Packaging bag

The packaging bag design with a 300 μm or less welded part and polyamide layers addresses the bulkiness issue in stacked bags, ensuring ease of handling and maintaining freshness.

JP2024140575APending Publication Date: 2024-10-10SUMITOMO BAKELITE CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023051766
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Packaging bags become bulky when stacked due to the thickness of the overlapped end portions, which is a common issue in existing packaging solutions.

Method used

A packaging bag design featuring a welded part with a width of 300 μm or less, utilizing a resin film containing polyamide and an anti-blocking agent, with specific color and carbide piece characteristics, and a laminated structure that includes polyamide layers to prevent bulkiness.

Benefits of technology

The design ensures that multiple packaging bags can be stacked without the overlapped end portions becoming bulky, with improved visibility, ease of handling, and no pinholes, while maintaining freshness and transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140575000001_ABST
    Figure 2024140575000001_ABST
Patent Text Reader

Abstract

To provide a packaging bag in which a part where ends of a plurality of packaging bags are overlapped is not bulky.SOLUTION: A packaging bag has a weld part obtained by melting and cutting resin films, wherein the resin film contains polyamide, and the width of the weld part of the packaging bag is 300 μm or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging bag. [Background technology]

[0002] Various preservation packages are used to contain and preserve objects. For example, when the object to be preserved is something that is ingested orally, such as food, it is required to preserve the object while maintaining good quality, and a package for achieving this purpose has been disclosed (see Patent Document 1).

[0003] For example, packaging materials used for packaging root vegetables such as potatoes are required to have oxygen barrier properties that prevent oxygen from passing through in order to guarantee the quality of the food, such as its taste and freshness.

[0004] Furthermore, when contents are stored in a packaging bag, the moisture in the contents can cause fogging or condensation inside the packaging bag, which can impair the appearance. For example, a packaging bag for fruits and vegetables is described in Patent Document 2. Patent Document 2 describes a multilayer film using a thermoplastic resin porous membrane layer having fine pores, and discloses that anti-fogging properties are imparted to the surface of the multilayer film.

[0005] A packaging bag is generally produced, for example, by laminating the end faces of resin films together by heat to form a bag. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 9-252718 [Patent Document 2] JP 2005-144830 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, when the end faces of the resin films are bonded together by heat, there is a problem that when a plurality of packaging bags are stacked, the overlapped portions of the ends become thicker and bulkier.

[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a packaging bag in which the overlapping ends do not become bulky even when a plurality of packaging bags are stacked together. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention employs the following configuration. [1] A packaging bag having a welded part obtained by fusing together a resin film, the resin film containing polyamide, and the width of the welded part of the packaging bag being 300 μm or less. [2].The welded portion is made of CIE1976L * a * b * In the coordinate system specified by the color system, lightness L * is between -25 and -17, and the chromaticity a * is between -1 and 1, and chromaticity b * The packaging bag according to [1], wherein the elastic modulus is 8.5 or more and 10.5 or less. [3] The packaging bag described in [1] or [2], wherein the welded portion has carbonized pieces of the resin film, and the size of the carbonized pieces is 50 μm or more and 1000 μm or less. [4] The packaging bag according to any one of [1] to [3], wherein the resin film further contains an antiblocking agent in addition to the polyamide, and the antiblocking agent is present in the resin film in areas on both surface sides of the resin film. [5]. The packaging bag according to any one of [1] to [4], wherein the resin film is a laminated film, the laminated film being configured by laminating an inner layer, an intermediate layer, and an outer layer in this order in the thickness direction, the inner layer and the outer layer containing polyamide and an antiblocking agent, and the intermediate layer containing polyamide. [6] The packaging bag according to any one of [1] to [5], wherein the polyamide is an unstretched polyamide. [7] The packaging bag according to any one of [1] to [6], wherein the polyamide is one or more selected from the group consisting of 6-nylon, 66-nylon, and a copolymer of 6-nylon and 66-nylon. [8] The packaging bag described in [5], wherein the coefficient of dynamic friction between the inner layers is 0.3 or more and 0.5 or less. [9] The packaging bag described in [5], wherein the coefficient of dynamic friction between the outer layers is 0.3 or more and 0.5 or less.

[10] The packaging bag according to any one of [1] to [9], wherein the resin film has a thickness of 20 μm or more. Effect of the Invention

[0010] According to the present invention, a packaging bag is provided in which the overlapping ends do not become bulky even when a plurality of packaging bags are stacked. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing a schematic example of a resin film constituting a packaging bag according to one embodiment of the present invention. [Diagram 2] 4 is a cross-sectional view showing a schematic diagram of another example of a resin film constituting a packaging bag according to one embodiment of the present invention. FIG. [Diagram 3] 1 is a cross-sectional view showing a schematic example of a packaging bag according to one embodiment of the present invention. [Figure 4] 1A to 1C are diagrams showing an example of a method for identifying a welded portion of a packaging bag according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] <<Resin film>> A packaging bag according to one embodiment of the present invention has a welded portion obtained by fusing together a resin film, the resin film containing polyamide, and the width of the welded portion of the packaging bag is 300 μm or less. The resin film may further contain an antiblocking agent in addition to the polyamide. It is preferable that the antiblocking agent is present in the regions on both surfaces of the resin film. The resin film may be a laminated film. The laminated film may be configured by laminating an inner layer, an intermediate layer, and an outer layer in this order in the thickness direction. The inner layer and the outer layer preferably contain polyamide and an antiblocking agent, and the intermediate layer preferably contains polyamide.

[0013] The present invention will be described in detail below with reference to the drawings. Note that the drawings used in the following description may show essential parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality.

[0014] FIG. 1 is a cross-sectional view that illustrates an example of a resin film that constitutes the packaging bag of the present embodiment.

[0015] The resin film 1 preferably has transparency.

[0016] The resin film 1 contains polyamide. By containing polyamide in the resin film 1, the oxygen barrier property and antifogging property of the resin film 1 can be improved, and the resin film 1 can be produced at low cost. In addition, since polyamide has high transparency, the transparency of the resin film 1 can be improved.

[0017] The polyamide is preferably unstretched polyamide. When the resin film 1 contains unstretched polyamide, it is possible to further improve the bag-breaking resistance of the resin film 1. In addition, since unstretched polyamide has low rigidity, in a packaging bag formed using the resin film 1, unwinding of the back seal portion is further suppressed. The resin film 1 preferably contains a polyamide that does not have an aromatic ring (sometimes referred to as a "non-aromatic polyamide" in this specification).

[0018] Examples of the polyamides not having an aromatic ring (non-aromatic polyamides) include polyamides obtained by polymerizing or copolymerizing nylon salts obtained by reacting cyclic lactams (lactams having 3 or more ring members), amino acids, or diamines with dicarboxylic acids.

[0019] Examples of the cyclic lactam include ε-caprolactam, ω-enantholactam, ω-laurolactam, α-pyrrolidone, and α-piperidone.

[0020] Examples of the amino acid include 6-aminocaproic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid.

[0021] Examples of the diamine that forms the nylon salt include aliphatic amines such as tetramethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2,2,4-trimethylhexamethylenediamine, and 2,4,4-trimethylhexamethylenediamine; Examples of the diamine include alicyclic diamines such as 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, isophoronediamine, piperazine, bis(4-aminocyclohexyl)methane, and 2,2-bis-(4-aminocyclohexyl)propane.

[0022] Examples of the dicarboxylic acid that forms the nylon salt include aliphatic dicarboxylic acids such as glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sepatic acid, undecanedioic acid, and dodecanedioic acid; Examples of the alicyclic carboxylic acids include hexahydroterephthalic acid and hexahydroisophthalic acid.

[0023] More specifically, the polyamide may be, for example, 4-nylon, 6-nylon, 7-nylon, 11-nylon, 12-nylon, 46-nylon, 66-nylon, 69-nylon, 610-nylon, 611-nylon, 612-nylon, 6T-nylon, 6I nylon, a copolymer of 6-nylon and 66-nylon (nylon 6 / 66), a copolymer of 6-nylon and 610-nylon, a copolymer of 6-nylon and 611-nylon, a copolymer of 6-nylon and 12-nylon (nylon 6 / 12), or a copolymer of 6-nylon and 612 nylon. , copolymers of 6-nylon and 6T-nylon, copolymers of 6-nylon and 6I-nylon, copolymers of 6-nylon, 66-nylon and 610-nylon, copolymers of 6-nylon, 66-nylon and 12-nylon (nylon 6 / 66 / 12), copolymers of 6-nylon, 66-nylon and 612-nylon, copolymers of 66-nylon and 6T-nylon, copolymers of 66-nylon and 6I-nylon, copolymers of 6T-nylon and 6I-nylon, copolymers of 66-nylon, 6T-nylon and 6I-nylon, and copolymers of 66-nylon, 6T-nylon and 6I-nylon.

[0024] The resin film 1 may contain only one type of polyamide, or two or more types. When two or more types are contained, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0025] In terms of heat resistance, mechanical strength, availability, and the like, the polyamide is preferably one or more types selected from the group consisting of 6-nylon (sometimes abbreviated as "Ny6" in this specification), 12-nylon, 66-nylon, nylon 6 / 66, nylon 6 / 12, and nylon 6 / 66 / 12, more preferably one or more types selected from the group consisting of 6-nylon, 66-nylon, and nylon 6 / 66, and from the viewpoint of low cost, further preferably 6-nylon.

[0026] In addition to polyamide, the resin film 1 preferably contains an antiblocking agent. When the resin film 1 contains an antiblocking agent, opening failure and adhesion between bags of a package formed using the resin film 1 are further suppressed.

[0027] Examples of the antiblocking agent include natural silica, synthetic silica, silicates, etc. Examples of the shape of the antiblocking agent include spherical, elliptical, and other irregular shapes.

[0028] The average particle size of the antiblocking agent is preferably 0.5 to 20 μm, more preferably 0.6 to 19 μm, and even more preferably 2 to 10 μm. By setting the average particle size of the antiblocking agent to be equal to or greater than the lower limit, poor opening of the packaging body formed using the resin film 1 and adhesion between bags are further suppressed. By setting the average particle size of the antiblocking agent to be equal to or less than the upper limit, excessive use of the antiblocking agent is further suppressed.

[0029] In this specification, not only in the case of an antiblocking agent, but also unless otherwise specified, the "average particle size" means the particle size at 50% accumulation of particles (D50) when the particle size distribution of particles is measured on a volume basis by a laser diffraction particle size distribution measurement method.

[0030] The resin film 1 may contain only one type of antiblocking agent, or two or more types. When two or more types are contained, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0031] In the resin film 1, an antiblocking agent may be present in regions on both surface sides of the resin film 1. This further suppresses poor opening of the packaging body formed using the resin film 1 and adhesion between bags.

[0032] The antiblocking agent is preferably present in a region having a depth of up to 40% from both surfaces of the resin film 1, more preferably in a region having a depth of up to 30%, and even more preferably in a region having a depth of up to 20%, with respect to the thickness of the resin film 1. By having the antiblocking agent present in a region having a depth of up to the upper limit value from both surfaces of the resin film 1 with respect to the thickness of the resin film 1, poor opening of the mouth of a package formed using the resin film 1 and adhesion between bags are further suppressed.

[0033] In the resin film 1, the content of the antiblocking agent relative to the total mass of the resin film 1 is preferably 0.0016 to 0.32 mass %, more preferably 0.0048 to 0.16 mass %, and even more preferably 0.048 to 0.112 mass %. By setting the ratio to be equal to or more than the lower limit, it is possible to further suppress opening defects and adhesion between bags of a package formed using the resin film 1. By setting the ratio to be equal to or less than the upper limit, it is possible to further suppress excessive use of the antiblocking agent.

[0034] The resin film 1 may contain only polyamide and an antiblocking agent (i.e., it may consist of polyamide and an antiblocking agent), or it may contain polyamide, antiblocking agent, and other components (sometimes referred to as "other components" in this specification) (i.e., it may consist of polyamide, antiblocking agent, and the other components).

[0035] The other components contained in the resin film 1 are not particularly limited and can be arbitrarily selected depending on the purpose, and may be, for example, either a resin component or a non-resin component. The other component, which is a resin component, is a resin that does not fall into either the aromatic polyamide or the non-aromatic polyamide category (that is, a resin other than polyamide). The other component, which is a resin component, may be a homopolymer, which is a polymer of one type of monomer, or a copolymer, which is a polymer of two or more types of monomers.

[0036] Examples of the other components that are non-resin components include additives known in the art. Examples of the additives include antifogging agents, antioxidants, antistatic agents, crystal nucleating agents, inorganic particles, viscosity reducers, thickeners, heat stabilizers, lubricants, infrared absorbing agents, and ultraviolet absorbing agents.

[0037] The resin film 1 may contain only one type of other component, or two or more types. When there are two or more types, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0038] The ratio of the polyamide content (parts by mass) in the resin film 1 to the total mass (parts by mass) of the resin film 1 ([polyamide content (parts by mass) in the resin film 1)] / [total mass (parts by mass) of the resin film 1)]×100) is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be, for example, any one of 97% by mass or more and 99% by mass or more. When the ratio is equal to or more than the lower limit, the oxygen barrier property and anti-fogging property of the resin film 1 can be further improved, and the resin film 1 can be manufactured at a lower cost. In addition, the variation in thickness of the resin film 1 can be suppressed, and the effect of preventing wrinkles from occurring can be further improved. Furthermore, the transparency of the resin film 1 can be further improved. On the other hand, the proportion is 99% by mass or less. The above ratio is usually the same as the ratio of the polyamide content (parts by mass) to the total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming a resin film described below ([polyamide content (parts by mass) in the resin composition for forming a resin film)]) / [total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming a resin film)]×100).

[0039] The resin film 1 may be composed of one layer (single layer) or may be composed of two or more layers. When the resin film 1 is composed of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0040] The resin film 1 may have other layers as long as the effects of the present invention are not impaired. The other layers that the resin film 1 has are not particularly limited as long as they do not fall under the resin film of this embodiment, and may be, for example, a resin layer that contains a resin, or a non-resin layer that does not contain a resin.

[0041] In the packaging bag of this embodiment, the resin film is a laminated film, and the laminated film is constructed by laminating an inner layer, an intermediate layer, and an outer layer in this order in the thickness direction, and the inner layer and the outer layer contain polyamide and an antiblocking agent, and the intermediate layer may contain polyamide. An example of such a laminate film is a resin film 1 shown in FIG. 1 which is composed of three or more layers, both of whose outermost layers contain polyamide and an antiblocking agent, and one or more layers disposed between these outermost layers contain polyamide.

[0042] FIG. 2 is a cross-sectional view that illustrates a schematic diagram of another example of the resin film that constitutes the packaging bag of the present embodiment. In FIG. 2 and subsequent figures, the same components as those shown in the figures already described are given the same reference numerals as in the figures already described, and detailed description thereof will be omitted.

[0043] The laminated film 2 shown here is constructed by laminating an inner layer 11, an intermediate layer 12, and an outer layer 13 in this order in the thickness direction. Each layer will be described below.

[0044] <Inner layer> The inner layer 11 imparts oxygen barrier properties and anti-fogging properties to the laminated film 2, and as shown in FIG. 3, the inner layers 11, 11 are partially welded together to form a storage space S described below, thereby constituting a packaging bag. The inner layer 11 is one of the outermost layers of the laminated film 2, and is disposed on one of the outermost sides in the lamination direction of the layers constituting the laminated film 2.

[0045] The inner layer 11 is preferably transparent.

[0046] The inner layer 11 preferably comprises a polyamide and an antiblocking agent. The polyamide contained in the inner layer 11 may be the same as the polyamide contained in the resin film 1 described above. The antiblocking agent contained in the inner layer 11 may be the same as the antiblocking agent contained in the resin film 1 described above.

[0047] The antiblocking agent may be present uniformly or non-uniformly in the inner layer 11. When the antiblocking agent is present non-uniformly, it is preferable that the antiblocking agent is unevenly distributed in a region on the surface side of the inner layer 11 opposite to the intermediate layer 12.

[0048] In the inner layer 11, the content ratio of the antiblocking agent relative to the total mass of the inner layer 11 is preferably 0.01 to 2 mass%, more preferably 0.03 to 1 mass%, and even more preferably 0.3 to 0.7 mass%. By setting the ratio to be equal to or greater than the lower limit, opening defects of a package formed using the laminated film 2 are further suppressed. By setting the ratio to be equal to or less than the upper limit, excessive use of the antiblocking agent is further suppressed.

[0049] The inner layer 11 may contain only polyamide and an antiblocking agent (i.e., it may consist of polyamide and an antiblocking agent), or it may contain polyamide, antiblocking agent, and other components (sometimes referred to as "other components" in this specification) (i.e., it may consist of polyamide, antiblocking agent, and the other components).

[0050] Examples of the other components contained in the inner layer 11 include the same components as those contained in the resin film 1 described above.

[0051] The ratio of the polyamide content (parts by mass) in the inner layer 11 to the total mass (parts by mass) of the inner layer 11 ([polyamide content (parts by mass) in the inner layer 11)] / [total mass (parts by mass) of the inner layer 11]×100) is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be, for example, any one of 97% by mass or more and 99% by mass or more. When the ratio is equal to or more than the lower limit, the oxygen barrier property and antifogging property of the inner layer 11 can be further improved, and the laminated film 2 can be produced at a lower cost. In addition, the variation in thickness of the laminated film 2 can be suppressed, and the effect of preventing wrinkles from occurring can be further improved. Furthermore, the transparency of the laminated film 2 can be further improved. On the other hand, the proportion is 99% by mass or less. The above ratio is usually the same as the ratio of the polyamide content (parts by mass) to the total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming the inner layer described below ([polyamide content (parts by mass) in the resin composition for forming the inner layer)]) / [total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming the inner layer)]×100).

[0052] The inner layer 11 may be composed of one layer (single layer) or may be composed of two or more layers. When the inner layer 11 is composed of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0053] The thickness of the inner layer 11 can be set arbitrarily depending on the application of the laminated film 2, and is not particularly limited. The thickness of the inner layer 11 is preferably from 2 to 20 μm, more preferably from 3 to 15 μm, and further preferably from 4 to 12 μm. When the thickness of the inner layer 11 is equal to or greater than the lower limit, the effect obtained by providing the inner layer 11 is enhanced. When the thickness of the inner layer 11 is equal to or less than the upper limit, the thickness of the inner layer 11 is further prevented from becoming excessive. Furthermore, the thinner the thickness of the inner layer 11, the more transparent the packaging bag is, and the easier it is to visually confirm the contents from outside the packaging bag. When the inner layer 11 is made up of a plurality of layers, the total thickness of these layers is preferably within the above-mentioned numerical range.

[0054] The ratio of the thickness of the inner layer 11 to the total thickness of the laminate film 2 ([thickness of the inner layer 11] / [total thickness of the laminate film 2]×100) is not particularly limited, but is preferably 1 to 50%, more preferably 1 to 45%, and even more preferably 5 to 30%, and may be, for example, 10 to 15%. When the ratio is equal to or greater than the lower limit, the effect obtained by providing the inner layer 11 is enhanced. When the ratio is equal to or less than the upper limit, the thickness of the inner layer 11 is further prevented from becoming excessive. In addition, the thinner the inner layer 11, the more transparent the packaging bag is, and the easier it is to visually confirm the contents from the outside of the packaging bag. When the inner layer 11 is made up of a plurality of layers, the ratio of the total thickness of these layers to the entire thickness of the laminate film 2 is preferably within the above-mentioned numerical range.

[0055] <Middle Class> The intermediate layer 12 imparts oxygen barrier properties and anti-fogging properties to the laminated film 2. The intermediate layer 12 is disposed between the inner layer 11 and the outer layer 13 in the laminated film 2 .

[0056] The intermediate layer 12 is preferably transparent.

[0057] The intermediate layer 12 preferably comprises a polyamide. The polyamide contained in the intermediate layer 12 may be the same as the polyamide contained in the resin film 1 described above.

[0058] The polyamide contained in the intermediate layer 12 and the polyamide contained in the inner layer 11 may be the same as or different from each other.

[0059] The intermediate layer 12 may contain only polyamide (i.e., it may consist of polyamide), or it may contain polyamide and other components (sometimes referred to as "other components" in this specification) (i.e., it may consist of polyamide and the other components).

[0060] The other components contained in the intermediate layer 12 are not particularly limited and can be arbitrarily selected depending on the purpose, and may be, for example, either a resin component or a non-resin component. The other component, which is a resin component, is a resin that does not fall into either the aromatic polyamide or the non-aromatic polyamide category (that is, a resin other than polyamide). The other component, which is a resin component, may be a homopolymer, which is a polymer of one type of monomer, or a copolymer, which is a polymer of two or more types of monomers.

[0061] Examples of the other components that are non-resin components include additives known in the art. Examples of the additives include antifogging agents, antiblocking agents, antioxidants, antistatic agents, crystal nucleating agents, inorganic particles, viscosity reducers, thickeners, heat stabilizers, lubricants, infrared absorbing agents, and ultraviolet absorbing agents.

[0062] The intermediate layer 12 may contain only one type of other component, or two or more types. When there are two or more types, the combination and ratio thereof can be arbitrarily selected depending on the purpose.

[0063] The ratio of the polyamide content (parts by mass) in the intermediate layer 12 to the total mass (parts by mass) of the intermediate layer 12 ([polyamide content (parts by mass) in the intermediate layer 12)] / [total mass (parts by mass) of the intermediate layer 12]×100) is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be, for example, any one of 97% by mass or more and 99% by mass or more. When the ratio is equal to or more than the lower limit, the oxygen barrier property and anti-fogging property of the intermediate layer 12 can be further improved, and the laminate film 2 can be manufactured at a lower cost. In addition, the variation in thickness of the laminate film 2 can be suppressed, and the effect of preventing wrinkles from occurring can be further improved. Furthermore, the transparency of the laminate film 2 can be further improved. On the other hand, the proportion is 100% by mass or less. The above ratio is usually the same as the ratio of the polyamide content (parts by mass) to the total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming an intermediate layer described below ([polyamide content (parts by mass) in the resin composition for forming an intermediate layer)]) / [total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming an intermediate layer)]×100).

[0064] The intermediate layer 12 may be composed of one layer (single layer) or may be composed of two or more layers. When the intermediate layer 12 is composed of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0065] The thickness of the intermediate layer 12 can be set arbitrarily depending on the application of the laminated film 2, and is not particularly limited. The thickness of the intermediate layer 12 is preferably from 15 to 36 μm, more preferably from 18 to 24 μm, and further preferably from 20 to 27 μm. When the thickness of the intermediate layer 12 is equal to or greater than the lower limit, the effect obtained by providing the intermediate layer 12 is enhanced. When the thickness of the intermediate layer 12 is equal to or less than the upper limit, the thickness of the intermediate layer 12 is further prevented from becoming excessive. In addition, the thinner the thickness of the intermediate layer 12, the more transparent the packaging bag is, and the easier it is to visually confirm the contents from outside the packaging bag. When the intermediate layer 12 is made up of a plurality of layers, the total thickness of these layers is preferably within the above numerical range.

[0066] The ratio of the thickness of the intermediate layer 12 to the total thickness of the laminate film 2 ([thickness of intermediate layer 12] / [total thickness of laminate film 2]×100) is not particularly limited, but is preferably 50 to 90%, more preferably 55 to 85%, and even more preferably 60 to 80%, and may be, for example, 65 to 75%. When the ratio is equal to or greater than the lower limit, the effect obtained by providing the intermediate layer 12 is enhanced. When the ratio is equal to or less than the upper limit, the thickness of the intermediate layer 12 is further prevented from becoming excessive. In addition, the thinner the intermediate layer 12 is, the more transparent the packaging bag is, and the easier it is to visually confirm the contents from the outside of the packaging bag. When the intermediate layer 12 is made up of a plurality of layers, the ratio of the total thickness of these layers to the entire thickness of the laminate film 2 is preferably within the above-mentioned numerical range.

[0067] <Outer layer> The outer layer 13 is a layer that imparts oxygen barrier properties and anti-fogging properties to the laminated film 2, and also protects the layers constituting the laminated film 2 other than the outer layer 13. The outer layer 13 is one of the outermost layers of the laminated film 2, and is disposed on one of the outermost sides in the lamination direction of the layers constituting the laminated film 2.

[0068] The outer layer 13 is preferably transparent.

[0069] The outer layer 13 preferably comprises a polyamide and an antiblocking agent. The polyamide contained in the outer layer 13 may be the same as the polyamide contained in the resin film 1 described above. The antiblocking agent contained in the outer layer 13 may be the same as the antiblocking agent contained in the resin film 1 described above.

[0070] The polyamide contained in the outer layer 13 and the polyamide contained in the inner layer 11 may be the same as or different from each other. The antiblocking agent contained in the outer layer 13 and the antiblocking agent contained in the inner layer 11 may be the same as or different from each other.

[0071] The antiblocking agent may be present uniformly or non-uniformly in the outer layer 13. When the antiblocking agent is present non-uniformly, it is preferable that the antiblocking agent is unevenly distributed in a region on the surface side of the outer layer 13 opposite to the intermediate layer 12.

[0072] In the outer layer 13, the content ratio of the antiblocking agent relative to the total mass of the outer layer 13 is preferably 0.01 to 2 mass%, more preferably 0.03 to 1 mass%, and even more preferably 0.3 to 0.7 mass%. By setting this ratio to be equal to or greater than the lower limit, adhesion between bags in a package formed using the laminated film 2 is further suppressed. By setting this ratio to be equal to or less than the upper limit, excessive use of the antiblocking agent is further suppressed.

[0073] The outer layer 13 may contain only polyamide and an antiblocking agent (i.e., it may consist of polyamide and an antiblocking agent), or it may contain polyamide, antiblocking agent, and other components (sometimes referred to as "other components" in this specification) (i.e., it may consist of polyamide, antiblocking agent, and the other components).

[0074] Examples of the other components contained in the outer layer 13 include the same components as those contained in the resin film 1 described above.

[0075] The ratio of the polyamide content (parts by mass) in the outer layer 13 to the total mass (parts by mass) of the outer layer 13 ([polyamide content (parts by mass) of the outer layer 13)] / [total mass (parts by mass) of the outer layer 13]×100) is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be, for example, any one of 97% by mass or more and 99% by mass or more. When the ratio is equal to or more than the lower limit, the oxygen barrier property and antifogging property of the outer layer 13 can be further improved, and the laminated film 2 can be produced at a lower cost. In addition, the variation in thickness of the laminated film 2 can be suppressed, and the effect of preventing wrinkles from occurring can be further improved. Furthermore, the transparency of the laminated film 2 can be further improved. On the other hand, the proportion is 99% by mass or less. The above ratio is usually the same as the ratio of the polyamide content (parts by mass) to the total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming the outer layer described below ([polyamide content (parts by mass) in the resin composition for forming the outer layer)]) / [total content (parts by mass) of components that do not vaporize at room temperature in the resin composition for forming the outer layer)]×100).

[0076] The outer layer 13 may be composed of one layer (single layer) or may be composed of two or more layers. When the outer layer 13 is composed of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0077] The thickness of the outer layer 13 can be set arbitrarily depending on the application of the laminated film 2, and is not particularly limited. The thickness of the outer layer 13 is preferably from 2 to 20 μm, more preferably from 3 to 15 μm, and further preferably from 4 to 12 μm. When the thickness of the outer layer 13 is equal to or greater than the lower limit, the effect obtained by providing the outer layer 13 is enhanced. When the thickness of the outer layer 13 is equal to or less than the upper limit, the thickness of the outer layer 13 is further prevented from becoming excessive. In addition, the thinner the thickness of the outer layer 13, the more transparent the packaging bag is, and the easier it is to visually confirm the contents from outside the packaging bag. When the outer layer 13 is made up of a plurality of layers, the total thickness of these layers is preferably within the above numerical range.

[0078] The ratio of the thickness of the outer layer 13 to the total thickness of the laminate film 2 ([thickness of outer layer 13] / [total thickness of laminate film 2]×100) is not particularly limited, but is preferably 7 to 67%, more preferably 10 to 50%, and even more preferably 13 to 40%, and may be, for example, 13 to 20%. When the ratio is equal to or greater than the lower limit, the effect obtained by providing the outer layer 13 is enhanced. When the ratio is equal to or less than the upper limit, the thickness of the outer layer 13 is further prevented from becoming excessive. In addition, the thinner the outer layer 13, the more transparent the packaging bag is, and the easier it is to visually confirm the contents from outside the packaging bag. When the outer layer 13 is made up of a plurality of layers, the ratio of the total thickness of these layers to the entire thickness of the laminate film 2 is preferably within the above-mentioned numerical range.

[0079] <Other layers> The laminated film 2 may have another layer that does not fall under any of the inner layer 11, the intermediate layer 12, and the outer layer 13, as long as the effect of the present invention is not impaired. The type, number and position of the other layers in the laminated film 2 are not particularly limited and may be selected as desired depending on the purpose. In particular, it is preferable that the other layers are disposed between the inner layer 11 and the outer layer 13. For example, the other layer included in the laminate film 2 may be of only one type, or of two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily depending on the purpose.

[0080] The other layers may each be one layer (single layer) or two or more layers. When the other layers are multiple layers, the multiple layers may be the same or different from each other, and the combination of the multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0081] The thickness of the other layer can be set arbitrarily depending on the type of the other layer, and is not particularly limited.

[0082] When the laminated film 2 includes the other layer, it may further include an adhesive layer for adhering the other layer to other layers.

[0083] <Characteristics of resin film> The packaging bag of this embodiment is made of the above-mentioned resin film. In this case, the packaging object may be, for example, Chinese radish, spinach, Japanese mustard spinach, Mizuna, Mibuna, asparagus, Kuusinsai, lettuce, thyme, sage, parsley, Italian parsley, rosemary, oregano, lemon balm, chives, lavender, salad burnet, lamb's ear, rocket, dandelion, nasturtium, basil, arugula, watercress, molokheiya, celery, kale, green onion, cabbage, Chinese cabbage, garland chrysanthemum, lettuce, and so on. Examples of suitable vegetables include radish, butterbur, turnip, bok choy, mitsuba, Japanese parsley, brussels sprouts, broccoli, cauliflower, myoga, radish, carrot, burdock, radish, turnip, sweet potato, potato, Chinese yam, yam, taro, Japanese yam, green pepper, paprika, shishito pepper, cucumber, eggplant, tomato, cherry tomato, pumpkin, bitter melon, okra, sweet corn, edamame, snow peas, green beans, broad beans, fungi, and mushrooms. Among these, sweet potato and potato are preferred, and potato is more preferred.

[0084] The thickness of the resin film is preferably 20 μm or more, more preferably 20 to 40 μm, and even more preferably 25 to 30 μm. When the thickness of the resin film is equal to or greater than the lower limit, the storage stability of the packaged item in the packaging bag obtained using the resin film is higher, and the property of stably maintaining the structure of the packaging bag is higher. When the thickness of the resin film is equal to or less than the upper limit, the formability of the resin film is higher. In addition, the thinner the resin film is, the more transparent the packaging bag is, and the easier it is to visually confirm the contents from the outside of the packaging bag. When the resin film is made up of multiple layers, the total thickness of these layers preferably falls within the above numerical range.

[0085] It is preferable that all layers of the resin film have transparency, that is, the resin film has transparency, i.e., the resin film is a transparent resin film. In a packaging bag obtained using such a resin film, the packaged item can be easily visually confirmed through the resin film.

[0086] [Oxygen barrier properties] The oxygen permeability of a resin film measured in accordance with JIS K 7126-2:2006 under conditions of a temperature of 23°C and a relative humidity (RH) of 60% is, for example, 200 ml / (m 2 ·atm·day) or less, 160ml / (m 2 ·atm·day) or less, 120ml / (m 2 ·atm·day) or less, and 80ml / (m 2 ·atm·day) may be any of the following: On the other hand, the oxygen permeability of the resin film is 5ml / (m 2 ·atm·day) or more. In other words, the oxygen permeability of the resin film is 5 to 200 ml / (m 2 ·atm·day), 5~160ml / (m 2 ·atm·day), 5~120ml / (m 2 ·atm·day), and 5~80ml / (m 2 ·atm·day).

[0087] The oxygen permeation amount of a resin film can be measured, for example, as the oxygen permeation amount per 24 hours for a resin film under the conditions of a pressure of 1 atmosphere, 23° C., and 60% RH.

[0088] The oxygen permeability of the resin film can be adjusted by adjusting the type, amount or thickness of the components contained in any of the layers constituting the resin film. For example, by forming the resin film into a layer containing polyamide, the oxygen permeation amount of the resin film can be easily reduced. However, this is only one example, and the oxygen permeation amount of the resin film can also be adjusted by adjusting other layers.

[0089] [Anti-fogging] The moisture permeability of the resin film measured according to JIS Z 0208 (cup method) is 100 to 400 g / m 2 day, 150~350g / m 2 ·day is preferable, and 200 to 300 g / m 2 ·day is more preferable. By setting the moisture permeability of the resin film to the lower limit or more, the antifogging property of the resin film can be further improved. By setting the moisture permeability of the resin film to the upper limit or less, the water vapor barrier property of the resin film can be further improved.

[0090] The moisture permeability of the resin film can be adjusted by adjusting the type or content of the components contained in any of the layers constituting the resin film. For example, the moisture permeability of the resin film can be easily adjusted by adjusting the type and content of the polyamide contained in the inner layer, intermediate layer, and outer layer.

[0091] [Workability] The coefficient of dynamic friction between the resin films measured in accordance with JIS K 7125 is preferably 0.2 or more and 0.4 or less, more preferably 0.23 or more and 0.37 or less, and even more preferably 0.27 or more and 0.33 or less. By setting the dynamic friction coefficient between the resin films within the above range, it is possible to further suppress defects in opening the bags and adhesion between the bags, thereby further improving workability.

[0092] The coefficient of dynamic friction between resin films can be adjusted, for example, by adjusting the type or content of the components contained in the resin film, or the surface condition (for example, surface roughness) of the resin film. More specifically, the coefficient of dynamic friction between resin films can be easily adjusted, for example, by adjusting the type or content of the antiblocking agent contained in the resin film. In addition, the coefficient of dynamic friction between resin films can be easily adjusted by adjusting the surface condition of the resin film by subjecting the surface of the resin film to a roughening or smoothing treatment.

[0093] When the resin film is a laminated film, the dynamic friction coefficient between the inner layers, measured in accordance with JIS K 7125, is preferably 0.3 or more and 0.5 or less, preferably 0.2 or more and 0.4 or less, more preferably 0.23 or more and 0.37 or less, and even more preferably 0.27 or more and 0.33 or less. By setting the dynamic friction coefficient between the inner layers within the above range, it is possible to further suppress opening defects and further improve workability.

[0094] When the resin film is a laminated film, the dynamic friction coefficient between the outer layers, measured in accordance with JIS K 7125, is preferably 0.3 or more and 0.5 or less, preferably 0.2 or more and 0.4 or less, more preferably 0.23 or more and 0.37 or less, and even more preferably 0.27 or more and 0.33 or less. By setting the dynamic friction coefficient between the outer layers within the above range, adhesion between the bags can be further suppressed, and workability can be further improved.

[0095] When the resin film is a laminated film, the coefficient of dynamic friction between the inner layers or between the outer layers can be adjusted, for example, by adjusting the type or content of the components contained in the inner layer or the outer layer. More specifically, the coefficient of dynamic friction between the inner layers or between the outer layers can be easily adjusted, for example, by adjusting the type or content of the antiblocking agent contained in the inner layer or the outer layer. The coefficient of dynamic friction between the inner layers or between the outer layers can also be adjusted by adjusting the surface condition (e.g., surface roughness) of the inner or outer layers. More specifically, the coefficient of dynamic friction between the inner layers or between the outer layers can be easily adjusted by adjusting the surface condition of the inner or outer layers, for example, by subjecting the surfaces of the inner or outer layers to a roughening or smoothing treatment.

[0096] [Tensile modulus] The tensile modulus of the resin film measured in accordance with JIS K 7161 is preferably 300 to 2000 MPa, more preferably 400 to 1500 MPa, and even more preferably 500 to 1000 MPa. When the tensile modulus of the resin film is equal to or greater than the lower limit, the resin film can have a luxurious feel. When the tensile modulus of the resin film is equal to or less than the upper limit, unwinding of the back seal portion is further suppressed in a packaging bag formed using the resin film.

[0097] The tensile modulus of the resin film can be adjusted by adjusting the type or content of the components contained in any of the layers constituting the resin film. For example, when the resin film is a laminate film such as the laminate film 2, the tensile modulus of the resin film (laminate film) can be easily adjusted by adjusting the type and content of the polyamide contained in the inner layer, intermediate layer, or outer layer.

[0098] [Fusing strength] The melting strength of the resin film is preferably 8 to 30 N / 15 mm, more preferably 10 to 25 N / 15 mm, and even more preferably 12 to 20 N / 15 mm, and it is particularly preferable that the elongation of the resin film is 300% or more. When the melting strength of the resin film is equal to or greater than the lower limit, the breakage of the packaging bag manufactured using the resin film can be further suppressed. When the melting strength of the resin film is equal to or less than the upper limit, the thickness of the melted surface end portion can be further suppressed from becoming too thick (the size of the resin ball can be further suppressed from becoming too large).

[0099] In this specification, the melting strength of a resin film means the melting strength measured by the method of JIS Z 0238, unless otherwise specified.

[0100] The melting strength of the resin film can be adjusted by adjusting the type or content of the components contained in any of the layers constituting the resin film. For example, when the resin film is a laminated film such as the laminated film 2, the melting strength of the resin film (laminated film) can be easily adjusted by adjusting the type and content of the polyamide contained in the inner layer, intermediate layer, or outer layer.

[0101] [Transparency] The haze of the resin film is preferably 16% or less, more preferably 12% or less, and even more preferably 8% or less. When the haze of the resin film is equal to or less than the upper limit, the contents of the package bag made using the resin film can be more clearly seen from the outside. The lower limit of the haze of the resin film is not particularly limited. For example, a resin film having a haze of 0.5% or more can be produced more easily. In one embodiment, the haze of the resin film may be any one of 3 to 16%, 4 to 12%, and 5 to 8%, although these are just examples of the haze of the resin film.

[0102] In this specification, the haze of a resin film means the haze measured from the outside of the inner layer side of the resin film in accordance with JIS K 1707, unless otherwise specified.

[0103] The haze of the resin film can be adjusted by adjusting the type or content of the components contained in any of the layers constituting the resin film. For example, when the resin film is a laminate film such as the laminate film 2, the haze of the resin film (laminated film) can be easily adjusted by adjusting the type and content of the polyamide contained in the inner layer, intermediate layer, or outer layer.

[0104] <Method of manufacturing resin film> The resin film constituting the packaging bag of the present embodiment can be produced, for example, by melt-extruding and molding a resin composition for forming a resin film, which is a material for forming the resin film, using an extruder.

[0105] Of the resin films constituting the packaging bag of this embodiment, a laminated film (a resin film consisting of multiple layers) can be produced, for example, by a feed block method in which several extruders are used to melt-extrude resins or resin compositions that serve as materials for forming each layer; a co-extrusion T-die method such as a multi-manifold method; or an air-cooled or water-cooled co-extrusion inflation method.

[0106] In addition, the laminated film constituting the packaging bag of this embodiment can also be produced by coating a resin or resin composition, etc. that will be the material for forming one of the layers therein, onto the surface of another layer that will form the resin film, and drying it as necessary to form a laminated structure in the resin film, and if necessary, further laminating other layers so as to achieve the desired arrangement.

[0107] In addition, the laminated film constituting the packaging bag of this embodiment can also be produced by separately preparing in advance two or more films for constituting any two or more of the layers, laminating these films together using an adhesive by any of a dry lamination method, an extrusion lamination method, a hot melt lamination method, and a wet lamination method, and, if necessary, further laminating other layers so as to achieve the desired arrangement.

[0108] In addition, the laminated film constituting the packaging bag of this embodiment can also be produced by laminating two or more films that have been prepared separately in advance, as described above, by a thermal lamination method or the like without using an adhesive, and, if necessary, further laminating other layers so as to achieve the desired arrangement.

[0109] Resin films produced by the co-extrusion inflation method, coating, etc. tend to wrinkle easily when left in the air, but resin films produced by the co-extrusion T-die method tend not to wrinkle easily even when left in the air, so it is preferable to produce resin films using the co-extrusion T-die method.

[0110] When producing the resin film constituting the packaging bag of this embodiment, two or more of the methods for forming any of the layers (films) in the resin film mentioned above may be combined.

[0111] Regardless of the manufacturing method, the resin composition that is the material for forming any layer in the resin film may be manufactured by adjusting the type and content of the components contained so that the layer to be formed contains the desired components (constituent materials) in the desired content. For example, the content ratio of the components that do not vaporize at room temperature in the resin composition is usually the same as the content ratio of the components in the layer formed from this resin composition.

[0112] Examples of resin compositions (sometimes referred to in this specification as "resin compositions for forming resin films") for forming regions of the resin film 1 shown in FIG. 1 other than the regions on both surface sides (regions where no antiblocking agent is present or where the amount of antiblocking agent is small) include resin compositions containing the above-mentioned polyamide and, if necessary, the other components. Examples of resin compositions (resin compositions for forming resin films) for forming the regions on both surface sides of the resin film 1 shown in FIG. 1 (regions where the antiblocking agent is unevenly distributed) include resin compositions containing the above-mentioned polyamide, the above-mentioned antiblocking agent, and, if necessary, the other components.

[0113] Examples of the resin composition (sometimes referred to in this specification as a "resin composition for forming an inner layer") for forming an inner layer (in the laminate film 2 shown in FIG. 2, the inner layer 11) include a resin composition containing the above-mentioned polyamide, the above-mentioned antiblocking agent, and, if necessary, the other components.

[0114] Examples of resin compositions (sometimes referred to in this specification as "resin compositions for forming an intermediate layer") for forming an intermediate layer (intermediate layer 12 in the laminate film 2 shown in Figure 2) include resin compositions containing the above-mentioned polyamide and, if necessary, the other components described above.

[0115] Examples of the resin composition (sometimes referred to in this specification as a "resin composition for forming an outer layer") for forming an outer layer (outer layer 13 in the laminate film 2 shown in FIG. 2) include a resin composition containing the above-mentioned polyamide, the above-mentioned antiblocking agent, and, if necessary, the other components.

[0116] <<Packaging bag>> The packaging bag of the present embodiment has a welded portion obtained by fusing together resin films. The packaging bag of this embodiment may be a packaging bag obtained using the above-mentioned resin film described above, in which case it has a welded portion obtained by fusing together the above-mentioned resin films described above.

[0117] When the packaging bag of this embodiment is obtained, for example, using a resin film having the above-mentioned inner layer, intermediate layer, and outer layer, the packaging bag has a storage space formed by welding parts of the inner layers together, and the intermediate layer is positioned on the storage space side relative to the outer layer.

[0118] The welded portion is formed by melt cutting a resin film into a bag.

[0119] The width of the welded portion of the packaging bag of this embodiment is 300 μm or less, which means that even when a plurality of packaging bags are stacked, the overlapping end portions do not become bulky.

[0120] The welded parts of the packaging bag can be identified, for example, by cutting in the cross-sectional direction using a microtome (HM340E, manufactured by PHC Corporation) as shown in the rotary microtome principle diagram in Figure 4, and then observing with a polarizing microscope (ECLIPSE LV100N POL, manufactured by Nikon Solutions Corporation) as shown in the enlarged schematic diagram of the end of the packaging bag in Figure 4.

[0121] In the packaging bag of this embodiment, the width of the welded part is the dimension of the welded part in a direction perpendicular to its longitudinal direction, and if the width of the welded part is not uniform, the maximum width of the welded part may be 300 μm or less.

[0122] The width of the welded portion is preferably 280 μm or less, and more preferably 250 μm or less. By making the width of the welded portion equal to or less than the upper limit, the effect of preventing the overlapping end portions from becoming bulky even when a plurality of packaging bags are stacked can be further improved.

[0123] The width of the welded part can be adjusted by adjusting the type or content of the components contained in any of the layers constituting the resin film. For example, when the resin film is a laminated film such as the laminated film 2, the width of the welded part can be easily adjusted by adjusting the type and content of the polyamide contained in the inner layer, intermediate layer, or outer layer. The width of the welded part can also be adjusted by adjusting the conditions for melt-cutting the resin film to form a bag (conditions for forming the welded part). For example, the width of the welded part can be easily adjusted by changing the temperature of the melt-cutting blade and the melt-cutting time when melt-cutting the resin film to form a bag.

[0124] The temperature of the fusion cutting blade is preferably 410°C to 490°C, more preferably 420°C to 480°C, and further preferably 430°C to 470°C.

[0125] The melting time is preferably 270 ms to 390 ms, more preferably 280 ms to 380 ms, and further preferably 290 ms to 370 ms.

[0126] Furthermore, since the packaging bag of the present embodiment includes the resin film, the color of the welded portions of the resin films is good.

[0127] The welded portion is CIE1976L * a * b * In the coordinate system specified by the color system, lightness L * is preferably -25 or more and -17 or less, and the chromaticity a * is preferably between -1 and 1, and the chromaticity b * It is preferable that the ratio is 8.5 or more and 10.5 or less. Lightness L * , chromaticity a * and chromaticity b * When the lightness L is within the above range, the color tone of the welded portion between the resin films becomes better. * , chromaticity a * and chromaticity b *However, when the lightness is equal to or greater than the lower limit, the welded portion becomes more visible. * , chromaticity a * and chromaticity b * However, by making the content equal to or less than the upper limit, the appearance of the welded portion becomes better.

[0128] The lightness L * is more preferably −24 or more and −17 or less, further preferably −23 or more and −16 or less, and particularly preferably −22 or more and −15 or less. The chromaticity a * is more preferably −1 or more and 1 or less, further preferably −0.9 or more and 0.9 or less, and particularly preferably −0.8 or more and 0.8 or less. The chromaticity b * is more preferably 8.5 or more and 10.5 or less, further preferably 8.2 or more and 10.3 or less, and particularly preferably 8.4 or more and 10.1 or less. Lightness L * , chromaticity a * and chromaticity b * However, when the lightness is equal to or greater than the lower limit, the welded portion becomes more visible. * , chromaticity a * and chromaticity b * However, by making the content equal to or less than the upper limit, the appearance of the welded portion becomes better.

[0129] The lightness L of the welded part * , chromaticity a * and chromaticity b * can be adjusted by adjusting the type or content of the component of any of the layers constituting the resin film. For example, when the resin film is a laminated film such as the laminated film 2, the lightness L of the welded portion can be adjusted by adjusting the type and content of the polyamide contained in the inner layer, intermediate layer, or outer layer. * , chromaticity a * and chromaticity b * The lightness L of the welded portion can be easily adjusted. * , chromaticity a * and chromaticity b *The lightness L of the welded portion can be adjusted by adjusting the conditions for melt-cutting the resin film to form a bag (conditions for forming the welded portion). For example, the lightness L of the welded portion can be adjusted by changing the melt-cutting time when melt-cutting the resin film to form a bag. * , chromaticity a * and chromaticity b * can be easily adjusted.

[0130] The melting time is preferably 270 ms to 390 ms, more preferably 280 ms to 380 ms, and further preferably 290 ms to 370 ms.

[0131] In the packaging bag of the present embodiment, the welded portion preferably has carbide pieces of the resin film. The carbide pieces are generated by heat during melt-cutting of the resin film to form a bag, for example. When the welded portion has carbonized pieces of the resin film, the welded portion can be picked up more easily. The welded portion having carbonized pieces of the resin film means that some of the carbonized pieces can be removed, but not all of them (e.g., some of the carbonized pieces are on the surface of the welded portion and some are inside the welded portion).

[0132] The size of the carbide pieces is preferably 50 μm or more and 1000 μm or less, more preferably 55 μm or more and 900 μm or less, and even more preferably 60 μm or more and 800 μm or less. When the size of the carbide pieces is equal to or larger than the lower limit, the effect of the welded portion being easily caught and easily picked up can be further improved. When the size of the carbide pieces is equal to or smaller than the upper limit, the welded portion can be more effectively prevented from being too caught and becoming difficult to pick up, and pinholes can be more effectively prevented from being formed in the welded portion.

[0133] An identification image of the carbide piece is obtained, and the maximum value of the length of a line segment connecting any two points located on the contour line in the identification image can be adopted as the size of the carbide piece. The identification image can be obtained, for example, from imaging data when the welded portion is observed with an optical microscope.

[0134] The size of the carbonized pieces can be adjusted by adjusting the type or content of the components contained in any of the layers constituting the resin film. For example, when the resin film is a laminated film such as the laminated film 2, the size of the carbonized pieces can be easily adjusted by adjusting the type and content of the polyamide contained in the inner layer, intermediate layer, or outer layer. The size of the carbonized pieces can also be adjusted by adjusting the conditions for melt-cutting the resin film to form a bag (the conditions for forming the welded portion). For example, the size of the carbonized pieces can be easily adjusted by changing the temperature of the melt-cutting blade when melt-cutting the resin film to form a bag.

[0135] The temperature of the fusion cutting blade is preferably 410°C to 490°C, more preferably 420°C to 480°C, and further preferably 430°C to 470°C.

[0136] FIG. 3 is a cross-sectional view that illustrates an example of the packaging bag of the present embodiment. The packaging bag 10 shown here is formed using the resin film 1 shown in Fig. 1. The packaging bag 10 is roughly configured to have a storage space S formed by partially welding a pair of resin films 1 to each other. Alternatively, the packaging bag 10 shown here is formed using the laminate film 2 shown in Fig. 2. The packaging bag 10 has a storage space S formed by partially welding together the inner layers 11, 11 of a pair of laminate films 2, and is roughly configured such that the intermediate layer 12 is disposed closer to the storage space S than the outer layer 11. That is, the pair of laminate films 2, 2 are disposed such that the inner layers 11, 11 face each other. In the storage space S of the packaging bag 10, a target item to be stored (not shown) is stored.

[0137] So far, the packaging bag of the present invention has been described as using the resin film 1 shown in Figure 1 and the laminate film 2 shown in Figure 2, but the packaging bag of the present invention may also be formed using the resin film of other embodiments of the present invention.

[0138] The packaging bag of the present embodiment is not limited to the above-described embodiment, and some of the configuration may be changed, deleted, or added without departing from the spirit of the present invention. For example, the packaging bag 10 shown in FIG. 3 uses a pair of the same type of resin films 1,1 or laminate films 2,2, but the packaging bag of the present invention may also use a pair of different types of resin films. Furthermore, the packaging bag of the present invention may have other components in addition to the resin film, as long as the effects of the present invention are not impaired. The other components are not particularly limited and may be appropriately selected depending on the purpose.

[0139] <Manufacturing method of packaging bags> The packaging bag of the present embodiment can be manufactured by using the resin film and welding parts of the resin film together so as to have a storage space. The resin films can be fused together by, for example, applying a known fusion-cut bag making method.

[0140] When the resin film is a laminated film (for example, laminated film 2 shown in FIG. 2), the packaging bag of this embodiment can be produced by welding parts of the inner layers of the laminated film together so as to have an accommodation space. The inner layers can be fused together by, for example, applying a known fusion-cut bag making method.

[0141] The fusion cutting bag making can be carried out under conditions where the fusion cutting blade temperature is 300°C to 500°C. EXAMPLES

[0142] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.

[0143] [Example 1] <<Laminated film manufacturing>> A laminated film having the structure shown in FIG. 2 was produced by the following procedure.

[0144] As a resin for forming the inner layer, intermediate layer, and outer layer, 6-nylon (Ny6, a non-aromatic polyamide, "1022B" manufactured by UBE Corporation) was prepared.

[0145] The Ny6 (99.5 parts by mass) and an antiblocking agent (AB, "HS-311" manufactured by Nippon Steel Chemical & Material Co., Ltd.) (0.5 parts by mass) were mixed together to produce a resin composition for forming the inner and outer layers.

[0146] The die temperature was set to 260°C, and the resin composition for forming the inner and outer layers, the Ny6, and the resin composition for forming the inner and outer layers were co-extruded in this order (co-extrusion T-die method) to obtain a laminated film (thickness 30 μm) composed of an inner layer (thickness 4 μm), an intermediate layer (thickness 22 μm), and an outer layer (thickness 4 μm) laminated in this order in the thickness direction.

[0147] <<Evaluation of laminated film>> <Measurement of dynamic friction coefficient> For the above laminated film, the dynamic friction coefficient between the inner layers and the dynamic friction coefficient between the outer layers were measured in accordance with JIS K 7125. The results are shown in Table 1.

[0148] <Oxygen transmission rate measurement> The oxygen transmission rate of the laminated film was measured at a temperature of 23° C. and a relative humidity (RH) of 60% in accordance with JIS K 7126. The results are shown in Table 1.

[0149] <Measurement of moisture permeability> The moisture permeability of the laminated film was measured in accordance with JIS Z 0208 (cup method). The results are shown in Table 1.

[0150] <Measurement of tensile modulus> The tensile modulus of elasticity of the above laminated film was measured under conditions of a temperature of 20° C. and a humidity of 50% in accordance with JIS K 7161. The results are shown in Table 1.

[0151] <Measurement of fusing strength> The fusing strength of the above laminated film was measured according to the method of JIS Z0238. The results are shown in Table 1.

[0152] <Haze measurement> The haze (%) of the above laminated film was measured from the outside of the inner layer side in accordance with JIS K 1707. The results are shown in Table 1.

[0153] << Packaging bag manufacturing >> Using the above laminated film, a melt-cutting bag making machine was used to perform melt-cutting bag making under conditions of melt-cutting blade temperature: 450°C, melt-cutting time (shot): 320 ms, and a packaging bag having a storage space formed by partially melting the inner layers together was produced.

[0154] <<Evaluation of packaging bags>> <Width of welded part> The width of the welded part of the above packaging bag was measured by cutting in the cross-sectional direction using a microtome (HM340E, manufactured by PHC Corporation) and observing with a polarizing microscope (ECLIPSE LV100N POL, manufactured by Nikon Solutions Co., Ltd.). The results are shown in Table 1.

[0155] <Bulking of the ends> 100 packaging bags were stacked, and the bulkiness of the overlapping ends was checked according to the following criteria. The results are shown in Table 1. (Evaluation Criteria) A: When workers touch the product, they can feel the difference in width between the overlapping parts at the ends and the overlapping part in the center (the ends are bulkier). B: The worker does not feel the difference in width between the overlapping parts at the ends and the overlapping part at the center (the ends are bulkier) when touching them, and feels that they are almost the same.

[0156] <Color of welded part> The welded parts of the inner layers that had no carbide particles attached were measured using a color difference meter (Konica Minolta's "Spectrophotometer CM-26dG") to measure the CIE1976L * a * b * Lightness L in the coordinates specified by the color system * , chromaticity a * and chromaticity b * The results are shown in Table 1.

[0157] <Visibility of welded parts> The visibility of the welded parts was visually confirmed according to the following criteria, and the results are shown in Table 1. (Evaluation Criteria) A: The welded parts are easy to see. B: The welded part is difficult to see.

[0158] <Appearance of welded part> The appearance of the welded parts was visually inspected according to the following criteria, and the results are shown in Table 1. (Evaluation Criteria) A: The appearance of the welded part is good. B: The welded part has a poor appearance.

[0159] <Size of carbide pieces> For the welded joints between the inner layers, a microscope (Nikon Solutions Corporation's "polarized microscope ECLIPSE LV100NPOL / Ci-POL") was used to measure the maximum length of the line segment connecting any two points located on the contour line in the identification image of the carbide piece. The results are shown in Table 1.

[0160] <Pickup ability of welded parts> The pick-up ability of the welded portion was checked according to the following criteria, and the results are shown in Table 1. (Evaluation Criteria) A: It is easy to pick up the welded part. B: It is difficult to pick up the welded part.

[0161] <Pinholes in welded parts> The pinhole occurrence in the welded portion was checked according to the following criteria, and the results are shown in Table 1. (Evaluation Criteria) A: There are no pinholes in the welded area. B: There is a pinhole in the welded area.

[0162] <Back seal suitability> The back seal of the above packaging bag was twisted 540° (3 rotations). After 9 days, the packaging bag was cut with scissors and the cross section was visually inspected. The angle of the twisted part was measured and the state of unwinding of the back seal was evaluated according to the following criteria. The results are shown in Table 1. (Evaluation Criteria) A: After 5 days, the angle of the twisted part is over 360°, and there is little rewinding of the back seal part. B: After 5 days, the angle of the twisted part is 360° or less, and there is a lot of rewinding of the back seal part.

[0163] <Bag break resistance> A drop test was carried out on 10 of the above packaging bags (500 g / bag) in accordance with JIS Z 0202, and the number of broken packages was visually confirmed. The results are shown in Table 1.

[0164] <Freshness retention performance> Potatoes were stored in the above-mentioned packaging bags for 5 days and the state of freshness was visually checked according to the following criteria. The results are shown in Table 1. (Evaluation Criteria) A: Freshness is well maintained. B: Freshness is not well maintained.

[0165] [Comparative Example 1] A laminated film was produced and evaluated in the same manner as in Example 1. A packaging bag was produced and evaluated in the same manner as in Example 1, except that the melt-cutting bag production was performed under the condition of a melt-cutting time (shot): 400 ms. The results are shown in Table 1.

[0166] [Comparative Example 2] A laminated film was produced and evaluated in the same manner as in Example 1. A packaging bag was produced and evaluated in the same manner as in Example 1, except that the melt-cutting bag production was performed under the condition of a melt-cutting time (shot): 260 ms. The results are shown in Table 1.

[0167] [Comparative Example 3] A laminated film was produced and evaluated in the same manner as in Example 1. A packaging bag was produced and evaluated in the same manner as in Example 1, except that the melt-cutting bag production was performed under the condition of a melt-cutting blade temperature of 500° C. The results are shown in Table 1.

[0168] [Comparative Example 4] A laminated film was produced and evaluated in the same manner as in Example 1. A packaging bag was produced and evaluated in the same manner as in Example 1, except that the melt-cutting bag production was performed under the condition of a melt-cutting blade temperature of 400° C. The results are shown in Table 1.

[0169] [Table 1]

[0170] As is clear from the above results, in Example 1, the width of the welded portion was 300 μm or less, so that the overlapping portion of the end portion was not bulky, as shown in Table 1. In addition, the lightness L * is between -25 and -17, and the chromaticity a * is between -1 and 1, and chromaticity b * However, because the tensile strength was between 8.5 and 10.5, the welded part was easy to see and had a good appearance. Furthermore, because the size of the carbide pieces was between 50 μm and 1000 μm, the welded part was easy to catch and pick up, and there were no pinholes in the welded part.

[0171] In Comparative Example 1, the width of the welded portion was more than 300 μm, so the overlapping portion of the end was bulky. * is less than -25, and the chromaticity a * is less than -1, and chromaticity b *However, since the value was less than 8.5, as shown in Table 1, the welded portion was difficult to visually confirm.

[0172] In Comparative Example 2, the width of the welded portion was more than 300 μm, so the overlapping portion of the end portion was bulky. * is greater than -17, and the chromaticity a * is greater than 1, and the chromaticity b * However, since the value exceeded 10.5, the appearance of the welded part was poor, as shown in Table 1.

[0173] In Comparative Example 3, the width of the welded portion was more than 300 μm, so the overlapping end portion was bulky, and the size of the carbide pieces was less than 50 μm, so the welded portion was difficult to catch and pick up, as shown in Table 1.

[0174] In Comparative Example 4, the width of the welded portion was more than 300 μm, so the overlapping end portion was bulky, and the size of the carbide pieces was more than 1000 μm, so as shown in Table 1, the welded portion was too difficult to pick up and had pinholes.

[0175] [Example 2] A laminated film having the structure shown in FIG. 2 was produced by the following procedure.

[0176] As a resin for forming the intermediate layer, copolymer nylon (copolymer Ny, non-aromatic polyamide, "5023" manufactured by UBE Corporation) was prepared.

[0177] The die temperature was set to 260°C, and the resin composition for forming the inner and outer layers, the copolymer Ny, and the resin composition for forming the inner and outer layers were used to obtain a laminated film (thickness 31 μm) by co-extrusion inflation method, in which an inner layer (thickness 3 μm), an intermediate layer (thickness 25 μm), and an outer layer (thickness 3 μm) were laminated in this order in the thickness direction.

[0178] This laminated film was evaluated in the same manner as in Example 1. In addition, a packaging bag was produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0179] [Example 3] A two-layer laminate film was produced according to the following procedure.

[0180] As the resin constituting the inner layer, an ethylene-vinyl alcohol copolymer (EVOH, "G156B" manufactured by Kuraray Co., Ltd., copolymerization ratio of ethylene: 48 mol %) was prepared.

[0181] As the resin constituting the outer layer, biaxially oriented nylon (biaxially oriented Ny, "ON" manufactured by Unitika Ltd.) was prepared.

[0182] The biaxially oriented nylon was formed into a monolayer film, and the EVOH was laminated onto its surface to obtain a laminated film (thickness 27 μm) in which an inner layer (thickness 2 μm) and an outer layer (thickness 25 μm) were laminated in the thickness direction.

[0183] This laminated film was evaluated in the same manner as in Example 1. In addition, a packaging bag was produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0184] [Reference example 1] A single-layer resin film was produced according to the following procedure.

[0185] Biaxially oriented polypropylene (biaxially oriented PP, "FOA" manufactured by Futamura Chemical Co., Ltd.) was prepared.

[0186] The biaxially oriented PP was molded into a monolayer film to obtain a resin film (thickness: 30 μm).

[0187] This resin film was evaluated in the same manner as in Example 1. In addition, a packaging bag was produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0188] [Table 2]

[0189] As is clear from the above results, in Examples 1 to 3, the width of the welded portion was 300 μm or less, so that the overlapping portion of the end portion was not bulky, as shown in Table 1. In addition, the lightness L * is between -25 and -17, and the chromaticity a * is between -1 and 1, and chromaticity b * However, because the tensile strength was between 8.5 and 10.5, the welded part was easy to see and had a good appearance. Furthermore, because the size of the carbide pieces was between 50 μm and 1000 μm, the welded part was easy to catch and pick up, and there were no pinholes in the welded part.

[0190] In Examples 1 and 2, all layers of the laminated film did not contain EVOH, but contained polyamide, and therefore production was possible at a lower cost than in Example 3. In Examples 1 and 2, although none of the layers of the laminated film contained EVOH, the oxygen permeability of the laminated film was 10 to 67 ml / (m 2 1 day atm, and Example 3 (oxygen permeability 20 ml / (m 2 The oxygen barrier properties were comparable to those of Reference Example 1 (oxygen permeability 1500 ml / (m 2 The oxygen barrier properties were far superior to those of the conventional 100-μm ... In Examples 1 and 2, although none of the layers of the laminated film contained EVOH, the moisture permeability of the laminated film was 150 to 200 g / (m 2 ·day) and Example 3 (moisture permeability 150g / (m 2 ·day)). Also, the moisture permeability of the sample was approximately the same as that of Reference Example 1 (moisture permeability of 10 g / (m 2 The anti-fogging properties were much better than those of the conventional coating.

[0191] In Examples 1 and 2, since the inner layer contained an antiblocking agent, the dynamic friction coefficient was 0.3, which was lower than Example 3 (dynamic friction coefficient 0.5), and opening failure was suppressed, resulting in excellent workability. In Examples 1 and 2, since the outer layer contained an antiblocking agent, the dynamic friction coefficient was 0.3, which was lower than that of Example 3 (dynamic friction coefficient 0.4), and adhesion between the bags was suppressed, resulting in excellent workability.

[0192] In Examples 1 and 2, none of the layers of the laminated film contained biaxially oriented Ny, so the tensile modulus was 600 MPa, which was lower than that of Example 3 (tensile modulus 1500 MPa), and the rigidity was suppressed. In Examples 1 and 2, none of the layers of the laminated film contained biaxially oriented Ny, so the fusing strength was "elongation of 300% or more," which was superior to Example 3 (fusing strength of 1.8 N / 15 mm). In Example 1, none of the layers of the laminated film contained EVOH, so the haze was 6%, lower than that of Example 3 (haze 10%), and transparency was excellent. In Example 1, none of the layers of the laminated film contained copolymerized Ny, and the manufacturing method of the laminated film was not coextrusion inflation, so the haze was 6%, lower than that of Example 2 (haze 14%), and transparency was excellent.

[0193] In Examples 1 and 2, the stiffness of the laminated film was suppressed, and therefore the back sealability was superior to that of Example 3. In Examples 1 and 2, the melt-cutting strength of the laminated film was superior, and therefore the bag-breaking resistance was superior to that of Example 3. In Examples 1 and 2, the rigidity of the laminated film was suppressed, and therefore the packaging bags had excellent back-sealing suitability, and thus had better freshness retention than Example 3. [Industrial Applicability]

[0194] INDUSTRIAL APPLICABILITY The present invention can be used to manufacture packaging bags in which the overlapped end portions are not bulky even when a plurality of packaging bags are stacked. [Explanation of symbols]

[0195] 1...Resin film 2...Laminated film 10...Packaging bag 11…Inner layer 12. Middle class 13…outer layer S: Packaging bag storage space

Claims

1. A packaging bag having a welded portion obtained by fusing together resin films, The resin film contains polyamide, A packaging bag, wherein the width of the welded portion of the packaging bag is 300 μm or less.

2. The welded portion is CIE1976L * a * b * In the coordinate system defined by the color system, lightness L * is -25 or more and -17 or less, and the chromaticity a * is greater than or equal to -1 and less than or equal to 1, and the chromaticity b * The packaging bag according to claim 1, wherein the elastic modulus is 8.5 or more and 10.5 or less.

3. the welded portion has a carbide piece of the resin film, 3. The packaging bag according to claim 1, wherein the size of the carbide pieces is 50 μm or more and 1000 μm or less.

4. The resin film further contains an antiblocking agent in addition to the polyamide, The packaging bag according to claim 1 , wherein the antiblocking agent is present in the resin film in regions on both surface sides of the resin film.

5. The resin film is a laminated film, The laminated film is configured by laminating an inner layer, an intermediate layer, and an outer layer in this order in a thickness direction, the inner layer and the outer layer comprise a polyamide and an antiblocking agent; The packaging bag of claim 1 , wherein the intermediate layer comprises a polyamide.

6. The packaging bag according to claim 4 or 5, wherein the polyamide is an unstretched polyamide.

7. 6. The packaging bag according to claim 4, wherein the polyamide is one or more selected from the group consisting of nylon 6, nylon 66, and a copolymer of nylon 6 and nylon 66.

8. The packaging bag according to claim 5 , wherein the dynamic friction coefficient between the inner layers is 0.3 or more and 0.5 or less.

9. The packaging bag according to claim 5 , wherein the coefficient of dynamic friction between the outer layers is 0.3 or more and 0.5 or less.

10. The packaging bag according to claim 1 , wherein the resin film has a thickness of 20 μm or more.

Citation Information

Patent Citations

  • Packaging material for retaining freshness of vegetable / fruit

    JP1997252718A

  • Multilayered porous film made of thermoplastic resin

    JP2005144830A