene (a4) containing only one partial structure selected from the group consisting of the above general formulas (I) and (II) in the molecule.
[0024] Examples of the non-conjugated polyene (a4) include 5-ethylidene-2-norbornene (ENB), 5-methylene-2-norbornene, 5-(2-propenyl)-2-norbornene, 5-(3-butenyl)-2-norbornene, 5-(1-methyl-2-propenyl)-2-norbornene, 5-(4-pentenyl)-2-norbornene, 5-(1-methyl-3-butenyl)-2-norbornene, 5-(5-hexenyl)-2-norbornene, 5-(1-methyl-4-pentenyl)-2-norbornene, 5-(2,3-dimethyl-3-butenyl)-2-norbornene, 5-(2-ethyl-3-butenyl)-2-norbornene, Examples of such compounds include 5-(1,2-dimethyl-5-hexenyl)-2-norbornene, 5-(6-heptenyl)-2-norbornene, 5-(3-methyl-5-hexenyl)-2-norbornene, 5-(3,4-dimethyl-4-pentenyl)-2-norbornene, 5-(3-ethyl-4-pentenyl)-2-norbornene, 5-(7-octenyl)-2-norbornene, 5-(2-methyl-6-heptenyl)-2-norbornene, 5-(1,2-dimethyl-5-hexenyl)-2-norbornene, 5-(5-ethyl-5-hexenyl)-2-norbornene, and 5-(1,2,3-trimethyl-4-pentenyl)-2-norbornene. Among these, ENB is preferred because it is easily available, has high reactivity with sulfur and vulcanization accelerators during the crosslinking reaction after polymerization, is easy to control the crosslinking rate, and is easy to obtain good mechanical properties. The non-conjugated polyene (a4) may be used alone or in combination of two or more kinds.
[0025] When the copolymer (A) contains a structural unit derived from the non-conjugated polyene (a4), the proportion thereof is not particularly limited as long as the object of the present invention is not impaired. Generally, the mass fraction thereof is about 0 to 20 mass%, preferably 0 to 8 mass%, and more preferably 0.01 to 8 mass% (wherein the sum of the mass fractions of (a1), (a2), (a3), and (a4) is taken as 100 mass%).
[0026] The copolymer (A) may contain a biomass-derived monomer as at least one monomer selected from the above-mentioned ethylene (a1), the α-olefin (a2) having 3 to 20 carbon atoms, the non-conjugated polyene (a3), and the non-conjugated polyene (a4).
[0027] The copolymer (A) satisfies the following requirements (i) to (v). (i) The molar ratio of the structural units derived from ethylene (a1) to the structural units derived from an α-olefin (a2) [(a1) / (a2)] is 40 / 60 to 99.9 / 0.1. (ii) The mass fraction of the structural units derived from the non-conjugated polyene (a3) is from 0.07% by mass to 10% by mass in 100% by mass of the copolymer (A). (iii) The weight average molecular weight (Mw) of the copolymer (A), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) (mass fraction (mass %) of (a3)), and the molecular weight of the non-conjugated polyene (a3) (molecular weight of (a3)) satisfy the following formula (1): 4.5≦Mw×(a3) mass fraction / 100 / (a3) molecular weight≦80 … (1) (iv) Complex viscosity η at frequency ω = 0.1 rad / s obtained by linear viscoelastic measurement (190 °C) using a rheometer * ( ω =0.1) (Pa sec) and the complex viscosity η at frequency ω = 100 rad / s * ( ω =100) (Pa sec) * ( ω =0.1) / η * ( ω =100) ), the intrinsic viscosity [η], and the mass fraction of the structural unit derived from the non-conjugated polyene (a3) (mass fraction of (a3)) satisfy the following formula (2). P / ([η] 2.9 ) ≦ (a3) mass fraction × 6 … (2) (v) Number of long chain branches (LCB) per 1000 carbon atoms obtained using 3D-GPC 1000C) and the natural logarithm of the weight average molecular weight (Mw) [Ln(Mw)] satisfy the following formula (3). LCB 1000C ≦1-0.07×Ln(Mw) ‥ Equation (3)
[0028] ≪Requirement (i)≫ The requirement (i) specifies that the molar ratio of ethylene (a1) / α-olefin (a2) in the copolymer (A) satisfies 40 / 60 to 99.9 / 0.1, and this molar ratio is preferably 50 / 50 to 90 / 10, more preferably 55 / 45 to 85 / 15, and even more preferably 55 / 45 to 78 / 22.
[0029] By using the copolymer (A) that satisfies the requirement (i), an ethylene copolymer composition excellent in rubber elasticity, mechanical strength, and flexibility can be obtained. The amount of ethylene (content of structural units derived from ethylene (a1)) and the amount of α-olefin (content of structural units derived from α-olefin (a2)) in the copolymer (A) are 13 It can be determined by C-NMR.
[0030] Requirement (ii) Requirement (ii) specifies that the mass fraction of the structural units derived from the non-conjugated polyene (a3) is in the range of 0.07% by mass to 10% by mass in 100% by mass of the copolymer (A) (i.e., 100% by mass of the total mass fractions of all structural units). The mass fraction of the structural units derived from the non-conjugated polyene (a3) is preferably 0.1% by mass to 8.0% by mass, more preferably 0.5% by mass to 5.0% by mass.
[0031] The copolymer (A) satisfying the requirement (ii) has sufficient hardness and excellent mechanical properties, and when crosslinked using a peroxide, it exhibits a fast crosslinking rate. The amount of non-conjugated polyene (a3) in the copolymer (A) (the content of the constitutional unit derived from the non-conjugated polyene (a3)) is: 13 It can be determined by C-NMR.
[0032] ≪Requirement (iii)≫ Requirement (iii) specifies that, in the copolymer (A), the weight average molecular weight (Mw) of the copolymer (A), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) in the copolymer (A) (mass fraction of (a3): mass %), and the molecular weight of the non-conjugated polyene (a3) (molecular weight of (a3)) satisfy the above formula (1). The above formula (1) in requirement (iii) is preferably the following formula (1'): 4.5≦Mw×(a3) mass fraction / 100 / (a3) molecular weight≦75 … (1')
[0033] When the copolymer (A) satisfies the requirement (iii), the content of the structural unit derived from the non-conjugated polyene (a3) is appropriate, and an ethylene copolymer composition that exhibits sufficient crosslinking performance, excellent crosslinking rate, and excellent mechanical properties can be produced. The weight average molecular weight (Mw) of the copolymer (A) means a value measured by 3D-GPC.
[0034] In the above copolymer (A), when "Mw×mass fraction (a3) / 100 / molecular weight (a3)" satisfies the above formula (1) or (1'), the degree of crosslinking becomes appropriate, and an ethylene-based copolymer composition having a good balance of mechanical properties and heat aging resistance can be produced. If the value of "Mw×mass fraction (a3) / 100 / molecular weight (a3)" is too low, the crosslinking may be insufficient, resulting in a slow crosslinking rate, and if the value is too high, excessive crosslinking may occur, resulting in deterioration of mechanical properties.
[0035] ≪Requirement (iv)≫ The requirement (iv) is that the complex viscosity η of the copolymer (A) at a frequency ω=0.1 rad / s obtained by linear viscoelasticity measurement (190° C.) using a rheometer * ( ω =0.1) (Pa sec) and the complex viscosity η at frequency ω = 100 rad / s * ( ω =100) (Pa sec) * ( ω =0.1) / η *( ω =100) ), the intrinsic viscosity [η], and the mass fraction of the structural unit derived from the non-conjugated polyene (a3) (mass fraction of (a3): mass %) satisfy the above formula (2). The above formula (2) in requirement (iv) is preferably the following formula (2'). P / ([η] 2.9 ) ≦ (a3) mass fraction × 5.7 … (2')
[0036] Here, the complex viscosity η at frequency ω=0.1rad / s * ( ω =0.1) and the complex viscosity η at frequency ω=100rad / s * ( ω =100) Relative to P(η * ( ω =0.1) / η * ( ω =100) ) represents the frequency dependence of viscosity and is the left side of equation (2), P / ([η] 2.9 ) tends to show a high value when there are many long chain branches, although it is influenced by short chain branches, molecular weight, etc. In general, in an ethylene-α-olefin-non-conjugated polyene copolymer, the more constitutional units derived from non-conjugated polyenes it contains, the more long chain branches it tends to contain. However, it is considered that the copolymer (A) of the present invention can satisfy the above formula (2) because it has fewer long chain branches than the conventionally known ethylene-α-olefin-non-conjugated polyene copolymers.
[0037] In the present invention, the P value is determined by performing measurements using a viscoelasticity measuring device Ares (manufactured by Rheometric Scientific) at 190° C., strain 1.0%, and various frequencies, and is calculated as the ratio (η * The intrinsic viscosity [η] is the value measured in decalin at 135°C.
[0038] ≪Requirement (v)≫ The copolymer (A) was determined by 3D-GPC using the long chain branching (LCB) per 1000 carbon atoms. 1000C ) and the natural logarithm of the weight average molecular weight (Mw) [Ln(Mw)] satisfy the following formula (3), and preferably satisfy the following formula (3'). LCB 1000C ≦1-0.07×Ln(Mw) …(3) LCB 1000C ≦1-0.071×Ln(Mw) …(3') The upper limit of the long chain branch content per unit carbon number of the copolymer (A) is specified by the above formula (3) or (3').
[0039] Such a copolymer (A) has a low proportion of long chain branches and is excellent in curing properties when crosslinked using a peroxide, and can give an ethylene copolymer composition having excellent heat aging resistance.
[0040] Here, the weight average molecular weight (Mw) and the number of long chain branches (LCB) per 1000 carbon atoms 1000C ) can be determined by a structural analysis method using 3D-GPC. Specifically, it is as follows.
[0041] Using a 3D-high temperature GPC device PL-GPC220 (Polymer Laboratories), the weight average molecular weight (Mw) and absolute molecular weight distribution are measured, and at the same time, the intrinsic viscosity is measured using a viscometer. The main measurement conditions are as follows: Detector: Differential refractometer / GPC device built-in 2-angle light scattering photometer PD2040 type (manufactured by Precison Detectors) Bridge type viscometer PL-BV400 (Polymer Laboratories) Column: TSKgel GMH HR -H(S)HT x 2 + TSKgel GMH HR -M(S)×1 piece (Each piece has an inner diameter of 7.8 mm and a length of 300 mm) Temperature: 140℃ Mobile phase: 1,2,4-trichlorobenzene (containing 0.025% BHT) Injection volume: 0.5mL Sample concentration: ca 1.5mg / mL Sample filtration: Filtration through a sintered filter with a pore size of 1.0 μm
[0042] In the above, the dn / dc value required to determine the absolute molecular weight is determined for each sample from the dn / dc value of standard polystyrene (molecular weight 190,000), 0.053, and the response intensity of the differential refractometer per unit injected mass.
[0043] From the relationship between the intrinsic viscosity obtained from the viscometer and the absolute molecular weight obtained from the light scattering photometer, the long chain branching parameter g'i for each eluted component is calculated from the following formula (v-1).
[0044]
number
[0045] Further, the average values of g' are calculated from the following formulas (v-2), (v-3), and (v-4). Note that the trendline assuming the presence of only short chain branches is determined for each sample.
[0046]
number
[0047] Furthermore, using g'w, the number of branching points per molecular chain, BrNo, and the number of long chain branches per 1000 carbon atoms, LCB, 1000C The branching degree λ per unit molecular weight is calculated. BrNo is calculated using the following Zimm-Stockmayer formula (v-5). 1000CThe following formulas (v-6) and (v-7) are used to calculate and λ. g is the long chain branching parameter calculated from the radius of gyration Rg, and the following simple correlation is made between g' calculated from the intrinsic viscosity. Various values have been proposed for ε in the formula depending on the shape of the molecule. Here, calculations are performed assuming ε=1 (i.e. g'=g).
[0048]
number
[0049] The intrinsic viscosity [η] of the copolymer (A) is preferably from 0.1 to 5 dL / g, more preferably from 0.5 to 5.0 dL / g, and even more preferably from 0.9 to 4.0 dL / g.
[0050] The weight average molecular weight (Mw) of the copolymer (A) is preferably 10,000 to 700,000, more preferably 30,000 to 600,000, and further preferably 50,000 to 500,000.
[0051] It is preferable that the copolymer (A) satisfies both of the above-mentioned intrinsic viscosity [η] and weight average molecular weight (Mw).
[0052] In the copolymer (A), as described above, the non-conjugated polyene (a3) preferably contains VNB, and more preferably is VNB. That is, in the above formula (1), formula (2), and formula (4) described later, the "mass fraction of (a3)" is preferably the "mass fraction of VNB" (mass%).
[0053] As described above, the copolymer (A) preferably contains, in addition to the structural units derived from the above (a1), (a2) and (a3), a structural unit derived from the non-conjugated polyene (a4) in a mass fraction of 0% to 20% by mass (where the total mass fractions of (a1), (a2), (a3) and (a4) are taken as 100% by mass). In this case, it is preferable that the following requirement (vi) is satisfied.
[0054] ≪Requirement (vi)≫ The weight average molecular weight (Mw) of the copolymer (A), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) (mass fraction (mass %) of (a3)), the mass fraction of the structural unit derived from the non-conjugated polyene (a4) (mass fraction (mass %) of (a4)), the molecular weight of the non-conjugated polyene (a3) (molecular weight of (a3)), and the molecular weight of the non-conjugated polyene (a4) (molecular weight of (a4)) satisfy the following formula (4). 4.5≦Mw×{(mass fraction of (a3) / 100 / molecular weight of (a3))+(mass fraction of (a4) / 100 / molecular weight of (a4))}≦85 …(4) Formula (4) specifies the content of non-conjugated diene (the sum of (a3) and (a4)) in one copolymer molecule.
[0055] When the copolymer (A) containing the structural unit derived from the above (a4) satisfies the formula (4), an ethylene-based copolymer composition excellent in mechanical properties and heat aging resistance can be obtained. If the requirement (vi) is not satisfied and the value of "Mw × {(mass fraction of (a3) / 100 / molecular weight of (a3)) + (mass fraction of (a4) / 100 / molecular weight of (a4))}" in formula (4) is too low, i.e., the content of non-conjugated diene is too low, sufficient crosslinking may not be achieved and appropriate mechanical properties may not be obtained. Conversely, if the value is too high, i.e., the content of non-conjugated diene is too high, excessive crosslinking may occur, resulting in deterioration of mechanical properties and further deterioration of heat aging resistance.
[0056] ≪Requirement (vii)≫ The copolymer (A) is not particularly limited, but has a complex viscosity η at a frequency ω=0.01 rad / s obtained by linear viscoelasticity measurement (190° C.) using a rheometer. * ( ω =0.01) (Pa sec) and the complex viscosity η at frequency ω=10rad / s * ( ω =10) It is preferable that the apparent iodine value (Pa·sec) and the apparent iodine value derived from the non-conjugated polyene (a3) satisfy the following formula (5). Log{η * ( ω =0.01)} / Log{η * ( ω =10)}≦0.0753×{apparent iodine value derived from non-conjugated polyene (a3)}+1.42 … (5)
[0057] Here, the complex viscosity η * ( ω =0.01) and the complex viscosity η * ( ω =10) is the complex viscosity η in requirement (iv) * ( ω =0.1) and the complex viscosity η * ( ω =100) The apparent iodine value derived from the non-conjugated polyene (a3) can be calculated in the same manner as above, except for the measurement frequency. Apparent iodine value derived from (a3) = mass fraction of (a3) × 253.81 / molecular weight of (a3)
[0058] In the above formula (5), the left side represents the shear rate dependency which is an index of the amount of long chain branches, and the right side represents an index of the content of non-conjugated polyene (a3) that is not consumed as long chain branches during polymerization. If the above copolymer (A) satisfies the above formula (5), the degree of long chain branches is not too high, which is preferable. On the other hand, if the above formula (5) is not satisfied, it is found that a large proportion of the copolymerized non-conjugated polyene (a3) is consumed to form long chain branches.
[0059] Furthermore, the copolymer (A) preferably contains a sufficient amount of structural units derived from the non-conjugated polyene (a3), and it is more preferable that the mass fraction of the structural units derived from the non-conjugated polyene (a3) in the copolymer (mass fraction (mass %) of (a3)) and the weight average molecular weight (Mw) of the copolymer satisfy the following formula (6). 6-0.45×Ln(Mw)≦(a3) mass fraction≦10 …(6)
[0060] In addition, the copolymer (A) has a number (n a3 ) is preferably 6 or more, more preferably 6 or more and 80 or less, further preferably 7 or more and 79 or less, and particularly preferably 10 or more and 78 or less.
[0061] Such a copolymer (A) contains a sufficient amount of structural units derived from a non-conjugated polyene (a3) such as VNB, has a low content of long chain branches, is excellent in curing characteristics when crosslinked using a peroxide, has good moldability, and is excellent in balance of physical properties such as mechanical properties, and is particularly excellent in heat aging resistance.
[0062] In addition, the copolymer (A) has a number (n a4 ) is preferably 29 or less, more preferably 10 or less, and even more preferably less than 1.
[0063] In such a copolymer (A), the content of structural units derived from a non-conjugated polyene (a4) such as ENB is controlled within a range that does not impair the object of the present invention, and it is less likely to undergo post-crosslinking and has sufficient heat aging resistance.
[0064] Here, the number of constitutional units derived from the non-conjugated polyene (a3) per weight average molecular weight (Mw) of the copolymer (A) (n a3 ) or the number of constitutional units derived from the non-conjugated polyene (a4) (n a4) can be calculated from the molecular weight of the non-conjugated polyene (a3) or (a4), the mass fraction of the structural units derived from the non-conjugated polyene (a3) or (a4) in the copolymer (the mass fraction (mass %) of (a3) or (a4)), and the weight average molecular weight (Mw) of the copolymer (A) according to the following formula.
[0065] (n a3 )=(Mw)×{mass fraction of (a3) / 100} / molecular weight of non-conjugated polyene (a3) (n a4 )=(Mw)×{mass fraction of (a4) / 100} / molecular weight of non-conjugated polyene (a4)
[0066] In the copolymer (A), the number of structural units derived from the non-conjugated polyenes (a3) and (a4) per weight average molecular weight (Mw) (n a3 ) and (n a4 ) satisfy the above ranges, the copolymer (A) has a low content of long chain branches, is excellent in curing characteristics when crosslinking is performed using a peroxide, has good moldability, and is excellent in balance of physical properties such as mechanical properties, and is less likely to cause post-crosslinking, and is particularly excellent in heat aging resistance, which is preferable.
[0067] <Production of Copolymer (A)> The copolymer (A) is a copolymer obtained by copolymerizing monomers consisting of ethylene (a1), an α-olefin (a2), a non-conjugated polyene (a3), and, if necessary, a non-conjugated polyene (a4).
[0068] The copolymer (A) may be prepared by any method as long as it satisfies the above requirements (i) to (v). However, it is preferable that the copolymer (A) is obtained by copolymerizing monomers in the presence of a metallocene compound, more preferable that the copolymer (A) is obtained by copolymerizing monomers in the presence of a catalyst system containing a metallocene compound, and even more preferable that the copolymer (A) is obtained by a method including a step (1) of copolymerizing in the presence of a polymerization catalyst containing a specific metallocene compound, and a step (2) of deactivating the polymerization catalyst by adding an alcohol as a catalyst deactivator.
[0069] As a specific production method for the copolymer (A), for example, the production method using a metallocene catalyst described in WO 2015 / 122495 and WO 2019 / 180802 can be adopted.
[0070] <Carbon black (B)> The carbon black (B) used in the present invention is one type of known rubber reinforcing agent that is compounded in rubber compositions, and is an inorganic substance generally called carbon black.
[0071] As the carbon black (B), for example, known carbon blacks such as Asahi #55G and Asahi #60G (all manufactured by Asahi Carbon Co., Ltd.) and Seast (SRF, GPF, FEF, MAF, HAF, ISAF, SAF, FT, MT, G-SO, etc.) (all manufactured by Tokai Carbon Co., Ltd.) can be used. These can be used alone or in combination. Carbon blacks that have been surface-treated with a silane coupling agent or the like can also be used.
[0072] The amount of carbon black (B) in the composition of the present invention is 10 to 300 parts by mass, preferably 15 to 200 parts by mass, more preferably 20 to 150 parts by mass, and even more preferably 25 to 120 parts by mass, per 100 parts by mass of the copolymer (A).
[0073] When the amount of carbon black (B) is within the above range, a crosslinked molded article having improved mechanical properties such as tensile strength and abrasion resistance can be obtained, the hardness of the crosslinked molded article can be increased without impairing other physical properties of the crosslinked molded article, and the production costs of the crosslinked molded article can be reduced.
[0074] <Modified silicone oil (C)> The modified silicone oil (C) used in the present invention contains an unsaturated carbon-carbon bond, such as a carbon-carbon double bond or a carbon-carbon triple bond.
[0075] The modified silicone oil (C) may be, for example, methacryl-modified silicone oil, acrylic-modified silicone oil, vinyl-modified silicone oil, etc. Among these, methacryl-modified silicone oil is preferred because it can form a crosslinked body that is excellent in maintaining low friction. The modified silicone oil (C) may be used alone or in combination of two or more.
[0076] The kinetic viscosity of the modified silicone oil (C) at 25° C. is preferably 30 to 500 mm 2 / s, more preferably 50 to 400 mm 2 / s, more preferably 100 to 300 mm 2 When the kinetic viscosity is within the above range, a crosslinked product that is excellent in maintaining low friction can be obtained.
[0077] The amount of the modified silicone oil (C) in the composition of the present invention is 0.1 to 40 parts by mass, preferably 0.5 to 20 parts by mass, and more preferably 1 to 10 parts by mass, based on 100 parts by mass of the copolymer (A). By having the amount of the modified silicone oil (C) within the above range, a crosslinked product excellent in maintaining low friction can be obtained.
[0078] <Organic peroxide crosslinking agent (D)> The organic peroxide-based crosslinking agent (D) which may be incorporated in the composition of the present invention is a type of crosslinking agent, and specific examples thereof include dicumyl peroxide (DCP), di-tert-butyl peroxide, 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butylperoxybenzoate, ert-butylperoxyisopropylcarbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.
[0079] Among these, bifunctional organic peroxides such as dicumyl peroxide (DCP), 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and n-butyl-4,4-bis(tert-butylperoxy)valerate are preferred, and among these, 2,5-di-(tert-butylperoxy)hexane and 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane are most preferred.
[0080] When an organic peroxide-based crosslinking agent (D) is used, the blending amount thereof is preferably 0.1 to 20 parts by mass, more preferably 0.2 to 15 parts by mass, and further preferably 0.5 to 10 parts by mass, based on 100 parts by mass of the copolymer (A). When the blending amount of the organic peroxide is within the above range, it is preferable because the copolymer composition exhibits excellent crosslinking properties.
[0081] In addition, when an organic peroxide-based crosslinking agent (D) is used, it is preferable to use a crosslinking assistant in combination. Examples of the crosslinking assistant include sulfur; quinone dioxime-based crosslinking assistant such as p-quinone dioxime; acrylic crosslinking assistant such as ethylene glycol dimethacrylate and trimethylolpropane trimethacrylate; allyl crosslinking assistant such as diallyl phthalate and triallyl isocyanurate; maleimide-based crosslinking assistant; divinylbenzene; and metal oxides such as zinc oxide (e.g., ZnO#1-zinc oxide type 2 (JIS standard (K-1410)), manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name: manufactured by Inoue Seki Kogyo Co., Ltd.)). The amount of the crosslinking assistant is usually 0.5 to 10 mol, preferably 0.5 to 7 mol, and more preferably 1 to 5 mol, per mol of the organic peroxide-based crosslinking agent (D).
[0082] <Softener (E)> Examples of the softener (E) that may be incorporated in the composition of the present invention include petroleum-based softeners such as process oil, lubricating oil, paraffin oil, liquid paraffin, petroleum asphalt, and Vaseline; coal tar-based softeners such as coal tar; fatty oil-based softeners such as castor oil, linseed oil, rapeseed oil, soybean oil, and coconut oil; waxes such as beeswax and carnauba wax; naphthenic acid, pine oil, rosin or derivatives thereof; synthetic polymeric substances such as terpene resins, petroleum resins, and coumarone-indene resins; ester-based softeners such as dioctyl phthalate and dioctyl adipate; and others, such as microcrystalline wax, liquid polybutadiene, modified liquid polybutadiene, hydrocarbon-based synthetic lubricating oils, tall oil, and sub(factice). Of these, petroleum-based softeners and hydrocarbon-based synthetic lubricating oils are preferred, and process oil and liquid ethylene-propylene copolymers are particularly preferred.
[0083] The amount of the softener (E) is preferably 1 to 100 parts by mass, more preferably 5 to 90 parts by mass, based on 100 parts by mass of the copolymer (A). When the amount of the softener (E) is within the above range, a rubber composition excellent in processability, heat aging resistance, mechanical properties, etc. can be obtained.
[0084] <Anti-aging agent (F)> Examples of the antioxidant (F) that may be incorporated in the composition of the present invention include conventionally known antioxidants, such as amine-based antioxidants, phenol-based antioxidants, and sulfur-based antioxidants.
[0085] Further examples of the antiaging agent include aromatic secondary amine-based antiaging agents such as phenylbutylamine and N,N-di-2-naphthyl-p-phenylenediamine; phenol-based antiaging agents such as dibutylhydroxytoluene and tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane; thioether-based antiaging agents such as bis[2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl]sulfide; dithiocarbamate-based antiaging agents such as nickel dibutyldithiocarbamate; and sulfur-based antiaging agents such as 2-mercaptobenzoylimidazole, 2-mercaptobenzimidazole, zinc salt of 2-mercaptobenzimidazole, dilaurylthiodipropionate, and distearylthiodipropionate.
[0086] These antioxidants (F) can be used alone or in combination of two or more. The amount of the antioxidant (F) is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 1.0 to 10 parts by mass, per 100 parts by mass of the copolymer (A).
[0087] <Other ingredients> The composition of the present invention may contain additives other than the above components (A) to (F), such as processing aids, activators, inorganic fillers, moisture absorbents, heat stabilizers, weather stabilizers, antistatic agents, colorants, lubricants, and thickeners.
[0088] <Processing aids> As the processing aid, a wide variety of processing aids that are generally compounded with rubber can be used.Specific examples include ricinoleic acid, stearic acid, palmitic acid, lauric acid, barium stearate, zinc stearate, calcium stearate, zinc laurate, and esters.Of these, stearic acid is preferred.
[0089] <Activator> Examples of the activator include amines such as di-n-butylamine, dicyclohexylamine, and monoethanolamine; activators such as diethylene glycol, polyethylene glycol, lecithin, triaryl methylate, and zinc compounds of aliphatic or aromatic carboxylic acids; zinc peroxide preparations; octadecyltrimethylammonium bromide, synthetic hydrotalcite, and special quaternary ammonium compounds.
[0090] <Inorganic fillers> Specific examples of inorganic fillers that can be used include one or more of light calcium carbonate, heavy calcium carbonate, talc, clay, etc., and of these, heavy calcium carbonate such as "Whiten SB" (product name: Shiraishi Calcium Co., Ltd.) is preferred.
[0091] Moisture absorbent Specific examples of the moisture absorbent include calcium oxide, silica gel, sodium sulfate, molecular sieve, zeolite, and white carbon.
[0092] <Method of preparing rubber composition> The rubber composition of the present invention can be prepared by kneading the above-mentioned components (A) to (C) and, if necessary, other components such as a softener (E), an antioxidant (F), and a processing aid, for 1 to 20 minutes at a temperature of 80 to 190° C. using an internal mixer (internal mixer) such as a Banbury mixer, a kneader, or an intermix. Next, additives such as a crosslinking agent, a crosslinking aid, and a vulcanization accelerator are added to the blend obtained using rolls such as an open roll or a kneader, and the vulcanization accelerator and crosslinking aid are further mixed as necessary, and the mixture is kneaded at a roll temperature of 40 to 80° C. for 5 to 30 minutes, followed by dispensing.
[0093] In addition, when the kneading temperature in an internal mixer is low, the above-mentioned components (A) to (C), and, if necessary, the softener (E), antioxidant (F), processing aid, etc. may be kneaded together with the above-mentioned organic peroxide-based crosslinking agent (D) and various additives at the same time.
[0094] [Crosslinked body] The crosslinked product of the present invention is obtained by crosslinking the rubber composition of the present invention. To produce a crosslinked product from the rubber composition, an unvulcanized rubber composition is prepared in the manner described above, similar to the vulcanization of general rubber, and then the rubber composition is molded into the intended shape and then vulcanized.
[0095] The unvulcanized rubber composition prepared as described above can be molded and vulcanized by various molding methods, but its properties can be best exhibited when it is molded and vulcanized by mold molding such as compression molding, injection molding, and casting.
[0096] In the case of compression molding, for example, a pre-weighed amount of unvulcanized rubber composition is placed in a mold, and after closing the mold, the composition is heated at a temperature of 120 to 270°C for 30 seconds to 120 minutes to obtain the desired crosslinked product.
[0097] In the case of injection molding, for example, a ribbon-shaped or pellet-shaped rubber composition is fed into a pot in a preset amount by a screw. Then, the preheated rubber composition is fed into a mold by a plunger in 1 to 20 seconds. After the rubber composition is injected, it is heated at a temperature of 120 to 270°C for 30 seconds to 120 minutes to obtain the desired crosslinked product.
[0098] In the case of injection molding, for example, a pre-weighed amount of the rubber composition is placed in a pot and injected into a mold by a piston in 1 to 20 seconds. After the rubber composition is injected, it is heated at a temperature of 120 to 270°C for 30 seconds to 120 minutes to obtain the desired crosslinked product.
[0099] <Applications of crosslinked bodies> The crosslinked product obtained from the rubber composition of the present invention can be molded into a desired shape to obtain various products. The crosslinked product of the present invention is excellent in maintaining low friction, and therefore can be suitably used as a sliding seal. EXAMPLES
[0100] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following description, "parts" refers to "parts by mass" unless otherwise specified.
[0101] [Measurement and evaluation method] In the following examples and comparative examples, the methods for measuring and evaluating the various physical properties and characteristics are as follows.
[0102] (1) Physical properties of ethylene-α-olefin-non-conjugated polyene copolymer (A) <Composition of Copolymer (A)> The molar ratio and mass fraction (mass%) of each structural unit of the copolymer (A) are 13 The measured values were obtained by C-NMR. The measured values were obtained by using an ECX400P nuclear magnetic resonance apparatus (manufactured by JEOL Ltd.) at a measurement temperature of 120°C, a measurement solvent of orthodichlorobenzene / deuterated benzene = 4 / 1, and an accumulation number of 8000 times. 13The C-NMR spectrum was obtained.
[0103] <Intrinsic viscosity> The intrinsic viscosity [η] was measured using a fully automatic intrinsic viscometer manufactured by Rigo Co., Ltd. at a temperature of 135° C. and in decalin as a measurement solvent.
[0104] <Complex viscosity η * > The rheometer used was the Ares viscoelasticity measuring device (manufactured by Rheometric Scientific), and the complex viscosity η at a frequency of ω = 0.01 rad / s was measured under the conditions of 190°C and 1.0% strain. * ( ω =0.01) , complex viscosity η at frequency ω=0.1rad / s * ( ω =0.1) , complex viscosity η at frequency ω=10rad / s * ( ω =10) and the complex viscosity η at frequency ω = 100 rad / s * ( ω =100) (All units are Pa sec) were measured. * ( ω =0.1) and η * ( ω =100) The ratio of complex viscosity to * The P-value (η * ( ω =0.1) / η * ( ω =100) ) was calculated.
[0105] Weight average molecular weight (Mw) and number of long chain branches (LCB) per 1000 carbon atoms 1000c )> The structure was determined by the above-mentioned 3D-GPC structural analysis method.
[0106] (2) Properties of Rubber Composition (Unvulcanized Rubber Properties) <Mooney Viscosity (ML (1+4) 100℃) Mooney viscosity at 100℃ (ML (1+4) 100°C) was measured at 100°C using a Mooney viscometer (SMV202 model, manufactured by Shimadzu Corporation) in accordance with JIS K6300.
[0107] (3) Physical properties of crosslinked products (physical properties of vulcanized rubber) <Modulus (MPa), Tensile stress at break (MPa), Tensile elongation at break (%)> The sheet was punched out to prepare a No. 3 dumbbell test piece as described in JIS K 6251 (1993). Using this test piece, a tensile test was carried out according to the method specified in JIS K6251, paragraph 3, at a measurement temperature of 25°C and a tensile speed of 500 mm / min. The modulus at 100% elongation (M 100 ), modulus at 200% elongation (M 200 ) Tensile stress at break (T B ) and tensile elongation at break (E B ) was measured.
[0108] <Durometer A hardness> According to JIS K 6253, the hardness of the sheet (Type A durometer, HA) was measured using six 2 mm thick crosslinked sheets with smooth surfaces, stacked on top of each other at the flat part to a thickness of approximately 12 mm. However, specimens with foreign matter, air bubbles, or scratches were not used. The dimensions of the measurement surface of the specimen were set so that the tip of the indenter could be measured at a position 12 mm or more away from the end of the specimen.
[0109] <Static and kinetic friction coefficients> The static and dynamic friction coefficients were measured using a reciprocating abrasion tester (30S manufactured by Shinto Scientific Co., Ltd.) using a cross-linked sheet with a thickness of 2 mm and a smooth surface, under the following conditions: temperature: 23±2°C, humidity: 50±5RH, test speed: 300mm / min, test load: 200gf, stroke: 30mm, mating material: SUS403, 12.7mmφ sphere.
[0110] <Static and dynamic friction coefficients after wiping the surface> The static and kinetic coefficients of friction after wiping the surface were measured by wiping the measurement surface of the test piece three times back and forth with a paper wiper (Kimwipe, manufactured by Nippon Paper Classia) thoroughly soaked in ethanol (special grade ethanol, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.), and using the wiped surface, the static and kinetic coefficients of friction were measured.
[0111] [Production Example 1] Production of ethylene-propylene-VNB copolymer (A-1) A 300-liter polymerization reactor was continuously fed with 58.3 L / hr of dehydrated hexane solvent from line 1, 4.5 mmol / hr of triisobutylaluminum (TiBA), 0.150 mmol / hr of (C6H5)3CB(C6F5)4, and 0.030 mmol / hr of di(p-tolyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride from line 2. At the same time, 6.6 kg / hr of ethylene, 9.3 kg / hr of propylene, 18 L / hr of hydrogen, and 340 g / hr of VNB were continuously fed into the polymerization reactor from separate lines, and copolymerization was carried out under the conditions of a polymerization temperature of 87°C, a total pressure of 1.6 MPaG, and a residence time of 1.0 hour.
[0112] The ethylene-propylene-VNB copolymer solution produced in the polymerization reactor was continuously discharged at a flow rate of 88.0 L / hr, heated to 170°C (pressure increased to 4.1 MPaG), and fed to a phase separator. At this time, ethanol, a polymerization inhibitor, was continuously introduced into the discharge line in an amount of 0.1 mol times the amount of TiBA in the liquid component extracted from the polymerization reactor.
[0113] In the phase separator, the ethylene-propylene-vinyl alcohol copolymer solution was separated into a dense phase (lower phase) containing most of the ethylene-propylene-vinyl alcohol copolymer and a dilute phase (upper phase) containing a small amount of the polymer.
[0114] The separated thick phase was led to a heat exchanger at 85.4 L / hr, and then to a hopper where the solvent was evaporated and separated to obtain ethylene-propylene-VNB copolymer (A-1) at a rate of 7.8 kg / hr.
[0115] The physical properties of the resulting ethylene-propylene-VNB copolymer (A-1) were evaluated as described above, and the results are shown in Table 1.
[0116] [Table 1]
[0117] [Example 1] In the first step, 100 parts by mass of the ethylene-propylene-VNB copolymer (A-1) obtained in Production Example 1 was masticated for 1 minute using a BB-4 type Banbury mixer (manufactured by Kobe Steel, Ltd.), and then 5 parts by mass of zinc oxide (ZnO#1, manufactured by Hakusui Tech Co., Ltd.), 80 parts by mass of carbon black (B-1) (Asahi#60UG, manufactured by Asahi Carbon Co., Ltd.), methacrylic modified silicone oil (C-1) (KF-2012, manufactured by Shin-Etsu Chemical Co., Ltd., 25°C kinematic viscosity: 60 mmHg), and 100 parts by mass of methacrylic modified silicone oil (C-2) (KF-2012, manufactured by Shin-Etsu Chemical Co., Ltd., 25°C kinematic viscosity: 60 mmHg) were added thereto. 2 5 parts by mass of paraffinic process oil (E-1) (Diana Process PW-380, manufactured by Idemitsu Kosan Co., Ltd.) as a softener (E) and 50 parts by mass of liquid ethylene-propylene copolymer (E-2) (100°C kinematic viscosity: 2000 mm 2 As the antioxidant (F), 15 parts by mass of phenol-based antioxidant (F-1) (Irganox 1010, manufactured by BASF) and 4 parts by mass of imidazole-based antioxidant (F-2) (Sandant MB, manufactured by Sanshin Chemical Industry Co., Ltd.) were added, and kneaded for 2 minutes at 140° C. After that, the ram was raised and cleaned, and kneaded for another minute, and the kneaded product was discharged at about 150° C. to obtain a first-stage compound.
[0118] Next, in the second step, the compound obtained in the first step was wound around a 6-inch roll (manufactured by Nippon Roll Co., Ltd., front roll surface temperature 50°C, rear roll surface temperature 50°C, front roll rotation speed 16 rpm, rear roll rotation speed 18 rpm), and 5.3 parts by mass of 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane (Perhexa 25B, manufactured by NOF Corp.) as an organic peroxide-based crosslinking agent (D-1) and 2 parts by mass of a mixture of zinc methacrylate and zinc oxide (ACTOR ZMA, manufactured by Kawaguchi Chemical Industry Co., Ltd.) as a co-crosslinking agent were added thereto in a compounding amount, and kneaded for 10 minutes to obtain an uncrosslinked rubber composition. The physical properties of this rubber composition were evaluated.
[0119] The uncrosslinked rubber composition was extruded into a sheet, and then pressed at 180°C for 20 minutes using a 100-ton press molding machine to obtain a crosslinked sheet having a thickness of 2 mm. The physical properties of the crosslinked sheet were measured using this. The results are shown in Table 2.
[0120] [Example 2] Instead of the methacrylic-modified silicone oil (C-1) used in Example 1, a methacrylic-modified silicone oil (C-2) (X-22-2456, manufactured by Shin-Etsu Chemical Co., Ltd., kinematic viscosity at 25°C: 200 mm 2 Except for using 5 parts by mass of 1,000 sucrose / s and 4.6 parts by mass of organic peroxide (D-1), the procedure of Example 1 was repeated to obtain an uncrosslinked rubber composition and a crosslinked sheet having a thickness of 2 mm, and the same evaluations were performed as in Example 1. The results are shown in Table 2. [Comparative Example 1] Except for not using the methacrylic modified silicone oil (C-1) used in Example 1 and changing the amount of organic peroxide (D-1) to 4.5 parts by mass, the same procedure as in Example 1 was carried out to obtain an uncrosslinked rubber composition and a crosslinked sheet having a thickness of 2 mm, and the same evaluations were carried out as in Example 1. The results are shown in Table 2.
[0121] [Comparative Example 2] Instead of the methacrylic modified silicone oil (C-1) used in Example 1, an unmodified silicone oil (KF-968, Shin-Etsu Chemical Co., Ltd., kinematic viscosity at 25°C: 100 mm 2An uncrosslinked rubber composition and a crosslinked sheet having a thickness of 2 mm were obtained in the same manner as in Example 1, except that 5 parts by mass of the rubber composition was used. The results were evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0122] [Table 2]
Claims
1. (A) 100 parts by mass of an ethylene / α-olefin / non-conjugated polyene copolymer having a structural unit derived from ethylene (a1), a structural unit derived from an α-olefin (a2) having 3 to 20 carbon atoms, and a structural unit derived from a non-conjugated polyene (a3); (B) 10 to 300 parts by mass of carbon black, and (C) 0.1 to 40 parts by mass of modified silicone oil containing an unsaturated carbon-carbon bond and the copolymer (A) satisfies the following requirements (i) to (v): (i) the molar ratio of ethylene / α-olefin is from 40 / 60 to 99.9 / 0.1; (ii) the mass fraction of the structural unit derived from the non-conjugated polyene (a3) is 0.07% by mass to 10% by mass in 100% by mass of the copolymer (A); (iii) the weight average molecular weight (Mw) of the copolymer (A), the mass fraction of the structural unit derived from the non-conjugated polyene (a3) (mass fraction (mass %) of (a3)), and the molecular weight of the non-conjugated polyene (a3) (molecular weight of (a3)) satisfy the following formula (1); 4.5≦Mw×mass fraction of (a3) / 100 / molecular weight of (a3)≦80 (1) (iv) Complex viscosity η at frequency ω = 0.1 rad / s obtained by linear viscoelastic measurement (190°C) using a rheometer * ( ω =0.1) (Pa sec) and the complex viscosity η at a frequency ω = 100 rad / s * ( ω =100) (Pa sec) P(η * ( ω =0.1) / * ( ω =100) ), the intrinsic viscosity [η], and the mass fraction of the structural unit derived from the non-conjugated polyene (a3) (mass fraction of (a3)) satisfy the following formula (2): P / ([η] 2.9 ) ≦ mass fraction of (a3) × 6 ... (2) (v) Long Chain Branches (LCB) per 1000 carbon atoms obtained using 3D-GPC 1000C ) and the natural logarithm of the weight average molecular weight (Mw) [Ln(Mw)] satisfy the following formula (3). LCB 1000C ≦1-0.07×Ln(Mw) ‥ Formula (3)
2. The rubber composition for sliding seals according to claim 1, further comprising 0.1 to 20 parts by mass of an organic peroxide-based crosslinking agent (D).
3. 2. The rubber composition for sliding seals according to claim 1, wherein the modified silicone oil (C) is a methacrylic-modified silicone oil.
4. The modified silicone oil (C) has a kinetic viscosity at 25° C. of 30 to 500 mm 2 The rubber composition for a sliding seal according to claim 1, wherein the molar ratio of the rubber composition for a sliding seal is 1:1 or more.
5. 2. The rubber composition for sliding seals according to claim 1, wherein the non-conjugated polyene (a3) contains, in the molecule, a total of two or more partial structures selected from the group consisting of the following general formulae (I) and (II): 【Chemistry 1】
6. The rubber composition for sliding seals according to claim 1, wherein the non-conjugated polyene (a3) comprises 5-vinyl-2-norbornene (VNB).
7. The rubber composition for a sliding seal according to claim 1, wherein the α-olefin (a2) is propylene.
8. The rubber composition for a sliding seal according to claim 1, further comprising 1 to 100 parts by mass of a softener (E).
9. The rubber composition for sliding seals according to claim 1, further comprising 0.1 to 20 parts by mass of an antioxidant (F).
10. A crosslinked body of the rubber composition for sliding seals according to any one of claims 1 to 9.
11. A sliding seal comprising the crosslinked body according to claim 10.
Citation Information
Patent Citations
Window sealing molded article and preparation thereof
JP2000191863A
Rubber composition and its application
JP2012031342A
ETHYLENE / $g(a)-OLEFIN / UNCONJUGATED POLYENE COPOLYMER RUBBER, RUBBER COMPOSITION FOR SEALING, MOLDED RUBBER FOR SEALING, AND PROCESS FOR PRODUCING THE MOLDED RUBBER
WO2000059962A1