Lining structure of AOD furnace

By employing magnesia carbon bricks with controlled carbon content in specific areas of the AOD furnace, the durability issues of conventional lining structures are addressed, leading to extended furnace life and reduced maintenance.

JP2024140797APending Publication Date: 2024-10-10KROSAKI HARIMA CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052135
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional lining structures for AOD furnaces, such as those using dolomite, maguro, or magnesia carbon bricks, suffer from durability issues due to hydration, thermal shock, and magcarbon reactions, leading to structural deterioration and increased maintenance costs.

Method used

The use of magnesia carbon bricks with a controlled carbon content (1-5% by mass for tuyere-related areas and 2-9% by mass for other areas) to reduce magcarbon reactions and enhance thermal shock resistance, improving durability.

Benefits of technology

Significantly extends the life of the AOD furnace, reduces repair frequency, and lowers maintenance costs by enhancing the lining structure's durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140797000001_ABST
    Figure 2024140797000001_ABST
Patent Text Reader

Abstract

To improve the durability of the lining structure of an AOD furnace.SOLUTION: In an AOD furnace 1, as tuyere peripheral bricks 6 configuring a tuyere body 5 and a tuyere peripheral part and tuyere upper stage part bricks 7 configuring a tuyere upper stage part, magnesia-carbon bricks or magnesia-chrome bricks having a C content of 1 or more to 5 mass% or less are lined, and magnesia-carbon bricks having a C content of 2 or more to 9 mass% or less are lined to a part other than the tuyere body, the tuyere peripheral part and the tuyere upper stage part so as to occupy 70% or more of the in-furnace surface area of the part.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lining structure of an AOD furnace in which decarburization is performed by blowing inert gases such as argon, nitrogen, etc. together with oxygen gas into molten steel during the refining of Cr-containing steel such as stainless steel. [Background technology]

[0002] Generally, the AOD process, the VOD process, the AOD-VOD process which combines these, and the converter-VOD process are known as methods for refining stainless steel, etc. Among these, dolomite bricks or magnesia-chrome bricks are usually used for the lining of AOD furnaces.

[0003] However, in the case of a lining structure using dolomite bricks, if left at room temperature before use or even during operation, slaking (destruction of structure due to hydration reaction) will progress, so it is necessary to preheat and start up the furnace as soon as possible after construction, and it is also necessary to wait for preheating even if the furnace is temporarily taken out of operation.

[0004] In addition, in the case of a lining structure using magnesia-chrome bricks, there is less concern about slaking compared to dolomite bricks even if the furnace is left unused after construction. However, if it is necessary to stop operation after startup, the dusting phenomenon on the working surface (calcium silicate (2CaO SiO 2 ) due to the low C / S composition of the infiltrated slag component) may occur when the temperature is lowered to room temperature. 2 The problem is that the slag-infiltrated layer falls off due to the volume change phenomenon of the slag. In addition, the thermal shock resistance of the bricks is generally inferior to that of dolomite bricks.

[0005] On the other hand, magnesia carbon bricks are generally less susceptible to scorching than dolomite bricks and have good corrosion resistance. In addition, magnesia carbon bricks do not have the problem of the slag-infiltrated layer falling off, and have excellent thermal shock resistance, so they can be used in AOD furnaces. However, in AOD furnaces, the CO gas partial pressure P COAs a result, the structure of the magnesia carbon brick deteriorates due to the magnesium-carbon reaction (MgO+C→Mg↑+CO↑), and the Cr in the slag 2 O 3 In the reduction process, the temperature reaches 1700 to 1800°C, which causes significant wear of the deteriorated structure, and it has been considered that magnesia carbon bricks cannot be used as refractories for the side walls of AOD furnaces, in particular. For example, Patent Document 1 discloses that tuyere bricks, consisting of tuyere bricks and tuyere receiving bricks arranged around them, are made of magnesia carbon bricks with a C content of 3 to 25% by mass, but it is considered that these cannot be used for the side walls of furnaces, etc.

[0006] As described above, the durability of the lining structure of conventional AOD reactors was not sufficient. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2002-115011 A Summary of the Invention [Problem to be solved by the invention]

[0008] The problem to be solved by the present invention is to improve the durability of the lining structure of an AOD reactor. [Means for solving the problem]

[0009] The present inventors considered that the use of magnesia carbon bricks with a low content of the C component that causes the magnesium-carbon reaction in the lining structure of an AOD furnace would reduce the effects of the magnesium-carbon reaction and inhibit structural deterioration to a certain extent. As a result of various investigations, the inventors discovered that by using magnesia carbon bricks or magnesia chrome bricks with a C content of 1% to 5% by mass for the tuyere body, tuyere peripheral bricks constituting the tuyere peripheral part, and tuyere upper stage bricks constituting the tuyere upper stage, which are most susceptible to wear, and by lining the parts other than the tuyere body, tuyere peripheral part, and tuyere upper stage with magnesia carbon bricks with a C content of 2% to 9% by mass, the durability of the lining structure of an AOD furnace is significantly improved compared to conventional lining structures lined with magnesia chrome bricks or dolomite bricks.

[0010] That is, according to one aspect of the present invention, there is provided the following lining structure for an AOD reactor. A lining structure of an AOD furnace, The tuyere body, the tuyere peripheral bricks constituting the tuyere peripheral portion, and the tuyere upper stage bricks constituting the tuyere upper stage portion are lined with magnesia carbon bricks or magnesia chrome bricks having a C content of 1% by mass or more and 5% by mass or less, The lining structure of an AOD furnace is such that the areas excluding the tuyere body, the periphery of the tuyere, and the upper stage of the tuyere are lined with magnesia carbon bricks having a C content of 2% by mass or more and 9% by mass or less, so that the lining occupies 70% or more of the furnace surface area of ​​those areas. Effect of the Invention

[0011] According to the present invention, the durability of the lining structure of the AOD furnace is significantly improved, which leads to a significant extension of the life of the AOD furnace, which leads to an improvement in the operation rate by reducing the number of furnace repairs, a reduction in the repair work costs, and a reduction in the unit cost of furnace materials. [Brief description of the drawings]

[0012] [Figure 1]1 is a schematic vertical cross-sectional view of an AOD furnace to which a lining structure of an AOD furnace according to one embodiment of the present invention is applied. [Diagram 2] Cross section AA of Figure 1. [Diagram 3] Cross-sectional view of FIG. 1 taken along line B-B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In the lining structure of the AOD furnace of the present invention, the tuyere body, the tuyere peripheral bricks constituting the tuyere peripheral portion, and the tuyere upper stage bricks constituting the tuyere upper stage portion are made of magnesia carbon bricks or magnesia chrome bricks with a C content of 1% to 5% by mass from the viewpoint of oxidation resistance and molten steel abrasion resistance, since they are greatly affected by oxidation due to blowing gas and abrasion by molten steel. If the C content of this magnesia carbon brick is less than 1% by mass, the thermal shock resistance is insufficient and wear becomes large, whereas if the C content exceeds 5% by mass, wear becomes large due to oxidation due to blowing gas and abrasion by molten steel.

[0014] Here, magnesia carbon bricks with a C content of 1% by mass or more and 5% by mass or less are not subject to slag infiltration like magnesia-chrome bricks, and therefore do not cause the dusting phenomenon. In addition, they have excellent thermal shock resistance, so their use, particularly in the upper stage of the tuyere, makes it possible to create a lining structure with even greater durability. Furthermore, magnesia carbon bricks with a C content of 1% by mass or more and 5% by mass or less have better thermal shock resistance than magnesia-chrome bricks, and can therefore be used for the tuyere body and its surrounding areas. By using magnesia carbon bricks with a C content of 1% by mass or more and 5% by mass or less for at least one of the tuyere body and the surrounding bricks, a lining structure with better durability can be achieved. In addition, since the tuyere body and the bricks around the tuyere are affected by oxidation due to blowing gas and abrasion by molten steel, a lower C content is advantageous in terms of these. From the viewpoint of thermal shock resistance, a certain level of C content must be ensured. In other words, by using magnesia carbon bricks with a C content of 2% by mass or more and less than 4% by mass for at least one of the tuyere body and the bricks around the tuyere, the durability of the lining structure can be further improved.

[0015] In the lining structure of the AOD furnace of the present invention, magnesia carbon bricks having a C content of 2% by mass to 9% by mass are used to line the areas other than the tuyere body, the periphery of the tuyere, and the upper stage of the tuyere, so as to occupy 70% or more of the surface area of ​​the furnace. If the C content of the magnesia carbon bricks is less than 2% by mass, the thermal shock resistance is insufficient, leading to large wear, whereas if the C content exceeds 9% by mass, the effect of structural deterioration due to the magnesia carbon reaction becomes large, resulting in a significant decrease in durability. The C content of the magnesia carbon bricks may be 4% by mass to 8% by mass in order to improve thermal shock resistance and corrosion resistance.

[0016] Thus, in the lining structure of the AOD furnace of the present invention, areas other than the tuyere body, the tuyere periphery, and the tuyere upper stage are lined with magnesia carbon bricks having a C content of 2% by mass or more and 9% by mass or less so as to occupy 70% or more of the in-furnace surface area of ​​those areas, and the areas other than 70% of the in-furnace surface area of ​​those areas can be lined with magnesia carbon bricks having a C content of more than 9% by mass and 15% by mass or less, for example. The furnace surface area refers to the total area of ​​the working surfaces of the bricks lining the AOD furnace, and the working surfaces refer to the surfaces of the bricks exposed inside the furnace.

[0017] The magnesia carbon brick used in the present invention can be obtained by the same manufacturing method as that for general magnesia carbon bricks, specifically, by adding an organic binder such as a phenolic resin to a refractory raw material mixture, kneading the mixture, forming the mixture, and then heat treating the mixture at 150° C. to 800° C. Then, the composition of the refractory raw material mixture and the amount of the organic binder added are adjusted so that the C content of the obtained magnesia carbon brick is a predetermined value.

[0018] Here, the carbon content of magnesia carbon bricks is the mass ratio (%) of the total carbon content in the bricks, which can be calculated from the total amount of fixed carbon in the refractory raw material mixture and the organic binder, and the amount of carbon contained in the carbide raw materials such as silicon carbide. The fixed carbon content in the refractory raw material mixture and the organic binder can be calculated from the specifications of the manufacturers of the raw materials. If the specifications of the raw material manufacturers are unknown, the fixed carbon of each raw material used can be measured according to JIS standards. Specifically, pitch can be measured and specified according to JIS K2425, graphite can be measured and specified according to JIS M8511, organic binder can be measured and specified according to JIS K6910, and materials other than pitch, graphite, and organic binder can be measured and specified according to JIS M8812. The total carbon content in the refractory raw material mixture and the organic binder is substantially the same as the total carbon content in the bricks.

[0019] On the other hand, when the composition of the magnesia carbon brick used in the present invention is specified from the viewpoint of the content of refractory raw materials, it preferably contains 88% by mass or more and 99% by mass or less of magnesia, 8% by mass or less (including 0) of graphite, and 1% by mass or more and 7% by mass or less of at least one of Al, Al-Mg alloy, Si, Al-Si alloy, boron carbide, silicon carbide, pitch and carbon black. Since the AOD furnace is operated intermittently and cooled during the operation, the magnesia carbon brick of the present invention preferably contains graphite, which has excellent thermal shock resistance, however, magnesia carbon bricks that do not contain graphite but contain small amounts of pitch, carbon black, etc. and have excellent thermal shock resistance have been developed in recent years, and it is also possible to use magnesia carbon bricks that do not contain graphite. That is, it is appropriate and sufficient to specify the composition of the magnesia carbon brick used in the present invention by the C content, and other components may be appropriately determined within the scope of common technical knowledge.

[0020] The magnesia-chrome bricks used in the present invention are manufactured from magnesia raw materials, magnesia-chrome raw materials, chromium ore, chromium oxide, etc., just like general magnesia-chrome bricks, and can be either fired or unfired. Note that magnesia-chrome bricks basically do not contain carbon components, but those containing 1% by mass or less of carbon components derived from organic binders can also be used.

[0021] Next, specific embodiments of the lining structure of an AOD furnace according to the present invention will be described with reference to Figures 1 to 3. Figure 1 is a schematic vertical cross-sectional view of an AOD furnace to which the lining structure of an AOD furnace according to one embodiment of the present invention is applied, Figure 2 is a cross-sectional view taken along line AA in Figure 1, i.e., the fourth stage, and Figure 3 is a cross-sectional view taken along line BB in Figure 1, i.e., the fifth stage.

[0022] As shown in Fig. 1, in the AOD furnace 1, the inside of the steel shell 2 is lined with a permanent refractory 3, and the inside of the permanent refractory 3 is lined with lining bricks 4. In addition, the AOD furnace 1 is provided with a tuyere body 5 for injecting gas into the furnace. Here, the tuyere body 5 is a refractory having a through hole into which a gas injection tube is inserted, and in this embodiment, as shown in Fig. 2, five tuyere bodies 5 are provided at approximately equal intervals in the circumferential direction of the AOD furnace 1.

[0023] 2, five tuyere peripheral bricks 6 are lined between each of the five tuyere bodies 5, for a total of 20 tuyere peripheral bricks 6. Furthermore, two tuyere peripheral bricks 6 are lined in the circumferential direction of the two outer tuyere bodies 51 on the opposite side to the tuyere bodies 5. These tuyere bodies 5 and tuyere peripheral bricks 6 are lined in a sector shape from the center of the furnace within an angle θ of 150°. On the other hand, FIG. 3 shows the lining structure of the fifth stage, in which only the bricks 6 around the tuyere are lined in a sector shape with an angle θ of 150° from the center of the furnace.

[0024] Although not shown in the drawings, the second stage is lined with a tuyere body 5 and peripheral bricks 6 in a pattern similar to that of the fourth stage (see Fig. 2). Also, the first and third stages, like the fifth stage (see Fig. 3), do not have a tuyere body installed, but are lined with peripheral bricks 6 in a sector-like range at an angle of 150° from the center of the furnace.

[0025] Here, in the present invention, the tuyere peripheral bricks (6) refer to the bricks arranged between the tuyere bodies (5), up to a maximum of five bricks arranged in succession in the circumferential direction on the opposite side of the tuyere body 5 in contact with the outer tuyere body (51), and the bricks in contact with the upper or lower surfaces of these bricks. These tuyere peripheral bricks are areas that are subject to greater wear due to the effect of the gas blown in from the tuyere during blowing, and so in many cases the bricks are made longer or made of a highly durable material to make them more durable than other areas.

[0026] In the present invention, the tuyere upper stage bricks (7) refer to at least the bricks in contact with the upper surface of the uppermost brick 61 of the tuyere peripheral bricks 6 in Fig. 1, and the bricks lining at least three stages and up to ten stages from this brick 61 upward. In Fig. 1, the tuyere upper stage bricks 7 are lined from the sixth stage to the thirteenth stage, and within an angle θ of 150° from the center of the furnace in a sector shape. In this embodiment, the height of the tuyere upper stage bricks 7 is 100 mm, and eight stages of the tuyere upper stage bricks 7 are stacked. Therefore, the height of the tuyere upper stage is 800 mm.

[0027] Here, the height of the lining bricks of the AOD furnace 1, i.e., the tuyere body 5, the tuyere peripheral bricks 6, and the tuyere upper stage bricks 7 used in the present invention, varies depending on the size and lining structure of the AOD furnace 1, but is generally within the range of 50 to 150 mm in the present invention. On the other hand, when lining with bricks of a height outside this range, the lining height of the tuyere upper stage can be at least 150 mm or more and at most 1500 mm or less. The brick height here refers to the length of the brick in the furnace length direction on the working surface of the brick when one brick is placed in the AOD furnace. Similarly, the lining height refers to the length of the working surface (inner surface) of the lining (brick assembly) in the furnace length direction. In the present invention, the area lined with the tuyere upper stage bricks in the AOD furnace is referred to as the tuyere upper stage, and the area lined with the tuyere peripheral bricks is referred to as the tuyere peripheral area.

[0028] The lining structure of the present invention can be applied to ordinary AOD furnaces, but especially to Cr 2 O 3 In AOD furnaces, where the reduction rate is relatively low, the Cr content in the slag after decarburization is 2 O 3 The AOD furnace can be suitably applied to an AOD furnace in which the concentration is 7 to 17.5 mass%. In the operation of such an AOD furnace, the decrease in CO partial pressure is suppressed, so that the magnesia-carbon reaction is suppressed, and the durability of the furnace can be significantly improved by using the magnesia-carbon brick. Such an AOD furnace corresponds to, for example, an AOD furnace used in the AOD-VOD method. EXAMPLES

[0029] Table 1 shows the details of the lining bricks used in the lining structure of the AOD furnace shown in Figures 1 to 3, as well as the results of actual equipment tests.

[0030] [Table 1]

[0031] In Table 1, the values ​​in the "Lining structure" column indicate the C content (mass%) of the magnesia carbon brick used in the lining structure of each example. As such, magnesia carbon bricks with different C contents were used. Specifically, a refractory raw material mixture containing magnesia as a base, at least one of graphite and pitch powder, and metal powder was used, and the mixture was kneaded and molded in a conventional manner, followed by heat treatment at 250°C for 10 hours to produce the magnesia carbon bricks. The C content of the magnesia carbon bricks was changed by the amount of at least one of graphite and pitch powder used. Here, the C content of the magnesia carbon bricks is a calculated value calculated from the usage ratio of graphite, organic binder, and fixed carbon such as pitch powder used in the production of the magnesia carbon bricks, based on the manufacturer's specifications for each of the graphite, organic binder, and fixed carbon such as pitch powder. In Table 1, "Magne-chrome" refers to magnesia-chrome bricks, and "dolomite" refers to dolomite bricks. Specifically, the magnesia-chrome bricks contain 65% MgO and 10% Cr. 2 O 3 The semi-rebonded type containing 20% ​​by mass of magnesium oxide and the dolomite bricks used were of a fired type containing 85% by mass of magnesium oxide and 11% by mass of calcium oxide. The C content of both the magnesia-chrome bricks and the dolomite bricks used was 0% by mass. In Table 1, "area ratio" refers to the total area of ​​the working surfaces of the bricks lining the AOD furnace except for the tuyere body, the tuyere periphery, and the tuyere upper stage, i.e., the ratio of the total area (M) of the working surfaces of the magnesia carbon bricks with a C content of 2% to 9% by mass to the in-furnace surface area (T) except for the tuyere body, the tuyere periphery, and the tuyere upper stage (100 × M(m 2 ) / T(m 2 )) is the issue.

[0032] In the actual machine test, an AOD furnace lined with bricks according to the lining structure of each example was used under normal operating conditions, and when the amount of wear of the bricks reached a standard limit, operation was stopped and the number of uses at that point was evaluated. Specifically, the number of uses for Comparative Example 1 was set to 100, and the number of uses for each of the other examples was expressed as an index. The Cr content in the slag after decarburization in the AOD furnace was 2 O3 The average concentration is 14 mass%, CaO / SiO 2 The average was 1.8.

[0033] Comparative Example 1 is a conventional lining structure in which the tuyere body, the periphery and the upper part of the tuyere are made of magnesia-chrome bricks, and the other parts are made of dolomite bricks. Comparative Example 2 is a conventional lining structure in which all parts are made of magnesia-chrome bricks.

[0034] On the other hand, Examples 1 and 2 as well as Examples 4 and 5 are examples of the present invention in which the tuyere body and the periphery of the tuyere are made of magnesia-chrome bricks, and other parts are lined with magnesia-carbon bricks with a C content of 2% by mass or more and 9% by mass or less. It can be seen that the number of times of use is significantly higher than in Comparative Examples 1 and 2. Example 3 is an example in which the tuyere body, the periphery of the tuyere and the upper stage of the tuyere are made of magnesia-chrome bricks, and other parts are lined with magnesia-carbon bricks with a C content of 4% by mass, and this also produced good results.

[0035] In contrast, in Comparative Example 3, magnesia carbon bricks with a C content of 1% by mass were used to line the areas other than the tuyere body, the tuyere periphery, and the tuyere upper stage, and durability was reduced. This was because the bricks peeled off due to thermal shock. In Comparative Example 4, the C content of the magnesia carbon bricks used to line the areas other than the tuyere body, the tuyere periphery, and the tuyere upper stage was too high, resulting in significant wear and insufficient durability.

[0036] Examples 6 to 9 are examples in which the C content of the magnesia carbon bricks lining the upper stage of the tuyere was different, but it was within the range of the present invention and the number of uses was sufficient. In contrast, Comparative Example 5 had an insufficient durability because the C content was too low. This was also due to the occurrence of peeling of the bricks due to thermal shock. Comparative Example 6 is an example in which the C content of the magnesia carbon bricks lining the upper stage of the tuyere exceeded the upper limit value of the present invention, and the excessive C content caused significant wear and resulted in insufficient durability.

[0037] In Examples 10 to 15, the C content of the magnesia carbon bricks used in the tuyere body and the periphery of the tuyere was different, but it was within the range of the present invention and showed good durability. Also, for example, a comparison between Example 7 and Example 11 showed that the use of magnesia carbon bricks in the tuyere body and the periphery of the tuyere resulted in more frequent use than the use of magnesia chrome bricks in these areas. In contrast, in Comparative Example 7, the C content of the magnesia carbon bricks used in the tuyere body and the periphery of the tuyere was too low, and the durability was insufficient. This was also due to the occurrence of peeling of the bricks due to thermal shock. Comparative Example 8 is an example in which the C content of the magnesia carbon bricks used in the tuyere body and the periphery of the tuyere exceeded the upper limit of the present invention, and the excessive C content caused significant wear and resulted in insufficient durability.

[0038] In Example 16, magnesia carbon bricks with a C content of 10% by mass were used in part of the cone of the AOD furnace, and magnesia carbon bricks with a C content of 6% by mass were used in the other part of the cone, and in Example 17, dolomite bricks were used for the cone, but since the cone was not in direct contact with molten steel, it did not suffer significant wear and had good durability. Note that the cone of the AOD furnace is the cone-shaped part at the top of the furnace in Figure 1. [Explanation of symbols]

[0039] 1 AOD furnace 2 Ironhide 3 Permanent refractories 4. Lining bricks 5. Tuyere body 51 Outer tuyere body 6 Bricks around the tuyere 61 Bricks around the top tuyere 7. Upper part of tuyere brick

Claims

1. A lining structure of an AOD furnace, comprising: The tuyere body, the tuyere peripheral bricks constituting the tuyere peripheral portion, and the tuyere upper stage bricks constituting the tuyere upper stage portion are lined with magnesia carbon bricks or magnesia chrome bricks having a C content of 1% by mass or more and 5% by mass or less, A lining structure of an AOD furnace, in which areas other than the tuyere body, the periphery of the tuyere, and the upper stage of the tuyere are lined with magnesia carbon bricks having a C content of 2% by mass or more and 9% by mass or less, so that the lining occupies 70% or more of the furnace surface area of ​​those areas.

2. 2. The lining structure of an AOD furnace according to claim 1, wherein the tuyere upper stage brick is a magnesia carbon brick having a C content of 1% by mass or more and 5% by mass or less.

3. 3. The lining structure of an AOD furnace according to claim 1, wherein at least one of the tuyere body and the bricks around the tuyere is a magnesia carbon brick having a C content of 1% by mass or more and 5% by mass or less.

4. 3. The lining structure of an AOD furnace according to claim 1, wherein at least one of the tuyere body and the bricks around the tuyere is a magnesia carbon brick having a C content of 2% by mass or more and 4% by mass or less.

5. 3. The lining structure of an AOD furnace as described in claim 1 or 2, wherein areas other than the tuyere body, the tuyere periphery, and the tuyere upper stage are lined with magnesia carbon bricks having a C content of 4% by mass or more and 8% by mass or less, so as to occupy 70% or more of the furnace surface area of ​​those areas.

Citation Information

Patent Citations

  • Structure for tuyere lining in refining furnace

    JP2002115011A