Double container, and manufacturing method of double container
The double container design with a constricted outer shell and controlled thickness variations simplifies the separation of the inner bag, addressing recycling challenges and reducing separation force, thereby enhancing recyclability.
Patent Information
- Application Number
- JP2023052391
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional double containers with different material compositions for the outer shell and inner bag cannot be recycled effectively due to adhesion issues, and separating the inner bag requires significant force.
A double container design featuring a constricted portion on the outer shell at a specific height position with a reduced thickness and a cam mechanism to facilitate easier removal of the inner bag, along with controlled thickness variations during biaxial stretch blow molding.
The design reduces the force required to separate the inner bag from the container body by minimizing the thickness of the inner bag at critical points, enabling easier recycling and reducing material waste.
Smart Images

Figure 2024140987000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a double container and a method for manufacturing the same. [Background technology]
[0002] Conventionally, a double container having a container body having an outer shell and an inner bag is known. For example, Patent Document 1 discloses a double container formed by performing biaxial stretch blow molding on an outer shell preform and an inner bag preform in a stacked state. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-10741 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, when the outer shell and inner bag of such a double container are molded from different materials, or when contents remain inside the inner bag after use, it is desirable to separate the outer shell and inner bag when recycling the double container.
[0005] It is envisioned that the outer shell and inner bag will be separated by pulling the inner bag from the container body, and it is desirable to reduce the force required to separate the inner bag from the container body.
[0006] The present invention has been made in view of the above circumstances, and provides a double container that can reduce the force required to separate the inner bag from the container body. [Means for solving the problem]
[0007] According to the present invention, the following inventions are provided. [1] A double container comprising a container body having an inner bag and an outer shell arranged to cover the inner bag, wherein the inner bag is configured to be removable from the container body, and a constriction is provided on the outer surface of the outer shell at a first height position which is the starting point of an undercut portion that interferes with the outer shell when the inner bag is pulled out of the container body. [2] A double container comprising an inner bag and a container body having an outer shell arranged to cover the inner bag, the inner bag being configured to be removable from the container body, the container body having a mouth, a body, and a bottom, the mouth being a tubular portion having an open end, the body being arranged adjacent to the mouth on a side farther from the open end than the mouth and having a larger outer diameter than the mouth, the bottom being configured to close the lower end of the body, the body having a shoulder portion whose outer diameter increases as it moves away from the mouth, the mouth being provided with a flange, and a constriction being provided between the flange and the shoulder portion. [3] The double container according to [1] or [2], wherein, when the thickness of the outer shell at the first height position is T1o and the depth of the constricted portion is D, D / T1o is 0.1 to 0.8. [4] The double container according to any one of [1] to [3], wherein the depth of the constricted portion is 0.2 to 1.0 mm. [5] A double container according to any one of [1] to [4], wherein the thickness of the inner bag at a second height position 2.5 mm away from the opening end of the container body from the first height position is 0.30 mm or less. [6] A double-walled container as described in any one of [1] to [5], wherein T2i is the thickness of the inner bag at a second height position 2.5 mm away from the opening end of the container body from the first height position, and T3 is the average thickness of the inner bag within a height range of 5 mm from the first height position to the opening end of the container body, such that T2i / T3 is 0.60 or less. [7] A double container comprising a container body having an inner bag and an outer shell arranged to cover the inner bag, wherein the inner bag is configured to be removable from the container body, and the thickness of the inner bag at a second height position 2.5 mm away from a first height position which is the starting point of an undercut portion that interferes with the outer shell when the inner bag is removed from the container body is 0.30 mm or less. [8] A double container comprising an inner bag and a container body having an outer shell arranged to cover the inner bag, wherein the inner bag is configured to be removable from the container body, and wherein T2i is the thickness of the inner bag at a second height position 2.5 mm away from a first height position which is the starting point of an undercut portion that interferes with the outer shell when the inner bag is pulled out of the container body, and T3 is the average thickness of the inner bag within a height range of 5 mm from the first height position to the opening end of the container body, such that T2i / T3 is 0.60 or less. [9] A method for manufacturing a double-layered container, comprising the step of biaxially stretch-blow molding a preform using a molding die to produce a container body, wherein the container body has an inner bag and an outer shell arranged to cover the inner bag, the preform comprises an inner preform corresponding to the inner bag and an outer preform corresponding to the outer shell, the outer preform comprises a non-stretched portion whose wall thickness has been reduced by less than 10% during the biaxially stretch-blow molding and an extended portion whose wall thickness has been reduced by 10% or more, and the molding die comprises a protrusion extending in the circumferential direction at a position abutting the outer surface of the outer preform in an adjacent portion of the extended portion adjacent to the non-stretched portion.
[10] A method for manufacturing a double-layered container, comprising a step of biaxially stretch-blow molding a preform using a molding die to produce a container body, wherein the container body has an inner bag and an outer shell arranged to cover the inner bag, the preform comprises an inner preform corresponding to the inner bag and an outer preform corresponding to the outer shell, the outer preform comprises a non-stretched portion whose wall thickness is reduced by less than 10% during the biaxially stretch-blow molding and a stretched portion whose wall thickness is reduced by 10% or more, the molding die comprises a flange accommodating portion that accommodates a flange of the preform and a shoulder forming surface for forming a shoulder of the container body, and comprises a protrusion extending in the circumferential direction at a position abutting the outer surface of the outer preform between the flange accommodating portion and the shoulder forming surface.
[11] The method according to [9] or
[10] , wherein the height of the protrusion is 0.2 to 1.0 mm. Effect of the Invention
[0008] The inventors have found that the force required to separate the inner bag is greater when the thickness of the undercut portion that becomes the undercut when the inner bag is pulled out from the container body is large. They also found that by providing a constricted portion on the outer surface of the outer shell at the first height position where the undercut portion starts, it is possible to move the first height position in a direction away from the open end of the container body compared to when there is no constricted portion. And since the thickness of the inner bag tends to become smaller the farther away from the open end of the container body, the inventors have found that according to the present invention, the thickness of the inner bag at the undercut portion can be reduced, thereby reducing the force required to separate the inner bag from the container body, and have completed the present invention. [Brief description of the drawings]
[0009] [Figure 1] 1 is a perspective view of a double container 1 according to a first embodiment of the present invention. The dashed and dotted lines in the figure represent the boundary lines at which the curvature of the faces that make up the surface shape changes. The same is true for the other figures. [Diagram 2] FIG. 2 is a perspective view of a container body 2 in FIG. [Diagram 3]FIG. 3 is an enlarged view of an area A in FIG. [Figure 4] 4 is an exploded perspective view of the inner bag 4. Only a portion of the inner bag 4 near the open end 5c is shown. [Diagram 5] FIG. 2 is a perspective view of the vicinity of an open end of the outer shell 3. [Figure 6] 3 is a vertical cross-sectional view of the container body 2 in FIG. 2, taken along the center of the mouth portion 5. FIG. [Figure 7] FIG. 7 is a view corresponding to FIG. 6, showing a container body 2 serving as a comparative example of the present invention. [Figure 8] FIG. 2 is a perspective view showing a state in which the inner preform 14 and the outer preform 13 are separated. [Figure 9] 1 is a perspective view of a preform 15 formed by covering an inner preform 14 with an outer preform 13. FIG. [Figure 10] 1 is a cross-sectional view showing a state in which a preform 15 is attached to a mouth support mold 21 and brought close to a heater 32. FIG. [Figure 11] 11 is a cross-sectional view showing a state after the preform 15 has been transferred from the state shown in FIG. 10 to a molding die 23. FIG. [Figure 12] 12 is a cross-sectional view showing a state after the bottom support mold 22 supports the bottom 13c of the outer preform 13 from the state shown in FIG. 11. FIG. [Figure 13] 13 is a cross-sectional view showing the state after the stretching bar 25 is extended and the bottom support mold 22 is retracted from the state shown in FIG. 12 to stretch the preform 15 in the first axis. [Figure 14] Fig. 14A is an enlarged view of region A in Fig. 13. Fig. 14B is a view of molding die 23 extracted from Fig. 14A. [Figure 15] FIG. 15 shows a comparative example of the present invention, and FIGS. 15A and 15B correspond to FIGS. 14A and 14B, respectively. [Figure 16] 1 is a cross-sectional view showing a preform 15 used in Example 1 and Comparative Example 1. FIG. [Figure 17] 2 is a diagram in which the shape of the container body 2 obtained in Example 1 is reproduced in a photograph taken after cutting the container body 2. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, embodiments of the present invention will be described. Various features shown in the following embodiments can be combined with each other. Also, each feature can be an invention independently.
[0011] 1. First embodiment 1-1. Structure of double container 1 <Basic configuration> As shown in FIG. 1, a double container 1 according to a first embodiment of the present invention comprises a container body 2 and a spout mounting member 8. The double container 1 has a container body 2 and a spout mounting member 8. The spout mounting member 8 is made of a material such as aluminum.
[0012] As shown in Figs. 2 and 3, the container body 2 has a mouth 5, a body 6, and a bottom 7. The mouth 5 is a tubular (preferably cylindrical) portion having an open end 5c. The mouth 5 has an engagement portion 4m to which the mouth attachment member 8 can be attached. Details of the engagement portion 4m will be described later. The mouth attachment member 8 is a cap 8a in this embodiment, but may be a pump. The mouth 5 is provided with a flange 5b. The flange 5b can be used to support the mouth 5 when the mouth attachment member 8 is attached to the mouth 5.
[0013] The body 6 is disposed adjacent to the mouth 5 on the side farther from the open end 5c than the mouth 5. The body 6 has a larger outer diameter (in this specification, "outer diameter" means a circular equivalent diameter when the cross section is not circular) than the mouth 5. The body 6 is cylindrical, and the bottom 7 is provided at the lower end of the body 6 and closes the lower end of the body 6. The body 6 has a shoulder 6b whose outer diameter increases with increasing distance from the mouth 5. The body 6 also has a body main body 6c on the bottom 7 side of the shoulder 6b. The body main body 6c has a shape in which the outer diameter is approximately constant toward the bottom 7, or a shape in which the diameter decreases toward the bottom 7, for example.
[0014] As shown in Fig. 4, the container body 2 includes an inner bag 4 and an outer shell 3 arranged to cover the inner bag 4. The inner bag 4 has an inner bag body 4d other than a protruding portion 4c housed within the outer shell 3. In the following description, the portions of the inner bag 4 that correspond to the mouth 5, body 6, and bottom 7 of the container body 2 will be referred to as the mouth 5, body 6, and bottom 7 of the inner bag 4, respectively. The same applies to the outer shell 3.
[0015] The average thickness of the shell 3 at the center of the height direction of the body 6 is, for example, 200 to 800 μm, and preferably 250 to 500 μm. Specifically, this thickness may be, for example, 250, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, or 800 μm, or may be within a range between any two of the numerical values exemplified here.
[0016] The average thickness of the inner bag 4 at the center in the height direction of the body 6 is, for example, 50 to 250 μm, and preferably 50 to 100 μm. Specifically, this thickness is, for example, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, or 250 μm, and may be within a range between any two of the numerical values exemplified here or less than any one of them. In this specification, the average thickness at a certain height position means the average value of the measured values at eight measurement points set at equal intervals in the circumferential direction at that height position.
[0017] If the mouth-mounted member 8 is not provided with a check valve, the inner bag 4 does not shrink even after the contents of the inner bag 4 are discharged, and it is therefore not easy to pull out the inner bag 4 through the mouth 5 of the outer shell 3. Since the present invention makes it easy to pull out the inner bag 4 through the mouth 5 of the outer shell 3, the significance of applying the present invention is particularly evident when the mouth-mounted member 8 is not provided with a check valve.
[0018] The inner diameter of the mouth 5 of the outer shell 3 is, for example, 20 to 50 mm, and preferably 25 to 40 mm. The inner diameter of the mouth 5 of the outer shell 3 is, specifically, for example, 20, 25, 30, 35, 40, 45, or 50 mm, and may be within a range between any two of the numerical values exemplified here. The length of the mouth 5 is, for example, 15 to 45 mm, and specifically, for example, 15, 20, 25, 30, 35, 40, or 45 mm, and may be within a range between any two of the numerical values exemplified here.
[0019] <Detailed structure of outer shell 3 and inner bag 4> 3 and 4, the inner bag 4 has a protruding portion 4c protruding from the open end 3a of the outer shell 3. The protruding portion 4c has a protruding tube 4c1, an engaging protruding portion 4c2, an annular protruding portion 4c5, and a contact flange 4c4.
[0020] The annular protrusion 4c5 engages with the mouth attachment member 8 in the axial direction. The engaging protrusion 4c2 engages with the mouth attachment member 8 in the circumferential direction. In this specification, the "axial direction" refers to the direction in which the central axis C of the mouth 5 extends, in other words, the direction in which the inner bag 4 is pulled out from the container body 2. The "circumferential direction" refers to the direction in which the mouth 5 rotates around the central axis C of the mouth 5, in other words, the direction in which the inner bag 4 is rotated relative to the outer shell 3 at the mouth 5.
[0021] The engaging protrusions 4c2 are preferably provided at a plurality of locations (eight locations in this embodiment) spaced apart in the circumferential direction. The engaging protrusions 4c2 are disposed on the annular protrusion 4c5 and are provided so as to protrude radially outward from the annular protrusion 4c5. The annular protrusion 4c5 and the engaging protrusions 4c2 are provided with tapered surfaces 4c8, 4c3 on their upper surfaces. This makes it easier for the annular protrusion (not shown) provided on the mouth mounting member 8 to climb over the annular protrusion 4c5 and the engaging protrusions 4c2.
[0022] The contact flange 4c4 is disposed at a position where it contacts the open end 3a and is an annular portion having a larger diameter than the protruding tube 4c1. The contact flange 4c4 contacts the open end 3a, thereby preventing the inner bag 4 from falling into the outer shell 3.
[0023] As shown in Fig. 4, a cam protrusion 4g is provided on the outer peripheral surface of the inner bag body 4d. The lower surface of the cam protrusion 4g is inclined counterclockwise when viewed from the opening end 5c of the mouth portion 5 so as to approach the opening end 5c.
[0024] As shown in Fig. 5, a cam rail 3l and an engagement recess 3m are provided on the inner peripheral surface of the outer shell 3. The engagement recess 3m is provided so that the lower surface of the engagement recess 3m is continuous with the upper surface of the cam rail 3l. The upper surface of the cam rail 3l and the lower surface of the engagement recess 3m are inclined so as to approach the opening end 3a as they proceed counterclockwise when viewed from the opening end 3a side.
[0025] Before the inner bag 4 is pulled out from the container body 2, the cam protrusion 4g is disposed in the engagement recess 3m, and the lower surface of the cam protrusion 4g abuts against the upper surface of the cam rail 3l. The cam protrusion 4g and the cam rail 3l form a cam mechanism 31. In this embodiment, the engagement recess 3m is a through hole, but it may be a non-through hole. When the inner bag 4 is rotated counterclockwise, the inner bag 4 moves in a direction to come out of the container body 2 due to the action of the cam mechanism 31. At this time, the inner bag 4 is twisted and reduced in diameter.
[0026] <Removing inner bag 4> The mouth attachment member 8 is configured to be attachable to the mouth 5 of the container body 2 in a plug-fitting manner, and by placing the mouth attachment member 8 over the mouth 5 and pressing the mouth attachment member 8 in the direction of the bottom 7, the mouth attachment member 8 can be engaged with the mouth 5 and attached.
[0027] The mouth attachment member 8 is engaged with the mouth 5 of the inner bag 4 in the circumferential and axial directions, and is configured so that the inner bag 4 rotates relative to the outer shell 3 as the mouth attachment member 8 rotates. The inner bag 4 is configured to move in a direction coming out of the container body 2 as the inner bag 4 rotates due to the action of a cam mechanism 31 provided between the inner bag 4 and the outer shell 3.
[0028] According to this configuration, by rotating the mouth attachment member 8, the inner bag 4 can be moved in a direction that allows it to be removed from the container body 2 while twisting, and then by pulling the mouth attachment member 8, the inner bag 4 can be pulled out of the container body 2. Note that the inner bag 4 may be separated from the container body 2 by pulling it in the axial direction without twisting it. Even in this case, according to the configuration of the present invention, the force required to separate the inner bag 4 is reduced.
[0029] <Undercut section> FIG. 7 shows the configuration of a container body 2x as a comparative example of the present invention. In the mouth 5 of the container body 2x, the inner surface 3b and the outer surface 3c of the outer shell 3 extend parallel to the central axis C of the mouth 5 in the first region 5d adjacent to the side approaching the opening end 5c with respect to the wall thickness reduction start height position Ha where the wall thickness of the outer shell 3 and the inner bag 4 starts to decrease. On the other hand, in the second region 5e adjacent to the side away from the opening end 5c with respect to the height position Ha, the outer surface 3c remains parallel to the central axis C, and the wall thickness of the outer shell 3 gradually decreases with increasing distance from the opening end 5c of the container body 2x. Therefore, the inner surface 3b of the outer shell 3 is an inclined surface whose diameter increases with increasing distance from the opening end 5c of the container body 2x. The outer surface 4v of the inner bag 4 is shaped along the inner surface 3b of the outer shell 3, so that the portion of the inner bag 4 present in the second region 5e has an undercut portion 4u that interferes with the outer shell 3 when the inner bag 4 is pulled out of the container body 2x. The undercut portion 4u is a portion closer to the outer shell 3 than the vertical plane V in Fig. 7. In the container body 2x, the wall thickness reduction start height position Ha coincides with the first height position H1 which is the starting point of the undercut portion 4u.
[0030] The undercut portion 4u is a factor that increases the force required to separate the inner bag 4 from the container body, and the greater the thickness of the inner bag 4 at the height position where the undercut portion 4u is located, the greater the effect. In the embodiment of Fig. 7, the first height position H1, which is the starting point of the undercut portion 4u, coincides with the height position Ha where the thickness reduction begins, and the reduction in thickness of the inner bag 4 is insufficient in the area directly below the first height position H1, so that the undercut portion 4u significantly increases the force required to separate the inner bag 4 from the container body.
[0031] Next, the container body 2 of this embodiment will be described with reference to FIG. 6. The container body 2 of this embodiment is mainly different from the comparative example of FIG. 7 in that a constricted portion 3d is provided on the outer surface 3c of the outer shell 3. The container body 2 of this embodiment is common to the embodiment of FIG. 7 in that the thickness of the outer shell 3 and the inner bag 4 gradually decreases in the second region 5e. However, in this embodiment, since the constricted portion 3d is provided, the thickness reduction start height position Ha is not the first height position H1 which is the starting point of the undercut portion 4u, and the first height position H1 is a height position farther from the opening end 5c than the thickness reduction start height position Ha. Since the thickness of the inner bag 4 decreases with increasing distance from the opening end 5c in the second region 5e, the first height position H1 is located farther from the opening end 5c than the thickness reduction start height position Ha, so that the thickness of the inner bag 4 at the portion directly below the first height position H1 becomes smaller than when the constricted portion 3d does not exist, as shown in FIG. 7. Therefore, by providing the constricted portion 3d, it is possible to reduce the force required to separate the inner bag 4 from the container body.
[0032] The constricted portion 3d is a recessed portion provided so as to extend in the circumferential direction of the outer surface 3c of the outer shell 3. The constricted portion 3d may be provided on a portion of the outer surface 3c in the circumferential direction, but is preferably provided on the entire circumference. The constricted portion 3d is preferably provided between the flange 5b and the shoulder portion 6b. It is preferable that there is a portion between the constricted portion 3d and the lower surface of the flange 5b where there is no constricted portion 3d. It is preferable that the constricted portion 3d is connected to the shoulder portion 6b without any step.
[0033] If the thickness of the outer shell 3 at the first height position H1 is T1o and the depth of the constricted portion 3d is D, then D / T1o is preferably 0.1 to 0.8. If the constricted portion 3d is too shallow, the effect of reducing the thickness of the inner bag 4 at the height position where the undercut portion 4u is located may be insufficient. If the constricted portion 3d is too deep, the force required to separate the inner bag 4 may increase due to the undercut caused by the constricted portion 3d. The depth D refers to the depth from the outer surface 3c at the first region 5d. The depth D can be calculated, for example, by (outer diameter of the outer shell 3 at the first region 5d - outer diameter of the outer shell 3 at the constricted portion 3d) / 2. D / T1o is preferably 0.2 to 0.7, and specifically, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, and may be in the range between any two of the numerical values exemplified here.
[0034] T1o is, for example, 0.8 to 2.0 mm, specifically, for example, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2.0 mm, or may be in the range between any two of the numerical values exemplified here. D is, for example, 0.2 to 1.0 mm, specifically, for example, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1.0 mm, or may be in the range between any two of the numerical values exemplified here. The thickness T1i of the inner bag 4 at the first height position H1 is, for example, 0.15 to 0.35 mm, and more specifically, for example, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, or 0.35 mm, and may be in a range between any two of the numerical values exemplified here.
[0035] The thickness T2i of the inner bag 4 at the second height position H2, which is 2.5 mm away from the opening end 5c from the first height position H1, is preferably 0.30 mm or less, and more preferably 0.20 mm or less. The smaller the thickness, the less the force required to separate the inner bag 4 is prevented from increasing due to the undercut portion 4u. The thickness T2i may be, for example, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, or 0.30 mm, or may be in a range between any two of the values exemplified here or less than any of them. The thickness T2o of the outer shell 3 at the second height position H2 is, for example, 0.5 to 1.5 mm, specifically, for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, or 1.5 mm, or may be in a range between any two of the numerical values exemplified here.
[0036] If the average thickness of the inner bag 4 in a height range of 5 mm from the first height position H1 toward the opening end 5c is T3, it is preferable that T2i / T3 is 0.60 or less. T2i / T3 indicates the degree of reduction in thickness of the inner bag 4 at the height position where the undercut portion 4u is located. The smaller T2i / T3 is, the more significant the reduction in thickness of the inner bag 4 at the height position where the undercut portion 4u is located, and the more suppressed the increase in the force required to separate the inner bag 4 due to the undercut portion 4u. T2i / T3 is,
[0037] 1-2. Manufacturing method of double container 1 As shown in FIGS. 8 to 13, the container body 2 can be produced by biaxially stretching and blow molding the preform 15 using a molding die .
[0038] <Configuration of inner preform 14, outer preform 13, and preform 15> The preform 15 includes an inner preform 14 which becomes the inner bag 4 and an outer preform 13 which becomes the outer shell 3 .
[0039] As shown in FIG. 8, the inner preform 14 is cylindrical with a bottom, and includes a mouth portion 14a, a body portion 14b, and a bottom portion 14c. A protrusion 14d is provided at the open end of the mouth portion 14a. The protrusion 14d does not deform during molding, and becomes the protrusion 4c in its original shape. Therefore, the matters described for the protrusion 4c also apply to the protrusion 14d. An engagement portion 14m is provided on the protrusion 14d. The engagement portion 14m becomes the engagement portion 4m after molding, and is used to pull out the inner bag 4. The bottom portion 14c is provided to close the lower end of the body portion 14b.
[0040] 8, the outer preform 13 is a cylindrical shape with a bottom, and includes a mouth portion 13a, a body portion 13b, and a bottom portion 13c. The bottom portion 13c is provided so as to close the lower end of the body portion 13b. The bottom portion 13c is provided with an annular protrusion 13d.
[0041] 9, a preform 15 can be formed by covering the inner preform 14 with the outer preform 13. In the preform 15, the mouth portion 14a faces the mouth portion 13a, and the body portion 14b faces the body portion 13b.
[0042] The mouth portions 13a and 14a become the mouth portion 15a of the preform 15, the body portions 13b and 14b become the body portion 15b of the preform 15, and the bottom portions 13c and 14c become the bottom portion 15c of the preform 15. The body portion 15b and the bottom portion 15c are primarily stretched in the biaxial stretch blow molding.
[0043] <Materials and manufacturing methods of inner preform 14, outer preform 13, and preform 15> The inner preform 14 and the outer preform 13 can be formed by direct blow molding, injection molding, or the like, of thermoplastic resins such as polyester (e.g., PET) and polyolefin (e.g., polypropylene, polyethylene). In one example, the inner preform 14 is made of polyolefin (e.g., polypropylene), and the outer preform 13 is made of PET. The polyolefin used for the inner preform 14 is preferably polypropylene rather than polyethylene. This is because the temperature suitable for biaxial stretch blow molding of polypropylene is closer to that of PET than that of polyethylene.
[0044] The preform 15 may be produced by separately producing the inner preform 14 and the outer preform 13, and then covering the inner preform 14 with the outer preform 13, or by multi-layer injection molding or two-color molding. Either method can be used to obtain the preform 15, which is formed by laminating the inner preform 14 and the outer preform 13.
[0045] In the multi-layer injection molding, a multi-layer preform 15 having layers corresponding to the inner preform 14 and the outer preform 13 can be manufactured in a single injection molding.
[0046] In two-color molding, one of the inner preform 14 and the outer preform 13 is molded in a first molding step, and the other of the inner preform 14 and the outer preform 13 is molded in a second molding step. The first molding step may be direct blow molding or injection molding. The second molding step is preferably injection molding.
[0047] <Biaxial stretch blow molding> In one example, biaxial stretch blow molding can be performed by a heating step, a first stretching step, and a second stretching step. The heating step can be performed using a heating device 35 shown in Fig. 10, and the first and second stretching steps can be performed using a blow molding device 36 shown in Figs. 11 to 13.
[0048] <Heating process> In the heating step, the preform 15 is heated and softened to a softened state. In one example, the heating step can be performed by placing the preform 15 close to a heater 32 while the preform 15 is attached to a mouth support mold 21 as shown in FIG. 10. The heating step is performed such that the body 15b and the bottom 15c are heated while the flange 15e provided on the preform 15 is covered with a heat shield 33. This softens the body 15b and the bottom 15c. On the other hand, the flange 15e and the mouth 15a covered with the heat shield 33 are not softened because little or no heat is applied from the heater 32. Furthermore, the portion 15f of the body portion 15b adjacent to the flange 15e is not easily softened because the heat from the heater 32 is blocked to some extent by the heat shield 33 and the heat from the heater 32 is easily dissipated to the flange 15e and the mouth portion 15a, which are relatively low in temperature even when the heat is applied from the heater 32. In one example, the preform 15 can be heated while being rotated. In one example, the heater 32 is composed of a plurality of rod-shaped heaters arranged along the side surface of the preform 15, but may have another configuration.
[0049] <First stretching process> In the first stretching step, the preform 15 is stretched along a first axial direction (i.e., vertical direction). The first axis is, for example, a direction parallel to the central axis C of the mouth portion 5, and is the up-down direction in FIG. 11. In one example, this step can be performed by setting the heated preform 15 in a molding die 23 as shown in FIG. 11, and pressing a stretching bar 25 against the inner bottom surface of the inner preform 14 to stretch it while the bottom portion 13c of the outer preform 13 is supported by a bottom supporting die 22 as shown in FIGS. 12 and 13. At this time, it is preferable to move the bottom supporting die 22 backward in synchronization with the stretching of the stretching bar 25. This allows the preform 15 to be stably stretched.
[0050] The preform 15 can be transferred from the heating device 35 to the blow molding device 36 while being supported by the mouth support mold 21. In the blow molding device 36, the mouth support mold 21 can be set on a pedestal 34. The first stretching step can be performed in a state where the mouth support mold 21 is in contact with the molding mold 23 by moving the pedestal 34 toward the molding mold 23. The molding mold 23 is composed of a split mold that can be opened and closed, and has a cavity surface 23a that corresponds to the outer surface shape of the container body 2.
[0051] <Second stretching process> In the second stretching step, air is blown into the inner preform 14 from the state shown in Fig. 13 to stretch (i.e. expand) the preform 15 in the second axial direction (i.e. lateral direction) and shape it into the shape of the cavity surface 23a, thereby obtaining the container body 2 shown in Fig. 2. Air can be blown in through the air passage 26 between the mouth support mold 21 and the stretch rod 25, but for example, an air passage may be provided in the stretch rod 25 so that air can be blown out from the side of the stretch rod 25.
[0052] Incidentally, the outer preform 13 has a portion where the wall thickness is significantly reduced during biaxial stretch blow molding, and a portion where the wall thickness is hardly reduced or not reduced at all. Here, a portion where the wall thickness reduction rate defined by (wall thickness of outer shell 3 / wall thickness of outer preform 13) for the corresponding portion is less than 10% is defined as a non-stretched portion, and a portion where the wall thickness reduction rate is 10% or more is defined as a stretched portion. The outer preform 13 has a non-stretched portion where the wall thickness reduction rate during biaxial stretch blow molding is less than 10% and a stretched portion where the wall thickness reduction rate is 10% or more.
[0053] Fig. 15 shows a molding die 23x as a comparative example of the present invention. By molding using this molding die 23x, a container body 2x as shown in Fig. 7 is obtained. In the adjacent region 15g on the bottom 15c side of the boundary B in Fig. 15A, the outer shapes of the outer preform 13 and the outer shell 3 match, so that the adjacent region 15g is not stretched in the second stretching step, but is stretched and thinned in the first stretching step. Then, by this thinning, an undercut portion 4u in which the inner bag 4 has a large thickness is formed, as described with reference to Fig. 7.
[0054] FIG. 14 shows a mold 23 according to an embodiment of the present invention. The mold 23 is different from the comparative example in that it has a protruding portion 23b extending in the circumferential direction at a position where the protruding portion abuts against the outer surface of the outer preform 13 in the adjacent portion 15g adjacent to the non-extended portion of the extended portion. By providing the protruding portion 23b on the mold 23, the constricted portion 3d shown in FIG. 6 is formed, and the inner bag 4 is thinned at the height position where the undercut portion 4u is provided. The protruding portion 23b may be provided in a part of the constricted portion 3d in the circumferential direction, but it is preferable to provide the protruding portion 23b on the entire circumference. The protruding portion 23b is preferably provided between the flange accommodating portion 23c that accommodates the flange 15e and the shoulder forming surface 23d for forming the shoulder 6b. It is preferable that there is a portion without the protruding portion 23b between the protruding portion 23b and the flange accommodating portion 23c. It is preferable that the protruding portion 23b is connected to the shoulder forming surface 23d without any step.
[0055] If the thickness of the outer preform 13 at the boundary B is Tb and the height of the protruding portion 23b is H, it is preferable that H / Tb is 0.1 to 0.8. If the protruding portion 23b is too low, the effect of reducing the thickness of the inner bag 4 at the height position where the undercut portion 4u is located may be insufficient. If the protruding portion 23b is too high, the constricted portion 3d becomes too deep, and the force required to separate the inner bag 4 by the constricted portion 3d may increase instead. The height H refers to the height of the boundary B from the adjacent region 23e on the open end side.
[0056] Tb is, for example, 0.8 to 2.0 mm, specifically, for example, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2.0 mm, or may be in a range between any two of the numerical values exemplified here. H is, for example, 0.2 to 1.0 mm, specifically, for example, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1.0 mm, or may be in a range between any two of the numerical values exemplified here.
[0057] 2. Other embodiments In the present invention, focusing on the fact that the thickness of the inner bag 4 is small at the height position where the undercut portion 4u is formed, the following can be specified. In this case, the constricted portion 3d is not essential. Instead of forming the constricted portion 3d, for example, the shape of the preform 15 can be changed to reduce the thickness of the inner bag 4 at the height position where the undercut portion 4u is formed.
[0058] A double container comprising an inner bag and a container body having an outer shell arranged to cover the inner bag, The inner bag is configured to be removable from the container body, A double container in which the thickness of the inner bag is 0.30 mm or less at a second height position 2.5 mm away from a first height position which is the starting point of an undercut portion that interferes with the outer shell when the inner bag is pulled out of the container body.
[0059] A double container comprising an inner bag and a container body having an outer shell arranged to cover the inner bag, The inner bag is configured to be removable from the container body, A double-walled container in which T2i is the thickness of the inner bag at a second height position 2.5 mm away from a first height position which is the starting point of an undercut portion that interferes with the outer shell when the inner bag is pulled out of the container body, and T3 is the average thickness of the inner bag within a height range of 5 mm from the first height position toward the opening end of the container body, such that T2i / T3 is 0.60 or less.
[0060] Moreover, in view of the provision of the constricted portion 3d between the flange 5b and the shoulder portion 6b, the present invention can be defined as follows.
[0061] A double container comprising an inner bag and a container body having an outer shell arranged to cover the inner bag, The inner bag is configured to be removable from the container body, the container body includes a mouth portion, a body portion, and a bottom portion, the mouth portion being a tubular portion having an open end, the body portion being disposed adjacent to the mouth portion on a side farther from the open end than the mouth portion and having an outer diameter larger than that of the mouth portion, and the bottom portion being configured to close a lower end of the body portion, The body portion has a shoulder portion whose outer diameter increases with increasing distance from the mouth portion, The mouth portion is provided with a flange, A double container having a constriction between the flange and the shoulder.
[0062] Furthermore, in view of the fact that the protrusion 23b is provided between the flange accommodating portion 23c that accommodates the flange 15e of the preform 15 and the shoulder forming surface 23d for forming the shoulder 6b, the present invention can be defined as follows.
[0063] A method for producing a double-layer container, comprising a step of producing a container body by biaxially stretching and blow molding a preform using a molding die, The container body has an inner bag and an outer shell arranged to cover the inner bag, The preform includes an inner preform corresponding to the inner bag and an outer preform corresponding to the outer shell, The outer preform has a non-stretched portion having a wall thickness reduction rate of less than 10% during the biaxial stretch blow molding, and a stretched portion having a wall thickness reduction rate of 10% or more; The method according to the present invention, wherein the mold has a flange receiving portion that receives the flange of the preform and a shoulder forming surface for forming a shoulder of the container body, and has a circumferentially extending protrusion at a position between the flange receiving portion and the shoulder forming surface that abuts against the outer surface of the outer preform. EXAMPLES
[0064] 1. Manufacturing of container body and thickness measurement <Example 1> The above-mentioned biaxial stretch blow molding was carried out using the preform 15 having the shape shown in Fig. 16 and the device having the structure shown in Fig. 10 to Fig. 14, to obtain the container body 2 (capacity 300 mL) having the shape shown in Fig. 1 to Fig. 6. The thickness of the inner preform 14 was about 0.7 mm within a range of 20 to 40 mm from the open end of the preform 15. The thickness of the outer preform 13 was about 1.9 mm at a position 20 mm away from the open end of the preform 15, and about 1.3 mm within a range of 27.5 to 40 mm.
[0065] The inner preform 14 was produced by direct blow molding a propylene-ethylene random copolymer (type: Wintec, manufactured by Japan Polypropylene). The outer preform 13 was produced by injection molding PET (type: titanium-based catalyst grade, manufactured by Teijin) at 300°C to form the shape of the outer preform, and then quenching to 20°C. The PET in a molten state was made amorphous by quenching. In the heating step, the preform 15 was heated to 110°C (the temperature at the center of the longitudinal direction of the preform 15). The height of the protruding portion 23b and the depth of the constricted portion 3d were each 0.5 mm. The protruding portion 23b was provided so that the distance in the first axial direction from the opening end of the preform 15 to the top surface of the protruding portion 23b was 31.6 mm when the preform 15 was set in the mold 23.
[0066] Next, the distance from the opening end 5c of the obtained container body 2 was changed in various ways, and the wall thickness was measured at each measurement position. The wall thickness was measured using a micrometer at two points at an angle of 90 degrees from the parting line, and the average value was calculated. The relationship between the cross-sectional shape of the container body 2 and the measurement positions is shown in FIG. 17. FIG. 17 is a diagram that reproduces the shape of the container body 2 in a photograph taken after cutting the obtained container body 2.
[0067] [Table 1]
[0068] 17, it can be seen that the first height position H1, which is the starting point of the undercut portion 4u, is located 32.5 mm away from the open end 5c. Referring to Table 1, the wall thickness T1o of the outer shell 3 at the first height position H1 is 1.178 mm, and as described above, the depth D of the constricted portion 3d is 0.5 mm, so that D / T1o is 0.34.
[0069] The second height position H2, which is 2.5 mm farther from the opening edge 5c than the first height position H1, is 35.0 mm from the opening edge 5c, and the thickness T2i of the inner bag 4 at this position is 0.165 mm. The range of 5 mm from the first height position H1 to the opening edge 5c side is 27.5 to 32.5 mm, and the average thickness T3 of the inner bag 4 within this range is 0.357 mm, so T2i / T3 is 0.46.
[0070] Furthermore, when comparing the thickness of the shell 3 in Table 1 with the thickness of the outer preform 13, it is found that the thickness reduction rate is about 5% at a distance of 3.0 mm from the open end 5c, and about 10% at a distance of about 32.5 mm. And, since the protrusion 23b is provided from a position 31.6 mm from the open end to the shoulder forming surface 23d, it is found that it is provided at a position abutting the outer surface of the outer preform 13 at an adjacent portion of the extended portion of the outer preform 13 adjacent to the non-extended portion.
[0071] <Comparative Example 1> A container body 2x was produced and its wall thickness was measured in the same manner as in Example 1, except that the mold 23 was changed to a mold 23x shown in Fig. 15. The results are shown in Table 2. Fig. 7 is a diagram that reproduces the shape of the container body 2x in a photograph taken by cutting the container body 2x obtained in Comparative Example 1.
[0072] [Table 2]
[0073] In Comparative Example 1, the thickness of the outer shell 3 decreases rapidly from a position 30.0 mm away from the open end 5c, and this position is the first height position H1, which is the starting point of the undercut portion. Referring to Table 2, the second height position H2, which is 2.5 mm away from the open end 5c than the first height position H1, is a position 32.5 mm from the open end 5c, and the thickness T2i of the inner bag 4 at this position is 0.343 mm. In addition, the range of 5 mm from the first height position H1 to the open end 5c is a range of 25.0 to 30.0 mm, and the average thickness T3 of the inner bag 4 within this range is 0.491 mm, so T2i / T3 is 0.70.
[0074] <Consideration> In Example 1, the wall thickness of the inner bag 4 at the second height position H2 was smaller than that in Comparative Example 1, and the value of T2i / T3 was smaller.
[0075] 2. Torque measurement The cap 8a of the above embodiment was attached to the mouth 5 of the container body 2, 2x of the examples and comparative examples, and the peak value when the cap 8a was rotated 180 degrees counterclockwise (in the direction in which the inner bag 4 is rotated when separating it from the container body 2, 2x) with the container body 2, 2x fixed, was recorded as the rotation torque. This rotation torque corresponds to the force required to pull out the inner bag 4 from the container body 2, 2x. Five measurement samples were prepared for each of the examples and comparative examples, and measurements were performed on each. The results are shown in Table 3.
[0076] Referring to Table 3, it was found that in Example 1, the rotation torque was smaller than in Comparative Example 1, and the force required to separate the inner bag 4 from the container body 2 was reduced.
[0077] [Table 3] [Explanation of symbols]
[0078] 1:Double container 2: Container body 2x: Container body of comparative example 3: Outer shell 3a: Open end 3b:Inner surface 3c: External surface 3d: Neck 3l: Cam rail 3m: Engagement recess 4: Inner bag 4c:Protrusion 4c1:Protruding tube 4c2: Engagement convex part 4c3: Tapered surface 4c4: Abutting flange 4c5: Circular convex part 4c8: Tapered surface 4d: Inner bag body 4g: Cam protrusion 4m: Engagement part 4u: Undercut section 4v: External 5: Mouth 5b: Flange 5c: Open end 5d: 1st area 5e: 2nd area 5e: 2nd area 6: Torso 6b:Shoulder 6c: Main body 7: Bottom 8: Mouth attachment member 8a: Cap 13: Outer preform 13a: Mouth 13b: Torso 13c: Bottom 13d: Annular protrusion 14: Inner preform 14a: Mouth 14b: Torso 14c: Bottom 14d:Protrusion 14m: Engagement part 15: Preform 15a: Mouth 15b: Torso 15c: bottom 15e: Flange 15f: part 15g: adjacent area 21: Mouth support type 22: Bottom support type 23: Molding mold 23x: Comparative example mold 23a: Cavity surface 23b:Protrusion 23c: Flange receiving section 23d: Shoulder formation surface 23e: Adjacent areas 25: Stretching rod 26: Air passage 31: Cam mechanism 31a: End face 32: Heater 33: Heat shielding section 34: Pedestal 35: Heating device 36: Blow molding equipment B : Boundary C: Central axis H1: First height position H2: Second height position Ha: Height position where thickness reduction begins
Claims
1. A double container comprising an inner bag and a container body having an outer shell arranged to cover the inner bag, The inner bag is configured to be removable from the container body, The double container has a constricted portion on the outer surface of the outer shell at a first height position which is the starting point of an undercut portion that interferes with the outer shell when the inner bag is pulled out of the container body.
2. A double container comprising an inner bag and a container body having an outer shell arranged to cover the inner bag, The inner bag is configured to be removable from the container body, the container body includes a mouth portion, a body portion, and a bottom portion, the mouth portion being a tubular portion having an open end, the body portion being disposed adjacent to the mouth portion on a side farther from the open end than the mouth portion and having an outer diameter larger than that of the mouth portion, and the bottom portion being configured to close a lower end of the body portion, The body portion has a shoulder portion whose outer diameter increases with increasing distance from the mouth portion, The mouth portion is provided with a flange, A double container having a constriction between the flange and the shoulder.
3. The double container according to claim 1 or 2, The double container has a wall thickness of the outer shell at a first height position of T1o and a depth of the constricted portion of D, where D / T1o is 0.1 to 0.
8.
4. The double container according to claim 1 or 2, The depth of the constricted portion is 0.2 to 1.0 mm.
5. The double container according to claim 1 or 2, A double container, wherein the thickness of the inner bag at a second height position 2.5 mm away from the opening end of the container body from the first height position is 0.30 mm or less.
6. The double container according to claim 1 or 2, A double container in which T2i is the thickness of the inner bag at a second height position 2.5 mm away from the opening end of the container body from the first height position, and T3 is the average thickness of the inner bag within a height range of 5 mm from the first height position to the opening end of the container body, such that T2i / T3 is 0.60 or less.
7. A double container comprising an inner bag and a container body having an outer shell arranged to cover the inner bag, The inner bag is configured to be removable from the container body, A double container in which the thickness of the inner bag is 0.30 mm or less at a second height position 2.5 mm away from a first height position which is the starting point of an undercut portion that interferes with the outer shell when the inner bag is pulled out of the container body.
8. A double container comprising an inner bag and a container body having an outer shell arranged to cover the inner bag, The inner bag is configured to be removable from the container body, A double container in which T2i is the thickness of the inner bag at a second height position 2.5 mm away from a first height position which is the starting point of an undercut portion that interferes with the outer shell when the inner bag is pulled out of the container body, and T3 is the average thickness of the inner bag within a height range of 5 mm from the first height position toward the opening end of the container body, such that T2i / T3 is 0.60 or less.
9. A method for producing a double-walled container, comprising the step of producing a container body by biaxially stretching and blow molding a preform using a mold, The container body has an inner bag and an outer shell arranged to cover the inner bag, The preform includes an inner preform corresponding to the inner bag and an outer preform corresponding to the outer shell, The outer preform has a non-stretched portion having a wall thickness reduction rate of less than 10% during the biaxial stretch blow molding, and a stretched portion having a wall thickness reduction rate of 10% or more; The mold has a protrusion extending in a circumferential direction at a position where the protrusion abuts against the outer surface of the outer preform at an adjacent portion of the extended portion adjacent to the non-extended portion.
10. A method for producing a double-walled container, comprising the step of producing a container body by biaxially stretching and blow molding a preform using a mold, The container body has an inner bag and an outer shell arranged to cover the inner bag, The preform includes an inner preform corresponding to the inner bag and an outer preform corresponding to the outer shell, The outer preform has a non-stretched portion having a wall thickness reduction rate of less than 10% during the biaxial stretch blow molding, and a stretched portion having a wall thickness reduction rate of 10% or more; The method according to the present invention, wherein the mold has a flange receiving portion that receives the flange of the preform and a shoulder forming surface for forming a shoulder of the container body, and has a circumferentially extending protrusion at a position between the flange receiving portion and the shoulder forming surface that abuts against the outer surface of the outer preform.
11. 11. The method of claim 9 or claim 10, The height of the protrusion is 0.2 to 1.0 mm.
Citation Information
Patent Citations
Method for molding double container
JP2019010741A