Stretchable woven fabric

A woven fabric with an elastic core and blended sheath yarns of high-performance and non-high-performance fibers addresses the limitations of existing cut-resistant fabrics by achieving high elongation, tensile strength, and cut resistance while maintaining good texture.

JP2024140320APending Publication Date: 2024-10-10DUPONT TORAY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023051410
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing cut-resistant fabrics made from core-sheath composite yarns lack sufficient stretchability, tensile strength, and elongation, and often have poor texture and complex processing.

Method used

A woven fabric using an elastic core yarn surrounded by a sheath yarn containing a blend of high-performance and non-high-performance fibers, with specific ratios and processing methods to achieve a high elongation rate, tensile strength, and cut resistance.

Benefits of technology

The fabric achieves an elongation rate of 15% or more, tensile strength of 100 N/cm or more, and cut resistance of 2.0 or higher, maintaining excellent stretch, texture, and tensile properties without significant drops in performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140320000001
    Figure 2024140320000001
  • Figure 2024140320000002
    Figure 2024140320000002
Patent Text Reader

Abstract

To provide a woven fabric which is excellent in stretchability, touch, tensile strength and cut resistance and has a high elongation.SOLUTION: There is provided a stretchable woven fabric obtained by using a core yarn which is an elastic yarn, and a sheath yarn which is a core-sheath composite yarn containing a highly functional fiber having a tensile strength of 17.5 cN / dtex or more and a non-highly functional fiber, in which the woven fabric contains 1-10 wt.% of the elastic yarns and 5-90 wt.% of the highly functional fibers. The elongation of the woven fabric is adjusted to 15% or more by increasing or decreasing the content of the elastic yarn and / or the highly functional fiber.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cut-resistant stretchable fabric made using a core-sheath composite yarn. [Background technology]

[0002] Core-sheath composite yarns, which use an elastic yarn as the core yarn and a high-performance fiber as the sheath yarn, are used in textile products by taking advantage of their excellent elasticity and cut resistance. For example, Patent Document 1 discloses a glove (knitted fabric) made of a core-sheath composite yarn, which uses an elastic yarn as the core yarn and a spun yarn of para-aramid staple fiber as the sheath yarn. Patent Document 2 discloses a protective garment (knitted fabric, woven fabric) made of a core-sheath composite yarn, which uses an elastic yarn as the core yarn and a filament yarn of para-aramid fiber as the sheath yarn. However, although the woven and knitted fabrics of Patent Documents 1 and 2 have excellent cut resistance, they have problems with elongation and tensile strength.

[0003] Furthermore, Patent Document 3 discloses that the tensile strength of a woven fabric can be increased by using a core-sheath composite yarn consisting of an elastic yarn and a spun yarn of a meta-aramid fiber. However, since a metal particle-containing layer and a colorant-containing resin layer are laminated on the fabric surface, not only is the processing process complicated, but the texture is also inferior.

[0004] Furthermore, Patent Document 4 discloses a plain weave fabric using a composite yarn of a composite fiber in which two components are bonded together in a side-by-side or eccentric core-sheath type, and a spun yarn containing a flame-retardant fiber such as an aramid fiber, in order to impart flame retardancy and elasticity. In order to make the fabric flame-retardant and elastic, the fabric is characterized by containing 75% by weight or more (of the fabric) of flame-retardant fiber and 5 to 15% by weight (of the fabric), but the elongation of the fabric is at most about 12%. Therefore, the elasticity is insufficient for applications such as work clothes (T-shirts and innerwear) and pants that generally have stretch. There is no mention of cut resistance.

[0005] Therefore, although the production of cut-resistant woven and knitted fabrics using high-performance fibers (flame-retardant fibers) has been investigated, no fabrics using high-performance fibers are known that have excellent elasticity, a good texture, and excellent tensile strength and cut resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2004-011060 A [Patent Document 2] JP 2003-193314 A [Patent Document 3] JP 2014-061646 A [Patent Document 4] JP 2014-240532 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in view of the above-mentioned background of the conventional technology, and an object of the present invention is to provide a woven fabric which is excellent in stretchability, texture, tensile strength and cut resistance, and also has a high elongation percentage. [Means for solving the problem]

[0008] In order to solve the above problems, the inventors conducted extensive research and discovered that the above problems could be solved at once by using a core-sheath composite yarn in which a core yarn made of an elastic yarn is surrounded by a sheath yarn containing a high-performance fiber having excellent tensile strength and a non-high-performance fiber, thereby completing the present invention.

[0009] That is, the present invention provides A woven fabric using an elastic yarn as a core yarn and a core-sheath composite yarn containing a high-performance fiber having a tensile strength of 17.5 cN / dtex or more and a non-high-performance fiber as a sheath yarn, The elastic woven fabric contains 1 to 10% by weight of the elastic yarn and 5 to 90% by weight of the high-performance fiber relative to the weight of the woven fabric, and the elongation rate of the woven fabric (based on JIS L1096 8.16B method) is adjusted by changing the content of the elastic yarn and / or the high-performance fiber.

[0010] The stretchable woven fabric of the present invention is characterized in that it has an elongation percentage (based on JIS L1096 8.16B method) of 15% or more. The stretchable fabric of the present invention is characterized in that it has a tensile strength (based on JIS L1096 8.14A method) of 100 N / cm or more in the warp and / or weft directions, and a cut resistance (based on JIS T8052 method) of 2.0 or more. Effect of the Invention

[0011] The elastic woven fabric of the present invention contains a certain ratio of elastic yarn in the core yarn and a certain ratio of high-performance fiber with excellent tensile strength in the sheath yarn, so that by changing the content of the elastic yarn or high-performance fiber, a woven fabric with high elongation (for example, 15% or more) can be obtained. The obtained woven fabric has excellent elasticity, texture, tensile strength, and cut resistance. Furthermore, even when the elongation of the woven fabric is adjusted by increasing or decreasing the content of the elastic yarn or high-performance fiber in the core-sheath composite yarn, the tensile strength and cut resistance of the woven fabric do not suddenly decrease. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The elastic woven fabric (hereinafter sometimes abbreviated as "woven fabric") of the present invention is made using a core-sheath composite yarn in which the core yarn is an elastic yarn and the sheath yarn contains an organic fiber having a tensile strength of 17.5 cN / dtex or more and a non-high-performance fiber.

[0013] [Sheath-core composite yarn] (core thread) Examples of the elastic yarn constituting the core yarn of the core-sheath composite yarn include polyurethane-based elastic yarn, polyester-based elastomer fiber, false twist crimp-processed yarn, etc. Among these, polyurethane-based elastic yarn is preferred because of its excellent elasticity and good processability.

[0014] The elastic yarn has a fineness in the range of preferably 10 to 200 dtex, more preferably 20 to 150 dtex, and further preferably 40 to 100 dtex. If it is 10 dtex or more, it will not cause yarn breakage during covering of the sheath yarn or during the knitting process of the fabric, and the fabric will have a good fit when worn. If it is 200 dtex or less, the power of expansion and contraction of the core-sheath composite yarn will not be too strong, so that the fit and feel of the fabric when worn will not be impaired.

[0015] From the viewpoint of imparting elasticity to the core-sheath composite yarn, the breaking elongation of the elastic yarn is preferably 200% or more, and more preferably 300% or more. If it is less than 200%, there is a risk that sufficient elasticity cannot be obtained when the woven fabric is knitted.

[0016] The elastic yarn is used in an amount ranging from 1 to 10% of the fabric weight. If the ratio of the elastic yarn is less than 1% by weight, the fabric will have poor elasticity and texture, and if it exceeds 10% by weight, the fabric will tend to become wrinkled and wrinkled, making it difficult to obtain a flat fabric. The ratio is more preferably 1 to 8% by weight, and even more preferably 2 to 8% by weight.

[0017] (sheath thread) The sheath yarn of the core-sheath composite yarn contains high-performance fibers and non-high-performance fibers. The weight ratio of the high-performance fiber should be in the range of 5 to 90% by weight based on the weight of the woven fabric. If the weight ratio is less than 5% by weight, the cut resistance and tensile strength of the woven fabric will be insufficient, and if it exceeds 90% by weight, the texture (softness, etc.) of the woven fabric will be poor and it may feel itchy. The weight ratio of the high-performance fiber is preferably 10 to 90% by weight, more preferably 15 to 85% by weight, and particularly preferably 20 to 75% by weight.

[0018] As the high-performance fiber, from the viewpoint of imparting high tensile strength to the woven fabric, a fiber having a tensile strength of 17.5 cN / dtex or more as a property of the raw yarn (filament) measured based on JIS L1013 is preferable. A fiber having a tensile modulus of elasticity of 400 cN / dtex or more, also measured based on JIS L1013, is more preferable. By using such a high-performance fiber, it is possible to impart sufficient tensile strength and cut resistance to the woven fabric. In addition, it is possible to eliminate thread breakage during weaving.

[0019] As the high-performance fiber, for example, one or more types of fibers selected from high-performance fibers such as para-aramid fibers, wholly aromatic polyester fibers, polyparaphenylene benzobisoxazole fibers, polybenzimidazole fibers, polyamideimide fibers, and ultra-high molecular weight polyethylene fibers can be preferably used.

[0020] Among the above-mentioned high-performance fibers, para-aramid fibers are preferred because the raw yarn has high strength, high elasticity, and excellent cut resistance and heat resistance. Examples include para-fully aromatic polyamide fibers such as polyparaphenylene terephthalamide fiber (manufactured by Toray DuPont Co., Ltd., product name "Kevlar") and copolyparaphenylene-3,4'-diphenyl ether terephthalamide fiber (manufactured by Teijin Limited, product name "Technora"). The para-aramid fiber may be manufactured by a known method or a method equivalent thereto, or the above-mentioned commercially available products may be used.

[0021] Non-high-performance fibers are fibers with a tensile strength of less than 17.5 cN / dtex. By combining such non-high-performance fibers with high-performance fibers, it is possible to increase the elongation of the woven fabric and improve its texture without significantly reducing the cut resistance of the woven fabric. In addition, by combining non-high-performance fibers, it is possible to prevent breakage of the core-sheath composite yarn during weaving.

[0022] Examples of non-high-performance fibers include synthetic fibers (nylon, vinylon, polyester, acrylic, polypropylene), regenerated fibers (rayon, cupra), semi-synthetic fibers (acetate), and natural fibers (cotton, linen); meta-aramid fibers (e.g., polymetaphenylene isophthalamide fibers (manufactured by DuPont, product name "Nomex"), etc.), and one or more types of fibers selected from these non-high-performance fibers can be used. Among these non-high-performance fibers, cellulosic fibers (rayon, cotton, etc.) are preferred, and cotton is particularly preferred, because they are highly effective in increasing the elongation and feel of the fabric without significantly reducing the cut resistance of the fabric.

[0023] The short fibers of the above-mentioned high-performance fibers and non-high-performance fibers (synthetic fibers, semi-synthetic fibers) are obtained by cutting crimped filament yarns (long fibers). The short fibers preferably have a fineness of 1.0 to 5.0 dtex measured based on JIS L1015, an average fiber length of 25 to 200 mm (more preferably 30 to 110 mm), and a crimp number of 3 to 12 peaks (more preferably 5 to 10 peaks) / 25.4 mm. If the crimp number is too small, it is difficult to obtain a spun yarn with a good texture and flexibility, and conversely, if the crimp number is too large, the strength may decrease due to buckling, abrasion, etc. of the aramid long fibers.

[0024] In addition, medium-staple cotton (fiber length: 26.2-27.8 mm) and long-staple cotton (fiber length: 28.6-33.3 mm) are used for the cotton fibers. In order to improve the quality stability of the blended yarn and prevent problems during the spinning process, it is best to make the staple fiber length of the high-performance fiber as close as possible to the fiber length of the natural fiber.

[0025] The amount of the non-high-performance fibers used varies depending on the amount of elastic yarn and high-performance fibers used, but is usually in the range of 1 to 94% by weight. From the viewpoint of improving the texture of the fabric, it is preferable to use 5% by weight or more of the non-high-performance fibers based on the weight of the fabric. In addition, since the high-performance fibers mainly contribute to improving the cut resistance and tensile strength of the fabric, whereas the non-high-performance fibers mainly contribute to improving the texture of the fabric, in order to impart the desired cut resistance (cut force: 3.0 N or more) and tensile strength (500 N / 5 cm or more) to the fabric, the non-high-performance fibers are preferably 80% by weight or less (based on the weight of the fabric).

[0026] The weight ratio of high-performance fiber / non-high-performance fiber is preferably 10 / 90 to 80 / 20, more preferably 15 / 85 to 70 / 30, and further preferably 18 / 82 to 68 / 32. By using the fibers in this range, the cut resistance and tensile strength of the high-performance fiber and the elongation and flexibility of the non-high-performance fiber can be imparted to the woven fabric.

[0027] The fibers constituting the sheath yarn can be selected from among filaments only, staple fibers only, or a combination of filaments and staple fibers, but it is preferable to use staple fibers only, since this makes it easy to cover the core yarn and results in a good texture of the woven fabric. Staple fibers are usually used in the form of spun yarn (blended spun yarn).

[0028] (Covering) The core-sheath composite yarn can be produced by a known method of covering the core yarn with the sheath yarn. For example, when covering the elastic yarn with a blended yarn (roving) of high-performance fiber and non-high-performance fiber, a known method of covering the roving of the crude blended yarn with the elastic yarn in the spinning process can be adopted. In addition, a method of covering the drawn sliver with an air vortex into the elastic yarn using an air spinning machine (for example, VORTEX spinning machine manufactured by Murata Machinery Co., Ltd.) may also be used. The number of twists during covering is preferably 10 to 20 t / in (inch), more preferably 10 to 15 t / inch. In addition, it is preferable to perform twisting with a twist coefficient (K) calculated by the following formula (1) in the range of 2.5 to 6.0. If the twist coefficient (K) is smaller than 2.5, the entanglement between the short fibers of the high-performance fiber becomes too weak, so that the ends of the short fibers protrude from the spun yarn, and the core-sheath composite yarn tends to have a prickly feel. On the other hand, if the twist coefficient (K) is larger than 6.0, the twist becomes too strong, and double twisting occurs more frequently, which deteriorates processability, reduces the tensile strength of the blended yarn, and deteriorates the texture. A more preferable twist coefficient (K) is in the range of 3.0 to 5.0. The twist direction of the spun yarn single yarn may be either S or Z.

[0029] K=T / √N (1) (where T is the number of twists (t / inch) and N is the cotton count)

[0030] The covering by the sheath yarn may be not only single covering in which the periphery of the core yarn is covered once, but also double covering in which the periphery of the core yarn is covered twice, but single covering is preferred because it allows the elastic effect of the elastic core yarn to be fully exerted and a lightweight, thin fabric can be obtained. In the case of double covering, it is preferable that the twist direction of the covering above the sheath yarn is opposite to the twist direction of the covering below the sheath yarn in order to cancel out torque.

[0031] [Cut-resistant stretch fabric] The cut-resistant stretchable woven fabric of the present invention can achieve a woven fabric elongation of 15% or more measured according to JIS L 1096 8.16B method by using the above-mentioned core-sheath composite yarn. If the elongation is less than 15%, the stretch and flexibility of the fabric are insufficient. There is no particular upper limit to the elongation, but it is preferably about 30%. More preferably, it is 25%. The reason is that when the elongation is set high, the ratio of the core yarn or non-high-performance fiber in the core-sheath composite yarn is increased, but in that case, the ratio of the high-performance fiber is reduced, making it difficult to impart the desired cutting strength to the woven fabric. In addition, this causes the surface of the woven fabric to become wrinkled or wrinkled, making it difficult to obtain stable cut resistance.

[0032] The woven fabric of the present invention is woven using 50 to 100% by weight of the core-sheath composite yarn of the present invention based on the weight of the fabric. If it is less than 50% by weight, the effects of the composite yarn of the present invention (elongation, tensile strength, cut resistance, stretchability) may be insufficient. It is more preferable to use 70% by weight or more, and even more preferable to use 100% by weight.

[0033] The sheath-core composite yarn of the present invention can also be used as a composite yarn obtained by mixing or twisting with other known fibers such as polyester fibers, nylon fibers, polyvinyl alcohol-based fibers, etc., within a range that does not impair the effects of the present invention. Furthermore, the sheath-core composite yarn of the present invention can be used as warp and weft yarns of a woven fabric, or as weft yarn, depending on the design of the final product (required stretch direction).

[0034] The weave may be any weave such as plain weave, twill weave, satin weave, or variegated weave, but twill weave (including twill modified weave) is preferred because it is easy to stretch and can secure a certain degree of elongation, and by increasing the number of jumps in the weave, the fabric becomes easy to stretch. If the number of jumps is too large, the cut resistance of the fabric decreases or there is a strong tendency for the weave to become misaligned, so the maximum number of jumps in the complete weave is preferably about 1 jump, 2 jumps, or 3 jumps. In other words, the weave is preferably twill (1 jump), 2 / 1 twill (2 jumps), 2 / 2 twill (2 jumps), etc., but this is not limited as it can be selected according to the application. The weave density is preferably determined by the fineness of the warp and weft threads, the weave, and the basis weight.

[0035] The weight of the fabric of the present invention is 200 g / m 2 Less than 200 g / m is preferable. 2 In the case of a woven fabric exceeding this value, the cut resistance is sufficient, but the elongation tends to be insufficient. A more preferable basis weight is 50 to 200 g / m 2 Particularly preferably, the thickness is 100 to 200 g / m 2 By increasing the basis weight, the tensile strength and cut resistance of the woven fabric are improved. The cover factor of the woven fabric is preferably in the range of 1800 to 2500, and within the above range, a woven fabric having the desired elongation, tensile strength, cut resistance and texture can be obtained.

[0036] In the present invention, the elongation percentage of the woven fabric is desirably 15% or more according to JIS L1096 8.16B method. It is preferably 15 to 30%, more preferably 15 to 25%, and even more preferably 15 to 20%. If it is less than 15%, there is a risk of problems when wearing clothing made using the woven fabric or when wearing it for work or sports that require vigorous movement.

[0037] The tensile strength of the woven fabric of the present invention is desirably 100 N / cm or more according to JIS L1096 8.14A method. It is preferably 120 N / cm or more, more preferably 150 N / cm or more, and even more preferably 180 N / cm or more. If it is less than 100 N / cm, clothing made using the woven fabric may break during use or washing.

[0038] Regarding the cut resistance of the woven fabric of the present invention, it is desirable that the cut resistance according to the JIS T8052 method is 2.0 or more. It is preferably 2.1 or more, more preferably 2.3 or more, and even more preferably 2.5 or more. If it is less than 2.0, there is a risk that the clothing made using the woven fabric will break during use. The cut resistance of the woven fabric of the present invention improves as the thickness (basis weight) increases, so the desired cut strength can be obtained by adjusting the basis weight of the woven fabric. EXAMPLES

[0039] The present invention will now be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the following examples. The physical properties and other properties were evaluated according to the following methods.

[0040] [Thread size] The fineness of the core-sheath composite yarn was determined according to JIS L1013:2010 Chemical fiber filament yarn test method 8.3 B method (simplified method). F0 = 1000 × m / L × (100 + R0) / 100 (F0: exact fineness (tex), m: absolute dry weight of sample (g), L: length of sample (m), R0: process moisture content (%) as defined in JIS L 0105, 4.1) The yarn count was calculated from the correct fineness.

[0041] [Fabric strength factor] It was calculated using the following formula. Cover factor (CF) = √ warp thread size × density + √ weft thread size × density

[0042] [Texture of the fabric] A wearing test was conducted by five subjects. According to 5.2 of EN 420:2003 Protective gloves-General requirements and test methods, all subjects rated the dexterity at level 5, and if five out of five subjects rated the fit as "good", it was marked as ◎ (pass), if three or more out of five subjects rated the fit as "good", it was marked as ○ (pass), if two out of five subjects rated the fit as "good", it was marked as △, and otherwise it was marked as × (fail).

[0043] (Sheath-core composite yarn A) A blended yarn (Kevlar / cotton = 65 / 35 (weight ratio)) consisting of aramid fiber (Kevlar (registered trademark) staple fiber (fiber length: 38 mm) and medium-length cotton was wound around polyurethane elastic yarn Lycra 44T (registered trademark) (manufactured by Toray Opelontex Co., Ltd., fineness: 44 dtex) in the Z direction with a twist rate of 16.0 turns / inch to produce sheath-core composite yarn A with a cotton count of 20 (s). The twist coefficient of the sheath-core composite yarn A was 3.6.

[0044] (Sheath-core composite yarn B) A blended yarn (Kevlar / cotton = 65 / 35 (weight ratio)) consisting of aramid fiber (Kevlar (registered trademark) staple fiber (fiber length: 38 mm) and medium-length cotton was wound around Lycra 78T (registered trademark) polyurethane elastic yarn (Toray Opelontex Co., Ltd., fineness: 78 dtex) in the Z direction with a twist rate of 16.0 turns / inch to produce sheath-core composite yarn B with a cotton count of 20 (s). The twist coefficient of the sheath-core composite yarn B was 3.6.

[0045] (Sheath-core composite yarn C) A blended yarn (Kevlar / cotton = 20 / 80 (weight ratio)) consisting of aramid fiber (Kevlar (registered trademark) staple fiber (fiber length: 38 mm) and medium-length cotton was wound around polyurethane elastic yarn Lycra 78T (registered trademark) (manufactured by Toray Opelontex Co., Ltd., fineness: 78 dtex) in the Z direction with a twist rate of 16.0 turns / inch to produce sheath-core composite yarn C with a cotton count of 20 (s). The twist coefficient of the sheath-core composite yarn C was 3.6.

[0046] (Sheath-core spun yarn D) A blended yarn (Kevlar / cotton = 65 / 35 (weight ratio)) consisting of aramid fiber (Kevlar (registered trademark) short fiber (fiber length: 38 mm) and medium-length cotton was wound around Lycra 78T (registered trademark) polyurethane elastic yarn (Toray Opelontex Co., Ltd., fineness: 78 dtex) in the Z direction with a twist rate of 12.0 turns / inch to produce sheath / core spun yarn D with a cotton count of 10 (s). The twist coefficient of the sheath / core spun yarn D was 3.8.

[0047] The physical properties of the core-sheath composite yarns A to C and the core-sheath spun yarn D are summarized in Table 1.

[0048] [Table 1]

[0049] Example 1 A 2 / 1 twill weave was produced on a rapier loom using Kevlar spun yarn (20s) as the warp yarn and core-sheath composite yarn A as the weft yarn, yielding a woven fabric with a width of 200 cm. The physical properties of the woven fabric are shown in Table 2.

[0050] Example 2 A 2 / 1 twill weave was produced on a rapier loom using Kevlar spun yarn (20s) as the warp yarn and core-sheath composite yarn B as the weft yarn, yielding a woven fabric with a width of 200 cm. The physical properties of the woven fabric are shown in Table 2.

[0051] Example 3 A 2 / 1 twill weave was produced on a rapier loom using the core-sheath composite yarn B as the warp and weft yarns to obtain a woven fabric with a width of 200 cm. The physical properties of the woven fabric are shown in Table 2.

[0052] Example 4 A 2 / 1 twill weave was produced on a rapier loom using the core-sheath composite yarn C for the warp and weft directions to obtain a woven fabric with a width of 200 cm. The physical properties of the woven fabric are shown in Table 2.

[0053] Comparative Example 1 A 2 / 2 twill weave was produced on a rapier loom using Kevlar spun yarn (20s) as the warp yarn and core-sheath spun yarn D as the weft yarn, to obtain a woven fabric with a width of 200 cm. The physical properties of the woven fabric are shown in Table 2.

[0054] Comparative Example 2 A 2 / 1 twill weave was produced on a rapier loom using Kevlar spun yarn (20s) for the warp and weft directions to obtain a woven fabric with a width of 200 cm. The physical properties of the woven fabric are shown in Table 2.

[0055] Comparative Example 3 A plain weave fabric was woven on a rapier loom using cotton spun yarn (20s) for the warp and weft directions. The physical properties of the woven fabric are shown in Table 2.

[0056] As can be seen from Table 2, the fabric of Comparative Example 1, woven using Kevlar spun yarn in the warp direction and core-sheath spun yarn in the weft direction, and the fabrics of Comparative Examples 2 and 3, woven using Kevlar spun yarn and cotton spun yarn, had a maximum elongation of about 3 to 5%. In particular, the fabrics of Comparative Examples 2 and 3, which used only spun yarn in the warp and weft directions, had an elongation of about 3%, which was far from the 15% targeted by the present invention.

[0057] In contrast, the fabrics of Examples 1 and 2, which were woven using Kevlar spun yarn as the warp yarn and core-sheath composite yarns (A or B) with different core yarn thicknesses as the weft yarn, had a weft elongation rate that was about five times higher than the fabrics of Comparative Examples 2 and 3, which used Kevlar spun yarn or cotton spun yarn as the weft yarn. In addition, by using a thicker core yarn, the elongation rate of the fabric increased by 1.1% and the cut strength increased by 0.3 N. The obtained fabric had sufficient tensile strength and cut resistance.

[0058] The fabrics of Examples 3 and 4, which were woven using core-sheath composite yarns (B or C) with Kevlar / cotton as the sheath yarn for the warp and weft directions, had better elongation in both the warp and weft directions than the fabrics of Examples 1 and 2, and the obtained fabrics had good tensile strength and cut resistance.

[0059] In addition, when fabrics woven using sheath-core composite yarn B (Kevlar-rich) and sheath-core composite yarn C (cotton-rich) were compared (Examples 3 and 4), the difference between the two in terms of elongation and cut resistance was relatively small. The sheath-core composite yarn B showed a higher tensile strength.

[0060] Therefore, it can be seen that in a core-sheath composite yarn containing high-performance fibers and non-high-performance fibers, the ratio of the two does not affect the elongation rate, but does affect the tensile strength and cut resistance.

[0061] [Table 2] [Industrial Applicability]

[0062] The cut-resistant stretchable woven fabric of the present invention has excellent stretchability, tensile strength, cut resistance, and texture, and can provide woven products that are both comfortable to wear and safe to use. Therefore, the fabric can be suitably used for work gloves, aprons, work clothes, hats, various sports products, outdoor products, etc. in civil engineering and construction work, agricultural work, fishery, forestry, food industry, medical care, high-tech industry, etc.

Claims

1. A woven fabric using an elastic yarn as a core yarn and a core-sheath composite yarn containing a high-performance fiber having a tensile strength of 17.5 cN / dtex or more and a non-high-performance fiber as a sheath yarn, The woven fabric contains 1 to 10% by weight of the elastic yarn and 5 to 90% by weight of the high-performance fiber, An elastic woven fabric, characterized in that the elongation of the woven fabric is adjusted by increasing or decreasing the content of the elastic yarn and / or high-performance fiber.

2. 2. The stretchable woven fabric according to claim 1, wherein the woven fabric has an elongation of 15% or more as measured by JIS L1096 8.16B method.

3. 2. The stretchable woven fabric according to claim 1, wherein the tensile strength of the woven fabric in the warp and / or weft directions, measured by JIS L1096 8.14A method (labeled strip method), is 100 N / cm or more.

4. The stretchable woven fabric according to claim 1, wherein the woven fabric has a cut resistance of 2.0 or more as measured by JIS T8052 method.

5. 2. The stretch woven fabric of claim 1, wherein the elastic yarn is a polyurethane elastic yarn.

6. The stretchable fabric according to claim 1, wherein the non-high-performance fiber is at least one selected from synthetic fibers (nylon, vinylon, polyester, acrylic, polypropylene), regenerated fibers (rayon, cupra), semi-synthetic fibers (acetate), and natural fibers (cotton, hemp).

7. The stretch fabric of claim 1 , wherein the fabric is a fabric having a twill weave.

8. A garment comprising the stretchable fabric according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Protective clothes

    JP2003193314A

  • Protective glove

    JP2004011060A

  • Stretch woven fabric, and method for producing the same

    JP2014061646A

  • Stretchable flame-retardant fabric and textile product

    JP2014240532A