Substrate for liquid filter, and liquid filter

The polyolefin microporous membrane with specified pore size and porosity effectively filters microparticles and easily removes residual metals, addressing the challenges of dense filtration and cleaning efficiency in liquid filters.

JP2024140876APending Publication Date: 2024-10-10TEIJIN LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023052235
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing liquid filters with polyolefin microporous membranes face challenges in achieving both a dense filtration medium for removing small foreign matter and efficiently removing residual metals during cleaning, as densification leads to decreased cleaning efficiency and residual metals are difficult to elute.

Method used

A polyolefin microporous membrane with a pore size of 1 nm to 35 nm, a porosity of 35% to 70%, and a water flow rate of 0.003L/min/ft²/psi to 0.180L/min/ft²/psi, allowing for easy removal of residual metals by washing, even if the membrane contains granular polyolefin that was not fully melted during production.

Benefits of technology

The solution enables effective filtration of microparticles while ensuring easy removal of residual metals, maintaining high cleaning efficiency and reducing the risk of metal elution into the processed liquid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140876000001
    Figure 2024140876000001
Patent Text Reader

Abstract

To provide a substrate for a liquid filter which has a relatively small bore diameter and allows for easily removing residual metal by cleaning.SOLUTION: A substrate for a liquid filter has a polyolefin microporous film which has a bore diameter of 1 nm to 35 nm, and in which the number of granular materials having a major axis 1 mm or more is 0 to 2 per 1 m2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a substrate for a liquid filter and a liquid filter. [Background technology]

[0002] Liquid compositions used in semiconductor lithography processes are filtered through a liquid filter before use in order to remove minute foreign matter from the liquid composition. The liquid filter contains a filter medium such as a pleated dense porous membrane or a bundle of hollow fibers. Conventionally, polyolefin microporous membranes have been known as porous membranes used as filter media for liquid filters. Patent Documents 1 to 7 disclose liquid filter substrates made of polyolefin microporous membranes with small pore sizes. Polyolefins do not contain halogen elements, and therefore liquid filters whose filter material is a polyolefin microporous membrane are advantageous in that there are fewer restrictions on disposal after use and that they impose a small burden on the environment. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2014 / 181760 [Patent Document 2] International Publication No. 2014 / 181761 [Patent Document 3] International Publication No. 2014 / 181762 [Patent Document 4] JP 2014-217800 A [Patent Document 5] JP 2014-218563 A [Patent Document 6] JP 2018-167198 A [Patent Document 7] International Publication No. 2020 / 022321 Summary of the Invention [Problem to be solved by the invention]

[0004] In general, the filter medium of a liquid filter is washed after manufacture and before use in order to remove fine powder generated during manufacture of the liquid filter and dust particles in the air from the filter medium and to prevent these foreign substances from being mixed into the liquid to be treated by the liquid filter. In addition, when the filter medium is washed, trace amounts of metals contained in the filter medium itself are dissolved and removed. The polyolefin microporous membrane may contain metals (calcium, zinc, etc., derived from the polyolefin polymerization catalyst or additives after polymerization (e.g., metal soap)) that are brought in by the polyolefin, which is the raw material for production, and these metals are dissolved and removed from the polyolefin microporous membrane when the filter medium is washed. Since there is a concern that the metals contained in the filter material may dissolve into the liquid composition used in the lithography process when the liquid composition is filtered, thereby reducing the semiconductor manufacturing yield, it is desirable to remove the metals from the filter material before use.

[0005] However, as semiconductor wiring patterns become finer and denser, there is an increasing need to remove even very small foreign matter (e.g., microparticles with a particle size of several nm) from liquid compositions used in lithography processes, which has led to a demand for liquid filters with denser filter media. However, the denser the filter medium, the lower the efficiency of cleaning the filter medium. In the case of a polyolefin microporous membrane, the smaller the pore size, the lower the efficiency of eluting and removing metals contained in the polyolefin microporous membrane during cleaning of the filter medium.

[0006] Furthermore, the densification of the microporous polyolefin membrane also makes it difficult to dissolve and remove metals due to the following mechanism. Generally, the densification of polyolefin microporous membrane is realized by using ultra-high molecular weight polyolefin as raw material.Therefore, it is considered that the molecular weight of ultra-high molecular weight polyolefin is increased as a method for making polyolefin microporous membrane more dense.However, ultra-high molecular weight polyolefin with a larger molecular weight does not melt completely during melt kneading, and may generate granular material made of polyolefin in polyolefin microporous membrane.The metal contained in raw material polyolefin remains in this granular material, and the metal inside the granular material is difficult to dissolve during cleaning of filter medium.

[0007] For the above reasons, it has been difficult to simultaneously densify the microporous polyolefin membrane and remove the residual metal.

[0008] It is against the above background that the present disclosure has been made. An object of the present disclosure is to provide a substrate for liquid filters that has a relatively small pore size but is easy to clean to remove residual metals. [Means for solving the problem]

[0009] Specific means for solving the above problems include the following aspects. <1> The number of particles with a pore size of 1 nm to 35 nm and a long diameter of 1 mm or more is 1 m 2 and a polyolefin microporous membrane having 0 to 2 microporous membranes per unit area. Substrate for liquid filters. <2> The polyolefin microporous membrane has a thickness of 3 μm to 20 μm. <1> The liquid filter substrate according to claim 1, <3> The porosity of the polyolefin microporous membrane is 35% to 70%. <1> or <2> The liquid filter substrate according to claim 1, <4> The water flow rate of the polyolefin microporous membrane is 0.003 L / min / ft 2 / psi~0.180L / min / ft 2 / psi, <1> ~ <3> 13. A liquid filter substrate according to claim 12, wherein the substrate is a substrate for a liquid filter. <5> The weight average molecular weight of the entire polyolefin constituting the polyolefin microporous membrane is 800,000 or more. <1> ~ <4> 13. A liquid filter substrate according to claim 12, wherein the substrate is a substrate for a liquid filter. <6> The polyolefin microporous membrane is a polyethylene microporous membrane; <1> ~ <5> 13. A liquid filter substrate according to claim 12, wherein the substrate is a substrate for a liquid filter. <7> <1> ~ <6> A liquid filter comprising the liquid filter substrate according to any one of the above items. Effect of the Invention

[0010] According to the present disclosure, a substrate for liquid filters is provided that has a relatively small pore size and yet is easy to clean to remove residual metals. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiments, and are not intended to limit the scope of the embodiments.

[0012] In the present disclosure, a numerical range indicated using "~" indicates a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.

[0013] In the present disclosure, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved.

[0014] In the present disclosure, when referring to the amount of each component in a composition, in cases where multiple substances corresponding to each component are present in the composition, unless otherwise specified, it means the total amount of those multiple substances present in the composition. In the present disclosure, the particles corresponding to each component may include multiple types. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified.

[0015] In this disclosure, MD (Machine Direction) means the longitudinal direction of a polyolefin microporous membrane produced in a long shape, and TD (Transverse Direction) means the direction perpendicular to MD in the plane direction of the polyolefin microporous membrane. In this disclosure, TD is also referred to as "width direction."

[0016] In the present disclosure, when the stacking relationship of each layer constituting a liquid filter or a substrate for liquid filters is expressed as "upper" and "lower," the layer closer to the polyolefin microporous membrane is referred to as "lower," and the layer farther from the polyolefin microporous membrane is referred to as "upper."

[0017] In this disclosure, the volume of a microporous membrane or a porous layer excluding pores is referred to as the "solids volume."

[0018] <Liquid filter substrate> The liquid filter substrate of the present disclosure has a microporous polyolefin membrane. The substrate for liquid filters of the present disclosure may be a substrate consisting of only a polyolefin microporous membrane, or a substrate in which a polyolefin microporous membrane is laminated with another porous membrane or porous layer. The substrate for liquid filters of the present disclosure may have one polyolefin microporous membrane, or may have two or more polyolefin microporous membranes (i.e., two or more polyolefin microporous membranes may be overlapped).

[0019] An example of an embodiment of the liquid filter substrate of the present disclosure is a substrate consisting of only a polyolefin microporous membrane. One example of an embodiment of the substrate for liquid filters of the present disclosure is a substrate having a single layer structure consisting of only one microporous polyolefin membrane.

[0020] The polyolefin microporous film of the liquid filter substrate of the present disclosure has a pore size of 1 nm to 35 nm, and the number of particulates with a major axis of 1 mm or more per m 2 There are 0 to 2 pieces per piece. The substrate for liquid filters of the present disclosure has a pore size of 1 nm to 35 nm in the polyolefin microporous membrane, and is therefore capable of filtering out fine particles (eg, particles with a particle size of 5 nm) contained in the liquid to be treated. The liquid filter substrate of the present disclosure is a polyolefin microporous membrane having a microporous membrane in which the number of particles having a major axis of 1 mm or more is 1 m 2 By having 0 to 2 particles per particle, even if residual metal is contained, the residual metal can be easily removed by washing.

[0021] The granules with a major axis of 1 mm or more that exist in the polyolefin microporous membrane are presumably polyolefins that did not completely melt during melt-kneading of the raw polyolefin. These granules contain residual metals that were contained in the raw polyolefin, and the metals inside the granules are not easily eluted during cleaning of the filter medium. The number of particles with a major axis of 1 mm or more present in a polyolefin microporous membrane is 1 m 2 If the number of particles per unit area is 0 to 2, even if metal is contained in the polyolefin microporous membrane, it can be easily removed by washing.

[0022] The polyolefin microporous membrane of the liquid filter substrate of the present disclosure will be described in detail below.

[0023] [Polyolefin microporous membrane] A polyolefin microporous membrane refers to a membrane in which fibril-like polyolefin forms a three-dimensional network structure, has numerous micropores inside, and has a structure in which the micropores are connected, allowing gas or liquid to pass from one side to the other.

[0024] In the microporous polyolefin membrane, the polyolefin preferably accounts for 90% by mass or more of the microporous polyolefin membrane, more preferably 95% by mass or more, and even more preferably 99% by mass or more. The polyolefin microporous membrane may contain a surfactant or the like to the extent that it does not affect the effects of the present disclosure.

[0025] The polyolefin microporous membrane may be hydrophobic or hydrophilic. Since polyolefin is a hydrophobic resin, the polyolefin microporous membrane itself is hydrophobic. The polyolefin microporous membrane may be a hydrophobic polyolefin microporous membrane that has not been subjected to hydrophilization treatment, or may be a polyolefin microporous membrane that has been given hydrophilicity by hydrophilization treatment.

[0026] Examples of treatment methods for hydrophilizing a polyolefin microporous membrane include physical hydrophilization treatments (plasma treatment, corona discharge treatment, ultraviolet irradiation, electron beam irradiation, etc.), coating treatments with surfactants or hydrophilic materials (cellulose, polyvinyl alcohol, etc.), and graft polymerization of hydrophilic monomers.

[0027] [Pore diameter] The pore size of the microporous polyolefin membrane is 1 nm to 35 nm. A polyolefin microporous membrane having a pore size of 1 nm or more can provide sufficient liquid permeability. From this viewpoint, the pore size of the polyolefin microporous membrane is preferably 5 nm or more, more preferably 10 nm or more, further preferably 11 nm or more, and particularly preferably 13 nm or more. The pore size of the polyolefin microporous membrane is 35 nm or less, so that microparticles (e.g., particles with a particle size of 5 nm) contained in the liquid to be treated can be filtered out. From this viewpoint, the pore size of the polyolefin microporous membrane is preferably 34 nm or less, more preferably 32 nm or less, further preferably 25 nm or less, and particularly preferably 22 nm or less.

[0028] The pore size of the polyolefin microporous membrane is a flow pore size measured by the half-dry method specified in ASTM E1294-89. The flow pore size is measured using a perm porometer (PMI, Capillary Flow Porometer, model: CFP-1500A) and a fluorine-based inert liquid (product name: Fluorinert, surface tension 16.0 dyn / cm) as an immersion liquid. The measurement temperature is 25°C, and the measurement pressure is changed in the range of 0 psi to 500 psi. The flow pore size is measured at a total of five points along the TD of the polyolefin microporous membrane: the center, two points 50 mm away from the center toward both ends, and two points 100 mm away from the center toward both ends, and the average value is the pore size of the polyolefin microporous membrane.

[0029] [Number of granules with major axis of 1 mm or more] From the viewpoint of easy removal of residual metals by washing, the polyolefin microporous membrane is designed to have granules with a major axis of 1 mm or more per 1 m 2 No more than 2 pieces per 1m 2 Preferably no more than one per 1m 2 0 per unit is more preferred.

[0030] The number of particulate matter having a major axis of 1 mm or more present in a polyolefin microporous membrane is determined by the following measurement method. A microporous polyolefin membrane with an area of ​​1 m 2 Remove any attached matter (fine powder generated during the production of the polyolefin microporous membrane, dust in the air, etc. that is not integrated with the polyolefin microporous membrane) from both sides. A flashlight is applied to one side of the polyolefin microporous membrane, and the side being irradiated with the flashlight is visually viewed from directly above in a plan view. Particles with a major axis length of 1 mm or more when viewed in a plan view of the polyolefin microporous membrane are found, and the number of such particles is visually counted. Since the fibers constituting the polyolefin microporous membrane are on the order of nanometers in thickness, particles with a major axis length of 1 mm or more when viewed in a plan view can be easily found if they exist. Area 1m 2 Repeat the measurement five times and average the five measurements.

[0031] [Film thickness] From the viewpoint of obtaining mechanical strength and durability, the thickness of the polyolefin microporous membrane is preferably 3 μm or more, more preferably 4 μm or more, further preferably 5 μm or more, and particularly preferably 6 μm or more. The thickness of the polyolefin microporous membrane is preferably 20 μm or less, more preferably 18 μm or less, even more preferably 16 μm or less, even more preferably 15 μm or less, and particularly preferably 14 μm or less, from the viewpoints of obtaining sufficient liquid permeability, relatively small filtration pressure, ability to increase the filtration area by pleating or the like, and ease of processing to increase the filtration area.

[0032] The thickness of the polyolefin microporous membrane is determined by measuring 10 points with a contact thickness meter and averaging the measurements. The measurement points are set at 10 equally spaced points along TD from near one end to near the other end.

[0033] [Porosity] The porosity of the polyolefin microporous membrane is preferably 35% or more, more preferably 38% or more, even more preferably 40% or more, and particularly preferably 42% or more, from the viewpoints of obtaining sufficient liquid permeability and relatively small filtration pressure. From the viewpoint of obtaining mechanical strength and durability, the porosity of the polyolefin microporous membrane is preferably 70% or less, more preferably 66% or less, even more preferably 60% or less, even more preferably 57% or less, and particularly preferably 55% or less.

[0034] The porosity ε (%) of the polyolefin microporous membrane is calculated by the following formula. ε(%)={1-Ws / (ds·t)}×100 Ws: basis weight of polyolefin microporous membrane (g / m 2 ): Cut out a polyolefin microporous membrane into pieces measuring 10 cm MD x 10 cm TD from three locations in total, the center and both ends, measure the mass, and divide the mass by the area. Calculate the average value of the center and both ends, and call this Ws. ds: True density of the polyolefin microporous membrane (g / cm 3 ): 0.96. t: thickness of the polyolefin microporous membrane (μm): determined as described above.

[0035] [Water flow rate] The water flow rate of the polyolefin microporous membrane is set to 0.003 L / min / ft in order to ensure sufficient liquid permeability over a long period of time. 2 / psi or more is preferred, 0.004L / min / ft 2 / psi or more is preferable, and 0.005L / min / ft 2 / psi or more is more preferable, and 0.013L / min / ft 2 / psi or more is particularly preferred. The water flow rate of the polyolefin microporous membrane is set to 0.180 L / min / ft from the viewpoint of obtaining the collection performance of fine particles (e.g., particles with a diameter of 5 nm). 2 / psi or less is preferred, with 0.150L / min / ft 2 / psi or less is more preferable, and 0.100L / min / ft 2 / psi or less is more preferable, and 0.090 L / min / ft 2 / psi or less is particularly preferred.

[0036] The water flow rate of the polyolefin microporous membrane is determined by the following measurement method. The polyolefin microporous membrane is cut into 40 mm x 40 mm squares from three locations in total, namely, the center and both ends of the TD, and then immersed in ethanol and dried at room temperature. The polyolefin microporous membrane is placed in a 37 mm diameter liquid permeation cell (liquid permeation area 10.75 cm2). 2 ) and pass 100 ml of pure water through it at a temperature of 24°C and a differential pressure of 90 kPa. The time Tl (min) required for the entire amount of pure water to pass through is measured. The volume of pure water V (100 ml), the time Tl (min), and the liquid permeation area S (10.75 cm 2 ) and the water flow rate Vs (unit time (min) under 1 psi differential pressure) × unit area (ft 2 ) and is expressed in L / min / ft 2 / psi) is calculated. In addition, the average value near the center and both ends of the TD is calculated. Vs=(V / 1000) / Tl / (S / 929.03) / (90 / 6.895)

[0037] [Heat shrinkage rate] The heat shrinkage rate of the polyolefin microporous membrane at a temperature of 105° C. in MD is preferably 45% or less, more preferably 40% or less, and even more preferably 30% or less, from the viewpoint of heat resistance. The heat shrinkage rate of the polyolefin microporous membrane at a temperature of 105° C. is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less in TD, from the viewpoint of heat resistance.

[0038] The heat shrinkage rate of the polyolefin microporous membrane is determined by the following measurement method. The polyolefin microporous membrane is cut into a size of 10 cm MD x 10 cm TD from three locations in total, the center and near both ends of the TD. The sample is placed in an oven with an internal temperature of 105°C for 30 minutes. The sample is removed from the oven and the MD and TD lengths of the sample are measured. The heat shrinkage rates (%) of MD and TD are calculated as follows: (length before heat treatment - length after heat treatment) ÷ length before heat treatment x 100). Furthermore, the average value of the center and near both ends of the TD is calculated.

[0039] [Polyolefin] Examples of polyolefins constituting the polyolefin microporous membrane include homopolymers of ethylene, propylene, butylene, methylpentene, etc. (ie, polyethylene, polypropylene, polybutylene, polymethylpentene, etc.), copolymers, and mixtures thereof.

[0040] The polyolefin microporous membrane is preferably a microporous membrane formed using two or more polyolefins that differ from each other in at least one of the types of monomers, polymerization degree, branching degree, crystallinity, stretchability, and molecular orientation. By using two or more polyolefins, a network structure is easily formed in the polyolefin microporous membrane by fibrillation during stretching.

[0041] The weight average molecular weight of all the polyolefins constituting the polyolefin microporous membrane is preferably 800,000 or more, more preferably 850,000 or more, even more preferably 900,000 or more, even more preferably 950,000 or more, and particularly preferably 970,000 or more, from the viewpoint of densifying the polyolefin microporous membrane. The weight average molecular weight of the entire polyolefin constituting the polyolefin microporous membrane is preferably 3.5 million or less, more preferably 3.2 million or less, even more preferably 3.1 million or less, and particularly preferably 3 million or less, from the viewpoint of ease of uniform melting during melt-kneading.

[0042] The weight average molecular weight of the entire polyolefin constituting the microporous polyolefin membrane is determined by dissolving the microporous polyolefin membrane in o-dichlorobenzene under heating, and measuring the molecular weight by gel permeation chromatography (system: Alliance GPC 2000 manufactured by Waters, columns: GMH6-HT and GMH6-HTL) under conditions of a column temperature of 135°C and a flow rate of 1.0 mL / min. Molecular weight monodisperse polystyrene (Tosoh Corporation) is used for molecular weight calibration.

[0043] The polyolefin constituting the polyolefin microporous membrane is preferably polyethylene. That is, the polyolefin microporous membrane is preferably a polyethylene microporous membrane. In the present disclosure, the polyethylene microporous membrane refers to a microporous membrane in which the resin that accounts for the largest proportion by mass of all the resins is polyethylene.

[0044] In the polyethylene microporous membrane, polyethylene preferably accounts for 90% by mass or more of the polyethylene microporous membrane, more preferably 95% by mass or more, and even more preferably 99% by mass or more. The polyethylene microporous membrane may contain a surfactant or the like to the extent that it does not affect the effects of the present disclosure.

[0045] The polyethylene microporous membrane is preferably a microporous membrane formed using two or more types of polyethylene that differ from each other in at least one of degree of polymerization, degree of branching, crystallinity, stretchability, and molecular orientation. By using two or more types of polyethylene, a network structure is easily formed in the polyethylene microporous membrane by fibrillation during stretching.

[0046] Examples of polyethylene constituting the microporous polyethylene membrane include ultra-high molecular weight polyethylene, high density polyethylene, and a mixture of ultra-high molecular weight polyethylene and high density polyethylene.

[0047] From the viewpoint of densifying the polyethylene microporous membrane, the polyethylene microporous membrane preferably contains ultra-high molecular weight polyethylene having a weight-average molecular weight of 3 million to 6 million. The polyethylene microporous membrane preferably contains 50% to 95% by mass, more preferably 60% to 90% by mass, and even more preferably 70% to 85% by mass of ultra-high molecular weight polyethylene having a weight-average molecular weight of 3 million to 6 million.

[0048] The polyethylene microporous membrane is made of ultra-high molecular weight polyethylene with a weight average molecular weight of 3 million to 6 million, and polyethylene with a weight average molecular weight of 200,000 to 800,000 and a density of 0.92 g / cm. 3 ~0.98g / cm 3 The mass ratio of the two polyethylenes in the polyethylene microporous membrane (ultra-high molecular weight polyethylene:high density polyethylene) is preferably 50:50 to 95:5, more preferably 60:40 to 90:10, and even more preferably 70:30 to 85:15, from the viewpoint of reducing particulate matter having a major axis of 1 mm or more in the polyethylene microporous membrane and from the viewpoint of producing a microporous membrane with a small pore size.

[0049] The weight average molecular weight of the whole polyethylene constituting the polyethylene microporous membrane is preferably 800,000 or more, more preferably 850,000 or more, even more preferably 900,000 or more, even more preferably 950,000 or more, and particularly preferably 970,000 or more, in order to densify the polyethylene microporous membrane. The weight average molecular weight of the entire polyethylene constituting the polyethylene microporous membrane is preferably 3.5 million or less, more preferably 3.2 million or less, even more preferably 3.1 million or less, and particularly preferably 3 million or less, from the viewpoint of ease of uniform melting during melt-kneading.

[0050] The calcium content in the polyolefin constituting the polyolefin microporous membrane varies depending on the raw material polyolefin, but is preferably within the following range, for example. In one embodiment, the calcium content in the polyolefin is preferably 50 ppm or less, more preferably 38 ppm or less, even more preferably 35 ppm or less, and particularly preferably 34 ppm or less. In one embodiment, the calcium content in the polyolefin is preferably 1000 ppb or less, more preferably 500 ppb or less, even more preferably 400 ppb or less, and particularly preferably 300 ppb or less. The calcium content in the polyolefin is, for example, 0 ppb or more, 10 ppb or more, 20 ppb or more, 50 ppb or more, or 100 ppb or more. Methods for adjusting the calcium content in polyolefins include adjusting the amount of metal soap (such as calcium stearate) added to the polyolefin after polymerization, washing the polyolefin with an acid, and removing the polymerization catalyst remaining in the polyolefin by a deashing process.

[0051] The calcium content of polyolefins is determined by adding ultra-high purity nitric acid to the polyolefin, decomposing it using microwaves, and using this as a sample to quantify it using ICP-MS (inductively coupled plasma mass spectrometry, device name: Aglient7500cs, Agilent Technologies, Inc.).

[0052] [Method of producing polyolefin microporous membrane] The microporous polyolefin membrane can be produced, for example, by a production method including the following steps (1) to (6).

[0053] Step (1): A step of preparing a polyolefin solution containing a polyolefin and a solvent. Step (2): A step of melt-kneading a polyolefin solution, extruding the molten kneaded product through a die, and cooling and solidifying the extrudate to obtain a gel-like molded product. Step (3): A step of squeezing the solvent out of the gel-like molding. Step (4): A step of stretching the gel-like molding in at least one direction to obtain a polyolefin microporous membrane. Step (5): A step of washing the polyolefin microporous membrane to remove the solvent. Step (6): A step of annealing the polyolefin microporous membrane.

[0054] By controlling the conditions of steps (1), (2), and (4), it is possible to suppress the generation of particulate matter with a major axis of 1 mm or more (presumably unmelted raw material polyolefin). In addition, by controlling the conditions of steps (1) to (6), it is possible to adjust the thickness, pore size, porosity, water flow rate, etc. of the polyolefin microporous membrane.

[0055] -Process (1)- Step (1) is a step of preparing a polyolefin solution containing a polyolefin and a solvent.

[0056] The polyolefin used in step (1) may be one type or two or more types. The polyolefin preferably contains polyethylene, and is preferably a polyethylene having an ultra-high molecular weight of 3 million to 6 million and a polyethylene having a weight-average molecular weight of 200,000 to 800,000 and a density of 0.92 g / cm. 3 ~0.98g / cm 3 and high density polyethylene.

[0057] Polyolefins are generally traded in the form of granular pellets or powder. When a polyolefin powder is used in step (1), the particle size of the powder is preferably 1 μm to 1000 μm, more preferably 5 μm to 500 μm, and even more preferably 10 μm to 300 μm, from the viewpoint of uniformly melt-kneading the polyolefin in step (2). The particle size is the median diameter (d50) of the volume-based particle size distribution. The volume-based particle size distribution is determined by dry measurement using a laser diffraction particle size distribution measuring device (device name: Mastersizer 2000, Malvern Instruments).

[0058] The solvent used in step (1) is not limited as long as it can swell or dissolve polyolefin. Solvents are broadly classified into non-volatile solvents having a boiling point of 210° C. or higher at atmospheric pressure and volatile solvents having a boiling point of less than 210° C. at atmospheric pressure.

[0059] Examples of non-volatile solvents include liquid paraffin, paraffin oil, mineral oil, castor oil, etc. The non-volatile solvents may be used alone or in combination of two or more. As the non-volatile solvent, liquid paraffin is preferred.

[0060] Examples of the volatile solvent include tetralin, ethylene glycol, decaline (also known as decahydronaphthalene), toluene, xylene, diethyltriamine, ethylenediamine, dimethylsulfoxide, and hexane. The volatile solvent may be used alone or in combination of two or more. The volatile solvent is preferably decaline or xylene.

[0061] The solvent used in step (1) is preferably a mixed solvent of a non-volatile solvent and a volatile solvent, more preferably a mixed solvent of liquid paraffin and decalin or xylene, and even more preferably a mixed solvent of liquid paraffin and decalin. The mixing ratio of the non-volatile solvent to the volatile solvent (mass ratio, non-volatile solvent:volatile solvent) is preferably 99:1 to 60:40.

[0062] When two or more kinds of polyolefins are used, the order of mixing the materials when mixing the polyolefins and the solvent is not limited. For example, either of the following form (a) and form (b) may be used.

[0063] Form (a): Two or more kinds of polyolefins are mixed one by one in a solvent. Two or more kinds of solvents may be mixed in advance to prepare a mixed solvent, and the polyolefins may be mixed one by one in the mixed solvent. In this embodiment, each polyolefin may be added to the solvent in one batch or in multiple batches. Polyolefins having relatively large molecular weights are preferably added to the solvent in multiple batches. Two or more polyolefins may be added alternately to the solvent.

[0064] Mode (b): Two or more polyolefins are mixed to prepare a polyolefin composition, and the polyolefin composition is mixed with a solvent. Two or more solvents may be mixed in advance to prepare a mixed solvent, and the mixed solvent may be mixed with the polyolefin composition. In this embodiment, the polyolefin composition may be added to the solvent in its entirety at one time, or may be added to the solvent in several portions.

[0065] From the viewpoint of imparting a good balance between mechanical strength, liquid permeability, and microparticle collection performance to the polyolefin microporous membrane, the polyolefin concentration of the polyolefin solution is preferably 10% by mass to 40% by mass, more preferably 15% by mass to 35% by mass, and even more preferably 20% by mass to 30% by mass. When the polyolefin concentration in the polyolefin solution is 10% by mass or more, the mechanical strength of the microporous polyolefin membrane is ensured. When the polyolefin concentration in the polyolefin solution is 40% by mass or less, pores are likely to be formed in the microporous polyolefin membrane.

[0066] -Process (2)- Step (2) is a step of melt-kneading a polyolefin solution, extruding the melt-kneaded mixture through a die, and cooling and solidifying the extrudate to obtain a gel-like molded product. The gel-like molded product is preferably formed into a sheet shape.

[0067] The melt kneading of the polyolefin solution is preferably carried out using a kneading extruder. The kneading extruder is a device that applies pressure and heat to the material to be treated while continuously conveying the material. The structure of the kneading extruder is generally roughly divided into a material inlet, a barrel, and a die from upstream to downstream. A screw is provided inside the barrel. A heater for heating the inside of the barrel is provided around the barrel. The screw may be a single-screw type or a twin-screw type, and the twin-screw type is preferable.

[0068] From the viewpoint of sufficiently melting the polyolefin, the temperature of the polyolefin solution in the most downstream region inside the barrel is preferably MP+30°C to MP+150°C, more preferably MP+40°C to MP+140°C, and even more preferably MP+50°C to MP+130°C, where MP°C is the melting point of the polyolefin (when two or more polyolefins are used, MP°C is the highest melting point among those polyolefins).

[0069] The time required for the material to pass through the inside of the barrel is preferably 1 to 10 minutes, more preferably 1 minute 30 seconds to 8 minutes, and even more preferably 2 to 7 minutes. The passing time of the material to be treated can be controlled by the rotation speed of the screw.

[0070] From the viewpoint of improving the film formability of the polyolefin microporous membrane, the temperature of the molten kneaded material in the die is preferably MP+30°C to MP+120°C, more preferably MP+40°C to MP+110°C, and even more preferably MP+50°C to MP+100°C, where MP°C is the melting point of the polyolefin (when two or more polyolefins are used, the highest melting point among those polyolefins is taken as MP°C).

[0071] Methods for cooling the extrudate include, for example, immersing the extrudate in water or an organic solvent, and contacting the extrudate with a cooled metal roll. The cooling temperature is preferably 10° C. to 40° C. When immersing the extrudate in water, it is preferable to create a water flow on the surface layer of the water bath to prevent the solvent released from the extrudate from adhering to the extrudate.

[0072] -Process (3)- The step (3) is a step of squeezing the solvent out of the gel-like molding. The step (3) is preferably realized by applying pressure to the gel-like molded product. For example, the method of applying pressure to the gel-like molded product may include conveying the gel-like molded product while pressing it against a roller or a belt, or passing the gel-like molded product between a pair of rollers. The pressure to which the gel-like molded product is subjected is preferably 0.01 MPa to 0.5 MPa, more preferably 0.05 MPa to 0.2 MPa. The surface temperature of the roller or belt is preferably 40°C to 100°C.

[0073] Between steps (2) and (3), it is preferable to heat-treat the gel-like molding for the purpose of volatilizing a part of the solvent from the gel-like molding. The heat-treating temperature is preferably 50°C to 100°C. The heat-treating may be performed once or may be performed two or more times at different temperatures. The heat-treating time is preferably 5 minutes to 10 minutes per time. By carrying out the above heat treatment in advance, it is possible to shorten the transport path in step (3) and to make the conditions (pressure and / or temperature) in step (3) milder.

[0074] -Process (4)- The step (4) is a step of stretching the gel-like molding in at least one direction to obtain a microporous polyolefin membrane.

[0075] The stretching in step (4) is preferably biaxial stretching. The biaxial stretching may be either sequential biaxial stretching in which longitudinal stretching and transverse stretching are performed separately, or simultaneous biaxial stretching in which longitudinal stretching and transverse stretching are performed simultaneously. The biaxial stretching may be performed by stretching multiple times in the longitudinal direction and then stretching in the transverse direction, stretching in the longitudinal direction and then stretching multiple times in the transverse direction, or sequential biaxial stretching followed by further stretching once or multiple times in the longitudinal direction and / or transverse direction.

[0076] The stretching ratio (the product of the longitudinal stretching ratio and the transverse stretching ratio) is preferably 40 to 240 times, more preferably 45 to 150 times, and even more preferably 50 to 120 times, from the viewpoint of imparting a good balance between liquid permeability and microparticle collection performance to the polyolefin microporous membrane.

[0077] The stretching temperature is preferably 80°C to 130°C, more preferably 90°C to 125°C, and even more preferably 100°C to 120°C, from the viewpoint of suppressing the generation of particulate matter made of polyolefin.

[0078] It is preferable to carry out a heat setting treatment after the stretching. The heat setting temperature is preferably 100°C to 140°C, more preferably 105°C to 130°C, and even more preferably 110°C to 120°C.

[0079] -Process (5)- Step (5) is a step of washing the polyolefin microporous membrane to remove the solvent. In step (5), the polyolefin microporous membrane is preferably washed with a solvent such as a halogenated hydrocarbon such as methylene chloride or a hydrocarbon such as hexane.

[0080] The cleaning of the polyolefin microporous membrane is preferably carried out by immersing the polyolefin microporous membrane in a bath containing a cleaning solvent. In this case, in order to enhance the cleaning effect, it is preferable to divide the bath into two or more tanks and make the purity of the cleaning solvent higher in the downstream tank. This can be achieved by pouring the cleaning solvent into the most downstream tank and flowing the cleaning solvent toward the upstream. When the bath is divided into two or more tanks, it may be two tanks or three or more tanks. From the viewpoint of making the purity gradient of the cleaning solvent in each tank more gentle, three or more tanks are preferable. The time required for the polyolefin microporous membrane to pass through the entire bath is preferably 60 to 150 seconds, more preferably 70 to 120 seconds, and even more preferably 80 to 100 seconds.

[0081] After the polyolefin microporous membrane is removed from the bath containing the cleaning solvent, the cleaning solvent is preferably removed by drying at a temperature slightly higher than the boiling point of the cleaning solvent.

[0082] -Process (6)- Step (6) is a step of annealing the polyolefin microporous membrane. The annealing is performed, for example, by conveying the polyolefin microporous membrane on rollers having a surface temperature of 100° C. to 130° C. or through a thermostatic bath having a temperature of 100° C. to 130° C. During the annealing, it is preferable to perform an operation of fixing the polyolefin microporous membrane in the width direction in order to suppress shrinkage of the polyolefin microporous membrane in the width direction.

[0083] Furthermore, the polyolefin microporous membrane may be subjected to a treatment to impart affinity to the liquid to be treated by the liquid filter.

[0084] <Liquid filter> The liquid filter of the present disclosure is a device for removing microparticles from a liquid to be treated that contains or may contain such particles in a solid or gel form.

[0085] The liquid filter of the present disclosure comprises the liquid filter substrate of the present disclosure as a filter medium. In general, the filter medium of a liquid filter is washed after its manufacture and before its use, but in the liquid filter substrate of the present disclosure, even if residual metals are contained, the residual metals can be easily removed by washing. Therefore, in the liquid filter of the present disclosure, if the filter medium is washed before use, there is little concern that metals will be eluted into the liquid to be treated when the liquid to be treated is filtered.

[0086] The liquid filter of the present disclosure includes, for example, a pleated liquid filter substrate and a cylindrical housing, and the pleated liquid filter substrate is housed inside the housing. The liquid filter of the present disclosure is, for example, a cartridge that is detachable from a filtration device.

[0087] The liquid filter of the present disclosure is suitable for removing microparticles having a particle size of about several nm from a liquid to be treated. The liquid filter of the present disclosure can be used, for example, in the manufacturing process of semiconductors and displays. EXAMPLES

[0088] The liquid filter substrate of the present disclosure will be described in more detail below with reference to examples. The materials, amounts, ratios, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the liquid filter substrate of the present disclosure should not be interpreted as being limited by the specific examples shown below.

[0089] In the following description, syntheses, treatments, manufactures, etc. were carried out at room temperature (25° C.±3° C.) unless otherwise specified.

[0090] <Measurement and evaluation methods> In all of the Examples and Comparative Examples, a polyolefin microporous membrane with a width of 270 mm was produced by winding it around a winding core with an inner diameter of 3 inches. Samples cut to appropriate dimensions from the produced polyolefin microporous membranes were subjected to physical property measurement or performance evaluation. The methods for measuring physical properties and evaluating performance were as follows.

[0091] [Calcium content of polyolefin] 0.1 g of polyolefin was weighed out into a fluororesin container, and ultra-high purity nitric acid was added and decomposed by microwave. The calcium (Ca) content was quantified in the order of ppb or ppm by ICP-MS (inductively coupled plasma mass spectrometry, Aglient7500cs, Agilent Technologies, Inc.).

[0092] [Polyolefin powder particle size] The volumetric particle size distribution of the polyolefin powder was determined by dry measurement using a laser diffraction particle size distribution analyzer (Mastersizer 2000, Malvern Instruments), and the median diameter (d50) was taken as the particle size.

[0093] [Polyolefin microporous membrane thickness] Using a contact-type thickness meter (Mitutoyo Corporation) and a cylindrical contact tip with a bottom diameter of 0.5 cm, the thickness (μm) of the polyolefin microporous membrane was measured at 10 points with 26 mm intervals on the TD of the membrane, and the measured values ​​were averaged. The measurement pressure of the contact tip was 0.1 N.

[0094] [Porosity of polyolefin microporous membrane] The porosity (ε) of the polyolefin microporous membrane was calculated from the following formula. ε(%)={1-Ws / (ds·t)}×100 Ws: basis weight of polyolefin microporous membrane (g / m 2 ): A polyolefin microporous membrane was cut into pieces measuring 10 cm MD x 10 cm TD from three locations in total, the center and both ends, and the mass was measured and divided by the area. The average value of the center and both ends was calculated and designated as Ws. ds: True density of the polyolefin microporous membrane (g / cm 3 ):0.96. t: thickness of the polyolefin microporous membrane (μm): measured as described above.

[0095] [Polyolefin microporous membrane pore size] The flow pore size was measured at five points along the TD of the polyolefin microporous membrane: the center, two points 50 mm away from the center toward both ends, and two points 100 mm away from the center toward both ends, and the measured values ​​were averaged. The flow pore size was measured as follows. Using a perm porometer (PMI, Capillary Flow Porometer, model: CFP-1500A) and a fluorine-based inert liquid (product name: Fluorinert, surface tension 16.0 dyn / cm) as the immersion liquid, the flow pore size was measured by the half-dry method specified in ASTM E1294-89. The measurement temperature was 25°C, and the measurement pressure was changed in the range of 0 psi to 500 psi, and the measurement was performed under the following conditions. Bubble point parameters: BUBLFLOW = 50, F / PT = 100, MINBPPRES = 0, ZEROTIME = 1, PULSEDELAY = 2 Wet parameters: V2INCR = 15, PREGINC = 0.9, MINEQTIME = 30, PRESSLEW = 30, FLOWSLEW = 30, EQITER = 50, AVEITER = 10, MAXPDIF = 1, MAXFDIF = 30 ·Dry parameters: V2INCR = 40, PREGINC = 2.4, MINEQTIME = 30, PRESSLEW = 30, FLOWSLEW = 30, EQITER = 40, AVEITER = 10, MAXPDIF = 1, MAXFDIF = 30

[0096] [Water flow rate of polyolefin microporous membrane] The polyolefin microporous membrane was cut into 40 mm x 40 mm squares from a total of three locations, namely, the center and both end portions of the TD, respectively, and immersed in ethanol and dried at room temperature. The polyolefin microporous membrane was placed in a stainless steel permeable cell with a diameter of 37 mm (permeable area: 10.75 cm). 2The polyolefin microporous membrane on the liquid permeation cell was moistened with a small amount (0.5 ml) of ethanol, and then 100 ml of pure water was passed through it at a room temperature of 24°C and a differential pressure of 90 kPa, and the time Tl (min) required for the entire amount of pure water to pass through was measured. The volume of pure water V (100 ml), time Tl (min), and permeable area S (10.75 cm 2 ) and the water flow rate Vs (unit time (min) under 1 psi differential pressure) × unit area (ft 2 ) and is expressed in L / min / ft 2 / psi) was calculated, and the average values ​​near the center and both ends of the TD were calculated. Vs=(V / 1000) / Tl / (S / 929.03) / (90 / 6.895)

[0097] [Polyolefin weight average molecular weight (Mw)] The polyolefin microporous membrane was dissolved in o-dichlorobenzene by heating, and the molecular weight was measured by gel permeation chromatography (system: Alliance GPC 2000 manufactured by Waters, columns: GMH6-HT and GMH6-HTL) at a column temperature of 135°C and a flow rate of 1.0 mL / min. Molecular weight monodisperse polystyrene (Tosoh Corporation) was used for molecular weight calibration.

[0098] [Number of granules] A polyolefin microporous membrane was placed on a 2 ) and any attached matter (fine powder generated during the production of the polyolefin microporous membrane, dust in the air, etc. that is not integrated with the polyolefin microporous membrane) was removed from both sides. A flashlight (product name: Cadnicalight) was applied to one side of the polyolefin microporous membrane, and the side being irradiated with the flashlight was visually observed from directly above. When the polyolefin microporous membrane was viewed in plan, granular objects with a major axis length of 1 mm or more were found and the number of such objects was visually counted. 2 The measurement was repeated five times and the five measurements were averaged.

[0099] [Collection performance] Gold colloid with a particle size of 5 nm (Funakoshi Co., Ltd., particle size range 4.5 to 6.0 nm) was dispersed in water to prepare a dispersion with a gold colloid concentration of 40 ppb. The polyolefin microporous membrane was cut into 50 mm x 50 mm squares from a total of three locations, namely, the center and both end portions of the TD, respectively, and immersed in ethanol and dried at room temperature. The polyolefin microporous membrane was placed in a stainless steel permeable cell with a diameter of 37 mm (permeable area: 10.75 cm 2 The polyolefin microporous membrane on the liquid permeation cell was moistened with a small amount (0.5 ml) of ethanol, and then 200 ml of the gold colloid dispersion was passed through the cell at a differential pressure of 0.1 MPa. The metal concentration of the colloidal gold dispersion after passing through the polyolefin microporous membrane was measured and quantified using ICP-OES (inductively coupled plasma optical emission spectroscopy, instrument name: Agilent-ICP-OES-5100, Agilent Technologies, Inc.). A calibration curve for quantification was created using standard colloidal gold dispersions (preparing five or more samples in the concentration range of 0 ppb to 100 ppb). The collection efficiency (%) = {(M1-M2)÷M1×100} was calculated from the initial metal concentration M1 (i.e., 40 ppb) of the colloidal gold dispersion and the metal concentration M2 of the colloidal gold dispersion after passing through the polyolefin microporous membrane. Furthermore, the average values ​​near the center and both ends of TD were calculated and classified as follows: A: The average capture rate is 90% or more. B: The average capture rate is less than 90% and more than 80% C: The average capture rate is less than 80%

[0100] [Metal elution] The deposits (fine powder generated during the production of the polyolefin microporous membrane and dust in the air, etc., which are not integrated with the polyolefin microporous membrane) were removed from both sides of the polyolefin microporous membrane. The polyolefin microporous membrane was cut into square pieces (10 cm x 10 cm, 40 pieces, total area 4000 cm). 2 ) and used as the sample. The sample was placed in a fluororesin container, and 200 g of hydrochloric acid extract (a liquid containing 10% hydrochloric acid by mass in a mixture of water and isopropyl alcohol = 40:60 (mass ratio)) was poured in to immerse the sample in the hydrochloric acid extract. After 24 hours, the sample was taken out and dried. The dried sample was placed in another fluororesin container, and 200 g of propylene glycol monomethyl ether (PGME) was poured into it to immerse the sample in PGME. After 24 and 168 hours, the Ca and Zn concentrations in the PGME were quantified to the order of 0.1 ppb using ICP-OES (inductively coupled plasma optical emission spectroscopy, Agilent-ICP-OES-5100, Agilent Technologies, Inc.). From the quantitatively determined Ca and Zn concentrations, the mass of PGME, and the sample area, the total amount of Ca and Zn eluted from the polyolefin microporous membrane (μg / m 2 The increase rate of the amount of dissolution (%) was calculated as follows: (total amount of dissolution after 168 hours - total amount of dissolution after 24 hours) / total amount of dissolution after 24 hours x 100) and classified as follows: A: The increase in the amount of elution is less than 5% B: The increase in the amount of elution is 5% or more and less than 10% C: Increase in amount of elution is 10% or more

[0101] [Product yield] A 270 mm wide polyolefin microporous membrane was produced by winding it around a winding core with an inner diameter of 3 inches to obtain a 200 m long roll of polyolefin microporous membrane. The surface of the roll was illuminated with a flashlight (product name: Cadnica Light) and visually observed from a distance of 30 cm from the surface, and the number of granular objects with a major axis of 2 mm or more present around one circumference of the roll was counted. A roll with 4 or fewer granular objects was deemed to be an acceptable product, and the number of acceptable products out of 10 rolls was classified as follows: A: 10 qualified products B: 9 or 8 qualified products C: 7 or less qualified products

[0102] <Manufacturing of substrates for liquid filters> Hereinafter, "UHMWPE" means ultra-high molecular weight polyethylene with a weight average molecular weight of 3 million to 6 million, and "HDPE" means polyethylene with a weight average molecular weight of 200,000 to 800,000 and a density of 0.92 g / cm 3 ~0.98g / cm 3 "High density polyethylene" means high density polyethylene of 1000 MPa.

[0103] [Example 1] -Process (1)- ·UHMWPE with Mw 4.6 million and Ca content 140 ppb: 22 parts by mass (UHMWPE powder particle size 60μm) HDPE with Mw 500,000 and Ca content 230 ppb: 5 parts by weight (HDPE powder particle size 250μm) Liquid paraffin: 73 parts by weight The above materials were prepared. 11 parts by mass of UHMWPE was added to liquid paraffin and mixed by stirring. Next, the entire amount of HDPE was added and mixed by stirring. Next, 11 parts by mass of UHMWPE was added and mixed by stirring. In this way, a polyethylene solution with a polyethylene concentration of 27% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 157 ppb.

[0104] -Process (2)- The polyethylene solution was fed into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating at a screw rotation speed of 300 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 200°C, and the polyethylene solution temperature at the die was adjusted so that it was 210°C. The polyethylene solution was extruded through a die into a sheet, and the extrudate was transported to a water bath at 20° C. and cooled to prepare a gel-like sheet base tape.

[0105] -Process (3)- The base tape was removed from the water bath and transported through a space at a temperature of 60° C. for 10 minutes, and then transported through a space at a temperature of 95° C. for 10 minutes. (If decalin was used in step (1), this transport process removes the decalin from the base tape.) The base tape was then conveyed over a roller having a surface temperature of 90° C. while being pressed at 0.05 MPa, to remove a portion of the liquid paraffin from the base tape.

[0106] -Process (4)- The base tape was stretched 7 times in MD at a temperature of 110°C (longitudinal stretching), then stretched 21 times in TD at a temperature of 115°C (transverse stretching), and then immediately heat-set at a temperature of 120°C to obtain a polyolefin microporous membrane.

[0107] -Process (5)- The polyolefin microporous membrane was immersed in three separate methylene chloride baths (referred to as tank 1, tank 2, and tank 3 from the upstream side) for 30 seconds each, and liquid paraffin was extracted from the polyolefin microporous membrane. Methylene chloride was poured into tank 3, and then allowed to flow from tank 3 to tank 1, forming a gradient in the purity of methylene chloride (tank 1 < tank 2 < tank 3). The polyolefin microporous membrane was removed from the methylene chloride bath and transported through a space at a temperature of 40° C. to remove the methylene chloride from the polyolefin microporous membrane.

[0108] -Process (6)- The polyolefin microporous membrane was annealed by conveying it through a thermostatic bath at 110° C. for 1 minute while keeping the TD length constant. The microporous polyolefin membrane was then transported through a space at 60° C. for 20 seconds, and then transported into a space at room temperature to be cooled.

[0109] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.

[0110] [Example 2] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that step (4) was changed as follows.

[0111] -Process (4)- The base tape was stretched 9 times in MD at a temperature of 115°C (longitudinal stretching), then stretched 26 times in TD at a temperature of 115°C (transverse stretching), and then immediately heat-set at a temperature of 120°C to obtain a polyolefin microporous membrane.

[0112] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.

[0113] [Example 3] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that steps (1), (2), and (4) were changed as follows.

[0114] -Process (1)- ·UHMWPE with Mw 4.6 million and Ca content 140 ppb: 18 parts by mass (UHMWPE powder particle size 60μm) HDPE with Mw 500,000 and Ca content 230 ppb: 5 parts by weight (HDPE powder particle size 250μm) Liquid paraffin: 76 parts by weight ·Decalin: 1 part by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. 9 parts by mass of UHMWPE were added to the mixed solvent and stirred and mixed. Next, the entire amount of HDPE was added and stirred and mixed. Next, 9 parts by mass of UHMWPE were added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 23% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 160 ppb.

[0115] -Process (2)- The polyethylene solution was fed into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating at a screw rotation speed of 450 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 180°C, and the polyethylene solution temperature at the die was adjusted so that it was 170°C. The polyethylene solution was extruded through a die into a sheet, and the extrudate was transported to a water bath at 20° C. and cooled to prepare a gel-like sheet base tape.

[0116] -Process (4)- The base tape was stretched 5 times in MD at a temperature of 115°C (longitudinal stretching), then stretched 15 times in TD at a temperature of 105°C (transverse stretching), and then immediately heat-set at a temperature of 115°C to obtain a polyolefin microporous membrane.

[0117] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.

[0118] [Example 4] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that steps (1), (2), and (4) were changed as follows.

[0119] -Process (1)- ·UHMWPE with Mw 4.6 million and Ca content 140 ppb: 12 parts by mass (UHMWPE powder particle size 60μm) HDPE with Mw 500,000 and Ca content 230 ppb: 5 parts by weight (HDPE powder particle size 250μm) Liquid paraffin: 53 parts by weight ·Decalin: 30 parts by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. 6 parts by mass of UHMWPE were added to the mixed solvent and stirred and mixed. Next, the entire amount of HDPE was added and stirred and mixed. Next, 6 parts by mass of UHMWPE were added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 17% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 166 ppb.

[0120] -Process (2)- The polyethylene solution was fed into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating at a screw rotation speed of 400 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 190°C, and the polyethylene solution temperature at the die was adjusted so that it was 175°C. The polyethylene solution was extruded through a die into a sheet, and the extrudate was transported to a water bath at 20° C. and cooled to prepare a gel-like sheet base tape.

[0121] -Process (4)- The base tape was stretched 10 times in MD at a temperature of 90°C (longitudinal stretching), then stretched 10 times in TD at a temperature of 105°C (transverse stretching), and then immediately heat-set at a temperature of 130°C to obtain a polyolefin microporous membrane.

[0122] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.

[0123] [Example 5] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that steps (1), (2), (4), and (6) were changed as follows.

[0124] -Process (1)- -UHMWPE with Mw 4.2 million and Ca content 31 ppm: 6 parts by mass (UHMWPE powder particle size 30μm) HDPE with Mw 400,000 and Ca content 34 ppm: 24 parts by mass (HDPE powder particle size 20μm) Liquid paraffin: 67 parts by weight ·Decalin: 3 parts by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. The entire amount of UHMWPE was added to the mixed solvent and stirred and mixed. Next, the entire amount of HDPE was added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 30 mass% was prepared. The Ca content in the mixture of UHMWPE and HDPE was 33.4 ppm.

[0125] -Process (2)- The polyethylene solution was fed into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating at a screw rotation speed of 200 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 180°C, and the polyethylene solution temperature at the die was adjusted so that it was 170°C. The polyethylene solution was extruded through a die into a sheet, and the extrudate was transported to a water bath at 20° C. and cooled to prepare a gel-like sheet base tape.

[0126] -Process (4)- The base tape was stretched 5 times in MD at a temperature of 90°C (longitudinal stretching), then stretched 15 times in TD at a temperature of 110°C (transverse stretching), and then immediately heat-set at a temperature of 120°C to obtain a polyolefin microporous membrane.

[0127] -Process (6)- The polyolefin microporous membrane was annealed by conveying it through a thermostatic bath at 105° C. for 1 minute while keeping the TD length constant. The microporous polyolefin membrane was then transported through a space at 60° C. for 20 seconds, and then transported into a space at room temperature to be cooled.

[0128] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.

[0129] [Example 6] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that steps (1) and (4) were changed as follows.

[0130] -Process (1)- -UHMWPE with Mw 4.2 million and Ca content 31 ppm: 5 parts by mass (UHMWPE powder particle size 30μm) HDPE with Mw 400,000 and Ca content 34 ppm: 25 parts by weight (HDPE powder particle size 20μm) Liquid paraffin: 70 parts by weight The above materials were prepared. 12 parts by mass of HDPE was added to liquid paraffin and mixed by stirring. Next, the entire amount of UHMWPE was added and mixed by stirring. Next, 13 parts by mass of HDPE was added and mixed by stirring. In this way, a polyethylene solution with a polyethylene concentration of 30% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 33.5 ppm.

[0131] -Process (4)- The base tape was stretched 5 times in MD at a temperature of 90°C (longitudinal stretching), then stretched 13 times in TD at a temperature of 115°C (transverse stretching), and then immediately heat-set at a temperature of 125°C to obtain a polyolefin microporous membrane.

[0132] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.

[0133] [Example 7] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that steps (1), (4), and (6) were changed as follows.

[0134] -Process (1)- ·UHMWPE with Mw 4.6 million and Ca content 140 ppb: 4 parts by mass (UHMWPE powder particle size 60μm) HDPE with Mw 500,000 and Ca content 230 ppb: 16 parts by weight (HDPE powder particle size 250μm) Liquid paraffin: 80 parts by weight The above materials were prepared. The entire amount of UHMWPE was added to liquid paraffin and mixed by stirring. Next, the entire amount of HDPE was added and mixed by stirring. In this way, a polyethylene solution with a polyethylene concentration of 20 mass% was prepared. The Ca content in the mixture of UHMWPE and HDPE was 212 ppb.

[0135] -Process (4)- The base tape was stretched 6 times in MD at a temperature of 110°C (longitudinal stretching), then stretched 20 times in TD at a temperature of 115°C (transverse stretching), and then immediately heat-set at a temperature of 122°C to obtain a polyolefin microporous membrane.

[0136] -Process (6)- The polyolefin microporous membrane was annealed by conveying it through a thermostatic bath at 115° C. for 1 minute while keeping the TD length constant. The microporous polyolefin membrane was then transported through a space at 60° C. for 20 seconds, and then transported into a space at room temperature to be cooled.

[0137] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane (liquid filter substrate of the present disclosure) are shown in Table 1.

[0138] [Comparative Example 1] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that steps (2) and (4) were changed as follows.

[0139] -Process (2)- The polyethylene solution was fed into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating at a screw rotation speed of 200 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 160°C, and the polyethylene solution temperature at the die was adjusted so that it was 165°C. The polyethylene solution was extruded through a die into a sheet, and the extrudate was transported to a water bath at 20° C. and cooled to prepare a gel-like sheet base tape.

[0140] -Process (4)- The base tape was stretched 9 times in MD at a temperature of 100°C (longitudinal stretching), then stretched 25 times in TD at a temperature of 105°C (transverse stretching), and then immediately heat-set at a temperature of 105°C to obtain a polyolefin microporous membrane.

[0141] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane are shown in Table 1.

[0142] [Comparative Example 2] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that steps (2) and (4) were changed as follows.

[0143] -Process (2)- The polyethylene solution was fed into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating at a screw rotation speed of 400 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 160°C, and the polyethylene solution temperature at the die was adjusted so that it was 165°C. The polyethylene solution was extruded through a die into a sheet, and the extrudate was transported to a water bath at 20° C. and cooled to prepare a gel-like sheet base tape.

[0144] -Process (4)- The base tape was stretched 9 times in MD at a temperature of 100°C (longitudinal stretching), then stretched 25 times in TD at a temperature of 115°C (transverse stretching), and then immediately heat-set at a temperature of 100°C to obtain a polyolefin microporous membrane.

[0145] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane are shown in Table 1.

[0146] [Comparative Example 3] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that steps (1) and (4) were changed as follows.

[0147] -Process (1)- ·UHMWPE with Mw 4.6 million and Ca content 140 ppb: 27 parts by mass (UHMWPE powder particle size 60μm) HDPE with Mw 500,000 and Ca content 230 ppb: 2 parts by mass (HDPE powder particle size 250μm) Liquid paraffin: 70 parts by weight ·Decalin: 1 part by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. The entire amount of UHMWPE was added to the mixed solvent and stirred and mixed. Next, the entire amount of HDPE was added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 29 mass% was prepared. The Ca content in the mixture of UHMWPE and HDPE was 146.2 ppb.

[0148] -Process (4)- The base tape was stretched 9 times in MD at a temperature of 105°C (longitudinal stretching), then stretched 25 times in TD at a temperature of 105°C (transverse stretching), and then immediately heat-set at a temperature of 108°C to obtain a polyolefin microporous membrane.

[0149] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane are shown in Table 1.

[0150] [Comparative Example 4] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that steps (1), (2), and (4) were changed as follows.

[0151] -Process (1)- UHMWPE with Mw 4.2 million and Ca content 31 ppm: 8 parts by mass (UHMWPE powder particle size 30μm) HDPE with Mw 400,000 and Ca content 34 ppm: 20 parts by mass (HDPE powder particle size 20μm) Liquid paraffin: 70 parts by weight ·Decalin: 2 parts by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. The entire amount of UHMWPE was added to the mixed solvent and stirred and mixed. Next, the entire amount of HDPE was added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 28 mass% was prepared. The Ca content in the mixture of UHMWPE and HDPE was 33.1 ppm.

[0152] -Process (2)- The polyethylene solution was fed into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating at a screw rotation speed of 400 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 165°C, and the polyethylene solution temperature at the die was adjusted so that it was 160°C. The polyethylene solution was extruded through a die into a sheet, and the extrudate was transported to a water bath at 20° C. and cooled to prepare a gel-like sheet base tape.

[0153] -Process (4)- The base tape was stretched 7 times in MD at a temperature of 90°C (longitudinal stretching), then stretched 16 times in TD at a temperature of 115°C (transverse stretching), and then immediately heat-set at a temperature of 128°C to obtain a polyolefin microporous membrane.

[0154] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane are shown in Table 1.

[0155] [Comparative Example 5] A microporous polyethylene membrane was produced in the same manner as in Example 1, except that steps (1), (2), (4), and (6) were changed as follows.

[0156] -Process (1)- ·UHMWPE with Mw 4.6 million and Ca content 140 ppb: 3 parts by mass (UHMWPE powder particle size 60μm) HDPE with Mw 500,000 and Ca content 230 ppb: 14 parts by weight (HDPE powder particle size 250μm) Liquid paraffin: 51 parts by weight ·Decalin: 32 parts by mass The above materials were prepared. Liquid paraffin and decalin were mixed to prepare a mixed solvent. The entire amount of UHMWPE was added to the mixed solvent and stirred and mixed. Next, the entire amount of HDPE was added and stirred and mixed. In this way, a polyethylene solution with a polyethylene concentration of 17% by mass was prepared. The Ca content in the mixture of UHMWPE and HDPE was 214.1 ppb.

[0157] -Process (2)- The polyethylene solution was fed into a twin-screw kneading extruder, and pressure and heat were applied to the polyethylene solution by operating at a screw rotation speed of 450 rpm. The temperature inside the barrel of the twin-screw kneading extruder was adjusted so that the polyethylene solution temperature in the most downstream region was 160°C, and the polyethylene solution temperature at the die was adjusted so that it was 155°C. The polyethylene solution was extruded through a die into a sheet, and the extrudate was transported to a water bath at 20° C. and cooled to prepare a gel-like sheet base tape.

[0158] -Process (4)- The base tape was stretched 4 times in MD at a temperature of 100°C (longitudinal stretching), then stretched 9 times in TD at a temperature of 115°C (transverse stretching), and then immediately heat-set at a temperature of 135°C to obtain a polyolefin microporous membrane.

[0159] -Process (6)- The polyolefin microporous membrane was annealed by conveying it through a thermostatic bath at 100° C. for 1 minute while keeping the TD length constant. The microporous polyolefin membrane was then transported through a space at 60° C. for 20 seconds, and then transported into a space at room temperature to be cooled.

[0160] The obtained polyethylene microporous membrane had a three-dimensional network structure of fibril polyolefin, numerous micropores inside, and a structure in which the micropores were connected, allowing gas or liquid to pass from one side to the other. The properties of this polyethylene microporous membrane are shown in Table 1.

[0161] [Table 1]

[0162] Comparative Example 5, in which the pore size of the polyolefin microporous membrane is 57 nm, is inferior in the evaluation item "collection performance". In contrast, Examples 1 to 7 (substrates for liquid filters of the present disclosure) in which the pore size of the polyolefin microporous membrane is 35 nm or less are excellent in the evaluation item "collection performance." That is, the substrate for liquid filters of the present disclosure is excellent in the performance of filtering out fine particles (e.g., particles with a particle size of 5 nm) contained in the liquid to be treated.

[0163] Comparative Examples 1 to 4, in which the number of granular objects having a major axis of 1 mm or more was 3 or more, were inferior in the evaluation item "metal elution." In contrast, Examples 1 to 7 (substrates for liquid filters of the present disclosure) in which the number of particulates with a major axis of 1 mm or more was 2 or less were excellent in the evaluation item "metal elution." That is, the substrate for liquid filters of the present disclosure has a relatively small pore size, but residual metals can be easily removed by washing.

[0164] All publications, patent applications, and standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or standard was specifically and individually indicated to be incorporated by reference.

Claims

1. The number of particles having a pore size of 1 nm to 35 nm and a major axis of 1 mm or more is 1 m 2 and a polyolefin microporous membrane having 0 to 2 microporous particles per unit area. Substrate for liquid filters.

2. The liquid filter substrate according to claim 1, wherein the polyolefin microporous membrane has a thickness of 3 μm to 20 μm.

3. The liquid filter substrate according to claim 1, wherein the polyolefin microporous membrane has a porosity of 35% to 70%.

4. The water flow rate of the polyolefin microporous membrane is 0.003 L / min / ft 2 / psi to 0.180L / min / ft 2 The liquid filter substrate according to claim 1 , wherein the pressure is 0.1 to 1.0 psi.

5. The liquid filter substrate according to claim 1 , wherein the weight average molecular weight of all the polyolefins constituting the polyolefin microporous membrane is 800,000 or more.

6. The liquid filter substrate according to claim 1 , wherein the polyolefin microporous membrane is a polyethylene microporous membrane.

7. A liquid filter comprising the liquid filter substrate according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Base material for liquid filter

    JP2014217800A

  • Base material for liquid filter

    JP2014218563A

  • Base material for liquid filter

    JP2018167198A

  • Liquid filter substrate

    WO2014181760A1

  • Liquid filter substrate

    WO2014181761A1