Print ink set, printed material, and packaging material

The printing ink set, featuring specific pigments and compounds, addresses the challenges of color reproducibility and durability by enhancing light resistance and color gamut, suitable for printed matter and packaging materials.

JP2024140643APending Publication Date: 2024-10-10TOYO INK MFG CO LTD

Patent Information

Application Number
JP2023051888
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing printing inks face challenges in achieving high color reproducibility and durability, particularly under sunlight and white LED illumination, with methods using specific pigments or ultraviolet absorbers leading to reduced color gamut or increased manufacturing costs, and stability issues such as gelation.

Method used

A printing ink set comprising yellow ink with an isoindoline compound or C.I. Pigment Yellow 180, cyan ink with a phthalocyanine pigment, magenta ink A with a dioxazine pigment, and magenta ink B with C.I. Pigment Red 122 or C.I. Pigment Violet 19, along with a diketopyrrolopyrrole or perylene pigment, to enhance color reproducibility and light resistance.

Benefits of technology

The ink set achieves a color gamut equivalent to or greater than conventional inks, with improved light resistance and high color reproducibility, suitable for printed matter and packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140643000001
    Figure 2024140643000001
  • Figure 2024140643000002
    Figure 2024140643000002
  • Figure 2024140643000003
    Figure 2024140643000003
Patent Text Reader

Abstract

To provide a print ink set with superior light resistance and superior color reproducibility, and also to provide a printed material and a packaging material with superior design as well as superior light resistance and adhesion of the printing layer.SOLUTION: A print ink set comprises yellow ink comprising isoindolin compound or C.I. Pigment Yellow 180, cyan ink comprising phthalocyanine pigment, magenta ink A comprising dioxazine pigment, and magenta ink B comprising at least one pigment selected from the group consisting of C.I. Pigment Red 122, C.I. Pigment Violet 19, diketopyrrolopyrrole pigment and perylene pigment.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] SUMMARY OF THE DISCLOSURE Embodiments of the present invention relate to printing ink sets, printed matter, and packaging materials comprising printing inks of at least three primary colors. [Background technology]

[0002] Printing inks contain a pigment and a dispersion medium as main materials and are used to form a printing layer on substrates such as various plastics and paper. Printing inks are broadly classified according to the printing method or application. For example, printing inks include offset printing inks, flexographic printing inks, gravure printing inks, and silk screen printing inks in terms of printing method. Printing inks are also made to suit various applications and can be broadly classified according to the form of the dispersion medium. For example, there are solventless (active energy ray curable) printing inks that contain a resin as a dispersion medium, and solvent-based printing inks that contain an organic solvent as a dispersion medium. Furthermore, there are water-based printing inks that contain a resin and water as a dispersion medium.

[0003] Thus, printing inks are used in various printing methods and are configured in various forms. Applications of printing inks include printed matter and packaging materials using printed matter. Examples of printed matter include posters, labels, medicine boxes, and other items in which a printed layer is formed on a substrate. Examples of packaging materials include packaging materials for packaging items such as food, beverages, daily necessities, cultural goods, and electronic components. Printing inks used for printed matter and packaging materials are required to have at least color reproducibility. However, in recent years, the applications of printed matter and packaging materials have expanded significantly, and the forms of use of printed matter and packaging materials have become more diverse. Therefore, various performance characteristics are also required for printing inks used for printed matter and packaging materials.

[0004] For example, packaging materials are required to have a function of properly displaying product information of the contents in addition to a function of maintaining the quality of the contents and improving the efficiency of transportation. In order to properly display product information, a printed layer is formed on the packaging material for the purpose of decoration, imparting aesthetic appeal, displaying the contents, expiration date, manufacturer or seller, etc. The display by such a printed layer is very important information for logistics personnel and consumers. A brand mark or brand color may be used as product information, and in this case, the printed matter and packaging material are required to have high designability, including imparting aesthetic appeal. Therefore, a printing ink having color reproducibility suitable for use in the application of printed matter and packaging material is required.

[0005] In addition, for example, when the printed matter or packaging material is used outdoors, there may be a problem of discoloration or fading due to sunlight. Furthermore, packaging materials and packages may be stored under light irradiation for a long period of time. Even under such storage conditions, there may be a problem of discoloration occurring, and the appearance of the package may deviate from the intended appearance. In addition, in packaging material applications, the influence of radicals generated by light irradiation during storage may cause a decrease in the cohesive force or adhesive force of the printed layer, resulting in a decrease in laminate strength. As a result, there may be a problem of interphase peeling of the laminate when opening packages and packaging materials stored for a long period of time under light irradiation.

[0006] From this perspective, it is desirable for printing inks used for printed matter or packaging materials to have excellent durability, such as weather resistance and light resistance, in addition to excellent color reproducibility. In particular, for light exposure during storage, sunlight or fluorescent lamps were traditionally the most common light source, but in recent years, the use of white LEDs for indoor illumination has become increasingly common. For this reason, printing inks may be required to have durability, such as light resistance, that is different from that of the past.

[0007] As described above, the performance required of printing inks typically includes excellent color reproducibility and durability such as weather resistance and light resistance, and various investigations are being carried out to address this. For example, methods for imparting light resistance to packaging materials have been studied. For example, Patent Document 1 discloses that a packaging material with excellent light resistance can be provided by using a printing ink containing a specific pigment and a polyurethane resin. Patent Document 2 discloses that a packaging material with excellent light resistance can be provided by using a printing ink to which a certain amount of an ultraviolet absorber or a light stabilizer is added, which suppresses deterioration of the coating film due to light exposure. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2012-136582 A [Patent Document 2] JP 2006-70190 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, when a specific pigment is used as in the method described in Patent Document 1, the reproducible color gamut is reduced compared to typical printing inks used for packaging materials, and it tends to be difficult to obtain the desired design. In addition, in the method described in Patent Document 2, the UV absorber or light stabilizer used is expensive, so the manufacturing cost of the printing ink is high. Furthermore, when a UV absorber or light stabilizer is added to the printing ink, the ink's stability over time decreases and gelation may occur. Thus, further research is needed to develop printing inks that have excellent color reproducibility and durability, such as weather resistance and light resistance. In particular, research is needed to develop printing ink sets, printed matter, and packaging materials that have excellent color reproducibility and excellent light resistance both under sunlight and under white LED lighting. In addition, there is a growing need for ink sets that can reproduce a wider color gamut and have little color change over time for applications that require high design quality, such as packaging materials.

[0010] In view of the above, the present invention provides a printing ink set having excellent lightfastness and excellent color reproducibility. The present invention also provides a printed matter and a packaging material using the printing ink set, which have excellent design, lightfastness, and adhesion of the printed layer. [Means for solving the problem]

[0011] The embodiments of the present invention relate to the following. However, the embodiments of the present invention are not limited to the following and include various embodiments. [1] A yellow ink comprising an isoindoline compound represented by the following general formula (1) or CI Pigment Yellow 180 and a dispersion medium: A cyan ink comprising a phthalocyanine pigment and a dispersion medium; a magenta ink A comprising a dioxazine pigment and a dispersing medium; and A printing ink set comprising a magenta ink B containing at least one pigment selected from the group consisting of CI Pigment Red 122, CI Pigment Violet 19, a diketopyrrolopyrrole pigment represented by the following general formula (101), and a perylene pigment represented by the following general formula (201), and a dispersion medium.

[0012] [ka]

[0013] [In general formula (1), R1 to R4 each independently represent a hydrogen atom, an alkyl group, or an alkoxy group. R5 and R6 each independently represent a hydrogen atom or an alkyl group. X1 represents -O- or -NH-, and R7 represents a hydrogen atom, an alkyl group, or an aryl group.] [In general formula (101), R 151 ~R 160 each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, a thioalkyl group, a cyano group, or an aryl group. [In the general formula (201), X2 is -O- or -NR 201 - represents R 201represents a hydrogen atom, an alkyl group, or an aryl group which may have a substituent.

[0014] [2] The printing ink set according to [1], wherein the isoindoline compound represented by the general formula (1) includes at least one compound selected from the group consisting of the following formulas (4) and (5):

[0015] [ka]

[0016] [3] The printing ink set according to [1] or [2], which is used for gravure printing. [4] The printing ink set according to [1] or [2], which is used for flexographic printing. [5] A printed matter having a substrate and a printed layer formed from the printing ink set according to any one of [1] to [4].

[0017] [6] A printed matter having four types of image areas consisting of at least yellow, cyan, and two types of magenta on a substrate, A yellow image portion containing an isoindoline compound represented by the following general formula (1) or CI Pigment Yellow 180 and a dispersion medium, a cyan image portion comprising a phthalocyanine pigment and a dispersing medium; a magenta image portion A comprising a dioxazine pigment and a dispersing medium; and A printed matter having a magenta image portion B containing at least one pigment selected from the group consisting of CI Pigment Red 122, CI Pigment Violet 19, a diketopyrrolopyrrole pigment represented by the following general formula (101), and a perylene pigment represented by the following general formula (201), and a dispersion medium.

[0018] [ka]

[0019] [In general formula (1), R1 to R4 each independently represent a hydrogen atom, an alkyl group, or an alkoxy group. R5 and R6 each independently represent a hydrogen atom or an alkyl group. X1 represents -O- or -NH-, and R7 represents a hydrogen atom, an alkyl group, or an aryl group.] [In general formula (101), R 151 ~R 160 each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, a thioalkyl group, a cyano group, or an aryl group. [In the general formula (201), X2 is -O- or -NR 201 - represents R 201 represents a hydrogen atom, an alkyl group, or an aryl group which may have a substituent. [7] A packaging material having the printed matter described in [5]. [8] A packaging material having the printed matter described in [6]. Effect of the Invention

[0020] According to the present invention, it is possible to provide a printing ink set having a color gamut equal to or greater than that of conventional printing ink sets, excellent lightfastness, and high color reproducibility. Furthermore, by using the printing ink set, it is possible to provide printed matter and packaging materials having excellent design and excellent lightfastness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] First, the terms used in this specification are defined. When written as "(meth)acryloyl" or "(meth)acrylic", it means "acryloyl and / or methacryloyl" or "acrylic and / or methacrylic", respectively, unless otherwise specified. Similarly, when written as "(meth)acrylic acid", "(meth)acrylate", or "(meth)acrylamide", it means "acrylic acid and / or methacrylic acid", "acrylate and / or methacrylate", or "acrylamide and / or methacrylamide", respectively. Also, "CI" stands for Color Index (CI). In this specification, any numerical range specified using "to" is intended to include the numerical values ​​before and after "to" as the lower and upper limit values ​​of the range. The various components described in this specification may be used independently, either alone or in combination of two or more, unless otherwise noted.

[0022] The average primary particle size of the pigment is a value obtained by directly measuring the size of the primary particles from electron micrographs taken with a transmission electron microscope (TEM). These can be measured by the method described in the Examples section.

[0023] Furthermore, the numerical values ​​specified in this specification are values ​​determined by the methods disclosed in the embodiments or examples.

[0024] Hereinafter, an embodiment of the present invention will be described. However, the present invention is not limited to the following description and includes various embodiments. <Printing ink set> One embodiment of the present invention relates to a printing ink set (hereinafter, also simply referred to as an ink set) having printing inks of at least three primary colors. The printing ink set includes a yellow ink containing an isoindoline compound represented by general formula (1) or CI Pigment Yellow 180 and a dispersion medium, a cyan ink containing a phthalocyanine pigment and a dispersion medium, a magenta ink A containing a dioxazine pigment and a dispersion medium, and a magenta ink B containing at least one pigment selected from the group consisting of CI Pigment Red 122, CI Pigment Violet 19, a diketopyrrolopyrrole pigment represented by general formula (101), and a perylene pigment represented by general formula (201), and a dispersion medium.

[0025] In one embodiment, the printing ink set may further include other inks, such as black ink, white ink, and special color ink, in addition to the above four printing inks.

[0026] The printing ink set of this embodiment can be applied to various printing methods. The printing ink set can be used as a printing ink set of, for example, offset printing ink, flexographic printing ink, gravure printing ink, screen printing ink, etc. Among them, gravure printing ink set and flexographic printing ink set are preferable, and these can be suitably used for packaging material applications. Since the printing ink set of this embodiment uses the above four printing inks and has high color reproducibility even without using special color inks, it has the effect of reducing the number of steps of changing plates or colors to use special color inks or toned inks each time, particularly in gravure printing and flexographic printing, and enabling efficient printing.

[0027] The inks of each color in the printing ink set of this embodiment will be described below. <Yellow ink> The yellow ink in the printing ink set of this embodiment contains an isoindoline compound represented by general formula (1) (isoindoline compound (1)) or CI Pigment Yellow 180, and a dispersion medium described below. The yellow ink forms a yellow image portion in a printed matter by printing.

[0028] [Isoindoline compound (1)] Hereinafter, the isoindoline compound represented by general formula (1) will also be referred to as isoindoline compound (1).

[0029] [ka]

[0030] In the general formula (1), R1 to R4 each independently represent a hydrogen atom, an alkyl group, or an alkoxy group. R5 and R6 each independently represent a hydrogen atom or an alkyl group. X1 represents -O- or NH-, and R7 represents a hydrogen atom, an alkyl group, or an aryl group.

[0031] The isoindoline compound (1) can be used alone or in combination of two or more kinds.

[0032] In general formula (1), the number of carbon atoms in the alkyl group (-R) in R1 to R4 is preferably 1 to 20, more preferably 1 to 10, even more preferably 1 to 4, and still more preferably 1 to 3. An alkyl group having 1 or 2 carbon atoms is most preferred. The alkyl group may be a straight chain structure, a branched structure, a single ring structure, or a fused polycyclic structure. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, an octadecyl group, an isopropyl group, an isobutyl group, an isopentyl group, a 2-ethylhexyl group, a 2-hexyldodecyl group, a sec-butyl group, a tert-butyl group, a sec-pentyl group, a tert-pentyl group, a tert-octyl group, a neopentyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, an adamantyl group, a norbornyl group, a bornyl group, and a 4-decylcyclohexyl group.

[0033] In the above alkyl group, at least one hydrogen atom may be substituted with another substituent such as a halogen atom, a hydroxyl group, an alkoxy group, a carboxyl group, an ester group, a sulfo group, a sulfanyl group, a sulfamoyl group, an amino group, an alkylamino group, or an amide group. In addition, a plurality of substituents may be present. The substituents are not limited to those mentioned above.

[0034] The alkyl group may have a structure in which two or more alkyl groups (one of which is an alkylene group) are bonded to each other via a linking group. Specific examples of the linking group include an ester bond (-COO-), an ether bond (-O-), and a sulfide bond (-S-). That is, in this specification, the alkyl group may be, for example, a group represented by "-R'-OR" (R' represents an atomic group obtained by removing one hydrogen atom from the alkyl group). A specific example is -C2H4-O-C2H5.

[0035] In the general formula (1), the alkoxy group in R1 to R4 is a group (-OR) in which an oxygen atom is bonded to the above-mentioned alkyl group (-R).

[0036] In general formula (1), the alkyl groups (-R) in R5 to R7 are the same as the alkyl groups in R1 to R4.

[0037] In the general formula (1), the aryl group (-Ar) in R7 is an atomic group obtained by removing one hydrogen atom from an aromatic hydrocarbon. The number of carbon atoms is preferably 6 to 30, and more preferably 6 to 20. Examples of the aryl group include a phenyl group, a tolyl group, a biphenylyl group, a terphenylyl group, a quaterphenylyl group, a pentalenyl group, an indenyl group, a naphthyl group, a binaphthalenyl group, a ternaphthalenyl group, a quaternaphthalenyl group, an azulenyl group, a heptalenyl group, a biphenylenyl group, an indacenyl group, a fluoranthenyl group, an acephenanthrylenyl group, an aceanthryllenyl group, a phenalenyl group, a fluorenyl group, an anthryl group, a bianthracenyl group, a tert ... Examples of the alkyl group include anthracenyl, quaternary anthracenyl, anthraquinolyl, phenanthryl, triphenylenyl, pyrenyl, chrysenyl, naphthacenyl, pleiadenyl, picenyl, perylenyl, pentaphenyl, pentacenyl, tetraphenylenyl, hexaphenyl, hexacenyl, rubicenyl, coronenyl, trinaphthylenyl, heptaphenyl, heptacenyl, pyrantrenyl, and ovalenyl. Of these, phenyl and tolyl groups are preferred.

[0038] The aryl group may have at least one hydrogen atom substituted with another substituent such as a halogen atom, a hydroxyl group, an alkoxy group, a carboxyl group, an ester group, a sulfo group, a sulfanyl group, a sulfamoyl group, an amino group, an alkylamino group, or an amide group. The aryl group may have a plurality of substituents. The substituents are not limited to those mentioned above.

[0039] In formula (1), X1 represents -O- or -NH-, and is preferably -NH-.

[0040] The isoindoline compound represented by the general formula (1) preferably includes at least one compound selected from the group consisting of the following formulae (4) and (5).

[0041] [ka]

[0042] By using an isoindoline compound represented by formula (4) (hereinafter also referred to as isoindoline compound (4)) or an isoindoline compound represented by formula (5) (hereinafter also referred to as isoindoline compound (5)), it is possible to achieve both higher color reproducibility and light fastness.

[0043] [Method for producing isoindoline compound (1)] As shown in the following scheme 1-1, the isoindoline compound (1) can be synthesized using 1,3-diiminoisoindoline represented by formula (6) (hereinafter also referred to as compound (6)) as a starting material. The synthesis method will be described below along with a specific example of the isoindoline compound (1). In the following description, the numbers in each formula are written as the compound numbers.

[0044] [ka]

[0045] Scheme 1-1 may include a first step (S1) of reacting compound (6) with compound (7) in the presence of an aqueous ammonia solution; and then a second step (S2) of reacting compound (8) with compound (9) in the presence of acetic acid. In the first step (S1) of Scheme 1-1, when a 28% aqueous ammonia solution is used, the amount of the aqueous ammonia used is preferably 1 to 20 times, and more preferably 1 to 5 times, 100 parts by mass of compound (6). The reaction temperature in each step in Scheme 1-1 is preferably about 10 to 100°C.

[0046] When the relationship between the substituents R1 and R4, the relationship between the substituents R2 and R3, or the relationship between the substituents R5 and R6 of the isoindoline compound (1) is asymmetric, the final product is obtained as a mixture containing isomers. The isoindoline compound (1) may be either a mixture containing isomers or a single compound.

[0047] It is preferable to prepare a pigment by subjecting the isoindoline compound (1) to a particle size regulation treatment or surface treatment by a known method, such as a dissolution precipitation method typified by acid pasting, solvent salt milling, dry milling, etc.

[0048] [CI Pigment Yellow 180] CI Pigment Yellow 180 is a pigment composed of a compound represented by the following formula (10) and is produced by a known method.

[0049] [ka]

[0050] The average primary particle diameter of CI Pigment Yellow 180 is preferably 70 to 250 nm, more preferably 100 to 200 nm. By making the average primary particle diameter 250 nm or less, transparency is improved and high color reproducibility can be obtained. In addition, by making the average primary particle diameter 70 nm or more, light resistance is further improved.

[0051] The yellow ink may further contain yellow pigments other than the above pigments (hereinafter referred to as other yellow pigments), resins, organic solvents, pigment dispersants, and other additives, etc., within the scope of the invention.

[0052] [Other yellow pigments] Other yellow pigments include, for example, isoindoline compounds represented by the following general formulas (2-1) and (2-2), CI Pigment Yellow 12, CI Pigment Yellow 13, CI Pigment Yellow 14, CI Pigment Yellow 17, CI Pigment Yellow 83, CI Pigment Yellow 93, CI Pigment Yellow 95, CI Pigment Yellow 109, CI Pigment Yellow 110, CI Pigment Yellow 120, CI Pigment Yellow 138, CI Pigment Yellow 151, CI Pigment Yellow 155, and CI Pigment Yellow 174. However, the use of these other yellow pigments should be kept to a minimum as there is a risk of reducing lightfastness or color gamut.

[0053] [ka]

[0054] In general formula (2-1), R 11 ~R 14 R each independently represents a hydrogen atom, an alkyl group, or an alkoxy group. 15 ~R 18 each independently represents a hydrogen atom or an alkyl group. In addition, in the general formula (2-2), R 19 represents an alkyl group which may have a substituent.

[0055] In general formula (2-1), R 11 ~R 14 The alkyl group (-R) and alkoxy group in R1 to R4 are the same as the alkyl group and alkoxy group in R1 to R4 in general formula (1). 15 ~R 18 The alkyl group (-R) in the formula (1) is the same as the alkyl group in R5 to R6 in the formula (1). In addition, in the general formula (2-2), R 19 The alkyl group (-R) in the formula (1) is the same as the alkyl group in R1 to R4 in the formula (1), and the same applies to the substituent.

[0056] From the viewpoint of color reproducibility, the higher the content of isoindoline compound (1) and CI Pigment Yellow 180 is, the more preferable it is, based on the total pigment contained in the yellow ink (100% by mass), and specifically, it is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. When both isoindoline compound (1) and CI Pigment Yellow 180 are contained, it is preferable that the total is equal to or more than the above content.

[0057] <Cyan ink> The cyan ink in the printing ink set of this embodiment contains a phthalocyanine pigment and a dispersion medium described below. The cyan ink forms a cyan image portion on a printed matter by printing.

[0058] [Phthalocyanine pigment] Magenta Ink A The phthalocyanine pigment is a pigment composed of a compound represented by the following general formula (3), and can be produced by a known method.

[0059] [ka]

[0060] In general formula (3), R 101 ~R 116Each independently represents a hydrogen atom, a halogen atom, and an alkyl group, an aryl group, an alkoxyl group, and an aryloxy group, which may have a substituent. M represents two hydrogen atoms, two monovalent metal atoms, a divalent metal atom, a trivalent substituted metal atom, a tetravalent substituted metal atom, or a metal oxide atom. In one embodiment, the phthalocyanine pigment is preferably a metal phthalocyanine pigment. That is, M is preferably two monovalent metal atoms, a divalent metal atom, a trivalent substituted metal atom, a tetravalent substituted metal atom, or a metal oxide atom. M is more preferably a divalent metal atom, a trivalent substituted metal atom, a tetravalent substituted metal atom, or a metal oxide atom, and even more preferably a divalent metal atom.

[0061] The alkyl group may be a straight-chain or branched-chain alkyl group. Specific examples include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, an octadecyl group, an isopropyl group, an isobutyl group, an isopentyl group, a 2-ethylhexyl group, a sec-butyl group, a tert-butyl group, a sec-pentyl group, a tert-pentyl group, a tert-octyl group, and a neopentyl group. The number of carbon atoms in the alkyl group is preferably within the range of 1 to 30.

[0062] Examples of the substituent in the alkyl group include halogen atoms such as fluorine, chlorine, and bromine, hydroxyl groups, amino groups, nitro groups, formyl groups, cyano groups, and carboxyl groups, as well as aryl groups, cycloalkyl groups, and heterocyclic groups, which will be described later. In addition, those in which a part of the structure is substituted with an ester bond (-COO-) or an ether bond (-O-) are also included as the substituent.

[0063] Therefore, the substituted alkyl group means an alkyl group substituted with the above-mentioned substituent. It may be substituted with one or more substituents. For example, specific examples of the alkyl group substituted with a halogen atom include a trifluoromethyl group, a 2,2,2-trifluoroethyl group, -(CF2)4CF3, -(CF2)5CF3, -(CF2)6CF3, -(CF2)7CF3, -(CF2)8CF3, a trichloromethyl group, and a 2,2-dibromoethyl group.

[0064] The aryl group may be a monocyclic or condensed polycyclic aryl group, such as a phenyl group, a 1-naphthyl group, a 2-naphthyl group, a p-biphenyl group, a m-biphenyl group, a 2-anthryl group, a 9-anthryl group, a 2-phenanthryl group, a 3-phenanthryl group, a 9-phenanthryl group, a 2-fluorenyl group, a 3-fluorenyl group, a 9-fluorenyl group, a 1-pyrenyl group, a 2-pyrenyl group, a 3-perylenyl group, an o-tolyl group, a m-tolyl group, a p-tolyl group, a 4-methylbiphenyl group, a terphenyl group, a 4-methyl-1-naphthyl group, a 4-tert-butyl-1-naphthyl group, a 4-naphthyl-1-naphthyl group, a 6-phenyl-2-naphthyl group, a 10-phenyl-9-anthryl group, a spirofluorenyl group, a 2-benzocyclobutenyl group, etc. The number of carbon atoms in the aryl group is preferably within the range of 6 to 18. Examples of the substituent of the substituted aryl group include the same substituents as the substituents in the alkyl group described above.

[0065] The alkoxyl group may be a linear or branched alkoxyl group. Specific examples include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a tert-butoxy group, a neopentyloxy group, a 2,3-dimethyl-3-pentyloxy group, an n-hexyloxy group, an n-octyloxy group, a stearyloxy group, and a 2-ethylhexyloxy group. The number of carbon atoms in the alkoxyl group is preferably within the range of 1 to 6. The substituent of the substituted alkoxyl group may be the same as the substituent in the alkyl group described above.

[0066] The aryloxy group may be a monocyclic or condensed polycyclic aryloxy group. Specific examples include a phenoxy group, a p-methylphenoxy group, a naphthyloxy group, and an anthryloxy group. The aryloxy group is preferably a monocyclic aryloxy group. In addition, an aryloxy group having 6 to 12 carbon atoms is preferable.

[0067] Examples of the monovalent metal atom of M include Na, K, and Li. Examples of the metal atom contained in the divalent metal atom, trivalent substituted metal atom, tetravalent substituted metal atom, or oxidized metal atom of M include metal atoms belonging to Groups 2 to 15 of the periodic table. Specific examples of the divalent metal atom include Cu, Zn, Fe, Co, Ni, Ru, Pb, Rh, Pd, Pt, Mn, Sn, Pb, Ca, and Mg. Examples of trivalent substituted metal atoms include metal atoms such as Al, Ga, In, Tl, Cr, Mn, Fe, and Ru, to which a substituent such as a halogen atom (-F, -Cl, -Br, -I), a hydroxyl group, an aryl group which may have a substituent, an aryloxy group, a silyloxy group, a phosphinyl group, or a phosphonyl group is bonded. Examples of tetravalent substituted metal atoms include metal atoms such as Cr, Si, Zr, Ge, Sn, Ti, and Mn to which two substituents such as a halogen atom (-F, -Cl, -Br, -I), a hydroxyl group, an aryl group which may have a substituent, an aryloxy group, a silyloxy group, a phosphinyl group, and a phosphonyl group are bonded. Examples of the metal oxide atom include VO, MnO, and TiO. M is preferably Cu, Zn, Fe, Ca, Mg, Al-OH, or TiO, more preferably Cu, Al-OH, or TiO, and even more preferably Cu.

[0068] Among the compounds of general formula (3), preferred are copper phthalocyanine (compound (11)) in which M is Cu, aluminum phthalocyanine (compound (12)) in which M is Al-OH, and titanyl phthalocyanine (compound (13)) in which M is TiO.

[0069] [ka]

[0070] In one embodiment, the phthalocyanine pigment may be CI Pigment Blue 15, CI Pigment Blue 15:1, CI Pigment Blue 15:2, CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 15:6, CI Pigment Blue 16, etc. Among them, it is preferable to include at least one copper phthalocyanine pigment selected from the group consisting of CI Pigment Blue 15:3, CI Pigment Blue 15:4, and CI Pigment Blue 15:6, and it is more preferable to include CI Pigment Blue 15:3 or CI Pigment Blue 15:4.

[0071] The cyan ink may further contain blue pigments other than the above pigments (hereinafter referred to as other blue pigments), resins, organic solvents, pigment dispersants, and other additives, etc., within the scope of the invention.

[0072] Other examples of blue pigments include CI Pigment Blue 60.

[0073] Among the pigments contained in the cyan ink, the higher the phthalocyanine pigment content, the better. Specifically, the content is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, and particularly preferably 95 mass% or more.

[0074] The printing ink set of this embodiment is characterized by including two types of magenta ink, magenta ink A and magenta ink B, which will be described later. <Magenta Ink A> The magenta ink A in the printing ink set of this embodiment contains a dioxazine pigment and a dispersion medium described below. The magenta ink A forms a magenta image portion A in a printed matter by printing.

[0075] [Dioxazine pigments] The dioxazine pigment may be a pigment made of a compound represented by the following general formula (301), and may be produced by a known method. The method for producing the dioxazine pigment used in the present invention is not particularly limited, and may be, for example, the method described on page 196 of High Performance Pigments published by Wiley-VCH Verlag-GmbH (2009). The method for producing the dioxazine pigment is not limited to this method.

[0076] [ka]

[0077] In general formula (301), R 201 ~R 203 R each independently represents a hydrogen atom, a hydroxyl group, an alkyl group, an aryl group, an amino group, an alkoxyl group, or an alkenyl group which may have a substituent. 204 and R 205 R each independently represents a hydrogen atom, an alkyl group, an aryl group, or an acyl group which may have a substituent. 206 and R 207 each independently represents a hydrogen atom, a halogen atom, an alkyl group which may have a substituent, an amino group, or a COOR 208 Represents R 208 R represents an alkyl group. 201 and R 202 , R 202 and R 204 , and R 203 and R 205 may be bonded to each other to form a ring.

[0078] In general formula (301), R 201 ~R 208The alkyl group in the formula (3) is 101 ~R 116 The alkyl groups are the same as those in the above.

[0079] In general formula (301), R 201 ~R 205 The aryl group in the formula (3) is R 101 ~R 116 The same applies to the aryl group in the above formula (I).

[0080] In general formula (301), R 201 ~R 203 The alkoxyl group in the formula (3) is R 101 ~R 116 The same applies to the alkoxyl group in the above formula (I).

[0081] In general formula (301), R 201 ~R 203 Examples of the alkenyl group in include a vinyl group, a 1-propenyl group, an allyl group, a 2-butenyl group, a 3-butenyl group, an isopropenyl group, an isobutenyl group, a 1-pentenyl group, a 2-pentenyl group, a 3-pentenyl group, a 4-pentenyl group, a 1-hexenyl group, a 2-hexenyl group, a 3-hexenyl group, a 4-hexenyl group, and a 5-hexenyl group. Of these, a vinyl group and an allyl group are preferred.

[0082] In general formula (301), R 201 ~R 203 are preferably each independently a hydrogen atom, an aryl group, or an alkoxy group. 204 and R 205 are each preferably independently a hydrogen atom, an alkyl group, or an acyl group. Among alkyl groups, an ethyl group is particularly preferred, and among acyl groups, a benzoyl group is particularly preferred. 206 and R 207 are each preferably independently a hydrogen atom, a halogen atom, or an amino group which may have a substituent. Among halogen atoms, a chlorine atom is particularly preferred. Among amino groups which may have a substituent, an acetylamino group is particularly preferred.

[0083] Preferred dioxazine pigments are dioxazine pigments (302) to (313) represented by the following formulas (302) to (313).

[0084] [ka]

[0085] [ka]

[0086] In one embodiment, the dioxazine pigment preferably includes at least one dioxazine pigment selected from the group consisting of CI Pigment Violet 23, CI Pigment Violet 37, and CI Pigment Violet 57, and more preferably includes CI Pigment Violet 23 and / or CI Pigment Violet 37.

[0087] From the viewpoint of color reproducibility, the higher the dioxazine pigment content is, the more preferable it is, based on the total pigments contained in magenta ink A (100% by mass), and specifically, it is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. When multiple types of pigments are contained as the dioxazine pigment, it is preferable that the total be equal to or greater than the above content.

[0088] <Magenta Ink B> Magenta ink B in the printing ink set of this embodiment contains at least one pigment selected from the group consisting of CI Pigment Red 122, CI Pigment Violet 19, a diketopyrrolopyrrole pigment represented by the following general formula (101), and a perylene pigment represented by the following general formula (201), and a dispersion medium described below. Magenta ink B forms magenta image portion B in a printed matter by printing.

[0089] The pigment contained in Magenta Ink B is not limited as long as it contains at least one of CI Pigment Red 122, CI Pigment Violet 19, a diketopyrrolopyrrole pigment represented by general formula (101), and a perylene pigment represented by general formula (201). However, it is preferable to use CI Pigment Red 122, CI Pigment Violet 19, a diketopyrrolopyrrole pigment represented by general formula (101), or a perylene pigment represented by general formula (201) alone. Furthermore, even if a dioxazine pigment is contained as a pigment, if the main component in the pigment is at least any one of CI Pigment Red 122, CI Pigment Violet 19, the diketopyrrolopyrrole pigment represented by general formula (101), and the perylene pigment represented by general formula (201), it is considered to be magenta ink B. However, if the content of the dioxazine pigment, CI Pigment Red 122, CI Pigment Violet 19, the diketopyrrolopyrrole pigment represented by general formula (101), and the perylene pigment represented by general formula (201) is the same, it is defined as magenta ink A.

[0090] [CI Pigment Red 122] CI Pigment Red 122 may be mixed with other quinacridone compounds such as CI Pigment Red 202, CI Pigment Red 209, and CI Pigment Violet 19. However, in order to maximize the effects of the present invention, it is preferable to use CI Pigment Red 122 alone as the pigment.

[0091] The average primary particle diameter of CI Pigment Red 122 is preferably 50 to 150 nm, more preferably 60 to 130 nm. When the average primary particle diameter is 150 nm or less, transparency is improved and high color reproducibility can be obtained. In addition, when the average primary particle diameter is 50 nm or more, light resistance is further improved.

[0092] [CI Pigment Violet 19] CI Pigment Violet 19 has a crystal polymorphism, and the crystal form is preferably the γ type.

[0093] CI Pigment Violet 19 may be mixed with other quinacridone compounds such as CI Pigment Red 122, CI Pigment Red 202, and CI Pigment Red 209. However, in order to maximize the effects of the present invention, it is preferable to use CI Pigment Violet 19 alone as the pigment.

[0094] The average primary particle diameter of CI Pigment Violet 19 is preferably 30 to 120 nm, more preferably 40 to 100 nm. When the average primary particle diameter is 120 nm or less, transparency is improved and high color reproducibility can be obtained. In addition, when the average primary particle diameter is 30 nm or more, light resistance can be further improved.

[0095] [Diketopyrrolopyrrole pigment (101)] Hereinafter, the diketopyrrolopyrrole pigment represented by the general formula (101) will also be referred to as diketopyrrolopyrrole pigment (101) or DPP pigment (101). [ka]

[0096] In general formula (101), R 151 ~R 160 each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, a thioalkyl group, a cyano group, or an aryl group.

[0097] The DPP pigment (101) can be used alone or in combination of two or more kinds.

[0098] In general formula (101), R 151 ~R 160 Examples of the halogen atom in the formula include fluorine, chlorine, and bromine.

[0099] In general formula (101), R 151~R 160 The alkyl group in this group is the same as the alkyl group in R1 to R4 in general formula (1).

[0100] In general formula (101), R 151 ~R 160 The alkoxy group in the above formula is a group (-OR) in which an oxygen atom is bonded to the above alkyl group (-R).

[0101] In general formula (101), R 151 ~R 160 The thioalkyl group in the formula (I) is a group (-SR) in which a sulfur atom is bonded to the above-mentioned alkyl group (-R).

[0102] In general formula (101), R 151 ~R 160 The aryl group in is the same as the aryl group in R7 in general formula (1).

[0103] The method for producing the DPP pigment (101) used in the present invention is not particularly limited. For example, as disclosed in JP-A-58-210084, the DPP pigment can be produced by reacting a corresponding aromatic nitrile with a succinic acid diester in an organic solvent.

[0104] The DPP pigment (101) is preferably DPP pigments (102) to (119) represented by the following formulas (102) to (119).

[0105] [ka]

[0106] [ka]

[0107] Further, examples of the DPP pigment (101) include CI Pigment Red 254, CI Pigment Red 255, CI Pigment Red 264, CI Pigment Red 272, CI Pigment Red 283, CI Pigment Red 291, CI Pigment Orange 71, and CI Pigment Orange 73. Among these, it is preferable to contain at least one DPP pigment (101) selected from the group consisting of CI Pigment Red 254, CI Pigment Red 255, CI Pigment Red 264, CI Pigment Red 272, CI Pigment Red 291, CI Pigment Orange 71, and CI Pigment Orange 73, and it is more preferable to contain CI Pigment Red 254, CI Pigment Red 255, CI Pigment Red 264, CI Pigment Red 272, or CI Pigment Orange 73. By using such a DPP pigment (101), when combined with a yellow ink containing the isoindoline compound (1) or CI Pigment Yellow 180, an ink set having a wider range of color reproducibility and high lightfastness can be obtained.

[0108] The average primary particle size of the DPP pigment (101) is preferably 30 to 350 nm, more preferably 50 to 150 nm. When the average primary particle size is 350 nm or less, transparency is improved and high color reproducibility can be obtained. In addition, when the average primary particle size is 30 nm or more, light resistance is further improved.

[0109] The average primary particle diameter of CI Pigment Red 254 is preferably 30 to 250 nm, more preferably 60 to 130 nm. By making the average primary particle diameter 250 nm or less, transparency is improved and high color reproducibility can be obtained. By making the average primary particle diameter 30 nm or more, light resistance is further improved.

[0110] The average primary particle diameter of CI Pigment Red 264 is preferably 30 to 250 nm, more preferably 40 to 150 nm. By making the average primary particle diameter 250 nm or less, transparency is improved and high color reproducibility can be obtained. In addition, by making the average primary particle diameter 30 nm or more, light resistance is further improved.

[0111] [Perylene pigments (201)] Hereinafter, the perylene pigment represented by general formula (201) will also be referred to as perylene pigment (201). [ka]

[0112] X2 is -O- or -NR 201 - represents R 201 represents a hydrogen atom, an alkyl group, or an aryl group which may have a substituent.

[0113] The perylene pigment (201) can be used alone or in combination of two or more kinds.

[0114] In the general formula (201), the alkyl group in X2 is the same as the alkyl group in R1 to R4 in the general formula (1).

[0115] In the general formula (201), the aryl group for X2 may have a substituent, and is the same as the aryl group for R7 in the general formula (1).

[0116] The method for producing the perylene pigment (201) used in the present invention is not particularly limited, and examples thereof include those described in W. Herbst, K. Hunger, Industrial Organic Pigments: Production, Properties, Applications, 1993, pp. 467-480, etc. The method for producing the perylene pigment is not limited to this method.

[0117] The perylene pigment (201) is preferably perylene pigments (202) to (214) represented by the following formulas (202) to (214).

[0118] [ka]

[0119] [ka]

[0120] Examples of the perylene pigment (201) include CI Pigment Red 123, CI Pigment Red 149, CI Pigment Red 178, CI Pigment Red 179, CI Pigment Red 189, CI Pigment Red 190, CI Pigment Red 224, and CI Pigment Violet 29. Among these, it is preferable to include at least one perylene pigment (201) selected from the group consisting of CI Pigment Red 149, CI Pigment Red 179, CI Pigment Red 190, and CI Pigment Red 224, and it is more preferable to include CI Pigment Red 149 or CI Pigment Red 179. The use of such a perylene pigment (201) is preferable because, when combined with an isoindoline compound (1) or a yellow ink containing CI Pigment Yellow 180, an ink set having a wider range of color reproducibility and high lightfastness can be obtained.

[0121] The average primary particle size of the perylene pigment (201) is preferably 20 to 200 nm, more preferably 40 to 150 nm. When the average primary particle size is 200 nm or less, transparency is improved and high color reproducibility can be obtained. In addition, when the average primary particle size is 20 nm or more, light resistance is further improved.

[0122] From the viewpoint of color reproducibility, the higher the content of CI Pigment Red 122, CI Pigment Violet 19, DPP Pigment (101) and Perylene Pigment (201) is, the more preferable it is, and specifically, it is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, based on the total pigments contained in Magenta Ink B (100% by mass). When two or more pigments from CI Pigment Red 122, CI Pigment Violet 19, DPP Pigment (101) and Perylene Pigment (201) are contained, it is preferable that the total is equal to or more than the above content.

[0123] In one embodiment, magenta ink A and magenta ink B may be a combination of inks whose hue angle (H°) calculated based on the following formula (A) is 0° or more and less than 90°, or 300° or more and less than 360°. In formula (A), * and b * is the L standard defined by the CIE (International Commission on Illumination). * a * b * In color space, a * and b * It represents the value obtained by measuring a * and b * The value of can be measured, for example, using a spectrophotometer (trade name: Spectrolino; manufactured by Gretag Macbeth). * and b * The spectrophotometer used for the measurement is not limited to the above. Formula (A) a * ≧0, b * ≧0 (first quadrant), H°=tan -1 (b * / a * ) a * ≦0, b * ≧0 (second quadrant), H°=180+tan -1 (b * / a *) a * ≦0, b * ≦0 (third quadrant), H°=180+tan -1 (b * / a * ) a * ≧0, b * ≦0 (fourth quadrant), H°=360+tan -1 (b * / a * )

[0124] In one embodiment, the hue angle of magenta ink A (H A °) and Magenta Ink B (H B It is preferable that the relationship between the temperature (°) and the surface area (°) satisfies the following criteria: (1) 300≦H A °<360, 300≦H B If °<360, H A ° <H B ° (2) 300≦H A °<360, 0≦H B If °<90, H A °>H B ° (3) 0≦H A °<90, 0≦H B If °<90, H A ° <H B °

[0125] Magenta ink A and magenta ink B may each further contain red pigments other than the above pigments (hereinafter referred to as other red pigments), resins, organic solvents, pigment dispersants, and other additives, etc., within the scope of the invention.

[0126] Other red pigments include, for example, CI Pigment Red 2, CI Pigment Red 32, CI Pigment Red 48:1, CI Pigment Red 48:2, CI Pigment Red 48:3, CI Pigment Red 53:1, CI Pigment Red 57:1, CI Pigment Red 63:1, CI Pigment Red 81, CI Pigment Red 144, CI Pigment Red 146, CI Pigment Red 150, CI Pigment Red 166, CI Pigment Red 170, C Pigment Red 238, CI Pigment Red 242, CI Pigment Red 260, CI Pigment Red 269, and the like. However, it is best to keep its use to a minimum as it may reduce light resistance and the color gamut.

[0127] Components other than the pigment will be described below. The components described below are included in the printing ink of the present embodiment, or can be added as necessary. <Pigments> The printing ink set of this embodiment may further contain the pigments shown below in addition to the pigments described above. Examples of the additional pigments include organic pigments and inorganic pigments other than the pigments described above. In addition, the content of the pigment in the ink, together with the above-mentioned pigment, is preferably in the range of 0.1 to 60 mass % based on the mass of the ink in order to ensure the concentration and coloring power of the ink, and is preferably in the range of 10 to 90 mass % based on the mass of the non-volatile matter of the ink.

[0128] [Organic pigments] The pigment to be added is preferably an organic pigment, such as a soluble azo pigment, an insoluble azo pigment, an azo pigment, a phthalocyanine pigment, a halogenated phthalocyanine pigment, anthraquinone pigment, anthanthrone pigment, dianthraquinonyl pigment, anthrapyrimidine pigment, perylene pigment, perinone pigment, quinacridone pigment, thioindigo pigment, isoindolinone pigment, quinophthalone pigment, azomethine azo pigment, flavanthrone pigment, diketopyrrolopyrrole pigment, isoindoline pigment, or indanthrone pigment.

[0129] Examples of these organic pigments are shown by their CI pigment numbers. An example of a purple pigment is CI Pigment Violet 32.

[0130] An example of a green pigment is CI Pigment Green 7.

[0131] Examples of orange pigments include CI Pigment Orange 13, CI Pigment Orange 34, CI Pigment Orange 38, CI Pigment Orange 43, and CI Pigment Orange 64.

[0132] The special color ink includes inks other than cyan, magenta, and yellow, such as purple, green, and vermilion. In one embodiment, the special color ink preferably contains the above-mentioned purple pigment, green pigment, orange pigment, and the like.

[0133] [Inorganic pigments] Examples of inorganic pigments include white inorganic pigments such as titanium oxide, zinc oxide, zinc sulfide, barium sulfate, calcium carbonate, magnesium carbonate, chromium oxide, silica, lithopone, antimony white, and gypsum, black inorganic pigments such as carbon black, iron black, and copper-chromium composite oxide, aluminum particles, mica, bronze powder, chrome vermilion, yellow lead, cadmium yellow, cadmium red, ultramarine, Prussian blue, red iron oxide, yellow iron oxide, zircon, etc. Among the above white inorganic pigments, barium sulfate, calcium carbonate, magnesium carbonate, silica, mica, etc. are often referred to as extender pigments.

[0134] For black ink, it is preferable to use carbon black, for example CI Pigment Black 7, from the viewpoint of excellent coloring power, hiding power, chemical resistance, and weather resistance. For white ink, it is preferable to use titanium oxide, for the viewpoint of excellent coloring power, hiding power, chemical resistance, and weather resistance. For the titanium oxide, it is preferable to use one that has been surface-treated with silica and / or alumina from the viewpoint of printing performance.

[0135] Each ink can use a single pigment or a combination of two or more pigments to achieve the desired color tone.

[0136] The average primary particle size of the pigment is preferably in the range of 10 to 200 nm, and more preferably in the range of 50 to 150 nm.

[0137] [Dye derivatives] Each of the inks constituting the printing ink set of this embodiment may contain a dye derivative. The dye derivative is a known compound having an acidic group, a basic group, a neutral group, etc. in an organic dye residue. Examples of the dye derivative include compounds having an acidic substituent such as a sulfo group, a carboxyl group, a phosphoric acid group, etc., and amine salts thereof, compounds having a sulfonamide group and a basic substituent such as a tertiary amino group at the terminal, and compounds having a neutral substituent such as a phenyl group and a phthalimidoalkyl group. Examples of organic pigments include diketopyrrolopyrrole pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, perinone pigments, perylene pigments, thiazine indigo pigments, triazine pigments, benzimidazolone pigments, indole pigments such as benzoisoindole, isoindoline pigments, isoindolinone pigments, quinophthalone pigments, naphthol pigments, threne pigments, metal complex pigments, and azo pigments such as azo, disazo, and polyazo.

[0138] The dye derivative may be a known dye derivative, and specific examples are described in the following documents: Diketopyrrolopyrrole dye derivatives: JP 2001-220520 A, WO 2009 / 081930 B, WO 2011 / 052617 B, WO 2012 / 102399 B, and JP 2017-156397 A Phthalocyanine dye derivatives: JP 2007-226161 A, WO2016 / 163351 Pamphlet, JP 2017-165820 A, and Japanese Patent No. 5753266 A Anthraquinone dye derivatives: JP-A-63-264674, JP-A-09-272812, JP-A-10-245501, JP-A-10-265697, JP-A-2007-079094, and WO2009 / 025325 pamphlet Quinacridone dye derivatives: JP-A-48-54128, JP-A-03-9961, and JP-A-2000-273383 Dioxazine dye derivatives: JP 2011-162662 A Thiazine indigo dye derivatives: JP 2007-314785 A Triazine dye derivatives: JP-A-61-246261, JP-A-11-199796, JP-A-2003-165922, JP-A-2003-168208, JP-A-2004-217842, and JP-A-2007-314681 Benzisoindole dye derivatives: JP 2009-57478 A Quinophthalone dye derivatives: JP2003-167112A, JP2006-291194A, JP2008-31281A, and JP2012-226110A Naphthol dye derivatives: JP 2012-208329 A and JP 2014-5439 A Azo dye derivatives: JP 2001-172520 A and JP 2012-172092 A

[0139] Acidic substituents are described in JP-A-2004-307854, and basic substituents are described in JP-A-2002-201377, JP-A-2003-171594, JP-A-2005-181383, JP-A-2005-213404, and the like. In the above-mentioned documents, the dye derivative may be referred to as a derivative, a pigment derivative, a dispersant, a pigment dispersant, or simply as a compound, etc. However, the compound having a substituent such as an acidic group, a basic group, or a neutral group in the organic dye residue is synonymous with the dye derivative.

[0140] The dye derivatives can be used alone or in combination of two or more kinds.

[0141] <Dispersion medium> Each ink constituting the printing ink set of this embodiment includes a dispersion medium. The dispersion medium appropriately disperses the pigment, exhibits the performance as an ink, and stabilizes the properties. Specific examples of the dispersion medium include a resin, a solvent, and a polymerizable compound. The resin may be a binder resin, a resin-type dispersant, etc. The solvent may be water or an organic solvent. The polymerizable compound may be a monomer or an oligomer. Furthermore, each ink may contain a low molecular weight dispersant such as a surfactant as a dispersion medium, if necessary. The dispersion medium can be appropriately selected depending on the form of the printing ink.

[0142] The dispersion medium will now be described in more detail. [resin] (binder resin) The binder resin may be any resin capable of forming a coating by printing. For example, it may be a polyolefin resin, a polyester resin, a styrene copolymer, an acrylic resin, or a modified resin thereof. Specifically, it may be a polyolefin resin such as polyethylene, such as high density polyethylene (HDPE), linear low density polyethylene (L-LDPE), low density polyethylene (LDPE), or polypropylene; a polyester resin such as polyethylene terephthalate; a styrene-p-chlorostyrene copolymer, a styrene-vinyl toluene copolymer, a styrene-vinyl naphthalene copolymer, a styrene-acrylic acid ester copolymer, a styrene-methacrylic acid ester copolymer, a styrene-α-chloromethyl methacrylate copolymer, a styrene-acrylonitrile copolymer, a styrene-vinyl methyl ether copolymer, a styrene-vinyl ethyl ether copolymer, a styrene-vinyl methyl ketone copolymer, a styrene-butadiene copolymer, or the like. copolymers, styrene copolymers such as styrene-isoprene copolymers and styrene-acrylonitrile-indene copolymers; acrylic resins, acrylic resins, and other acrylic resins; polyvinyl chloride, phenolic resins, naturally modified phenolic resins, natural resin modified maleic acid resins, silicone resins, polyurethane resins, ethylene-vinyl acetate copolymer resins, vinyl acetate resins, nitrocellulose resins, polyamide resins, epoxy resins, xylene resins, polyvinyl butyral resins, polyvinyl acetal resins, cellulose ester resins, alkyd resins, rosin resins, ketone resins, cyclized rubbers, chlorinated polyolefin resins, terpene resins, coumarone-indene resins, amino resins, petroleum resins, and modified resins thereof.

[0143] (Resin-type dispersant) The resin-type dispersant has a pigment affinity site that adsorbs to the pigment, and a relaxation site that has high affinity to components other than the pigment and causes steric repulsion between dispersed particles. The resin-type dispersant has an acidic group or a basic group. Examples of the acidic group include a carboxyl group, a sulfo group, and a phosphate group. Examples of the basic group include primary to tertiary amino groups and quaternary ammonium bases. Examples of acidic resin-type dispersants include urethane-based dispersants such as polyurethane, polycarboxylates such as polyacrylates, unsaturated polyamides, polycarboxylic acids, polycarboxylate (partial) amine salts, polycarboxylate ammonium salts, polycarboxylate alkylamine salts, polysiloxanes, long-chain polyaminoamide phosphates, hydroxyl-containing polycarboxylates, and modified products thereof; amides and salts thereof formed by the reaction of poly(lower alkyleneimines) with polyesters having free carboxyl groups; (meth)acrylic acid-styrene copolymers, (meth)acrylic acid-(meth)acrylic acid ester copolymers, styrene-maleic acid copolymers, polyvinyl alcohol, polyvinylpyrrolidone, and the like; polyesters, modified polyacrylates, ethylene oxide / propylene oxide adducts, and phosphate-based esters. Examples of basic resin-type dispersants for resin types such as acrylic resin, polyester resin, and urethane resin include nitrogen-atom-containing graft copolymers, and nitrogen-atom-containing acrylic block copolymers or urethane-based polymer dispersants having functional groups on the side chains including tertiary amino groups, quaternary ammonium bases, and nitrogen-containing heterocycles.

[0144] Resin-type dispersants are available as commercial products. Examples include the following: BASF Japan Ltd.'s JONCRYL67, JONCRYL678, JONCRYL586, JONCRYL611, JONCRYL683, JONCRYL690, JONCRYL57J, JONCRYL60J, JONCRYL61J, JONCRYL62J, JONCRYL63J, JONCRYLHPD-96J, JONCRYL501J, JONCRYLPDX-6102B, BYK-Chemie's DISPERBYK180, DISPERBYK187, DISPERBYK190, DISPERBYK191, DISPERBYK194, DISPERBYK2010, DISPERBYK2015, DISPERBYK2090, DISPERBYK2091, DISPERBYK2095, DISPERBYK2155, SOLSPERSE24000, SOLSPERSE32000, SOLSPERSE39000, SOLSPERSE41000 manufactured by Lubrizol Japan, Sartomer Corporation's SMA1000H, SMA1440H, SMA2000H, SMA3000H, SMA17352H, etc.

[0145] [solvent] (water) The water is preferably ion-exchanged water from which metal ions and the like have been removed, or distilled water.

[0146] (Organic solvent) Organic solvents can be classified into water-soluble solvents and water-insoluble solvents. Examples of the water-soluble solvent include methanol, ethanol, n-propanol, isopropanol, isobutanol, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, and glycerin. Examples of the non-water-soluble solvent include toluene, xylene, ethyl acetate, n-propyl acetate, butyl acetate, methyl ethyl ketone, methyl isobutyl ketone, butyl alcohol, and aliphatic hydrocarbons.

[0147] [Polymerizable compound] The polymerizable compound is a compound having one or more ethylenically unsaturated bonds in the molecule. The polymerizable compound includes a monomer and an oligomer.

[0148] (monomer) The monomer has a polymerizable group such as a (meth)acryloyl group, an allyl group, a vinyl group, a vinyl ether group, etc. In terms of curability, the monomer preferably contains a monomer having either a (meth)acryloyl group or a vinyl group, more preferably contains a monomer having 3 to 6 (meth)acryloyl groups in the molecule, and even more preferably contains a monomer having 6 (meth)acryloyl groups in the molecule.

[0149] Specific examples of monomers having a (meth)acryloyl group include, but are not limited to, the following: Monofunctional (meth)acrylate monomers having one (meth)acryloyl group in the molecule: 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, β-carboxyethyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, alkoxylated tetrahydrofurfuryl acrylate, caprolactone (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isoamyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, isodesyl (meth)acrylate, (meth)acrylate, 3,3,5-trimethylcyclohexanol (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, norbornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (oxyethyl) (meth)acrylate, 1,4-cyclohexanedimethanol (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, benzyl (meth)acrylate, EO-modified (2) nonylphenol acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate, acryloylmorpholine, etc.

[0150] Bifunctional (meth)acrylate monomers having two (meth)acryloyl groups in the molecule: 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol (200) di(meth)acrylate, polyethylene glycol (300) di(meth)acrylate, polyethylene glycol (400) di(meth)acrylate, polyethylene glycol Ricol (600) di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, EO modified (2) 1,6-hexanediol di(meth)acrylate, PO modified (2) neopentyl glycol di(meth)acrylate, (neopentyl glycol modified) trimethylolpropane di(meth)acrylate, EO modified (4) bisphenol A di(meth)acrylate, PO modified (4) bisphenol A di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate, dicyclopentanyl di(meth)acrylate, etc.

[0151] Trifunctional (meth)acrylate monomers having three (meth)acryloyl groups in the molecule: trimethylolpropane tri(meth)acrylate, EO-modified (3) trimethylolpropane tri(meth)acrylate, EO-modified (6) trimethylolpropane tri(meth)acrylate, PO-modified (3) trimethylolpropane tri(meth)acrylate, ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate, ethoxylated isocyanuric acid tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, etc. Tetrafunctional (meth)acrylate monomers having four acryloyl groups in the molecule: pentaerythritol tetra(meth)acrylate, EO-modified (4) pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc. Pentafunctional (meth)acrylate monomers having five (meth)acryloyl groups in the molecule: dipentaerythritol penta(meth)acrylate, etc. Hexafunctional (meth)acrylate monomers having six (meth)acryloyl groups in the molecule: dipentaerythritol hexa(meth)acrylate, etc.

[0152] Specific examples of the monomer having a vinyl group include N-vinyl-2-pyrrolidone and N-vinylcaprolactam.

[0153] (Oligomer) Examples of the oligomer include urethane (meth)acrylate oligomers such as aliphatic urethane (meth)acrylate oligomers and aromatic urethane (meth)acrylate oligomers, (meth)acrylic ester oligomers, polyester (meth)acrylate oligomers, and epoxy (meth)acrylate oligomers. The oligomer preferably contains about 2 to 16 ethylenically unsaturated bonds. Among them, urethane (meth)acrylate oligomers are preferred, and urethane (meth)acrylate oligomers having 6 to 12 (meth)acryloyl groups are more preferred.

[0154] The weight average molecular weight (Mw) of the oligomer is preferably 400 to 10,000, more preferably 500 to 5,000, more preferably 800 to 4,000, and more preferably 1,000 to 2,000. Here, the "weight average molecular weight (Mw)" can be determined as a polystyrene-equivalent molecular weight by general gel permeation chromatography (hereinafter, GPC).

[0155] The 6-12 functional urethane (meth)acrylate oligomers can be obtained as commercial products. Specific examples include EBECRYL1290 (6 functional, Mw1,000), EBECRYL5129 (6 functional, Mw800), EBECRYL8254 (6 functional, Mw1,200), KRM8200 (6 functional, Mw1,000), KRM8904 (9 functional, Mw1,800), EBECRYL8602 (9 functional, Mw2,000), KRM8452 (10 functional, Mw1,200), EBECRYL225 (10 functional, Mw1,200), and EBECRYL8415 (10 functional, Mw1,200), all of which are manufactured by Daicel-Allnex Corporation. Other examples include Miramer PU5000 (6 functional, Mw 1,800), Miramer PU610 (6 functional, Mw 1,800), Miramer PU6140 (6 functional, Mw 1,500), Miramer MU9800 (9 functional, Mw 3,500), and Miramer MU9500 (10 functional, Mw 3,200), all of which are manufactured by Miwon Specialty Chemical Co., Ltd.

[0156] [Other ingredients] Each of the inks constituting the printing ink set of this embodiment may further contain other components such as various additives in addition to the above components depending on the application, as long as the effects of the present invention are not reduced.

[0157] Examples of other components include waxes, antiblocking agents, surfactants, leveling agents, defoamers, preservatives, pH adjusters, UV absorbers, flame retardants, and antioxidants. If necessary, these various additives can be further added to the ink.

[0158] Examples of waxes include natural waxes and synthetic waxes. Examples of natural waxes include carnauba wax, Japan wax, lanolin, montan wax, paraffin wax, and microcrystalline wax. Examples of synthetic waxes include Fischer-Tropsch wax, polyethylene wax, polypropylene wax, polytetrafluoroethylene wax, polyamide wax, and silicone compounds. Adding wax can improve abrasion resistance, blocking prevention, slipperiness, and scratch prevention.

[0159] Examples of the anti-blocking agent include silica particles, polyethylene wax, fatty acid amide, cellulose acetate butyrate resin, cellulose acetate propionate resin, and soluble nitrocellulose.

[0160] Examples of the surfactant include anionic surfactants and nonionic surfactants. Examples of the anionic surfactant include fatty acid salts, alkyl sulfate salts, alkylaryl sulfonates, alkylnaphthalenesulfonates, dialkylsulfonates, dialkylsulfosuccinates, alkyldiaryletherdisulfonates, alkylphosphates, polyoxyethylene alkylether sulfates, polyoxyethylene alkylarylether sulfates, naphthalenesulfonate-formaldehyde condensates, and polyoxyethylene alkylphosphate salts. Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene alkylaryl ethers, polyoxyethylene oxypropylene block copolymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters polyoxyethylene alkylamines, glycerol borate fatty acid esters, and polyoxyethylene glycerol fatty acid esters.

[0161] Examples of the leveling agent include a fluorine-based leveling agent, an acrylic polymer-based leveling agent, and a silicone-based leveling agent.

[0162] Examples of the defoaming agent include mineral oil-based defoaming agents, silicone-based defoaming agents, non-silicone polymer-based defoaming agents, and acetylene glycol-based defoaming agents.

[0163] Examples of preservatives include sodium dehydroacetate, sodium benzoate, sodium pyridinethione-1-oxide, zinc pyridinethione-1-oxide, 1,2-benzisothiazolin-3-one, and amine salts of 1-benzisothiazolin-3-one.

[0164] Examples of pH adjusters include various amines, inorganic bases, ammonia, various buffer solutions, and the like.

[0165] Examples of the ultraviolet absorber include a benzotriazole-based ultraviolet absorber having an ethylenically unsaturated bond, a benzophenone-based ultraviolet absorber, a salicylic acid-based ultraviolet absorber, a cyanoacrylate-based ultraviolet absorber, a hindered phenol-based ultraviolet absorber, and a triazine-based ultraviolet absorber.

[0166] Examples of the flame retardant include phosphorus-based flame retardants, phosphate-based flame retardants, boron-based flame retardants, and bromine-based flame retardants.

[0167] Examples of the antioxidant include phenol-based antioxidants, amine-based antioxidants, and dithiocarbamic acid-based antioxidants.

[0168] Although not particularly limited, in one embodiment, the combination of each color printing ink in the printing ink set is a yellow ink containing an isoindoline compound represented by formula (1) and a dispersion medium; a cyan ink containing a metal phthalocyanine pigment containing at least one selected from the group consisting of copper phthalocyanine, aluminum phthalocyanine, and titanyl phthalocyanine described above and a dispersion medium; a magenta ink A containing a dioxazine pigment and a dispersion medium described above; and CI Pigment Red 254, CI Pigment Red 255, The magenta ink B may be a DPP pigment including at least one selected from the group consisting of CI Pigment Red 264, CI Pigment Red 272, CI Pigment Red 291, CI Pigment Orange 71, and CI Pigment Orange 73, a perylene pigment including at least one selected from the group consisting of CI Pigment Red 149, CI Pigment Red 179, CI Pigment Red 190, and CI Pigment Red 224, CI Pigment Red 122, or CI Pigment Violet 19, and a dispersion medium.

[0169] In another embodiment, the combination of the printing inks of each color may be a yellow ink including CI Pigment Yellow 180 and a dispersion medium; a cyan ink including a metal phthalocyanine pigment including at least one selected from the group consisting of copper phthalocyanine, aluminum phthalocyanine, and titanyl phthalocyanine as described above and a dispersion medium; a magenta ink A including a dioxazine pigment and a dispersion medium as described above; and a magenta ink B including a DPP pigment including at least one selected from the group consisting of CI Pigment Red 254, CI Pigment Red 255, CI Pigment Red 264, CI Pigment Red 272, CI Pigment Red 291, CI Pigment Orange 71, and CI Pigment Orange 73, a perylene pigment including at least one selected from the group consisting of CI Pigment Red 149, CI Pigment Red 179, CI Pigment Red 190, and CI Pigment Red 224, CI Pigment Red 122, or CI Pigment Violet 19 and a dispersion medium.

[0170] In these embodiments, it is more preferred that the metal phthalocyanine pigment in the cyan ink is copper phthalocyanine. Also, in these embodiments, the dioxazine pigment in Magenta Ink A is more preferably CI Pigment Violet 23 or CI Pigment Violet 37. The combination of pigments (coloring materials) in these printing inks can easily achieve both excellent light resistance and excellent color reproducibility. In particular, the combination of magenta ink A and magenta ink B has the effect of improving the adhesion of the printed layer (ink film). In the above embodiment, when a polyurethane resin is used as the dispersion medium, it becomes easy to increase the adhesion of the printed layer (ink film). Furthermore, when polybutylvinylal is used as the dispersion medium in addition to the polyurethane resin, it tends to become easy to further increase the adhesion.

[0171] <Printing ink manufacturing> The printing inks constituting the printing ink set of this embodiment can be produced by dispersing the pigment in a dispersion medium. The printing inks can be produced by blending additives, water and / or an organic solvent, etc., as necessary, into the dispersion.

[0172] As the dispersing machine, a commonly used one can be used. Examples include a roller mill, a ball mill, a pebble mill, an attritor, a sand mill, and other bead mills. Among them, the use of a bead mill is preferable. The particle size distribution of the pigment in the pigment dispersion can be adjusted by appropriately adjusting the size of the media beads of the dispersing machine, the filling rate of the media beads, the dispersion time, the outflow rate of the pigment dispersion, the viscosity of the pigment dispersion, and the like.

[0173] The printing ink set of the present embodiment is preferably in the form of a gravure printing ink set or a flexographic printing ink set. The printing inks constituting these printing ink sets are preferably in the form of gravure ink, water-based flexographic ink, flexographic ink, and active energy ray-curable flexographic ink. These various inks will be specifically described below.

[0174] <Gravure ink> The gravure ink contains a pigment and a binder resin as a dispersion medium, and preferably further contains an organic solvent.

[0175] (Pigments) The content of the pigment in the gravure ink is not particularly limited, but is preferably from 4 to 20% by mass, and more preferably from 5 to 15% by mass.

[0176] (binder resin) Examples of the binder resin include polyurethane resin, ethylene-vinyl acetate copolymer resin, vinyl acetate resin, nitrocellulose resin, polyamide resin, polyvinyl acetal resin, cellulose ester resin, polystyrene resin, acrylic resin, polyester resin, alkyd resin, rosin resin, rosin-modified maleic acid resin, ketone resin, cyclized rubber, butyral resin, petroleum resin, and chlorinated polyolefin resin.

[0177] The content of the binder resin in the gravure ink is preferably from 4 to 25% by mass, and more preferably from 6 to 20% by mass.

[0178] [Polyurethane resin] The binder resin used in the gravure ink is preferably a polyurethane resin, which includes a polyurethane urea resin. The synthesis of polyurethane resins can be carried out, for example, by (1) A two-stage method in which a polyol and a diisocyanate compound are reacted in such a ratio that the isocyanate group is in excess to synthesize a urethane prepolymer having an isocyanate group at the end, and then the urethane prepolymer having the isocyanate group is reacted in a solvent with the chain extender and / or end blocking agent having an amino group to synthesize the urethane prepolymer; (2) A one-step method in which polypropylene glycol, a polyol, a diisocyanate compound, and a chain extender and / or a terminal blocking agent having an amino group are reacted at once in a suitable solvent.

[0179] Examples of the solvent used in the synthesis include ester-based solvents such as ethyl acetate, propyl acetate, and butyl acetate; ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; alcohol-based solvents such as methanol, ethanol, isopropanol, and n-butanol; hydrocarbon-based solvents such as methylcyclohexane and ethylcyclohexane; and mixed solvents thereof. Among these methods, the two-stage method is preferred from the viewpoint of obtaining a more uniform polyurethane resin. When producing a polyurethane resin by the two-stage method, the equivalent ratio (moles of isocyanate groups / moles of amino groups) of the isocyanate groups of the urethane prepolymer and the amino groups of the chain extender and end-capping agent is preferably 1 / 1.3 to 1 / 0.9. When the equivalent ratio of the isocyanate groups to the amino groups is 1 / 1.3 or more, the amount of the chain extender and / or end-capping agent remaining unreacted is reduced, and yellowing of the polyurethane resin and odor after printing can be suppressed. When the equivalent ratio of the isocyanate groups to the amino groups is 1 / 0.9 or less, the molecular weight of the resulting polyurethane resin becomes appropriate, and a resin that provides suitable film strength after printing can be obtained.

[0180] The weight-average molecular weight of the polyurethane resin is preferably in the range of 15,000 to 100,000. When the weight-average molecular weight of the polyurethane resin is 15,000 or more, the ink has excellent blocking resistance, the printed film has excellent strength, and the printed film has excellent oil resistance, and when it is 100,000 or less, the viscosity of the obtained ink falls within an appropriate range, and the printed film has excellent gloss.

[0181] From the viewpoints of printability and laminate strength, the polyurethane resin preferably has an amine value of preferably 0.5 to 20 mgKOH / g, and more preferably 1 to 15 mgKOH / g.

[0182] In one embodiment, when the printing ink set of the present embodiment is used for packaging material applications, the content of the polyurethane resin is preferably 80 mass% or more based on the binder resin in the ink. By setting the content of the polyurethane resin within the above range, boil retort properties and adhesion to polyester films can be easily improved.

[0183] [Polyvinyl butyral resin] In one embodiment, the binder resin used in the gravure ink preferably further contains a polyvinyl butyral resin, which tends to facilitate the enhancement of adhesion of the ink film to the substrate. Polyvinyl butyral resin can be obtained by reacting polyvinyl alcohol with butyraldehyde or formaldehyde to form an acetal.

[0184] The polyvinyl butyral resin preferably has an acetyl group content of 4% by mass or less, a hydroxyl group content of 1% by mass to 30% by mass, and more preferably 1% by mass to 25% by mass, and a weight average molecular weight of 10,000 to 50,000.

[0185] The content of polyvinyl butyral resin is preferably in the range of 1.0 to 15.0% by mass based on the binder resin in the ink. By making the content of polyvinyl butyral resin in the binder resin 1.0% by mass or more, the blocking resistance of the resulting printing ink and its adhesion to polyester film can be easily improved. In addition, by making the content 15.0% by mass or less, the storage stability of the ink can be easily improved.

[0186] (Organic solvent) Examples of organic solvents used in gravure inks include aromatic organic solvents such as toluene and xylene, ketone-based organic solvents such as acetone, methyl ethyl ketone and methyl isobutyl ketone, ester-based organic solvents such as ethyl acetate, n-propyl acetate, butyl acetate and propylene glycol monomethyl ether acetate, alcohol-based organic solvents such as methanol, ethanol, n-propanol, isopropanol and n-butanol, glycol ether-based solvents such as ethylene glycol monopropyl ether and propylene glycol monomethyl ether, and aliphatic organic solvents such as methylcyclohexane. It is preferable to use two or more of these organic solvents in combination. In the gravure ink, it is preferable to use a mixed solvent of an ester-based organic solvent and an alcohol-based organic solvent. The mass ratio of the ester-based organic solvent to the alcohol-based organic solvent (mass of the ester-based organic solvent:mass of the alcohol-based organic solvent) is preferably 95:5 to 40:60, and more preferably 90:10 to 50:50. The content of the organic solvent in the ink is preferably 60 to 90 mass %, and more preferably in the range of 70 to 85 mass %, based on the mass of the ink.

[0187] (water) In one embodiment, the gravure ink may further contain water. By containing a predetermined amount of water, the pigment dispersibility by the polyurethane resin is improved, and printing suitability such as highlight transferability, plate fogging property, and trapping property is improved. The water content is preferably 0.1 to 10 mass %, more preferably 0.5 to 7 mass %, further preferably 0.5 to 5 mass %, and particularly preferably 0.5 to 4 mass %, based on the mass of the gravure ink.

[0188] (Silica particles) In one embodiment, the gravure ink can further contain silica particles, which improves wetting and spreading of the ink during overprinting, improves trapping, and maintains highlight transfer. The silica particles may be either naturally occurring or synthetic. They may be either crystalline or non-crystalline, or hydrophobic or hydrophilic. The silica particles may be synthesized by dry or wet methods. Dry methods include combustion and arc methods, and wet methods include precipitation and gel methods. The silica particles may be synthesized by either method. The silica particles may be hydrophilic silica having hydrophilic functional groups on the surface. Alternatively, the silica particles may be hydrophobic silica in which the hydrophilic functional groups are modified with alkylsilane or the like to make them hydrophobic. Hydrophilic silica is preferable. Such silica particles are also available as commercial products, for example, Nipgel series and Nipsil series manufactured by Tosoh Silica Corporation, and Mizukasil series manufactured by Mizusawa Chemical Industries, Ltd.

[0189] The silica particles preferably have an average particle diameter of 1 to 10 μm, more preferably 1 to 8 μm, and even more preferably 1 to 6 μm, in order to create unevenness on the surface of the ink layer. The average particle diameter of the silica particles is the cumulative value of 50% (D 50 ) and can be determined by the Coulter counter method. The specific surface area of ​​silica particles is 50 to 600 m by the BET method. 2 / g, more preferably 100 to 450 m 2 The silica particles used in gravure inks can be a combination of two or more types with different average particle sizes or BET specific surface areas.

[0190] The content of silica particles in the gravure ink is preferably 0.1 to 3 mass %, more preferably 0.2 to 2.5 mass %, further preferably 0.2 to 2 mass %, and particularly preferably 0.2 to 1.5 mass %.

[0191] (Other ingredients) In addition to the above components, the gravure ink may further contain other components such as various additives, as necessary. Examples of other components include various additives such as extender pigments, pigment dispersants, waxes, antiblocking agents, leveling agents, defoamers, plasticizers, antistatic agents, infrared absorbing agents, ultraviolet absorbing agents, fragrances, and flame retardants. These various additives may be further added to the ink as necessary.

[0192] The viscosity of the gravure ink may be preferably 10 mPa s or more from the viewpoint of preventing sedimentation of the pigment and dispersing the pigment appropriately. On the other hand, from the viewpoint of workability during ink production or printing, the viscosity of the gravure ink may be preferably 1,000 mPa s or less. The above viscosity is a value measured at 25°C using a B-type viscometer manufactured by Tokimec Co., Ltd.

[0193] <Gravure printing method and printed matter> The gravure printing can be appropriately selected from known methods. That is, a gravure printing machine capable of multi-color printing, equipped with a rotary intaglio plate (gravure plate) and a doctor blade in contact with it, is used, and gravure ink is supplied from an ink container (ink pan). A dedicated viscosity controller may be used to adjust the viscosity. The substrate for printing is supplied by a winding method, and the printed matter passes through a drying unit after printing. The temperature of the drying unit is preferably 30 to 100°C. The printing speed is preferably 50 to 250 m / min.

[0194] Gravure printing is broadly divided into front printing and back printing. For example, in front printing, when the substrate is white paper or white film, a printed matter can be obtained by printing on the substrate in the order of yellow ink, magenta ink, cyan ink, and black ink. Furthermore, for example, in reverse printing, when the substrate is a transparent film, it is preferable to produce a print by printing black ink, cyan ink, magenta ink, yellow ink, and white ink on the substrate in this order. The thickness of the printed layer can be appropriately selected depending on the application, the type and number of inks used, and the number of overprints. In one embodiment, the thickness of the printed layer may usually be in the range of 0.5 to 10 μm.

[0195] [Base material] Examples of the substrate include polyolefin substrates such as polyethylene and polypropylene; polycarbonate substrates; polyester substrates such as polyethylene terephthalate and polylactic acid; polystyrene substrates; polystyrene-based resin substrates such as AS and ABS; polyamide substrates such as nylon; polyvinyl chloride substrates; polyvinylidene chloride substrates; cellophane substrates; paper substrates; aluminum foil substrates; and composite substrates made of composite materials thereof. The substrate may be in the form of either a film or a sheet. Among them, polyester substrates and polyamide substrates, which have high glass transition temperatures, are preferably used.

[0196] The surface of the substrate may be vapor-deposited with a metal oxide or coated with polyvinyl alcohol. Examples of substrates that have been surface-treated in this way include GL-AE manufactured by Toppan Printing Co., Ltd. and IB-PET-PXB manufactured by Dai Nippon Printing Co., Ltd., which have aluminum oxide vapor-deposited on the surface. The substrate may be treated with additives such as an antistatic agent and an ultraviolet ray inhibitor, if necessary, and may be corona-treated or low-temperature plasma-treated.

[0197] The thickness of the substrate is not particularly limited and may usually be in the range of 5 to 100 μm.

[0198] <Flexographic ink> Flexographic inks can be broadly classified into water-based flexographic inks, oil-based flexographic inks, and active energy ray-curable flexographic inks. <Water-based flexographic ink> The water-based flexographic ink contains a pigment and a binder resin as a dispersion medium, and preferably further contains an aqueous solvent.

[0199] (Pigments) The content of the pigment in the water-based flexographic ink is not particularly limited, but is preferably 10 to 30% by mass, and more preferably 15 to 25% by mass.

[0200] (binder resin) The aqueous flexographic ink preferably contains a binder resin. Examples of the binder resin include aqueous resins such as aqueous polyurethane resin, aqueous acrylic urethane resin, polyester resin, acrylic resin, styrene-acrylic resin, styrene-maleic anhydride resin, rosin-modified maleic acid resin, cellulose-based resin, and chlorinated polyolefin. Among them, it is preferable to contain at least an aqueous polyurethane resin. The binder resin can be used alone or in combination of two or more kinds.

[0201] [Water-based polyurethane resin] A polyurethane resin is generally a resin obtained by reacting a polyisocyanate having two or more isocyanate groups in one molecule with a hydroxyl group-containing compound having two or more hydroxyl groups in one molecule. In one embodiment, the aqueous polyurethane resin has the following configuration. This configuration can be preferably introduced by appropriately selecting the structure and type of the hydroxyl group-containing compound.

[0202] The number of urethane bonds (mmol / g) of the aqueous polyurethane resin is not particularly limited. In one embodiment, from the viewpoint of adjusting the molecular weight of the aqueous polyurethane resin and the hardness of the coating film, the number of urethane bonds is preferably 2.2 to 3.0 mmol / g, more preferably 2.3 to 2.9 mmol / g. This number of urethane bonds can be adjusted to a desired range by appropriately adjusting the amounts of the hydroxyl group-containing compound and the polyisocyanate, and the reaction conditions.

[0203] The glass transition temperature (Tg) of the aqueous polyurethane resin is not particularly limited, but is preferably −70° C. or lower, and more preferably −70° C. to −90° C. When the Tg of the aqueous polyurethane resin is −70° C. or lower, the film-forming property of the ink is improved, and the adhesion of the coating film is improved.

[0204] The weight average molecular weight (measured by GPC, calculated as standard polystyrene) of the aqueous polyurethane resin is not particularly limited, but is preferably from 10,000 to 100,000, and more preferably from 30,000 to 70,000.

[0205] The hydroxyl value (mgKOH / g) of the aqueous polyurethane resin is not particularly limited, but is preferably 35 mgKOH / g or less, and more preferably 20 mgKOH / g or less, from the viewpoint of water resistance, etc. In one embodiment, the hydroxyl value (mgKOH / g) may be 0 mgKOH / g.

[0206] The aqueous polyurethane resin may be either water-soluble or in the form of an aqueous emulsion, but is preferably water-soluble. Here, the aqueous emulsion refers to a resin solution in which a resin that is poorly soluble in water is in the form of particulates and stabilized in an emulsion state. The content of the aqueous polyurethane resin is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more, based on the total mass of the aqueous flexo ink, while the content of the aqueous polyurethane resin is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 17% by mass or less, based on the total mass of the aqueous flexo ink.

[0207] [Polyvinyl butyral resin] In one embodiment, the binder resin used in the water-based flexographic ink preferably further contains a polyvinyl butyral resin. According to such an embodiment, it tends to be easier to further increase the adhesion of the ink film to the substrate. As the polyvinyl butyral resin, the polyvinyl butyral resin described in the above description of the gravure ink is preferable.

[0208] (Water-based solvent) The aqueous flexographic ink contains an aqueous solvent, which may be water, an alcohol solvent such as n-propanol or isopropanol, a glycol solvent such as propylene glycol, butylene glycol, dipropylene glycol or tripropylene glycol, or a glycol monoalkyl ether solvent such as propylene glycol monoethyl ether or propylene glycol monopropyl ether.

[0209] The content of the aqueous solvent is preferably 40 to 70% by mass based on the total mass of the aqueous flexographic ink.

[0210] (Other ingredients) The water-based flexographic ink may further contain other components such as various additives in addition to the above components, as necessary. Examples of other components include various known additives such as extender pigments, pigment dispersants, waxes, leveling agents, surfactants, defoamers, preservatives, thickeners, pH adjusters, hardeners, and ultraviolet absorbers. These various additives may be further added to the ink as necessary. In addition, non-aqueous solvents other than alcohol solvents (e.g., ketone-based solvents and ester-based solvents) may be added within a range that can solve the problem. The content of the non-aqueous solvent is preferably 20% by mass or less, more preferably 10% by mass or less, based on the total mass of the ink.

[0211] <Flexographic printing method and printed matter> The flexographic printing method is not particularly limited and can be appropriately selected from known methods. For example, the two-roll method, the doctor method, the doctor chamber method, etc. can be mentioned. In the doctor method and the doctor chamber method, the flexographic ink is supplied to an anilox roll having cells formed on the surface, and the excess flexographic ink on the anilox roll surface is scraped off by a doctor blade, and the ink is finally printed (applied) on the substrate through a resin plate.

[0212] The anilox used in flexographic printing can be a ceramic anilox roll with cell engraving, a chrome-plated anilox roll, etc. The shape of the cells can be a honeycomb pattern, a diamond pattern, a helical pattern, etc., and any pattern can be used.

[0213] Plates used in flexographic printing include photosensitive resin plates that use ultraviolet light curing with a UV light source, and elastomer material plates that use direct laser engraving. Any sleeve and cushion tape can be used to attach the plate.

[0214] Flexographic printing presses include CI type multi-color flexographic printing presses and unit type multi-color flexographic printing presses. Ink supply methods include chamber method and two-roll method. A suitable combination of these methods can be used.

[0215] [Base material] Examples of the substrate include plastic films such as polyethylene, polypropylene, polyethylene terephthalate, and nylon, cellophane, paper, aluminum foil, and films and sheets made of composite materials thereof. The paper substrate is preferably a paper substrate selected from uncoated paper, one-side glossy kraft paper in which one side of the substrate is treated, bleached kraft paper, unbleached kraft paper, and the like. Other substrates such as plastic films can be used that are similar to those used for gravure ink prints.

[0216] <Oil-based flexographic ink> Flexographic ink contains a pigment and a binder resin as a dispersion medium, and preferably further contains an organic solvent.

[0217] (Pigments) The content of the pigment in the oil-based flexographic ink is not particularly limited, but is preferably 4 to 25% by mass, and more preferably 5 to 20% by mass.

[0218] (binder resin) Examples of the binder resin include polyurethane resin, polyvinyl acetal resin, cellulose ester resin, polyamide resin, ethylene-vinyl acetate copolymer resin, vinyl acetate resin, polystyrene resin, acrylic resin, polyester resin, alkyd resin, rosin resin, rosin-modified maleic acid resin, ketone resin, cyclized rubber, butyral resin, petroleum resin, and chlorinated polyolefin resin. Among them, the binder resin preferably contains a polyurethane resin, a polyvinyl acetal resin, or a cellulose ester resin.

[0219] As the polyurethane resin and the polyvinyl acetal resin, the polyurethane resin and the polyvinyl acetal resin described above in the explanation of the gravure ink are preferable.

[0220] As the cellulose ester resin, a nitrocellulose resin, a cellulose acetate propionate resin, or a cellulose acetate butyrate resin is preferable.

[0221] Nitrocellulose resin is obtained by converting some or most of the hydroxyl groups of cellulose into nitric acid esters (nitrification) using a mixed acid of sulfuric acid and nitric acid. The solubility of nitrocellulose resin in solvents varies depending on the degree of nitrification. Nitrocellulose resins with a high degree of nitrification are usually used in hydrocarbon-based or ester-based solvents. Nitrocellulose resins with a low degree of nitrification are used in alcohol-based solvents.

[0222] The cellulose acetate propionate resin is obtained by triesterifying cellulose with acetic acid and propionic acid, followed by hydrolysis. Generally, resins with 0.6 to 2.5% by mass of acetylation, 42 to 46% by mass of propionation, and 1.8 to 5% by mass of hydroxyl groups are commercially available. In one embodiment of the present invention, from the viewpoint of compatibility with polyurethane resin, it is preferable to use a cellulose acetate propionate resin with a propionyl group content of 40 to 50% by mass (median value 45%), an acetyl group content of 0.5 to 3% by mass (median value 2.5%), a hydroxyl group content of 2 to 6% by mass (median value 2.5%), and a viscosity of 0.05 to 0.2 Pa·s.

[0223] Cellulose acetate butyrate resin is obtained by triesterifying cellulose with acetic acid and butyric acid, followed by hydrolysis. Generally, resins with 2 to 30% by mass of acetylation, 17 to 53% by mass of butyrylation, and 1 to 5% by mass of hydroxyl groups are commercially available.

[0224] (Organic solvent) Examples of organic solvents used in oil-based flexographic inks include ester-based organic solvents such as ethyl acetate, n-propyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate; alcohol-based organic solvents such as methanol, ethanol, n-propanol, isopropanol, and n-butanol; glycol ether-based solvents such as ethylene glycol monopropyl ether and propylene glycol monomethyl ether; and aliphatic organic solvents such as methylcyclohexane. It is preferable to use two or more of these organic solvents in combination.

[0225] (Other ingredients) The oil-based flexographic ink may contain other components such as various additives in addition to the above components, as necessary. Examples of other components include various additives such as extender pigments, pigment dispersants, waxes, antiblocking agents, leveling agents, defoamers, plasticizers, antistatic agents, infrared absorbing agents, ultraviolet absorbing agents, fragrances, and flame retardants. These various additives may be further added to the ink as necessary.

[0226] <Active energy ray curable flexographic ink> The active energy ray-curable flexographic ink contains a pigment and a polymerizable compound as a dispersion medium, and preferably further contains a photopolymerization initiator.

[0227] (Pigments) The content of the pigment in the active energy ray-curable flexographic ink is not particularly limited, but is preferably from 5 to 30% by mass, and more preferably from 10 to 25% by mass.

[0228] (polymerizable compound) The polymerizable compound is as described above as the dispersion medium.

[0229] The polymerizable compounds can be used alone or in combination of two or more kinds.

[0230] The content of the polymerizable compound is preferably from 25 to 90% by mass, and more preferably from 35 to 80% by mass, based on the total mass of the active energy ray-curable flexographic ink.

[0231] (Polymerization initiator) The active energy ray-curable flexographic ink contains a polymerization initiator. The polymerization initiator preferably contains a radical polymerization initiator, and more preferably contains a photopolymerization initiator. The polymerization initiator is a compound that undergoes a chemical change and generates radicals through the action of light or through interaction with the electronically excited state of the sensitizing dye. Among them, a photoradical polymerization initiator is preferred because it can initiate polymerization by exposure to light.

[0232] The photoradical polymerization initiator is not particularly limited, and known ones can be used. Specific examples include benzophenone compounds, dialkoxyacetophenone compounds, α-hydroxyalkylphenone compounds, α-aminoalkylphenone compounds, acylphosphine oxide compounds, and thioxanthone compounds.

[0233] Examples of the benzophenone-based compounds include benzophenone, 4-methylbenzophenone, 4-phenylbenzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, and [4-(methylphenylthio)phenyl]-phenylmethanone.

[0234] Examples of the dialkoxyacetophenone compounds include 2,2-dimethoxy-2-phenylacetophenone, dimethoxyacetophenone, and diethoxyacetophenone.

[0235] Examples of the α-hydroxyalkylphenone compounds include 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxymethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one.

[0236] Examples of the α-aminoalkylphenone compounds include 2-methyl-1-[4-(methoxythio)-phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-(dimethylamino)-1-(4-morpholinophenyl)-1-butanone, and 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone.

[0237] Examples of the acylphosphine oxide compound include diphenylacylphenylphosphine oxide, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide.

[0238] Examples of the thioxanthone compounds include 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, and 2,4-diethylthioxanthone.

[0239] The above polymerization initiators can be used alone or in combination of two or more kinds.

[0240] The content of the polymerization initiator is preferably from 0.5 to 20% by mass, and more preferably from 5 to 15% by mass, based on the total mass of the active energy ray-curable flexographic ink.

[0241] (Polymerization initiator aid) The active energy ray curable flexographic ink may also contain a polymerization initiator aid. By containing a polymerization initiator aid, the curability can be further improved. Examples of the polymerization initiator aid include triethanolamine, methyldiethanolamine, triisopropanolamine, aliphatic amines, ethyl 2-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, isoamyl 4-dimethylaminobenzoate, and dibutylethanolamine.

[0242] The content of the polymerization initiator aid is preferably 0.1 to 5 mass %, and more preferably 0.5 to 3 mass %, based on the total mass of the active energy ray-curable flexographic ink.

[0243] (Dispersant) The active energy ray-curable flexographic ink preferably further contains a dispersant in order to further improve pigment dispersibility. The dispersant is not particularly limited, and any known dispersant can be used. Specific examples include polymer dispersants mainly composed of polyoxyalkylene polyalkylene polyamines, vinyl polymers and copolymers, acrylic polymers and copolymers, polyesters, polyamides, polyimides, polyurethanes, amine polymers, etc. Among these, from the viewpoint of the dispersion stability of the pigment, pigment dispersants containing basic functional groups having a block structure or a comb structure are preferred. Such pigment dispersants are also available as commercial products, such as the Ajisper series (Ajisper PB821, PB822, PB824, etc.) manufactured by Ajinomoto Fine-Techno Co., Ltd., the Solsperse series (SOLSPERSE24000, SOLSPERSE32000, SOLSPERSE38500, SOLSPERSE39000, etc.) manufactured by The Lubrizol Corporation, and the Disperbyk series (BYK-162, BYK-168, BYK-183, etc.) manufactured by BYK-Chemie.

[0244] The content of the dispersant is preferably 0.1 to 10% by mass based on the total mass of the active energy ray-curable flexographic ink.

[0245] (wax) The active energy ray curable flexographic ink preferably contains a wax in order to further improve the abrasion resistance, blocking prevention, smoothness, and scratch prevention. The wax is not particularly limited, and known waxes can be used. For example, there are natural waxes and synthetic waxes. Examples of natural waxes include carnauba wax, Japan wax, lanolin, montan wax, paraffin wax, and microcrystalline wax. Examples of synthetic waxes include Fischer-Tropsch wax, polyethylene wax, polypropylene wax, polytetrafluoroethylene wax, polyamide wax, silicone compounds, and the like.

[0246] From the viewpoint of the balance between abrasion resistance, gloss, and piling, the content of the wax is preferably 0.1 to 5 mass %, and more preferably 0.5 to 4 mass %, based on the total mass of the active energy ray-curable flexographic ink.

[0247] (binder resin) The active energy ray-curable flexographic ink may contain a binder resin, which reduces the cure shrinkage of the coating film that occurs during curing, suppresses curling of the substrate, and improves adhesion to the substrate.

[0248] Examples of binder resins include polyvinyl chloride, poly(meth)acrylic acid ester, epoxy resin, polyester resin, polyurethane resin, cellulose derivatives (e.g., ethyl cellulose, cellulose acetate, nitrocellulose), vinyl chloride-vinyl acetate copolymer, polyamide resin, polyvinyl acetal resin, diallyl phthalate resin, alkyd resin, rosin-modified alkyd resin, rosin-modified alkyd resin, petroleum resin, urea resin, synthetic rubber such as butadiene-acrylonitrile copolymer, etc. Among them, diallyl phthalate resin and polyester resin are preferred. Diallyl phthalate resin is more preferred.

[0249] The weight average molecular weight of the binder resin is preferably 1,000 to 100,000, and more preferably 2,000 to 70,000.

[0250] The binder resins can be used alone or in combination of two or more kinds. From the viewpoint of curability, the content of the binder resin is preferably 1 to 15% by mass, more preferably 1 to 5% by mass, based on the total mass of the active energy ray-curable flexographic ink.

[0251] (Polymerization inhibitor) The active energy ray-curable flexographic ink may contain a polymerization inhibitor, such as 4-methoxyphenol, hydroquinone, methylhydroquinone, t-butylhydroquinone, 2,6-di-t-butyl-4-methylphenol, phenothiazine, and aluminum salt of N-nitrosophenylhydroxylamine.

[0252] The content of the polymerization inhibitor is preferably 0.01 to 2% by mass based on the total mass of the active energy ray-curable flexographic ink, from the viewpoint of improving the storage stability of the active energy ray-curable flexographic ink while maintaining the curability.

[0253] (Other ingredients) The active energy ray-curable flexographic ink may contain other components such as various additives in addition to the above components, as necessary, within the range in which the effects of the present invention are not impaired. As various additives, extender pigments, leveling agents, surfactants, defoamers, UV absorbers, antistatic agents, antioxidants, etc. can be added to the ink as necessary.

[0254] It is preferable that the active energy ray-curable flexographic ink contains substantially no water, which means that the water content is 1% by mass or less based on the total mass of the ink composition.

[0255] <Printing method and printed matter using active energy ray-curable flexographic ink> The active energy ray curable flexographic ink can be printed on a recording medium by a flexographic printing method and cured with active energy rays to form a printed matter. The recording medium is not particularly limited, and any known recording medium can be used. Specific examples include coated paper such as art paper, coated paper, and cast paper, uncoated paper such as fine paper, medium quality paper, and newsprint, synthetic paper such as Yupo paper, and plastic films such as PET (polyethylene terephthalate), PP (polypropylene), and OPP (biaxially oriented polypropylene).

[0256] The method for curing the active energy ray-curable flexographic ink is not particularly limited, and any known method can be used. For example, the ink can be cured by irradiating it with α-rays, γ-rays, electron beams, X-rays, ultraviolet rays, visible light, infrared light, or the like. Among these, ultraviolet rays and electron beams are preferred, and ultraviolet rays are more preferred. The peak wavelength of the active energy rays is preferably 200 to 600 nm, and more preferably 350 to 420 nm.

[0257] The active energy ray source is not particularly limited, and known sources can be used.Specific examples include mercury lamps, xenon lamps, metal hydride lamps, LEDs (light-emitting diodes) such as ultraviolet light-emitting diodes (UV-LEDs) and ultraviolet laser diodes (UV-LDs), and gas / solid-state lasers.Of these, ultraviolet light-emitting diodes (UV-LEDs) are preferred because of their small size, long life, high efficiency, and low cost.

[0258] <Packaging materials> One embodiment of the present invention relates to a packaging material. The packaging material includes a printed matter at least in a part thereof. The printed matter on the packaging material is formed by using the printing ink set of the above embodiment according to various printing methods as described above. In one embodiment, the packaging material can be used in the form of a printed matter itself in which a printed layer is formed on a substrate. Examples of such packaging materials include stickers, labels, and the like. In another embodiment, the packaging material may have a laminated structure in which, for example, at least a printed matter, an adhesive layer, and a sealant substrate are laminated in order. A package can be obtained by processing a packaging material having such a laminated structure. Examples of the package include a four-sided sealed package, a three-sided sealed package, a pillow package, a stick bag, a gusset bag, a square bottom bag, a standing pouch, a deep-draw container, a vacuum package, a skin pack, a zipper bag, a spout pouch, a twist package, a wrap package, a shrink package, a label, a liquid paper carton, and a paper tray. In one embodiment, the packaging material can be suitably used for packages having various shapes.

[0259] Examples of items to be packaged in the packaging material include food products (e.g., rice, confectionery, seasonings, edible oils and fats, cooked foods, etc.), beverages (e.g., alcoholic beverages, soft drinks, mineral water, etc.), daily necessities and cultural products (e.g., medicines, cosmetics, stationery, etc.), and electronic components.

[0260] The packaging material having the above-mentioned laminated structure will now be described in more detail.

[0261] [Adhesive layer] In the packaging material having the laminated structure, the adhesive components that can be used to form the adhesive layer include laminating adhesives, hot melt adhesives, and thermoplastic resins. Among the above adhesive components, examples of laminating adhesives and hot melt adhesives include polyether adhesives, polyurethane adhesives, epoxy adhesives, polyvinyl acetate adhesives, cellulose adhesives, and (meth)acrylic adhesives. Among these adhesive components, polyurethane adhesives are preferably used.

[0262] The adhesive components may be used alone or in combination of two or more.

[0263] The polyurethane adhesive may be a reactive adhesive containing polyol and polyisocyanate and may have releasability. Examples of the polyurethane adhesive having releasability include the lamination adhesive described in JP 2020-084130 A. The polyurethane adhesive having such releasability preferably has an acid value of 5 to 45 mgKOH / g. Furthermore, it is preferable that the polyol constituting the polyurethane adhesive contains a polyester polyol, and the polyisocyanate contains one selected from the group consisting of an aliphatic polyisocyanate and an araliphatic polyisocyanate. The thickness of the adhesive layer may usually be in the range of 1 to 6 μm.

[0264] [Sealant base material] In the packaging material having the laminated structure, the sealant substrate is a substrate constituting the innermost layer of the laminate film. As the sealant substrate, a resin material capable of being fused to each other by heat (having heat sealability) is used. Examples of the sealant substrate include non-oriented polypropylene (CPP), vapor-deposited non-oriented polypropylene film (VMCPP), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ethylene-vinyl acetate copolymer (EVA), etc. The thickness of the sealant base material is not particularly limited. In consideration of the processability into packaging materials, heat sealability, etc., the thickness is preferably in the range of 10 to 200 μm, more preferably in the range of 15 to 150 μm. In addition, by providing the sealant base material with unevenness with a height difference of 5 to 20 μm, it is possible to impart properties such as slipperiness and tearability of packaging materials to the sealant base material. The method for laminating the sealant substrate is not particularly limited, and examples thereof include a method for laminating the adhesive layer and the sealant substrate film by heat (thermal lamination, dry lamination), and a method for melting the sealant substrate resin, extruding it onto the adhesive layer, and cooling and solidifying it to laminate (extrusion lamination method).

[0265] Conventional printing inks used in packaging materials may not have sufficient light resistance to various light sources. Therefore, design properties such as fading may occur. In addition, radicals generated by light irradiation during storage may cause a decrease in cohesive force or adhesion of the printed layer, resulting in a decrease in laminate strength. As a result, when opening a package or packaging material stored for a long time under light irradiation, a problem of interphase peeling of the laminate may occur. In contrast, the packaging material of the present embodiment can maintain high design properties because the printing ink set has excellent color reproducibility. In addition, the printing layer formed using the printing ink set has excellent light resistance and excellent adhesion, so that the occurrence of defects such as interlayer peeling as seen in conventional packaging materials can be suppressed. From this perspective, in one embodiment, the printing ink set of the above embodiment can be suitably used for applications of packaging materials having a laminated structure. According to such an embodiment, a packaging material with high laminate strength can be easily provided. EXAMPLES

[0266] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples, but the embodiments of the present invention are not limited to the following examples. Note that "parts" means "parts by mass" and "%" means "% by mass". The blend amounts in the table are in parts by mass, and amounts other than the solvent are calculated as non-volatile contents. Note that blank spaces in the table indicate that no blend was made. In addition, the color difference ΔE * ab is the value calculated by the following formula. ΔE * ab = {(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2} 1 / 2

[0267] (Average primary particle size of pigment) The average primary particle size of the pigment was measured by using a transmission electron microscope (TEM) to directly measure the size of the primary particles from electron micrographs. Specifically, the minor axis and major axis diameters of each pigment primary particle were measured, and the average was taken as the particle size of the pigment primary particles. Next, the volume of 100 or more pigment particles was calculated by approximating each to a cube of the calculated particle size, and the volume average particle size was taken as the average primary particle size.

[0268] <Production of isoindoline compounds> (Production Example 1-1) (Process 1) In a four-neck flask equipped with a reflux condenser, a dropping funnel, and a stirrer, 800 parts of water, 60 parts of 1,3-diiminoisoindoline, and 120 parts of 28% aqueous ammonia were added in this order and stirred. A solution of 42.58 parts of 2-cyano-N-methylacetamide dissolved in 160 parts of water was added dropwise using a dropping funnel over 30 minutes. The mixture was heated and stirred at 30°C until the raw material 1,3-diiminoisoindoline disappeared. The reaction slurry was filtered using a Buchner funnel. The filtrate was added to 1600 parts of water and stirred at 40°C for 30 minutes to remove unreacted 2-cyano-N-methylacetamide. The slurry was filtered to obtain non-volatile matter. The disappearance of 1,3-diiminoisoindoline was confirmed by UPLC (ultra-high performance high-resolution liquid chromatography, Waters). (Process 2) The non-volatile matter equivalent to 60 parts and 480 parts of water were added to a four-neck flask equipped with a reflux condenser, a dropping funnel, and a stirrer, and stirred. Meanwhile, 461 parts of water, 194 parts of 80% acetic acid, and 35.67 parts of barbituric acid were added to a glass flask, and stirred at 65°C. The heated solution of this mixture was poured into the stirred liquid of the non-volatile matter, and the temperature was raised to 85°C and stirring was continued to complete the reaction. Heating and stirring were continued until the non-volatile matter used as the raw material disappeared. The disappearance of the raw material was confirmed by UPLC. Thereafter, the slurry was filtered and washed three times with 2400 parts of water to obtain a non-volatile fraction, which was then dried in a hot air dryer at 80° C. to obtain 89.45 parts of isoindoline compound (1-1).

[0269] (Production Example 1-2) The same reaction procedure as in Production Example 1-1 was carried out except that in step 2 of Production Example 1-1, 35.67 parts of barbituric acid was changed to 43.48 parts of 1,3-dimethylbarbituric acid, to obtain 92.05 parts of isoindoline compound (1-2).

[0270] (Production Example 1-3) The same reaction procedure as in Production Example 1-1 was carried out except that in step 2 of Production Example 1-1, 35.67 parts of barbituric acid was changed to 33.89 parts of barbituric acid and 2.17 parts of 1,3-dimethylbarbituric acid, to obtain 85.34 parts of isoindoline compound (1-3).

[0271] (Production Example 1-4) (Process 1) In a four-neck flask equipped with a reflux condenser, a dropping funnel, and a stirrer, 800 parts of water, 60 parts of 1,3-diiminoisoindoline, and 120 parts of 28% aqueous ammonia were added in this order and stirred. A solution of 42.58 parts of 2-cyano-N-methylacetamide dissolved in 160 parts of water was added dropwise using a dropping funnel over 30 minutes. The mixture was heated and stirred at 30°C until the raw material 1,3-diiminoisoindoline disappeared. The reaction slurry was filtered using a Buchner funnel. The filtrate was added to 1600 parts of water and stirred at 40°C for 30 minutes to remove unreacted 2-cyano-N-methylacetamide. The slurry was filtered to obtain a non-volatile fraction. The disappearance of 1,3-diiminoisoindoline was confirmed by UPLC. (Process 2) In a four-neck flask equipped with a reflux condenser, a dropping funnel, and a stirrer, 60 parts of the non-volatile matter obtained in the previous preparation, 480 parts of water, and 162 parts of 80% acetic acid were added as raw materials and stirred. Meanwhile, 480 parts of water and 162 parts of 80% acetic acid were added to a glass flask, and 33.89 parts of barbituric acid were added thereto and stirred at 65°C. The heated solution of this mixture was poured into the stirred liquid of the non-volatile matter and stirred at 30°C for 3 hours. Furthermore, 48 parts of water and 16 parts of 80% acetic acid were added to a separately prepared glass flask, and 2.17 parts of 1,3-dimethylbarbituric acid were added thereto and stirred at 65°C. The heated solution of this mixture was poured into the previous reaction stirred liquid, and the temperature was raised to 85°C and stirring was performed to complete the reaction. Heating and stirring were performed until the non-volatile matter used as the raw material disappeared. The disappearance of the raw material was confirmed by UPLC. Thereafter, the slurry was filtered and washed three times with 2400 parts of water to obtain a non-volatile fraction, which was then dried in a hot air dryer at 80° C. to obtain 85.45 parts of an isoindoline compound (1-4).

[0272] (Production Example 1-5) In step 1 of Production Example 1-1, 42.58 parts of 2-cyano-N-methylacetamide was changed to 40.45 parts of 2-cyano-N-methylacetamide and 1.82 parts of 2-cyano-acetamide, and in step 2, 60 parts of nonvolatile matter was changed to 59.81 parts, but the reaction was carried out in the same manner as in Production Example 1-1, and 84.81 parts of isoindoline compound (1-5) was obtained.

[0273] (Production Example 1-6) In step 1 of Production Example 1-1, 42.58 parts of 2-cyano-N-methylacetamide was changed to 40.45 parts of 2-cyano-N-methylacetamide and 3.48 parts of 2-cyano-N-phenylacetamide, and in step 2, 60 parts equivalent of non-volatile matter was changed to 60.82 parts equivalent, but the reaction operation was performed in the same manner as in Production Example 1-1, and 85.76 parts of isoindoline compound (1-6) was obtained.

[0274] (Production Example 1-7) In step 1 of Production Example 1-1, 42.58 parts of 2-cyano-N-methylacetamide was changed to 40.45 parts of 2-cyano-N-methylacetamide and 3.50 parts of cyanophenylacetate, and in step 2, 60 parts equivalent of non-volatile matter was changed to 60.84 parts equivalent, but the reaction operation was performed in the same manner as in Production Example 1-1, and 85.78 parts of isoindoline compound (1-7) was obtained.

[0275] (Production Example 1-8) In step 1 of Production Example 1-1, 60 parts of 1,3-diiminoisoindoline was changed to 57 parts of 1,3-diiminoisoindoline and 3.29 parts of 5-methyl-1,3-diiminoisoindoline, and in step 2, 60 parts equivalent of nonvolatile matter was changed to 60.19 parts equivalent, but the reaction operation was performed in the same manner as in Production Example 1-1, and 85.16 parts of isoindoline compound (1-8) was obtained.

[0276] (Production Example 1-9) In step 1 of Production Example 1-1, 60 parts of 1,3-diiminoisoindoline was changed to 57 parts of 1,3-diiminoisoindoline and 3.62 parts of 5-methoxy-1,3-diiminoisoindoline, and in step 2, 60 parts equivalent of nonvolatile matter was changed to 60.40 parts equivalent, but the reaction operation was performed in the same manner as in Production Example 1-1, and 85.36 parts of isoindoline compound (1-9) was obtained.

[0277] (Production Example 1-10) In step 1 of Production Example 1-1, 60 parts of 1,3-diiminoisoindoline was changed to 57 parts of 1,3-diiminoisoindoline and 3.62 parts of 4-methoxy-1,3-diiminoisoindoline, and in step 2, 60 parts equivalent of nonvolatile matter was changed to 60.40 parts equivalent, but the reaction operation was performed in the same manner as in Production Example 1-1, and 85.36 parts of isoindoline compound (1-10) was obtained.

[0278] (Production Example 1-11) The same reaction procedure as in Production Example 1-1 was carried out except that in step 2 of Production Example 1-1, 35.67 parts of barbituric acid was changed to 33.89 parts of barbituric acid and 1.98 parts of 1-methylbarbituric acid, to obtain 85.16 parts of isoindoline compound (1-11).

[0279] (Production Example 1-12) The same reaction procedure as in Production Example 1-1 was carried out except that in step 2 of Production Example 1-1, 35.67 parts of barbituric acid was changed to 33.89 parts of barbituric acid and 2.56 parts of 1,3-diethylbarbituric acid, to obtain 85.34 parts of isoindoline compound (1-12).

[0280] The structures of the isoindoline compounds obtained in Production Examples 1-1 to 1-12 are shown in Table 1. The structures are represented by general formula (1). In the table, H represents hydrogen, Me represents a methyl group, Et represents an ethyl group, Ph represents a phenyl group, and OMe represents a methoxy group. The isoindoline compounds obtained in Production Examples 1-3 to 1-12 were mixtures of the isoindoline compounds shown in (1)-1 and (1)-2, respectively.

[0281] [Table 1]

[0282] The obtained isoindoline compounds were identified by comparing the molecular ion peak of the mass spectrum with the mass number (theoretical value) obtained by calculation. The molecular ion peak of the mass spectrum was measured using Waters ACQUITY UPLS H-Class (column used: ACQUITY UPLC BEH C18 Column 130 Å, 1.7 μm, 2.1 mm × 50 mm) / Ms TAP XEVO TQD. The theoretical molecular weight and the measured value obtained by mass spectrometry for each of the isoindoline compounds (Production Examples 1-1 to 1-12) are shown in Table 1. Due to the nature of the measurement, the H (proton) of the compound is eliminated, so if the measured value is the mass number of the theoretical molecular weight minus 1, the compound will match.

[0283] (Production Example 1-13) 95 parts of isoindoline compound (1-1), 5 parts of isoindoline compound (1-2), 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 8 hours at 60° C. Next, the kneaded mixture was poured into warm water at about 70° C. and stirred for 1 hour to form a slurry, which was then repeatedly filtered and washed with water to remove sodium chloride and diethylene glycol, and then dried overnight at 80° C. and pulverized to obtain 95 parts of isoindoline compound (1-13).

[0284] (Production Example 2-1) 800 parts of water and 800 parts of 80% acetic acid were added to a 4-neck flask equipped with a reflux condenser, a dropping funnel, and a stirrer, and the mixture was stirred. 111.18 parts of barbituric acid were added thereto, and the mixture was stirred at 65°C to dissolve the barbituric acid. Meanwhile, 800 parts of water and 60.00 parts of 1,3-diiminoisoindoline were added to a glass flask, and the mixture was stirred at 30°C. The stirred solution was poured into the above-mentioned heated solution, and the temperature was raised to 85°C and stirring was continued to complete the reaction. Heating and stirring were continued until the non-volatile content used as the raw material disappeared. The disappearance of the raw material was confirmed by UPLC. Thereafter, the mixture was washed three times with 2000 parts of water to obtain a non-volatile fraction, which was then dried in a hot air dryer at 80° C. to obtain 133.59 parts of an isoindoline compound (2-1).

[0285] (Production Example 2-2) The same reaction procedure as in Production Example 2-1 was carried out except that 111.18 parts of barbituric acid in Production Example 2-1 was changed to 135.53 parts of 1,3-dimethylbarbituric acid, to obtain 154.00 parts of isoindoline compound (2-2).

[0286] (Production Example 2-3) (Process 1) In a four-neck flask equipped with a reflux condenser, a dropping funnel, and a stirrer, 800 parts of water, 60 parts of 1,3-diiminoisoindoline, and 120 parts of 28% aqueous ammonia were added in this order and stirred. A solution of 42.58 parts of 2-cyano-N-methylacetamide dissolved in 160 parts of water was added dropwise using a dropping funnel over 30 minutes. The mixture was heated and stirred at 30°C until the raw material 1,3-diiminoisoindoline disappeared. The reaction slurry was filtered using a Buchner funnel to obtain a non-volatile fraction. The disappearance of 1,3-diiminoisoindoline was confirmed by UPLC (ultra-high performance high-resolution liquid chromatography, manufactured by Waters). (Process 2) To a four-necked flask equipped with a reflux condenser, a dropping funnel, and a stirrer, 60 parts equivalent of the above non-volatile content and 480 parts of water were added and stirred. Then, 53.54 parts of a 40% aqueous methylamine solution was added thereto, and the mixture was stirred at 40 °C. Stirring was carried out until the above non-volatile content used as a raw material disappeared. The disappearance of the raw material was confirmed by UPLC. Thereafter, it was washed three times with 2400 parts of water to obtain a non-volatile content. This non-volatile content was dried in a hot air dryer at 80 °C to obtain 58.62 parts of an isoindoline compound (2-3).

[0287] The structures of the isoindoline compounds obtained in Production Examples 2-1, 2-2, and 2-3 are shown in Table 2. The structures of the isoindoline compounds (2-1) and (2-2) are represented by the general formula (2-1), and the structure of the isoindoline compound (2-3) is represented by the general formula (2-2). In the table, H represents hydrogen and Me represents a methyl group.

[0288] [Table 2]

[0289] The identification of the obtained isoindoline compound was carried out by comparing the molecular ion peak of the mass spectrum with the mass number (theoretical value) obtained by calculation in the same manner as above.

[0290] <Production of C.I. Pigment Yellow 180> (Production Example 3-1) PY180-2 While stirring 1300 parts of water, 100 parts of 1,2-bis(2-aminophenoxy)ethane was added and dispersed. After 1 hour, 223.9 parts of 35% hydrochloric acid was added. After further stirring for 1 hour, ice was added to adjust the temperature to 0 to 5 °C, and 148.7 parts of a 38% aqueous sodium nitrite solution was added to carry out a diazotization reaction. Sulfamic acid was added to remove excess nitrite, and the mixture was stirred for 30 minutes or more to obtain a diazo component. On the other hand, 190.9 parts of 5-acetoacetylamino-benzimidazolone was dispersed in 1,500 parts of methanol, and then 393.0 parts of a 25% aqueous sodium hydroxide solution was added to dissolve it, and 4.4 parts of sodium dialkylsulfosuccinate (Pelex OT-P, manufactured by Kao Corporation) was further added to obtain a coupler component.

[0291] Separately, 500 parts of ice was added to 813.5 parts of 80% aqueous acetic acid, and 223.9 parts of 25% aqueous sodium hydroxide was added while stirring to prepare an acetic acid-sodium acetate buffer solution. The diazo component and the coupler component were simultaneously added dropwise to the buffer solution held at 20°C while stirring to carry out a coupling reaction. The dropping speed was adjusted so that the diazo component and the coupler component each finished dropping in 2 hours. After the coupling reaction was completed, it was confirmed that no unreacted diazo component was contained in the reaction solution, and the solution was heated to 90°C and held for 30 minutes. The solution was then filtered and washed with water to obtain a water-containing wet cake. The entire amount of the above-mentioned wet cake in a water-containing state was charged into a pressurizable reaction vessel equipped with a stirrer. Water was added to make the mass in the vessel 3500 parts and stirred, and then 200 parts of ortho-xylene and 20 parts of coconut oil fatty acid diethanolamide (Toho N-220, manufactured by Toho Chemical Industry Co., Ltd.) were added, followed by heating at 150°C for 2 hours in an autoclave under autogenous pressure. After removing ortho-xylene by steam distillation, the mixture was filtered, washed with water, dried at 80°C, and pulverized to obtain 257.9 parts of PY180-2. The average primary particle diameter was 260 nm.

[0292] (Manufacturing example 3-2) PY180-3 The entire amount of the wet cake obtained in Production Example 3-1 in a pressurizable reaction vessel equipped with a stirrer was charged. Water was added to the vessel to bring the mass to 3500 parts, and the mixture was stirred. 1800 parts of isobutanol were then added, followed by heating at 110°C for 2 hours in an autoclave under autogenous pressure. After removing the isobutanol by steam distillation, the mixture was filtered, washed with water, dried at 80°C, and pulverized to obtain 258.2 parts of PY180-3. The average primary particle size was 208 nm.

[0293] (Manufacturing example 3-3) PY180-4 100 parts of PY180-2, 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 8 hours at 80° C. Next, the kneaded mixture was poured into warm water at about 70° C. and stirred for 1 hour to form a slurry, which was then repeatedly filtered and washed with water to remove the sodium chloride and diethylene glycol, and then dried overnight at 80° C. and pulverized to obtain 95 parts of PY180-4. The average primary particle size was 93 nm.

[0294] (Manufacturing example 3-4) PY180-5 100 parts of PY180-3, 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 8 hours at 60° C. Next, the kneaded mixture was poured into warm water at about 70° C. and stirred for 1 hour to form a slurry, which was then repeatedly filtered and washed with water to remove the sodium chloride and diethylene glycol, and then dried overnight at 80° C. and pulverized to obtain 95 parts of PY180-5. The average primary particle size was 65 nm.

[0295] <Production of phthalocyanine pigments> (Production Example 4-1) Aluminum phthalocyanine In a reaction vessel, 1250 parts of n-amyl alcohol, 225 parts of phthalodinitrile, and 78 parts of aluminum chloride anhydride were added and mixed and stirred. 266 parts of DBU (1,8-diazabicyclo[5.4.0]undec-7-ene) were added to the mixture, and the mixture was heated and refluxed at 136°C for 5 hours. The reaction solution was cooled to 30°C while stirring, and poured into a mixed solvent consisting of 5000 parts of methanol and 10000 parts of water while stirring, to obtain a blue slurry. The slurry was filtered, washed with a mixed solvent consisting of 2000 parts of methanol and 4000 parts of water, and dried to obtain 135 parts of chloroaluminum phthalocyanine represented by the following chemical formula (14).

[0296] [ka]

[0297] Next, 1500 parts of concentrated sulfuric acid was added to the reaction vessel, and then 100 parts of the above chloroaluminum phthalocyanine was added in an ice bath, followed by stirring for 4 hours at 25° C. Subsequently, this sulfuric acid solution was poured into 9000 parts of cold water at 3° C., and the resulting precipitate was filtered, washed with water, washed with a 1% aqueous sodium hydroxide solution, and washed with water, in that order, and then dried to obtain 98 parts of aluminum phthalocyanine represented by the following chemical formula (12).

[0298] [ka]

[0299] (Production Example 4-2) Titanyl phthalocyanine In a reaction vessel, 1280 parts of 1-hexanol, 320 parts of quinoline, 320 parts of 1,3-diiminoisoindoline, and 206.3 parts of tetrabutyl orthotitanate were added and mixed and stirred. The mixture was heated to 155°C and refluxed for 8 hours. The n-butanol generated in the system was collected so as not to return to the system. The reaction solution was cooled to 60°C while being stirred, and 1000 parts of methanol was added. The slurry was filtered, washed with 1000 parts of methanol, 500 parts of N-methylpyrrolidone, and 1000 parts of methanol in that order, and dried to obtain 250 parts of titanyl phthalocyanine crude represented by the following chemical formula (13).

[0300] [ka]

[0301] Next, 1500 parts of concentrated sulfuric acid was added to the reaction vessel, and then 100 parts of the titanyl phthalocyanine crude was added in an ice bath, and the mixture was stirred at 25°C for 4 hours. Subsequently, this sulfuric acid solution was poured into 9000 parts of cold water at 3°C, and the resulting precipitate was filtered, washed with water, washed with 1% aqueous sodium hydroxide solution, and washed with water in that order to obtain a cake. Next, 1000 parts of diethylene glycol and the resulting cake were added to the reaction vessel, and the mixture was stirred to form a slurry, which was then stirred at 120°C for 3 hours. The slurry was cooled to 60°C, filtered, washed with 5000 parts of water, and dried to obtain 87 parts of titanyl phthalocyanine.

[0302] <Production of dioxazine pigments> (Production Example 5-1) Dioxazine Pigment 1 In a reaction vessel equipped with a stirrer, 110.6 parts of 3-amino-N-ethylcarbazole and 900 parts of 1,2-dichlorobenzene were placed and stirred to dissolve. The temperature was then raised to 36°C, and a solution of 73.8 parts of chloranil and 55.3 parts of triethylamine mixed and dissolved in 600 parts of 1,2-dichlorobenzene was added to the reaction vessel and stirred at 36°C for 4 hours. The reaction liquid was filtered, and the residue was washed with 900 parts of 1,2-dichlorobenzene and then with 1500 parts of hot water at 60°C. The residue was dried in a 100°C blower dryer for 18 hours to obtain 187.4 parts of intermediate 1. Next, 1,500 parts of 1,2-dichlorobenzene, 80.7 parts of benzenesulfonyl chloride, and the entire amount of the intermediate 1 obtained above were added to a reaction vessel equipped with a reflux condenser, a thermometer, and a stirrer, and the mixture was stirred at 160°C for 2 hours. After cooling to 150°C, the reaction liquid was filtered, and the residue was washed with 900 parts of 1,2-dichlorobenzene preheated to 120°C. Next, the residue was washed with 900 parts of mixed alcohol (methanol:ethanol = 50%:50%) preheated to 45°C and 500 parts of methanol preheated to 45°C. The obtained wet cake was thoroughly washed with water, and then dried for 18 hours in a 100°C blower dryer to obtain 179.6 parts of dioxazine compound 1 represented by the following formula (304).

[0303] Next, 150 parts of dioxazine compound 1, 1000 parts of sodium chloride, and 200 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 6 hours at 80° C. Next, the kneaded mixture was poured into warm water at about 70° C. and stirred for 1 hour to form a slurry, which was then repeatedly filtered and washed with water to remove the sodium chloride and diethylene glycol, and then dried overnight at 80° C. and pulverized to obtain 147 parts of dioxazine pigment 1.

[0304] [ka]

[0305] (Production Example 5-2) Dioxazine Pigment 2 In Production Example 5-1, 110.6 parts of 3-amino-N-ethylcarbazole and 73.8 parts of chloranil were replaced with 134.9 parts of N-(4-amino-2-methoxyphenyl)benzamide and 87.3 parts of 2,5-diacetylamino-3,6-dichloro-1,4-benzoquinone, but the reaction was carried out in the same manner as in Production Example 5-1 to obtain 221.4 parts of dioxazine compound 2 represented by the following formula (312) and 147 parts of dioxazine pigment 2.

[0306] [ka]

[0307] (Production Example 5-3) Dioxazine pigment 3 In Production Example 5-1, except that 110.6 parts of 3-amino-N-ethylcarbazole was changed to 93.2 parts of 5-amino-1-ethylbenzimidazolone, the same reaction operation as in Production Example 5-1 was carried out to obtain 159.4 parts of dioxazine compound 3 represented by the following formula (310) and 147 parts of dioxazine pigment 3.

[0308] [ka]

[0309] (Production Example 5-4) Dioxazine Pigment 4 In Production Example 5-1, the reaction operation was carried out in the same manner as in Production Example 5-1 except that 110.6 parts of 3-amino-N-ethylcarbazole and 73.8 parts of chloranil were changed to 134.9 parts of N-(4-amino-2-methoxyphenyl)benzamide and 96.3 parts of 2,5-dichloro-3,6-dicarboethoxy-1,4-benzoquinone, and 230.5 parts of dioxazine compound 4 represented by the following formula (313) and 147 parts of dioxazine pigment 4 were obtained.

[0310]

Chemical formula

[0311] (Production Example 5-5) Dioxazine Pigment 5 In Production Example 5-1, the reaction operation was carried out in the same manner as in Production Example 5-1 except that 110.6 parts of 3-amino-N-ethylcarbazole and 73.8 parts of chloranil were changed to 123.3 parts of N-phenyl-1,4-naphthalenediamine and 61.5 parts of 2,5-dichloro-3,6-dimethyl-1,4-benzoquinone, and 181.8 parts of dioxazine compound 5 represented by the following formula (307) and 147 parts of dioxazine pigment 5 were obtained.

[0312]

Chemical formula

[0313] <Manufacture of C.I. Pigment Red 122> (Production Example 6-1) PR122-3 45.60 parts (0.2 mol) of well-dried 1,4-cyclohexanedione-2,5-di(methyl carboxylate), 53.5 parts (0.5 mol) of p-toluidine, 500 parts of methanol, and 4.65 parts (0.045 mol) of 35% hydrochloric acid were weighed into a 1-liter pressure-resistant glass autoclave, sealed, and then the oxygen in the reaction vessel was sufficiently replaced with nitrogen gas, and then the gauge pressure was 0 kg / cm 2The temperature was raised from room temperature to 100°C in 15 minutes with strong stirring, and the reaction was carried out for 3 hours. The maximum pressure in the reaction vessel during the reaction was 3.8 kg / cm 2 After the reaction, the mixture was cooled to below 30°C and then opened to atmospheric pressure. 18 parts of a 10% aqueous sodium hydroxide solution was added and stirred for 10 minutes, after which the product was filtered. The filtered cake was thoroughly washed with methanol heated to 60°C. The yield of the produced 2,5-di-p-toluidino-3,6-dihydroterephthalic acid dimethyl ester was 75.07 parts, which was 99.3% of the theoretical yield. The purity was 99.5%.

[0314] Next, 30 parts of the 2,5-di-p-toluidino-3,6-dihydroterephthalic acid dimethyl ester obtained above and 150 parts of the dimethylnaphthalene isomer mixture were heated to 120 to 170°C while stirring in a nitrogen gas atmosphere in a 200-mL flask having an outlet valve at the bottom. Meanwhile, 150 parts of the dimethylnaphthalene isomer mixture was heated to 280°C or higher in a 500-mL flask while stirring in a nitrogen gas atmosphere. The above hot mixture was introduced therein over 20 to 40 minutes, and the mixture was then held at 280 to 283°C (reflux) for 30 minutes. From the moment that 2,5-dianilino-3,6-dihydroterephthalic acid dimethyl ester and dimethylnaphthalene isomer mixture at 120-170°C were introduced into the boiling dimethylnaphthalene isomer mixture, a reaction to produce 2,9-dimethyl-6,13-dihydroquinacridone was initiated accompanied by the generation of methanol, and the generation of methanol almost ceased immediately after the start of reflux at 283°C. After cooling to 100°C, the nitrogen gas atmosphere was released, and the contents were filtered, washed with 500 parts of hot methanol, and dried to obtain 24.44 parts of 2,9-dimethyl-6,13-dihydroquinacridone (96.71% of the theoretical amount).

[0315] 10 parts of the 2,9-dimethyl-6,13-dihydroquinacridone obtained above and 80 parts of methanol were charged into a 200 ml flask equipped with a reflux condenser and stirred. 12 parts of 50% aqueous sodium hydroxide solution were added and stirred at 40°C for 30 minutes, then 26 parts of 10% sulfuric acid were added dropwise to hydrolyze, after which 10 parts of sodium m-nitrobenzenesulfonate was quickly added, and 3 parts of 50% aqueous sodium hydroxide solution was immediately added, followed by refluxing for 4 hours. The mixture was filtered, washed with water, dried, and pulverized to obtain 9.60 parts of crude 2,9-dimethyl-quinacridone.

[0316] Then, the mixture was cooled to 10°C or less in an ice bath, and 90 parts of the crude 2,9-dimethyl-quinacridone obtained above was added to 90 parts of 98% sulfuric acid stirred in a flask, while being careful not to raise the temperature above 30°C. After the entire amount was added, the mixture was stirred at 30°C or less for 1 hour. The sulfuric acid solution was added dropwise to 1000 parts of stirred water at 10°C, while being careful not to bump. After the dropwise addition was completed, the mixture was filtered and washed with water until it became neutral, to obtain a press cake. Water was added to the obtained press cake, and the pH was adjusted to 9.0 with sodium hydroxide. Next, 0.09 parts of a condensation product of stearic acid chloride and taurine, water and isobutanol were added so that the pigment solid content in a 35% isobutanol-water mixed solution became a 4% suspension. This suspension was refluxed for 4 hours, and then isobutanol was distilled off until the liquid temperature reached 99°C. After cooling to 70° C., the mixture was filtered, washed with hot water at 60° C., dried, and pulverized to obtain 8.9 parts of PR122-3. The average primary particle size was 163 nm.

[0317] (Manufacturing example 6-2) PR122-4 100 parts of PR122-3, 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded for 4 hours at 140° C. Next, the kneaded mixture was poured into warm water at about 70° C. and stirred for 1 hour to form a slurry, which was then repeatedly filtered and washed with water to remove the sodium chloride and diethylene glycol, and then dried overnight at 80° C. and pulverized to obtain 95 parts of PR122-4. The average primary particle size was 140 nm.

[0318] (Production Example 6-3) PR122-5 100 parts of PR122-3, 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a 1-gallon stainless steel kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded at 90°C for 8 hours. Next, the kneaded mixture was poured into warm water at about 70°C and stirred for 1 hour to form a slurry. After repeating filtration and washing with water to remove sodium chloride and diethylene glycol, it was dried at 80°C for a whole day and night and pulverized to obtain 95 parts of PR122-4. The average primary particle size was 55 nm.

[0319] (Production Example 6-4) PR122-6 Cooled to 10°C or lower in an ice bath, and 9.5 parts of the crude 2,9-dimethyl-quinacridone obtained in Production Example 6-1 and 0.5 part of PV19-3 obtained in Production Example 7-1 described below were added to 90 parts of 98% sulfuric acid stirred in a flask while taking care that the temperature did not exceed 30°C. After adding all of these, it was stirred at 30°C or lower for 1 hour. The sulfuric acid solution was added dropwise to 1000 parts of stirred water at 10°C while taking care of bumping. After completion of the dropwise addition, it was filtered and washed with water until it became neutral to obtain a press cake. Water was added to the obtained press cake and the pH was adjusted to 9.0 with sodium hydroxide. Next, 0.09 part of the condensation product of stearic acid chloride and taurine, and water and isobutanol were added so that the pigment solid content in a 35% isobutanol-water mixed solution became a 4% suspension. This suspension was refluxed for 2 hours, and then isobutanol was distilled off until the liquid temperature reached 99°C. After cooling to 70°C, filtration, washing with 60°C warm water, drying, and pulverization were carried out to obtain 8.9 parts of PR122-6. The average primary particle size was 44 nm.

[0320] (Production of C.I. Pigment Violet 19) (Production Example 7-1) PV19-3 Thoroughly dried 1,4-cyclohexanedione-2,5-di(methyl ester) 45.6 parts (0.2 moles), aniline 46.57 parts (0.5 moles), methanol 500 parts, and 35% hydrochloric acid 4.65 parts (0.045 moles) were weighed and placed in a 1-liter pressure-resistant glass autoclave, sealed, and then oxygen in the reaction vessel was thoroughly replaced with nitrogen gas, and the gauge pressure was reduced to 0 kg / cm. 2 The temperature was raised from room temperature to 100°C in 15 minutes with strong stirring, and the reaction was carried out for 3 hours. The maximum pressure in the reaction vessel during the reaction was 3.8 kg / cm 2 After the reaction, the mixture was cooled to below 30°C and released to atmospheric pressure, and 18 parts of a 10% aqueous sodium hydroxide solution was added and stirred for 10 minutes, after which the product was filtered. The filtered cake was thoroughly washed with methanol heated to 60°C. The yield of the produced 2,5-dianilino-3,6-dihydroterephthalic acid dimethyl ester was 75.07 parts, which was 99.3% of the theoretical yield. The purity was 99.5%.

[0321] Next, 30 parts of the 2,5-dianilino-3,6-dihydroterephthalic acid dimethyl ester obtained above and 150 parts of the dimethylnaphthalene isomer mixture were heated to 120 to 170°C while stirring in a nitrogen gas atmosphere in a 200-mL flask having an outlet valve at the bottom. Meanwhile, 150 parts of the dimethylnaphthalene isomer mixture was heated to 280°C or higher in a 500-mL flask while stirring in a nitrogen gas atmosphere. The above hot mixture was introduced therein over 20 to 40 minutes, and the mixture was then maintained at 280 to 283°C (reflux) for 30 minutes. From the moment that 2,5-dianilino-3,6-dihydroterephthalic acid dimethyl ester and dimethylnaphthalene isomer mixture at 120-170°C were introduced into the boiling dimethylnaphthalene isomer mixture, the reaction to produce 6,13-dihydroquinacridone was initiated, accompanied by the evolution of methanol, and the evolution of methanol almost ceased immediately after the start of reflux at 283°C. After cooling to 100°C, the nitrogen gas atmosphere was removed, and the contents were filtered, washed with 500 parts of hot methanol, and dried to obtain 24.47 parts of 6,13-dihydroquinacridone (98.2% of the theoretical amount). The purity was 99% or more by IR and absorbance.

[0322] 10 parts of 6,13-dihydroxyquinacridone obtained above and 80 parts of methanol were charged into a 200 ml flask equipped with a reflux condenser and stirred. 12 parts of a 50% aqueous sodium hydroxide solution was added, and the mixture was stirred at 40 °C for 30 minutes. Then, 26 parts of 10% sulfuric acid was added dropwise and hydrolyzed. Immediately thereafter, 10 parts of sodium m-nitrobenzenesulfonate was added, and immediately after that, 3 parts of a 50% aqueous sodium hydroxide solution was added. The mixture was then refluxed for 4 hours. The mixture was filtered, washed with water, dried, and pulverized to obtain 9.82 parts of PV19-3. The average primary particle diameter was 130 nm.

[0323] (Production Example 7-2) PV19-4 100 parts of PV19-3, 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a 1-gallon stainless steel kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded at 120 °C for 4 hours. Next, the kneaded mixture was poured into warm water at about 70 °C and stirred for 1 hour to form a slurry. After repeating filtration and washing with water to remove sodium chloride and diethylene glycol, it was dried at 80 °C for one day and night and pulverized to obtain 95 parts of PV19-4. The average primary particle diameter was 108 nm.

[0324] (Production Example 7-3) PV19-5 95 parts of PV19-3, 5 parts of PR122-5, 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a 1-gallon stainless steel kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded at 60 °C for 4 hours. Next, the kneaded mixture was poured into warm water at about 70 °C and stirred for 1 hour to form a slurry. After repeating filtration and washing with water to remove sodium chloride and diethylene glycol, it was dried at 80 °C for one day and night and pulverized to obtain 95 parts of PV19-5. The average primary particle diameter was 31 nm.

[0325] (Production of C.I. Pigment Red 254) (Production Example 8-1) PR254-7 300 parts of Cinilex DPP Red SR2P (manufactured by Shin-Nippon Chemicals Co., Ltd.), 1000 parts of sodium chloride, and 400 parts of diethylene glycol were charged into a 1-gallon stainless steel kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded at 100 °C for 6 hours. Next, the kneaded mixture was poured into warm water at about 70 °C and stirred for 1 hour to form a slurry. After repeating filtration and washing with water to remove sodium chloride and diethylene glycol, it was dried at 80 °C for 24 hours and pulverized to obtain 290 parts of PR254-7. The average primary particle size was 115 nm.

[0326] (Production Example 8-2) PR254-8 200 parts of Cinilex DPP Red SR2P (manufactured by Shin-Nippon Chemicals Co., Ltd.), 1000 parts of sodium chloride, and 250 parts of diethylene glycol were charged into a 1-gallon stainless steel kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded at 65 °C for 8 hours. Next, the kneaded mixture was poured into warm water at about 70 °C and stirred for 1 hour to form a slurry. After repeating filtration and washing with water to remove sodium chloride and diethylene glycol, it was dried at 80 °C for 24 hours and pulverized to obtain 190 parts of PR254-8. The average primary particle size was 63 nm.

[0327] (Production of C.I. Pigment Red 272) (Production Example 9-1) PR272-3 100 parts of Irgazin Flame Red K3800 (manufactured by BASF C&E), 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a 1-gallon stainless steel kneader (manufactured by Inoue Seisakusho Co., Ltd.) and kneaded at 60 °C for 8 hours. Next, the kneaded mixture was poured into warm water at about 70 °C and stirred for 1 hour to form a slurry. After repeating filtration and washing with water to remove sodium chloride and diethylene glycol, it was dried at 80 °C for 24 hours and pulverized to obtain 95 parts of PR272-3. The average primary particle size was 47 nm.

[0328] (Production of C.I. Pigment Red 255) (Production Example 10-1) PR255-2 200 parts of Irgazin Scarlet L3550HD (manufactured by BASF C&E), 1000 parts of sodium chloride, and 250 parts of diethylene glycol were charged into a 1-gallon stainless steel kneader (manufactured by Inoue Seisakusho) and kneaded at 100 °C for 8 hours. Next, the kneaded mixture was poured into warm water at about 70 °C and stirred for 1 hour to form a slurry. After repeating filtration and washing with water to remove sodium chloride and diethylene glycol, it was dried at 80 °C for a whole day and night and pulverized to obtain 190 parts of PR255-2. The average primary particle size was 123 nm.

[0329] (Production Example 10-2) PR255-3 100 parts of Irgazin Scarlet L3550HD (manufactured by BASF C&E), 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a 1-gallon stainless steel kneader (manufactured by Inoue Seisakusho) and kneaded at 60 °C for 8 hours. Next, the kneaded mixture was poured into warm water at about 70 °C and stirred for 1 hour to form a slurry. After repeating filtration and washing with water to remove sodium chloride and diethylene glycol, it was dried at 80 °C for a whole day and night and pulverized to obtain 95 parts of PR255-3. The average primary particle size was 46 nm.

[0330] <Production of C.I. Pigment Orange 73> (Production Example 11-1) PO73-3 100 parts of Irgazin Orange L2990HD (manufactured by BASF C&E), 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a 1-gallon stainless steel kneader (manufactured by Inoue Seisakusho) and kneaded at 100 °C for 8 hours. Next, the kneaded mixture was poured into warm water at about 70 °C and stirred for 1 hour to form a slurry. After repeating filtration and washing with water to remove sodium chloride and diethylene glycol, it was dried at 80 °C for a whole day and night and pulverized to obtain 95 parts of PO73-3. The average primary particle size was 116 nm.

[0331] <Production of C.I. Pigment Red 179> (Manufacturing example 12-1) PR179-5 100 parts of Paliogen Red K4180 (BASF C&E), 1000 parts of sodium chloride, and 150 parts of diethylene glycol were charged into a stainless steel 1-gallon kneader (Inoue Seisakusho) and kneaded for 8 hours at 80° C. Next, the kneaded mixture was poured into warm water at about 70° C. and stirred for 1 hour to form a slurry, which was then repeatedly filtered and washed with water to remove sodium chloride and diethylene glycol, and then dried overnight at 80° C. and pulverized to obtain 95 parts of PR179-5. The average primary particle size was 78 nm.

[0332] <1> Evaluation of gravure ink sets First, the measurement method for the resin will be described below. (Hydroxyl value) Calculated in accordance with JIS K0070. (Acid value) Calculated in accordance with JIS K0070. (amine value) The amine value was determined by the following method in accordance with JIS K0070, in terms of the equivalent amount of hydrochloric acid and the equivalent amount of potassium hydroxide required to neutralize the amino groups contained in 1 g of resin. 0.5 to 2 g of sample was precisely weighed out (non-volatile content of sample: Sg). 50 mL of a mixed solution of methanol / methyl ethyl ketone = 60 / 40 (mass ratio) was added to the precisely weighed sample to dissolve it. Bromophenol blue was added to the obtained solution as an indicator, and the obtained solution was titrated with 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the color of the solution changed from green to yellow was set as the endpoint, and the titration amount (A mL) at this point was used to calculate the amine value according to the following formula. Amine value = (A x f x 0.2 x 56.108) / S [mgKOH / g]

[0333] (Weight average molecular weight) The weight average molecular weight was determined by measuring the molecular weight distribution using a GPC (gel permeation chromatography) device (HLC-8220 manufactured by Tosoh Corporation) and calculating the molecular weight converted using polystyrene as a standard substance. The measurement conditions are shown below. Columns: The following columns were used in series connection: Tosoh Guard Column HXL-H Tosoh TSKgelG5000HXL Tosoh TSKgelG4000HXL Tosoh TSKgelG3000HXL Tosoh TSKgelG2000HXL Detector: RI (differential refractometer) Measurement conditions: Column temperature 40℃ Eluent: Tetrahydrofuran Flow rate: 1.0mL / min

[0334] (glass transition temperature) The glass transition temperature (Tg) was determined by DSC (differential scanning calorimetry) using a Rigaku DSC8231 measuring device, with a measurement temperature range of -70 to 250°C, a heating rate of 10°C / min, and the midpoint between the endothermic start and end temperatures due to the glass transition in the DSC curve being taken as the glass transition temperature.

[0335] (Synthesis Example 1) Polyurethane resin solution [PU1] 54.719 parts of polyester diol having a number average molecular weight of 2,000 obtained from adipic acid and 3-methyl-1,5-pentanediol, 3.989 parts of isophorone diisocyanate (hereinafter "IPDI"), and 10.0 parts of n-propyl acetate (hereinafter "nPAc") were reacted at 85°C for 3 hours under a nitrogen stream, 10.0 parts of nPAc was added, and the mixture was cooled to obtain 78.708 parts of a solvent solution of a terminal isocyanate prepolymer. Next, 78.708 parts of the obtained solvent solution of the isocyanate-terminated prepolymer was gradually added at room temperature to a mixture of 1.031 parts of isophorone diamine (hereinafter "IPDA"), 0.261 parts of di-n-butylamine, 72.96 parts of nPAc, and 47.04 parts of isopropanol (hereinafter "IPA"), and then the mixture was allowed to react at 50°C for 1 hour to obtain a polyurethane resin solution [PU1] with a non-volatile content of 30%, a weight average molecular weight of 60,000, and an amine value of 3.0 mgKOH / g.

[0336] (Synthesis Example 2) Polyurethane resin solution [PU2] 200 parts of polypropylene glycol (hereinafter "PPG700") having a number average molecular weight of 700, 127 parts of IPDI, and 81.8 parts of ethyl acetate were reacted at 80°C for 4 hours under a nitrogen stream to obtain a resin solution of a terminal isocyanate urethane prepolymer. Next, 49.5 parts of IPDA, 3 parts of 2-ethanolamine, and 803.9 parts of a mixed solvent of ethyl acetate / isopropanol (hereinafter "IPA") = 50 / 50 (mass ratio) were mixed, and the obtained resin solution of the terminal isocyanate urethane prepolymer was gradually added at 40°C, and then reacted at 80°C for 1 hour to obtain a polyurethane resin solution [PU2] with a non-volatile content of 30%, an amine value of 3.5 mgKOH / g, a hydroxyl value of 7.3 mgKOH / g, and a weight average molecular weight of 40,000. The glass transition temperature was -32°C.

[0337] (Preparation of polyvinyl butyral resin solution [PVB1]) A polyvinyl butyral resin (weight average molecular weight 19,000) having vinyl alcohol units, vinyl acetate units, and vinyl butyral units, and containing 73 mass% butyral ring groups and 26 mass% hydroxyl groups, was dissolved in a mixed solvent of ethyl acetate / IPA = 1 / 1 (mass ratio) to prepare a polyvinyl butyral resin solution [PVB1] with a solid content of 30%.

[0338] (Preparation of polyvinyl butyral resin solution [PVB2]) A polyvinyl butyral resin (weight average molecular weight 33,000) having vinyl alcohol units, vinyl acetate units, and vinyl butyral units, and containing 77 mass% butyral ring groups and 21 mass% hydroxyl groups, was dissolved in a mixed solvent of ethyl acetate / IPA = 1 / 1 (mass ratio) to prepare a polyvinyl butyral resin solution [PVB2] with a solid content of 30%.

[0339] (Preparation of polyvinyl butyral resin solution [PVB3]) A polyvinyl butyral resin (weight average molecular weight 33,000) having vinyl alcohol units, vinyl acetate units, and vinyl butyral units, and containing 84 mass% butyral ring groups and 14 mass% hydroxyl groups, was dissolved in a mixed solvent of ethyl acetate / IPA = 1 / 1 (mass ratio) to prepare a polyvinyl butyral resin solution [PVB3] with a solid content of 30%.

[0340] [Production of gravure ink] (Production Example Y1-1) [Preparation of Yellow Ink [Y1-1]] 7.0 parts of isoindoline compound (1-1), 29.5 parts of polyurethane resin solution [PU1], 5.0 parts of polyurethane resin solution [PU2], 20 parts of nPAc, and 5 parts of IPA were mixed and ground with a sand mill. Next, 20 parts of polyurethane resin solution [PU2], 11 parts of nPAc, and 3 parts of IPA were added and mixed and stirred to obtain yellow ink [Y1-1].

[0341] (Production Examples Y1-2 to Y1-28, C1-1 to C1-5, M1-1 to M1-54) [Preparation of Yellow Inks [Y1-2] to [Y1-28], Cyan Inks [C1-1] to [C1-5], and Magenta Inks [M1-1] to [M1-54]] In the preparation method of yellow ink [Y1-1] described in Production Example Y1-1, except that 7.0 parts of the isoindoline compound (1-1) was changed to the compound shown in Table 3 and in the amount shown in Table 3, the same procedure as in Production Example Y1-1 was carried out to obtain the ink described in Table 3.

[0342] [Table 3-1]

[0343] [Table 3-2]

[0344] (Production Example Y2-1) [Preparation of Yellow Ink [Y2-1]] 7.0 parts of isoindoline compound (1-3), 29.5 parts of polyurethane resin solution [PU1], 5.0 parts of polyvinyl butyral resin solution [PVB1], 20 parts of nPAc, and 5 parts of IPA were mixed and ground with a sand mill. Next, 20 parts of polyurethane resin solution [PU2], 11 parts of nPAc, and 3 parts of IPA were further added and mixed and stirred to obtain yellow ink [Y2-1].

[0345] (Production Examples Y2-2 to Y2-5, C2-1 to C2-3, M2-1 to M2-17) [Preparation of Yellow Inks [Y2-2] to [Y2-5], Cyan Inks [C2-1] to [C2-3], and Magenta Inks [M2-1] to [M2-17]] In the preparation method of yellow ink [Y2-1] described in Production Example Y2-1, except that 7.0 parts of the isoindoline compound (1-3) and 5.0 parts of the polyvinyl butyral resin solution [PVB1] were changed to the compounds shown in Table 4, in the amounts shown in Table 4, and to the polyvinyl butyral resin shown in Table 4, the same procedures as in Production Example Y2-1 were followed to obtain the inks shown in Table 4.

[0346] [Table 4]

[0347] The pigments used in making the inks are shown in Table 5.

[0348] [Table 5]

[0349] <Evaluation of printing ink set> (Examples AS-1 to AS-99, Comparative Examples AS-1 to AS-11) The inks obtained were combined as shown in Table 6 to form ink sets A1 to A110. The resulting printing ink sets were evaluated for gamut, lightfastness, and adhesion by the following methods. The results are shown in Tables 7, 8, and 9.

[0350] [Table 6-1]

[0351] [Table 6-2]

[0352] [Table 6-3]

[0353] [Initial gamut evaluation] The yellow ink, cyan ink, and magenta ink were each diluted with mixed solvent 1 (methyl ethyl ketone: nPAc: IPA = 40:40:20) so that the viscosity became 16 seconds (25°C, Zahn cup No. 3). Using each diluted ink, printing was performed in the order of cyan, magenta A, magenta B, and yellow, to obtain printed matter having a single-color solid area (cyan, magenta A, magenta B, yellow) and a single-color solid overprint area (yellow x cyan, cyan x magenta A, yellow x magenta B, or yellow x magenta A). The printing conditions are as follows:

[0354] (Printing conditions) Printing machine: Fuji Kikai 5 color machine Cyan version: Helio 175L / inch, stylus angle 120°, elongated Magenta version: Helio 175L / inch, stylus angle 120°, compressed Yellow version: Helio 175L / inch, stylus angle 120°, compressed Printing speed: 150m / min Substrate: Corona-treated biaxially oriented polypropylene (OPP) film (Toyobo Pylen P-2161, 20 μm) Drying temperature: 50℃

[0355] The density values ​​of the monochrome solid areas (yellow, magenta A, magenta B, cyan) of the obtained prints were measured using a Gretagmacbeth D196. In addition, the monochrome solid areas and overprinted areas were measured using a Gretagmacbeth SpectroEye as a measuring instrument under the conditions of a D50 light source, a 2-degree observation field, a white back (a standard white board was used), and no filters were used. a * on the horizontal axis, b * In the two-dimensional space with the vertical axis, the monochrome solid areas (yellow, magenta A, magenta B, cyan) and monochrome solid overprint areas (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A) are printed in a total of 6 or 7 colors. * vs. b * The values ​​were plotted to determine the area. The area ratio was calculated based on the area of ​​the comparative example AS-1, which served as the standard, being taken as 100%, and the results were evaluated based on the area ratio according to the following criteria. The results are shown in Table 7. The practical level is 3 or higher.

[0356] (Evaluation Criteria) 6: Area ratio is 115% or more 5: Area ratio is 110% or more and less than 115% 4: Area ratio is 105% or more and less than 110% 3: Area ratio is 100% or more and less than 105% 2: Area ratio is 98% or more but less than 100% 1: Area ratio is less than 98%

[0357] [Lightfastness rating 1] (UV radiation test using a fadeometer) The printed matter obtained above was irradiated with ultraviolet light for 48 hours using a fadeometer (ultraviolet carbon arc lamp type lightfastness tester), and the color was measured in the same manner as above after the test. The ultraviolet light irradiation conditions were in accordance with JIS L0842:2004 and JIS B7751:2007.

[0358] (Gamut) In the same manner as in the initial gamut evaluation method, the solid color area and the overprinted area of ​​the printed matter after the ultraviolet irradiation test were measured, and* vs. b * The values ​​were plotted to determine the area. The area after the ultraviolet irradiation test for each Example and Comparative Example was divided by the area at the initial evaluation to determine the area ratio, and the area ratio was used to evaluate the product according to the following criteria. The results are shown in Table 7. The practical level is 3 or higher.

[0359] (Evaluation Criteria) 6: Area ratio is 98% or more 5: Area ratio is 97.5% or more and less than 98% 4: Area ratio is 97% or more and less than 97.5% 3: Area ratio is 96.5% or more and less than 97% 2: Area ratio is 96% or more and less than 96.5% 1: Area ratio is less than 96%

[0360] (color difference ΔE * ab) The color difference ΔE before and after the UV irradiation test was measured from the color measurement results of the single-color solid area (yellow, magenta A, magenta B, cyan). * The ab was calculated and evaluated according to the following criteria. The results are shown in Table 7. The practical level is 3 or higher.

[0361] (Evaluation Criteria) 6:ΔE * ab is less than 1.0 5:ΔE * ab is greater than or equal to 1.0 and less than 1.5 4:ΔE * ab is 1.5 or more and less than 2.0 3:ΔE * ab is 2.0 or more and less than 3.0 2:ΔE * ab is 3.0 or more and less than 5.0 1:ΔE * ab is 5.0 or more

[0362] (Hue difference ΔH * ) From the color measurement results of the single-color solid print overlapping parts (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A), the hue difference ΔH before and after the ultraviolet irradiation test * was determined and evaluated according to the following criteria. The results are shown in Table 7. The practical level is 3 or higher. If the hue angle (H°) after the test was larger than the H° before the test, a "+" was added, and if the hue angle (H°) after the test was smaller than the H° before the test, a "-" was added.

[0363] (Evaluation Criteria) 6:ΔH * is less than 0.5 5:ΔH * is greater than or equal to 0.5 and less than 0.75 4:ΔH * is greater than or equal to 0.75 and less than 1.0 3:ΔH * is greater than or equal to 1.0 and less than 1.5 2:ΔH * is greater than or equal to 1.5 and less than 3.0 1:ΔH * is 3.0 or higher

[0364] [Lightfastness rating 2] (White LED irradiation test) The prints obtained above were subjected to a white LED irradiation test using the following test method. After the test, the color was measured in the same manner as above to evaluate the stability of the hue under white LED irradiation. (Test Method) Testing machine: Illuminated incubator FLI-2010H-LED (Tokyo Rikakikai) Light source: white LED Illuminance: 15000Lux Irradiation temperature: 10℃ Irradiation humidity: 70%RH Irradiation period: 96 hours

[0365] (Gamut) In the same manner as the initial gamut evaluation method, the solid color area and the overprinted area were measured using the printed matter after the white LED irradiation test, and * vs. b *The values ​​were plotted to determine the area. The area after the white LED irradiation test for each Example and Comparative Example was divided by the area at the initial evaluation to determine the area ratio, and the area ratio was used to evaluate the product according to the following criteria. The results are shown in Table 8. The practical level is 3 or higher.

[0366] (Evaluation Criteria) 6: Area ratio is 98% or more 5: Area ratio is 97.5% or more and less than 98% 4: Area ratio is 97% or more and less than 97.5% 3: Area ratio is 96.5% or more and less than 97% 2: Area ratio is 96% or more and less than 96.5% 1: Area ratio is less than 96%

[0367] (color difference ΔE * ab) The color difference ΔE before and after the white LED irradiation test was measured based on the color measurement results of the single-color solid area (yellow, magenta A, magenta B, cyan). * The ab was calculated and evaluated according to the following criteria. The results are shown in Table 8. The practical level is 3 or higher.

[0368] (Evaluation Criteria) 6:ΔE * ab is less than 1.0 5:ΔE * ab is greater than or equal to 1.0 and less than 1.5 4:ΔE * ab is 1.5 or more and less than 2.0 3:ΔE * ab is 2.0 or more and less than 3.0 2:ΔE * ab is 3.0 or more and less than 5.0 1:ΔE * ab is 5.0 or more

[0369] (Hue difference ΔH * ) The hue difference ΔH before and after the white LED irradiation test was measured from the color measurement results of the single-color solid print overlapping area (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A). *was determined and evaluated according to the following criteria. The results are shown in Table 8. The practical level is 3 or higher. If the hue angle (H°) after the test was larger than the H° before the test, a "+" was added, and if the hue angle (H°) after the test was smaller than the H° before the test, a "-" was added.

[0370] (Evaluation Criteria) 6:ΔH * is less than 0.5 5:ΔH * is greater than or equal to 0.5 and less than 0.75 4:ΔH * is greater than or equal to 0.75 and less than 1.0 3:ΔH * is greater than or equal to 1.0 and less than 1.5 2:ΔH * is greater than or equal to 1.5 and less than 3.0 1:ΔH * is 3.0 or higher

[0371] [Table 7-1]

[0372] [Table 7-2]

[0373] [Table 7-3]

[0374] [Table 8-1]

[0375] [Table 8-2]

[0376] [Table 8-3]

[0377] In Tables 7 and 8, Y represents yellow, C represents cyan, MA represents magenta A, and MB represents magenta B. Also, Y×C represents yellow×cyan, C×MA represents cyan×magenta A, Y×MB represents yellow×magenta B, and Y×MA represents yellow×magenta A.

[0378] From the results of Tables 7 and 8, it was confirmed that the gravure printing ink set according to one embodiment of the present invention had high color reproducibility and good lightfastness. In particular, when a yellow ink containing isoindoline compound (4) or isoindoline compound (5) was used, the color reproducibility was higher and the lightfastness was better. In addition, when a yellow ink containing CI Pigment Yellow 180 having an optimal particle size was used, the color reproducibility was higher and the lightfastness was better. Furthermore, when a cyan ink containing CI Pigment Blue 15:3 or CI Pigment Blue 15:4 was used, the color reproducibility was higher and the light resistance was good. Furthermore, when Magenta Ink A containing CI Pigment Violet 23 or CI Pigment Violet 37 was used, the color reproducibility was higher and the lightfastness was good.

[0379] In addition, when magenta ink B containing CI Pigment Red 122 with the optimal particle size, CI Pigment Violet 19 with the optimal particle size, DPP pigment with the optimal particle size, or perylene pigment with the optimal particle size was used, the color reproducibility was higher and the lightfastness was better. In particular, in the yellow x magenta region, the printing ink set of the comparative example showed a significant change in hue to blue (smaller hue angle) in the lightfastness test using ultraviolet light irradiation, while the hue changed significantly to yellow (larger hue angle) in the lightfastness test using white LED irradiation. In other words, it is clear that the printing ink set of the comparative example shows different changes in hue over time depending on the light source, making it difficult to achieve sufficient lightfastness. In contrast, it is clear that the printing ink set of the embodiment of the present invention shows good lightfastness regardless of the light source.

[0380] [Adhesiveness] For the prints obtained as described above using the ink sets A3, A20, A80 to A99, and A110, 3 hours after printing, a 12 mm wide adhesive tape (cellophane tape manufactured by Nichiban Co., Ltd.) was attached to the printed surface, and the tape was quickly peeled off, and the degree of peeling of the ink coating was visually judged. The judgment criteria were as follows. The results are shown in Table 9. The practical level is 2 or higher.

[0381] (Evaluation Criteria) 5: Less than 1% of the ink coating on the printed surface has peeled off, or there is no peeling at all. 4: The peeled area of ​​the ink film is 1% or more but less than 2% 3: The peeled area of ​​the ink film is 2% or more but less than 3% 2: The peeled area of ​​the ink film is between 3% and 5%. 1: Ink coating peeling area is 5% or more

[0382] [Table 9]

[0383] As can be seen from the results in Table 9, the printing ink set containing polyvinyl butyral resin had better adhesion. In particular, the ink set containing polyvinyl butyral resin with a hydroxyl group content of 25% or less had even better adhesion. The printing ink set of the comparative example did not have good adhesion even though it contained polyvinyl butyral resin.

[0384] <Production of packaging materials> (Example BP-1) [Preparation of packaging material B1] The cyan ink [C1-1], magenta ink [M1-2], magenta ink [M1-17], and yellow ink [Y1-1] were each diluted with the above mixed solvent 1 so that the viscosity became 16 seconds (25° C., Zahn cup No. 3). Using each diluted ink, a gravure proofing 6-color press equipped with a gravure plate with a plate depth of 20 μm and an ink set B1 containing black ink (Rio Alpha R92 Black (manufactured by Toyo Ink Co., Ltd.)), cyan ink [C1-1], magenta ink [M1-2], magenta ink [M1-17], yellow ink [Y1-1], and white ink (Rio Alpha R631 White (manufactured by Toyo Ink Co., Ltd.)) was used to overprint a 20 μm-thick corona-treated stretched polypropylene film (OPP substrate) in the order of black ink, cyan ink [C1-1], magenta ink [M1-2], magenta ink [M1-17], yellow ink [Y1-1], and white ink. Each unit was dried at 50° C. to obtain a printed matter having a configuration of "OPP substrate / black, cyan, magenta A, magenta B, yellow, or white printed layer".

[0385] Next, a urethane-based laminating adhesive (TM320 / CAT13B manufactured by Toyo-Morton Co., Ltd., 30% non-volatile content in ethyl acetate solution) was applied onto the printed layer of the obtained printed matter in such a manner that the coating amount after drying was 2.0 g / m 2 Then, a 50 μm-thick unstretched polyethylene (PE) film was laminated onto the adhesive layer to obtain a packaging material B1 having a structure of "OPP substrate / five-color overlapping print layer / adhesive layer / PE substrate."

[0386] (Examples BP-2 to BP-99, Comparative Examples BP-1 to BP-2) [Preparation of Packaging Materials B2 to B101] Packaging materials B2 to B101 were obtained in the same manner as in Example BP-1, except that the ink set B1 used in Example BP-1 was changed to the ink set shown in Table 10.

[0387] [Table 10-1]

[0388] [Table 10-2]

[0389] As described above, packaging materials were made using the present and comparative gravure ink sets.

[0390] Among these packaging materials, the lamination strength of packaging materials B3, B20, and B80 to B101 was evaluated according to the following method. The results are shown in Table 11.

[0391] [Initial laminate strength evaluation] Each packaging material was cut to a width of 15 mm, and the printed layer and adhesive layer were peeled off, after which the peel strength was measured using an Intesco 201 universal tensile tester. The evaluation criteria were as follows. The results are shown in Table 11. The practical level is 2 or higher.

[0392] (Evaluation Criteria) 5: 2.0N / 15mm or more 4: 1.5N / 15mm or more, less than 2.0N / 15mm 3: 1.0N / 15mm or more, less than 1.5N / 15mm 2: 0.5N / 15mm or more, less than 1.0N / 15mm 1: Less than 0.5N / 15mm

[0393] [Laminate strength evaluation after light resistance test 1] (UV radiation test using a fadeometer) Each packaging material was irradiated with ultraviolet light for 48 hours using a fadeometer (ultraviolet carbon arc lamp type light resistance tester), and the peel strength was measured after the test in the same manner as above. The ultraviolet light irradiation conditions were in accordance with JIS L0842:2004 and JIS B7751:2007.

[0394] [Laminate strength evaluation after light resistance test 2] (White LED irradiation test) Each packaging material was subjected to a white LED irradiation test using the following test method. After the test, the peel strength was measured in the same manner as above. (Test Method) Testing machine: Illuminated incubator FLI-2010H-LED (Tokyo Rikakikai) Light source: white LED Illuminance: 15000Lux Irradiation temperature: 10℃ Irradiation humidity: 70%RH Irradiation period: 96 hours

[0395] [Table 11]

[0396] As can be seen from the results shown in Table 11, the packaging material using the printing ink set of this embodiment had good laminate strength even after the light fastness test. The packaging material using the ink set containing polyvinyl butyral resin had better laminate strength after the light fastness test. In particular, the packaging material using the printing ink set containing polyvinyl butyral resin with a hydroxyl group content of 25% or less had even better laminate strength after the light fastness test. On the other hand, the packaging material using the printing ink set of the comparative example did not reach a practical level of laminate strength after the light fastness test, and even if it contained polyvinyl butyral resin, good laminate strength was not obtained.

[0397] <2> Evaluation of water-based flexographic ink sets (Synthesis Example 3) (Synthesis of Water-Based Polyurethane Resin [PU3]) In a four-necked 2000 ml flask equipped with a reflux condenser, a dropping funnel, a gas inlet tube, a stirrer, and a thermometer, 82.3 parts of polytetramethylene ether glycol having a number average molecular weight of 2,000, 3 parts of polyethylene glycol having a number average molecular weight of 2,000, 13 parts of dimethylolbutanoic acid, and 1.7 parts of 1,4-cyclohexanedimethanol were charged, substituted with dry nitrogen, and heated to 100°C. With stirring, 33.3 parts of IPDI were dropped over 20 minutes, and the temperature was gradually raised to 140°C (NCO / OH=0.98). The reaction was continued for another 30 minutes to obtain a urethane resin. Next, 399.8 parts of distilled water containing 5.3 parts of 28% aqueous ammonia was added while cooling to obtain an aqueous polyurethane resin [PU3] (weight average molecular weight approximately 40,000, non-volatile content 25%, acid value 36.9 (mgKOH / g), hydroxyl value 11.1 (mgKOH / g)).

[0398] (Preparation of polyvinyl butyral resin solution [PVB4]) A polyvinyl butyral resin (weight average molecular weight 19,000) having vinyl alcohol units, vinyl acetate units, and vinyl butyral units, and containing 73 mass% butyral ring groups and 26 mass% hydroxyl groups, was dissolved in IPA to prepare a polyvinyl butyral resin solution [PVB4] with a solid content of 30%.

[0399] (Preparation of polyvinyl butyral resin solution [PVB5]) A polyvinyl butyral resin (weight average molecular weight 33,000) having vinyl alcohol units, vinyl acetate units and vinyl butyral units, and containing 77 mass% butyral ring groups and 21 mass% hydroxyl groups, was dissolved in IPA to prepare a polyvinyl butyral resin solution [PVB5] with a solid content of 30%.

[0400] (Preparation of polyvinyl butyral resin solution [PVB6]) A polyvinyl butyral resin (weight average molecular weight 33,000) having vinyl alcohol units, vinyl acetate units, and vinyl butyral units, and containing 84 mass% butyral ring groups and 14 mass% hydroxyl groups, was dissolved in IPA to prepare a polyvinyl butyral resin solution [PVB6] with a solid content of 30%.

[0401] [Production of Water-Based Flexographic Ink] (Production Example Y3-1) [Preparation of Yellow Ink [Y3-1]] Aqueous polyurethane resin [PU3] 45 parts, isoindoline compound (1-1) 15 parts, polyethylene wax (W310 manufactured by Mitsui Chemicals, Inc., particle size 9.5 μm, softening point 132° C., needle penetration hardness 0.8) 2 parts, adipic dihydrazide 0.2 parts, ammonia water (28%) 0.2 parts, water 18.8 parts, and isopropanol 18.8 parts were dispersed in an Eiger mill until the particle size measured with a grind gauge was 10 μm or less, to produce a yellow ink [Y3-1].

[0402] (Production Examples Y3-2 to Y3-28, C3-1 to C3-5, M3-1 to M3-54) [Preparation of Yellow Inks [Y3-2] to [Y3-28], Cyan Inks [C3-1] to [C3-5], and Magenta Inks [M3-1] to [M3-54]] The ink shown in Table 12 was obtained in the same manner as in Production Example Y3-1, except that in the production method of the yellow ink [Y3-1] described in Production Example Y3-1, 15 parts of the isoindoline compound (1-1) was changed to the compound shown in Table 12 and in the amount shown in Table 12.

[0403] [Table 12-1]

[0404] [Table 12-2]

[0405] (Production Example Y4-1) [Preparation of Yellow Ink [Y4-1]] Aqueous polyurethane resin [PU3] 45 parts, isoindoline compound (1-3) 15 parts, polyvinyl butyral resin solution [PVB4] 5 parts, polyethylene wax (W310 manufactured by Mitsui Chemicals, Inc., particle size 9.5 μm, softening point 132° C., needle penetration hardness 0.8) 2 parts, adipic acid dihydrazide 0.2 parts, ammonia water (28%) 0.2 parts, water 18.8 parts, and isopropanol 18.8 parts were dispersed in an Eiger mill until the particle size was 10 μm or less as measured by a grind gauge, to produce a yellow ink [Y4-1].

[0406] (Production Examples Y4-2 to Y4-5, C4-1 to C4-3, M4-1 to M4-17) [Preparation of Yellow Inks [Y4-2] to [Y4-5], Cyan Inks [C4-1] to [C4-3], and Magenta Inks [M4-1] to [M4-17]] In the preparation method of yellow ink [Y4-1] described in Production Example Y4-1, except that 15 parts of isoindoline compound (1-3) and 5 parts of polyvinyl butyral resin solution [PVB4] were changed to the compounds shown in Table 13, the amounts shown in Table 13, and the polyvinyl butyral resin shown in Table 13, the same procedure as in Production Example Y4-1 was carried out to obtain the ink described in Table 13.

[0407] [Table 13]

[0408] The pigments used in the preparation of the inks are as shown in Table 5 for the preparation of the gravure inks.

[0409] <Evaluation of printing ink set> (Examples CS-1 to CS-99, Comparative Examples CS-1 to CS-11) The inks obtained were combined as shown in Table 14 to form ink sets C1 to C110. The resulting printing ink sets were evaluated for gamut, lightfastness, and adhesion by the following methods. The results are shown in Tables 15, 16, and 17.

[0410] [Table 14-1]

[0411] [Table 14-2]

[0412] [Table 14-3]

[0413] [Initial gamut evaluation] Using the obtained printing ink set, printing was performed in the following printing conditions in the order of cyan, magenta A, magenta B, and yellow, to obtain a print having a single-color solid area (cyan, magenta A, magenta B, yellow) and a single-color solid overprint area (yellow x cyan, cyan x magenta A, yellow x magenta B, or yellow x magenta A).

[0414] (Printing conditions) Printing machine: Windmuller & Hoelscher MIRAFLEX CM Flexo plate: Photopolymer plate, KODAK FLEXCEL NXH digital flexo plate, plate thickness 1.14mm, screen ruling 150lpi Anilox roll: 900lpi 3cc / m 2 Substrate: Corona-treated polyester (PET) film (Toyobo E5100, thickness 12 μm) Speed: 300m / min Drying temperature: Intercolor dryer 100℃, tunnel dryer 100℃

[0415] The density values ​​of the monochrome solid areas (yellow, magenta A, magenta B, cyan) of the obtained prints were measured using a Gretagmacbeth D196. In addition, the monochrome solid areas and overprinted areas were measured using a Gretagmacbeth SpectroEye as a measuring instrument under the conditions of a D50 light source, a 2-degree observation field, a white back (a standard white board was used), and no filters were used. a* on the horizontal axis, b * In the two-dimensional space with the vertical axis, the monochrome solid areas (yellow, magenta A, magenta B, cyan) and monochrome solid overprint areas (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A) are printed in a total of 6 or 7 colors. * vs. b * The values ​​were plotted to determine the area. The area ratio was calculated based on the area of ​​the comparative example CS-1, which served as the standard, being taken as 100%, and the results were evaluated based on the following criteria. The results are shown in Table 15. The practical level is 3 or higher.

[0416] (Evaluation Criteria) 6: Area ratio is 115% or more 5: Area ratio is 110% or more and less than 115% 4: Area ratio is 105% or more and less than 110% 3: Area ratio is 100% or more and less than 105% 2: Area ratio is 98% or more but less than 100% 1: Area ratio is less than 98%

[0417] [Lightfastness rating 1] (UV radiation test using a fadeometer) The printed matter obtained above was irradiated with ultraviolet light for 48 hours using a fadeometer (ultraviolet carbon arc lamp type lightfastness tester), and the color was measured in the same manner as above after the test. The ultraviolet light irradiation conditions were in accordance with JIS L0842:2004 and JIS B7751:2007.

[0418] (Gamut) In the same manner as in the initial gamut evaluation method, the solid color area and the overprinted area of ​​the printed matter after the ultraviolet irradiation test were measured, and * vs. b * The values ​​were plotted to determine the area. The area after the ultraviolet irradiation test for each Example and Comparative Example was divided by the area at the initial evaluation to determine the area ratio, and the area ratio was used to evaluate the product according to the following criteria. The results are shown in Table 15. The practical level is 3 or higher.

[0419] (Evaluation Criteria) 6: Area ratio is 98% or more 5: Area ratio is 97.5% or more and less than 98% 4: Area ratio is 97% or more and less than 97.5% 3: Area ratio is 96.5% or more and less than 97% 2: Area ratio is 96% or more and less than 96.5% 1: Area ratio is less than 96%

[0420] (color difference ΔE * ab) The color difference ΔE before and after the UV irradiation test was measured from the color measurement results of the single-color solid area (yellow, magenta A, magenta B, cyan). * The ab was calculated and evaluated according to the following criteria. The results are shown in Table 15. The practical level is 3 or higher.

[0421] (Evaluation Criteria) 6:ΔE * ab is less than 1.0 5:ΔE * ab is greater than or equal to 1.0 and less than 1.5 4:ΔE * ab is 1.5 or more and less than 2.0 3:ΔE * ab is 2.0 or more and less than 3.0 2:ΔE * ab is 3.0 or more and less than 5.0 1:ΔE * ab is 5.0 or more

[0422] (Hue difference ΔH * ) From the color measurement results of the single-color solid print overlapping parts (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A), the hue difference ΔH before and after the ultraviolet irradiation test * was determined and evaluated according to the following criteria. The results are shown in Table 15. The practical level is 3 or higher. If the hue angle (H°) after the test was larger than the H° before the test, a "+" was added, and if the hue angle (H°) after the test was smaller than the H° before the test, a "-" was added.

[0423] (Evaluation Criteria) 6:ΔH * is less than 0.5 5:ΔH * is greater than or equal to 0.5 and less than 0.75 4:ΔH * is greater than or equal to 0.75 and less than 1.0 3:ΔH * is greater than or equal to 1.0 and less than 1.5 2:ΔH * is greater than or equal to 1.5 and less than 3.0 1:ΔH * is 3.0 or higher

[0424] [Lightfastness rating 2] (White LED irradiation test) The prints obtained above were subjected to a white LED irradiation test using the following test method. After the test, the color was measured in the same manner as above to evaluate the stability of the hue under white LED irradiation. (Test Method) Testing machine: Illuminated incubator FLI-2010H-LED (Tokyo Rikakikai) Light source: white LED Illuminance: 15000Lux Irradiation temperature: 10℃ Irradiation humidity: 70%RH Irradiation period: 96 hours

[0425] (Gamut) In the same manner as the initial gamut evaluation method, the solid color area and the overprinted area were measured using the printed matter after the white LED irradiation test, and * vs. b * The values ​​were plotted to determine the area. The area after the white LED irradiation test for each Example and Comparative Example was divided by the area at the initial evaluation to determine the area ratio, and the area ratio was used to evaluate the product according to the following criteria. The results are shown in Table 16. The practical level is 3 or higher.

[0426] (Evaluation Criteria) 6: Area ratio is 98% or more 5: Area ratio is 97.5% or more and less than 98% 4: Area ratio is 97% or more and less than 97.5% 3: Area ratio is 96.5% or more and less than 97% 2: Area ratio is 96% or more and less than 96.5% 1: Area ratio is less than 96%

[0427] (color difference ΔE * ab) The color difference ΔE before and after the white LED irradiation test was measured based on the color measurement results of the single-color solid area (yellow, magenta A, magenta B, cyan). * The ab was calculated and evaluated according to the following criteria. The results are shown in Table 16. The practical level is 3 or higher.

[0428] (Evaluation Criteria) 6:ΔE * ab is less than 1.0 5:ΔE * ab is greater than or equal to 1.0 and less than 1.5 4:ΔE * ab is 1.5 or more and less than 2.0 3:ΔE * ab is 2.0 or more and less than 3.0 2:ΔE * ab is 3.0 or more and less than 5.0 1:ΔE * ab is 5.0 or more

[0429] (Hue difference ΔH * ) The hue difference ΔH before and after the white LED irradiation test was measured from the color measurement results of the single-color solid print overlapping area (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A). * was determined and evaluated according to the following criteria. The results are shown in Table 16. The practical level is 3 or higher. If the hue angle (H°) after the test was larger than the H° before the test, a "+" was added, and if the hue angle (H°) after the test was smaller than the H° before the test, a "-" was added.

[0430] (Evaluation Criteria) 6:ΔH * is less than 0.5 5:ΔH * is greater than or equal to 0.5 and less than 0.75 4:ΔH* is greater than or equal to 0.75 and less than 1.0 3:ΔH * is greater than or equal to 1.0 and less than 1.5 2:ΔH * is greater than or equal to 1.5 and less than 3.0 1:ΔH * is 3.0 or higher

[0431] [Table 15-1]

[0432] [Table 15-2]

[0433] [Table 15-3]

[0434] [Table 16-1]

[0435] [Table 16-2]

[0436] [Table 16-3]

[0437] In Tables 15 and 16, Y represents yellow, C represents cyan, MA represents magenta A, and MB represents magenta B. Also, Y×C represents yellow×cyan, C×MA represents cyan×magenta A, Y×MB represents yellow×magenta B, and Y×MA represents yellow×magenta A.

[0438] From the results of Tables 15 and 16, it was confirmed that the water-based flexographic printing ink set of the present invention has high color reproducibility and good lightfastness. In particular, when a yellow ink containing isoindoline compound (4) or isoindoline compound (5) was used, the color reproducibility was higher and the lightfastness was better. In addition, when a yellow ink containing CI Pigment Yellow 180 having an optimal particle size was used, the color reproducibility was higher and the lightfastness was better. Furthermore, when a cyan ink containing CI Pigment Blue 15:3 or CI Pigment Blue 15:4 was used, the color reproducibility was higher and the light resistance was good. Furthermore, when Magenta Ink A containing CI Pigment Violet 23 or CI Pigment Violet 37 was used, the color reproducibility was higher and the lightfastness was good.

[0439] In addition, when magenta ink B containing CI Pigment Red 122 with the optimal particle size, CI Pigment Violet 19 with the optimal particle size, DPP pigment with the optimal particle size, or perylene pigment with the optimal particle size was used, the color reproducibility was higher and the lightfastness was better. In particular, in the yellow x magenta region, the printing ink set of the comparative example showed a significant change in hue to blue (smaller hue angle) in the lightfastness test using ultraviolet light irradiation, while the hue changed significantly to yellow (larger hue angle) in the lightfastness test using white LED irradiation. In other words, it is clear that the printing ink set of the comparative example shows different changes in hue over time depending on the light source, making it difficult to achieve sufficient lightfastness. In contrast, it is clear that the printing ink set of the embodiment of the present invention shows good lightfastness regardless of the light source.

[0440] [Adhesiveness] For the prints obtained as described above using ink sets C3, C20, C80 to C99, and C110, 3 hours after printing, a 12 mm wide adhesive tape (cellophane tape manufactured by Nichiban Co., Ltd.) was applied to the printed surface, and the tape was quickly peeled off, and the degree of peeling of the ink coating was judged visually. The judgment criteria were as follows. The results are shown in Table 17. The practical level is 2 or higher.

[0441] (Evaluation Criteria) 5: Less than 1% of the ink coating on the printed surface has peeled off, or there is no peeling at all. 4: The peeled area of ​​the ink film is 1% or more but less than 2% 3: The peeled area of ​​the ink film is 2% or more but less than 3% 2: The peeled area of ​​the ink film is between 3% and 5%. 1: Ink coating peeling area is 5% or more

[0442] [Table 17]

[0443] As can be seen from the results in Table 17, the printing ink set containing polyvinyl butyral resin had better adhesion. In particular, the printing ink set containing polyvinyl butyral resin with a hydroxyl group content of 25% or less had even better adhesion. The printing ink set of the comparative example did not have good adhesion even though it contained polyvinyl butyral resin.

[0444] <Production of packaging materials> (Example DP-1) [Preparation of packaging material D1] Using a flexographic printing machine and ink set D1 containing black ink (Aquariona R92F black (manufactured by Toyo Ink Co., Ltd.)), cyan ink [C3-1], magenta ink [M3-2], magenta ink [M3-17], yellow ink [Y3-1], and white ink (Aquariona R63 white (manufactured by Toyo Ink Co., Ltd.)), a 20 μm thick corona-treated stretched polypropylene film (OPP substrate) was printed in the following order: black ink, cyan ink [C3-1], magenta ink [M3-2], magenta ink [M3-17], yellow ink [Y3-1], and white ink. Each unit was dried at 100°C to obtain a printed matter having a configuration of "OPP substrate / black, cyan, magenta A, magenta B, yellow, or white printed layer". Next, a urethane-based laminating adhesive (TM320 / CAT13B manufactured by Toyo-Morton, 30% non-volatile content in ethyl acetate solution) was applied onto the printed layer of the obtained printed matter so that the coating amount after drying was 2.0 g / m2, and then dried. Next, a 50 μm-thick unstretched polyethylene (PE) film was laminated onto the adhesive layer to obtain a packaging material D1 having a structure of "OPP substrate / color overprinting layer / adhesive layer / PE substrate."

[0445] (Examples DP-2 to DP-99, Comparative Examples DP-1 to DP-2) [Preparation of Packaging Materials D2 to D101] Packaging materials D2 to D101 were obtained in the same manner as in Example DP-1, except that the ink set D1 used in Example DP-1 was changed to the ink set shown in Table 18.

[0446] [Table 18-1]

[0447] [Table 18-2]

[0448] As described above, packaging materials were made using the present and comparative water-based flexographic ink sets.

[0449] Among these packaging materials, the lamination strength of packaging materials D3, D20, and D80 to D101 was evaluated according to the following method. The results are shown in Table 19.

[0450] [Initial laminate strength evaluation] Each packaging material was cut to a width of 15 mm, and the printed layer and the adhesive layer were peeled off, after which the peel strength was measured using an Intesco 201 universal tensile tester. The evaluation criteria were as follows. The results are shown in Table 19. The practical level is 2 or higher.

[0451] (Evaluation Criteria) 5: 2.0N / 15mm or more 4: 1.5N / 15mm or more, less than 2.0N / 15mm 3: 1.0N / 15mm or more, less than 1.5N / 15mm 2: 0.5N / 15mm or more, less than 1.0N / 15mm 1: Less than 0.5N / 15mm

[0452] [Laminate strength evaluation after light resistance test 1] (UV radiation test using a fadeometer) Each packaging material was irradiated with ultraviolet light for 48 hours using a fadeometer (ultraviolet carbon arc lamp type light resistance tester), and the peel strength was measured after the test in the same manner as above. The ultraviolet light irradiation conditions were in accordance with JIS L0842:2004 and JIS B7751:2007.

[0453] [Laminate strength evaluation after light resistance test 2] (White LED irradiation test) Each packaging material was subjected to a white LED irradiation test using the following test method. After the test, the peel strength was measured in the same manner as above. (Test Method) Testing machine: Illuminated incubator FLI-2010H-LED (Tokyo Rikakikai) Light source: white LED Illuminance: 15000Lux Irradiation temperature: 10℃ Irradiation humidity: 70%RH Irradiation period: 96 hours

[0454] [Table 19]

[0455] As can be seen from the results shown in Table 19, the packaging material using the printing ink set of the embodiment of the present invention had good laminate strength even after the light fastness test. The packaging material using the printing ink set containing polyvinyl butyral resin had better laminate strength after the light fastness test. In particular, the packaging material using the printing ink set containing polyvinyl butyral resin with a hydroxyl group content of 25% or less had even better laminate strength after the light fastness test. In the packaging material using the printing ink set of the comparative example, the laminate strength after the light fastness test did not reach a practical level, and even if the packaging material contained polyvinyl butyral resin, good laminate strength was not obtained.

[0456] <3> Evaluation of flexographic ink sets (Synthesis Example 4) (Synthesis of polyurethane resin [PU4]) In a four-neck flask equipped with a reflux condenser, a dropping funnel, a gas inlet tube, a stirrer, and a thermometer, 219.6 parts of polytetramethylene ether glycol having a number average molecular weight of 2,000 and 56.6 parts of IPDI were charged, and while introducing nitrogen gas, the temperature was gradually raised to 90°C, and the reaction was carried out until the NCO% reached 4.4%. Next, 11.6 parts of diethylaminoethanol was added to the obtained reaction product, and the reaction was further carried out at 90°C for 3 hours to obtain a prepolymer. The prepolymer was transferred to a dropping tank using 115 parts of ethyl acetate. Next, 12.2 parts of IPDA, 0.002 parts of dibutylamine, 345.0 parts of IPA, and 240.0 parts of ethyl acetate were charged into the reaction tank, and the prepolymer was dripped into the reaction tank from the drip tank over 30 minutes. After the dripping was completed, the reaction was carried out at 40°C for 1 hour to obtain a polyurethane resin [PU4] with a non-volatile content of 30%, a weight average molecular weight of 51,000, and an amine value of 9.5 mgKOH / g.

[0457] (Preparation of CAP varnish) A cellulose acetate propionate resin (hereinafter referred to as CAP resin) was mixed with each solvent in the following mixing ratio and dissolved to prepare a CAP varnish. The CAP resin used was Eastman Chemical Company's product name "CAP-504-0.2". The CAP resin had an acetyl group content of 2.5% by mass, a propionyl group content of 45% by mass, a hydroxyl group content of 2.6% by mass, and a glass transition temperature of 142°C. (Mixing ratio) CAP resin: 20% nPAc: 40% IPA: 40%

[0458] (Preparation of polyvinyl butyral resin solution [PVB7]) A polyvinyl butyral resin (weight average molecular weight 33,000) having vinyl alcohol units, vinyl acetate units, and vinyl butyral units, and containing 77 mass% butyral ring groups and 21 mass% hydroxyl groups, was dissolved in a mixed solvent of ethyl acetate / IPA = 1 / 1 (mass ratio) to prepare a polyvinyl butyral resin solution [PVB7] with a solid content of 20%.

[0459] <Flexographic ink manufacturing> (Production Example Y5-1) [Preparation of Yellow Ink [Y5-1]] The following materials were stirred and mixed in advance using a high-speed mixer until a homogeneous mixture was obtained, and then the resulting mixture was dispersed using a benchtop sand mill filled with 2 mm diameter glass beads to obtain yellow ink [Y5-1]. Isoindoline compound (1-1): 13.0 parts Polyurethane resin [PU4]: 37.6 parts CAP varnish: 1.2 parts Polyvinyl butyral resin solution [PVB7]: 2.4 parts Polyethylene wax (W310, manufactured by Mitsui Chemicals): 0.5 parts ·nPAc: 13.8 copies IPA: 31.5 parts

[0460] (Production Examples Y5-2 to Y5-28, C5-1 to C5-5, M5-1 to M5-54) [Preparation of Yellow Inks [Y5-2] to [Y5-28], Cyan Inks [C5-1] to [C5-5], and Magenta Inks [M5-1] to [M5-54]] In the preparation method of yellow ink [Y5-1] described in Production Example Y5-1, except that 13.0 parts of the isoindoline compound (1-1) was changed to the compound shown in Table 20 and in the amount shown in Table 20, the same procedure as in Production Example Y5-1 was repeated to obtain the ink described in Table 20.

[0461] [Table 20-1]

[0462] [Table 20-2]

[0463] The pigments used in the preparation of the inks are as shown in Table 5 for the preparation of the gravure inks.

[0464] <Evaluation of printing ink set> (Examples ES-1 to ES-85, Comparative Examples ES-1 to ES-10) The resulting inks were combined as shown in Table 21 to form ink sets E1 to E95. The resulting printing ink sets were evaluated for gamut and lightfastness by the following methods. The results are shown in Tables 22 and 23.

[0465] [Table 21-1]

[0466] [Table 21-2]

[0467] [Initial gamut evaluation] Using the obtained printing ink set, printing was performed in the following printing conditions in the order of cyan, magenta A, magenta B, and yellow, to obtain a print having a single-color solid area (cyan, magenta A, magenta B, yellow) and a single-color solid overprint area (yellow x cyan, cyan x magenta A, yellow x magenta B, or yellow x magenta A).

[0468] (Printing conditions) Printing machine: Windmuller & Hoelscher MIRAFLEX CM Flexo plate: Photopolymer plate, KODAK FLEXCEL NXH digital flexo plate, plate thickness 1.14mm, screen ruling 150lpi Anilox roll: 900lpi 3cc / m 2 Substrate: Corona-treated oriented polypropylene (OPP) film (Toyobo Co., Ltd., Pylen P2161, thickness 40 μm) Speed: 300m / min Drying temperature: Intercolor dryer 100℃, tunnel dryer 100℃

[0469] The density values ​​of the monochrome solid areas (yellow, magenta A, magenta B, cyan) of the obtained prints were measured using a Gretagmacbeth D196. In addition, the monochrome solid areas and overprinted areas were measured using a Gretagmacbeth SpectroEye as a measuring instrument under the conditions of a D50 light source, a 2-degree observation field, a white back (a standard white board was used), and no filters were used. a * on the horizontal axis, b * In the two-dimensional space with the vertical axis, the monochrome solid areas (yellow, magenta A, magenta B, cyan) and monochrome solid overprint areas (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A) are printed in a total of 6 or 7 colors. * vs. b * The values ​​were plotted to determine the area. The area ratio was calculated based on the area of ​​the comparative example ES-1, which served as the standard, being taken as 100%, and the results were evaluated based on the area ratio according to the following criteria. The results are shown in Table 22. The practical level is 3 or higher.

[0470] (Evaluation Criteria) 6: Area ratio is 115% or more 5: Area ratio is 110% or more and less than 115% 4: Area ratio is 105% or more and less than 110% 3: Area ratio is 100% or more and less than 105% 2: Area ratio is 98% or more but less than 100% 1: Area ratio is less than 98%

[0471] [Lightfastness rating 1] (UV radiation test using a fadeometer) The printed matter obtained above was irradiated with ultraviolet light for 48 hours using a fadeometer (ultraviolet carbon arc lamp type lightfastness tester), and the color was measured in the same manner as above after the test. The ultraviolet light irradiation conditions were in accordance with JIS L0842:2004 and JIS B7751:2007.

[0472] (Gamut) In the same manner as in the initial gamut evaluation method, the solid color area and the overprinted area of ​​the printed matter after the ultraviolet irradiation test were measured, and * vs. b * The values ​​were plotted to determine the area. The area after the ultraviolet irradiation test for each Example and Comparative Example was divided by the area at the initial evaluation to determine the area ratio, and the area ratio was used to evaluate the product according to the following criteria. The results are shown in Table 22. The practical level is 3 or higher.

[0473] (Evaluation Criteria) 6: Area ratio is 98% or more 5: Area ratio is 97.5% or more and less than 98% 4: Area ratio is 97% or more and less than 97.5% 3: Area ratio is 96.5% or more and less than 97% 2: Area ratio is 96% or more and less than 96.5% 1: Area ratio is less than 96%

[0474] (color difference ΔE * ab) The color difference ΔE before and after the UV irradiation test was measured from the color measurement results of the single-color solid area (yellow, magenta A, magenta B, cyan). * The ab was calculated and evaluated according to the following criteria. The results are shown in Table 22. The practical level is 3 or higher.

[0475] (Evaluation Criteria) 6:ΔE * ab is less than 1.0 5:ΔE * ab is greater than or equal to 1.0 and less than 1.5 4:ΔE * ab is 1.5 or more and less than 2.0 3:ΔE * ab is 2.0 or more and less than 3.0 2:ΔE * ab is 3.0 or more and less than 5.0 1:ΔE * ab is 5.0 or more

[0476] (Hue difference ΔH * ) From the color measurement results of the single-color solid print overlapping parts (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A), the hue difference ΔH before and after the ultraviolet irradiation test * was determined and evaluated according to the following criteria. The results are shown in Table 22. The practical level is 3 or higher. If the hue angle (H°) after the test was larger than the H° before the test, a "+" was added, and if the hue angle (H°) after the test was smaller than the H° before the test, a "-" was added.

[0477] (Evaluation Criteria) 6:ΔH * is less than 0.5 5:ΔH * is greater than or equal to 0.5 and less than 0.75 4:ΔH * is greater than or equal to 0.75 and less than 1.0 3:ΔH * is greater than or equal to 1.0 and less than 1.5 2:ΔH * is greater than or equal to 1.5 and less than 3.0 1:ΔH * is 3.0 or higher

[0478] [Lightfastness rating 2] (White LED irradiation test) The prints obtained above were subjected to a white LED irradiation test using the following test method. After the test, the color was measured in the same manner as above to evaluate the stability of the hue under white LED irradiation. (Test Method) Testing machine: Illuminated incubator FLI-2010H-LED (Tokyo Rikakikai) Light source: white LED Illuminance: 15000Lux Irradiation temperature: 10℃ Irradiation humidity: 70%RH Irradiation period: 96 hours

[0479] (Gamut) In the same manner as the initial gamut evaluation method, the solid color area and the overprinted area were measured using the printed matter after the white LED irradiation test, and * vs. b * The values ​​were plotted to determine the area. The area after the white LED irradiation test for each Example and Comparative Example was divided by the area at the initial evaluation to determine the area ratio, and the area ratio was used to evaluate the product according to the following criteria. The results are shown in Table 23. The practical level is 3 or higher.

[0480] (Evaluation Criteria) 6: Area ratio is 98% or more 5: Area ratio is 97.5% or more and less than 98% 4: Area ratio is 97% or more and less than 97.5% 3: Area ratio is 96.5% or more and less than 97% 2: Area ratio is 96% or more and less than 96.5% 1: Area ratio is less than 96%

[0481] (color difference ΔE * ab) The color difference ΔE before and after the white LED irradiation test was measured based on the color measurement results of the single-color solid area (yellow, magenta A, magenta B, cyan). * The ab was calculated and evaluated according to the following criteria. The results are shown in Table 23. The practical level is 3 or higher.

[0482] (Evaluation Criteria) 6:ΔE * ab is less than 1.0 5:ΔE * ab is greater than or equal to 1.0 and less than 1.5 4:ΔE * ab is 1.5 or more and less than 2.0 3:ΔE * ab is 2.0 or more and less than 3.0 2:ΔE * ab is 3.0 or more and less than 5.0 1:ΔE * ab is 5.0 or more

[0483] (Hue difference ΔH * ) The hue difference ΔH before and after the white LED irradiation test was measured from the color measurement results of the single-color solid print overlapping area (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A). * was determined and evaluated according to the following criteria. The results are shown in Table 23. The practical level is 3 or higher. If the hue angle (H°) after the test was larger than the H° before the test, a "+" was added, and if the hue angle (H°) after the test was smaller than the H° before the test, a "-" was added.

[0484] (Evaluation Criteria) 6:ΔH * is less than 0.5 5:ΔH * is greater than or equal to 0.5 and less than 0.75 4:ΔH * is greater than or equal to 0.75 and less than 1.0 3:ΔH * is greater than or equal to 1.0 and less than 1.5 2:ΔH * is greater than or equal to 1.5 and less than 3.0 1:ΔH * is 3.0 or higher

[0485] [Table 22-1]

[0486] [Table 22-2]

[0487] [Table 23-1]

[0488] [Table 23-2]

[0489] In Tables 22 and 23, Y represents yellow, C represents cyan, MA represents magenta A, and MB represents magenta B. Also, Y×C represents yellow×cyan, C×MA represents cyan×magenta A, Y×MB represents yellow×magenta B, and Y×MA represents yellow×magenta A.

[0490] From the results of Tables 22 and 23, it was confirmed that the flexographic printing ink set of the present invention has high color reproducibility and good lightfastness. In particular, when a yellow ink containing isoindoline compound (4) or isoindoline compound (5) was used, the color reproducibility was higher and the lightfastness was better. In addition, when a yellow ink containing CI Pigment Yellow 180 having an optimal particle size was used, the color reproducibility was higher and the lightfastness was better. Furthermore, when a cyan ink containing CI Pigment Blue 15:3 or CI Pigment Blue 15:4 was used, the color reproducibility was higher and the light resistance was good. Furthermore, when Magenta Ink A containing CI Pigment Violet 23 or CI Pigment Violet 37 was used, the color reproducibility was higher and the lightfastness was good.

[0491] In addition, when magenta ink B containing CI Pigment Red 122 with the optimal particle size, CI Pigment Violet 19 with the optimal particle size, DPP pigment with the optimal particle size, or perylene pigment with the optimal particle size was used, the color reproducibility was higher and the lightfastness was better. In particular, in the yellow x magenta region, the printing ink set of the comparative example showed a significant change in hue to blue (smaller hue angle) in the lightfastness test using ultraviolet light irradiation, while the hue changed significantly to yellow (larger hue angle) in the lightfastness test using white LED irradiation. In other words, it is clear that the printing ink set of the comparative example shows different changes in hue over time depending on the light source, making it difficult to achieve sufficient lightfastness. In contrast, it is clear that the printing ink set of the embodiment of the present invention shows good lightfastness regardless of the light source.

[0492] <4> Evaluation of actinic radiation curable flexographic ink sets. [Production of active energy ray-curable flexographic ink] (Production Example Y6-1) [Preparation of Yellow Ink [Y6-1]] The following materials were mixed and stirred using a butterfly mixer, and dispersed using a three-roll mill so that the maximum particle size was 15 μm or less, to obtain a yellow ink [Y6-1]. Isoindoline compound (1-1): 18.0 parts EBECRYL225: 8.4 parts (5.0 parts active ingredient) (10-functional urethane acrylate oligomer) 4-Acryloylmorpholine: 15.0 parts (monofunctional monomer) EO modified trimethylolpropane triacrylate: 20.0 parts Dipentaerythritol pentaacrylate: 5.0 parts Dipentaerythritol hexaacrylate: 16.6 parts Irgacure 369: 3.0 parts (photopolymerization initiator) Chemrk DEABP: 3.0 parts (photopolymerization initiator) SB-PI718: 4.0 parts (photopolymerization initiator) AJISPER PB821: 3.0 parts (dispersant) T-Wax Compound: 4.0 parts (wax)

[0493] Details of the materials used are as follows: [Acrylate oligomer] EBECRYL225: Daicel-Allnex Corporation, 10-functional aliphatic urethane acrylate oligomer, Mw 1,200, active ingredient 60% by mass [Polymerization initiator] Irgacure 369: BASF, 2-benzyl-2-(dimethylamino)-1-(4-morpholinophenyl)-1-butanone Chemrk DEABP: 4,4'-bis(diethylamino)benzophenone, manufactured by Sort SB-PI718: 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, manufactured by Sort [Dispersant] AJISPER PB821: Ajinomoto Fine-Techno Co., Ltd., comb-shaped dispersant containing basic functional groups [wax] T wax compound: Polyethylene wax manufactured by Toshin Yushi Co., Ltd.

[0494] (Production Examples Y6-2 to Y6-28, C6-1 to C6-5, M6-1 to M6-54) [Preparation of Yellow Inks [Y6-2] to [Y6-28], Cyan Inks [C6-1] to [C6-5], and Magenta Inks [M6-1] to [M6-54]] In the preparation method of yellow ink [Y6-1] described in Production Example Y6-1, except that 18.0 parts of the isoindoline compound (1-1) was changed to the compound shown in Table 24 and in the amount shown in Table 24, the same procedure as in Production Example Y6-1 was repeated to obtain the ink described in Table 24.

[0495] [Table 24-1]

[0496] [Table 24-2]

[0497] The pigments used in the preparation of the inks are as shown in Table 5 for the preparation of the gravure inks.

[0498] <Evaluation of printing ink set> (Examples FS-1 to FS-85, Comparative Examples FS-1 to FS-10) The resulting inks were combined as shown in Table 25 to form ink sets F1 to F95. The resulting printing ink sets were evaluated for gamut and lightfastness by the following methods. The results are shown in Tables 26 and 27.

[0499] [Table 25-1]

[0500] [Table 25-2]

[0501] [Initial gamut evaluation] (Solid color part) Coated paper, 800 lpi, cell volume 3.72 cm 3 / m 2 After printing the ink using an anilox roller and a Flexiproof machine, the conveyor speed was set to 50 m / min and the ink was then turned on using an air-cooled mercury lamp (output 160 W / cm 2 The resulting print was cured under the following conditions to obtain a print for evaluation.

[0502] (Single-color solid printing overlapping area) Coated paper, 800 lpi, cell volume 3.72 cm 3 / m 2 After printing with cyan ink using an anilox roller and a Flexiproof machine, the conveyor speed was set to 50 m / min and the image was printed with an air-cooled mercury lamp (output 160 W / cm 2Thereafter, the magenta ink was printed on the cyan ink layer under the same conditions as for the cyan ink, to obtain a printed matter for evaluation in which the substrate, the cyan ink layer, and the magenta ink layer were laminated in this order. Also, printing was carried out under similar conditions using yellow ink instead of magenta ink to obtain a printed matter for evaluation in which the substrate, the cyan ink layer and the yellow ink layer were laminated in this order. Also, printing was performed under similar conditions using magenta ink instead of cyan ink and yellow ink instead of magenta ink to obtain a printed material for evaluation having the substrate, magenta ink layer, and yellow ink layer laminated in this order.

[0503] The density values ​​of the monochrome solid areas (yellow, magenta A, magenta B, cyan) of the obtained prints were measured using a Gretagmacbeth D196. In addition, the monochrome solid areas and overprinted areas were measured using a Gretagmacbeth SpectroEye as a measuring instrument under the conditions of a D50 light source, a 2-degree observation field, a white back (a standard white board was used), and no filters were used. a * on the horizontal axis, b * In the two-dimensional space with the vertical axis, the monochrome solid areas (yellow, magenta A, magenta B, cyan) and monochrome solid overprint areas (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A) are printed in a total of 6 or 7 colors. * vs. b * The values ​​were plotted to determine the area. The area ratio was calculated based on the area of ​​the comparative example FS-1, which served as the standard, being taken as 100%, and the results were evaluated based on the following criteria. The results are shown in Table 26. The practical level is 3 or higher.

[0504] (Evaluation Criteria) 6: Area ratio is 115% or more 5: Area ratio is 110% or more and less than 115% 4: Area ratio is 105% or more and less than 110% 3: Area ratio is 100% or more and less than 105% 2: Area ratio is 98% or more but less than 100% 1: Area ratio is less than 98%

[0505] [Lightfastness rating 1] (UV radiation test using a fadeometer) The printed matter obtained above was irradiated with ultraviolet light for 48 hours using a fadeometer (ultraviolet carbon arc lamp type lightfastness tester), and the color was measured in the same manner as above after the test. The ultraviolet light irradiation conditions were in accordance with JIS L0842:2004 and JIS B7751:2007.

[0506] (Gamut) In the same manner as in the initial gamut evaluation method, the solid color area and the overprinted area of ​​the printed matter after the ultraviolet irradiation test were measured, and * vs. b * The values ​​were plotted to determine the area. The area after the ultraviolet irradiation test for each Example and Comparative Example was divided by the area at the initial evaluation to determine the area ratio, and the area ratio was used to evaluate the product according to the following criteria. The results are shown in Table 26. The practical level is 3 or higher.

[0507] (Evaluation Criteria) 6: Area ratio is 98% or more 5: Area ratio is 97.5% or more and less than 98% 4: Area ratio is 97% or more and less than 97.5% 3: Area ratio is 96.5% or more and less than 97% 2: Area ratio is 96% or more and less than 96.5% 1: Area ratio is less than 96%

[0508] (color difference ΔE * ab) The color difference ΔE before and after the UV irradiation test was measured from the color measurement results of the single-color solid area (yellow, magenta A, magenta B, cyan). * The ab was calculated and evaluated according to the following criteria. The results are shown in Table 26. The practical level is 3 or higher.

[0509] (Evaluation Criteria) 6:ΔE * ab is less than 1.0 5:ΔE * ab is greater than or equal to 1.0 and less than 1.5 4:ΔE * ab is 1.5 or more and less than 2.0 3:ΔE * ab is 2.0 or more and less than 3.0 2:ΔE * ab is 3.0 or more and less than 5.0 1:ΔE * ab is 5.0 or more

[0510] (Hue difference ΔH * ) From the color measurement results of the single-color solid print overlapping parts (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A), the hue difference ΔH before and after the ultraviolet irradiation test * was determined and evaluated according to the following criteria. The results are shown in Table 26. The practical level is 3 or higher. If the hue angle (H°) after the test was larger than the H° before the test, a "+" was added, and if the hue angle (H°) after the test was smaller than the H° before the test, a "-" was added.

[0511] (Evaluation Criteria) 6:ΔH * is less than 0.5 5:ΔH * is greater than or equal to 0.5 and less than 0.75 4:ΔH * is greater than or equal to 0.75 and less than 1.0 3:ΔH * is greater than or equal to 1.0 and less than 1.5 2:ΔH * is greater than or equal to 1.5 and less than 3.0 1:ΔH * is 3.0 or higher

[0512] [Lightfastness rating 2] (White LED irradiation test) The prints obtained above were subjected to a white LED irradiation test using the following test method. After the test, the color was measured in the same manner as above to evaluate the stability of the hue under white LED irradiation. (Test Method) Testing machine: Illuminated incubator FLI-2010H-LED (Tokyo Rikakikai) Light source: white LED Illuminance: 15000Lux Irradiation temperature: 10℃ Irradiation humidity: 70%RH Irradiation period: 96 hours

[0513] (Gamut) In the same manner as the initial gamut evaluation method, the solid color area and the overprinted area were measured using the printed matter after the white LED irradiation test, and * vs. b * The values ​​were plotted to determine the area. The area after the white LED irradiation test for each Example and Comparative Example was divided by the area at the initial evaluation to determine the area ratio, and the area ratio was used to evaluate the product according to the following criteria. The results are shown in Table 27. The practical level is 3 or higher.

[0514] (Evaluation Criteria) 6: Area ratio is 98% or more 5: Area ratio is 97.5% or more and less than 98% 4: Area ratio is 97% or more and less than 97.5% 3: Area ratio is 96.5% or more and less than 97% 2: Area ratio is 96% or more and less than 96.5% 1: Area ratio is less than 96%

[0515] (color difference ΔE * ab) The color difference ΔE before and after the white LED irradiation test was measured based on the color measurement results of the single-color solid area (yellow, magenta A, magenta B, cyan). * The ab was calculated and evaluated according to the following criteria. The results are shown in Table 27. The practical level is 3 or higher.

[0516] (Evaluation Criteria) 6:ΔE * ab is less than 1.0 5:ΔE * ab is greater than or equal to 1.0 and less than 1.5 4:ΔE * ab is 1.5 or more and less than 2.0 3:ΔE * ab is 2.0 or more and less than 3.0 2:ΔE * ab is 3.0 or more and less than 5.0 1:ΔE * ab is 5.0 or more

[0517] (Hue difference ΔH * ) The hue difference ΔH before and after the white LED irradiation test was measured from the color measurement results of the single-color solid print overlapping area (yellow x cyan, cyan x magenta A, yellow x magenta B or yellow x magenta A). * was determined and evaluated according to the following criteria. The results are shown in Table 27. The practical level is 3 or higher. If the hue angle (H°) after the test was larger than the H° before the test, a "+" was added, and if the hue angle (H°) after the test was smaller than the H° before the test, a "-" was added.

[0518] (Evaluation Criteria) 6:ΔH * is less than 0.5 5:ΔH * is greater than or equal to 0.5 and less than 0.75 4:ΔH * is greater than or equal to 0.75 and less than 1.0 3:ΔH * is greater than or equal to 1.0 and less than 1.5 2:ΔH * is greater than or equal to 1.5 and less than 3.0 1:ΔH * is 3.0 or higher

[0519] [Table 26-1]

[0520] [Table 26-2]

[0521] [Table 27-1]

[0522] [Table 27-2]

[0523] In Tables 26 and 27, Y represents yellow, C represents cyan, MA represents magenta A, and MB represents magenta B. Also, Y×C represents yellow×cyan, C×MA represents cyan×magenta A, Y×MB represents yellow×magenta B, and Y×MA represents yellow×magenta A.

[0524] From the results of Tables 26 and 27, it was confirmed that the active energy ray-curable flexographic printing ink set according to one embodiment of the present invention had high color reproducibility and good lightfastness. In particular, when a yellow ink containing isoindoline compound (4) or isoindoline compound (5) was used, the color reproducibility was higher and the lightfastness was better. In addition, when a yellow ink containing CI Pigment Yellow 180 having an optimal particle size was used, the color reproducibility was higher and the lightfastness was better. Furthermore, when a cyan ink containing CI Pigment Blue 15:3 or CI Pigment Blue 15:4 was used, the color reproducibility was higher and the light resistance was good. Furthermore, when Magenta Ink A containing CI Pigment Violet 23 or CI Pigment Violet 37 was used, the color reproducibility was higher and the lightfastness was good.

[0525] In addition, when magenta ink B containing CI Pigment Red 122 with the optimal particle size, CI Pigment Violet 19 with the optimal particle size, DPP pigment with the optimal particle size, or perylene pigment with the optimal particle size was used, the color reproducibility was higher and the lightfastness was better. In particular, in the yellow x magenta region, the printing ink set of the comparative example showed a significant change in hue to blue (smaller hue angle) in the lightfastness test using ultraviolet light irradiation, while the hue changed significantly to yellow (larger hue angle) in the lightfastness test using white LED irradiation. In other words, it is clear that the printing ink set of the comparative example shows different changes in hue over time depending on the light source, making it difficult to achieve sufficient lightfastness. In contrast, it is clear that the printing ink set of the embodiment of the present invention shows good lightfastness regardless of the light source.

Claims

1. A yellow ink comprising an isoindoline compound represented by the following general formula (1) or C.I. Pigment Yellow 180 and a dispersion medium, A cyan ink comprising a phthalocyanine pigment and a dispersion medium; Magenta ink A comprising a dioxazine pigment and a dispersion medium; and A printing ink set comprising a magenta ink B containing at least one pigment selected from the group consisting of C.I. Pigment Red 122, C.I. Pigment Violet 19, a diketopyrrolopyrrole pigment represented by the following general formula (101), and a perylene pigment represented by the following general formula (201), and a dispersion medium. [Formula 1] [In general formula (1), R 1 ~R 4 R each independently represents a hydrogen atom, an alkyl group, or an alkoxy group. 5 and R 6 Each of X independently represents a hydrogen atom or an alkyl group. 1 represents -O- or -NH-; R 7 represents a hydrogen atom, an alkyl group, or an aryl group. [In general formula (101), R 151 ~R 160 each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, a thioalkyl group, a cyano group, or an aryl group. [In general formula (201), X 2 is -O- or -NR 201 - represents R 201 represents a hydrogen atom, an alkyl group, or an aryl group which may have a substituent.

2. The printing ink set according to claim 1, wherein the isoindoline compound represented by the general formula (1) includes at least one compound selected from the group consisting of the following formulas (4) and (5): [chemical 2]

3. 2. The printing ink set according to claim 1, which is used for gravure printing.

4. 2. The printing ink set according to claim 1, which is used for flexographic printing.

5. A printed matter comprising a substrate and a printed layer formed from the printing ink set according to any one of claims 1 to 4.

6. A printed matter having four types of image areas, at least yellow, cyan, and two types of magenta, on a substrate, A yellow image portion containing an isoindoline compound represented by the following general formula (1) or C.I. Pigment Yellow 180 and a dispersion medium, a cyan image portion comprising a phthalocyanine pigment and a dispersion medium; a magenta image portion A comprising a dioxazine pigment and a dispersing medium; and A printed matter having a magenta image portion B including at least one pigment selected from the group consisting of C. I. Pigment Red 122, C. I. Pigment Violet 19, a diketopyrrolopyrrole pigment represented by the following general formula (101), and a perylene pigment represented by the following general formula (201), and a dispersion medium. [Formula 1] [In general formula (1), R 1 ~R 4 R each independently represents a hydrogen atom, an alkyl group, or an alkoxy group. 5 and R 6 Each of X independently represents a hydrogen atom or an alkyl group. 1 represents -O- or -NH-; R 7 represents a hydrogen atom, an alkyl group, or an aryl group. [In general formula (101), R 151 ~R 160 each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, a thioalkyl group, a cyano group, or an aryl group. [In general formula (201), X 2 is -O- or -NR 201 - represents R 201represents a hydrogen atom, an alkyl group, or an aryl group which may have a substituent.

7. A packaging material comprising the printed matter according to claim 5.

8. A packaging material comprising the printed matter according to claim 6.

Citation Information

Patent Citations

  • Printing ink and packaging material

    JP2006070190A

  • Ink composition and packaging material

    JP2012136582A

Cited By

  • Anti-reflective film and active energy ray curable composition

    JP2026110200A

  • Anti-reflection film and active energy ray-curable composition

    JP7793748B1

  • Antireflection film and active energy ray-curable composition

    WO2026133995A1