Acid-modified polyester resin composition and laminate
Incorporating a fatty acid ester into acid-modified polyester resin compositions addresses processing and adhesive stability issues, enhancing flexibility and compatibility to achieve strong interlayer adhesion in laminates with PVA and biodegradable resins.
Patent Information
- Application Number
- JP2024049861
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-09
AI Technical Summary
Conventional acid-modified polyester resins face issues with processing stability and adhesive stability during granulation, leading to surging and reduced adhesive function, making it difficult to achieve both stability and strong adhesion in laminates with polyvinyl alcohol (PVA) and biodegradable resin layers.
Incorporating a fatty acid ester into the acid-modified polyester resin composition, which improves processing stability and adhesion by enhancing flexibility and compatibility, thereby stabilizing the resin composition and ensuring strong interlayer adhesion.
The addition of a fatty acid ester results in a resin composition with improved processing stability and high adhesive strength, preventing surging and zipping, allowing for a biodegradable laminate with excellent adhesiveness between PVA and biodegradable resin layers.
Smart Images

Figure 2024139768000001 
Figure 2024139768000002 
Figure 2024139768000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an acid-modified polyester resin composition and a laminate having a layer containing the acid-modified polyester resin composition. More specifically, the present invention relates to an acid-modified polyester resin composition that is preferably used for bonding a polyvinyl alcohol resin layer (hereinafter, polyvinyl alcohol is referred to as "PVA") to a biodegradable resin layer such as polylactic acid, and a laminate having a layer containing the acid-modified polyester resin composition. [Background technology]
[0002] Plastics are widely used as packaging materials because of their excellent moldability, strength, water resistance, transparency, etc. Examples of plastics used in such packaging materials include polyolefin resins such as polyethylene and polypropylene, vinyl resins such as polystyrene and polyvinyl chloride, and aromatic polyester resins such as polyethylene terephthalate. However, these plastics are poorly biodegradable, and if dumped in the natural environment after use, they may remain for a long time, damaging the scenery and causing environmental destruction.
[0003] In response to this, in recent years, biodegradable resins that are biodegraded or hydrolyzed in soil or water and are useful for preventing environmental pollution have attracted attention and are being put to practical use. Examples of such biodegradable resins include aliphatic polyester resins, cellulose acetate, and modified starch. As packaging materials, polylactic acid, condensation polymers of adipic acid / terephthalic acid / 1,4-butanediol, and condensation polymers of succinic acid / 1,4-butanediol / lactic acid are used because of their excellent transparency, heat resistance, and strength.
[0004] However, since aliphatic polyester resins such as polylactic acid have insufficient oxygen gas barrier properties, they cannot be used alone as packaging materials for contents that may be subject to oxidative deterioration, such as foods, medicines, etc. Therefore, aliphatic polyester resins such as polylactic acid and PVA resins are laminated to form laminates.
[0005] However, since the surface characteristics of an aliphatic polyester resin layer such as polylactic acid and a PVA resin layer are significantly different, the two layers have poor adhesion, and it is difficult to obtain a practical interlayer adhesive strength by directly laminating the two layers.
[0006] Therefore, an adhesive layer is provided to bond these resin layers, and in order to take advantage of the biodegradability of aliphatic polyester resins such as polylactic acid and PVA resins, the adhesive layer is also required to be biodegradable.
[0007] As a biodegradable adhesive resin, for example, Patent Document 1 proposes a biodegradable acid-modified polyester resin obtained by graft polymerizing an α,β-unsaturated carboxylic acid or an anhydride thereof onto a biodegradable polyester resin and having an acid value of 2.0 to 6.5 mg KOH / g. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2019 / 049798 Summary of the Invention [Problem to be solved by the invention]
[0009] Here, in the process of acid-modifying the polyester resin, the extrusion discharge rate becomes unstable, which may cause surging. Therefore, it is possible to reduce the amount of acid-modification of the polyester resin in order to suppress surging. However, if the amount of acid-modification of the polyester resin is reduced, the adhesive function may decrease, and zipping (repeated vibration of sticking and sliding) may occur. Therefore, in the past, when using acid-modified polyester resin, it was difficult to achieve both processing stability and adhesive stability during granulation.
[0010] Therefore, an object of the present invention is to provide a resin composition having excellent processing stability and adhesiveness. [Means for solving the problem]
[0011] As a result of intensive research, the inventors discovered that the above-mentioned object can be achieved by further containing a fatty acid ester in a resin composition containing an acid-modified polyester resin as a main component, and thus completed the present invention.
[0012] That is, the gist of the present invention is as follows.
[0013] A first aspect of the present invention is an acid-modified polyester resin composition containing an acid-modified polyester resin as a main component and containing a fatty acid ester.
[0014] A second aspect of the present invention is characterized in that in the acid-modified polyester resin composition of the first aspect, the fatty acid ester is a fatty acid ester composed of a polyhydric alcohol and a fatty acid having 1 to 18 carbon atoms.
[0015] A third aspect of the present invention is characterized in that in the acid-modified polyester resin composition of the first or second aspect, the content of the fatty acid ester is 0.01 to 20% by mass.
[0016] A fourth aspect of the present invention is characterized in that in the acid-modified polyester resin composition of any one of the first to third aspects, the acid-modified polyester resin is biodegradable.
[0017] A fifth aspect of the present invention is an adhesive containing the acid-modified polyester resin composition according to any one of the first to fourth aspects.
[0018] A sixth aspect of the present invention is a laminate having at least one layer containing the acid-modified polyester resin composition according to any one of the first to fourth aspects.
[0019] A seventh aspect of the present invention is a laminate having an adhesive layer between a first layer and a second layer, at least one of the first layer and the second layer being a polyvinyl alcohol-based resin layer, and the adhesive layer containing the acid-modified polyester-based resin composition described in any one of aspects 1 to 4. Effect of the Invention
[0020] The acid-modified polyester resin composition of the present invention contains a fatty acid ester, which improves the flexibility of the acid-modified polyester resin and prevents or suppresses the occurrence of surging, so that the composition has excellent processing stability and is easy to handle. In addition, when the acid-modified polyester resin composition of the present invention is used as an adhesive layer for both layers in a laminate containing a PVA resin layer and a biodegradable resin layer, the excellent adhesion prevents the occurrence of zipping (repeated vibration of sticking and sliding), and the high adhesion provides a biodegradable laminate with excellent adhesion between both layers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The configuration of the present invention will be described in detail below, but these are merely examples of preferred embodiments.
[0022] In addition, in this specification, "biodegradable" means meeting the conditions specified in JIS K 6953-1:2011 (ISO 14855-12005).
[0023] The acid-modified polyester resin composition of the present invention contains an acid-modified polyester resin as a main component, and also contains a fatty acid ester. Here, the main component of the acid-modified polyester resin composition refers to a component that occupies 50% by mass or more of the entire composition, preferably 80% by mass or more, and more preferably 90% by mass or more.
[0024] (Acid-modified polyester resin) The acid-modified polyester resin is a polyester resin obtained by graft polymerizing an α,β-unsaturated carboxylic acid or its anhydride (hereinafter, the α,β-unsaturated carboxylic acid or its anhydride may be referred to as "α,β-unsaturated carboxylic acids") onto various polyester resins, and serves as the base resin for the acid-modified polyester resin composition of the present invention.
[0025] In addition, the acid-modified polyester resin is preferably biodegradable, because by using a biodegradable acid-modified polyester resin, the entire laminate using an adhesive layer containing the acid-modified polyester resin becomes biodegradable.
[0026] Examples of the polyester resin include an aliphatic-aromatic copolymer polyester resin, an aliphatic polyester resin, and an aromatic polyester resin.
[0027] The aliphatic-aromatic copolymer polyester resin is an aromatic-aliphatic copolymer polyester resin containing an aliphatic diol unit, an aliphatic dicarboxylic acid unit, and an aromatic dicarboxylic acid unit as main constituent units. Specifically, for example, the main constituent units are an aliphatic diol unit represented by the following formula (1), an aliphatic dicarboxylic acid unit represented by the following formula (2), and an aromatic dicarboxylic acid unit represented by the following formula (3), and the resin is preferably biodegradable.
[0028] -OR 1 -O- ···(1) In formula (1), R 1 represents a divalent aliphatic hydrocarbon group. -OC-R 2 -CO- ···(2) In formula (2), R 2 represents a single bond or a divalent aliphatic hydrocarbon group. -OC-R 3 -CO- ···(3) In formula (3), R 3 represents a divalent aromatic hydrocarbon group.
[0029] The aliphatic diol that gives the aliphatic diol unit of formula (1) is not particularly limited, but is preferably one having 2 to 10 carbon atoms in terms of the balance between cost and mechanical strength. Examples include ethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,4-cyclohexandimethanol. Among them, aliphatic diols having 2 to 4 carbon atoms are preferred, ethylene glycol and 1,4-butanediol are more preferred, and 1,4-butanediol is particularly preferred. It is also possible to use two or more of the above aliphatic diols.
[0030] The aliphatic dicarboxylic acid component that gives the aliphatic dicarboxylic acid unit of formula (2) is not particularly limited, but is preferably one having 2 to 12 carbon atoms in terms of the balance between cost and biodegradability. Examples include succinic acid, adipic acid, suberic acid, sebacic acid, azelaic acid, dodecanedioic acid, and derivatives thereof such as alkyl esters. Among these, sebacic acid, adipic acid, azelaic acid, and derivatives thereof such as alkyl esters are preferred. Two or more kinds of the above aliphatic dicarboxylic acid components can also be used.
[0031] Examples of aromatic dicarboxylic acid components that provide the aromatic dicarboxylic acid unit of formula (3) include terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, furandicarboxylic acid, and the like, and derivatives thereof such as alkyl esters. Among these, from the viewpoint of biodegradability, R 3 is preferably a phenylene group, and the aromatic dicarboxylic acid component that gives the aromatic dicarboxylic acid unit of formula (3) is preferably terephthalic acid, isophthalic acid, or a derivative thereof such as an alkyl ester, and more preferably terephthalic acid or a derivative thereof such as an alkyl ester. In addition, it may be an aromatic dicarboxylic acid in which a part of the aromatic ring is substituted with a sulfonate. Two or more kinds of the aromatic dicarboxylic acid components may be used.
[0032] The content of aromatic dicarboxylic acid units in the aliphatic-aromatic copolymerized polyester resin is preferably 5 mol% or more, more preferably 35 mol% or more, particularly preferably 40 mol% or more, and preferably 95 mol% or less, more preferably 65 mol% or less, particularly preferably 60 mol% or less, based on 100 mol% of the total of aliphatic dicarboxylic acid units and aromatic dicarboxylic acid units as the total dicarboxylic acid units, from the viewpoint of melting point and biodegradability. That is, the content of aromatic dicarboxylic acid units is preferably 5 mol% or more and 95 mol% or less, based on 100 mol% of the total of aliphatic dicarboxylic acid units and aromatic dicarboxylic acid units as the total dicarboxylic acid units.
[0033] In addition, when two or more aromatic dicarboxylic acids are used, the aliphatic-aromatic copolymer polyester resin preferably has a ratio of terephthalic acid units in all aromatic dicarboxylic acid units of 40 mol% or more and 60 mol% or less. If this ratio is less than 40 mol%, heat resistance is insufficient, and if it exceeds 60 mol%, biodegradability tends to deteriorate. From this viewpoint, the ratio of terephthalic acid units in all aromatic dicarboxylic acid units in the aliphatic-aromatic copolymer polyester resin is more preferably 42 mol% or more and 58 mol% or less, and even more preferably 45 mol% or more and 55 mol% or less.
[0034] The aliphatic-aromatic copolymer polyester resin may have an aliphatic oxycarboxylic acid unit. Specific examples of the aliphatic oxycarboxylic acid component that gives the aliphatic oxycarboxylic acid unit include lactic acid, glycolic acid, 2-hydroxy-n-butyric acid, 2-hydroxycaproic acid, 6-hydroxycaproic acid, 2-hydroxy-3,3-dimethylbutyric acid, 2-hydroxy-3-methylbutyric acid, 2-hydroxyisocaproic acid, or a mixture thereof. Furthermore, it may be a derivative such as a lower alkyl ester or an intramolecular ester thereof. When optical isomers exist in these, they may be any of D-form, L-form, or racemic form, and may be in the form of a solid, liquid, or aqueous solution. Among these, preferred is lactic acid or glycolic acid, or a derivative thereof. These aliphatic oxycarboxylic acid components may be used alone or as a mixture of two or more kinds.
[0035] When the aliphatic-aromatic copolymer polyester resin contains these aliphatic oxycarboxylic acid units, the content thereof is preferably 20 mol % or less, more preferably 10 mol % or less, assuming that all constituent units constituting the aliphatic-aromatic copolymer polyester resin are 100 mol %.
[0036] The aliphatic polyester resin is an aliphatic polyester resin containing an aliphatic diol unit and an aliphatic dicarboxylic acid unit as main constituent units. The aliphatic polyester resin is distinguished from the aliphatic-aromatic copolymer polyester resin by not containing an aromatic dicarboxylic acid unit.
[0037] More specifically, the aliphatic polyester resin is a polyester resin containing an aliphatic diol unit represented by the following formula (4) and an aliphatic dicarboxylic acid unit represented by the following formula (5). -OR 4 -O-...(4) In formula (4), R 4 represents a divalent aliphatic hydrocarbon group. -OC-R 5 -CO- ···(5) In formula (5), R 5represents a divalent aliphatic hydrocarbon group.
[0038] The aliphatic diol unit represented by the above formula (4) and the aliphatic dicarboxylic acid unit represented by the above formula (5) may be derived from a compound derived from petroleum or from a compound derived from a plant raw material, but are preferably derived from a compound derived from a plant raw material.
[0039] When the aliphatic polyester resin is a copolymer, the aliphatic polyester resin may contain two or more types of aliphatic diol units represented by formula (4), and the aliphatic polyester resin may contain two or more types of aliphatic dicarboxylic acid units represented by formula (5).
[0040] The aliphatic diol that gives the diol unit represented by formula (4) is not particularly limited, but from the viewpoint of moldability and mechanical strength, an aliphatic diol having 2 to 10 carbon atoms is preferred, and an aliphatic diol having 4 to 6 carbon atoms is particularly preferred. Examples include ethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,4-cyclohexanedimethanol, and among these, 1,4-butanediol is particularly preferred. Note that two or more of the above aliphatic diols can be used.
[0041] The aliphatic dicarboxylic acid component that gives the aliphatic dicarboxylic acid unit represented by formula (5) is not particularly limited, but is preferably an aliphatic dicarboxylic acid having 2 to 40 carbon atoms or a derivative thereof such as an alkyl ether, and particularly preferably an aliphatic dicarboxylic acid having 4 to 10 carbon atoms or a derivative thereof such as an alkyl ester. Examples of the aliphatic dicarboxylic acid or a derivative thereof such as an alkyl ester include succinic acid, adipic acid, suberic acid, sebacic acid, dodecanedioic acid, dimer acid, etc., and derivatives thereof such as alkyl esters, among which succinic acid, adipic acid, and sebacic acid are preferred, and succinic acid and adipic acid are particularly preferred. It is also possible to use two or more kinds of the above aliphatic dicarboxylic acid components.
[0042] The aliphatic polyester resin may have a repeating unit (aliphatic oxycarboxylic acid unit) derived from an aliphatic oxycarboxylic acid. Specific examples of the aliphatic oxycarboxylic acid component that gives the aliphatic oxycarboxylic acid unit include, for example, lactic acid, glycolic acid, 2-hydroxy-n-butyric acid, 2-hydroxycaproic acid, 6-hydroxycaproic acid, 2-hydroxy-3,3-dimethylbutyric acid, 2-hydroxy-3-methylbutyric acid, 2-hydroxyisocaproic acid, and the like, or derivatives thereof such as lower alkyl esters or intramolecular esters. When optical isomers exist in these, they may be any of D-form, L-form, or racemic form, and may be in the form of a solid, liquid, or aqueous solution. Among these, lactic acid or glycolic acid or derivatives thereof are particularly preferred. These aliphatic oxycarboxylic acids may be used alone or as a mixture of two or more.
[0043] When the aliphatic polyester resin contains these aliphatic oxycarboxylic acid units, from the viewpoint of moldability, the content thereof is preferably 20 mol % or less, more preferably 10 mol % or less, even more preferably 5 mol % or less, and most preferably 3 mol % or less, based on 100 mol % of all constituent units constituting the aliphatic polyester resin.
[0044] The polyester resin may be obtained by synthesis or may be a commercially available product. When synthesizing, a known method for producing polyester may be adopted. In addition, the polyester resin is not limited to one type, and two or more types of polyester resins having different types of constituent units, ratios of constituent units, production methods, physical properties, etc. may be blended and used.
[0045] Examples of polyester-based resins include polybutylene adipate terephthalate (hereinafter sometimes referred to as "PBAT"), polybutylene succinate terephthalate (hereinafter sometimes referred to as "PBST"), polybutylene succinate adipate (hereinafter sometimes referred to as "PBSA"), polybutylene succinate (hereinafter sometimes referred to as "PBS"), polybutylene sebacate terephthalate (hereinafter sometimes referred to as "PBSeT"), polybutylene succinate adipate terephthalate (hereinafter sometimes referred to as "PBSAT"), polycaprolactone (hereinafter sometimes referred to as "PCL"), and the like.
[0046] Examples of commercially available polyester resins include "Ecoflex (registered trademark)" manufactured by BASF, which contains a condensation polymer of adipic acid / terephthalic acid / 1,4-butanediol as its main component, and "BioPBS" manufactured by Mitsubishi Chemical Corporation, which contains a condensation polymer of succinic acid / 1,4-butanediol as its main component.
[0047] As described above, the acid-modified polyester resin is modified by graft polymerizing an α,β-unsaturated carboxylic acid onto a raw material polyester resin.
[0048] Specific examples of α,β-unsaturated carboxylic acids include α,β-unsaturated monocarboxylic acids such as acrylic acid and methacrylic acid; α,β-unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, citrus acid, tetrahydrophthalic acid, crotonic acid, and isocrotonic acid, or their anhydrides, and are preferably anhydrides of α,β-unsaturated dicarboxylic acids, and more preferably maleic anhydride. These α,β-unsaturated carboxylic acids may be used not only as a single type but also as a combination of two or more types.
[0049] The method for graft-polymerizing the α,β-unsaturated carboxylic acid to the polyester resin as the raw material is not particularly limited, and a known method can be used. Although only a thermal reaction is possible, it is preferable to use a radical initiator in order to increase the reactivity. In addition, examples of the reaction method include a solution reaction, a reaction in a suspension, and a reaction in a molten state without using a solvent (melting method), and among these, the melting method is preferable.
[0050] The melting method will now be described in detail. As the melting method, a method in which the raw material polyester resin, α,β-unsaturated carboxylic acid, and radical initiator are mixed in advance and then melt-kneaded in a kneader to react, or a method in which the α,β-unsaturated carboxylic acid and radical initiator are added to the polyester resin in a molten state in a kneader can be used.
[0051] As a mixer used when premixing the raw materials, for example, a Henschel mixer, a ribbon blender, etc. can be used, and as a kneader used for melt kneading, for example, a single-screw or twin-screw extruder, a roll, a Banbury mixer, a kneader, a Brabender mixer, etc. can be used.
[0052] The temperature during melt kneading may be appropriately set within a range that is equal to or higher than the melting point of the raw material polyester resin and does not cause thermal degradation, preferably 100 to 250°C, more preferably 160 to 230°C.
[0053] The amount of α,β-unsaturated carboxylic acid is usually 0.0001 to 5 parts by mass, preferably 0.001 to 2 parts by mass, more preferably 0.02 to 1 part by mass, based on 100 parts by mass of the raw material polyester resin. If the amount is too small, a sufficient amount of polar groups is not introduced into the polyester resin, and the interlayer adhesion, especially the adhesion to the PVA resin layer, tends to be insufficient. If the amount is too large, the α,β-unsaturated carboxylic acid that has not been graft-polymerized may remain in the resin, which tends to cause poor appearance.
[0054] The radical initiator is not particularly limited, and known radical initiators can be used. For example, organic or inorganic peroxides such as t-butyl hydroperoxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-bis(t-butyloxy)hexane, 3,5,5-trimethylhexanoyl peroxide, t-butyl peroxybenzoate, benzoyl peroxide, m-toluoyl peroxide, dicumyl peroxide, 1,3-bis(t-butylperoxyisopropyl)benzene, dibutyl peroxide, methyl ethyl ketone peroxide, potassium peroxide, and hydrogen peroxide; azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(isobutylamide)dihalide, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide] and azodi-t-butane; and carbon radical generators such as dicumyl. These may be used alone or in combination of two or more kinds.
[0055] The amount of the radical initiator to be added is usually 0.00001 to 5.0 parts by mass, particularly 0.0001 to 1.0 part by mass, and especially 0.002 to 0.5 part by mass, per 100 parts by mass of the raw material polyester resin.
[0056] If the amount of the radical initiator is too small, graft polymerization may not occur sufficiently, and the effects of the present invention may not be obtained. If the amount of the radical initiator is too large, the polyester resin may decompose to reduce its molecular weight, and the adhesive strength may tend to be insufficient due to insufficient cohesive force.
[0057] In the present invention, the acid-modified polyester resin is preferably an acid-modified aliphatic-aromatic copolymer polyester resin or an acid-modified aliphatic polyester resin, and more preferably an acid-modified aliphatic-aromatic copolymer polyester resin.
[0058] The weight average molecular weight of the acid-modified polyester resin is preferably 50,000 to 400,000, more preferably 100,000 to 200,000, and particularly preferably 140,000 to 180,000. If the weight average molecular weight is too large, the melt viscosity tends to increase and melt molding tends to become difficult, whereas if it is too small, the molded product tends to become brittle. The weight average molecular weight of the acid-modified polyester resin is measured by gel permeation chromatography (GPC).
[0059] The acid-modified polyester resin preferably has an acid value of 1.0 to 6.5 mg·KOH / g, more preferably 1.1 to 6.0 mg·KOH / g, and further preferably 1.2 to 5.0 mg·KOH / g. If the acid value is too high, the appearance tends to be poor, and if it is too low, the adhesion to other resins tends to decrease. If the acid value is too high or too low, the effects of the present invention tend to be difficult to obtain.
[0060] The method for measuring the acid value will be described in detail below. First, the acid-modified polyester resin to be measured is thoroughly washed with a solvent. This washing is for washing away impurities in the acid-modified polyester resin, mainly unreacted α,β-unsaturated carboxylic acid or its anhydride. As such a solvent, it is necessary to use a solvent in which the acid-modified polyester resin does not dissolve, and examples of such a solvent include water, acetone, methanol, ethanol, and isopropanol. Next, after drying the washed acid-modified polyester, 100 ml of tetrahydrofuran is placed in a test bottle as a solvent, and 5 g of acid-modified polyester resin is added while stirring with a hot stirrer (set temperature 75°C, stirrer rotation speed 400 rpm). Stir for 5 to 6 hours until the acid-modified polyester resin dissolves. After dissolution, 4 ml of ultrapure water is added and stirred for an additional 10 minutes to prepare a test solution. The test solution is titrated with an aqueous potassium hydroxide solution (N / 10) using an automatic titrator, and the acid value is calculated using the following formula.
[0061] (formula) Acid value AV (mg KOH / g)=((AB)×f×5.61) / S A = Amount (ml) of potassium hydroxide solution N / 10 required for acid-modified polyester resin B = Amount (ml) of potassium hydroxide solution N / 10 required for blank test f = Titer of potassium hydroxide solution N / 10 S = Amount (g) of acid-modified aliphatic polyester resin (B) collected
[0062] The titration device may be, for example: Titration measurement device: Kyoto Electronics Manufacturing Co., Ltd. automatic potentiometric titrator AT-610 Reference electrode: Composite glass electrode C-171 Titration solution: Fujifilm Wako Pure Chemical Corporation Potassium hydroxide aqueous solution (N / 10)
[0063] The acid value can be controlled, for example, by the following methods. (i) A method of adjusting the amount of a radical initiator when graft polymerizing an α,β-unsaturated carboxylic acid or anhydride thereof onto a polyester resin. (ii) A method in which the acid-modified polyester resin is dried to reduce the water absorption rate. Among these, the method (i) is preferred because of the ease of controlling the acid value.
[0064] The melt flow rate (MFR) of the acid-modified polyester resin is preferably 1.0 to 20.0 g / 10 min, more preferably 1.5 to 10.0 g / 10 min, and particularly preferably 2.0 to 8.0 g / 10 min, when measured at 210° C. and 2.16 kg. The MFR of the acid-modified polyester resin can be adjusted by the molecular weight.
[0065] The melting point of the acid-modified polyester resin is preferably 65 to 260°C, more preferably 70 to 200°C, and further preferably 75 to 140°C.
[0066] In the present invention, the acid-modified polyester resin is not limited to one type, and a blend of two or more types of acid-modified polyester resins differing in the types and ratios of constituent units, production methods, physical properties, etc. may be used.
[0067] (Fatty acid ester) The acid-modified polyester resin composition of the present invention contains a fatty acid ester as an additive. It is presumed that the acid-modified polyester resin is softened by the fatty acid ester contained in the acid-modified polyester resin composition, and when a laminate having an adhesive layer containing the acid-modified polyester resin composition is formed, the interlayer adhesion is improved. In addition, the fatty acid ester has excellent compatibility with the acid-modified polyester resin.
[0068] From the viewpoint of compatibility with the acid-modified polyester resin, the fatty acid ester is preferably a fatty acid ester composed of a polyhydric alcohol and a fatty acid having 1 to 18 carbon atoms. Here, the number of carbon atoms of the fatty acid constituting the fatty acid ester is preferably 1 to 18, more preferably 1 to 12, and further preferably 1 to 6. In addition, suitable specific examples of the fatty acid ester include, for example, glycerin fatty acid ester, sugar ester, polyglycerin fatty acid ester, etc. In addition, the fatty acid ester may be used alone or in combination of two or more kinds.
[0069] (Acid-modified polyester resin composition) As described above, the acid-modified polyester resin composition of the present invention contains an acid-modified polyester resin as a base resin and a fatty acid ester.
[0070] The content of the acid-modified polyester resin in the acid-modified polyester resin composition is preferably 50 to 99.99% by mass, more preferably 80 to 99.70% by mass, and even more preferably 90 to 99.50% by mass. When the content of the acid-modified polyester resin is 50% by mass or more, sufficient adhesive strength is easily exhibited, and when it is 99.99% by mass or less, processability is easily improved.
[0071] The fatty acid ester is preferably contained in the acid-modified polyester resin composition in the range of 0.01 to 20% by mass. When the fatty acid ester is contained in the acid-modified polyester resin composition in the range of 0.01% by mass or more, the desired effect of the present invention is easily obtained. In addition, if the fatty acid ester content is too high, vent-up due to the volatilization of the fatty acid ester during extrusion processing tends to occur, so the fatty acid ester is preferably contained in an amount of 20% by mass or less. The fatty acid ester content in the acid-modified polyester resin composition is more preferably 0.05% by mass or more, even more preferably 0.1% by mass or more, and more preferably 7% by mass or less, and even more preferably 5% by mass or less.
[0072] The acid-modified polyester resin composition of the present invention may contain other components within the range that does not impair the effects of the present invention, such as reinforcing agents, fillers, plasticizers, pigments, dyes, lubricants, antioxidants, antistatic agents, UV absorbers, heat stabilizers, light stabilizers, surfactants, antibacterial agents, antistatic agents, drying agents, antiblocking agents, flame retardants, crosslinking agents, curing agents, foaming agents, and crystal nucleating agents.
[0073] The acid-modified polyester resin composition of the present invention is usually made into a molded product such as pellets or powder in order to be used as a molding material. Among them, the pellet shape is preferred from the viewpoints of ease of feeding into a molding machine, handling, and minimizing problems of fine powder generation. While known methods can be used for forming the material into pellets, it is efficient to extrude the material in the form of a strand from an extruder, cool it, and then cut it to a predetermined length to form cylindrical pellets. The size of such cylindrical pellets is usually 1 to 4 mm, preferably 2 to 3 mm in length, and usually 1 to 4 mm, preferably 2 to 3 mm in diameter.
[0074] The method for producing the acid-modified polyester resin composition of the present invention is not particularly limited, and any known method can be used. Examples of the method include a method in which a fatty acid ester is added and mixed when the acid-modified polyester resin is produced, and a method in which a fatty acid ester is added and mixed after the acid-modified polyester resin is produced. For example, the following (i) to (ix) can be mentioned. (i) A method in which an α,β-unsaturated carboxylic acid, a radical initiator, and a fatty acid ester are mixed in advance with a polyester resin as a raw material, and then the mixture is melt-kneaded in a kneader to cause a reaction. (ii) A method in which an α,β-unsaturated carboxylic acid, a radical initiator, and a fatty acid ester are mixed with a polyester resin in a molten state in a kneader, and the mixture is melt-kneaded to cause a reaction. (iii) A method in which an α,β-unsaturated carboxylic acid and a radical initiator are mixed with a polyester resin and a fatty acid ester in a molten state in a kneader, and the mixture is melt-kneaded to cause a reaction. (iv) A method in which an α,β-unsaturated carboxylic acid and a radical initiator are mixed with a raw material polyester resin in advance, and then the mixture is melted and kneaded in a kneader to react, while a fatty acid ester is added and kneaded. (v) A method in which α,β-unsaturated carboxylic acids, a radical initiator, and a fatty acid ester are dissolved in a solvent in the raw material polyester resin, and the mixture is reacted in solution form. (vi) A method in which α,β-unsaturated carboxylic acids, a radical initiator, and a fatty acid ester are dissolved in a solvent and mixed in a suspension state with a polyester resin as a raw material to cause a reaction. (vii) A method in which an acid-modified polyester resin and a fatty acid ester are dry-blended, then melted and kneaded. (viii) A method in which an acid-modified polyester resin and a fatty acid ester are dissolved in a solvent and mixed in the form of a solution. (ix) A method in which a laminate containing an acid-modified polyester resin layer and a fatty acid ester layer is pulverized, melted, and kneaded. Although the methods (i) to (vi) can be carried out by thermal reaction alone, it is preferable to use a radical initiator in order to increase reactivity. As the reaction method, a solution reaction, a reaction in a suspension, a reaction in a molten state without using a solvent, etc. (melting method), etc. can be mentioned, and among them, the melting method is preferable. The method (ix) is mainly used for recycling the ends of a laminate.
[0075] As a mixer used when premixing the raw materials, for example, a Henschel mixer, a ribbon blender, etc. can be used, and as a kneader used for melt kneading, for example, a single-screw or twin-screw extruder, a roll, a Banbury mixer, a kneader, a Brabender mixer, etc. can be used. As a method of melt-kneading, in the production method (iv) above, for example, an acid-modified polyester resin, an aliphatic ester and any optional components are mixed using a mixer such as a Henschel mixer or a ribbon blender, and then melted and kneaded using a melt kneader such as a single-screw or twin-screw extruder, a roll, a Banbury mixer, a kneader or a Brabender mixer. As for the manufacturing method of the above (ix), for example, there can be mentioned a method in which unnecessary parts such as both ends of a multilayer film having layers each containing an acid-modified polyester resin and an aliphatic ester are crushed, and optional components are added as necessary, and the mixture is melted and kneaded in a melt kneader such as a single-screw or twin-screw extruder, a roll, a Banbury mixer, a kneader, or a Brabender mixer.
[0076] The temperature during melt kneading can be set appropriately within a temperature range that is equal to or higher than the melting points of the acid-modified polyester resin and the aliphatic ester and does not cause thermal degradation, but is preferably 100 to 300°C, more preferably 140 to 250°C, and particularly preferably 160 to 230°C.
[0077] The resin composition used in the present invention has excellent fluidity and is easy to handle, and is therefore useful as a molding material. As a melt molding method, known molding methods such as extrusion molding, inflation molding, injection molding, blow molding, vacuum molding, pressure molding, compression molding, and calendar molding can be used.
[0078] The molded article of the present invention may have a wide variety of shapes, such as a film, a sheet, a pipe, a disk, a ring, a bag, a bottle, or a fiber.
[0079] [Laminate] The acid-modified polyester resin composition of the present invention is preferably used as an adhesive resin (adhesive) to bond two members together. The laminate of the present invention has at least one layer containing the acid-modified polyester resin composition of the present invention. Moreover, a laminate according to one embodiment of the present invention includes an adhesive layer between a first layer and a second layer, at least one of the first layer and the second layer being a PVA-based resin layer, and the adhesive layer contains the acid-modified polyester-based resin composition of the present invention. Among them, the laminate of the present invention is preferably one using a PVA-based resin layer as a gas barrier layer and a biodegradable resin layer as an outer layer. Hereinafter, the laminate including an adhesive (A) layer containing the acid-modified polyester resin composition of the present invention, a PVA-based resin (B) layer, and a biodegradable resin (C) layer will be mainly described, but the present invention is not limited thereto.
[0080] (Adhesive (A) layer) The adhesive (A) layer is an adhesive layer used when laminating a PVA-based resin (B) layer and a biodegradable resin (C) layer, and is formed from an adhesive resin containing the acid-modified polyester-based resin composition of the present invention described above. The adhesive resin contains the acid-modified polyester resin composition of the present invention as a main component, and the content of the acid-modified polyester resin composition is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, with the upper limit being 100% by mass.
[0081] (PVA resin (B) layer) The PVA-based resin (B) layer preferably provides gas barrier properties to the laminate of the present invention. The PVA-based resin (B) layer used in the present invention is a layer mainly composed of the PVA-based resin (B), and preferably contains 70% by mass or more of the PVA-based resin (B), more preferably 80% by mass or more, and even more preferably 90% by mass or more. The upper limit is 100% by mass. If the content is too low, the gas barrier property tends to be insufficient.
[0082] The PVA resin (B) used in the present invention is a resin mainly composed of vinyl alcohol structural units, which is obtained by saponifying a polyvinyl ester resin obtained by polymerizing a vinyl ester monomer, and is composed of vinyl alcohol structural units and vinyl ester structural units corresponding to the degree of saponification.
[0083] Examples of the vinyl ester monomer include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl versatate, with vinyl acetate being economically preferred.
[0084] The average degree of polymerization (measured in accordance with JIS K6726) of the PVA resin (B) used in the present invention is preferably 200 to 1800, particularly 300 to 1500, and even more preferably 300 to 1000.
[0085] If the average polymerization degree is too low, the mechanical strength of the PVA resin (B) layer tends to be insufficient, whereas if the average polymerization degree is too high, the flowability tends to decrease and moldability tends to decrease when the PVA resin (B) layer is formed by hot melt molding, and shear heat may be abnormally generated during molding, making the PVA resin (B) susceptible to thermal decomposition.
[0086] The PVA resin (B) used in the present invention preferably has a saponification degree (average saponification degree measured in accordance with JIS K6726) of 80 to 100 mol %, particularly preferably 90 to 99.9 mol %, and more particularly preferably 98 to 99.9 mol %. If the degree of saponification is too low, the gas barrier properties tend to decrease.
[0087] In the present invention, the PVA-based resin (B) may be one obtained by copolymerizing various monomers during the production of a polyvinyl ester-based resin and then saponifying the copolymer, or one of various modified PVA-based resins obtained by introducing various functional groups into unmodified PVA by post-modification.
[0088] Examples of monomers used for copolymerization with vinyl ester monomers include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, 5-hexen-1-ol, and 3,4-dihydroxy-1-butene; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid; salts, monoesters, or dialkyl esters of the same; nitriles such as acrylonitrile and methacrylonitrile; diacetone acrylate; Examples of suitable vinyl acetates include amides such as olefin sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, and the like, and salts thereof; alkyl vinyl ethers, dimethylallyl vinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinyl ethylene carbonate, 2,2-dialkyl-4-vinyl-1,3-dioxolane, glycerin monoallyl ether, and 3,4-diacetoxy-1-butene, and other vinyl compounds; substituted vinyl acetates such as isopropenyl acetate and 1-methoxyvinyl acetate; vinylidene chloride, 1,4-diacetoxy-2-butene, and vinylene carbonate.
[0089] In addition, examples of modified PVA-based resins into which functional groups have been introduced by post-modification include those having acetoacetyl groups by reaction with diketene, those having polyalkylene oxide groups by reaction with ethylene oxide, those having hydroxyalkyl groups by reaction with epoxy compounds, and those obtained by reacting aldehyde compounds having various functional groups with PVA.
[0090] The content of modified species in such modified PVA-based resins, i.e., constituent units derived from various monomers in the copolymer or functional groups introduced by post-reaction, cannot be generally determined because the characteristics vary greatly depending on the modified species, but is preferably 1 to 20 mol %, and particularly preferably in the range of 2 to 10 mol %.
[0091] Among these various modified PVA-based resins, in the present invention, a PVA-based resin having a structural unit having a 1,2-diol structure in a side chain, as represented by the following general formula (6) (hereinafter, sometimes referred to as a "1,2-diol structural unit"), is preferably used because it facilitates melt molding in the production method of the laminate of the present invention described below.
[0092] [ka]
[0093] In addition, R in the 1,2-diol structural unit represented by the general formula (6) 11 ~R 14 each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 4 carbon atoms.
[0094] Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a tert-butyl group. If necessary, the alkyl group may have a functional group such as a halogen group, a hydroxyl group, an ester group, a carboxylic acid group, or a sulfonic acid group.
[0095] Furthermore, X in the 1,2-diol structural unit represented by the general formula (6) represents a single bond or a bonding chain. Examples of such a bonding chain include hydrocarbons such as linear or branched alkylene groups having 1 to 6 carbon atoms, linear or branched alkenylene groups having 1 to 6 carbon atoms, linear or branched alkynylene groups having 1 to 6 carbon atoms, phenylene groups, and naphthylene groups (these hydrocarbons may be substituted with halogen atoms such as fluorine atoms, chlorine atoms, and bromine atoms), as well as -O-, -(CH 2 O) t -, -(OCH 2 ) t -, -(CH 2 O) t CH 2 -, -CO-, -COCO-, -CO(CH2) t CO-, -CO(C 6 H 4 )CO-, -S-, -CS-, -SO-, -SO 2 -, -NR-, -CONR-, -NRCO-, -CSNR-, -NRCS-, -NRNR-, -HPO 4 -, -Si(OR) 2 -, -OSi (OR) 2 -, -OSi (OR) 2 O-, -Ti(OR) 2 -, -OTi(OR) 2 -, -OTi(OR) 2 Examples thereof include -O-, -Al(OR)-, -OAl(OR)-, -OAl(OR)O- and the like (each R is independently an arbitrary substituent and represents a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms, and t represents an integer of 1 to 5). Among these, the linking chain is preferably a linear or branched alkylene group having 1 to 6 carbon atoms, particularly a methylene group, or a -CH 2 OCH 2 - is preferred.
[0096] X is most preferably a single bond in terms of thermal stability and stability under high temperature and acidic conditions.
[0097] Among the 1,2-diol structural units represented by general formula (6), R11 ~R 14 A structural unit represented by the following general formula (6'), in which all of are hydrogen atoms and X is a single bond, is most preferred.
[0098] [ka]
[0099] Examples of a method for producing such a PVA-based resin having a 1,2-diol structural unit in a side chain include the method described in paragraphs
[0026] to
[0034] of JP-A No. 2015-143356.
[0100] The content of the 1,2-diol structural unit contained in the PVA resin having the 1,2-diol structural unit in the side chain is preferably 1 to 20 mol%, more preferably 2 to 10 mol%, and particularly preferably 3 to 8 mol%. If the content is too low, it is difficult to obtain the effect of the 1,2-diol structure in the side chain, and conversely, if the content is too high, the gas barrier property at high humidity tends to decrease significantly.
[0101] The content of 1,2-diol structural units in PVA resin is calculated based on the content of the PVA resin after complete saponification. 1 The content can be determined from H-NMR spectrum (solvent: DMSO-d6, internal standard: tetramethylsilane). Specifically, the content may be calculated from the peak areas derived from the hydroxyl group protons, methine protons, and methylene protons in the 1,2-diol structural unit, the methylene protons of the main chain, and the protons of the hydroxyl group linked to the main chain.
[0102] The PVA resin (B) used in the present invention may be one type or a mixture of two or more types. When the PVA resin (B) is a mixture of two or more types, the following combinations may be used: unmodified PVAs, unmodified PVA and a PVA resin having a structural unit represented by general formula (6), PVA resins having structural units represented by general formula (6) with different degrees of saponification, polymerization, modification, etc., unmodified PVA, or a PVA resin having a structural unit represented by general formula (6) and another modified PVA resin.
[0103] The PVA-based resin (B) layer used in the present invention may contain, in addition to the PVA-based resin (B), a heat stabilizer, an antioxidant, an ultraviolet absorber, a crystal nucleating agent, an antistatic agent, a flame retardant, a plasticizer, a lubricant, a filler, a lubricant, or a crystal nucleating agent.
[0104] (Biodegradable resin (C) layer) The biodegradable resin (C) layer is a layer mainly composed of the biodegradable resin (C) and contains preferably 70% by mass or more, more preferably 80% by mass or more, and more preferably 90% by mass or more of the biodegradable resin (C), with the upper limit being 100% by mass.
[0105] Examples of the biodegradable resin (C) include aliphatic polyesters such as polylactic acid (PLA), adipic acid / terephthalic acid / 1,4-butanediol condensation polymer (polybutylene adipate terephthalate (PBAT)), succinic acid / 1,4-butanediol / lactic acid condensation polymer, polybutylene succinate terephthalate (PBST), polybutylene succinate adipate (PBSA), polybutylene succinate (PBS), polybutylene sebacate terephthalate (PBSeT), polybutylene succinate adipate terephthalate (PBSAT), polycaprolactone (PCL), and polyglycolic acid; modified starch; casein plastic; and cellulose, and these can be used alone or in combination of two or more.
[0106] Among these, polylactic acid and polybutylene adipate terephthalate are preferred from the viewpoint of strength, and a mixture of polylactic acid and polybutylene adipate terephthalate is more preferred from the viewpoint of adhesiveness and strength.
[0107] Polylactic acid is an aliphatic polyester resin whose main component is a lactic acid structural unit, and is a polymer made from L-lactic acid, D-lactic acid, or its cyclic dimers, L-lactide, D-lactide, and DL-lactide.
[0108] The polylactic acid used in the biodegradable resin (C) layer is preferably a homopolymer of these lactic acids, but may contain copolymer components other than lactic acids in an amount that does not impair the properties, for example, 10 mol % or less.
[0109] Examples of such copolymerization components include aliphatic hydroxycarboxylic acids such as glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxyvaleric acid, 4-hydroxyvaleric acid, and 6-hydroxycaproic acid; lactones such as caprolactone; aliphatic diols such as ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, and 1,4-butanediol; and aliphatic dibasic acids such as succinic acid, oxalic acid, malonic acid, glutaric acid, and adipic acid.
[0110] The content ratio of L-lactic acid and D-lactic acid in polylactic acid (mass of L-lactic acid / mass of D-lactic acid) is preferably 95 / 5 or more, particularly 99 / 1 or more, and especially 99.8 / 0.2 or more. The larger this value is, the higher the melting point is and the better the heat resistance is, whereas the smaller this value is, the lower the melting point is and the more the heat resistance tends to be insufficient.
[0111] Specifically, in the case of a homopolymer of polylactic acid, the melting point of one with the above content ratio of 95 / 5 is approximately 152°C, that of one with the content ratio of 99 / 1 is approximately 171°C, and that of one with the content ratio of 99.8 / 0.2 is 175°C or higher.
[0112] The weight-average molecular weight of the polylactic acid is preferably 20,000 to 1,000,000, particularly preferably 30,000 to 300,000, and even more preferably 40,000 to 200,000. If the weight-average molecular weight is too large, the melt viscosity during hot melt molding tends to be too high, making it difficult to form a good film, whereas if the weight-average molecular weight is too small, the mechanical strength of the resulting laminate tends to be insufficient.
[0113] Such weight average molecular weight can be measured by size exclusion chromatography (GPC, gel permeation chromatography) as polystyrene equivalent according to the ISO 16014-1 and ISO 16014-3 standards using tetrahydrofuran as eluent and a column (polystyrene gel) heated to 40° C.
[0114] Examples of commercially available polylactic acid include "Ingeo" manufactured by NatureWorks, "Lacea" manufactured by Mitsui Chemicals, Inc., "REVODE" manufactured by Zhejiang Haizheng Biomaterials Co., Ltd., and "Vyloecol" manufactured by Toyobo Co., Ltd.
[0115] Polybutylene adipate terephthalate is obtained by condensation polymerization of adipic acid, terephthalic acid, and 1,4-butanediol.
[0116] The content of adipic acid in polybutylene adipate terephthalate is preferably from 10 to 50 mol %, more preferably from 15 to 40 mol %. The content of terephthalic acid in polybutylene adipate terephthalate is preferably from 5 to 45 mol %, more preferably from 8 to 35 mol %. The content of 1,4-butanediol in polybutylene adipate terephthalate is preferably from 5 to 45 mol %, and more preferably from 10 to 30 mol %. If the content of each component is too high or too low, the workability and corrosion resistance tend to decrease.
[0117] The weight average molecular weight of polybutylene adipate terephthalate is 3,000 to 1,000,000, preferably 20,000 to 600,000, and more preferably 50,000 to 400,000. If the weight average molecular weight is too small, production becomes difficult, whereas if the weight average molecular weight is too large, the melt viscosity increases and moldability tends to decrease.
[0118] The weight average molecular weight can be measured by the method described above.
[0119] Polybutylene adipate terephthalate may contain other copolymerization components in addition to adipic acid, terephthalic acid, and 1,4-butanediol.
[0120] Other copolymerization components include, for example, dihydroxy compounds such as diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, and polytetrahydrofuran (poly-THF); glycolic acid, D-lactic acid, L-lactic acid, D,L-lactic acid, 6-hydroxyhexanoic acid, and cyclic derivatives thereof such as glycolide (1,4-dioxane-2,5-dione), D-dilactide, and L-dilactide (3,6-dimethyl-1,4-dioxane-2,5-dione); and hydroxycarboxylic acids such as p-hydroxybenzoic acid and oligomers and polymers of p-hydroxybenzoic acid.
[0121] The content of such other copolymerization components is about 0.1 to 30 mol % based on the entire polybutylene adipate terephthalate.
[0122] When a mixture of polylactic acid and polybutylene adipate terephthalate is used, the mixing ratio of polylactic acid / polybutylene adipate terephthalate (mass ratio) is preferably 10 / 90 to 90 / 10, and more preferably 20 / 80 to 60 / 40.
[0123] In addition, the biodegradable resin (C) layer used in the present invention may contain, in addition to the biodegradable resin (C), a heat stabilizer, an antioxidant, an ultraviolet absorber, a crystal nucleating agent, an antistatic agent, a flame retardant, a plasticizer, a lubricant, a filler, a lubricant, a crystal nucleating agent, etc.
[0124] The laminate of the present invention preferably has 3 to 15 layers, more preferably 3 to 7 layers, and particularly preferably 5 to 7 layers.
[0125] The structure of the laminate of the present invention is not particularly limited, but when the adhesive (A) layer containing the acid-modified polyester resin composition of the present invention is a, the PVA resin (B) layer is b, and the biodegradable resin (C) layer is c, any combination such as c / a / b, c / a / b / a / c, c / b / a / b / a / b / c, etc. is possible. When there are multiple biodegradable resin (C) layers in the laminate, the multiple biodegradable resin (C) layers may be the same or different. The same applies when there are multiple PVA resin (B) layers and when there are multiple adhesive (A) layers in the laminate.
[0126] In order to prevent deterioration of the gas barrier performance due to moisture absorption by the PVA-based resin (B) layer, it is usually preferable to provide a layer structure in which a biodegradable resin (C) layer is provided in the PVA-based resin (B) layer in a portion that comes into contact with the outside air or a moisture-containing content.
[0127] The thickness of the laminate of the present invention is usually 1 to 30,000 μm, and is preferably in the range of particularly 3 to 13,000 μm, and particularly 10 to 3,000 μm.
[0128] As for the thickness of each layer constituting the laminate, the thickness of the biodegradable resin (C) layer is usually 0.4 to 14,000 μm, preferably 1 to 6,000 μm, and particularly preferably 4 to 1,400 μm. If the thickness of the biodegradable resin (C) layer is too thick, the laminate tends to be too hard, whereas if the thickness of the biodegradable resin (C) layer is too thin, the laminate tends to be brittle.
[0129] The thickness of the PVA resin (B) layer is usually 0.1 to 1,000 μm, preferably 0.3 to 500 μm, and particularly preferably 1 to 100 μm. If the PVA resin (B) layer is too thick, the laminate tends to be hard and brittle, whereas if the PVA resin (B) layer is too thin, the gas barrier properties tend to be poor.
[0130] The thickness of the adhesive (A) layer containing the acid-modified polyester resin composition of the present invention is usually 0.1 to 500 μm, preferably 0.15 to 250 μm, and particularly preferably 0.5 to 50 μm. If the adhesive (A) layer is too thick, the appearance may be poor, and conversely, if the adhesive (A) layer is too thin, the adhesive strength tends to be weak.
[0131] Furthermore, when there are a plurality of each layer, the ratio of the thickness of the biodegradable resin (C) layer to the thickness of the PVA-based resin (B) layer (thickness of biodegradable resin (C) layer / thickness of PVA-based resin (B) layer) is the ratio of the total thicknesses thereof and is usually 1 to 100, preferably 2.5 to 50. If this ratio is too large, the barrier property tends to be reduced, and if this ratio is too small, the laminate tends to be hard and brittle.
[0132] Furthermore, the thickness ratio of the laminate of the present invention and the adhesive (A) layer (adhesive layer) (thickness of adhesive (A) layer / thickness of the laminate of the present invention) is the ratio of the total thickness of the adhesive (A) layers when there are multiple adhesive (A) layers, and is usually 0.005 to 0.5, preferably 0.01 to 0.3. If this ratio is too large, the appearance tends to deteriorate, and if this ratio is too small, the adhesive strength tends to weaken.
[0133] The laminate of the present invention can be produced by a conventionally known molding method, specifically, a melt molding method or a molding method from a solution state can be used.
[0134] Examples of melt molding methods include a method in which an adhesive (A) containing the acid-modified polyester resin of the present invention and a PVA-based resin (B) are sequentially or simultaneously melt extrusion laminated to a film or sheet of a biodegradable resin (C); a method in which an adhesive (A) and a biodegradable resin (C) are sequentially or simultaneously melt extrusion laminated to a film or sheet of a PVA-based resin (B); and a method in which the biodegradable resin (C), adhesive (A) and PVA-based resin (B) are co-extruded.
[0135] As a molding method from a solution state, there can be mentioned a method in which a solution of the adhesive (A) dissolved in a good solvent is solution-coated onto a film or sheet of the biodegradable resin (C), and after drying, an aqueous solution of the PVA-based resin (B) is solution-coated.
[0136] Among them, the melt molding method is preferred, and the co-extrusion method is particularly preferred, since it can be produced in one step and can give a laminate with excellent interlayer adhesion. When using such a melt molding method, it is preferred to use a PVA resin having a 1,2-diol structural unit in the side chain as the PVA resin (B).
[0137] Specific examples of the co-extrusion method include the inflation method, the T-die method, the multi-manifold die method, the feed block method, and the multi-slot die method. The shape of the die that can be used may be a T-die, a round die, or the like. The melt molding temperature during melt extrusion is usually 140 to 250°C, and preferably in the range of 160 to 230°C.
[0138] The laminate of the present invention may be further subjected to a heat stretching treatment, and such a stretching treatment is expected to improve the strength and gas barrier properties.
[0139] For the stretching treatment, a known stretching method can be used. Specific examples of such methods include uniaxial stretching and biaxial stretching, in which both edges of a multilayer structure sheet are gripped and expanded; die forming methods such as deep drawing, vacuum forming, pressure forming, and vacuum pressure forming, in which a multilayer structure sheet is stretched using a die; and methods in which a preformed multilayer structure such as a parison is processed using a tubular stretching method, stretch blow method, etc.
[0140] As such a stretching method, when a film or sheet-like molded product is intended, it is preferable to employ a uniaxial stretching method or a biaxial stretching method.
[0141] In the case of a die forming method such as deep drawing, vacuum forming, pressure forming, or vacuum pressure forming, it is preferable to uniformly heat the laminate using a hot air oven, a heater type oven, or a combination of both, and stretch the laminate using a chuck, a plug, vacuum force, compressed air force, or the like.
[0142] When the object is to produce a molded product such as a cup or a tray having a drawing ratio (depth of molded product (mm) / maximum diameter of molded product (mm)) of usually 0.1 to 3, it is preferable to adopt a mold molding method in which a mold is used for stretching processing, such as a deep drawing method, a vacuum forming method, a pressure forming method, or a vacuum pressure forming method.
[0143] The laminate of the present invention thus obtained has strong adhesive strength between any of the layers, for example, between the biodegradable resin (C) layer and the adhesive (A) layer, and between the PVA resin (B) layer and the adhesive (A) layer.
[0144] In addition, at least the biodegradable resin (C) and the PVA-based resin (B) are both biodegradable, and the laminate of the present invention is also excellent in biodegradability. From this viewpoint, it is also preferable that the acid-modified polyester-based resin composition contained in the adhesive (A) is biodegradable.
[0145] Since the laminate of the present invention is biodegradable, it is suitable for use in products that can be disposed of directly in compost, such as coffee capsules (coffee bean containers for capsule-type coffee makers), shrink films, and other food and beverage containers.
[0146] Furthermore, when the laminate of the present invention has a PVA-based resin (B) layer, the PVA-based resin (B) layer can be removed by dissolving it in water, and only the remaining water-insoluble resin can be recycled. EXAMPLES
[0147] The present invention will be described below with reference to examples. However, the present invention is not limited to the description of the examples as long as it does not depart from the gist of the present invention. In the examples, "parts" and "%" are based on mass.
[0148] The raw material resins and additives used in each example are as follows: <Raw material resin> (A) Polybutylene adipate terephthalate (PBAT): BASF Ecoflex C1200 (B) Polybutylene succinate terephthalate (PBST): polyester copolymer produced in Production Example 1 below <Additives> (a) Glycerol fatty acid ester: "Triacetin" manufactured by Tokyo Chemical Industry Co., Ltd. (number of carbon atoms of fatty acid: 2) (b) Glycerin fatty acid ester: "Tributyrin" manufactured by Tokyo Chemical Industry Co., Ltd. (number of carbon atoms of fatty acid: 5) (c) Sugar ester: "S-070" manufactured by Mitsubishi Chemical Corporation (number of fatty acid carbon atoms: 18) (d) Fatty acid amide: NOF Corp. "Alflow H-50F-P"
[0149] (Production Example 1: Production of Polybutylene Succinate Terephthalate (PBST)) [Preparation of polycondensation catalyst] 343.5 parts by mass of magnesium acetate tetrahydrate was placed in a reactor equipped with a stirrer, and 1434 parts by mass of anhydrous ethanol (purity 99% by mass or more) was added. 218.3 parts by mass of ethyl acid phosphate (mixture mass ratio of monoester and diester is 45:55) was added and stirred at 23°C. After confirming that magnesium acetate was completely dissolved, 410.0 parts by mass of tetra-n-butyl titanate was added. Stirring was continued for another 10 minutes to obtain a homogeneous mixed solution. This mixed solution was concentrated under reduced pressure while controlling the temperature at 60°C or less. Approximately half of the amount of ethanol added was distilled off, leaving a translucent viscous liquid. 1108 parts by mass of 1,4-butanediol was added thereto, and further concentration was performed under reduced pressure while controlling the temperature at 80°C or less to obtain a catalyst solution with a titanium atom content of 3.5% by mass.
[0150] [Polymerization of polybutylene succinate terephthalate (PBST)] In a reaction vessel equipped with a stirrer, a nitrogen inlet, a heater, a thermometer and a pressure reducing port, 33.6 parts by mass of succinic acid, 38.6 parts by mass of terephthalic acid, 69.7 parts by mass of 1,4-butanediol, 0.138 parts by mass of trimethylolpropane (0.200 mol% relative to 100 mol% of the total of succinic acid and terephthalic acid), 0.10 parts by mass of polyethylene wax (Honeywell's "ACumistB6", melting point: 124°C), and 0.0017 parts by mass of sodium hydroxide (NaOH) were charged as raw materials, and tetra-n-butyl titanate was added so that the titanium atom amount was 30 ppm by mass per polyester resin obtained. Nitrogen gas was introduced into the vessel while stirring the contents of the vessel, and the system was placed under a nitrogen atmosphere by vacuum replacement. Next, the temperature of the system was raised from 160°C to 230°C over 1 hour while stirring, and the reaction was carried out at this temperature for 3 hours. The terminal acid value of the resulting ester oligomer was measured and found to be 90 eq. / ton. To this ester oligomer, the catalyst solution was added in an amount to give 70 ppm by mass of titanium atom per polyester resin obtained, and the temperature was raised to 250° C. over 45 minutes. At the same time, 0.07×10 3The pressure was reduced to below 1 Pa, and polycondensation was continued while maintaining the heated and reduced pressure state. When a predetermined viscosity was reached, the polymerization was terminated to obtain polybutylene succinate terephthalate (PBST). The obtained PBST had an MFR of 4.5 g / 10 min. The MFR was measured at 190°C and a load of 2.16 kg according to JIS K7210 (2014).
[0151] Example 1 [Preparation of Acid-Modified Polyester Resin Composition] As the raw polyester resin, 100 parts of (A) PBAT, 0.05 parts of maleic anhydride, and 0.08 parts of 2,5-dimethyl-2,5-bis(t-butyloxy)hexane ("Trigonox 101-50D-PD" manufactured by Kayaku Nouryon Co., Ltd.) as a radical initiator were dry-blended. As an additive, (a) glycerin fatty acid ester was added to this mixture in an amount of 1 mass% relative to the total mass, and the mixture was melt-kneaded in a twin-screw extruder under the following conditions, extruded into a strand shape, cooled with water, and cut with a pelletizer to obtain a cylindrical pellet of an acid-modified polyester resin composition.
[0152] Twin Screw Extruder Diameter (D): 15mm L / D:60 Screw rotation speed: 200 rpm Mesh: 60 / 90 / 60mesh Processing temperature: 160℃
[0153] (Example 2, Comparative Examples 1 to 4) Except for changing the resin composition to that shown in Table 1, the same procedure as in Example 1 was carried out to obtain an acid-modified polyester resin composition.
[0154] (Examples 3 to 16, Comparative Examples 5 to 10) An acid-modified polyester resin composition was obtained in the same manner as in Example 1, except that the resin composition was as shown in Table 2.
[0155] For each of the acid-modified polyester resin compositions obtained in Examples 1 to 16 and Comparative Examples 1 to 10, the strand stability during granulation was evaluated, and the adhesive strength was measured and a peel test was carried out. The results are shown in Tables 1 and 2.
[0156] [Evaluation of strand stability during granulation] The behavior of the strands discharged from the die during granulation was observed. <Evaluation criteria> A: The strands are stable. B: The strands are surging a little. C: The strands are surging significantly.
[0157] [Laminated body production] Using polybutylene succinate (C1) ("BioPBS" manufactured by Mitsubishi Chemical Corporation), PVA resin (B) ("Nichigo G-Polymer" manufactured by Mitsubishi Chemical Corporation), and acid-modified polyester resin composition (A), a three-kind, five-layer laminate of polybutylene succinate (C1) layer / acid-modified polyester resin composition (A) layer / PVA resin (B) layer / acid-modified polyester resin composition (A) layer / polybutylene succinate (C1) layer was produced in a three-kind, five-layer multilayer inflation film production apparatus equipped with five extruders. The thickness of the obtained laminate was 100 μm, and the thicknesses of the layers were 30 μm / 10 μm / 20 μm / 10 μm / 30 μm.
[0158] The set temperatures of each extruder and roll were as follows (C1 to C3: cylinders, H: head, J: joint, D1 to 5: dies). Polylactic acid (C1): C1 / C2 / H / J=140 / 160 / 160 / 160℃ PVA resin (B): C1 / C2 / C3 / H / J=170 / 180 / 190 / 180 / 170℃ Acid-modified polyester resin composition (A): C1 / C2 / C3 / H / J=180 / 200 / 210 / 200 / 190°C Dice: D1 / D2 / D3 / D4 / D5=190 / 190 / 190 / 190 / 190℃ Cooling method: air cooling
[0159] [Adhesion evaluation] The adhesive strength of the obtained laminate was evaluated based on the following criteria. The laminate was cut into a rectangular shape with a width of 15 mm, and the adhesive strength at the interface between the layers was measured using a 50 N load cell of a tensile tester "AGS-X" (manufactured by Shimadzu Corporation). The test speed was set at 100 mm / min, and the average value of five tests was taken as the adhesive strength value. The measurement was performed in an environment of 23°C / 50% RH. From the viewpoint of practicality, the adhesive strength is preferably 3 [N / 15 mm] or more. Here, adhesive strength of 3 [N / 15 mm] or more was evaluated as high adhesive strength, and adhesive strength of less than 3 [N / 15 mm] was evaluated as low adhesive strength.
[0160] In the above measurements, peelability (zipping) was evaluated based on the following criteria: Zipping refers to a phenomenon in which the adhesive strength value is not stable and fluctuates. <Evaluation criteria> A: No zipping occurs within 30 mm after the peel strength stabilizes B: Zipping occurs within 30 mm after the peel strength stabilizes
[0161] Based on the above criteria, a sample having a high adhesive strength of 3 [N / 15 mm] or more and free of zipping was rated as having excellent adhesiveness.
[0162] Furthermore, for Examples 1 to 5, 7, and 11 to 16, and Comparative Examples 1 to 6, and 9 to 10, the acid values of the acid-modified polyester resins were measured by the above-mentioned acid value measuring method, and the results are shown in Tables 1 and 2. Tetrahydrofuran was used as the solvent.
[0163] [Table 1]
[0164] [Table 2]
[0165] Each example in Table 1 uses PBAT as the raw resin, and each example in Table 2 uses PBST as the raw resin. It was found that all of Examples 1 to 16 using acid-modified polyester resin compositions containing fatty acid esters had high adhesive strength and did not cause zipping, i.e., excellent adhesive strength, and the strands during granulation were stable. On the other hand, Comparative Examples 1 to 10 using acid-modified polyester resin compositions containing no fatty acid esters or containing aliphatic amides (used as lubricants in molding) showed poor performance in either case, and none of them showed sufficient effects in all evaluation items. It is presumed that the reason for the low adhesive strength in Comparative Examples 2, 4, 6, and 10 using acid-modified polyester resin compositions containing fatty acid amides is the low compatibility between the fatty acid amides and the acid-modified polyester resins.
Claims
1. An acid-modified polyester resin composition comprising an acid-modified polyester resin as a main component and also containing a fatty acid ester.
2. 2. The acid-modified polyester resin composition according to claim 1, wherein the fatty acid ester is a fatty acid ester composed of a polyhydric alcohol and a fatty acid having 1 to 18 carbon atoms.
3. 2. The acid-modified polyester resin composition according to claim 1, wherein the content of the fatty acid ester is 0.01 to 20% by mass.
4. The acid-modified polyester resin composition according to claim 1 , wherein the acid-modified polyester resin is biodegradable.
5. An adhesive comprising the acid-modified polyester resin composition according to any one of claims 1 to 4.
6. A laminate having at least one layer containing the acid-modified polyester resin composition according to any one of claims 1 to 4.
7. A laminate having an adhesive layer between a first layer and a second layer, At least one of the first layer and the second layer is a polyvinyl alcohol-based resin layer, A laminate comprising the acid-modified polyester resin composition according to any one of claims 1 to 4, wherein the adhesive layer comprises:
Citation Information