Silicon-carbon composite material and production method of the same, electrochemical device, electronic device

The silicon-carbon composite material addresses the volume changes and efficiency issues of silicon-based electrodes by controlling surface area and pore volume, enhancing stability and conductivity for improved lithium-ion battery performance.

JP2024139676AActive Publication Date: 2024-10-09AESC JAPAN LTD

Patent Information

Application Number
JP2023215327
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2023-12-20
Publication Date
2024-10-09
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

Silicon-based negative electrode materials for lithium-ion batteries face issues such as large volume changes during lithium intercalation and deintercalation, leading to material damage, low initial Coulombic efficiency, and continuous interfacial side reactions, limiting their commercialization due to rapid capacity decrease during cycling.

Method used

A silicon-carbon composite material is developed, comprising an amorphous carbon matrix with silicon material located on or within it, controlled by specific surface area and pore volume coefficients to suppress expansion and enhance conductivity, ensuring long-term cycle stability and improved capacity.

Benefits of technology

The silicon-carbon composite material achieves enhanced capacity and initial efficiency, ensuring long-term cycle stability and improved conductivity, facilitating large-scale industrial production and commercialization of silicon-based negative electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139676000001_ABST
    Figure 2024139676000001_ABST
Patent Text Reader

Abstract

To provide: a silicon-carbon composite material having a capacitance of a final material and an initial efficiency effectively improved by restricting expansion of a silicon-based material as far as possible and retaining long-term cycle stability and excellent conductivity thereof and a production method thereof; an anode sheet; and an electrochemical device and electronic device.SOLUTION: A silicon-carbon composite material includes an amorphous carbon matrix and a silicon material located on a surface and / or an inside of the amorphous carbon matrix, and has a specific surface area coefficient B of 20-1,250. A production method thereof includes obtaining the silicon-carbon composite material by synthesizing the amorphous carbon matrix material and a silicon source by a chemical vapor deposition method.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of secondary batteries, in particular to silicon-carbon composite materials and their manufacturing methods, electrochemical devices, and electronic devices. [Background technology]

[0002] With the increasing popularity of various portable electronic devices and the rapid development of electric vehicles and renewable energy storage systems, today the requirements for energy density, power density, cycle life and safety of lithium-ion batteries are higher than ever before. At present, the energy density of common NCM ternary material (cathode) / graphite (anode) based lithium-ion batteries is approaching its theoretical limit. In terms of anode materials, the actual specific capacity of graphite (up to 360mAh / g) is close to the theoretical specific capacity (372mAh / g). Silicon has a much higher theoretical specific capacity (-3600mAh / g) and a lower discharge platform (-0.2V vs. Li) than graphite. + Silicon-based anode materials have attracted widespread attention due to their high lithium content (100 / Li) and abundant resources. However, the large volume change during the lithium insertion and extraction process makes the materials prone to crushing, damage, and peeling from the current collector, and the continuous occurrence of interfacial side reactions causes the specific capacity of the materials to rapidly decrease during cycling, limiting the commercialization of silicon-based anode materials.

[0003] To solve the above problems, structural design of silicon-based materials such as nanoscale, composite, hollow / porous, etc. has become a popular research topic. x Although the pure silicon material can buffer the expansion to some extent, its first-time coulombic efficiency is only about 75%. Prelithiation or graphite composite also has a first-time coulombic efficiency of only about 80% to 85%. Both of these are based on the positive electrode ternary layered material (LiNi x Co y Mn 1-x-yThe initial efficiency is lower than the initial efficiency of 88% for the cathode of lithium iron phosphate (LiFePO4) and 98% for the anode of the battery, and has no advantage over batteries using graphite as the anode material. It has been reported that the surface coating layer of hollow / porous silicon materials is often prone to cracking or shattering under large pressure, and although the space reserved for expansion inside the material is compressed and released, the material and the battery are still subject to large volume expansion during charging and discharging. The interfacial side reaction between the material and the electrolyte continues, thus losing the inherent advantages of the material. Summary of the Invention [Problem to be solved by the invention]

[0004] Provided are a silicon-carbon composite material that structurally suppresses the expansion of silicon-based materials to the maximum extent possible, a manufacturing method thereof, a negative electrode sheet, an electrochemical device, and an electronic device. [Means for solving the problem]

[0005] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a silicon-carbon composite material, a manufacturing method thereof, a negative electrode sheet, an electrochemical device, and an electronic device, which structurally suppress the expansion of silicon-based materials to the maximum extent, ensure long-term cycle stability and excellent electrical conductivity, solve the problem of low capacity and initial efficiency of silicon-based materials in the prior art, and ensure certain processing performance.

[0006] To achieve the above and other related objectives, a first aspect of the present invention provides a silicon-carbon composite material comprising an amorphous carbon matrix and a silicon material located on and / or within the amorphous carbon matrix.

[0007] Silicon-carbon composite materials satisfy the following relationship:

[0008] B=B A / B a

[0009] The value range of B is 20 to 1250.

[0010] B is the specific surface area coefficient (i.e., the BET coefficient) of the silicon-carbon composite, and B A is the specific surface area of ​​the amorphous carbon matrix, and B a is the specific surface area of ​​the silicon-carbon composite.

[0011] The range B of the specific surface area coefficient of the silicon-carbon composite material is 100-900, and preferably 150-500.

[0012] In addition, the specific surface area B of the amorphous carbon matrix A Range is 500m 2 / g~2500m 2 / g, preferably 800m 2 / g~1800m 2 / g.

[0013] In addition, the specific surface area B a The range is 2m 2 / g~25m 2 / g, preferably 2m 2 / g~8m 2 / g.

[0014] Furthermore, the silicon-carbon composite material satisfies the following relationship:

[0015] P v =P v1 / P v2

[0016] P v The value range is 0.4 to 120.

[0017] P v represents the pore volume coefficient of the silicon-carbon composite, and P v1 represents the pore volume diameter of the amorphous carbon matrix, and P v2 represents the pore volume diameter of the silicon-carbon composite material.

[0018] In addition, the pore volume coefficient P vThe range is 1 to 100, preferably 10 to 90.

[0019] In addition, the pore volume diameter P of the amorphous carbon matrix v1 The value range is 0.2 cm 3 / g~0.9cm 3 / g, preferably 0.2 cm 3 / g~0.8cm 3 / g, more preferably 0.2 cm 3 / g~0.7cm 3 / g.

[0020] In addition, the pore volume diameter P v2 The range is 0.005 cm 3 / g~0.2cm 3 / g, preferably 0.008 cm 3 / g~0.02cm 3 / g.

[0021] Furthermore, the weight loss due to thermal decomposition of a silicon-carbon composite material heated to 1400° C. in an air atmosphere is 5% to 60%, and preferably 24% to 42%, or 15% to 40%.

[0022] A second aspect of the present invention provides a method for producing a silicon-carbon composite material, comprising the steps of: synthesizing an amorphous carbon matrix material and a silicon source by chemical vapor deposition to obtain a silicon-carbon composite material, the silicon-carbon composite material comprising an amorphous carbon matrix and a silicon material located on and / or within the amorphous carbon matrix.

[0023] Silicon-carbon composite materials satisfy the following relationship:

[0024] B=B A / B a .

[0025] The value range of B is 20 to 1250.

[0026] B is the specific surface area coefficient of the silicon-carbon composite, and B A is the specific surface area of ​​the amorphous carbon matrix, and B a is the specific surface area of ​​the silicon-carbon composite.

[0027] The silicon source is at least one selected from monosilane (SiH4), dimethyldichlorosilane, trichloromethylsilane, tetramethylsilane, trichlorosilane, tetrachlorosilane, methylsilicate, and ethylsilicate.

[0028] Additionally, the amorphous carbon matrix material is porous amorphous carbon.

[0029] The amorphous carbon matrix material can also be a porous amorphous carbon-metal composite, which includes a porous amorphous carbon matrix and metal nanoparticles located on and / or within the porous amorphous carbon matrix.

[0030] A third aspect of the present invention provides a negative electrode sheet. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material. The negative electrode active material includes the silicon-carbon composite material according to the first aspect and / or the silicon-carbon composite material produced according to the method according to the second aspect.

[0031] A fourth aspect of the present invention provides an electrochemical device comprising the negative electrode sheet according to the third aspect.

[0032] A fifth aspect of the present invention provides an electronic device comprising an electrochemical device according to the fourth aspect.

[0033] As described above, the silicon-carbon composite material and its manufacturing method, negative electrode sheet, electrochemical device, and electronic device of the present invention provide the following advantages.

[0034] In the present invention, the specific surface area coefficient B of the silicon-carbon composite material is controlled within the above range to ensure long-term cycle stability and improve capacity and initial efficiency. On the basis that the specific surface area of ​​the silicon-carbon composite material is within a certain range, if the specific surface area coefficient is too high, the specific surface area of ​​the amorphous carbon matrix will be too large, the uniformity of the subsequent introduction of silicon material will be reduced, and the cycle stability of the subsequent silicon-carbon composite material will be reduced. If the specific surface area coefficient is too low, the specific surface area of ​​the amorphous carbon matrix will be too small, which will reduce the active sites for silicon introduction, leading to a reduction in the amount of silicon added, and the capacity of the completed material will be low, which will not contribute to the realization of high energy density of the battery cell.

[0035] Pore ​​volume coefficient P of silicon-carbon composites v By maintaining the pore volumes of the silicon-carbon composite and amorphous carbon within the above ranges, the content of silicon subsequently introduced can be controlled, thereby controlling the capacity of the material and helping to balance the energy density and cycling performance of the lithium-ion battery.

[0036] By controlling the contents of various elements and the loss due to pyrolysis in the silicon-carbon composite material within the above ranges, it is possible to ensure long-term cycle stability and improve the capacity and initial efficiency. If the loss due to pyrolysis is too high and the C content is too high, it is difficult to achieve high capacity of the material and high energy density of the battery cell. If the loss due to pyrolysis is too low and the Si content is too high, it is difficult to obtain better cycle stability. Effect of the Invention

[0037] The present invention relates to the structure, specific surface area coefficient B, pore volume coefficient P of silicon-carbon composite materials. vBy controlling the content of various elements and the weight loss due to thermal decomposition, the expansion of the silicon-based material can be suppressed to the maximum extent, and long-term cycle stability and excellent electrical conductivity can be ensured, thereby effectively improving the capacity and initial efficiency of the final material, and promoting the commercialization process of silicon-based negative electrode materials while maintaining a certain processing performance. At the same time, the method for producing the silicon-carbon composite material of the present invention is simple and easy to operate. It is suitable for large-scale industrial production. The silicon-carbon composite material provided by the present invention can be used as a negative electrode active material, and can be applied to a negative electrode active material layer to prepare a negative electrode sheet, which can then be packaged with a positive electrode sheet, a separator, an electrolyte, etc. to form an electrochemical device such as a lithium-ion battery, thereby greatly improving its electrical performance. [Brief description of the drawings]

[0038] [Figure 1] FIG. 1 shows a schematic structural diagram of a silicon-carbon composite material in one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] Hereinafter, the present invention will be described with reference to specific examples, and those skilled in the art will be able to easily understand other advantages and effects of the present invention from the contents disclosed in the present specification. The present invention may be implemented or applied through other different specific embodiments, and the details of the specification may be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.

[0040] One embodiment of the present invention provides a silicon-carbon composite material that includes an amorphous carbon matrix and a silicon material located on and / or within the amorphous carbon matrix.

[0041] Silicon-carbon composite materials satisfy the following relationship:

[0042] B=B A / B a

[0043] The value range of B is 20 to 1250.

[0044] B is the specific surface area coefficient of the silicon-carbon composite, and B A is the specific surface area of ​​the amorphous carbon matrix, and B a is the specific surface area of ​​the silicon-carbon composite.

[0045] In some embodiments, the specific surface area coefficient B of the silicon-carbon composite material is in the range of 100 to 900, more preferably 150 to 500. A The value range is 500m 2 / g~2500m 2 / g, preferably 800m 2 / g~1800m 2 / g. The specific surface area B of the silicon-carbon composite a The value range is 2m 2 / g~25m 2 / g, preferably 2m 2 / g~8m 2 / g.

[0046] In the above embodiment, the specific surface area coefficient B of the silicon-carbon composite material is controlled within the above range to ensure long-term cycle stability and contribute to improving capacity and initial efficiency. On the basis that the specific surface area of ​​the silicon-carbon composite material is within a certain range, if the specific surface area coefficient is too high, the specific surface area of ​​the amorphous carbon matrix will be too large, which is conducive to the uniformity of the subsequent silicon material introduction, but will reduce the subsequent cycle stability of the silicon-carbon composite material. If the specific surface area coefficient is too low, the specific surface area of ​​the amorphous carbon matrix will be too small, which will reduce the active sites for silicon introduction, leading to a reduction in the amount of silicon added, and the subsequent capacity of the final material will be low, which will not contribute to achieving a higher energy density of the battery cell.

[0047] In another embodiment of the present invention, the silicon-carbon composite material satisfies the following relationship:

[0048] P v =Pv1 / P v2

[0049] P v The value range is 0.4 to 120.

[0050] P v represents the pore volume coefficient of the silicon-carbon composite, and P v1 represents the pore volume diameter of the amorphous carbon matrix, and P v2 represents the pore volume diameter of the silicon-carbon composite material.

[0051] In some embodiments, the P of the silicon-carbon composite material v The value ranges from 1 to 100, and preferably from 10 to 90. The pore volume diameter Pv1 of the amorphous carbon matrix is ​​0.2 cm 3 / g~0.9cm 3 / g, preferably 0.2 cm 3 / g~0.8cm 3 / g, more preferably 0.2 cm 3 / g~0.7cm 3 / g. The pore volume diameter P v2 is 0.005 cm 3 / g~0.2cm 3 / g, preferably 0.008 cm 3 / g~0.02cm 3 / g.

[0052] In the above embodiments, maintaining the pore volume coefficient of the silicon-carbon composite, and the pore volumes of the silicon-carbon composite and amorphous carbon within the above ranges helps control the subsequent silicon incorporation, thereby controlling the capacity of the material and helping to balance the energy density and cycling performance of the lithium ion battery.

[0053] In another embodiment of the present invention, the range of pyrolysis weight loss of the silicon-carbon composite material heated to 1400° C. in air atmosphere is 5%-60%, preferably 24%-42% or 15%-40%.

[0054] In another embodiment of the present invention, the mass ratio of carbon:silicon in the silicon-carbon composite material is 3-8:2-7.

[0055] In the above embodiment, the contents of various elements in the silicon-carbon composite material and the loss due to pyrolysis are controlled within the above ranges to ensure long-term cycle stability and contribute to improving capacity and initial efficiency. If the loss due to pyrolysis is too high and the C content is too high, it is difficult to achieve high capacity of the material and high energy density of the battery cell. If the loss due to pyrolysis is too low and the Si content is too high, it is difficult to achieve better cycle stability.

[0056] In some embodiments, the amorphous carbon matrix is ​​a porous carbon material, and the silicon material is uniformly distributed on the surface and / or pore walls of the amorphous carbon matrix. Figure 1 shows a schematic structural diagram of a silicon-carbon composite material provided by an embodiment of the present invention. The amorphous carbon matrix is ​​a porous carbon material, and the silicon material is uniformly distributed on the pore walls of the amorphous carbon matrix.

[0057] In some embodiments, the silicon material is Si and SiO x At least one selected from the following:

[0058] In some embodiments, the silicon material is nanoscale, and the grain size of the silicon material is between 1 nm and 20 nm, preferably between 1 nm and 5 nm.

[0059] In some embodiments, the silicon material is rod-shaped and / or granular, including but not limited to spherical, quasi-spherical, or acicular particles.

[0060] In another embodiment of the present invention, the silicon-carbon composite further comprises nano-metal particles attached to the surface and / or inside of the amorphous carbon matrix. In some embodiments, the amorphous carbon matrix is ​​a porous carbon material, and the nano-metal is uniformly distributed on the surface and / or pore walls of the amorphous carbon matrix. The mass ratio of the nano-metal particles in the silicon-carbon composite may be greater than 0% to 2%. The nano-metal particles are at least one selected from titanium, iron, copper, nickel, cobalt, manganese, silver, gold, and tin particles. The nano-metal particles have a particle size of 2 nm to 5 nm.

[0061] One embodiment of the present invention provides a method for producing a silicon-carbon composite material, comprising the steps of: synthesizing an amorphous carbon matrix material and a silicon source by chemical vapor deposition to obtain a silicon-carbon composite material, the silicon-carbon composite material comprising an amorphous carbon matrix and a silicon material located on and / or within the amorphous carbon matrix.

[0062] Silicon-carbon composite materials satisfy the following relationship:

[0063] B=B A / B a

[0064] The value range of B is 20 to 1250.

[0065] B is the specific surface area coefficient of the silicon-carbon composite, and B A is the specific surface area of ​​the amorphous carbon matrix, and B a is the specific surface area of ​​the silicon-carbon composite.

[0066] In some embodiments, the silicon source is at least one selected from monosilane (SiH4), dimethyldichlorosilane, and trichloromethylsilane.

[0067] In some embodiments, the amorphous carbon matrix material is porous amorphous carbon.

[0068] In some embodiments, the amorphous carbon matrix material is a porous amorphous carbon-metal composite, which comprises a porous amorphous carbon matrix and nanometal particles attached to the surface and / or within the porous amorphous carbon matrix.

[0069] In some embodiments, the method for producing a porous amorphous carbon-metal composite includes the following steps: attaching metal nanoparticles to the surface and / or inside of a porous amorphous carbon matrix by mechanical mixing (e.g., stirring), liquid phase reduction, or gas phase reduction. Preferably, the nanometal particles are at least one selected from titanium, iron, copper, nickel, cobalt, manganese, silver, gold, and tin particles. Specifically, in the embodiments of the present invention, the mechanical mixing method, liquid phase reduction method, and gas phase reduction method adopted to attach nanometal particles to the surface and / or inside of a porous amorphous carbon matrix are conventional and well-known techniques, and no special requirements are applied. Therefore, further details are omitted.

[0070] In another embodiment of the present invention, a method for producing a silicon-carbon composite material includes the following steps: placing an amorphous carbon matrix material and a silicon source in a chemical vapor deposition reactor, using hydrogen as a carrier gas and hydrogen and / or argon as a dilution gas at a flow rate of 1 L / min-5 L / min, raising the temperature to 400°C-600°C, and reacting for 1 hour-20 hours, and then obtaining a silicon-carbon composite material by pyrolysis synthesis.

[0071] The silicon-carbon composite material described in the above embodiment can be produced by the method described in the above example, but is not limited to this.

[0072] One embodiment of the present invention provides a negative electrode sheet. The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, the negative electrode active material including a silicon-carbon composite material described in the above embodiment and / or a silicon-carbon composite material produced according to the method described in the above embodiment. In some embodiments, the negative electrode active material includes 24% to 45% by mass of the silicon-carbon composite material.

[0073] An embodiment of the present invention provides an electrochemical device including the negative electrode sheet, the positive electrode sheet, the separator, and the electrolyte described in the above embodiment.

[0074] The electrochemical device in accordance with embodiments of the present invention may be any electrochemical device, such as, but not limited to, a lithium ion battery or a sodium ion battery.

[0075] The positive electrode sheet generally includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material.

[0076] The positive electrode active material generally includes lithium-containing composite oxides. Specific examples include LiMnO2, LiFeO2, LiMn2O4, Li2FeSiO4, and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi5CO2Mn3O2, Li z Ni (1-x-y) Co x M y O2 (wherein 0.01≦x≦0.20, 0≦y≦0.20, 0.97≦z≦1.20, and M represents at least one element selected from Mn, V, Mg, Mo, Nb, and Al), LiFePO4, and Li z CO (1-x) M x O2 (wherein 0≦x≦0.1, 0.97≦z≦1.20, and M represents at least one element selected from the group consisting of Mn, Ni, V, Mg, Mo, Nb, and Al).

[0077] In general, materials such as a conductive agent and a binder are added to the active material. The amount of the additive can be adjusted as necessary within the range of 1% to 50% of the total mass of the positive electrode active material, or 55% to 76% of the total mass of the active material.

[0078] Conductive agents are reagents used to improve the charge / discharge performance of electrodes. Examples of conductive agents include graphite materials such as natural graphite and artificial graphite, carbon black materials such as conductive carbon black (Super P), conductive fibers such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, carbon fibers and metal fibers, metal powders such as carbon fluoride powder, aluminum powder, and nickel powder, conductive whiskers such as zinc oxide and potassium titanate, and conductive metal oxides such as titanium dioxide and polyphenylene derivatives.

[0079] Binders are components that promote the binding between active materials and conductive materials, and between active materials and current collectors. Typically, binders can be selected from polyvinylidene fluoride, polyvinyl alcohol, polyacrylic acid (PAA), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, styrene-propylene rubber, fluororubber, and various copolymers.

[0080] The current collector functions as a substrate for supporting the electrode active material, and is usually made of a metal foil having a thickness of 3 to 500 microns. There are no particular limitations on the material as long as it has high conductivity and does not cause a chemical reaction in the secondary battery system. For example, the material may be a foil material obtained by surface treatment of nickel, titanium, aluminum, silver, stainless steel, carbon, etc. The surface of the current collector is usually smooth, but fine lines may be formed on the surface to improve adhesion between the positive electrode active material and the current collector. The current collector may be in any one or combination of various forms such as a film, mesh, porous material, foam, nonwoven fabric, etc., in addition to foil.

[0081] The separator is placed between the positive electrode sheet and the negative electrode sheet, and is usually made of an insulating film with high ion permeability and high mechanical strength. The thickness of the separator is usually 9 μm to 18 μm, the pore size is 5 μm to 300 μm, the air permeability is 180 sec / 100 mL to 380 sec / 100 mL, and the porosity is 30% to 50%. The separator is formed using a sheet or nonwoven fabric made of an olefin polymer such as polypropylene, glass fiber, or polyethylene, which has chemical resistance and hydrophobicity.

[0082] The electrolytes used in lithium-ion batteries generally include a non-aqueous solvent, a lithium salt, and an additive.

[0083] The non-aqueous solvent may be a conventional non-aqueous solvent in the art, preferably an ester solvent, more preferably a carbonate solvent. Specifically, the carbonate solvent may be at least one selected from ethylene carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC).

[0084] Lithium salts include LiPF6, LiBF4, LiN(SO2F)2 (abbreviated as LiFSI), LiClO4, LiAsF6, LiB(C2O4)2 (abbreviated as LiBOB), LiBF2(C2O4) (abbreviated as LiDFOB), LiN(SO2R F)2, and LiN(SO2F)(SO2R F ) The content of the lithium salt in the electrolyte is preferably 5% to 20%.

[0085] The additive may be at least one selected from vinylene carbonate (VC), fluoroethylene carbonate (FEC), vinyl ethylene carbonate (VEC), vinyl sulfate (DTD), vinylene sulfate, 1,3-propane sultone (PS), 1-propene 1,3-sultone, and 1,4-butane sultone. The typical amount of additive in the electrolyte is 1% to 4% of the electrolyte, for example 2%.

[0086] In some embodiments, the negative electrode active material includes a silicon-carbon composite material, graphite, conductive carbon black, and a binder. The negative electrode active material preferably contains, by mass, 24% to 45% of the silicon-carbon composite material, 40% to 63% of the graphite, 2% to 8% of the conductive carbon black, and 2% to 18% of the binder.

[0087] In some embodiments, the method for producing the negative electrode sheet described in the above embodiments includes the following steps.

[0088] A silicon-carbon composite material and graphite are mixed at high speed in a mass ratio of 30-50:70-50 to prepare a negative electrode active material mixed powder, and then conductive carbon black and a binder are thoroughly stirred and mixed in a suitable amount of deionized water in a mass ratio of 80-90:2-8:2-18 to form a uniform negative electrode slurry. The negative electrode slurry is applied to the surface of the copper foil of the negative electrode current collector, dried, and cold pressed to obtain a negative electrode sheet.

[0089] It should be noted that in the above-mentioned embodiments of the present invention, the details of other process conditions and parameters in the preparation process of the negative electrode sheet are not described in detail. Those skilled in the art can obtain the negative electrode sheet by using the method described in the above-mentioned embodiments in combination with conventional technical means and common sense.

[0090] One embodiment of the present invention provides an electronic device including the electrochemical device described in the above embodiments.

[0091] The electronic device in the embodiment of the present invention may be any electronic device, such as, but not limited to, a notebook computer, a pen-input computer, a mobile computer, an e-book player, a mobile phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headphone, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini disc, a walkie-talkie, an electronic organizer, a calculator, a memory card, a portable tape recorder, a radio, a backup power source, a motor, an automobile, a motorcycle, an electrically assisted bicycle, a bicycle, a lighting device, a toy, a game machine, a clock, an electric tool, a flashlight, a camera, a large-scale household storage battery, a lithium-ion capacitor, etc. It should be noted that the electrochemical device of the present invention can be applied not only to the electronic devices listed above, but also to an energy storage power plant, a marine transport vehicle, and an air transport vehicle. An air transport vehicle includes an air transport vehicle in the atmosphere and an air transport vehicle outside the atmosphere.

[0092] It should be noted that the above-mentioned embodiments of the present invention do not describe in detail the packaging method and packaging steps of the lithium ion battery. Those skilled in the art can combine the positive electrode sheet and the negative electrode sheet according to conventional or common technical means and common knowledge in the field to package the positive electrode sheet, the negative electrode sheet, the electrolyte and the separator to form a lithium ion battery.

[0093] The following specific examples are provided to explain the present invention in detail. It should also be understood that the following examples are used solely to specifically explain the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art according to the above content of the present invention all belong to the scope of protection of the present invention. The specific process parameters in the following examples are merely examples of suitable ranges. Those skilled in the art can select within the appropriate range through the description of this specification, and are not limited to the specific numerical values ​​exemplified below.

[0094] Example 1

[0095] In this embodiment, a silicon-carbon composite material is prepared, and the specific preparation process is as follows:

[0096] Specific surface area 1000m 2 / g, pore volume 0.54 cm 3 500 g of porous amorphous carbon material with a molecular weight of 1000 g / g was added to the fluidized bed, nitrogen gas was introduced at 10 L / min to fluidize the material, and the fluidized bed was heated to 500°C. After the temperature was stabilized, monosilane was introduced at 3 L / min for 95 minutes, and the pressure of the fluidized bed was controlled at 6 kPa. The introduction of monosilane gas was stopped, The inert gas was continued to be introduced until the reaction product was cooled to room temperature, yielding a silicon-carbon composite material.

[0097] Example 2

[0098] In this embodiment, a silicon-carbon composite material is prepared, and the specific preparation process is as follows:

[0099] Specific surface area 800m 2 / g, pore volume 0.54 cm 3500 g of porous amorphous carbon material with a molecular weight of 1000 g / g was added to the fluidized bed, nitrogen gas was introduced at 10 L / min to fluidize the material, and the fluidized bed was heated to 500°C. After the temperature stabilized, monosilane was introduced at 2 L / min for 95 minutes, and the pressure of the fluidized bed was controlled at 6 kPa. The introduction of monosilane gas was stopped, and inert gas was continued to be introduced until the reaction product was cooled to room temperature, obtaining a silicon-carbon composite material.

[0100] Example 3

[0101] In this embodiment, a silicon-carbon composite material is prepared, and the specific preparation process is as follows:

[0102] Specific surface area 1000m 2 / g, pore volume 0.2 cm 3 500 g of porous amorphous carbon material with a molecular weight of 1000 g / g was added to the fluidized bed, nitrogen gas was introduced at 10 L / min to fluidize the material, and the fluidized bed was heated to 500°C. After the temperature stabilized, monosilane was introduced at 5 L / min for 95 minutes, and the pressure of the fluidized bed was controlled at 6 kPa. The introduction of monosilane gas was stopped, and inert gas was continued to be introduced until the reaction product was cooled to room temperature, obtaining a silicon-carbon composite material.

[0103] Example 4

[0104] In this embodiment, a silicon-carbon composite material is prepared, and the specific preparation process is as follows:

[0105] Specific surface area 1200m 2 / g, pore volume 0.7 cm 3 500 g of porous amorphous carbon material with a molecular weight of 1000 g / g was added to the fluidized bed, nitrogen gas was introduced at 10 L / min to fluidize the material, and the fluidized bed was heated to 600°C. After the temperature stabilized, monosilane was introduced at 1 L / min for 60 minutes, and the pressure of the fluidized bed was controlled at 6 kPa. The introduction of monosilane gas was stopped, and inert gas was continued to be introduced until the reaction product was cooled to room temperature, obtaining a silicon-carbon composite material.

[0106] Comparative Example 1

[0107] In this embodiment, a silicon-carbon composite material is prepared, and the specific preparation process is as follows:

[0108] Specific surface area 1800m 2 / g, pore volume 0.68 cm 3 500 g of porous amorphous carbon material with a molecular weight of 1000 g / g was added to the fluidized bed, nitrogen gas was introduced at 10 L / min to fluidize the material, and the fluidized bed was heated to 500°C. After the temperature stabilized, monosilane was introduced at 1 L / min for 60 minutes, and the pressure of the fluidized bed was controlled at 6 kPa. The introduction of monosilane gas was stopped, and inert gas was continued to be introduced until the reaction product was cooled to room temperature, obtaining a silicon-carbon composite material.

[0109] Comparative Example 2

[0110] In this embodiment, a silicon-carbon composite material is prepared, and the specific preparation process is as follows:

[0111] Specific surface area 200m 2 / g, pore volume 0.4 cm 3 500 g of porous amorphous carbon material with a molecular weight of 1000 g / g was added to the fluidized bed, nitrogen gas was introduced at 10 L / min to fluidize the material, and the fluidized bed was heated to 500°C. After the temperature stabilized, monosilane was introduced at 1 L / min for 60 minutes, and the pressure of the fluidized bed was controlled at 6 kPa. The introduction of monosilane gas was stopped, and inert gas was continued to be introduced until the reaction product was cooled to room temperature, obtaining a silicon-carbon composite material.

[0112] Comparative Example 3

[0113] Specific surface area 1000m 2 / g, pore volume 0.12 cm 3500 g of porous amorphous carbon material with a molecular weight of 1000 g / g was added to the fluidized bed, nitrogen gas was introduced at 10 L / min to fluidize the material, and the fluidized bed was heated to 500°C. After the temperature stabilized, monosilane was introduced at 1 L / min for 60 minutes, and the pressure of the fluidized bed was controlled at 6 kPa. The introduction of monosilane gas was stopped, and inert gas was continued to be introduced until the reaction product was cooled to room temperature, obtaining a silicon-carbon composite material.

[0114] Example 5

[0115] In this example, lithium ion batteries were produced according to the following method using the silicon-carbon composite materials of Examples 1 to 4 and Comparative Examples 1 to 3. The specific steps are as follows.

[0116] 1. Preparation of Positive Electrode Sheet

[0117] Ternary material LiNi 0.8 Co 0.1 Mn 0.1 O2 was mixed at high speed to prepare a positive electrode active material mixed powder. Conductive carbon black (Super P), conductive carbon tubes (CNT), nitrogen methylpyrrolidone solvent (NMP), and polyvinylidene fluoride (PVDF) were dispersed in a mass ratio of 1:0.5:40 and stirred at high speed for 2 hours. The mixed active material powder and conductive slurry were mixed at high speed to prepare a positive electrode slurry with a predetermined viscosity. The prepared slurry was uniformly applied onto aluminum foil using a doctor blade, placed in a blower drying oven, and dried at 120 °C for 20 minutes. Finally, the dried electrode sheet was rolled and cut to prepare a positive electrode sheet.

[0118] 2. Preparation of negative electrode sheet

[0119] The prepared silicon-based material and graphite with a D50 of 10 μm were mixed at high speed in a mass ratio of 40:60 to prepare a negative electrode active material mixture powder. Next, Super P and PAA (polyacrylic acid) were mixed in an appropriate amount of deionized water in a mass ratio of 85:5:10 and thoroughly stirred to form a uniform negative electrode slurry. The negative electrode slurry was applied to the surface of the copper foil of the negative electrode current collector, dried, and cold pressed to obtain a negative electrode sheet.

[0120] 3. Preparation of electrolyte:

[0121] The organic solvent was a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC), with a volume ratio of EC, EMC and DEC of 20:20:60. In an argon atmosphere glove box with a water content of less than 10 ppm, completely dried lithium salt (LiPF6) was dissolved in the above organic solvent and mixed uniformly to obtain an electrolyte with a LiPF6 concentration of 1 mol / L.

[0122] 4. Preparation of insulating films:

[0123] A polypropylene insulating film with a thickness of 12 μm was selected.

[0124] 5. Battery Construction:

[0125] The positive electrode sheet, separator, and negative electrode sheet prepared as described above were laminated in order, and a separator was placed between the positive electrode sheet and the negative electrode sheet to provide insulation. Next, the outside was wrapped in aluminum plastic film, transferred to a vacuum oven and dried at 120°C, and 3.0g / Ah of electrolyte was injected and sealed. After leaving it to stand, hot and cold pressing, chemical formation, fixing, and grading, a pouch battery (i.e., a lithium-ion battery) with a capacity of 1Ah was finally obtained.

[0126] According to the following method, powder tests were carried out on the silicon-carbon composite materials of Examples 1 to 4 and Comparative Examples 1 to 3. Specifically, the methods are as follows.

[0127] 1. Test method for BET coefficient and pore volume:

[0128] The test sample (80mg~2g) was placed in the sample tube of the degassing tank, and nitrogen was added to the inside of the sample tube and heated at 300℃ for 1 hour to remove the gas adsorbed on the surface. After the degassing was completed and the test sample was cooled to room temperature, the quality of the test sample was measured and the weighed sample tube was placed in the analysis station. The Dewar vessel was filled with liquid nitrogen and the mass of the test sample was entered into the analysis file. The test parameters were set and the adsorption and desorption test process was carried out. The specific surface area, pore volume and other information of the material were calculated by the adsorption and desorption isotherm. Here, the specific surface area of ​​the porous carbon is B A The pore volume is P v1 The specific surface area of ​​the silicon-carbon composite material was B a The pore volume is P v2 It was decided.

[0129] 2.TG Test Method:

[0130] A 5 mg test sample was placed in the sample chamber and heated to 1400° C. at a rate of 10° C. / min under air atmosphere, and mass versus temperature curves were collected.

[0131] The initial mass was recorded as W0 and the mass after heating was recorded as W1. The weight loss was:

[0132] W loss=(W0-W1) / W0× 100%

[0133] Powder test results for Examples 1 to 4 and Comparative Examples 1 to 3

[0134] [Table 1]

[0135] The electrical characteristics of the lithium ion battery implemented in Example 5 were tested according to the following method as follows.

[0136] The mounted lithium-ion battery was charged to 4.2V at a constant current of 1C, then charged to 0.05C at a constant voltage of 4.2V and left for 10 minutes, then discharged to 2.8V at a constant current of 1C and left for 10 minutes. The above charge and discharge were cycles of the charge and discharge process, and the discharge capacity of this cycle was recorded. The charge and discharge process was repeated 100 times, and the discharge capacity of each cycle was recorded.

[0137] Cycle capacity retention rate (%) = 100th cycle discharge capacity / 1st cycle discharge capacity × 100%

[0138] Mass energy density of battery (Wh / kg) = first discharge energy / battery mass.

[0139] Electrical performance test results of lithium ion batteries manufactured from the powders of Examples 1 to 4 and Comparative Examples 1 to 3

[0140] [Table 2]

[0141] In Table 1, the W loss is mainly due to carbon, i.e. the actual silicon content is 1-W loss.

[0142] From the data analysis of Tables 1 and 2, it can be seen that in the manufacturing process of silicon-carbon composites, the loading amount of silicon is determined according to the specific surface area and pore volume of the porous amorphous carbon. If the specific surface area is large and the pore volume is large, silicon will precipitate in the pores. However, if the specific surface area and pore volume are too large, the amount of silicon will increase and circulation will be poor. If the specific surface area is large and the pore volume is small, silicon will precipitate on the surface and circulation will be difficult. If the specific surface area is small and the pore volume is large, the amount of silicon precipitation will be limited, silicon will be easily agglomerated, and circulation will be difficult. If the specific surface area is small and the pore volume is small, silicon cannot be precipitated, and volume loss will be large.

[0143] The lithium ion batteries produced using the silicon-carbon composite materials of Examples 1 to 4 have higher cycle capacity and cycle capacity retention rates of 90% or more in all cases, compared to the lithium ion batteries produced using the silicon-carbon composite materials of Comparative Examples 1 and 3. This is because the amount of silicon filled is determined by the specific surface area and pore volume of the porous amorphous carbon in the manufacturing process of the silicon-carbon composite material. If the specific surface area is large and the pore volume is large, silicon precipitates in the pores. However, if the specific surface area and pore volume are too large, silicon becomes too much and circulation becomes poor. If the specific surface area is large and the pore volume is small, silicon precipitates on the surface and circulation becomes difficult. If the specific surface area is small and the pore volume is large, the amount of silicon precipitated is limited, silicon is easily aggregated, and circulation becomes difficult. If the specific surface area is small and the pore volume is small, silicon cannot precipitate, and capacity loss becomes large.

[0144] The lithium ion battery produced using the silicon-carbon composite material of Comparative Example 2 has a cycle capacity retention rate of 95.4%, but the mass energy density is significantly lower than those of Examples 1 to 4. This is because the specific surface area of ​​the porous amorphous carbon and the BET coefficient of the composite material are too small, so that the active sites for silicon to be introduced are reduced, the amount of silicon added is reduced, and the capacity of the final product is reduced, making it difficult to achieve a higher energy density of the battery cell.

[0145] The weight loss due to thermal decomposition of the silicon-carbon composite material of Comparative Example 1 is low compared to Examples 1 to 4. Correspondingly, the cycle capacity retention rate of the lithium ion battery obtained by using the silicon-carbon composite material of Comparative Example 1 is significantly lower than those of Examples 1 to 4. This is because the Si content is too high, making it difficult to achieve better cycle performance.

[0146] In summary, the embodiments of the present invention provide a silicon-carbon composite structure, specific surface area coefficient B, pore volume coefficient P vBy controlling the content of various elements and the weight loss due to thermal decomposition, the expansion of the silicon-based material can be suppressed to the maximum extent, and long-term cycle stability and excellent electrical conductivity can be ensured, thereby effectively improving the capacity and initial efficiency of the final material, and promoting the commercialization process of silicon-based negative electrode materials while maintaining a certain processing performance. At the same time, the method for producing the silicon-carbon composite material of the present invention is simple and easy to operate. It is suitable for large-scale industrial production. The silicon-carbon composite material provided in the present invention is used as a negative electrode active material, and is applied to a negative electrode active material layer to prepare a negative electrode sheet, which is then assembled with a positive electrode sheet, a separator, an electrolyte, etc. to form a lithium ion battery, which can greatly improve the electrical performance of the lithium ion battery and promote the development of lithium ion batteries. [Industrial Applicability]

[0147] The silicon-carbon composite material and its manufacturing method, anode sheet, electrochemical device and electronic device of the present invention can facilitate the commercialization process of silicon-based anode materials, and are suitable for large-scale industrial production.

[0148] The above-described embodiments are illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Those skilled in the art may modify or change the above-described embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those skilled in the art without departing from the spirit and technical ideas disclosed in the present invention are still intended to be included in the scope of the claims of the present invention.

Claims

1. an amorphous carbon matrix and a silicon material located on and / or within the amorphous carbon matrix; A silicon-carbon composite material that satisfies the following relationship: B=B A / B a The value range of B is 20 to 1250. B is the specific surface area coefficient of the silicon-carbon composite material, and B A is the specific surface area of ​​the amorphous carbon matrix, B a is the specific surface area of ​​the silicon-carbon composite material.

2. The silicon-carbon composite material of claim 1 , which satisfies at least one of the following conditions (a) to (c): (a) the specific surface area coefficient B of the silicon-carbon composite material is in the range of 100 to 900; (b) the specific surface area B of the amorphous carbon matrix A The range is 500m 2 / g~2500m 2 / g. (c) the specific surface area B of the silicon-carbon composite material a The range is 2m 2 / g to 25m 2 / g.

3. The silicon-carbon composite material according to claim 1 , which satisfies at least one of the following conditions (I) to (II): (I) The silicon-carbon composite material satisfies the following relationship: P v =P v1 / P v2 P v The value range is 0.4 to 120. In the formula, P v represents the pore volume coefficient of the silicon-carbon composite material, P v1 represents the pore volume diameter of the amorphous carbon matrix, P v2 represents the pore volume diameter of the silicon-carbon composite material. (II) When heated to 1400° C. in an air atmosphere, the weight loss due to pyrolysis of the silicon-carbon composite material ranges from 5% to 60%.

4. The silicon-carbon composite material of claim 3, which satisfies at least one of the following conditions (d) to (f): (d) the pore volume coefficient P of the silicon-carbon composite material v The range is 1 to 100. (e) the pore volume diameter P of the amorphous carbon matrix v1 The range is 0.2 cm 3 / g ~ 0.9 cm 3 / g. (f) the pore volume diameter P of the silicon-carbon composite material v2 The range is 0.005 cm 3 / g to 0.2 cm 3 / g.

5. 10. The silicon-carbon composite of claim 1, further comprising nanometal particles attached to the surface and / or the interior of the amorphous carbon matrix.

6. 1. A method for producing a silicon-carbon composite material, comprising synthesizing an amorphous carbon matrix material and a silicon source by chemical vapor deposition to obtain a silicon-carbon composite material, comprising: the silicon-carbon composite material comprises an amorphous carbon matrix and a silicon material located on and / or within the amorphous carbon matrix; The method for producing a silicon-carbon composite material, wherein the silicon-carbon composite material satisfies the following relationship: B=B A / B a The value range of B is 20 to 1250. B is the specific surface area coefficient of the silicon-carbon composite material, and B A is the specific surface area of ​​the amorphous carbon matrix, B a is the specific surface area of ​​the silicon-carbon composite material.

7. The method for producing a silicon-carbon composite material according to claim 6, which satisfies at least one of the following conditions (1) to (2): (1) The silicon source is at least one selected from the group consisting of monosilane, dimethyldichlorosilane, and trichloromethylsilane. (2) The amorphous carbon matrix material is at least one selected from the group consisting of porous amorphous carbon and porous amorphous carbon-metal composites.

8. A positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator, an anode sheet comprising an anode current collector and an anode active material layer disposed on the anode current collector, the anode active material layer comprising an anode active material, the anode active material comprising the silicon-carbon composite material according to any one of claims 1 to 5. An electrochemical device.

9. An electronic device comprising the electrochemical device according to claim 8.

Citation Information

Patent Citations

  • Electroactive materials for metal-ion batteries

    WO2022029422A1

Cited By

  • Negative electrode active material, manufacturing method of negative electrode active material, negative electrode composition, negative electrode for lithium secondary battery comprising same, and lithium secondary battery comprising negative electrode

    KR103048322B1

  • Anode active material, preparation method for anode active material, anode composition, anode for lithium secondary battery comprising same, and lithium secondary battery comprising anode