Copolymer composition for conveyor belts and applications thereof

A copolymer composition for conveyor belts, combining ethylene/α-olefin/non-conjugated polyene and ethylene/α-olefin/5-vinyl-2-norbornene copolymers, addresses the need for improved heat aging and abrasion resistance, offering high rigidity and oil bleed resistance in high-temperature applications.

JP2024141020AInactive Publication Date: 2024-10-10MITSUI CHEMICALS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052446
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conveyor belts used in high-temperature environments require improved heat aging resistance and abrasion resistance to minimize maintenance and extend service life, with a need for higher abrasion resistance than conventional rubber compositions.

Method used

A copolymer composition comprising ethylene/α-olefin/non-conjugated polyene copolymers, ethylene/α-olefin copolymers, carbon black, anti-aging agents, and ethylene/α-olefin/5-vinyl-2-norbornene copolymers, formulated to achieve high modulus, excellent oil bleed resistance, and enhanced heat aging and abrasion resistance.

Benefits of technology

The copolymer composition provides high rigidity, excellent oil bleed resistance, and maintains processability while ensuring superior heat aging and abrasion resistance, making it suitable for high-temperature conveyor belts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141020000001
    Figure 2024141020000001
  • Figure 2024141020000002
    Figure 2024141020000002
  • Figure 2024141020000003
    Figure 2024141020000003
Patent Text Reader

Abstract

To provide a copolymer composition for conveyor belts that is suitable for producing a conveyor belt with high modulus (high rigidity) and superior oil bleeding resistance, as well as superior resistance to thermal aging and wear.SOLUTION: The present invention relates to a copolymer composition for conveyor belts that contains the following components (S), (F), (G), (H) and (R). Component (S): an ethylene α-olefin nonconjugated polyene copolymer (S) that fulfills specific requirements. Component (F): an ethylene α-olefin copolymer (F). Component (G): carbon black (G). Component (H): an aging resister (H). Component (R): an ethylene α-olefin 5-vinyl-2-norbornene copolymer (R) that fulfills specific requirements.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copolymer composition for use in a conveyor belt, which has excellent processability, mechanical properties, heat aging resistance and abrasion resistance. [Background technology]

[0002] In various industrial fields such as steel, coal, and cement, belt conveyor devices are used as a means of transporting goods, and in particular, there are many cases where high-temperature goods such as clinker, which are about 150 to 250°C, are transported by belt conveyor devices. In view of this situation, there is a demand for conveyor belts with excellent heat aging resistance and wear resistance in order to minimize maintenance work and extend the service life.

[0003] As a method for improving the heat aging resistance, abrasion resistance, etc. of conveyor belts, it has been proposed to use a rubber composition containing an ethylene-1-octene copolymer and an ethylene-propylene copolymer (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-246017 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in recent years, there has been an increasing demand for higher abrasion resistance in conveyor belts, and it is desired that rubber compositions for heat-resistant conveyor belts that replace conventional products maintain or exceed the heat resistance, mechanical properties, and processability of conventional products.

[0006] An object of the present invention is to obtain a copolymer composition for a conveyor belt which is suitable for obtaining a conveyor belt having a high modulus (high rigidity), excellent oil-bleed resistance, and good resistance to heat aging and abrasion. [Means for solving the problem]

[0007] The present invention relates to the following items [1] to [8]. [1] A copolymer composition for a conveyor belt, comprising the following components (S), (F), (G), (H) and (R): Ingredients (S): An ethylene-α-olefin-non-conjugated polyene copolymer (S) having structural units derived from ethylene (A), an α-olefin (B) having 3 to 20 carbon atoms, and a non-conjugated polyene (C) containing in the molecule a total of two or more partial structures selected from the group consisting of the following general formulas (I) and (II), and satisfying the following requirements (i) to (v): (i) The molar ratio of ethylene / α-olefin is 40 / 60 to 99.9 / 0.1. (ii) The weight fraction of the constitutional units derived from the non-conjugated polyene (C) is 0.07% by weight to 10% by weight in 100% by weight of the ethylene-α-olefin-non-conjugated polyene copolymer. (iii) The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer, the weight fraction of the constitutional unit derived from the non-conjugated polyene (C) (weight fraction (wt%) of (C)), and the molecular weight of the non-conjugated polyene (C) (molecular weight of (C)) satisfy the following formula (1). 4.5≦Mw×weight fraction of (C) / 100 / molecular weight of (C)≦80 Equation (1) (iv) The ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, which are obtained by linear viscoelastic measurement (190°C) using a rheometer, the intrinsic viscosity [η], and the weight fraction of the constituent units derived from the non-conjugated polyene (C) (weight fraction of (C)), satisfy the following formula (2): P / ([η] 2.9 ) ≦ Weight fraction of (C) × 6 Equation (2) (v) The number of long chain branches per 1,000 carbon atoms (LCB1000C) and the natural logarithm of the weight average molecular weight (Mw) [Ln(Mw)] obtained using 3D-GPC satisfy the following formula (3). LCB 1000C ≦1-0.07×Ln(Mw)···Equation (3)

[0008] [ka]

[0009] Component (F): Ethylene-α-olefin copolymer (F) Component (G); Carbon black (G) Ingredient (H); Anti-aging agent (H) Component(R); Ethylene / α-olefin / 5-vinyl-2-norbornene copolymer (R) satisfying the following requirements (1) to (6): (1) The weight average molecular weight is in the range of 1,000 to 50,000. (2) The molecular weight distribution (Mw / Mn, Mw: weight average molecular weight, Mn: number average molecular weight) measured by gel permeation chromatography (GPC) is 2.7 or less. (3) 13 The intensity ratio Tαβ / Tαα of the C-NMR spectrum is 0.0 to 0.1. (4) The content of structural units derived from 5-vinyl-2-norbornene is in the range of 0.1 to 20.0 mass %. (5) The structural units derived from 5-vinyl-2-norbornene contain an endo structure and an exo structure, and the ratio of the endo structure / exo structure is 2.5 or less. (6) The intrinsic viscosity [η] measured in decahydronaphthalene at 135°C is in the range of 0.01 to 0.8 dl / g.

[0010] [2] The copolymer composition for a conveyor belt according to item [1], wherein the ethylene-α-olefin-5-vinyl-2-norbornene copolymer (R) as the component (R) further satisfies the following requirement (7): (7) The B value represented by the following formula (i) is 1.10 or more. B value=([EX]+2[Y]) / [2×[E]×([X]+[Y])]···(i) [where [E], [X] and [Y] represent the mole fractions of ethylene, α-olefin and 5-vinyl-2-norbornene, respectively, and [EX] represents the ethylene-α-olefin dyad chain fraction.]

[0011] [3] The copolymer composition for a conveyor belt according to item [1], further comprising the following component (J): (J) Organic peroxide crosslinking agent

[0012] [4] The copolymer composition for a conveyor belt according to any one of Items [1] to [3], wherein the ethylene-α-olefin-non-conjugated polyene copolymer (S) as the component (S) further has an intrinsic viscosity [η] of 0.1 to 5 dL / g and a weight average molecular weight (Mw) of 10,000 to 600,000.

[0013] [5] The copolymer composition for a conveyor belt according to any one of Items [1] to [4], wherein the non-conjugated polyene (C) constituting the ethylene-α-olefin-non-conjugated polyene copolymer (S), which is the component (S), is 5-vinyl-2-norbornene (VNB).

[0014] [6] The copolymer composition for a conveyor belt according to any one of items [1] to [5], wherein the ethylene-α-olefin-non-conjugated polyene copolymer (S) as the component (S) further contains a constitutional unit derived from a non-conjugated polyene (D) containing only one partial structure selected from the group consisting of the formulae (I) and (II) in the molecule in a weight fraction of 0 to 20% by weight (wherein the total weight fractions of (A), (B), (C) and (D) is 100% by weight), and satisfies the requirement (vi) below; (vi) The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer, the weight fraction of the constituent unit derived from the non-conjugated polyene (C) (weight fraction (wt%) of (C)), the weight fraction of the constituent unit derived from the conjugated polyene (D) (weight fraction (wt%) of (D)), the molecular weight of the non-conjugated polyene (C) (molecular weight of (C)), and the molecular weight of the conjugated polyene (D) (molecular weight of (D)) satisfy the following formula (4): 4.5≦Mw×{(weight fraction of (C) / 100 / molecular weight of (C))+(weight fraction of (D) / 100 / molecular weight of (D))}≦45...Equation (4)

[0015] [7] Item [3]. A copolymer composition for a conveyor belt according to Item [3], comprising 95 to 5 parts by mass of the component (S), 5 to 95 parts by mass of the component (F), and 5 to 120 parts by mass of the component (G), 0.1 to 20 parts by mass of the component (H), and 0.1 to 20 parts by mass of the component (R) per 100 parts by mass of the total amount of the components (S) and (F).

[0016] [8] A heat-resistant conveyor belt obtained by using the copolymer composition for conveyor belts according to any one of items [1] to [7]. Effect of the Invention

[0017] The rubber composition for conveyor belts of the present invention has high rigidity and excellent oil-bleeding resistance while maintaining processability, heat aging resistance, and abrasion resistance, and is therefore useful as a raw material for conveyor belts, and heat-resistant conveyor belts can be obtained from the composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] <Ethylene-α-olefin-non-conjugated polyene copolymer (S)> An ethylene-α-olefin-non-conjugated polyene copolymer (S) (hereinafter may be abbreviated as "component (S)" or "copolymer (S)"), which is one of the components contained in the copolymer composition for conveyor belts of the present invention (hereinafter may be abbreviated as "copolymer composition"), has constitutional units derived from ethylene (A), an α-olefin (B) having 3 to 20 carbon atoms, and a non-conjugated polyene (C) containing, in the molecule, two or more partial structures selected from the group consisting of the following general formulae (I) and (II):

[0019] [ka]

[0020] The component (S) according to the present invention may further have a structural unit derived from a non-conjugated polyene (D) containing in the molecule only one partial structure selected from the group consisting of the general formulae (I) and (II) in addition to the structural units derived from the above (A), (B), and (C).

[0021] Examples of the α-olefin (B) having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-eicosene. Among these, α-olefins having 3 to 8 carbon atoms such as propylene, 1-butene, 1-hexene, and 1-octene are preferred, and propylene is particularly preferred. Such α-olefins are preferred because the raw material cost is relatively low, the resulting copolymer composition for conveyor belts exhibits excellent mechanical properties, and a conveyor belt having rubber elasticity can be obtained. These α-olefins may be used alone or in combination.

[0022] Component (S) according to the present invention contains structural units derived from at least one type of α-olefin (B) having 3 to 20 carbon atoms, and may contain structural units derived from two or more types of α-olefins (B) having 3 to 20 carbon atoms.

[0023] Examples of the non-conjugated polyene (C) containing two or more partial structures selected from the group consisting of the general formulae (I) and (II) in the molecule in total include 5-vinyl-2-norbornene (VNB), norbornadiene, 1,4-hexadiene, and dicyclopentadiene. Among these, it is preferable that the non-conjugated polyene (C) contains VNB, and it is more preferable that the non-conjugated polyene (C) is VNB, because it is highly available, has good reactivity with peroxide during crosslinking reaction after polymerization, and is likely to improve the heat resistance of the copolymer composition for conveyor belts. The non-conjugated polyene (C) may be used alone or in combination of two or more kinds.

[0024] The component (S) according to the present invention may contain, in addition to the structural units derived from ethylene (A), the α-olefin (B) having 3 to 20 carbon atoms, and the non-conjugated polyene (C), a structural unit derived from a non-conjugated polyene (D) containing in the molecule only one partial structure selected from the group consisting of the general formulae (I) and (II). Examples of such non-conjugated polyenes (D) include 5-ethylidene-2-norbornene (ENB), 5-methylene-2-norbornene, 5-(2-propenyl)-2-norbornene, 5-(3-butenyl)-2-norbornene, 5-(1-methyl-2-propenyl)-2-norbornene, 5-(4-pentenyl)-2-norbornene, 5-(1-methyl-3-butenyl)-2-norbornene, 5-(5-hexenyl)-2-norbornene, 5-(1-methyl-4-pentenyl)-2-norbornene, 5-(2,3-dimethyl-3-butenyl)-2-norbornene, 5-(2-ethyl-3-butenyl)-2-norbornene, 5-(6-heptenyl)-2-norbornene, 5-(3-methyl-5-hexenyl)-2-norbornene, 5-(3,4-dimethyl-4-pentenyl)-2-norbornene, 5-(3-ethyl-4-pentenyl)-2-norbornene, 5-(7-octenyl)-2-norbornene, 5-(2-methyl-6-heptenyl)-2-norbornene, 5-(1,2-dimethyl-5-hexenyl)-2-norbornene, 5-(5-ethyl-5-hexenyl)-2-norbornene, 5-(1,2,3-trimethyl-4-pentenyl)-2-norbornene, and the like. Among these, ENB is preferred because it is easily available, has high reactivity with crosslinking agents and crosslinking accelerators such as organic peroxides and sulfur during the crosslinking reaction after polymerization, is easy to control the crosslinking rate, and is easy to obtain good mechanical properties. The non-conjugated polyene (D) may be used alone or in combination of two or more kinds.

[0025] When the component (S) according to the present invention contains a structural unit derived from a non-conjugated polyene (D) containing only one partial structure selected from the group consisting of the general formulae (I) and (II) in the molecule, the proportion thereof is not particularly limited as long as it does not impair the object of the present invention, but is usually contained in a weight fraction of about 0 to 20% by weight, preferably 0 to 8% by weight, and more preferably 0.01 to 8% by weight (wherein the total weight fractions of (A), (B), (C), and (D) is taken as 100% by weight).

[0026] As described above, the component (S) according to the present invention is a copolymer having structural units derived from ethylene (A), an α-olefin (B) having 3 to 20 carbon atoms, the non-conjugated polyene (C), and, if necessary, the non-conjugated polyene (D), and satisfies the following requirements (i) to (v).

[0027] [Requirement (i)] The molar ratio of ethylene / α-olefin is 40 / 60 to 99.9 / 0.1.

[0028] [Requirement (ii)] The weight fraction of the constitutional units derived from the non-conjugated polyene (C) is 0.07% by weight to 10% by weight.

[0029] [Requirement (iii)] The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer (S), the weight fraction of the constitutional unit derived from the non-conjugated polyene (C) (weight fraction (wt%) of (C)), and the molecular weight of the non-conjugated polyene (C) (molecular weight of (C)) satisfy the following formula (1). 4.5≦Mw×weight fraction of (C) / 100 / molecular weight of (C)≦80 Equation (1)

[0030] [Requirement (iv)] Complex viscosity η at frequency ω = 0.1 rad / s obtained by linear viscoelastic measurements (190 °C) using a rheometer * ( ω =0.1) (Pa sec) and the complex viscosity η at frequency ω = 100 rad / s * ( ω=100) (Pa sec) * ( ω =0.1) / η * ( ω =100) ), the intrinsic viscosity [η], and the weight fraction of the constitutional unit derived from the non-conjugated polyene (C) (weight fraction of (C)) satisfy the following formula (2). P / ([η] 2.9 ) ≦ Weight fraction of (C) × 6 Equation (2)

[0031] [Requirement (v)] The number of long chain branches (LCB) per 1000 carbon atoms obtained using 3D-GPC 1000C ) and the natural logarithm of the weight average molecular weight (Mw) [Ln(Mw)] satisfy the following formula (3). LCB 1000C ≦1-0.07×Ln(Mw)···Equation (3) In this specification, "α-olefin having 3 to 20 carbon atoms" may also be simply referred to as "α-olefin".

[0032] [Requirement (i)] Requirement (i) specifies that the molar ratio of ethylene / α-olefin in component (S) according to the present invention satisfies 40 / 60 to 99.9 / 0.1, and this molar ratio preferably satisfies 50 / 50 to 90 / 10, more preferably 55 / 45 to 85 / 15, and further preferably 55 / 45 to 78 / 22. When such an ethylene / α-olefin / non-conjugated polyene copolymer (S) according to the present invention is used as a raw material for a crosslinked molded article, the resulting crosslinked molded article exhibits excellent rubber elasticity and is excellent in mechanical strength and flexibility, which is preferable.

[0033] The amount of ethylene (the amount of structural units derived from ethylene (A)) and the amount of α-olefin (the amount of structural units derived from α-olefin (B)) in component (S) are 13 It can be determined by C-NMR.

[0034] [Requirement (ii)] Requirement (ii) specifies that the weight fraction of the constituent units derived from the non-conjugated polyene (C) in the component (S) according to the present invention is in the range of 0.07 to 10% by weight in 100% by weight of the ethylene-α-olefin-non-conjugated polyene copolymer (S) (i.e., in the total weight fraction of all the constituent units, 100% by weight). The weight fraction of the constituent units derived from the non-conjugated polyene (C) is preferably 0.1 to 8.0% by weight, more preferably 0.5 to 5.0% by weight.

[0035] If the component (S) according to the present invention satisfies the requirement (ii), then the component (S) according to the present invention will have sufficient hardness and excellent mechanical properties, which is preferable, and when crosslinked using a peroxide, it will exhibit a fast crosslinking rate, and the component (S) according to the present invention will be suitable for producing a crosslinked molded article, which is preferable. The amount of non-conjugated polyene (C) in component (S) (the content of constitutional units derived from non-conjugated polyene (C)) is 13 It can be determined by C-NMR.

[0036] [Requirement (iii)] Requirement (iii) specifies that in component (S) according to the present invention, the weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer, the weight fraction of the constituent units derived from the non-conjugated polyene (C) in the copolymer (weight fraction of (C): weight %), and the molecular weight of the non-conjugated polyene (C) (molecular weight of (C)) satisfy the following relationship (1). 4.5≦Mw×weight fraction of (C) / 100 / molecular weight of (C)≦80 Equation (1)

[0037] When the component (S) according to the present invention satisfies the requirement (iii), the content of the structural unit derived from the non-conjugated polyene (C) such as VNB is appropriate, and sufficient crosslinking performance is exhibited. In addition, when a conveyor belt is produced using a copolymer composition containing the component (S) according to the present invention, the crosslinking rate is excellent and the conveyor belt after crosslinking exhibits excellent mechanical properties, which is preferable.

[0038] It is more preferable that the component (S) according to the present invention satisfies the following relational formula (1'). 4.5≦Mw×weight fraction of (C) / 100 / molecular weight of (C)≦75...Equation (1') The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer (S) refers to the value measured by 3D-GPC.

[0039] When the "Mw × weight fraction of (C) / 100 / molecular weight of (C)" of the component (S) according to the present invention satisfies the above formula (1) or (1'), the degree of crosslinking is appropriate, and by using this, molded articles with excellent balance between mechanical properties and heat aging resistance can be produced. If the "Mw × weight fraction of (C) / 100 / molecular weight of (C)" is too low, the crosslinking property may be insufficient and the crosslinking rate may be slow, and if it is too high, excessive crosslinking may occur, resulting in deterioration of mechanical properties.

[0040] [Requirement (iv)] Requirement (iv) is the complex viscosity η of the component (S) according to the present invention at a frequency ω=0.1 rad / s obtained by linear viscoelasticity measurement (190° C.) using a rheometer. * ( ω =0.1) (Pa sec) and the complex viscosity η at frequency ω = 100 rad / s * ( ω =100) (Pa sec) * ( ω =0.1) / η * ( ω =100) ), the intrinsic viscosity [η], and the weight fraction of the structural unit derived from the non-conjugated polyene (C) (weight fraction of (C): weight %) satisfy the following formula (2). P / ([η] 2.9 ) ≦ Weight fraction of (C) × 6 Equation (2)

[0041] Here, the complex viscosity η at frequency ω=0.1rad / s * ( ω =0.1)and the complex viscosity η at frequency ω=100rad / s * ( ω =100) Relative to P(η * ( ω =0.1) / η * ( ω =100) ) represents the frequency dependence of viscosity and is the left side of equation (2), P / ([η] 2.9 ) tends to show a high value when there are many long chain branches, although it is influenced by short chain branches and molecular weight. In general, in an ethylene-α-olefin-non-conjugated polyene copolymer, the more constitutional units derived from non-conjugated polyenes are contained, the more long chain branches are contained. However, it is considered that the component (S) according to the present invention satisfies the above formula (2) by having less long chain branches than the conventionally known ethylene-α-olefin-non-conjugated polyene copolymers. In the present invention, the P value is calculated as the ratio (η* ratio) of the complex viscosity at 0.1 rad / s and the complex viscosity at 100 rad / s, which are measured by using a viscoelasticity measuring device Ares (manufactured by Rheometric Scientific) under conditions of 190°C, strain 1.0%, and various frequencies.

[0042] The component (S) according to the present invention preferably satisfies the following formula (2'). P / ([η] 2.9 ) ≦ Weight fraction of (C) × 5.7 Equation (2') The intrinsic viscosity [η] means a value measured in decalin at 135°C.

[0043] [Requirement (v)] Requirement (v) is the number of long chain branches (LCB) per 1,000 carbon atoms of component (S) obtained by 3D-GPC. 1000C ) and the natural logarithm of the weight average molecular weight (Mw) [Ln(Mw)] satisfy the following formula (3). LCB 1000C ≦1-0.07×Ln(Mw)···Equation (3)

[0044] The upper limit of the long chain branch content per unit carbon number of component (S) is specified by the above formula (3). Such a component (S) is preferred because it contains a small proportion of long chain branches, has excellent curing properties when crosslinked using a peroxide, and provides a conveyor belt obtained by using this component with excellent heat aging resistance.

[0045] The component (S) according to the present invention preferably satisfies the following formula (3'). LCB 1000C ≦1-0.071×Ln(Mw)...Equation (3') Here, Mw and the number of long chain branches (LCB) per 1000 carbon atoms 1000C ) can be determined by a structural analysis method using 3D-GPC. In this specification, it was specifically determined as follows.

[0046] The absolute molecular weight distribution was measured using a 3D-high temperature GPC device PL-GPC220 (Polymer Laboratories), and the intrinsic viscosity was measured using a viscometer. The main measurement conditions were as follows: Detector: Differential refractometer / GPC device built-in 2-angle light scattering photometer PD2040 type (manufactured by Precison Detectors) Bridge type viscometer PL-BV400 (Polymer Laboratories) Column: TSKgel GMH HR -H(S)HT x 2 + TSKgel GMH HR -M(S)×1 piece (Each piece has an inner diameter of 7.8 mm and a length of 300 mm) Temperature: 140℃ Mobile phase: 1,2,4-trichlorobenzene (containing 0.025% BHT) Injection volume: 0.5mL Sample concentration: ca 1.5mg / mL Sample filtration: Filtration through a sintered filter with a pore size of 1.0 μm The dn / dc value required to determine the absolute molecular weight was determined for each sample from the dn / dc value of standard polystyrene (molecular weight 190,000), 0.053, and the response intensity of the differential refractometer per unit injected mass.

[0047] The long chain branching parameter g'i for each eluted component was calculated from the relationship between the intrinsic viscosity obtained from the viscometer and the absolute molecular weight obtained from the light scattering photometer using formula (v-1).

[0048]

number

[0049] Here, [η] = KM v The relational equation of v = 0.725 was applied. M is the absolute molecular weight value obtained by 3D-GPC, and K is the viscosity coefficient. Further, the average values ​​of g' were calculated from the following formulas (v-2), (v-3), and (v-4). Note that a trendline assuming the presence of only short chain branches was determined for each sample.

[0050]

number

[0051] Furthermore, using g'w, the number of branch points per molecular chain, BrNo, and the number of long chain branches per 1000 carbon atoms, LCB, 1000C The branching degree λ per unit molecular weight was calculated. BrNo was calculated using the Zimm-Stockmayer formula (v-5). 1000C Equations (v-6) and (v-7) were used to calculate and λ. g is the long chain branching parameter calculated from the radius of gyration Rg, and the following simple correlation is made between g' calculated from the intrinsic viscosity. Various values ​​have been proposed for ε in the equation depending on the shape of the molecule. Here, calculations were performed assuming ε=1 (i.e. g'=g).

[0052]

number

[0053] λ = BrNo / M (V-6) LCB 1000C =λ × 14000 (V-7) *In formula (V-7), 14,000 represents the molecular weight of 1,000 methylene (CH2) units.

[0054] The component (S) according to the present invention preferably has an intrinsic viscosity [η] of 0.1 to 5 dL / g, more preferably 0.5 to 5.0 dL / g, and even more preferably 0.9 to 4.0 dL / g.

[0055] Furthermore, the component (S) according to the present invention preferably has a weight average molecular weight (Mw) of 10,000 to 600,000, more preferably 30,000 to 500,000, and even more preferably 50,000 to 400,000.

[0056] The component (S) according to the present invention preferably satisfies both of the above-mentioned intrinsic viscosity [η] and weight average molecular weight (Mw). In the component (S) according to the present invention, the non-conjugated polyene (C) preferably contains VNB, and more preferably is VNB. That is, in the above-mentioned formula (1), formula (2) and formula (4) described later, it is preferable that the "weight fraction of (C)" is the "weight fraction of VNB" (% by weight).

[0057] As described above, in addition to the structural units derived from the above (A), (B) and (C), the component (S) according to the present invention also preferably contains a structural unit derived from a non-conjugated polyene (D) containing only one partial structure selected from the group consisting of the general formulas (I) and (II) in the molecule, in a weight fraction of 0 to 20% by weight (where the total weight fractions of (A), (B), (C) and (D) are taken as 100% by weight). In this case, it is preferable that the following requirement (vi) is satisfied.

[0058] [Requirement (vi)] The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer, the weight fraction of the constituent unit derived from the non-conjugated polyene (C) (weight fraction (wt%) of (C)), the weight fraction of the constituent unit derived from the conjugated polyene (D) (weight fraction (wt%) of (D)), the molecular weight of the non-conjugated polyene (C) (molecular weight of (C)), and the molecular weight of the conjugated polyene (D) (molecular weight of (D)) satisfy the following formula (4).

[0059] 4.5≦Mw×{(weight fraction of (C) / 100 / molecular weight of (C))+(weight fraction of (D) / 100 / molecular weight of (D))}≦85...Equation (4) Equation (4) specifies the content of non-conjugated diene (the sum of (C) and (D)) in one copolymer molecule.

[0060] When the ethylene-α-olefin-non-conjugated polyene copolymer containing the structural unit derived from (D) satisfies formula (4), a conveyor belt obtained from the ethylene-α-olefin-non-conjugated polyene copolymer preferably exhibits excellent mechanical properties and heat aging resistance.

[0061] If the requirement (vi) is not satisfied and "Mw × {(weight fraction of (C) / 100 / molecular weight of (C)) + (weight fraction of (D) / 100 / molecular weight of (D))}" in formula (4) is too small, that is, if the content of non-conjugated diene is too small, sufficient crosslinking may not be achieved and appropriate mechanical properties may not be obtained. Conversely, if the content is too high, excessive crosslinking may result in deterioration of mechanical properties and / or heat aging resistance.

[0062] [Requirement (vii)] The component (S) according to the present invention is not particularly limited, but it is preferably a compound having a complex viscosity η at a frequency ω=0.01 rad / s obtained by linear viscoelasticity measurement (190° C.) using a rheometer. * ( ω =0.01) (Pa sec) and the complex viscosity η at frequency ω=10rad / s * ( ω =10)It is preferable that the apparent iodine value (Pa·sec) and the apparent iodine value derived from the non-conjugated polyene (c) satisfy the following formula (5).

[0063] Log{η * ( ω =0.01)} / Log{η * ( ω =10)}≦0.0753×{apparent iodine value derived from non-conjugated polyene (C)}+1.42···Equation (5) Here, the complex viscosity η * ( ω =0.01) and the complex viscosity η * ( ω =10) is the complex viscosity η in requirement (vi) * ( ω =0.1) and the complex viscosity η * ( ω =100) The same procedure is used to calculate the value of the frequency of the measurement.

[0064] The apparent iodine value derived from the non-conjugated polyene (C) is calculated by the following formula: Apparent iodine value derived from (C) = weight fraction of (C) × 253.81 / molecular weight of (C) In the above formula (5), the left side represents the shear rate dependency which is an index of the amount of long chain branches, and the right side represents an index of the content of non-conjugated polyene (C) that is not consumed as long chain branches during polymerization. When requirement (vii) and formula (5) are satisfied, the degree of long chain branching is not too high, which is preferable. On the other hand, when formula (5) is not satisfied, it is found that a large proportion of the copolymerized non-conjugated polyene (C) is consumed to form long chain branches.

[0065] Furthermore, it is preferable that the component (S) according to the present invention contains a sufficient amount of structural units derived from the non-conjugated polyene (C), and it is preferable that the weight fraction of the structural units derived from the non-conjugated polyene (C) in the copolymer (weight fraction (wt%) of (C)) and the weight average molecular weight (Mw) of the copolymer satisfy the following formula (6). 6-0.45×Ln(Mw)≦weight fraction of (C)≦10...Equation (6)

[0066] The component (S) according to the present invention is a copolymer having a number (n C ) is preferably 6 or more, more preferably 6 to 80, even more preferably 7 to 79, and even more preferably 10 to 78.

[0067] Such component (S) according to the present invention contains a sufficient amount of structural units derived from a non-conjugated polyene (C) such as VNB, has a low content of long chain branches, is excellent in curing characteristics when crosslinked using a peroxide, has good moldability, and is excellent in balance of physical properties such as mechanical properties, as well as being particularly excellent in heat aging resistance.

[0068] Furthermore, the component (S) according to the present invention has a number of constitutional units (n D ) is preferably 29 or less, more preferably 10 or less, and even more preferably less than 1.

[0069] Such component (S) according to the present invention is preferable because the content of structural units derived from non-conjugated polyene (D) such as ENB is controlled within a range that does not impair the object of the present invention, it is less likely to cause post-crosslinking, and it has sufficient heat aging resistance.

[0070] Here, the number of constitutional units derived from the non-conjugated polyene (C) per weight average molecular weight (Mw) of the component (S) (n C ) or the number of constitutional units derived from non-conjugated polyene (D) (n D ) can be calculated from the molecular weight of the non-conjugated polyene (C) or (D), the weight fraction of the structural units derived from the non-conjugated polyene (C) or (D) in the copolymer (weight fraction (wt%) of (C) or (D)), and the weight average molecular weight (Mw) of the copolymer, according to the following formula: (n C)=(Mw)×{weight fraction of (C) / 100} / molecular weight of non-conjugated polyene (C) (n D )=(Mw)×{weight fraction of (D) / 100} / molecular weight of non-conjugated polyene (D)

[0071] The ethylene-α-olefin-non-conjugated polyene copolymer (S) according to the present invention has a weight average molecular weight (Mw) of 100 to 1500 nm, and the number of constituent units (n c ) and (n D ) satisfy the above ranges, the ethylene-α-olefin-non-conjugated polyene copolymer is preferable because it has a low content of long chain branches, excellent curing characteristics when crosslinked using a peroxide, good moldability, and an excellent balance of physical properties such as mechanical properties, and is less likely to cause post-crosslinking and is particularly excellent in heat aging resistance.

[0072] <Production of ethylene-α-olefin-non-conjugated polyene copolymer (S)> The ethylene-α-olefin-non-conjugated polyene copolymer (S) according to the present invention is a copolymer obtained by copolymerizing monomers consisting of ethylene (A), an α-olefin (B) having 3 to 20 carbon atoms, a non-conjugated polyene (C) containing in the molecule a total of two or more partial structures selected from the group consisting of the general formulae (I) and (II), and, if necessary, a non-conjugated polyene (D) containing in the molecule only one partial structure selected from the group consisting of the general formulae (I) and (II).

[0073] The component (S) according to the present invention may be prepared by any method as long as it satisfies the above-mentioned requirements (i) to (v). However, it is preferable that the component (S) is obtained by copolymerizing monomers in the presence of a metallocene compound, and it is more preferable that the component (S) is obtained by copolymerizing monomers in the presence of a catalyst system containing a metallocene compound.

[0074] As a specific method for producing the copolymer (S) according to the present invention, for example, the production method using a metallocene catalyst described in JP 2018-119096 A and WO 2015 / 122495 A pamphlet can be adopted. In this case, the ethylene (A), the α-olefin (B), and the non-conjugated polyenes (C) and (D) may each be derived from biomass.

[0075] <Ethylene-α-olefin copolymer (F)> The ethylene-α-olefin copolymer (F), which is one of the components contained in the copolymer composition for a conveyor belt of the present invention (hereinafter sometimes abbreviated as "component (F)"), is a copolymer of ethylene and an α-olefin having 3 to 20 carbon atoms.

[0076] The α-olefin is preferably an α-olefin having 3 to 12 carbon atoms, more preferably 4 to 8 carbon atoms, in order to obtain a conveyor belt having excellent mechanical strength. Specific examples of such α-olefins include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 9-methyl-1-decene, 11-methyl-1-dodecene, and 12-ethyl-1-tetradecene. Among these, propylene, 1-butene, 1-hexene, and 1-octene are preferably used. These α-olefins may be used alone or in combination of two or more.

[0077] In the component (F) of the present invention, the content of the structural units derived from ethylene is preferably 50 to 85 mol %, more preferably 50 to 80 mol % (however, the total of the structural units derived from ethylene and the structural units derived from an α-olefin having 3 to 20 carbon atoms is 100 mol %). When the content of the structural units derived from ethylene is within the above range, a copolymer composition for a conveyor belt having excellent compatibility with the component (S) can be obtained.

[0078] The component (F) according to the present invention preferably satisfies the following requirements (i) to (iv). (i) Melting point The melting point of component (F) according to the present invention is preferably 110° C. or lower, more preferably 0 to 105° C., and even more preferably 0 to 100° C. When the melting point of component (F) is within the above range, unmelted component (F) does not remain even at low kneading temperatures, and a conveyor belt that has a small mold shrinkage rate and excellent abrasion resistance can be obtained. The melting point of the component (F) according to the present invention can be measured by the method described in JIS K 7121.

[0079] (ii) Density The density of the component (F) according to the present invention is preferably 840 to 920 kg / m 3 and more preferably 850 to 915 kg / m 3 and more preferably 860 to 915 kg / m 3 When the density is within the above range, a conveyor belt having a small molding shrinkage rate and excellent strength characteristics and abrasion resistance can be obtained. The density of the component (F) according to the present invention can be measured by the method described in ASTM D1505.

[0080] (iii) MFR The MFR of the component (F) according to the present invention at 190° C. and 2.16 kg is preferably 0.1 to 50 g / 10 min, more preferably 0.2 to 30.0 g / 10 min, and even more preferably 0.3 to 10 g / 10 min. When the MFR is within the above range, a copolymer composition for a conveyor belt having a small mold shrinkage rate and excellent processability can be obtained. The MFR of the component (F) according to the present invention can be measured by the method described in ASTM D1238.

[0081] (iv) Mw / Mn The component (F) according to the present invention preferably has a ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn, determined by GPC analysis, in the range of 1.5 to 10.0.

[0082] The component (F) according to the present invention has a weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) of preferably 10,000 to 500,000, more preferably 20,000 to 300,000, and even more preferably 20,000 to 200,000.

[0083] Furthermore, the component (F) according to the present invention is preferably solid at temperatures from room temperature to about 100°C, and more preferably at temperatures around 90°C. When the weight average molecular weight of the component (F) according to the present invention is within the above range, a conveyor belt having a small molding shrinkage rate and excellent abrasion resistance can be obtained. In addition, since the amount of low molecular weight components is small, the volatilization or protrusion of the low molecular weight components is less likely to occur in the obtained conveyor belt, which is preferable.

[0084] Specifically, the Mw, Mn and Mw / Mn of the component (F) according to the present invention can be measured by a method similar to the method for measuring the molecular weight of the copolymer (S) described in the examples below. The component (F) according to the present invention can be produced by copolymerizing ethylene and an α-olefin by a conventional method using, for example, a vanadium catalyst, a Ziegler-Natta catalyst, or a metallocene catalyst. A synthesis method using a metallocene catalyst is preferred from the viewpoint of being able to easily obtain a copolymer satisfying the above physical properties, and specifically, a synthesis method using a catalyst containing a metallocene compound and an aluminum-containing compound as described in International Publication No. 2008 / 152935 or a catalyst consisting of a metallocene compound and an organoaluminum oxy compound or an ionized ionic compound as described in Japanese Patent Application Laid-Open No. 9-40586 is more preferred. In producing the component (F) according to the present invention, the ethylene and the α-olefin may each be derived from biomass.

[0085] <Carbon black (G)> Carbon black (G), which is one of the components contained in the copolymer composition for a conveyor belt of the present invention (hereinafter, may be abbreviated as "component (G)"), is a type of known rubber reinforcing agent blended in rubber compositions, and is an inorganic substance generally called carbon black.

[0086] Specific examples of the carbon black (G) used in the present invention include Asahi #55G, Asahi #60G, and Asahi #60UG (all manufactured by Asahi Carbon Co., Ltd.), VULCAN3 and STERLING (SO, V, VH, 142, etc.) carbon blacks (all manufactured by Cabot Corporation), and Seast (V, SO, 116, 3, 6, 9, SP, TA, etc.) carbon blacks (manufactured by Tokai Carbon Co., Ltd.), and these carbon blacks which have been surface-treated with a silane coupling agent or the like.

[0087] <Anti-aging agent (H)> The antioxidant (H), which is one of the components contained in the copolymer composition for a conveyor belt of the present invention (hereinafter, sometimes abbreviated as "component (H)"), is a conventionally known antioxidant, such as an amine-based antioxidant, a phenol-based antioxidant, or a sulfur-based antioxidant.

[0088] Further, examples of the antiaging agents include aromatic secondary amine-based antiaging agents such as phenylbutylamine and N,N-di-2-naphthyl-p-phenylenediamine; phenol-based antiaging agents such as dibutylhydroxytoluene and tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane (trade name: Irganox 1010, manufactured by BASF); thioether-based antiaging agents such as bis[2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl]sulfide; dithiocarbamate-based antiaging agents such as nickel dibutyldithiocarbamate; 2-mercaptobenzoylimidazole (trade name: Examples of such antioxidants include sulfur-based antioxidants such as Sandant MB (manufactured by Sanshin Chemical Industry Co., Ltd.), 2-mercaptobenzimidazole, zinc salt of 2-mercaptobenzimidazole, dilauryl thiodipropionate, and distearyl thiodipropionate. These antioxidants can be used alone or in combination of two or more.

[0089] <Ethylene-α-olefin-5-vinyl-2-norbornene copolymer(R)> An ethylene-α-olefin-5-vinyl-2-norbornene copolymer (R), which is one of the components contained in the copolymer composition for a conveyor belt of the present invention (hereinafter, sometimes referred to as "component (R)"), is a copolymer that satisfies the following requirements (1) to (6).

[0090] <Requirement (1)> The weight average molecular weight (Mw) is in the range of 1,000 to 50,000, preferably 1,500 to 35,000, more preferably 2,000 to 30,000, and most preferably 2,300 to 10,000.

[0091] When the molecular weight of component (R) according to the present invention is within this range, component (R) acts as a softening agent, has good fluidity and can be molded at low pressure, and the resulting molded article, such as a conveyor belt, does not bleed out (oil-bleed resistance), and has high rigidity (modulus).

[0092] <Requirement (2)> The molecular weight distribution (Mw / Mn, Mw: weight average molecular weight, Mn: number average molecular weight) measured by gel permeation chromatography (GPC) is 2.7 or less, and preferably 2.6 or less. When the component (R) according to the present invention has such a molecular weight distribution, the rigidity (modulus) of a conveyor belt obtained from a copolymer composition containing the component (R) is high.

[0093] The Mw and molecular weight distribution were determined using a gel permeation chromatograph HLC-8321 GPC / HT type (manufactured by Tosoh Corporation). The main measurement conditions were as follows: Detector: Differential refractometer Column: TSKgel GMH6-HT x 2 + TSKgel GMH6-HTL x 1 (Each piece has an inner diameter of 7.8 mm and a length of 300 mm) Temperature: 140℃ Mobile phase: o-dichlorobenzene (containing 0.025% BHT) Injection volume: 400 μL Sample concentration: ca 0.15% (w / v) Sample filtration: Filtration through a sintered filter with a pore size of 1.0 μm Column calibration: Monodisperse polystyrene (Tosoh Corporation) Molecular weight conversion: EPR conversion / calibration method taking viscosity into account A universal calibration curve of a third-order polynomial was created by measuring 16 monodisperse standard polystyrenes (molecular weights: 20.6 million to 580) manufactured by Tosoh Corporation. EPR conversion parameters K: 0.000403, α: 0.700

[0094] <Requirement (3)> 13 The intensity ratio Tαβ / Tαα of the C-NMR spectrum is 0.0 to 0.2, preferably 0.0 to 0.15, and more preferably 0.0 to 0.1. Here, as shown below, Tαβ is 13 indicates the peak intensity of a carbon atom having branches at the α- and β-positions in a C-NMR spectrum, and Tαα indicates the peak intensity of a carbon atom having branches at both α-positions.

[0095] [ka]

[0096] When the strength ratio Tαβ / Tαα is within this range, the conveyor belt obtained from the copolymer composition containing component (R) has high rigidity (modulus) and is excellent in strength.

[0097] <Requirement (4)> The content of structural units derived from 5-vinyl-2-norbornene (hereinafter sometimes referred to as "VNB") is in the range of 0.1 to 20.0 mass %, preferably 0.5 to 15.0 mass %, and more preferably 1.0 to 10.0 mass %.

[0098] <Requirement (5)> The constitutional units derived from VNB contain an endo structure and an exo structure, and the ratio of the endo structure / exo structure is 2.5 or less, preferably 2.4 or less, and more preferably 2.3 or less.

[0099] When the ratio of endo structure / exo structure is within this range, the conveyor belt obtained from the copolymer composition containing component (R) has high rigidity (modulus) and is excellent in strength.

[0100] The endo body 13 The C-NMR spectrum shows a peak intensity of a carbon atom (9n) at around 114 ppm, and the exo isomer 13 The peak intensity (9x) of the carbon atom at around 111.5 ppm in the C-NMR spectrum is shown.

[0101] [ka]

[0102] <Measurement of the intensity ratio Tαβ / Tαα and the endo / exo structure ratio> The intensity ratio Tαβ / Tαα and the endo structure / exo structure ratio can be determined as follows.

[0103] Copolymer 13 The C-NMR spectrum is measured using, for example, a 400 MHz NMR measurement device manufactured by JEOL Ltd. The measurement is performed at 67.8 MHz, 25°C, and d6-benzene (128 ppm) as the standard using a mixed solution of hexachlorobutadiene / d6-benzene = 2 / 1 (volume ratio) prepared so that the sample concentration is 5 wt%. 13 C-NMR spectra are analyzed according to the suggestions of Lindeman Adams (Analysis Chemistry 43, p. 1245 (1971)) and JC Randal (Review Macromolecular Chemistry Physics, C29, 201 (1989)).

[0104] <Requirement (6)> The intrinsic viscosity [η] measured in decahydronaphthalene at 135° C. is in the range of 0.01 to 0.8 dl / g, preferably 0.03 to 0.6 dl / g, more preferably 0.05 to 0.5 dl / g, and most preferably 0.05 to 0.4 dl / g.

[0105] When the intrinsic viscosity [η] is within the above range, the fluidity of component (R) is good and low-pressure moldable, and the conveyor belt obtained from the copolymer composition containing component (R) has high rigidity (modulus) and is excellent in strength.

[0106] The component (R) according to the present invention preferably satisfies the following requirement (7) in addition to the above requirements (1) to (6).

[0107] <Requirement (7)> The B value represented by the following formula (i) is 1.10 or more, more preferably 1.15 to 1.60, and most preferably in the range of 1.20 to 1.55.

[0108] B value=([EX]+2[Y]) / [2×[E]×([X]+[Y])]···(i) Here, [E], [X] and [Y] respectively represent the molar fractions of ethylene (a1), α-olefin (a2) having 3 to 20 carbon atoms and VNB (c), and [EX] represents the ethylene (a1)-α-olefin (a2) having 3 to 20 carbon atoms dyad chain fraction.

[0109] Component (R) whose B value falls within the above range has an excellent balance between rubber elasticity at low temperatures and tensile strength at room temperature. Component (R) whose B value is 1.20 or more has high alternation of the monomer units constituting the copolymer and low crystallinity, improving the processability of the resulting composition.

[0110] The above B value was measured at 120°C using o-dichlorobenzene-d4 / benzene-d6 (4 / 1 [v / v]) as the measurement solvent. 13 A C-NMR spectrum (100 MHz, JEOL ECX400P) was measured, and calculation was performed based on the above formula (i).

[0111] The component (R) according to the present invention usually has a molar ratio of structural units derived from ethylene (k1) to structural units derived from an α-olefin (k2) having 3 to 20 carbon atoms [(k1) / (k2)] of 40 / 60 to 99.9 / 0.1, preferably 50 / 50 to 90 / 10, more preferably 55 / 45 to 85 / 15, and even more preferably 55 / 45 to 78 / 22.

[0112] By using a component (R) that satisfies such requirements, a conveyor belt that has higher rigidity and is free from bleed-out can be obtained. The amount of ethylene (the amount of structural units derived from ethylene (a1)) and the amount of α-olefin (the amount of structural units derived from α-olefin (a2)) in component (R) are 13 It can be determined by C-NMR.

[0113] α-Olefin (a2) Examples of the α-olefin (a2) having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-eicosene. Among these, α-olefins having 3 to 8 carbon atoms such as 1-butene, 1-hexene, and 1-octene are preferred, and propylene and 1-butene are particularly preferred. Such α-olefins are preferred because the raw material cost is relatively low.

[0114] The above α-olefins (k2) may be used alone or in combination of two or more kinds. In producing the component (R) as described below, the ethylene (a1) and the α-olefin (a2) may each be derived from biomass.

[0115] <Production method of ethylene-α-olefin-VNB copolymer(R)> The component (R) according to the present invention can be produced by the following production method. (a) a bridged metallocene compound represented by the following general formula [I], and (b) at least one compound (b) selected from the group consisting of an organometallic compound (b-1), an organoaluminum oxy compound (b-2) and a compound (b-3) that reacts with the bridged metallocene compound (a) to form an ion pair; The copolymerization process can be carried out by a process comprising the step of copolymerizing ethylene, an α-olefin, and 5-vinyl-2-norbornene in the presence of an olefin polymerization catalyst comprising:

[0116] This production method makes it possible to produce an ethylene / α-olefin / 5-vinyl-2-norbornene copolymer (R) that satisfies the following requirements (1) to (6). (1) The weight average molecular weight is in the range of 1,000 to 50,000. (2) The molecular weight distribution (Mw / Mn, Mw: weight average molecular weight, Mn: number average molecular weight) measured by gel permeation chromatography (GPC) is 2.7 or less. (3)13 The intensity ratio Tαβ / Tαα of the C-NMR spectrum is 0.0 to 0.1. (4) The content of structural units derived from 5-vinyl-2-norbornene is in the range of 0.1 to 20.0 mass %. (5) The structural unit derived from 5-vinyl-2-norbornene contains an endo structure and an exo structure, and The endo / exo structure ratio is 2.5 or less. (6) The intrinsic viscosity [η] measured in decahydronaphthalene at 135°C is in the range of 0.01 to 0.8 dl / g.

[0117] [ka]

[0118] (In formula [I], R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 , R 10 , R 11 and R 12 are atoms or substituents selected from the group consisting of hydrogen atoms, hydrocarbon groups having 1 to 20 carbon atoms, silicon-containing groups, nitrogen-containing groups, oxygen-containing groups, halogen atoms and halogen-containing groups, and may be the same or different; R 13 and R 14 one of the groups is an aryl group or a substituted aryl group, and the other is an atom or a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silicon-containing group, a nitrogen-containing group, an oxygen-containing group, a halogen atom, and a halogen-containing group; R 1 From R 14 adjacent substituents up to may be bonded together to form a ring, Y is selected from Group 14 atoms, M is a titanium atom, a zirconium atom, or a hafnium atom, Q is selected from halogen atoms, hydrocarbon groups having 1 to 20 carbon atoms, anionic ligands, and neutral ligands capable of coordinating with lone pairs of electrons, either the same or in different combinations, n is an integer of 1 to 4, and j is an integer of 1 to 4.

[0119] The bridged metallocene compound (a) represented by the above general formula [I] is R 13 and R 14 It is preferable that one of R is an aryl group or a substituted aryl group, and the other is a hydrocarbon group having 1 to 20 carbon atoms. 13 and R 14 In the relationship between 13 If so, the other is R 14 or one is R 14 If so, the other is R 13 This refers to the fact that...

[0120] ≪Compound (b)≫ The compound (b) is at least one compound selected from (b-1) an organometallic compound, (b-2) an organoaluminum oxy compound, and (b-3) an ionizing ionic compound, and preferably contains at least the organometallic compound (b-1).

[0121] (b-1) Organometallic compound As the organometallic compound (b-1), for example, organometallic compounds of Groups 1, 2, 12 and 13 of the periodic table, such as those represented by the following general formulas [VII] to [IX], are used.

[0122] (b-1a) General formula: R a m Al(OR b ) n H p X q ...[VII] (In formula [VII], R a and R bmay be the same as or different from each other, and represents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; X represents a halogen atom; m is a number where 0 < m ≦ 3, n is a number where 0 ≦ n < 3, p is a number where 0 ≦ p < 3, q is a number where 0 ≦ q < 3, and m + n + p + q = 3. An organoaluminum compound represented by.)

[0123] Examples of such compounds include trialkylaluminums such as trimethylaluminum, triethylaluminum, triisobutylaluminum, tri-n-octylaluminum, tricycloalkylaluminum, isobutylaluminum dichloride, diethylaluminum chloride, ethylaluminum dichloride, ethylaluminum sesquichloride, methylaluminum dichloride, dimethylaluminum chloride, diisobutylaluminum hydride.

[0124] (b-1b) General formula: M 2 AlR a 4···[VIII] (In formula [VIII], M 2 represents Li, Na or K; R a is a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms.) A complex alkyl compound of a Group 1 metal of the periodic table and aluminum. Examples of such compounds include LiAl(C2H5)4, LiAl(C7H 15 )4, etc.

[0125] (b-1c) General formula: R a R b M 3 ···[IX] (In formula [IX], R a and R b may be the same as or different from each other, and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; M 3 is Mg, Zn or Cd.) A dialkyl compound having a Group 2 or Group 12 metal of the periodic table.

[0126] Among the above organometallic compounds (b-1), organoaluminum compounds such as triethylaluminum, triisobutylaluminum, tri-n-octylaluminum, etc. are preferred. Moreover, such organometallic compounds (b-1) may be used alone or in combination of two or more.

[0127] (b-2) Organoaluminum oxy compounds The organoaluminum oxy compound (b-2) may be a conventionally known aluminoxane, or may be a benzene-insoluble organoaluminum oxy compound such as those exemplified in JP-A-2-78687.

[0128] Conventionally known aluminoxanes can be produced, for example, by the following methods, and are usually obtained as a solution in a hydrocarbon solvent. (1) A method in which an organoaluminum compound such as trialkylaluminum is added to a hydrocarbon medium suspension of a compound containing adsorbed water or a salt containing water of crystallization, such as magnesium chloride hydrate, copper sulfate hydrate, aluminum sulfate hydrate, nickel sulfate hydrate, or cerous chloride hydrate, to react the adsorbed water or water of crystallization with the organoaluminum compound. (2) A method in which water, ice, or water vapor is directly applied to an organoaluminum compound such as trialkylaluminum in a medium such as benzene, toluene, ethyl ether, or tetrahydrofuran. (3) A method in which an organoaluminum compound such as trialkylaluminum is reacted with an organotin oxide such as dimethyltin oxide or dibutyltin oxide in a medium such as decane, benzene, or toluene.

[0129] The aluminoxane may contain a small amount of an organometallic component. After the solvent or unreacted organoaluminum compound is removed by distillation from the recovered aluminoxane solution, the aluminoxane may be redissolved in a solvent or suspended in a poor solvent for the aluminoxane.

[0130] As the organoaluminum compound used in preparing the aluminoxane, there can be mentioned the same organoaluminum compounds as those exemplified as the organoaluminum compounds belonging to the above (b-1a).

[0131] Of these, trialkylaluminum and tricycloalkylaluminum are preferred, and among these, trimethylaluminum and triisobutylaluminum are particularly preferred. The above organoaluminum compounds may be used singly or in combination of two or more.

[0132] The benzene-insoluble organoaluminum oxy-compound, which is one embodiment of the organoaluminum oxy-compound (b-2) used in the present invention, is preferably one in which the Al component soluble in benzene at 60°C is usually 10% by weight or less, preferably 5% by weight or less, and particularly preferably 2% by weight or less, calculated as Al atoms, relative to 100% by weight of benzene, i.e., one which is insoluble or poorly soluble in benzene.

[0133] The organoaluminum oxy compound (b-2) used in the present invention may also include boron-containing organoaluminum oxy compounds represented by the following general formula [X].

[0134] [ka]

[0135] (In formula [X], R 1 represents a hydrocarbon group having 1 to 10 carbon atoms, R 2 ~R 5 may be the same or different and represent a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms.)

[0136] The organoaluminum oxy compound containing boron represented by the general formula [X] is General formula: R 1 -B(OH)2···[XI] (In formula [XI], R1 is R in the general formula [X] 1 The compound can be produced by reacting an alkylboronic acid represented by the following formula (1) with an organoaluminum compound in an inert solvent under an inert gas atmosphere at a temperature of from -80°C to room temperature for 1 minute to 24 hours.

[0137] Examples of the alkylboronic acid represented by the general formula [XI] include methylboronic acid, ethylboronic acid, isopropylboronic acid, n-propylboronic acid, n-butylboronic acid, isobutylboronic acid, n-hexylboronic acid, cyclohexylboronic acid, phenylboronic acid, 3,5-difluorophenylboronic acid, pentafluorophenylboronic acid, and 3,5-bis(trifluoromethyl)phenylboronic acid.

[0138] Among these, methylboronic acid, n-butylboronic acid, isobutylboronic acid, 3,5-difluorophenylboronic acid, and pentafluorophenylboronic acid are preferred, and these may be used alone or in combination of two or more.

[0139] Examples of the organoaluminum compound to be reacted with such an alkylboronic acid include the same organoaluminum compounds as those exemplified as the organoaluminum compounds belonging to the above (b-1a). Among these, trialkylaluminum and tricycloalkylaluminum are preferred, and trimethylaluminum, triethylaluminum and triisobutylaluminum are particularly preferred.

[0140] The above organoaluminum oxy compounds (b-2) may be used singly or in combination of two or more.

[0141] (b-3) Ionized ionic compounds Examples of the ionized ionic compound (b-3) include Lewis acids, ionic compounds, borane compounds, and carborane compounds described in JP-T-1-501950, JP-T-1-502036, JP-A-3-179005, JP-A-3-179006, JP-A-3-207703, JP-A-3-207704, and USP 5321106.Furthermore, examples include heteropoly compounds and isopoly compounds.Such ionized ionic compounds (b-3) can be used alone or in combination of two or more.

[0142] Specifically, Lewis acids include compounds represented by BR3 (R is fluorine or a phenyl group which may have a substituent such as fluorine, a methyl group, or a trifluoromethyl group), such as trifluoroboron, triphenylboron, tris(4-fluorophenyl)boron, tris(3,5-difluorophenyl)boron, tris(4-fluoromethylphenyl)boron, tris(pentafluorophenyl)boron, tris(p-tolyl)boron, tris(o-tolyl)boron, and tris(3,5-dimethylphenyl)boron.

[0143] The ionic compound may, for example, be a compound represented by the following general formula [XII].

[0144] [ka]

[0145] (In formula [XII], R 1+ As for H + , carbonium cation, oxonium cation, ammonium cation, phosphonium cation, cycloheptyltrienyl cation, ferrocenium cation having a transition metal, etc. 2 ~R 5 may be the same or different and are organic groups, preferably aryl groups or substituted aryl groups.

[0146] Specific examples of the carbonium cation include tri-substituted carbonium cations such as triphenylcarbonium cation, tri(methylphenyl)carbonium cation, and tri(dimethylphenyl)carbonium cation.

[0147] Specific examples of the ammonium cation include trialkylammonium cations such as trimethylammonium cation, triethylammonium cation, tripropylammonium cation, tributylammonium cation, and tri(n-butyl)ammonium cation; N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N,2,4,6-pentamethylanilinium cation; Examples of the cation include dialkylammonium cations such as di(isopropyl)ammonium cation and dicyclohexylammonium cation.

[0148] Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tri(methylphenyl)phosphonium cation, and tri(dimethylphenyl)phosphonium cation.

[0149] R 1+ As the cation, a carbonium cation, an ammonium cation, etc. are preferred, and in particular, a triphenylcarbonium cation, an N,N-dimethylanilinium cation, and an N,N-diethylanilinium cation are preferred.

[0150] Further, examples of the ionic compound include trialkyl-substituted ammonium salts, N,N-dialkylanilinium salts, dialkylammonium salts, and triarylphosphonium salts.

[0151] Specific examples of trialkyl-substituted ammonium salts include triethylammonium tetra(phenyl)boron, tripropylammonium tetra(phenyl)boron, tri(n-butyl)ammonium tetra(phenyl)boron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o-tolyl)boron, tri(n-butyl)ammonium tetra(pentafluorophenyl)boron, tripropylammonium tetra(o,p-dimethylphenyl)boron, tri(n-butyl)ammonium tetra(N,N-dimethylphenyl)boron, tri(n-butyl)ammonium tetra(p-trifluoromethylphenyl)boron, tri(n-butyl)ammonium tetra(3,5-ditrifluoromethylphenyl)boron, and tri(n-butyl)ammonium tetra(o-tolyl)boron.

[0152] Specific examples of N,N-dialkylanilinium salts include N,N-dimethylanilinium tetra(phenyl)boron, N,N-diethylanilinium tetra(phenyl)boron, and N,N,2,4,6-pentamethylanilinium tetra(phenyl)boron.

[0153] Specific examples of dialkylammonium salts include di(1-propyl)ammonium tetra(pentafluorophenyl)boron, dicyclohexylammonium tetra(phenyl)boron, and the like.

[0154] Further examples of the ionic compound include triphenylcarbenium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, ferrocenium tetra(pentafluorophenyl)borate, triphenylcarbenium pentaphenylcyclopentadienyl complex, N,N-diethylanilinium pentaphenylcyclopentadienyl complex, and boron compounds represented by the following formula [XIII] or [XIV]. In the following formula, Et represents an ethyl group.

[0155] [ka]

[0156] [ka]

[0157] Specific examples of the borane compound include decaborane; salts of anions such as bis[tri(n-butyl)ammonium]nonaborate, bis[tri(n-butyl)ammonium]decaborate, bis[tri(n-butyl)ammonium]undecaborate, bis[tri(n-butyl)ammonium]dodecaborate, bis[tri(n-butyl)ammonium]decachlorodecaborate, and bis[tri(n-butyl)ammonium]dodecachlorododecaborate; and salts of metal borane anions such as tri(n-butyl)ammonium bis(dodecahydridedodecaborate)cobaltate(III) and bis[tri(n-butyl)ammonium]bis(dodecahydridedodecaborate)nickelate(III).

[0158] Specific examples of the carborane compound include 4-carbanonaborane, 1,3-dicarbanonaborane, 6,9-dicarbadecaborane, dodecahydride-1-phenyl-1,3-dicarbanonaborane, dodecahydride-1-methyl-1,3-dicarbanonaborane, undecahydride-1,3-dimethyl-1,3-dicarbanonaborane, 7,8-dicarbaundecaborane, 2,7-dicarbaundecaborane, and undecahydride-7,8-dimethyl-7,8 -Dicarbaundecaborane, dodecahydride-11-methyl-2,7-dicarbaundecaborane, tri(n-butyl)ammonium 1-carbadecaborate, tri(n-butyl)ammonium-1-carbaundecaborate, tri(n-butyl)ammonium-1-carbadodecaborate, tri(n-butyl)ammonium-1-trimethylsilyl-1-carbadecaborate, tri(n-butyl)ammonium bromo-1-carbadodecaborate, tri(n-butyl)ammonium ) ammonium-6-carbadecaborate, tri(n-butyl)ammonium-7-carbaundecaborate, tri(n-butyl)ammonium-7,8-dicaundecaborate, tri(n-butyl)ammonium-2,9-dicaundecaborate, tri(n-butyl)ammonium dodecahydride-8-methyl-7,9-dicaundecaborate, tri(n-butyl)ammonium undecahydride-8-ethyl-7,9-dicaundecaborate salts of anions such as tri(n-butyl)ammonium undecahydride-8-butyl-7,9-dicarboxaundecaborate, tri(n-butyl)ammonium undecahydride-8-allyl-7,9-dicarboxaundecaborate, tri(n-butyl)ammonium undecahydride-9-trimethylsilyl-7,8-dicarboxaundecaborate, and tri(n-butyl)ammonium undecahydride-4,6-dibromo-7-carbaundecaborate; Tri(n-butyl)ammonium bis(nonahydride-1,3-dicarbanonaborate)cobaltate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)ferrate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)cobaltate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)nickelate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)cuprate(III), tri(n-butyl)ammonium bis(undecahydride-7,8-dicarbandecaborate)aurate(III), tri(n-butyl)ammonium bis(nonahydride-7,8-dimethyl-7,8-dicarbandecaborate)ferrate salt (III), tri(n-butyl)ammonium bis(nonahydride-7,8-dimethyl-7,8-dicarboxaborate)chromate (III), tri(n-butyl)ammonium bis(tribromooctahydride-7,8-dicarboxaborate)cobaltate (III), tris[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)chromate (III), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)manganate (IV), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)cobaltate (III), bis[tri(n-butyl)ammonium]bis(undecahydride-7-carbowndecaborate)nickelate (IV), and the like.

[0159] The heteropoly compound is composed of an atom selected from silicon, phosphorus, titanium, germanium, arsenic and tin, and one or more atoms selected from vanadium, niobium, molybdenum and tungsten. Specifically, usable are phosphovanadic acid, germanovanadic acid, arsenic vanadic acid, phosphoniobic acid, germanoniobic acid, siliconomolybdic acid, phosphomolybdic acid, titanomolybdic acid, germanomolybdic acid, arsenic molybdic acid, tinmolybdic acid, phosphotungstic acid, germanotungstic acid, tintungstic acid, phosphomolybdovanadic acid, phosphotungstovanadic acid, germanotungstovanadic acid, phosphomolybdotungstovanadic acid, germanomolybdotungstovanadic acid, phosphomolybdotungstic acid, phosphomolybdoniobic acid, and salts of these acids, for example, salts with metals of Group 1 or 2 of the periodic table, specifically, lithium, sodium, potassium, rubidium, cesium, beryllium, magnesium, calcium, strontium, barium, etc., and organic salts such as triphenylethyl salts. However, the present invention is not limited to these.

[0160] Among the ionizing ionic compounds (b-3), the above-mentioned ionic compounds are preferred, and among them, triphenylcarbenium tetrakis(pentafluorophenyl)borate and N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate are more preferred.

[0161] In the present invention, when a metallocene catalyst containing the above-mentioned bridged metallocene compound (a), an organometallic compound (b-1) such as triisobutylaluminum, an organoaluminum oxy compound (b-2) such as methylaluminoxane, and an ionizing ionic compound (b-3) such as triphenylcarbenium tetrakis(pentafluorophenyl)borate is used as a polymerization catalyst, a very high polymerization activity can be exhibited in the production of a copolymer.

[0162] (c) Particulate carrier In the present invention, the particulate carrier (c) used as necessary is an inorganic or organic compound, and is a granular or fine particle solid.

[0163] The inorganic compound is preferably a porous oxide, an inorganic halide, a clay, a clay mineral, or an ion-exchangeable layered compound, specific examples of which are described in WO2015 / 122495.

[0164] The clay, clay mineral, and ion-exchangeable layered compound used in the present invention may be used as is, or may be used after treatment such as ball milling or sieving. They may also be used after newly adding and adsorbing water or after heat dehydration treatment. Furthermore, they may be used alone or in combination of two or more kinds.

[0165] Of these, clay or clay minerals are preferred, and montmorillonite, vermiculite, hectorite, taeniolite and synthetic mica are particularly preferred. The organic compound may be a granular or particulate solid having a particle size in the range of 10 to 300 μm.Specific examples include (co)polymers mainly made of α-olefins having 2 to 14 carbon atoms, such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, or (co)polymers mainly made of vinylcyclohexane and styrene, and their modifications.

[0166] The polymerization catalyst used in the present invention comprises a metallocene compound (a), at least one compound (b) selected from an organometallic compound (b-1), an organoaluminum oxy compound (b-2) and an ionizing ionic compound (b-3), and a carrier (c) used as needed, and may further contain a specific organic compound component (d) as needed.

[0167] (d) Organic compound component In the present invention, the organic compound component (d) is used as necessary for the purpose of improving the polymerization performance and the physical properties of the resulting polymer. Examples of such organic compounds include, but are not limited to, alcohols, phenolic compounds, carboxylic acids, phosphorus compounds, and sulfonates.

[0168] <Production method and conditions of copolymer (R)> The copolymer (R) according to the present invention is produced by copolymerizing ethylene (a1), an α-olefin (a2), and VNB. In this case, the ethylene (a1), the α-olefin (a2), and the 5-vinyl-2-norbornene may each be derived from biomass.

[0169] When copolymerizing such monomers, the use method and order of addition of each component constituting the above-mentioned polymerization catalyst may be selected arbitrarily, and examples thereof include the following methods (1) to (5): (1) A method of adding the bridged metallocene compound (a) alone to a polymerization reactor. (2) A method of adding the bridged metallocene compound (a) and the compound (b) to a polymerization reactor in an arbitrary order. (3) A method of adding a catalyst component in which the bridged metallocene compound (a) is supported on a carrier (c) and the compound (b) to a polymerization reactor in an arbitrary order. (4) A method of adding a catalyst component in which the compound (b) is supported on a carrier (c) and the bridged metallocene compound (a) to a polymerization reactor in an arbitrary order. (5) A method of adding a catalyst component in which the bridged metallocene compound (a) and the compound (b) are supported on a carrier (c) to a polymerization reactor.

[0170] In each of the above methods (2) to (5), at least two of the bridged metallocene compound (a), the compound (b) and the support (c) may be contacted in advance. In the above methods (4) and (5) in which the compound (b) is supported, the unsupported compound (b) may be added in any order, if necessary. In this case, the compound (b) may be the same as or different from the compound (b) supported on the support (c).

[0171] In addition, the solid catalyst component in which the bridged metallocene compound (a) is supported on the support (c) and the solid catalyst component in which the bridged metallocene compound (a) and the compound (b) are supported on the support (c) may be prepolymerized with an olefin, or a catalyst component may be further supported on the prepolymerized solid catalyst component.

[0172] The copolymer (R) according to the present invention can be suitably obtained by copolymerizing ethylene, an α-olefin, and VNB in ​​the presence of the above-mentioned polymerization catalyst. When ethylene, α-olefins, and VNB are polymerized using the above-mentioned polymerization catalyst, the bridged metallocene compound (a) is usually used in an amount of 10 -12 ~10 -2 Molar, preferably 10 -10 ~10 -8 It is used in molar amounts.

[0173] The compound (b-1) is used in an amount such that the molar ratio [(b-1) / M] of the compound (b-1) to the total transition metal atoms (M) in the bridged metallocene compound (a) is usually 0.01-50000, preferably 0.05-10000. The compound (b-2) is used in an amount such that the molar ratio [(b-2) / M] of the aluminum atoms in the compound (b-2) to the total transition metal atoms (M) in the bridged metallocene compound (a) is usually 10-50000, preferably 20-10000. The compound (b-3) is used in an amount such that the molar ratio [(b-3) / M] of the compound (b-3) to the transition metal atoms (M) in the bridged metallocene compound (a) is usually 1-20, preferably 1-15.

[0174] In the present invention, the method for producing the copolymer (R) can be carried out by any of liquid phase polymerization methods such as solution (dissolution) polymerization and suspension polymerization, or gas phase polymerization methods, and is not particularly limited. However, it is preferable that the method includes a step of obtaining the following polymerization reaction liquid.

[0175] The step of obtaining a polymerization reaction liquid is a step of copolymerizing ethylene, an α-olefin, and VNB in ​​the presence of the above-mentioned bridged metallocene compound (a) using an aliphatic hydrocarbon as a polymerization solvent to obtain a polymerization reaction liquid of a copolymer.

[0176] Examples of the polymerization solvent include aliphatic hydrocarbons and aromatic hydrocarbons. Specific examples include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene, alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane, aromatic hydrocarbons such as benzene, toluene, and xylene, and halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane. These can be used alone or in combination of two or more. Olefin itself can also be used as the solvent. Among these, hexane is preferred from the viewpoint of separation and purification from the resulting copolymer.

[0177] The polymerization temperature is usually in the range of -50 to +200°C, preferably in the range of 0 to +150°C, and more preferably in the range of +70 to +110°C. Although it depends on the attained molecular weight and polymerization activity of the metallocene catalyst system used, a higher temperature (+70°C or higher) is desirable from the viewpoints of catalytic activity, copolymerizability, and productivity.

[0178] The polymerization pressure is usually normal pressure to 10 MPa gauge pressure, preferably 1.1 to 5 MPa gauge pressure, more preferably 1.2 to 2.0 MPa gauge pressure, and the polymerization reaction can be carried out by any of batch, semi-continuous, and continuous methods. Furthermore, the polymerization can be carried out in two or more stages with different reaction conditions. Among these, in the present invention, it is preferable to adopt a method in which ethylene and a non-conjugated polyene are continuously fed to a reactor to carry out copolymerization.

[0179] The reaction time (average residence time when copolymerization is carried out by a continuous method) varies depending on conditions such as catalyst concentration and polymerization temperature, but is usually 0.5 minutes to 5 hours, preferably 5 minutes to 3 hours, and more preferably 10 minutes to 2 hours.

[0180] The molecular weight of the resulting copolymer can be adjusted by making hydrogen exist in the polymerization system or by changing the polymerization temperature. Furthermore, it can also be adjusted by the amount of compound (b) used. Specific examples include triisobutylaluminum, methylaluminoxane, and diethylzinc. When hydrogen is added, the amount is suitably about 0.001 to 100 NL per kg of olefin.

[0181] In the present invention, it is preferable to include a step (2) of deactivating the polymerization catalyst by adding a catalyst deactivator after the step (1) of carrying out copolymerization in the presence of the polymerization catalyst. As the catalyst deactivator, alcohols can be used, and methanol or ethanol is preferred, with ethanol being particularly preferred.

[0182] In the step (2), the catalyst deactivator is preferably added in an amount of 0.05 to 3.0 mol times, more preferably 0.06 to 2.5 mol times, and even more preferably 0.08 to 2.0 mol times, relative to the organometallic compound (b-1), so that a small amount of catalyst degraded by the catalyst deactivator such as ethanol is generated and the low molecular weight components are moderately polymerized, resulting in a copolymer with a moderately wide molecular weight distribution. On the other hand, if the amount of catalyst deactivator added is too large, almost no modified catalyst is generated and almost no polymerization of low molecular weight components is performed, so the molecular weight distribution of the obtained copolymer tends to be narrow. In addition, if the catalyst deactivator is not added or the amount added is too small, a large amount of modified catalyst is generated and a large amount of low molecular weight components are polymerized, so the content of low molecular weight components in the obtained copolymer tends to be too high.

[0183] <Organic peroxide crosslinking agent (J)> An organic peroxide-based crosslinking agent (J) (hereinafter sometimes abbreviated as "component (J)"), which is one of the components that may be contained in the copolymer composition for a conveyor belt of the present invention, ] is a type of crosslinking agent, and specific examples thereof include dicumyl peroxide (DCP), di-tert-butyl peroxide, 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butylperoxybenzoate, ert-butylperoxyisopropylcarbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.

[0184] Of these, organic peroxide-based crosslinking agents such as dicumyl peroxide (DCP), 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, and n-butyl-4,4-bis(tert-butylperoxy)valerate are preferred.

[0185] <Copolymer composition for conveyor belts> The copolymer composition for a conveyor belt of the present invention is a copolymer composition for a conveyor belt characterized by containing the above-mentioned components (S), (F), (G), (H) and (R), preferably the above-mentioned component (J).

[0186] The copolymer composition for a conveyor belt of the present invention contains the above-mentioned components, and thus has excellent processability, and a conveyor belt obtained from the copolymer composition for a conveyor belt has excellent mechanical properties, heat aging resistance, abrasion resistance, and oil bleed resistance.

[0187] The copolymer composition for a conveyor belt of the present invention preferably contains, relative to 100 parts by mass of the total amount of the above-mentioned components (S) and (F), 95 to 5 parts by mass, preferably 90 to 10 parts by mass, and more preferably 80 to 20 parts by mass of the above-mentioned component (S) and 5 to 95 parts by mass, preferably 10 to 90 parts by mass, and more preferably 20 to 80 parts by mass of the above-mentioned component (F), and contains 5 to 120 parts by mass of the above-mentioned component (G) per 100 parts by mass of the total amount of the above-mentioned components (S) and (F). parts by mass, more preferably 10 to 100 parts by mass, the above component (H) is 0.1 to 20 parts by mass, more preferably 0.2 to 15 parts by mass, and the above component (R) is 0.1 to 20 parts by mass, more preferably 0.2 to 15 parts by mass, and when the copolymer composition for a conveyor belt further contains the above component (J), the total amount of the above component (S) and the above component (F) is 0.1 to 30 parts by mass, more preferably 0.2 to 25 parts by mass, per 100 parts by mass.

[0188] The copolymer composition for a conveyor belt of the present invention may contain, in addition to the above-mentioned components, other compounding agents, such as at least one selected from a crosslinking aid, an antiaging agent, a processing aid, an activator, a heat stabilizer, a weathering stabilizer, an antistatic agent, a colorant, a lubricant, a thickener, an antifoaming agent, a foaming agent, and a foaming aid, depending on the purpose. Each additive may be used alone or in combination of two or more.

[0189] <Crosslinking aid> Examples of the crosslinking aid include sulfur; quinone dioxime-based crosslinking aids such as p-quinone dioxime; acrylic crosslinking aids such as ethylene glycol dimethacrylate and trimethylolpropane trimethacrylate; allyl crosslinking aids such as diallyl phthalate and triallyl isocyanurate; maleimide-based crosslinking aids; divinylbenzene; and metal oxides such as zinc oxide (e.g., ZnO#1·zinc oxide type 2 (JIS standard (K-1410)), manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and activated zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name, manufactured by Inoue Lime Industry Co., Ltd.)).

[0190] When a crosslinking auxiliary is used, the amount of the crosslinking auxiliary in the copolymer composition for a conveyor belt is usually 0.5 to 10 mol, preferably 0.5 to 7 mol, and more preferably 1 to 6 mol, per mol of the organic peroxide-based crosslinking agent.

[0191] <Processing aids> As the processing aid, a wide variety of processing aids that are generally compounded with rubber can be used.Specific examples include ricinoleic acid, stearic acid, palmitic acid, lauric acid, barium stearate, zinc stearate, calcium stearate, zinc laurate, and esters.Of these, stearic acid is preferred.

[0192] When the copolymer composition for a conveyor belt contains a processing aid, it can be appropriately blended in an amount of usually 1 to 3 parts by mass per 100 parts by mass of the total amount of component (S) and component (F). When the blending amount of the processing aid is within the above range, it is preferable since the processability such as kneading processability, extrusion processability, and injection moldability is excellent. The processing aid may be used alone or in combination with two or more kinds.

[0193] <Activator> Examples of the activator include amines such as di-n-butylamine, dicyclohexylamine, and monoethanolamine; activators such as diethylene glycol, polyethylene glycol, lecithin, triaryl methylate, and zinc compounds of aliphatic or aromatic carboxylic acids; zinc peroxide preparations; octadecyltrimethylammonium bromide, synthetic hydrotalcite, and special quaternary ammonium compounds.

[0194] When the copolymer composition for a conveyor belt contains an activator, the amount of the activator is usually 0.2 to 10 parts by mass, and preferably 0.3 to 5 parts by mass, per 100 parts by mass of the total amount of component (S) and component (F).

[0195] <Foaming agent and foaming assistant> The molded article formed by using the copolymer composition for a conveyor belt of the present invention may be a non-foamed article or a foamed article. When the conveyor belt is a foamed article, it is preferable that the copolymer composition for a conveyor belt contains a foaming agent.

[0196] As the foaming agent, any of commercially available foaming agents can be suitably used. Examples of such foaming agents include inorganic foaming agents such as sodium bicarbonate, sodium carbonate, ammonium bicarbonate, ammonium carbonate, and ammonium nitrite; nitroso compounds such as N,N'-dinitrosoterephthalamide and N,N'-dinitrosopentamethylenetetramine; azo compounds such as azodicarbonamide, azobisisobutyronitrile, azocyclohexylnitrile, azodiaminobenzene, and barium azodicarboxylate; sulfonyl hydrazide compounds such as benzenesulfonyl hydrazide, toluenesulfonyl hydrazide, and p,p'-oxybis(benzenesulfonyl hydrazide)diphenylsulfone-3,3'-disulfonyl hydrazide; and azide compounds such as calcium azide, 4,4'-diphenyldisulfonyl azide, and paratoluenemalonyl azide. Among them, azo compounds, sulfonyl hydrazide compounds, and azide compounds are preferably used.

[0197] When the copolymer composition for a conveyor belt contains a foaming agent, the amount of the foaming agent is appropriately selected depending on the performance required for a molded article produced from the copolymer composition, but the foaming agent is usually used in a ratio of 0.5 to 30 parts by mass, preferably 1 to 20 parts by mass, per 100 parts by mass of the total amount of component (S) and component (F).

[0198] If necessary, a foaming assistant may be used together with the foaming agent. The addition of the foaming assistant is effective in adjusting the decomposition temperature of the foaming agent and uniformizing the bubbles. Specific examples of the foaming assistant include organic acids such as salicylic acid, phthalic acid, stearic acid, and oxalic acid, urea, and its derivatives.

[0199] When the copolymer composition for a conveyor belt contains a foaming aid, the foaming aid is usually used in an amount of 1 to 100 parts by mass, preferably 2 to 80 parts by mass, based on 100 parts by mass of the foaming agent.

[0200] <Method of producing copolymer composition for conveyor belt> The copolymer composition for conveyor belts of the present invention is prepared by kneading the above-mentioned components (S), (F), (G), and (R), preferably as well as a processing aid and a crosslinking aid, etc., as required, for 2 to 20 minutes at a temperature of 80 to 170° C., using an internal mixer (internal mixer) such as a Banbury mixer, a kneader, or an intermix. Next, the above-mentioned component (J), additives such as a softener, a crosslinking aid, and a vulcanization accelerator are added to the obtained blend using rolls such as an open roll or a kneader, and the vulcanization accelerator and crosslinking aid are added as required, and the mixture is kneaded at a roll temperature of 40 to 80° C. for 5 to 30 minutes, followed by dispensing.

[0201] When the kneading temperature in an internal mixer is low, the component (J) may be kneaded simultaneously with the components (S), (F), (G), (H) and (R).

[0202] <Conveyor belt> The conveyor belt of the present invention is produced by using the copolymer composition for conveyor belts of the present invention, and specific configurations thereof include the following.

[0203] The conveyor belt is made of canvas as a core material and has an outer periphery covered with a copolymer composition for conveyor belts. A conveyor belt comprising a steel cord embedded as a core material in a copolymer composition for conveyor belts.

[0204] The canvas is made of a woven fabric of synthetic fibers such as nylon, vinylon, polyester, etc., and the number of layers of the canvas, the thickness of the copolymer composition for a conveyor belt, the belt width, etc. are appropriately determined depending on the purpose of use, but the thickness of the copolymer composition for a conveyor belt is usually about 1.5 to 20 mm.

[0205] The core material made of steel cord is made by twisting together multiple wires with a diameter of about 0.2 to 0.4 mm to form a wire rope with a diameter of about 2.0 to 9.5 mm, and arranging about 50 to 230 steel cords in parallel to form the core material. Generally, the total thickness of the conveyor belt is about 10 to 50 mm.

[0206] The conveyor belt of the present invention can be easily produced by interposing the canvas or steel cord serving as the core material between uncrosslinked sheets formed from the copolymer composition for conveyor belts of the present invention, and crosslinking the sheets by heating and pressurizing them in accordance with a conventional method. The crosslinking conditions are usually 120 to 180°C and 10 to 50 kg / cm. 2 The duration is approximately 10 to 90 minutes. EXAMPLES

[0207] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following description, "parts" refers to "parts by mass" unless otherwise specified. The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0208] In the examples and comparative examples, the following copolymers were used. (1) Ethylene-α-olefin-non-conjugated polyene copolymer (S) [Composition of ethylene-α-olefin-non-conjugated polyene copolymer (S)] The molar ratio and mass fraction (mass%) of each structural unit of the ethylene-α-olefin-non-conjugated polyene copolymer (S) are as follows: 13 The measured values ​​were obtained by C-NMR. The measured values ​​were obtained by using an ECX400P nuclear magnetic resonance apparatus (manufactured by JEOL Ltd.) at a measurement temperature of 120°C, a measurement solvent of orthodichlorobenzene / deuterated benzene = 4 / 1, and an accumulation number of 8000 times. 13 The C-NMR spectrum was obtained.

[0209] [Production Example 1] Production of ethylene-α-olefin-non-conjugated polyene copolymer (S) Ethylene-propylene-5-vinyl-2-norbornene (VNB) copolymer (S-1) was produced using a continuous polymerization apparatus as follows.

[0210] A 300-liter polymerization reactor was continuously fed with 58.3 L / hr of dehydrated hexane solvent from line 1, 4.5 mmol / hr of triisobutylaluminum (TiBA), 0.150 mmol / hr of (C6H5)3CB(C6F5)4, and 0.030 mmol / hr of di(p-tolyl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorenyl)zirconium dichloride from line 2. At the same time, 6.6 kg / hr of ethylene, 9.3 kg / hr of propylene, 18 L / hr of hydrogen, and 340 g / hr of VNB were continuously fed into the polymerization reactor from separate lines, and copolymerization was carried out under the conditions of a polymerization temperature of 87°C, a total pressure of 1.6 MPaG, and a residence time of 1.0 hour.

[0211] The ethylene-propylene-VNB copolymer solution produced in the polymerization reactor was continuously discharged at a flow rate of 88.0 L / hr, heated to 170°C (pressure increased to 4.1 MPaG), and fed to a phase separator. At this time, ethanol, a polymerization inhibitor, was continuously introduced into the discharge line in an amount of 0.1 mol times the amount of TiBA in the liquid component extracted from the polymerization reactor.

[0212] In the phase separator, the ethylene-propylene-vinyl alcohol copolymer solution was separated into a dense phase (lower phase) containing most of the ethylene-propylene-vinyl alcohol copolymer and a dilute phase (upper phase) containing a small amount of the polymer.

[0213] The separated thick phase was introduced into heat exchanger K at a rate of 85.4 L / hr, and then into a hopper where the solvent was evaporated and separated to obtain an ethylene-propylene-VNB copolymer at a rate of 7.8 kg / hr.

[0214] The molar ratio (ethylene unit / propylene unit) of the obtained copolymer (S-1) was 70 / 30, the content of VNB units was 1.4 mass%, and the intrinsic viscosity [η] measured in decalin at 135° C. was 2.8 dL / g. The molecular weight distribution of the obtained copolymer (S-1) was bimodal, and the chart obtained by GPC measurement showed two or more peaks, and the area of ​​the peak appearing on the side with the smallest molecular weight was 5% of the total peak area.

[0215] P / ([η] 2.9 ):1.0 LCB 1000C :0.03 1-0.07×Ln(Mw):0.18

[0216] (2) Ethylene-α-olefin-5-vinyl-2-norbornene copolymer (R) [Production Example 2] Production of ethylene-α-olefin-5-vinyl-2-norbornene copolymer(R) Ethylene-propylene-VNB copolymer (R-1) was prepared as follows.

[0217] The metallocene catalyst used in the polymerization examples in the examples, [methylphenylmethylene(η5-cyclopentadienyl)(η5-2,7-di-t-butylfluorenyl)]zirconium dichloride, was synthesized by the method described in WO2015 / 147215. The symbols (a) to (t) in Production Example 2 represent the amounts of each unit shown in Table 1 below.

[0218] Dehydrated and purified n-hexane was fed at a rate of (a) liters / h to one feed inlet of a 136-liter continuous polymerization reactor, and a hexane solution of [methylphenylmethylene(η5-cyclopentadienyl)(η5-2,7-di-t-butylfluorenyl)]zirconium dichloride (ZD) (b) mmol / liter) was fed at a rate of (c) liters / h to the other feed inlets, a hexane solution of triisobutylaluminum (5 mmol / liter) was fed at a rate of (d) liters / h to a hexane slurry of N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate (e) mmol-B / liter) was fed at a rate of (f) liters / h to a hexane slurry of 5-vinyl-2-norbornene (VNB) (g) g / h (total hexane (h) liters / hr). At the same time, ethylene (i) kg / h, propylene (j) kg / h, and hydrogen (k) NL / h were continuously fed to another feed inlet of the polymerization reactor, and continuous solution polymerization was carried out under the conditions of a polymerization temperature of (l) °C, a total pressure of (m) MPaG, and a residence time of (n) minutes.

[0219] The hexane solution of ethylene-propylene-vinyl chloride copolymer produced in the polymerization reactor was continuously discharged through an outlet on the side wall of the polymerization reactor at a pressure of 8 kg / cm. 2The hexane solution of ethylene-propylene-VNB copolymer heated to about 170℃ in the steam-jacketed connecting pipe was continuously sent to the flash tank through the inner pipe of the double piping heated with 10 kg / cm2 steam. The piping at the OUT of the polymerization reactor was equipped with a supply port for injecting methanol, a catalyst deactivator, and the methanol was injected as a 0.5 vol% hexane diluted solution at a rate of 1.0 liter / h and merged with the hexane solution. As a result, ethylene-1-propene-VNB copolymer was obtained. The intrinsic viscosity [η] of the ethylene-propylene-VNB copolymer was (r) dl / g, the ethylene content was (s) mass%, and the VNB content was (t) mass%.

[0220] [Table 1]

[0221] (3) Ethylene-α-olefin copolymer (F) (3-1) Ethylene-1-butene copolymer (F-1) Density: 864kg / m 3 , melting point <50℃, MFR: 3.6g / 10min [manufactured by Mitsui Chemicals, product name Toughmer TM DF640〕.

[0222] [Physical Properties of Copolymer Composition for Conveyor Belt] [Mooney viscosity (ML(1+4)100℃)] The Mooney viscosity at 100°C (ML(1+4)100°C) was measured at 100°C using a Mooney viscometer (SMV202 model, manufactured by Shimadzu Corporation) in accordance with JIS K6300.

[0223] [Oil bleeding resistance] A crosslinked sheet having a thickness of 2 mm was pressed at 180°C for 10 minutes and stored in a dark place at 25°C for 30 days, and the surface condition was observed. Score 1: Oil has bled onto the surface. Score 2: There is no oil bleeding on the surface, but there are white marks. Score 3: No oil bleeding or marks on the surface.

[0224] <Physical properties of copolymer composition (crosslinked product) for conveyor belts> [Modulus (MPa), Tensile stress at break (MPa), Tensile elongation at break (%)] The sheet was punched out to prepare No. 3 dumbbell test pieces as described in JIS K 6251 (1993). Using these test pieces, tensile tests were carried out according to the method specified in JIS K6251, section 3, at a measurement temperature of 25°C and a tensile speed of 500 mm / min, and the modulus at 100% elongation (M100), the modulus at 200% elongation (M200), the tensile stress at break (TB), and the tensile elongation at break (EB) were measured.

[0225] [Durometer A hardness] According to JIS K 6253, the hardness of the sheet (Type A durometer, HA) was measured using six 2 mm thick crosslinked sheets with smooth surfaces, stacked on top of each other at the flat part to a thickness of approximately 12 mm. However, specimens with foreign matter, air bubbles, or scratches were not used. The dimensions of the measurement surface of the specimen were set so that the tip of the indenter could be measured at a position 12 mm or more away from the end of the specimen.

[0226] [Heat aging resistance] The sheet was subjected to a heat aging test in which the sheet was held at 180°C for 168 hours (hrs) in accordance with JIS K 6257. The hardness, tensile stress at break (MPa), and tensile elongation at break (%) of the sheet after the heat aging test were measured in the same manner as in the above [Hardness (Durometer-A)] item and the above [Modulus, tensile stress at break, and tensile elongation at break] items.

[0227] AH (Duro-A) was calculated from the difference in hardness before and after the heat aging test, and Ac(TB) and Ac(EB) were calculated from the tensile stress at break (TB) and tensile elongation at break (EB) before and after the heat aging test to determine the rate of change after the test from the values ​​before the heat aging test, respectively.

[0228] [DIN friction test (amount of wear)] In accordance with JIS-K6264-2:2005, three 2 mm thick crosslinked sheets were stacked to prepare a disk-shaped test piece with a diameter of 16.0±0.2 mm and a thickness of 6 mm. The test piece was then subjected to a DIN abrasion test using a drum with a diameter of 150.0±0.2 mm and a length of 500 mm, which was rotated at 40 revolutions per minute under a load of 1 kgf and an abrasion distance of 40.0±0.2 m, to measure the amount of abrasion (DIN abrasion amount: unit: mm3).

[0229] Example 1 In the first step, 40 parts by mass of the ethylene-α-olefin-non-conjugated polyene copolymer (S-1) obtained in Production Example 1 and 60 parts by mass of the ethylene-1-butene copolymer (F-1) were masticated for 1 minute using a BB-4 type Banbury mixer (manufactured by Kobe Steel, Ltd.), and then 5 parts by mass of zinc oxide (ZnO#1, manufactured by Hakusui Tech Co., Ltd.), 50 parts by mass of carbon black (G-1) (VULCAN3D, manufactured by Cabot), 10 parts by mass of ethylene-propylene-VNB copolymer (R-1), 3 parts by mass of a phenol-based antioxidant (trade name Irganox 1010, manufactured by BASF) as the antioxidant (H-1), 6 parts by mass of an imidazole-based antioxidant (trade name Sandant MB, manufactured by Sanshin Chemical Industry Co., Ltd.) as the antioxidant (H-2), and 1 part by mass of stearic acid were added thereto, and the mixture was kneaded at 140°C for 2 minutes. Thereafter, the ram was raised and cleaned, and kneading was further carried out for 1 minute, and the kneaded product was discharged at about 150° C. to obtain a first-stage compound.

[0230] Next, in the second step, the mixture obtained in the first step was wound around a 6-inch roll (manufactured by Nippon Roll Co., Ltd., front roll surface temperature 50°C, rear roll surface temperature 50°C, front roll rotation speed 16 rpm, rear roll rotation speed 18 rpm), and 5.1 parts by mass of dicumyl peroxide (DCP) [trade name Parkmil D-40, manufactured by Nippon Oil & Fats Co., Ltd.] as an organic peroxide-based crosslinking agent (J-1) and 2.0 parts by mass of triallylisocyanurate (TAIC) [trade name Taiku, manufactured by Shinryo Co., Ltd.] as a co-crosslinking agent (K-1) were added thereto in amounts of blended, and kneaded for 10 minutes to obtain an uncrosslinked copolymer composition for conveyor belts. The physical properties of this copolymer composition were evaluated.

[0231] The uncrosslinked copolymer composition for conveyor belts was extruded into a sheet, and then pressed at 180°C for 10 minutes using a 100-ton press molding machine to prepare a crosslinked sheet having a thickness of 2 mm. The physical properties of the crosslinked sheet were measured using the extrusion. The results are shown in Table 2.

[0232] Comparative Example 1 The same procedure as in Example 1 was carried out, except that the (R-1) used in Example 1 was not used, and 10 parts by mass of softener (I-1) (product name: Diana Process Oil PW-380, manufactured by Idemitsu Kosan Co., Ltd.) was used instead. The physical properties of the uncrosslinked copolymer composition for conveyor belts and the crosslinked sheet obtained were measured. The results are shown in Table 2.

[0233] [Table 2] [Industrial Applicability]

[0234] The heat-resistant conveyor belt made of the copolymer composition for conveyor belts of the present invention is suitable as a conveyor belt for transporting combustion products and return ore, coke, cement clinker, raw coal, special chemicals, various high-temperature powdery materials, and the like in sintering plants, coke plants, cement plants, and chemical plants.

Claims

1. A copolymer composition for a conveyor belt, comprising the following components (S), (F), (G), (H) and (R): Ingredient (S): An ethylene / α-olefin / non-conjugated polyene copolymer (S) having structural units derived from ethylene (A), an α-olefin (B) having 3 to 20 carbon atoms, and a non-conjugated polyene (C) containing in the molecule two or more partial structures selected from the group consisting of the following general formulas (I) and (II), and satisfying the following requirements (i) to (v): (i) The molar ratio of ethylene to α-olefin is from 40 / 60 to 99.9 / 0.

1. (ii) The weight fraction of the constituent units derived from the non-conjugated polyene (C) is 0.07% by weight to 10% by weight in 100% by weight of the ethylene / α-olefin / non-conjugated polyene copolymer. (iii) The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer, the weight fraction of the constituent unit derived from the non-conjugated polyene (C) (weight fraction (wt %) of (C)), and the molecular weight of the non-conjugated polyene (C) (molecular weight of (C)) satisfy the following formula (1): 4.5≦Mw×weight fraction of (C) / 100 / molecular weight of (C)≦80...Equation (1) (iv) The ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, which are obtained by linear viscoelasticity measurement (190° C.) using a rheometer, the intrinsic viscosity [η], and the weight fraction of the constituent unit derived from the non-conjugated polyene (C) (weight fraction of (C)), satisfy the following formula (2): P / ([η] 2.9 ) ≦ weight fraction of (C) × 6 ... formula (2) (v) The number of long chain branches per 1,000 carbon atoms (LCB1000C) and the natural logarithm of the weight average molecular weight (Mw) [Ln(Mw)], both obtained using 3D-GPC, satisfy the following formula (3): LCB 1000C ≦1-0.07×Ln(Mw)・・・Formula (3) 【Chemistry 1】 Component (F): Ethylene / α-olefin copolymer (F) Component (G): Carbon black (G) Component (H): Antiaging agent (H) Component (R); An ethylene / α-olefin / 5-vinyl-2-norbornene copolymer (R) that satisfies the following requirements (1) to (6): (1) The weight average molecular weight is in the range of 1,000 to 50,000. (2) The molecular weight distribution (Mw / Mn, Mw: weight average molecular weight, Mn: number average molecular weight) measured by gel permeation chromatography (GPC) is 2.7 or less. (3) 13 The intensity ratio Tαβ / Tαα in the C-NMR spectrum is 0.0 to 0.

1. (4) The content of structural units derived from 5-vinyl-2-norbornene is in the range of 0.1 to 20.0 mass %. (5) The structural units derived from 5-vinyl-2-norbornene contain an endo structure and an exo structure, and the ratio of the endo structure / exo structure is 2.5 or less. (6) The intrinsic viscosity [η] measured in decahydronaphthalene at 135° C. is in the range of 0.01 to 0.8 dl / g.

2. The copolymer composition for a conveyor belt according to claim 1, characterized in that the ethylene / α-olefin / 5-vinyl-2-norbornene copolymer (R), which is the component (R), further satisfies the following requirement (7): (7) The B value represented by the following formula (i) is 1.10 or more. B value = ([EX] + 2[Y]) / [2 x [E] x ([X] + [Y])]... (i) [Here, [E], [X] and [Y] represent the mole fractions of ethylene, α-olefin and 5-vinyl-2-norbornene, respectively, and [EX] represents the ethylene-α-olefin dyad sequence fraction.]

3. The copolymer composition for a conveyor belt according to claim 1, further comprising the following component (J): (J) Organic peroxide crosslinking agent

4. The copolymer composition for a conveyor belt according to claim 1, wherein the ethylene-α-olefin-non-conjugated polyene copolymer (S) which is the component (S) further has an intrinsic viscosity [η] of 0.1 to 5 dL / g and a weight average molecular weight (Mw) of 10,000 to 600,000.

5. 2. The copolymer composition for a conveyor belt according to claim 1, wherein the non-conjugated polyene (C) constituting the ethylene-α-olefin-non-conjugated polyene copolymer (S), which is the component (S), is 5-vinyl-2-norbornene (VNB).

6. The copolymer composition for a conveyor belt according to claim 1, wherein the ethylene-α-olefin-non-conjugated polyene copolymer (S) as the component (S) further contains a constitutional unit derived from a non-conjugated polyene (D) containing only one partial structure selected from the group consisting of the formulae (I) and (II) in the molecule in a weight fraction of 0 to 20% by weight (wherein the total of the weight fractions of (A), (B), (C), and (D) is 100% by weight), and satisfies the following requirement (vi); (vi) the weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer, the weight fraction of the structural unit derived from the non-conjugated polyene (C) (weight fraction (wt%) of (C)), the weight fraction of the structural unit derived from the conjugated polyene (D) (weight fraction (wt%) of (D)), the molecular weight of the non-conjugated polyene (C) (molecular weight of (C)), and the molecular weight of the conjugated polyene (D) (molecular weight of (D)) satisfy the following formula (4): 4.5≦Mw×{(weight fraction of (C) / 100 / molecular weight of (C))+(weight fraction of (D) / 100 / molecular weight of (D))}≦45...Equation (4)

7. The copolymer composition for a conveyor belt according to claim 3, comprising: 95 to 5 parts by mass of the component (S); 5 to 95 parts by mass of the component (F); and 5 to 120 parts by mass of the component (G), 0.1 to 20 parts by mass of the component (H), and 0.1 to 20 parts by mass of the component (R) per 100 parts by mass of the total amount of the components (S) and (F).

8. A heat-resistant conveyor belt comprising the copolymer composition for conveyor belts according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Heat-resisting belt

    JP1999246017A