Copper-clad laminate
The copper-clad laminate with a composite sheet and oriented boron nitride filler addresses flexibility and thermal resistance issues, offering improved adhesion and conductivity.
Patent Information
- Application Number
- JP2023052029
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional copper-clad laminates face challenges in achieving a balance between flexibility, low thermal resistance, and adhesion, particularly in the thickness direction.
A copper-clad laminate is developed using a composite sheet containing a sulfur-based crosslinking agent, a thermoplastic resin, and boron nitride filler, with boron nitride oriented at an angle of 60° to 90° relative to the main surface, and a filler content of 45% to 75% by volume, enhancing flexibility and thermal conductivity.
The laminate exhibits excellent flexibility, low heat resistance, and improved adhesion, with enhanced thermal conductivity and dielectric properties.
Smart Images

Figure 2024140725000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to copper clad laminates. [Background technology]
[0002] 2. Description of the Related Art Conventionally, laminates in which a metal base material or metal foil is bonded to an insulating layer have been used in the manufacture of circuit boards (hereinafter sometimes referred to as "printed boards") for electronic components such as semiconductor elements.
[0003] For example, Patent Document 1 discloses a metal base substrate having excellent insulation and heat dissipation properties, which is a metal base substrate having an insulating layer and a conductive layer provided in this order on a metal base material, and the insulating layer is made of a cured product of a resin composition containing an epoxy resin, a curing agent, and 50% to 85% by volume of hexagonal boron nitride particles, and uses a thermally conductive insulating sheet having a longitudinally oriented sheet in which the hexagonal boron nitride particles are oriented in the thickness direction. Patent Document 1 further discloses that it is preferable to use copper foil for the conductive layer. Patent Document 2 discloses a resin-attached metal foil that has a first insulating layer and a second insulating layer formed in this order on a metal foil, as a resin-attached metal foil that can maintain good adhesion, flexibility, heat resistance, and circuit filling properties while having low resin fluidity during molding and suppressing extrusion, in which the first insulating layer is formed of a polyimide resin layer, a polyamideimide resin layer, a liquid crystal polymer resin layer, a fluororesin layer, or a polyphenylene ether resin layer, the second insulating layer is formed of a polyolefin resin layer in a semi-cured state, and the polyolefin resin layer contains a polyolefin-based elastomer (A) and a thermosetting resin (B), and the proportion of the polyolefin-based elastomer (A) in the entire polyolefin resin layer is 50 to 95 mass %. Furthermore, in the examples of Patent Document 2, a copper foil is used as the metal foil. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6023474 [Patent Document 2] JP 2022-133347 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, with regard to conventional copper-clad laminates, such as metal base substrates using copper foil and metal foils coated with resin, there was room for improvement in terms of the balance between improving the flexibility of the copper-clad laminate and the low thermal resistance in the thickness direction of the copper-clad laminate (hereinafter sometimes simply referred to as "low thermal resistance"), and ensuring the adhesion between the insulating layer and the copper foil of the copper-clad laminate (hereinafter sometimes simply referred to as "adhesion").
[0006] Therefore, an object of the present invention is to provide a copper-clad laminate which is excellent in flexibility, low heat resistance, and adhesion. [Means for solving the problem]
[0007] The present inventors have conducted extensive research with the aim of solving the above problems. The present inventors have newly discovered that the above problems can be solved by a copper-clad laminate using a predetermined composite sheet as an insulating layer, specifically, a copper-clad laminate obtained by crosslinking a crosslinkable laminate including a composite sheet containing a sulfur-based crosslinking agent, a thermoplastic resin crosslinkable by the sulfur-based crosslinking agent, and a predetermined amount of filler, and a copper foil provided directly on at least one of the main surface and the back surface of the composite sheet, in which the filler contains boron nitride and the orientation angle of the boron nitride with respect to the main surface of the composite sheet is 60° or more and 90° or less, and have completed the present invention.
[0008] That is, the present invention aims to advantageously solve the above-mentioned problems, and [1] the present invention provides a copper-clad laminate obtained by crosslinking a crosslinkable laminate comprising a composite sheet containing a sulfur-based crosslinking agent, a thermoplastic resin crosslinkable by the sulfur-based crosslinking agent, and a filler, and a copper foil provided directly on at least one of the main surface and back surface of the composite sheet, wherein the content of the filler in the composite sheet is 45 volume % or more and 75 volume % or less, when the total of the thermoplastic resin and the filler is 100 volume %, the filler contains boron nitride, and the orientation angle of the boron nitride with respect to the main surface of the composite sheet is 60° or more and 90° or less. The above-mentioned copper-clad laminate is excellent in flexibility and low heat resistance, as well as in adhesion. In this specification, the "principal surface" of a composite sheet means the surface of the composite sheet that has the largest area, and the "reverse surface" of the composite sheet means the surface opposite to the principal surface. In this specification, the orientation angle of boron nitride with respect to the main surface of the composite sheet can be measured by the method described in the Examples. In this specification, resin includes rubber. In this specification, "excellent low heat resistance" means excellent low heat resistance under both low pressure (e.g., 0.1 MPa) and high pressure (e.g., 0.9 MPa).
[0009] [2] In the copper-clad laminate of the above [1], the boron nitride is preferably in the form of flakes. If the boron nitride is in a flake form, the flexibility and thermal conductivity of the copper clad laminate can be improved.
[0010] [3] In the copper-clad laminate of [1] or [2] above, the content of the boron nitride in the composite sheet is preferably 40% by volume or more and 65% by volume or less, when the total of the thermoplastic resin and the filler is 100% by volume. If the content of boron nitride in the composite sheet is equal to or higher than the lower limit, the low thermal resistance of the copper-clad laminate under high pressure can be improved, and the thermal conductivity in the thickness direction of the copper-clad laminate (hereinafter sometimes simply referred to as "thermal conductivity") can be improved. On the other hand, if the content of boron nitride in the composite sheet is equal to or less than the above upper limit, the flexibility, low heat resistance under low pressure, and adhesion of the copper-clad laminate can be improved.
[0011] [4] In the copper-clad laminate of any one of the above [1] to [3], the content of the sulfur-based crosslinking agent in the composite sheet is preferably 1.00 parts by mass or more and 5.00 parts by mass or less per 100 parts by mass of the thermoplastic resin. When the content of the sulfur-based crosslinking agent in the composite sheet is equal to or more than the above lower limit, the adhesion of the copper-clad laminate can be improved. On the other hand, if the content of the sulfur-based crosslinking agent in the composite sheet is equal to or less than the above upper limit, the flexibility of the copper-clad laminate and the low heat resistance under low pressure can be improved.
[0012] [5] In the copper-clad laminate according to any one of the above [1] to [4], the thermoplastic resin satisfies the following conditions (1) and (2): (1) SP value is 18.45 (MPa) 1 / 2 is less than or equal to (2) At least one selected from the group consisting of polybutene, butyl rubber, styrene butadiene rubber, isoprene rubber, and ethylene propylene rubber. It is preferable that at least one of the above conditions is satisfied. If the thermoplastic resin satisfies the above conditions, the flexibility, thermal conductivity, and low dielectric loss of the copper-clad laminate can be improved. In this specification, the SP value of a thermoplastic resin can be calculated by the method described in the Examples. Effect of the Invention
[0013] According to the present invention, it is possible to provide a copper-clad laminate which is excellent in flexibility, low heat resistance, and adhesion. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic perspective view showing an example of a copper-clad laminate of the present invention. [Diagram 2] FIG. 1 is a schematic perspective view showing an example of a composite sheet. [Diagram 3] FIG. 1 is a schematic perspective view showing an example of a composite sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will now be described in detail with reference to the embodiments thereof. The copper-clad laminate of the present invention can be used in the production of printed circuit boards for electronic components such as semiconductor elements.
[0016] (Copper-clad laminate) The copper-clad laminate of the present invention is obtained by crosslinking a crosslinkable laminate comprising a composite sheet containing a sulfur-based crosslinking agent, a thermoplastic resin crosslinkable by the sulfur-based crosslinking agent, and a filler, and a copper foil provided directly on at least one of the main surface and the back surface of the composite sheet. The content of the filler in the composite sheet is 45% by volume or more and 75% by volume or less, assuming that the total of the thermoplastic resin and the filler is 100% by volume. Furthermore, the filler contains boron nitride, and the orientation angle of the boron nitride with respect to the main surface of the composite sheet is 60° or more and 90° or less. The above-mentioned copper-clad laminate has excellent flexibility and low heat resistance, and also has excellent adhesion between the composite sheet and the copper foil. Although the reason for this is unclear, it is presumed that the flexibility of the copper-clad laminate is improved by the composite sheet containing a thermoplastic resin, that the composite sheet contains a predetermined proportion of filler and contains boron nitride oriented in a predetermined direction as a filler, and that the low heat resistance of the copper-clad laminate is improved by the composite sheet containing a sulfur-based crosslinking agent and a thermoplastic resin that can be crosslinked by the sulfur-based crosslinking agent, so that a crosslinking reaction occurs well within the composite sheet and a crosslinking reaction occurs between the copper foil and the sulfur-based crosslinking agent, resulting in improved adhesion between the composite sheet and the copper foil. In this specification, the phrase "obtained by crosslinking a crosslinkable laminate" means that the crosslinkable laminate is subjected to heat, pressure, or the like to cause the above-mentioned crosslinking reaction, etc.
[0017] Fig. 1 is a schematic perspective view showing an example of a copper-clad laminate of the present invention. The copper-clad laminate 100 shown in Fig. 1 is formed by crosslinking a crosslinkable laminate including a composite sheet 110, a copper foil 120 provided directly on a main surface 111 of the composite sheet 110, and a copper foil 120 provided directly on a back surface 112 of the composite sheet 110. The copper foils provided on both the main and back surfaces of the composite sheet may be the same or may differ from each other in at least one of composition, physical properties, thickness, and surface condition. In addition, in the copper-clad laminate shown in FIG. 1, copper foil is provided on both the main surface and the back surface of the composite sheet, but the copper-clad laminate of the present invention is not limited to this, and may be, for example, a copper-clad laminate in which the copper foil is provided directly only on the main surface of the composite sheet, or a copper-clad laminate in which the copper foil is provided directly only on the back surface of the composite sheet.
[0018] <Composite sheet> The composite sheet contains a sulfur-based crosslinking agent, a thermoplastic resin that can be crosslinked by the sulfur-based crosslinking agent (hereinafter may be referred to as a "crosslinkable thermoplastic resin"), and a filler, and may optionally further contain components other than the sulfur-based thermal crosslinking agent, the crosslinkable thermoplastic resin, and the filler (hereinafter may be referred to as "other components").
[0019] <<Sulfur-based crosslinking agent>> The sulfur-based crosslinking agent is a crosslinking agent containing sulfur, and examples thereof include powdered sulfur, oil-treated powdered sulfur, precipitated sulfur, colloidal sulfur, and dispersible sulfur; organic sulfur-containing compounds such as tetramethylthiuram disulfide and N,N-dithiobismorpholine; and the like. These may be used alone or in combination of two or more. Among these, sulfur is preferred, and powdered sulfur is more preferred, from the viewpoint of improving the adhesion of the copper-clad laminate.
[0020] The content of the sulfur-based crosslinking agent in the composite sheet is preferably 0.50 parts by mass or more, more preferably 1.00 parts by mass or more, and even more preferably 1.50 parts by mass or more, relative to 100 parts by mass of the crosslinkable thermoplastic resin, and is preferably 5.00 parts by mass or less, more preferably 3.00 parts by mass or less, and even more preferably 2.00 parts by mass or less. If the content of the sulfur-based crosslinking agent in the composite sheet is equal to or higher than the above lower limit, The adhesion can be improved. On the other hand, if the content of the sulfur-based crosslinking agent in the composite sheet is equal to or less than the upper limit, the flexibility of the composite sheet is improved, and as a result, the flexibility of the copper-clad laminate can be improved, and the low heat resistance of the copper-clad laminate under low pressure can be improved.
[0021] <<Crosslinkable thermoplastic resin>> The crosslinkable thermoplastic resin is not particularly limited as long as it can be crosslinked with a sulfur-based crosslinking agent.
[0022] Here, the crosslinkable thermoplastic resin satisfies the following conditions (1) and (2): (1) SP value is 18.45 (MPa) 1 / 2 is less than or equal to (2) At least one selected from the group consisting of polybutene, butyl rubber, styrene butadiene rubber, isoprene rubber, and ethylene propylene rubber. It is preferable to satisfy at least one of the above conditions, and it is more preferable to satisfy both conditions (1) and (2). If the crosslinkable thermoplastic resin satisfies the above conditions, the flexibility, thermal conductivity, and low dielectric loss of the composite sheet are improved, and as a result, the flexibility, thermal conductivity, and low dielectric loss of the copper-clad laminate can be improved.
[0023] The above condition (1), "SP value of cross-linkable thermoplastic resin", is 18.25 (MPa) 1 / 2 It is preferable that the value is less than 18.04 (MPa). 1 / 2 More preferably, it is 12.30 (MPa) or less. 1 / 2 It is preferable that the value is equal to or higher than 16.40 (MPa).1 / 2 More preferably, it is equal to or greater than this. When the SP value of the crosslinkable thermoplastic resin is equal to or less than the upper limit, the flexibility, thermal conductivity, and low dielectric loss of the composite sheet are further improved, and as a result, the flexibility, thermal conductivity, and low dielectric loss of the copper-clad laminate can be further improved. On the other hand, when the SP value of the crosslinkable thermoplastic resin is equal to or greater than the above lower limit, sufficient strength of the composite sheet can be ensured. When the composite sheet contains a plurality of types of crosslinkable thermoplastic resins, the SP values of all the resins contained must satisfy the respective conditions.
[0024] As the crosslinkable thermoplastic resin listed in the above condition (2), specifically, the following can be used. As the polybutene, a homopolymer of isobutene, a copolymer of isobutene and n-butene, etc. can be used. The butyl rubber may be a copolymer of isobutylene and isoprene. As the styrene-butadiene rubber, a copolymer of styrene and butadiene can be used. As the isoprene rubber, a homopolymer of isoprene can be used. As the ethylene propylene rubber, a copolymer of ethylene and propylene can be used. The polymer may have any molecular weight as long as it does not impede the object of the present invention. The polymer may be unsubstituted or may have a substituent. Furthermore, when the polymer is a copolymer, the ratio of the polymers may be selected as long as it does not impede the object of the present invention. These polymers may be used alone or in combination of two or more.
[0025] Furthermore, as the crosslinkable thermoplastic resin, either a solid crosslinkable thermoplastic resin or a liquid crosslinkable thermoplastic resin can be used. Such a composite sheet has better strength and flexibility. When a solid crosslinkable thermoplastic resin and a liquid crosslinkable thermoplastic resin are used in combination as the crosslinkable thermoplastic resin, the mass ratio between them can be adjusted within a range in which the desired effect of the present invention can be obtained.
[0026] As the liquid crosslinkable thermoplastic resin, a crosslinkable thermoplastic resin that is liquid at normal temperature and normal pressure can be used. In this specification, "normal temperature" refers to 23°C, and "normal pressure" refers to 1 atm (absolute pressure). On the other hand, as the solid crosslinkable thermoplastic resin, a crosslinkable thermoplastic resin that is solid at room temperature and normal pressure can be used.
[0027] The content of the crosslinkable thermoplastic resin in the composite sheet must be 25% by volume or more, preferably 30% by volume or more, and more preferably 35% by volume or more, when the total of the crosslinkable thermoplastic resin and the filler is 100% by volume, and must be 55% by volume or less, preferably 50% by volume or less, and more preferably 45% by volume or less. When the content of the crosslinkable thermoplastic resin in the composite sheet is equal to or higher than the above lower limit, the flexibility of the composite sheet is improved, and as a result, the flexibility of the copper-clad laminate can be improved, and the low heat resistance and adhesion of the copper-clad laminate under low pressure can be improved. On the other hand, if the content of the crosslinkable thermoplastic resin in the composite sheet is equal to or less than the above upper limit, it becomes possible to relatively increase the content of the filler, thereby improving the low thermal resistance and thermal conductivity of the copper-clad laminate under high pressure.
[0028] <<Filler>> The filler includes boron nitride, and may optionally further include an organic filler and an inorganic filler other than boron nitride.
[0029] Here, the filler content in the composite sheet must be 45 volume % or more, preferably 50 volume % or more, and more preferably 55 volume % or more, when the total of the crosslinkable thermoplastic resin and the filler is 100 volume %, and must be 75 volume % or less, preferably 70 volume % or less, and more preferably 65 volume % or less. When the content of the filler in the composite sheet is equal to or higher than the lower limit, the thermal conductivity of the composite sheet is improved, and as a result, the thermal conductivity of the copper-clad laminate is improved, and the low thermal resistance of the copper-clad laminate under high pressure can be improved. On the other hand, if the filler content in the composite sheet is equal to or less than the above upper limit, it becomes possible to relatively increase the crosslinkable thermoplastic resin content, thereby improving the flexibility, low heat resistance under low pressure, and adhesion of the copper-clad laminate.
[0030] [Boron nitride] The boron nitride is not particularly limited, and for example, scaly (plate-like) boron nitride and spherical boron nitride can be used. These may be used alone or in combination of two or more. Among these, it is preferable to use scaly boron nitride, from the viewpoint of improving the thermal conductivity and flexibility (particularly in terms of bending strength) of the composite sheet, improving the thermal conductivity and flexibility of the copper-clad laminate, and further improving the low dielectric property described below.
[0031] Here, boron nitride can be classified according to its crystal structure into, for example, hexagonal boron nitride (h-BN), cubic boron nitride (c-BN), wurtzite boron nitride (w-BN), rhombohedral boron nitride (r-BN), and turbostratic boron nitride (t-BN). As boron nitride, these may be used alone or in combination of two or more. Among these, hexagonal boron nitride (h-BN) is preferred because it improves the thermal conductivity and flexibility of the composite sheet and can improve the thermal conductivity and flexibility of the copper-clad laminate. Note that hexagonal boron nitride is usually a scaly (plate-like) particle.
[0032] The volume average particle size of the boron nitride is preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, even more preferably 25 μm or more, and is preferably 70 μm or less, more preferably 50 μm or less, even more preferably 40 μm or less. When the volume average particle size of the boron nitride is equal to or greater than the lower limit, it is possible to reduce the contact resistance between the boron nitride particles in the composite sheet, thereby improving the thermal conductivity of the copper-clad laminate. On the other hand, when the volume average particle size of boron nitride is equal to or less than the above upper limit, it becomes possible to appropriately fill the composite sheet with boron nitride, thereby improving the thermal conductivity of the copper-clad laminate. In this specification, the term "volume average particle size" refers to a particle size at which the cumulative volume calculated from the small diameter side is 50% in a particle size distribution (volume basis) that can be measured in accordance with JIS Z8825 and is measured by a laser diffraction method.
[0033] The content of boron nitride in the composite sheet is preferably 40 volume% or more, more preferably 45 volume% or more, and even more preferably 50 volume% or more, and is preferably 65 volume% or less, more preferably 60 volume% or less, and even more preferably 55 volume% or less, when the total of the crosslinkable thermoplastic resin and the filler is 100 volume%. If the content of boron nitride in the composite sheet is equal to or higher than the lower limit, the low thermal resistance of the copper-clad laminate under high pressure can be improved, and the thermal conductivity of the composite sheet can be improved, which in turn improves the thermal conductivity of the copper-clad laminate. On the other hand, if the content of boron nitride in the composite sheet is equal to or less than the upper limit, the flexibility of the composite sheet is improved, and as a result, the flexibility of the copper-clad laminate can be improved, and the low heat resistance and adhesion of the copper-clad laminate under low pressure can be improved.
[0034] [Organic filler] The organic filler that may be optionally contained in the filler may have the function of reducing the dielectric constant and dielectric loss of the composite sheet. If the filler contains an organic filler, i.e., if the composite sheet contains an organic filler, the low dielectric property and low dielectric loss property of the composite sheet are improved, and as a result, the low dielectric property and low dielectric loss property of the copper clad laminate can be improved.
[0035] Here, the organic filler is not particularly limited, but examples thereof include fluororesin fillers such as polytetrafluoroethylene (PTFE), tetrafluoroethylene / ethylene copolymer (ETFE), tetrafluoroethylene / perfluoroalkylvinylether copolymer (PFA), tetrafluoroethylene / hexafluoropropylene copolymer (FEP), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), and polyvinyl fluoride (PVF); and hydrocarbon resin fillers such as cycloolefin polymer (COP) and cycloolefin copolymer (COC). As the organic filler, these may be used alone or in combination of two or more. Among these, fluororesin fillers are preferred, and PTFE fillers are more preferred, because the low dielectric properties and low dielectric loss properties of the composite sheet are further improved, and the low dielectric properties and low dielectric loss properties of the copper-clad laminate can be further improved.
[0036] The organic filler may be fibrillated through a pre-sheet forming step or the like in the manufacturing method of the composite sheet described below. That is, the organic filler in the composite sheet may be present in a fibrillated state.
[0037] When the composite sheet contains an organic filler, the content of the organic filler in the composite sheet is preferably 5% by volume or more and 10% by volume or less, where the total of the crosslinkable thermoplastic resin and the filler is 100% by volume. When the content of the organic filler in the composite sheet is equal to or higher than the lower limit, the low dielectric property and low dielectric loss property of the composite sheet are further improved, and as a result, the low dielectric property and low dielectric loss property of the copper-clad laminate can be further improved. On the other hand, if the content of the organic filler in the composite sheet is equal to or less than the above upper limit, it becomes possible to relatively increase the content of boron nitride, thereby improving the low thermal resistance and thermal conductivity of the copper-clad laminate under high pressure.
[0038] [Inorganic fillers other than boron nitride] The inorganic filler other than boron nitride is not particularly limited as long as it does not impair the object of the present invention, and examples thereof include alumina, aluminum nitride, etc. These may be used alone or in combination of two or more.
[0039] The content of inorganic filler other than boron nitride in the composite sheet is preferably 1 vol% or less, more preferably 0.5 vol% or less, even more preferably 0.1 vol% or less, and particularly preferably 0 vol% when the total of the crosslinkable thermoplastic resin and the filler is 100 vol%. That is, it is preferable that the composite sheet does not contain inorganic filler other than boron nitride.
[0040] <<Other ingredients>> Other components that may be contained in the composite sheet are not particularly limited, and examples thereof include non-sulfur-based crosslinking agents, reaction initiators, crosslinking accelerators and crosslinking accelerator assistants, antiaging agents, etc. These may be used alone or in combination of two or more in any ratio.
[0041] The non-sulfur crosslinking agent is not particularly limited, and examples thereof include isocyanurates such as triallyl isocyanurate (for example, TAIC (registered trademark) manufactured by Mitsubishi Chemical Corporation); cyanurates such as triallyl cyanurate; maleimides such as N,N'-m-phenylenedimaleimide; allyl esters of polyvalent acids such as diallyl phthalate, diallyl isophthalate, diallyl maleate, diallyl fumarate, diallyl sebacate, and triallyl phosphate; diethylene glycol bisallyl carbonate; allyl ethers such as ethylene glycol diallyl ether, triallyl ether of trimethylolpropane, and partial allyl ether of pentaerythritol; allyl-modified resins such as allylated novolac and allylated resol resin; trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, and other trifunctional to pentafunctional methacrylate and acrylate compounds; and the like. These may be used alone or in combination of two or more in any ratio.
[0042] The reaction initiator is not particularly limited, and examples thereof include organic peroxides that function as radical reaction initiators, such as dibenzoyl peroxide (e.g., Niper E manufactured by Nippon Oil & Fats Co., Ltd.), t-butyl peroxyacetate, 2,2-di-(t-butylperoxy)butane, t-butyl peroxybenzoate, t-butylcumyl peroxide, dicumyl peroxide, di-t-hexyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (e.g., Perhexa (registered trademark) 25B manufactured by Nippon Oil & Fats Co., Ltd.), di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexene-3, t-butyl hydroperoxide, t-butyl peroxyisobutyrate, lauroyl peroxide, dipropionyl peroxide, and p-menthane hydroperoxide. These may be used alone or in combination of two or more in any ratio.
[0043] The crosslinking accelerator and the crosslinking accelerator assistant are not particularly limited, and examples thereof include a sulfur-containing crosslinking accelerator containing a sulfur atom in its chemical structure (hereinafter, may be referred to as a "sulfur-containing crosslinking accelerator"), zinc oxide, stearic acid, and the like. Examples of the sulfur-containing crosslinking accelerator include thiuram-based crosslinking accelerators, thiazole-based crosslinking accelerators, sulfenamide-based crosslinking accelerators, and dithiocarbamate-based crosslinking accelerators.
[0044] Examples of thiuram crosslinking accelerators include tetramethylthiuram monosulfide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, and dipentamethylenethiuram tetrasulfide. Examples of the thiazole-based crosslinking accelerator include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, zinc 2-mercaptobenzothiazole, (dinitrophenyl)mercaptobenzothiazole, and (N,N-diethyldithiocarbamoyl)benzothiazole. Examples of the sulfenamide crosslinking accelerator include N-ethyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazolyl sulfenamide, N-cyclohexyl-2-benzothiazole sulfenamide (e.g., Noccela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), N,N-diisopropyl-2-benzothiazole sulfenamide, and N,N-dicyclohexyl-2-benzothiazole sulfenamide. Examples of the dithiocarbamate crosslinking accelerator include lead dimethyldithiocarbamate, lead diamyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diamyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, zinc dibenzyldithiocarbamate, zinc pentamethylenedithiocarbamate, zinc ethylphenyldithiocarbamate, sodium dimethyldithiocarbamate, sodium diethyldithiocarbamate, and di Examples of the dimethyldithiocarbamate include sodium butyldithiocarbamate, selenium dimethyldithiocarbamate, selenium diethyldithiocarbamate, tellurium diethyldithiocarbamate, cadmium diethyldithiocarbamate, copper dimethyldithiocarbamate, iron dimethyldithiocarbamate, bismuth dimethyldithiocarbamate, dimethylammonium dimethyldithiocarbamate, piperidine pentamethylenedithiocarbamate, and pipecoline methylpentamethylenedithiocarbamate. The above-mentioned sulfur-containing crosslinking accelerator may be used alone or in any combination of two or more kinds at any ratio. As the sulfur-containing crosslinking accelerator, a sulfenamide crosslinking accelerator is preferable, and N-cyclohexyl-2-benzothiazole sulfenamide is more preferable.
[0045] The antioxidant is not particularly limited, and examples thereof include amine-based antioxidants such as phenyl-1-naphthylamine, alkylated diphenylamine, octylated diphenylamine, 4,4-bis(α,α-dimethylbenzyl)diphenylamine, p-(p-toluenesulfonylamide)diphenylamine, N,N-di-2-naphthyl-p-phenylenediamine, N,N-diphenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (e.g., Nocrac 6C manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), and N-(3-methacryloyloxy-2-hydroxypropyl)-N'-phenyl-p-phenylenediamine; 2,2,4-trimethyl-1,2-dihydroquinoline, 6-ethoxy-1,2-dihydroquinoline, amine ketone-based antioxidants such as b-2,2,4-trimethylquinoline; phenol-based antioxidants such as 2,6-di-tert-butyl-4-methylphenol, 2,6-di-tert-butyl-4-ethylphenol, 2,2-methylenebis(4-ethyl-6-tert-butylphenol), 2,2-methylenebis(4-methyl-6-tert-butylphenol), 4,4-butylidenebis(3-methyl-6-tert-butylphenol), 4,4-thiobis(3-methyl-6-tert-butylphenol), 2,5-di-tert-butylhydroquinone, and 2,5-di-tert-amylhydroquinone; and benzimidazole-based antioxidants such as 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole, and metal salts of 2-mercaptomethylbenzimidazole. The above-mentioned antioxidants may be used alone or in any combination of two or more in any ratio. As the antioxidant, an amine-based antioxidant is preferred, and N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine is more preferred.
[0046] <<Composite sheet composition>> The composite sheet is not particularly limited, but preferably has a structure in which a plurality of strips are directly joined in parallel within the main surface of the composite sheet, or a structure in which a plurality of strips are indirectly joined in parallel within the main surface of the composite sheet. When the composite sheet has a structure in which a plurality of strips are indirectly joined in parallel within the main surface of the composite sheet, the composite sheet may further include an adhesive layer located between adjacent strips. In the composite sheet as described above, the major axis of the boron nitride can be easily oriented in the thickness direction of the composite sheet, improving the thermal conductivity of the composite sheet, and as a result, improving the thermal conductivity of the copper-clad laminate.
[0047] Hereinafter, an example of the configuration of the composite sheet will be described with reference to Figs. 2 and 3, but the composite sheet provided in the copper-clad laminate of the present invention is not limited to this.
[0048] The composite sheet 110 shown in Fig. 2 has a main surface 111 and a back surface 112 opposite to the main surface 111, and has a structure in which a plurality of strips 113 are directly joined in parallel within the main surface of the composite sheet 110. More specifically, in the composite sheet 110 shown in Fig. 1, within the main surface of the composite sheet 110, each strip 113 is joined (in the X direction in Fig. 2) to an adjacent strip 113 so as to share a side extending in the longitudinal direction (the Y direction in Fig. 2). Here, the X direction in Fig. 2 corresponds to the width direction of the strip 113, the Y direction corresponds to the longitudinal direction of the strip 113, and the Z direction corresponds to the thickness direction of the composite sheet 110.
[0049] The composite sheet 110 shown in FIG. 3 has a main surface 111 and a back surface 112 opposite to the main surface 111, and has a structure in which strips 113 and adhesive layers 114 located between adjacent strips 113 are joined in parallel within the main surface of the composite sheet 110. That is, the composite sheet 110 shown in FIG. 3 has a structure in which a plurality of strips 113 are indirectly joined in parallel within the main surface of the composite sheet 110. More specifically, in the composite sheet 110 shown in FIG. 3, the strips 113 and the adhesive layer 114 are joined (in the X direction in FIG. 3) so as to share a side extending in the longitudinal direction (Y direction in FIG. 3) within the main surface of the composite sheet 110. Here, the X direction in FIG. 3 corresponds to the width direction of the strips 113 and the adhesive layer 114, the Y direction corresponds to the longitudinal direction of the strips 113 and the adhesive layer 114, and the Z direction corresponds to the thickness direction of the composite sheet 110. Although FIG. 3 shows a case where the widths of strip 113 and adhesive layer 114 (the lengths of strip 111 and adhesive layer 114 in the X direction) are approximately equal, the widths of strip 113 and adhesive layer 114 may be different.
[0050] Composite sheet 110 may further include layers other than strip 113 and adhesive layer 114 (hereinafter, these layers may be referred to as "optional layers"). However, from the viewpoint of productivity of the composite sheet, it is preferable that the composite sheet is made of only the strips, or of only the strips and adhesive layer. And, from the viewpoint of thermal conductivity of the copper-clad laminate, it is more preferable that the composite sheet is made of only the strips.
[0051] [Strip] The composite sheet may comprise a strip that includes a sulfur-based crosslinking agent, a crosslinkable thermoplastic resin, and a predetermined proportion of a filler, and may optionally further include other ingredients. Here, the sulfur-based crosslinking agent, crosslinkable thermoplastic resin, filler, and any other optional components contained in the strip may be the sulfur-based crosslinking agent, crosslinkable thermoplastic resin, filler, and any other optional components described above in the sections <<Sulfur-based crosslinking agent>>, <<Crosslinkable thermoplastic resin>>, <<Filler>>, and <<Other components>>, in the ratios described above.
[0052] The width of the strip is preferably 1 mm or more, more preferably 1.2 mm or more, and even more preferably 1.5 mm or more, and is preferably 3 mm or less, more preferably 2.8 mm or less, and even more preferably 2.5 mm or less. The width of the strip may depend on the thickness of the pre-sheet in the manufacturing method described below. Therefore, in a composite sheet having a strip width equal to or greater than the lower limit, the number of layers, folds, or windings of the pre-sheet is reduced. As a result, the laminate formation speed described below is improved in such a composite sheet, and productivity is improved. On the other hand, in a composite sheet in which the width of the strips is equal to or less than the above upper limit, the boron nitride is well oriented in the thickness direction in the composite sheet, and therefore the thermal conductivity is improved.
[0053] [Adhesive layer] The adhesive layer that the composite sheet may have is not particularly limited as long as it can bond the strips together. The adhesive layer can be formed using a layered adhesive material such as a commercially available adhesive tape or a film formed by applying an adhesive. A resin sheet that melts at high temperatures (for example, about 100°C) can also be used as the layered adhesive material.
[0054] The width of the adhesive layer is preferably 1 μm or more, more preferably 5 μm or more, and is preferably 30 μm or less, more preferably 20 μm or less, and further preferably 15 μm or less. If the width of the adhesive layer is within the above range, the adhesive strength between the strips can be effectively improved.
[0055] When the composite sheet has an adhesive layer, the ratio of the width of the strip to the width of the adhesive layer (width of strip / width of adhesive layer) is preferably 60 or more, more preferably 80 or more, and even more preferably 90 or more. If the ratio of the width of the strip to the width of the adhesive layer is equal to or greater than the above lower limit, the proportion of the strip in the composite sheet is increased, effectively improving the thermal conductivity of the composite sheet, and as a result, effectively improving the thermal conductivity of the copper-clad laminate. On the other hand, the ratio of the width of the strip to the width of the adhesive layer is, for example, 500 or less, or may be 300 or less, or may be 100 or less.
[0056] <<Properties of the composite sheet>> The orientation angle of the boron nitride in the composite sheet must be 60° or more and 90° or less with respect to the main surface of the composite sheet. The orientation angle of boron nitride in the composite sheet is preferably 70° or more, more preferably 75° or more, and even more preferably 80° or more. If the orientation angle of boron nitride is equal to or more than the lower limit, the thermal conductivity of the composite sheet is improved, and as a result, the thermal conductivity of the copper-clad laminate can be improved.
[0057] The thickness of the composite sheet is preferably 0.05 mm or more, more preferably 0.10 mm or more, and is preferably 0.50 mm or less, more preferably 0.40 mm or less, and even more preferably 0.35 mm or less. When the thickness of the composite sheet is equal to or greater than the above lower limit, the strength of the composite sheet can be improved. On the other hand, when the thickness of the composite sheet is equal to or less than the above upper limit, the flexibility of the composite sheet is improved, and as a result, the flexibility of the copper-clad laminate can be improved.
[0058] The thermal conductivity of the composite sheet in the thickness direction is preferably 15 W / m·K or more, more preferably 20 W / m·K or more, and even more preferably 25 W / m·K or more. When the thermal conductivity in the thickness direction of the composite sheet is equal to or higher than the above lower limit, the thermal conductivity of the copper-clad laminate can be improved. On the other hand, the thermal conductivity of the composite sheet in the thickness direction is, for example, 100 W / m·K or less, may be 50 W / m·K or less, or may be 30 W / m·K or less. In this specification, the thermal conductivity in the thickness direction of the composite sheet can be measured by the method described in the Examples. The thermal conductivity of the composite sheet in the thickness direction can be adjusted by the types and proportions of materials and components (sulfur-based crosslinking agents, crosslinkable thermoplastic resins, fillers, etc.) contained in the composite sheet, as well as the manufacturing method and manufacturing conditions of the composite sheet.
[0059] The composite sheet preferably has a dielectric constant of less than 5.0 F / m, more preferably less than 4.3 F / m, and even more preferably less than 4.0 F / m. If the dielectric constant of the composite sheet is less than the above upper limit, the low dielectric properties of the copper-clad laminate can be improved. On the other hand, the dielectric constant of the composite sheet is, for example, 0.5 F / m or more, may be 1.0 F / m or more, 2.0 F / m or more, or may be 3.0 F / m or more. In this specification, the dielectric constant of the composite sheet can be measured by the method described in the Examples. The dielectric constant of the composite sheet can be adjusted by the types and proportions of materials and components (sulfur-based crosslinking agent, crosslinkable thermoplastic resin, filler, etc.) contained in the composite sheet, as well as the manufacturing method and manufacturing conditions for the composite sheet.
[0060] The composite sheet has a dielectric loss of 5.5×10 -4 Preferably, it is less than 5.0×10 -4 More preferably, it is less than 4.5×10 -4 It is even more preferable that it is less than 1000 .mu.m. If the dielectric loss of the composite sheet is less than the above upper limit, the low dielectric loss properties of the copper-clad laminate can be improved. On the other hand, the dielectric loss of the composite sheet is, for example, 1.0×10 -4 That is 2.0 x 10 -4 More than 3.5×10 is fine. -4 More than that is fine. In this specification, the dielectric loss of the composite sheet can be measured by the method described in the Examples. The dielectric loss of the composite sheet can be adjusted by the types and proportions of the materials and components (sulfur-based crosslinking agent, crosslinkable thermoplastic resin, filler, etc.) contained in the composite sheet, as well as the manufacturing method and manufacturing conditions of the composite sheet.
[0061] <<Manufacturing method of composite sheet>> The composite sheet is not particularly limited, and can be produced by a method including, for example, (A) a pre-sheet forming step of roll-forming a composition containing a sulfur-based crosslinking agent, a crosslinkable thermoplastic resin, and a filler into a sheet shape to obtain a pre-sheet; (B) a laminate forming step of stacking a plurality of pre-sheets in the thickness direction or folding or rolling the pre-sheet to obtain a laminate; and (C) a slicing step of slicing the laminate at an angle of 45° or less with respect to the stacking direction to obtain a composite sheet.
[0062] The method for producing the composite sheet may optionally include further steps other than the above steps (A) to (C).
[0063] [(A) Pre-sheet molding process] In the pre-sheet molding step, a composition containing a sulfur-based crosslinking agent, a crosslinkable thermoplastic resin, and a filler is roll-molded into a sheet to obtain a pre-sheet.
[0064] -Composition- The composition includes a sulfur-based crosslinking agent, a crosslinkable thermoplastic resin, and a filler. The composition may further include other components as desired. As the sulfur-based crosslinking agent, crosslinkable thermoplastic resin, filler, and other optional components included in the composition, the sulfur-based crosslinking agent, crosslinkable thermoplastic resin, filler, and other optional components described above in the sections <<Sulfur-based crosslinking agent>>, <<Crosslinkable thermoplastic resin>>, <<Filler>>, and <<Other components>> can be used in the ratios described above.
[0065] -Preparation of Composition- The composition is not particularly limited, and can be prepared by mixing the above-mentioned components. The mixing of the above-mentioned components is not particularly limited, and can be performed using a known mixing device such as a kneader, a mixer such as a Henschel mixer, a Hobart mixer, or a high-speed mixer, a twin-screw kneader, or a roll.
[0066] The mixing may be carried out in the presence of a solvent such as ethyl acetate. The crosslinkable thermoplastic resin may be dissolved or dispersed in advance in a solvent to form a resin solution, which may then be mixed with the sulfur-based crosslinking agent, the filler, and any other components that may be added.
[0067] The mixing time is, for example, from 5 minutes to 60 minutes.
[0068] The mixing temperature is, for example, 5°C or higher and 150°C or lower.
[0069] -Molding of the composition- The prepared composition may be optionally defoamed and crushed, and then rolled into a sheet. The sheet-like product obtained by roll-molding the composition in this manner may be used as a pre-sheet. When a solvent is used during mixing, it is preferable to remove the solvent before forming into a sheet. For example, by performing degassing using vacuum degassing, the solvent can be removed at the same time as degassing.
[0070] Here, in the roll molding, it is preferable to pass the composition between a first roll and a second roll having a faster peripheral speed than the first roll. By such roll molding, the composition can be molded by applying a high shear stress, and as a result, the filler (particularly boron nitride) in the pre-sheet is well oriented, and the composite sheet obtained by using the same has excellent thermal conductivity. In addition, by such roll molding, it is possible to increase the content ratio of the filler (particularly boron nitride) in the composite sheet, and as a result, a composite sheet having high thermal conductivity can be obtained.
[0071] The peripheral speed ratio of the second roll to the first roll ("peripheral speed of the second roll" / "peripheral speed of the first roll") is preferably 1.03 / 1 or more, more preferably 1.05 / 1 or more, and even more preferably 1.1 / 1 or more, and is preferably 2 / 1 or less, more preferably 1.3 / 1 or less, and even more preferably 1.2 / 1 or less. When the peripheral speed ratio of the second roll to the first roll is equal to or higher than the above lower limit, the composition can be molded by applying a higher shear stress, thereby improving the thermal conductivity of the composite sheet. On the other hand, if the peripheral speed ratio of the second roll to the first roll is equal to or less than the upper limit, the compressibility of the composite sheet can be improved. Also, if the peripheral speed ratio of the second roll to the first roll is equal to or less than the upper limit, the occurrence of wrinkles on the surface of the pre-sheet can be suppressed. In other words, the occurrence of defective products of the pre-sheet can be suppressed, and the productivity of the composite sheet obtained by using the pre-sheet can be improved. The peripheral speed ratio can be adjusted by changing the diameter and / or rotation speed of the roll.
[0072] The difference in peripheral speed between the first roll and the second roll ("peripheral speed of the second roll" - "peripheral speed of the first roll") is preferably 0.06 m / min or more, more preferably 0.1 m / min or more, and even more preferably 0.2 m / min or more, and is preferably 1 m / min or less, more preferably 0.7 m / min or less, and even more preferably 0.5 m / min or less. When the peripheral speed difference between the first roll and the second roll is equal to or greater than the above lower limit, the composition can be molded by applying a higher shear stress, thereby improving the thermal conductivity of the composite sheet. On the other hand, if the peripheral speed difference between the first roll and the second roll is equal to or less than the upper limit, the compressibility of the composite sheet can be improved. Also, if the peripheral speed ratio of the second roll to the first roll is equal to or less than the upper limit, the occurrence of wrinkles on the surface of the pre-sheet can be suppressed. In other words, the occurrence of defective products in the pre-sheet can be suppressed, and the productivity of the composite sheet obtained by using the pre-sheet can be improved. The peripheral speed ratio can be adjusted by changing the diameter and / or rotation speed of the roll.
[0073] The distance between the first roll and the second roll is preferably 1 mm or more, more preferably 1.2 mm or more, and even more preferably 1.5 mm or more, and is preferably 3 mm or less, more preferably 2.8 mm or less, and even more preferably 2.5 mm or less.
[0074] [(B) Laminate formation process] In the laminate formation process, a plurality of pre-sheets obtained in the pre-sheet molding process are laminated in the thickness direction, or the pre-sheets are folded or rolled to obtain a laminate in which a plurality of pre-sheets containing a sulfur-based cross-linking agent, a cross-linkable thermoplastic resin, and a filler are formed in the thickness direction. In addition, when obtaining a laminate, a layered adhesive material may be disposed on the surface of the pre-sheet to form a laminate having a structure in which the adhesive material is interposed between the pre-sheets. Examples of layered adhesive materials that can be used in the laminate formation step include commercially available adhesive tapes, films formed by applying adhesives, and resin sheets that melt at high temperatures (e.g., about 100°C).
[0075] Here, the formation of a laminate by folding a pre-sheet is not particularly limited, and can be performed by folding the pre-sheet at a fixed width using a folding machine. The formation of a laminate by winding a pre-sheet is not particularly limited, and can be performed by winding the pre-sheet around an axis parallel to the short side direction or long side direction of the pre-sheet. The formation of a laminate by stacking pre-sheets is not particularly limited, and can be performed using a stacking device. For example, if a sheet stacking device (manufactured by Nikkiso Co., Ltd., product name "Hi-Stacker") is used, it is possible to suppress the intrusion of air between the layers, and therefore a good laminate can be efficiently obtained.
[0076] In the laminate formation step, the obtained laminate may be pressurized in the lamination direction or from all directions while being heated at a temperature at which the sulfur-based crosslinking agent and the crosslinkable thermoplastic resin do not undergo a crosslinking reaction. Here, in the laminate formation step, pressing the laminate in the lamination direction or pressing from all directions is called secondary pressurization. By applying secondary pressurization to the laminate, it is possible to promote fusion between the laminated pre-sheets. Pressurization from all directions can be performed, for example, using an autoclave. Hereinafter, the laminate before pressurization may be referred to as a "first laminate," and the laminate after pressurization (pressurized laminate) may be referred to as a "second laminate."
[0077] Here, the pressure when the first laminate is pressed in the stacking direction or when pressed from all directions can be 0.05 MPa or more and 0.90 MPa or less. The heating temperature of the first laminate is not particularly limited, but is preferably 50° C. or more and 150° C. or less. The heating time of the first laminate can be, for example, 10 seconds or more and 30 minutes or less.
[0078] In addition, it is presumed that in a laminate obtained by stacking, folding or rolling the pre-sheet, the boron nitride is oriented in a direction approximately perpendicular to the stacking direction.
[0079] (C) Slicing step In the slicing step, the laminate is sliced at an angle of 45° or less with respect to the lamination direction to obtain a composite sheet made of slices of the laminate.
[0080] The method for slicing the laminate is not particularly limited, and examples thereof include a multi-blade method, a laser processing method, a water jet method, a knife processing method, etc. Among these, the knife processing method is preferred in that it is easy to make the thickness of the composite sheet uniform.
[0081] The cutting tool used for slicing the laminate is not particularly limited, and a slicing member having a smooth surface with a slit and a blade portion protruding from the slit portion (e.g., a plane or slicer with a sharp blade) can be used.
[0082] From the viewpoint of increasing the thermal conductivity of the composite sheet, the angle at which the laminate is sliced is preferably 30° or less with respect to the stacking direction, more preferably 15° or less with respect to the stacking direction, and preferably approximately 0° with respect to the stacking direction (i.e., in the direction along the stacking direction).
[0083] <Copper foil> The copper foil is not particularly limited as long as it is a foil containing copper, and examples thereof include foils made of copper or copper alloys. Examples of copper alloys include alloys containing copper and at least one selected from the group consisting of nickel, phosphorus, tungsten, arsenic, molybdenum, chromium, cobalt, and zinc. In addition, the surface of the copper foil is preferably subjected to various surface treatments such as anodizing, degreasing, sandblasting, etching, various plating treatments, and primer treatment using a coupling agent, etc., in order to improve adhesion to the composite sheet.
[0084] From the viewpoint of adhesion to the composite sheet, the ten-point average roughness (Rz) of the copper foil surface is preferably 3.0 μm or less, more preferably 2.0 μm or less, and is preferably 0.3 μm or more, and more preferably 0.5 μm or more. In this specification, the ten-point average roughness (Rz) can be measured in accordance with JIS B0601.
[0085] The thickness of the copper foil is not particularly limited, and is usually 3 μm or more, preferably 8 μm or more, more preferably 15 μm or more, and usually 40 μm or less, preferably 35 μm or less, more preferably 20 μm or less.
[0086] Commercially available copper foils can also be used. The copper foil may be rolled copper foil or electrolytic copper foil. Examples of rolled copper foils include BHY-22B-T (product name) and GHY5-93F-T (product name) manufactured by JX Nippon Mining & Metals Corporation. Examples of electrolytic copper foils include F1-WS (product name) manufactured by Furukawa Electric Co., Ltd., HLS (product name), HLS-Type2 (product name), and HLB (product name) manufactured by Nippon Denkai Co., Ltd., and AMFN (product name) manufactured by JX Nippon Mining & Metals Corporation.
[0087] <Properties of copper-clad laminate> The copper-clad laminate preferably has a peel strength of 0.8 N or more, more preferably 1.0 N or more, and even more preferably 1.5 N or more. If the peel strength of the copper-clad laminate is equal to or higher than the above lower limit, the adhesion of the copper-clad laminate can be improved. On the other hand, the peel strength of the copper-clad laminate is, for example, 10N or less, may be 5N or less, or may be 3N or less. In this specification, the peel strength of the copper-clad laminate can be measured by the method described in the Examples. The peel strength of the copper-clad laminate can be adjusted by the types and proportions of materials and components (sulfur-based crosslinking agents, crosslinkable thermoplastic resins, fillers, etc.) contained in the composite sheet, the manufacturing method and manufacturing conditions of the composite sheet, and the type of copper foil, etc.
[0088] The thermal resistance value of the copper-clad laminate when a pressure of 0.1 MPa is applied is preferably 1.200° C. / W or less, more preferably 1.000° C. / W or less, and even more preferably 0.900° C. / W or less. If the thermal resistance value of the copper-clad laminate when a pressure of 0.1 MPa is applied is equal to or less than the above upper limit, the low thermal resistance of the copper-clad laminate under low pressure can be improved. On the other hand, the thermal resistance value of the copper-clad laminate when a pressure of 0.1 MPa is applied is, for example, 0.100° C. / W or more, or may be 0.300° C. / W or more, or may be 0.500° C. / W or more.
[0089] The thermal resistance value of the copper-clad laminate when a pressure of 0.9 MPa is applied is preferably 1.000° C. / W or less, more preferably 0.650° C. / W or less, and even more preferably 0.500° C. / W or less. If the thermal resistance value of the copper-clad laminate when a pressure of 0.9 MPa is applied is equal to or less than the above upper limit, the low thermal resistance of the copper-clad laminate under high pressure can be improved. On the other hand, the thermal resistance value of the copper-clad laminate when a pressure of 0.9 MPa is applied is, for example, 0.050° C. / W or more, may be 0.100° C. / W or more, or may be 0.300° C. / W or more.
[0090] In this specification, each thermal resistance value in the thickness direction of the copper-clad laminate can be measured by the method described in the Examples. The thermal resistance value in the thickness direction of the copper-clad laminate can be adjusted by the types and proportions of materials and components (sulfur-based crosslinking agents, crosslinkable thermoplastic resins, fillers, etc.) contained in the composite sheet, the manufacturing method and manufacturing conditions of the composite sheet, and the type of copper foil.
[0091] The thickness of the copper-clad laminate is preferably 0.05 mm or more, more preferably 0.10 mm or more, and is preferably 1.00 mm or less, more preferably 0.40 mm or less, and even more preferably 0.35 mm or less.
[0092] The thickness of the copper clad laminate is defined as T0, and the thickness of the copper clad laminate when pressed in the thickness direction with 0.9 MPa is defined as T 0.9 As shown in the following formula (1): C = 100 × {1-(T 0.9 / T0)}[%]···(1) The compression ratio C calculated by is preferably 0.5% or more, more preferably 1% or more, preferably 10% or less, more preferably 5% or less, even more preferably 3% or less, and even more preferably 2.5% or less. The compression ratio C of the copper-clad laminate can be adjusted by the types and proportions of materials and components (sulfur-based crosslinking agent, crosslinkable thermoplastic resin, filler, etc.) contained in the composite sheet, as well as the manufacturing method and manufacturing conditions of the composite sheet.
[0093] <Method of manufacturing copper-clad laminate> A copper-clad laminate can be obtained, for example, by placing copper foil on both sides (main and back sides) or one side (main or back side) of a composite sheet to obtain a crosslinkable laminate, and then hot compressing this crosslinkable laminate at a temperature at which the sulfur-based crosslinking agent and the crosslinkable polymer in the composite sheet crosslink and a crosslinking reaction between the copper foil and the sulfur-based crosslinking agent occurs. The temperature during the thermal compression is not particularly limited, but is usually 160° C. to 200° C. The pressure during the thermal compression is not particularly limited, but is usually 0.2 MPa to 0.5 MPa. The time for the thermal compression is not particularly limited, but is usually 0.5 hours to 3 hours. EXAMPLES
[0094] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, the amounts "%" and "parts" are based on mass unless otherwise specified. In addition, when calculating the volume fraction, the volume of each blended component was calculated by dividing the mass of each blended component by its theoretical specific gravity. Various measurements and evaluations in the examples were performed according to the following methods.
[0095] <SP value of crosslinkable thermoplastic resin> SP value (MPa) of crosslinkable thermoplastic resin used in examples and comparative examples 1 / 2 ) was determined by turbidimetric titration. Toluene was used as a good solvent and hexane as a poor solvent.
[0096] <Orientation angle of boron nitride> The orientation angle of boron nitride in the composite sheet obtained in each Example and Comparative Example was observed by cutting the cross section of the composite sheet into a regular octagon with a scanning electron microscope (SEM, Hitachi High-Technologies Corporation, "SU-3500") at a magnification that could fit the top and bottom of the sheet. The magnification was 700x. 50 lines were drawn along the long axis of boron nitride in this cross section, and the average angle of the long axis with respect to the surface of the composite sheet was calculated. If the angle was 90° or more, the supplementary angle was used. This was performed for 8 faces, and the largest value among the 8 faces was taken as the orientation angle of boron nitride in the composite sheet. In addition, since the composite sheet containing boron nitride has high insulating properties, it may be difficult to obtain an SEM image (so-called "charge-up"). In this case, a treatment such as providing a conductive coating of platinum or the like may be carried out.
[0097] <Thermal conductivity> The thermal diffusivity α(m 2 / s), specific heat at constant pressure Cp (J / g K) and specific gravity ρ (g / m 3 ) was measured by the following method. [Thermal diffusivity in the thickness direction α(m 2 / s)] The thermal diffusivity of the composite sheet in the thickness direction was measured using a thermal property measuring device (manufactured by Bethel Corporation, product name "Thermowave Analyzer TA35"). [Specific heat at constant pressure Cp(J / g K)] The specific heat was measured using a differential scanning calorimeter (manufactured by Rigaku, product name "DSC8230") under a temperature increase condition of 10°C / min. [Specific gravity ρ(g / m 3 )] Specific gravity (density) (g / m) was measured using an automatic specific gravity meter (manufactured by Toyo Seiki, product name "DENSIMETER-H") 3 ) was measured. Then, the obtained measured values are used to calculate the following formula (2): λ = α × Cp × ρ (2) The thermal conductivity λ (W / m K) of the composite sheet in the thickness direction was calculated by substituting
[0098] <Dielectric constant and dielectric loss> The dielectric constant (F / m) and dielectric loss (unitless quantity) of the composite sheets obtained in each of the Examples and Comparative Examples were measured using a network analyzer (manufactured by Keysight Technologies: product name "N5227A"). Specifically, measurements were performed using the balanced disk resonator method (BCDR method), and the dielectric constant and dielectric loss at 10 GHz were calculated.
[0099] <Peel strength> The peel strength between the composite sheet and the copper foil in the copper-clad laminate obtained in each of the Examples and Comparative Examples was measured using a peel analysis device (manufactured by Kyowa Interface Science Co., Ltd., "VPA-H100"). Specifically, first, the copper-clad laminate was cut to a width of 2 cm. Next, the copper-clad laminate was fixed on a flat table so that the copper foil on the back side of the composite sheet of the copper-clad laminate was facing down. Next, at one end of the copper-clad laminate, a part of the copper foil on the main surface side of the composite sheet was peeled off. Next, the copper foil of the peeled part was held, and the copper foil was peeled off in a 180° direction at a speed of 200 mm / min in an atmosphere of 25°C. The maximum tensile strength measured when the copper foil was then peeled off was taken as the peel strength (peel strength).
[0100] <Thermal resistance and compressibility> The thermal resistance value and compression ratio of the copper-clad laminates produced in each of the Examples and Comparative Examples were measured using a thermal resistance tester (manufactured by Hitachi Technology and Services, Ltd., product name "Resin Material Thermal Resistance Measuring Device"). Specifically, first, a copper-clad laminate cut into an approximately 1 cm square was used as a sample, and the thermal resistance and thickness of the copper-clad laminate were measured at a sample temperature of 50°C when pressures of 0.1 MPa and 0.9 MPa were applied in the thickness direction. The thickness of the sample before pressure was applied was defined as T0, and the thickness of the sample when a pressure of 0.9 MPa was applied was defined as T 0.9 Let T0 and T 0.9 The compression ratio C was calculated according to the following formula (1). C = 100 × {1-(T 0.9 / T0)}[%]···(1)
[0101] <Flexibility> One side of the composite sheet obtained in each Example and Comparative Example was pressed against a pin gauge with a diameter of 1.0 mm and repeatedly folded 20 times, and then the composite sheet was turned over and the other side was pressed against the same pin gauge and repeatedly folded 20 times. The parts of both sides of the composite sheet where the pin gauge had been in contact were visually evaluated for cracks, etc. The pin gauge was set perpendicular to the strips forming the composite sheet during the test. A good evaluation in the bending test means that the copper-clad laminate using the composite sheet has excellent bending strength and is highly flexible. A: There were no cracks and it was in good condition. B: Cracks occurred at the joints of the strips. C: Cracks occurred in areas other than the strip. D: It was difficult to bend and broke when bent forcibly.
[0102] <Low heat resistance under low pressure> Using the thermal resistance value measured above when a pressure of 0.1 MPa was applied, low thermal resistance under low pressure was evaluated according to the following criteria. A: The thermal resistance value is 0.900℃ / W or less when a pressure of 0.1 MPa is applied. B: The thermal resistance value when a pressure of 0.1 MPa is applied is more than 0.900°C / W and not more than 1.000°C / W. C: The thermal resistance value when a pressure of 0.1 MPa is applied is greater than 1,000°C / W and less than 1,200°C / W. D: The thermal resistance value when a pressure of 0.1 MPa is applied is more than 1.200°C / W.
[0103] <Low heat resistance under high pressure> Using the thermal resistance value measured above when a pressure of 0.9 MPa was applied, the low thermal resistance under high pressure was evaluated according to the following criteria. A: The thermal resistance value is 0.500℃ / W or less when a pressure of 0.9MPa is applied. B: The thermal resistance value when a pressure of 0.9 MPa is applied is greater than 0.500°C / W and not greater than 0.650°C / W. C: The thermal resistance value when a pressure of 0.9 MPa is applied is more than 0.650°C / W and not more than 1,000°C / W. D: The thermal resistance value exceeds 1.000℃ / W when a pressure of 0.9MPa is applied.
[0104] <Adhesion> Using the peel strength measured above, the adhesion was evaluated according to the following criteria. A: Peel strength is 1.5N or more. B: The peel strength is 1.0 N or more and less than 1.5 N. C: The peel strength is 0.8 N or more and less than 1.0 N. D: The peel strength is less than 0.8 N.
[0105] <Thermal conductivity> Using the thermal conductivity measured above, the thermal conductivity was evaluated according to the following criteria: The higher the thermal conductivity of the composite sheet, the more excellent the thermal conductivity of the copper-clad laminate. A: Thermal conductivity is 25 W / m K or higher. B: Thermal conductivity is 20 W / m K or more and less than 25 W / m K. C: Thermal conductivity is 15 W / m K or more and less than 20 W / m K. D: Thermal conductivity is less than 15 W / m K.
[0106] <Low dielectric properties> Using the dielectric constant measured above, the low dielectric property was evaluated according to the following criteria. Note that the lower the dielectric constant of the composite sheet, the more excellent the low dielectric property of the copper-clad laminate. A: The dielectric constant is less than 4.0 F / m. B: The dielectric constant is 4.0 F / m or more and less than 4.3 F / m. C: The dielectric constant is 4.3 F / m or more and less than 5.0 F / m. D: The dielectric constant is 5.0 F / m or more.
[0107] <Low dielectric loss> Using the dielectric loss measured above, the low dielectric loss property was evaluated according to the following criteria. Note that the smaller the dielectric loss of the composite sheet, the more excellent the low dielectric loss property of the copper-clad laminate. A: Dielectric loss is 4.5×10 -4 is less than. B: Dielectric loss is 4.5×10 -4 Above 5.0×10 -4 is less than. C: Dielectric loss is 5.0×10 -4 More than 5.5 x 10 -4 is less than. D: Dielectric loss is 5.5×10 -4 That's all.
[0108] Example 1 <Manufacturing of composite sheets> [Preparation of Composition] As a crosslinkable thermoplastic resin, styrene butadiene rubber, which is solid at room temperature and pressure (manufactured by Nippon Zeon Co., Ltd., product name "Nipole 1502", specific gravity: 0.94, SP value: 17.84 (MPa) 1 / 2 )) was prepared. Then, the prepared crosslinkable thermoplastic resin, 450 parts of hexagonal boron nitride (h-BN) particles (manufactured by Dandong Chemical Engineering, trade name "HSL", volume average particle size: 30 μm, aspect ratio: 1.25) which is scale-like (plate-like) boron nitride as a filler, 45 parts of polytetrafluoroethylene (PTFE) powder (manufactured by 3M, trade name "Dyneon TM PTFE Micropowder", organic filler), and 2.45 parts of sulfur (Kinkajirushi Fine Sulfur 325 Mesh: manufactured by Tsurumi Chemical Industry Co., Ltd.) as a sulfur-based crosslinking agent were added, and the mixture was stirred at a temperature of 120° C. for 20 minutes using a pressure kneader (manufactured by Nippon Spindle) to obtain a composition.
[0109] [Pre-sheet molding process] Next, 500 g of the obtained composition was rolled into a sheet using a first roll and a second roll under the following conditions: a gap between the first roll and the second roll of 2 mm, a roll temperature of 25° C., a sheet discharge speed (peripheral speed of the first roll) of 2 m / min, and a peripheral speed ratio of the second roll to the first roll (second roll / first roll): 1.15 / 1. The rolling process was repeated while keeping the sheet conveying direction the same. The rolling process was performed 10 times in total to obtain a pre-sheet having a thickness of 2 mm.
[0110] [Laminate molding process] Next, the obtained pre-sheet was cut into a size of 50 mm length x 50 mm width, and 25 sheets were stacked in the thickness direction of the pre-sheet to obtain a first laminate. The obtained first laminate was then pressed (secondary pressurization) in the stacking direction at a temperature of 120°C and a pressure of 0.1 MPa for 3 minutes to obtain a second laminate with a height of about 50 mm.
[0111] [Slicing process] Next, while pressing the laminated surface of the second laminate with a pressure of 0.3 MPa, a wood slicer (manufactured by Marunaka Iron Works Co., Ltd., product name "Super Finish Planer Super Mecha S") was used to slice at an angle of 0 degrees to the lamination direction (in other words, in the normal direction of the main surface of the laminated pre-sheets), to obtain a flat composite sheet of about 50 mm length x 50 mm width x 0.30 mm thickness. The obtained composite sheet is composed of strips joined in parallel in a direction perpendicular to the thickness direction of the composite sheet (a direction at an angle of 90° to the thickness direction). In other words, the composite sheet has a structure in which each strip is joined in parallel to another adjacent strip within the main surface of the composite sheet. The width of the strip in the approximately perpendicular direction is approximately the same as the thickness of the pre-sheet. The orientation angle of boron nitride, thermal conductivity, dielectric constant and dielectric loss, flexibility, thermal conductivity, low dielectric property, and low dielectric loss property of the obtained composite sheet were measured and evaluated. The results are shown in Table 1.
[0112] <Manufacturing of copper-clad laminates> Copper foil was placed on both sides (main surface and back surface) of the obtained composite sheet to obtain a crosslinkable laminate, and then this crosslinkable laminate was pressed at 0.3 MPa for 1 hour in an atmosphere of 170°C to attach copper foil to both sides of the composite sheet, thereby obtaining a copper-clad laminate with a thickness of approximately 0.30 mm. The obtained copper-clad laminate was used to measure and evaluate the peel strength, heat resistance, compression ratio, low heat resistance under low pressure, low heat resistance under high pressure, and adhesion. The results are shown in Table 1.
[0113] Example 2 In preparing the composition, the amount of sulfur used as the sulfur-based crosslinking agent was changed from 2.45 parts to 1.2 parts, but the same operations, measurements, and evaluations were carried out as in Example 1. The results are shown in Table 1.
[0114] Example 3 In preparing the composition, the amount of hexagonal boron nitride used as a filler was changed from 450 parts to 280 parts, but the same operations, measurements, and evaluations were carried out as in Example 1. The results are shown in Table 1.
[0115] Example 4 <Manufacturing of composite sheets> [Preparation of Composition] A composition was prepared in the same manner as in Example 1.
[0116] [Pre-sheet molding process] Next, a pre-sheet was obtained in the same manner as in Example 1 using the obtained composition.
[0117] [Laminate molding process] Next, the obtained pre-sheet was cut to 50 mm long x 50 mm wide. In addition, an adhesive sheet made of acrylic resin as a layered adhesive material (manufactured by Toa Gosei, product name "Aronmighty AF60", thickness: 10 μm) was cut to 50 mm long x 50 mm wide. The cut adhesive sheet was placed on the cut pre-sheet, and 25 pre-sheets (24 adhesive sheets were used) were stacked in the thickness direction with the adhesive sheets interposed between them, to obtain a first laminate with a height of about 50 mm in which the adhesive sheets were located between the pre-sheets. The obtained first laminate was wrapped in release PET (polyethylene terephthalate), taped, and vacuum-packaged in a PET retort package. This was heated and pressurized (secondary pressurization) for 30 minutes in an autoclave (Hanyu Iron Works, small autoclave "DANDELION") at a temperature of 150°C and a pressure (absolute pressure) of 0.8 MPa from all directions to obtain a second laminate.
[0118] [Slicing process] Next, the laminated surface of the second laminate was pressed with a pressure of 0.3 MPa, and sliced at an angle of 0 degrees to the lamination direction (in other words, in the normal direction of the main surface of the laminated pre-sheets) using a wood slicer (Marunaka Iron Works Co., Ltd., product name "Super Finishing Planer Super Mecha S") to obtain a flat composite sheet of about 50 mm length x 50 mm width x 0.30 mm thickness. The obtained composite sheet is composed of strips and adhesive layers that are joined in parallel in a direction perpendicular to the thickness direction of the composite sheet (a direction at an angle of 90 degrees to the thickness direction). In other words, the composite sheet has a structure in which strips and adhesive layers located between adjacent strips are joined in parallel within the main surface of the composite sheet. The width of the strips in the approximately perpendicular direction is approximately the same as the thickness of the pre-sheet. In the composite sheet, the strips originate from the pre-sheets, and the adhesive layers originate from the adhesive sheets. The orientation angle of boron nitride, thermal conductivity, dielectric constant and dielectric loss, flexibility, thermal conductivity, low dielectric property, and low dielectric loss property of the obtained composite sheet were measured and evaluated. The results are shown in Table 1.
[0119] <Manufacturing of copper-clad laminates> Copper foil was placed on both sides (main surface and back surface) of the obtained composite sheet to obtain a crosslinkable laminate, and then this crosslinkable laminate was pressed at 0.3 MPa for 1 hour in an atmosphere of 170°C to attach copper foil to both sides of the composite sheet, thereby obtaining a copper-clad laminate with a thickness of approximately 0.30 mm. The obtained copper-clad laminate was used to measure and evaluate the peel strength, heat resistance, compression ratio, low heat resistance under low pressure, low heat resistance under high pressure, and adhesion. The results are shown in Table 1.
[0120] Example 5 In preparing the composition, except that no polytetrafluoroethylene powder was added as an organic filler, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0121] Comparative Example 1 In preparing the composition, 3 parts of triallyl isocyanurate (manufactured by Mitsubishi Chemical Corporation, product name "TAIC (registered trademark)") was added as a non-sulfur crosslinking agent instead of 2.45 parts of sulfur as a sulfur crosslinking agent, and 4 parts of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (manufactured by Nippon Oil & Fats Corporation, product name "Perhexa (registered trademark) 25B") was added as a reaction initiator. The operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.
[0122] Comparative Example 2 Various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that in the preparation of the composition, sulfur was not added as a sulfur-based crosslinking agent, and in the production of the copper-clad laminate, an adhesive sheet made of acrylic resin (manufactured by Toa Gosei, product name "Aronmighty AF60", thickness: 10 μm) was interposed between the main surface of the composite sheet and the copper foil, and between the back surface of the composite sheet and the copper foil, respectively, to bond the composite sheet to the copper foil. The results are shown in Table 1.
[0123] [Table 1]
[0124] As is clear from Table 1, the copper-clad laminates of Examples 1 to 5 are excellent in flexibility and low heat resistance, as well as in adhesion. [Industrial Applicability]
[0125] According to the present invention, it is possible to provide a copper-clad laminate which is excellent in flexibility, low heat resistance, and adhesion. [Explanation of symbols]
[0126] 100: Copper-clad laminate 110: Composite sheet 111: Main surface 112: Back side 113: strip 114: Adhesive layer 120: Copper foil
Claims
1. A composite sheet including a sulfur-based crosslinking agent, a thermoplastic resin crosslinkable by the sulfur-based crosslinking agent, and a filler; A copper foil provided directly on at least one of the main surface and the back surface of the composite sheet; A copper-clad laminate obtained by crosslinking a crosslinkable laminate comprising: a content ratio of the filler in the composite sheet is 45% by volume or more and 75% by volume or less, when the total content of the thermoplastic resin and the filler is 100% by volume; the filler comprises boron nitride; A copper-clad laminate, wherein the orientation angle of the boron nitride relative to the main surface of the composite sheet is 60° or more and 90° or less.
2. The copper clad laminate of claim 1 , wherein the boron nitride is in the form of flakes.
3. 2. The copper clad laminate according to claim 1, wherein the content of the boron nitride in the composite sheet is 40% by volume or more and 65% by volume or less, when the total of the thermoplastic resin and the filler is 100% by volume.
4. 2. The copper-clad laminate according to claim 1, wherein the content of the sulfur-based crosslinking agent in the composite sheet is 1.00 parts by mass or more and 5.00 parts by mass or less with respect to 100 parts by mass of the thermoplastic resin.
5. The thermoplastic resin satisfies the following conditions (1) and (2): (1) SP value: 18.45 (MPa) 1 / 2 Is less than or equal to (2) At least one selected from the group consisting of polybutene, butyl rubber, styrene butadiene rubber, isoprene rubber, and ethylene propylene rubber. The copper-clad laminate according to any one of claims 1 to 4, which satisfies at least one of the above.
Citation Information
Patent Citations
Heat-developable color photographic material
JP1985023474A
Resin-coated metal foil, flexible printed wiring board
JP2022133347A