Sealing resin composition and sealant for organic el display elements
The sealing resin composition with episulfide groups and aromatic rings addresses the issues of poor light extraction and handling in top-emission type organic EL display elements by providing fast curing and high refractive index, enhancing light extraction efficiency.
Patent Information
- Application Number
- JP2023050009
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Top-emission type organic EL display elements face issues with poor light extraction efficiency due to refractive index differences between electrodes, passivation films, and encapsulants, and existing encapsulants struggle with handling properties and curing speed.
A sealing resin composition containing a curable resin with episulfide groups and aromatic rings, having a viscosity of 2000 mPa·s or less and a refractive index of 1.60 or more, along with a photopolymerization initiator, to enhance curing speed and handling properties.
The composition achieves fast curing, improved handling, and high refractive index, resulting in enhanced light extraction efficiency for organic EL display elements.
Smart Images

Figure 2024139180000001 
Figure 2024139180000002 
Figure 2024139180000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an encapsulating resin composition. The present invention also relates to a sealant for an organic EL display element, comprising the encapsulating resin composition. [Background technology]
[0002] Conventionally, encapsulating resin compositions containing a curable resin and a polymerization initiator have been used as encapsulating resin compositions for use in electronic devices, display elements, etc. Specifically, encapsulating resin compositions and their cured products have been used to seal organic electroluminescence (hereinafter also referred to as "organic EL") display elements and the like.
[0003] An organic EL display element has a laminate structure in which an organic light-emitting material layer is sandwiched between a pair of opposing electrodes, and when electrons are injected into this organic light-emitting material layer from one electrode and holes are injected from the other electrode, the electrons and holes combine in the organic light-emitting material layer to emit light. As such, organic EL display elements emit light themselves, and therefore have the advantages of better visibility than liquid crystal display elements and the like that require a backlight, can be made thinner, and can be driven with a low DC voltage.
[0004] The organic light-emitting material layer and electrodes constituting an organic EL display element have a problem in that their characteristics are easily deteriorated by moisture, oxygen, and the like. Therefore, in order to obtain a practical organic EL display element, it is necessary to extend the life of the organic light-emitting material layer and electrodes by isolating them from the atmosphere. As a method for isolating the organic light-emitting material layer and electrodes from the atmosphere, the organic EL display element is sealed with a sealant (for example, Patent Document 1). When sealing an organic EL display element with a sealant, a method is usually used in which an inorganic material film called a passivation film is provided on a laminate having an organic light-emitting material layer, and the inorganic material film is sealed with a sealant in order to sufficiently suppress the permeation of moisture, oxygen, and the like.
[0005] In recent years, instead of bottom-emission organic EL display elements in which light emitted from an organic light-emitting material layer is extracted from the substrate surface side on which the light-emitting element is formed, top-emission organic EL display elements in which light is extracted from the top surface side of the organic light-emitting material layer have been attracting attention. This method has the advantage of being advantageous in terms of long life because of its high aperture ratio and low-voltage drive. In such top-emission organic EL display elements, the top surface side of the light-emitting layer must be transparent, so that the light-emitting element is sealed by laminating a transparent moisture-proof base material such as glass on the top surface side of the light-emitting element via a transparent sealing layer (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2007-115692 A Summary of the Invention [Problem to be solved by the invention]
[0007] In a top-emission organic EL display element, even if a transparent moisture-proof substrate or a sealant having a sufficiently high transparency is used, the efficiency of extracting light emitted from the laminate may be poor due to the difference in refractive index between the sealant and the electrodes or passivation film. In order to improve the light extraction efficiency, it is possible to use a high refractive index resin with high crystallinity as the sealant, but when such a high refractive index resin is used, the resulting sealant may have poor handling properties. On the other hand, when a low-viscosity curable resin is used to improve the handleability of the sealant, display defects may occur due to the sealant before curing seeping into the laminate, etc., and therefore, there has been a demand for the sealant to have both fast curing properties and handleability. The present invention aims to provide an encapsulating resin composition that has excellent fast curing properties and handleability, and provides a cured product with a high refractive index. The present invention also aims to provide a sealant for an organic electroluminescence display element that contains the encapsulating resin composition. [Means for solving the problem]
[0008] Disclosure 1 relates to an encapsulating resin composition containing a curable resin and a photopolymerization initiator, wherein the curable resin contains an episulfide compound having one or more episulfide groups and one or more aromatic rings in one molecule, and the encapsulating resin composition has a viscosity of 2000 mPa s or less as measured at 25°C using an E-type viscometer, and a refractive index of the cured product at 25°C for sodium D lines of 1.60 or more. Disclosure 2 relates to the encapsulating resin composition of Disclosure 1, in which the episulfide compound is a compound having one episulfide group and one or more aromatic rings in one molecule. The present disclosure 3 is the encapsulating resin composition according to the present disclosure 1 or 2, in which the content of the episulfide compound in 100 parts by mass of the curable resin is 40 parts by mass or more. The present disclosure 4 is the encapsulating resin composition according to the present disclosure 1, 2, or 3, wherein the curable resin further contains an epoxy compound. The present disclosure 5 is the encapsulating resin composition according to the present disclosure 1, 2, 3, or 4, wherein the photopolymerization initiator is a cationic photopolymerization initiator. The present disclosure 6 is a sealant for an organic EL display device, comprising the encapsulating resin composition of the present disclosure 1, 2, 3, 4 or 5. The present invention will be described in detail below.
[0009] The present inventors have investigated the use of an episulfide compound having one or more episulfide groups and one or more aromatic rings in one molecule as the curable resin in an encapsulating resin composition containing a curable resin and a photopolymerization initiator, and then setting the viscosity to a specific value or less and setting the refractive index of the cured product to a specific value or more. As a result, it has been found that an encapsulating resin composition having excellent fast curing properties and handleability and a high refractive index of the cured product can be obtained, and the present invention has been completed. Since the encapsulating resin composition of the present invention has a high refractive index of the cured product, when it is used as an encapsulant for a display element such as an organic EL display element, the resulting display element has excellent light extraction efficiency.
[0010] The encapsulating resin composition of the present invention contains a curable resin. The curable resin contains an episulfide compound having one or more episulfide groups and one or more aromatic rings in one molecule (hereinafter also referred to as "episulfide compound according to the present invention"). By containing the episulfide compound according to the present invention, the encapsulating resin composition of the present invention has excellent fast curing properties and can easily adjust the viscosity and the refractive index of the cured product to the ranges described below.
[0011] The preferred upper limit of the number of episulfide groups in one molecule of the episulfide compound according to the present invention is 4. When the number of episulfide groups is 4 or less, the obtained encapsulating resin composition has excellent storage stability. In particular, it is preferred that the number of episulfide groups is 1, that is, the episulfide compound according to the present invention is a compound having one episulfide group and one or more aromatic rings in one molecule.
[0012] The preferred upper limit of the number of aromatic rings in one molecule of the episulfide compound according to the present invention is 4. When the number of aromatic rings is 4 or less, it becomes easier to adjust the viscosity of the resulting encapsulating resin composition to the range described below. The number of aromatic rings is, for example, one in the case of a benzene ring, two in the case of a naphthalene ring, and three in the case of an anthracene ring.
[0013] The episulfide compound according to the present invention preferably has a biphenyl skeleton as the structure containing the aromatic ring, since this makes it easier to adjust the refractive index of the cured product to within the range described below.
[0014] The episulfide compound according to the present invention has an episulfide group equivalent of preferably 50 at its lower limit and 500 at its upper limit. When the episulfide group equivalent of the episulfide compound according to the present invention is within this range, the resulting encapsulating resin composition has better adhesion, low outgassing properties, and coatability. The episulfide compound according to the present invention has an episulfide group equivalent of more preferably 100 at its lower limit and 300 at its upper limit. In this specification, the episulfide group equivalent means (molecular weight of episulfide compound) / (number of episulfide groups in one molecule of episulfide compound).
[0015] The preferred lower limit of the molecular weight of the episulfide compound according to the present invention is 100, and the preferred upper limit is 1000. When the molecular weight of the episulfide compound according to the present invention is within this range, the resulting encapsulating resin composition has better adhesion, low outgassing properties, and coatability. The more preferred lower limit of the molecular weight of the episulfide compound according to the present invention is 200, and the preferred upper limit is 600. In this specification, the "molecular weight" is the molecular weight calculated from the structural formula for compounds with specific molecular structures, but may be expressed as the weight average molecular weight for compounds with a wide distribution of polymerization degrees and compounds with unspecified modified sites. The "weight average molecular weight" is a value calculated in terms of polystyrene by measuring with gel permeation chromatography (GPC) using tetrahydrofuran as a solvent. Examples of columns used in measuring the weight average molecular weight calculated in terms of polystyrene by GPC include Shodex LF-804 (manufactured by Showa Denko KK).
[0016] The episulfide compound according to the present invention is preferably in a liquid state at 25° C. When the episulfide compound according to the present invention is in a liquid state at 25° C., the resulting encapsulating resin composition has superior coatability.
[0017] Specific examples of the episulfide compound according to the present invention include a compound represented by the following formula (1) and a compound represented by the following formula (2). Among these, the compound represented by the following formula (1) is preferred because the resulting encapsulating resin composition has excellent fast curing properties and the viscosity and refractive index of the cured product can be more easily adjusted to the ranges described below.
[0018] [ka]
[0019] [ka]
[0020] The curable resin may contain only the episulfide compound according to the present invention, or may contain other curable resins in addition to the episulfide compound according to the present invention. When the curable resin contains the other curable resin, the preferred lower limit of the episulfide compound according to the present invention in 100 parts by mass of the curable resin is 30 parts by mass. When the content of the episulfide compound according to the present invention is 30 parts by mass or more, the obtained encapsulating resin composition has excellent fast curing properties, and it becomes easier to adjust the viscosity and the refractive index of the cured product to the range described below. A more preferred lower limit of the content of the episulfide compound according to the present invention is 40 parts by mass. From the viewpoint of increasing the cure rate of the cured product, the upper limit of the episulfide compound according to the present invention per 100 parts by mass of the curable resin is preferably 80 parts by mass, and more preferably 60 parts by mass.
[0021] The other curable resin is preferably an epoxy compound. From the viewpoint of increasing the cure rate of the obtained cured product of the encapsulating resin composition and facilitating adjustment of the refractive index, the epoxy compound is preferably a compound having a biphenyl skeleton and an epoxy group.
[0022] Specific examples of the compound having a biphenyl skeleton and an epoxy group include o-phenylphenol glycidyl ether, p-phenylphenol glycidyl ether, 4,4-biphenyldiyl bis(glycidyl ether), 4,4'-bis(glycidyloxy)-1,1'-biphenyl, 3,3',5,5'-tetramethyl-4,4'-bis(glycidyloxy)-1,1'-biphenyl, etc. Among these, o-phenylphenol glycidyl ether is preferred.
[0023] Examples of the epoxy compounds other than the compound having a biphenyl skeleton and an epoxy group include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol E type epoxy compounds, bisphenol S type epoxy compounds, 3,4-epoxycyclohexylmethyl (3,4-epoxy)cyclohexane carboxylate, 4,4'-bis(1,2-epoxycyclohexane), bis(3,4-epoxycyclohexylmethyl)ether, bis(3,4-epoxycyclohexylmethyl) adipate, 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol, and ((3,4-epoxycyclohexane)-1-yl)methyl methacrylate. tyl, 1,6-bis(glycidyloxy)naphthalene, fluorene type epoxy compound, 1,7-octadiene diepoxide, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, dipropylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, phenyl glycidyl ether, and phenylene diglycidyl ether.
[0024] Examples of the other curable resins other than the epoxy compounds include oxetane compounds and vinyl ether compounds.
[0025] Examples of the oxetane compound include 3-ethyl-3-(((3-ethyloxetan-3-yl)methoxy)methyl)oxetane, 3-ethyl-3-((2-ethylhexyloxy)methyl)oxetane, 3-ethyl-3-((3-(triethoxysilyl)propoxy)methyl)oxetane, phenol novolak oxetane, and 1,4-bis(((3-ethyl-3-oxetanyl)methoxy)methyl)benzene.
[0026] Examples of the vinyl ether compound include benzyl vinyl ether, cyclohexanedimethanol monovinyl ether, dicyclopentadiene vinyl ether, 1,4-butanediol divinyl ether, cyclohexanedimethanol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, dipropylene glycol divinyl ether, and tripropylene glycol divinyl ether.
[0027] The encapsulating resin composition of the present invention contains a photopolymerization initiator. The photopolymerization initiator is preferably a cationic photopolymerization initiator. The photocationic polymerization initiator is not particularly limited as long as it generates a protonic acid or a Lewis acid upon irradiation with light, and may be an ionic photoacid generating type or a nonionic photoacid generating type.
[0028] The anion portion of the ionic photoacid generating cationic photopolymerization initiator is, for example, BF4 - , PF6 - , SbF6 - , (BX4) - (wherein X represents a phenyl group substituted with at least two fluorine or trifluoromethyl groups). The anion moiety may be PF m (C n F 2n+1 )6-m - (wherein, m is an integer of 0 or more and 5 or less, and n is an integer of 1 or more and 6 or less). Examples of the ionic photoacid generating type photocationic polymerization initiator include aromatic sulfonium salts, aromatic iodonium salts, aromatic diazonium salts, aromatic ammonium salts, (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe salts, and the like, each of which has the anion moiety.
[0029] Examples of the aromatic sulfonium salt include bis(4-(diphenylsulfonio)phenyl)sulfide bishexafluorophosphate, bis(4-(diphenylsulfonio)phenyl)sulfide bishexafluoroantimonate, bis(4-(diphenylsulfonio)phenyl)sulfide bistetrafluoroborate, bis(4-(diphenylsulfonio)phenyl)sulfide tetrakis(pentafluorophenyl)borate, diphenyl-4-(phenylthio)phenylsulfonium hexafluorophosphate, diphenyl-4-(phenylthio)phenylsulfonium hexafluoroantimonate, diphenyl-4-(phenylthio)phenylsulfonium tetrafluoroborate, diphenyl-4-(phenylthio)phenylsulfonium tetrakis(pentafluorophenyl)borate, and triphenylsulfonium hexafluorophosphate. Examples of the sulfonium tetrakis(pentafluorophenyl)borate include triphenylsulfonium hexafluoroantimonate, triphenylsulfonium tetrafluoroborate, triphenylsulfonium tetrakis(pentafluorophenyl)borate, bis(4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl)sulfide bishexafluorophosphate, bis(4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl)sulfide bishexafluoroantimonate, bis(4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl)sulfide bistetrafluoroborate, bis(4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl)sulfide tetrakis(pentafluorophenyl)borate, and tris(4-(4-acetylphenyl)thiophenyl)sulfonium tetrakis(pentafluorophenyl)borate. Of these, triarylsulfonium tetrakis(pentafluorophenyl)borate such as triphenylsulfonium tetrakis(pentafluorophenyl)borate is preferred.
[0030] Examples of the aromatic iodonium salt include diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, diphenyliodonium tetrafluoroborate, diphenyliodonium tetrakis(pentafluorophenyl)borate, bis(dodecylphenyl)iodonium hexafluorophosphate, bis(dodecylphenyl)iodonium hexafluoroantimonate, bis(dodecylphenyl)iodonium tetrafluoroborate, bis(dodecylphenyl)iodonium tetrakis(pentafluorophenyl)borate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluorophosphate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluoroantimonate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium tetrafluoroborate, and 4-methylphenyl-4-(1-methylethyl)phenyliodonium tetrakis(pentafluorophenyl)borate.
[0031] Examples of the aromatic diazonium salt include phenyldiazonium hexafluorophosphate, phenyldiazonium hexafluoroantimonate, phenyldiazonium tetrafluoroborate, and phenyldiazonium tetrakis(pentafluorophenyl)borate.
[0032] Examples of the aromatic ammonium salt include 1-benzyl-2-cyanopyridinium hexafluorophosphate, 1-benzyl-2-cyanopyridinium hexafluoroantimonate, 1-benzyl-2-cyanopyridinium tetrafluoroborate, 1-benzyl-2-cyanopyridinium tetrakis(pentafluorophenyl)borate, 1-(naphthylmethyl)-2-cyanopyridinium hexafluorophosphate, 1-(naphthylmethyl)-2-cyanopyridinium hexafluoroantimonate, 1-(naphthylmethyl)-2-cyanopyridinium tetrafluoroborate, and 1-(naphthylmethyl)-2-cyanopyridinium tetrakis(pentafluorophenyl)borate.
[0033] Examples of the (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe salt include (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe(II) hexafluorophosphate, (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe(II) hexafluoroantimonate, (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe(II) tetrafluoroborate, and (2,4-cyclopentadiene-1-yl)((1-methylethyl)benzene)-Fe(II) tetrakis(pentafluorophenyl)borate.
[0034] Examples of the nonionic photoacid generating cationic photopolymerization initiator include nitrobenzyl esters, sulfonic acid derivatives, phosphoric acid esters, phenolsulfonic acid esters, diazonaphthoquinones, and N-hydroxyimide sulfonates.
[0035] Among the above-mentioned photocationic polymerization initiators, commercially available ones include, for example, photocationic polymerization initiators manufactured by Midori Chemical Industry Co., Ltd., photocationic polymerization initiators manufactured by Union Carbide Corporation, photocationic polymerization initiators manufactured by ADEKA Corporation, photocationic polymerization initiators manufactured by 3M Corporation, photocationic polymerization initiators manufactured by BASF Corporation, photocationic polymerization initiators manufactured by Solvay Corporation, and photocationic polymerization initiators manufactured by San-Apro Corporation. An example of the photocationic polymerization initiator manufactured by Midori Kagaku Co., Ltd. is DTS-200. Examples of the photocationic polymerization initiator manufactured by Union Carbide include UVI6990 and UVI6974. Examples of the photocationic polymerization initiator manufactured by ADEKA Corporation include SP-150 and SP-170. Examples of the photocationic polymerization initiator manufactured by 3M include FC-508 and FC-512. Examples of the cationic photopolymerization initiator manufactured by BASF include IRGACURE261 and IRGACURE290. An example of the photocationic polymerization initiator manufactured by Solvay is PI2074. Examples of the photocationic polymerization initiators manufactured by San-Apro include CPI-100P, CPI-200K, and CPI-210S.
[0036] The content of the photopolymerization initiator is preferably 0.05 parts by mass at the lower limit and 10 parts by mass at the upper limit with respect to 100 parts by mass of the curable resin. By the content of the photopolymerization initiator being within this range, the obtained encapsulating resin composition has better curability, storage stability and photocurability. The more preferred lower limit of the content of the photopolymerization initiator is 0.1 parts by mass, and the more preferred upper limit is 5 parts by mass.
[0037] The encapsulating resin composition of the present invention may contain a thermal polymerization initiator. However, when the composition is used as a sealant for an organic EL display element, it is preferable that the composition is cured only by light irradiation without containing a thermal polymerization initiator in order to reduce damage to the light emitting element, etc., due to heating.
[0038] The encapsulating resin composition of the present invention may contain a stabilizer. By containing the stabilizer, the encapsulating resin composition of the present invention has better storage stability.
[0039] Examples of the stabilizer include triethanolamine, benzylamine, triglycidyl-p-aminophenol, and the like. These stabilizers may be used alone or in combination of two or more kinds.
[0040] The content of the stabilizer is preferably 0.001 parts by mass at the lower limit and 2 parts by mass at the upper limit with respect to 100 parts by mass of the curable resin. By the content of the stabilizer being within this range, the obtained encapsulating resin composition has excellent storage stability while maintaining excellent curability. The more preferable lower limit of the content of the stabilizer is 0.005 parts by mass, and the more preferable upper limit is 1 part by mass.
[0041] The encapsulating resin composition of the present invention may contain a silane coupling agent. The silane coupling agent plays a role in improving the adhesion between the encapsulating resin composition of the present invention and a substrate or the like.
[0042] Examples of the silane coupling agent include 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-isocyanatopropyltrimethoxysilane. These silane coupling agents may be used alone or in combination of two or more kinds.
[0043] The content of the silane coupling agent is preferably 0.1 parts by mass and 10 parts by mass relative to 100 parts by mass of the curable resin.By the content of the silane coupling agent being within this range, the effect of improving adhesion is excellent while suppressing the bleeding out of excess silane coupling agent.The more preferred lower limit of the content of the silane coupling agent is 0.5 parts by mass and the more preferred upper limit is 5 parts by mass. From the viewpoint of low outgassing, the content of the silane coupling agent is preferably at most 0.5 parts by mass, more preferably at most 0.1 parts by mass, and even more preferably at most 0.01 parts by mass, relative to 100 parts by mass of the curable resin.
[0044] The encapsulating resin composition of the present invention may further contain a surface modifier within a range that does not impair the object of the present invention. By containing the surface modifier, the flatness of the coating film of the encapsulating resin composition of the present invention can be improved. Examples of the surface modifier include a surfactant and a leveling agent.
[0045] Examples of the surface modifier include silicone-based, acrylic-based, and fluorine-based ones. Among the above surface modifiers, commercially available ones include, for example, surface modifiers manufactured by BYK Japan KK and surface modifiers manufactured by AGC Seimi Chemical Co., Ltd. Examples of the surface modifiers manufactured by BYK Japan include BYK-330, BYK-340, and BYK-345. An example of the surface modifier manufactured by AGC Seimi Chemical Co., Ltd. is Surflon S-611.
[0046] The encapsulating resin composition of the present invention may contain a compound that reacts with the acid generated in the encapsulating resin composition or an ion exchange resin in order to improve the durability of the element electrode, etc., within a range that does not impair the object of the present invention.
[0047] The compound that reacts with the generated acid includes a substance that neutralizes the acid, such as an alkali metal carbonate or hydrogen carbonate, or an alkaline earth metal carbonate or hydrogen carbonate, etc. Specific examples of the compound that can be used include calcium carbonate, calcium hydrogen carbonate, sodium carbonate, and sodium hydrogen carbonate.
[0048] The ion exchange resin may be of any of the cation exchange type, anion exchange type and amphoteric ion exchange type, with the cation exchange type and amphoteric ion exchange type being particularly suitable for adsorbing chloride ions.
[0049] The encapsulating resin composition of the present invention may contain a solvent for the purpose of adjusting the viscosity or the like. However, there is a risk of problems such as outgassing due to the remaining solvent, or deterioration of the organic light-emitting material layer when used as a encapsulant for an organic EL display element. Therefore, it is preferable that the encapsulating resin composition does not contain a solvent or that the solvent content is 0.05 mass % or less.
[0050] Furthermore, the encapsulating resin composition of the present invention may contain various known additives, such as a curing retarder, a reinforcing agent, a softener, a plasticizer, a viscosity modifier, an ultraviolet absorber, and an antioxidant, as necessary.
[0051] The encapsulating resin composition of the present invention has an upper limit of 2000 mPa·s in viscosity measured at 25°C using an E-type viscometer. When the viscosity is 2000 mPa·s or less, the resulting encapsulating resin composition has excellent coatability and handleability. The upper limit of the viscosity is preferably 1500 mPa·s, and more preferably 1000 mPa·s. From the viewpoint of maintaining the applied shape, the lower limit of the viscosity of the encapsulating resin composition of the present invention is preferably 20 mPa·s, and more preferably 50 mPa·s. The viscosity of the encapsulating resin composition can be measured, for example, using an E-type viscometer at a rotation speed of 1 rpm or 10 rpm. Examples of the E-type viscometer include VISCOMETER TV-22 (manufactured by Toki Sangyo Co., Ltd.), and the viscosity can be measured using a No. 1 rotor.
[0052] The encapsulating resin composition of the present invention has a lower limit of the refractive index of the sodium D line at 25°C of the cured product of 1.60. When the cured product has a refractive index of 1.60 or more and is used as a sealant for a display device such as an organic EL display device, the difference in refractive index between the electrode or passivation film is small, and as a result, the display device obtained has excellent light extraction efficiency. The preferred lower limit of the refractive index of the cured product is 1.61. Although there is no particular upper limit to the refractive index, the substantial upper limit is 1.90. The above-mentioned "refractive index of sodium D line" can be measured using an Abbe refractometer. The refractive index of the cured product to be measured is, for example, a measurement piece having a length of 20 mm, a width of 10 mm, and a thickness of 100 μm. The refractive index of the cured product to be measured is measured by irradiating the encapsulating resin composition with light having an absorption wavelength of the photopolymerization initiator at an illuminance of 10 to 1000 mW / cm. 2 (Preferably 80-120mW / cm 2 ), Accumulated light intensity 500~5000mJ / cm 2 (Preferably 1000 to 3000 mJ / cm 2 As a light source for irradiating the light, for example, a metal halide lamp, an LED light source, etc. can be used.
[0053] The encapsulating resin composition of the present invention can be suitably used as an encapsulant for an organic EL display element. The encapsulating resin composition of the present invention also constitutes the present invention.
[0054] The sealant for an organic EL display device of the present invention is particularly suitably used as an in-plane sealant that covers and seals a laminate having an organic light-emitting material layer. The sealant for an organic EL display device of the present invention is also suitable for use in sealing a top-emission type organic EL display device.
[0055] Examples of a method for sealing an organic EL display element using the sealant for an organic EL display element of the present invention include a method having a step of applying the sealant for an organic EL display element of the present invention to a substrate by printing, a dispensing method, an inkjet method or the like, and a step of curing the applied sealant for an organic EL display element by light irradiation.
[0056] In the step of applying the sealant for an organic EL display element of the present invention to a substrate, the sealant for an organic EL display element of the present invention may be applied to the entire surface of the substrate, or may be applied to a part of the substrate. The shape of the sealing part of the sealant for an organic EL display element of the present invention formed by application is not particularly limited as long as it is a shape that can protect the laminate having the organic light-emitting material layer from the outside air, and may be a shape that completely covers the laminate, a closed pattern may be formed on the periphery of the laminate, or a pattern with a shape that is partially provided with an opening on the periphery of the laminate may be formed.
[0057] In the step of curing the sealant for an organic EL display element of the present invention by light irradiation, the sealant for an organic EL display element of the present invention is cured by irradiating light having an illuminance of 10 to 1000 mW / cm with light that matches the absorption wavelength of the photopolymerization initiator. 2 (Preferably 80-120mW / cm 2 ), Accumulated light intensity 500~5000mJ / cm 2 (Preferably 1000 to 3000 mJ / cm 2 ) to allow the resin to be cured appropriately.
[0058] Examples of light sources used for the light irradiation include low pressure mercury lamps, medium pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, excimer lasers, chemical lamps, black light lamps, microwave excited mercury lamps, metal halide lamps, sodium lamps, halogen lamps, xenon lamps, LED lamps, fluorescent lamps, sunlight, electron beam irradiation devices, etc. These light sources may be used alone or in combination of two or more. These light sources are appropriately selected in accordance with the absorption wavelength of the photopolymerization initiator.
[0059] Examples of the means for irradiating the sealant for an organic EL display element of the present invention with light include simultaneous irradiation from various light sources, sequential irradiation with a time lag, and a combination of simultaneous irradiation and sequential irradiation, and any of the irradiation means may be used.
[0060] The cured product obtained by the step of curing the sealant for an organic EL display element by at least one of heating and light irradiation may be further covered with an inorganic material film. As the inorganic material constituting the inorganic material film, a conventionally known material can be used. For example, silicon nitride (SiN x ) and silicon oxide (SiO x The inorganic material film may be a single layer or a laminate of a plurality of layers. The inorganic material film and a resin film composed of the sealant for an organic EL display element of the present invention may be alternately repeated to cover the laminate.
[0061] The method for producing the organic EL display element may include a step of bonding a substrate coated with the sealant for an organic EL display element of the present invention (hereinafter also referred to as "one substrate") to another substrate. The one substrate may be a substrate on which a laminate having an organic light-emitting material layer is formed, or may be a substrate on which no such laminate is formed. When the one substrate is a substrate on which the laminate is not formed, the sealant for an organic EL display element of the present invention may be applied to the one substrate so that the laminate can be protected from the outside air when the other substrate is bonded to the substrate. That is, the sealant may be applied to the entire surface of the area where the laminate will be located when the other substrate is bonded to the substrate, or a sealing part having a closed pattern may be formed in a shape that completely fits the area where the laminate will be located when the other substrate is bonded to the substrate. Also, as a method for sealing the organic EL display element, a so-called dam-fill sealing method may be used. That is, first, a curable paste is applied to the substrate of the organic EL display element so as to surround the periphery of the display part. Next, the sealant for organic EL display element of the present invention is applied inside the applied curable paste, and the opposing sealing substrate is bonded while the sealant is prevented from protruding by the curable paste on the periphery. Then, a method may be used in which the curable paste on the periphery and the sealant for organic EL display element of the present invention that has been pressed and spread inward are cured by at least one of heating and light irradiation.
[0062] The step of curing the sealant for an organic EL display element by at least one of heating and light irradiation may be performed before the step of bonding the one substrate to the other substrate, or may be performed after the step of bonding the one substrate to the other substrate. When the step of curing the sealant for an organic EL display element by at least one of heating and light irradiation is carried out before the step of bonding the one substrate and the other substrate, the sealant for an organic EL display element of the present invention preferably has a pot life of 1 minute or more from the time of at least one of heating and light irradiation until the curing reaction progresses and adhesion becomes impossible. By having the pot life of 1 minute or more, it is possible to obtain a higher adhesive strength without excessive curing progress before bonding the one substrate and the other substrate.
[0063] In the step of bonding the one substrate to the other substrate, the method for bonding the one substrate to the other substrate is not particularly limited, but it is preferable to bond the substrate to the other substrate in a reduced pressure atmosphere. The preferred lower limit of the degree of vacuum under the reduced pressure atmosphere is 0.01 kPa, and the preferred upper limit is 10 kPa. When the degree of vacuum under the reduced pressure atmosphere is within this range, it is possible to more efficiently remove air bubbles in the sealant for an organic EL display element of the present invention when bonding the one substrate and the other substrate, without spending a long time to achieve a vacuum state due to the airtightness of the vacuum device or the capacity of the vacuum pump. Effect of the Invention
[0064] According to the present invention, it is possible to provide an encapsulating resin composition that has excellent fast curing properties and handleability, and the cured product has a high refractive index. Also, according to the present invention, it is possible to provide a sealant for an organic EL display element that contains the encapsulating resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0065] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0066] (Preparation of compound represented by formula (1)) In a flask, o-phenylphenol glycidyl ether (manufactured by Yokkaichi Chemical Co., Ltd., "OPP-EP") was dissolved in a mixed solvent of toluene and methanol, and 1.2 equivalents of thiourea was added to the o-phenylphenol glycidyl ether, followed by reaction for 5 hours at 40°C in a nitrogen atmosphere. Next, extraction with acetic acid and saturated saline was performed twice. After that, the mixture was dehydrated with magnesium sulfate, and the solvent was distilled off under reduced pressure to obtain the compound represented by the above formula (1).
[0067] (Preparation of compound represented by formula (2)) In a flask, 1,6-bis(glycidyloxy)naphthalene (DIC Corporation, "EPICLON HP-4032SS") was dissolved in a mixed solvent of toluene and methanol, and 1.2 equivalents of thiourea was added to the 1,6-bis(glycidyloxy)naphthalene, followed by reaction for 5 hours at 40°C in a nitrogen atmosphere. Next, extraction with acetic acid and saturated saline was performed twice. Thereafter, the mixture was dehydrated with magnesium sulfate, and the solvent was distilled off under reduced pressure to obtain the compound represented by the above formula (2).
[0068] (Examples 1 to 5, Comparative Examples 1 to 6) Each of the encapsulating resin compositions of Examples 1 to 5 and Comparative Examples 1 to 6 was prepared by stirring and mixing each material at a stirring speed of 2000 rpm using a stirring mixer according to the compounding ratios shown in Table 1. The stirring mixer used was an AR-250 (manufactured by Thinky Corporation).
[0069] (viscosity) The viscosity of each of the encapsulating resin compositions obtained in the Examples and Comparative Examples was measured at 25° C. using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd., "VISCOMETER TV-22"). The encapsulating resin compositions obtained in Examples 1 to 5 and Comparative Examples 3 to 6 were measured at a rotation speed of 10 rpm using rotor No. 1, and the encapsulating resin compositions obtained in Comparative Examples 1 and 2 were measured at a rotation speed of 1 rpm using rotor No. 1. The viscosity measurement results are shown in Table 1.
[0070] (Refractive index of cured product) A mold was prepared by cutting out a silicone rubber sheet having a thickness of 100 μm into a rectangle having a length of 20 mm and a width of 10 mm. This mold was placed on a release PET film, and the encapsulating resin composition obtained in each of the Examples and Comparative Examples was filled into the mold. Another release PET film was then placed on top of the mold so as to eliminate any air bubbles, thereby obtaining a laminate. The obtained laminate was sandwiched between two glass plates and fixed, and a UV-LED was used to illuminate the laminate at a wavelength of 365 nm and an illuminance of 100 mW / cm. 2 The cumulative amount of ultraviolet light is 3000mJ / cm 2 The encapsulating resin composition was cured by irradiating the silicone rubber sheet with light so that the cured encapsulating resin composition was cured. Thereafter, the PET film was peeled off, and the cured encapsulating resin composition was taken out from the silicone rubber sheet to obtain a test piece having a length of 10 mm, a width of 20 mm, and a thickness of 100 μm. The refractive index of the sodium D line of the obtained test piece at 25° C. was measured using an Abbe refractometer. As the Abbe refractometer, NAR-4T (manufactured by Atago Co., Ltd.) was used. The measurement results of the refractive index are shown in Table 1.
[0071] <Evaluation> The encapsulating resin compositions obtained in the Examples and Comparative Examples were evaluated as follows, and the results are shown in Table 1.
[0072] (Handling) Each of the encapsulating resin compositions obtained in the Examples and Comparative Examples was filled into a 10 mL syringe (manufactured by Musashi Engineering Co., Ltd.). A precision nozzle (manufactured by Musashi Engineering Co., Ltd., nozzle tip diameter 0.3 mm) was attached to the tip of the syringe, and the encapsulating resin composition was applied onto a glass substrate using a dispenser device (manufactured by Musashi Engineering Co., Ltd., "SHOT MASTER300") under conditions of a discharge pressure of 0.4 MPa, a gap between the semiconductor chip and the needle of 200 μm, and an average application amount of 5 mg. The handling properties were evaluated by rating "O" when the coating variation was within ±0.5 mg, and rating "X" when the coating variation was greater than ±0.5 mg.
[0073] (curable) 0.3 g of each of the encapsulating resin compositions obtained in the Examples and Comparative Examples was dropped onto a glass substrate. Then, the encapsulating resin composition on the glass substrate was irradiated with a UV-LED at a wavelength of 365 nm and an illuminance of 100 mW / cm. 2 The cumulative amount of ultraviolet light is 3000mJ / cm 2 After the light irradiation, the curable resin composition was examined to see whether it was cured and whether it had surface tack or adhesion. The curability was evaluated as follows: if the composition cured but had no surface tack or stickiness, it was rated as "○"; if the composition cured but had surface tack or stickiness, it was rated as "△"; if the composition did not cure, it was rated as "×".
[0074] (Fast curing) For each of the encapsulating resin compositions obtained in the Examples and Comparative Examples, the gelation time at 170° C. was determined in accordance with JIS C2161B. The rapid curing property was evaluated as follows: a gelation time of less than 5 seconds was rated as "O", a gelation time of 5 to less than 8 seconds was rated as "Δ", and a gelation time of 8 seconds or more was rated as "X".
[0075] [Table 1] [Industrial Applicability]
[0076] According to the present invention, it is possible to provide an encapsulating resin composition that has excellent fast curing properties and handleability, and the cured product has a high refractive index. Also, according to the present invention, it is possible to provide a sealant for an organic EL display element that contains the encapsulating resin composition.
Claims
1. An encapsulating resin composition comprising a curable resin and a photopolymerization initiator, the curable resin contains an episulfide compound having one or more episulfide groups and one or more aromatic rings in one molecule, The encapsulating resin composition has a viscosity of 2000 mPa·s or less as measured at 25° C. using an E-type viscometer, and a refractive index of the cured product at 25° C. with respect to sodium D lines of 1.60 or more.
1. An encapsulating resin composition comprising:
2. 2. The encapsulating resin composition according to claim 1, wherein the episulfide compound is a compound having one episulfide group and one or more aromatic rings in one molecule.
3. 3. The encapsulating resin composition according to claim 1, wherein the episulfide compound is present in an amount of 40 parts by mass or more per 100 parts by mass of the curable resin.
4. The encapsulating resin composition according to claim 1 , wherein the curable resin further comprises an epoxy compound.
5. The encapsulating resin composition according to claim 1 or 2, wherein the photopolymerization initiator is a cationic photopolymerization initiator.
6. A sealant for an organic EL display element, comprising the encapsulating resin composition according to claim 1 or 2.
Citation Information
Patent Citations
Organic electroluminescent display device and method of manufacturing same
JP2007115692A