Cross-linking reaction simulation apparatus
The crosslinking reaction simulation device addresses the challenge of estimating temperature history in polymers by using carbon black mass ratio to determine thermal diffusivity, improving prediction accuracy of reaction rates and product properties.
Patent Information
- Application Number
- JP2023052539
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing methods struggle to accurately estimate the temperature history of polymers during crosslinking reactions due to variations in shape and filler composition, which affect heat conduction, making it difficult to predict the reaction rate and properties of the final product.
A crosslinking reaction simulation device that includes a storage unit for data, a heat transfer analysis section, and a crosslinking reaction analysis section to determine polymer thermal diffusivity based on the mass ratio of carbon black, allowing for precise estimation of temperature history and reaction rates.
The device accurately predicts the temperature and reaction rates of polymers during crosslinking, enhancing the precision of predicting the final product's properties and reducing the likelihood of internal bubbles.
Smart Images

Figure 2024141084000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a crosslinking reaction simulation device. [Background technology]
[0002] Conventionally, the physical properties of chemical substances have been improved by crosslinking polymers. An example of such a polymer is rubber. Rubber is made by adding sulfur or other crosslinking agents, vulcanization accelerators, etc. to raw rubber and then heating it, forming a three-dimensional network-like crosslinked structure between or within the rubber molecular chains.
[0003] A technique for estimating the degree of vulcanization of rubber, i.e., the reaction rate of the crosslinking reaction of rubber, is described in Non-Patent Document 1. The above technique estimates the degree of vulcanization from the temperature history of rubber based on the Arrhenius equation, and estimates appropriate vulcanization conditions (mold temperature, vulcanization time). [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Toshio Arimatsu, "Practical aspects of vulcanization process design", Journal of the Society of Rubber Industry of Japan, Vol. 59, No. 3, (1986) Summary of the Invention [Problem to be solved by the invention]
[0005] When using the above-mentioned technique, it is preferable to estimate the temperature history of the polymer during the crosslinking reaction as accurately as possible. However, it has been difficult to estimate the temperature history of the polymer during the crosslinking reaction. This will be explained below.
[0006] For example, when a crosslinking reaction is carried out with a polymer placed in a mold, the local temperature of the mold can be controlled and measured. However, the heat conduction from the mold to the polymer, and furthermore, the heat conduction inside the polymer, is affected by the shape of the polymer and the composition of the filler contained in the polymer. Therefore, the temperature history of the rubber differs for each product when the shapes of the products are different. Furthermore, even if the products have the same shape, the temperature history differs for each product with a different composition when the filler composition is different. In particular, when the thermal diffusivity of the polymer and the thermal diffusivity of the filler are different, it is very difficult to estimate the temperature history of the polymer.
[0007] The present invention has been made in view of the above background, and aims to provide a crosslinking reaction simulator capable of accurately estimating the temperature history of a polymer during a crosslinking reaction. [Means for solving the problem]
[0008] One aspect of the present invention is A storage unit that stores data used in the simulation; a heat transfer analysis unit that performs a heat transfer analysis during a cross-linking reaction of a polymer part of a target workpiece model; A crosslinking reaction simulation device comprising: The storage unit is A molded model; A target work model having the polymer portion including a raw material polymer and carbon black; a thermal diffusivity characteristic representing a relationship between a mass ratio of the carbon black to the raw polymer and a thermal diffusivity of the polymer portion; The heat transfer analysis unit is a condition input unit for inputting a mass ratio of the carbon black to the raw material polymer in the target workpiece model and a temperature condition of the mold model; a polymer thermal diffusivity determination unit that determines a polymer thermal diffusivity, which is the thermal diffusivity of the polymer portion of the target workpiece model, based on the mass ratio input by the condition input unit and the thermal diffusivity characteristics stored in the storage unit; The crosslinking reaction simulation device includes an analysis unit that performs heat transfer analysis using the polymer thermal diffusivity determined by the polymer thermal diffusivity determination unit and the temperature conditions stored in the memory unit while the target work model is placed on the mold model. Effect of the Invention
[0009] Since carbon black is more conductive to heat than the polymer portion, the mass ratio of carbon black has a large effect on the thermal diffusivity of the polymer portion. According to one aspect of the present invention, the polymer thermal diffusivity, which is the thermal diffusivity of the polymer portion of the target workpiece model, can be determined based on the mass ratio of carbon black to the raw material polymer. As a result, the temperature history of the polymer during the crosslinking reaction can be accurately estimated. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a block diagram showing a crosslinking reaction simulation device according to a first embodiment. [Diagram 2] FIG. 4 is a diagram showing a state in which a target workpiece model is placed on a molding die model in the first embodiment. [Diagram 3] FIG. 2 is a diagram showing a target workpiece model according to the first embodiment. [Figure 4] 4 is a flowchart showing the operation of the crosslinking reaction simulator of the first embodiment. [Diagram 5] FIG. 4 is a diagram showing changes in temperature over time at various parts when a target workpiece model is placed on a molding die model in the first embodiment. [Figure 6] 1 is a graph showing actual measured values and predicted values of the temperature of a polymer portion in the prior art. [Figure 7] 4 is a graph showing actual measured values and predicted values of the temperature of a polymer portion in the first embodiment. [Figure 8] 4 is a graph showing the change in thermal conductivity versus the carbon black content in the first embodiment. [Figure 9]FIG. 4 is a diagram for explaining the state of an analysis mesh in a state in which a target workpiece model is placed on a forming die model in the first embodiment. [Figure 10] FIG. 1 is a schematic diagram showing a structure of a vulcanization tester according to a first embodiment. [Figure 11] 1A and 1B are diagrams for explaining a method of converting the torque measured by the vulcanization tester of embodiment 1 into a reaction rate, in which (a) is a graph showing a change in torque versus reaction time, and (b) is a graph showing a change in reaction rate versus reaction time. [Figure 12] FIG. 4 is a diagram for explaining a method of calculating a gradient coefficient in the crosslinking reaction analysis process according to the first embodiment. [Figure 13] FIG. 4 is a diagram for explaining a method for calculating an equivalent reaction amount in the crosslinking reaction analysis process according to the first embodiment. [Figure 14] FIG. 4 is a diagram for explaining a method for calculating an equivalent reaction amount from an equivalent reaction amount increase amount in the crosslinking reaction analysis process of the first embodiment. [Figure 15] FIG. 4 is a diagram for explaining a method of converting an equivalent reaction amount into a reaction rate in the crosslinking reaction analysis process according to the first embodiment. [Figure 16] FIG. 1 is a diagram showing the actual measured values and the predicted values of the reaction rate of the polymer portion in the conventional technology. [Figure 17] FIG. 1 is a diagram for explaining a method for dividing the crosslinking reaction into sections according to the progress of the reaction and calculating the activation energy for each section in the first embodiment. [Figure 18] FIG. 4 is a graph showing the actual measured values and the predicted values of the reaction rate of the polymer portion in the first embodiment. [Figure 19] FIG. 2 is a diagram for explaining a method of expressing the amount of change in reaction rate with respect to reaction time in the first embodiment. [Figure 20] FIG. 4 is a graph showing the change in reaction rate versus reaction time in the first embodiment. [Figure 21] FIG. 4 is a diagram showing a second function according to the first embodiment. [Figure 22] FIG. 4 is a diagram for explaining the state of an analysis mesh of a target workpiece model in the first embodiment. [Figure 23] FIG. 13 is a diagram showing a state in which internal bubbles have occurred in a polymer portion. [Figure 24] FIG. 2 is a graph showing the reaction rate at the blow point, the reaction rate at demolding, and the final reaction rate in a crosslinking reaction. [Diagram 25] Graph (a) showing the reaction rate at the blow point of a number of samples, and graph (b) showing the torque measured by a curing tester at the blow point of a number of samples. [Figure 26] FIG. 2 is a diagram for explaining the mechanism for suppressing internal bubbles. [Figure 27] FIG. 3 is a heat map showing the reaction rate distribution of a polymer portion in the first embodiment. [Figure 28] FIG. 11 is a diagram showing the change in elastic modulus in the axis-perpendicular direction of a target workpiece model versus reaction time when the mold temperature is low in embodiment 1. [Figure 29] FIG. 11 is a graph showing the change in elastic modulus in the axis-perpendicular direction of a target workpiece model versus reaction time when the mold temperature is medium in embodiment 1. [Diagram 30] FIG. 11 is a diagram showing the change in elastic modulus in the axis-perpendicular direction of a target workpiece model versus reaction time when the mold temperature is high in embodiment 1. [Diagram 31] FIG. 4 is a graph showing changes in elastic modulus of a polymer portion and generation of internal bubbles with respect to reaction time in the first embodiment. [Diagram 32] FIG. 4 is a diagram visually displaying the predicted results of internal bubble generation in the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] (Embodiment 1) 1. Configuration of crosslinking reaction simulation device 1 1-1. Overall configuration of crosslinking reaction simulation device 1 The overall configuration of a crosslinking reaction simulator 1 of the first embodiment will be described with reference to Fig. 1. The crosslinking reaction simulator 1 of this embodiment performs a simulation of a crosslinking reaction that crosslinks molecular chains of a raw material polymer.
[0012] The raw polymer is not particularly limited as long as the molecular chains can undergo crosslinking reaction, and any polymer can be appropriately selected, such as thermosetting resins such as phenolic resins, epoxy resins, melamine resins, urea resins, unsaturated polyester resins, alkyd resins, silicone resins, and polyurethanes, thermoplastic resins such as crosslinked polyethylene and crosslinked polypropylene, and synthetic rubbers such as natural rubber, styrene-butadiene rubber, butadiene rubber, and isoprene rubber. In this embodiment, rubbers including natural rubber and synthetic rubber are used as polymers. In the case of rubber, when heated with a crosslinking agent such as sulfur added, the molecular chains that make up the rubber are crosslinked, causing a so-called vulcanization reaction.
[0013] As shown in FIG. 1, the crosslinking reaction simulation device 1 includes a storage unit 2, a heat transfer analysis unit 3, a crosslinking reaction analysis unit 4, a structure analysis unit 5, an internal bubble estimation unit 6, and a display unit .
[0014] 1-2. Configuration of storage unit 2 The storage unit 2 stores data used in the simulation. The data includes the mold model MM, the target workpiece model WM, heat transfer analysis data TD used by the heat transfer analysis unit 3, crosslinking reaction analysis data RD used by the crosslinking reaction analysis unit 4, and internal bubble estimation data BD used by the internal bubble estimation unit 6.
[0015] The molding die model MM will be described with reference to FIG. 2. As shown in FIG. 2, the molding die model MM includes a die 10 and a hot plate 11 attached to the die 10. The die 10 includes a lower die 10A located on the lower side and an upper die 10B attached to the lower die 10A from above. The hot plate 11 includes a lower hot plate 11A attached to the lower surface of the lower die 10A and an upper hot plate 11B attached to the upper surface of the upper die 10B. The lower die 10A is formed with a lower cavity 100A that opens upward. The upper die 10B is formed with an upper cavity 100B that opens downward. With the lower die 10A and the upper die 10B assembled, a target work model WM is placed in the space formed by the lower cavity 100A and the upper cavity 100B.
[0016] The target workpiece model WM will be described with reference to FIG. 3. As shown in FIG. 3, the target workpiece model WM includes a polymer portion 12. The polymer portion 12 includes a raw polymer. Furthermore, the polymer portion 12 may include additives such as antioxidants, carbon black, and the like. The polymer portion 12 of this embodiment includes a raw polymer and carbon black. The raw polymer is not particularly limited, and any material such as rubber or thermosetting resin can be appropriately selected. In this embodiment, the raw polymer is made of rubber. The polymer portion 12 of this embodiment is a rubber portion configured to exhibit vibration-proof performance, and the target workpiece model WM is a model of a vibration-proof rubber device. However, the polymer portion 12 may be configured to include a thermosetting resin as a raw polymer, or may not include carbon black.
[0017] The polymer part 12 in this embodiment is formed in a tubular shape along an axis A extending in the vertical direction. An outer joint member 13 (one example of a joint member) formed in a cylindrical shape extending in the vertical direction is disposed on the outer periphery of the polymer part 12. The outer joint member 13 is made of metal, resin, or a composite of metal and resin. The outer joint member 13 in this embodiment is made of metal and is joined to the outer periphery of the polymer part 12. An inner joint member 14 (one example of a joint member) formed in a cylindrical shape extending in the vertical direction is disposed on the inner periphery of the polymer part 12. The inner joint member 14 is made of metal, resin, or a composite of metal and resin. The inner joint member 14 in this embodiment is made of metal and is joined to the inner periphery of the polymer part 12. The vertical length dimension of the inner joint member 14 is formed to be larger than the vertical length dimension of the outer joint member 13. The upper surface and the lower surface of the polymer part 12 are formed in a concave shape. However, the shape of the polymer part 12 is not limited to the above shape. Moreover, the target workpiece model WM may be configured without both or either of the outer joint member 13 and the inner joint member 14.
[0018] Returning to FIG. 2, with the target workpiece model WM placed on the forming die model MM, gaps 15 are formed between the forming die model MM and the outer joint member 13 and between the forming die model MM and the inner joint member 14, respectively.
[0019] Returning to Figure 1, the heat transfer analysis data TD includes a thermal diffusivity characteristic TS indicating the relationship between the mass ratio of carbon black to the raw polymer and the thermal diffusivity of the polymer part 12, a contact heat transfer coefficient CH which is the heat transfer coefficient between the mold model MM and the outer joining member 13 and the inner joining member 14 when the target work model WM is placed in the mold model MM, an air heat transfer coefficient AC which is the heat transfer coefficient of the air surrounding the target work model WM when the target work model WM is demolded from the mold model MM, a temperature condition TC of the mold model MM input from a condition input unit 30 described later, and an outside air condition OC which includes the air temperature surrounding the demolded target work model WM.
[0020] The crosslinking reaction analysis data RD defines an equivalent reaction amount as the ratio of the reaction amount of the crosslinking reaction at a target reaction temperature and a target reaction time to the reaction amount of the crosslinking reaction at a reference reaction temperature and a reference reaction time, and includes an equivalent reaction amount calculation model EM defined including a slope coefficient representing the slope of the Arrhenius plot, and a slope coefficient SC set according to the progress of the crosslinking reaction of the polymer portion 12. The crosslinking reaction analysis data RD further includes a first relationship data map DM1, a second relationship data map DM2, a first function F1, a second function F2, and a reference reaction curve RC, which will be described later.
[0021] The data BD for estimating internal bubbles includes a crosslinking reaction curve CC that defines the relationship between the elapsed time from the start of the crosslinking reaction and a torque that corresponds to the progress of the crosslinking reaction in the polymer part 12 of the target work model WM and can be measured by a crosslinking reaction characteristic tester using a test target polymer material corresponding to the polymer part 12.
[0022] 1-3. Configuration of heat transfer analysis section 3 The heat transfer analysis unit 3 performs a heat transfer analysis during a crosslinking reaction of the polymer part 12 of the target workpiece model WM. As shown in FIG. 1, the heat transfer analysis unit 3 includes a condition input unit 30, a polymer thermal diffusivity determination unit 31, and an analysis unit 32.
[0023] The mass ratio of carbon black to the raw material polymer in the target workpiece model WM and the temperature condition TC of the mold model MM are inputted into the condition input unit 30. The condition input unit 30 may be an input device such as a keyboard, a mouse, a trackball, or a joystick, or may be an external storage medium such as a semiconductor memory or a hard disk memory.
[0024] The polymer thermal diffusivity determination unit 31 determines the polymer thermal diffusivity, which is the thermal diffusivity of the polymer part 12 of the target work model WM, based on the mass ratio of carbon black input by the condition input unit 30 and the thermal diffusivity characteristic TS stored in the memory unit 2.
[0025] With the target work model WM placed on the molding die model MM, the analysis unit 32 performs heat transfer analysis during the crosslinking reaction of the polymer part 12 of the target work model WM using the polymer thermal diffusivity determined by the polymer thermal diffusivity determination unit 31 and the temperature condition TC stored in the memory unit 2.
[0026] 1-4. Configuration of crosslinking reaction analysis section 4 The crosslinking reaction analysis unit 4 analyzes the reaction rate of the crosslinking reaction of the polymer part 12 using the result of the heat transfer analysis by the heat transfer analysis unit 3. As shown in FIG. 1, the crosslinking reaction analysis unit 4 includes a temperature acquisition unit 40 and a reaction rate calculation processing unit 41.
[0027] The temperature acquisition unit 40 acquires, as a result of the heat transfer analysis by the heat transfer analysis unit 3, the temperature at each time for each element of the polymer part 12 of the target workpiece model WM in the crosslinking reaction.
[0028] The reaction rate calculation processing unit 41 calculates the equivalent reaction amount of the polymer part 12 for each time based on the temperature for each element of the polymer part 12 in the acquired crosslinking reaction for each time, the equivalent reaction amount calculation model EM, and the slope coefficient SC according to the progress of the crosslinking reaction at the target time, and calculates the reaction rate of the crosslinking reaction of the polymer part 12 based on the calculated equivalent reaction amount.
[0029] 1-5. Configuration of structural analysis section 5 The structure analysis unit 5 performs structure analysis using the reaction rate of the crosslinking reaction of the polymer portion 12 analyzed by the crosslinking reaction analysis unit 4. As shown in Fig. 1, the structure analysis unit 5 includes a temperature acquisition unit 50, a reaction rate acquisition unit 51, an elastic modulus assignment unit 52, and a characteristic acquisition unit 53. However, the temperature acquisition unit 50 may be omitted.
[0030] The temperature acquisition unit 50 acquires, as a result of the heat transfer analysis by the heat transfer analysis unit 3, the temperature at each time for each element of the polymer part 12 of the target workpiece model WM in the crosslinking reaction.
[0031] The reaction rate acquisition unit 51 acquires the reaction rate of each element of the polymer portion 12 calculated by the reaction rate calculation processing unit 41 of the crosslinking reaction analysis unit 4.
[0032] The elastic modulus allocating unit 52 allocates an elastic modulus to the polymer portion 12 according to the obtained reaction rate.
[0033] The characteristic acquisition unit 53 acquires the characteristics of the target workpiece model WM by performing a structural analysis with the elastic modulus assigned to the polymer portion 12.
[0034] 1-6. Configuration of internal bubble estimation unit 6 The internal bubble estimation unit 6 is applied to a crosslinking reaction process in which the polymer part 12 of the target work model WM is crosslinked in the mold model MM and then the mold model MM is demolded, and estimates the generation of internal bubbles inside the polymer part 12 of the target work model WM that accompanies the demolding of the mold model MM. As shown in FIG. 1, the internal bubble estimation unit 6 includes a reaction rate acquisition unit 60, a torque calculation unit 61, and an estimation unit 62.
[0035] The reaction rate acquisition unit 60 acquires the reaction rate of the cross-linking reaction of the polymer portion 12 of the target workpiece model WM. The reaction rate is the reaction rate at the time when the mold 10 is opened, that is, at the time when the mold clamping pressure is released. When the polymer portion 12 is rubber, the reaction rate is also called the degree of vulcanization at the time of demolding.
[0036] The torque calculation unit 61 calculates the torque (also called demolding torque) corresponding to the acquired reaction rate based on the reaction rate (demolding reaction rate) acquired by the reaction rate acquisition unit 60 and the crosslinking reaction curve CC stored in the memory unit 2.
[0037] The estimation unit 62 compares the torque (torque at demolding) calculated by the torque calculation unit 61 with the blow point torque (described in detail later) calculated from the blow point vulcanization degree (described in detail later) in the polymer portion 12, and estimates whether or not air bubbles will be generated inside the polymer portion 12.
[0038] 1-7. Configuration of display unit 7 The display unit 7 displays a value obtained from the reaction rate according to the reaction time, based on the analysis results of the crosslinking reaction analysis unit 4. Furthermore, the display unit 7 displays characteristics according to the temperature of the mold model MM used in the crosslinking reaction of the polymer part 12 and the in-mold reaction time from the start of the crosslinking reaction to the demolding of the mold model MM, based on the results of the structure analysis of the structure analysis unit 5.
[0039] The display unit 7 also displays the presence or absence of internal bubbles depending on the temperature of the mold model MM and the in-mold reaction time from the start of the crosslinking reaction to the demolding of the mold model MM, based on the estimation results of the internal bubble estimation unit 6. The display unit 7 also displays a value obtained from a reaction rate depending on the temperature of the mold model MM and the in-mold reaction time from the start of the crosslinking reaction to the demolding of the mold model MM, based on the analysis results of the crosslinking reaction analysis unit 4, in accordance with the presence or absence of internal bubbles. The display unit 7 also displays a characteristic depending on the temperature of the mold model MM and the in-mold reaction time from the start of the crosslinking reaction to the demolding of the mold model MM, in accordance with the presence or absence of internal bubbles, based on the results of the structure analysis of the structure analysis unit 5.
[0040] 2. Overall Operation of the Crosslinking Reaction Simulation Device 1 The overall operation of the crosslinking reaction simulation device 1 according to the present embodiment will be described with reference to Fig. 4. However, the following description is an example of the operation of the crosslinking reaction simulation device 1, and the operation of the crosslinking reaction simulation device 1 is not limited to the following description.
[0041] When the crosslinking reaction simulation device 1 is started, a heat transfer analysis process S1 is executed. The heat transfer analysis process S1 obtains the temperature at each time for each element of the polymer part 12 of the target workpiece model WM in the crosslinking reaction. The details will be described later.
[0042] Next, a crosslinking reaction analysis process S2 is executed. In the crosslinking reaction analysis process S2, the equivalent reaction amount of the polymer part 12 at each time is calculated based on the temperature at each time for each element of the polymer part 12 of the target workpiece model WM in the crosslinking reaction obtained as a result of the heat transfer analysis, the equivalent reaction amount calculation model EM, and the slope coefficient SC according to the progress of the crosslinking reaction at the target time, and the reaction rate of the crosslinking reaction of the polymer part 12 is calculated based on the calculated equivalent reaction amount. Details will be described later.
[0043] Next, a structural analysis process S3 is executed. In the structural analysis process S3, an elastic modulus is assigned according to the reaction rate of each element of the polymer portion 12 calculated by the crosslinking reaction analysis unit 4, and a structural analysis is performed in a state in which the elastic modulus is assigned to the polymer portion 12, thereby acquiring the characteristics of the target work model WM. Details will be described later.
[0044] Next, an internal bubble estimation process S4 is executed. In the internal bubble estimation process S4, a torque corresponding to the reaction rate of the polymer portion 12 is calculated based on the reaction rate of the polymer portion 12 calculated by the crosslinking reaction analysis process and the crosslinking reaction curve CC stored in the storage unit 2, and the generation of internal bubbles inside the polymer portion 12 of the target workpiece model WM is estimated based on the torque at the time of demolding. Details will be described later.
[0045] Next, the display process S5 is executed. In the display process S5, the presence or absence of internal bubbles is displayed according to the temperature of the mold model MM and the in-mold reaction time from the start of the crosslinking reaction to the demolding of the mold model MM, based on the estimation result by the internal bubble estimation unit 6. In addition, based on the analysis result by the crosslinking reaction analysis unit 4, a value obtained from the reaction rate according to the temperature of the mold model MM and the in-mold reaction time from the start of the crosslinking reaction to the demolding of the mold model MM is displayed in accordance with the presence or absence of internal bubbles. In addition, based on the result of the structure analysis by the structure analysis unit 5, a characteristic according to the temperature of the mold model MM and the in-mold reaction time from the start of the crosslinking reaction to the demolding of the mold model MM is displayed in accordance with the presence or absence of internal bubbles.
[0046] When the display process S5 ends, the operation of the crosslinking reaction simulator 1 ends.
[0047] 3.Heat transfer analysis processing S1 3-1. Carbon black mass ratio Next, the details of the heat transfer analysis process S1 will be described with reference to Fig. 2 and Figs. 5 to 8. As shown in Fig. 2, in a state where the lower mold 10A and the upper mold 10B are combined, an outer joining member 13 and an inner joining member 14 are placed in a space formed by the lower cavity 100A and the upper cavity 100B. Furthermore, a raw material polymer is injected into the space formed by the lower cavity 100A and the upper cavity 100B. Thereafter, in the mold 10, a cross-linking reaction of molecular chains constituting the polymer portion 12 progresses.
[0048] As shown in FIG. 5, the temperature of the hot plate 11 is set to a constant value. The temperature of the mold 10 is set to the same temperature as the hot plate 11. The temperature of the polymer portion 12 during injection is lower than the set temperature of the mold 10. Therefore, the temperature of the mold 10 temporarily drops after the raw polymer is injected. The temperature of the mold 10 then rises and becomes the same as the temperature of the hot plate 11. The temperature of the polymer portion 12 rises after being injected into the mold 10, and becomes the same as the temperature of the mold 10 after a sufficient amount of time has passed. The temperature of the inner joining member 14 and the outer joining member 13 may be the same as the outside air temperature before being placed in the mold 10, or may be preheated. When the temperature is the same as the outside air temperature, it may drop to about 0°C in winter, for example. When preheated, the temperature may be raised to any temperature, for example, to around 100°C. After the inner bonding member 14 and the outer bonding member 13 are placed in the mold 10, the temperatures of the inner bonding member 14 and the outer bonding member 13 rise due to thermal conduction from the mold 10, and after the raw polymer is injected, the temperatures rise further and become the same as the temperature of the mold 10 after sufficient time has passed.
[0049] As shown in Fig. 5, it takes a certain amount of time for the temperature of the polymer part 12 to reach the temperatures of the hot plate 11 and the mold 10 and reach an equilibrium state. The following equation (1) is used to calculate the unsteady process until the equilibrium state is reached. Equation (1) is a so-called unsteady heat conduction equation.
[0050]
number
[0051] The thermal diffusivity α is expressed by the following formula (2).
[0052]
number
[0053] The thermal diffusivity α and the thermal conductivity λ correspond to the thermal diffusivity characteristic TS. However, the thermal diffusivity characteristic TS is not limited to the thermal diffusivity α and the thermal conductivity λ.
[0054] When the thermal diffusivity α is known, the thermal diffusivity α can be directly used to calculate the temperature of the polymer portion 12 according to the unsteady heat conduction equation (1). When the thermal diffusivity α is not known, the thermal diffusivity α can be calculated using the thermal conductivity λ, density ρ, and specific heat C from equation (2), and the calculated α can be used to calculate the temperature of the polymer portion 12 according to equation (1).
[0055] However, when using the formula (1) to calculate the temperature of the polymer part 12, if a value described as the thermal diffusivity α of rubber in general JIS or the like is used, or if using the formula (2) and a value described as the thermal conductivity λ in JIS or the like is used, a problem occurs in that the value when the temperature of the polymer part 12 of the target workpiece model WM placed in the mold 10 is actually measured and the value when the temperature of the polymer part 12 is predicted based on the formula (1) do not match with sufficient accuracy, as shown in Fig. 6. As a result of intensive investigation by the inventors, it was found that the cause was that the value of the thermal diffusivity α or thermal conductivity λ of the raw material polymer of the polymer part 12 described in JIS or the like was different from the value of the thermal diffusivity α or thermal conductivity λ of the actual polymer part 12.
[0056] Therefore, the temperature of the polymer part 12 of the target work model WM to be measured was actually measured, and the thermal diffusivity α or thermal conductivity λ of the polymer part 12 was identified, thereby obtaining the thermal diffusivity α or thermal conductivity λ of the polymer part 12 of the target work model WM to be measured.
[0057] Fig. 7 shows the measured temperature of the polymer part 12 of the target workpiece model WM and the temperature calculated using the measured thermal diffusivity α or thermal conductivity λ obtained as described above. It was found that the measured temperature of the polymer part 12 coincided with the predicted temperature with high accuracy.
[0058] However, the thermal diffusivity α or thermal conductivity λ of the polymer part 12 constituting the target workpiece model WM varies depending on the type of raw material polymer of the polymer part 12, the amount or type of additive material added to the raw material polymer, etc. For this reason, it is cumbersome to actually measure the thermal diffusivity α or thermal conductivity λ for all polymer parts 12 with different compositions.
[0059] Therefore, the inventors focused on carbon black among the additive materials added to the polymer portion 12. The rubber constituting the polymer portion 12 is a material that does not easily transmit heat. On the other hand, carbon black is a material that transmits heat easily. For this reason, it is considered that the thermal diffusivity α or thermal conductivity λ of the polymer portion 12 is highly related to the mass ratio of carbon black to the raw material polymer constituting the polymer portion 12. Examples of carbon black include furnace black, acetylene black, and ketjen black.
[0060] Fig. 8 shows the relationship between the mass ratio of carbon black to the raw polymer and the thermal conductivity λ of the polymer portion 12 when experiments were conducted using multiple types of raw polymers and different mass ratios of carbon black. In Fig. 8, the mass ratio of carbon black to the raw polymer is expressed in parts by mass. However, the mass ratio of carbon black to the raw polymer may also be expressed in % by mass.
[0061] As shown in FIG. 8, the thermal conductivity λ of the polymer portion 12 has a linear relationship with the mass ratio of carbon black to the raw polymer. It was also found that the thermal conductivity λ of the polymer portion 12 has a relationship independent of the type of raw polymer. This makes it possible to accurately predict the thermal conductivity λ of the polymer portion 12 based on the blending amount of carbon black, regardless of the type of raw polymer. In addition, since the thermal diffusivity α can be calculated from the thermal conductivity λ using formula (2), it is also possible to accurately predict the thermal diffusivity α.
[0062] 3-2.Contact heat transfer coefficient CH As shown in FIG. 2, when the outer joint member 13 is disposed in the mold 10, an outer gap 15A may be formed between the inner surface of the mold 10 and the outer joint member 13. In this case, heat is transferred from the inner surface of the mold 10 to the outer joint member 13 through the air in the outer gap 15A. In the heat transfer analysis process S1, a state in which the inner surface of the mold 10 and the outer joint member 13 are in contact with each other is assumed, and the surfaces of the mold 10 and the outer joint member 13 that take the outer gap 15A into consideration are selected, and the contact heat transfer coefficient CH is set according to the size of the outer gap 15A. The contact heat transfer coefficient CH is determined by measuring the temperature behavior when the size of the outer gap 15A is changed in an experiment using a test piece, and a value that can reproduce each temperature behavior is obtained by analysis.
[0063] In addition, when the inner joint member 14 is disposed in the mold 10, an inner gap 15B may be formed between the inner surface of the mold 10 and the inner joint member 14. In this case, heat is transferred from the inner surface of the mold 10 to the inner joint member 14 through the air in the inner gap 15B. In the heat transfer analysis process S1, a state in which the inner surface of the mold 10 and the inner joint member 14 are in contact with each other is assumed, and the surfaces of the mold 10 and the inner joint member 14 that take the inner gap 15B into consideration are selected, and the contact heat transfer coefficient CH is set according to the size of the inner gap 15B. The contact heat transfer coefficient CH is determined by measuring the temperature behavior when the size of the inner gap 15B is changed in an experiment using a test piece, and a value that can reproduce each temperature behavior is obtained by analysis.
[0064] As described above, the storage unit 2 stores the contact heat transfer coefficient CH in the gaps 15A, 15B between the forming die model MM and the metal fitting in a state in which the target workpiece model WM is placed on the forming die model MM.
[0065] In the heat transfer analysis process S1, the analysis unit 32 is configured to perform a heat transfer analysis using the polymer thermal diffusivity determined by the polymer thermal diffusivity determination unit 31, and the temperature condition TC and contact heat transfer coefficient CH stored in the storage unit 2, with the target workpiece model WM placed on the mold model MM. This makes it possible to predict the temperature of the polymer part 12 with high accuracy.
[0066] 3-3.Air heat transfer coefficient AC Even after the target work model WM is released from the mold model MM, the temperature of the polymer portion 12 of the target work model WM does not immediately drop, so the cross-linking reaction progresses in the polymer portion 12. Therefore, in this embodiment, in order to predict the temperature of the polymer portion 12 even after the target work model WM is released from the mold model MM, the condition input unit 30 is configured to input the outside air condition OC including the air temperature around the target work model WM released from the mold model MM. Furthermore, the memory unit 2 stores the air heat transfer coefficient AC, which is the heat transfer coefficient of the air around the target work model WM released from the mold model MM.
[0067] The analysis unit 32 of this embodiment performs heat transfer analysis using the polymer thermal diffusivity determined by the polymer thermal diffusivity determination unit 31, the air heat transfer coefficient AC, and the outside air condition OC stored in the storage unit 2, in a state in which the target work model WM is released from the mold model MM after the polymer part 12 of the target work model WM has been subjected to a crosslinking reaction in the mold model MM. This makes it possible to accurately predict the temperature of the polymer part 12 in a state in which the target work model WM has been released from the mold model MM.
[0068] As shown in Fig. 9, an analytical mesh is created for a state in which the target workpiece model WM is placed on the forming mold model MM. The size of the analytical mesh may be determined in advance, or may be input from the condition input unit 30. The analytical mesh is created taking into consideration the characteristics (e.g., symmetry) of the shapes of the forming mold model MM and the target workpiece model WM. An eight-node solid element is used as the mesh type. However, any model may be used for the mesh type, and for example, a four-node solid element may be used.
[0069] By using the analytical mesh, it is possible to predict the temperature at each node of the target workpiece model WM. In other words, it is possible to predict the temperature distribution of the polymer part 12 of the target workpiece model WM. In particular, it is possible to predict the temperature of each node of the polymer part 12 at each time.
[0070] 4. Cross-linking reaction analysis process S2 Next, the crosslinking reaction analysis process S2 will be described. Regarding the crosslinking reaction analysis process S2, first, the reaction rate will be described. Next, the conventional technology will be described, followed by the problems with the conventional technology. After that, the crosslinking reaction analysis process of this embodiment will be described. 4-1. Response rate The reaction rate of the crosslinking reaction is measured as follows. As shown in FIG. 10, the reaction rate of the rubber according to this embodiment is calculated from the relationship between the torque and the reaction time obtained using a vulcanization tester 70 (one example of a crosslinking reaction tester) in accordance with JIS K6300-2. For example, a Curastometer (registered trademark) can be used as the vulcanization tester 70. In addition, when outputting vibration characteristics taking into account the reaction rate (vulcanization degree), the reaction behavior (vulcanization behavior) can be measured under desired vibration conditions using, for example, a rubber processability tester (RPA). The RPA is configured so that the vibration frequency and amplitude can be set in a wide range.
[0071] As shown in Fig. 10, in a vulcanization tester 70, a disk 75 attached to the tip of a rotor 74 is placed between a lower die 72 having a cavity 71 and an upper die 73. The lower die 72 and the upper die 73 can be set to a predetermined temperature. The torsion angle of the rotor 74 can be selected from +3° to -3° or +1° to -1°. A measurement sample 76 is placed between the cavity 71 and the disk 75, and a crosslinking reaction is caused while a rotational torque is applied from the disk 75 at a constant temperature, and the progress of the crosslinking reaction is detected from the change in torque.
[0072] FIG. 11 shows an example of the measurement results. FIG. 11(a) is a graph (crosslinking reaction curve CC) of the change in torque with respect to reaction time at a predetermined reaction temperature. Meanwhile, the reaction rate is defined as 0% reaction rate at the minimum torque and 100% reaction rate at the maximum torque. FIG. 11(b) shows a graph (reference reaction curve RC) showing the change in reaction rate with respect to reaction time at a predetermined reaction temperature. In the case of the rubber according to this embodiment, the reaction rate is called the degree of vulcanization. The degree of vulcanization is defined as the degree of vulcanization when the physical properties (elastic modulus, elongation, tensile strength, hardness, etc.) of the vulcanized rubber are used as indicators. In FIG. 11(a), the region from reaction time 0 to the reaction time showing the minimum torque is a plastic region where the crosslinking reaction of the polymer portion 12 has not yet reacted. For this reason, in FIG. 11(b), the reaction rate in this region is set to 0%.
[0073] 4-2. Calculation method of response rate Next, a method for calculating the reaction rate will be described. In the above-mentioned Non-Patent Document 1, the equivalent reaction amount of the crosslinking reaction is estimated using the formula (4) relating to the equivalent reaction amount obtained by modifying the Arrhenius formula (3). The formula (4) relating to the equivalent reaction amount indicates how many times the reaction amount at the reaction temperature T and reaction time t is larger than the reaction amount at a certain reference temperature T0 and reference time t0. The formula (4) is called the equivalent vulcanization formula in the vulcanization reaction of rubber. By using this equivalent vulcanization formula, the reaction rate in the reaction reversion period described later can be predicted. As will be described in detail later, in this embodiment, it is possible to further improve the prediction accuracy in the reaction reversion period compared to the case where the equivalent vulcanization formula is simply used. In addition, the reaction rate in the reaction reversion period cannot be predicted by the formula (e.g., Kamal's reaction rate formula) used to predict the behavior of the thermosetting reaction of rubber, epoxy, etc. in general analysis software.
[0074]
number
[0075]
number
[0076] The Arrhenius equation (3) can be transformed as follows to derive the equivalent reaction amount equation (4).
[0077] The reaction amount Z of the crosslinking reaction at reaction time t is expressed by formula (5).
[0078]
number
[0079] The reaction amount Z is calculated from the Arrhenius equation (3) and the above equation (5) as shown in the following equation (6).
[0080]
number
[0081] Here, considering the reaction amount Z0 at a certain reference reaction temperature T0 and reaction time t0, Z0 is expressed by the following equation (7).
[0082]
number
[0083] If we take the ratio U of the reaction amount Z at reaction temperature T and reaction time t to the reaction amount Z0 at reaction temperature T0 and reaction time t0, the ratio U is expressed by the following equation (8).
[0084]
number
[0085] Substituting equations (6) and (7) into equation (8), we obtain equation (9) for the ratio U.
[0086]
number
[0087] In equation (9), when t0=1, equation (9) is expressed as equation (4) above.
[0088] When the reaction temperature T changes moment by moment, the equivalent reaction amount increase in a small time period at the target time is calculated based on the temperature at the target time, the above formula (4), and the slope coefficient SC, and the equivalent reaction amount integrated value from the start of the crosslinking reaction to the target time is calculated based on the equivalent reaction amount increase, and the reaction rate at the target time is calculated based on the equivalent reaction amount integrated value from the start of the crosslinking reaction to the target time.
[0089] Based on equation (4), the equivalent reaction increase ΔU i is expressed by the following equation (10).
[0090]
number
[0091] When the reaction temperature T changes from moment to moment, the equivalent reaction amount U can be calculated by accumulating it per unit time as shown in the following equation (11).
[0092]
number
[0093] The above equation (4) is the equation inside Σ in the above equation (11), and corresponds to each equivalent reaction amount to be accumulated.
[0094] In order to calculate the formula (4) or (11), the value of (-E / R) is required. In the prior art, (-E / R) was calculated as follows:
[0095] By taking the natural logarithm of both sides of Arrhenius equation (3), we obtain the following equation (12).
[0096]
number
[0097] For the above reaction amount, the reaction time t γ and the reaction rate k, the following formula (13) is considered to hold: The reaction rate γ can be any value between 0% and 100%, such as 5%, 90%, etc., as appropriate.
[0098]
number
[0099] Taking the natural logarithm of both sides of equation (13), substituting it into equation (12) and transforming the equation gives equation (14).
[0100]
number
[0101] From equation (14), ln(1 / t γ If we plot the time at which the reaction rate reaches α% and each measured temperature with (1 / T) on the vertical axis and (1 / T) on the horizontal axis, we can approximate the line, and it can be seen that the slope of this line is (-E / R) (see Figure 12).
[0102] In an actual reaction, the temperature changes over time as shown in Figure 13. In such a case, the equivalent reaction amount is calculated using formulas (4) and (11) as follows:
[0103] First, the reaction time is divided into predetermined intervals (for example, 1 minute) as shown in Fig. 13. Next, the temperature is read at each predetermined interval.
[0104] Next, the equivalent reaction amount per predetermined interval is calculated using formula (4). The calculation is performed by substituting the predetermined interval Δt into formula (4). The calculation can be simplified by setting the predetermined interval to, for example, Δt = 1.
[0105] Next, ΔU per given interval Δt calculated by equation (4) i A specific calculation method will be described with reference to FIG.
[0106] As shown in Figure 14, the reaction time t i-1 , reaction temperature T i-1 The equivalent reaction amount U i-1 is calculated using equation (4). Similarly, the reaction time t i , reaction temperature T i The equivalent reaction amount U i Calculate.
[0107] Next, U i-1 × Δt and U i × Δt. This gives us the reaction time t i-1 ~t i In this embodiment, Δt = 1 / 2t. Similarly, according to formula (11), the equivalent reaction amount ΔU per given time from t = 1 to t = n is obtained. i By integrating these, the equivalent reaction amount U can be obtained.
[0108] Next, we will explain how to calculate the reaction rate from the equivalent reaction amount U. First, the reaction amount Z at reaction temperature T0 and reaction time t is expressed by formula (5). Next, from formula (5), the reaction amount Z0 at reaction temperature T0 and reaction time t0 is expressed by the following formula (15). Here, since the reaction temperature in formula (5) and formula (15) is the same value T0, each k has the same value from formula (3).
[0109]
number
[0110] By substituting the above equations (5) and (15) into the above equation (8), the reaction rate k is reduced to obtain the following equation (16).
[0111]
number
[0112] In equation (16), if t0=1, equation (16) can be expressed as equation (17) below.
[0113]
number
[0114] 4-3. Issues with response rate calculation methods However, when the reaction rate is estimated based on the above-mentioned method, there is a problem that the difference from the actually measured value is large and sufficient accuracy cannot be obtained.
[0115] The change in reaction rate versus reaction time is shown in Figure 16. When using formula (4), the reference temperature was set to 160°C, so when the reaction temperature was 160°C, the measured values and predicted values matched with good precision.
[0116] However, for reaction temperatures of 170°C and 180°C, the actual and predicted values do not match sufficiently. In general, the predicted values are larger than the actual values. The reason why the maximum values of the reaction rate match is because, as mentioned above, the maximum value of the reaction rate is defined as 100%.
[0117] The reason why the actual measured value and the predicted value do not sufficiently match in the conventional technology will be described with reference to Fig. 17. Fig. 17 shows a graph showing the change in reaction rate with respect to reaction time. The crosslinking reaction according to this embodiment proceeds through the following process.
[0118] In the early stage of the reaction, when the reaction starts, the reaction rate gradually increases. After a certain amount of time has passed and the reaction reaches the accelerated stage, the reaction rate increases rapidly. Then, in the later stage of the reaction, the rate of increase in the reaction rate slows down and the reaction rate reaches a maximum value. After the reaction rate reaches its maximum value, the reaction enters the reaction return stage, where the return reaction proceeds. In this reaction return stage, the reaction rate gradually decreases.
[0119] In the above-mentioned technology, the period from the initial stage of reaction to the reversion stage was regarded as one crosslinking reaction. Therefore, the reaction rate was predicted using one activation energy E. As a result, it is considered that the actual reaction rate did not sufficiently match the predicted value.
[0120] 4-4. Crosslinking reaction analysis process of this embodiment In this embodiment, multiple activation energies are calculated according to the progress of the reaction, and the equivalent reaction amount is predicted based on the obtained activation energies. Based on this concept, the formula (4) is transformed into the following formula (18).
[0121]
number
[0122] FIG. 17 shows an example in which the reaction progress state is divided into four stages: an early stage of reaction progress, a reaction promotion stage, a late stage of reaction progress, and a reaction return stage. However, the reaction progress state may be divided into any two to three stages, or five or more stages. Also, the entire period including the reaction progress stage and the reaction return stage may be divided into equal intervals. As an index for dividing into equal intervals, the progress of the crosslinking reaction over the entire period may be used as a standard, and the progress of the crosslinking reaction may be divided into 5% increments, for example. However, the index for division is not limited to 5%, and may be 1% to 4%, or 6% or more.
[0123] In this embodiment, the reaction rate of 0% to 5% is defined as the early stage of reaction progress, the reaction rate of 5% to 50% is defined as the accelerated reaction progress period, the reaction rate of 50% to 100% is defined as the late stage of reaction progress, and the range after the late stage of reaction progress where the reaction rate decreases from 100% to 90% is defined as the reaction return period.
[0124] At each reaction step, the activation energy E is calculated using the above equation (14). N The term containing (E N As shown in FIG. 17, (E1 / R) was about 12,000 in the early stage of reaction (reaction rate 0% to 5%), (E2 / R) was about 9,000 in the accelerated reaction stage (reaction rate 5% to 50%), (E3 / R) was about 13,000 in the late reaction stage (reaction rate 50% to 100%), and (E4 / R) was about 16,000 in the reversal stage (reaction rate 100% to 90%). N The value of (E / R) is not limited to the above value. When the reaction proceeds from the initial stage to the return stage as one reaction stage, (E / R) was 11,000.
[0125] Figure 18 shows the results of predicting the reaction rate using the activation energies E1 to E4 obtained as described above, along with the actual measured values. Not only did the actual measured value and the predicted value match at the reference temperature of 160°C, but the actual measured value and the predicted value also matched with good accuracy at reaction temperatures of 170°C and 180°C. This allows the reaction rate to be predicted with good accuracy.
[0126] In this embodiment, the slope coefficient SC is set to a different value in the reaction progress period until the crosslinking reaction rate reaches a peak and in the reaction return period after the reaction rate has exceeded the peak. Also, in this embodiment, the slope coefficient SC is set to a smaller value in the reaction return period than in the reaction progress period.
[0127] In this embodiment, the slope coefficient SC is set to different values in the early reaction stage, the reaction promotion stage, the late reaction stage, and the reaction return stage. In this embodiment, the slope coefficient SC in the reaction promotion stage is set to a value larger than those in the early reaction stage and the late reaction stage.
[0128] Furthermore, when the entire period of the crosslinking reaction is divided into equal intervals, the slope coefficient SC is set to a value corresponding to each interval.
[0129] 4-5.How to express the reaction rate of crosslinking reaction A method of expressing the reaction rate of the crosslinking reaction in this embodiment will be described with reference to Fig. 19. Fig. 19 is a graph showing the change in the reaction rate of the crosslinking reaction with respect to reaction time. The graph shown by the solid line is the actual measured value of the reaction rate.
[0130] The crosslinking reaction rate shown by the solid line gradually decreases after it reaches a maximum value as the back reaction progresses. For this reason, for example, there will be a point where the reaction rate is 80% before it reaches a maximum value, and a point where the reaction rate is 80% after it reaches a maximum value. In this case, if we simply compare the reaction rate figures, we cannot distinguish between the value of 80% before the reaction rate reaches a maximum value and the value of 80% after the reaction rate reaches a maximum value.
[0131] Therefore, in this embodiment, the reaction rate of the crosslinking reaction is defined as 0% at the start of the crosslinking reaction during the reaction progress phase until the reaction rate of the crosslinking reaction reaches its peak, and the degree of increase in the reaction rate of the crosslinking reaction is defined in the range of 0% to 100%, and in the reaction return phase when the reaction rate has exceeded its peak, the degree of decrease in the reaction rate from the peak reaction rate is defined as a value obtained by adding 100% to the degree of increase.
[0132] To explain this using the graph in Figure 19, the line extending parallel to the horizontal axis from the point where the reaction rate is 100% is used as the axis of symmetry, and the graph of the reaction return period when the reaction rate has passed its peak is inverted as shown by arrow B. As a result, the point where the reaction rate is 80% after the reaction rate has reached its maximum value can be expressed as a reaction rate of 120%. As a result, it is possible to clearly distinguish between the reaction rate before the reaction rate reaches its maximum value and the reaction rate after the reaction rate has reached its maximum value (see Figure 20).
[0133] 4-6. How to determine values calculated by simulation Next, a method for determining values calculated by simulation will be described. In this embodiment, the slope coefficient SC and the reaction rate are determined using one or both of a database and a function. By using a database, the accuracy of the estimated value can be improved. On the other hand, by using a function, the calculation speed can be improved.
[0134] (1) Using a database 1, the memory unit 2 stores a first relationship data map DM1 that defines the correspondence relationship between the reaction rate and the slope coefficient SC of the crosslinking reaction of the polymer portion 12. The reaction rate calculation processing unit 41 determines the slope coefficient SC by using the reaction rate at the previous time and the first relationship data map DM1.
[0135] The memory unit 2 stores a second relationship data map DM2 that defines the correspondence between the equivalent reaction amount integrated value and the reaction rate at the target time. The reaction rate calculation processing unit 41 determines the reaction rate at the target time using the equivalent reaction amount integrated value at the target time and the second relationship data map DM2.
[0136] The second relationship data map DM2 is set from a reference reaction curve RC based on the relationship between the crosslinking reaction time and the torque generated in the test polymer material at a reference reaction temperature measured by a vulcanization tester 70 using a test polymer material corresponding to the polymer part 12 of the target work model WM.
[0137] (2) Using functions 1, the memory unit 2 stores a first function F1 that defines the correspondence relationship between the reaction rate and the slope coefficient SC of the crosslinking reaction of the polymer portion 12. The reaction rate calculation processing unit 41 determines the slope coefficient SC using the reaction rate at the previous time and the first function F1.
[0138] The first function F1 is set to a different function according to a plurality of reaction rate divisions set according to the progress of the crosslinking reaction of the polymer portion 12. The number of divisions of the progress of the crosslinking reaction is arbitrary, and may be one or more than two. Regarding the function, any function can be appropriately selected, such as an n-th order function including linear interpolation, a spline curve, etc. In this embodiment, for example, a sextic function is preferably used. The number of divisions of the first function F1 is determined by the activation energy E N This can be set independently of the category used to calculate the value.
[0139] The storage unit 2 stores a second function F2 that defines the correspondence relationship between the equivalent reaction amount integrated value and the reaction rate at the target time. The reaction rate calculation processing unit 41 determines the reaction rate at the target time using the equivalent reaction amount integrated value at the target time and the second function F2.
[0140] The second function F2 is set from a reference reaction curve RC based on the relationship between the crosslinking reaction time and the torque generated in the test polymer material at a reference reaction temperature measured by a vulcanization tester 70 using a test polymer material corresponding to the polymer part 12 of the target work model WM.
[0141] The second function F2 is set to a different function according to a plurality of reaction rate divisions set according to the progress of the crosslinking reaction of the polymer portion 12. The number of divisions of the progress of the crosslinking reaction is arbitrary, and may be one or more than two. Regarding the function, any function can be appropriately selected, such as an n-th order function including linear interpolation, a spline curve, etc. In this embodiment, for example, a sextic function is preferably used. The number of divisions of the second function F2 is determined by the activation energy E N This can be set independently of the category used to calculate the value.
[0142] Fig. 21 shows an example of the second function F2 when the progress of the crosslinking reaction is divided into four stages. In this embodiment, the stage is divided into an early stage of reaction progress, a reaction promotion stage, a late stage of reaction progress, and a reaction return stage. In each stage, the reaction rate and the reaction time are approximated by a mutually different function.
[0143] Next, an analytical mesh of the target workpiece model WM is created. The size of the analytical mesh may be determined in advance, or may be input from the condition input unit 30. To create the analytical mesh, an analytical mesh as shown in FIG. 22 is created taking into consideration the shape characteristics (e.g., symmetry) of the target workpiece model WM. An eight-node solid element is used as the mesh type. However, any model may be used as the mesh type, and for example, a four-node solid element may be used.
[0144] Using the analytical mesh, the reaction rate of each node can be calculated from the temperature of each node at each time of only the polymer part 12 of the target workpiece model WM.
[0145] 5.Structural analysis processing S3 5-1.Initial processing Next, the structural analysis process S3 will be described. The structural analysis unit 5 creates an analytical mesh of the target workpiece model WM. The analytical mesh of the target workpiece model WM may be the same as the analytical mesh created in the crosslinking reaction analysis process S2, or may be different. In this embodiment, the analytical mesh used in the structural analysis process S3 is the same as the analytical mesh used in the crosslinking reaction analysis process S2.
[0146] 5-2. Temperature and reaction rate acquisition Next, the structure analysis unit 5 acquires the analysis result of the temperature distribution of the polymer part 12 of the target work model WM analyzed by the heat transfer analysis unit 3. In addition, the structure analysis unit 5 acquires the analysis result of the reaction rate of the polymer part 12 of the target work model WM analyzed by the crosslinking reaction analysis unit 4.
[0147] 5-3. Elasticity prediction Next, the structure analysis unit 5 calculates the elastic modulus of each node at each time of the polymer part 12 of the target workpiece model WM. First, a test piece with a reaction rate of 100% of the crosslinking reaction is created, and the elastic modulus of this test piece is actually measured. Next, a correction coefficient is calculated based on the quotient obtained by dividing the torque at the target reaction rate by the torque at the reaction rate of 100%. The above torque is a torque that can be measured by the vulcanization tester 70. The structure analysis unit 5 calculates the elastic modulus of each node at each time by multiplying the actually measured elastic modulus by the calculated correction coefficient.
[0148] 5-4.Characteristics prediction Next, the structural analysis unit 5 predicts the characteristics of the target workpiece model WM. The input conditions used in the finite element analysis are the temperature of each node at each time, the elastic modulus of each node at each time, and the boundary conditions of the outer joining member 13 and the inner joining member 14.
[0149] After the input conditions are set, a force or strain in a direction perpendicular to the axis A of the target workpiece model WM is applied to the target workpiece model WM.
[0150] The structural analysis unit 5 outputs the overall elastic modulus of the target workpiece model WM. In this embodiment, the elastic modulus against a force statically applied in a direction perpendicular to the axis A of the target workpiece model WM is predicted as a characteristic. However, the predicted characteristic is not limited to the elastic modulus against a force or strain in a direction perpendicular to the axis A, and any physical property value can be predicted as a characteristic, such as the elastic modulus against a force vibrating in a direction perpendicular to the axis A, the elastic modulus against a force or strain statically applied in a direction along the axis A, or the elastic modulus against a force vibrating in a direction along the axis A.
[0151] 6. Internal bubble estimation process S4 Next, the internal bubble estimation process S4 will be described. A rubber product, which is an example of this embodiment, is made by molding and vulcanization. Therefore, gas originally dissolved in the rubber or gas generated by the vulcanization reaction is dissolved in the rubber under the high temperature and high pressure conditions of vulcanization. When the mold 10 is opened, the pressure applied to the rubber decreases, and the solubility of the gas in the rubber decreases. Therefore, if the vulcanization is not fully advanced, internal bubbles 80 may occur in the polymer portion 12 made of rubber (see FIG. 23).
[0152] When the vulcanization time is extended while the rubber is placed in the mold 10, the internal bubbles 80 do not occur. In the vulcanization of an actual product, the total amount of heat received differs at points inside the product that are different in distance from the mold 10, which is the heat source, due to differences in temperature rise history, and the progress of vulcanization differs even for the same vulcanization time. Therefore, it is necessary to heat and vulcanize in the mold 10 until the generation of internal bubbles 80 is no longer observed in the slowest vulcanization part. The degree of vulcanization of the rubber in the slowest vulcanization part at the time when the mold 10 is opened when the rubber is molded for the vulcanization time until the generation of internal bubbles 80 is no longer observed in the slowest vulcanization part is called the blow point vulcanization degree (hereinafter, blow point) (see FIG. 24).
[0153] In order to suppress the internal bubbles 80, it is preferable that the heating time in the mold 10 be as long as possible. However, if the heating time in the mold 10 is excessively extended, the production efficiency of the product will decrease. Therefore, in order to determine the vulcanization time of the product, it is important to estimate the above-mentioned blow point.
[0154] Fig. 25(a) shows the blow point reaction rates when a plurality of types of fillers are added to a plurality of types of polymers in different compounding amounts. The blow point reaction rate is the reaction rate of the crosslinking reaction of the polymer part 12 at the blow point.
[0155] Eight types of polymers from A to H were used as the raw material polymers. Samples A1 to A3 are those in which the compounding amount of the filler was changed using the raw material polymer A. Similarly, samples B1 to B3 are those in which the compounding amount of the filler was changed for the raw material polymer B, and samples C1 to C3 are those in which the compounding amount of the filler was changed for the raw material polymer C. Since commercially available products were used for the samples, the types and compounding amounts of the fillers are not exactly known.
[0156] As shown in Fig. 25(a), the blow point reaction rates vary greatly depending on the type of the raw material polymer and the compounding amount of the filler. Therefore, it was found that it is difficult to predict the blow point of the polymer part 12 using the blow point reaction rate.
[0157] As shown in Fig. 26, when the pressure P1 at which the internal bubbles 80 tend to expand and the pressure P2 at which the polymer part tries to suppress the internal bubbles 80 satisfy P1 < P2, it is considered that the internal bubbles 80 are suppressed by the rubber and disappear. Therefore, the blow point reaction rate was converted into the torque measured by the vulcanization tester 70 corresponding to the blow point reaction rate and compared for each sample.
[0158] Fig. 25(b) shows the blow point torque when different amounts of different fillers are added to different polymers. As described above, the blow point torque is obtained by converting the blow point reaction rate into the torque measured by the vulcanization tester 70 corresponding to the blow point reaction rate.
[0159] As shown in FIG. 25(b), the torque (blow point torque) at which internal bubbles 80 are no longer generated is almost the same regardless of the type of raw polymer or the amount of filler. In other words, by using a torque that is easily measurable, the blow point can be easily predicted. The vertical axis of FIG. 25(b) shows the threshold value. The estimation unit 62 of the internal bubble estimation unit 6 estimates that internal bubbles 80 have been generated in the polymer part 12 of the target workpiece model WM when the torque at the time when the target workpiece model WM is demolded does not exceed the threshold value.
[0160] The threshold value is set to a uniform value for multiple types of raw material polymers. The threshold value is a torque corresponding to a reaction rate higher than the reaction rate of the crosslinking reaction at the blow point of the polymer portion 12. However, the threshold value may be set in multiple groups and a threshold value may be set for each group. The multiple groups can be divided by any criteria.
[0161] The reaction rate acquisition unit 51 acquires the reaction rate for each part of the polymer portion 12, the torque calculation unit 61 calculates the torque for each part of the polymer portion 12, and the estimation unit 62 estimates the occurrence of internal bubbles 80 for each part of the polymer portion 12.
[0162] 7. Display process S5 Next, the display process S5 will be described. As shown in Fig. 1, the display unit 7 displays a value obtained from the reaction rate according to the reaction time based on the analysis result of the crosslinking reaction analysis unit 4.
[0163] Furthermore, based on the analysis results of the structural analysis unit 5, the display unit 7 displays characteristics corresponding to the temperature of the mold model MM used for the crosslinking reaction of the polymer part 12 and the in-mold reaction time from the start of the crosslinking reaction to the demolding of the mold model MM.
[0164] Furthermore, based on the estimation results of the internal bubble estimation unit 6, the display unit 7 displays the presence or absence of internal bubbles 80 depending on the temperature of the molding die model MM and the in-mold reaction time from the start of the crosslinking reaction to the demolding of the molding die model MM.
[0165] Furthermore, the display unit 7 displays a value obtained from a reaction rate corresponding to the temperature of the molding die model MM and the in-mold reaction time from the start of the crosslinking reaction to the demolding of the molding die model MM, based on the analysis results of the crosslinking reaction analysis unit 4, together with the presence or absence of internal bubbles 80. However, the contents displayed by the display unit 7 are not limited to those described above.
[0166] 7-1.Table display method (1) Form of displaying response rate With reference to Tables 1 to 4, a form for displaying the reaction rate of the crosslinking reaction using a table will be described.
[0167] [Table 1]
[0168] Table 1 summarizes the relationship between the mold temperature and the reaction time for the crosslinking reaction rate in the element of the target workpiece model WM that has the smallest crosslinking reaction rate.
[0169] The reaction times listed in Table 1 represent the reaction times when the target workpiece model WM is placed inside the mold 10. The reaction rate values listed in Table 1 are calculated based on the temperature history of both the reaction time when the target workpiece model WM is placed inside the mold 10 and the time after the target workpiece model WM is released from the mold 10. Since the crosslinking reaction continues even after the target workpiece model WM is released from the mold 10, the above consideration is required. In the following explanation, the same applies to the reaction times and reaction rates listed in Tables 2 to 4.
[0170] In Table 1, the region enclosed by a thick line in the upper right corner has a reaction rate greater than 115%. In this region, the reverse reaction of the crosslinking reaction is proceeding excessively, which is undesirable. However, the reaction rate range can be set arbitrarily, and a value other than 115% can be used as the threshold value.
[0171] The region surrounded by a thick line in the lower left of Table 1 has a reaction rate lower than 95%. This region is not preferable because the crosslinking reaction has not progressed sufficiently. However, the reaction rate range can be set arbitrarily, and a value other than 95% can be used as the threshold value.
[0172] In Table 1, the region surrounded by the thick ruled line, excluding the upper right region and the lower left region, is a preferable region from the viewpoint of the reaction rate of the crosslinking reaction. Note that Table 1 does not include information on the internal bubbles 80 described later.
[0173] Table 2 summarizes the relationship between the mold temperature and the reaction time for the average value of the crosslinking reaction of all elements of the target workpiece model WM.
[0174] [Table 2]
[0175] In Table 2, the region surrounded by a thick line in the upper right corner has a reaction rate greater than 115%. In this region, the reverse reaction of the crosslinking reaction is proceeding excessively, which is undesirable. However, the range of the reaction rate can be set arbitrarily, and a value other than 115% can be used as the threshold value.
[0176] The region surrounded by a thick line in the lower left of Table 2 has a reaction rate lower than 95%. This region is not preferable because the crosslinking reaction has not progressed sufficiently. However, the reaction rate range can be set arbitrarily, and a value other than 95% can be used as the threshold value.
[0177] In Table 2, the regions other than the upper right region and the lower left region are preferable regions from the viewpoint of the reaction rate of the crosslinking reaction. Note that Table 2 does not include information on the internal bubbles 80 described later.
[0178] Table 3 summarizes the relationship between the mold temperature and the reaction time for the crosslinking reaction rate in the element with the highest crosslinking reaction rate in the target workpiece model WM.
[0179] [Table 3]
[0180] In Table 3, the region surrounded by a thick line in the upper right corner has a reaction rate greater than 115%. In this region, the reverse reaction of the crosslinking reaction is proceeding excessively, which is undesirable. However, the reaction rate range can be set arbitrarily, and a value other than 115% can be used as the threshold value.
[0181] The region surrounded by a thick line in the lower left of Table 3 has a reaction rate lower than 95%. This region is not preferable because the crosslinking reaction has not progressed sufficiently. However, the reaction rate range can be set arbitrarily, and a value other than 95% can be used as the threshold value.
[0182] In Table 3, the regions other than the upper right region and the lower left region are preferable regions from the viewpoint of the reaction rate of the crosslinking reaction. Note that Table 3 does not include information on the internal bubbles 80 described later.
[0183] Table 4 is Table 2 with the addition of information regarding the internal bubbles 80.
[0184] [Table 4]
[0185] In Table 4, the region surrounded by a thick line in the upper right corner has a reaction rate greater than 115%. In this region, the reverse reaction of the crosslinking reaction is proceeding excessively, which is undesirable. However, the reaction rate range can be set arbitrarily, and a value other than 115% can be used as the threshold value.
[0186] In Table 4, the portion enclosed by the double ruled line indicates that an internal bubble 80 was generated in the polymer portion 12 of the target workpiece model WM.
[0187] In the area below the dashed line in the double-lined area in the lower left of Table 4, the reaction rate is less than 95%. This area is not preferable because the crosslinking reaction has not progressed sufficiently. However, the reaction rate range can be set arbitrarily, and a value other than 95% can be used as the threshold value.
[0188] In Table 4, among the regions surrounded by the double ruled line, the region above the dashed line indicates that the reaction rate of the crosslinking reaction was within the range of 95% to 115%, but internal bubbles 80 occurred in the polymer part 12 of the target work model WM. Since internal bubbles 80 occurred in the polymer part 12 in this region, it is not preferable as a product.
[0189] In this embodiment, Table 4 was created by adding information about the internal bubbles 80 to the prediction results shown in Table 2, but this is not limited to this, and information about the internal bubbles 80 can be added to the prediction results of the reaction rate at any temperature.
[0190] (2) Form for displaying elastic modulus Table 5 summarizes the relationship between the elastic modulus of the target workpiece model WM, the mold temperature, and the reaction time.
[0191] The reaction times listed in Table 5 represent the reaction times when the target workpiece model WM is placed inside the mold 10. The elastic modulus values listed in Table 5 are calculated based on the temperature histories of both the reaction time when the target workpiece model WM is placed inside the mold 10 and the time after the target workpiece model WM is released from the mold 10. Since the crosslinking reaction continues even after the target workpiece model WM is released from the mold 10, the above consideration is necessary. Note that in the following explanation, the same applies to the reaction times and elastic moduli listed in Figs. 28 to 31.
[0192] [Table 5]
[0193] The elastic modulus is the elastic modulus when a static force is applied in a direction perpendicular to the axis A of the target work model WM. The values in the table are the ratios to the elastic modulus when the reaction rate of the crosslinking reaction is 100%. However, the direction of the force applied to the target work model WM is not limited, and the elastic modulus when a force is applied in any direction can be adopted, such as when a static force is applied in a direction parallel to the axis A of the target work model WM, when a static force is applied in a direction rotating around the axis A of the target work model WM, when a static force is applied in a direction tilting against the axis A of the target work model WM, etc. In addition, the force applied to the target work model WM is not limited to a static force, and may be, for example, the elastic modulus when vibration is applied to the target work model WM.
[0194] Table 5 is a table that summarizes the relationship between the elastic modulus obtained as a result of performing a structural analysis by assigning an elastic modulus according to the degree of vulcanization to each element of the target workpiece model WM, and the mold temperature and reaction time. The meanings of the thick lines, double lines, and dashed lines in Table 5 are the same as those in Table 4, so duplicate explanations will be omitted. In Table 5, the cells with "-" written in them indicate the locations where a calculation error occurred in the elastic modulus simulation.
[0195] Additionally, any information may be added to Table 5, such as information regarding internal bubbles 80.
[0196] In this embodiment, lines are used to separate the numbers in the table, but this is not limited to the above. The numbers in the table can be separated by any method, such as changing the color of the numbers in the table, changing the font, changing the typeface to italics or bold, changing the background color of the cells in which the numbers are written, or changing the background pattern of the cells.
[0197] 7-2. Display method using heat map 90 A form of displaying the reaction rate of the crosslinking reaction using a heat map diagram 90 will be described with reference to Fig. 27. Fig. 27 shows a heat map diagram 90 in which the distribution of the reaction rate of the crosslinking reaction is displayed in shades of gray for the target workpiece model WM.
[0198] In the heat map diagram 90, the outer bonding member 13 and the inner bonding member 14 of the target workpiece model WM are displayed in white. Also, the polymer part 12 of the target workpiece model WM is displayed divided into regions 91 to 94 according to the magnitude of the crosslinking reaction rate, and each of the divided regions 91 to 94 is displayed in shade according to the magnitude of the crosslinking reaction rate.
[0199] Region 91 has the highest cross-linking reaction rate and is displayed in the darkest color tone. Region 92 has the second highest cross-linking reaction rate and is displayed in the second darkest color tone. Region 93 has the third highest cross-linking reaction rate and is displayed in the third darkest color tone. Region 94 has the lowest cross-linking reaction rate and is displayed in the lightest color tone.
[0200] The display unit 7 displays to the operator a heat map diagram 90. The operator can intuitively understand the distribution of the reaction rate of the crosslinking reaction in the polymer portion 12 by visually checking the regions 91 to 94 displayed in shading, regarding the reaction rate of the crosslinking reaction in the polymer portion 12 of the target work model WM.
[0201] The heat map diagram 90 can be created and output for all reaction conditions (e.g., temperature, time, etc.) related to the target workpiece model WM. The heat map diagram 90 may also be created and output only for a predetermined reaction condition.
[0202] The method of displaying the heat map 90 by the display unit 7 is not particularly limited, and for example, the display unit 7 may display the above-mentioned Table 5, and the operator may select each cell in the displayed Table 5 to display the heat map 90 for the reaction conditions corresponding to the selected cell. Alternatively, the operator may input reaction conditions for the crosslinking reaction, and the heat map 90 corresponding to the input reaction conditions may be displayed.
[0203] In this embodiment, the heat map diagram 90 is configured so that the polymer portion 12 is divided into regions 91 to 94, but is not limited thereto, and the polymer portion 12 may be divided into two, three, or five or more regions. In the heat map diagram 90, regions with high reaction rates may be displayed in lighter shades, and regions with low reaction rates may be displayed in darker shades.
[0204] In addition, in the heat map diagram 90, areas with high response rates may be displayed in warm colors such as red, and areas with low response rates may be displayed in cool colors such as blue, or areas with high response rates may be displayed in cool colors such as blue, and areas with low response rates may be displayed in warm colors such as red.
[0205] 7-3.Graph display method (1) Form for displaying elastic modulus With reference to Figs. 28 to 30, a form of displaying the elastic modulus of the target workpiece model WM using a graph will be described. Figs. 28 to 30 are graphs of the elastic modulus of the target workpiece model WM versus the reaction time of the crosslinking reaction. Fig. 28 is a graph when the crosslinking reaction of the polymer part 12 of the target workpiece model WM is performed at the lowest temperature of the mold 10, Fig. 29 is a graph when the crosslinking reaction of the polymer part 12 of the target workpiece model WM is performed at a medium temperature of the mold 10, and Fig. 30 is a graph when the crosslinking reaction of the polymer part 12 of the target workpiece model WM is performed at the highest temperature of the mold 10. In Figs. 28 to 30, the solid line indicates the actual measured value of the elastic modulus, and the dashed line indicates the predicted value.
[0206] As shown in Figs. 28 to 30, the elastic modulus increases after the start of the crosslinking reaction and reaches a maximum value, and then decreases after reaching the maximum value.
[0207] In FIG. 28, where the temperature of the mold 10 is the lowest, the measured elastic modulus values and the predicted elastic modulus values matched with good accuracy.
[0208] In Fig. 29, where the temperature of the mold 10 is moderate, the measured and predicted values of the elastic modulus did not match up to 2 minutes after the start of the reaction, but after 2 minutes, the measured and predicted values matched with good accuracy. Up to 2 minutes after the start of the reaction, the predicted elastic modulus was smaller than the measured value. However, the area within 2 minutes after the start of the reaction is not considered to be used as a product, so there is little impact on the product.
[0209] In FIG. 30, where the mold 10 temperature is the highest, the measured and predicted values of the elastic modulus did not match up to 2 minutes after the start of the reaction, but after 2 minutes, the measured and predicted values matched with good accuracy. Up to 2 minutes after the start of the reaction, the predicted elastic modulus was smaller than the measured value. The difference between the measured and predicted values was larger than when the mold 10 temperature was at an intermediate level. However, as described above, the region within 2 minutes after the start of the reaction is not considered to be used as a product, so there is little impact on the product.
[0210] (2) A form in which the elastic modulus and the internal air bubbles 80 are displayed together 31, a mode of displaying the elastic modulus of the polymer portion 12 of the target workpiece model WM and the predicted results of the generation of internal bubbles 80 using a graph will be described. The temperature of the mold 10 is set to a medium temperature, as in the case of FIG. 29 described above.
[0211] FIG. 31 shows a graph of the elastic modulus versus reaction time when a force is applied in a direction perpendicular to the axis A of the target workpiece model WM. The square symbols indicate the elastic modulus in the element where the temperature of the polymer portion 12 of the target workpiece model WM is the highest. The circular symbols indicate the elastic modulus in the element where the temperature of the polymer portion 12 of the target workpiece model WM is the median. The triangular symbols indicate the elastic modulus in the element where the temperature of the polymer portion 12 of the target workpiece model WM is the lowest. In FIG. 31, the open symbols indicate cases where it is predicted that internal bubbles 80 will be generated, and the filled symbols indicate cases where it is predicted that internal bubbles 80 will not be generated.
[0212] The graphs for the element where the temperature of the polymer portion 12 is the maximum value and the element where the temperature is the median value are graphs for the reaction reversion period after the reaction progress period.
[0213] In the element where the temperature of the polymer portion 12 is the highest, the crosslinking reaction proceeds most quickly. For this reason, it was predicted that the internal bubbles 80 would not be generated when the reaction time exceeded 3 minutes and 3 minutes and 30 seconds had elapsed. In the element where the temperature of the polymer portion 12 is the highest, the return reaction of the crosslinking reaction also proceeds quickly, and therefore the elastic modulus is the lowest when the reaction time has elapsed for 6 minutes.
[0214] In the element where the temperature of the polymer portion 12 is the median, the progress of the crosslinking reaction is also at a moderate level. For this reason, it was predicted that when the reaction time exceeds 3 minutes 30 seconds and 4 minutes has elapsed, the internal bubbles 80 would not be generated. The elastic modulus at the reaction time of 6 minutes is larger than that of the element where the temperature of the polymer portion 12 is the highest.
[0215] In the element where the temperature of the polymer portion 12 is the lowest, the crosslinking reaction proceeds the slowest. Therefore, before the reaction time is 4 minutes, the reaction is in the progress phase, and it was predicted that the elastic modulus would increase with the reaction time. After the reaction time has passed 4 minutes, the return reaction of the crosslinking reaction proceeds, and the elastic modulus was predicted to gradually decrease. In the element where the temperature of the polymer portion 12 is the lowest, it was predicted that the internal bubbles 80 would not be generated when the reaction time exceeds 5 minutes and 5 minutes and 30 seconds have passed. At this point, it was predicted that the internal bubbles 80 had disappeared in the entire region of the polymer portion 12 of the target workpiece model WM. It was predicted that the elastic modulus at the time when the reaction time has passed 6 minutes would be the largest in the entire region of the polymer portion 12.
[0216] As described above, it was predicted that the internal bubbles 80 would disappear in the entire region of the polymer portion 12 of the target workpiece model WM when the reaction time had passed 5 minutes and 30 seconds, but in consideration of the risk ratio, the reaction time when the reaction time had passed 6 minutes was adopted as the reaction time of this target workpiece model WM. At the reaction time of 6 minutes, the variation in the elastic modulus of the polymer portion 12 was predicted to be 12%.
[0217] In this manner, according to this embodiment, it is possible to predict the reaction time at which the internal bubbles 80 no longer occur for the target workpiece model WM, and also to predict the variation in the elastic modulus of the polymer portion 12 at that reaction time.
[0218] (3) A form that visually displays the internal bubbles 80 With reference to FIG. 32, a form for visually displaying the predicted results of the generation of internal bubbles 80 in the polymer portion 12 of the target workpiece model WM will be described.
[0219] 32 is a diagram showing, by using a cross-sectional view of the target workpiece model WM, the degree of possibility of generation of internal bubbles 80 in the polymer part 12, using shading. The outer bonding member 13 and the inner bonding member 14 of the target workpiece model WM are shown by the darkest pattern in FIG.
[0220] The polymer portion 12 of the target workpiece model WM is shown by the lightest pattern in Fig. 32. An elliptical region P and an elliptical region Q located inside region P are displayed inside the polymer portion 12. Region P is displayed by a pattern that is slightly darker than the light pattern representing the polymer portion 12. Region Q is displayed by a pattern that is slightly darker than region P.
[0221] An example will be described in which, as a result of the internal bubble estimation process S4, for example, region P is determined to be a region in which internal bubbles 80 are relatively likely to occur, and region Q is determined to be a region in which internal bubbles 80 are more likely to occur than region P. Regions P and Q actually correspond to regions in which internal bubbles 80 are likely to occur (see FIG. 23).
[0222] When the internal bubble estimation process S4 is completed, the display unit 7 displays the target workpiece model WM shown in FIG. 32. By looking at FIG. 32 displayed on the display unit 7, the worker visually recognizes the outer bonding member 13 and the inner bonding member 14 shown in a relatively dark pattern and the polymer portion 12 shown in a relatively light pattern. The worker can intuitively understand that the outer bonding member 13 and the inner bonding member 14 shown in a dark pattern are different parts from the polymer portion 12. This allows the worker to intuitively understand that in order to find the internal bubble 80, it is sufficient to check the polymer portion 12 shown in a relatively light pattern. However, the outer bonding member 13 and the inner bonding member 14 may be displayed in white.
[0223] Next, the worker visually confirms that the regions P and Q shown in a relatively dark pattern are displayed in the polymer portion 12 shown in a light pattern. This allows the worker to intuitively understand that the internal bubbles 80 are likely to occur in the regions P and Q of the polymer portion 12. Furthermore, since the region Q is displayed in a darker pattern than the region P, the worker can intuitively understand that the internal bubbles 80 are most likely to occur in the region P. This allows the worker to efficiently consider the manufacturing conditions of the target workpiece model WM, since it is only necessary to search for the internal bubbles 80 in the region where the internal bubbles 80 are likely to occur when considering the manufacturing conditions of the target workpiece model WM. However, the region where the internal bubbles 80 are likely to occur may be displayed in a relatively light pattern.
[0224] The present invention is not limited to the above-described embodiments, and can be applied to various embodiments without departing from the gist of the present invention.
[0225] In this embodiment, the internal bubble estimation unit 6 is configured to include a torque calculation unit 61, but is not limited thereto. The internal bubble estimation unit 6 may be configured to include a reaction rate acquisition unit 60 that acquires the reaction rate (vulcanization degree) of the crosslinking reaction of the polymer part 12 of the target work model WM, and an estimation unit 62 that estimates the generation of bubbles in the polymer part 12 of the target work model WM based on the reaction rate at the time of demolding. In this case, before performing the reaction analysis of the vulcanization reaction, the vulcanization degree at the torque that is the threshold value is obtained from the reference reaction curve RC, and this vulcanization degree can be set as the blow point vulcanization degree. In addition, the blow point vulcanization degree may be directly measured using a known measuring device such as a blow point analyzer or a blow point tester. After that, the reaction analysis of the vulcanization reaction is performed, and the calculation result (vulcanization degree) of the reaction rate acquisition unit 60 is compared with the above blow point vulcanization degree to estimate the generation of internal bubbles. For example, when the vulcanization degree does not exceed the blow point vulcanization degree, it is estimated that the internal bubbles 80 have been generated in the polymer part 12 of the target work model WM. [Explanation of symbols]
[0226] 1: crosslinking reaction simulation device, 2: memory unit, 3: heat transfer analysis unit, 4: crosslinking reaction analysis unit, 5: structural analysis unit, 6: internal bubble estimation unit, 7: display unit, 10: mold, 11: hot plate, 12: polymer unit, 13: outer bonding member, 14: inner bonding member, 15: gap, 15A: outer gap, 15B: inner gap, 30: condition input unit, 31: polymer thermal diffusivity determination unit, 32: analysis unit, 40: temperature acquisition unit, 41: reaction rate calculation processing unit, 50: temperature acquisition unit, 51: reaction rate acquisition unit, 52: elastic modulus assignment unit, 53: characteristic acquisition unit, 60: reaction rate acquisition unit, 61: torque calculation unit, 62: estimation unit, 70: vulcanization tester, 80: internal bubble, A: axis, AC: air heat transfer coefficient, BD: data for estimating internal bubble, C: specific heat, CC: crosslinking reaction curve, DM1: first relationship data map, DM2: second relationship data map, E: activation energy, EM: equivalent reaction amount calculation model, E N: activation energy, F1: first function, F2: second function, CH: contact heat transfer coefficient, k: reaction rate, MM: mold model, OC: ambient conditions, RC: reference reaction curve, RD: data for crosslinking reaction analysis, S1: heat transfer analysis process, S2: crosslinking reaction analysis process, S3: structural analysis process, S4: internal bubble estimation process, S5: display process, SC: coefficient, t: reaction time, T: reaction temperature, t0: reference time, T0: reference temperature, TC: temperature conditions, TD: data for heat transfer analysis, TS: thermal diffusivity characteristics, U: equivalent reaction amount, WM: target workpiece model, Z: reaction amount, α: thermal diffusivity, Δt: minute time, ΔUi: equivalent reaction amount increase, λ: thermal conductivity
Claims
1. A storage unit that stores data used in the simulation; a heat transfer analysis unit that performs a heat transfer analysis during a cross-linking reaction of a polymer part of a target workpiece model; A crosslinking reaction simulation device comprising: The storage unit is A molded model; A target work model having the polymer portion including a raw material polymer and carbon black; a thermal diffusivity characteristic representing a relationship between a mass ratio of the carbon black to the raw polymer and a thermal diffusivity of the polymer portion; The heat transfer analysis unit is a condition input unit for inputting a mass ratio of the carbon black to the raw material polymer in the target workpiece model and a temperature condition of the mold model; a polymer thermal diffusivity determination unit that determines a polymer thermal diffusivity, which is the thermal diffusivity of the polymer portion of the target workpiece model, based on the mass ratio input by the condition input unit and the thermal diffusivity characteristics stored in the storage unit; an analysis unit that performs heat transfer analysis using the polymer thermal diffusivity determined by the polymer thermal diffusivity determination unit and the temperature conditions stored in the memory unit while the target work model is placed on the mold model.
2. 2. The crosslinking reaction simulation device according to claim 1, wherein the thermal diffusivity characteristic is independent of the type of the raw material polymer.
3. 2. The crosslinking reaction simulator according to claim 1, wherein the thermal diffusivity characteristics are a relationship established from actual measured values in experiments using a plurality of types of raw material polymers at different mass ratios of carbon black.
4. The crosslinking reaction simulation device according to claim 1 , wherein the thermal diffusivity characteristic has a linear relationship with the mass ratio of the carbon black.
5. The target workpiece model is The polymer portion; a joining member joined to the polymer portion, The storage unit further includes: storing a contact heat transfer coefficient, which is a heat transfer coefficient between the mold model and the joining member, in a state in which the target workpiece model is disposed on the mold model; 2. The crosslinking reaction simulation device according to claim 1, wherein the analysis unit performs the heat transfer analysis using the polymer thermal diffusivity determined by the polymer thermal diffusivity determination unit, the temperature conditions stored in the memory unit, and the contact heat transfer coefficient with the target work model placed on the mold model.
6. The condition input unit includes: The outside air conditions including the ambient temperature of the target workpiece model released from the mold model are input, The storage unit further The air heat transfer coefficient is stored as the heat transfer coefficient of air; 2. The crosslinking reaction simulation device according to claim 1, wherein the analysis unit performs the heat transfer analysis using the polymer thermal diffusivity determined by the polymer thermal diffusivity determination unit, the air heat transfer coefficient stored in the memory unit, and the outside air conditions, in a state in which the polymer part of the target work model is subjected to a crosslinking reaction within the mold model and then the target work model is removed from the mold model.
Citation Information
Patent Citations
Resin-bonded body deformation simulation method, device, program, and resin-bonded body mounting system using these
JP2006284249A
Critical vulcanization degree testing device for foaming in rubber sample and its method for determining vulcanization limit
JP2009085791A
Vulcanization mold for specifying blowing limit vulcanization degree and testing device having the same
JP2017071057A
Process for producing mold
WO2011158673A1