Overcoat agent, overcoat layer, laminate, and printed matter
The overcoat agent with a binder resin forms a protective layer on UV laser-marked ink compositions, addressing visibility and thermal damage issues, thereby improving the quality of laser markings on plastic films.
Patent Information
- Application Number
- JP2024046466
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-09
AI Technical Summary
Existing ink compositions for UV laser marking on plastic films suffer from poor visibility and thermal damage issues, particularly when used for surface printing on packaging materials.
An overcoat agent containing a binder resin, such as acrylic or polyurethane resin, is applied to form an overcoat layer on top of an ink layer containing titanium oxide, enhancing visibility and reducing thermal damage during UV laser marking.
The overcoat agent improves the visibility of UV laser markings by forming a protective layer that enhances printability and reduces thermal stress on the film.
Smart Images

Figure 2024139742000001 
Figure 2024139742000002 
Figure 2024139742000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an overcoat agent, an overcoat layer, a laminate, and a printed matter. [Background technology]
[0002] For various packaging materials such as beverage containers, food containers, and pharmaceutical packaging, front printing is performed by printing on the surface of the substrate of the packaging material, or reverse printing is performed by applying an adhesive or anchor agent to the printed surface of the substrate of the packaging material as necessary and laminating the film. Furthermore, for packaging materials, printing or marking of various traceability variable information such as production lot number, production date, expiration date of contents, best-before date, etc. As a marking method, the laser marking method is effective in establishing traceability by preventing tampering because the printing or marking does not peel off or disappear compared to the hot stamp method or inkjet method.
[0003] Patent Documents 1 to 3 disclose ink compositions for use in the above-mentioned laser marking method, which contain a white pigment such as titanium oxide and are used for reverse printing laser marking using VYO4 laser light. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-2258 A [Patent Document 2] JP 2020-2259 A [Patent Document 3] JP 2020-1261 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when the ink composition for laser marking disclosed in the above patent document is printed on a plastic film by surface printing and then laser marking is performed by irradiating a laser from the printed surface or the plastic film surface, it has been found that the black characters printed by the marking are faint, and there is a problem with the visibility of the information. In addition, a printing method using a UV laser is required as the laser light in order to reduce thermal damage to the film and the printing layer.
[0006] Therefore, the present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide an overcoat agent capable of surface printing UV laser marking with good visibility.
[0007] Another object of the present invention is to provide an overcoat layer formed from the above-mentioned overcoat agent, a laminate provided with the overcoat layer, and a printed matter. [Means for solving the problem]
[0008] That is, the present invention relates to an overcoat agent containing a binder resin, the overcoat agent being used to cover an ink layer formed from an ink composition for surface-printing UV laser marking that contains titanium oxide.
[0009] The present invention also relates to an overcoat layer formed from the overcoat agent.
[0010] The present invention also relates to a laminate comprising a base film provided on one side of the ink layer and an overcoat layer provided on the other side of the ink layer.
[0011] The present invention also relates to a printed matter obtained by irradiating the laminate with a UV laser. Effect of the Invention
[0012] The overcoat agent of the present invention can cover an ink layer formed from an ink composition for surface-printing UV laser marking that contains titanium oxide, and therefore, when UV laser marking is performed, a printed matter having good visibility (laser printability) can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] <Overcoat agent> The overcoat agent of the present invention contains a binder resin and is used for covering an ink layer formed from an ink composition for surface-printing UV laser marking containing titanium oxide. The above "for covering an ink layer" means that the overcoat agent is applied (printed) onto the surface of the ink layer to form an overcoat layer.
[0014] The binder resin may be any resin capable of forming a coating layer that transmits UV laser, and examples thereof include polyester resin, acrylic resin, vinyl chloride resin, vinyl chloride-vinyl acetate resin, ethylene-vinyl acetate resin, styrene-acrylic resin, styrene-maleic acid resin, rosin resin, rosin ester resin, petroleum resin, coumarone-indene resin, terpene phenol resin, phenol resin, polyurethane resin, melamine resin, urea resin, epoxy resin, cellulose resin, xylene resin, alkyd resin, aliphatic hydrocarbon resin, butyral resin, maleic acid resin, fumaric acid resin, etc. Among these, from the viewpoint of various resistances (abrasion resistance, blocking resistance, water resistance, solvent resistance, etc.), flexibility, and residual solvent amount of the coating layer, the binder resin is preferably an acrylic resin or a polyurethane resin, and more preferably a combination of an acrylic resin and a polyurethane resin. The binder resin may be used alone or in combination of two or more kinds. When an acrylic resin and a polyurethane resin are used in combination as the binder resin, the mass ratio thereof (acrylic resin / polyurethane resin) is preferably 3.0 or less, and more preferably 2.0 or less, from the viewpoint of the amount of residual solvent.
[0015] From the viewpoint of various resistances of the coating layer, the binder resin preferably contains a resin having a glass transition temperature (Tg) of 0°C or higher, more preferably contains a resin having a glass transition temperature (Tg) of 20°C or higher, and even more preferably contains a resin having a glass transition temperature (Tg) of 40°C or higher; and from the viewpoint of flexibility and residual solvent amount of the coating layer, the binder resin preferably contains a resin having a glass transition temperature (Tg) of 100°C or lower, more preferably contains a resin having a glass transition temperature (Tg) of 90°C or lower, and even more preferably contains a resin having a glass transition temperature (Tg) of 80°C or lower.
[0016] When the binder resin is an acrylic resin or a styrene-acrylic resin, the above glass transition temperature is a theoretical glass transition temperature calculated by the following Wood's formula: Wood's formula: 1 / Tg=W1 / Tg1+W2 / Tg2+W3 / Tg3+····+Wx / Tgx [wherein Tg1 to Tgx represent the glass transition temperatures of the respective homopolymers of monomers 1, 2, 3···x constituting the anionic group-containing resin, W1 to Wx represent the respective polymerization fractions of monomers 1, 2, 3···x, and Tg represents the theoretical glass transition temperature. However, the glass transition temperature in Wood's formula is an absolute temperature.]
[0017] The glass transition temperature of the resin other than the acrylic resin or the styrene-acrylic resin is an actually measured glass transition temperature obtained by thermal analysis. The thermal analysis method is based on JIS K7121 (Method for measuring the glass transition temperature of plastics), and for example, the glass transition temperature can be measured using a Pyris1 DSC manufactured by PerkinElmer under conditions of a temperature rise rate of 20° C. / min and a nitrogen gas flow rate of 20 ml / min.
[0018] However, when the above binder resins are commercially available products, the glass transition temperature is based on the catalog value.
[0019] From the viewpoint of various resistances of the coating layer, the binder resin preferably has a functional group capable of reacting with a crosslinking agent, and examples of such functional groups include a hydroxyl group, an amino group, an epoxy group, etc. The crosslinking agents may be used alone or in combination of two or more kinds.
[0020] Examples of the crosslinking agent include an isocyanate-based crosslinking agent, an organic peroxide-based crosslinking agent, and an epoxy crosslinking agent. From the viewpoints of pot life and reactivity, an isocyanate-based crosslinking agent is preferred.
[0021] Examples of the isocyanate crosslinking agent include aromatic isocyanates such as tolylene diisocyanate and xylylene diisocyanate, alicyclic isocyanates such as isophorone diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate.
[0022] Examples of the isocyanate-based crosslinking agent include lower aliphatic diisocyanates such as butylene diisocyanate and hexamethylene diisocyanate, alicyclic diisocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate, aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate and polymethylene polyphenyl isocyanate, trimethylolpropane / tolylene diisocyanate trimer adduct ... Examples of such polyisocyanates include polyisocyanate / hexamethylene diisocyanate trimer adduct, isocyanurate adduct of hexamethylene diisocyanate, trimethylolpropane adduct of xylylene diisocyanate, trimethylolpropane adduct of isophorone diisocyanate, trimethylolpropane adduct of hexamethylene diisocyanate; polyether polyisocyanate, polyester polyisocyanate, and adducts of these with various polyols; polyisocyanates multifunctionalized with isocyanurate bonds, biuret bonds, allophanate bonds, etc. Among these, crosslinking agents having three or more isocyanate groups in the molecule are preferred.
[0023] In addition, the overcoat agent preferably contains an organic solvent to disperse or dissolve the above-mentioned components. The organic solvent can be used without any particular limitation, and examples thereof include alcohol-based organic solvents such as methanol, ethanol, n-propanol, isopropanol, butanol, etc.; ketone-based organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.; ester-based organic solvents such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, etc.; aliphatic hydrocarbon-based organic solvents such as n-hexane, n-heptane, n-octane, etc.; alicyclic hydrocarbon-based organic solvents such as cyclohexane, methylcyclohexane, ethylcyclohexane, cycloheptane, cyclooctane, etc.; aromatic hydrocarbon-based organic solvents such as toluene, xylene, etc. The organic solvents can be used alone or in combination of two or more.
[0024] From the viewpoint of applying the overcoat agent to flexographic printing or gravure printing, it is preferable to use the alcohol-based organic solvent and / or the ester-based organic solvent as the organic solvent. In this case, the ratio of the alcohol-based organic solvent and / or the ester-based organic solvent in the organic solvent is preferably 90 mass % or more, more preferably 95 mass % or more.
[0025] The total proportion of the binder resin, the crosslinking agent, and the organic solvent in the overcoat agent is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, from the viewpoint of coating (printing) suitability.
[0026] The overcoat agent may further contain additives such as a leveling agent, an antioxidant, and an antifoaming agent, if necessary.
[0027] The total proportion of the binder resin and the crosslinking agent in the solid content of the overcoat agent is preferably 80 mass % or more, more preferably 90 mass % or more, and even more preferably 95 mass % or more, from the viewpoint of taking into account various resistances of the overcoat layer.
[0028] <Ink composition for surface UV laser marking> The ink composition for surface-printing UV laser marking of the present invention is an ink composition for surface-printing UV laser marking containing titanium oxide (hereinafter, also simply referred to as "ink composition"). Here, surface printing refers to printing intended to make an ink layer (printed surface) formed from the ink composition provided on a substrate or the like the front side, i.e., the side opposite to the contents, when the printed matter is processed into a packaging material or the like.
[0029] From the viewpoint of improving visibility (laser printability), the titanium oxide preferably has an average particle size of 0.30 μm or less, more preferably 0.28 μm or less, and even more preferably 0.26 μm or less. From the viewpoint of improving doctor cutting, the titanium oxide preferably has an average particle size of 0.20 μm or more, and more preferably 0.23 μm or more. The average particle size can be determined by a method of statistically processing images taken with a transmission electron microscope. As the method, for example, the methods disclosed in JP-A-2003-26856 and JP-A-2006-341628 may be adopted. The titanium oxide may have a surface treated with various materials such as alumina, silica, barium titanate, and the like, and may be in the form of anatase type, rutile type, or titanium sol. The titanium oxide may be used alone or in combination of two or more kinds.
[0030] From the viewpoint of visibility of the laser-printed area, the titanium oxide content is preferably 60 mass % or more, more preferably 65 mass % or more, and even more preferably 70 mass % or more of the solid content of the ink composition, and from the viewpoint of the viscosity of the ink and stability over time, the titanium oxide content is preferably 90 mass % or less, and more preferably 85 mass % or less of the solid content of the ink composition.
[0031] The ink composition for surface printing UV laser marking preferably contains a polyurethane resin as a resin component for forming an ink layer. The polyurethane resin is a resin having two or more urethane bonds in the molecule, and can be used without particular limitation, but examples thereof include polyurethane resins obtained by reacting a diisocyanate compound, a diol compound, a chain extender, and a reaction terminator (a polyurethane prepolymer obtained by reacting a diisocyanate compound with a diol compound, and a chain extender and a reaction terminator). The polyurethane resins can be used alone or in combination of two or more kinds.
[0032] Examples of the diisocyanate compound include aliphatic diisocyanate compounds such as hexamethylene diisocyanate and 2,2,4-trimethylhexamethylene diisocyanate; alicyclic diisocyanate compounds such as isophorone diisocyanate and hydrogenated xylylene diisocyanate; aromatic aliphatic diisocyanate compounds such as xylylene diisocyanate and α,α,α',α'-tetramethyl xylylene diisocyanate; and aromatic diisocyanate compounds such as tolylene diisocyanate and diphenylmethane diisocyanate. Among these, from the viewpoint of easy reaction control and good balance of performance of the obtained polyurethane resin, alicyclic or aromatic aliphatic diisocyanate compounds are preferred, and isophorone diisocyanate and α,α,α',α'-tetramethyl xylylene diisocyanate are particularly preferred. The diisocyanate compounds can be used alone or in combination of two or more.
[0033] Examples of the diol compound include polymer diols such as polyester diol compounds, polyether diol compounds, polycarbonate compounds, polybutadiene glycol compounds, etc. The diol compounds can be used alone or in combination of two or more kinds.
[0034] From the viewpoint of obtaining an ink layer for laser marking having good film properties, the number average molecular weight of the diol compound is preferably 400 or more, and more preferably 1,000 or more. Also, from the viewpoint of increasing the reactivity with the diisocyanate compound, the number average molecular weight of the diol compound is preferably 10,000 or less, and more preferably 6,000 or less.
[0035] Examples of the polyester diol compound include those obtained by reacting a low molecular weight diol component (linear glycols such as ethylene glycol, 1,3-propanediol, and 1,4-butanediol; branched glycols such as 1,2-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, and 2,4-diethyl-1,5-pentanediol; and ether-based diols such as diethylene glycol and triethylene glycol) with a dicarboxylic acid component (saturated and unsaturated aliphatic dicarboxylic acids such as succinic acid, adipic acid, and maleic acid; and aromatic dicarboxylic acids such as phthalic acid).
[0036] Examples of the polyether diol compound include polyester diol compounds obtained by ring-opening reaction of cyclic ester compounds (lactones, etc.), and polyether diol compounds obtained by polyaddition of oxyalkylenes (ethylene oxide, propylene oxide, etc.) or tetrahydrofuran to diol compounds ((poly)alkylene glycol compounds, bisphenols, etc.).
[0037] From the viewpoint of various physical properties of the ink, the diol compound is preferably a polyester diol or a polyether diol.
[0038] The chain extender can be a compound having two or more functional groups (amino group, hydroxyl group, etc.) that can react with an isocyanate group in the molecule. Examples of compounds having two or more amino groups in the molecule include diamines having two primary amino groups (ethylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, hexamethylenediamine, isophoronediamine, etc.), diamines having one primary amino group and one secondary amino group (2-ethylaminoethylamine, etc.), and polyamines having two primary amino groups and one or more secondary amino groups (diethylenetriamine, triethylenetetramine, etc.). Examples of hydroxyl-containing compounds having two or more hydroxyl groups in the molecule include low molecular weight diols (ethylene glycol, propylene glycol, butylene glycol, diethylene glycol, triethylene glycol, etc.). Further, examples of compounds having two amino groups and one hydroxyl group in the molecule include 1-mol adducts of ethylene oxide to diamines having two primary amino groups such as aminoethylethanolamine and aminopropylethanolamine. The chain extenders can be used alone or in combination of two or more kinds.
[0039] From the viewpoint of introducing functional groups such as hydroxyl groups and amino groups into the polyurethane resin molecule, the chain extender can be a compound having three or more functional groups such as amino groups and hydroxyl groups. Examples of the compound having three or more functional groups such as amino groups and hydroxyl groups include glycerin and aminoethylethanolamine.
[0040] The reaction terminator may be a compound having one or more functional groups (amino group, hydroxyl group, etc.) capable of reacting with an isocyanate group in the molecule, and specifically, may be monoalcohols (methanol, ethanol, etc.), monoamines (n-butylamine, di-n-butylamine, etc.), alkanolamines having one amino group and one hydroxyl group in the molecule (monoethanolamine, ethylethanolamine, diethanolamine), etc. The reaction terminator may also be a compound listed as the chain extender. From the viewpoint of introducing functional groups such as hydroxyl groups and amino groups into the polyurethane resin molecule, the reaction terminator may be an alkanolamine having one amino group and one hydroxyl group in the molecule, a diamine having two primary amino groups, or a low molecular weight diol, which are listed as examples of the chain extender. The reaction terminator may be used alone or in combination of two or more kinds.
[0041] In producing the urethane prepolymer obtained by reacting the diisocyanate compound with the diol compound, the equivalent ratio of NCO of the diisocyanate compound to OH of the diol compound (equivalent of NCO of the diisocyanate compound / equivalent of OH of the diol compound) is preferably 1.3 to 3, and more preferably 1.5 to 2.
[0042] The chain extender is preferably reacted in an amount of about 0.5 to 0.95 equivalents relative to the remaining isocyanate groups of the prepolymer, and the reaction terminator is preferably reacted in an amount of about 2 moles relative to 1 mole of the polyurethane resin after chain extension.
[0043] The weight average molecular weight of the polyurethane resin is preferably 5,000 to 50,000, more preferably 10,000 to 30,000. The weight average molecular weight of the present invention can be measured by gel permeation chromatography (GPC). As an example, chromatography is performed using a Water2690 (manufactured by Waters) as a GPC device and a PLgel, 5μ, MIXED-D (manufactured by Polymer Laboratories) as a column under the conditions of tetrahydrofuran as a developing solvent, a column temperature of 25°C, a flow rate of 1 milliliter / minute, an RI detector, a sample injection concentration of 10 milligrams / milliliter, and an injection amount of 100 microliters, and the weight average molecular weight can be calculated as a polystyrene-equivalent weight average molecular weight.
[0044] The polyurethane resin is preferably a polyurethane resin having a functional group such as a hydroxyl group or an amino group. As a method for obtaining a polyurethane resin having such a functional group, a known method can be adopted, such as a method using a compound having three or more functional groups such as the amino group or the hydroxyl group as a chain extender, or a method of reacting the diisocyanate compound at a molar ratio less than 1.0 times that of the diol compound without using the chain extender or the reaction terminator. When the polyurethane resin has an amino group, the amine value is preferably in the range of 0.1 to 10 mgKOH / g. The amine value indicates the total amount of free base and base, and is expressed as mg of potassium hydroxide equivalent to hydrochloric acid required to neutralize 1 g of sample.
[0045] In addition, the polyurethane resin may contain a biomass polyurethane resin in consideration of the environmental aspect. The biomass polyurethane resin will be described. In addition, among the descriptions of the biomass polyurethane resin, descriptions common to the above-mentioned polyurethane resin will be omitted as appropriate. The biomass polyurethane resin is a polyurethane resin containing a component derived from biomass (derived from plants). Since the biomass polyurethane resin can contribute to preventing global warming and reducing the environmental load compared to the case of using other exhaustible resources, it is preferable that the biomass polyurethane resin is obtained by synthesizing a urethane prepolymer by reacting a biopolyol component with an isocyanate component, and reacting this with a chain extender and a reaction terminator as necessary, and it is more preferable that the isocyanate component is a bioisocyanate derived from plants.
[0046] The binder resin may be a resin other than the polyurethane resin, as long as the performance of the ink composition is not deteriorated. Examples of the other resin include polyamide resin, vinyl chloride / vinyl acetate copolymer, (meth)acrylic copolymer, butyral resin, and cellulose derivative.
[0047] In addition, the ink composition for surface printing UV laser marking preferably contains an organic solvent to disperse or dissolve the above-mentioned components. The organic solvent can be used without any particular limitation, and examples thereof include alcohol-based organic solvents such as methanol, ethanol, n-propanol, isopropanol, butanol, etc.; ketone-based organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.; ester-based organic solvents such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, etc.; aliphatic hydrocarbon-based organic solvents such as n-hexane, n-heptane, n-octane, etc.; alicyclic hydrocarbon-based organic solvents such as cyclohexane, methylcyclohexane, ethylcyclohexane, cycloheptane, cyclooctane, etc.; aromatic hydrocarbon-based organic solvents such as toluene, xylene, etc. The organic solvents can be used alone or in combination of two or more.
[0048] From the viewpoint of applying the ink composition for surface-printing UV laser marking to flexographic printing or gravure printing and from the viewpoint of environmental considerations, it is preferable to use the alcohol-based organic solvent and / or the ester-based organic solvent as the organic solvent. In this case, the ratio of the alcohol-based organic solvent and / or the ester-based organic solvent in the organic solvent is preferably 90 mass % or more, and more preferably 95 mass % or more.
[0049] From the viewpoint of printability, the total proportion of the titanium oxide, the resin, and the organic solvent in the ink composition is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.
[0050] To the ink composition of the present invention, any of the following may be added, within the scope of not decreasing the performance of the ink composition: metal chelate crosslinking agents such as titanium chelate, zirconium chelate, etc.; waxes such as polyolefin wax, paraffin wax, etc.; fatty acid amides such as saturated fatty acid amides, unsaturated fatty acid amides, modified fatty acid amides, etc.; hard resins such as dimer acid resins, rosin resins, maleic acid resins, petroleum resins, terpene resins, ketone resins, dammar resins, copal resins, chlorinated polypropylene, and oxidized polypropylene; leveling agents, surfactants, plasticizers, etc.
[0051] The total proportion of the titanium oxide and the resin in the solid content of the ink composition is preferably 80 mass % or more, more preferably 90 mass % or more, and even more preferably 95 mass % or more, from the viewpoint of the various resistances and whiteness of the ink layer.
[0052] <Method of preparing overcoat agent and ink composition for surface UV laser marking> The method for preparing the overcoat agent and the ink composition for surface-printing UV laser marking is not particularly limited, and for example, the above-mentioned components may be added in order or simultaneously, and prepared using a roll mill, kneader, high-speed mixer, bead mill, ball mill, sand mill, ultrasonic disperser, high-pressure disperser, or the like.
[0053] <Overcoat layer> The overcoat layer of the present invention is formed from the overcoat agent. Specifically, the ink composition for surface-printing UV laser marking is coated (printed) on a substrate film described later to form an ink layer, and then the overcoat agent is coated (printed) on the surface of the ink layer to form an overcoat layer. The coating (printing) method can be offset printing, sheet-fed printing, digital printing (inkjet method, toner method), flexographic printing, or gravure printing, and flexographic printing and gravure printing are preferred. In addition, the coating (printing) may include a drying step for evaporating the solvent. Conventionally known conditions can be appropriately adopted as printing conditions.
[0054] The thickness of the ink layer is usually preferably 0.1 to 20 μm, and more preferably 0.2 to 15 μm, and the thickness of the overcoat layer is preferably 0.1 to 20 μm, and more preferably 0.2 to 15 μm, from the viewpoint of preventing cracks and curling.
[0055] <Laminate> In the laminate of the present invention, a base film is provided on one side of the ink layer, and the overcoat layer is provided on the other side of the ink layer. The ink layer and the overcoat layer may be a single layer or multiple layers (multilayers).
[0056] Examples of the material of the base film include films of metal, wood, paper, plastic, etc., and among these, plastic films are preferred. Examples of the plastic film include films of polyesters such as polyethylene terephthalate and polyethylene naphthalate, polycycloolefins, polyacetates, polyethersulfones, polycarbonates, polyamides, polyimides, (meth)acrylic polymers, polyvinyl chloride, polyvinylidene chloride, polyethylene, polypropylene, polystyrene, polyvinyl alcohol, polyarylates, polyphenylene sulfides, and cellulose polymers such as diacetyl cellulose and triacetyl cellulose.
[0057] The surface of the base film may be subjected to a surface treatment such as a corona treatment or a plasma treatment in order to improve the printability (wettability and adhesion) of the ink composition. In addition, in order to improve the gas barrier properties, a vapor deposition layer of a transparent inorganic oxide may be laminated thereon.
[0058] <Printed material> The printed matter of the present invention can be obtained by irradiating the laminate with a UV laser, which is a laser beam having a central wavelength in the range of 300 to 380 nm.
[0059] The laser light may be irradiated from the substrate film side of the laminate, or from the overcoat layer side of the laminate. From the viewpoint of obtaining a printed matter with a thinner overcoat layer in the laminate, it is preferable to irradiate the laser light from the overcoat layer side of the laminate. The irradiation conditions of the laser light may be appropriately set in consideration of the equipment used and the printing quality such as the printability of the printed matter. EXAMPLES
[0060] The present invention will be described below with reference to examples, but the present invention is not limited to these.
[0061] <Production Example> <Production of polyurethane resin varnish 1> In a four-neck flask equipped with a stirrer, a cooling tube, and a nitrogen gas inlet tube, 200 parts by mass of polyester diol having an average molecular weight of 2000 obtained from sebacic acid and 1,3-propanediol, 17.6 parts by mass of isophorone diisocyanate, and 21.0 parts by mass of hydrogenated diphenylmethane diisocyanate were charged, and reacted for 6 hours at 100 to 105 ° C. while introducing nitrogen gas. After cooling to near room temperature, 562 parts by mass of propyl acetate and 187 parts by mass of isopropyl alcohol were added, and then 8.2 parts by mass of isophorone diamine were added to extend the chain, and 0.35 parts by mass of monoethanolamine were added to react, and then 1.3 parts by mass of isophorone diamine and 0.6 parts by mass of diethylene triamine were added to stop the reaction, and polyurethane resin varnish 1 (solid content 25% by mass) was obtained.
[0062] <Preparation of overcoat agent and ink composition for surface UV laser marking> Each overcoat agent and ink composition for surface-printing UV laser marking were prepared by mixing the materials according to the compositions shown in Tables 1 and 2. The values shown in each table are parts by mass.
[0063] [Table 1]
[0064] [Table 2]
[0065] In Table 1-2, acrylic resin varnish 1 is an acrylic resin (acrylic polyol having a glass transition temperature of about 78°C, solid content 40% by mass); Acrylic resin varnish 2 is an acrylic resin (acrylic polyol having a glass transition temperature of about 50°C, solid content 40% by mass); The crosslinking agent was a polyfunctional isocyanate-based crosslinking agent (product name "Curing Agent No. 5000", manufactured by Sakata Inx Corporation, solid content 45% by mass); Titanium oxide 1 is titanium oxide coated with alumina and barium titanate (average particle size 0.23 μm); Titanium dioxide 2 is alumina and silica coated titanium dioxide (average particle size 0.29 μm); The wax refers to polyethylene wax (average particle size: 8 μm).
[0066] <Examples 1-11 and Comparative Examples 1-2> <Method of manufacturing laminate> Each ink composition obtained above was printed in a single layer or multiple layers on a polypropylene film (product name "P-2161", manufactured by Toyobo Co., Ltd.) using a printing plate. Then, each overcoat agent obtained above was applied in a single layer or multiple layers on the printed surface using a printing plate to produce each laminate. The ink composition, overcoat agent, printing plate, and number of prints (single layer or multiple layers) for each laminate are shown in Table 3.
[0067] The laminates obtained above were subjected to the following evaluations, and the results are shown in Table 3.
[0068] <Visibility> Using a UV laser marker FP-1000 manufactured by Keyence Corporation, laser light was irradiated from the side of each laminate obtained above other than the polypropylene film side to print (printing conditions: number of laser lines: 3), and the laser printability (visibility) was evaluated on the following 3-point scale, with ○ being the pass criterion. ○: The printed part is visible. △: The printed portion is visible, but is not sufficiently blackened and is gray. ×: The printed portion is difficult to see or printing is not possible.
[0069] <Measurement of Residual Solvents> Each laminate of Examples 8 to 11 (0.2 m 2 ) was placed in a 500 ml flask and heated in an oven at 80°C for 30 minutes to vaporize the solvent remaining in the printed matter. 1 ml of gas was sampled from the flask and the amount of residual solvent (mg / m 2 The residual solvent amount (mg / m 2) is considered to be 40 (mg / m2) from the viewpoint of odor in printed matter and packaging materials. 2 ) or less.
[0070] [Table 3]
[0071] In Table 3, H175lpi is Helio 175 line solid version; L32μ: Indicates a laser 175 line plate with a depth of 32μ solid plate.
Claims
1. An overcoat agent comprising a binder resin, The overcoat agent is used for covering an ink layer formed from an ink composition for surface-printing UV laser marking, which contains titanium oxide.
2. An overcoat layer formed from the overcoat agent according to claim 1.
3. 3. A laminate comprising: a base film provided on one side of said ink layer; and an overcoat layer according to claim 2 provided on the other side of said ink layer.
4. A printed matter obtained by irradiating the laminate according to claim 3 with a UV laser.
Citation Information
Patent Citations
Ink composition for laser marking, ink layer for laser marking, laminate, and laser marking method
JP2020001261A
Ink composition for laser marking, ink layer for laser marking, laminate, and laser marking method
JP2020002258A
Ink composition for laser marking, ink layer for laser marking, laminate, and laser marking method
JP2020002259A