Polyester film

A polyester film with a crystal nucleating agent and polybutylene terephthalate addresses surface irregularity control, enhancing smoothness and scratch resistance for thinner ceramic green sheets, improving productivity in multilayer ceramic capacitors.

JP2024139258APending Publication Date: 2024-10-09MITSUBISHI CHEM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023050119
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Conventional polyester films used as supports for ceramic green sheets in multilayer ceramic capacitors face challenges in achieving precise control of surface irregularities, leading to issues such as pinholes and reduced productivity as ceramic green sheets become thinner.

Method used

A polyester film with a specific configuration containing a crystal nucleating agent and polybutylene terephthalate on one surface, with controlled average surface roughness and limited large protrusions, enhances smoothness and scratch resistance, allowing for longer film rolls and thinner ceramic green sheets.

Benefits of technology

The film achieves high smoothness and excellent scratch prevention, enabling the production of thinner ceramic green sheets with reduced defects, thus improving productivity and suitability for multilayer ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139258000001_ABST
    Figure 2024139258000001_ABST
Patent Text Reader

Abstract

To provide a polyester film which has high smoothness by controlling fine irregularities on the surface of the polyester film, has excellent scratch preventing properties, can accommodate long-sized polyester films to improve productivity, and can accommodate the film thinning of a ceramic green sheet during production of the ceramic green sheet.SOLUTION: One surface (A) of a polyester film contains a crystal nucleating agent and polybutylene terephthalate. The surface (A) satisfies the following (1) and (2). (1) The average surface roughness (Sa) is 2.0 to 10 nm. (2) The percentage of the number of protrusions having a size of 50 nm or more is 0.2% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester film suitable as a support for a release film for use in the production process of a multilayer ceramic capacitor. [Background technology]

[0002] In recent years, with the increasing use of electrical equipment in automobiles and the increasing functionality of smartphones, multi-layered ceramic capacitors (MLCCs) have become increasingly smaller and have higher capacitance. The multilayer ceramic capacitor is manufactured as follows. First, a ceramic slurry containing ceramic components and a binder resin is applied onto a release film and dried to produce a ceramic green sheet (dielectric sheet), on which electrodes are printed by screen printing or the like to form internal electrodes, and after drying, the printed ceramic green sheet is peeled off from the release film and multiple such green sheets are stacked. The stacked green sheets are pressed together and then cut into individual chips. Thereafter, the internal electrodes and the dielectric layers are sintered in a firing furnace to produce a multilayer ceramic capacitor.

[0003] Ceramic green sheets are becoming thinner as MLCCs become smaller and higher capacity. When ceramic green sheets are further thinned to 0.5 μm (thickness after drying) or less, if there are minute protrusions on the surface of the release film used as a carrier film, these will cause pinholes and the like to form in the ceramic green sheets. For this reason, the release film is required to have a higher degree of surface smoothness.

[0004] Conventionally, as a support for this type of release film, Patent Document 1 discloses a support having a substrate having a first surface and a second surface, a smoothing layer provided on the first surface side of the substrate, and a release agent layer provided on the surface side of the smoothing layer opposite the substrate, the smoothing layer being formed by heating and curing a smoothing layer-forming composition containing a thermosetting compound having a weight-average molecular weight of 950 or less, and the arithmetic mean roughness Ra of the outer surface of the release agent layer being 100 mm or less. 1 is 8 nm or less, and the maximum protrusion height Rp of the outer surface of the release agent layer 1 A release film for producing a ceramic green sheet is disclosed, characterized in that the surface roughness is 50 nm or less.

[0005] In addition, Patent Document 2 describes a polyester film for release that is excellent in surface smoothness and has few fine defects on the film surface, and has a number of depression defects of 0.5 μm or more in depth of 5 / m 2 and at least one surface of the film has a center line average roughness SRa of 15 to 35 nm and a ten-point average roughness SRz of 1000 nm or less.

[0006] In addition, Patent Document 3 discloses a polyester film roll obtained by winding up a polyester film, in which slack defects present in the polyester film are reduced within 100 m. 2 No. 5,513,233 is disclosed. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2014-177093 A [Patent Document 2] JP 2013-7054 A [Patent Document 3] JP 2018-90803 A Summary of the Invention [Problem to be solved by the invention]

[0008] Conventionally, the state of the film surface was controlled by forming fine irregularities by adjusting the type of particles used, the average particle size, the amount added, etc. However, as ceramic green sheets are now being made thinner, more precise control of irregularities is required, and there are limitations to the control of the film surface state using conventional particles. For this reason, there is a demand for polyester films that allow precise design of the film surface irregularities, have minimal loss when switching between raw materials, and can be produced continuously over long periods of time, thereby contributing to improved productivity.

[0009] Therefore, an object of the present invention is to provide a polyester film having a controlled fine unevenness on the surface thereof, high smoothness, excellent scratch resistance, and capable of improving productivity by adapting to longer polyester rolls, and further capable of adapting to thinner ceramic green sheets during production of the ceramic green sheets. [Means for solving the problem]

[0010] In view of the above-mentioned circumstances, the present inventors have conducted extensive research and found that the above-mentioned problems can be easily solved by using a polyester film having a specific structure, and have completed the present invention. That is, the present invention provides the following items [1] to

[11] .

[0011] [1] A polyester film, one surface (A) of which contains a crystal nucleating agent and polybutylene terephthalate, and said surface (A) satisfies the following (1) and (2): (1) The average surface roughness (Sa) is 2.0 to 10 nm. (2) The percentage of protrusions larger than 50 nm is 0.2% or less. [2] The polyester film according to the above [1], wherein the crystal nucleating agent is a fatty acid metal salt represented by the following general formula (I): (CH 3 (CH 2 ) n COO) m M (I) (In the above formula (I), n is an integer of 4 or more, and M is Na, Ca, or Li. Also, m is 1 when M is Na or Li, and 2 when M is Ca.) [3] The polyester film according to the above [2], wherein the melting point of the fatty acid metal salt is 140°C or higher and 220°C or lower. [4] The polyester film according to any one of the above [1] to [3], which is a three-layer polyester film. [5] The polyester film according to the above [4], wherein the intermediate layer of the polyester film contains 50% by mass or more of recycled polyester raw materials. [6] The polyester film according to any one of the above [1] to [5], which has a surface layer C on the side opposite to the one surface (A) of the polyester film. [7] The polyester film according to the above [6], wherein the surface layer C contains two or more types of particles having different average particle sizes. [8] The polyester film according to the above [7], wherein the maximum difference in average particle size between the two or more types of particles having different average particle sizes is 0.1 μm or more. [9] The polyester film according to any one of the above [1] to [8], which has a release layer on one surface (A) of the polyester film.

[10] The polyester film according to any one of [1] to [9], which is used as a support for a ceramic green sheet in a production process of a multilayer ceramic capacitor.

[11] The polyester film according to any one of [1] to [9], which is used as a support for a ceramic green sheet in a production process of an automotive ceramic capacitor. Effect of the Invention

[0012] According to the present invention, a polyester film can be provided in which the fine irregularities on the surface of the polyester film are controlled and the polyester film has high smoothness, resulting in excellent scratch resistance, and can accommodate longer polyester rolls to improve productivity, and can also accommodate thinner ceramic green sheets during production of the ceramic green sheets. In addition, since the polyester film of the present invention has extremely excellent surface smoothness, for example, in the manufacturing process of multilayer ceramic capacitors, by using it as a support for ceramic green sheets, there is an advantage that there is little possibility of defects occurring in the ceramic green sheets due to the fine irregularities on the surface of the polyester film of the present invention.

Brief Description of the Drawings

[0013] [Figure 1] Shows the crystallization mechanism (estimated) of polyester thermodynamically by using a crystal nucleating agent in the polyester resin. [Diagram 2] Shows the mechanism (estimated) of the formation of surface irregularities by using a crystal nucleating agent during the production of the polyester film. [Diagram 3] Shows the surface state of one surface (A) of the polyester film obtained in Example 1. [Figure 4] Shows the surface state of one surface (A) of the polyester film obtained in Example 2. [Diagram 5] Shows the surface state of one surface (A) of the polyester film obtained in Example 3. [Figure 6] Shows the surface state of one surface (A) of the polyester film obtained in Comparative Example 2. [Figure 7] Shows the surface state of one surface (A) of the polyester film obtained in Comparative Example 3. [Figure 8] Shows the surface state of one surface (A) of the polyester film obtained in Reference Example 1.

Modes for Carrying Out the Invention

[0014] Hereinafter, the present invention will be described in detail. In this specification, the term "A to B" regarding the description of numerical values means "A or more and B or less" (when A < B) or "A or less and B or more" (when A > B). Also, in the present invention, a combination of preferred embodiments is a more preferred embodiment.

[0015] [Polyester film] The polyester film of the present invention is characterized in that one surface (A) contains a crystal nucleating agent, and the surface (A) satisfies the following (1) and (2). (1) The average surface roughness (Sa) is 2.0 to 10 nm. (2) The percentage of protrusions larger than 50 nm is 0.2% or less.

[0016] In the present invention, one surface (A) of the polyester film refers to the surface side on which a ceramic green sheet is laminated when the polyester film is used as a support for the ceramic green sheet in the manufacturing process of a multilayer ceramic capacitor. When the one surface (A) of the polyester film satisfies the above (1) and (2), the polyester film can be made thin, and the multilayer capacitor can be manufactured in a suitable state. In addition, from the viewpoint of using the polyester film as a support for the ceramic green sheet, the one surface (A) of the polyester film is suitable as a surface on which a release layer described later is provided.

[0017] The polyester film of the present invention has the above-mentioned configuration, and since the fine irregularities on the surface of the polyester film are controlled and the polyester film has high smoothness, it has excellent scratch resistance, can accommodate longer polyester films, thereby improving productivity, and can also accommodate thinner ceramic green sheets during production of the ceramic green sheets. The reason why the polyester film of the present invention can achieve the above-mentioned effect can be presumed as follows. That is, it is considered that when one surface (A) of the polyester film contains a crystal nucleating agent represented by the following general formula (I), the crystal nucleating agent suppresses the aggregation of polyester in the molten polyester raw material during the production of the polyester film, and allows the crystals to be present uniformly. Furthermore, as shown in FIG. 1, the crystallization speed of polyester in the polyester film can be increased, and the size of the formed crystals can be reduced. Therefore, the polyester film of the present invention can control the fine unevenness of the surface of the polyester film, and as a result, one surface (A) of the polyester film can satisfy the above (1) and (2), and the polyester film can have high smoothness and excellent scratch resistance. In addition, since the polyester film of the present invention has the above-mentioned configuration, the occurrence of wrinkles and pinholes during the production of the polyester film can be suppressed, and the polyester film can be made longer, thereby improving productivity. Furthermore, since one surface (A) of the polyester film of the present invention has the above-mentioned configuration, the occurrence of pinholes due to surface unevenness can be suppressed, making it possible to accommodate thinner ceramic green sheets and to produce multilayer capacitors under optimal conditions.

[0018] As described above, the polyester film of the present invention has the above-mentioned configuration, which enables more precise control of the uneven shape of the film surface, and can be suitably used for the production of multilayer ceramic capacitors, and can be particularly suitably used in situations where it is necessary to form thin ceramic green sheets having a thickness (after drying) of 0.5 μm or less.

[0019] The polyester film of the present invention can be stored in the form of a roll of polyester film obtained by winding up the polyester film. The polyester film roll is a polyester film roll wound around a core such as a paper tube, a metal tube, a plastic tube, etc., and has a width of preferably 0.2 m or more, more preferably 0.3 m or more, particularly preferably 1.0 m or more, and most preferably 1.5 m or more. The upper limit of the film width is not particularly limited, but is preferably 2.3 m or less, more preferably 2.0 m or less, from the viewpoint of handleability. The length of the present film wound onto the polyester film roll is not particularly limited, but is preferably 1000 m or more, more preferably 6000 m or more, and even more preferably 12000 m or more. Furthermore, the thickness of the present film is preferably from 9 μm to 38 μm, more preferably from 9 μm to 32 μm, and particularly from 9 μm to 25 μm.

[0020] (Surface properties) In the present invention, one surface (A) of the polyester film is characterized by satisfying the following (1) and (2). (1) The average surface roughness (Sa) is 2.0 to 10 nm. (2) The percentage of protrusions larger than 50 nm is 0.2% or less.

[0021] (1) Average surface roughness (Sa) In the present invention, the average surface roughness (Sa) of one surface (A) of the polyester film is required to be 2.0 to 10 nm. When the average surface roughness (Sa) of one surface (A) of the polyester film is greater than 10 nm, defects such as pinholes are likely to occur due to fine irregularities on the polyester film surface, the scratch resistance is reduced, and the polyester film cannot be made longer and the ceramic green sheet cannot be made thinner. On the other hand, when the average surface roughness (Sa) is less than 2.0 nm, the film surface becomes too flat, the film has poor slipperiness, and is easily scratched, so the scratch resistance is reduced and the polyester film cannot be made longer. In the present invention, the average surface roughness (Sa) of one surface (A) of the polyester film is preferably 2.0 to 8 nm, more preferably 2.5 to 8 nm, and even more preferably 3.0 to 8 nm, from the viewpoints of improving scratch resistance and of responding to longer polyester films and thinner ceramic green sheets.

[0022] The average surface roughness (Sa) is one of the surface roughness parameters (ISO 25178), and is a three-dimensional extension of the two-dimensional Ra. It is calculated by dividing the volume enclosed by the surface profile and the average surface by the measured area, and is calculated by the following formula (i). When the surface is the XY plane and the height direction is the Z axis, A is the defined area (the entire image), and Z(x,y) is the height of the image point (x,y) from the plane with height 0, then it is expressed as in the following formula (1).

[0023]

number

[0024] (2) Proportion of protrusions of 50 nm or more In the present invention, one surface (A) of the polyester film has a ratio of the number of protrusions of 50 nm or more of 0.2% or less, more preferably 0.1% or less, and even more preferably 0.0%. By keeping the number of protrusions within the above range, a polyester film having a smoother surface can be obtained, scratch resistance can be reduced, and it can accommodate longer polyester films and thinner ceramic green sheets. The number of protrusions can be specifically measured by the method described in the Examples.

[0025] In the present invention, the surface properties of one surface (A) of the polyester film can be adjusted, for example, by adjusting the type and content of a crystal nucleating agent, adjusting the content of polybutylene terephthalate (PBT), or controlling the conditions of the cooling roll during production of the polyester film.

[0026] (Maximum mountain height (Sp)) In the present invention, the maximum peak height (Sp) of one surface (A) of the polyester film is preferably 200 nm or less. When the maximum peak height (Sp) of one surface (A) of the polyester film is 200 nm or less, defects such as pinholes due to fine irregularities on the polyester film surface are unlikely to occur, scratch resistance is improved, and the polyester film can be made longer and the ceramic green sheet can be made thinner. In the present invention, the maximum peak height (Sp) of one surface (A) of the polyester film is preferably 190 nm or less, more preferably 180 nm or less, from the viewpoint of improving scratch prevention and responding to longer polyester films and thinner ceramic green sheets. The lower limit of the maximum peak height (Sp) is not particularly limited, but is preferably 5 nm or more, more preferably 10 nm or more, and even more preferably 15 nm or more, from the viewpoint of improving winding properties of the polyester film.

[0027] The maximum peak height (Sp) is one of the surface roughness parameters (ISO 25178), and represents the maximum value of the height from the average plane of the surface, and is expressed by the following formula (ii).

[0028]

number

[0029] In the present invention, the relationship Sp / Sa between the average surface roughness (Sa) and the maximum peak height (Sp) of one surface (A) of the polyester film is preferably 50 or less, more preferably 40 or less, and even more preferably 30 or less. By making the relationship between the average surface roughness (Sa) and the maximum peak height (Sp), Sp / Sa, 50 or less, it is possible to achieve a balance between a high average surface roughness (Sa) and a low maximum peak height (Sp), making it easier to form thin ceramic green sheets, and thus enabling the production of thinner ceramic green sheets. In addition, the lower limit of the relationship Sp / Sa between the average surface roughness (Sa) and the maximum peak height (Sp) is not particularly limited, but from the viewpoint of adjusting the balance between high Sa and low Sp, it is preferably 3 or more, more preferably 5 or more, and particularly preferably 10 or more.

[0030] (Nucleating agent) The crystal nucleating agent used in the present invention is preferably a fatty acid metal salt represented by the following general formula (I), from the viewpoints of promoting the crystallization of the polyester resin, controlling the unevenness of the polyester film surface, and ensuring that one surface (A) of the polyester film satisfies the above (1) and (2). (CH 3 (CH 2 ) n COO) m M (I) (In the above formula, n is an integer of 4 or more, and M is Na, Ca, or Li. Also, m is 1 when M is Na or Li, and 2 when M is Ca.)

[0031] In the above general formula (I), M represents a metal ion in the fatty acid metal salt, and is any one of Na, Ca, and Li, and is preferably Na. By using any one of Na, Ca, and Li as the metal ion, it is possible to suppress a decrease in the molecular weight of the polyester resin due to heat retention during the production of the polyester film, and it is possible to accommodate long polyester films.

[0032] In the above general formula (I), n is an integer of 4 or more, preferably 6 to 35, more preferably 8 to 33, even more preferably 10 to 30, and even more preferably 15 to 28. In general formula (I), when n is within the above range, the compatibility between the crystal nucleating agent and the polyester resin can be improved, and the polyester film can be made longer and the ceramic green sheet can be made thinner. In the fatty acid metal salt represented by the above general formula (I), specific examples of the fatty acid include caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, tridecanoic acid, myristic acid, pentadecanoic acid, palmitic acid, margaric acid, stearic acid, nonadecanoic acid, arachic acid, behenic acid, and montanic acid, and among these, montanic acid is preferred.

[0033] In the present invention, the melting point of the fatty acid metal salt used as the crystal nucleating agent is preferably 140°C or more and 220°C or less, more preferably 150°C or more and 210°C or less, and even more preferably 160°C or more and 200°C or less. When the fatty acid metal salt has a melting point of 220°C or less, the maximum peak height (Sp) of the polyester film surface can be prevented from becoming too large, and when the melting point is 140°C or more, fine irregularities can be formed on one surface (A) of the polyester film. Therefore, the above (1) and (2) can be easily satisfied, and the scratch prevention property can be improved and it is easy to deal with the long polyester film and the thin ceramic green sheet. In the present invention, the melting point of the fatty acid metal salt can be measured by TG-DTA, specifically, by the method described in the Examples.

[0034] From the viewpoint of improving handling, the amount of the crystal nucleating agent is preferably 2000 ppm or more, more preferably 3000 ppm or more and 28000 ppm or less, even more preferably 5000 ppm or more and 25000 ppm or less, and even more preferably 5000 ppm or more and 20000 ppm or less, by mass ratio relative to the film.

[0035] The above crystal nucleating agents may be used alone or in combination of two or more kinds.

[0036] (polyester) In the present invention, the polyester refers to a polyester that is a raw material for a polyester film, and refers to a polymer compound having continuous ester bonds in the main chain. In the present invention, the polyester may be a homopolyester or a copolymer polyester, and specifically, a polyester obtained by polycondensation reaction of a dicarboxylic acid component and a diol component can be mentioned.

[0037] In the present invention, it is preferable to use a polyester containing more than 50 mol % of an aromatic dicarboxylic acid or an aliphatic dicarboxylic acid when the dicarboxylic acid component is taken as 100 mol %.

[0038] Examples of the dicarboxylic acid component include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, and 4,4'-diphenylsulfonedicarboxylic acid, and aliphatic dicarboxylic acids such as adipic acid, suberic acid, sebacic acid, dimer acid, dodecanedioic acid, cyclohexanedicarboxylic acid, and ester derivatives thereof.

[0039] Examples of the diol component include ethylene glycol, 1,2-propanediol, 1,3-propanediol, neopentyl glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-hexanedimethanol, diethylene glycol, triethylene glycol, polyalkylene glycol, 2,2-bis(4-hydroxyethoxyphenyl)propane, isosorbate, and spiroglycol.

[0040] When the polyester is a homopolyester, it is preferably one obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of the aromatic dicarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid, and examples of the aliphatic glycol include ethylene glycol, diethylene glycol, 1,3-butanediol, 1,4-butanediol, and 1,4-cyclohexanedimethanol. Representative examples of polyester include polyethylene terephthalate (PET), polyethylene-2,6-naphthalenedicarboxylate (PEN), polybutylene terephthalate (PBT), and the like.

[0041] On the other hand, when the polyester is a copolymer polyester, it is preferable that the polyester is a copolymer containing 30 mol % or less of a third component. The third component is a component other than the compound that is the main component of the dicarboxylic acid component constituting the polyester and the compound that is the main component of the diol component, and in the case of polyethylene terephthalate, it is a component other than terephthalic acid and ethylene glycol. Examples of the dicarboxylic acid component of the copolymer polyester include isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, and oxycarboxylic acid, and the like, which may be used alone or in combination. Examples of the glycol component of the copolymer polyester include one or more of ethylene glycol, diethylene glycol, propylene glycol, butanediol, 1,4-cyclohexanedimethanol, and neopentyl glycol.

[0042] As the polyester, preferred are polyethylene terephthalate in which 80 mol % or more, preferably 90 mol % or more, is an ethylene terephthalate unit, and polyethylene-2,6-naphthalate in which ethylene-2,6-naphthalate unit is, and the like.

[0043] <Polybutylene terephthalate> In the present invention, in order to impart a fine uneven shape, it is necessary to use polybutylene terephthalate in the surface layer A together with the crystal nucleating agent. The polyester mainly composed of polybutylene terephthalate in the present invention is not limited to a homopolybutylene terephthalate resin consisting only of butylene terephthalate units, but may be a copolymer containing 80 mol % or more, preferably 90 mol % or more, and even 95 mol % or more of butylene terephthalate units. In the present invention, a copolymer containing 90 mol% or more of butylene terephthalate units is preferable, and homopolybutylene terephthalate is particularly preferable. If the content of butylene terephthalate units is 80 mol% or more, a sufficient crystallization speed is obtained, and when combined with a crystal nucleating agent, a desired uneven shape is easily formed. In the present invention, it is possible to obtain a concave-convex shape that cannot be obtained by using either a crystal nucleating agent or polybutylene terephthalate (PBT) alone by using both of them in combination. Although the details of the mechanism are unknown, it is speculated that both have fast crystallization rates, and furthermore, due to the difference in crystallization rates between the two, they have the advantage of being able to maintain a high level of smoothness while still being able to adjust the uneven shape over a wide range.

[0044] <Polyester polycondensation catalyst> Examples of the polycondensation catalyst used in polycondensing the polyester include antimony compounds, germanium compounds, aluminum compounds, titanium compounds, etc. Among these, at least one of antimony compounds and titanium compounds is preferred, and it is particularly preferred to use a polyester obtained by using a titanium compound. Therefore, the polyester film preferably contains at least one of an antimony compound and a titanium compound, and more preferably contains a titanium compound. By using the titanium compound, the number of metal-containing aggregates, so-called coarse foreign matter, originating from the titanium compound in the film can be reduced, and a film having high surface smoothness, in particular a small maximum peak height (Sp) on at least one side, can be obtained.

[0045] It is preferable that the polyester constituting the outermost layer of the present film (also called the "surface layer", for example, one surface (A) of a polyester film, or the surface layer onto which a release layer is laminated) uses a titanium compound as its polycondensation catalyst. The content of titanium element derived from the titanium compound in the outermost layer is preferably 3 ppm or more and 40 ppm or less, and more preferably 4 ppm or more and 35 ppm or less. Within the above range, it is possible to reduce the amount of foreign matter caused by the catalyst without decreasing the production efficiency of the polyester. When the polyester film is a laminated polyester film, it is preferable from the viewpoint of productivity that the polyester constituting the intermediate layer described below does not use a titanium compound as a polycondensation catalyst. From the same viewpoint, the content of antimony compounds in the outermost layer of the present film is preferably 100 ppm or less. For example, the surface layer A described below contains at least one of an antimony compound and a titanium compound, and the content of the antimony compound in the surface layer A is preferably 100 ppm or less. In this case, the surface layer A does not necessarily need to contain an antimony compound.

[0046] <Intrinsic viscosity of polyester (IV)> The intrinsic viscosity (IV) of the polyester constituting the polyester film of the present invention is preferably 0.50 dL / g or more, more preferably 0.55 dL / g or more, and even more preferably 0.60 dL / g or more. In the present invention, by using a polyester having an intrinsic viscosity (IV) of 0.50 dL / g or more as the polyester constituting the polyester film, the shear stress during kneading of the polyester increases, the crystal nucleating agent in the polyester resin is easily highly dispersed, and the surface characteristics of one surface (A) of the polyester film can be easily adjusted to the above range. In addition, the upper limit of the intrinsic viscosity (IV) of the polyester is preferably 1.00 dL / g or less, more preferably 0.85 dL / g or less, and even more preferably 0.75 dL / g or less, from the viewpoint of the fluidity of the crystal nucleating agent.

[0047] From the same viewpoint as above, when the polyester film of the present invention has a laminated structure, the intrinsic viscosity (IV) of the polyester constituting the surface layer, specifically the outermost layer of the present film (for example, one surface (A) of the polyester film, the surface layer on which the release layer is laminated) is preferably 0.50 dL / g or more, more preferably 0.55 dL / g or more, and even more preferably 0.60 dL / g or more. From the viewpoint of the fluidity of the crystal nucleating agent, the upper limit of the intrinsic viscosity (IV) of the polyester constituting the surface layer is preferably 1.00 dL / g or less, more preferably 0.85 dL / g or less, and even more preferably 0.75 dL / g or less.

[0048] In addition, when two or more polyesters with different intrinsic viscosities (IV) are used, the "intrinsic viscosity (IV) of the polyester constituting the present film" refers to the intrinsic viscosity (IV) of the mixed resin.

[0049] (Structure of polyester film) In the present invention, the polyester film may be a single-layer polyester film or a laminated polyester film having two or more layers. For example, in the case of a single-layer polyester film, by setting the film thickness to 9 μm or more and 38 μm or less, and by setting the crystal nucleating agent and polybutylene terephthalate in a predetermined blend ratio and setting an appropriate line speed, it is possible to ensure the slow cooling time, and the desired uneven shape can be formed by utilizing the difference in crystallization rate between the crystal nucleating agent and polybutylene terephthalate on the film surface. In the present invention, the polyester film is preferably a laminated polyester film having two or more layers, more preferably a three-layer polyester film, from the viewpoint of easily controlling the surface properties of one surface (A) within the above range. In the present invention, when the polyester film is a laminated polyester film having two or more layers, a three-layer structure of A / B / C structure consisting of a surface layer A, an intermediate layer B and a surface layer C is preferred.

[0050] In the present invention, when the polyester film is a laminated polyester film having two or more layers, the surface layer A preferably contains the above-mentioned crystal nucleating agent and polybutylene terephthalate (PBT). Here, the above-mentioned surface layer A is a surface layer forming one surface (A) of the polyester film in the present invention, and in the laminated polyester film, by the surface layer A containing the above-mentioned crystal nucleating agent and polybutylene terephthalate (PBT), the surface properties of one surface (A) of the polyester film can be easily controlled within the above range, and scratch resistance can be improved and it is easy to accommodate longer polyester films and thinner ceramic green sheets.

[0051] The content of the crystal nucleating agent in the surface layer A is, in terms of mass ratio, preferably 2000 ppm or more, more preferably 3000 ppm or more and 28000 ppm or less, even more preferably 5000 ppm or more and 25000 ppm or less, and particularly preferably 5000 ppm or more and 20000 ppm or less, from the viewpoints of improving scratch resistance and of responding to the need for longer polyester films and thinner ceramic green sheets.

[0052] The surface layer C is a surface layer formed on the surface opposite to the surface layer A. That is, the polyester film of the present invention preferably has the surface layer C on the surface opposite to the surface layer A, i.e., one surface (A) of the polyester film. The surface layer C preferably has an average surface roughness (Sa) or a maximum peak height (Sp) equal to or greater than those of the surface layer A, and the surface layer C preferably has an average surface roughness (Sa) of 10 nm or greater or a maximum peak height (Sp) of 50 nm or greater. By having the average surface roughness (Sa) and maximum peak height (Sp) of the surface layer C within the above ranges, the surface layer C can be provided with a rough surface necessary for improving handleability.

[0053] The surface layer C preferably contains particles from the viewpoint of improving the handling properties and scratch resistance of the present film. Examples of the particles include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide; crosslinked polymers such as crosslinked silicone resin particles, crosslinked acrylic resin particles, crosslinked styrene-acrylic resin particles, and crosslinked polyester particles; and organic particles such as calcium oxalate and ion exchange resin. Among these, crosslinking molecules, silica, calcium carbonate, and aluminum oxide are preferred. In addition, the composition of the crosslinked polymer of the organic particles includes crosslinked polymer particles such as divinylbenzene polymer, ethylvinylbenzene-divinylbenzene copolymer, styrene-divinylbenzene copolymer, styrene-ethylvinylbenzene-divinylbenzene copolymer, ethylene glycol dimethacrylate polymer, styrene-ethylene glycol dimethacrylate copolymer, and methyl methacrylate-divinylbenzene copolymer. Furthermore, the crosslinked polymer particles may be composed of a system of three or more components, and are preferably copolymers of divinylbenzene, methylstyrene, methacrylic acid, and styrene. In the surface layer C, the above particles may be used alone or in combination of two or more kinds.

[0054] From the viewpoint of improving the handling properties and scratch resistance of the present film, the average particle size of the particles is preferably from 0.1 to 1.5 μm, more preferably from 0.1 to 1.2 μm, and even more preferably from 0.2 to 1.0 μm.

[0055] Moreover, it is particularly preferable that the particles have a substantially uniform average particle size with a narrow particle size distribution (so-called monodispersity). As particles having a narrow particle size distribution and a substantially uniform average particle size, when the particle size distribution of the particles is such that the particle size at which the cumulative number is 10% is D10, the particle size at which the cumulative number is 50%, and the particle size at which the cumulative number is 90% is D50, and the particle size at which the cumulative number is 90%, respectively, the ratio (D90-D10) / D50 is preferably 0.4 or less, and particularly preferably 0.2 or less. The relational expression (D90-D10) / D50 indicates the variation in particle size based on D50, and particles with (D90-D10) / D50 of 0.4 or less have a sharp particle size distribution with a small difference between D90 and D10. This can impart extremely high smoothness to the present film while maintaining excellent handleability, making it easier to improve scratch resistance. The particle size distribution of the particles is measured by a laser diffraction measuring device.

[0056] From the viewpoint of improving the handling properties and scratch resistance of the present film, the surface layer C preferably contains two or more types of particles having different average particle sizes. The maximum difference in average particle size between two or more kinds of particles having different average particle sizes is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more. By making the difference in average particle size 0.1 μm or more, the slipperiness of the polyester film surface can be easily improved, and the handling property and scratch resistance of the film can be easily improved. The upper limit of the maximum difference in average particle diameter is preferably 1.5 μm or less, more preferably 1.2 μm or less, and even more preferably 1.0 μm or less, from the viewpoint of suppressing the occurrence of pinholes due to unevenness and corresponding to the increase in length of the polyester film roll.

[0057] In addition, when the polyester film has a three-layer structure of A / B / C, it is preferable that the surface layer C has an average surface roughness (Sa) and a maximum peak height (Sp) equal to or less than those of the surface layer A, and it is preferable that the surface layer C has an average surface roughness (Sa) of 10 nm or more or a maximum peak height (Sp) of 50 nm or more.

[0058] The intermediate layer B preferably functions as the thickest main layer, and in order to reduce costs, it preferably does not substantially contain particles or contains particles at a lower concentration than the surface layer C. The particles used in the intermediate layer B may be the same as those used in the intermediate layer C described above, and the preferred ranges are also the same. The term "substantially not contained" means that it is not intentionally contained, and specifically means that the particle content (particle concentration) is 200 ppm or less, more preferably 150 ppm or less.

[0059] In the present invention, the intermediate layer B of the polyester film preferably contains 50% by mass or more of recycled polyester raw materials, more preferably 70% by mass or more, more preferably 90% by mass or more, and even more preferably 100% by mass. By containing the recycled polyester raw materials in the above range, for example, CO 2 This will reduce emissions and contribute to reducing the burden on the environment.

[0060] Furthermore, the polyester film of the present invention particularly preferably has a configuration comprising the surface layer A and / or the surface layer C shown in the following (X). By adopting such a configuration, the polyester film can have excellent handling properties and surface smoothness.

[0061] (X) Particularly preferred embodiments (1) In the above-mentioned A / B / C structure, the surface layer A contains a titanium compound, a crystal nucleating agent which is a fatty acid metal salt, and polybutylene terephthalate (PBT). (2) In the above (1), the surface layer C contains particles. (3) In either of (1) or (2), the surface layer C contains an antimony compound and / or a titanium compound, and the content of the antimony compound is 100 ppm or less. (4) In any one of (1) to (3), the particles in the surface layer C have a particle diameter of 10% of the cumulative number, D10, a particle diameter of 50% of the cumulative number, and D90, where D90 is a particle diameter of 90% of the cumulative number, and (D90-D10) / D50 is 0.4 or less. (5) In the above (4), the crystal nucleating agent is a fatty acid sodium salt.

[0062] In the above (X), by using polyester polycondensed using a titanium compound as a catalyst in each of the surface layer A and the surface layer C, it is possible to reduce foreign matter caused by the catalyst and to provide a high surface smoothness.

[0063] (Production method of polyester film) An example of a method for producing the present film will be described below. First, using a known method, raw materials, such as polyester chips, are fed into an extruder and heated to above the melting point of each polymer, the molten polymer is extruded through a die, and cooled and solidified on a rotating cooling drum to a temperature below the glass transition point of the polymer, thereby obtaining an unoriented sheet in a substantially amorphous state.

[0064] Next, the unoriented sheet is stretched in one direction by a roll or tenter type stretching machine, at a stretching temperature of usually 25 to 120° C., preferably 35 to 100° C., and a stretching ratio of usually 2.5 to 7 times, preferably 2.8 to 6 times.

[0065] Then, the film is stretched in a direction perpendicular to the first-stage stretching direction. At this time, the stretching temperature is usually 50 to 140° C., and the stretching ratio is usually 3.0 to 7 times, preferably 4.5 times or more, and more preferably 4.5 to 5.0 times.

[0066] Then, the polyester film of the present invention can be obtained as a biaxially oriented film by subsequently carrying out a heat setting treatment under tension or relaxation of 30% or less at a temperature of 180 to 220° C. This heat setting treatment may be carried out in two or more steps at different temperatures. After the heat setting treatment, the film may be cooled in a cooling zone. The cooling temperature is preferably higher than the glass transition temperature (Tg) of the polyester resin constituting the polyester film, and more specifically, is preferably in the range of 100 to 160° C. This cooling may be performed in two or more steps at different temperatures. In the above-mentioned stretching, a method in which the stretching in one direction is carried out in two or more stages can also be adopted. By combining with the above-mentioned stretching conditions, the thickness of the surface layer can be increased to further promote crystallization, thereby adjusting the uneven shape. Furthermore, by increasing the stretch ratio while increasing the thickness of the surface layer, it is also possible to make it easier to form protrusions. For example, when the present film has a thickness of 9 μm or more and 38 μm or less and is made up of three layers, the desired uneven shape can be achieved by adjusting the thickness of the surface layer within the range of 0.5 μm to 5 μm.

[0067] In the method for producing a polyester film of the present invention, the thermodynamic mechanism of crystallization of polyester and the mechanism of formation of irregularities in the melt extrusion process of the polyester raw material are presumed to be as follows. The crystallization mechanism of polyester from a thermodynamic viewpoint is considered as follows based on the following formula (B). ΔG=-NΔg+Aσ (B) In the above formula (B), ΔG represents the crystal nucleus formation, N represents the volume of the crystal nucleus, Δg represents the free energy of fusion, A represents the number of repeating units of the crystal, and σ represents the free energy. When a crystal nucleating agent is blended into polyester, the energy barrier required to generate primary crystal nuclei is lowered, and the crystallization rate increases, as shown in Figure 1. This allows a large number of primary crystal nuclei to form within the polyester film, which is presumably why the crystal size becomes smaller. The mechanism by which the irregularities are formed is considered as follows. We noticed that when polyester raw material containing a crystal nucleating agent is melt-extruded and comes into contact with a casting drum from a nozzle, the surface condition of the film differs between the air side and the side in contact with the casting drum. As shown in Figure 2, it is presumed that the surface of the polyester film in contact with the casting drum is rapidly cooled, suppressing crystal growth and reducing the size of the crystals that are formed, so that unevenness is less likely to form even after longitudinal and transverse stretching. On the other hand, it is presumed that the surface of the film facing the atmosphere, which is not in close contact with the casting drum, is slowly cooled, which promotes crystal growth and increases the size of the crystals that are formed, resulting in the formation of minute irregularities after longitudinal stretching and then transverse stretching.

[0068] (Release layer) The polyester film of the present invention can be used in a form having a release layer on at least one surface thereof. The release layer is preferably laminated on one surface (A) of the polyester film. That is, the polyester film of the present invention preferably has a release layer on one surface (A) of the polyester film. Therefore, for example, in the case of an A / B / C structure, a release layer is laminated on the surface of the surface layer A, resulting in a structure of release layer / A / B / C. By laminating a release layer on one surface (A) of the polyester film, pinholes and the like are less likely to occur when an ultrathin ceramic layer is laminated on the release layer to form a ceramic green sheet, which is preferable.

[0069] The release layer is laminated to the polyester film directly or via another layer. Examples of other layers include an easy-adhesion coating layer for improving adhesion to the present film, an antistatic layer, an antiblocking layer, and the like.

[0070] The release layer is formed from a release agent composition containing a release agent, and from the viewpoint of obtaining good release performance, it is preferable that the release agent composition contains a silicone resin. Specifically, it is preferable that the release agent composition contains a type mainly composed of a curable silicone resin, a modified silicone type obtained by graft polymerization with an organic resin such as a urethane resin, an epoxy resin, or an alkyd resin, or a fluorosilicone resin.

[0071] As the curable silicone resin, any of the existing curing reaction types can be used, such as heat curable types such as addition types and condensation types, and electron beam curable types such as ultraviolet curable types. In addition, multiple types of curable silicone resins may be used in combination. Furthermore, there is no particular limitation on the form in which the curable silicone resin is applied when forming the release layer, and it may be in any form, such as a solution in an organic solvent, a water-based emulsion, or a solventless form.

[0072] The release agent composition forming the release layer may further contain, as necessary, a binder, an antifoaming agent, a coatability improving agent, a thickener, inorganic or organic particles, an organic lubricant, an antistatic agent, a conductive agent, an ultraviolet absorber, an antioxidant, a foaming agent, a dye, a pigment, and the like.

[0073] The release layer is formed by coating the film with a release agent composition. Either in-line coating, which is performed during the film production process, or so-called off-line coating, in which the release layer is applied outside the system onto a film that has already been produced, may be used.

[0074] The method for providing a release layer on the present film includes conventionally known coating methods such as reverse gravure coating, direct gravure coating, roll coating, die coating, bar coating, and curtain coating.

[0075] The curing conditions for forming the release layer are not particularly limited. When forming the release layer by offline coating, the heat treatment is usually performed at 80°C or higher for 10 seconds or more, preferably at 100 to 200°C for 3 to 40 seconds, and more preferably at 120 to 180°C for 3 to 40 seconds.

[0076] If necessary, the heat treatment may be combined with irradiation with active energy rays such as ultraviolet rays. As the energy source for curing by irradiation with active energy rays, known devices and energy sources can be used.

[0077] The coating amount of the release layer (after drying) is usually 0.005 to 5 g / m2 from the viewpoint of coatability. 2 , preferably 0.005 to 1 g / m 2 , and more preferably 0.005 to 0.1 g / m 2 The coating amount (after drying) is in the range of 0.005 g / m 2 If it is less than this, the coating property will lack stability, and it may be difficult to obtain a uniform coating film.

[0078] On the other hand, 5g / m 2 If the coating thickness exceeds this value, the coating adhesion and curing properties of the release layer itself may decrease.

[0079] The coating amount is calculated from the liquid mass per coating time (before drying), the non-volatile content of the coating liquid, the coating width, the stretching ratio, the line speed, and the like.

[0080] (Application) The polyester film of the present invention can be suitably used for various release applications. For example, it can be used for various release and process applications such as dry film resist (DFR), multilayer circuit boards, and ceramic green sheet manufacturing for multilayer ceramic capacitors. In release and process applications, the film is used, for example, as a support, and various materials such as ceramic slurries may be applied or laminated on the support.

[0081] In particular, the polyester film of the present invention has excellent smoothness as described above, while at the same time contributing to improved productivity, and therefore can be suitably used as a support for ceramic green sheets in the production process of multilayer ceramic capacitors.

[0082] Furthermore, in the case of multilayer ceramic capacitors for automobiles, which are becoming increasingly electrified in the future, it is predicted that the ceramic green sheets used will become thinner as the capacitors become smaller and their capacitance increases. Therefore, the polyester film of the present invention can be suitably used as a support for ceramic green sheets used in laminated ceramic capacitors for automobiles. EXAMPLES

[0083] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0084] <Production of polyester> (1) Production of Polyester A 100 parts by mass of dimethyl terephthalate and 65 parts by mass of ethylene glycol were charged into an ester exchange reaction vessel equipped with a stirrer, a temperature raising device, and a distillate separation column, and heated to 150° C. to melt the dimethyl terephthalate.

[0085] Next, an ethylene glycol solution of magnesium acetate tetrahydrate was added so that the amount of magnesium acetate added was 0.09% by mass based on the obtained polyester. The mixture was then heated to 225°C over 3 hours under normal pressure, and then held at 225°C for 1 hour and 15 minutes with stirring while distilling off methanol to carry out an ester exchange reaction. The ester exchange reaction was essentially completed, yielding a polyester oligomer.

[0086] The oligomer was then transferred to a polycondensation reaction vessel equipped with a stirrer and a distillation tube. An ethylene glycol solution of magnesium acetate tetrahydrate was added to the transferred oligomer so that the amount of magnesium acetate added was 0.09% by mass relative to the resulting polyester resin content. Thereafter, an ethylene glycol solution of phosphoric acid was added as a heat stabilizer so that the amount of phosphoric acid added to the resulting polyester was 0.017% by mass.

[0087] Next, an ethylene glycol solution of tetrabutyl titanate, a polycondensation catalyst, was added to the oligomer so that the titanium atom content was 4.5 ppm by mass relative to the resulting polyester. The pressure was then reduced from 101.3 kPa to 0.4 kPa over 85 minutes and maintained at 0.4 kPa, while the temperature was raised from 225°C to 280°C over 2 hours and maintained at 280°C for 1.5 hours to carry out a melt polycondensation reaction, yielding polyester A with an intrinsic viscosity (IV) of 0.63 dL / g.

[0088] (2) Manufacture of Polyester B The polyester A was subjected to solid phase polymerization to obtain a polyester B having an intrinsic viscosity (IV) of 0.70 dL / g.

[0089] (3) Production of Polyester C Polyester C having an intrinsic viscosity (IV) of 0.63 dL / g was obtained in the same manner as Polyester A, except that instead of adding tetrabutyl titanate to Polyester A, antimony trioxide, a polycondensation catalyst, was added so that the amount of antimony atom was 300 ppm by mass relative to the obtained polyester resin content.

[0090] (4) Manufacture of polyester D Polyester D having an intrinsic viscosity (IV) of 0.63 dL / g was obtained in the same manner as Polyester A, except that tetrabutyl titanate was added so that the titanium atom amounted to 210 ppm by mass relative to the obtained polyester.

[0091] (5) Manufacture of polyester E In the polyester D, a crystal nucleating agent of fatty acid metal salt (Clariant: Licomont NaV101 (CH 3 (CH 2 ) 26 COO (a), melting point 171° C.) was added in an amount of 10 mass %, and the mixture was kneaded using a vented twin-screw kneader to obtain Polyester E.

[0092] (6) Manufacture of Polyester F Polybutylene terephthalate resin (Novaduran 5007) manufactured by Mitsubishi Engineering Plastics was used.

[0093] (7) Manufacture of Polyester G Polyester G was obtained by adding 0.75 mass % of alumina particles having an average primary particle size of 0.05 μm to the above polyester D and kneading them using a vented twin-screw kneader.

[0094] (8) Manufacture of Polyester H 1.0% by mass of organic particles ((D90-D10) / D50=0.46: divinylbenzene-ethylstyrene-methacrylic acid-styrene copolymer) with an average primary particle size of 0.3 μm was added to the above polyester D and kneaded using a vented twin-screw kneader to obtain polyester H.

[0095] [Example 1] The raw material for the surface layer A was a blend of 50% polyester D, 10% polyester E, and 40% polyester F by mass, the raw material for the middle layer B was 100% polyester D, and the raw material for the surface layer C was a blend of 70% polyester D and 30% polyester H by mass. The raw materials were fed to a vented extruder and melt-extruded at 290°C. The raw materials for the surface layers A and C were the outermost layer (surface layer), and the middle layer B was the middle layer, resulting in a layer structure of three types of three layers (A / B / C). The extrusion conditions were such that the thickness composition ratio was A / B / C=1.5 / 28 / 1.5. The layer structure was then cooled and solidified on a cooling roll with a surface temperature set at 40°C using a coextrusion electrostatic application adhesion method to obtain an amorphous film. In this case, the surface layer C was the side that contacted the cooling roll.

[0096] Next, the film was stretched 3.4 times in the longitudinal direction, i.e., in the MD direction, at a film temperature of 85°C using the difference in roll peripheral speed, and then this longitudinally stretched film was introduced into a tenter and stretched 4.6 times in the transverse direction, i.e., in the TD direction, at 120°C. Heat treatment was then performed at 215°C, 205°C, 150°C, and 110°C in heat treatment (fixing) zones 1 and 2 and cooling zones 3 and 4 within the tenter, respectively. After that, the film was wound up into a roll on a 6-inch plastic core to obtain a polyester film with a thickness of 31 μm.

[0097] [Example 2] and [Example 3] A polyester film was obtained in the same manner as in Example 1, except that the blending ratio of the raw materials in the surface layer A was changed as shown in Table 1.

[0098] [Comparative Example 1] to [Comparative Example 3] A polyester film was obtained in the same manner as in Example 1, except that the blending ratio of the raw materials for the surface layer A and the surface layer C in Example 1 was changed as shown in Table 1.

[0099] [Reference Example 1] and [Reference Example 2] A polyester film was obtained in the same manner as in Example 1, except that the blending ratio of the raw materials for the surface layer A and the surface layer C in Example 1 was changed as shown in Table 1. The properties of each of the films obtained are shown in Table 1 below.

[0100] <Measurement and evaluation methods> The measurement and evaluation methods used in the examples and comparative examples are as follows. The measurement and evaluation results are summarized in Table 1.

[0101] (1) Intrinsic viscosity (IV) 1 g of polyester was precisely weighed, dissolved in 100 mL of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (mass ratio), and the viscosity was measured at 30 °C using a viscosity (IV) measuring device (Rigo Co., Ltd. "VMS-022UPC·F10").

[0102] (2) Average particle size and particle size distribution The powder was observed from the surface of the surface layer A side of the polyester films of the Examples and Comparative Examples using a scanning electron microscope (manufactured by HITACHI, "S3400N"). The size of each particle was measured from the obtained image data, and the average value of 10 points was taken as the average primary particle size. In addition, a dispersion liquid with a solid content of 0.03 g / mL was prepared by adding a mixed solvent of phenol / tetrachloroethane = 2 / 3 to the particles, and for this dispersion liquid, the particle diameter D10 at which the cumulative number is 10%, the particle diameter D50 at which the cumulative number is 50%, and the particle diameter D90 at which the cumulative number is 90% were measured by a laser diffraction scattering method using a Microtrackbell "MT3300EXII", and (D90-D10) / D50 was calculated.

[0103] (3) Thermal analysis of crystal nucleating agents (TG-DTA) Using a DSC (manufactured by Hitachi High-Tech Science Corporation, model: STA200RV AS), the temperature was increased from room temperature to 290° C. at a heating rate of 120° C. / min, and then the sample was held at 290° C. for 10 minutes. During this process, the change in state of the crystal nucleating agent was confirmed, and the change in state of the crystal nucleating agent when it reached 200°C was observed. (Judgment criteria) A: It was confirmed that it was in a molten state at 200°C. B: It was confirmed that the material was in an unmelted state at 200°C.

[0104] (4) Average surface roughness (Sa), maximum peak height (Sp) The surface of the surface layer A of the polyester film of the Examples and Comparative Examples was measured using a surface roughness measuring device ("NewView" (registered trademark) manufactured by Ametec Co., Ltd.), and the average surface roughness (Sa) and maximum peak height (Sp) were calculated from the obtained surface profile curves.

[0105] (5) Measuring the number of protrusions The surface of the surface layer A of the polyester films of the Examples and Comparative Examples was measured using a white light interferometer (Bruker's "Contour") under the following measurement conditions, and the number of protrusions with a height of less than 50 nm, the number of protrusions with a height of 50 nm or more but less than 100 nm, and the number of protrusions with a height of 100 nm or more were measured. (Measurement conditions) Measurement mode: VXI mode Objective lens: 20x Internal lens: 0.55x ·Viewing area: 586μm×460μm

[0106] (6) Scratch resistance Regarding scratches on the film surface, the polyesters of the examples and comparative examples were used as A4 size sample films, and it was confirmed whether scratches (fine scratches, scratch-like defects, grainy patterns, etc.) could be visually recognized using "transmitted light under indoor three-wavelength fluorescent lamps" and "reflected light from a halogen lamp in a dark room." If scratches were confirmed, the number of scratches was counted and judged according to the following evaluation criteria. <Evaluation criteria> A: 0 to 4 scratches with a depth of 0.3 μm or more that can be seen using transmitted light under indoor three-wavelength fluorescent lamps or reflected light from a halogen lamp. B: Five or more scratches with a depth of 0.3 μm or more that can be seen using transmitted light under indoor three-wavelength fluorescent lighting or reflected light from a halogen lamp.

[0107] (7) Thinner ceramic green sheets The maximum peak height (Sp) of the surface of the surface layer A of the polyester film in the examples and comparative examples is 200 nm or less, and the number of protrusions of 100 nm or more is 0 / mm 2 If the maximum peak height (Sp) exceeds 200 nm, or the number of protrusions of 100 nm or more is 0 / mm 2 If the test result exceeded this limit, it was judged to be defective (B). For example, in forming a thin ceramic green sheet having a thickness of 0.5 μm or less, if the maximum peak height (Sp) exceeds 200 nm, the high protrusions that exist tend to increase the risk of pinholes occurring.

[0108] (8) Support for longer polyester film rolls When the polyester films of the Examples and Comparative Examples were wound into a roll of 12,000 m, those that did not develop wrinkles and could be made into long lengths were rated as good (A), and those that developed wrinkles and made it difficult to make into long lengths were rated as poor (B).

[0109] [Table 1]

[0110] The polyester films of Examples 1 to 3 had high smoothness, and by using a crystal nucleating agent and polybutylene terephthalate (PBT), the maximum peak height (Sp) was made moderately rougher than in the conventional examples (Comparative Examples 1 and 2 and Reference Examples 1 and 2) while maintaining the average surface roughness (Ra), and yet had good scratch resistance.

[0111] Furthermore, the results of Examples 1 to 3 showed that in order to adjust the surface of surface layer A to have low Sa and high Sp, a combination of a crystal nucleating agent and polybutylene terephthalate (PBT) was required as the materials used for the surface layer. Furthermore, it was found that it is preferable that surface layer A contains an antimony compound and / or a titanium compound, that the content of the antimony compound is 100 ppm or less, and that the intrinsic viscosity (IV) of the polyester constituting surface layer A is 0.50 dL / g or more.

[0112] In addition, the number of protrusions on the surface of the surface layer A in Examples 1 to 3 shows a tendency to decrease as the size of the protrusions increases. In addition, when the number of protrusions in Examples 1 to 3 is compared with Comparative Example 3 (particle system) and the Reference Example, it was confirmed that Comparative Example 3 and the Reference Example are overwhelmingly larger in both the number of protrusions of 50 nm or more and less than 100 nm and the number of protrusions of 100 nm or more. In addition, when the Sa and Sp are compared between Examples 1 to 3 and Comparative Example 2, it was found that Comparative Example 2 has too low an average roughness (Sa) and a low maximum peak height (Sp), making it difficult to lengthen the polyester film. Comparative Example 1 is an example in which no particles were added, and a particle-free surface was used, but it was too smooth and prone to wrinkles, making it difficult to produce a long roll. In the present invention, PBT is selected from the viewpoints of crystallization speed and fluidity. In Example 1, PET and PBT are in an antagonistic state, which is presumed to be similar to the phase separation of a block copolymer. In Example 2, PBT is dominant, and it is considered to be in a state in which there are many tall fine protrusions. This is thought to be due to the fact that PBT has a faster crystallization rate than PET, and the crystal nuclei derived from PBT become larger. In Example 3, PET was predominant, and it is presumed that the crystallization of PBT or the crystal nucleating agent did not grow significantly, resulting in a large number of fine protrusions. It is presumed that the trends in Examples 1 to 3 are also due to the quantitative relationship (mixing ratio) between polybutylene terephthalate and other polyester resins. From the above, it was confirmed that by appropriately selecting the nucleating agent and polybutylene terephthalate (PBT) used in the surface layer A of the polyester film, it is possible to suppress the aggregation of the nucleating agent and to widen the adjustment range of the unevenness formation while maintaining a high level of smoothness on the polyester film surface. [Industrial Applicability]

[0113] The polyester film of the present invention has the advantage of being highly smooth and capable of being made longer with improved productivity. Furthermore, when used as a support for a ceramic green sheet in the manufacturing process of a multilayer ceramic capacitor, a uniform thin dielectric layer can be formed. In particular, it can be suitably used as a support for a ceramic green sheet used in a multilayer ceramic capacitor for automobiles.

Claims

1. A polyester film, one surface (A) of which contains a crystal nucleating agent and polybutylene terephthalate, and the surface (A) satisfies the following (1) and (2): (1) The average surface roughness (Sa) is 2.0 to 10 nm. (2) The percentage of protrusions having a size of 50 nm or more is 0.2% or less.

2. The polyester film according to claim 1 , wherein the crystal nucleating agent is a fatty acid metal salt represented by the following general formula (I): (CH 3 (CH 2 ) n COO) m M (I) (In the above formula (I), n is an integer of 4 or more, and M is Na, Ca, or Li. Also, m is 1 when M is Na or Li, and is 2 when M is Ca.)

3. The polyester film according to claim 2 , wherein the fatty acid metal salt has a melting point of 140° C. or more and 220° C. or less.

4. The polyester film according to claim 1 , which is a three-layer polyester film.

5. The polyester film according to claim 4 , wherein the intermediate layer of the polyester film contains 50% by mass or more of recycled polyester raw materials.

6. The polyester film according to claim 1 , further comprising a surface layer C on the opposite side of the one surface (A) of the polyester film.

7. The polyester film according to claim 6 , wherein the surface layer C contains two or more types of particles having different average particle sizes.

8. The polyester film according to claim 7 , wherein the maximum difference in average particle diameter between the two or more kinds of particles having different average particle diameters is 0.1 μm or more.

9. The polyester film according to any one of claims 1 to 8, further comprising a release layer on one surface (A) of the polyester film.

10. 2. The polyester film according to claim 1, which is used as a support for a ceramic green sheet in a process for producing a multilayer ceramic capacitor.

11. 10. The polyester film according to claim 1, which is used as a support for ceramic green sheets in the production process of automotive ceramic capacitors.

Citation Information

Patent Citations

  • Laminated polyester film

    JP2017002254A

  • Polyester film

    JP2020084187A

  • Release film for producing ceramic green sheet

    JP2020175668A

  • Release polyester film

    JP2013007054A

  • Release film for production of green sheet and method of producing release film for production of green sheet

    JP2014177093A