Laminate with incombustibility and flame retardant wood
A laminate with specific thermal and optical properties improves flame retardancy and texture when applied to wood, addressing durability and productivity issues of chemical treatments.
Patent Information
- Application Number
- JP2023217831
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-12-25
- Publication Date
- 2024-10-09
AI Technical Summary
Existing flame-retardant laminates do not effectively maintain the texture of wood when attached, and existing methods for making wood flame retardant using chemicals lead to durability issues and poor productivity.
A laminate comprising a transparent base material with a heat shrinkage rate of 5.0% or less at 250°C and an infrared reflective film with specific reflectance and transmittance properties, which is laminated on the base material to improve flame retardancy while maintaining the texture of wood.
The laminate enhances flame retardancy by reflecting radiant heat during combustion while maintaining the visibility and texture of wood, suitable for use in architectural interior materials.
Smart Images

Figure 2024139679000002 
Figure 2024139679000003 
Figure 2024139679000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a flame-retardant laminate and a flame-retardant wood material comprising the same. [Background technology]
[0002] Wood used for architectural interior materials and the like has an excellent texture, but is prone to burn, and therefore attempts have been made to make it flame retardant. Generally, wood is made flame retardant by impregnating it with chemicals such as phosphoric acid or boric acid. However, when chemicals are used to make wood flame retardant, the chemicals rise to the surface of the wood and crystallize, causing efflorescence, which is a problem in terms of durability. In addition, special pressure equipment is required to impregnate wood with chemicals, which is poor in productivity.
[0003] Incidentally, a method of using an infrared reflective layer is known as a method for achieving flame retardancy. Patent Document 1 describes an invention relating to a flame-retardant laminate, characterized in that an infrared reflective layer having an average reflectance of 20% or more for infrared rays of 800 to 1300 nm is laminated on a resin substrate. In the examples, it is shown that a flame-retardant laminate in which an infrared reflective layer is formed by adhering silver nanowires to the surface of a polycarbonate resin substrate can reduce the total heat generation in a combustion test. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6308469 Summary of the Invention [Problem to be solved by the invention]
[0005] The flame-retardant laminate described in the above Patent Document 1 does not describe applications in which the laminate is laminated to wood, and does not consider maintaining the texture of wood when the flame-retardant laminate is applied. In addition, although the flame-retardant laminate described in Patent Document 1 has a certain degree of flame retardancy, further improvement in flame retardancy is desired in consideration of applications in which the laminate is laminated to wood or the like to impart flame retardancy. Therefore, an object of the present invention is to provide a flame-retardant laminate which, when used on an adherend such as wood, can improve the flame retardancy while maintaining the texture of the adherend. [Means for solving the problem]
[0006] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by a flame-retardant laminate comprising a transparent substrate having a heat shrinkage rate of a certain level or less at 250° C. and an infrared reflective film, and the flame-retardant laminate has an average reflectance in a specific wavelength region and an average transmittance in a specific wavelength region of a certain level or more, and have completed the present invention as described below. That is, the present invention provides the following items [1] to [8].
[0007] [1] A flame-retardant laminate comprising a transparent substrate having a heat shrinkage rate of 5.0% or less at 250°C and an infrared reflective film laminated on the transparent substrate, the flame-retardant laminate having an average reflectance of 80% or more for light in a wavelength range of 1000 to 2500 nm and an average transmittance of 40% or more for light in a wavelength range of 400 to 800 nm. [2] The flame-retardant laminate according to the above [1], wherein the transparent substrate is glass or a resin film. [3] The flame-retardant laminate according to the above [2], wherein the resin film is made of an engineering plastic. [4] The flame-retardant laminate according to any one of the above [1] to [3], wherein the infrared reflective film has a multilayer structure. [5] The flame-retardant laminate according to any one of the above [1] to [4], wherein the infrared reflective film comprises a metal layer and an optical adjustment layer. [6] The flame-retardant laminate according to any one of the above [1] to [5], further comprising a protective film on the surface of the infrared reflective film. [7] The flame-retardant laminate according to any one of the above [1] to [6], which has a pressure-sensitive adhesive layer on the surface of the transparent substrate. [8] A flame-retardant wood material comprising a wood material and the flame-retardant laminate according to any one of the above [1] to [7], in which the wood material, a transparent substrate, and an infrared reflective film are laminated in this order. Effect of the Invention
[0008] According to the present invention, it is possible to provide a flame-retardant laminate which, when used on an adherend such as wood, can improve the flame retardancy while maintaining the texture of the adherend. [Brief description of the drawings]
[0009] [Figure 1] 1 is a cross-sectional view showing a schematic diagram of one embodiment of a flame-retardant laminate of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a schematic diagram of another embodiment of the flame-retardant laminate of the present invention. [Diagram 3] FIG. 2 is a cross-sectional view showing a schematic diagram of another embodiment of the flame-retardant laminate of the present invention. [Figure 4] 1 is a cross-sectional view showing a schematic diagram of one embodiment of a flame-retardant wood material according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the present invention will be described in detail with reference to embodiments. [Flame-retardant laminate] The present invention relates to a flame-retardant laminate comprising a transparent substrate having a heat shrinkage rate of 5.0% or less at 250° C. and an infrared reflective film laminated on the transparent substrate, the flame-retardant laminate having an average reflectance of 80% or more for light in a wavelength range of 1000 to 2500 nm and an average transmittance of 40% or more for light in a wavelength range of 400 to 800 nm. The flame-retardant laminate is used to impart flame retardancy to an adherend such as wood, and is used, for example, by being attached to the surface of wood.
[0011] One embodiment of the flame retardant laminate of the present invention is shown in Fig. 1. The flame retardant laminate of the present invention is not limited to the drawing. As shown in Fig. 1, the flame retardant laminate of the present invention is a laminate including a transparent substrate 12 and an infrared reflective film 11 laminated on the transparent substrate 12.
[0012] <Transparent base material> The transparent substrate has a heat shrinkage rate of 5.0% or less at 250° C. If the heat shrinkage rate at 250° C. exceeds 5.0%, the flame-retardant laminate is likely to deform or crack under high temperatures such as during a fire, and therefore, when the flame-retardant laminate is used on wood, it becomes difficult to improve the flame retardancy of the wood. From the viewpoint of improving flame retardancy, the heat shrinkage rate of the transparent substrate at 250° C. is preferably 5.0% or less, more preferably 2.0% or less, and further preferably 1.5% or less. The thermal shrinkage rate can be adjusted to a desired range by appropriately selecting the type of transparent substrate. The heat shrinkage rate can be measured by the method described in the examples.
[0013] Since the transparent substrate is transparent, it is easy to adjust the average transmittance of the flame-retardant laminate to a certain level or higher for light in the wavelength region of 400 to 800 nm, as described below. Therefore, even when the flame-retardant laminate is attached to an adherend such as wood, the visibility of the adherend surface is not hindered, and the texture of the adherend can be well maintained. The average transmittance of the transparent substrate for light in the wavelength region of 400 to 800 nm is not particularly limited, but is preferably 40% or more, and more preferably 50% or more.
[0014] The transparent substrate is not particularly limited as long as the thermal shrinkage at 250° C. is within the above-mentioned range, but is preferably glass or a resin film, and from the viewpoint of handling, a resin film or a thin glass film is more preferable.
[0015] When the transparent substrate is a resin film, the resin film preferably has a melting point (Tm) of 280° C. or higher, or a glass transition temperature (Tg) of 200° C. or higher. More specifically, when the resin film is a crystalline resin film, the melting point (Tm) is preferably 280° C. or higher, and when the resin film is a non-crystalline resin film, the glass transition temperature (Tg) is preferably 200° C. or higher. In this way, when a resin film having a melting point (Tm) or glass transition temperature (Tg) of a certain level or higher is used, the flame retardancy of wood can be easily improved when the flame retardant laminate is used on wood. The melting point (Tm) of the above-mentioned resin film is more preferably 290°C or higher, further preferably 310°C or higher, and preferably 400°C or lower. The glass transition temperature (Tg) of the above-mentioned resin film is more preferably 220°C or higher, further preferably 250°C or higher, and preferably 400°C or lower. The melting point (Tm) and glass transition temperature (Tg) of the resin film can be measured by the method described in the Examples.
[0016] The resin film is not particularly limited as long as it is a material that can set the heat shrinkage rate at 250°C within the above-mentioned range, but is preferably made of engineering plastic. Examples of the engineering plastic are preferably polyether ether ketone (PEEK), polyimide (PI), polyparaphenylene terephthalamide (PPTA), polyetherimide (PEI), and thermoplastic polyimide (TPI). The resin film may be made of a single material or a plurality of materials.
[0017] The thickness of the transparent substrate is not particularly limited, but is, for example, 5 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 20 μm to 50 μm. By making the thickness of the transparent substrate equal to or greater than the lower limit, the flame retardancy of wood is easily improved when the flame retardant laminate is used for wood, and by making the thickness of the transparent substrate equal to or less than the upper limit, the overall thickness of the flame retardant laminate can be reduced, improving the handleability.
[0018] <Infrared reflective film> The flame retardant laminate of the present invention includes an infrared reflective film on the transparent substrate described above. By providing the infrared reflective film, radiant heat during combustion can be reflected, thereby improving flame retardancy. The infrared reflective film may be any film that has the function of reflecting infrared rays, and may include, for example, either a metal layer or an optical adjustment layer, or both.
[0019] The infrared reflective film may have a single layer structure or a multilayer structure, but is preferably a multilayer structure from the viewpoint of increasing the average transmittance of light in the wavelength region of 400 to 800 nm through the flame retardant laminate. The multi-layered infrared reflective film preferably includes a metal layer and an optical adjustment layer, and more preferably includes metal layers and optical adjustment layers stacked alternately. The number of layers in the multilayer structure is not particularly limited, but is, for example, from 2 to 10 layers, preferably from 2 to 4 layers, and more preferably 3 layers. It is particularly preferable that the infrared reflective film has a three-layer structure in which an optical adjustment layer, a metal layer, and an optical adjustment layer are laminated in this order.
[0020] Examples of materials for the metal layer include aluminum, copper, silver, gold, palladium, titanium, iron, nickel, zinc, zirconium, chromium, molybdenum, tantalum, tungsten, indium, tin, and alloys containing these. Of these, silver, aluminum, titanium, copper, gold, and iron are preferred, and silver is particularly preferred. The thickness of the metal layer is not particularly limited, but is, for example, from 1 nm to 500 nm, preferably from 5 nm to 100 nm, and more preferably from 10 nm to 50 nm.
[0021] Examples of the optical adjustment layer include metal oxides, such as titanium dioxide (TiO2), titanium oxide (TiO), zinc oxide (ZnO), zinc sulfide (ZnS), niobium oxide (Nb2O5), cerium oxide (CeO2), tantalum oxide (Ta2O5), aluminum oxide (Al2O3), zirconium oxide (ZrO2), silicon dioxide (SiO2), tin dioxide (SnO2), tin-doped indium oxide (ITO), cerium-doped indium oxide (ICO), gallium-doped zinc oxide (GZO), aluminum-doped zinc oxide (AZO), indium oxide-zinc oxide (IZO), and antimony-doped tin oxide (ATO). Among these, aluminum-doped zinc oxide (AZO) is preferred. The thickness of the optical adjustment layer is not particularly limited, but is, for example, from 1 nm to 500 nm, preferably from 5 nm to 100 nm, and more preferably from 10 nm to 50 nm.
[0022] The thickness of the infrared reflective film is not particularly limited, but is, for example, 5 nm to 1000 nm, preferably 10 nm to 200 nm, and more preferably 30 nm to 100 nm. By making the thickness of the infrared reflective film equal to or greater than the lower limit, the flame retardancy is easily improved, and by making the thickness of the infrared reflective film equal to or less than the upper limit, the transparency is easily improved. The method for laminating the infrared reflective film on the transparent substrate is not particularly limited, but it is preferably performed by a sputtering method.
[0023] <Protective film> As shown in Fig. 2, the flame retardant laminate 10 of the present invention may have a protective film 14 on the surface of an infrared reflective film 11. By providing the flame retardant laminate with a protective film, the infrared reflective film can be appropriately protected, for example, by improving the scratch resistance of the infrared reflective film. In addition, the protective film may have an embossed surface. The protective film may be a resin film, or an inorganic film such as diamond-like carbon (DLC), alumina, or silicon dioxide. The thickness of the protective film is not particularly limited, but is, for example, from 0.1 μm to 10 μm, and preferably from 0.5 μm to 5 μm.
[0024] <Adhesive layer> As shown in Fig. 3, the flame-retardant laminate 10 of the present invention may have an adhesive layer 13 on the surface of a transparent substrate 12. By providing the flame-retardant laminate with an adhesive layer, the flame-retardant laminate can be attached and fixed to an adherend such as wood via the adhesive layer. The pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive. The pressure-sensitive adhesive is not particularly limited, and examples thereof include acrylic pressure-sensitive adhesives, urethane pressure-sensitive adhesives, polyolefin pressure-sensitive adhesives, polyester pressure-sensitive adhesives, vinyl alkyl ether pressure-sensitive adhesives, polyamide pressure-sensitive adhesives, rubber pressure-sensitive adhesives, silicone pressure-sensitive adhesives, and fluorine pressure-sensitive adhesives. The adhesive layer may be a double-sided tape (double-sided adhesive tape) having adhesives on both sides of a substrate. The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is, for example, from 10 μm to 150 μm, and preferably from 30 μm to 100 μm.
[0025] The flame retardant laminate of the present invention may include both the protective film and the pressure-sensitive adhesive layer described above, or may include layers other than the protective film and the pressure-sensitive adhesive layer as long as the effects of the present invention are not impaired.
[0026] <Average reflectance> The average reflectance of the flame retardant laminate of the present invention for light in the wavelength region of 1000 to 2500 nm is 80% or more. If the average reflectance is less than 80%, it becomes difficult to reflect radiant heat during combustion, and the flame retardancy decreases. The average reflectance of the flame retardant laminate for light in the wavelength region of 1000 to 2500 nm is preferably 85% or more. The upper limit of the average reflectance is 100%. The average reflectance can be adjusted by the type, thickness, etc. of the infrared reflective film. The average reflectance is measured by a spectrophotometer from the surface of the flame-retardant laminate on the infrared reflective film side. The details of the measurement are as described in the Examples.
[0027] <Average transmittance> The average transmittance of the flame retardant laminate of the present invention for light in the wavelength region of 400 to 800 nm is 40% or more. If the average transmittance is less than 40%, the pattern of the adherend (e.g., wood) to which the flame retardant laminate of the present invention is attached becomes difficult to see through the flame retardant laminate, and the texture deteriorates. From the viewpoint of maintaining the texture of the adherend when the flame retardant laminate is attached to the adherend, the average transmittance of the flame retardant laminate for light in the wavelength region of 400 to 800 nm is preferably 45% or more, more preferably 50% or more, and even more preferably 55% or more. The upper limit of the average transmittance is 100%. The average transmittance can be adjusted by the type and thickness of the transparent substrate and the infrared reflective film. The average transmittance is measured by a spectrophotometer. The details of the measurement are as described in the Examples.
[0028] <Fire-retardant wood> The flame-retardant laminate of the present invention can be used on wood to obtain flame-retardant wood with improved flame retardancy. As shown in Fig. 4, the flame-retardant wood 20 of the present invention comprises wood 15 and a flame-retardant laminate 10 laminated on the surface of the wood 15. The flame-retardant wood 20 comprises wood 15, a transparent substrate 12, and an infrared reflective film 11 laminated in this order. When the flame-retardant laminate 10 comprises an adhesive layer 13, the adhesive layer 13 is provided between the wood 15 and the transparent substrate 12, and the wood 15 and the flame-retardant laminate 10 are fixed via the adhesive layer 13. The thickness of the wooden piece 15 is not particularly limited and depends on the application, but is, for example, from 2 mm to 50 mm, and preferably from 5 mm to 40 mm. The flame-retardant wood of the present invention has excellent flame retardancy and maintains the texture of wood because it includes the flame-retardant laminate described above. The flame-retardant wood can be suitably used for architectural interior materials such as gypsum boards and heat insulating panels. EXAMPLES
[0029] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0030] The various measurement methods are as follows. [Average reflectance] The average reflectance of light in the wavelength region of 1000 to 2500 nm was measured for the flame-retardant laminates produced in each of the Examples and Comparative Examples using a spectrophotometer ("V-670" manufactured by JASCO Corporation). The measurement was performed at room temperature (25°C). The average reflectance was measured for the surface of the flame-retardant laminate on the infrared reflective film side.
[0031] [Average transmittance] The average transmittance of light in the wavelength region of 400 to 800 nm was measured for each of the flame-retardant laminates produced in the Examples and Comparative Examples using a spectrophotometer ("V-670" manufactured by JASCO Corporation). The measurement was performed at room temperature (25°C).
[0032] [Heat shrinkage rate] The thermal shrinkage of the transparent substrate used in each of the Examples and Comparative Examples was measured as follows. The thermal shrinkage refers to the ratio of dimensions before and after heat treatment of a transparent substrate (rectangular shape with a length of 50 mm and a width of 50 mm) at 250°C for 5 minutes and then returned to room temperature (25°C), and can be calculated by the following formula. The thermal shrinkage was measured in both the vertical and horizontal directions of the transparent substrate, and the average value was calculated. That is, the thermal shrinkage of the vertical and horizontal dimensions was calculated by the following formula, and the thermal shrinkage in the present invention was calculated by averaging these values. Heat shrinkage rate (%) = 100 x (dimension before heating - dimension after heating) / dimension before heating
[0033] [Melting point (Tm), glass transition temperature (Tg)] The melting point (Tm) and glass transition temperature (Tg) of the transparent substrate (resin film) used in each of the Examples and Comparative Examples were measured as follows. A transparent substrate made of a resin film was used as a measurement sample and measured using a differential scanning calorimeter ("DSC7020" manufactured by Hitachi High-Tech Science Corporation) at a temperature range of -40 to 400°C and a heating rate of 10°C / min. The endothermic peak obtained was taken as the melting point (Tm) or glass transition temperature (Tg).
[0034] [Cone calorimeter test] The flame-retardant wood produced in each Example and Comparative Example was subjected to a cone calorimeter test in accordance with ISO5660-1 with a radiant heat intensity of 50 kW / m 2 The test was carried out to confirm whether the material had flame retardant, semi-nonflammable, or nonflammable properties. Flame retardant performance is equivalent to a radiation heat intensity of 50kW / m in a heat generation test using a cone calorimeter tester in accordance with ISO5660-1. 2 When heated at 40°C, the total heat generated after 5 minutes is 8MJ / m 2 In addition, the performance equivalent to quasi-noncombustible is a total heat release of 8MJ / m after 10 minutes. 2 In addition, non-combustible performance is when the total heat generated after 20 minutes is 8MJ / m 2 The result is as follows. In addition, the radiant heat intensity is 50kW / m 2 The time from the start of the test to the ignition of the flame-retardant wood when heated at 400° C. was measured and recorded as the ignition time (seconds).
[0035] [Wood texture] For the flame-retardant wood produced in each Example and Comparative Example, when observed from the flame-retardant laminate side, the wood surface was marked with "◎" if its visibility was good and its texture was maintained, and marked with "◯" if its visibility and texture were maintained but slightly inferior to that of ◎. The wood surface was marked with "X" if its visibility and texture were not maintained.
[0036] <Example 1> A 25 μm thick polyimide (PI) film (IST Corporation's "TORMED Type C") was prepared as a transparent substrate. Aluminum-doped zinc oxide (AZO), silver (Ag), and aluminum-doped zinc oxide (AZO) were laminated in this order on one surface of the polyimide film using a sputtering device (ULVAC Kyushu Corporation's "QAM-4") to form an infrared reflective film and produce a flame-retardant laminate. The thickness of each AZO and Ag layer was calculated from the amount of adhesion and specific gravity obtained by fluorescent X-ray analysis, and is shown in Table 1. The transparent substrate side of the flame-retardant laminate was attached to wood (MonotaRO's SPF1063, thickness 19 mm) with double-sided tape (Sekisui Chemical's Double Tack Tape No. 570E, thickness 120 μm) to produce flame-retardant wood. The thickness of the infrared reflective film from the transparent substrate side was AZO 19 nm, Ag 19 nm, and AZO 28 nm. The various evaluation results are shown in Table 1.
[0037] <Examples 2 to 5, Comparative Example 1> Flame-retardant wood materials were produced in the same manner as in Example 1, except that the type of transparent substrate and the thickness of each layer constituting the infrared reflective film were as shown in Table 1. The evaluation results are shown in Table 1. In the table, "PEEK" means polyether ether ketone, and "PEN" means polyethylene naphthalate. The PEEK used was "EXPEEK" manufactured by Kurabo Industries, Ltd., the glass used was "G-Leaf" manufactured by Nippon Electric Glass Co., Ltd., and the PEN used was "Teonex Q51" manufactured by Toyobo Co., Ltd.
[0038] [Table 1]
[0039] As shown in the above examples, the flame-retardant laminates of each example, which have a transparent substrate with a thermal shrinkage rate of 5.0% or less at 250°C, an infrared reflective film, and an average reflectance at 1000 to 2500 nm and an average transmittance at 400 to 800 nm of at least a certain level, were found to have excellent flame retardancy and texture when applied to wood to make flame-retardant wood. In contrast, the laminate of Comparative Example 1, which used a transparent substrate with a thermal shrinkage rate of more than 5.0% at 250° C., was found to have poor flame retardancy when applied to wood to make it a flame-retardant wood. [Explanation of symbols]
[0040] 10 Flame retardant laminate 11 Infrared reflective film 12 Transparent base material 13 Adhesive layer 14 Protective film 15 wood
Claims
1. The flame-retardant laminate comprises a transparent substrate having a heat shrinkage rate of 5.0% or less at 250°C and an infrared reflective film laminated on the transparent substrate, the flame-retardant laminate having an average reflectance of 80% or more for light in a wavelength region of 1000 to 2500 nm and an average transmittance of 40% or more for light in a wavelength region of 400 to 800 nm.
2. The flame retardant laminate according to claim 1 , wherein the transparent substrate is glass or a resin film.
3. The flame-retardant laminate according to claim 2 , wherein the resin film is made of an engineering plastic.
4. The flame retardant laminate according to claim 1 or 2, wherein the infrared reflective film has a multi-layer structure.
5. The flame retardant laminate according to claim 1 or 2, wherein the infrared reflective film comprises a metal layer and an optical adjustment layer.
6. The flame-retardant laminate according to claim 1 or 2, further comprising a protective film on a surface of the infrared reflective film.
7. The flame-retardant laminate according to claim 1 or 2, further comprising a pressure-sensitive adhesive layer on a surface of the transparent substrate.
8. 3. A flame-retardant wood product comprising a wood material and the flame-retardant laminate according to claim 1 or 2, the wood material being laminated in this order with a transparent substrate and an infrared reflective film.
Citation Information