Sealant resin composition, and electronic part sealed with sealant resin composition
Patent Information
- Application Number
- JP2023051550
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
【0010】 本発明の封止材用樹脂組成物における効果の作用メカニズムの詳細は不明な部分があるが、以下のように推定される。但し、本発明は、この作用メカニズムに限定して解釈されない。
Smart Images

Figure 2024140418000001 
Figure 2024140418000002 
Figure 2024140418000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition for an encapsulant used for electronic components. In particular, the present invention relates to a resin composition for an encapsulant that has high storage stability at room temperature in an uncured state, and has high adhesion to a substrate and excellent barrier properties after curing. The present invention also relates to an electronic component encapsulated with an encapsulant made of the resin composition for an encapsulant. [Background technology]
[0002] Electronic devices such as televisions and smartphones are sealed with resin compositions to protect the inside of the devices from mechanical and chemical effects. In recent years, electronic devices have become lighter, thinner, and smaller, and there is a demand for smaller electronic components, and further thinner electronic devices. In order to meet the demand for lighter, thinner, and smaller packages, the encapsulant is also required to have higher functionality, specifically, it is required to have further improved barrier properties and adhesion to the substrate. The resin composition for the encapsulant is generally composed of an acrylic resin, which is a photocurable resin, and a filler such as silica, but in order to meet the above-mentioned demand for higher performance, a technology has been proposed in which various additives are blended into the resin composition for the encapsulant (Patent Document 1).
[0003] Moreover, it is known that the addition of a polymerization inhibitor or making a curing agent latent is effective for improving the pot life of a resin composition containing an acrylic resin or the like (Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-072999 A [Patent Document 2] JP 2014-077024 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when a filler is added to improve the performance of the encapsulant as in Patent Document 1, there is a problem that the adhesion to the substrate decreases with the filling amount of the filler, making the encapsulant more susceptible to peeling.
[0006] In addition, as electronic components become lighter, thinner, and smaller, the volume of the sealing part also becomes lighter, thinner, and smaller, and it is necessary to apply the sealing material more precisely. However, the viscosity of the resin composition for sealing material is easily changed when it is handled at room temperature, and there is a problem with storage stability at room temperature. When the viscosity of the resin composition for sealing material increases, coating unevenness of the sealing material is easily caused during coating, and in order to precisely apply the resin composition for sealing material with increased viscosity, it is necessary to change the coating conditions from time to time. However, even with the method described in Patent Document 2, the viscosity increases over time, so there is still a problem with storage stability at room temperature. In addition, there is also a problem that the curing property of the resin composition for sealing material is inhibited when a polymerization inhibitor or the like is added.
[0007] An object of the present invention is to provide an encapsulant resin composition which has high storage stability at room temperature in an uncured state, and has high adhesion to a substrate and excellent barrier properties after curing, and to provide an electronic component encapsulated with the encapsulant resin composition. [Means for solving the problem]
[0008] That is, the present invention relates to the following [1] and [2]. [1] A resin composition for use as a sealant for electronic components, comprising (A) a polyfunctional thiol having 2 to 6 thiol groups, (B) a polyphenol having two or more phenolic hydroxyl groups, (C) a filler, and (D) a curable compound.
[0009] [2] An electronic component encapsulated using the encapsulant resin composition according to [1] above. Effect of the Invention
[0010] Although the details of the mechanism of action of the effect of the encapsulant resin composition of the present invention are unclear, it is presumed as follows: However, the present invention is not interpreted as being limited to this mechanism of action.
[0011] It is presumed that the phenolic hydroxyl group of the polyphenol having two or more phenolic hydroxyl groups (B) contributes to the polarization of the thiol group of the multifunctional thiol having 2 to 6 thiol groups (A), and promotes the reaction between the multifunctional thiol having 2 to 6 thiol groups (A) and the curable compound (D) during curing. As a result, a denser polymer network is formed, and a resin composition for sealing materials for electronic components having excellent barrier properties is obtained. Furthermore, it is presumed that the phenolic hydroxyl group of the polyphenol having two or more phenolic hydroxyl groups (B) improves the compatibility between the filler (C) and the resin, and the resin becomes more compatible with the surface of the filler (C), resulting in excellent adhesion to the substrate. Moreover, when the sealing material composition is stored at room temperature, the polyphenol having two or more phenolic hydroxyl groups (B) strongly inhibits the generation of thiyl radicals from the multifunctional thiol having 2 to 6 thiol groups (A), and has high storage stability at room temperature. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention relates to a resin composition for an encapsulant, comprising (A) a polyfunctional thiol having 2 to 6 thiol groups, (B) a polyphenol having two or more phenolic hydroxyl groups, (C) a filler, and (D) a curable compound.
[0013] In the present invention, the term "XX to XX" indicating a numerical range includes the lower limit ("XX") and the upper limit ("XX") unless otherwise specified. In other words, it strictly means "not less than XX and not more than XX."
[0014] The present invention will be described in detail below. The encapsulant resin composition of the present invention is used as an encapsulant for electronic components, and contains the following (A), (B), (C), and (D) as essential components.
[0015] <(A) Multifunctional thiol having 2 to 6 thiol groups> (A) The polyfunctional thiol having 2 to 6 thiol groups may be a compound having 2 to 6 thiol groups in one molecule, and one type may be used alone or two or more types may be used in combination. By containing such a compound, a thiol-ene or thiol-epoxy reaction proceeds with other components, and adhesion to the substrate can be improved. The thioether bond formed can flexibly change the bond angle compared to the bond of atoms such as C, O, and N, so that the cured product has high flexibility and can improve the adhesion of the sealing material to the substrate. In addition, the cured product formed from the thioether bond has high flexibility of the bond angle and can be cured at a high density so that the atoms fill the gaps between the bonds, so that it has high barrier properties against moisture and can suppress an increase in moisture permeability even when exposed to a severe moist heat test. (A) The polyfunctional thiol having 2 to 6 thiol groups is preferably a compound represented by the following formula 1. [ka] (wherein a is an integer of 2 to 6; R 1 is a divalent to hexavalent organic group having 10 to 60 carbon atoms.
[0016] In the formula, a is preferably an integer of 3 to 6 from the viewpoint of enhancing the barrier properties of the sealing material for electronic components and suppressing an increase in moisture permeability even when exposed to a severe wet heat test. If a in the formula is within this range, the curing shrinkage after curing is small, and a good cured product can be obtained without a decrease in adhesion to the substrate. Among them, it is most preferable that a in the formula is 6 from the viewpoint of barrier properties. In addition, R 1 From the same viewpoint, R is preferably 3 to 6. 1 R has 10 to 60 carbon atoms, preferably 10 to 45 carbon atoms, and more preferably 12 to 30 carbon atoms. 1 When the number of carbon atoms is within this range, the crosslink density of the cured product of the encapsulant resin composition is sufficient, the encapsulant has excellent barrier properties, and an increase in moisture permeability can be suppressed even when exposed to a severe moist heat test.
[0017] The organic group is a group that contains C and may further contain at least one element selected from the group consisting of Si, N, P, O, and S. The organic group may be a polymer having a repeating unit. In addition, the organic group may contain, for example, a ketone group, an ester group, an ether group, a hydroxyl group, an amide group, a thioether group, an isocyanurate group, a glycoluril group, or the like in its structure. Specific examples of (A) polyfunctional thiols having 2 to 6 thiol groups include ethylene glycol bis(3-mercaptopropionate), tetraethylene glycol bis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), trimethylolpropane tris(2-mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), trimethylolethane tris(2-mercaptoacetate), trimethylolethane tris(3-mercaptopropionate), pentaerythritol tetrakis(2-mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), 1,2,3-tris(2-mercaptoethylene mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, tetrakis(2-mercaptoethylthiomethyl)methane, tetrakis(3-mercaptopropylthiomethyl)methane, 1,3,5-tris(mercaptoethyleneoxy)benzene, tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, and the like.
[0018] Among the compounds represented by the above formula 1, preferred are polyfunctional thiols having a pentaerythritol skeleton, polyfunctional thiols having a dipentaerythritol skeleton, and polyfunctional thiols having an isocyanurate skeleton. Among them, preferred are dipentaerythritol hexakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), and tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, because they can increase the flexibility of the cured product of the resin composition for encapsulant, provide excellent barrier properties for the encapsulant, and suppress an increase in moisture permeability even when exposed to a severe wet heat test.
[0019] (A) The polyfunctional thiol having 2 to 6 thiol groups may be a commercially available product or a synthesized product. Specifically, the polyfunctional thiol may be obtained by esterification reaction of a polyhydric alcohol such as pentaerythritol with a mercapto group-containing carboxylic acid such as 3-mercaptopropionic acid by a known method.
[0020] <(B) Polyphenols having two or more phenolic hydroxyl groups> (B) polyphenol having two or more phenolic hydroxyl groups may be any one having two or more phenolic hydroxyl groups in one molecule, and one type may be used alone or two or more types may be used in combination. By containing such a compound, it is presumed that the phenolic hydroxyl group of (B) polyphenol having two or more phenolic hydroxyl groups contributes to the polarization of the thiol group (SH bond) of (A) polyfunctional thiol having 2 to 6 thiol groups, and promotes the reaction between (A) polyfunctional thiol having 2 to 6 thiol groups and (D) curable compound during curing. As a result, a denser polymer network is formed, and a resin composition for sealing materials of electronic components having excellent barrier properties is obtained. Furthermore, it is presumed that the phenolic hydroxyl group of (B) polyphenol having two or more phenolic hydroxyl groups improves the compatibility of (C) filler and resin, improving the compatibility of the resin with the surface of the filler, and providing excellent adhesion to the substrate. Furthermore, (B) a polyphenol having two or more phenolic hydroxyl groups strongly inhibits the generation of thiyl radicals from (A) a polyfunctional thiol having 2 to 6 thiol groups when the sealing material composition is stored at room temperature.
[0021] (B) Examples of polyphenols having two or more phenolic hydroxyl groups include 4,4'-isopropylidenediphenol, 2,2-methylene-bis(4-methyl-6-tert-butylphenol), N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxybenzenepropionamide), 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-butylidenebis(3-methyl-6 -tert-butylphenol), 3,9-bis[1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, triethylene glycol bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate], 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,1,3-tris(2-methyl-4-hydroxy-5-ter t-Butylphenyl)butane, Tetrakis-[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, Tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, Catechol, 4-Methylcatechol, 4-Chlorocatechol, tert-Butylcatechol, 3,5-Di-tert-Butylcatechol, Hydroquinone, Chlorohydroquinone, Methoxyhydroquinone, Bromohydroquinone, 2-Methylhydroquinone, tert-Butylhydroquinone, Phenylhydroquinone Quinones, 2,6-dimethylhydroquinone, 2,5-di-tert-butylhydroquinone, 2,5-di-tert-amylhydroquinone, trimethylhydroquinone, tetramethylhydroquinone, resorcinol, 2-methylresorcinol, 5-methylresorcinol, 2-nitroresorcinol, 4-hexylresorcinol, 4-chlororesorcinol, 2-acetylresorcinol, 5-acetylresorcinol, 4,6-dichlororesorcinol, 2,5-di-tert-butylsorcinol, pyrogallol, phloroglucinone, 1,2,Examples of the gallic acid include 4-benzenetriol, gallic acid, methyl gallate, ethyl gallate, propyl gallate, isobutyl gallate, butyl gallate, isoamyl gallate, n-octyl gallate, dodecyl gallate, hexadecyl gallate, and stearyl gallate.
[0022] Among these, polyphenols having two or more phenolic hydroxyl groups are preferably those having 2 to 3 phenolic hydroxyl groups in one aromatic ring, because the acid dissociation constant (pKa) of the phenolic hydroxyl group is low, improving storage stability at room temperature in the uncured state, and promoting the reaction between (A) a polyfunctional thiol having 2 to 6 thiol groups and (D) a curable compound during curing, thereby forming a denser polymer network, and also improving the compatibility between (C) the filler and the resin component, thereby improving adhesion to the substrate. Specifically, catechol, 4-methylcatechol, 4-chlorocatechol, tert-butylcatechol, 3,5-di-tert-butylcatechol, hydroquinone, chlorohydroquinone, methoxyhydroquinone, bromohydroquinone, 2-methylhydroquinone, tert-butylhydroquinone, phenylhydroquinone, 2,6-dimethylhydroquinone, 2,5-di-tert-butylhydroquinone, 2,5-di-tert-amylhydroquinone, trimethylhydroquinone, tetramethylhydroquinone, Examples of the phenolic compounds include non, resorcinol, 2-methylresorcinol, 5-methylresorcinol, 2-nitroresorcinol, 4-hexylresorcinol, 4-chlororesorcinol, 2-acetylresorcinol, 5-acetylresorcinol, 4,6-dichlororesorcinol, 2,5-di-tert-butylresorcinol, pyrogallol, phloroglucinol, 1,2,4-benzenetriol, gallic acid, methyl gallate, ethyl gallate, propyl gallate, isobutyl gallate, butyl gallate, isoamyl gallate, n-octyl gallate, dodecyl gallate, hexadecyl gallate, and stearyl gallate. From the same viewpoint, it is most preferable that one aromatic ring has three phenolic hydroxyl groups, and specific examples thereof include pyrogallol, gallic acid, and ethyl gallate.
[0023] <(C) Filler> The (C) filler is a filler made of an inorganic substance and / or an organic substance. The (C) filler may be used alone or in combination of two or more types. The inclusion of the (C) filler can adjust the viscosity and improve the thixotropy of the encapsulant composition. The adhesion to the substrate is improved by the physical interaction between the resin component and the substrate, but the addition of the filler tends to inhibit the physical interaction between the resin component and the substrate, and the adhesion tends to decrease. On the other hand, the combination of the (C) filler and (B) polyphenol having two or more phenolic hydroxyl groups increases the compatibility of the resin component and the filler, improves the compatibility of the resin with the surface of the (C) filler, and allows the viscosity and thixotropy to be adjusted without impairing the adhesion of the encapsulant resin composition to the substrate.
[0024] Specific examples of the filler (C) made of an inorganic substance include silica, silicon carbide, calcium carbonate, magnesium carbonate, alumina, titania, calcium oxide, magnesium oxide, magnesium hydroxide, and aluminum hydroxide. Among these, silica is preferred because it interacts with polyphenols, does not impair the barrier properties of the sealing material, and can improve leveling properties during printing while maintaining the performance of suppressing an increase in moisture permeability even when exposed to a severe wet heat test. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. Commercially available silicas include "SO-C1" and "SO-C2" manufactured by Admatechs Co., Ltd., and "AEROSIL 200", "AEROSIL 300", "AEROSIL 380", and "AEROSIL RX-200" manufactured by Nippon Aerosil Co., Ltd.
[0025] Among fillers made of inorganic and / or organic substances, fillers (C) made of organic substances are more preferred from the viewpoint of storage stability at room temperature, and specific examples include acrylic particles, urethane particles, styrene particles, melamine particles, acrylic-styrene particles, etc. Among these, acrylic particles and urethane particles are preferred from the viewpoint of improving leveling properties during printing while maintaining the flexibility of the encapsulant resin composition and the interaction with polyphenols in the substrate, not impairing the barrier properties of the encapsulant, and maintaining the performance of suppressing an increase in moisture permeability even when exposed to a severe moist heat test.
[0026] (C) The shape of the filler is not particularly specified, but is preferably spherical. The average particle size is preferably 30 μm or less from the viewpoint of not reducing the leveling property during printing. More preferably, it is 15 μm or less. The average particle size can be measured using a commercially available laser diffraction type particle size distribution measuring device such as Microtrac MT-3300II manufactured by Microtrac Bell. Specifically, 0.1 to 0.5 g of filler and 30 g of PMA (propylene glycol monomethyl ether acetate) were weighed in a beaker and pre-dispersed with an ultrasonic disperser, and the particle size was measured using the sample. The ultrasonic dispersion used for pre-dispersion is preferably performed under constant conditions, and the ultrasonic disperser US-300T (manufactured by Nippon Seiki Seisakusho Co., Ltd.) was used as the ultrasonic disperser, and the pre-dispersion was performed under constant conditions for 60 seconds at a current value of 300 μA. In addition, the laser diffraction type particle size distribution measuring device used was the above-mentioned Microtrac MT-3300II. The sample preparation and measurement were carried out within 5 minutes, and the value at 50% of the cumulative average diameter displayed as the measurement result was taken as the average particle diameter.
[0027] <(D) Curable compound> The (D) curable compound is not particularly limited as long as it is a compound that is cured by light, heat, or the like, but is preferably a (meth)acrylate compound, a (meth)allyl compound, or an epoxy compound. Examples of the (meth)acrylate compound include urethane (meth)acrylate, ester (meth)acrylate, and epoxy (meth)acrylate. Examples of the (meth)allyl compound include polyfunctional (meth)allyl compounds. Examples of the epoxy compound include epoxy resins.
[0028] [Urethane (meth)acrylate] The urethane (meth)acrylate is obtained by reacting a polyisocyanate compound with a polyol compound and a (meth)acrylate compound having a hydroxyl group, or a polyisocyanate compound with a (meth)acrylate compound having a hydroxyl group, by a known method. The urethane (meth)acrylate can be used alone or in combination of two or more types. The urethane group contained in such a compound can exhibit strong interactions such as hydrogen bonds between the urethane groups and with other polar groups. In addition, since the above-mentioned hydrogen bonds are more flexible than covalent bonds, the cured product of the encapsulant resin composition can maintain its flexibility. The urethane (meth)acrylate is not particularly limited as long as it has a urethane bond in the molecule, but is preferably a compound having 2 to 3 (meth)acrylic groups. By having the number of (meth)acrylic groups in this range, the cured product of the encapsulant resin composition can have high flexibility and high adhesion to the substrate.
[0029] The polyisocyanate compound may be a known compound. Examples of the polyisocyanate compound include aliphatic polyisocyanates, alicyclic polyisocyanates, and aromatic polyisocyanates. More specifically, examples of the polyisocyanate compound include aliphatic polyisocyanates such as pentamethylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate polyisocyanate, alicyclic polyisocyanates such as isophorone diisocyanate, hydrogenated diphenyl diisocyanate, and norbornene diisocyanate, aromatic polyisocyanates such as xylylene diisocyanate, tolylene diisocyanate, and diphenylmethane diisocyanate, and isocyanuric skeleton-containing triisocyanates, which are trimers of diisocyanates. Among these, divalent diisocyanate compounds are preferred from the viewpoint of high flexibility of the cured product of the resin composition for sealing material and excellent adhesion to the substrate.
[0030] The polyol compound may be a known compound. Specific examples include polyester polyol, polyether polyol, polycarbonate polyol, and polyols made of hydrocarbons. From the viewpoint of flexibility of the urethane (meth)acrylate compound obtained after the reaction, the polyol compound is preferably a divalent diol compound.
[0031] The polyester polyol may be a compound obtained by condensation reaction of a dicarboxylic acid compound and a polyol compound. In addition, a polyester polyol may be obtained by ring-opening addition polymerization of a cyclic ester to a dihydroxycarboxylic acid in the presence of a basic compound. Specific examples of the dicarboxylic acid compound include succinic acid, adipic acid, pimelic acid, and sebacic acid. Among them, adipic acid and pimelic acid are preferred. In addition, examples of the polyol compound include a diol compound and a triol compound. Specific examples of the diol compound include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, diethylene glycol, and dipropylene glycol. Specific examples of the triol compound include glycerin, 1,2,4-butanetriol, and trimethylolpropane. Among these, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, and glycerin are preferred from the viewpoint of adhesion to the substrate.
[0032] The cyclic esters may usually be composed of lactones. Specifically, lactones (or cyclic monoesters) are preferably lactones having 3 to 20 carbon atoms, such as β-propiolactone, β-butyrolactone, γ-butyrolactone, δ-valerolactone, δ-caprolactone, ε-caprolactone, γ-valerolactone, γ-caprolactone, γ-caprylolactone, γ-laurolactone, enantholactone, dodecanolactone, stearolactone, and alkyl-ε-caprolactone, and more preferably lactones having 4 to 15 carbon atoms.
[0033] The polyether polyol may be a known compound.Specific examples of the polyether polyol include diol compounds such as polyethylene glycol, polypropylene glycol, polybutylene glycol, and polytetramethylene glycol, and triol compounds such as polyoxypropylene triol and polyoxyethylene polyoxypropylene triol.Among these, polyethylene glycol, polypropylene glycol, and polyoxypropylene triol are preferred.
[0034] The polycarbonate polyol may be a compound obtained by transesterification of a carbonic acid diester and a polyol compound. Specific examples of carbonic acid diester include diphenyl carbonate, dimethyl carbonate, and diethylene carbonate. Among them, diethylene carbonate is preferred. Examples of polyol compounds include diol compounds and triol compounds. Specific examples of diol compounds include ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, diethylene glycol, and dipropylene glycol. Specific examples of triol compounds include glycerin, 1,2,4-butanetriol, and trimethylolpropane. Among these, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, and glycerin are preferred.
[0035] The polyol made of hydrocarbon may be a known compound.Specific examples of the polyol made of hydrocarbon include diol compounds such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, and 1,8-octanediol, and triol compounds such as glycerin, 1,2,4-butanetriol, and trimethylolpropane.Among these, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, and glycerin are preferred.
[0036] The (meth)acrylate compound having a hydroxyl group can be a known compound. Specifically, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxycyclohexyl (meth)acrylate, 5-hydroxycyclooctyl (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, propylene glycol monoacrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polycaprolactone mono(meth)acrylate, etc. can be used. Among them, 2-hydroxyethyl (meth)acrylate, propylene glycol mono(meth)acrylate, and polycaprolactone mono(meth)acrylate are preferred from the viewpoint of increasing the barrier properties of the cured product of the resin composition for sealing material.
[0037] The weight average molecular weight of the urethane (meth)acrylate compound is preferably 1,600 or more, more preferably 2,000 or more, from the viewpoint of maintaining the adhesion of the encapsulant to the substrate. Also, from the viewpoint of suppressing the decrease in barrier properties, it is preferably 20,000 or less, more preferably 12,500 or less. That is, in order to obtain excellent adhesion to the substrate of the cured product of the encapsulant resin composition and excellent barrier properties, the weight average molecular weight of the urethane (meth)acrylate compound is preferably 1,600 to 20,000, more preferably 2,000 to 12,500. The weight average molecular weight of the urethane (meth)acrylate compound is determined by gel permeation chromatography (GPC) using a calibration curve of standard polystyrene.
[0038] [Ester (meth)acrylate] The ester (meth)acrylate can be obtained by a known method by reacting an alcohol with (meth)acrylic acid. The ester (meth)acrylate can be used alone or in combination of two or more. Specific examples of the ester (meth)acrylate include N-acryloyloxyethylhexahydrophthalimide, acryloylmorpholine, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, cyclohexane-1,4-dimethanol mono(meth)acrylate, tetrahydrofurfuryl (meth)acrylate, phenoxyethyl (meth)acrylate, phenylpolyethoxy (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, methyl ethyl acrylate, ethyl ... (meth)acrylate, o-phenylphenol monoethoxy (meth)acrylate, o-phenylphenol polyethoxy (meth)acrylate, p-cumylphenoxyethyl (meth)acrylate, isobornyl (meth)acrylate, tribromophenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, 1,4-butanediol di(meth)acrylate, Examples of monomers include 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, tricyclodecane dimethanol (meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tris(acryloxyethyl)isocyanurate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, tripentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ester diacrylate of neopentyl glycol and hydroxypivalic acid, and diacrylate of an ε-caprolactone adduct of an ester of neopentyl glycol and hydroxypivalic acid.
[0039] [Epoxy (meth)acrylate] Epoxy (meth)acrylate is obtained by a known method by reacting epoxy resin with (meth)acrylic acid. The epoxy resin as a raw material is not particularly limited, but is a bifunctional or higher epoxy resin, specifically, resorcinol diglycidyl ether, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, bisphenol F novolac type epoxy resin, alicyclic epoxy resin, aliphatic chain epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, hydantoin type epoxy resin, isocyanurate type epoxy resin, phenol novolac type epoxy resin having a triphenolmethane skeleton, and other diglycidyl ethers of bifunctional phenols such as catechol and resorcinol, diglycidyl ethers of bifunctional alcohols, and their halides and hydrogenated products.
[0040] [Polyfunctional (meth)allyl compounds] The polyfunctional (meth)allyl compound has two or more (meth)allyl groups. The polyfunctional (meth)allyl compound can be used alone or in combination of two or more. By containing the polyfunctional (meth)allyl compound, the crosslinked network of the cured product of the resin composition for sealing material is excellent, so that the barrier property of the sealing material is excellent, and the increase in moisture permeability can be suppressed even when exposed to a severe moist heat test.
[0041] Specific examples of the polyfunctional (meth)allyl compound include 1,4-cyclohexanedicarboxylic acid di(meth)allyl ester, isophthalic acid di(meth)allyl ester, phthalic acid di(meth)allyl ester, hexahydrophthalic acid di(meth)allyl ester, di(meth)allyl methylglycidyl isocyanurate, magnolol, di(meth)allyl diphenyl silane, trimethylolpropane di(meth)allyl ether, 2,2'-bis(3-(meth)allyl-4-hydroxyphenyl)propane, 2,2-bis(3-(meth)allyl-4-allyloxyphenyl)propane, 2,2-bis(3 -(meth)allyl-4-glycidyloxyphenyl)propane, 1,3-di(meth)allyl-5-glycidyl isocyanurate, 1,3-di(meth)allyl cyanurate, triallyl isocyanurate, pentaerythritol tri(meth)allyl ether, glycerin tri(meth)allyl ether, trimethylolpropane triallyl ether, 1,3,4,6 tetra(meth)allyl glycoluril, 1,3,4,6 tetra(meth)allyl-3a-methyl glycoluril, pentaerythritol tetra(meth)allyl ether, and tetra(meth)allyloxyethane.
[0042] Among the polyfunctional (meth)allyl compounds, from the viewpoints of preventing coloration of the encapsulant for electronic components, providing excellent barrier properties for the encapsulant, suppressing an increase in moisture permeability even when exposed to a severe wet heat test, and further increasing the toughness of the cured product of the encapsulant resin composition and increasing adhesion to the substrate, (meth)allyl compounds having an isocyanurate skeleton, (meth)allyl compounds having a pentaerythritol skeleton, etc. are preferred. Specifically, 1,3-diallyl-5-glycidyl isocyanurate, triallyl isocyanurate, pentaerythritol triallyl ether, and pentaerythritol tetraallyl ether are preferred.
[0043] [Epoxy resin] The epoxy resin has two or more epoxy groups. The epoxy resin can be used alone or in combination of two or more. Specific examples of the epoxy resin include resorcinol diglycidyl ether, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, bisphenol F novolac type epoxy resin, alicyclic epoxy resin, aliphatic chain epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, hydantoin type epoxy resin, isocyanurate type epoxy resin, phenol novolac type epoxy resin having a triphenolmethane skeleton, and other diglycidyl etherified products of bifunctional phenols such as catechol and resorcinol, diglycidyl etherified products of bifunctional alcohols, and their halides and hydrogenated products.
[0044] <(E) Photopolymerization initiator> The (E) photopolymerization initiator is added to promote the light-induced curing reaction of the above (A) and (D), and can reduce the light irradiation required for curing the encapsulant resin composition. The (E) photopolymerization initiator can be used alone or in combination of two or more. Examples of the photopolymerization initiator include a photoradical polymerization initiator, a photocationic polymerization initiator, and a photoanionic polymerization initiator. The photoradical polymerization initiator is preferably used to shorten the reaction time, the photocationic polymerization initiator is preferably used to improve the adhesive strength, and the photoanionic polymerization initiator is preferably used to impart water resistance.
[0045] Specifically, the photoradical polymerization initiator may be 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one, 2-methyl -1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyloxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3yl]ethanone-1-(O-acetyloxime), and the like.
[0046] Specific examples of the photocationic polymerization initiator include bis(4-tert-butylphenyl)iodonium hexafluorophosphate, bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate, cyclopropyldiphenylsulfonium tetrafluoroborate, diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroarsenate, 2-(3,4-dimethoxystyryl)-4,6-bis(trichloromethyl)-1,3,5-triazine, triphenylsulfonium tetrafluoroborate, triphenylsulfonium bromide, tri-p-tolylsulfonium hexafluorophosphate, and tri-p-tolylsulfonium trifluoromethanesulfonate.
[0047] Specific examples of the photoanionic polymerization initiator include acetophenone o-benzoyloxime, nifedipine, 2-(9-oxoxanthen-2-yl)propionic acid 1,5,7-triazabicyclo[4,4,0]dec-5-ene, 2-nitrophenylmethyl 4-methacryloyloxypiperidine-1-carboxylate, 1,2-diisopropyl-3-[bis(dimethylamino)methylene]guanidinium 2-(3-benzoylphenyl)propionate, and 1,2-dicyclohexyl-4,4,5,5-tetramethylbiguanidinium n-butyltriphenylborate.
[0048] <Other ingredients> The resin composition for encapsulant of the present invention may contain additives such as a surfactant, a silane coupling agent, a curing accelerator, an ultraviolet absorber, a light stabilizer, an antioxidant, a polymerization inhibitor, a leveling agent, an adhesion imparting agent, a plasticizer, an antifoaming agent, a light shielding material, a conductive material, and a spacer, as long as the additives do not impair the object of the present invention.
[0049] <Composition ratio> From the viewpoints of improving the storage stability at room temperature and the barrier properties of the sealing material for electronic components, and suppressing an increase in moisture permeability even when exposed to a severe moist heat test, the molar mass concentration of the polyphenol having two or more phenolic hydroxyl groups (B) in the sealing material resin composition of the present invention is preferably 0.01 to 40 (mmol / 100 g), and more preferably 0.08 to 23 (mmol / 100 g), relative to the total of (A), (B), and (D) (the molar mass concentration of (B) (mmol / 100 g)=parts by mass (g) of (B) / molecular weight (g / mmol) of (B) / parts by mass (g) of (A), (B), and (D)×100).
[0050] The content of the filler (C) in the resin composition for encapsulant of the present invention is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 90 parts by mass or less, relative to 100 parts by mass of the total of (A) and (D), from the viewpoint of improving adhesion to a substrate. The content of the filler (C) is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, relative to 100 parts by mass of the total of (A) and (D), from the viewpoint of improving the barrier property of the encapsulant and suppressing an increase in moisture permeability even when exposed to a severe moist heat test.
[0051] In order for the resin composition for encapsulating material of the present invention to have high adhesion to a substrate and to exhibit excellent barrier properties, the ratio of the amount of thiol groups in (A) the polyfunctional thiol having 2 to 6 thiol groups to the amount of functional groups in (D) the curable compound (amount of thiol groups / amount of functional groups in the curable compound) is preferably 0.5 to 5.0, and more preferably 0.7 to 3.0.
[0052] In the solid content of the resin composition for encapsulating material, the total proportion of (A) the polyfunctional thiol having 2 to 6 thiol groups, (B) the polyphenol having two or more phenolic hydroxyl groups, (C) the filler, and (D) the curable compound is preferably 70 mass% or more, more preferably 80 mass% or more, and even more preferably 90 mass% or more.
[0053] In the case where a (E) photopolymerization initiator is used, the total proportion of the (A) polyfunctional thiol having 2 to 6 thiol groups, the (B) polyphenol having two or more phenolic hydroxyl groups, the (C) filler, the (D) curable compound, and the (E) photopolymerization initiator in the solid content of the resin composition for encapsulant is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, and even more preferably 95 mass% or more.
[0054] <Electronic components> The resin composition for encapsulation of the present invention can be used for a wide range of applications of electronic parts, and in particular, can be used for electronic parts applications such as encapsulation materials for printed wiring boards, encapsulation materials for build-up substrates, encapsulation materials for LEDs, encapsulation materials for solar cell substrates, and encapsulation materials for liquid crystal display devices.
[0055] <Electronic component formation> The electronic component of the present invention can be formed by applying the encapsulant resin composition of the present invention to a substrate and curing the encapsulant resin composition by light irradiation, or by applying the encapsulant resin composition of the present invention to one of two substrates, superimposing the substrates, and curing the encapsulant resin composition by light irradiation.
[0056] The method for applying the encapsulant resin composition is not particularly limited, and specifically, a dispenser coating method, an inkjet method, a screen printing method, a hand-coating method with a syringe or a brush, or the like can be applied.
[0057] The light source for irradiating the resin composition for an encapsulant with light is not particularly limited, and specifically, mercury lamps such as high-pressure mercury lamps and ultra-high-pressure mercury lamps, black light lamps, LED lamps, halogen lamps, electrodeless lamps, xenon lamps, mercury fluorescent lamps, LED fluorescent lamps, sunlight, electron beam irradiation devices, and the like can be used. EXAMPLES
[0058] Next, the present invention will be described more specifically with reference to examples and comparative examples.
[0059] <Evaluation method> The performance of the encapsulating resin composition in each of the Examples and Comparative Examples was evaluated by the following method.
[0060] <Storage stability at room temperature> Storage stability at room temperature was evaluated based on the increase in viscosity when the encapsulant resin composition was stored in a thermo-hygrostat at 25°C / 55%RH. The viscosity was measured using an RE80 viscometer (manufactured by Toki Sangyo Co., Ltd., cone rotor: 3°×R9.7) after rotating the encapsulant resin composition to be measured (0.25-0.50 mL) at a rotor speed of 1.0 rpm for 120 seconds (unit: Pa s). From the obtained results, the viscosity increase rate was calculated using the following formula. ((Viscosity after storage at 25°C) / (Initial viscosity when mixed)-1) x 100 = Viscosity increase rate (%) The number of days until the viscosity increase rate exceeds 30% from the initial viscosity was evaluated. Note that the longer the number of days until the viscosity increase rate exceeds 30% from the initial viscosity, the more excellent the storage stability at room temperature. ◎: 30 days or more 〇: 7 days or more ×: Less than 7 days
[0061] <Adhesion> The resin composition for encapsulation produced in the Examples and Comparative Examples was applied to one of two PET films (Cosmoshine A4300, manufactured by Toyobo Co., Ltd., thickness 100 μm, 25 mm × 100 mm) using a screen printer, and the other PET film was placed on top of it, leaving an overlap length of 10 mm (adhesion area 250 mm 2 The resin composition for sealing material sandwiched between two PET films was irradiated with a high-pressure mercury lamp (illuminance in i-line equivalent: 100 mW / cm 2 ) for 30 seconds (accumulated light quantity: 3000 mJ / cm 2 ) to cure the resin composition for encapsulation, thereby obtaining a test piece. The tensile shear strength of the obtained test piece was measured in accordance with JIS-K-6850 using a tensile tester (Autograph AG-IS manufactured by Shimadzu Corporation) (measurement environment: temperature 25°C, tensile speed: 5 mm / min). The tensile shear strength was calculated according to the following formula. (Formula): Tensile shear strength (N / mm 2 )=Maximum load (N) / Adhesive area (mm 2 ) ◎: 15N / mm 2 This completes the peeling process. ○: 10N / mm 2 More than 15N / mm 2 It peels off in less than ×:10N / mm 2 It peels off in less than
[0062] <Barrier properties> Regarding the barrier property, the encapsulant resin composition was applied to a polyimide film (trade name "Kapton 100H" manufactured by Toray DuPont Co., Ltd.) with an applicator to a thickness of 100 μm, and the encapsulant resin composition was then exposed to a high-pressure mercury lamp (illuminance in terms of i-line: 100 mW / cm 2 ) for 30 seconds (accumulated light quantity: 3000 mJ / cm 2 ) to obtain a hardened test piece. The moisture permeability of the obtained test piece was evaluated by a method based on JIS Z 0208 "Test method for moisture permeability of moisture-proof packaging material". The temperature and humidity conditions were 40°C / 90% RH. The evaluation criteria for barrier properties are as follows: ◎: 40g / m 2 ·24 hours or less ○: 40g / m 2 24h higher, 100g / m 2 ·24 hours or less ×:100g / m 2 Higher than 24 hours
[0063] <Synthesis of urethane (meth)acrylate compounds> (Production of diol compound (b-1): Raw material 1 of urethane (meth)acrylate compound (D-1)) In a reaction vessel equipped with a stirrer, a distillation column, a nitrogen inlet tube, and a thermometer, 150.2 parts by mass of adipic acid and 161.3 parts by mass of 3-methyl-1,5-pentanediol were charged, and the mixture was heated to 140°C under a nitrogen atmosphere and stirred. 0.01 parts by mass of tetrabutyl titanate was charged, and the mixture was heated to 220°C to carry out a dehydration reaction. The mixture was then held at 220°C to carry out a dehydration reaction. 18 hours after the start of the dehydration reaction, the contents were cooled to obtain a diol compound (b-1) (weight average molecular weight: 1,600).
[0064] (Production of diol compound (b-2): Raw material 2 of urethane (meth)acrylate compound (D-2)) In a reaction vessel equipped with a stirrer, a distillation column, a nitrogen inlet tube, and a thermometer, 175 parts by mass of diethylene carbonate, 185 parts by mass of 1,6-hexanediol, and 0.01 parts by mass of tetraisopropyl titanate were charged, and the reaction was carried out while refluxing diethylene carbonate in a nitrogen atmosphere under normal pressure and distilling off the generated ethanol together with diethylene carbonate. The temperature was gradually raised from the point where the distillation of the generated ethanol decreased, and when it reached 200°C and the distillation of ethanol stopped, it was allowed to cool. The pressure was reduced with a vacuum pump, and the excess diol component was distilled off while heating again to obtain diol compound (b-2) (weight average molecular weight: 2,100).
[0065] (Production of diol compound (b-3): Raw material 3 of urethane (meth)acrylate compound (D-3)) In a reaction vessel equipped with a stirrer, a distillation column, a nitrogen inlet tube, and a thermometer, 144.3 parts by mass of adipic acid and 202.1 parts by mass of 1,6-hexanediol were charged, and the mixture was heated to 140°C under a nitrogen atmosphere and stirred. 0.01 parts by mass of tetrabutyl titanate was charged, and the mixture was heated to 220°C to carry out a dehydration reaction. The mixture was then held at 220°C to carry out a dehydration reaction. Six hours after the start of the dehydration reaction, the contents were cooled to obtain a diol compound (b-3) (weight average molecular weight: 1,000).
[0066] (Production of diol compound (b-4): Raw material 4 of urethane (meth)acrylate compound (D-4)) In a reaction vessel equipped with a stirrer, a distillation column, a nitrogen inlet tube, and a thermometer, 158.5 parts by mass of pimelic acid and 202.1 parts by mass of 3-methyl-1,5-pentanediol were charged, and the mixture was heated to 140°C under a nitrogen atmosphere and stirred. 0.01 parts by mass of tetrabutyl titanate was charged, and the mixture was heated to 220°C to carry out a dehydration reaction. The mixture was then held at 220°C to carry out a dehydration reaction. 18 hours after the start of the dehydration reaction, the contents were cooled to obtain a diol compound (b-4) (weight average molecular weight: 1,750).
[0067] (Production of urethane (meth)acrylate compound (D-1)) A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 160.3 parts by mass of the diol compound (b-1) obtained above, and stirring was started. Next, 0.1 parts by mass of dibutyltin laurate and 44.5 parts by mass of 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate as a polyisocyanate compound were added, and the internal temperature was raised to 80°C while paying attention to heat generation, and then the temperature was maintained while stirring for 3 hours. Furthermore, 0.1 parts by mass of methoquinone as a polymerization inhibitor and 23.2 parts by mass of 2-hydroxyethyl acrylate as a (meth)acrylate compound were added, and the mixture was stirred at 85°C for 2 hours to obtain a urethane (meth)acrylate compound (D-1) (weight average molecular weight: 6,500, number of functional groups: 2).
[0068] Urethane (meth)acrylate compounds (D-2) to (D-5) were obtained in the same manner as above, except that the diol compound, polyisocyanate compound, and acrylate compound in Table 1 were used.
[0069] (Production of urethane (meth)acrylate compound (D-6)) A reaction vessel equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, and a thermometer was charged with 51.6 parts by mass of "Placcel FA2D" (manufactured by Daicel Chemical Industries, polycaprolactone modified hydroxyethyl acrylate) as a (meth)acrylate compound, and stirring was started. Next, 0.1 parts by mass of dibutyltin laurate, 53.8 parts by mass of "Duranate TPA-100" (manufactured by Asahi Kasei Corporation, NCO = 23.1%) as a polyisocyanate compound, and 0.1 parts by mass of methoquinone as a polymerization inhibitor were added, and the internal temperature was raised to 80 ° C. while paying attention to heat generation, and then the mixture was stirred for 3 hours while maintaining the temperature to obtain a urethane (meth)acrylate compound (D-6) (weight average molecular weight: 3,000, number of functional groups: 3).
[0070] [Table 1]
[0071] The materials used are listed below. (A-1) Multifunctional thiol: dipentaerythritol hexakis(3-mercaptopropionate) (Tokyo Chemical Industry Co., Ltd.) (A-2) Multifunctional thiol: pentaerythritol tetrakis(3-mercaptopropionate) (Tokyo Chemical Industry Co., Ltd.) (A-3) Multifunctional thiol: Tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate (Tokyo Chemical Industry Co., Ltd.) (A-4) Multifunctional thiol: Ethylene glycol bis(3-mercaptopropionate) (Tokyo Chemical Industry Co., Ltd.) (B-1) Polyphenol: Pyrogallol (Tokyo Chemical Industry Co., Ltd.) (B-2) Polyphenol: Catechol (Tokyo Chemical Industry Co., Ltd.) (B-3) Polyphenol: Gallic acid (Tokyo Chemical Industry Co., Ltd.) (B-4) Polyphenol: Ethyl gallate (Tokyo Chemical Industry Co., Ltd.) (B-5) Monofunctional phenol: 4-methoxyphenol (manufactured by Wako Pure Chemical Industries, Ltd.) (B-6) Triphenyl phosphite (Tokyo Chemical Industry Co., Ltd.) (C-1) Filler: J4P [average particle size: 2.2 μm] (acrylic particles manufactured by Negami Chemical Industries, Ltd.) (C-2) Filler: FH-S008 [average particle size: 8 μm] (acrylic particles manufactured by Nippon Exlan Kogyo Co., Ltd.) (C-3) Filler: SO-C1 [average particle size: 0.3 μm] (silica particles manufactured by Admatechs Co., Ltd.) (C-4) Filler: AEROSIL RX-200 [average particle size: 0.012 μm] (silica particles manufactured by Nippon Aerosil Co., Ltd.) (C-5) Filler: P-400T [average particle size: 15 μm] (urethane particles manufactured by Negami Chemical Industries, Ltd.) (C-6) Filler: C-600T [average particle size: 10 μm] (urethane particles manufactured by Negami Chemical Industries, Ltd.) (D-7) Curable compound: Triallyl isocyanurate (manufactured by Tokyo Chemical Industry Co., Ltd.) (E) Photopolymerization initiator: 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide
[0072] <Examples 1-26 and Comparative Examples 1-4> The above components were added to a planetary mixer in the amounts shown in Table 2-4 below and mixed for 2 hours to obtain a curable resin composition. The above evaluations were carried out using each of the obtained curable resins. The results are shown in Table 2-4.
[0073] [Table 2]
[0074] [Table 3]
[0075] [Table 4]
[0076] As a result of the above tests, the encapsulating resin composition of each Example, containing the components (A) to (D), had high storage stability at room temperature in an uncured state, and had high adhesion and excellent barrier properties after curing.
[0077] On the other hand, in Comparative Example 1, a monofunctional phenol compound that is not the component (B) of the present invention was used, and therefore the cured product of the encapsulant resin composition had poor barrier properties.
[0078] In Comparative Example 2, a compound was used for the purpose of improving storage stability, and did not contain a phenolic hydroxyl group. Therefore, in the uncured state, the storage stability was reduced at room temperature, and the cured product of the encapsulant resin composition had poor adhesion to substrates and poor barrier properties.
[0079] In Comparative Example 3, since the component (C) was not contained, the barrier property of the encapsulant resin composition after curing was reduced.
[0080] In Comparative Example 4, since the component (A) was not contained, the cured product of the encapsulant resin composition had poor adhesion to the substrate.
Claims
1. The resin composition for use as a sealant for electronic components contains (A) a polyfunctional thiol having 2 to 6 thiol groups, (B) a polyphenol having two or more phenolic hydroxyl groups, (C) a filler, and (D) a curable compound.
2. An electronic component encapsulated with the encapsulant resin composition according to claim 1.
Citation Information
Patent Citations
Resin composition
JP2014077024A
Photocurable composition
JP2022072999A