Thermosetting resin, cured product thereof, and thermosetting composition
A thermosetting resin with monovinyl, divinyl, and aromatic ring-fused cyclic olefin units addresses the balance of dielectric properties and glass transition temperature, enhancing processability and suitability for electronic materials.
Patent Information
- Application Number
- JP2023216007
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-12-21
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional thermosetting resins face challenges in achieving a balance between dielectric properties, glass transition temperature, and low melt viscosity, with many exhibiting poor processability.
A thermosetting resin composed of repeating units derived from monovinyl aromatic compounds, divinyl aromatic compounds, and aromatic ring-fused cyclic olefin compounds, with specific molecular arrangements and contents to enhance dielectric properties and reduce melt viscosity.
The resin achieves both excellent dielectric properties and glass transition temperature while maintaining low melt viscosity, enabling improved processability and suitability for electronic materials.
Smart Images

Figure 2024139678000001 
Figure 2024139678000002 
Figure 2024139678000003
Abstract
Description
[Technical field]
[0001] FIELD OF THEINVENTION The present invention relates to a thermosetting resin and a cured product thereof, and also to a thermosetting composition containing the thermosetting resin. [Background technology]
[0002] In recent years, electronic devices have become smaller and more powerful, and the performance requirements for the materials used in them are increasing accordingly. For example, there is a demand for printed circuit board materials with low dielectric tangents that can be used for high-frequency communications.
[0003] Patent Document 1 discloses a thermosetting resin composition having excellent dielectric properties, heat resistance, adhesion and moisture resistance, which contains a copolymer containing an acenaphthylene-based structural unit and a hydroxystyrene-based structural unit, a compound having at least two epoxy groups in one molecule, and a curing agent. Patent Document 1 discloses a copolymer of styrene, pt-butoxystyrene, divinylbenzene and acenaphthylene as a specific example of the copolymer, which has a branched chain.
[0004] Patent Document 2 discloses a copolymer that provides a curable composition excellent in heat resistance, compatibility, dielectric properties, wet heat reliability, and thermal oxidation deterioration resistance, and contains a structural unit derived from a divinyl aromatic compound, a structural unit derived from a monovinyl aromatic compound, and a structural unit derived from a cycloolefin compound. In Patent Document 2, the copolymer is polymerized using a mixed liquid of a divinyl aromatic compound, a monovinyl aromatic compound, and a cycloolefin compound, and therefore the obtained copolymer has a branched chain. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-192539 A [Patent Document 2] JP 2018-039995 A Summary of the Invention [Problem to be solved by the invention]
[0006] Conventional thermosetting resins are not necessarily satisfactory in terms of dielectric properties, and even those with excellent dielectric properties have problems such as a low glass transition temperature and high melt viscosity, resulting in poor processability.
[0007] In view of the above, an object of an embodiment of the present invention is to provide a thermosetting resin that can achieve both dielectric properties and glass transition temperature and has a low melt viscosity. [Means for solving the problem]
[0008] The present invention includes the embodiments set forth below. [1] A thermosetting resin that is a linear copolymer having a repeating unit corresponding to a monovinyl aromatic compound, a repeating unit corresponding to a divinyl aromatic compound, and a repeating unit corresponding to an aromatic ring-fused cyclic olefin compound. [2] The thermosetting resin according to [1], wherein the content of the repeating units corresponding to the aromatic ring-fused cyclic olefin compound is 5 to 80 mol % in 100 mol % of all repeating units. [3] The linear copolymer has a terminal end having the general formula (1): R 1 -N=NR 2 In the general formula (1), R 1 and R 2 each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group. [4] The thermosetting resin according to any one of [1] to [3], wherein the total content of the repeating units corresponding to the monovinyl aromatic compound, the repeating units corresponding to the divinyl aromatic compound, and the repeating units corresponding to the aromatic-ring-fused cyclic olefin compound is 80 mol % or more, based on 100 mol % of all repeating units. [5] The thermosetting resin according to any one of [1] to [4], wherein the aromatic ring-fused cyclic olefin compound has 3 or less rings. [6] A cured product obtained by curing the thermosetting resin according to any one of [1] to [5]. [7] A thermosetting composition comprising the thermosetting resin according to any one of [1] to [5]. [8] The thermosetting composition according to [7], which is a printed circuit board material. Effect of the Invention
[0009] According to an embodiment of the present invention, a thermosetting resin that can achieve both dielectric properties and glass transition temperature and has a low melt viscosity can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The thermosetting resin according to this embodiment is a copolymer having (A) a repeating unit corresponding to a monovinyl aromatic compound, (B) a repeating unit corresponding to a divinyl aromatic compound, and (C) a repeating unit corresponding to an aromatic ring-fused cyclic olefin compound.
[0011] The repeating unit corresponding to the monovinyl aromatic compound of (A) (hereinafter also referred to as "monovinyl aromatic compound unit") is a structural unit of the copolymer, and is a structural unit having a structure formed by addition polymerization of a monovinyl aromatic compound as a monomer. The repeating unit is not necessarily limited to one obtained by polymerization using the monovinyl aromatic compound, as long as it has a structure corresponding to the monovinyl aromatic compound, and may be one that is further reacted after polymerization to form a structure corresponding to the monovinyl aromatic compound.
[0012] The monovinyl aromatic compound unit may be a repeating unit having a structure in which the vinyl group of a monovinyl aromatic compound becomes a single bond through addition polymerization, as represented by the following general formula (2). [ka]
[0013] In formula (2), R 3 represents a monovalent aromatic hydrocarbon group having 6 to 30 carbon atoms. 3 is a monovalent aromatic hydrocarbon group having 6 to 30 carbon atoms (more preferably 6 to 20 carbon atoms) selected from the group consisting of a phenyl group which may have a substituent, a biphenylyl group which may have a substituent, a naphthyl group which may have a substituent, and a terphenylyl group which may have a substituent. 3 When R has a substituent such as an alkyl group, the number of carbon atoms in the substituent is included in the number of carbon atoms in the substituent. 3 The total number of carbon atoms.
[0014] The monovinyl aromatic compound forming such a repeating unit may be any aromatic compound having one vinyl group, and examples thereof include vinyl aromatic compounds such as styrene, vinylnaphthalene, and vinylbiphenyl, and nuclear alkyl-substituted vinyl aromatic compounds such as alkylstyrenes (e.g., o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, and p-ethylstyrene), dialkylstyrenes (e.g., 3,5-dimethylstyrene, 2,5-dimethylstyrene, and 2,5-diethylstyrene), alkylvinylbiphenyls (e.g., ethylvinylbiphenyl), and alkylvinylnaphthalenes (e.g., ethylvinylnaphthalene), and any of these may be used alone or in combination of two or more.
[0015] In one embodiment, the monovinyl aromatic compound preferably contains at least one (A1) selected from the group consisting of styrene, vinylnaphthalene, vinylbiphenyl, alkylstyrene, dialkylstyrene, alkylvinylbiphenyl, and alkylvinylnaphthalene. In this case, the amount of repeating units corresponding to the at least one (A1) in 100 mol% of the monovinyl aromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.
[0016] In one embodiment, the monovinyl aromatic compound preferably contains styrene. In this case, the amount of repeating units corresponding to styrene (hereinafter also referred to as "styrene units") in 100 mol% of the monovinyl aromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.
[0017] The repeating unit corresponding to the divinylaromatic compound of (B) (hereinafter also referred to as "divinylaromatic compound unit") is a structural unit of the copolymer, and is a structural unit having a structure with one vinyl group formed by addition polymerization of a divinylaromatic compound as a monomer. The repeating unit is not necessarily limited to one obtained by polymerization using the divinylaromatic compound, as long as it has a structure corresponding to the divinylaromatic compound, and may be one that is further reacted after polymerization to form a structure corresponding to the divinylaromatic compound.
[0018] The divinylaromatic compound unit may be a repeating unit having a structure in which one vinyl group of the divinylaromatic compound is converted into a single bond by addition polymerization, as represented by the following general formula (3). [ka]
[0019] In formula (3), R 4 represents a divalent aromatic hydrocarbon group having 6 to 30 carbon atoms. 4 is a divalent aromatic hydrocarbon group having 6 to 30 carbon atoms (more preferably 6 to 20 carbon atoms) selected from the group consisting of a phenylene group which may have a substituent, a biphenyldiyl group which may have a substituent, a naphthylene group which may have a substituent, and a terphenyldiyl group which may have a substituent. 4 When R has a substituent such as an alkyl group, the number of carbon atoms in the substituent is included in the number of carbon atoms in the substituent. 4 The total number of carbon atoms.
[0020] The divinyl aromatic compound forming such a repeating unit may be any aromatic compound having two vinyl groups, such as divinylbenzene (including each positional isomer or a mixture thereof), divinylnaphthalene (including each positional isomer or a mixture thereof), and divinylbiphenyl (including each positional isomer or a mixture thereof), and any one of these may be used alone or in combination of two or more.
[0021] In one embodiment, the divinylaromatic compound preferably contains at least one (B1) selected from the group consisting of divinylbenzene, divinylnaphthalene, and divinylbiphenyl. In this case, the amount of repeating units corresponding to the at least one (B1) in 100 mol% of the divinylaromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.
[0022] In one embodiment, the divinylaromatic compound preferably contains divinylbenzene (m-isomer, p-isomer, or a mixture of positional isomers thereof). In this case, the amount of repeating units corresponding to divinylbenzene (hereinafter also referred to as "divinylbenzene units") in 100 mol% of the divinylaromatic compound units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.
[0023] The repeating unit (hereinafter also referred to as "cyclic olefin unit") corresponding to the aromatic ring-fused cyclic olefin compound of (C) above is a constituent unit of the copolymer, and is a constituent unit having a structure formed by addition polymerization of an aromatic ring-fused cyclic olefin compound as a monomer. The repeating unit is not necessarily limited to one obtained by polymerization using the aromatic ring-fused cyclic olefin compound, so long as it has a structure corresponding to the aromatic ring-fused cyclic olefin compound, and may be one that is further reacted after polymerization to form a structure corresponding to the aromatic ring-fused cyclic olefin compound.
[0024] The aromatic ring fused cyclic olefin compound is a cyclic olefin compound in which an aromatic ring is fused, and more specifically, a compound having a fused ring of an aliphatic ring having a carbon-carbon double bond and an aromatic ring. The condensation may be ortho-condensation or ortho-peri-condensation. Examples of the aromatic ring fused cyclic olefin compound include indene-based compounds, acenaphthylene-based compounds, phenalene-based compounds, acephenanthrylene-based compounds, aceanthrylene-based compounds, benzofuran-based compounds, and benzothiophene-based compounds, and any one or more of these may be used in combination. Among these, the aromatic ring fused cyclic olefin compound is preferably one having three or less rings. Specifically, the aromatic ring fused cyclic olefin compound is preferably one having two rings, such as indene-based compounds, benzofuran-based compounds, and benzothiophene-based compounds; the aromatic ring fused cyclic olefin compound is preferably one having three rings, such as acenaphthylene-based compounds and phenalene-based compounds, and more preferably one having indene-based compounds and / or acenaphthylene-based compounds.
[0025] In one embodiment, the aromatic ring-fused cyclic olefin compound preferably contains at least one (C1) selected from the group consisting of indene-based compounds, acenaphthylene-based compounds, phenalene-based compounds, acephenanthrylene-based compounds, aceanthrylene-based compounds, benzofuran-based compounds, and benzothiophene-based compounds. In this case, the amount of repeating units corresponding to the at least one (C1) in 100 mol% of cyclic olefin units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.
[0026] The indene-based compound may, for example, be at least one selected from the group consisting of indene, alkylindene, halogenated indene, arylindene, and alkoxyindene.
[0027] The acenaphthylene-based compound may be, for example, at least one selected from the group consisting of acenaphthylene, alkylacenaphthylene, halogenated acenaphthylene, arylacenaphthylene, and alkoxyacenaphthylene.
[0028] As for the phenalene-based compounds, acephenanthrylene-based compounds, aceanthrylene-based compounds, benzofuran-based compounds, and benzothiophene-based compounds, in addition to phenalene, acephenanthrylene, aceanthrylene, benzofuran, and benzothiophene, examples thereof include compounds having the same substituents as the above-mentioned indene-based compounds.
[0029] In one embodiment, the cyclic olefin unit includes a repeating unit represented by the following general formula (4). [ka]
[0030] In formula (4), R 5 and R 6 each independently represents an alkyl group having 1 to 20 carbon atoms, a halogen atom, an aryl group having 6 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms. m and n each independently represent an integer of 0 to 3. When m and n are 2 or more, R 5 and R 6 may be the same or different.
[0031] The aromatic ring-fused cyclic olefin compound forming the repeating unit of formula (4) is an acenaphthylene-based compound represented by the following general formula (5). [ka] R in Equation (5) 5 , R 6 , m and n are R in formula (4). 5 , R 6 , m and n.
[0032] In one embodiment, the aromatic ring-fused cyclic olefin compound preferably contains an acenaphthylene-based compound represented by the above formula (5), more preferably contains acenaphthylene. In this case, the amount of the repeating unit represented by formula (4) (preferably a repeating unit corresponding to acenaphthylene (hereinafter also referred to as "acenaphthylene unit")) in 100 mol% of the cyclic olefin units is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, and may be 100 mol%.
[0033] The thermosetting resin according to the present embodiment is a linear copolymer having the above three repeating units. The linear structure causes molecular chain entanglement, improving moldability. Here, linear refers to a structure in which the repeating units constituting the copolymer are linked together in a one-dimensional chain shape and bonded to each other, and refers to a structure without a cross-linked structure.
[0034] In the thermosetting resin, the monovinyl aromatic compound units, the divinylaromatic compound units and the cyclic olefin units may be arranged in a regular order or in a random order, and the thermosetting resin is preferably a random copolymer in which the monovinyl aromatic compound units, the divinylaromatic compound units and the cyclic olefin units are arranged in a random order.
[0035] In addition to the monovinyl aromatic compound unit, the divinyl aromatic compound unit, and the cyclic olefin unit, the thermosetting resin may contain repeating units corresponding to other monomers, such as trivinyl aromatic compounds, trivinyl aliphatic compounds, divinyl aliphatic compounds, and monovinyl aliphatic compounds, to the extent that the effect of the thermosetting resin is not impaired.
[0036] In the thermosetting resin, the content of the monovinyl aromatic compound unit is not particularly limited, but is preferably 15 to 90 mol% out of 100 mol% of all repeating units constituting the copolymer. By being 15 mol% or more, the effect of reducing the melt viscosity is excellent. The content of the monovinyl aromatic compound unit is more preferably 30 to 80 mol%, further preferably 40 to 75 mol%, and further preferably 50 to 70 mol%. In this specification, the total repeating units of 100 mol% does not include the structure derived from the polymerization initiator present at the end of the copolymer.
[0037] In the thermosetting resin, the content of the divinyl aromatic compound unit is not particularly limited, but is preferably 3 to 30 mol% in 100 mol% of all repeating units constituting the copolymer. By having a content of 3 mol% or more, it is possible to improve the thermosetting property to obtain a good cured product, and also to improve the glass transition temperature. The content of the divinyl aromatic compound unit is more preferably 5 to 25 mol%, further preferably 8 to 22 mol%, and further preferably 10 to 20 mol%.
[0038] In the thermosetting resin, the content of the cyclic olefin unit is not particularly limited, but is preferably 5 to 80 mol % relative to 100 mol % of all repeating units constituting the copolymer. When it is 5 mol % or more, the effect of improving the glass transition temperature is excellent. When it is 80 mol % or less, the effect of reducing the melt viscosity is excellent. The content of the cyclic olefin unit is more preferably 7 to 50 mol %, further preferably 8 to 35 mol %, and further preferably 10 to 30 mol %.
[0039] The total content of the monovinyl aromatic compound units, divinyl aromatic compound units and cyclic olefin units is preferably 80 mol % or more, more preferably 90 mol % or more, and may be 100 mol %, based on 100 mol % of all repeating units constituting the copolymer.
[0040] In one embodiment, the thermosetting resin is preferably a copolymer having a repeating unit represented by the above formula (2) (preferably a styrene unit), a repeating unit represented by the above formula (3) (preferably a divinylbenzene unit), and a repeating unit represented by the above formula (4) (preferably an acenaphthylene unit). In this case, the thermosetting resin preferably contains each repeating unit as follows, with the total repeating units constituting the copolymer being 100 mol %. In this case, the thermosetting resin may contain, together with these repeating units, the repeating units (A), (B), or (C) other than the repeating units. Repeating units represented by formula (2) (preferably styrene units): 15 to 90 mol %, preferably 30 to 80 mol %, more preferably 40 to 75 mol %, and even more preferably 50 to 70 mol %. Repeating units represented by formula (3) (preferably divinylbenzene units): 3 to 30 mol %, preferably 5 to 25 mol %, more preferably 8 to 22 mol %, and even more preferably 10 to 20 mol %. Repeating units represented by formula (4) (preferably acenaphthylene units): 5 to 80 mol %, preferably 7 to 50 mol %, more preferably 8 to 35 mol %, and even more preferably 10 to 30 mol %.
[0041] The thermosetting resin may have at least one of a structure derived from a polymerization initiator represented by the following general formula (1) or a structure derived from a polymerization initiator represented by the following general formula (6) at the end of a linear copolymer. The polymerization initiator represented by formula (1) is an azo initiator having no cyano group, unlike azobisisobutyronitrile (AIBN), which is a general-purpose azo initiator. The polymerization initiator represented by formula (6) is an organic peroxide such as dialkyl peroxide. By using the polymerization initiator represented by formula (1) among these, better dielectric properties can be imparted. R 1 -N=NR 2 (1) R 7 -OOR 8 (6)
[0042] In formula (1) and formula (6), R1 , R 2 , R 7 and R 8 each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group, and does not contain a heteroatom. The number of carbon atoms in the saturated hydrocarbon group is not particularly limited, but is preferably 1 to 23, and more preferably 4 to 13. The number of carbon atoms in the aromatic hydrocarbon group is not particularly limited, but is preferably 6 to 23, and more preferably 6 to 13.
[0043] The saturated hydrocarbon group may be a branched or straight-chain saturated aliphatic hydrocarbon group (alkyl group) or a saturated alicyclic hydrocarbon group. Specific examples of the saturated hydrocarbon group include alkyl groups such as tert-butyl group, tert-pentyl group, tert-hexyl group, and 1,1,3,3-tetramethylbutyl group, and saturated alicyclic hydrocarbon groups such as cyclohexyl group.
[0044] Specific examples of the aromatic hydrocarbon group include aryl groups such as a phenyl group, a tolyl group, and a naphthyl group, a cumyl group, a benzyl group, and a phenethyl group. base Examples of aralkyl groups include the following.
[0045] In one embodiment, R 1 , R 2 , R 7 and R 8 may each independently be a group represented by the following general formula (7): [ka]
[0046] In formula (7), R 9 , R 10 and R 11 each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group. More preferably, R 9 represents a monovalent saturated hydrocarbon group having 1 to 20 carbon atoms (more preferably 1 to 10 carbon atoms) or a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms (more preferably 6 to 10 carbon atoms); R 10 and R 11R represents a methyl group. 9 , R 10 and R 11 (Preferably R 9 The saturated hydrocarbon group for R may be branched or linear, and examples thereof include alkyl groups such as methyl, ethyl, propyl, butyl, heptyl, isopropyl, tert-butyl, and 2,2-dimethylpropyl, and saturated alicyclic hydrocarbon groups such as cyclohexyl. 9 , R 10 and R 11 (Preferably R 9 ) Aromatic hydrocarbons include a phenyl group, a tolyl group, a naphthyl group, and the like.
[0047] When a vinyl copolymer is synthesized by radical polymerization using these polymerization initiators, both ends of the obtained vinyl copolymer usually have a structure derived from the polymerization initiator. 1 - and / or R 2 - at both ends of the copolymer. 1 -But it's okay, both are R 2 - is also acceptable, and one end is R 1 - and the other end is R 2 On the other hand, when polymerization is performed using the polymerization initiator of the above formula (6), R 7 O- and / or R 8 A copolymer having O- at both ends is obtained. In other words, both ends of the copolymer are R 7 O- is also acceptable, both are R 8 O- is also acceptable, and one end is R 7 O- and the other end is R 8 O- is also acceptable.
[0048] The weight average molecular weight Mw of the thermosetting resin is not particularly limited, and may be, for example, 1,000 to 100,000, 2,000 to 50,000, or 3,000 to 20,000. When the weight average molecular weight Mw is 1,000 or more, the concentration of terminal groups derived from the polymerization initiator can be reduced, thereby improving the dielectric properties. Furthermore, when the weight average molecular weight Mw is 100,000 or less, the melt viscosity can be reduced. Here, the weight average molecular weight Mw is a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).
[0049] The method for producing the thermosetting resin is not particularly limited. As a method for synthesizing a linear copolymer, in a preferred embodiment of the production method, a vinylbenzylphosphonium salt, a monovinyl aromatic compound, and an aromatic ring condensed cyclic olefin compound are copolymerized using at least one of the polymerization initiator represented by the above formula (1) or the polymerization initiator represented by the formula (6), and the obtained copolymer is reacted with formaldehyde. However, the production method is not limited to this method.
[0050] As the vinylbenzyl phosphonium salt, it is preferable to use vinylbenzyl phosphonium halide.As the phosphonium group in the vinylbenzyl phosphonium salt, for example, quaternary phosphonium groups such as trialkyl phosphonium, triaryl phosphonium, and triaryl alkyl phosphonium can be mentioned.In addition, as the halogen that forms a salt with the phosphonium group, for example, chlorine, bromine, etc. can be mentioned.
[0051] The vinylbenzylphosphonium salt can be copolymerized with a monovinyl aromatic compound and an aromatic ring condensed cyclic olefin compound by a known vinyl polymerization method. By using the radical polymerization initiator represented by the above formula (1) and / or formula (6) as a polymerization initiator, a copolymer having a repeating unit derived from a vinylbenzylphosphonium salt, a repeating unit derived from a monovinyl aromatic compound, and a repeating unit derived from an aromatic ring condensed cyclic olefin compound can be obtained. During polymerization, a chain transfer agent may be added to adjust the molecular weight of the copolymer.
[0052] The method for reacting the obtained copolymer with formaldehyde can be the well-known Wittig reaction, in which the copolymer is treated with a base and then reacted with formaldehyde, whereby the phosphonium group is removed and a vinyl group is introduced.
[0053] In this production method, since the vinylbenzyl phosphonium salt is monovinyl in the copolymerization step, a linear copolymer without branches can be obtained, and since a vinyl group is introduced into the repeating unit derived from the vinylbenzyl phosphonium salt after copolymerization, a linear copolymer without branches can be obtained while having a repeating unit corresponding to the divinyl aromatic compound.
[0054] The thermosetting composition according to the present embodiment contains the thermosetting resin. The content of the thermosetting resin in the thermosetting composition is not particularly limited as long as the composition has the property of being cured by heat. For example, the content may be 1 to 99% by mass or 10 to 95% by mass relative to 100% by mass of the solid content of the thermosetting composition (the amount excluding the organic solvent when the organic solvent described below is contained, and the amount of the entire composition when the organic solvent is not contained).
[0055] In addition to the above-mentioned thermosetting resin, the thermosetting composition may contain various components such as other thermosetting resins (thermosetting crosslinking agents), thermoplastic resins, fillers, flame retardants, curing accelerators, polymerization initiators, defoamers, heat stabilizers, antistatic agents, ultraviolet absorbers, colorants such as dyes and pigments, lubricants, and dispersants.
[0056] The thermosetting composition may contain an organic solvent to adjust its viscosity, and the thermosetting composition may be a solution containing the thermosetting resin. The organic solvent used may be one capable of dissolving the thermosetting resin, and examples of the organic solvent include ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, esters such as ethyl acetate, propyl acetate, and butyl acetate, amides such as dimethylacetamide and dimethylformamide, and aromatic hydrocarbons such as toluene and xylene, and any one or more of these may be used in combination.
[0057] The thermosetting resin or thermosetting composition of the present embodiment has a vinyl group in the molecular chain of the copolymer, and therefore can be crosslinked by polymerization, and a cured product can be obtained by thermal curing. The cured product has a low dielectric tangent and dielectric constant and excellent dielectric properties, and can be used for electronic materials such as printed circuit board materials and semiconductor sealing materials. That is, the thermosetting composition according to one embodiment is a thermosetting composition for electronic materials.
[0058] Examples of the printed circuit board material include rigid printed circuit board materials such as single-sided boards, double-sided boards, multilayer boards, and build-up boards, and film- or sheet-shaped flexible printed circuit board materials. In addition, because of its excellent dielectric properties, it is suitably used as a high-frequency board material for use in high-frequency communication devices. EXAMPLES
[0059] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0060] <Measurement and evaluation methods> [Molar ratio of styrene / divinylbenzene / acenaphthylene] The products and compositions obtained in Examples 1 to 9, 11 to 13, and Comparative Examples 1, 4 to 6, and 9 were dissolved in deuterated chloroform and analyzed by a nuclear magnetic resonance spectrometer (JEOL). 1H-NMR measurement was carried out to determine the molar ratios of the repeating units corresponding to styrene, the repeating units corresponding to divinylbenzene, and the repeating units to acenaphthylene, and the content of the repeating units corresponding to styrene (styrene ratio), the content of the repeating units corresponding to divinylbenzene (divinylbenzene ratio), and the content of the repeating units corresponding to acenaphthylene (acenaphthylene ratio) relative to 100 mol% of all repeating units were calculated.
[0061] [Molar ratio of styrene / divinylbenzene / acenaphthylene / vinylcyclohexane] The products obtained in Example 10, Comparative Examples 2 and 7 were dissolved in deuterated chloroform and analyzed by a nuclear magnetic resonance spectrometer (JEOL). 1 H-NMR measurement was carried out to determine the molar ratios of repeating units corresponding to styrene, repeating units corresponding to divinylbenzene, repeating units relative to acenaphthylene, and repeating units relative to vinylcyclohexane, and the content of repeating units corresponding to styrene relative to 100 mol% of all repeating units (styrene ratio), the content of repeating units corresponding to divinylbenzene (divinylbenzene ratio), the content of repeating units corresponding to acenaphthylene (acenaphthylene ratio), and the content of repeating units corresponding to vinylcyclohexane (vinylcyclohexane ratio) were calculated.
[0062] [Molar ratio of styrene / divinylbenzene / isobornyl acrylate] The products obtained in Comparative Examples 3 and 8 were dissolved in deuterated chloroform and analyzed by a nuclear magnetic resonance spectrometer (JEOL). 1 H-NMR measurement was carried out to determine the molar ratios of the repeating units corresponding to styrene, the repeating units corresponding to divinylbenzene, and the repeating units corresponding to isobornyl acrylate, and the content of the repeating units corresponding to styrene (styrene ratio), the content of the repeating units corresponding to divinylbenzene (divinylbenzene ratio), and the content of the repeating units corresponding to isobornyl acrylate (isobornyl acrylate ratio) relative to 100 mol% of all repeating units were calculated.
[0063] [Weight average molecular weight] The products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 9 were dissolved in tetrahydrofuran, and the weight average molecular weight Mw in terms of polystyrene was measured by gel permeation chromatography (GPC) (Prominence, Shimadzu Corporation) connected to four columns (Shodex GPC columns KF-601, KF-602, KF-603, KF-604, Showa Denko Corporation) filled with polystyrene gel. A differential refractive index detector (Shodex RI-504, Showa Denko Corporation) was used, with the column oven temperature at 40°C, the THF flow rate at 0.6 mL / min, the sample concentration at 0.1 mass%, and the sample injection amount at 10 μL.
[0064] [Dielectric constant, dielectric loss tangent] The products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 9 were used as samples. Using a single-action compression molding machine for testing (manufactured by Yasuda Seiki Seisakusho), 1.5 g of sample was pressed for 15 minutes at a pressure of 10 MPa and a temperature of 220°C to produce a flat plate of 30 mm x 30 mm x 1 mm thickness. The obtained flat plate was cut to produce a test piece of 2 mm width, 1 mm thickness, and 30 mm length. The dielectric constant and dielectric loss tangent of the test piece at 10 GHz were measured using a cavity resonator method dielectric constant measuring device (manufactured by KEYSIGHT), and evaluated according to the following criteria.
[0065] Those with a dielectric constant of less than 2.4 were rated as "A" (excellent), those between 2.4 and 2.5 were rated as "B" (good), those between 2.5 and 2.6 were rated as "C" (fair), those between 2.6 and 2.7 were rated as "D" (poor), and those above 2.7 were rated as "E" (poor).
[0066] Those with a dielectric tangent of less than 0.001 were rated as "A" (excellent), those between 0.001 and 0.002 were rated as "B" (good), those between 0.002 and 0.003 were rated as "C" (fair), those between 0.003 and 0.004 were rated as "D" (poor), and those 0.004 or greater were rated as "E" (poor).
[0067] [Glass transition temperature Tg] The flat plate prepared according to the above [dielectric constant, dielectric tangent] was cut to prepare a test piece with a width of 5 mm, a thickness of 1 mm, and a length of 25 mm. The glass transition temperature of this test piece was measured using a dynamic viscoelasticity measuring device: Rheogel-E4000 (manufactured by UBM Co., Ltd.). The maximum value of the loss tangent (tan δ) measured for the test piece under the conditions of a tensile sine wave, dynamic strain of 5 μm, frequency of 1 Hz, and temperature rise rate of 3 ° C. / min was determined as the glass transition temperature. Glass transition temperatures of 180 ° C. or higher were rated as "A" (excellent), those of 170 ° C. or higher and lower than 180 ° C. were rated as "B" (good), those of 160 ° C. or higher and lower than 170 ° C. were rated as "C" (average), and those of less than 160 ° C. were rated as "D" (poor).
[0068] [Melt viscosity (minimum melt viscosity)] The products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 9 were used as samples. 0.4 g of sample was pressed for 1 minute at a pressure of 10 MPa using a manual hydraulic pump: P-1B (manufactured by Riken) to produce pellets with a diameter of 20 mm and a thickness of 1 mm. The obtained pellets were used as samples and heated from 50°C to 200°C at a heating rate of 5°C / min using a rheometer: MCR 302 (manufactured by Anton Paar). The minimum value of the complex viscosity was taken as the minimum melt viscosity, and a minimum melt viscosity of less than 100,000 poise was rated as "○" (low viscosity), and a minimum melt viscosity of 100,000 poise or more was rated as "×" (high viscosity).
[0069] (Synthesis Example 1) Compound 1: Synthesis of vinylbenzyltriphenylphosphonium chloride Vinylbenzyl chloride (trade name: CMS-14, manufactured by AGC Seimi Chemical Co., Ltd.) 1.5 mol (228.9 g), triphenylphosphine 1.8 mol (472.1 g), and dimethylformamide 622.4 g were charged into a 2.0 L reactor and reacted at 70° C. for 3 hours under nitrogen conditions to precipitate a white solid. The solid was thoroughly washed with acetone and then dried under reduced pressure at 92° C. to recover 490 g of compound 1.
[0070] (Synthesis Example 2) Synthesis of Copolymer A 15.1 g of styrene, 13.2 g of compound 1, 5.5 g of acenaphthylene, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene as a chain transfer agent, 1.28 g of 2,2'-azobis(2,4,4-trimethylpentane) (product name: VR-110, Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator, and 78.8 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer A as a dimethylformamide solution.
[0071] (Synthesis Example 3) Synthesis of Copolymer B 12.7 g of styrene, 16.0 g of compound 1, 5.0 g of acenaphthylene, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene, 1.28 g of 2,2'-azobis(2,4,4-trimethylpentane), and 78.7 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer B as a dimethylformamide solution.
[0072] (Synthesis Example 4) Synthesis of Copolymer C 18.5 g of styrene, 10.1 g of compound 1, 6.3 g of acenaphthylene, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.33 g of 2,2'-azobis(2,4,4-trimethylpentane), and 81.5 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer C as a dimethylformamide solution.
[0073] (Synthesis Example 5) Synthesis of Copolymer D 17.3 g of styrene, 13.5 g of compound 1, 2.8 g of acenaphthylene, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene, 1.27 g of 2,2'-azobis(2,4,4-trimethylpentane), and 78.2 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer D as a dimethylformamide solution.
[0074] (Synthesis Example 6) Synthesis of Copolymer E 12.8 g of styrene, 12.8 g of compound 1, 8.0 g of acenaphthylene, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene, 1.28 g of 2,2'-azobis(2,4,4-trimethylpentane), and 78.4 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer E as a dimethylformamide solution.
[0075] (Synthesis Example 7) Synthesis of Copolymer F 17.7 g of styrene, 10.3 g of compound 1, 8.0 g of acenaphthylene, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 1.37 g of 2,2'-azobis(2,4,4-trimethylpentane), and 83.9 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer F as a dimethylformamide solution.
[0076] (Synthesis Example 8) Synthesis of Copolymer G 13.4 g of styrene, 15.8 g of compound 1, 3.7 g of acenaphthylene, 3.4 g of 2,4-diphenyl-4-methyl-1-pentene, 1.25 g of 2,2'-azobis(2,4,4-trimethylpentane), and 76.7 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer G as a dimethylformamide solution.
[0077] (Synthesis Example 9) Synthesis of Copolymer H 10.2 g of styrene, 15.0 g of compound 1, 7.0 g of acenaphthylene, 3.4 g of 2,4-diphenyl-4-methyl-1-pentene, 1.22 g of 2,2'-azobis(2,4,4-trimethylpentane), and 75.2 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer H as a dimethylformamide solution.
[0078] (Synthesis Example 10) Synthesis of Copolymer I 21.7 g of styrene, 10.6 g of compound 1, 3.3 g of acenaphthylene, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 1.35 g of 2,2'-azobis(2,4,4-trimethylpentane), and 82.9 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer I as a dimethylformamide solution.
[0079] (Synthesis Example 11) Synthesis of Copolymer J 9.7 g of styrene, 12.0 g of compound 1, 5.0 g of acenaphthylene, 8.5 g of vinylcyclohexane, 3.8 g of 2,4-diphenyl-4-methyl-1-pentene, 1.34 g of 2,2'-azobis(2,4,4-trimethylpentane), and 82.2 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer J as a dimethylformamide solution.
[0080] (Synthesis Example 12) Synthesis of Copolymer K 18.5 g of styrene, 10.1 g of compound 1, 6.3 g of acenaphthylene, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 0.77 g of di-tert-butyl peroxide (product name: Perbutyl D, manufactured by NOF Corp.) as a polymerization initiator, and 81.5 g of dimethylformamide were placed in a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions to obtain copolymer K as a dimethylformamide solution.
[0081] (Synthesis Example 13) Synthesis of Copolymer L 15.1 g of styrene, 13.2 g of compound 1, 5.5 g of acenaphthylene, 1.8 g of 2,4-diphenyl-4-methyl-1-pentene, 1.28 g of 2,2'-azobis(2,4,4-trimethylpentane), and 78.8 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3.5 hours under nitrogen conditions to obtain copolymer L as a dimethylformamide solution.
[0082] (Synthesis Example 14) Synthesis of Copolymer M 18.5 g of styrene, 10.1 g of compound 1, 6.3 g of acenaphthylene, 7.3 g of 2,4-diphenyl-4-methyl-1-pentene, 2.65 g of 2,2'-azobis(2,4,4-trimethylpentane), and 81.5 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 1.5 hours under nitrogen conditions to obtain copolymer M as a dimethylformamide solution.
[0083] (Comparative Synthesis Example 1) Synthesis of Copolymer N 22.0 g of styrene, 15.5 g of compound 1, 3.9 g of 2,4-diphenyl-4-methyl-1-pentene, 0.82 g of di-tert-butyl peroxide, and 87.4 g of dimethylformamide were charged into a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions to obtain copolymer N as a dimethylformamide solution.
[0084] (Comparative Synthesis Example 2) Synthesis of Copolymer O 14.3 g of styrene, 12.4 g of compound 1, 8.0 g of vinylcyclohexane, 3.7 g of 2,4-diphenyl-4-methyl-1-pentene, 0.76 g of di-tert-butyl peroxide, and 81.0 g of dimethylformamide were placed in a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions to obtain copolymer O as a dimethylformamide solution.
[0085] (Comparative Synthesis Example 3) Synthesis of Copolymer P 14.1 g of styrene, 11.4 g of compound 1, 8.0 g of isobornyl acrylate, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene, 0.74 g of di-tert-butyl peroxide, and 78.3 g of dimethylformamide were placed in a 500 mL reactor and reacted at 132°C for 3 hours under nitrogen conditions to obtain copolymer P as a dimethylformamide solution.
[0086] (Comparative Synthesis Example 4) Synthesis of Copolymer Q 22.0 g of styrene, 15.5 g of compound 1, 3.9 g of 2,4-diphenyl-4-methyl-1-pentene, 1.42 g of 2,2'-azobis(2,4,4-trimethylpentane), and 87.4 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 2 hours under nitrogen conditions to obtain copolymer Q as a dimethylformamide solution.
[0087] (Comparative Synthesis Example 5) Synthesis of Copolymer R 10.6 g of compound 1, 22.0 g of acenaphthylene, 3.4 g of 2,4-diphenyl-4-methyl-1-pentene, 1.24 g of 2,2'-azobis(2,4,4-trimethylpentane), and 76.0 g of dimethylformamide were placed in a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer R as a dimethylformamide solution.
[0088] (Comparative Synthesis Example 6) Synthesis of Copolymer S 14.3 g of styrene, 12.4 g of compound 1, 8.0 g of vinylcyclohexane, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.32 g of 2,2'-azobis(2,4,4-trimethylpentane), and 81.0 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer S as a dimethylformamide solution.
[0089] (Comparative Synthesis Example 7) Synthesis of Copolymer T 14.1 g of styrene, 11.4 g of compound 1, 8.0 g of isobornyl acrylate, 3.5 g of 2,4-diphenyl-4-methyl-1-pentene, 1.27 g of 2,2'-azobis(2,4,4-trimethylpentane), and 78.3 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 3 hours under nitrogen conditions to obtain copolymer T as a dimethylformamide solution.
[0090] (Comparative Synthesis Example 8) Synthesis of Polymer U 35.0 g of acenaphthylene, 3.6 g of 2,4-diphenyl-4-methyl-1-pentene, 1.33 g of 2,2'-azobis(2,4,4-trimethylpentane), and 81.7 g of dimethylformamide were charged into a 500 mL reactor and reacted at 120°C for 4 hours under nitrogen conditions. This reaction solution was reprecipitated in a large excess of methanol, and the supernatant was decanted. The remaining solid was dried under reduced pressure at 92°C to recover 33.9 g of polymer U.
[0091] Example 1 117.4g of the dimethylformamide solution of copolymer A obtained in Synthesis Example 2, 117.4g of toluene, 31.1g of 37% by mass formalin, and 38.3g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 18.2g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 14.2g of product 1. The Mw of product 1 was 5500, the styrene ratio was 62.1 mol%, the divinylbenzene ratio was 16.2 mol%, and the acenaphthylene ratio was 21.7 mol%.
[0092] Example 2 117.2 g of the dimethylformamide solution of copolymer B obtained in Synthesis Example 3, 117.2 g of toluene, 37.6 g of 37% by mass formalin, and 46.5 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 22.1 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 2 was dried under reduced pressure at 60°C to recover 13.0 g. The Mw of product 2 was 5400, the styrene ratio was 57.9 mol%, the divinylbenzene ratio was 20.8 mol%, and the acenaphthylene ratio was 21.3 mol%.
[0093] Example 3 121.4 g of the dimethylformamide solution of copolymer C obtained in Synthesis Example 4, 121.4 g of toluene, 23.7 g of 37 mass% formalin, and 29.3 g of 28 mass% potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 13.9 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 16.4 g of product 3. The Mw of product 3 was 5500, the styrene ratio was 66.9 mol%, the divinylbenzene ratio was 10.4 mol%, and the acenaphthylene ratio was 22.7 mol%.
[0094] Example 4 116.5 g of the dimethylformamide solution of copolymer D obtained in Synthesis Example 5, 116.5 g of toluene, 31.6 g of 37 mass% formalin, and 39.0 g of 28 mass% potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 18.6 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 14.0 g of product 4. The Mw of product 4 was 5700, the styrene ratio was 73.5 mol%, the divinylbenzene ratio was 17.0 mol%, and the acenaphthylene ratio was 9.5 mol%.
[0095] Example 5 116.8g of the dimethylformamide solution of copolymer E obtained in Synthesis Example 6, 116.8g of toluene, 30.1g of 37% by mass formalin, and 37.2g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 17.7g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 5 was recovered in 14.6g by drying under reduced pressure at 60°C. The Mw of product 5 was 5100, the styrene ratio was 52.3 mol%, the divinylbenzene ratio was 15.7 mol%, and the acenaphthylene ratio was 32.0 mol%.
[0096] Example 6 125.0 g of the dimethylformamide solution of copolymer F obtained in Synthesis Example 7, 125.0 g of toluene, 24.1 g of 37% by mass formalin, and 29.7 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 14.1 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 16.9 g of product 6. The Mw of product 6 was 5200, the styrene ratio was 63.0 mol%, the divinylbenzene ratio was 10.6 mol%, and the acenaphthylene ratio was 26.4 mol%.
[0097] Example 7 114.3 g of the dimethylformamide solution of copolymer G obtained in Synthesis Example 8, 114.3 g of toluene, 37.1 g of 37% by mass formalin, and 45.9 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 21.8 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 12.7 g of product 7. The Mw of product 7 was 5700, the styrene ratio was 63.5 mol%, the divinylbenzene ratio was 20.8 mol%, and the acenaphthylene ratio was 15.7 mol%.
[0098] Example 8 111.9g of the dimethylformamide solution of copolymer H obtained in Synthesis Example 9, 111.9g of toluene, 35.1g of 37% by mass formalin, and 43.4g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 20.6g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 12.9g of product 8. The Mw of product 8 was 6000, the styrene ratio was 49.1 mol%, the divinylbenzene ratio was 20.2 mol%, and the acenaphthylene ratio was 30.7 mol%.
[0099] Example 9 123.5 g of the dimethylformamide solution of copolymer I obtained in Synthesis Example 10, 123.5 g of toluene, 24.9 g of 37% by mass formalin, and 30.7 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 14.6 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 16.6 g of product 9. The Mw of product 9 was 5100, the styrene ratio was 79.0 mol%, the divinylbenzene ratio was 9.7 mol%, and the acenaphthylene ratio was 11.3 mol%.
[0100] Example 10 122.5 g of the dimethylformamide solution of copolymer J obtained in Synthesis Example 11, 122.5 g of toluene, 28.2 g of 37 mass% formalin, and 34.9 g of 28 mass% potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 16.6 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solid was removed by filtration, and 15.7 g of product 10 was recovered by drying under reduced pressure at 60°C. The Mw of product 10 was 6400, the styrene ratio was 42.9 mol%, the divinylbenzene ratio was 16.8 mol%, the acenaphthylene ratio was 21.9 mol%, and the vinylcyclohexane ratio was 18.4 mol%.
[0101] Example 11 120.8 g of the dimethylformamide solution of copolymer K obtained in Synthesis Example 12, 120.8 g of toluene, 23.7 g of 37 mass% formalin, and 29.3 g of 28 mass% potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 13.9 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 16.5 g of product 11. The Mw of product 11 was 5200, the styrene ratio was 62.7 mol%, the divinylbenzene ratio was 16.0 mol%, and the acenaphthylene ratio was 21.3 mol%.
[0102] Example 12 115.7g of the dimethylformamide solution of copolymer L obtained in Synthesis Example 13, 115.7g of toluene, 31.1g of 37% by mass formalin, and 38.3g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 18.2g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 14.3g of product 12. The Mw of product 12 was 10900, the styrene ratio was 60.7 mol%, the divinylbenzene ratio was 16.9 mol%, and the acenaphthylene ratio was 22.4 mol%.
[0103] (Example 13) 126.3 g of the dimethylformamide solution of copolymer M obtained in Synthesis Example 14, 126.3 g of toluene, 23.7 g of 37 mass% formalin, and 29.3 g of 28 mass% potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 13.9 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the mixture was dried under reduced pressure at 60°C to recover 16.5 g of product 13. The Mw of product 13 was 2600, the styrene ratio was 64.7 mol%, the divinylbenzene ratio was 15.0 mol%, and the acenaphthylene ratio was 20.3 mol%.
[0104] Comparative Example 1 129.7 g of the dimethylformamide solution of copolymer N obtained in Comparative Synthesis Example 1, 129.7 g of toluene, 36.2 g of 37% by mass formalin, and 44.7 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 21.3 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and 15.6 g of product 14 was recovered by drying under reduced pressure at 60°C. The Mw of product 14 was 5600, the styrene ratio was 83.2 mol%, and the divinylbenzene ratio was 16.8 mol%.
[0105] Comparative Example 2 120.1 g of the dimethylformamide solution of copolymer O obtained in Comparative Synthesis Example 2, 120.1 g of toluene, 29.1 g of 37% by mass formalin, and 35.9 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 17.1 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solid was removed by filtration, and 15.2 g of product 15 was recovered by drying under reduced pressure at 60°C. The Mw of product 15 was 6000, the styrene ratio was 63.9 mol%, the divinylbenzene ratio was 15.8 mol%, and the vinylcyclohexane ratio was 20.3 mol%.
[0106] Comparative Example 3 116.1g of the dimethylformamide solution of copolymer P obtained in Comparative Synthesis Example 3, 116.1g of toluene, 26.9g of 37% by mass formalin, and 33.1g of 28% by mass potassium hydroxide aqueous solution were charged into a 500mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 15.8g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and 14.9g of product 16 was recovered by drying under reduced pressure at 60°C. The Mw of product 16 was 5500, the styrene ratio was 63.2 mol%, the divinylbenzene ratio was 15.7 mol%, and the isobornyl acrylate ratio was 21.1 mol%.
[0107] Comparative Example 4 130.2 g of the dimethylformamide solution of copolymer Q obtained in Comparative Synthesis Example 4, 130.2 g of toluene, 36.3 g of 37% by mass formalin, and 44.9 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 21.3 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 17 was recovered in 15.7 g by drying under reduced pressure at 60°C. The Mw of product 17 was 6200, the styrene ratio was 84.4 mol%, and the divinylbenzene ratio was 15.6 mol%.
[0108] Comparative Example 5 77.6g of styrene, 20.0g of acenaphthylene, 10.2g of 2,4-diphenyl-4-methyl-1-pentene, 3.71g of 2,2'-azobis(2,4,4-trimethylpentane), and 227.6g of dimethylformamide were charged into a 500mL reactor and reacted at 120°C for 3 hours under nitrogen conditions. This reaction solution was reprecipitated in a large excess of methanol, and the supernatant was decanted. The remaining solid was dried under reduced pressure at 80°C to recover 58.2g of product 18. The Mw of product 18 was 4900, the styrene ratio was 76.9 mol%, and the acenaphthylene ratio was 23.1 mol%.
[0109] Comparative Example 6 113.2 g of the dimethylformamide solution of copolymer R obtained in Comparative Synthesis Example 5, 113.2 g of toluene, 24.9 g of 37% by mass formalin, and 30.7 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 14.6 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solid was removed by filtration, and 14.9 g of product 19 was recovered by drying under reduced pressure at 60°C. The Mw of product 19 was 4700, the divinylbenzene ratio was 13.0 mol%, and the acenaphthylene ratio was 87.0 mol%.
[0110] Comparative Example 7 120.6 g of the dimethylformamide solution of copolymer S obtained in Comparative Synthesis Example 6, 120.6 g of toluene, 29.1 g of 37% by mass formalin, and 35.9 g of 28% by mass potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 17.1 g of anhydrous magnesium chloride was charged and stirred at 65°C for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 20 was recovered in 15.2 g by drying under reduced pressure at 60°C. The Mw of product 20 was 6300, the styrene ratio was 62.1 mol%, the divinylbenzene ratio was 16.5 mol%, and the vinylcyclohexane ratio was 21.4 mol%.
[0111] Comparative Example 8 116.6 g of the dimethylformamide solution of copolymer T obtained in Comparative Synthesis Example 7, 116.6 g of toluene, 26.9 g of 37 mass% formalin, and 33.1 g of 28 mass% potassium hydroxide aqueous solution were charged into a 500 mL reactor and reacted at room temperature for 4 hours. The reaction solution was diluted with toluene, and the organic layer was washed with distilled water and isopropyl alcohol. After the organic layer was dehydrated and concentrated, 15.8 g of anhydrous magnesium chloride was charged and stirred at 65 ° C. for 2 hours. Solids were removed by filtration, and the filtrate diluted with toluene was reprecipitated in methanol. Next, the solids were removed by filtration, and the product 21 was recovered in 15.0 g by drying under reduced pressure at 60 ° C. The Mw of product 21 was 5700, the styrene ratio was 63.8 mol%, the divinylbenzene ratio was 15.5 mol%, and the isobornyl acrylate ratio was 20.7 mol%.
[0112] Comparative Example 9 5.7 g of the product 17 obtained in Comparative Example 4 was mixed with 2.0 g of the polymer U obtained in Comparative Synthesis Example 8, and dissolved in toluene to obtain a homogeneous solution. This solution was dried under reduced pressure at 60°C to recover 7.3 g of composition 1. The Mw of composition 1 was 6100, the styrene ratio was 67.5 mol%, the divinylbenzene ratio was 12.5 mol%, and the acenaphthylene ratio was 20.0 mol%.
[0113] The dielectric constant, dielectric tangent, glass transition temperature, and melt viscosity were evaluated for the products and compositions obtained in Examples 1 to 13 and Comparative Examples 1 to 9. The results are shown in Tables 1 to 5 below.
[0114] [Table 1]
[0115] [Table 2]
[0116] [Table 3]
[0117] [Table 4]
[0118] [Table 5]
[0119] Example 11 and Comparative Examples 1 to 3 are examples in which a peroxide-type polymerization initiator was used. In Comparative Example 1, since there was no acenaphthylene unit, the glass transition temperature was poor. In Comparative Example 2, vinylcyclohexane was added as a monomer to Comparative Example 1 for copolymerization, but the glass transition temperature was not improved. In Comparative Example 3, isobornyl acrylate was added as a monomer to Comparative Example 1 for copolymerization, and although the glass transition temperature was improved, both the dielectric constant and the dielectric loss tangent were deteriorated due to the presence of an ester group.
[0120] In contrast, in Example 11, by incorporating acenaphthylene units compared to Comparative Example 1, the dielectric constant and dielectric loss tangent were somewhat improved, while the glass transition temperature was significantly improved, and it was possible to achieve both dielectric properties and glass transition temperature. In Example 11, the minimum melt viscosity was also low.
[0121] Examples 1 to 10, 12 to 13 and Comparative Examples 4 to 9 are examples in which the azo-based initiator of the above formula (1) was used. Comparative Example 4 had improved dielectric properties compared to Comparative Example 1, but had an inferior glass transition temperature like Comparative Example 1 due to the absence of an acenaphthylene unit.
[0122] In Comparative Example 5, the divinylbenzene unit was not present, and the heat curing did not proceed. Therefore, it was not possible to prepare test pieces for evaluating the dielectric constant, the dielectric tangent, and the glass transition temperature, and these items could not be evaluated. In addition, since the heat curing did not proceed, the melt viscosity continued to decrease monotonically, and therefore the minimum melt viscosity could not be observed.
[0123] In Comparative Example 6, the dielectric properties and glass transition temperature were excellent, but since it did not contain a styrene unit, the minimum melt viscosity was high and the processability was poor. In Comparative Example 7, vinylcyclohexane was added as a monomer to Comparative Example 4 for copolymerization, but the glass transition temperature did not improve. In Comparative Example 8, isobornyl acrylate was added as a monomer to Comparative Example 4 for copolymerization, and although the glass transition temperature was improved, both the dielectric constant and the dielectric loss tangent were deteriorated due to the presence of the ester group.
[0124] In Comparative Example 9, the product 17 of Comparative Example 4 was mixed with polymer U, which was a homopolymer of acenaphthylene, and the composition contained styrene units, divinylbenzene units, and acenaphthylene units. However, the glass transition temperature was poor, the minimum melt viscosity was high, and the processability was poor.
[0125] In contrast, in Examples 1 to 10 and 12 to 13, by incorporating acenaphthylene units compared to Comparative Example 4, excellent dielectric constant and dielectric loss tangent were generally maintained while excellent glass transition temperature was obtained, and both dielectric properties and glass transition temperature were achieved. In addition, the minimum melt viscosity was low.
[0126] Furthermore, the products of Examples 1 to 13 were excellent in moldability, being capable of being molded into sheets sufficient to stand on their own without the use of a thermoplastic resin or a crosslinking agent.
[0127] In addition, the various numerical ranges described in the specification can be arbitrarily combined with their upper and lower limits, and all such combinations are considered to be preferred numerical ranges described in the specification. In addition, a numerical range described as "X to Y" means from X to Y.
[0128] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.
Claims
1. A thermosetting resin that is a linear copolymer having a repeating unit corresponding to a monovinyl aromatic compound, a repeating unit corresponding to a divinyl aromatic compound, and a repeating unit corresponding to an aromatic ring-fused cyclic olefin compound.
2. 2. The thermosetting resin according to claim 1, wherein the content of the repeating unit corresponding to the aromatic ring-fused cyclic olefin compound is 5 to 80 mol % in 100 mol % of all repeating units.
3. The linear copolymer has a terminal end having the general formula (1): R 1 -N=N-R 2 In the general formula (1), R 1 and R 2 The thermosetting resin according to claim 1 , wherein each independently represents a monovalent saturated hydrocarbon group or a monovalent aromatic hydrocarbon group.
4. 2. The thermosetting resin according to claim 1, wherein the total content of the repeating units corresponding to the monovinyl aromatic compound, the repeating units corresponding to the divinyl aromatic compound, and the repeating units corresponding to the aromatic ring-fused cyclic olefin compound is 80 mol % or more in 100 mol % of all repeating units.
5. The thermosetting resin according to claim 1 , wherein the aromatic ring-fused cyclic olefin compound has 3 or less rings.
6. A cured product obtained by curing the thermosetting resin according to any one of claims 1 to 5.
7. A thermosetting composition comprising the thermosetting resin according to any one of claims 1 to 5.
8. The thermosetting composition of claim 7 which is a printed circuit board material.
Citation Information
Patent Citations
Thermosetting resin composition, its cured item, and circuit board including the cured item
JP2001192539A
Soluble polyfunctional vinyl aromatic copolymer, method for producing the same, curable resin composition, and cured product of the same
JP2018039995A
Cited By
Resin compositions, cured products, prepregs, resin composites, printed circuit boards, and semiconductor devices
CN123125250A