Decorative material and method for producing decorative material

A triaxial fabric-based decorative material cured with resin and optionally combined with a base material and pattern layer addresses the inflexibility and weight issues of existing materials, offering enhanced workability and design flexibility.

JP2024139774APending Publication Date: 2024-10-09TOPPAN HOLDINGS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024050041
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-26
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing decorative materials such as punched metal, louvers, and triaxial fabric-based materials are heavy, inflexible, and have poor workability, making them difficult to handle and manipulate.

Method used

A decorative material comprising a triaxial fabric cured with a curable resin, optionally with a base material and adhesive layer, and a pattern layer provided on the fabric or resin, which can be manufactured using methods like inkjet printing to enhance workability and design.

Benefits of technology

The solution results in a lightweight, flexible decorative material with improved workability and design capabilities, allowing for controlled light transmittance and aesthetic versatility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139774000001_ABST
    Figure 2024139774000001_ABST
Patent Text Reader

Abstract

To provide a decorative material capable of improving installability while aiming weight saving and a method for producing the decorative material.SOLUTION: A decorative material 10 comprises a surface material 20 having a triaxial fabric 21, and the triaxial fabric 21 is hardened by a curable resin 22. The decorative material 10 further comprises a substrate 4 which is a porous fiber assembly, and an adhesive layer 3 disposed between the substrate 4 and the surface material 20, and the basis weight of the substrate 4 is 150 g / m2 or less. A producing method for the decorative material 10 comprising the surface material 20 having the triaxial fabric 21 includes hardening the triaxial fabric 21 with the curable resin 22 to produce the surface material 20. The producing method for the decorative material 10 further comprises bonding the surface material 20 to the substrate 4 which is a porous fiber assembly, and setting the basis weight of the substrate 4 to 150 g / m2 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative material and a method for manufacturing a decorative material. [Background technology]

[0002] Widely used decorative materials that transmit light include punched metal, which is a metal plate with holes drilled into it, and louver materials, which are long, thin slats made of wood, metal, or glass arranged in parallel with gaps between them.

[0003] Furthermore, membrane materials using triaxial woven fabrics as surface materials as described in Patent Document 1 have been proposed recently as decorative light-transmitting materials to replace heavy materials such as metal, wood, and glass. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-146622 Summary of the Invention [Problem to be solved by the invention]

[0005] The punched metal and louver materials described above are heavy and inflexible, making them difficult to install and handle.

[0006] In addition, the stiffness of the membrane material described in Patent Document 1 varies greatly depending on the material and weaving structure of the triaxial fabric, so it cannot be said that the workability is necessarily sufficient.

[0007] In view of the above, an object of the present invention is to provide a decorative material and a manufacturing method thereof that can improve workability while reducing the weight. [Means for solving the problem]

[0008] [1] The decorative material according to the present invention comprises a surface material having a triaxial fabric, the triaxial fabric being hardened by a hardenable resin.

[0009] [2] In the decorative material described in [1], the curable resin may cover the surface of the triaxial fabric.

[0010] [3] The decorative material according to [1] or [2], further comprising a substrate which is a porous fiber assembly, and an adhesive layer disposed between the surface material and the substrate, wherein the substrate has a basis weight of 150 g / m 2 It may be the following.

[0011] [4] In the decorative material described in [3], the substrate may be made of a glass fiber nonwoven fabric.

[0012] [5] The decorative material according to any one of [1] to [4] may further comprise a pattern layer provided on the triaxial fabric, and the pattern layer may be provided three-dimensionally in the thickness direction of the triaxial fabric.

[0013] [6] In the decorative material described in [5], the design layer may have a cured UV ink.

[0014] [7] In the decorative material described in [5] or [6], the triaxial fabric has a first thread extending in a first direction, a second thread extending in a second direction intersecting the first direction, and a third thread extending in a third direction intersecting the first and second directions, and the pattern layer is provided on the first thread, the second thread, and the third thread, and when viewed in the thickness direction of the triaxial fabric, the pattern layer provided on the first thread, the pattern layer provided on the second thread, and the pattern layer provided on the third thread may be continuous.

[0015] [8] The method for producing a decorative material according to the present disclosure is a method for producing a decorative material having a surface material with a triaxial fabric, in which the triaxial fabric is hardened with a curable resin to produce the surface material.

[0016] [9] In the method for producing a decorative material according to [8], a surface material is bonded to a substrate which is a porous fiber aggregate, and the basis weight of the substrate is 150 g / m2 The following may also be used.

[0017]

[10] In the method for producing a decorative material described in [8] or [9], a pattern layer may be provided on the triaxial woven fabric.

[0018]

[11] In the method for producing a decorative material according to

[10] , a pattern layer may be provided on the surface of the curable resin.

[0019]

[12] In the method for producing a decorative material according to

[10] or

[11] , a pattern layer may be provided on the surface of the triaxial woven fabric.

[0020]

[13] In the method for producing a decorative material according to any one of [8] to

[12] , the pattern layer may be provided by inkjet printing.

[0021]

[14] In the method for producing a decorative material described in

[13] , after inkjet printing is performed using a UV ink, the UV ink may be cured by exposure to ultraviolet light to provide a design layer. Effect of the Invention

[0022] According to the present invention, it is possible to provide a decorative material that can improve workability while reducing the weight, and a method for manufacturing a decorative material. [Brief description of the drawings]

[0023] [Figure 1] 1 is a schematic cross-sectional view of a decorative material according to one embodiment of the present disclosure. [Diagram 2] FIG. 1 is a schematic plan view of a triaxial woven fabric of the present disclosure. [Diagram 3] FIG. 2 is a schematic cross-sectional view of a decorative material according to another embodiment of the present disclosure. [Figure 4] FIG. 2 is a schematic cross-sectional view of a decorative material according to another embodiment of the present disclosure. [Diagram 5] FIG. 2 is a schematic cross-sectional view of the decorative material according to the embodiment of FIG. 1, in which a pattern layer is provided. [Figure 6]FIG. 5 is a schematic cross-sectional view of the decorative material according to the embodiment of FIG. 4, in which a pattern layer is provided. [Figure 7] FIG. 2 is a schematic cross-sectional view of the decorative material according to the embodiment of FIG. 1, where a pattern layer is provided on the decorative material. [Figure 8] FIG. 2 is a schematic cross-sectional view of the decorative material according to the embodiment of FIG. 1, where a pattern layer is provided on the decorative material. [Figure 9] FIG. 2 is a schematic cross-sectional view of the decorative material according to the embodiment of FIG. 1, where a pattern layer is provided on the decorative material. [Figure 10] FIG. 6 is a schematic cross-sectional view of the decorative material according to the embodiment of FIG. 5, in which a pattern layer is provided. [Figure 11] FIG. 9 is a schematic cross-sectional view of the decorative material according to the embodiment of FIG. 8, in which a pattern layer is provided on the decorative material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Here, the drawings are schematic, and the relationship between thickness and planar dimensions, the ratio of thicknesses of each layer, and the like differ from the actual ones. In addition, the embodiments shown below are examples of configurations for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention is not limited to the materials, shapes, structures, and the like of the components described below. The technical idea of ​​the present invention can be modified in various ways within the technical scope defined by the claims described in the claims.

[0025] A decorative material 10 according to an embodiment of the present invention will now be described. Fig. 1 is a cross-sectional view illustrating the layered structure of the decorative material 10.

[0026] As shown in FIG. 1, the decorative material 10 includes a surface material 20 , an adhesive layer 3 , and a substrate 4 .

[0027] The surface material 20 is composed of a triaxial fabric 21 and a curable resin 22. The triaxial fabric 21 is cured by the curable resin 22. In other words, the surface material 20 is produced by curing the triaxial fabric 21 by the curable resin 22. This allows for a reduction in weight and provides appropriate rigidity.

[0028] Fig. 2 is a schematic plan view of the triaxial fabric 21. As shown in Fig. 2, the triaxial fabric 21 has a plurality of first threads 21a extending in a first direction D1, a plurality of second threads 21b extending in a second direction D2 intersecting the first direction D1, and a plurality of third threads 21c extending in a third direction D3 intersecting the first direction D1 and the second direction D2. The triaxial fabric 21 is configured by interweaving the plurality of first threads 21a, the plurality of second threads 21b, and the plurality of third threads 21c with each other.

[0029] The fibers constituting the triaxial fabric 21 are preferably made of a non-combustible material. Examples of fibers made of a non-combustible material include glass fibers, carbon fibers, and metal fibers. When fibers made of a non-combustible material are used, they can be used in places where non-combustibility is required. They can also be made weather resistant.

[0030] The triaxial fabric 21 is hardened by a hardening resin 22. The hardening resin 22 is provided for the purposes of hardening the triaxial fabric 21 and protecting the surface thereof.

[0031] The curable resin 22 coats the surface of the triaxial fabric 21. Here, coating may refer to either a state in which the resin does not permeate the triaxial fabric 21 and covers only the surface, or a state in which the resin permeates the triaxial fabric and coats its surface.

[0032] As the curable resin 22, polyethylene, polypropylene, silicone-based curable resin, fluorine-based curable resin, acrylic-based curable resin, polyvinyl chloride-based curable resin, polycarbonate-based resin, etc. can be used. In particular, when silicone-based curable resin, fluorine-based curable resin, acrylic-based curable resin, polyvinyl chloride-based curable resin, or polycarbonate-based resin is used, weather resistance is higher. Weather resistance agents such as ultraviolet absorbers (UVA) and light stabilizers (HALS) may be added.

[0033] When a resin with high transparency is used as the hardening resin 22, the designability is particularly improved.

[0034] When a weather-resistant non-flammable material is used as the fiber constituting the triaxial fabric 21 and a weather-resistant hardening resin is applied to the surface, the fabric can be suitably used particularly for exterior applications.

[0035] The adhesive layer 3 is disposed between the surface material 20 and the base material 4, and bonds the surface material 20 to the base material 4. In other words, the adhesive layer 3 is disposed between the surface material 20 and the base material 4 by bonding the surface material 20 to the base material 4 with an adhesive. The adhesive constituting the adhesive layer 3 is preferably a 100% solids hot melt (EVA-based, polyamide-based, etc.) or PUR (moisture curing type), or a high viscosity rubber-based or urethane curing resin-based adhesive.

[0036] The base material 4 may be a porous fiber aggregate made of fibers such as paper, nonwoven fabric, woven fabric, etc. The base material 4 may be, for example, a glass fiber nonwoven fabric.

[0037] The basis weight of the substrate 4 is 150 g / m 2 For the substrate 4, the basis weight can be 150 g / m 2 The total light transmittance of the decorative material 1 should be set to 40% or more within the following range: The basis weight of the base material is 151 g / m 2 If the total light transmittance of the decorative material falls below 39% as described above, the product will be less flexible and will be less workable. 2 That is, the decorative material 10 may be in a state where no substrate is attached (the decorative material does not have a substrate). In this case, the total light transmittance of the decorative material 10 can be set to 100%.

[0038] Here, in conventional decorative materials using punched metal or louver material, light is blocked in areas where components are present, resulting in a light transmittance of 0%, creating shadows. On the other hand, in areas where no components are present, such as holes in punched metal or between components of louver material, light penetrates without being blocked, resulting in a light transmittance of 100%. For this reason, when using these decorative materials, it is difficult to appropriately control the light transmittance to a value in the range greater than 0% and less than 100%.

[0039] In addition, in the membrane material described in Patent Document 1, the light transmittance can be changed by changing the area ratio of the void spaces in the triaxial fabric. However, changing the area ratio of the void spaces in the triaxial fabric requires significant changes to the manufacturing method and conditions, which is not easy.

[0040] In contrast, in this embodiment, the basis weight of the base material 4 is 150 g / m 2 By adjusting the light transmittance within the following range, it is possible to adjust the light transmittance without significantly changing the manufacturing method or conditions.

[0041] 4, a curable resin 4' can be provided on the surface of the base material 4. As with the curable resin 22, the curable resin 4' may be in either a state in which the resin does not permeate the base material 4 and covers only the surface, or a state in which the resin permeates the base material 4 and covers the surface.

[0042] As the curable resin 4', polyethylene, polypropylene, silicone-based curable resin, fluorine-based curable resin, acrylic-based curable resin, polyvinyl chloride-based curable resin, polycarbonate-based, etc. can be used, as in the curable resin 22. In particular, when a silicone-based curable resin, a fluorine-based curable resin, an acrylic-based curable resin, a polyvinyl chloride-based curable resin, or a polycarbonate-based resin is used, weather resistance is higher. Weather resistance agents such as ultraviolet absorbers (UVA) and light stabilizers (HALS) may be added. In addition, from the viewpoint of design, a curable resin with high transparency is preferably used.

[0043] When the curable resin 4' is provided on the surface of the base material 4, the surface of the base material 4 is protected, and therefore durability and weather resistance are improved.

[0044] As shown in FIGS. 5 to 9, a pattern layer 23 may be provided on the triaxial woven fabric 21.

[0045] In decorative material 13 shown in Figure 5, decorative material 14 shown in Figure 6, and decorative material 15 shown in Figure 7, a pattern layer 23 is provided on the surface of triaxial fabric 21, thereby providing a pattern layer 23 on triaxial fabric 21.

[0046] In the decorative material 13 shown in Figure 5, a pattern layer 23 is provided on a side of the triaxial fabric 21 constituting the surface material 20 in Figure 1, other than the side on which the adhesive layer 3 is provided, and then a curable resin 22 is provided over the entire surface of the laminate consisting of the triaxial fabric 21 and the pattern layer 23, thereby providing the pattern layer 23 on the surface of the triaxial fabric 21.

[0047] In the decorative material 14 shown in Figure 6, a pattern layer 23 is provided on a side of the triaxial fabric 21 constituting the surface material 20 in Figure 4, other than the side on which the adhesive layer 3 is provided, and then a curable resin 22 is provided over the entire surface of the laminate consisting of the triaxial fabric 21 and the pattern layer 23, thereby providing the pattern layer 23 on the surface of the triaxial fabric 21.

[0048] In the decorative material 15 shown in Figure 7, a pattern layer 23 is provided on the front and back surfaces of the triaxial fabric 21 constituting the surface material 20 in Figure 1, and then a curable resin 22 is provided over the entire surface of the laminate consisting of the triaxial fabric 21 and the pattern layers 23 provided on the front and back surfaces of the triaxial fabric 21, thereby providing the pattern layer 23 on the surface of the triaxial fabric 21.

[0049] When providing the pattern layer 23 on the front and back surfaces of the triaxial woven fabric 21, the pattern layer 23 may be of the same color and pattern on the front and back surfaces of the triaxial woven fabric 21, or the pattern layer 23 of different hues or patterns may be provided on the front and back surfaces of the triaxial woven fabric 21. Also, the pattern layer 23 may be black on one side of the triaxial woven fabric 21. By providing the pattern layer 23 of the same color and pattern on the front and back surfaces of the triaxial woven fabric 21, it is possible to prevent a sense of incongruity from being created when the triaxial woven fabric 21 is bent or rolled and placed in an interior space. By providing the pattern layer 23 of different hues or patterns on the front and back surfaces of the triaxial woven fabric 21, it is possible to reproduce spaces with different atmospheres when the triaxial woven fabric 21 is used as an interior decoration material that divides one space into two. By providing the pattern layer 23 of black on one side of the triaxial woven fabric 21, it is possible to use the triaxial woven fabric 21 as an interior decoration material that does not reflect the color and pattern on the wall surface.

[0050] In the decorative material 16 shown in Fig. 8 and the decorative material 17 shown in Fig. 9, the pattern layer 23 is provided on the surface of the curable resin 22, thereby providing the pattern layer 23 on the triaxial fabric 21. The fibers that make up the triaxial fabric 21 may be fibers to which ink does not easily adhere, such as glass fibers. In such cases, providing the pattern layer 23 on the surface of the curable resin 22 improves the fixation of the pattern layer 23.

[0051] In the decorative material 16 shown in Figure 8, a pattern layer 23 is provided on the surface of the curable resin 22 by providing a pattern layer 23 on a surface of the curable resin 22 constituting the surface material 20 in Figure 1, different from the surface on which the adhesive layer 3 is provided.

[0052] In the decorative material 17 shown in FIG. 9, a pattern layer 23 is provided on the front and back surfaces of the hardening resin 22 constituting the surface material 20 in FIG.

[0053] When the pattern layer 23 is provided on the surface of the hardening resin 22, the pattern layer 23 may be of the same color and pattern on the front and back sides of the hardening resin 22, or the pattern layer 23 of different hues or patterns may be provided on the front and back sides of the hardening resin 22. Also, a black pattern layer 23 may be provided on one side of the hardening resin 22. By providing the pattern layer 23 of the same color and pattern on the front and back sides of the hardening resin 22, it is possible to prevent a sense of incongruity from being created when the hardening resin 22 is bent or rolled and placed in an interior space. By providing the pattern layer 23 of different hues or patterns on the front and back sides of the hardening resin 22, it is possible to reproduce spaces with different atmospheres when the hardening resin 22 is used as an interior decoration material that divides one space into two. By providing the black pattern layer 23 on one side of the hardening resin 22, it is possible to use the hardening resin 22 as an interior decoration material that does not reflect the color and pattern on the wall surface.

[0054] Furthermore, as shown in FIGS. 10 and 11, a design layer 23 may be provided on the substrate 4. As shown in FIG.

[0055] In the decorative material 18 shown in FIG. 10, a pattern layer 23 is provided on the base material 4 by providing the pattern layer 23 on a surface of the base material 4 in FIG. 5 that is different from the surface on which the adhesive layer 3 is provided.

[0056] In the decorative material 19 shown in FIG. 11, a pattern layer 23 is provided on the base material 4 by providing the pattern layer 23 on a surface of the base material 4 in FIG. 8 that is different from the surface on which the adhesive layer 3 is provided.

[0057] The pattern layer 23 is provided on the triaxial fabric 21, and is three-dimensionally provided in the thickness direction of the triaxial fabric 21 (direction perpendicular to the paper surface of Figure 2) so as to follow the weaving structure of the triaxial fabric 21.

[0058] When a pattern layer 23 is provided on the triaxial fabric 21, the design of the triaxial fabric 21 is improved, making it possible to provide a decorative material with a particularly high design quality.

[0059] The ink constituting the design layer 23 may be an organic pigment ink or an inorganic pigment ink.

[0060] As the organic pigment, azo pigments, phthalocyanine pigments, anthraquinone pigments, quinacridone pigments, isoindolinone pigments, quinophthalone pigments, dye lake pigments, fluorescent pigments, etc. can be used.

[0061] As the inorganic pigment, natural mineral pigments and rigid inorganic pigments can be used, such as titanium oxide, zinc white, zinc sulfide, calcium carbonate, talc, black iron oxide, cadmium red, red iron oxide, titanium yellow, yellow iron oxide, cobalt green, viridian, cobalt blue, ultramarine, Prussian blue, manganese violet, and the like.

[0062] The design layer 23 can be formed by selecting from known printing methods such as gravure printing, inkjet printing, and screen printing.

[0063] The pattern layer 23 can also be formed by known coating methods such as brush coating, roller brush coating, spatula coating, air spray coating, airless spray coating, dip coating, electrostatic coating, electrodeposition coating, powder coating, curtain flow coater coating, and roller coater coating.

[0064] When the pattern layer 23 is provided by inkjet printing, a UV ink can be used. The UV ink contains, for example, a photopolymerization initiator and a low molecular weight monomer component for annual adjustment, and the pattern layer 23 also contains these components. In inkjet printing using UV ink, after inkjet printing is performed using the UV ink, the UV ink is cured by irradiating it with ultraviolet light. In this way, the pattern layer 23 having the cured UV ink is provided on the triaxial fabric 21.

[0065] For example, an inkjet printer is used to apply UV ink to the fiber parts of the triaxial fabric 21 other than the voids, and the UV ink is cured by irradiating it with ultraviolet light before it drips to the other side of the fiber. This makes it possible to prevent the UV ink from penetrating into the glass nonwoven fabric, allowing for vivid reproduction of patterns and colors.

[0066] In addition, for example, a UV inkjet printer is used to apply UV ink to the fiber parts other than the void parts of the triaxial fabric 21, and the UV ink is subsequently cured by UV irradiation. This makes it possible to prevent the UV ink from dripping onto the surface on which the pattern layer 23 is already formed, and also to prevent the UV ink from seeping into the base material 4, so that clear patterns and colors can be reproduced.

[0067] The pattern layer 23 is provided on the first thread 21a, the second thread 21b, and the third thread 21c. The pattern layer 23 provided on the first thread 21a is referred to as the pattern layer 23a, the pattern layer 23 provided on the second thread 21b is referred to as the pattern layer 23b, and the pattern layer 23 provided on the third thread 21c is referred to as the pattern layer 23c.

[0068] When the pattern layer 23 is formed by gravure printing and screen printing, the first thread 21a, the second thread 21b, and the third thread 21c are woven with each other, so that when viewed in the thickness direction of the triaxial fabric 21, the pattern layer 23a, the pattern layer 23b, and the pattern layer 23 are spaced apart from each other at the locations where the first thread 21a, the second thread 21b, and the third thread 21c are woven with each other.

[0069] In contrast, when the pattern layer 23 is provided by inkjet printing, ink droplets are ejected in the thickness direction of the triaxial fabric 21. Therefore, when viewed in the thickness direction of the triaxial fabric 21, the pattern layer 23a, the pattern layer 23b, and the pattern layer 23 are continuous with each other or closer than in gravure printing and screen printing, even in the areas where the first thread 21a, the second thread 21b, and the third thread 21c are woven together. This further improves the design. EXAMPLES

[0070] The following examples illustrate specific embodiments of the present disclosure, but the present invention is not limited thereto.

[0071] (Example 1-1)

[0072] The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2 A triaxial woven fabric with a porosity of 33% was produced. This triaxial woven fabric was impregnated with a silicone-based hardening resin and hardened by air drying to produce the decorative material of Example 1-1, which is made of only a surface material without a substrate (see FIG. 3).

[0073] (Example 1-2) The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2 A triaxial fabric with a porosity of 33% was produced. The triaxial fabric was impregnated with a silicone-based hardening resin and hardened by air drying to produce a surface material (see Figure 1).

[0074] Next, the basis weight is 30 g / m 2 The glass fiber nonwoven fabric was impregnated with a silicone-based hardening resin and then air-dried to harden the resin, thereby preparing a substrate.

[0075] Finally, a polyamide-based hot melt was sandwiched between the surface material and the substrate, and the surface material and substrate were bonded together by heating at 120° C. for 60 seconds to produce the decorative material of Example 1-2 (see FIG. 4).

[0076] (Examples 1-3) The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 40 g / m 2 A decorative material of Example 1-3 was produced in the same manner as in Example 1-2, except for the above (see FIG. 4).

[0077] (Examples 1 to 4) The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 50 g / m 2 A decorative material of Example 1-4 was produced in the same manner as in Example 1-2, except for the above (see FIG. 4).

[0078] (Examples 1 to 5) The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 80 g / m 2 A decorative material of Example 1-5 was produced in the same manner as in Example 1-2, except for the above (see FIG. 4).

[0079] (Examples 1 to 6) The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 150 g / m 2 A decorative material of Example 1-6 was produced in the same manner as in Example 1-2, except for the above (see FIG. 4).

[0080] (Examples 1 to 7) The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 151 g / m 2 Except for the above, a decorative material was produced in the same manner as in Example 1-2 (see FIG. 4).

[0081] (Example 2-1) The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2 A triaxial woven fabric having a porosity of 33% was produced. A pattern layer was formed on one side of this triaxial woven fabric by printing inorganic pigment ink using an inkjet method, and then the fabric was impregnated with a silicone-based curable resin and cured by air drying to form the decorative material of Example 2-1, which is made of only a surface material without a substrate.

[0082] (Example 2-2) The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2 A triaxial fabric with a porosity of 33% was produced. A pattern layer was created on one side of this triaxial fabric by printing inorganic pigment ink using the inkjet method, and then the fabric was impregnated with a silicone-based curable resin and cured by air drying to produce a surface material.

[0083] Next, the basis weight is 30 g / m 2 The glass fiber nonwoven fabric was impregnated with a silicone-based hardening resin and then air-dried to harden the resin, thereby preparing a substrate.

[0084] Finally, a polyamide-based hot melt was sandwiched between the surface of the surface material other than the surface on which the pattern layer was formed and the substrate, and the surface material and substrate were bonded together by heating at 120°C for 60 seconds to produce the decorative material of Example 2-2 (see Figure 6).

[0085] (Example 2-3) The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 40 g / m 2 A decorative material of Example 2-3 was produced in the same manner as in Example 2-2, except for the above (see FIG. 6).

[0086] (Examples 2-4) The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 50 g / m 2 A decorative material of Example 2-4 was produced in the same manner as in Example 2-2, except for the above (see FIG. 6).

[0087] (Examples 2-5) The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 80 g / m 2 A decorative material of Example 2-5 was produced in the same manner as in Example 2-2, except for the above (see FIG. 6).

[0088] (Examples 2-6) The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 150 g / m 2 A decorative material of Example 2-6 was produced in the same manner as in Example 2-2, except for the above (see FIG. 6).

[0089] (Examples 2-7) The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 151 g / m 2 A decorative material of Example 2-7 was produced in the same manner as in Example 2-2, except for the above (see FIG. 6).

[0090] (Example 3-1) The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2 A triaxial woven fabric having a porosity of 33% was produced. A wood grain pattern was printed as a design layer on one side (first side) of this triaxial woven fabric using a UV inkjet printer (Canon Inc., Colorado 1640). In this printing, UV ink was applied to the glass fiber parts other than the void parts of the triaxial woven fabric, and the UV ink was cured by exposure to ultraviolet light before it dripped to the opposite side (second side). The rest of the process was the same as in Example 1-2, and the decorative material of Example 3-1 was produced (see FIG. 5).

[0091] This decorative material prevents UV ink from penetrating into the nonwoven glass fabric, allowing for vivid reproduction of patterns and colors.

[0092] (Example 3-2) The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2 A triaxial fabric with a void ratio of 33% was produced. A wood grain pattern was printed as a design layer on one side (first side) of this triaxial fabric using a UV inkjet printer (Canon Inc., Colorado 1640). In this printing, UV ink was applied to the glass fiber parts other than the void parts of the triaxial fabric, and the UV ink was cured by exposure to ultraviolet light before it dripped to the opposite side (second side).

[0093] In addition, a single black color was printed as a pattern layer on the other opposite surface (second surface) using a UV inkjet printer (Canon Inc., Colorado 1640). In this printing, UV ink was applied to the glass fiber parts other than the void parts of the triaxial woven fabric, and the UV ink was cured by continuous exposure to ultraviolet light. The rest of the process was the same as in Example 1-2, and the decorative material of Example 3-2 was produced (see FIG. 7).

[0094] This decorative material can prevent UV ink from dripping onto the opposite side (second side) where the wood grain pattern is already printed, and also prevents UV ink from seeping into the glass nonwoven fabric, allowing for clear patterns and colors to be reproduced. The decorative material thus produced can be used as an interior decorative material near a wall. Furthermore, the opposite side (second side) of the triaxial fabric thus produced is black, so it can be used as an interior decorative material that does not cause the color pattern to be reflected on the wall.

[0095] (Example 3-3) The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2A triaxial fabric with a void ratio of 33% was produced. A dark wood grain pattern was printed as a design layer on one side (first side) of this triaxial fabric using a UV inkjet printer (Canon Inc., Colorado 1640). In this printing, UV ink was applied to the glass fiber parts other than the void parts of the triaxial fabric, and the UV ink was cured by exposure to ultraviolet light before it dripped to the opposite side (second side).

[0096] A light-hued wood grain pattern was printed as a design layer on the other side (second side) using a UV inkjet printer (Canon Inc., Colorado 1640), and the UV ink was subsequently cured by UV irradiation. The rest of the process was the same as in Example 1-2 to produce the decorative material of Example 3-3 (see FIG. 7).

[0097] This decorative material was able to prevent UV ink from dripping onto the opposite side (second side) where the wood grain pattern was already printed, and at the same time, it was also able to prevent UV ink from seeping into the glass nonwoven fabric, allowing for the reproduction of clear patterns and colors. Furthermore, because the triaxial fabric produced in this way has wood grain patterns of different hues on both sides, when it is used as an interior decorative material to divide one space into two, it can recreate spaces with different atmospheres.

[0098] (Examples 3-4) The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2 A triaxial fabric with a void ratio of 33% was produced. A wood grain pattern was printed as a design layer on one side (first side) of this triaxial fabric using a UV inkjet printer (Canon Inc., Colorado 1640). In this printing, UV ink was applied to the glass fiber parts other than the void parts of the triaxial fabric, and the UV ink was cured by exposure to ultraviolet light before it dripped to the opposite side (second side).

[0099] On the other opposite side (second side), a wood grain pattern was printed in the same color and pattern as the wood grain pattern already printed as the design layer using a UV inkjet printer (Canon, Colorado 1640), and the UV ink was then applied to the glass fiber parts other than the voids in the triaxial fabric by UV irradiation, and the UV ink was cured by UV irradiation before it dripped to the opposite side (second side).Otherwise, the decorative material of Example 3-4 was produced in the same manner as in Example 1-2 (see Figure 7).

[0100] This decorative material can prevent UV ink from dripping onto the opposite side (second side) where the wood grain pattern is already printed, and at the same time, it can also prevent UV ink from soaking into the glass nonwoven fabric, allowing for clear patterns and colors to be reproduced. Furthermore, because both sides of this triaxial fabric have the same color and wood grain pattern, it does not look out of place when bent or rolled up and placed in an interior space.

[0101] (Examples 3-5) The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2 A triaxial woven fabric having a porosity of 33% was produced. A wood grain pattern was printed as a design layer on one side (first side) of this triaxial woven fabric using a UV inkjet printer (Canon Inc., Colorado 1640). In this printing, UV ink was applied to the glass fiber parts other than the void parts of the triaxial woven fabric, and the UV ink was cured by exposure to ultraviolet rays before it dripped to the opposite side (second side). Otherwise, the decorative materials of Examples 3-5 were produced in the same manner as in Examples 1-2.

[0102] In addition, a single black color was printed as a pattern layer on the base material side of the decorative material using a UV inkjet printer (Canon Inc., Colorado 1640), and the UV ink was subsequently cured by exposure to ultraviolet light to produce the decorative material (see Figure 10).

[0103] This decorative material can reproduce clear patterns and colors because it is possible to prevent UV ink from seeping into the base material side, which is already printed with a wood grain pattern. The decorative material produced in this way can be used as an interior decorative material near walls. In addition, because the opposite side (second side) is black, there is less reflection of the color pattern on the wall.

[0104] (Examples 3 to 6) The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2 A triaxial woven fabric having a porosity of 33% was produced. A wood grain pattern was printed as a design layer on one side (first side) of this triaxial woven fabric using a UV inkjet printer (Canon Inc., Colorado 1640). In this printing, UV ink was applied to the glass fiber parts other than the void parts of the triaxial woven fabric, and then the UV ink was cured by exposure to ultraviolet rays before it dripped onto the opposite side (second side). Otherwise, the decorative material was produced in the same manner as in Example 1-2.

[0105] In addition, a wood grain pattern different from the wood grain pattern already printed on the glass fiber side was printed as a design layer on the base material side of the decorative material prepared using a UV inkjet printer (Canon Inc., Colorado 1640), and the UV ink was subsequently cured by exposure to ultraviolet light to prepare the decorative material of Example 3-6 (see Figure 10).

[0106] This decorative material can prevent UV ink from seeping into the base material, allowing for vivid patterns and colors to be reproduced. The decorative material produced in this way can be used as an interior decorative material near walls. In addition, since the base material side has a different wood grain pattern, it can be used as an interior decorative material for partitioning spaces.

[0107] Comparative Example 1 The glass fiber with a thread width of 2 mm is woven triaxially to produce a basis weight of 700 g / m 2A triaxial woven fabric having a porosity of 33% was produced. A decorative material of Comparative Example 1 was produced in the same manner as in Example 1-1, except that this triaxial woven fabric was not impregnated with a silicone-based hardening resin.

[0108] Comparative Example 2 The decorative material of Comparative Example 2 was produced in the same manner as Comparative Example 1, except that a wood grain pattern was printed as a design layer on one side (first side) of the triaxial fabric using a UV inkjet printer (Colorado 1640, manufactured by Canon Inc.).

[0109] Comparative Example 3 Basis weight 50g / m 2 The glass fiber nonwoven fabric was impregnated with a silicone-based hardening resin and then air-dried to harden it, to produce a substrate. A polyamide-based hot melt was sandwiched between the substrate and the triaxial woven fabric of Comparative Example 1, and the surface material and substrate were bonded together by heating at 120°C for 60 seconds, to produce the decorative material of Comparative Example 3.

[0110] Comparative Example 4 The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 150 g / m 2 A decorative material of Comparative Example 4 was produced in the same manner as Comparative Example 3, except for the above.

[0111] Comparative Example 5 By weaving glass fibers with a thread width of 2 mm biaxially, the basis weight is 700 g / m 2 A biaxial woven fabric having a porosity of 33% was produced. A decorative material of Comparative Example 5 was produced in the same manner as in Example 1-1, except that this biaxial woven fabric was not impregnated with the silicone-based hardening resin.

[0112] Comparative Example 6 Basis weight 50g / m 2 The glass fiber nonwoven fabric was impregnated with a silicone-based hardening resin and then air-dried to harden it, to produce a substrate. A polyamide-based hot melt was sandwiched between the substrate and the biaxial woven fabric of Comparative Example 5, and the surface material and substrate were bonded together by heating at 120°C for 60 seconds, to produce the decorative material of Comparative Example 6.

[0113] Comparative Example 7 The basis weight of the glass fiber nonwoven fabric that constitutes the base material is 150 g / m 2 A decorative material of Comparative Example 7 was produced in the same manner as Comparative Example 5, except for the above.

[0114] <Evaluation items and evaluation methods> Decorative materials were prepared according to the configurations described in Examples 1-1 to 1-7, Examples 2-1 to 2-7, Examples 3-1 to 3-6, and Comparative Examples 1 to 6, and were tested and evaluated according to the following evaluation items and methods.

[0115] [Total light transmittance] The total light transmittance of the decorative materials of Examples 1-1 to 1-7, Examples 2-1 to 2-7, Examples 3-1 to 3-6, and Comparative Examples 1 to 6 was measured by the following method.

[0116] Several types of substrates with different basis weights cut to 30mm x 40mm were set in a Shimadzu UV-3600 (Shimadzu ultraviolet / visible / near-infrared spectrophotometer) and the total light transmittance in the visible light range (360nm to 860nm) was measured.

[0117] [Workability] The decorative materials of Examples 1-1 to 1-7, Examples 2-1 to 2-7, Examples 3-1 to 3-6, and Comparative Examples 1 to 6 were placed closely around a pillar with a radius of 150 mm, and the appearance of the decorative materials was evaluated.

[0118] The evaluation indicators are as follows: A: When bent along the pillar, there is no change. B: When bent along the column, slight wrinkles appear on the base material or surface material. C: When bent along the column, cracks or large wrinkles appear in the base material or surface material.

[0119] [Moldability] The decorative materials of Examples 1-1 to 1-7, Examples 2-1 to 2-7, Examples 3-1 to 3-6, and Comparative Examples 1 to 6 were molded by sandwiching them between dies having ridges and pressing them. The appearance of the obtained molded products was evaluated.

[0120] The evaluation indicators are as follows: A: The desired shape is obtained by embossing. B: There are some parts that do not follow the mold shape. C: The desired shape is not obtained even after embossing.

[0121] [Design] The design was evaluated for Examples 2-1 to 2-7, Examples 3-1 to 3-6, and Comparative Example 2, in which designs were printed by inkjet printing.

[0122] The evaluation indicators are as follows: A: The pattern is clearly visible. B: The image can be seen without any problems. C: Part of the design is missing or peeling.

[0123] <Evaluation Results> The evaluation results of the above tests are shown in Table 1.

[0124] [Table 1]

[0125] In Examples 1-1 to 1-7, Examples 2-1 to 2-7, and Examples 3-1 to 3-6, the workability was good, but the basis weight of the base material was 150 g / m 2 It can be seen that in the following Examples 1-1 to 1-6 and Examples 2-1 to 2-6, the total light transmittance of the decorative material can be continuously adjusted by changing the basis weight of the base material.

[0126] On the other hand, the basis weight of the base material is 151 g / m 2 In the above-mentioned Examples 1-7 and 2-7, the workability is not bad, but the basis weight of the base material is 150 g / m 2It can be seen that the workability is lower than that of Examples 1-1 to 1-6 and Examples 2-1 to 2-6 described below. In addition, it was found that in Comparative Examples 1 to 4, in which the triaxial fabric was not cured with resin, the triaxial fabric itself was too soft, causing wrinkles in the surface material during application. It can also be seen that all cases in which the triaxial fabric was not cured with resin, regardless of the presence or absence of a base fabric, were inferior in workability. In addition, it can be seen that Comparative Examples 5 to 7, in which the surface material was a biaxial fabric, had no rigidity due to the biaxial fabric, and were also inferior in workability. In addition, when a biaxial fabric was used, the workability was not improved even if the fabric was impregnated with resin or a base fabric was provided.

[0127] In addition, in Examples 1-1 to 1-7, Examples 2-1 to 2-7, and Examples 3-1 to 3-6, the moldability was good, but the basis weight of the substrate was 151 g / m 2 In the above-mentioned Examples 1-7 and 2-7, the rigidity of the decorative material increases due to the increase in the basis weight of the base material, and the moldability is somewhat reduced. In addition, in Comparative Examples 1 to 4, in which the triaxial fabric was not cured with resin, the triaxial fabric itself is too soft and the processability is poor. In addition, regardless of whether or not a base fabric is used, all cases in which the triaxial fabric is not cured with resin are poor in processability. In addition, in Comparative Examples 5 to 7, in which the surface material is a biaxial fabric, the biaxial fabric has no rigidity and is also poor in processability. When a biaxial fabric is used, the processability was not improved even if the biaxial fabric was impregnated with resin or a base fabric was provided.

[0128] It was found that the design was good in Examples 2-1 to 2-7 and Examples 3-1 to 3-6, in which the triaxial fabric was impregnated with resin before or after printing the pattern to provide a pattern layer. On the other hand, in Comparative Example 2, in which the fabric was not impregnated with resin, the adhesion between the ink and the surface material was poor, and the ink was easily removed by rubbing the ink surface with a finger. This resulted in poor design.

[0129] Therefore, according to the decorative material of this embodiment, the light transmittance can be easily changed by changing the basis weight of the base material while maintaining excellent workability. At the same time, workability, formability, and designability can be improved. [Explanation of symbols]

[0130] 10, 11, 12, 13, 14, 15, 16, 17, 18, 19...decorative material, 20...surface material, 21...triaxial fabric, 21a...first thread, 21b...second thread, 21c...third thread, 22...curable resin, 23...pattern layer, 23a...pattern layer, 23b...pattern layer, 23c...pattern layer, 3...adhesive layer, 4...substrate, 4'...curable resin, D1...first direction, D2...second direction, D3...third direction.

Claims

1. A surface material having a triaxial weave, The triaxial fabric is hardened by a hardening resin. Decorative material.

2. The curable resin coats the surface of the triaxial fabric. The decorative material according to claim 1.

3. A substrate which is a porous fiber assembly; An adhesive layer disposed between the surface material and the substrate, The basis weight of the substrate is 150 g / m 2 Below is the The decorative material according to claim 1.

4. The substrate is made of a glass fiber nonwoven fabric. The decorative material according to claim 3.

5. A pattern layer is further provided on the triaxial woven fabric, The pattern layer is provided three-dimensionally in the thickness direction of the triaxial woven fabric. The decorative material according to claim 1.

6. The design layer has a cured product of a UV ink. The decorative material according to claim 5.

7. The triaxial fabric has first yarns extending in a first direction, second yarns extending in a second direction intersecting the first direction, and third yarns extending in a third direction intersecting the first direction and the second direction, The pattern layer is provided on the first thread, the second thread, and the third thread, When viewed from the thickness direction of the triaxial woven fabric, the pattern layer provided on the first thread, the pattern layer provided on the second thread, and the pattern layer provided on the third thread are continuous. The decorative material according to claim 5.

8. A method for manufacturing a decorative material having a surface material with a triaxial woven fabric, comprising the steps of: hardening the triaxial fabric with a hardening resin to produce the surface material; A method for manufacturing decorative materials.

9. The surface material is bonded to a substrate which is a porous fiber assembly; The basis weight of the substrate is 150 g / m 2 The following shall apply: A method for producing the decorative material according to claim 8.

10. A pattern layer is provided on the triaxial woven fabric. A method for producing the decorative material according to claim 8.

11. Providing the design layer on the surface of the curable resin. The method for producing the decorative material according to claim 10.

12. The pattern layer is provided on the surface of the triaxial woven fabric. The method for producing the decorative material according to claim 10.

13. The pattern layer is provided by inkjet printing. The method for producing the decorative material according to claim 10.

14. After performing inkjet printing using a UV ink, the UV ink is cured by irradiating it with ultraviolet light to provide the design layer. The method for producing the decorative material according to claim 13.

Citation Information

Patent Citations

  • Film material