Copolymer composition and use thereof

The copolymer composition, featuring ethylene/α-olefin/non-conjugated polyene copolymers with specific properties, addresses the need for enhanced abrasion and heat resistance in conveyor belts, offering improved mechanical properties and extended service life.

JP2024141022AInactive Publication Date: 2024-10-10MITSUI CHEMICALS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023052448
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conveyor belts used in high-temperature industrial applications require improved abrasion resistance and heat aging resistance to extend service life and reduce maintenance, with existing ethylene/α-olefin copolymers not meeting the increasing demand for higher performance.

Method used

A copolymer composition comprising ethylene/α-olefin/non-conjugated polyene copolymers with specific intrinsic viscosities, molar ratios, and structural unit fractions, combined with carbon black and liquid polymers, to enhance wear resistance and processability.

Benefits of technology

The copolymer composition exhibits excellent abrasion resistance and processability, making it suitable for conveyor belts with improved mechanical properties and extended service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141022000001
    Figure 2024141022000001
  • Figure 2024141022000002
    Figure 2024141022000002
  • Figure 2024141022000003
    Figure 2024141022000003
Patent Text Reader

Abstract

To provide a copolymer composition suitable for obtaining a molded product having more excellent wear resistance, especially a conveyor belt.SOLUTION: The present invention relates to: a copolymer composition which satisfies two specific requirements different in intrinsic viscosity [η] and comprises an ethylene / α-olefin / non-conjugated polyene copolymer, carbon black and a liquid polymer; and a use thereof.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copolymer composition having excellent abrasion resistance. [Background technology]

[0002] In various industrial fields such as steel, coal, and cement, belt conveyor devices are used as a means of transporting goods, and in particular, there are many cases where high-temperature goods such as clinker, which are about 150 to 250°C, are transported by belt conveyor devices. In view of this situation, there is a demand for conveyor belts with excellent heat aging resistance and wear resistance in order to minimize maintenance work and extend the service life.

[0003] As a method for improving the heat aging resistance, abrasion resistance, etc. of conveyor belts, it has been proposed to use a rubber composition containing an ethylene-1-octene copolymer and an ethylene-propylene copolymer (Patent Document 1).

[0004] Also, a copolymer composition for conveyor belts suitable for obtaining conveyor belts having excellent processability, mechanical properties, heat aging resistance and abrasion resistance has been proposed (Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 11-246017 [Patent Document 2] JP 2022-147453 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in recent years, there has been an increasing demand for higher abrasion resistance in conveyor belts, and it is desired that rubber compositions for heat-resistant conveyor belts that replace conventional products maintain or exceed the heat resistance, mechanical properties, and processability of conventional products.

[0007] An object of the present invention is to obtain a copolymer composition suitable for producing molded articles having superior abrasion resistance, particularly conveyor belts. [Means for solving the problem]

[0008] The present invention relates to the following [1] to [3]. [1] An ethylene-α-olefin-non-conjugated polyene copolymer (S1) (hereinafter referred to as "ethylene-based copolymer (S1)"), which has an intrinsic viscosity [η] in the range of 2.0 to 4.0 dL / g and has structural units derived from ethylene (A1), an α-olefin (B1) having 3 to 20 carbon atoms, and a non-conjugated polyene (C1) containing in the molecule two or more partial structures selected from the group consisting of the following general formulas (I) and (II), in total, and which satisfies the following requirements (i) to (iv): An ethylene-α-olefin-non-conjugated polyene copolymer (S2) (hereinafter referred to as "ethylene-based copolymer (S2)") having structural units derived from ethylene (A2), an α-olefin (B2) having 3 to 20 carbon atoms, and a non-conjugated polyene (C2) containing in the molecule a total of two or more partial structures selected from the group consisting of the following general formulas (I) and (II), and having an intrinsic viscosity [η] in the range of 0.5 dL / g or more and less than 2.0 dL / g, and satisfying the following requirements (i) to (iv): 0.1 to 200 parts by mass of carbon black (B) per 100 parts by mass of the total of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2), and A copolymer composition comprising 0.1 to 100 parts by mass of at least one liquid polymer (C) having an average molecular weight (Mn) of 1,000 to 100,000 selected from an ethylene-α-olefin copolymer (C1), a liquid polyisoprene (C2), and a liquid polybutadiene (C3). [Ethylene-α-olefin-non-conjugated polyene copolymer (S1)] (i) The molar ratio of ethylene / α-olefin is 40 / 60 to 99.9 / 0.1. (ii) The weight fraction of the constitutional units derived from the non-conjugated polyene (C1) is in the range of 0.07 to 10% by weight in 100% by weight of the ethylene-α-olefin-non-conjugated polyene copolymer. (iii) The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer (S1), the weight fraction of the constitutional unit derived from the non-conjugated polyene (C1) [weight fraction (wt%) of (C1)], and the molecular weight of the non-conjugated polyene (C1) [molecular weight of (C1)] satisfy the following formula (1-1). 4.5≦Mw×weight fraction of (C1) / 100 / [molecular weight of (C1)]≦40 ...Formula (1-1) (iv) The ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, which are obtained by linear viscoelastic measurement (190°C) using a rheometer, the intrinsic viscosity [η], and the weight fraction of the constituent units derived from the non-conjugated polyene (C1) (weight fraction of (C1)), satisfy the following formula (2-1): P / ([η] 2.9 ) ≦ Weight fraction of (C1) × 6 Equation (2-1) [Ethylene-α-olefin-non-conjugated polyene copolymer (S2)] (i) The molar ratio of ethylene / α-olefin is 40 / 60 to 99.9 / 0.1. (ii) The weight fraction of the constitutional units derived from the non-conjugated polyene (C2) is in the range of 0.07 to 10% by weight in 100% by weight of the ethylene-α-olefin-non-conjugated polyene copolymer. (iii) The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer (S2), the weight fraction of the constitutional unit derived from the non-conjugated polyene (C2) [weight fraction (wt%) of (C2)], and the molecular weight of the non-conjugated polyene (C2) [molecular weight of (C2)] satisfy the following formula (1-2). 4.5≦Mw×weight fraction of (C2) / 100 / [molecular weight of (C2)]≦40 ...Formula (1-2) (iv) The ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, which are obtained by linear viscoelastic measurement (190°C) using a rheometer, the intrinsic viscosity [η], and the weight fraction of the constituent units derived from the non-conjugated polyene (C2) (weight fraction of (C2)), satisfy the following formula (2-2): P / ([η] 2.9 ) ≦ Weight fraction of (C2) × 6 Equation (2-2)

[0009] [ka]

[0010] [2] The copolymer composition according to item [1], wherein the non-conjugated polyene (C1) and the non-conjugated polyene (C2) are 5-vinyl-2-norbornene (VNB). [3] A conveyor belt made using the copolymer composition according to item [1] or [2]. Effect of the Invention

[0011] The copolymer composition of the present invention has excellent processability and abrasion resistance, and therefore can be suitably used for molded articles requiring abrasion resistance, particularly for conveyor belts. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] <Ethylene-α-olefin-non-conjugated polyene copolymer (S1)> The ethylene-α-olefin-non-conjugated polyene copolymer (S1), which is one of the components contained in the copolymer composition of the present invention, has structural units derived from ethylene (A1), an α-olefin (B1) having 3 to 20 carbon atoms, and a non-conjugated polyene (C1) containing, in the molecule, two or more partial structures selected from the group consisting of the following general formulas (I) and (II), and satisfies the following requirements (i) to (iv) [hereinafter referred to as "ethylene-based copolymer (S1)]. The intrinsic viscosity [η] of the ethylene copolymer (S1) was measured at 135° C. using decalin as a solvent.

[0013] [ka]

[0014] <Requirement (i)> The requirement (i) specifies that the molar ratio of ethylene / α-olefin in the ethylene-based copolymer (S1) satisfies 40 / 60 to 99.9 / 0.1, and this molar ratio preferably satisfies 50 / 50 to 90 / 10, more preferably 55 / 45 to 85 / 15, and even more preferably 55 / 45 to 78 / 22.

[0015] The ethylene content (content of structural units derived from ethylene (A1)) and the α-olefin content (content of structural units derived from α-olefin (B1)) in the ethylene copolymer (S1) are 13 It can be determined by C-NMR.

[0016] The α-olefin (B1) constituting the ethylene copolymer (S1) is preferably an α-olefin having 3 to 20 carbon atoms, and specific examples thereof include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-eicosene. Among these, α-olefins having 3 to 8 carbon atoms such as propylene, 1-butene, 1-hexene, and 1-octene are preferred, and propylene is particularly preferred. Such α-olefins are preferred because the raw material cost is relatively low, the resulting ethylene copolymer (S1) exhibits excellent mechanical properties, and a molded article having rubber elasticity can be obtained. These α-olefins may be used alone or in combination.

[0017] <Requirement (ii)> Requirement (ii) specifies that the mass fraction of the structural units derived from the non-conjugated polyene (C1) in the ethylene-based copolymer (S1) is in the range of 0.07 to 10 mass% in 100 mass% of the ethylene-based copolymer (S1) (i.e., in the total mass fraction of all structural units, 100 mass%). The mass fraction of the structural units derived from the non-conjugated polyene (C1) is preferably 0.1 to 8.0 mass%, more preferably 0.5 to 5.0 mass%.

[0018] When the ethylene-based copolymer (S1) according to the present invention satisfies the requirement (ii), the copolymer composition of the present invention has sufficient hardness and excellent mechanical properties, which is preferable. When crosslinked using a peroxide, the copolymer composition of the present invention exhibits a fast crosslinking rate, which is preferable because the copolymer composition of the present invention is suitable for producing a crosslinked molded article.

[0019] The amount of non-conjugated polyene (C1) in the ethylene copolymer (S1) (the content of structural units derived from the non-conjugated polyene (C1)) is 13 It can be determined by C-NMR. Examples of the non-conjugated polyene (C1) containing two or more partial structures selected from the group consisting of the general formulae (I) and (II) in the molecule in total include 5-vinyl-2-norbornene (VNB), norbornadiene, 1,4-hexadiene, and dicyclopentadiene. Among these, it is preferable that the non-conjugated polyene (C1) contains VNB, and it is more preferable that the non-conjugated polyene (C1) is VNB, because it is highly available, has good hydrosilyl crosslinking, and is likely to improve the heat resistance of the polymer composition. The non-conjugated polyene (C1) may be used alone or in combination of two or more kinds.

[0020] The ethylene-α-olefin-non-conjugated polyene copolymer (S1) according to the present invention may contain, in addition to structural units derived from ethylene (A), the α-olefin (B) having 3 to 20 carbon atoms, and the non-conjugated polyene (C), a structural unit derived from a non-conjugated polyene (D) containing in the molecule only one partial structure selected from the group consisting of the general formulae (I) and (II).

[0021] Examples of such non-conjugated polyenes (D) include 5-ethylidene-2-norbornene (ENB), 5-methylene-2-norbornene, 5-(2-propenyl)-2-norbornene, 5-(3-butenyl)-2-norbornene, 5-(1-methyl-2-propenyl)-2-norbornene, 5-(4-pentenyl)-2-norbornene, 5-(1-methyl-3-butenyl)-2-norbornene, 5-(5-hexenyl)-2-norbornene, 5-(1-methyl-4-pentenyl)-2-norbornene, 5-(2,3-dimethyl-3-butenyl)-2-norbornene, 5-(2-ethyl-3-butenyl)-2-norbornene, 5-(6-heptenyl)-2-norbornene, 5-(3-methyl-5-hexenyl)-2-norbornene, 5-(3,4-dimethyl-4-pentenyl)-2-norbornene, 5-(3-ethyl-4-pentenyl)-2-norbornene, 5-(7-octenyl)-2-norbornene, 5-(2-methyl-6-heptenyl)-2-norbornene, 5-(1,2-dimethyl-5-hexenyl)-2-norbornene, 5-(5-ethyl-5-hexenyl)-2-norbornene, 5-(1,2,3-trimethyl-4-pentenyl)-2-norbornene, etc. Among these, ENB is preferred because it is highly available, the crosslinking rate during hydrosilyl crosslinking is easily controlled, and good mechanical properties are easily obtained. The non-conjugated polyenes (D) may be used alone or in combination of two or more.

[0022] <Requirement (iii)> The requirement (iii) is that the weight average molecular weight (Mw) of the ethylene-based copolymer (S1), the weight fraction of the constitutional unit derived from the non-conjugated polyene (C1) [weight fraction (wt%) of (C1)], and the molecular weight of the non-conjugated polyene (C1) [molecular weight of (C1)] satisfy the following formula (1-1): 4.5≦Mw×weight fraction of (C1) / 100 / [molecular weight of (C1)]≦40 ...Formula (1-1)

[0023] When the ethylene-based copolymer (S1) according to the present invention satisfies the requirement (iii), the content of the structural unit derived from the non-conjugated polyene (C1) such as VNB is appropriate, and the copolymer composition according to the present invention exhibits sufficient crosslinking performance and a molded article obtained from the copolymer composition according to the present invention has excellent abrasion resistance.

[0024] It is more preferable that the ethylene copolymer (S1) according to the present invention satisfies the following relational formula (1'-1). 4.5≦Mw×mass fraction of (C1) / 100 / (C1) molecular weight≦35 ...Formula (1'-1) The weight average molecular weight (Mw) of the ethylene copolymer (S1) can be determined as a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0025] When the ethylene copolymer (S1) according to the present invention satisfies the above formula (1-1) or (1'-1) in terms of "Mw×mass fraction (C1) / 100 / molecular weight (C1)", the degree of crosslinking is appropriate, and by using this, a molded article having a good balance between mechanical properties and heat aging resistance can be produced. When the "Mw×mass fraction (C1) / 100 / molecular weight (C1)" is too low, the crosslinking rate may be slow due to insufficient crosslinking, and when it is too high, excessive crosslinking may occur, resulting in deterioration of the mechanical properties of the resulting foam.

[0026] <Requirement (iv)> The ethylene-based copolymer (S1) according to the present invention has a ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, which are obtained by linear viscoelastic measurement (190°C) using a rheometer, a limiting viscosity [η], and a weight fraction of the constitutional unit derived from the non-conjugated polyene (C1) (weight fraction of (C1)), which satisfy the following formula (2-1): P / ([η] 2.9 ) ≦ Weight fraction of (C1) × 6 Equation (2-1)

[0027] Here, the complex viscosity η at frequency ω=0.1rad / s * ( ω =0.1) and the complex viscosity η at frequency ω=100rad / s * ( ω =100) Relative to P(η * ( ω =0.1) / η * ( ω =100) ) represents the frequency dependence of viscosity and is the left side of equation (2), P / ([η] 2.9 ) tends to show a high value when there are many long chain branches, although it is influenced by short chain branches and molecular weight. In general, in an ethylene-α-olefin-non-conjugated polyene copolymer, the more constitutional units derived from non-conjugated polyenes are contained, the more long chain branches are contained. However, the ethylene-based copolymer (S1) according to the present invention has less long chain branches than the conventionally known ethylene-α-olefin-non-conjugated polyene copolymers, and is therefore considered to be able to satisfy the above formula (2). In the present invention, the P value is determined as the ratio (η* ratio) of the complex viscosity at 0.1 rad / s and the complex viscosity at 100 rad / s, which are measured using a viscoelasticity measuring device Ares (manufactured by Rheometric Scientific) under conditions of 190°C, strain 1.0%, and various frequencies.

[0028] The ethylene copolymer (S1) according to the present invention preferably satisfies the following formula (2'-1). P / ([η] 2.9 ) ≦ mass fraction of (C1) × 5.7 Equation (2'-1) The intrinsic viscosity [η] means a value measured in decalin at 135°C.

[0029] <Ethylene-α-olefin-non-conjugated polyene copolymer (S2)> The ethylene-α-olefin-non-conjugated polyene copolymer (S2), which is one of the components contained in the copolymer composition of the present invention, has structural units derived from ethylene (A2), an α-olefin (B2) having 3 to 20 carbon atoms, and a non-conjugated polyene (C2) containing, in the molecule, two or more partial structures selected from the group consisting of the following general formulas (I) and (II), and satisfies the following requirements (i) to (iv) [hereinafter referred to as "ethylene-based copolymer (S2)], having an intrinsic viscosity [η] in the range of 0.5 dL / g or more and less than 2.0 dL / g, preferably 0.6 to 1.8 dL / g, and more preferably 0.8 to 1.5 dL / g. The intrinsic viscosity [η] of the ethylene copolymer (S2) was measured at 135° C. using decalin as a solvent.

[0030] [ka]

[0031] <Requirement (i)> The requirement (i) specifies that the molar ratio of ethylene / α-olefin in the ethylene-based copolymer (S2) satisfies 40 / 60 to 99.9 / 0.1, and this molar ratio preferably satisfies 50 / 50 to 90 / 10, more preferably 55 / 45 to 85 / 15, and even more preferably 55 / 45 to 78 / 22.

[0032] The ethylene content (content of structural units derived from ethylene (A2)) and the α-olefin content (content of structural units derived from α-olefin (B2)) in the ethylene copolymer (S2) are 13 It can be determined by C-NMR.

[0033] The α-olefin (B2) constituting the ethylene copolymer (S2) is preferably an α-olefin having 3 to 20 carbon atoms, and specific examples thereof include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-eicosene. Among these, α-olefins having 3 to 8 carbon atoms such as propylene, 1-butene, 1-hexene, and 1-octene are preferred, and propylene is particularly preferred. Such α-olefins are preferred because the raw material cost is relatively low, the resulting ethylene copolymer (S1) exhibits excellent mechanical properties, and a molded article having rubber elasticity can be obtained. These α-olefins may be used alone or in combination.

[0034] <Requirement (ii)> Requirement (ii) specifies that the mass fraction of the structural units derived from the non-conjugated polyene (C2) in the ethylene copolymer (S2) is in the range of 0.07 to 10 mass% in 100 mass% of the ethylene copolymer (S2) (i.e., in the total mass fraction of all structural units, 100 mass%). The mass fraction of the structural units derived from the non-conjugated polyene (C2) is preferably 0.1 to 8.0 mass%, more preferably 0.5 to 5.0 mass%.

[0035] When the ethylene-based copolymer (S2) according to the present invention satisfies the requirement (ii), the copolymer composition of the present invention has sufficient hardness and excellent mechanical properties, which is preferable. When crosslinked using a peroxide, the copolymer composition of the present invention exhibits a fast crosslinking rate, which is preferable because the copolymer composition of the present invention is suitable for producing a crosslinked molded article.

[0036] The amount of non-conjugated polyene (C2) in the ethylene copolymer (S2) (the content of constitutional units derived from non-conjugated polyene (C2)) is 13 It can be determined by C-NMR. Examples of the non-conjugated polyene (C2) containing two or more partial structures selected from the group consisting of the general formulae (I) and (II) in the molecule in total include 5-vinyl-2-norbornene (VNB), norbornadiene, 1,4-hexadiene, and dicyclopentadiene. Among these, it is preferable that the non-conjugated polyene (C2) contains VNB, and it is more preferable that the non-conjugated polyene (C2) is VNB, because it is highly available, has good hydrosilyl crosslinking, and is likely to improve the heat resistance of the polymer composition. The non-conjugated polyene (C2) may be used alone or in combination of two or more kinds.

[0037] The ethylene-α-olefin-non-conjugated polyene copolymer (S2) according to the present invention may contain, in addition to structural units derived from ethylene (A2), the α-olefin (B2) having 3 to 20 carbon atoms, and the non-conjugated polyene (C2), a structural unit derived from a non-conjugated polyene (D2) containing in the molecule only one partial structure selected from the group consisting of the general formulae (I) and (II).

[0038] Examples of such non-conjugated polyenes (D2) include 5-ethylidene-2-norbornene (ENB), 5-methylene-2-norbornene, 5-(2-propenyl)-2-norbornene, 5-(3-butenyl)-2-norbornene, 5-(1-methyl-2-propenyl)-2-norbornene, 5-(4-pentenyl)-2-norbornene, 5-(1-methyl-3-butenyl)-2-norbornene, 5-(5-hexenyl)-2-norbornene, 5-(1-methyl-4-pentenyl)-2-norbornene, 5-(2,3-dimethyl-3-butenyl)-2-norbornene, 5-(2-ethyl-3-butenyl)-2-norbornene, 5-(6-heptenyl)-2-norbornene, 5-(3-methyl-5-hexenyl)-2-norbornene, 5-(3,4-dimethyl-4-pentenyl)-2-norbornene, 5-(3-ethyl-4-pentenyl)-2-norbornene, 5-(7-octenyl)-2-norbornene, 5-(2-methyl-6-heptenyl)-2-norbornene, 5-(1,2-dimethyl-5-hexenyl)-2-norbornene, 5-(5-ethyl-5-hexenyl)-2-norbornene, 5-(1,2,3-trimethyl-4-pentenyl)-2-norbornene, etc. Among these, ENB is preferred because it is highly available, the crosslinking rate during hydrosilyl crosslinking is easily controlled, and good mechanical properties are easily obtained. The non-conjugated polyenes (D2) may be used alone or in combination of two or more.

[0039] <Requirement (iii)> The requirement (iii) is a provision that the weight average molecular weight (Mw) of the ethylene copolymer (S2), the weight fraction of the constitutional unit derived from the non-conjugated polyene (C2) [weight fraction (wt%) of (C2)], and the molecular weight of the non-conjugated polyene (C2) [molecular weight of (C2)] satisfy the following formula (1-2): 4.5≦Mw×weight fraction of (C1) / 100 / [molecular weight of (C1)]≦40 ...Formula (1-2)

[0040] When the ethylene-based copolymer (S2) according to the present invention satisfies the requirement (iii), the content of the structural unit derived from the non-conjugated polyene (C2) such as VNB is appropriate, and the copolymer composition according to the present invention exhibits sufficient crosslinking performance, and the molded article obtained from the copolymer composition according to the present invention has excellent abrasion resistance.

[0041] The ethylene copolymer (S1) according to the present invention more preferably satisfies the following relational formula (1'-2). 4.5≦Mw×(C2) mass fraction / 100 / (C2) molecular weight≦35 ...Formula (1'-2) The weight average molecular weight (Mw) of the ethylene copolymer (S2) can be determined as a polystyrene-equivalent value measured by gel permeation chromatography (GPC).

[0042] The ethylene copolymer (S2) according to the present invention has an appropriate degree of crosslinking when "Mw×mass fraction of (C2) / 100 / molecular weight of (C2)" satisfies the above formula (1-2) or (1'-2), and by using this, a molded article having a good balance of mechanical properties and heat aging resistance can be produced. If "Mw×mass fraction of (C2) / 100 / molecular weight of (C2)" is too low, the crosslinking property may be insufficient, resulting in a slow crosslinking rate.

[0043] <Requirement (iv)> The ethylene-based copolymer (S2) according to the present invention has a ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, which are obtained by linear viscoelastic measurement (190°C) using a rheometer, a limiting viscosity [η], and a weight fraction of the constitutional unit derived from the non-conjugated polyene (C2) (weight fraction of (C1)), which satisfy the following formula (2-2): P / ([η] 2.9 ) ≦ Weight fraction of (C2) × 6 Equation (2-2)

[0044] Here, the complex viscosity η at frequency ω=0.1rad / s * ( ω =0.1) and the complex viscosity η at frequency ω=100rad / s * ( ω =100) Relative to P(η * ( ω =0.1) / η * ( ω =100) ) represents the frequency dependence of viscosity, and is the left side of equation (2-2) P / ([η] 2.9 ) tends to show a high value when there are many long chain branches, although it is influenced by short chain branches and molecular weight. In general, in an ethylene-α-olefin-non-conjugated polyene copolymer, the more structural units derived from non-conjugated polyenes are contained, the more long chain branches are contained. However, the ethylene-based copolymer (S2) according to the present invention has less long chain branches than the conventionally known ethylene-α-olefin-non-conjugated polyene copolymers, and is therefore considered to be able to satisfy the above formula (2-2). In the present invention, the P value is determined by calculating the ratio (η* ratio) of the complex viscosity at 0.1 rad / s and the complex viscosity at 100 rad / s, which are measured using a viscoelasticity measuring device Ares (manufactured by Rheometric Scientific) under conditions of 190°C, strain 1.0%, and various frequencies.

[0045] The ethylene copolymer (S2) according to the present invention preferably satisfies the following formula (2'-2). P / ([η] 2.9 ) ≦ mass fraction of (C2) × 5.7 Equation (2'-2) The intrinsic viscosity [η] means a value measured in decalin at 135°C.

[0046] <Production method of ethylene-α-olefin-non-conjugated polyene copolymer (S1) and ethylene-α-olefin-non-conjugated polyene copolymer (S2)> The ethylene copolymer (S1) and the ethylene copolymer (S2) according to the present invention may be prepared by any method as long as they satisfy the above requirements (i) to (v), but are preferably obtained by copolymerizing monomers in the presence of a metallocene compound, and more preferably obtained by copolymerizing monomers in the presence of a catalyst system containing a metallocene compound. When copolymerizing, the monomers (ethylene, α-olefin, non-conjugated polyene) may be derived from biomass.

[0047] As a specific method for producing the above-mentioned copolymer (S1) and copolymer (S2) according to the present invention, for example, the production method using a metallocene catalyst described in JP 2018-119096 A and WO 2015 / 122495 A can be adopted.

[0048] <Carbon black (B)> Carbon black (B), which is one of the components contained in the copolymer composition of the present invention (hereinafter, may be abbreviated as "component (B)"), is a type of known rubber reinforcing agent blended into the copolymer composition, and is an inorganic substance generally known as carbon black.

[0049] Specific examples of the carbon black (B) used in the present invention include Asahi #55G, Asahi #60G, Asahi #60UG, and Asahi #70G (all manufactured by Asahi Carbon Co., Ltd.), Seast (V, SO, 116, 3, 6, 9, SP, TA, etc.) carbon blacks (manufactured by Tokai Carbon Co., Ltd.), and VULCAN3 and STERLING (SO, V, VH, 142, etc.) carbon blacks (all manufactured by Cabot Corporation), as well as carbon blacks which have been surface-treated with a silane coupling agent or the like.

[0050] <Liquid Polymer (C)> The liquid polymer (C), which is one of the components contained in the copolymer composition of the present invention, has an average molecular weight (Mn) in the range of 1,000 to 100,000, more preferably 2,000 to 90,000, and even more preferably 2,500 to 80,000, and is at least one liquid polymer selected from ethylene-α-olefin copolymer (C1), liquid polyisoprene (C2), and liquid polybutadiene (C3).

[0051] Ethylene-α-olefin copolymer (C1) The ethylene-α-olefin copolymer (C1), which is one of the liquid polymers according to the present invention, is a liquid polymer that is a copolymer of ethylene and an α-olefin. The α-olefin is preferably an α-olefin having 3 to 20 carbon atoms, and specific examples thereof include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-eicosene. Among these, α-olefins having 3 to 8 carbon atoms, such as propylene, 1-butene, 1-hexene, and 1-octene, are preferred, and propylene is particularly preferred.

[0052] The ethylene-α-olefin copolymer (C1) according to the present invention is particularly preferably a liquid ethylene-propylene copolymer, and has a dynamic viscosity at 40° C. of 1 to 80,000 mm 2 / s is preferred.

[0053] Dynamic viscosity at 40℃ is 1mm 2 Ethylene-propylene copolymers with a viscosity of less than 80,000 mm / s contain a large amount of low molecular weight components that are easily volatile, which may result in a deterioration in the heat resistance of the resulting ethylene copolymer composition. 2 If the ratio exceeds 1 / s, the amount of high molecular weight components increases, which may result in insufficient viscosity, and the effect of improving the tackiness of the resulting copolymer composition for a conveyor belt may be reduced.

[0054] Liquid polyisoprene (C2) Liquid polyisoprene (C2), which is one of the liquid polymers according to the present invention, is manufactured and sold, for example, by Kuraray Co., Ltd. under the name Kuraray Liquid Rubber Liquid Isoprene Rubber (L-IR).

[0055] Liquid polybutadiene (C3) Liquid polybutadiene (C3), which is one of the liquid polymers according to the present invention, is manufactured and sold, for example, by Kuraray Co., Ltd. under the name Kuraray Liquid Rubber Liquid Butadiene Rubber (L-BR).

[0056] ≪Copolymer composition≫ The copolymer composition of the present invention contains the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2), and the ratio (mass ratio) of the ethylene-based copolymer (S1) to the ethylene-based copolymer (S2) in the copolymer composition is 90 / 10 to 10 / 90, preferably 80 / 20 to 20 / 80, more preferably 70 / 30 to 30 / 70, where the total of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2) is 100 mass. By satisfying the above range, the copolymer composition obtained has excellent processability.

[0057] The copolymer composition of the present invention is a composition containing the ethylene-based copolymer (S1), the ethylene-based copolymer (S2), the carbon black (B), and the liquid polymer (C), and contains 0.1 to 200 parts by mass of carbon black (B) and 0.1 to 100 parts by mass of liquid polymer (C) per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0058] The copolymer composition of the present invention contains the ethylene-based copolymer (S1), the ethylene-based copolymer (S2), the carbon black (B), and the liquid polymer (C) in the above-mentioned ranges, respectively, and therefore the resulting copolymer composition has excellent abrasion resistance and moldability.

[0059] The copolymer composition of the present invention may contain, in addition to the above-mentioned components, other compounding agents, such as at least one selected from a crosslinking agent, a crosslinking assistant, a softener, an antiaging agent, a processing assistant, an activator, a heat stabilizer, a weathering stabilizer, an antistatic agent, a colorant, a lubricant, a thickener, an antifoaming agent, a foaming agent, and a foaming assistant, within the scope of the object of the present invention. Each additive may be used alone or in combination of two or more.

[0060] <Crosslinking Agent> Examples of the crosslinking agent include crosslinking agents that are generally used when crosslinking rubber, such as organic peroxides, sulfur-based compounds, phenolic resins, hydrosilicone-based compounds, amino resins, quinones or their derivatives, amine-based compounds, azo-based compounds, epoxy-based compounds, and isocyanate-based compounds. Among these, organic peroxides and sulfur-based compounds (also called vulcanizing agents) are preferred.

[0061] 《Organic peroxide》 Examples of organic peroxides include dicumyl peroxide, di-tert-butyl peroxide, 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butyl peroxybenzoate, tert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.

[0062] In the copolymer composition of the present invention, when an organic peroxide is used as a crosslinking agent, the content of the organic peroxide is usually 0.1 to 20 parts by mass, preferably 0.2 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0063] When an organic peroxide is used as a crosslinking agent, it is preferable to use a crosslinking auxiliary in combination. In this case, the copolymer composition of the present invention further containing a crosslinking auxiliary may be used, and the organic peroxide may be blended with the copolymer composition before the crosslinking step, and the crosslinking step may be performed.

[0064] <Crosslinking aid> Examples of the crosslinking aid include sulfur; quinone dioxime-based crosslinking aids such as p-quinone dioxime; crosslinking aids having two or more ethylenic double bonds; maleimide-based crosslinking aids; and metal oxides such as zinc oxide (e.g., ZnO#1 / zinc oxide type 2 (JIS standard (K-1410)), manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name, manufactured by Inoue Lime Industry Co., Ltd.)). Of these, crosslinking aids having two or more ethylenic double bonds are preferred.

[0065] The number of ethylenic double bonds in the crosslinking aid having two or more ethylenic double bonds is preferably 2 to 6, more preferably 2 to 4. Examples of the crosslinking aid having two or more ethylenic double bonds include (meth)acrylic crosslinking aids such as ethylene glycol di(meth)acrylate and trimethylolpropane tri(meth)acrylate; allyl crosslinking aids such as diallyl phthalate and triallyl isocyanurate; and vinyl crosslinking aids such as divinylbenzene. Among these, (meth)acrylic crosslinking aids are preferred, and ethylene glycol dimethacrylate is more preferred.

[0066] When the copolymer composition of the present invention contains a crosslinking auxiliary, the content of the crosslinking auxiliary is usually 0.5 to 10 mol, preferably 0.5 to 7 mol, more preferably 1 to 5 mol, per 1 mol of the organic peroxide.

[0067] 《Sulfur compounds》 Specific examples of sulfur-based compounds include sulfur, sulfur chloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, tetramethylthiuram disulfide, and selenium dithiocarbamate.

[0068] In the copolymer composition of the present invention, when a sulfur-based compound is used as a crosslinking agent, the content of the sulfur-based compound is usually 0.3 to 10 parts by mass, preferably 0.5 to 7.0 parts by mass, and more preferably 0.7 to 5.0 parts by mass, relative to 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0069] When a sulfur-based compound is used as a crosslinking agent, it is preferable to use a vulcanization accelerator in combination. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, N,N'-diisopropyl-2-benzothiazole sulfenamide, 2-mercaptobenzothiazole, 2-(4-morpholinodithio)benzothiazole, 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-diethyl-4-morpholinothio)benzothiazole, and dibenzothiazyl disulfide; guanidine-based vulcanization accelerators such as diphenylguanidine, triphenylguanidine, and diorthotolylguanidine; aldehyde amine-based vulcanization accelerators such as acetaldehyde-aniline condensation product and butylaldehyde-aniline condensation product; 2-mercaptoimidazoline; imidazoline-based vulcanization accelerators such as diethylthiourea and dibutylthiourea; thiuram-based vulcanization accelerators such as tetramethylthiuram monosulfide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, and dipentamethylenethiuram tetrasulfide; dithioacid salt-based vulcanization accelerators such as zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, and tellurium diethyldithiocarbamate; thiourea-based vulcanization accelerators such as ethylenethiourea (for example, Suncerer 22C (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), N,N'-diethylthiourea, and N,N'-dibutylthiourea; xanthate-based vulcanization accelerators such as zinc dibutylxatogenate; and others such as zinc oxide.

[0070] When the copolymer composition for sealing parts of the present invention contains a vulcanization accelerator, the content of the vulcanization accelerator is usually 0.1 to 20 parts by mass, preferably 0.2 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0071] The vulcanization aid can be preferably used when the crosslinking agent is a sulfur-based compound, and examples thereof include zinc oxide (e.g., ZnO#1 / zinc oxide type 2, manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name; manufactured by Inoue Seki Kogyo Co., Ltd.)).

[0072] When the copolymer composition for sealing parts of the present invention contains a vulcanization aid, the content of the vulcanization aid is usually 1 to 20 parts by mass per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0073] The copolymer composition of the present invention may further contain at least one selected from inorganic fillers, reinforcing materials other than carbon black, antioxidants, processing aids, activators, moisture absorbents, antistatic agents, colorants, lubricants, and thickeners. The copolymer composition of the present invention may further contain other polymers, such as elastomers and / or rubbers, in addition to the copolymers (S1) and (S2). Each of the components described below may be used alone or in combination of two or more.

[0074] <Crosslinking aid> Examples of the crosslinking aid include sulfur; quinone dioxime-based crosslinking aids such as p-quinone dioxime; acrylic crosslinking aids such as ethylene glycol dimethacrylate and trimethylolpropane trimethacrylate; allyl crosslinking aids such as diallyl phthalate and triallyl isocyanurate; maleimide-based crosslinking aids; divinylbenzene; and metal oxides such as zinc oxide (e.g., ZnO#1·zinc oxide type 2 (JIS standard (K-1410)), manufactured by Hakusui Tech Co., Ltd.), magnesium oxide, and activated zinc oxide (e.g., zinc oxide such as "META-Z102" (trade name, manufactured by Inoue Lime Industry Co., Ltd.)).

[0075] When a crosslinking auxiliary is used, the amount of the crosslinking auxiliary in the copolymer composition is usually 0.5 to 10 mol, preferably 0.5 to 7 mol, more preferably 1 to 6 mol, per mol of the organic peroxide-based crosslinking agent.

[0076] <Inorganic fillers> Examples of inorganic fillers include light calcium carbonate, heavy calcium carbonate, talc, and clay. Of these, heavy calcium carbonate is preferred.

[0077] When the copolymer composition of the present invention contains an inorganic filler, the content of the inorganic filler is usually 2 to 50 parts by mass, preferably 5 to 50 parts by mass, per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0078] <Reinforcing agent> Examples of the reinforcing agent include silica, calcium carbonate, activated calcium carbonate, fine talc, and differential silicic acid, except for the above-mentioned carbon black (B).

[0079] When the copolymer composition of the present invention contains a reinforcing agent, the content of the reinforcing agent is usually 0.1 to 100 parts by mass, preferably 5 to 30 parts by mass, per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0080] <Softener> Examples of the softener that may be contained in the copolymer composition of the present invention include petroleum-based softeners such as process oil, lubricating oil, paraffin oil, liquid paraffin, petroleum asphalt, and Vaseline; coal tar-based softeners such as coal tar; fatty oil-based softeners such as castor oil, linseed oil, rapeseed oil, soybean oil, and coconut oil; waxes such as beeswax and carnauba wax; naphthenic acid, pine oil, rosin or derivatives thereof; synthetic polymer substances such as terpene resins, petroleum resins, and coumarone-indene resins; ester-based softeners such as dioctyl phthalate and dioctyl adipate; and other microcrystalline waxes, liquid polybutadiene, modified liquid polybutadiene, hydrocarbon-based synthetic lubricating oils, tall oil, and sub(factice). Of these, petroleum-based softeners and hydrocarbon-based synthetic lubricating oils are preferred, and process oils are particularly preferred.

[0081] When the copolymer composition of the present invention contains a reinforcing agent, the content of the reinforcing agent is usually 0.1 to 100 parts by mass, preferably 5 to 30 parts by mass, per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0082] <Anti-aging agent (stabilizer)> The copolymer composition for sealing parts of the present invention contains an antioxidant (stabilizer), which can extend the life of a (crosslinked) molded article formed from the copolymer composition for sealing parts. Examples of the antioxidant include amine-based antioxidants, phenol-based antioxidants, and sulfur-based antioxidants.

[0083] Examples of the amine-based antiaging agents include aromatic secondary amine-based antiaging agents such as phenylbutylamine and N,N-di-2-naphthyl-p-phenylenediamine. Examples of the phenol-based antiaging agents include dibutylhydroxytoluene and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]. Examples of the sulfur-based antiaging agents include thioether-based antiaging agents such as bis[2-methyl-4-(3-n-alkylthiopropionyloxy)-5-t-butylphenyl]sulfide; dithiocarbamate-based antiaging agents such as nickel dibutyldithiocarbamate; 2-mercaptobenzoylimidazole, 2-mercaptobenzimidazole, zinc salt of 2-mercaptobenzimidazole, dilaurylthiodipropionate, and distearylthiodipropionate.

[0084] When the copolymer composition for sealing parts of the present invention contains an antioxidant, the content of the antioxidant is usually 0.3 to 10 parts by mass, preferably 0.5 to 7.0 parts by mass, per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0085] <Processing aids> As the processing aid, a wide variety of processing aids that are generally compounded with rubber can be used. Examples of processing aids include ricinoleic acid, stearic acid, palmitic acid, lauric acid, barium stearate, zinc stearate, calcium stearate, and esters. Among these, stearic acid is preferred.

[0086] When the copolymer composition for sealing parts of the present invention contains a processing aid, the content of the processing aid is usually 10 parts by mass or less, and preferably 8.0 parts by mass or less, per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0087] <Activator> Examples of the activator include amines such as di-n-butylamine, dicyclohexylamine, and monoethanolamine; activators such as diethylene glycol, polyethylene glycol, lecithin, triaryl methylate, and zinc compounds of aliphatic or aromatic carboxylic acids; zinc peroxide preparations; octadecyltrimethylammonium bromide, synthetic hydrotalcite, and special quaternary ammonium compounds.

[0088] When the copolymer composition for sealing parts of the present invention contains an activator, the content of the activator is usually 0.2 to 10 parts by mass, preferably 0.3 to 5 parts by mass, per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0089] <Moisture absorbent> Examples of moisture absorbents include calcium oxide, silica gel, sodium sulfate, molecular sieves, zeolite, and white carbon.

[0090] When the copolymer composition for sealing parts of the present invention contains a moisture absorbent, the content of the moisture absorbent is usually 0.5 to 15 parts by mass, preferably 1.0 to 12 parts by mass, per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0091] <Other polymers> The copolymer composition for sealing parts of the present invention may further contain other polymers in addition to the copolymer (S1) and the copolymer (S2).

[0092] Other polymers that require crosslinking include, for example, rubbers such as natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, chloroprene rubber, nitrile rubber, butyl rubber, acrylic rubber, silicone rubber, fluororubber, and urethane rubber.

[0093] Other polymers that do not require crosslinking include, for example, elastomers such as styrene-butadiene block copolymers (SBS), styrene-based thermoplastic elastomers (TPS) such as polystyrene-poly(ethylene-butylene)-polystyrene (SEBS) and polystyrene-poly(ethylene-propylene)-polystyrene (SEPS), olefin-based thermoplastic elastomers (TPO), vinyl chloride-based elastomers (TPVC), ester-based thermoplastic elastomers (TPC), amide-based thermoplastic elastomers (TPA), urethane-based thermoplastic elastomers (TPU), and other thermoplastic elastomers (TPZ).

[0094] When the copolymer composition for sealing parts of the present invention contains another polymer, the content of the other polymer is usually 100 parts by mass or less, preferably 80 parts by mass or less, per 100 parts by mass of the total amount of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2).

[0095] <Method for preparing copolymer composition> Examples of the method for preparing the copolymer composition include a method in which the above-mentioned components contained in the copolymer composition are mixed using a conventionally known kneading machine such as a mixer, a kneader, or a roll, or further a continuous kneading machine such as a twin-screw extruder.

[0096] The preparation method of the copolymer composition is not particularly limited, and a preparation method of a general rubber compound can be adopted without any particular limitation. For example, when the copolymer composition of the present invention contains an optional component, at least a part of the optional component may be mixed in advance with the ethylene copolymer (S1) and the ethylene copolymer (S2), and then the remaining optional component may be added. Also, the ethylene copolymer (S1), the ethylene copolymer (S2), the carbon black (B), and the liquid polymer (C) may be mixed, and then the optional component may be added and mixed.

[0097] For example, the ethylene copolymer (S1), the ethylene copolymer (S2), the carbon black (B), the liquid polymer (C) and other components to be mixed as required are kneaded at a temperature of 80 to 170°C for 3 to 10 minutes using internal mixers such as a Banbury mixer, a kneader, and an intermix, and then a crosslinking agent and a crosslinking accelerator, a crosslinking assistant, etc. are added as required, and the mixture is kneaded at a roll temperature of 40 to 80°C for 5 to 30 minutes using rolls such as an open roll or a kneader, and then separated out to prepare the copolymer composition. In this way, a ribbon-shaped or sheet-shaped copolymer composition is usually obtained. When the kneading temperature in the internal mixers is low, the crosslinking agent, the crosslinking accelerator, the foaming agent, etc. can also be kneaded at the same time.

[0098] <Method of manufacturing molded body> The molded article made of the copolymer composition of the present invention can be obtained by vulcanizing (also referred to as crosslinking) the above-mentioned copolymer composition of the present invention. Note that a mold may or may not be used during vulcanization. When a mold is not used, the copolymer composition is usually molded and crosslinked continuously.

[0099] Examples of methods for vulcanizing the copolymer composition include a method in which (a) a copolymer composition containing a vulcanizing agent is preformed into a desired shape, usually by a molding method such as extrusion molding, press molding, or injection molding, or by roll processing, and then heated while molding or by introducing the molded product into a crosslinking tank; and a method in which (b) a copolymer composition containing a vulcanizing agent is preformed by the same method as in method (a), and then irradiated with an electron beam.

[0100] In the method (a), a crosslinking reaction occurs by the crosslinking agent in the copolymer composition by heating, and a molded article is obtained. In the method (b), a crosslinking reaction occurs by electron beams, and a molded article is obtained. In the method (b), the copolymer composition that has been preformed is usually irradiated with an electron beam having an energy of 0.1 to 10 MeV so that the absorbed dose of the copolymer composition is usually 0.5 to 36 Mrad, preferably 0.5 to 20 Mrad, and more preferably 1 to 10 Mrad.

[0101] The vulcanization (crosslinking) of the copolymer composition can be carried out by preforming the uncrosslinked copolymer composition into a desired shape by various molding methods using a molding machine such as an extrusion molding machine, a calendar roll, a press, an injection molding machine, or a transfer molding machine, and then heating the molded product in a crosslinking tank or by irradiating it with radiation such as electron beams, X-rays, γ-rays, α-rays, and β-rays. As the molding or preforming method, a known molding method for molding into a desired shape by extrusion molding, injection molding, inflation molding, blow molding, extrusion blow molding, press molding, vacuum molding, calendar molding, and foam molding can be appropriately adopted. In addition, when the crosslinked molded product is a foam, it can be produced by foam molding an uncrosslinked copolymer composition containing a foaming agent and then crosslinking it by electron beam irradiation or heating, or by proceeding with crosslinking simultaneously with foam molding. Furthermore, the step of crosslinking the copolymer composition may be carried out by combining crosslinking by heating and crosslinking by electron beam crosslinking.

[0102] When the copolymer composition is crosslinked by heating, it is usually preferable to use a copolymer composition containing a vulcanizing agent such as sulfur, a sulfur-based compound, or a peroxide, and heat the copolymer composition for 1 to 30 minutes at a temperature of 150 to 270° C. using a crosslinking bath with a heating form such as hot air, a glass bead fluidized bed, UHF (ultra-high frequency electromagnetic waves), steam, or an LCM (molten salt bath). Sulfur crosslinking or peroxide crosslinking has the advantage that no special equipment is required for the crosslinking step, and therefore has been widely used in the crosslinking step of copolymer compositions.

[0103] In addition, when crosslinking is performed by electron beam crosslinking, it is usually preferable to use a copolymer composition that does not contain a crosslinking agent, and irradiate the preformed copolymer composition with electron beams to produce a crosslinked molded product. Crosslinking by electron beam irradiation can be performed without using a crosslinking agent, and has the advantage that less volatile matter is generated in the crosslinking process.

[0104] Specifically, the manufacture of a crosslinked molded product involving a crosslinking step by electron beam irradiation can be carried out, for example, as follows. First, using a mixer such as a Banbury mixer, the copolymer composition, and if necessary, various additives and crosslinking aids, etc. are kneaded at a temperature of 80 to 170 ° C. for 3 to 10 minutes, and then using rolls such as open rolls, the mixture is kneaded at a roll temperature of 40 to 80 ° C. for 5 to 30 minutes, and then separated to prepare a ribbon-shaped or sheet-shaped copolymer composition, or the copolymer composition is prepared by blending each component in a container or the like. The copolymer composition thus prepared is molded into a desired shape as it is in a sheet shape, etc., or by an extrusion molding machine, a calendar roll, an injection molding machine, or a press, or extruded from an extruder into a strand shape, pulverized by a cutter, etc., into pellets, and irradiated with an electron beam. Alternatively, a powder of a diene rubber (Z) and a copolymer (X) impregnated with a compound such as a crosslinking aid may be directly irradiated with an electron beam to prepare a crosslinked product of the copolymer composition. The electron beam irradiation is carried out using an electron beam having an energy of usually 0.1 to 10 MeV (megaelectronvolts), preferably 0.3 to 5 MeV, so that the absorbed dose is usually 0.5 to 100 kGy (kilograys), preferably 0.5 to 70 kGy.

[0105] Gamma ray irradiation has a higher penetration rate into the copolymer composition than electron beam irradiation, and in particular, when the copolymer composition is irradiated in the form of pellets, a small amount of direct irradiation can sufficiently crosslink the inside of the pellets. Gamma ray irradiation can be performed so that the dose of gamma ray irradiation on the copolymer composition is usually 0.1 to 50 kGy, preferably 0.3 to 50 kGy.

[0106] <Molded body> The copolymer composition of the present invention and the molded articles obtained from the composition, such as crosslinked articles and foamed articles, can be used in various applications. Specifically, they are preferably used for O-rings, industrial rolls, packings (e.g., condenser packings), gaskets, belts (e.g., heat insulating belts, copier belts, conveyor belts), hoses such as automobile hoses (e.g., turbocharger hoses, water hoses, brake reservoir hoses, radiator hoses, air hoses), vibration-proof rubber, vibration-proof or vibration-damping materials (e.g., engine mounts, motor mounts), muffler hangers, sponges (e.g., weather strip sponges, heat insulating sponges, protective sponges, microfoam sponges), cables (ignition cables, cab-tire cables, high tension cables), electric wire coating materials (high voltage electric wire coating materials, low voltage electric wire coating materials, marine electric wire coating materials), glass run channels, colored skin materials, paper feed rolls, roofing sheets, etc.

[0107] <Conveyor belt> The copolymer composition of the present invention is particularly suitable as a material for a conveyor belt because of its excellent abrasion resistance. The conveyor belt made of the copolymer composition of the present invention is produced by using the copolymer composition of the present invention, and specific examples of the structure thereof include the following.

[0108] The conveyor belt has a canvas core and is coated on its outer periphery with a copolymer composition. A conveyor belt comprising a steel cord embedded as a core material in a copolymer composition. The canvas is made of a woven fabric of synthetic fibers such as nylon, vinylon, polyester, etc., and the number of layers of the canvas, the thickness of the copolymer composition, the belt width, etc. are appropriately determined depending on the purpose of use, but the thickness of the copolymer composition is usually about 1.5 to 20 mm.

[0109] The core material made of steel cord is made by twisting together multiple wires with a diameter of about 0.2 to 0.4 mm to form a wire rope with a diameter of about 2.0 to 9.5 mm, and arranging about 50 to 230 steel cords in parallel to form the core material. Generally, the total thickness of the conveyor belt is about 10 to 50 mm.

[0110] The conveyor belt of the present invention can be easily produced by interposing the canvas or steel cord serving as the core material between uncrosslinked sheets formed from the copolymer composition of the present invention, and crosslinking the material by heating and pressing in accordance with a conventional method. The crosslinking conditions are usually 120 to 180°C and 10 to 50 kg / cm. 2 The duration is approximately 10 to 90 minutes. EXAMPLES

[0111] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The methods for evaluating the various properties in the examples and comparative examples are as follows.

[0112] In the examples and comparative examples, the ethylene copolymer (S1-1) produced in the following Production Example 1 was used as the ethylene copolymer (S1).

[0113] [Production Example 1] A 300 L volume polymerization vessel equipped with an agitator was used to continuously polymerize ethylene, propylene, 5 The polymerization reaction of -vinyl-2-norbornene (VNB) was carried out at 87°C.

[0114] Hexane was used as the polymerization solvent (feed rate: 32.6 L / h). Ren feed rate: 3.6 kg / h, propylene rate: 6.1 kg / h, VNB feed rate: The polymerization reactor was continuously fed with 290 g / h and hydrogen feed rate of 6.3 NL / h. Ta.

[0115] The polymerization pressure was kept at 1.6 MPaG and the polymerization temperature at 87°C. aryl)methylene(cyclopentadienyl)(octamethyloctahydrodibenzofluorene Using zirconium dichloride, the feed rate was set at 0.0015 mmol / h. The cocatalyst was (C6H5)3CB(C6F5)4(CB-3 ) was fed at a rate of 0.0075 mmol / h, and triisobutyl ether was used as the organoaluminum compound. The feed rate of triethylammonium tetrahydrofuran (TIBA) was 20 mmol / h. was continuously fed into the vessel.

[0116] Thus, the ethylene-propylene copolymer formed from ethylene, propylene and VNB was A solution containing 15.2% by mass of ethylene-VNB copolymer was obtained. A small amount of methanol is added to the polymerization reaction liquid to terminate the polymerization reaction, and steam stripping is performed. After separating the ethylene-propylene-VNB copolymer from the solvent by a mixing process, it was heated at 80°C for 1 hour. It was dried under vacuum overnight.

[0117] By the above procedure, ethylene propylene formed from ethylene, propylene and VNB was obtained. Propylene-VNB copolymer (S1-1) was obtained at a rate of 4.7 kg / h.

[0118] In the examples and comparative examples, the ethylene copolymer (S2-1) prepared in Production Example 2 below was used as the ethylene copolymer (S2).

[0119] [Production Example 2] <Production of ethylene-propylene-VNB copolymer (S2-1)> In the method for producing an ethylene-propylene-VNB copolymer described in Example 1 (

[0386] to

[0391] ) of WO 2019 / 180802, the amount of hydrogen fed was adjusted to produce the ethylene-propylene-VNB copolymer (S2-1) shown in Table 1 below.

[0120] <Composition of ethylene-propylene-VNB copolymer (S2-1)> The mass fraction (mass%) of each structural unit of the copolymer (S2-1) is 13 The measured values ​​were obtained by C-NMR. The measured values ​​were obtained by using an ECX400P nuclear magnetic resonance apparatus (manufactured by JEOL Ltd.) at a measurement temperature of 120°C, a measurement solvent of orthodichlorobenzene / deuterated benzene = 4 / 1, and an accumulation number of 8000 times. 13 The results were obtained by measuring the C-NMR spectrum.

[0121] <Iodine value> The iodine value of the copolymer (S2-1) was determined by a titration method. Specifically, the measurement was performed by the following method.

[0122] 0.5g of copolymer (S2-1) was dissolved in 60ml of carbon tetrachloride, a small amount of Wiss's reagent and 20% potassium iodide solution were added, and the solution was titrated with 0.1mol / L sodium thiosulfate solution. Near the end point, starch indicator was added, and the solution was titrated while stirring well until the light purple color disappeared. The amount of halogen consumed per 100g of sample was calculated as the number of grams of iodine.

[0123] <Intrinsic viscosity> The intrinsic viscosity [η] was measured using a fully automatic intrinsic viscometer manufactured by Rigo Co., Ltd. at a temperature of 135° C. and in decalin as a measurement solvent.

[0124] <Mooney viscosity> The Mooney viscosity ML(1+4)100°C was measured at 100°C using a Mooney viscometer "SMV-202" (manufactured by Shimadzu Corporation) in accordance with JIS K6300 (1994).

[0125] <Weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) of ethylene copolymers (S1) and (S2)> The weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) are values ​​calculated in terms of polystyrene measured by gel permeation chromatography (GPC). The measuring device and conditions are as follows. The molecular weight was calculated based on a conversion method using a calibration curve prepared using commercially available monodisperse polystyrene.

[0126] The Mw, Mn, and Mw / Mn (molecular weight distribution) were determined using a gel permeation chromatograph HLC-8321 GPC / HT type (manufactured by Tosoh Corporation). The main measurement conditions were as follows: Detector: Differential refractometer Column: TSKgel GMH6-HT x 2 + TSKgel GMH6-HTL x 1 (Each piece has an inner diameter of 7.8 mm and a length of 300 mm) Temperature: 140℃ Mobile phase: o-dichlorobenzene (containing 0.025% BHT) Injection volume: 400 μL Sample concentration: ca 0.15% (w / v) Sample filtration: Filtration through a sintered filter with a pore size of 1.0 μm Column calibration: Monodisperse polystyrene (Tosoh Corporation) Molecular weight conversion: EPR conversion / calibration method taking viscosity into account A universal calibration curve of a third-order polynomial was created by measuring 16 monodisperse standard polystyrenes (molecular weights: 20.6 million to 580) manufactured by Tosoh Corporation. EPR conversion parameters K: 0.000403, α: 0.700 The physical properties of the ethylene-based copolymer (S1-1) and the ethylene-based copolymer (S2-1) were measured by the methods described above. The results are shown in Table 1.

[0127] [Table 1]

[0128] In the examples and comparative examples, the following carbon blacks were used as the carbon black (B). HAF carbon (manufactured by Asahi Carbon Co., Ltd., product name Asahi #70) In the examples, the following liquid polymers were used as the liquid polymer (C).

[0129] As the ethylene / α-olefin copolymer (C1), an ethylene / α-olefin copolymer having Mn=7,900 (manufactured by Mitsui Chemicals, product name LUCANT LX900Z) (C1-1) was used.

[0130] As the liquid polybutadiene (C3), a liquid polybutadiene having Mn=26,000 (manufactured by Kuraray, trade name LBR-305) (C3-1) was used. As the liquid polybutadiene (C3), a liquid polybutadiene having Mn=9,000 (manufactured by Kuraray, trade name LBR-352) (C3-2) was used.

[0131] Example 1 The copolymer composition was prepared in the following manner. [Uncrosslinked Copolymer Composition] A total of 100 parts by mass of 50 parts by mass of the copolymer (S-1-1) obtained in Production Example 1 above and 50 parts by mass of the copolymer (S-2-1) obtained in Production Example 2 above, 5 parts by mass of zinc oxide, 1 part by mass of stearic acid, 1 part by mass of tetrakis[methylene(3,5-di-t-butyl-4-hydroxy)hydrocinnamate]methane (trade name Irganox 1010, manufactured by BASFF Japan Co., Ltd.) as an antiaging agent, 2 parts by mass of 2-mercaptobenzimidazole (trade name Sandant MB, manufactured by Sanshin Chemical Industry Co., Ltd.), 50 parts by mass of carbon black (B), 10 parts by mass of process oil (trade name DIANA Process Oil PW-380) as a softening agent, and 15 parts by mass of the ethylene-α-olefin copolymer (C-1-1) as a liquid polymer (C) were added to a 1.7-liter Banbury mixer and kneaded for 5 minutes.

[0132] Next, this kneaded mixture was wound around a 6-inch roll with a surface temperature of 50°C, and then 2.7 parts by mass of dicumyl peroxide (product name: Percumyl D, manufactured by NOF Corporation) as a peroxide-based crosslinking agent and 4 parts by mass of ethylene glycol dimethacrylate (product name: Sunester EG, manufactured by Sanshin Chemical Industry Co., Ltd.) as a crosslinking aid were added to 174 parts by mass of this mixture, and the mixture was kneaded for 8 minutes. The resulting mixture was allowed to cool, and a copolymer composition (unvulcanized rubber) was obtained. With respect to the obtained copolymer composition before crosslinking (hereinafter also referred to as "unvulcanized rubber"), the physical properties of the unvulcanized rubber were measured by the following methods. The physical properties of the copolymer composition were measured by the following methods.

[0133] [Measurement and evaluation method] The physical properties of the copolymer composition before crosslinking (hereinafter also referred to as "unvulcanized rubber") and its crosslinked product (hereinafter also referred to as "vulcanized rubber") were measured or evaluated by the following methods.

[0134] (1) Mooney Viscosity The Mooney viscosity (ML(1+4)100°C) was measured using a Mooney viscometer (Shimadzu Corporation, SMV202 type) in accordance with JIS K6300 (1994).

[0135] (2) Vulcanization speed (TC90 (min)) Using an uncrosslinked copolymer composition as a sample, the vulcanization rate (TC90) was measured as follows under the measurement conditions of a temperature of 170° C. and a time of 30 minutes using an MDR2000 (manufactured by ALPHA TECHNOLOGIES) as a measuring device.

[0136] The sample was set in the measuring device, and the torque change obtained under the conditions of a constant temperature and a constant shear rate was measured to obtain a vulcanization curve. The minimum torque value S'Min and maximum torque value S'Max were obtained from this vulcanization curve, and the time until the torque reached (S'Max-S'Min) x 0.9 based on the start of the measurement, that is, the time until the torque reached 90% of the difference between the maximum and minimum torque values, was determined as the vulcanization rate (TC90; min).

[0137] [Crosslinked Copolymer Composition (Crosslinked Sheet Properties)] [Vulcanized rubber properties] (1) Hardness test (Duro-A hardness) The unvulcanized rubber was vulcanized at 170°C for 15 minutes using a press molding machine to obtain a crosslinked sheet having a thickness of 2 mm. According to JIS K 6253, the hardness of the sheet (Type A durometer, HA) was measured using six 2 mm crosslinked sheets with smooth surfaces, stacked on the flat parts to a thickness of approximately 12 mm. However, specimens with foreign matter, air bubbles, or scratches were not used. The dimensions of the measurement surface of the specimen were set so that the tip of the indenter could be measured at a position 12 mm or more away from the end of the specimen.

[0138] (2) Tensile test The unvulcanized rubber was vulcanized at 170°C for 15 minutes using a press molding machine to obtain a crosslinked sheet having a thickness of 2 mm. The crosslinked sheet thus obtained was punched out to prepare a No. 3 dumbbell test piece as described in JIS K 6251 (2001). Using this test piece, a tensile test was carried out according to the method specified in JIS K 6251 under the conditions of a measurement temperature of 25°C and a tensile speed of 500 mm / min, and the 100% modulus (M 100 ), 200% modulus (M 200 ), 300% modulus (M 300 ), tensile stress at break (T B ) [MPa] and tensile elongation at break (E B )〔%〕was measured.

[0139] (3) [DIN friction test (amount of wear)] In accordance with JIS-K6264-2:2005, three 2 mm thick crosslinked sheets were stacked to prepare a disk-shaped test piece with a diameter of 16.0±0.2 mm and a thickness of 6 mm. The test piece was then subjected to a DIN abrasion test using a drum with a diameter of 150.0±0.2 mm and a length of 500 mm, which was rotated at 40 revolutions per minute under a load of 1 kgf and an abrasion distance of 40.0±0.2 m. The amount of abrasion (DIN abrasion amount: unit mm 3 ) was measured.

[0140] (4) [Gakushin Wear (friction coefficient)] In accordance with JIS-K6404-16, a crosslinked sheet with a thickness of 2 mm was prepared, and the friction coefficient was measured at a test temperature of 23±2°C, 50±5% RH, test speed of 4200 mm / min, test number of times: 143, test load of 200 gf, stroke of 140 mm, mating material of sandpaper A-60, abrasion element of SUS14 mmφ, and abrasion distance of 40.0±0.4 m. The results are shown in Table 2.

[0141] [Examples 2 to 9, Comparative Examples 1 and 2] A copolymer composition was obtained in the same manner as in Example 1, except that the ingredients and their amounts were changed to those shown in Table 2 instead of the copolymer composition used in Example 1. The physical properties of the obtained copolymer composition were measured by the above-mentioned methods. The results are shown in Table 2.

[0142] [Table 2]

Claims

1. An ethylene / α-olefin / non-conjugated polyene copolymer (S1) (hereinafter referred to as "ethylene-based copolymer (S1)"), which has a limiting viscosity [η] in the range of 2.0 to 4.0 dL / g and has structural units derived from ethylene (A1), an α-olefin (B1) having 3 to 20 carbon atoms, and a non-conjugated polyene (C1) containing in the molecule two or more partial structures selected from the group consisting of the following general formulas (I) and (II), in total, and which satisfies the following requirements (i) to (iv): An ethylene / α-olefin / non-conjugated polyene copolymer (S2) (hereinafter referred to as "ethylene-based copolymer (S2)"), which has structural units derived from ethylene (A2), an α-olefin (B2) having 3 to 20 carbon atoms, and a non-conjugated polyene (C2) containing, in the molecule, a total of two or more partial structures selected from the group consisting of the following general formulas (I) and (II), and which satisfies the following requirements (i) to (iv); 0.1 to 200 parts by mass of carbon black (B) per 100 parts by mass of the total of the ethylene-based copolymer (S1) and the ethylene-based copolymer (S2), and A copolymer composition comprising 0.1 to 100 parts by mass of at least one liquid polymer (C) having an average molecular weight (Mn) of 1,000 to 100,000 selected from an ethylene-α-olefin copolymer (C1), a liquid polyisoprene (C2), and a liquid polybutadiene (C3). [Ethylene / α-olefin / non-conjugated polyene copolymer (S1)] (i) The molar ratio of ethylene / α-olefin is from 40 / 60 to 99.9 / 0.

1. (ii) The weight fraction of the constituent units derived from the non-conjugated polyene (C1) is in the range of 0.07 to 10% by weight based on 100% by weight of the ethylene / α-olefin / non-conjugated polyene copolymer. (iii) The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer (S1), the weight fraction of the constituent unit derived from the non-conjugated polyene (C1) [weight fraction (wt %) of (C1)], and the molecular weight of the non-conjugated polyene (C1) [molecular weight of (C1)] satisfy the following formula (1-1): 4.5≦Mw×weight fraction of (C1) / 100 / [molecular weight of (C1)]≦40 ...Formula (1-1) (iv) The ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, which are obtained by linear viscoelasticity measurement (190° C.) using a rheometer, the intrinsic viscosity [η], and the weight fraction of the constituent unit derived from the non-conjugated polyene (C1) (weight fraction of (C1)) satisfy the following formula (2-1): P / ([η] 2.9 ) ≦ weight fraction of (C1) × 6 ... formula (2-1) [Ethylene / α-olefin / non-conjugated polyene copolymer (S2)] (i) The molar ratio of ethylene / α-olefin is from 40 / 60 to 99.9 / 0.

1. (ii) The weight fraction of the constituent units derived from the non-conjugated polyene (C2) is in the range of 0.07 to 10% by weight based on 100% by weight of the ethylene / α-olefin / non-conjugated polyene copolymer. (iii) The weight average molecular weight (Mw) of the ethylene-α-olefin-non-conjugated polyene copolymer (S2), the weight fraction of the constitutional unit derived from the non-conjugated polyene (C2) [weight fraction (wt%) of (C2)], and the molecular weight of the non-conjugated polyene (C2) [molecular weight of (C2)] satisfy the following formula (1-2). 4.5≦Mw×weight fraction of (C2) / 100 / [molecular weight of (C2)]≦40 ...Formula (1-2) (iv) The ratio P(η*(ω=0.1) / η*(ω=100)) of the complex viscosity η*(ω=0.1) (Pa sec) at a frequency ω=0.1 rad / s to the complex viscosity η*(ω=100) (Pa sec) at a frequency ω=100 rad / s, which are obtained by linear viscoelasticity measurement (190° C.) using a rheometer, the intrinsic viscosity [η], and the weight fraction of the constituent unit derived from the non-conjugated polyene (C2) (weight fraction of (C2)) satisfy the following formula (2-2): P / ([η] 2.9 ) ≦ weight fraction of (C2) × 6 ... formula (2-2) 【Chemistry 1】

2. 2. The copolymer composition according to claim 1, wherein the non-conjugated polyene (C1) and the non-conjugated polyene (C2) are 5-vinyl-2-norbornene (VNB).

3. A conveyor belt comprising the copolymer composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Heat-resisting belt

    JP1999246017A

  • Copolymer composition for conveyor belts and applications thereof

    JP2022147453A