Method for producing poly(3-hydroxyalkanoate)-based resin pellet, and resin pellet
By controlling resin residence time and temperature during extrusion through a polymer filter, the method addresses thermal decomposition and foreign matter issues in poly(3-hydroxyalkanoate) resin pellet production, resulting in high-quality resin pellets suitable for molding.
Patent Information
- Application Number
- JP2023050604
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for producing poly(3-hydroxyalkanoate) resin pellets face challenges in maintaining resin strength due to thermal decomposition and high foreign matter content, particularly when using polymer filters, which compromise productivity.
A method involving a specific resin residence time and temperature relationship during melt extrusion through a polymer filter, setting the residence time to within 60/(resin temperature - 165°C) minutes, ensures the resin pellets maintain strength and reduce foreign matter content.
The method effectively suppresses thermal decomposition and produces resin pellets with reduced foreign substances, enhancing productivity and suitability for molding applications.
Smart Images

Figure 2024139592000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing resin pellets containing a poly(3-hydroxyalkanoate) resin, and to the resin pellets. [Background technology]
[0002] In recent years, the separate collection and composting of food waste has been promoted, particularly in Europe, and there is a demand for plastic products that can be composted together with food waste.
[0003] On the other hand, environmental problems caused by discarded plastics have been highlighted, and it has become clear that large amounts of plastic, especially plastic that has been dumped in the ocean or has flowed into the ocean via rivers, are drifting in the ocean on a global scale. Because such plastics maintain their shape for a long period of time, they have been pointed out to have an impact on the ecosystem, such as by restricting and capturing marine organisms, a phenomenon known as ghost fishing, and by causing feeding disorders when ingested by marine organisms, as they remain in the digestive tract.
[0004] Furthermore, there is also the problem that microplastics, which are plastics that have broken down and fallen into small particles due to ultraviolet rays, adsorb harmful compounds in seawater, and when marine organisms ingest these, harmful substances are introduced into the food chain.
[0005] The use of biodegradable plastics is expected to combat marine pollution caused by this type of plastic, but a report compiled by the United Nations Environment Programme in 2015 pointed out that plastics that can be biodegraded through compost, such as polylactic acid, cannot be expected to decompose in a short period of time in the cold ocean temperatures, and therefore cannot be used to combat marine pollution.
[0006] In this context, poly(3-hydroxyalkanoate) resins are attracting attention as a material that can solve the above problems because they are capable of biodegrading even in seawater.
[0007] When printing product designs or the like on plastic film, there is a problem that some areas are not printed (printing gaps) due to protrusions caused by foreign matter in the plastic film. In response to this problem, a technology is known that uses a polymer filter on molten resin to remove foreign matter contained in the resin with good productivity and high foreign matter removal performance (Patent Document 1). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 7-165896 Summary of the Invention [Problem to be solved by the invention]
[0009] Patent Document 1 discloses a method for filtering a polymer discharged from an extruder set at 190°C with a 20 μm filter when producing resin pellets containing polylactic acid by melt extrusion. However, when a resin mainly composed of a poly(3-hydroxyalkanoate) resin is used, since the melting point and thermal decomposition temperature of the poly(3-hydroxyalkanoate) resin are close to each other, for example, when a resin melted at a temperature of 190°C passes through a polymer filter, the resin is thermally decomposed, and the strength of the resin is reduced. On the other hand, when the temperature during filtration is lowered to suppress thermal decomposition, the melt viscosity of the molten resin increases, which increases the burden on the polymer filter, and there is a problem that the productivity is significantly reduced by lowering the filtration speed to keep the pressure below the limit of the polymer filter. As described above, when producing resin pellets containing a poly(3-hydroxyalkanoate) resin by melt extrusion, it is difficult to use a polymer filter, so it is difficult to produce pellets with a reduced number of foreign matters.
[0010] In view of the above-mentioned current situation, the present invention aims to provide a method for producing resin pellets containing a poly(3-hydroxyalkanoate)-based resin, which can produce resin pellets containing less foreign matter in the resin with excellent productivity while suppressing a decrease in strength of the resin due to thermal decomposition. [Means for solving the problem]
[0011] As a result of intensive research aimed at solving the above-mentioned problems, the inventors have discovered that when producing resin pellets containing a poly(3-hydroxyalkanoate) resin using a polymer filter, by setting the relationship between the resin residence time during which the molten resin passes through the polymer filter and the resin temperature within a specific range, it is possible to suppress a decrease in resin strength due to thermal decomposition and produce resin pellets with good productivity and little foreign matter, thereby completing the present invention.
[0012] That is, the present invention relates to a method for producing resin pellets containing a poly(3-hydroxyalkanoate)-based resin by a melt extrusion method, which includes a step of passing a resin composition containing a molten poly(3-hydroxyalkanoate)-based resin through a polymer filter, in which the resin residence time passing through the polymer filter is within 60 / (resin temperature - 165°C) minutes (provided that the resin temperature is > 165°C).
[0013] The present invention also relates to poly(3-hydroxyalkanoate) resin pellets produced by the above-mentioned production method. Effect of the Invention
[0014] According to the present invention, a production method can be provided for producing resin pellets containing a poly(3-hydroxyalkanoate)-based resin, which can suppress a decrease in strength due to thermal decomposition, has excellent productivity, and can produce resin pellets with little foreign matter in the resin. [Brief description of the drawings]
[0015] [Figure 1]FIG. 1 is a diagram illustrating an example of an apparatus for producing resin pellets according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment.
[0017] In the present invention, a resin composition containing a poly(3-hydroxyalkanoate)-based resin is molded into resin pellets. The pellets can be produced by any known or conventional method, and the melt extrusion method is preferably used from the viewpoint of productivity, etc. For example, an extruder (single-screw extruder, twin-screw extruder), kneader, etc. is used to melt-knead the resin and / or additives, and then the resin and / or additives are extruded from a die in the form of strands, which are then cooled and solidified in water, and the strands are cut into pellets of any length.
[0018] FIG. 1 is a diagram showing a schematic diagram of an example of an apparatus for producing resin pellets. A resin composition, which is a raw material for the resin pellets, is fed into an extruder 10, and is heated to a temperature equal to or higher than the glass transition temperature in the extruder 10, becoming molten. The molten resin composition is transferred to a polymer filter 11 attached to the outlet side of the extruder. The resin composition is retained in the polymer filter 11, transferred to a die 12 attached to the outlet side of the polymer filter 11, and discharged in a molten state from a die outlet 13 at the tip of the die. At the time of discharge, the molten resin composition 14 becomes a strand depending on the shape of the die outlet.
[0019] The strands of this molten thermoplastic resin composition are solidified in a water tank 15 and sent to a pelletizer 17 by a guide roll 16. The strands are cut by the pelletizer 17 to pelletize the resin composition, thereby obtaining resin pellets.
[0020] Moreover, by replacing the die 12 with a T-die, it is also possible to mold the thermoplastic resin composition retained in the polymer filter 11 directly into a resin film. (Polymer filter) The polymer filter according to the present embodiment may be attached to the outlet side of the extruder, or may be attached to the outlet side of a gear pump for flow control between the extruder and the polymer filter. The structure of the polymer filter may be, for example, a structure in which fiber bundles are twisted together, a mesh structure, a nonwoven fabric structure, a powder sintered body structure, etc., and from the viewpoint of removing foreign matter in the molten resin composition, the nonwoven fabric structure is preferred among these. The shape of the polymer filter may be, for example, a sheet shape (leaf disk type) or a pleated shape, and a sheet shape (leaf disk type) polymer filter can be preferably used because it has a large filtration area and is easily applicable to filtration of high viscosity resins. In the case of the leaf disk type, it is preferable to stack a filter support member, which also serves as a flow path for the molten resin after filtration, in parallel with the axis.
[0021] Examples of materials forming the structure of the polymer filter include metals (stainless steel, nickel steel, etc.) and resins. Among these, metals (stainless steel, nickel steel, etc.) are preferred, and stainless steel is more preferred.
[0022] From the viewpoint of removing foreign matter in the resin composition, the filtration accuracy of the polymer filter is preferably 50 μm or less, more preferably 30 μm or less, and particularly preferably 20 μm or less. In particular, fibrous foreign matter has a small diameter of 20 to 30 μm per unraveled fiber, so it easily passes through the polymer filter and is detected as foreign matter when the fiber length is several tens to several hundreds of μm. Therefore, when removing fibrous foreign matter, it is preferable to use a filtration accuracy of 50 μm or less.
[0023] In the present invention, the resin residence time when the molten resin passes through the polymer filter is within 60 / (resin temperature - 165°C) minutes (however, the resin temperature is > 165°C). The resin residence time when passing through the polymer filter is the time when the molten resin flows into the polymer filter, is filtered, and flows out of the polymer filter. It can be calculated from the difference between the time from the input of the raw material to the die when a polymer filter is not used and the time when a polymer filter is used at a certain discharge amount, and the resin residence time at an arbitrary discharge amount can be calculated from the discharge amount ratio to the residence time. It is also possible to obtain it by simulation using parameters required for calculation such as melt viscosity, discharge amount, and polymer filter size.
[0024] The resin temperature is the resin temperature at the extruder outlet, and is the resin temperature when flowing into the polymer filter. In order to ensure the flowability of the poly(3-hydroxyalkanoate)-based resin in the polymer filter, it is preferably a temperature higher than 165°C. The resin temperature is the resin temperature at the extruder outlet, and is, for example, a temperature measured by a resin thermometer provided at the extruder outlet. If the resin residence time passing through the polymer filter exceeds 60 / (resin temperature - 165°C) minutes, the resin will undergo thermal decomposition, and the strength of a molded product produced using the resin pellets will decrease, which is not preferable. The resin residence time passing through the polymer filter is preferably within 60 / (resin temperature - 165°C) minutes, and more preferably within 50 / (resin temperature - 165°C) minutes.
[0025] In order to achieve the above-mentioned resin residence time passing through the polymer filter, the molding resin temperature, the volume of the polymer filter and / or the extruder resin discharge amount may be appropriately set. For example, in the case of a leaf disc filter, the volume of the polymer filter can be changed by changing the diameter and number of the leaf disc filters. The leaf disc filter has a design upper limit of pressure resistance, and it is necessary to select the resin temperature, volume and discharge amount and determine the residence time so as not to exceed this limit. When molding a poly(3-hydroxyalkanoate) resin, the polymer filter may not be designed to suit the requirements, making it impossible to select conditions that can suppress thermal decomposition, but the present invention makes it possible to design a polymer filter suitable for the desired production.
[0026] When using poly(3-hydroxyalkanoate) resins, the higher the resin temperature, the more rapidly the thermal decomposition will progress. The resin temperature is preferably 210°C or lower, more preferably 195°C or lower, and particularly preferably lower than 185°C. Even at 185°C or lower, thermal decomposition will progress as the resin residence time increases, so by calculating 60 / (resin temperature - 165°C) according to the resin temperature as described above and setting the residence time below this, it is possible to suppress the resin thermal decomposition and produce pellets.
[0027] When the thermal decomposition of the resin progresses, for example, the melt flow rate (MFR) of the obtained resin pellets increases, so that the resin tends to flow and become unsuitable for molding. In particular, from the viewpoint of moldability into films, tubes, bottles, etc. by extrusion, the MFR of the resin is preferably 10 g / 10 min, more preferably 8 g / 10 min.
[0028] The resin pellets according to the present embodiment are resin pellets containing a poly(3-hydroxyalkanoate)-based resin.
[0029] The poly(3-hydroxyalkanoate)-based resin (hereinafter sometimes referred to as "P3HA-based resin") is a biodegradable aliphatic polyester (a polyester not containing an aromatic ring), and is a polyhydroxyalkanoate containing 3-hydroxyalkanoic acid repeating units represented by the general formula: [-CHR-CH2-CO-O-] (wherein R is an alkyl group represented by CnH2n+1, and n is an integer of 1 to 15). Among these, those containing the repeating units in an amount of 50 mol % or more, more preferably 70 mol % or more, based on the total monomer repeating units (100 mol %).
[0030] Among the poly(3-hydroxyalkanoate)-based resins, poly(3-hydroxybutyrate)-based resins can be preferably used because they are easily available and can be easily processed.
[0031] The poly(3-hydroxybutyrate)-based resin (hereinafter sometimes referred to as "P3HB-based resin") is an aliphatic polyester resin that can be produced from a microorganism, and is a polyester resin having 3-hydroxybutyrate as a repeating unit. The poly(3-hydroxybutyrate)-based resin may be a poly(3-hydroxybutyrate) having only 3-hydroxybutyrate as a repeating unit, or may be a copolymer of 3-hydroxybutyrate and another hydroxyalkanoate. The poly(3-hydroxybutyrate)-based resin may be a mixture of a homopolymer and one or more types of copolymers, or a mixture of two or more types of copolymers.
[0032] Specific examples of the poly(3-hydroxybutyrate)-based resin include poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter sometimes referred to as "P3HB3HH"), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (hereinafter sometimes referred to as "P3HB3HV"), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate), etc. Among them, poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), and poly(3-hydroxybutyrate-co-4-hydroxybutyrate) are preferred because they are easy to produce industrially.
[0033] Furthermore, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) is preferred from the viewpoints that by changing the composition ratio of the repeating units, it is possible to change the melting point, the degree of crystallinity, and physical properties such as Young's modulus and heat resistance, and it is possible to impart physical properties between polypropylene and polyethylene, and that it is easy to produce industrially and is a physically useful plastic. In particular, among poly(3-hydroxybutyrate)-based resins that tend to be thermally decomposed when heated at 180° C. or higher, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) is preferred from the viewpoints that it can lower the melting point and enable molding and processing at low temperatures.
[0034] Commercially available products of poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) include "Kaneka Biodegradable Polymer Green Planet" (registered trademark) manufactured by Kaneka Corporation.
[0035] The melting point, Young's modulus, etc. of the poly(3-hydroxybutyrate-co-3-hydroxyvalerate) vary depending on the ratio of the 3-hydroxybutyrate component and the 3-hydroxyvalerate component. However, since the two components co-crystallize, the degree of crystallinity is high at 50% or more, and although it is more flexible than poly(3-hydroxybutyrate), the improvement in brittleness is insufficient.
[0036] When the poly(3-hydroxybutyrate) resin contains a copolymer of 3-hydroxybutyrate units and other hydroxyalkanoate units, the average content ratio of 3-hydroxybutyrate units and other hydroxyalkanoate units in all monomer units constituting the poly(3-hydroxybutyrate) resin is preferably 3-hydroxybutyrate units / other hydroxyalkanoates=99 / 1 to 80 / 20 (mol % / mol %), and more preferably 97 / 3 to 85 / 15 (mol % / mol %), from the viewpoint of achieving both strength and productivity of the stretched film.
[0037] The average content ratio of each monomer unit in all monomer units constituting the poly(3-hydroxybutyrate)-based resin can be determined by a method known to those skilled in the art, for example, the method described in paragraph
[0047] of WO 2013 / 147139. The average content ratio means the molar ratio of each monomer unit in all monomer units constituting the poly(3-hydroxybutyrate)-based resin, and when the poly(3-hydroxybutyrate)-based resin is a mixture of two or more poly(3-hydroxybutyrate)-based resins, it means the molar ratio of each monomer unit contained in the entire mixture.
[0038] The poly(3-hydroxybutyrate) resin may be a mixture of at least two poly(3-hydroxybutyrate) resins having different types of constituent monomers and / or different content ratios of the constituent monomers. In this case, at least one highly crystalline poly(3-hydroxybutyrate) resin and at least one lowly crystalline poly(3-hydroxybutyrate) resin may be used in combination.
[0039] In general, highly crystalline poly(3-hydroxybutyrate)-based resins have excellent productivity but poor mechanical strength, while low-crystalline poly(3-hydroxybutyrate)-based resins have poor productivity but excellent mechanical properties. It is presumed that when both resins are used in combination, the highly crystalline poly(3-hydroxybutyrate)-based resin forms fine resin crystal particles, and the low-crystalline poly(3-hydroxybutyrate)-based resin forms tie molecules that crosslink the resin crystal particles. The strength and productivity of the stretched film can be improved by using these resins in combination.
[0040] The content ratio of 3-hydroxybutyrate units contained in the highly crystalline poly(3-hydroxybutyrate) resin is preferably higher than the average content ratio of 3-hydroxybutyrate units in all monomer units constituting the mixture of poly(3-hydroxybutyrate) resins.
[0041] When a highly crystalline poly(3-hydroxybutyrate) resin contains 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of the other hydroxyalkanoate units in the highly crystalline resin is preferably 1 mol % or more and less than 5 mol %, and more preferably 2 mol % or more and 4 mol % or less.
[0042] The highly crystalline poly(3-hydroxybutyrate)-based resin is preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate), and more preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
[0043] In addition, the content ratio of 3-hydroxybutyrate units contained in the low-crystalline poly(3-hydroxybutyrate) resin is preferably lower than the average content ratio of 3-hydroxybutyrate units in all monomer units constituting the mixture of poly(3-hydroxybutyrate) resins.
[0044] When a low-crystalline poly(3-hydroxybutyrate) resin contains 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of the other hydroxyalkanoate units in the low-crystalline resin is preferably 24 to 99 mol%, more preferably 24 to 50 mol%, even more preferably 24 to 35 mol%, and particularly preferably 24 to 30 mol%.
[0045] The low-crystalline poly(3-hydroxybutyrate) resin is preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate), and more preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
[0046] When a highly crystalline poly(3-hydroxybutyrate) resin and a low crystalline poly(3-hydroxybutyrate) resin are used in combination, the proportion of each resin relative to the total amount of both resins is not particularly limited, but it is preferable that the former be from 10% by weight to 60% by weight and the latter be from 40% by weight to 90% by weight, and it is more preferable that the former be from 25% by weight to 45% by weight and the latter be from 55% by weight to 75% by weight.
[0047] According to one embodiment, in addition to the highly crystalline poly(3-hydroxybutyrate)-based resin and the low crystalline poly(3-hydroxybutyrate)-based resin, a medium crystalline poly(3-hydroxybutyrate)-based resin having a crystallinity intermediate between the two resins can be used in combination.
[0048] When a moderately crystalline poly(3-hydroxybutyrate) resin contains 3-hydroxybutyrate units and other hydroxyalkanoate units, the content of other hydroxyalkanoate units in the moderately crystalline resin is preferably 5 mol% or more and less than 24 mol%, more preferably 5 mol% or more and 22 mol% or less, even more preferably 5 mol% or more and 20 mol% or less, and preferably 5 mol% or more and 18 mol% or less.
[0049] The moderately crystalline poly(3-hydroxybutyrate)-based resin is preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate), and more preferably poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
[0050] When the moderately crystalline poly(3-hydroxybutyrate) resin is further used in combination, the proportion of the moderately crystalline poly(3-hydroxybutyrate) resin to the total of the high crystalline poly(3-hydroxybutyrate) resin, the low crystalline poly(3-hydroxybutyrate) resin, and the moderately crystalline poly(3-hydroxybutyrate) resin is preferably 1% by weight or more and 99% by weight or less, more preferably 5% by weight or more and 90% by weight or less, and even more preferably 8% by weight or more and 85% by weight or less.
[0051] The method for obtaining a blend of two or more poly(3-hydroxybutyrate) resins is not particularly limited, and may be a method for obtaining a blend by microbial production or a method for obtaining a blend by chemical synthesis. In addition, a blend may be obtained by melt-kneading two or more resins using an extruder, kneader, Banbury mixer, roll, etc., or by dissolving two or more resins in a solvent, mixing, and drying the mixture.
[0052] The weight average molecular weight of the entire poly(3-hydroxybutyrate) resin is not particularly limited, but from the viewpoint of achieving both strength and productivity of the stretched film, it is preferably from 200,000 to 2,000,000, more preferably from 250,000 to 1,500,000, and even more preferably from 300,000 to 1,000,000.
[0053] In addition, when the poly(3-hydroxybutyrate) resin is a mixture of two or more poly(3-hydroxybutyrate) resins, the weight-average molecular weight of each poly(3-hydroxybutyrate) resin constituting the mixture is not particularly limited. However, when the above-mentioned high crystalline poly(3-hydroxybutyrate) resin and low crystalline poly(3-hydroxybutyrate) resin are used in combination, the weight-average molecular weight of the high crystalline poly(3-hydroxybutyrate) resin is preferably 200,000 to 1,000,000, more preferably 220,000 to 800,000, and even more preferably 250,000 to 600,000 from the viewpoint of achieving both the strength and productivity of the stretched film. On the other hand, the weight-average molecular weight of the low crystalline poly(3-hydroxybutyrate) resin is preferably 200,000 to 2,500,000, more preferably 250,000 to 2,300,000, and even more preferably 300,000 to 2,000,000 from the viewpoint of achieving both the strength and productivity of the stretched film. Furthermore, when the aforementioned moderately crystalline poly(3-hydroxybutyrate) resin is further used, the weight average molecular weight of the moderately crystalline poly(3-hydroxybutyrate) resin is preferably from 200,000 to 2,500,000, more preferably from 250,000 to 2,300,000, and even more preferably from 300,000 to 2,000,000, from the viewpoint of achieving both strength and productivity of the stretched film.
[0054] The weight average molecular weight of the poly(3-hydroxybutyrate) resin can be measured in terms of polystyrene using gel permeation chromatography (HPLC GPC system manufactured by Shimadzu Corporation) using a chloroform solution. As the column for the gel permeation chromatography, a column suitable for measuring the weight average molecular weight may be used.
[0055] The method for producing poly(3-hydroxybutyrate) resin is not particularly limited, and may be a production method by chemical synthesis or a production method using a microorganism. Among them, a production method using a microorganism is preferable. A known method can be applied to the production method using a microorganism. For example, Aeromonas caviae, which produces P3HB3HV and P3HB3HH, and Alcaligenes eutrophus, which produces P3HB4HB, are known as bacteria that produce copolymers of 3-hydroxybutyrate and other hydroxyalkanoates. In particular, with regard to P3HB3HH, in order to increase the productivity of P3HB3HH, it is more preferable to use Alcaligenes eutrophus AC32 (FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, p4821-4830 (1997)) into which genes of P3HA synthase group have been introduced, and microbial cells in which P3HB3HH has been accumulated in the cells by culturing these microorganisms under appropriate conditions are used. In addition to the above, genetically modified microorganisms into which various poly(3-hydroxybutyrate) resin synthesis-related genes have been introduced may be used according to the poly(3-hydroxybutyrate) resin to be produced, or the culture conditions, including the type of substrate, may be optimized.
[0056] The resin pellet according to the present embodiment can be suitably used as a resin pellet for molding, particularly as a molded product having a small amount of foreign matter, such as a film, a sheet, a bag, a straw, or an injection molded product. The resin pellets according to this embodiment preferably have 50 or less foreign objects having a size of 50 μm or more per 1 kg of the resin pellets.
[0057] The foreign matter according to the present embodiment is a foreign matter having a size of 50 μm or more (the diameter measured at the largest point of the lump solid, the length of the fiber) that is likely to cause defects such as printing defects in the molded product, and the material is not particularly limited, but examples thereof include a resin different from the resin pellet material, metal powder, fiber waste, etc. The number of foreign matter is preferably 50 or less per 1 kg of resin pellets, more preferably 30 or less, and particularly preferably 10 or less.
[0058] The resin pellet according to the present embodiment may contain additives that can be used together with the poly(3-hydroxyalkanoate) resin, as long as the effects of the invention are not impaired. Examples of additives include colorants such as pigments and dyes, odor absorbents such as activated carbon and zeolite, fragrances such as vanillin and dextrin, fillers, plasticizers, antioxidants, weather resistance improvers, ultraviolet absorbers, crystal nucleating agents, lubricants, release agents, water repellents, antibacterial agents, and sliding property improvers. Only one type of additive may be contained, or two or more types may be contained. The content of these additives can be appropriately set by a person skilled in the art depending on the purpose of use.
[0059] The crystal nucleating agent, lubricant, filler, and plasticizer will be described in more detail below.
[0060] (Crystal nucleating agent) The resin pellets may also contain a crystal nucleating agent. Examples of crystal nucleating agents include polyhydric alcohols such as pentaerythritol, galactitol, and mannitol; orotic acid, aspartame, cyanuric acid, glycine, zinc phenylphosphonate, and boron nitride. Among them, pentaerythritol is preferred because it is particularly effective in promoting the crystallization of poly(3-hydroxyalkanoate) resins. The crystal nucleating agent may be used alone or in combination with two or more other agents, and the ratio of use may be appropriately adjusted depending on the purpose.
[0061] The amount of the crystal nucleating agent used is not particularly limited, but is preferably 0.1 to 5 parts by weight, more preferably 0.5 to 3 parts by weight, and even more preferably 0.7 to 1.5 parts by weight, based on 100 parts by weight of the total amount of the poly(3-hydroxyalkanoate) resin.
[0062] (lubricant) The resin pellet may also contain a lubricant. Examples of lubricants include behenamide, oleamide, erucamide, stearamide, palmitamide, N-stearylbehenamide, N-stearylerucamide, ethylenebisstearamide, ethylenebisoleamide, ethylenebiserucamide, ethylenebislauramide, ethylenebiscapricamide, p-phenylenebisstearamide, and polycondensates of ethylenediamine, stearic acid, and sebacic acid. Among them, behenamide or erucamide is preferred because of its particularly excellent lubricant effect on poly(3-hydroxyalkanoate) resins. One or more types of lubricants may be used, and the ratio of use may be appropriately adjusted depending on the purpose.
[0063] The amount of the lubricant used is not particularly limited, but is preferably 0.01 to 5 parts by weight, more preferably 0.05 to 3 parts by weight, and even more preferably 0.1 to 1.5 parts by weight, relative to 100 parts by weight of the total amount of the poly(3-hydroxyalkanoate) resin.
[0064] (filling material) The resin pellets may contain a filler. By containing a filler, a stretched film with higher strength can be obtained. The filler may be either an inorganic filler or an organic filler, or both may be used in combination. The inorganic filler is not particularly limited, and examples thereof include silicates, carbonates, sulfates, phosphates, oxides, hydroxides, nitrides, and carbon black. Only one type of inorganic filler may be used, or two or more types may be used in combination.
[0065] The content of the filler is not particularly limited, but is preferably 1 to 100 parts by weight, more preferably 3 to 80 parts by weight, even more preferably 5 to 70 parts by weight, and even more preferably 10 to 60 parts by weight, relative to 100 parts by weight of the poly(3-hydroxyalkanoate) resin. However, the film raw material or the stretched film does not necessarily need to contain a filler.
[0066] (Plasticizer) The resin pellets may contain a plasticizer. Examples of the plasticizer include glycerin ester compounds, citrate compounds, sebacic acid ester compounds, adipate compounds, polyether ester compounds, benzoic acid ester compounds, phthalic acid ester compounds, isosorbide ester compounds, polycaprolactone compounds, and dibasic acid ester compounds. Among them, glycerin ester compounds, citrate compounds, sebacic acid ester compounds, and dibasic acid ester compounds are preferred because of their particularly excellent plasticizing effect on poly(3-hydroxyalkanoate) resins. Examples of the glycerin ester compounds include glycerin diacetomonolaurate. Examples of the citrate compounds include acetyl tributyl citrate. Examples of the sebacic acid ester compounds include dibutyl sebacate. Examples of the dibasic acid ester compounds include benzyl methyl diethylene glycol adipate. One type of plasticizer may be used, or two or more types may be used, and the ratio of use can be appropriately adjusted depending on the purpose.
[0067] The amount of the plasticizer used is not particularly limited, but is preferably 1 to 20 parts by weight, more preferably 2 to 15 parts by weight, and even more preferably 3 to 10 parts by weight, relative to 100 parts by weight of the total amount of the poly(3-hydroxyalkanoate) resin.
[0068] The following items enumerate preferred aspects of the present disclosure, but the present invention is not limited to the following items. [Item 1] A method for producing resin pellets containing a poly(3-hydroxyalkanoate)-based resin by a melt extrusion method, comprising a step of passing a resin composition containing molten poly(3-hydroxyalkanoate)-based resin through a polymer filter, in which the resin residence time in the polymer filter is within 60 / (resin temperature - 165°C) minutes (with the proviso that the resin temperature is > 165°C). [Item 2] 2. The method for producing poly(3-hydroxyalkanoate) resin pellets according to item 1, wherein in the step of passing the resin through a polymer filter, the resin temperature is higher than 165° C. and lower than 185° C. [Item 3] 3. The method for producing poly(3-hydroxyalkanoate)-based resin pellets according to item 1 or 2, wherein the poly(3-hydroxyalkanoate)-based resin comprises a poly(3-hydroxybutyrate)-based resin. [Item 4] 4. The method for producing poly(3-hydroxyalkanoate)-based resin pellets according to item 3, wherein the poly(3-hydroxybutyrate)-based resin comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate). [Item 5] Poly(3-hydroxyalkanoate) resin pellets produced by the production method according to any one of items 1 to 4. [Item 6] 6. The poly(3-hydroxyalkanoate) resin pellet according to item 5, wherein the number of foreign objects having a size of 50 μm or more contained per 1 kg of the resin pellet is 0 to 50. [Item 7] 7. The poly(3-hydroxyalkanoate)-based resin pellet according to item 6, wherein the poly(3-hydroxyalkanoate)-based resin comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate). EXAMPLES
[0069] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.
[0070] In the examples, the following raw materials were used:
[0071] (Poly(3-hydroxyalkanoate) resin) The P3HA-based resins used were the poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH) resins A-1 to A-4 below, where 3HB represents a 3-hydroxybutyrate repeating unit and 3HH represents a 3-hydroxyhexanoate repeating unit. A-1: P3HB3HH (average content ratio 3HB / 3HH=97.2 / 2.8 (mol% / mol%), weight average molecular weight is 660,000 g / mol, glass transition temperature is 6°C) It was produced in accordance with the method described in Example 2 of WO 2019 / 142845. A-2: P3HB3HH (average content ratio 3HB / 3HH=71.8 / 28.2 (mol% / mol%), weight average molecular weight is 660,000 g / mol, glass transition temperature is 1°C) It was produced in accordance with the method described in Example 9 of WO 2019 / 142845. A-3: P3HB3HH (average content ratio 3HB / 3HH=94 / 6 (mol% / mol%), weight average molecular weight is 600,000 g / mol, glass transition temperature is 6°C) It was produced in accordance with the method described in Example 1 of WO 2019 / 142845. A-4: P3HB3HH (average content ratio 3HB / 3HH=94 / 6 (mol% / mol%), weight average molecular weight is 400,000 g / mol, glass transition temperature is 6°C) It was produced in accordance with the method described in Example 1 of WO 2019 / 142845. (lubricant) B-1: Behenamide (Nippon Fine Chemicals: BNT-22H) (Nucleating agent) C-1: Pentaerythritol (Mitsubishi Chemical, NeuRizer P) In each of the Examples and Comparative Examples, the following evaluations were carried out.
[0072] [Foreign matter] Resin pellets were placed in the hopper of a single-screw extruder, extruded from a T-die in the form of a sheet, and cooled on a cooling roll to produce a film wound into a roll with a thickness of 30 μm and a width of 300 mm. This film was inspected for foreign matter of 50 μm or more over 500 m using a defect inspection machine, and the amount of foreign matter per 1 kg of pellets was evaluated by converting it into a weight per 1 kg.
[0073] In addition, if the number of foreign objects was 50 or less per 1 kg, it was marked as ◯, if it was 200 or more per 1 kg, it was marked as ×, and if it was in between, it was marked as △.
[0074] [Melt flow rate (MFR)] The melt flow rate of the resin pellets was measured using a melt flow rate measuring device (No. 120-FWP, manufactured by Yasuda Seiki Seisakusho Co., Ltd.) under a load of 5.0 kgf at a measurement temperature of 165°C. In addition, when the melt flow rate was 10 g / 10 min or less, it was marked as ◯, when it was 15 g / 10 min or more, it was marked as ×, and when it was in between, it was marked as △.
[0075] Example 1 (Method of producing resin composition) 30 parts by weight of poly(3-hydroxyalkanoate) resin A-1, 30 parts by weight of A-2, 10 parts by weight of A-3, and 30 parts by weight of A-4 were dry-blended with 0.5 parts by weight of B-1 as a lubricant and 1.0 parts by weight of C-1 as a crystal nucleating agent. The obtained resin composition was put into a hopper of a φ26 mm same-direction twin-screw extruder, melt-kneaded, and passed through a leaf disk polymer filter (filtration accuracy 20 μm cut, 5 inches, 12 sheets inserted) at a resin temperature of 170 ° C and a residence time of 8 minutes, extruded in the form of a strand from a die, passed through a water tank filled with water at 45 ° C to solidify the strand, and cut with a pelletizer to obtain resin pellets. The MFR of the obtained resin pellets was 5 g / 10 min. The resin pellets were molded into a film and inspected, and the number of foreign bodies of 50 μm or more was 1 piece / kg. The evaluation results are shown in Table 1.
[0076] Example 2 The procedure was the same as in Example 1, except that the resin was passed through a polymer filter at a resin temperature of 180°C and a residence time of 3 minutes. The MFR of the resin pellets was 6.5 g / 10 minutes, and when the resin was molded into a resin pelletizer and inspected, the number of foreign bodies of 50 μm or more was 0 / kg. The evaluation results are shown in Table 1.
[0077] Comparative Example 1 The same procedure as in Example 1 was repeated, except that the resin was passed through a polymer filter at a resin temperature of 170°C and a residence time of 15 minutes. The MFR of the resin pellets was 15g / 10 minutes, and the resin pellets were molded into a film and inspected, resulting in 2 foreign bodies of 50μm or more per kg. The evaluation results are shown in Table 1.
[0078] Comparative Example 2 The procedure was the same as in Example 1, except that the resin was passed through a polymer filter at a resin temperature of 170°C and a residence time of 20 minutes. The MFR of the resin pellets was 19.5 g / 10 minutes, and when the resin pellets were molded into a film and inspected, the number of foreign bodies of 50 μm or more was 2 / kg. The evaluation results are shown in Table 1.
[0079] Comparative Example 3 The same procedure as in Example 1 was repeated, except that the resin was passed through a polymer filter at a resin temperature of 180°C and a residence time of 8 minutes. The MFR of the resin pellets was 23.5 g / 10 minutes, and the resin pellets were molded into a film and inspected to find that the number of foreign bodies of 50 μm or more was 1 piece / kg. The evaluation results are shown in Table 1.
[0080] Comparative Example 4 The same procedure as in Example 1 was carried out, except that a wire mesh with an opening of 200 was used between the extruder and the die instead of using a polymer filter. The MFR of the resin pellets was 4.2 g / 10 min, and the resin pellets were molded into a film and inspected, resulting in 250 foreign bodies of 50 μm or more per kg. The evaluation results are shown in Table 1.
[0081] [Table 1] As can be seen from Table 1, the resin pellets shown in Examples 1 and 2 have a practical balance between the number of foreign matter particles and moldability due to being filtered under suitable conditions using a polymer filter, and therefore can be preferably used as resin pellets for molding processing.
[0082] On the other hand, the resin pellets shown in Comparative Examples 1 to 3 were filtered using a polymer filter, so the number of foreign matter was small, but the filtration was performed for a time exceeding the suitable range, so the melt flow rate was high and the pellets were not suitable for molding applications.
[0083] In addition, in Comparative Example 4, the resin pellets were produced without using a polymer filter, and therefore contained a large amount of foreign matter, making it unsuitable for molding applications. [Explanation of symbols]
[0084] 10 Extruder 11 Polymer Filter 12 Dice 13 Dice Exit 14 Resin Strand 15. Aquarium 17 Pelletizer
Claims
1. A method for producing resin pellets containing a poly(3-hydroxyalkanoate)-based resin by a melt extrusion method, comprising a step of passing a resin composition containing a molten poly(3-hydroxyalkanoate)-based resin through a polymer filter, in which the resin residence time in the polymer filter is within 60 / (resin temperature-165°C) minutes (with the proviso that the resin temperature is >165°C).
2. 2. The method for producing poly(3-hydroxyalkanoate) resin pellets according to claim 1, wherein the resin temperature is higher than 165° C. and not higher than 185° C. in the step of passing the resin through the polymer filter.
3. The method for producing poly(3-hydroxyalkanoate)-based resin pellets according to claim 1 or 2, wherein the poly(3-hydroxyalkanoate)-based resin includes a poly(3-hydroxybutyrate)-based resin.
4. The method for producing poly(3-hydroxyalkanoate)-based resin pellets according to claim 3, wherein the poly(3-hydroxybutyrate)-based resin comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
5. 3. A poly(3-hydroxyalkanoate) resin pellet produced by the method according to claim 1 or 2.
6. The poly(3-hydroxyalkanoate) resin pellet according to claim 5, wherein the number of foreign objects having a size of 50 μm or more contained per 1 kg of the resin pellet is 0 to 50.
7. The poly(3-hydroxyalkanoate)-based resin pellets of claim 6, wherein the poly(3-hydroxyalkanoate)-based resin comprises poly(3-hydroxybutyrate-co-3-hydroxyhexanoate).
Citation Information
Patent Citations
Biodegradable copolyester, its production, and molded article produced from it
JP1995165896A
Cited By
Method for producing molded articles containing poly(3-hydroxyalkanoate) resin
JP2026148314A