Water-based coating composition, heat seal layer composition, and laminate
By incorporating hydrophobized hemicellulose and biodegradable emulsifiers in aqueous coating compositions, the water resistance of dried coatings and heat seal layers is significantly enhanced, addressing the inadequacies of existing formulations.
Patent Information
- Application Number
- JP2023051000
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The dried product of existing water-based coating compositions, particularly those containing hemicellulose, lack sufficient water resistance.
Aqueous coating compositions comprising biodegradable thermoplastic resin with hydrophobized hemicellulose, along with biodegradable emulsification aids like polysuccinimide and polyaspartate, are formulated to enhance water resistance, with specific DS values and component ratios optimized for improved dispersibility and film formation.
The resulting dried coating and heat seal layer exhibit excellent water resistance, ensuring the laminate's durability and performance.
Smart Images

Figure 2024140016000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-based coating composition, a composition for a heat-sealing layer, and a laminate. [Background technology]
[0002] A water-based coating composition containing hemicellulose is known (see, for example, Patent Document 1 below). In Patent Document 1, the water-based coating composition is applied and dried to produce a dried product (dried film). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] WO2021 / 019468 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the dried product of the water-based coating composition described in Patent Document 1 does not have sufficient water resistance.
[0005] The present invention provides a water-based coating composition which exhibits excellent water resistance when dried, and a composition for a heat-seal layer which exhibits excellent water resistance of the heat-seal layer, and a laminate. [Means for solving the problem]
[0006] The present invention [1] includes an aqueous coating composition comprising an aqueous medium and a biodegradable thermoplastic resin dispersed in the aqueous medium, the biodegradable thermoplastic resin containing hydrophobized hemicellulose.
[0007] The present invention [2] includes the aqueous coating composition according to [1], wherein the DS value of the hydrophobized hemicellulose, represented by the following formula (1), is 0.1 or more and 2.8 or less.
[0008] DS value=C / D (1) C: The number of moles of hydrophobic groups in 1 mole of the hydrophobized hemicellulose D: The number of moles of repeating units in 1 mole of the hydrophobized hemicellulose
[0009] The present invention [3] includes the water-based coating composition according to [2], wherein the DS value is 1.0 or more and 2.0 or less.
[0010] The present invention [4] includes the aqueous coating composition according to any one of [1] to [3], further comprising a biodegradable emulsifier, the biodegradable emulsifier comprising polysuccinimide and / or polyaspartic acid salt.
[0011] The present invention [5] includes the water-based coating composition according to [4], wherein the biodegradable emulsifier aid is polysuccinimide.
[0012] The present invention [6] includes the aqueous coating composition according to any one of [1] to [5], wherein the total amount of lignin-derived components in the biodegradable thermoplastic resin is 20 mass% or less.
[0013] The present invention [7] includes the aqueous coating composition according to any one of [1] to [6], wherein the total amount of cellulose-derived components in the biodegradable thermoplastic resin is 20 mass% or less.
[0014] The present invention [8] includes a composition for a heat seal layer, comprising the aqueous coating composition according to any one of [1] to [7].
[0015] The present invention [9] includes a laminate comprising, in the thickness direction, a paper base material and a heat seal layer made of a dried product of the composition for a heat seal layer described in [8]. Effect of the Invention
[0016] The dried product of the water-based coating composition of the present invention has excellent water resistance because the biodegradable thermoplastic resin contains hydrophobized hemicellulose.
[0017] According to the composition for a seal layer and the laminate of the present invention, the heat seal layer has excellent water resistance.
[0018] The laminate of the present invention has excellent water resistance since it has a heat seal layer made of a dried product of the water-based coating composition. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a cross-sectional view of one embodiment of a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] 1. Water-based coating composition The water-based coating composition of the present invention contains an aqueous medium and a biodegradable thermoplastic resin.
[0021] 1.1 Aqueous media Examples of the aqueous medium include water, alcohol, and a water / alcohol mixed medium. The aqueous medium is preferably water.
[0022] The blending ratio of the aqueous medium in the aqueous coating composition is, for example, 10 mass % or more, preferably 20 mass % or more, and for example, 90 mass % or less, preferably 80 mass % or less.
[0023] 1.2 Biodegradable thermoplastic resin The biodegradable thermoplastic resin is dispersed in an aqueous medium. The biodegradable thermoplastic resin contains hydrophobized hemicellulose.
[0024] Hydrophobized hemicellulose can be obtained by hydrophobizing hemicellulose.
[0025] 1.2.1 Hemicellulose Hemicellulose is a polysaccharide that constitutes the cell walls of plants (including wood). As described below, hemicellulose is obtained by digesting wood. Hemicellulose contains multiple hydroxyl groups. Hemicellulose and a method for producing it are described, for example, in WO2014 / 002674.
[0026] 1.2.2 Hydrophobization Examples of hydrophobization include acetylation. Specifically, all or part of the multiple hydroxyl groups in hemicellulose react with acetic acid to form ester bonds, thereby acetylating the hydroxyl groups of hemicellulose. A method for hydrophobizing (acetylating) hemicellulose is described, for example, in JP 2019-073625 A. Substituents such as acetonyl groups and ionized substituents can also be used in combination with hydrophobization.
[0027] 1.2.3 DS value of hydrophobized hemicellulose The DS value of the hydrophobized hemicellulose is, for example, 0.1 or more, preferably 0.3 or more, more preferably 1.0 or more, and for example, 3.0 or less, preferably 2.9 or less, more preferably 2.8 or less, and even more preferably 2.0 or less.
[0028] The DS value of hydrophobized hemicellulose is the degree of hydrophobization in the repeating units of the hydrophobized hemicellulose. Specifically, the DS value of hydrophobized hemicellulose is expressed by the following formula (1).
[0029] DS value=C / D (1) C: number of moles of hydrophobic groups in 1 mole of hydrophobized hemicellulose D: number of moles of repeating units in 1 mole of hydrophobized hemicellulose
[0030] Details of the measurement of the DS value are described in the Examples below.
[0031] When the DS value of the hydrophobized hemicellulose is equal to or higher than the above-mentioned lower limit and equal to or lower than the above-mentioned upper limit, the water resistance of the dried product of the aqueous coating composition is excellent.
[0032] The blending ratio of the hydrophobized hemicellulose in the biodegradable thermoplastic resin is, for example, 30% by mass or more, preferably 50% by mass or more, more preferably 75% by mass or more, particularly preferably 90% by mass or more, and most preferably 95% by mass or more, and is, for example, 100% by mass or less.
[0033] 1.2.5 Lignin- and cellulose-derived components The biodegradable thermoplastic resin may further contain lignin-derived and cellulose-derived components, which are by-products produced along with hemicellulose during wood digestion.
[0034] The total amount of lignin-derived components in the biodegradable thermoplastic resin is, for example, 20% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less. If the total amount of lignin-derived components is equal to or less than the upper limit, the dispersibility of the biodegradable thermoplastic resin in the water-based coating composition can be improved, and a heat seal layer (described later) with little coloring can be obtained. The method for measuring the total amount of lignin-derived components is described in the examples below.
[0035] In the water-based coating composition, the total amount of cellulose-derived components in the biodegradable thermoplastic resin is, for example, 20% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 2% by mass or less, and particularly preferably 1% by mass or less. If the total amount of cellulose-derived components is less than the above upper limit, the dispersibility of the biodegradable thermoplastic resin in the water-based coating composition can be improved, and a heat seal layer with excellent heat sealability can be obtained. The method for measuring the total amount of cellulose-derived components is described in the following examples.
[0036] 1.2.6 Volume mean diameter of biodegradable thermoplastic resin The volume average diameter of the biodegradable thermoplastic resin is, for example, 20 μm or less, preferably 10 μm or less, more preferably 5 μm or less, even more preferably 4 μm or less, and particularly preferably 3 μm or less. If the volume average diameter of the biodegradable thermoplastic resin is equal to or less than the above upper limit, the dispersibility of the biodegradable thermoplastic resin in the water-based coating composition is good, and the film-forming property and coating uniformity when applied to a substrate are excellent.
[0037] The lower limit of the volume average diameter of the biodegradable thermoplastic resin is not limited, and the volume average diameter of the biodegradable thermoplastic resin is, for example, 0.1 μm or more.
[0038] The volume average diameter of the biodegradable thermoplastic resin means the volume average diameter of the biodegradable thermoplastic resin dispersed in the aqueous medium in the aqueous coating composition. The method for measuring the volume average diameter of the biodegradable thermoplastic resin will be described in the examples below.
[0039] 1.2.7 Biodegradable thermoplastic resin blend ratio The mixing ratio of the biodegradable thermoplastic resin in the water-based coating composition is, for example, 10 mass % or more, preferably 20 mass % or more, and for example, 90 mass % or less, preferably 80 mass % or less.
[0040] 1.3 Biodegradable emulsifiers The water-based coating composition may further contain a biodegradable emulsifier. The biodegradable thermoplastic resin improves the dispersibility (emulsification) of the biodegradable thermoplastic resin in the water-based medium. The biodegradable emulsifier contains, for example, polysuccinimide and / or polyaspartic acid salt. Preferably, the biodegradable emulsifier is polysuccinimide.
[0041] 1.3.1 Polysuccinimide Polysuccinimide is obtained, for example, as a reaction product of aspartic acid. Polysuccinimide, its properties, and the method for producing polysuccinimide are described, for example, in JP-A-2000-239379 and JP-A-2000-273173. Polysuccinimide is more suitable as a biodegradable emulsifier than polyaspartic acid salts from the viewpoint of improving the water resistance of the dried product of the water-based coating composition.
[0042] 1.3.2 Polyaspartates Examples of salts forming polyaspartic acid salts include alkali metal salts. Examples of alkali metal salts include lithium salts, sodium salts, and potassium salts. Polyaspartic acid salts are obtained, for example, as hydrolysates of a solution in which polysuccinimide is dissolved in an alkali metal hydroxide. Polyaspartic acid salts, their properties, and methods for producing polyaspartic acid salts are described, for example, in JP-A-2000-239379 and JP-A-2000-273173.
[0043] 1.3.3 Weight average molecular weight (Mw) of biodegradable thermal emulsification aid The weight average molecular weight (Mw) of the biodegradable thermal emulsification aid is, for example, 10,000 or more, preferably 20,000 or more, and for example, 100,000 or less, preferably 50,000 or less. If the weight average molecular weight (Mw) of the biodegradable thermal emulsification aid is above the above-mentioned lower limit and below the above-mentioned upper limit, the dispersibility of the biodegradable thermoplastic resin is good, and a dry coating film (heat seal layer) with excellent heat sealability is formed. The weight average molecular weight (Mw) of the biodegradable thermal emulsification aid is measured by gel permeation chromatography (GPC) using a calibration curve prepared with standard polystyrene.
[0044] 1.3.4 Physical properties of biodegradable emulsifiers 1.3.4.1 Ring opening rate The biodegradable emulsifier may be partially ring-opened. The ring-opening rate of the biodegradable emulsifier is, for example, 3% or more, and is, for example, 90% or less, preferably 70% or less, more preferably 50% or less, and even more preferably 30% or less. If the ring-opening rate of the biodegradable emulsifier is below the upper limit, the water resistance of the dried product of the water-based coating composition can be improved. The method for measuring the ring-opening rate of the biodegradable emulsifier will be described in the following examples. The biodegradable emulsifier is partially ring-opened by the incorporation of hydroxide during the production process.
[0045] 1.3.5 Ratio of biodegradable emulsifier The blending ratio of polysuccinimide in the biodegradable emulsification aid is, for example, 40% by mass or more, preferably 60% by mass or more, more preferably 75% by mass or more, and for example, 100% by mass or less. The blending ratio of polyaspartate in the biodegradable emulsification aid is, for example, 40% by mass or more, preferably 60% by mass or more, more preferably 75% by mass or more, and for example, 100% by mass or less.
[0046] The blending ratio of the biodegradable emulsification aid in the water-based coating composition is, for example, 0.1 mass % or more, preferably 1 mass % or more, and for example, 25 mass % or less, preferably 15 mass % or less.
[0047] The mixing ratio of the biodegradable emulsification aid per 100 parts by mass of the biodegradable thermoplastic resin is, for example, 1 part by mass or more, preferably 5 parts by mass or more, and for example, 50 parts by mass or less, preferably 25 parts by mass or less.
[0048] The water-based coating composition may contain known additives in appropriate proportions.
[0049] The solids concentration in the water-based coating composition is, for example, 10 mass % or more, preferably 20 mass % or more, more preferably 25 mass % or more, and for example, 80 mass % or less.
[0050] 1.4 Preparation of Water-Based Coating Composition To prepare the water-based coating composition, a biodegradable thermoplastic resin is dispersed in a water-based medium. For example, a biodegradable thermoplastic resin (and a mixture of a biodegradable emulsifier, if necessary) is kneaded to prepare a solid, and then the solid is dispersed in a water-based medium. The kneading conditions are not limited.
[0051] 1.5 Application The use of the water-based coating composition is not limited. For example, the use of the water-based coating composition is a composition for a heat seal layer. That is, the composition for a heat seal layer includes the water-based coating composition described above. The heat seal layer melts by heat and adheres to an adherend, or the heat seal layers adhere to each other.
[0052] 1.6 Laminates With reference to FIG. 1, one embodiment of a laminate 1 will be described.
[0053] The laminate 1 has a thickness. The laminate 1 extends in a planar direction. The planar direction is perpendicular to the thickness. The laminate 1 has a sheet shape. The laminate 1 includes a paper base material 2 and a heat seal layer 3 in this order in the thickness direction. In this embodiment, the laminate 1 preferably includes only the paper base material 2 and the heat seal layer 3.
[0054] 1.6.1 Paper base material 2 The paper base material 2 is a backing material that supports the heat seal layer 3 from the other side in the thickness direction. The raw material of the paper base material 2 includes paper.
[0055] The basis weight of the paper base material 2 is, for example, 10 g / m 2 More than 30 g / m 2 or more, for example, 500 g / m 2 Preferably, 300 g / m or less 2 The thickness of the paper base material 2 is, for example, 1 μm or more and, for example, 1,000 μm or less.
[0056] 1.5.2 Heat seal layer 3 In this embodiment, the heat seal layer 3 is disposed on one surface of the paper base material 2 in the thickness direction.
[0057] The heat seal layer 3 is made of the dried product of the composition for the heat seal layer described above. The basis weight of the heat seal layer 3 is, for example, 0.1 g / m 2 More than 1 g / m 2 or more, for example, 100 g / m 2 Preferably, 10 g / m or less 2 The heat seal layer 3 has a thickness of, for example, 0.1 μm or more, or preferably 1 μm or more, and for example, 100 μm or less, or preferably 50 μm or less.
[0058] 1.6.3 Physical properties of laminate 1 The water absorption amount (Cobb300) of the laminate 1 after 300 seconds based on the Cobb method (JIS P8140) is, for example, 20 g / m 2 Less than 10 g / m 2 Less than 5 g / m 2 When the water absorption amount is below the above upper limit, the laminate 1 has excellent water resistance.
[0059] 1.6.4 Manufacturing method of laminate 1 To produce the laminate 1, first, a paper base material 2 is prepared.
[0060] Next, the composition for the heat seal layer is applied (coated) to one surface of the laminate 1 in the thickness direction. The number of applications may be one or more. Then, the composition for the heat seal layer is dried. Specifically, it is heated, for example, at 80° C. or higher, preferably 100° C. or higher, and, for example, at 160° C. or lower, preferably 140° C. or lower. The heating time is, for example, 5 seconds or higher, preferably 10 seconds or higher, and 100 seconds or lower, preferably 30 seconds or lower.
[0061] By the above-mentioned coating and drying, the heat seal layer 3 is formed as a dried product.
[0062] 2. Effects The dried product of the water-based coating composition has excellent water resistance because the biodegradable thermoplastic resin contains hydrophobized hemicellulose.
[0063] The heat seal layer 3, which is a dried product of the composition for the seal layer, has excellent water resistance.
[0064] The laminate of the present invention has excellent water resistance since it includes the heat seal layer 3 described above.
[0065] The laminate 1 shown in FIG. 1 has a heat seal layer 3 made of a dried product of a water-based coating composition, and therefore has excellent water resistance. EXAMPLES
[0066] The present invention will be described in more detail below with reference to examples and comparative examples. The present invention is not limited to the examples and comparative examples. The specific numerical values of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit (a numerical value defined as "not more than" or "less than") or lower limit (a numerical value defined as "not less than" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".
[0067] 1. Measurement methods for physical properties First, the measurement of physical properties will be described.
[0068] 1.1 DS value of acetylated hemicellulose Each of the heat seal layer compositions of Examples 2 to 5 was dried, and 0.5 g of biodegradable thermoplastic resin (acetylated hemicellulose) (A) was accurately weighed. 75 mL of ethanol and 50 mL (0.025 mol) of 0.5N NaOH (B) were added thereto, and the mixture was stirred for 3 to 4 hours. The mixture was filtered, washed with water, and dried, and the sample on the filter paper was subjected to FT-IR measurement. In FT-IR, it was confirmed that the absorption peak due to the carbonyl group of the ester bond had disappeared, that is, the ester bond had been hydrolyzed.
[0069] The filtrate was then used for the back titration described below. The filtrate contained sodium acetate salt produced as a result of hydrolysis and excess NaOH. The NaOH was neutralized by titration using 1N HCl and phenolphthalein. The DS value was calculated using the following formula (1).
[0070] DS value=C / D (1) C: number of moles of hydrophobic groups in 1 mole of hydrophobized hemicellulose D: number of moles of repeating units in 1 mole of hydrophobized hemicellulose
[0071] The above C and D were each calculated using the following formula.
[0072] 0.025 mol (B) - (moles of HCl used for neutralization) = moles of acetyl groups ester-bonded to the hydroxyl groups of hemicellulose (C) (2)
[0073] (Molecular weight of hemicellulose repeating unit 162 × moles of hemicellulose repeating unit (unknown (D))) + (molecular weight of acetyl group 43 × (C)) = 0.5 g of weighed sample (A) (3)
[0074] The DS value of hemicellulose was determined in the same manner as the DS value of acetylated hemicellulose.
[0075] 1.2 Weight average molecular weight (Mw) of polysuccinimide and polyaspartate The weight average molecular weight (Mw) of each of the polysuccinimide and polyaspartate salts was measured by gel permeation chromatography (GPC). The weight average molecular weight (Mw) was calculated using a calibration curve prepared using monodisperse standard polystyrene.
[0076] 1.3 Ring-opening ratio of polysuccinimide and polyasparagine For each of the polysuccinimide and the polyaspartate, the infrared absorption spectrum was measured by Fourier transform infrared spectroscopy, and the ring-opening ratio was calculated based on the following formula (1).
[0077] Ring opening rate (%)=D1550cm -1 / (D1550cm -1 +D1700cm -1 ) (1) D1550cm -1 : Absorbance from ring-opened cyclic imide D1700cm -1 : Absorbance from closed cyclic imide
[0078] 1.4 Measurement of volume average diameter of biodegradable thermoplastic resin (water dispersion) The volume average diameter of the biodegradable thermoplastic resin (water dispersion) in the composition for the heat seal layer was measured using Microtrac HRA (manufactured by Honeywell).
[0079] 2.Synthesis of biodegradable thermoplastic resin 2.1 Synthesis of hemicellulose <Synthesis Example 1> Wood was crushed into small pieces to produce wood chips. The wood chips were placed in an aqueous butanol solution and heated to 100°C. After cooling, the aqueous phase containing hemicellulose was separated and dried to obtain hemicellulose powder. The DS value of hemicellulose (biodegradable thermoplastic resin (A)) was 0.
[0080] Next, the cellulose-derived components and lignin-derived components in the biodegradable thermoplastic resin (A) were measured. Specifically, 10 g of ionic liquid (N-methyl-N-(2-methoxyethyl)pyrrolidinium lysine) and 1 g of biodegradable thermoplastic resin (A) were weighed into a Spitz tube, and the mixture was stirred at 60 ° C for 12 hours. Next, the ionic liquid layer was collected by centrifugation, and the following operation was repeated twice: 3 g of ionic liquid was added to the Spitz tube, stirred at 60 ° C for 1 hour, centrifuged, and the ionic liquid layer was collected. The collected ionic liquid layer was diluted with ethanol, and the precipitated lignin was separated by centrifugation. After vacuum drying, the mass was measured and the proportion of the lignin-derived components in the biodegradable thermoplastic resin (A) was calculated.
[0081] Furthermore, the residue remaining in the test tube after centrifugation was washed three times with water, and hemicellulose was extracted with a 0.1 M aqueous sodium solution. The remaining residue was washed three times with water, vacuum dried, and then the mass was measured to calculate the proportion of cellulose-derived components in the biodegradable thermoplastic resin (A). As a result, the proportion of cellulose-derived components in the biodegradable thermoplastic resin (A) was 1 mass%, and the proportion of lignin-derived components was 2 mass% (see Table 1).
[0082] 2.2 Synthesis of acetylated hemicellulose <Synthesis Example 2> 60 g of hemicellulose was dissolved in 1 kg of 1-ethyl-3-methylimidazolium acetate. Then, 1.5 L of dimethyl sulfoxide and 2 L of isopropenyl acetate were added dropwise, and the mixture was reacted at 50°C for 30 minutes. After the reaction was completed, acetone was added to the reaction solution, and the precipitated acetylated hemicellulose was collected and dried. The DS value of the obtained acetylated hemicellulose (biodegradable thermoplastic resin (B)) was 0.5 (see Table 1).
[0083] 1 g of biodegradable thermoplastic resin (B) was dissolved in 10 g of 1-ethyl-3-methylimidazolium acetate, and the mixture was dried under reduced pressure at 80°C for 2 hours under stirring conditions. Acetone was then added, and the insolubilized material was separated by filtration. The filtrate was concentrated, and methanol was added. The insolubilized cellulose-derived components were separated by filtration and weighed precisely to calculate the ratio of the cellulose-derived components in the biodegradable thermoplastic resin (acetylated hemicellulose). The filtrate remaining after the addition of methanol was used to remove and recover the ionic liquid using a cation exchange resin. Finally, water was added to the filtrate, and the insolubilized lignin-derived components were separated by filtration and weighed precisely to calculate the ratio of the lignin-derived components in the biodegradable thermoplastic resin. As a result, the ratio of the cellulose-derived components in the biodegradable thermoplastic resin (B) was 1 mass%, and the ratio of the lignin-derived components was 2 mass% (see Table 1).
[0084] <Synthesis Example 3> 60 g of hemicellulose was dissolved in 1 kg of 1-ethyl-3-methylimidazolium acetate. Then, 1.5 L of dimethyl sulfoxide and 2 L of isopropenyl acetate were added dropwise and reacted at 50°C for 3 hours. After the reaction was completed, acetone was added to the reaction solution, and the precipitated acetylated hemicellulose was collected and dried. The DS value of the obtained acetylated hemicellulose (biodegradable thermoplastic resin (C)) was 1.8 (see Table 1).
[0085] Next, the respective proportions of the cellulose-derived component and the lignin-derived component were determined in the same manner as in Synthesis Example 2. As a result, the proportion of the cellulose-derived component in the biodegradable thermoplastic resin (C) was 1 mass %, and the proportion of the lignin-derived component was 2 mass %.
[0086] <Synthesis Example 4> 60 g of bagasse (sugarcane residue, particle size: 250 μm or less) was dissolved in 1 kg of 1-ethyl-3-methylimidazolium acetate and dried under reduced pressure at 80 °C for 2 hours under stirring conditions. After that, the inside of the reaction vessel was replaced with Ar (argon). Next, 1.5 L of dimethyl sulfoxide and 2 L of isopropenyl acetate were dropped and reacted at 50 °C for 3 hours. After the reaction was completed, acetone was added to the reaction solution and the precipitate was collected. The filtrate was concentrated and then methanol was added, and the insolubilized substances were also separated and collected by filtration. The filtrate remaining after the addition of methanol was used to remove and collect the ionic liquid using a cation exchange resin, water was added to the filtrate, and the insolubilized substances were collected by filtration. All the precipitates obtained above were collected and dried to obtain biodegradable thermoplastic resin (D). The DS value of biodegradable thermoplastic resin (D) was 1.8 (see Table 1).
[0087] Next, the respective proportions of the cellulose-derived component and the lignin-derived component were determined in the same manner as in Synthesis Example 2. As a result, the proportion of the cellulose-derived component in the biodegradable thermoplastic resin (D) was 13% by mass, and the proportion of the lignin-derived component was 10% by mass (see Table 1).
[0088] 2.3 Synthesis of biodegradable emulsifiers <Synthesis Example 5> (Synthesis of polysuccinimide) In a 500 ml flask, 30.0 g of L-aspartic acid and 15.6 g of 85% by mass phosphoric acid were charged, and the mixture was stirred and mixed at 80°C to 90°C for 60 minutes under normal pressure in a nitrogen atmosphere to obtain a liquid reaction mixture. The mixture was then heated at a temperature of 160°C and a pressure of 500 mmHg to 20 mmHg (0.0667 MPa to 0.0027 MPa) for 3 hours to obtain a solid polysuccinimide. The weight average molecular weight (Mw) of the obtained polysuccinimide (biodegradable emulsifier (a)) was 30,000, and the ring opening rate was 20% (Table 2).
[0089] <Synthesis Example 6> (Synthesis of polyaspartic acid salt) 10g of polysuccinimide was added to a solution of 4.2g of sodium hydroxide dissolved in 100g of ion-exchanged water, and the solution was stirred at room temperature for 3 hours to hydrolyze the mixture. 600ml of methanol was added to the solution, and the precipitate formed was filtered under reduced pressure, washed with methanol, and dried under reduced pressure at 80°C for 2 hours to obtain a polyaspartate. The weight-average molecular weight (Mw) of the obtained polyaspartate (biodegradable emulsifier (b)) was 30,000, and the ring-opening rate was 80% (Table 2).
[0090] 3. Preparation of the composition for the heat seal layer <Example 1> 100 parts of biodegradable thermoplastic resin (C) was fed to a co-rotating twin screw extruder (manufactured by Ikegai Iron Works, PCM-30, L / D=40) at a rate of 100 kg / hour, and melt-kneaded at a set temperature of 200°C and a screw rotation speed of 150 rpm, while water was continuously fed from a feed port provided in the middle of the extruder at a rate of 40 kg / hour. The extruded kneaded product (biodegradable thermoplastic resin (C)) was cooled to 90°C by passing through a single screw extruder installed at the outlet of the extruder, and discharged. The discharged product was a white or white transparent solid (biodegradable thermoplastic resin (C)), and the solid content concentration calculated from the mass difference before and after drying was 70% by mass. The solid was added to warm water (water at 40°C) and dispersed in water to produce a white heat seal layer composition. The solid content concentration in the heat seal layer composition was 30% by mass.
[0091] <Example 2> 90 parts of biodegradable thermoplastic resin (C) and 10 parts of biodegradable emulsifier (a) were fed into a co-rotating twin screw extruder (Ikegai Iron Works, PCM-30, L / D=40) at a rate of 100 kg / hour, and melt-kneaded at a set temperature of 200°C and a screw rotation speed of 150 rpm, while a 20% by mass aqueous solution of potassium hydroxide was continuously fed at a rate of 40 kg / hour from a feed port provided in the middle of the extruder. The extruded kneaded product (a mixture of biodegradable thermoplastic resin (C) and biodegradable emulsifier (a)) was cooled to 90°C by passing it through a single screw extruder installed at the outlet of the extruder, and discharged. The discharged product was a white or white transparent solid (a mixture of biodegradable thermoplastic resin (C) and biodegradable emulsifier (a)), and the solid content concentration calculated from the mass difference before and after drying was 70% by mass. The solid was added to warm water (40° C.) and dispersed in the water to produce a white heat seal layer composition.
[0092] <Example 3> A composition for a heat seal layer was produced in the same manner as in Example 2, except that the biodegradable emulsifier (a) was replaced with the biodegradable emulsifier (b).
[0093] <Example 4> A composition for a heat seal layer was produced in the same manner as in Example 2, except that the biodegradable thermoplastic resin (C) was changed to the biodegradable thermoplastic resin (B).
[0094] <Example 5> A composition for a heat seal layer was produced in the same manner as in Example 2, except that the biodegradable thermoplastic resin (C) was changed to the biodegradable thermoplastic resin (D).
[0095] <Comparative Example 1> A composition for a heat seal layer was produced in the same manner as in Example 2, except that the biodegradable thermoplastic resin (C) was changed to the biodegradable thermoplastic resin (A).
[0096] <Comparative Example 2> A composition for a heat seal layer was produced in the same manner as in Example 2. The biodegradable thermoplastic resin (C) was changed to the biodegradable thermoplastic resin (A). However, only a viscous liquid was obtained, and a composition for a heat seal layer could not be produced.
[0097] 4. Evaluation 4.1 Dispersibility of the composition for the heat seal layer The solid content concentration in each of the heat-seal layer compositions of Examples 1 to 5 and Comparative Examples 1 to 2 was adjusted to 40% by mass to 50% by mass. The heat-seal layer compositions were then filtered through a 100-mesh wire screen. The dispersibility (emulsification ability) of the filtrate was evaluated according to the following criteria.
[0098] ⊚: No undispersed matter was observed, and the dispersion state was very good. ◯: A small amount of undispersed matter was found, but the dispersion state was good. Δ: Undispersed matter was observed, but the dispersion state was not poor. ×: Undispersed matter was found, and the dispersion state was poor.
[0099] 4.2 Water resistance of dried products Cup base paper (basis weight 170g / m) manufactured by Tami Nadu Newsprint and Papers 2 ) was used as a substrate, and the compositions for the heat seal layer of each of Examples 1 to 5 and Comparative Example 1 were dried to give a heat seal layer 3 (solid content) having a basis weight of 6 g / m 2 The laminate was coated twice using an air knife coater so that the thickness was such that the coating thickness was 130 mm, and then dried at 130° C. for 20 seconds to produce Laminate 1. The Cobb value of Laminate 1 was measured by the Cobb method (JIS P8140) to measure the amount of water absorption after 300 seconds (Cobb300), and evaluated according to the following criteria. A low water absorption (Cobb300) indicates excellent water resistance.
[0100] ◎: Water absorption (Cobb300) is 5g / m 2 It was less than. 〇: Water absorption (Cobb300) is 5g / m 2 More than 10g / m2 It was less than. △: Water absorption (Cobb300) is 10g / m 2 More than 20g / m 2 It was less than. ×: Water absorption (Cobb300) is 20g / m 2 That was all.
[0101] [Table 1]
[0102] [Table 2]
[0103] [Table 3] [Explanation of symbols]
[0104] 1. Laminate 2 Paper base material 3 Heat seal layer
Claims
1. An aqueous medium; A biodegradable thermoplastic resin dispersed in the aqueous medium, The water-based coating composition, wherein the biodegradable thermoplastic resin contains hydrophobized hemicellulose.
2. 2. The aqueous coating composition according to claim 1, wherein the hydrophobized hemicellulose has a DS value of 0.1 or more and 2.8 or less, as represented by the following formula (1): DS value = C / D (1) C: the number of moles of hydrophobic groups in 1 mole of the hydrophobized hemicellulose D: the number of moles of repeating units in 1 mole of the hydrophobized hemicellulose
3. The water-based coating composition according to claim 2, wherein the DS value is 1.0 or more and 2.0 or less.
4. Further containing a biodegradable emulsifier, 3. The aqueous coating composition according to claim 1, wherein the biodegradable emulsifier comprises polysuccinimide and / or polyaspartic acid salt.
5. The water-based coating composition according to claim 4, wherein the biodegradable emulsifier is polysuccinimide.
6. 3. The aqueous coating composition according to claim 1, wherein a total amount of lignin-derived components in the biodegradable thermoplastic resin is 20 mass% or less.
7. 3. The aqueous coating composition according to claim 1, wherein the total amount of cellulose-derived components in the biodegradable thermoplastic resin is 20 mass % or less.
8. A composition for a heat seal layer, comprising the aqueous coating composition according to claim 1 or 2.
9. A laminate comprising, in order in a thickness direction, a paper substrate and a heat seal layer comprising the dried product of the composition for a heat seal layer according to claim 8 .
Citation Information
Patent Citations
Aqueous dispersion composition for paper
JP1998168793A
Polysuccinimide and production of polyaspartate
JP2000273173A
Aqueous coating material composition
JP2003165954A
Polymeric films or coatings containing hemicellulose
JP2006520843A
Hemicellulose-containing polymer film or coating