Resin composition, molded product, and damping material

The resin composition of polyurethane and vinyl chloride resin addresses bleed-out issues in damping materials, enhancing performance near room temperature through specific structural components and blending ratios.

JP2024141082AInactive Publication Date: 2024-10-10MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023052537
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing vibration damping materials face issues such as additive bleed-out, weight concerns, and limited performance near room temperature, particularly with PVC and TPU blends.

Method used

A resin composition comprising polyurethane and vinyl chloride resin, with specific structural components and blending ratios, to enhance vibration damping performance while minimizing bleed-out.

Benefits of technology

The composition suppresses stabilizer bleed-out and improves damping performance near room temperature, offering high vibration energy absorption and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141082000001
    Figure 2024141082000001
  • Figure 2024141082000002
    Figure 2024141082000002
  • Figure 2024141082000003
    Figure 2024141082000003
Patent Text Reader

Abstract

To provide a damping material that reduces bleed-out due to a stabilizer contained in PVC, and exhibits high damping performance at approximately room temperature.SOLUTION: A resin composition includes polyurethane and polyvinyl chloride resin, where the polyurethane includes a structure derived from a monomer with an isocyanate structure of formula (1) below. (In formula (1), A represents an alicyclic structure, and L, L' each represent a linking group consisting of a single bond or a divalent hydrocarbon group).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a molded article made of the resin composition, and a vibration damping material including the molded article. [Background technology]

[0002] As the vibration-damping material, a material used for the purpose of absorbing the energy of individual sounds and vibrations is preferred, and examples of the types include rubber-based, plastic-based, and asphalt-based materials. These materials are evaluated using viscoelasticity (tan δ) near the glass transition temperature (Tg) and mechanical impedance methods, and traditionally, halogen-based materials such as chlorinated polyethylene and polyvinyl chloride (PVC) have been used as vibration-damping materials because they are inexpensive and easy to manufacture. However, these halogen-based materials have the problem of additives such as plasticizers and heat stabilizers bleeding out. Asphalt-based materials also have the problem of weight during transportation and installation. Rubber-based materials generally use a method of kneading carbon black, but this has issues with vibration-damping performance, which is the ability to both damp and prevent vibration. Thermoplastic polyurethane (TPU) is also used as a damping material, but TPU has issues with color changes (yellowing) due to ultraviolet rays and the high price range of raw materials. As described above, there are various types of vibration-damping materials, and each material has its own advantages and disadvantages.

[0003] Up to now, vibration-damping materials that are mainly made of a mixture of an organic binder and a filler, the essential components of which are vinyl chloride resin or vinyl chloride copolymer and thermoplastic polyurethane resin, have been known. More specifically, a vibration-damping material that is made of a mixture of polyvinyl chloride (PVC) and thermoplastic polyurethane (TPU) in a ratio of 95:5 to 40:60 has been disclosed (see Patent Document 1). The technology disclosed in Patent Document 1 is a method of blending PVC as the main raw material with TPU. However, the vibration-damping material disclosed in Patent Document 1 had to be mainly composed of vinyl chloride in order to exhibit vibration-damping properties in the normal temperature range. PVC requires the addition of a stabilizer for stabilization, which poses the problem of the stabilizer bleeding out.

[0004] Also, a formulation is known in which a liquid plasticizer, trimellitic acid ester (TOTAE), is blended with TPU to create a polymer alloy of PVC and TPU for use as an automotive interior skin material, thereby controlling bleed-out (see Patent Document 2). However, there is a problem in that the use of a liquid plasticizer limits the possible material properties. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Unexamined Patent Publication No. 61-192753 [Patent Document 2] JP 2006-124509 A Summary of the Invention [Problem to be solved by the invention]

[0006] As mentioned above, although blending TPU and PVC as a vibration-damping material is known, there is a problem of additive bleeding caused by PVC, and a new formulation for obtaining a vibration-damping material with less risk of bleeding is required. Under these circumstances, an object of the present invention is to provide a vibration-damping material which suppresses bleed-out caused by the stabilizers contained in PVC and has high vibration-damping performance at around room temperature. [Means for solving the problem]

[0007] In view of the above circumstances, the present inventors conducted intensive research and found that by blending vinyl chloride with a specific polyurethane, it is possible to impart hardness to the polyurethane alone while increasing the vibration energy absorption property, thereby improving the vibration damping material performance at around room temperature. The present invention was completed based on this finding. That is, the present invention provides the following [1] to

[10] .

[0008] [1] A resin composition comprising a polyurethane and a vinyl chloride resin, the polyurethane comprising a structure derived from a monomer having an isocyanate structure represented by the following formula (1):

[0009] [ka]

[0010] (In formula (1), A represents an alicyclic structure, and L and L' represent a linking group consisting of a single bond or a divalent hydrocarbon group.) [2] The resin composition according to [1] above, wherein the polyurethane has a structure derived from a polycarbonate polyol and / or a polycaprolactone polyol. [3] The resin composition according to the above [1] or [2], wherein the monomer having an isocyanate structure is an isocyanate monomer represented by the following formula (2):

[0011] [ka]

[0012] [4] The resin composition according to any one of the above [1] to [3], which has a peak of dielectric tangent (tan δ) at -20 to 80°C. [5] The resin composition according to the above [4], wherein the dielectric tangent (tan δ) has a single peak at -80 to 150°C. [6] The resin composition according to any one of the above [1] to [5], wherein the polyurethane and the vinyl chloride resin are blended in a mass ratio of 95:5 to 40:60. [7] The resin composition according to any one of the above [1] to [6], wherein the polyurethane has a number average molecular weight of 60,000 to 120,000. [8] The resin composition according to any one of the above [1] to [7], wherein the vinyl chloride has a degree of polymerization of 500 to 1,300. [9] A molded article made of the resin composition according to any one of [1] to [8] above.

[10] A vibration-damping material comprising the molded article described in [9] above. Effect of the Invention

[0013] According to the present invention, it is possible to provide a vibration-damping material which inhibits bleed-out caused by the stabilizer contained in PVC and has high vibration-damping performance at around room temperature. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below, and can be modified as desired without departing from the gist of the present invention.

[0015] [Resin composition] The resin composition of the present invention (hereinafter sometimes referred to as "the present resin composition") is a resin composition containing a polyurethane having a specific structure and a vinyl chloride resin. Since the resin composition can be mainly composed of polyurethane, there is little concern about bleeding out caused by vinyl chloride stabilizers. Note that the main component here refers to the material with the largest content in the resin composition, and is usually 50% by mass or more, preferably 70% by mass or more, and more preferably 80% by mass or more.

[0016] <Polyurethane> The resin composition contains, as a main component, a structure derived from a monomer having an isocyanate structure of the following formula (1): The monomer of the following formula (1) is a polyisocyanate having an alicyclic structure, and is a compound having an alicyclic structure and two isocyanate groups bonded thereto.

[0017] [ka]

[0018] In formula (1), A represents an alicyclic structure, and L and L' represent a linking group consisting of a single bond or a divalent hydrocarbon group. The alicyclic structure represented by A is not particularly limited, but is preferably a cycloalkylene group having 3 to 8 carbon atoms. Examples of polyisocyanates having an alicyclic structure include diisocyanates having an alicyclic structure such as bis(isocyanate methyl)cyclohexane, cyclohexane diisocyanate, bis(isocyanate cyclohexyl)methane, and isophorone diisocyanate. The polyisocyanates having an alicyclic structure have the function of improving the weather resistance of the cured product obtained by curing the resin composition. In addition, since the polyisocyanates have an alicyclic structure and have appropriate rigidity, when blended with vinyl chloride described later, the peak of the dielectric tangent (tan δ) of the resin composition can be easily adjusted to -20 to 80°C, and the effect of exhibiting vibration damping performance at around room temperature can be obtained.

[0019] L and L' each represent a single bond or a linking group made of a divalent hydrocarbon group. The linking group is preferably a linking group made of a divalent hydrocarbon group, and examples thereof include an alkylene group having 1 to 10 carbon atoms and an arylene group having 6 to 12 carbon atoms. More specific examples thereof include a methylene group, an ethylene group, a propylene group, and a phenylene group.

[0020] The isocyanate monomer of the above formula (1) is particularly preferably an isocyanate monomer of the following formula (2): By using this monomer, a polyurethane having excellent weather resistance and heat resistance can be obtained.

[0021] [ka]

[0022] The polyurethane of the present composition preferably has a structure derived from a polycarbonate polyol and / or a polycaprolactone polyol. The polycarbonate polyol and the polycaprolactone polyol react with a monomer having an isocyanate structure of the above formula (1) to form a polyurethane. The polycarbonate polyol and the polycaprolactone polyol may be used alone, or both may be used in combination and reacted with a monomer having an isocyanate structure of the above formula (1) to obtain a polyurethane.

[0023] Polycaprolactone polyols are obtained by ring-opening polymerization of cyclic lactone compounds with low molecular weight polyols. Examples of cyclic lactone compounds include ε-caprolactone, γ-butyrolactone, δ-valerolactone, etc., which can be used alone or in combination. The low molecular weight polyol has a molecular weight of several tens to several hundreds and has two or more hydroxyl groups per molecule. Specifically, the low molecular weight polyol includes ethylene glycol, diethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 2-methyl-1,3-propanediol, 2-methyl-1,4-butanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, 1,10-decanediol, Examples of the monomer include low molecular weight compounds such as neopentyl glycol, 2-ethyl-2-n-butyl-1,3-propanediol, 2-ethyl-2-hexyl-1,3-propanediol, cyclohexanedimethanol, glycerin, trimethylolpropane, 1,2,6-hexanetriol, diglycerin, and pentaerythritol, and oligomers such as alkylene oxide adducts of bisphenol A. These may be used alone or in combination.

[0024] The polycarbonate polyol can be obtained, for example, by reacting at least one carbonate compound selected from the group consisting of alkylene carbonates, diaryl carbonates, and dialkyl carbonates with a diol or polyether polyol. Examples of diols that are raw materials for polycarbonate polyols include ethylene glycol, propylene glycol, 1,4-butanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 1,4-cyclohexanedimethanol, 1,12-dodecanediol, diethylene glycol, dipropylene glycol, polybutadiene diol, etc. Among these, from the viewpoint of abrasion resistance, it is preferable to include at least one selected from 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol.

[0025] Furthermore, the polyurethane compound may be a reaction product of a polyol, a polyisocyanate and a chain extender. The chain extender is a compound having two or more active hydrogens that react with an isocyanate group. Examples of the chain extender include low molecular weight diamine compounds having a number average molecular weight of 500 or less, such as aromatic diamines such as 2,4- or 2,6-tolylenediamine, xylylenediamine, and 4,4'-diphenylmethanediamine; ethylenediamine, 1,2-propylenediamine, 1,6-hexanediamine, 2,2-dimethyl-1,3-propanediamine, 2-methyl-1,5-pentanediamine, 2,2,4- or 2,4,4-trimethylhexanediamine, and 2-butyl- Aliphatic diamines such as 2-ethyl-1,5-pentanediamine, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine; and alicyclic diamines such as 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, 4,4'-dicyclohexylmethanediamine, isopropylidenecyclohexyl-4,4'-diamine, 1,4-diaminocyclohexane, 1,3-bisaminomethylcyclohexane, and tricyclodecanediamine. These may be used alone or in combination of two or more.

[0026] The number average molecular weight of the polyurethane of the present invention is preferably 60,000 to 200,000. A number average molecular weight of 60,000 or more is advantageous in terms of mechanical properties. On the other hand, a number average molecular weight of 200,000 or less is advantageous in terms of processability (fluidity). From the above viewpoints, the number average molecular weight of the polyurethane is more preferably in the range of 70,000 to 180,000, and even more preferably in the range of 80,000 to 160,000. The number average molecular weight of polyurethane is a value calculated in terms of standard polystyrene, measured by gel permeation chromatography (GPC).

[0027] The polyurethane of the present invention can be produced by a known method, which may be prepared by reacting the above-mentioned polyol with a polyisocyanate in the presence of a catalyst. The mixing ratio of the polyol and the polyisocyanate is preferably such that the equivalent ratio of the isocyanate group in the polyisocyanate to the hydroxyl value in the polyol is 0.5 or more and less than 1.0, and more preferably 0.8 or more and less than 1.0. If the ratio is equal to or more than the lower limit, the vibration damping performance can be improved. If the ratio is equal to or less than the upper limit, the moldability can be improved.

[0028] Examples of the catalyst include tin-based catalysts such as dibutyltin laurate, dibutyltin dioctate, dioctyltin dilaurate, and dioctyltin dioctate; and bismuth-based catalysts such as bismuth tris(2-ethylhexanoate). The catalyst may be used alone or in combination of two or more. Among these, dioctyltin dilaurate and bismuth tris(2-ethylhexanoate) are preferred from the viewpoints of environmental adaptability, catalytic activity, storage stability, and the like. The amount of the catalyst used is preferably 2000 ppm or less, more preferably 1000 ppm or less, based on the total content of the raw material compounds. Also, it is preferably 10 ppm or more, more preferably 30 ppm or more.

[0029] When producing polyurethane, organic solvents can be used.The solvent to be used is preferably a solvent that does not have active hydrogen such as hydroxyl group or amino group, and can be ether-based solvents such as methyl cellosolve, cellosolve, butyl cellosolve, methyl carbitol, carbitol, butyl carbitol, diethyl carbitol, propylene glycol monomethyl ether, and tetrahydrofuran; aromatic solvents such as Swazol 1000 (trade name, manufactured by Maruzen Petrochemical Co., Ltd.), Supersol 100 (trade name, manufactured by Nippon Petrochemical Co., Ltd.), and Supersol 150 (trade name, manufactured by Nippon Petrochemical Co., Ltd.), benzene, toluene, and xylene; cyclic hydrocarbon-based solvents such as cyclohexane; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, and cyclohexanone; acetate-based solvents such as ethyl acetate, n-butyl acetate, isobutyl acetate, n-amyl acetate, and propylene glycol acetate. Among these, a solvent composition containing either a ketone-based solvent or an acetate-based solvent is preferred because of its excellent solubility in polyurethane compounds.

[0030] <Vinyl chloride resin> The composition preferably contains a vinyl chloride resin in addition to the polyurethane. By blending the vinyl chloride resin, the polyurethane can be given hardness due to the vinyl chloride, and the vibration energy absorption can be increased. As a result, the vibration damping performance at around room temperature can be improved.

[0031] The type of vinyl chloride resin that can be used in the present invention is not particularly limited, and examples thereof include a homopolymer of vinyl chloride, a chlorinated vinyl chloride polymer, a partially crosslinked vinyl chloride polymer, or a copolymer of vinyl chloride and another vinyl compound that can be copolymerized with vinyl chloride, and a mixture thereof.

[0032] Other vinyl compounds that can be copolymerized with the vinyl chloride are not particularly limited, but specific examples include fatty acid vinyl esters such as vinyl acetate and vinyl propionate; methacrylic acid alkyl esters such as methyl methacrylate and ethyl methacrylate; acrylic acid alkyl esters such as ethyl acrylate and butyl acrylate; α-olefins such as ethylene, propylene, and styrene; alkyl vinyl ethers such as vinyl methyl ether and vinyl butyl ether; and unsaturated carboxylic acids or acid anhydrides such as acrylic acid, methacrylic acid, and maleic anhydride, which may be used alone or in combination of two or more. If the copolymerization amount of the other vinyl compounds that can be copolymerized is 30% by mass or less, it is preferable because the inherent characteristics of the vinyl chloride resin are not impaired. Furthermore, these vinyl chloride resins may be used alone or in combination of two or more.

[0033] The vinyl chloride resin used in the present invention preferably has an average degree of polymerization in the range of 100 to 5000. By making the average degree of polymerization 100 or more, the impact strength becomes good. By making the average degree of polymerization 5000 or less, it is advantageous in terms of moldability. From the above viewpoints, the average polymerization degree of the vinyl chloride resin is more preferably in the range of 200 to 4,000, and further preferably in the range of 300 to 3,000.

[0034] There is no particular limitation on the method for producing the vinyl chloride resin used in the present invention, and those produced by various polymerization methods such as emulsion polymerization, suspension polymerization, and bulk polymerization can be used.

[0035] In addition, since the molding temperature and the thermal decomposition temperature of polyvinyl chloride resin are close to each other, it is necessary to add a heat stabilizer during processing. Specifically, it is possible to mix lead-based, organotin-based, complex metal soap-based, and other heat stabilizers. The heat stabilizer is preferably a complex metal soap type, and a complex metal soap type heat stabilizer containing zinc is particularly preferred. The complex metal soap type heat stabilizer containing zinc is made of a metal soap containing zinc. Examples of metal soaps include a zinc salt of a long-chain fatty acid (Zn-based heat stabilizer) alone, a Ca / Zn complex heat stabilizer, a Ba / Zn complex heat stabilizer, and a Ca / Ba / Zn complex heat stabilizer, each of which contains either or both of a calcium salt of a long-chain fatty acid (Ca-based heat stabilizer) and a barium salt of a long-chain fatty acid (Ba-based heat stabilizer). Among these, a Ca / Zn complex heat stabilizer is preferred because of its excellent thermal stability. Examples of long-chain fatty acids include, but are not limited to, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, lauric acid, myristic acid, pentadecylic acid, palmitic acid, isostearic acid, stearic acid, oleic acid, linoleic acid, ricinoleic acid, octylic acid, arachidic acid, arachidonic acid, behenic acid, lignoceric acid, montanic acid, etc. The heat stabilizers may be used alone or in combination of two or more kinds.

[0036] The heat stabilizer is added in an amount of 1 to 10 parts by mass, preferably 1 to 8 parts by mass, and more preferably 2 to 6 parts by mass, per 100 parts by mass of vinyl chloride resin. By adding 1 part by mass or more, the effect of improving the heat stability of the vinyl chloride resin is more easily obtained. On the other hand, if the amount is 10 parts by mass or less, the vinyl chloride resin is easily melted and kneaded, and the mechanical properties of the molded product are further improved.

[0037] <Chlorinated polyvinyl chloride resin> The chlorinated vinyl chloride resin is a vinyl chloride resin obtained by chlorinating a vinyl chloride resin. In the resin composition of the present invention, it is more preferable to use a chlorinated vinyl chloride resin as the vinyl chloride resin. When a chlorinated vinyl chloride resin is used in the resin composition of the present invention, the dielectric loss tangent (tan δ) described in detail later can be improved. Chlorinated polyvinyl chloride resin has a BET specific surface area of ​​1.3 to 8 m 2 / g. The BET specific surface area is preferably 1.3 m2 / g or more, there are sufficient micropores of 0.1 μm or less inside the vinyl chloride resin particles, so that the chlorination rate in the subsequent steps does not slow down. In addition, there is no deterioration in the processability of the obtained chlorinated vinyl chloride resin due to the poor processability of the vinyl chloride resin particles themselves before chlorination. 2 When the BET specific surface area is 1.5 to 5 m / g or less, the thermal stability of the vinyl chloride resin particles before chlorination is maintained, and the processability of the obtained chlorinated vinyl chloride resin is improved. 2 / g.

[0038] <Polyurethane and vinyl chloride resin blend ratio> In the present resin composition, the blending ratio (mass ratio) of polyurethane to vinyl chloride resin is preferably 95:5 to 40:60. When the blending ratio of vinyl chloride resin is equal to or greater than the lower limit, the polyurethane alone can be given sufficient hardness by vinyl chloride, and the vibration energy absorption can be improved. On the other hand, when the blending ratio of vinyl chloride resin is equal to or less than the upper limit, the amount of vinyl chloride resin used is reduced, and the bleed-out of additives such as stabilizers and plasticizers added to the vinyl chloride resin can be suppressed. In addition, when the content of vinyl chloride resin is high, it is less expensive than polyurethane alone, and is therefore advantageous in terms of cost.

[0039] The resin composition may contain various additives, such as lubricants, fillers, processing aids, and auxiliary stabilizers, as long as the additives do not impair the effects of the present invention.

[0040] Examples of lubricants include pure hydrocarbon-based lubricants such as liquid paraffin, natural paraffin, microwax, synthetic paraffin, and low molecular weight polyethylene; fatty acid-based lubricants such as halogenated hydrocarbon-based lubricants, higher fatty acids, and oxyfatty acids; fatty acid amide-based lubricants such as fatty acid amides and bisfatty acid amides; polyhydric alcohol esters of fatty acids such as lower alcohol esters of fatty acids and glycerides; ester-based lubricants such as polyglycol esters of fatty acids and fatty alcohol esters of fatty acids (ester waxes); metal soaps, fatty alcohols, polyhydric alcohols, polyglycols, polyglycerols, partial esters of fatty acids and polyhydric alcohols, and partial esters of fatty acids and polyglycols or polyglycerols, and these can be used alone or in combination of two or more kinds. The amount of the lubricant to be added is not particularly limited, but is preferably 0.1 to 15 parts by mass, and more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the total amount of the (A) and (B) components. By making the amount 0.1 part by mass or more, adhesion of the resin composition to the molding machine can be reduced, and by making the amount 15 parts by mass or less, a decrease in gelling properties can be prevented.

[0041] Examples of fillers include metal powders, oxides, hydroxides, silicic acid and silicates, carbonates, silicon carbide, vegetable fibers, animal fibers, and synthetic fibers, and specific representative examples thereof include aluminum powder, copper powder, iron powder, alumina, natural wood, paper, calcium carbonate, talc, glass fibers, magnesium carbonate, mica, kaolin, calcium sulfate, barium sulfate, aluminum hydroxide, magnesium hydroxide, silica, clay, zeolite, acetate powder, silk powder, aramid fibers, azodicarbonamide, graphite, and recycled filler materials. These can be used alone or in combination of two or more.

[0042] When a filler is added to improve flame retardancy, for example, a metal hydroxide, a bromine-based compound, a triazine ring-containing compound, a zinc compound, a phosphorus-based compound, a halogen-based compound, a silicon-based compound, an intumescent compound, or antimony oxide can be used. These can be used alone or in combination of two or more. The amount of the filler to be added is not particularly limited, but is preferably 0 to 300 parts by mass, more preferably 0 to 100 parts by mass, further preferably 1 to 50 parts by mass, and particularly preferably 1 to 15 parts by mass, relative to 100 parts by mass of the total amount of the (A) and (B) components. By making the amount 300 parts by mass or less, the smoothness of the appearance of the molded article can be improved. Also, by making the amount 1 part by mass or more, the rigidity can be increased.

[0043] Examples of the processing aid include acrylic processing aids, chlorinated polyethylene, and polytetrafluoroethylene. These may be used alone or in combination of two or more. The amount of the processing aid is not particularly limited, but is preferably 0.1 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and particularly preferably 1 to 4 parts by mass, based on 100 parts by mass of the total amount of the (A) and (B) components. By making the amount 10 parts by mass or less, the load on the molding machine can be reduced. Also, by making the amount 0.1 parts by mass or more, the gloss of the molded product can be increased.

[0044] Examples of the auxiliary stabilizer include epoxy compounds such as epoxy resins and epoxidized fatty acid alkyl esters, and non-metallic stabilizers such as organic phosphites, which may be used alone or in combination of two or more. The amount of the auxiliary stabilizer to be added is not particularly limited, but is preferably 0 to 5 parts by mass, more preferably 1 to 4 parts by mass, based on 100 parts by mass of the total amount of the (A) and (B) components. By making the amount 5 parts by mass or less, deterioration in the appearance of the molded product can be suppressed. In addition, by making the amount 1 part by mass or more, the thermal stability during molding can be further improved.

[0045] In addition, a release agent, a flow improver, a colorant, an antistatic agent, a surfactant, an antifogging agent, an antibacterial agent, a plasticizer, a foaming agent, and the like can be arbitrarily blended depending on the purpose, so long as the effect of the present invention is not impaired.

[0046] <Dielectric tangent> The resin composition of the present invention preferably has a peak of dielectric tangent (tan δ) at -20 to 80°C. When the dielectric tangent is in this temperature range, the peak temperature of tan δ is close to room temperature, and therefore the vibration damping performance at room temperature is improved. From the above viewpoint, it is more preferable that the peak temperature of tan δ is in the range of -13°C to 60°C. Moreover, the resin composition of the present invention preferably has a single peak of the dielectric tangent (tan δ) at −80 to 150° C. The fact that the peak is single indicates that the polyurethane and the vinyl chloride resin are compatible with each other or are in a good dispersion state.

[0047] <Explanation of terms> In the present invention, the term "film" also includes the term "sheet", and the term "sheet" also includes the term "film". Furthermore, when the term "panel" is used, such as an image display panel or a protective panel, it encompasses a plate, a sheet, and a film. In the present invention, when it is described as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as the meaning of "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified. EXAMPLES

[0048] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. The evaluation methods in the examples and comparative examples are as follows.

[0049] [Evaluation method] Using the films obtained in the Examples and Comparative Examples, strip-shaped sample pieces cut to MD 4 mm and TD 30 mm were used to perform dynamic viscoelasticity measurements at -100 to 200°C and a frequency of 10 Hz, and the storage modulus (E'), loss modulus (E''), and tan δ (=E'' / E'), which is the ratio of storage modulus (E') to loss modulus (E''), were calculated. The temperatures at which the peak of tan δ (=E'' / E') appears are shown in Table 1.

[0050] Examples 1 to 3 The thermoplastic polyurethane used was TPU (Mitsui Chemicals Fortimo XCT-A1095, molecular weight: 121,000), and the polyvinyl chloride resin used was PVC (Kaneka S1003, degree of polymerization 1300) containing metal soap stabilizers (Ca stearate and Zn stearate). As shown in Table 1, TPU and PVC were blended in a ratio of 9:1 to 7:3, melt-kneaded at 190 to 210°C, and heat-pressed at a pressure of 3 MPa for 30 seconds to produce an unstretched film with a thickness of 100 μm. The evaluation results are shown in Table 1.

[0051] Examples 4 to 6 A film was produced in the same manner as in Examples 1 to 3, except that TPU (Mitsui Chemicals Fortimo XCT-P1095) was used as the thermoplastic polyurethane. The evaluation results are shown in Table 1.

[0052] Examples 7 and 8 A film was produced in the same manner as in Examples 1 and 3, except that a chlorinated polyvinyl chloride resin (C-PVC, Sekisui Chemical HA-05K, polymerization degree 500, chlorination rate 67%) was used as the polyvinyl chloride resin. The evaluation results are shown in Table 1.

[0053] Comparative Examples 1 and 2 As shown in Table 1, a film was produced in the same manner as in the Examples using only thermoplastic polyurethane without using any vinyl chloride resin. The evaluation results are shown in Table 1.

[0054] [Table 1]

[0055] From the results in Table 1, by adding vinyl chloride resin to polyurethane, the peak temperature of tan δ can be shifted to the higher temperature side, closer to room temperature. In other words, it became clear that blending vinyl chloride into polyurethane, the main component, can increase the vibration energy absorption and improve the vibration damping material performance around room temperature. [Industrial Applicability]

[0056] According to the present invention, it is possible to provide a vibration-damping material that can suppress the bleed-out caused by the stabilizer contained in PVC and improve the vibration-damping performance at around room temperature. This material with high vibration-damping performance can be used in a wide range of applications, and is of great industrial value.

Claims

1. A resin composition comprising a polyurethane and a vinyl chloride resin, the polyurethane comprising a structure derived from a monomer having an isocyanate structure represented by the following formula (1): 【Chemistry 1】 (In formula (1), A represents an alicyclic structure, and L and L′ represent a linking group consisting of a single bond or a divalent hydrocarbon group.)

2. The resin composition according to claim 1 , wherein the polyurethane has a structure derived from a polycarbonate polyol and / or a polycaprolactone polyol.

3. The resin composition according to claim 1 , wherein the monomer having an isocyanate structure is an isocyanate monomer represented by the following formula (2): 【Chemistry 2】

4. The resin composition according to claim 1, having a peak of dielectric tangent (tan δ) at -20 to 80°C.

5. The resin composition according to claim 4, wherein the dielectric tangent (tan δ) has a single peak at -80 to 150 ° C.

6. The resin composition according to claim 1, wherein the polyurethane and the vinyl chloride resin are blended in a mass ratio of 95:5 to 40:

60.

7. The resin composition according to claim 1, wherein the polyurethane has a number average molecular weight of 60,000 to 120,000.

8. The resin composition according to claim 1, wherein the degree of polymerization of the vinyl chloride is 500 to 1,300.

9. A molded article made of the resin composition according to any one of claims 1 to 8.

10. A vibration damping material comprising the molded article according to claim 9.

Citation Information

Patent Citations

  • Vibration damper composed of vinyl chloride resin

    JP1986192753A

  • Upholstery material for automobile interior

    JP2006124509A

Cited By

  • Efficient composite damping material and preparation method and injection molding method thereof

    CN120518994A