Polishing composition, polishing method, and method for producing semiconductor substrate

A polishing composition with specific abrasive grains and amine oxide compounds at pH 5 to 10 addresses the challenge of high-speed polycrystalline silicon polishing while minimizing silicon nitride and oxide film polishing, enhancing semiconductor manufacturing efficiency.

JP2024141119AActive Publication Date: 2024-10-10FUJIMI INCORPORATED
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023052593
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Existing polishing compositions fail to achieve high-speed polishing of polycrystalline silicon films while simultaneously suppressing the polishing rate of silicon nitride and silicon oxide films, which is crucial for improving semiconductor manufacturing efficiency.

Method used

A polishing composition containing abrasive grains with a negative zeta potential and an amine oxide compound, formulated at a pH of 5 to 10, with specific alkyl group configurations and association degrees, enhances the polishing rate of polycrystalline silicon while reducing the polishing rate of silicon nitride and silicon oxide films.

Benefits of technology

The composition enables high-speed polishing of polycrystalline silicon films while maintaining low polishing rates for silicon nitride and silicon oxide films, thereby improving polishing selectivity and manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141119000001
    Figure 2024141119000001
  • Figure 2024141119000002
    Figure 2024141119000002
  • Figure 2024141119000003
    Figure 2024141119000003
Patent Text Reader

Abstract

To provide a polishing composition that enables high-speed polishing of a polycrystalline silicon film while reducing the polishing rate for at least one of a silicon nitride film and a silicon oxide film.SOLUTION: A polishing composition contains abrasive grains and an amine oxide compound, and has a pH greater than 5 and less than or equal to 10. The abrasive grains have a negative zeta potential in the polishing composition, and has an average degree of association from 3.0 to 6.0 inclusive. The amine oxide compound has a structure represented by formula (1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a polishing composition, a polishing method, and a method for producing a semiconductor substrate. [Background technology]

[0002] BACKGROUND ART In recent years, with the trend toward multilayer wiring on semiconductor substrate surfaces, a technique known as chemical mechanical polishing (CMP) is used to polish and flatten semiconductor substrates when manufacturing devices.

[0003] CMP has been applied to various processes in semiconductor manufacturing, and one example of its application is the gate formation process in transistor fabrication. During transistor fabrication, materials such as metal, silicon, silicon oxide, polycrystalline silicon, and silicon nitride are often polished, and there is a demand for high-speed polishing of each material to improve productivity. To meet this demand, for example, Patent Document 1 discloses a technology that aims to improve the polishing speed of polycrystalline silicon. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2013-041992 Summary of the Invention [Problem to be solved by the invention]

[0005] While studying the application of CMP to various steps in semiconductor manufacturing, the present inventors have found that in some cases, it is preferable from a manufacturing perspective to polish a polycrystalline silicon film at high speed in the presence of a silicon nitride film or a silicon oxide film. On the other hand, they have found that in some cases, it is preferable from a manufacturing perspective to minimize the polishing rate for a silicon nitride film or a silicon oxide film. However, there is no polishing composition yet available that can polish a polycrystalline silicon film at high speed while suppressing the polishing rate for a silicon nitride film or a silicon oxide film.

[0006] Therefore, an object of the present invention is to provide a polishing composition that can polish a polycrystalline silicon film at high speed while suppressing the polishing rate of at least one of a silicon nitride film and a silicon oxide film. [Means for solving the problem]

[0007] In order to solve the above problems, the present inventors have conducted extensive research and have found a polishing composition containing abrasive grains and an amine oxide compound, the polishing composition having a pH of more than 5 and not more than 10, the abrasive grains having a negative zeta potential in the polishing composition and an average degree of association of 3.0 or more and 6.0 or less, and the amine oxide compound having a structure represented by the following formula (1):

[0008] [ka]

[0009] In formula (1), R 1 ~R 3 are each independently an alkyl group having 1 to less than 14 carbon atoms, where R 1 ~R 3 At least one of the groups is an alkyl group having more than 8 and less than 14 carbon atoms. The present invention has been completed based on the discovery that the above problems can be solved by a polishing composition represented by the formula: [Effects of the Invention]

[0010] According to the present invention, there is provided a polishing composition which can polish a polycrystalline silicon film at high speed and suppress the polishing rate of at least one of a silicon nitride film and a silicon oxide film. DETAILED DESCRIPTION OF THE INVENTION

[0011] The following describes in detail the embodiments of the present invention. The embodiments described herein are provided as examples to embody the technical concept of the present invention and are not intended to limit the present invention. Therefore, all other embodiments, methods of use, and operational techniques conceivable by those skilled in the art that do not deviate from the gist of the present invention are included within the scope and spirit of the present invention, as well as within the scope of the claims and their equivalents. The embodiments described herein can be arbitrarily combined to form other embodiments. Furthermore, unless otherwise specified herein, operations and measurements of physical properties are performed at room temperature (20°C to 25°C) and a relative humidity of 40% RH to 60% RH.

[0012] The present invention provides a polishing composition comprising abrasive grains and an amine oxide compound, the polishing composition having a pH of more than 5 and not more than 10, wherein the abrasive grains have a negative zeta potential in the polishing composition and an average degree of association of 3.0 or more and 6.0 or less, and the amine oxide compound is represented by the following formula (1):

[0013] [ka]

[0014] In formula (1), R 1 ~R 3 are each independently an alkyl group having 1 to less than 14 carbon atoms, where R 1 ~R 3 At least one of the groups is an alkyl group having more than 8 and less than 14 carbon atoms. This polishing composition is capable of polishing a polycrystalline silicon film at high speed and suppressing the polishing rate of at least one of a silicon nitride film and a silicon oxide film. The inventors speculate that the mechanism by which this effect is achieved by the present invention is as follows. However, the following mechanism is merely speculation, and the scope of the present invention is not limited thereby.

[0015] In the present invention, the object to be polished preferably includes at least a polycrystalline silicon film and at least one of a silicon nitride film and a silicon oxide film. The polishing composition of the present invention effectively polishes the polycrystalline silicon film at high speed and suppresses the polishing rate of at least one of a silicon nitride film and a silicon oxide film. In a polishing composition having a pH greater than 5 and less than 10, abrasive grains with a negative zeta potential are easily adsorbed to polycrystalline silicon films, silicon nitride films, and silicon oxide films, resulting in an increase in the number of abrasive grains present on the surfaces of the polycrystalline silicon films, silicon nitride films, and silicon oxide films during polishing. When the degree of association of the abrasive grains is high (e.g., abrasive grains with a degree of association of 3.0 to 6.0), the abrasive grains assume a rod-like shape and tend to remain on the surface of the object to be polished. This further improves the polishing rate of the polycrystalline silicon film, silicon nitride film, and silicon oxide film. However, increasing the polishing rate for silicon nitride films and silicon oxide films reduces the ratio of the polishing rate for polycrystalline silicon to the polishing rate for silicon nitride (polishing rate for polycrystalline silicon / polishing rate for silicon nitride) and the ratio of the polishing rate for polycrystalline silicon to the polishing rate for silicon oxide (polishing rate for polycrystalline silicon / polishing rate for silicon oxide). The inventors have found that, when the polishing composition of the present invention has a pH greater than 5 and not greater than 10, it contains a specific amine oxide compound, thereby improving the polishing rate for polycrystalline silicon films and suppressing or maintaining the polishing rates for silicon nitride films and silicon oxide films. Hereinafter, the ratio of the polishing rate for polycrystalline silicon to the polishing rate for silicon nitride or silicon oxide is also referred to as the "polishing selectivity for polycrystalline silicon."

[0016] That is, it is thought that certain amine oxide compounds are more likely to adsorb to polycrystalline silicon films at certain pH levels. When an amine oxide compound adsorbs to a polycrystalline silicon film, the lone electron pair on the nitrogen atom of the amine oxide compound interacts with the silicon-silicon bond on the surface of the polycrystalline silicon film, embrittling the surface of the polycrystalline silicon film. This makes it easier for abrasive particles on the surface of the polycrystalline silicon film to act on the polycrystalline silicon film, improving the polishing rate of the polycrystalline silicon film.

[0017] On the other hand, the above-mentioned interaction of specific amine oxide compounds with silicon nitride film and silicon oxide film is not as strong as with polycrystalline silicon film, and the effect of embrittling the silicon nitride film surface and silicon oxide film surface is weak.In other words, it is speculated that silicon nitride film and silicon oxide film are chemically stable in the presence of the polishing composition of the present invention, and pH and the potential of abrasive grains are dominant, and as a result, the polishing speed of polycrystalline silicon film is improved, and the polishing selectivity of polycrystalline silicon can be improved.As described above, it is considered that the polishing composition of the present invention can polish polycrystalline silicon film at high speed, and can suppress the polishing speed of silicon nitride film and silicon oxide film.

[0018] As described above, the present inventors have found that a polishing composition having a pH greater than 5 and not greater than 10, which contains abrasive grains having a negative zeta potential and a degree of association of 3.0 or more and 6.0 or less, and a specific amine oxide compound, can solve the problem of polishing polycrystalline silicon films at high speed while suppressing the polishing rate for silicon nitride films and silicon oxide films.

[0019] The above mechanism is based on speculation, and the present invention is not limited to the above mechanism in any way.

[0020] [Polished object] The object to be polished according to the present invention preferably comprises a polycrystalline silicon (polysilicon) film and at least one of a silicon nitride (Si3N4) film and a silicon oxide (SiO2) film. That is, the polishing composition according to a preferred embodiment of the present invention is used for polishing an object to be polished that comprises a polycrystalline silicon film and at least one of a silicon nitride film and a silicon oxide film.

[0021] According to one embodiment of the present invention, the use of the object to be polished is not limited, and examples thereof include semiconductor substrates, solar cell substrates, TFTs for liquid crystal displays (LCDs), etc. The present invention is also suitable for use as test wafers, monitor wafers, transport check wafers, dummy wafers, etc.

[0022] The object to be polished according to the present invention may contain other materials in addition to the polycrystalline silicon film, silicon nitride film, and silicon oxide film. Examples of other materials include silicon carbonitride (Si x C y N z ), doped polycrystalline silicon (doped polysilicon), undoped amorphous silicon (undoped amorphous silicon), metal, SiGe, etc.

[0023] Examples of films containing silicon oxide include TEOS (Tetraethyl Orthosilicate) type silicon oxide films (hereinafter simply referred to as "TEOS films") produced using tetraethyl orthosilicate as a precursor, HDP (High Density Plasma) films, USG (Undoped Silicate Glass) films, PSG (Phosphorus Silicate Glass) films, BPSG (Boron-Phospho Silicate Glass) films, and RTO (Rapid Thermal Oxidation) films.

[0024] Examples of films containing metal include tungsten (W) films, titanium nitride (TiN) films, ruthenium (Ru) films, platinum (Pt) films, silver (Ag) films, gold (Au) films, hafnium (Hf) films, cobalt (Co) films, palladium (Pd), iridium (Ir), osmium (Os), nickel (Ni) films, copper (Cu) films, aluminum (Al) films, and tantalum (Ta) films.

[0025] Furthermore, the shape of the object to be polished is not particularly limited. In one embodiment of the present invention, the polishing composition can be preferably used for polishing an object to be polished having a flat surface, such as a plate-like or polyhedral shape.

[0026] [Abrasive grain] The polishing composition of the present invention contains abrasive grains. The abrasive grains contained in the polishing composition of the present invention have a negative zeta potential. When the zeta potential of the abrasive grains is 0 mV or positive, the polishing rate for polycrystalline silicon films decreases, or the polishing rate for silicon nitride films or silicon oxide films increases, resulting in a lower polishing rate for polycrystalline silicon films compared to the polishing rate for silicon nitride films or silicon oxide films (lower polishing selectivity for polycrystalline silicon). The abrasive grains are preferably anion-modified silica (silica having anionic groups), and more preferably anion-modified colloidal silica (colloidal silica having anionic groups). The abrasive grains may be used alone or in combination of two or more types. Furthermore, commercially available products or synthetic products may be used as the abrasive grains.

[0027] The polishing composition of the present invention preferably contains anion-modified colloidal silica as abrasive grains. The anion-modified colloidal silica is colloidal silica whose surface is modified with anionic groups, and in the polishing composition, has the effect of mechanically polishing an object to be polished.

[0028] Preferred examples of anion-modified colloidal silica include colloidal silica having anionic groups, such as carboxyl groups, sulfonic acid groups, phosphonic acid groups, and aluminate groups, immobilized on the surface. There are no particular limitations on the method for producing colloidal silica having such anionic groups, and examples include a method of reacting colloidal silica with a silane coupling agent having an anionic group at its terminal.

[0029] As a specific example, sulfonic acid groups can be immobilized on colloidal silica by the method described in "Sulfonic acid-functionalized silica through thiol groups," Chem. Commun. 246-247 (2003). Specifically, a silane coupling agent having a thiol group, such as 3-mercaptopropyltrimethoxysilane, is coupled to colloidal silica, and then the thiol group is oxidized with hydrogen peroxide to obtain colloidal silica with sulfonic acid groups immobilized on the surface (sulfonic acid-modified colloidal silica).

[0030] Carboxy groups can be immobilized on colloidal silica by, for example, the method described in "Novel Silane Coupling Agents Containing a Photolabile 2-Nitrobenzyl Ester for Introduction of a Carboxy Group on the Surface of Silica Gel," Chemistry Letters, 3, 228-229 (2000). Specifically, colloidal silica with carboxy groups immobilized on the surface (carboxylic acid-modified colloidal silica) can be obtained by coupling a silane coupling agent containing a photolabile 2-nitrobenzyl ester to colloidal silica and then irradiating it with light.

[0031] The lower limit of the zeta potential of the abrasive grains in the polishing composition is preferably -50mV or more, more preferably -45mV or more, even more preferably -40mV or more, particularly preferably -35mV or more, and most preferably -30mV or more.The upper limit of the zeta potential of the abrasive grains in the polishing composition is preferably -1mV or less, more preferably -5mV or less, even more preferably -10mV or less, particularly preferably -15mV or less, and most preferably -20mV or less.That is, the zeta potential of the abrasive grains in the polishing composition is preferably -50mV or more and -1mV or less, more preferably -45mV or more and -5mV or less, even more preferably -40mV or more and -10mV or less, particularly preferably -35mV or more and -15mV or less, and most preferably -30mV or more and -20mV or less.

[0032] Abrasive grains having the above-described zeta potential can polish a polycrystalline silicon film at a higher polishing rate, and the polishing rate for a polycrystalline silicon film is higher than the polishing rate for a silicon nitride film or a silicon oxide film (the polishing selectivity for polycrystalline silicon is higher).

[0033] The average primary particle size of the abrasive grains is preferably 1 nm or more, more preferably 3 nm or more, and even more preferably 5 nm or more. As the average primary particle size of the abrasive grains increases, the polishing rate for polycrystalline silicon films increases. Furthermore, the average primary particle size of the abrasive grains is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 30 nm or less. As the average primary particle size of the abrasive grains decreases, the polishing rate for polycrystalline silicon films becomes higher compared to the polishing rate for silicon nitride films or silicon oxide films (the polishing selectivity for polycrystalline silicon becomes higher).

[0034] That is, the average primary particle size of the abrasive grains is preferably 1 nm or more and 100 nm or less, more preferably 3 nm or more and 50 nm or less, and even more preferably 5 nm or more and 30 nm or less. The average primary particle size of the abrasive grains can be calculated, for example, based on the specific surface area (SA) of the abrasive grains calculated by the BET method and the density of the abrasive grains.

[0035] The average secondary particle diameter of the abrasive grains is preferably 15 nm or more, more preferably 20 nm or more, and even more preferably 25 nm or more. As the average secondary particle diameter of the abrasive grains increases, the resistance during polishing decreases, enabling stable polishing of polycrystalline silicon films. The average secondary particle diameter of the abrasive grains is preferably 200 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less. As the average secondary particle diameter of the abrasive grains decreases, the surface area per unit mass of the abrasive grains increases, increasing the frequency of contact with the workpiece to be polished and further improving the polishing rate of the polycrystalline silicon film. That is, the average secondary particle diameter of the abrasive grains is preferably 15 nm or more and 200 nm or less, more preferably 20 nm or more and 150 nm or less, and even more preferably 25 nm or more and 100 nm or less. The average secondary particle diameter of the abrasive grains can be measured, for example, by dynamic light scattering, such as laser diffraction scattering. Specifically, values ​​measured by the method described in the Examples are used.

[0036] The ratio of the average secondary particle size to the average primary particle size of the abrasive grains (average secondary particle size / average primary particle size, hereinafter also referred to as "average degree of association") is 3.0 or more and 6.0 or less. If the average degree of association of the abrasive grains is less than 3.0, the abrasive grains tend to roll on the workpiece, escaping from between the polishing pad and the workpiece, resulting in inefficient polishing and a reduced polishing rate for the polycrystalline silicon film. If the average degree of association of the abrasive grains exceeds 6.0, the abrasive grains tend to remain on the surface of the workpiece, increasing the polishing rate for the silicon nitride film or silicon oxide film and decreasing the polishing rate for the polycrystalline silicon film relative to the polishing rate for the silicon nitride film or silicon oxide film (polishing selectivity for the polycrystalline silicon film). The average degree of association of the abrasive grains is preferably 3.5 or more, more preferably 3.6 or more, even more preferably 3.7 or more, particularly preferably 3.8 or more, and most preferably 4.0 or more. As the average degree of association of the abrasive grains increases, the polishing rate of the polycrystalline silicon film increases. The average degree of association of the abrasive grains is preferably 5.9 or less, more preferably 5.8 or less, even more preferably 5.5 or less, particularly preferably 5.0 or less, and most preferably 4.8 or less. As the average degree of association of the abrasive grains decreases, the polishing rate of the polycrystalline silicon film becomes higher than the polishing rate of the silicon nitride film or silicon oxide film (the polishing selectivity of polycrystalline silicon becomes higher). That is, the average degree of association of the abrasive grains is preferably 3.5 or more and 5.9 or less, more preferably 3.6 or more and 5.8 or less, even more preferably 3.7 or more and 5.5 or less, particularly preferably 3.8 or more and 5.0 or less, and most preferably 4.0 or more and 4.8 or less.

[0037] The average degree of association of the abrasive grains can be obtained by dividing the average secondary particle size of the abrasive grains by the average primary particle size of the abrasive grains.

[0038] The shape of the primary particles of the abrasive grains is not particularly limited and may be spherical or non-spherical. Specific examples of non-spherical shapes include polygonal prisms such as triangular prisms and quadrangular prisms, cylinders, bale-shaped cylinders in which the center is more bulging than the ends, doughnut-shaped discs with a central hole, plate-shaped discs, cocoon-shaped discs with a central constriction, confetti-shaped discs with multiple protrusions on the surface, and rugby ball-shaped discs, and are not particularly limited.

[0039] The shape of the secondary particles of the abrasive grains is not particularly limited, and may be peanut-shaped, with two primary particles of the abrasive grains connected in parallel, or bead-shaped, with three or more primary particles connected in parallel, or a three-dimensional spherical shape with three or more primary particles integrated together, or a polygonal shape with three or more primary particles integrated together (e.g., triangular, rectangular, rhombic, hexagonal, etc.). Of these, the bead-shaped shape is preferred from the viewpoint of achieving a good balance between the polishing speed for the polycrystalline silicon film and the polishing speed for the silicon nitride film or silicon oxide film.

[0040] The size of the abrasive grains (average primary particle diameter, average secondary particle diameter, aspect ratio, primary particle shape, secondary particle shape, etc.) can be appropriately controlled by selecting the manufacturing method of the abrasive grains, etc.

[0041] In this specification, the zeta potential of the abrasive grains is a value measured by the method described in the Examples. The zeta potential of the abrasive grains can be adjusted by the amount of anionic groups in the abrasive grains, the pH of the polishing composition, etc.

[0042] In the polishing composition of the present invention, the abrasive grains may be used alone or in combination of two or more kinds. In addition, the abrasive grains to be used may be commercially available products or synthetic products.

[0043] The content (concentration) of abrasive grains in the polishing composition is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, even more preferably 0.5% by mass or more, and particularly preferably more than 0.5% by mass, based on the total mass of the polishing composition. The upper limit of the content (concentration) of abrasive grains in the polishing composition is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 4% by mass or less, and particularly preferably less than 4% by mass, based on the total mass of the polishing composition. That is, the content (concentration) of abrasive grains in the polishing composition is preferably 0.1% by mass or more and 10% by mass or less, more preferably 0.2% by mass or more and 5% by mass or less, even more preferably 0.5% by mass or more and 4% by mass or less, and particularly preferably more than 0.5% by mass but less than 4% by mass, based on the total mass of the polishing composition. In one embodiment, the content (concentration) of abrasive grains in the polishing composition is 0.01% by mass or more and 3.0% by mass or less.

[0044] When the content of the abrasive grains is within this range, the polishing rate for the polycrystalline silicon film is higher than the polishing rate for the silicon nitride film or the silicon oxide film (the polishing selectivity for polycrystalline silicon is higher). When the polishing composition contains two or more types of abrasive grains, the content of the abrasive grains refers to the total amount of these.

[0045] The polishing composition of the present invention may further contain abrasive particles other than anion-modified silica, as long as the abrasive particles have a negative zeta potential in the polishing composition, within a range that does not impair the effects of the present invention. Such other abrasive particles may be inorganic particles, organic particles, or organic-inorganic composite particles. Specific examples of inorganic particles include unmodified silica, particles made of metal oxides such as alumina, ceria, and titania, silicon nitride particles, silicon carbide particles, and boron nitride particles. Specific examples of organic particles include polymethyl methacrylate (PMMA) particles.

[0046] [Amine oxide compounds] The polishing composition of the present invention contains an amine oxide compound represented by the following formula (1).

[0047] [ka]

[0048] In formula (1), R 1 ~R 3 are each independently an alkyl group having 1 to less than 14 carbon atoms, where R 1 ~R 3 At least one of them is an alkyl group having more than 8 and less than 14 carbon atoms. The alkyl group having 1 or more and less than 14 carbon atoms may be a linear alkyl group, branched alkyl group, or cyclic alkyl group having 1 or more and less than 14 carbon atoms, but a linear alkyl group having 1 or more and less than 14 carbon atoms is preferred.

[0049] Specific examples of alkyl groups having 1 or more and less than 14 carbon atoms include, for example, a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tet-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a 2-ethylhexyl group, a hexyl group, a heptyl group, an octyl group, a 3,7-dimethyloctyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group (a lauryl group), and a tridecyl group.

[0050] Here, in formula (1), R 1 ~R 3at least one of the three alkyl groups is an alkyl group having more than 8 and less than 14 carbon atoms. That is, in the amine oxide compound according to the present invention, at least one of the three alkyl groups has more than 8 and less than 14 carbon atoms. When the amine oxide compound has at least one alkyl group having more than 8 and less than 14 carbon atoms, it can more easily act on the polycrystalline silicon film and improve the polishing rate of the polycrystalline silicon film. The alkyl groups other than the alkyl group having more than 8 and less than 14 carbon atoms may be alkyl groups having 1 to 8 carbon atoms. The amine oxide compound is required to have at least one alkyl group having more than 8 and less than 14 carbon atoms, and may have two or three alkyl groups having more than 8 and less than 14 carbon atoms, but preferably has only one alkyl group having more than 8 and less than 14 carbon atoms.

[0051] Examples of the alkyl group having more than 8 and less than 14 carbon atoms include a nonyl group, a decyl group, an undecyl group, a dodecyl group (a lauryl group), a tridecyl group, etc. The alkyl group having more than 8 and less than 14 carbon atoms is preferably an alkyl group having from 9 to 13 carbon atoms, more preferably an alkyl group having from 10 to 12 carbon atoms, and particularly preferably an alkyl group having 10 or 12 carbon atoms.

[0052] In one embodiment, the amine oxide compound has only one alkyl group having more than 8 but less than 14 carbon atoms. Thus, this form of amine oxide compound has one alkyl group having more than 8 but less than 14 carbon atoms and two alkyl groups having from 1 to 8 carbon atoms. That is, in one embodiment, in formula (1), R 1 and R 2 are each independently an alkyl group having 1 to 8 carbon atoms, and R 3 is an alkyl group having more than 8 but less than 14 carbon atoms.

[0053] In one embodiment, the amine oxide compound has three alkyl groups having more than 8 but less than 14 carbon atoms. That is, in one embodiment, in formula (1), R 1 ~R 3 are each independently an alkyl group having more than 8 and less than 14 carbon atoms.

[0054] In one embodiment, the amine oxide compound has two alkyl groups having more than 8 but less than 14 carbon atoms and one alkyl group having 1 to 8 carbon atoms. That is, in one embodiment, in formula (1), R 1 and R 2 are each independently an alkyl group having more than 8 but less than 14 carbon atoms, and R 3 is an alkyl group having 1 to 8 carbon atoms.

[0055] In a preferred embodiment, the amine oxide compound has one alkyl group having more than 8 and less than 14 carbon atoms and two alkyl groups having 1 or more and 8 or less carbon atoms. When the amine oxide compound has the above structure, a good balance is achieved between the polishing rate for the polycrystalline silicon film and the polishing rate for the silicon nitride film or silicon oxide film.

[0056] Specific examples of the amine oxide compound include decyl dimethyl amine oxide, methyl didecyl amine oxide, decyl diethyl amine oxide, ethyl didecyl amine oxide, decyl dipropyl amine oxide, propyl didecyl amine oxide, dodecyl dimethyl amine oxide, methyl didodecyl amine oxide, dodecyl diethyl amine oxide, ethyl didodecyl amine oxide, dodecyl dipropyl amine oxide, propyl didodecyl amine oxide, tridecyl dimethyl amine oxide, methyl ditridecyl amine oxide, tridecyl diethyl amine oxide, ethyl ditridecyl amine oxide, tri(tridecyl) amine oxide, and decyl di(tridecyl) amine oxide. Among these, the amine oxide compound is preferably decyldimethylamine oxide, methyldidecylamine oxide, decyldiethylamine oxide, ethyldidecylamine oxide, dodecyldimethylamine oxide, methyldidodecylamine oxide, dodecyldiethylamine oxide, or ethyldidodecylamine oxide, from the viewpoint of the polishing selectivity of the polycrystalline silicon film. The amine oxide compound is more preferably at least one of decyldimethylamine oxide and dodecyldimethylamine oxide.

[0057] In the polishing composition of the present invention, the amine oxide compound may be used alone or in combination of two or more kinds. In addition, the amine oxide compound may be a commercially available product or a synthetic product.

[0058] The content (concentration) of the amine oxide compound in the polishing composition is not particularly limited, but is preferably 0.001% by mass or more, more preferably 0.002% by mass or more, even more preferably 0.005% by mass or more, particularly preferably 0.01% by mass or more, and most preferably 0.03% by mass or more, relative to the total mass of the polishing composition. The upper limit of the content (concentration) of the amine oxide compound in the polishing composition is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass or less, particularly preferably 0.2% by mass or less, and most preferably 0.1% by mass or less, relative to the total mass of the polishing composition. That is, the content (concentration) of the amine oxide compound is preferably 0.001% by mass or more and 5% by mass or less, more preferably 0.002% by mass or more and 1% by mass or less, even more preferably 0.005% by mass or more and 0.5% by mass or less, particularly preferably 0.01% by mass or more and 0.2% by mass or less, and most preferably 0.03% by mass or less and 0.1% by mass or less, relative to the total mass of the polishing composition. In one embodiment, the content (concentration) of the amine oxide compound in the polishing composition is 0.01% by mass or more and 0.1% by mass or less.

[0059] When the content (concentration) of the amine oxide compound is within this range, the polishing rate for a polycrystalline silicon film is higher than the polishing rate for a silicon nitride film or a silicon oxide film (the polishing selectivity for polycrystalline silicon is higher). When the polishing composition contains two or more amine oxide compounds, the content (concentration) of the amine oxide compound refers to the total amount thereof.

[0060] [Compounds having a nitrogen atom and a phosphonic acid group] The polishing composition of the present invention may further contain a compound having a nitrogen atom and a phosphonic acid group, which can embrittle the polycrystalline silicon film, further improve the polishing rate of the polycrystalline silicon film, and further improve the polishing selectivity of polycrystalline silicon.

[0061] The compound having a nitrogen atom and a phosphonic acid group is, for example, at least one selected from the group consisting of nitrilotrismethylenephosphonic acid or a salt thereof, alendronic acid or a salt thereof trihydrate, alendronic acid or a salt thereof, (1-aminoethyl)phosphonic acid or a salt thereof, N,N,N,N-ethylenediaminetetrakis(methylenephosphonic acid) or a salt thereof, and glycine N,N-bis(methylenephosphonic acid) or a salt thereof. Among these, nitrilotrismethylenephosphonic acid or a salt thereof, and N,N,N,N-ethylenediaminetetrakis(methylenephosphonic acid) or a salt thereof are preferred.

[0062] In the polishing composition of the present invention, the compound having a nitrogen atom and a phosphonic acid group may be used alone or in combination of two or more kinds. In addition, the compound having a nitrogen atom and a phosphonic acid group may be a commercially available product or a synthetic product.

[0063] The content (concentration) of the compound having nitrogen atom and phosphonic acid group in the polishing composition is not particularly limited, but is preferably 0.001 mass% or more, more preferably 0.002 mass% or more, even more preferably 0.005 mass% or more, particularly preferably 0.01 mass% or more, and most preferably 0.03 mass% or more, based on the total mass of the polishing composition.In addition, the upper limit of the content (concentration) of the compound having nitrogen atom and phosphonic acid group in the polishing composition is preferably 5 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less, particularly preferably 0.2 mass% or less, and most preferably 0.1 mass% or less, based on the total mass of the polishing composition. That is, the content (concentration) of the compound having a nitrogen atom and a phosphonic acid group is preferably 0.001% by mass or more and 5% by mass or less, more preferably 0.002% by mass or more and 1% by mass or less, even more preferably 0.005% by mass or more and 0.5% by mass or less, particularly preferably 0.01% by mass or more and 0.2% by mass or less, and most preferably 0.03% by mass or less and 0.1% by mass or less, based on the total mass of the polishing composition. In one embodiment, the content (concentration) of the compound having a nitrogen atom and a phosphonic acid group in the polishing composition is 0.01% by mass or more and 0.1% by mass or less.

[0064] [pH and pH adjusters] The pH of the polishing composition of the present invention is greater than 5 and less than 10. When the pH of the polishing composition is 5 or less, the abrasive grains in the polishing composition have low adsorption to the object to be polished, resulting in a decrease in the polishing rate of the polycrystalline silicon film. When the pH of the polishing composition exceeds 10, the polishing rate of the silicon nitride film and the silicon oxide film increases, resulting in a decrease in the polishing selectivity of the polycrystalline silicon. The pH of the polishing composition is preferably 5.5 or higher, more preferably 5.8 or higher, even more preferably 6.0 or higher, particularly preferably 6.5 or higher, and most preferably 6.8 or higher. The pH of the polishing composition is preferably 9.8 or lower, more preferably 9.5 or lower, even more preferably 8.0 or lower, particularly preferably 7.8 or lower, and most preferably 7.5 or lower. That is, the pH of the polishing composition is preferably 5.5 or more and 9.8 or less, more preferably 5.8 or more and 9.5 or less, even more preferably 6.0 or more and 8.0 or less, particularly preferably 6.5 or more and 7.8 or less, and most preferably 6.8 or more and 7.5 or less. In one embodiment, the pH of the polishing composition is 6 or more and less than 9. When the pH of the polishing composition is in this range, the polishing rate of a polycrystalline silicon film is higher than the polishing rate of a silicon nitride film or a silicon oxide film (the polishing selectivity of polycrystalline silicon is higher).

[0065] The polishing composition of the present invention may contain a pH adjuster to adjust the pH to more than 5 but not more than 10. Examples of pH adjusters include inorganic acids, organic acids, and alkalis. These may be used alone or in combination of two or more.

[0066] Specific examples of inorganic acids that can be used as pH adjusters include hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid. Among these, hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid are preferred, and nitric acid is more preferred. By using nitric acid as a pH adjuster, the polishing selectivity for polycrystalline silicon film can be improved, and the polishing rate for polycrystalline silicon film can be suitably improved.

[0067] Specific examples of organic acids that can be used as pH adjusters include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diglycolic acid, 2-furancarboxylic acid, 2,5-furandicarboxylic acid, 3-furancarboxylic acid, 2-tetrahydrofurancarboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, phenoxyacetic acid, methanesulfonic acid, ethanesulfonic acid, 10-camphorsulfonic acid, and isethionic acid.

[0068] Instead of or in combination with inorganic or organic acids, salts such as alkali metal salts of inorganic or organic acids may be used as pH adjusters. When a weak acid and a strong base, a strong acid and a weak base, or a weak acid and a weak base are combined, a pH buffering effect can be expected.

[0069] Specific examples of alkalis that can be used as pH adjusters include ammonia, hydroxides of Group 1 elements (e.g., sodium hydroxide, potassium hydroxide), hydroxides of Group 2 elements (e.g., barium hydroxide), quaternary ammonium hydroxides (e.g., tetramethylammonium hydroxide), and salts thereof. Examples of salts include carbonates, bicarbonates, sulfates, acetates, and the like. Of these, ammonia and hydroxides of Group 1 elements are preferred, and ammonia is more preferred. By using ammonia as a pH adjuster, the polishing selectivity for polycrystalline silicon films can be improved, and the polishing rate for polycrystalline silicon films can be suitably improved.

[0070] In one embodiment, the polishing composition of the present invention further contains one or more pH adjusters selected from nitric acid and ammonia, which can improve the polishing selectivity for the polycrystalline silicon film and suitably improve the polishing rate for the polycrystalline silicon film.

[0071] The content of the pH adjuster can be appropriately adjusted within the range in which the effects of the present invention are exhibited. The pH of the polishing composition can be measured, for example, with a pH meter (for example, a pH meter (model: LAQUA) manufactured by Horiba, Ltd.).

[0072] [Dispersion medium] The polishing composition of the present invention preferably contains a dispersion medium for dispersing each component. Examples of dispersion mediums include water; alcohols such as methanol, ethanol, and ethylene glycol; ketones such as acetone; and mixtures thereof. Of these, water is preferred as the dispersion medium. That is, according to a preferred embodiment of the present invention, the dispersion medium contains water. According to a more preferred embodiment of the present invention, the dispersion medium consists essentially of water. Note that the above term "substantially" means that a dispersion medium other than water may be included as long as the effects of the present invention can be achieved. More specifically, the dispersion medium preferably consists of 90% by mass to 100% by mass of water and 0% by mass to 10% by mass of a dispersion medium other than water, more preferably 99% by mass to 100% by mass of water and 0% by mass to 1% by mass of a dispersion medium other than water. Most preferably, the dispersion medium is water.

[0073] From the viewpoint of not inhibiting the action of the components contained in the polishing composition, the dispersion medium is preferably water containing as few impurities as possible. Specifically, pure water or ultrapure water, which has been subjected to removal of impurity ions with an ion exchange resin and then passed through a filter to remove foreign matter, or distilled water is more preferred.

[0074] [Other ingredients] The polishing composition of the present invention may further contain known additives that can be used in polishing compositions, such as complexing agents, preservatives, antifungal agents, oxidizing agents, surfactants, water-soluble polymers, and solubilizing agents, within limits that do not impair the effects of the present invention. The polishing composition of the present invention has a pH of greater than 5 and equal to or less than 10. For this reason, it is more preferable that the polishing composition contain an antifungal agent. That is, in one embodiment of the present invention, the polishing composition is substantially composed of abrasive grains, an amine oxide compound, a dispersing medium, and at least one selected from the group consisting of a compound having a nitrogen atom and a phosphonic acid group, a pH adjuster, and an antifungal agent. In one embodiment of the present invention, the polishing composition is substantially composed of abrasive grains, an amine oxide compound, a dispersing medium, and at least one selected from the group consisting of a compound having a nitrogen atom and a phosphonic acid group, a pH adjuster, and an antifungal agent. Here, the phrase "the polishing composition is substantially composed of at least one selected from the group consisting of abrasive grains, an amine oxide compound, a dispersing medium, and a compound having a nitrogen atom and a phosphonic acid group, a pH adjuster, and an anti-fungal agent" means that the total content of at least one selected from the group consisting of abrasive grains, an amine oxide compound, a dispersing medium, a compound having a nitrogen atom and a phosphonic acid group, a pH adjuster, and an anti-fungal agent exceeds 99% by mass (upper limit: 100% by mass) relative to the polishing composition. Preferably, the polishing composition is composed of abrasive grains, an amine oxide compound, a dispersing medium, a compound having a nitrogen atom and a phosphonic acid group, a pH adjuster, and an anti-fungal agent (the total content = 100% by mass).

[0075] The antifungal agent (preservative) is not particularly limited and can be appropriately selected depending on the desired use and purpose. Specific examples include isothiazolin-based preservatives such as 1,2-benzisothiazol-3(2H)-one (BIT), 2-methyl-4-isothiazolin-3-one, and 5-chloro-2-methyl-4-isothiazolin-3-one, and phenoxyethanol.

[0076] [Polishing method and semiconductor substrate manufacturing method] The polishing composition of the present invention is suitable for use in polishing an object to be polished, for example, containing polycrystalline silicon and at least one of silicon nitride and silicon oxide. Therefore, the present invention provides a polishing method comprising polishing an object to be polished with the polishing composition of the present invention. The present invention also provides a method for producing a semiconductor substrate comprising polishing a semiconductor substrate with the polishing composition of the present invention. The present invention also provides a method for producing a semiconductor substrate comprising polishing a semiconductor substrate by the polishing method of the present invention.

[0077] As the polishing device, a general polishing device can be used, which is equipped with a holder for holding a substrate or the like having an object to be polished, a motor whose rotation speed can be changed, and a polishing platen onto which a polishing pad (polishing cloth) can be attached.

[0078] The polishing pad may be made of any material, including ordinary nonwoven fabric, polyurethane, porous fluororesin, etc. The polishing pad is preferably provided with grooves to allow the polishing liquid to accumulate.

[0079] Regarding the polishing conditions, for example, the rotation speed of the polishing platen and carrier was 10 rpm (0.17 s -1 ) or more 500rpm (8.33s -1 The pressure (polishing pressure) applied to the substrate having the object to be polished is preferably 0.5 psi (3.4 kPa) or more and 10 psi (68.9 kPa).

[0080] The method for supplying the polishing composition to the polishing pad is not particularly limited, and for example, a method of continuously supplying the polishing composition using a pump, etc. There is no limit to the amount of the polishing composition supplied, but it is preferable that the surface of the polishing pad is always covered with the polishing composition of the present invention.

[0081] After polishing, the substrate is washed with running water, and water droplets adhering to the substrate are removed by a spin dryer or the like, followed by drying, to obtain a substrate having a metal-containing layer.

[0082] The polishing composition of the present invention may be a one-component type or a multi-component type such as a two-component type. The polishing composition of the present invention may also be prepared by diluting the stock solution of the polishing composition with a diluent such as water, for example, 3 times or more (or, for example, 5 times or more).

[0083] [Polishing speed] When polishing is performed using the polishing composition of the present invention, the polishing rate for polycrystalline silicon films is preferably 1500 Å / min to 7000 Å / min, more preferably 2000 Å / min to 6800 Å / min, even more preferably 2200 Å / min to 6500 Å / min, and particularly preferably 2500 Å / min to 6000 Å / min. When polishing is performed using the polishing composition of the present invention, the polishing rate for silicon nitride films and / or silicon oxide films is preferably 150 Å / min or less, more preferably 100 Å / min or less, even more preferably 50 Å / min or less, and particularly preferably 40 Å / min or less. There is no particular lower limit to the polishing rate for silicon nitride films and / or silicon oxide films, but in practice it is 5 Å / min or more.

[0084] [Polishing selectivity] When the polishing composition of the present invention is used to polish an object containing polycrystalline silicon and silicon nitride, the ratio of the polishing rate of polycrystalline silicon to the polishing rate of silicon nitride (polycrystalline silicon / silicon nitride) is preferably 50 or more, more preferably 60 or more, even more preferably 70 or more, particularly preferably 75 or more, and most preferably 80 or more. When the polishing composition of the present invention is used to polish an object containing polycrystalline silicon and silicon oxide, the ratio of the polishing rate of polycrystalline silicon to the polishing rate of silicon oxide (polycrystalline silicon / silicon oxide) is preferably 40 or more, more preferably 50 or more, even more preferably 55 or more, particularly preferably 60 or more, and most preferably 70 or more.

[0085] Although the embodiments of the present invention have been described in detail, it is clear that this is by way of illustration and example only and not of limitation, and that the scope of the present invention should be interpreted by the appended claims.

[0086] The present invention encompasses the following aspects and configurations.

[0087] [1] A polishing composition comprising an abrasive grain and an amine oxide compound, and having a pH of more than 5 and not more than 10, the abrasive grains have a negative zeta potential in the polishing composition and an average degree of association of 3.0 or more and 6.0 or less; The amine oxide compound has the following formula (1):

[0088] [ka]

[0089] In formula (1), R 1 ~R 3 are each independently an alkyl group having 1 to 12 carbon atoms, 1 ~R 3 At least one of the groups is an alkyl group having more than 8 and less than 14 carbon atoms. A polishing composition represented by the formula:

[0090] [2] The polishing composition according to [1] above, wherein the amine oxide compound has only one alkyl group having more than 8 and less than 14 carbon atoms.

[0091] [3] The polishing composition according to [1] or [2] above, wherein the amine oxide compound is at least one of decyldimethylamine oxide and dodecyldimethylamine oxide.

[0092] [4] The polishing composition according to any one of the above [1] to [3], further comprising a compound having a nitrogen atom and a phosphonic acid group.

[0093] [5] The polishing composition according to any one of [1] to [4] above, wherein the compound having a nitrogen atom and a phosphonic acid group is at least one selected from the group consisting of nitrilotrismethylenephosphonic acid or a salt thereof, alendronic acid or a salt thereof trihydrate, alendronic acid or a salt thereof, (1-aminoethyl)phosphonic acid or a salt thereof, N,N,N,N-ethylenediaminetetrakis(methylenephosphonic acid) or a salt thereof, and glycine N,N-bis(methylenephosphonic acid) or a salt thereof.

[0094] [6] The polishing composition according to any one of the above [1] to [5], wherein the abrasive grains are anion-modified colloidal silica.

[0095] [7] The polishing composition according to any one of the above [1] to [6], which has a pH of 6 or more and less than 9.

[0096] [8] The polishing composition according to any one of the above [1] to [7], further comprising one or more pH adjusters selected from nitric acid and ammonia.

[0097] [9] The polishing composition according to any one of the above [1] to [8], which is used for polishing an object to be polished, which comprises polycrystalline silicon and at least one of silicon nitride and silicon oxide.

[0098]

[10] The polishing composition according to [9] above, which is used for polishing an object containing polycrystalline silicon and silicon nitride, and has a ratio of the polishing rate of the polycrystalline silicon to the polishing rate of the silicon nitride (polishing rate of polycrystalline silicon / polishing rate of silicon nitride) of 80 or more.

[0099]

[11] The polishing composition according to [9] above, which is used for polishing an object containing polycrystalline silicon and silicon oxide, and has a ratio of the polishing rate of the polycrystalline silicon to the polishing rate of the silicon oxide (polishing rate of polycrystalline silicon / polishing rate of silicon oxide) of 60 or more.

[0100]

[12] A polishing method comprising the step of polishing an object containing polycrystalline silicon and at least one of silicon nitride and silicon oxide, using the polishing composition according to any one of [1] to

[11] above.

[0101]

[13] A method for producing a semiconductor substrate, comprising a step of polishing a semiconductor substrate containing polycrystalline silicon and at least one of silicon nitride and silicon oxide by the polishing method according to

[12] above. [Example]

[0102] The present invention will be described in more detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. Unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.

[0103] <Average primary particle size of abrasive grains> The average primary particle size of the abrasive grains was calculated from the specific surface area of ​​the silica particles measured by the BET method using a Micromeritics "Flow Sorb II 2300" and the density of the abrasive grains.

[0104] <Average secondary particle size of abrasive grains> The average secondary particle diameter of the abrasive grains was measured as the volume-average particle diameter (arithmetic mean diameter on a volume basis; Mv) using a dynamic light scattering particle diameter / particle size distribution analyzer UPA-UTI151 (manufactured by Nikkiso Co., Ltd.).

[0105] <Average degree of association of abrasive grains> The average degree of association of the abrasive grains was calculated by dividing the value of the average secondary particle size of the abrasive grains by the value of the average primary particle size of the abrasive grains.

[0106] <Zeta potential of abrasive grains> The zeta potential of the abrasive grains in the polishing composition was calculated by subjecting the polishing composition to a Zetasizer Nano manufactured by Malvern Panalytical, measuring it using the laser Doppler method (electrophoretic light scattering measurement method) at a measurement temperature of 25°C, and analyzing the obtained data using the Smoluchowski equation.

[0107] <Grain shape> The shape of the abrasive grains was analyzed by observing images of the abrasive grains using an HD-2700 scanning transmission electron microscope (Hitachi High-Tech Corporation) according to the following procedure.

[0108] After dispersing the abrasive grains in alcohol (abrasive grain concentration 0.01% by mass), the dried material was placed in a transmission electron microscope (TEM), irradiated with an electron beam at 5.0 kV, and several observation fields were photographed at magnifications from 50,000x to 200,000x.

[0109] In the TEM images taken, the shape of the abrasive grains was confirmed based on the following criteria. (Standards for abrasive grain shape) When grains with the following shapes are observed in TEM images at 50% or more by number, the abrasive grains are judged to have that shape. Beaded: Three or more spherical abrasive grains are connected together, with the grains at the edges not connected together. Peanut-shaped: Two spherical abrasive grains are connected together.

[0110] <pH of polishing composition> The pH of the polishing composition was measured using a glass electrode hydrogen ion concentration indicator (Model No. F-23, manufactured by Horiba, Ltd.) and three-point calibration was performed using standard buffer solutions (phthalate pH buffer solution pH: 4.01 (25°C), neutral phosphate pH buffer solution pH: 6.86 (25°C), carbonate pH buffer solution pH: 10.01 (25°C)).The glass electrode was then placed in the polishing composition and the value measured after stabilizing for at least two minutes was taken as the pH value.

[0111] <Electrical Conductivity of Polishing Composition> The electrical conductivity (EC) of the polishing composition was measured using a desktop electrical conductivity meter (manufactured by Horiba, Ltd., model number: DS-71 LAQUA (registered trademark)).

[0112] [Preparation of abrasive grains] [Preparation of abrasive grains 1 to 3] As the anion-modified colloidal silica, anion-modified colloidal silica of abrasive grains 1 to 3 was prepared by the method described in "Sulfonic acid-functionalized silica through quantitative oxidation of thiol groups", Chem. Commun. 246-247 (2003).

[0113] Abrasive grain 1: Average primary particle size: 22 nm, average secondary particle size: 80 nm, average degree of association: 3.6 Abrasive grain 2: Average primary particle size: 11 nm, average secondary particle size: 50 nm, average degree of association: 4.5 Abrasive grain 3: Average primary particle size: 35 nm, average secondary particle size: 70 nm, average degree of association: 2.

[0114] [Preparation of abrasive grain 4] In the same manner as described in Example 1 of JP 2005-162533 A, cation-modified colloidal silica was prepared as abrasive grain 4 (average primary particle size: 22 nm, average secondary particle size: 80 nm, average degree of association: 3.6) using γ-aminopropyltriethoxysilane (APTES) as a silane coupling agent at a concentration of 0.113 mmol (0.113 mM) per 1 L of an aqueous dispersion of silica sol (silica concentration = 20 mass %).

[0115] [Preparation of Polishing Composition] Example 1 The abrasive grains 1 (anion-modified colloidal silica) obtained above were added to pure water as a dispersion medium at room temperature (25°C) to a final concentration of 2% by mass, and 2-methyl-4-isothiazolin-3-one (manufactured by The Dow Chemical Company) was added as an antifungal agent to a final concentration of 0.014 mM to obtain a mixed solution.

[0116] Thereafter, decyldimethylamine oxide (manufactured by Lion Specialty Chemical Co., Ltd.) was added as an amine oxide compound to a final concentration of 0.05% by mass, and ammonia was added as a pH adjuster to pH 9. The mixture was stirred and mixed at room temperature (25°C) for 30 minutes to prepare Polishing Composition A1. The pH of the resulting Polishing Composition A1 was measured to be 9, and the electrical conductivity was 2 mS / cm.

[0117] The zeta potential of the abrasive grains 1 (anion-modified colloidal silica) in the resulting polishing composition was measured according to the method described above and found to be -35 mV. Furthermore, the particle size of the abrasive grains 1 (anion-modified colloidal silica) in the polishing composition was similar to that of the abrasive grains 1 (anion-modified colloidal silica) used.

[0118] (Examples 2 to 5, Comparative Examples 1 to 8) Polishing compositions A2 to A5 of Examples 2 to 5 and polishing compositions B1 to B8 of Comparative Examples 1 to 8 were prepared in the same manner as in Example 1, except that the type and concentration of each component, as well as the pH, were changed as shown in Table 1 below. The compound having a nitrogen atom and a phosphonic acid group (represented as "additive" in Table 1) was added before the addition of the pH adjuster, and the pH was adjusted with the pH adjuster after the addition. Nitrilotrismethylenephosphonic acid (product name: Chelest PH-320, manufactured by Chelest Co., Ltd.) was used as the compound having a nitrogen atom and a phosphonic acid group. The composition of each polishing composition is shown in Table 1 below. A "-" in Table 1 below indicates that the agent was not used. The pH of each polishing composition and the particle size of the abrasive grains in each polishing composition were measured, and the values ​​shown in Table 1 were obtained.

[0119] [evaluation] <Evaluation of Polishing Rate of Polishing Composition> Using each of the polishing compositions A1 to A5 and B1 to B8, the surface of each object to be polished was polished under the following conditions: The following objects to be polished (1) to (3) were prepared.

[0120] (1) Polycrystalline silicon film (poly-Si film): A silicon wafer with a 5000 Å thick polycrystalline silicon film formed on its surface. (2) Silicon nitride film (Si3N4 film): A silicon wafer (200 mm, blanket wafer) with a 2000 Å thick silicon nitride film formed on the surface. (3) Silicon oxide film (TEOS film): A silicon wafer (200 mm, blanket wafer) with a 10,000 Å thick TEOS type silicon oxide (SiO2) film formed on its surface.

[0121] (Polishing equipment and polishing conditions) Polishing equipment: Applied Materials 200mm CMP single-sided polishing equipment Mirra Polishing pad: Nitta Haas IC1010 hard polyurethane pad Polishing pressure: 4.0 psi (1 psi = 6894.76 Pa) Polishing platen rotation speed: 47 rpm Head (carrier) rotation speed: 43 rpm Supply of polishing composition: free-flowing Polishing composition supply amount: 200mL / min Polishing time: 60 seconds.

[0122] (Calculation of polishing rate) The thickness of each polished object was measured before and after polishing using an optical film thickness measuring device (ASET-f5x, manufactured by KLA-Tencor Corporation).

[0123] The polishing rate for each object was calculated by dividing the difference in film thickness before and after polishing [(thickness before polishing) - (thickness after polishing)] by the polishing time. For polycrystalline silicon films, a polishing rate of 1500 Å / min or higher is practical, with 2000 Å / min or higher being preferred. Regarding the polishing rate ratio between polycrystalline silicon films and silicon nitride films, a polishing rate of polycrystalline silicon film / polishing rate of silicon nitride film (poly-Si / Si3N4 in Table 1) of 50 or higher is practical. Regarding the polishing rate ratio between polycrystalline silicon films and silicon oxide films, a polishing rate of polycrystalline silicon film / polishing rate of silicon oxide film (poly-Si / TEOS in Table 1) of 40 or higher is practical.

[0124] The above evaluation results are also shown in Table 1. In Table 1, polycrystalline silicon films are indicated as "poly-Si", silicon nitride films are indicated as "Si3N4", and TEOS films are indicated as "SiO2".

[0125] [Table 1]

[0126] As is clear from Table 1 above, the polishing compositions of Examples have a high polishing rate for polycrystalline silicon films and can suppress the polishing rate for at least one of silicon nitride films and silicon oxide films, resulting in a high polishing rate ratio for polycrystalline silicon films. On the other hand, the polishing compositions of Comparative Examples do not provide a high polishing rate ratio for polycrystalline silicon films because the polishing rate for polycrystalline silicon films is low or the polishing rate for silicon nitride films and / or silicon oxide films is too high.

[0127] Therefore, it is clear that the polishing composition of the present invention can polish a polycrystalline silicon film at high speed, and can suppress the polishing rate of at least one of a silicon nitride film and a silicon oxide film.

[0128] The results shown in Table 1 were obtained by separately polishing an object having a polycrystalline silicon film, an object having a silicon nitride film, and an object having a silicon oxide film. However, it is expected that the same polishing speed and polishing selectivity for polycrystalline silicon as those shown in Table 1 will be obtained even when polishing an object having polycrystalline silicon and at least one of silicon nitride and silicon oxide.

Claims

1. A polishing composition comprising an abrasive grain and an amine oxide compound, the polishing composition having a pH of more than 5 and not more than 10, the abrasive grains have a negative zeta potential in the polishing composition and an average degree of association of 3.0 or more and 6.0 or less; The amine oxide compound is represented by the following formula (1): 【Chemistry 1】 In formula (1), R 1 ~R 3 are each independently an alkyl group having 1 to less than 14 carbon atoms, where R 1 ~R 3 At least one of the above is an alkyl group having more than 8 and less than 14 carbon atoms. Represented by Polishing composition.

2. The polishing composition according to claim 1 , wherein the amine oxide compound has only one alkyl group having more than 8 and less than 14 carbon atoms.

3. The polishing composition according to claim 1 or 2, wherein the amine oxide compound is at least one of decyl dimethylamine oxide and dodecyl dimethylamine oxide.

4. The polishing composition according to claim 1 or 2, further comprising a compound having a nitrogen atom and a phosphonic acid group.

5. The polishing composition according to claim 4, wherein the compound having a nitrogen atom and a phosphonic acid group is at least one selected from the group consisting of nitrilotrismethylenephosphonic acid or a salt thereof, alendronic acid or a salt thereof, alendronic acid or a salt thereof, (1-aminoethyl)phosphonic acid or a salt thereof, N,N,N,N-ethylenediaminetetrakis(methylenephosphonic acid) or a salt thereof, and glycine N,N-bis(methylenephosphonic acid) or a salt thereof.

6. 3. The polishing composition according to claim 1, wherein the abrasive grains are anion-modified colloidal silica.

7. The polishing composition according to claim 1 or 2, which has a pH of 6 or more and less than 9.

8. The polishing composition according to claim 1 or 2, further comprising one or more pH adjusters selected from nitric acid and ammonia.

9. 3. The polishing composition according to claim 1, which is used for polishing an object containing polycrystalline silicon and at least one of silicon nitride and silicon oxide.

10. Used to polish objects including polycrystalline silicon and silicon nitride, 10. The polishing composition according to claim 9, wherein the ratio of the polishing rate of the polycrystalline silicon to the polishing rate of the silicon nitride (polishing rate of the polycrystalline silicon / polishing rate of the silicon nitride) is 80 or more.

11. It is used to polish objects containing polycrystalline silicon and silicon oxide, 10. The polishing composition according to claim 9, wherein the ratio of the polishing rate of the polycrystalline silicon to the polishing rate of the silicon oxide (polishing rate of polycrystalline silicon / polishing rate of silicon oxide) is 60 or more.

12. 2. A polishing method comprising the step of polishing an object containing polycrystalline silicon and at least one of silicon nitride and silicon oxide with the polishing composition according to claim 1.

13. A method for producing a semiconductor substrate, comprising a step of polishing a semiconductor substrate containing polycrystalline silicon and at least one of silicon nitride and silicon oxide by the polishing method according to claim 12.

Citation Information

Patent Citations

  • Polishing composition, manufacturing method thereof, polishing method and method for manufacturing semiconductor substrate

    JP2018157164A

  • Surface treatment composition, method for producing the same, surface treatment method, and method for producing semiconductor substrate

    JP2020158616A

  • Polishing composition

    WO2016158324A1

  • Polishing composition, polishing composition production method, polishing method, and semiconductor substrate production method

    WO2023021963A1

  • Aqueous dispersion for chemical mechanical polishing and chemical mechanical polishing method using the same

    JP2013041992A