Nonaqueous electrolyte for battery, lithium secondary battery precursor, lithium secondary battery, and method for manufacturing lithium secondary battery
Patent Information
- Application Number
- JP2023052347
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
【0012】 本開示によれば、高温環境下で充放電が繰り返し行われても、電池容量の低下を抑制するとともに、常温及び低温での電池抵抗の上昇を抑制することができる電池用非水電解液、リチウム二次電池前駆体、リチウム二次電池及びリチウム二次電池の製造方法が提供される。
Smart Images

Figure 00000025_0000 
Figure 00000025_0001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a nonaqueous electrolyte for a battery, a lithium secondary battery precursor, a lithium secondary battery, and a method for producing a lithium secondary battery. [Background technology]
[0002] Lithium secondary batteries have been attracting attention as batteries with high energy density. Patent Document 1 discloses a non-aqueous electrolyte battery (hereinafter also referred to as "lithium secondary battery"). The lithium secondary battery disclosed in Patent Document 1 includes a positive electrode and a negative electrode capable of absorbing and releasing metal ions, and a non-aqueous electrolyte (hereinafter also referred to as "non-aqueous electrolyte"). The non-aqueous electrolyte contains an electrolyte, a non-aqueous solvent, and a specific compound. The specific compound is at least one selected from the group consisting of lithium fluorosulfonate, lithium bis(fluorosulfonyl)imide, and lithium difluorophosphate. The negative electrode has a negative electrode active material. The negative electrode active material contains Si or Si metal oxide and graphite particles. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2021-106174 A Summary of the Invention [Problem to be solved by the invention]
[0004] The capacity of a lithium secondary battery may decrease when it is repeatedly charged and / or discharged (hereinafter, also referred to as "charge and discharge"). Therefore, there is a demand for a nonaqueous electrolyte for a battery that can suppress the decrease in battery capacity even when the lithium secondary battery is repeatedly charged and discharged in a high-temperature environment.
[0005] Lithium secondary batteries are sometimes used not only in warm regions (e.g., 25°C) but also in cold regions (e.g., -10°C). In cold regions, the battery performance of lithium secondary batteries may be degraded. Therefore, there is a demand for a nonaqueous electrolyte for batteries that can suppress an increase in battery resistance at room temperature (e.g., 25°C) and low temperature (e.g., -10°C) even when the lithium secondary batteries are repeatedly charged and discharged in a high-temperature environment.
[0006] In view of the above circumstances, an object of the present disclosure is to provide a nonaqueous electrolyte for a battery, a nonaqueous electrolyte for a battery, a lithium secondary battery precursor, a lithium secondary battery, and a method for manufacturing a lithium secondary battery, which are capable of suppressing a decrease in battery capacity and suppressing an increase in battery resistance at room temperature and low temperature even when charging and discharging are repeatedly performed in a high-temperature environment. [Means for solving the problem]
[0007] Means for solving the above problems include the following aspects. <1> It is used in lithium secondary batteries that contain Si elements as the negative electrode active material, A non-aqueous electrolyte for a battery, comprising a compound (I) represented by the following formula (I):
[0008] [ka]
[0009] [In formula (I), L is a single bond or -O-; R 11 is a hydrocarbon group having 1 to 10 carbon atoms (at least one hydrogen atom in the hydrocarbon group may be substituted with a halogen atom), and at least one carbon atom of the hydrocarbon group may be substituted with an oxygen atom, a nitrogen atom, a sulfur atom, or a sulfonyl group. <2> Further comprising compound (A), The compound (A) is at least one selected from the group consisting of a compound (II) represented by the following formula (II), a compound (III) represented by the following formula (III), a compound (IV) represented by the following formula (IV), and a compound (V) which is at least one selected from the group consisting of lithium monofluorophosphate and lithium difluorophosphate. The above <1> The non-aqueous electrolyte for a battery according to claim 1.
[0010] [ka]
[0011] [In formula (II), R 21 ~R 24 each independently represents a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 3 carbon atoms, or a fluorohydrocarbon group having 1 to 3 carbon atoms. 21 ~R 24 cannot all be hydrogen atoms. In formula (III), R 31 ~R 32 each independently represents a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 3 carbon atoms, or a fluorohydrocarbon group having 1 to 3 carbon atoms. In formula (IV), R 41 represents an alkylene group having 1 to 6 carbon atoms, an alkenylene group having 2 to 6 carbon atoms, a group represented by formula (iv-1), or a group represented by formula (iv-2), * indicates the bond position. In formula (iv-1), R 42 represents an oxygen atom, an alkylene group having 1 to 6 carbon atoms, an alkenylene group having 2 to 6 carbon atoms, or an oxymethylene group, In formula (ii-2), R 43 represents an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms. <3> The compound (A) contains at least the compound (II). <2> The non-aqueous electrolyte for a battery according to claim 1. <4> The content of the compound (A) is 0.01% by mass to 10.0% by mass based on the total amount of the nonaqueous electrolyte for a battery. <2> or <3> The non-aqueous electrolyte for a battery according to claim 1. <5> The content of the compound (I) is 0.01% by mass to 5.0% by mass based on the total amount of the nonaqueous electrolyte for a battery. <1> ~ <4> 13. The nonaqueous electrolyte for a battery according to claim 12, <6> Case and a positive electrode, a negative electrode, a separator, and an electrolyte solution contained in the case; Equipped with the positive electrode comprises a positive electrode active material including lithium metal phosphate; the negative electrode comprises a negative electrode active material containing Si element, The electrolyte solution is <1> ~ <5> The nonaqueous electrolyte for a battery according to any one of the above items. Lithium secondary battery precursor. <7> The above <6> A lithium secondary battery obtained by charging and discharging the lithium secondary battery precursor described in claim 1. <8> The negative electrode active material further contains a graphite material. <7> The lithium secondary battery precursor according to claim 1. <9> The above <6> preparing a lithium secondary battery precursor according to the present invention; Charging and discharging the lithium secondary battery precursor; A method for producing a lithium secondary battery, comprising:
[0012] The present disclosure provides a nonaqueous electrolyte for a battery, a lithium secondary battery precursor, a lithium secondary battery, and a method for manufacturing a lithium secondary battery, which are capable of suppressing a decrease in battery capacity and suppressing an increase in battery resistance at room temperature and low temperature even when charging and discharging are repeatedly performed in a high-temperature environment. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a laminate type battery, which is an example of a lithium secondary battery precursor according to the present disclosure. [Diagram 2]FIG. 2 is a schematic cross-sectional view showing a coin-type battery, which is another example of a lithium secondary battery precursor according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, the amount of each component in a composition means, when a plurality of substances corresponding to each component are present in the composition, the total amount of the plurality of substances present in the composition, unless otherwise specified.
[0015] (Nonaqueous electrolyte for batteries) The nonaqueous electrolyte for batteries (hereinafter also referred to as "nonaqueous electrolyte") of the present disclosure is used in lithium secondary batteries containing Si element as a negative electrode active material, and contains a compound (I) represented by the following formula (I) (hereinafter also referred to as "fluorine-containing sulfonyl compound (I)").
[0016] [ka]
[0017] In formula (I), L is a single bond or -O-. 11 is a hydrocarbon group having 1 to 10 carbon atoms (at least one hydrogen atom in the hydrocarbon group may be substituted with a halogen atom), and at least one carbon atom of the hydrocarbon group may be substituted with an oxygen atom, a nitrogen atom, a sulfur atom, or a sulfonyl group.
[0018] Since the nonaqueous electrolyte of the present disclosure has the above-mentioned configuration, it is possible to suppress the decrease in battery capacity even when the lithium secondary battery is repeatedly charged and discharged in a high-temperature environment. In addition, the nonaqueous electrolyte of the present disclosure can suppress the increase in battery resistance at room temperature and low temperature even when the lithium secondary battery is repeatedly charged and discharged in a high-temperature environment. This effect is believed to be due to, but not limited to, the following reasons. The fluorine-containing sulfonyl compound (I) contained in the nonaqueous electrolyte solution of the present disclosure is reductively decomposed on the Si element. This is believed to result in the formation of a solid electrolyte interphase (SEI) film (hereinafter also referred to as "SEI film") with excellent mechanical flexibility on the Si element. Furthermore, it is believed that an SEI film is also formed on the surface of the positive electrode by charging and discharging the lithium secondary battery. Hereinafter, the SEI film of the negative electrode and the SEI film of the positive electrode are also simply referred to as "SEI film". The SEI film is considered to be formed mainly by lithium ions in the non-aqueous electrolyte and decomposition products of the non-aqueous electrolyte that are decomposed during charging and discharging of the lithium secondary battery. It is believed that when the SEI film is formed, side reactions that are not the normal battery reactions are less likely to proceed during the charge / discharge cycle of the lithium secondary battery. The battery reaction is a reaction in which lithium ions enter and leave (intercalate) the positive and negative electrodes. Side reactions include the reductive decomposition reaction of the non-aqueous electrolyte by the negative electrode, the oxidative decomposition reaction of the non-aqueous electrolyte by the positive electrode, and the elution of metal elements in the positive electrode active material. Therefore, in the present disclosure, even if the negative electrode active material contains Si element, it is considered that the progression of side reactions during charging and discharging is suppressed. As a result, it is presumed that the nonaqueous electrolyte of the present disclosure can suppress the decrease in battery capacity and the increase in battery resistance at room temperature and low temperature.
[0019] The non-aqueous electrolyte for batteries of the present disclosure is used in lithium secondary batteries containing elemental Si as a negative electrode active material. The lithium secondary batteries will be described in detail later.
[0020] <Fluorine-containing sulfonyl compound (I)> The non-aqueous electrolyte solution of the present disclosure contains a fluorine-containing sulfonyl compound (I) represented by the following formula (I): The non-aqueous electrolyte solution may contain one type of fluorine-containing sulfonyl compound (I) alone, or may contain two or more types.
[0021] [ka]
[0022] In formula (I), L is a single bond or -O-. 11 represents a hydrocarbon group having 1 to 10 carbon atoms which may be substituted with a halogen atom (at least one hydrogen atom in the hydrocarbon group may be substituted with a halogen atom), and at least one carbon atom of the hydrocarbon group may be substituted with an oxygen atom, a nitrogen atom, a sulfur atom, or a sulfonyl group.
[0023] R 11 Examples of the hydrocarbon group having 1 to 10 carbon atoms represented by the formula (I) include an aliphatic group having 1 to 10 carbon atoms (at least one hydrogen atom in the aliphatic group may be substituted with a halogen atom), and an aryl group having 6 to 10 carbon atoms (at least one hydrogen atom in the aryl group may be substituted with a halogen atom).
[0024] R 11 is preferably a group represented by an alkyl group having 1 to 4 carbon atoms (at least one hydrogen atom in the alkyl group may be substituted with a halogen atom), an alkenyl group having 2 to 4 carbon atoms (at least one hydrogen atom in the alkenyl group may be substituted with a halogen atom), an alkynyl group having 2 to 4 carbon atoms (at least one hydrogen atom in the alkynyl group may be substituted with a halogen atom), or an aryl group (at least one hydrogen atom in the aryl group may be substituted with a halogen atom, an alkoxy group having 1 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms). This makes it possible for the nonaqueous electrolyte to further suppress the decrease in battery capacity and the increase in battery resistance at normal and low temperatures.
[0025] In formula (I), R 11 The "alkyl group having 1 to 4 carbon atoms" represented by the formula (I) is preferably a straight-chain or branched-chain alkyl group having 1 to 4 carbon atoms. Examples of the "alkyl group having 1 to 4 carbon atoms" include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, and the like. Among these, the "alkyl group having 1 to 4 carbon atoms" is more preferably an alkyl group having 1 to 3 carbon atoms.
[0026] In formula (I), R 11 The "alkenyl group having 2 to 4 carbon atoms" represented by the formula (I) is preferably a straight-chain or branched-chain alkenyl group having 2 to 4 carbon atoms. Examples of the "alkenyl group having 2 to 4 carbon atoms" include a vinyl group, a 2-propenyl group, a 2-butenyl group, and a 3-butenyl group. Among these, the "alkenyl group having 2 to 4 carbon atoms" is more preferably an alkenyl group having 2 to 3 carbon atoms.
[0027] In formula (I), R 11 The "alkynyl group having 2 to 4 carbon atoms" represented by the formula (I) is preferably a straight-chain or branched-chain alkynyl group having 2 to 4 carbon atoms. Examples of the "alkynyl group having 2 to 4 carbon atoms" include an ethynyl group, a propargyl group (2-propynyl group), a 2-butynyl group, and a 3-butynyl group. Among these, the "alkynyl group having 2 to 4 carbon atoms" is more preferably an alkynyl group having 2 to 3 carbon atoms.
[0028] At least one hydrogen atom in the "hydrocarbon group having 1 to 10 carbon atoms" may be substituted with a halogen atom. The halogen atom in the "hydrocarbon group having 1 to 10 carbon atoms" is preferably a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom, more preferably a fluorine atom, a chlorine atom, or a bromine atom, further preferably a fluorine atom or a chlorine atom, and particularly preferably a fluorine atom. In the "hydrocarbon group having 1 to 10 carbon atoms", the number of hydrogen atoms substituted with halogen atoms is not particularly limited and is appropriately selected depending on the number of carbon atoms in the alkyl group, with 1 to 7 being preferred.
[0029] Among them, R in formula (I) 11 is preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a vinyl group, an allyl group, an ethynyl group, a phenyl group, or a 4-fluorophenyl group. This makes it possible for the nonaqueous electrolyte to further suppress a decrease in battery capacity and an increase in battery resistance at room temperature and low temperature.
[0030] Specific examples of the fluorine-containing sulfonyl compound (I) include compounds represented by the following formulae (I-1) to (I-2). Hereinafter, the compound represented by formula (I-1) will also be referred to as "fluorine-containing sulfonyl compound (I-1)," and the compound represented by formula (I-2) will also be referred to as "fluorine-containing sulfonyl compound (I-2)." In the fluorine-containing sulfonyl compound (I-1), in formula (I), L is a single bond, R 11 In the fluorine-containing sulfonyl compound (I-2), in formula (I), L is a single bond and R 11 is an ethyl group.
[0031] [ka]
[0032] The fluorine-containing sulfonyl compound (I) preferably contains a fluorine-containing sulfonyl compound (I-1) or a fluorine-containing sulfonyl compound (I-2), more preferably contains a fluorine-containing sulfonyl compound (I-1), and even more preferably is a fluorine-containing sulfonyl compound (I-1). When the fluorine-containing sulfonyl compound (I) contains a fluorine-containing sulfonyl compound (I-1) or a fluorine-containing sulfonyl compound (I-2), the non-aqueous electrolyte can further suppress the decrease in battery capacity and the increase in battery resistance at room temperature and low temperature. When the fluorine-containing sulfonyl compound (I) contains a fluorine-containing sulfonyl compound (I-1), the resistance increase rate at room temperature and low temperature can be further suppressed than when the non-aqueous electrolyte contains a compound (I-2). When the fluorine-containing sulfonyl compound (I) is a fluorine-containing sulfonyl compound (I-1), the non-aqueous electrolyte can further suppress the resistance increase rate at room temperature and low temperature.
[0033] The content of the fluorine-containing sulfonyl compound (I) is not particularly limited, and is preferably 0.01% by mass to 5.0% by mass based on the total amount of the nonaqueous electrolyte, which allows the nonaqueous electrolyte to suppress a decrease in battery capacity and an increase in battery resistance at normal and low temperatures, compared to when the content of the fluorine-containing sulfonyl compound (I) is outside the range of 0.01% by mass to 5.0% by mass. The content of the fluorine-containing sulfonyl compound (I) is more preferably 0.05% by mass to 3.0% by mass, and further preferably 0.1% by mass to 2.0% by mass, from the viewpoints of suppressing a decrease in battery capacity and an increase in battery resistance at normal and low temperatures.
[0034] <Compound (A)> The non-aqueous electrolyte preferably further contains a compound (A). The compound (A) is at least one selected from the group consisting of a compound (II) represented by the following formula (II) (hereinafter also referred to as "cyclic carbonate compound (II)"), a compound (III) represented by the following formula (III) (hereinafter also referred to as "cyclic carbonate compound (III)"), a compound (IV) represented by the following formula (IV) (hereinafter also referred to as "cyclic sulfate compound (IV)"), and a compound (V) (hereinafter referred to as "lithium fluorophosphate compound (V)") which is at least one selected from the group consisting of lithium monofluorophosphate and lithium difluorophosphate.
[0035] [ka]
[0036] [In formula (II), R 21 ~R 24 each independently represents a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 3 carbon atoms, or a fluorohydrocarbon group having 1 to 3 carbon atoms. 21 ~R 24 cannot all be hydrogen atoms. In formula (III), R 31 ~R 32each independently represents a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 3 carbon atoms, or a fluorohydrocarbon group having 1 to 3 carbon atoms. In formula (IV), R 41 represents an alkylene group having 1 to 6 carbon atoms, an alkenylene group having 2 to 6 carbon atoms, a group represented by formula (iv-1), or a group represented by formula (iv-2), * indicates the bond position. In formula (iv-1), R 42 represents an oxygen atom, an alkylene group having 1 to 6 carbon atoms, an alkenylene group having 2 to 6 carbon atoms, or an oxymethylene group, In formula (ii-2), R 43 represents an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms.
[0037] By containing the compound (A) in addition to the fluorine-containing sulfonyl compound (I), the nonaqueous electrolyte can further suppress the decrease in battery capacity and the increase in battery resistance at room temperature and low temperature.
[0038] The compound (A) preferably contains at least the compound (II), which enables the non-aqueous electrolyte to further suppress a decrease in battery capacity and an increase in battery resistance at room temperature and low temperature.
[0039] The compound (A) preferably contains a cyclic sulfate compound (IV), which allows the non-aqueous electrolyte to suppress a decrease in battery capacity and an increase in battery resistance at room temperature and low temperature in a well-balanced manner.
[0040] The compound (A) is preferably a lithium fluorophosphate compound (V), which enables the non-aqueous electrolyte to particularly suppress a decrease in battery capacity and an increase in battery resistance at room temperature and low temperature.
[0041] When the non-aqueous electrolyte contains the compound (A), the content of the compound (A) is preferably in the following range. The content of compound (A) is preferably 0.01% by mass to 10.0% by mass based on the total amount of the nonaqueous electrolyte for a battery, which enables the nonaqueous electrolyte to further suppress a decrease in battery capacity and an increase in battery resistance at room temperature and low temperature. The content of compound (A) is more preferably 0.01 mass% to 5.0 mass%, particularly preferably 0.03 mass% to 4.5 mass%, even more preferably 0.05 mass% to 4.0 mass%, still more preferably 0.10 mass% to 3.0 mass%, and even more preferably 0.2 to 2.0 mass%. When the content of the compound (A) relative to the total amount of the nonaqueous electrolyte for a battery is within the above range, the nonaqueous electrolyte can further suppress the decrease in battery capacity.
[0042] The total content of compound (I) and compound (A) is preferably 10.0% by mass or less, more preferably 5.0% by mass or less, and even more preferably less than 4.5% by mass. When the total content of compound (I) and compound (A) is within the above range, the nonaqueous electrolyte can suppress the decrease in battery capacity even when charging and discharging are repeated in a high-temperature environment, compared to when the total content of compound (I) and compound (A) is not within the above range.
[0043] From the viewpoint of more effectively obtaining the effects of the nonaqueous electrolyte solution of the present disclosure, the ratio of the content of compound (I) to the content of compound (A) in the nonaqueous electrolyte solution of the present disclosure is preferably 0.05 to 5.0, more preferably 0.05 to 1.5, even more preferably 0.05 or more and less than 1.0, particularly preferably 0.05 or more and less than 0.5, and even more preferably 0.05 to 0.3.
[0044] From the viewpoint of more effectively obtaining the effects of the nonaqueous electrolyte solution of the present disclosure, the ratio of the content of compound (I) to the total content of compound (I) and compound (A) in the nonaqueous electrolyte solution of the present disclosure is preferably 0.05 to 3.0, more preferably 0.05 to 1.0, even more preferably 0.05 to 0.5, particularly preferably 0.05 or more and less than 0.5, and even more preferably 0.05 to 0.3.
[0045] (Cyclic carbonate compound (II)) The non-aqueous electrolyte preferably contains a cyclic carbonate compound (II) represented by the following formula (II).
[0046] [ka]
[0047] In formula (II), R 21 ~R 24 each independently represents a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 3 carbon atoms, or a fluorohydrocarbon group having 1 to 3 carbon atoms. 21 ~R 24 cannot all be hydrogen atoms.
[0048] By further containing a cyclic carbonate compound (II) in addition to the fluorine-containing sulfonyl compound (I), the nonaqueous electrolyte can further suppress a decrease in battery capacity and an increase in battery resistance at room temperature and low temperature. This effect is presumably due to the following reasons. During charging and discharging of a lithium secondary battery, the cyclic carbonate compound (II) is easily reductively decomposed by the negative electrode before the non-aqueous electrolyte is reductively decomposed on the negative electrode, forming an SEI film. This suppresses the decomposition of the non-aqueous electrolyte at the negative electrode. As a result, the non-aqueous electrolyte can further suppress the decrease in battery capacity and the increase in battery resistance at room temperature and low temperature.
[0049] R 21 ~R 24 Examples of the hydrocarbon group having 1 to 3 carbon atoms represented by the formula (I) include an aliphatic group having 1 to 3 carbon atoms. 21 ~R 22Examples of the hydrocarbon group having 1 to 3 carbon atoms represented by the formula (I) include an alkyl group having 1 to 3 carbon atoms (e.g., a methyl group, an ethyl group, a propyl group, an isopropyl group), an alkenyl group having 2 to 3 carbon atoms (e.g., a vinyl group, a 2-propenyl group), and an alkynyl group having 2 to 3 carbon atoms (e.g., an ethynyl group, a propargyl group (2-propynyl group)). At least one hydrogen atom in the "hydrocarbon group having 1 to 3 carbon atoms" may be substituted with a halogen atom. The halogen atom in the "hydrocarbon group having 1 to 3 carbon atoms" is preferably a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom, more preferably a fluorine atom, a chlorine atom, or a bromine atom, further preferably a fluorine atom or a chlorine atom, and particularly preferably a fluorine atom. In the "hydrocarbon group having 1 to 3 carbon atoms", the number of hydrogen atoms substituted with halogen atoms is not particularly limited and is appropriately selected depending on the number of carbon atoms in the alkyl group, with 1 to 7 being preferred.
[0050] Specific examples of the cyclic carbonate compound (II) include compounds represented by the following formulas (II-1) to (II-7).
[0051] [ka]
[0052] The non-aqueous electrolyte may contain only one type of cyclic carbonate compound (II), or may contain two or more types.
[0053] When the non-aqueous electrolyte contains a cyclic carbonate ester compound (II), the content of the cyclic carbonate ester compound (II) is preferably 0.10% by mass to 10.0% by mass, more preferably 0.20% by mass to 5.0% by mass, and even more preferably 0.30% by mass to 3.0% by mass, based on the total amount of the non-aqueous electrolyte. If the content of the cyclic carbonate ester compound (II) is within the above range, the increase in the thickness of the SEI film can be suppressed while suppressing the decomposition of the non-aqueous solvent on the positive electrode or the negative electrode, and an SEI film having a thickness capable of suppressing the decomposition of the non-aqueous solvent in the non-aqueous electrolyte is formed. As a result, the non-aqueous electrolyte can further suppress the decrease in battery capacity and the increase in battery resistance at room temperature and low temperature.
[0054] (Cyclic carbonate compound (III)) The non-aqueous electrolyte preferably contains a cyclic carbonate compound (III) represented by the following formula (III).
[0055] [ka]
[0056] In formula (III), R 31 ~R 32 each independently represents a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 3 carbon atoms, or a fluorohydrocarbon group having 1 to 3 carbon atoms.
[0057] By further containing a cyclic carbonate ester compound (III) in addition to the fluorine-containing sulfonyl compound (I), the nonaqueous electrolyte can further suppress a decrease in battery capacity and an increase in battery resistance at room temperature and low temperature. This effect is presumably due to the following reasons. During charging and discharging of a lithium secondary battery, the cyclic carbonate compound (III) is easily reductively decomposed by the negative electrode before the non-aqueous electrolyte is reductively decomposed on the negative electrode, forming an SEI film. This suppresses the decomposition of the non-aqueous electrolyte at the negative electrode. As a result, the non-aqueous electrolyte can further suppress the decrease in battery capacity and the increase in battery resistance at room temperature and low temperature.
[0058] R 31 ~R 32 Examples of the hydrocarbon group having 1 to 3 carbon atoms represented by the formula (I) include an aliphatic group having 1 to 3 carbon atoms. 31 ~R 32 Examples of the hydrocarbon group having 1 to 3 carbon atoms represented by the formula (I) include an alkyl group having 1 to 3 carbon atoms (e.g., a methyl group, an ethyl group, a propyl group, an isopropyl group), an alkenyl group having 2 to 3 carbon atoms (e.g., a vinyl group, a 2-propenyl group), and an alkynyl group having 2 to 3 carbon atoms (e.g., an ethynyl group, a propargyl group (2-propynyl group)). At least one hydrogen atom in the "hydrocarbon group having 1 to 3 carbon atoms" may be substituted with a halogen atom. The halogen atom in the "hydrocarbon group having 1 to 3 carbon atoms" is preferably a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom, more preferably a fluorine atom, a chlorine atom, or a bromine atom, further preferably a fluorine atom or a chlorine atom, and particularly preferably a fluorine atom. In the "hydrocarbon group having 1 to 3 carbon atoms", the number of hydrogen atoms substituted with halogen atoms is not particularly limited and is appropriately selected depending on the number of carbon atoms in the alkyl group, with 1 to 7 being preferred.
[0059] Specific examples of the cyclic carbonate compound (III) include compounds represented by the following formulas (III-1) to (III-7).
[0060] [ka]
[0061] The non-aqueous electrolyte may contain only one type of cyclic carbonate compound (III), or may contain two or more types.
[0062] When the non-aqueous electrolyte contains a cyclic carbonate compound (III), the content of the cyclic carbonate compound (III) is preferably 0.10% by mass to 5.0% by mass, more preferably 0.20% by mass to 5.0% by mass, even more preferably 0.30% by mass to 3.0% by mass, particularly preferably 0.30% by mass to 2.0% by mass, and even more preferably 0.30% by mass to 1.0% by mass, based on the total amount of the non-aqueous electrolyte. If the content of the cyclic carbonate compound (III) is within the above range, the increase in the thickness of the SEI film can be suppressed while suppressing the decomposition of the non-aqueous solvent on the positive electrode or the negative electrode, and an SEI film having a thickness capable of suppressing the decomposition of the non-aqueous solvent in the non-aqueous electrolyte is formed. As a result, the non-aqueous electrolyte can further suppress the decrease in battery capacity and the increase in battery resistance at room temperature and low temperature.
[0063] <Cyclic sulfate compounds (IV)> The non-aqueous electrolyte of the present disclosure contains a cyclic sulfate ester compound (IV) represented by the following formula (IV): The non-aqueous electrolyte may contain one type of cyclic sulfate ester compound (IV) alone, or may contain two or more types.
[0064] [ka]
[0065] In formula (IV), R 41 is an alkylene group having 1 to 6 carbon atoms, an alkenylene group having 2 to 6 carbon atoms, a group represented by formula (iv-1), or a group represented by formula (iv-2). * indicates a bonding position. In formula (iv-1), R 42 is an oxygen atom, an alkylene group having 1 to 6 carbon atoms, an alkenylene group having 2 to 6 carbon atoms, or an oxymethylene group. 43 is an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms.
[0066] In formula (IV), R 41 is preferably a group represented by formula (iv-1) or a group represented by formula (iv-2). In formula (iv-1), R 42is preferably an alkylene group having 1 to 3 carbon atoms, an alkenylene group having 1 to 3 carbon atoms, or an oxymethylene group, and more preferably an oxymethylene group. In formula (i-2), R 43 is preferably an alkyl group having 1 to 3 carbon atoms or an alkenyl group having 2 to 3 carbon atoms, and more preferably a propyl group.
[0067] Specific examples of the cyclic sulfate compound (IV) include the following compounds (IV-1) to (IV-7).
[0068] [ka]
[0069] When the non-aqueous electrolyte contains a cyclic sulfate ester compound (IV), the content of the cyclic sulfate ester compound (IV) is preferably 0.10% by mass to 5.0% by mass, more preferably 0.20% by mass to 5.0% by mass, even more preferably 0.30% by mass to 3.0% by mass, particularly preferably 0.30% by mass to 2.0% by mass, and even more preferably 0.30% by mass to 1.0% by mass, based on the total amount of the non-aqueous electrolyte. If the content of the cyclic sulfate ester compound (IV) is within the above range, the increase in the thickness of the SEI film can be suppressed while suppressing the decomposition of the non-aqueous solvent on the positive electrode or the negative electrode, and an SEI film having a thickness capable of suppressing the decomposition of the non-aqueous solvent in the non-aqueous electrolyte is formed. As a result, the non-aqueous electrolyte can further suppress the decrease in battery capacity and the increase in battery resistance at room temperature and low temperature.
[0070] <Lithium fluorophosphate compound(V)> The non-aqueous electrolyte preferably contains a lithium fluorophosphate compound (V). The lithium fluorophosphate compound (V) is at least one of lithium monofluorophosphate and lithium difluorophosphate. Lithium difluorophosphate is represented by the following formula (V-1), and lithium monofluorophosphate is represented by the following formula (V-2). Hereinafter, the compound represented by formula (V-1) is also referred to as "lithium fluorophosphate compound (V-1)". The compound represented by formula (V-2) is also referred to as "lithium fluorophosphate compound (V-2)".
[0071] [ka]
[0072] By containing the lithium fluorophosphate compound (V) in addition to the fluorine-containing sulfonyl compound (I), the nonaqueous electrolyte can further suppress the decrease in battery capacity and the increase in battery resistance at room temperature and low temperature.
[0073] The nonaqueous electrolyte may contain only one of lithium fluorophosphate (V-1) and lithium fluorophosphate (V-2), or may contain both lithium fluorophosphate (V-1) and lithium fluorophosphate (V-2).
[0074] When the non-aqueous electrolyte contains the lithium fluorophosphate compound (V), the content of the lithium fluorophosphate compound (V) is preferably 0.10 mass% to 5.0 mass%, more preferably 0.20 mass% to 5.0 mass%, even more preferably 0.30 mass% to 3.0 mass%, particularly preferably 0.30 mass% to 2.0 mass%, and even more preferably 0.30 mass% to 1.0 mass% based on the total amount of the non-aqueous electrolyte. If the content of the lithium fluorophosphate compound (V) is within the above range, the solubility of the lithium fluorophosphate compound (V) in the non-aqueous solvent can be ensured, and the direct current resistance of the lithium secondary battery can be further reduced.
[0075] <Other additives> The nonaqueous electrolyte of the present disclosure may contain other additives. The other additives are not particularly limited, and any known additives can be used. As other additives, for example, the additives described in paragraphs 0042 to 0055 of JP 2019-153443 A can be used.
[0076] <Non-aqueous solvent> The non-aqueous electrolyte generally contains a non-aqueous solvent. As the non-aqueous solvent, various known ones can be appropriately selected, and the non-aqueous solvent may be one kind or two or more kinds.
[0077] Examples of non-aqueous solvents include cyclic carbonates, chain carbonates, fluorine-containing chain carbonates, aliphatic carboxylate esters, fluorine-containing aliphatic carboxylate esters, γ-lactones, fluorine-containing γ-lactones, cyclic ethers, fluorine-containing cyclic ethers, chain ethers, fluorine-containing chain ethers, nitriles, amides, lactams, nitromethane, nitroethane, sulfolane, trimethyl phosphate, dimethyl sulfoxide, and dimethyl sulfoxide phosphate. Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC). Examples of chain carbonates include dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and dipropyl carbonate (DPC). Examples of aliphatic carboxylate esters include methyl formate, methyl acetate, methyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylbutyrate, ethyl formate, ethyl acetate, ethyl propionate, ethyl butyrate, ethyl isobutyrate, and ethyl trimethylbutyrate. Examples of γ-lactones include γ-butyrolactone and γ-valerolactone. Examples of cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, and 1,4-dioxane. Examples of chain ethers include 1,2-ethoxyethane (DEE), ethoxymethoxyethane (EME), diethyl ether, 1,2-dimethoxyethane, and 1,2-dibutoxyethane. Examples of nitriles include acetonitrile, glutaronitrile, adiponitrile, methoxyacetonitrile, and 3-methoxypropionitrile. The amides include, for example, N,N-dimethylformamide. Examples of lactams include N-methylpyrrolidinone, N-methyloxazolidinone, and N,N'-dimethylimidazolidinone.
[0078] The non-aqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates. In this case, the total proportion of cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates relative to the total amount of the non-aqueous solvent is preferably 50 mass% or more and 100 mass% or less, more preferably 60 mass% or more and 100 mass% or less, and even more preferably 80 mass% or more and 100 mass% or less.
[0079] The non-aqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates and chain carbonates. In this case, the total proportion of cyclic carbonates and chain carbonates in the non-aqueous solvent is preferably 50% by mass or more and 100% by mass or less, more preferably 60% by mass or more and 100% by mass or less, and even more preferably 80% by mass or more and 100% by mass or less, based on the total amount of the non-aqueous solvent.
[0080] The content of the non-aqueous solvent is preferably 60 mass % or more, and more preferably 70 mass % or more, based on the total amount of the non-aqueous electrolyte. The content of the non-aqueous solvent is preferably 99 mass % or less, more preferably 97 mass % or less, and further preferably 90 mass % or less, based on the total amount of the non-aqueous electrolyte.
[0081] <Electrolyte> The non-aqueous electrolyte generally contains an electrolyte.
[0082] The electrolyte preferably contains at least one of a fluorine-containing lithium salt (hereinafter sometimes referred to as a "fluorine-containing lithium salt") and a fluorine-free lithium salt.
[0083] Examples of the fluorine-containing lithium salt include inorganic acid anion salts and organic acid anion salts. Examples of inorganic acid anion salts include lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), and lithium hexafluorotantalate (LiTaF6). Examples of organic acid anion salts include lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethanesulfonyl)imide (Li(CF3SO2)2N), and lithium bis(pentafluoroethanesulfonyl)imide (Li(C2F5SO2)2N). Among them, lithium hexafluorophosphate (LiPF6) is more preferable as the fluorine-containing lithium salt.
[0084] Fluorine-free lithium salts include lithium perchlorate (LiClO4), lithium aluminium tetrachloride (LiAlCl4), and lithium decachlorodecaborate (Li2B 10 Cl 10 ) etc.
[0085] When the electrolyte contains a fluorine-containing lithium salt, the content of the fluorine-containing lithium salt is preferably 50 mass % or more and 100 mass % or less, more preferably 60 mass % or more and 100 mass % or less, and even more preferably 80 mass % or more and 100 mass % or less, based on the total amount of the electrolyte. When the fluorine-containing lithium salt contains lithium hexafluorophosphate (LiPF6), the content of lithium hexafluorophosphate (LiPF6) is preferably 50 mass% or more and 100 mass% or less, more preferably 60 mass% or more and 100 mass% or less, and even more preferably 80 mass% or more and 100 mass% or less, based on the total amount of the electrolyte.
[0086] When the non-aqueous electrolyte contains an electrolyte, the concentration of the electrolyte in the non-aqueous electrolyte is preferably 0.1 mol / L to 3 mol / L, more preferably 0.2 mol / L to 2 mol / L, and even more preferably 0.5 mol / L to 2 mol / L.
[0087] When the non-aqueous electrolyte contains lithium hexafluorophosphate (LiPF6), the concentration of lithium hexafluorophosphate (LiPF6) in the non-aqueous electrolyte is preferably 0.1 mol / L or more and 3 mol / L or less, more preferably 0.2 mol / L or more and 2 mol / L or less, and even more preferably 0.5 mol / L or more and 2 mol / L or less.
[0088] <Other ingredients> The non-aqueous electrolyte may contain other components as necessary, such as an acid anhydride.
[0089] [Lithium secondary battery precursor] The lithium secondary battery precursor of the present disclosure includes a case, a positive electrode, a negative electrode, a separator, and an electrolyte solution housed in the case. The positive electrode includes a positive electrode active material including lithium metal phosphate. The negative electrode includes a negative electrode active material including Si element. The electrolyte solution is the nonaqueous electrolyte solution for batteries of the present disclosure.
[0090] In the present disclosure, a lithium secondary battery precursor refers to a lithium secondary battery before being charged and discharged.
[0091] According to the lithium secondary battery precursor of the present disclosure, a lithium secondary battery that contains lithium iron phosphate as a positive electrode active material and has an excellent capacity retention rate during storage can be manufactured. Such an effect is brought about by the fluorine-containing sulfonyl compound (I) in the non-aqueous electrolyte.
[0092] <Case> The shape of the case and the like are not particularly limited, and are appropriately selected according to the use of the lithium secondary battery precursor of the present disclosure and the like. Examples of the case include a case containing a laminate film, a case composed of a battery can and a battery can lid, and the like.
[0093] <Positive electrode> The positive electrode contains a positive electrode active material containing lithium metal phosphate. Examples of the lithium metal phosphate include lithium iron phosphate (LiFePO4), lithium manganese phosphate (LiMnPO4), lithium manganese iron phosphate (LiMn x Fe 1-x PO4; 0 <x <1), lithium cobalt phosphate (LiCoPO4), lithium nickel phosphate (LiNiPO4), and the like.
[0094] The positive electrode active material preferably contains lithium iron phosphate.
[0095] The positive electrode active material may contain components other than lithium metal phosphate. Examples of the components other than lithium metal phosphate include; Transition metal oxides or transition metal sulfides such as MoS2, TiS2, MnO2, and V2O5; LiCoO2, LiMnO2, LiMn2O4, LiNiO2, LiNi X Co (1-X) O2 [0 <X <1], LiNi x Co y Mn z O2 (x, y, and z are each independently greater than 0 and less than 1.00, and the sum of x, y, and z is 0.99 to 1.00.) (so-called "NCM"; for example, LiNi 0.33 Co 0.33 Mn 0.33 O2, LiNi 0.5 Co 0.3 Mn0.2 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2), and other composite oxides of lithium and transition metals; Li t Ni 1-x-y Co x Al y O2 [t is 0.95 to 1.15, x is 0 to 0.3, y is 0.01 to 0.2, and the sum of x and y is less than 0.5.] (so-called "NCA"; e.g., LiNi 0.8 Co 0.15 Al 0.05 O2), etc., composite oxides of lithium, transition metals, and typical metals; Conductive polymeric materials such as polyaniline, polythiophene, polypyrrole, polyacetylene, polyacene, dimercaptothiadiazole, polyaniline composites; etc.
[0096] The proportion of lithium metal phosphate in the positive electrode active material is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. The proportion of lithium metal phosphate in the positive electrode active material may be 100% by mass or less than 100% by mass.
[0097] The proportion of lithium iron phosphate in the positive electrode active material is preferably 70 mass % or more, more preferably 80 mass % or more, and even more preferably 90 mass % or more. The proportion of lithium iron phosphate in the positive electrode active material may be 100% by mass or less than 100% by mass.
[0098] The positive electrode preferably comprises a positive electrode mixture layer containing a positive electrode active material. The positive electrode mixture layer may contain components other than the positive electrode active material. Examples of the components other than the positive electrode active material include a conductive assistant and a binder. Examples of the conductive assistant include carbon materials such as carbon black (for example, acetylene black), amorphous whiskers, and graphite. The binder may be polyvinylidene fluoride or the like.
[0099] The positive electrode mixture layer can be formed by applying a positive electrode mixture slurry containing a positive electrode active material and a solvent onto a positive electrode current collector, which will be described later, and drying the slurry. The positive electrode mixture slurry may contain components other than the positive electrode active material (for example, a conductive assistant, a binder, etc.). The solvent in the positive electrode mixture slurry may be, for example, an organic solvent such as N-methylpyrrolidone.
[0100] The proportion of the positive electrode active material in the total solid content of the positive electrode mixture layer is preferably 70 mass % or more, more preferably 80 mass % or more, and even more preferably 90 mass % or more. The proportion of the positive electrode active material in the total solid content of the positive electrode mixture layer may be 100 mass %. Here, the total solid content of the positive electrode mixture layer means the total amount excluding the solvent from the positive electrode mixture layer when the solvent remains in the positive electrode mixture layer, and means the total amount of the positive electrode mixture layer when no solvent remains in the positive electrode mixture layer.
[0101] The proportion of lithium metal phosphate in the total solid content of the positive electrode mixture layer is preferably 70 mass % or more, more preferably 80 mass % or more, and even more preferably 90 mass % or more. The proportion of lithium metal phosphate in the total solid content of the positive electrode mixture layer may be 100 mass % or less than 100 mass %.
[0102] The proportion of lithium iron phosphate in the total solid content of the positive electrode mixture layer is preferably 70 mass % or more, more preferably 80 mass % or more, and even more preferably 90 mass % or more. The proportion of lithium iron phosphate in the total solid content of the positive electrode mixture layer may be 100 mass % or less than 100 mass %.
[0103] The positive electrode preferably includes a positive electrode current collector. There is no particular limitation on the material of the positive electrode current collector, and any known material can be used. Specific examples of the positive electrode current collector include metal materials such as aluminum, aluminum alloys, stainless steel, nickel, titanium, and tantalum; carbon materials such as carbon cloth and carbon paper; and the like.
[0104] <Negative electrode> The negative electrode contains a negative electrode active material containing an Si element. This provides the lithium secondary battery with excellent battery capacity.
[0105] The negative electrode active material containing Si element is silicon oxide (hereinafter, simply referred to as "SiO X That is, the non-aqueous electrolyte may contain SiO X The negative electrode active material may be used in a battery comprising the negative electrode active material.
[0106] Formula (1): SiO X [In formula (1), X represents 0.5 or more and less than 1.6.]
[0107] SiO X may be coated with amorphous carbon.
[0108] SiO X may be a known compound. X For more information, see International Publication No. 2013 / 094668, Japanese Patent Application Laid-Open No. 2016-143642, etc.
[0109] SiO X The content is not particularly limited, and is preferably 1 mass % to 20 mass %, more preferably 1 mass % to 10 mass %, and further preferably 2 mass % to 8 mass %, based on the total amount of the negative electrode active material.
[0110] The negative electrode active material may further contain a graphite material in addition to elemental Si, which provides a longer battery life than a negative electrode active material that does not contain a graphite material.
[0111] Examples of the graphite material include natural graphite and artificial graphite. The negative electrode active material may contain only one type of graphite material, or may contain two or more types. The graphite material preferably contains natural graphite, and more preferably contains natural graphite coated with amorphous carbon (hereinafter also referred to as "amorphous coated natural graphite"). When the graphite material contains natural graphite, the ratio of natural graphite in the graphite material is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 80 mass% or more. The ratio of amorphous carbon in the natural graphite coated with amorphous carbon is preferably 0.1 mass% to 10 mass%, more preferably 0.2 mass% to 5 mass%, and even more preferably 0.3 mass% to 3 mass%. As the graphite material, a graphite material having a lattice spacing d(002) of 0.340 nm or less, as measured by X-ray analysis, is particularly preferred. The true density of the graphite material is 1.70 g / cm 3 More preferably, it is equal to or greater than this.
[0112] The negative electrode active material is graphite material and SiO X When the negative electrode active material contains the graphite material, the content of the graphite material is preferably 80% by mass to 99% by mass, more preferably 90% by mass to 99% by mass, and further preferably 92% by mass to 98% by mass, based on the total amount of the negative electrode active material.
[0113] The negative electrode active material may contain other components in addition to the Si element and the graphite material. Examples of other components include carbon materials other than graphite materials (for example, carbon black, activated carbon, amorphous carbon materials, etc.); metals or alloys such as silicon, silicon alloys, tin, and tin alloys; and lithium titanate. Examples of amorphous carbon materials include hard carbon, coke, mesocarbon microbeads (MCMB) calcined at 1500° C. or less, and mesophase pitch carbon fiber (MCF). As the negative electrode active material, natural graphite coated with an amorphous carbon material; natural graphite coated with a metal such as gold, platinum, silver, copper, or tin; and the like may be used.
[0114] The negative electrode preferably includes a negative electrode mixture layer containing a negative electrode active material. The negative electrode mixture layer may contain components other than the negative electrode active material. Examples of components other than the negative electrode active material include a conductive assistant and a binder. Examples of the conductive assistant include the same conductive assistants as those exemplified as the conductive assistants that can be contained in the positive electrode mixture layer. Examples of the binder include carboxymethyl cellulose and SBR latex.
[0115] The negative electrode mixture layer can be formed by applying a negative electrode mixture slurry containing a negative electrode active material and a solvent onto a negative electrode current collector, which will be described later, and drying the slurry. The negative electrode mixture slurry may contain components other than the negative electrode active material (for example, a conductive assistant, a binder, etc.). An example of the solvent in the negative electrode mixture slurry is water.
[0116] The proportion of the negative electrode active material in the total solid content of the negative electrode mixture layer is preferably 70 mass % or more, more preferably 80 mass % or more, and even more preferably 90 mass % or more. The proportion of the negative electrode active material in the total solid content of the negative electrode mixture layer may be 100 mass %. Here, the total solid content of the negative electrode mixture layer means the total amount excluding the solvent from the negative electrode mixture layer when the solvent remains in the negative electrode mixture layer, and means the total amount of the negative electrode mixture layer when no solvent remains in the negative electrode mixture layer.
[0117] The negative electrode preferably includes a negative electrode current collector. The material of the negative electrode current collector is not particularly limited, and any known material can be used. Specific examples of the negative electrode current collector include metal materials such as copper, nickel, stainless steel, nickel-plated steel, etc. Among these, copper is particularly preferred from the viewpoint of ease of processing.
[0118] <separator> The separator may be, for example, a porous resin plate. The material of the porous resin plate may be a resin, a nonwoven fabric containing the resin, etc. The resin may be polyethylene (PE), polypropylene (PP), polymethylpentene (PMP), polyester, cellulose, polyamide, etc. In particular, the separator is preferably a porous resin sheet having a single layer or a multilayer structure. The material of the porous resin sheet is mainly made of one or more polyolefin resins. The thickness of the separator is preferably 5 μm or more and 30 μm or less. The separator is preferably disposed between the positive electrode and the negative electrode.
[0119] <Specific examples of lithium secondary battery precursors> FIG. 1 is a schematic cross-sectional view showing a laminated type lithium secondary battery precursor, which is an example of the lithium secondary battery precursor of the present disclosure.
[0120] As shown in FIG. 1, a lithium secondary battery precursor 1 is a laminated type battery precursor. Specifically, in the lithium secondary battery precursor 1, the battery element 10 is enclosed inside an exterior body 30. The exterior body 30 is formed of a laminate film. A positive electrode lead 21 and a negative electrode lead 22 are attached to the battery element 10. The positive electrode lead 21 and the negative electrode lead 22 are led out in opposite directions from the inside to the outside of the exterior body 30.
[0121] As shown in Fig. 1, the battery element 10 is formed by laminating a positive electrode 11, a separator 13, and a negative electrode 12. The positive electrode 11 is formed by forming a positive electrode mixture layer 11B on both main surfaces of a positive electrode current collector 11A. The negative electrode 12 is formed by forming a negative electrode mixture layer 12B on both main surfaces of a negative electrode current collector 12A. The positive electrode mixture layer 11B formed on one main surface of the positive electrode current collector 11A of the positive electrode 11 and the negative electrode mixture layer 12B formed on one main surface of the negative electrode current collector 12A of the negative electrode 12 adjacent to the positive electrode 11 face each other via the separator 13.
[0122] The nonaqueous electrolyte solution of the present disclosure is injected into the interior of the exterior body 30 of the lithium secondary battery precursor 1. The nonaqueous electrolyte solution of the present disclosure permeates the positive electrode mixture layer 11B, the separator 13, and the negative electrode mixture layer 12B. In the lithium secondary battery precursor 1, one single cell layer 14 is formed by the adjacent positive electrode mixture layer 11B, the separator 13, and the negative electrode mixture layer 12B. Note that the positive electrode and the negative electrode may each have a mixture layer formed on one side of each current collector.
[0123] The lithium secondary battery precursor 1 is a laminated type lithium secondary battery precursor, but the lithium secondary battery precursor of the present disclosure is not limited thereto and may be, for example, a wound type lithium secondary battery precursor. The wound type lithium secondary battery precursor is formed by stacking a positive electrode, a separator, a negative electrode, and a separator in this order and winding them into a layered shape. The wound type lithium secondary battery precursor includes a cylindrical lithium secondary battery precursor and a prismatic lithium secondary battery precursor.
[0124] 1, in the lithium secondary battery precursor 1, the directions in which the positive electrode lead and the negative electrode lead each protrude from the inside of the exterior body 30 to the outside are opposite directions with respect to the exterior body 30, but the present disclosure is not limited thereto. For example, the directions in which the positive electrode lead and the negative electrode lead each protrude from the inside of the exterior body 30 to the outside may be the same direction with respect to the exterior body 30.
[0125] An example of the lithium secondary battery of the present disclosure described below is a lithium secondary battery obtained by charging and discharging the lithium secondary battery precursor 1.
[0126] FIG. 2 is a schematic cross-sectional view showing a coin-type lithium secondary battery precursor, which is another example of the lithium secondary battery precursor of the present disclosure.
[0127] 2, a disk-shaped negative electrode 42, a separator 45 filled with a non-aqueous electrolyte, a disk-shaped positive electrode 41, and, if necessary, spacer plates 47, 48 made of stainless steel, aluminum, or the like are stacked in this order and housed between a positive electrode can 43 (hereinafter also referred to as a "battery can") and a sealing plate 44 (hereinafter also referred to as a "battery can lid"). The positive electrode can 43 and the sealing plate 44 are crimped and sealed with a gasket 46 interposed therebetween. In this example, the nonaqueous electrolyte of the present disclosure is used as the nonaqueous electrolyte injected into separator 45 .
[0128] An example of the lithium secondary battery of the present disclosure described below is a lithium secondary battery obtained by charging and discharging a coin-type lithium secondary battery precursor shown in FIG.
[0129] [Lithium secondary battery and manufacturing method thereof] The method for producing a lithium secondary battery according to the present disclosure includes: A step of preparing the lithium secondary battery precursor of the present disclosure described above (hereinafter also referred to as a "preparation step"); charging and discharging the lithium secondary battery precursor; Includes. The lithium secondary battery of the present disclosure is a lithium secondary battery obtained by charging and discharging the above-mentioned lithium secondary battery precursor of the present disclosure.
[0130] According to the lithium secondary battery and the method for producing the same of the present disclosure, it is possible to improve the capacity retention rate of the lithium secondary battery during storage.
[0131] The preparation step may be a step of simply preparing a previously manufactured lithium secondary battery precursor of the present disclosure for a step of charging and discharging, or may be a step of manufacturing a lithium secondary battery precursor of the present disclosure. The lithium secondary battery precursor is as described above.
[0132] In the step of charging and discharging, the lithium secondary battery precursor can be charged and discharged according to a known method. In this step, the lithium secondary battery precursor may be subjected to a cycle of charging and discharging multiple times. As described above, this charging and discharging preferably forms an SEI (Solid Electrolyte Interface) film on the surface of the positive electrode (particularly the positive electrode active material) and / or the negative electrode (particularly the negative electrode active material) in the lithium secondary battery precursor.
[0133] In the step of charging and discharging, the lithium secondary battery precursor is preferably subjected to a combination of charging and discharging at least once in an environment of 25°C to 70°C.
[0134] In the lithium secondary battery of the present disclosure, the negative electrode active material preferably further contains a graphite material. This improves the battery life of the lithium secondary battery compared to when the negative electrode active material does not contain a graphite material. Examples of the graphite material include the same as those exemplified as the graphite material of the negative electrode active material. EXAMPLES
[0135] Examples of the present disclosure will be described below, but the present disclosure is not limited to the following examples. In the following, "addition amount" means the content relative to the total amount of the finally obtained nonaqueous electrolyte, and "wt%" means mass%.
[0136] Example 1 A lithium secondary battery (test battery) was fabricated according to the following procedure.
[0137] <Preparation of negative electrode> Amorphous-coated natural graphite (92 parts by mass), SiO (i.e., silicon oxide in which X is 1 in the composition formula SiOx; manufactured by Osaka Titanium Technologies Co., Ltd.) (5 parts by mass), carboxymethyl cellulose (1 part by mass), and SBR (2 parts by mass) were kneaded with an aqueous solvent to prepare a paste-like negative electrode mixture slurry. Next, this negative electrode mixture slurry was applied to a negative electrode current collector (material: copper foil, thickness: 10 μm), dried, and then compressed by a roll press to obtain a sheet-shaped negative electrode. The negative electrode was composed of a negative electrode current collector and a negative electrode active material layer. The coating density of the negative electrode active material layer was 11 mg / cm. 2 The packing density of the negative electrode active material layer was 1.5 g / mL. The amorphous-coated natural graphite was natural graphite coated with amorphous carbon. The proportion of natural graphite in the amorphous-coated natural graphite was 99% by mass. The proportion of amorphous carbon in the amorphous-coated natural graphite was 1% by mass.
[0138] <Preparation of positive electrode> LiNi 0.5 Mn 0.3 Co 0.2 O2 (92 parts by mass), acetylene black (5 parts by mass), and polyvinylidene fluoride (3 parts by mass) were kneaded using N-methylpyrrolidone as a solvent to prepare a paste-like positive electrode mixture slurry. Next, this positive electrode mixture slurry was applied to a positive electrode current collector (material: strip-shaped aluminum foil, thickness: 20 μm), dried, and then compressed with a roll press to obtain a sheet-shaped positive electrode. The positive electrode was composed of a positive electrode current collector and a positive electrode active material layer. The coating density of the positive electrode active material layer was 22 mg / cm. 2 The packing density of the positive electrode active material layer was 2.5 g / mL.
[0139] <Preparation of non-aqueous electrolyte> Ethylene carbonate (EC), dimethyl carbonate (DMC), and methyl ethyl carbonate (EMC) were mixed as non-aqueous solvents in a ratio of 30:35:35 (volume ratio) to obtain a mixed solvent. LiPF6 was dissolved as an electrolyte in the obtained mixed solvent so that the concentration of LiPF6 in the final non-aqueous electrolyte was 1.0 mol / L.
[0140] To the solution obtained above, 0.5 mass % of a fluorine-containing sulfonyl compound (I-1) represented by the following (I-1) was added to obtain a nonaqueous electrolyte solution.
[0141] [ka]
[0142] <Preparation of lithium secondary battery> The above-mentioned negative electrode was punched into a disk shape with a diameter of 14 mm to obtain a coin-shaped negative electrode. The above-mentioned positive electrode was punched into a disk shape with a diameter of 13 mm to obtain a coin-shaped positive electrode. A microporous polyethylene film (thickness: 20 μm) was punched into a disk shape with a diameter of 17 mm to obtain a separator. The obtained coin-shaped negative electrode, separator, and coin-shaped positive electrode were stacked in this order in a stainless steel battery can (2032 size). Next, 20 μL of nonaqueous electrolyte was poured into the battery can, and the separator, positive electrode, and negative electrode were impregnated with the nonaqueous electrolyte. Next, an aluminum plate (thickness: 1.2 mm, diameter: 16 mm) and a spring were placed on the positive electrode, and the battery can lid was crimped via a polypropylene gasket to seal the battery. As a result, a coin-type lithium secondary battery having the configuration shown in Fig. 2 was obtained. The diameter of the lithium secondary battery was 20 mm. The height of the lithium secondary battery was 3.2 mm.
[0143] <Initial capacity measurement> The obtained lithium secondary battery was subjected to aging in a thermostatic chamber at 25°C by repeating charging and discharging twice between 2.5V and 4.2V. The aged lithium secondary battery was subjected to CC-CV charging at a charge rate of 0.2C to 4.2V and CC discharging at a discharge rate of 0.2C to 2.5V to measure the initial capacity of the lithium secondary battery. "CC-CV charging" means constant current - constant voltage. "CC discharging" means discharging at a constant current.
[0144] <Measurement of initial resistance (25℃)> The SOC (State of Charge) of the lithium secondary battery after the initial capacity measurement was adjusted to 50%, and then the initial resistance of the lithium secondary battery was measured by the following method. Using the lithium secondary battery adjusted to SOC 50% described above, CC10s discharge was performed at a discharge rate of 0.2 C at a temperature of 25° C. “CC10s discharge” means discharging at a constant current for 10 seconds. The DC resistance was calculated based on the current value in the above "CC10s discharge at a discharge rate of 0.2C" (i.e., the current value corresponding to a discharge rate of 0.2C) and the amount of voltage drop (=voltage before the start of discharge-voltage 10 seconds after the start of discharge), and the obtained DC resistance was designated as the initial resistance (25°C) (Ω) of the lithium secondary battery.
[0145] <Initial resistance measurement (-10℃)> After the measurement of the initial resistance (25°C), the initial resistance of the lithium secondary battery was measured in the same manner as for the initial resistance (25°C), except that the temperature was set to -10°C.
[0146] <High temperature cycle operation> After measuring the initial resistance (-10°C), the lithium secondary battery was subjected to CC-CV charging at a charge rate of 1C at 55°C up to 4.2V, and then CC discharging at a discharge rate of 1C down to 2.5V 200 times.
[0147] <Capacity measurement after high temperature cycle> The lithium secondary battery after the high-temperature cycle was subjected to CC-CV charging at 4.2 V at a charge rate of 0.2 C and CC discharging at 2.5 V at a discharge rate of 0.2 C in a thermostatic chamber at 25° C., and the capacity after the high-temperature cycle was measured from the capacity at the time of discharge. The capacity after the high-temperature cycle relative to the initial capacity was determined and this was taken as the "capacity retention rate after the high-temperature cycle."
[0148] (Evaluation of capacity retention rate after high-temperature cycle) The capacity retention rate after high temperature cycles of Example 1 was determined based on the capacity retention rate after high temperature cycles of Comparative Example 1 described below taken as 100, and this was taken as the "capacity retention rate after high temperature cycles (relative value)."
[0149] <Measurement of resistance after high temperature cycle (25℃)> The SOC of the lithium secondary battery after the high-temperature cycle was adjusted to 50%, and then the resistance (25° C.) after the high-temperature cycle of the lithium secondary battery was measured by the same method as for measuring the initial resistance (25° C.). The resistance after the high-temperature cycle (25°C) relative to the initial resistance (25°C) was determined and this was taken as the "resistance increase rate after the high-temperature cycle (25°C)."
[0150] (Evaluation of resistance increase rate (25℃) after high temperature cycle) The resistance increase rate after high-temperature cycle (25°C) of Example 1 was determined relative to the resistance increase rate after high-temperature cycle (25°C) of Comparative Example 1 described below, which was set to 100, and this was taken as the "resistance increase rate after high-temperature cycle (25°C) (relative value)."
[0151] <Measurement of resistance after high temperature cycle (-10℃)> After measuring the resistance (25° C.) after the high-temperature cycle, the resistance (−10° C.) of the lithium secondary battery was measured in the same manner as in measuring the initial resistance (−10° C.). The resistance after the high-temperature cycle (-10°C) relative to the initial resistance (-10°C) was determined and this was recorded as the "resistance increase rate after the high-temperature cycle (-10°C)."
[0152] (Evaluation of resistance increase rate (-10℃) after high temperature cycle) The resistance increase rate after high temperature cycle (-10°C) of Example 1 was determined relative to the resistance increase rate after high temperature cycle (-10°C) of Comparative Example 1 described below, which was set to 100, and this was taken as the "resistance increase rate after high temperature cycle (-10°C) (relative value)."
[0153] [Examples 2 to 12, Comparative Example 1] The same operation as in Example 1 was carried out, except that the amount of the compound represented by the following formula was changed to that shown in Table 1. The results are shown in Table 1. In Table 1, "-" means that the content of the corresponding additive is 0 mass%.
[0154] [ka]
[0155] [Table 1]
[0156] The nonaqueous electrolytes of Examples 1 to 12 are used in lithium secondary batteries containing Si element as a negative electrode active material, and contain compound (I). Therefore, as shown in Table 1, the capacity retention rate after high-temperature cycle of Examples 1 to 12 was higher than that of Comparative Example 1 that does not contain an additive. Furthermore, the resistance increase rate after high-temperature cycle (25°C) (relative value) and the resistance increase rate after high-temperature cycle (-10°C) (relative value) of Examples 1 to 12 were lower than that of Comparative Example 1. As a result, it was found that the nonaqueous electrolytes of Examples 1 to 12 are nonaqueous electrolytes for batteries that can suppress the decrease in battery capacity and the increase in battery resistance at room temperature and low temperature even when charging and discharging are repeatedly performed in a high-temperature environment.
[0157] In Examples 1 to 4, 6 to 10, and 12, the total of the content of compound (I) and the content of compound (A) is less than 4.5% by mass. In Examples 5 and 11, the total of the content of compound (I) and the content of compound (A) is 4.5% by mass or more. The capacity retention rates after high-temperature cycles in Examples 1 to 4, 6 to 10, and 12 are higher than the capacity retention rates after high-temperature cycles in Examples 5 and 11. This shows that by making the total of the content of compound (I) and the content of compound (A) less than 4.5% by mass, the nonaqueous electrolyte can further suppress the decrease in battery capacity even when charging and discharging are repeatedly performed in a high-temperature environment.
[0158] Comparisons between Example 2 and Example 9, between Example 3 and Example 10, between Example 4 and Example 11, and between Example 5 and Example 12 reveal that the nonaqueous electrolyte solution containing compound (I-1) is more effective at suppressing an increase in battery resistance at room temperature and low temperature, even when charging and discharging are repeatedly performed in a high-temperature environment, than the nonaqueous electrolyte solution containing compound (I-2). [Explanation of symbols]
[0159] 1. Lithium secondary battery precursor 10 Battery element 11 Positive electrode 11A positive electrode current collector 11B Positive electrode composite layer 12 Negative electrode 12A negative electrode current collector 12B Negative electrode composite layer 13 Separator 14 Cell Layer 21 Positive lead 22 Negative lead 30 Exterior body 41 Positive electrode 42 Negative electrode 43 Positive electrode can 44 Sealing plate 45 Separator 46 Gasket 47, 48 Spacer plate
Claims
1. It is used in a lithium secondary battery containing Si element as a negative electrode active material, A non-aqueous electrolyte for a battery, comprising a compound (I) represented by the following formula (I): [Case 1] [In formula (I), L is a single bond or -O-; R 11 is a hydrocarbon group having 1 to 10 carbon atoms (at least one hydrogen atom in the hydrocarbon group may be substituted with a halogen atom), and at least one carbon atom of the hydrocarbon group may be substituted with an oxygen atom, a nitrogen atom, a sulfur atom, or a sulfonyl group.
2. Further comprising compound (A), The compound (A) is at least one selected from the group consisting of a compound (II) represented by the following formula (II), a compound (III) represented by the following formula (III), a compound (IV) represented by the following formula (IV), and a compound (V) which is at least one selected from the group consisting of lithium monofluorophosphate and lithium difluorophosphate. The nonaqueous electrolyte for a battery according to claim 1 . [Case 2] [In formula (II), R 21 ~R 24 each independently represents a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 3 carbon atoms, or a fluorohydrocarbon group having 1 to 3 carbon atoms. 21 ~R 24 cannot all be hydrogen atoms. In formula (III), R 31 ~R 32 each independently represents a hydrogen atom, a fluorine atom, a hydrocarbon group having 1 to 3 carbon atoms, or a fluorohydrocarbon group having 1 to 3 carbon atoms. In formula (IV), R 41 represents an alkylene group having 1 to 6 carbon atoms, an alkenylene group having 2 to 6 carbon atoms, a group represented by formula (iv-1), or a group represented by formula (iv-2), * indicates the bond position. In formula (iv-1), R 42 represents an oxygen atom, an alkylene group having 1 to 6 carbon atoms, an alkenylene group having 2 to 6 carbon atoms, or an oxymethylene group; In formula (ii-2), R 43 represents an alkyl group having 1 to 6 carbon atoms or an alkenyl group having 2 to 6 carbon atoms.
3. The nonaqueous electrolyte for a battery according to claim 2 , wherein the compound (A) contains at least the compound (II).
4. 3. The nonaqueous electrolyte solution for a battery according to claim 2, wherein the content of the compound (A) is 0.01% by mass to 10.0% by mass based on the total amount of the nonaqueous electrolyte solution for a battery.
5. 2. The nonaqueous electrolyte solution for a battery according to claim 1, wherein the content of the compound (I) is 0.01% by mass to 5.0% by mass based on the total amount of the nonaqueous electrolyte solution for a battery.
6. Case and a positive electrode, a negative electrode, a separator, and an electrolyte solution contained in the case; Equipped with the positive electrode comprises a positive electrode active material including lithium metal phosphate; The negative electrode includes a negative electrode active material including a Si element, The electrolyte is the nonaqueous electrolyte for a battery according to any one of claims 1 to 5. Lithium secondary battery precursor.
7. A lithium secondary battery obtained by charging and discharging the lithium secondary battery precursor according to claim 6.
8. The lithium secondary battery precursor according to claim 7 , wherein the negative electrode active material further comprises a graphite material.
9. A step of preparing a lithium secondary battery precursor according to claim 6; Charging and discharging the lithium secondary battery precursor; A method for producing a lithium secondary battery, comprising:
Citation Information
Patent Citations
Nonaqueous electrolyte battery
JP2003346899A
Electrochemical device
JP2013051342A
Nonaqueous electrolyte composition containing fluorinated sulfone
JP2019523521A
Nonaqueous electrolyte solution for batteries and lithium secondary battery
WO2020022452A1
Nonaqueous electrolyte solution for lithium secondary batteries, lithium secondary battery precursor, lithium secondary battery, and method for manufacturing lithium secondary battery