Adhesive composition

The use of a (meth)acrylic resin with a tackifier polymer derived from isopropenyltoluene and a high molecular weight component addresses the challenge of maintaining adhesive strength and holding power under high temperatures, enhancing performance through improved molecular binding and mobility suppression.

JP2024141123AActive Publication Date: 2024-10-10MITSUI CHEMICALS INC

Patent Information

Application Number
JP2023052603
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Adhesive compositions face challenges in maintaining adhesive strength and holding power under high temperature conditions.

Method used

Incorporating a (meth)acrylic resin with a tackifier that is a polymer containing a structural unit derived from isopropenyltoluene, having a molecular weight of 2000 or more, and ensuring a high molecular weight component content of 10% by mass or more, along with specific ratios of structural units from isopropenyltoluene and a C5 fraction.

Benefits of technology

The adhesive composition exhibits excellent adhesive strength and holding power under high temperature conditions due to the inclusion of high molecular weight components and improved compatibility with the (meth)acrylic resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141123000003
    Figure 2024141123000003
  • Figure 2024141123000004
    Figure 2024141123000004
  • Figure 2024141123000001
    Figure 2024141123000001
Patent Text Reader

Abstract

To provide an adhesive composition that exhibits superior adhesive strength and holding power in high temperature ranges.SOLUTION: An adhesive composition contains a (meth)acrylic resin and a tackifier. The tackifier is a polymer containing a structural unit derived from isopropenyl toluene. The polymer contains a high-molecular-weight component with a molecular weight of 2000 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive composition. [Background technology]

[0002] 2. Description of the Related Art It is conventionally known to add a tackifier to a pressure-sensitive adhesive composition in order to improve the adhesive strength.

[0003] As such a pressure-sensitive adhesive composition, for example, a pressure-sensitive adhesive composition containing a (meth)acrylic polymer and rosin (a tackifier resin) has been proposed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 01-016882 Summary of the Invention [Problem to be solved by the invention]

[0005] On the other hand, adhesive compositions are required to have adhesive strength and holding power in high temperature regions.

[0006] The present invention provides an adhesive composition having excellent adhesive strength and holding power in high temperature regions. [Means for solving the problem]

[0007] The present invention [1] is an adhesive composition comprising a (meth)acrylic resin and a tackifier, the tackifier being a polymer containing a structural unit derived from isopropenyl toluene, the polymer containing a high molecular weight component having a molecular weight of 2000 or more.

[0008] The present invention [2] includes the adhesive composition according to the above [1], in which the content of the high molecular weight component is 10 mass % or more relative to the polymer.

[0009] The present invention [3] includes an adhesive composition according to claim 1 or 2, wherein the polymer contains structural units derived from a C5 fraction.

[0010] The present invention [4] includes the adhesive composition described in [3] above, in which the structural units derived from isopropenyl toluene are 90 mol % or more and 99 mol % or less of the polymer, and the structural units derived from a C5 fraction are 1 mol % or more and 10 mol % or less of the polymer. Effect of the Invention

[0011] In the pressure-sensitive adhesive composition of the present invention, the tackifier is a polymer containing a structural unit derived from isopropenyl toluene. The polymer contains a high molecular weight component. Therefore, the composition has excellent adhesive strength and holding power. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a gel permeation chromatogram showing the content of high molecular weight components. [Diagram 2] 2A and 2B are schematic diagrams showing the relationship between the molecular motion of a (meth)acrylic polymer chain and a tackifier. Fig. 2A shows a case where the polymer in the tackifier does not contain a high molecular weight component. Fig. 2B shows a case where the polymer in the tackifier contains a high molecular weight component. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The adhesive composition contains a (meth)acrylic resin and a tackifier.

[0014] <(Meth)acrylic resin> The (meth)acrylic resin can be obtained, for example, as a polymer of a first polymerization component containing an alkyl (meth)acrylate ester, where (meth)acrylic refers to acrylic and / or methacrylic.

[0015] Examples of (meth)acrylic acid alkyl esters include (meth)acrylic acid alkyl esters having an alkyl moiety with 1 to 12 carbon atoms. Examples of (meth)acrylic acid alkyl esters having an alkyl moiety with 1 to 12 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate.

[0016] As the (meth)acrylic acid alkyl ester, preferably, methyl (meth)acrylate and an acrylic acid alkyl ester having 2 to 8 carbon atoms are used. As the (meth)acrylic acid alkyl ester, more preferably, butyl (meth)acrylate is used. As the (meth)acrylic acid alkyl ester, further preferably, butyl acrylate is used.

[0017] The (meth)acrylic acid alkyl esters can be used alone or in combination of two or more kinds.

[0018] The mixing ratio of the (meth)acrylic acid alkyl ester relative to 100 parts by mass of the first polymerization component is, for example, 60 parts by mass or more, preferably 70 parts by mass or more, more preferably 80 parts by mass or more, even more preferably 90 parts by mass or more, particularly preferably 95 parts by mass or more, and most preferably 99 parts by mass or more, and for example, 100 parts by mass or less, preferably 99.9 parts by mass or less.

[0019] The first polymerization component may also contain a copolymerizable monomer that is copolymerizable with the (meth)acrylic acid alkyl ester.

[0020] Examples of copolymerizable monomers include functional group-containing vinyl monomers, vinyl esters, aromatic vinyl monomers, N-substituted unsaturated carboxylic acid amides, heterocyclic vinyl compounds, vinylidene halide compounds, α-olefins, and dienes.

[0021] Examples of functional group-containing vinyl monomers include carboxy group-containing vinyl monomers, hydroxyl group-containing vinyl monomers, amino group-containing vinyl monomers, glycidyl group-containing vinyl monomers, cyano group-containing vinyl monomers, sulfonic acid group-containing vinyl monomers and salts thereof, acetoacetoxy group-containing vinyl monomers, phosphoric acid group-containing compounds, and amide group-containing vinyl monomers.

[0022] Examples of the carboxyl group-containing vinyl monomer include (meth)acrylic acid, maleic anhydride, maleic acid, fumaric acid, itaconic acid, and crotonic acid. A preferred example of the carboxyl group-containing vinyl monomer is acrylic acid.

[0023] Examples of the hydroxyl group-containing vinyl monomer include 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate. A preferred example of the hydroxyl group-containing vinyl monomer is 2-hydroxyethyl (meth)acrylate. A more preferred example of the hydroxyl group-containing vinyl monomer is 2-hydroxyethyl acrylate.

[0024] Examples of amino group-containing vinyl monomers include 2-aminoethyl (meth)acrylate, 2-(N-methylamino)ethyl (meth)acrylate, and 2-(N,N-dimethylamino)ethyl (meth)acrylate.

[0025] An example of the glycidyl group-containing vinyl monomer is glycidyl (meth)acrylate.

[0026] An example of the cyano group-containing vinyl monomer is (meth)acrylonitrile.

[0027] Examples of the sulfonic acid group-containing vinyl monomer include allyl sulfonic acid and methallyl sulfonic acid. Examples of the salts include alkali metal salts (e.g., sodium salts and potassium salts) of the sulfonic acid group-containing vinyl monomer, such as ammonium salts. Specific examples include sodium allyl sulfonate, sodium methallyl sulfonate, and ammonium methallyl sulfonate.

[0028] An example of the acetoacetoxy group-containing vinyl monomer is acetoacetoxyethyl (meth)acrylate.

[0029] An example of the phosphate group-containing compound is 2-methacryloyloxyethyl acid phosphate.

[0030] An example of the amide group-containing vinyl monomer is (meth)acrylamide.

[0031] As the functional group-containing vinyl monomer, preferably, a hydroxyl group-containing vinyl monomer is used.

[0032] Examples of vinyl esters include vinyl acetate and vinyl propionate. Of the vinyl esters, vinyl acetate is preferred.

[0033] Aromatic vinyl monomers include, for example, styrene, α-methylstyrene, and divinylbenzene.

[0034] An example of the N-substituted unsaturated carboxylic acid amide is N-methylol (meth)acrylamide.

[0035] An example of the heterocyclic vinyl compound is vinylpyrrolidone.

[0036] Examples of vinylidene halide compounds include vinylidene chloride and vinylidene fluoride.

[0037] Examples of the α-olefins include ethylene and propylene.

[0038] An example of the dienes is butadiene.

[0039] Further, the copolymerizable monomer may be a crosslinkable vinyl monomer.

[0040] Examples of crosslinkable vinyl monomers include compounds containing two or more vinyl groups. Examples of compounds containing two or more vinyl groups include methylene bis(meth)acrylamide, divinylbenzene, and polyethylene glycol chain-containing di(meth)acrylate.

[0041] As the copolymerizable monomer, preferably, a functional group-containing vinyl monomer is used.

[0042] The copolymerizable monomers can be used alone or in combination of two or more kinds.

[0043] The blending ratio of the copolymerizable monomer, relative to 100 parts by mass of the first polymerization component, is, for example, 0 parts by mass or more, preferably 0.1 parts by mass or more, and for example, 40 parts by mass or less, preferably 30 parts by mass or less, more preferably 20 parts by mass or less, even more preferably 10 parts by mass or less, particularly preferably 5 parts by mass or less, and most preferably 1 part by mass or less.

[0044] The polymerization method for the first polymerization component is not particularly limited, and a known polymerization method can be used.

[0045] As a method for polymerizing the first polymerization component, the first polymerization component is preferably radically polymerized in a solvent (e.g., ethyl acetate). In this method, for example, the first polymerization component and a polymerization initiator are mixed in a solvent and polymerized in the solvent.

[0046] The polymerization initiator is not particularly limited. Examples of the polymerization initiator include persulfates, organic peroxides, and azo compounds. Examples of the polymerization initiator include organic peroxides. Examples of the organic peroxide include benzoyl peroxide.

[0047] The mixing ratio of the polymerization initiator is appropriately set depending on the purpose and application.

[0048] The polymerization initiators can be used alone or in combination of two or more kinds.

[0049] In the above polymerization, a molecular weight regulator can be added, if necessary.

[0050] Examples of the molecular weight regulator include mercaptans, allyl compounds, and low molecular weight halogen compounds. Examples of the mercaptans include t-dodecyl mercaptan and n-dodecyl mercaptan. Examples of the allyl compounds include allyl sulfonic acid, methallyl sulfonic acid, and soda salts thereof.

[0051] The blending ratio of the molecular weight regulator is appropriately set depending on the purpose and application.

[0052] The molecular weight regulator can be used alone or in combination of two or more kinds.

[0053] The polymerization conditions are, under normal pressure, a polymerization temperature of, for example, 30° C. or more, preferably 50° C. or more, and for example, 150° C. or less, preferably 120° C. or less, and a polymerization time of, for example, 1 hour or more, preferably 2 hours or more, and for example, 30 hours or less, preferably 20 hours or less.

[0054] This gives a (meth)acrylic resin (a (meth)acrylic resin solution).

[0055] The glass transition temperature of the (meth)acrylic resin is, for example, 20° C. or less, preferably 0° C. or less, and for example, −30° C. or more.

[0056] The glass transition temperature can be calculated, for example, by the FOX formula.

[0057] The (meth)acrylic resin solution has a solids concentration of, for example, 5 mass % or more, preferably 10 mass % or more, and for example, 70 mass % or less, preferably 60 mass % or less.

[0058] The (meth)acrylic resins can be used alone or in combination of two or more kinds.

[0059] The content of the (meth)acrylic resin, relative to 100 parts by mass of the total amount of the (meth)acrylic resin and the tackifier, is, for example, 60 parts by mass or more, preferably 70 parts by mass or more, more preferably 75 parts by mass or more, and for example, 98 parts by mass or less, preferably 90 parts by mass or less, more preferably 82 parts by mass or less.

[0060] The content of the (meth)acrylic resin in the adhesive composition is, for example, 60 mass% or more, preferably 70 mass% or more, more preferably 75 mass% or more, and for example, 98 mass% or less, preferably 90 mass% or less, more preferably 82 mass% or less.

[0061] <Tackifier> The tackifier comprises structural units derived from isopropenyl toluene.

[0062] Such a polymer is formed by polymerizing a second polymerization component.

[0063] The second polymerization component contains, as an essential component, isopropenyl toluene.

[0064] The second polymerization component may also contain other components (components other than isopropenyl toluene), such as, for example, α-methyl styrene, indene, vinyl toluene, and unsaturated aliphatic hydrocarbons.

[0065] The unsaturated aliphatic hydrocarbons are components copolymerizable with isopropenyltoluene, α-methylstyrene, indene, and vinyltoluene, and examples thereof include C4 fractions and C5 fractions.

[0066] The C4 fraction is obtained by refining and / or cracking petroleum. The C4 fraction is a fraction having a boiling point range of −15° C. or more and 45° C. or less under normal pressure, and includes, for example, unsaturated aliphatic hydrocarbons having 4 carbon atoms and no conjugated double bonds, and unsaturated aliphatic hydrocarbons having 4 carbon atoms and containing conjugated double bonds.

[0067] Examples of unsaturated aliphatic hydrocarbons having 4 carbon atoms and containing no conjugated double bonds include 1-butene, isobutene, and 2-butene.

[0068] An example of an unsaturated aliphatic hydrocarbon having 4 carbon atoms and containing a conjugated double bond is 1,3-butadiene.

[0069] The C4 fraction preferably does not contain unsaturated aliphatic hydrocarbons having 4 carbon atoms which contain conjugated double bonds, and is composed of unsaturated aliphatic hydrocarbons having 4 carbon atoms which do not contain conjugated double bonds.

[0070] The C5 fraction is obtained by refining and / or cracking petroleum, and generally has a boiling point range of -15°C to 45°C under normal pressure, and includes, for example, unsaturated aliphatic hydrocarbons having 5 carbon atoms and no conjugated double bonds, and unsaturated aliphatic hydrocarbons having 5 carbon atoms and containing conjugated double bonds.

[0071] Examples of unsaturated aliphatic hydrocarbons having 5 carbon atoms and containing no conjugated double bonds include 1-pentene, 2-methyl-1-butene, 3-methyl-1-butene, and 2-pentene.

[0072] Examples of unsaturated aliphatic hydrocarbons having 5 carbon atoms and containing a conjugated double bond include isoprene, 1,3-pentadiene, and cyclopentadiene.

[0073] The C5 fraction preferably does not contain unsaturated aliphatic hydrocarbons having 5 carbon atoms which contain conjugated double bonds, and is composed of unsaturated aliphatic hydrocarbons having 5 carbon atoms which do not contain conjugated double bonds.

[0074] As the other components, preferably, unsaturated aliphatic hydrocarbons are used. As the other components, more preferably, C5 fractions are used. That is, as the polymer, more preferably, a copolymer of isopropenyl toluene and C5 fractions is used.

[0075] The other components may be used alone or in combination of two or more kinds.

[0076] In addition, all or a part of the monomers constituting the second polymer component may be derived from fossil fuels or biomass.

[0077] Fossil fuels include petroleum, coal, natural gas, shale gas, or combinations thereof.Biomass is any renewable natural source and its residues, such as from plants or animals, including fungi, yeasts, algae, and bacteria.

[0078] The polymer is then obtained by polymerizing the second polymerization component in the presence of a Friedel-Crafts catalyst.

[0079] Friedel-Crafts catalysts include, for example, phenol complexes (eg, boron trifluoride phenolate complexes).

[0080] The mixing ratio of the Friedel-Crafts catalyst is, for example, 0.01 part by mass or more and, for example, 1 part by mass or less, relative to 100 parts by mass of the second polymerization component.

[0081] As for the polymerization conditions, the polymerization temperature is, for example, −50° C. or higher and, for example, 50° C. or lower. The polymerization time is, for example, 10 minutes or longer and, for example, 10 hours or shorter.

[0082] The reaction is carried out in the presence of a solvent or without a solvent, and is preferably carried out in the presence of a solvent.

[0083] Examples of the solvent include aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, ketones, and alkyl esters. Examples of the solvent include aromatic hydrocarbons. Examples of the aromatic hydrocarbons include toluene and xylene. Examples of the aromatic hydrocarbons include toluene.

[0084] The solvents can be used alone or in combination of two or more kinds.

[0085] This gives a polymer (a polymer solution).

[0086] The solids concentration of the polymer solution is, for example, 5 mass % or more, preferably 10 mass % or more, and for example, 70 mass % or less, preferably 60 mass % or less.

[0087] In such a polymer, the constituent units derived from isopropenyl toluene are, for example, 65 mol% or more, preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, particularly preferably 95 mol% or more, and for example, 100 mol% or less, preferably 97 mol% or less.

[0088] In such a polymer, the content of structural units derived from other components (preferably, the C5 fraction) is, for example, 0% or more, preferably 3 mol% or more, and for example, 35 mol% or less, preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, and particularly preferably 5 mol% or less.

[0089] The ratio of the above constituent units is as follows: 13 It can be measured by C-NMR spectroscopy.

[0090] The softening point of the polymer is, for example, 85°C or higher, preferably 90°C or higher, more preferably 95°C or higher, even more preferably 110°C or higher, particularly preferably 120°C or higher, and for example, 150°C or lower, preferably 140°C or lower, more preferably 130°C or lower.

[0091] If the softening point is within the above range, the adhesive strength and holding power in high temperature regions can be improved.

[0092] The softening point can be measured by the ring and ball method (in accordance with JIS K2207).

[0093] The number average molecular weight (Mn) of the polymer, as calculated using standard polystyrene standards by gel permeation chromatography (GPC), is, for example, 500 or more, preferably 700 or more, more preferably 900 or more, and even more preferably 1000 or more, and for example, 2000 or less, preferably 1200 or less, and more preferably 1100 or less.

[0094] If the number average molecular weight (Mn) is within the above range, the adhesive strength and holding power in high temperature regions can be improved.

[0095] The weight average molecular weight (Mw) of the polymer, as calculated using standard polystyrene standards by gel permeation chromatography (GPC), is, for example, 600 or more, preferably 1000 or more, more preferably 1200 or more, even more preferably 1500 or more, particularly preferably 1800 or more, and for example, 5000 or less, preferably 3000 or less, more preferably 2000 or less, even more preferably 1900 or less.

[0096] If the weight average molecular weight (Mw) is within the above range, the adhesive strength and holding power in high temperature regions can be improved.

[0097] The z-average molecular weight (Mz) of the polymer, calculated based on standard polystyrene by gel permeation chromatography (GPC), is, for example, 700 or more, preferably 1000 or more, more preferably 1500 or more, even more preferably 1800 or more, particularly preferably 2500 or more, and most preferably 3000 or more, and for example, 5000 or less, preferably 4000 or less, more preferably 3500 or less, and even more preferably 3100 or less.

[0098] If the z-average molecular weight (Mz) is within the above range, the adhesive strength and holding power in high temperature regions can be improved.

[0099] In addition, in the polymer, the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is, for example, 1.10 or more, preferably 1.30 or more, more preferably 1.50 or more, even more preferably 1.70 or more, and for example, 2.00 or less, preferably 1.80 or less.

[0100] If the ratio is within the above range, the adhesive strength and holding power in high temperature regions can be improved.

[0101] The polymer contains a high molecular weight component having a molecular weight of 2000 or more as calculated as standard polystyrene by gel permeation chromatography (GPC).

[0102] The content of the high molecular weight component is, relative to the polymer, for example, 10 mass % or more, preferably 20 mass % or more, more preferably 30 mass % or more, and for example, 50 mass % or less, preferably 40 mass % or less.

[0103] When the content of the high molecular weight component is equal to or higher than the above lower limit, the adhesive strength and holding power in high temperature regions can be improved.

[0104] The content of the high molecular weight component can be measured by gel permeation chromatography (GPC). In detail, as shown in Fig. 1, the molecular weight distribution is measured by gel permeation chromatography (GPC), and the area of ​​the region with a standard polystyrene-equivalent molecular weight of 2000 or more in the obtained chromatogram (shaded area in Fig. 1) is regarded as the content of the high molecular weight component.

[0105] The tackifiers can be used alone or in combination of two or more kinds.

[0106] The content of the tackifier is, relative to 100 parts by mass of the total amount of the (meth)acrylic resin and the tackifier, for example, 2 parts by mass or more, preferably 10 parts by mass or more, more preferably 18 parts by mass or more, and for example, 40 parts by mass or less, preferably 30 parts by mass or less, more preferably 25 parts by mass or less.

[0107] The content of the tackifier in the adhesive composition is, for example, 2 mass% or more, preferably 10 mass% or more, more preferably 18 mass% or more, and for example, 40 mass% or less, preferably 30 mass% or less, more preferably 25 mass% or less.

[0108] <Crosslinking agent> From the viewpoint of improving adhesive strength, the adhesive composition preferably contains a crosslinking agent.

[0109] Examples of the crosslinking agent include an epoxy compound, an isocyanate compound, an aziridine compound, and a melamine compound.

[0110] Examples of epoxy compounds include sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, glycerol polyglycidyl ether, neopentyl glycol diglycidyl ether, and resorcin diglycidyl ether.

[0111] Examples of the isocyanate compound include derivatives of hexamethylene diisocyanate (for example, trimethylolpropane adducts, isocyanurate derivatives) and derivatives of tolylene diisocyanate (for example, trimethylolpropane adducts, isocyanurate derivatives).

[0112] Examples of the aziridine compound include trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), N,N'-toluene-2,4-bis(1-aziridinecarboxamide), and trimethylolpropane-tri-β-(2-methylaziridine)propionate.

[0113] An example of the melamine compound is hexamethoxymethylolmelamine.

[0114] As the crosslinking agent, preferably, an isocyanate compound is used.

[0115] The crosslinking agents can be used alone or in combination of two or more kinds.

[0116] The content of the crosslinking agent relative to the pressure-sensitive adhesive composition is, for example, 0.1 mass % or more, preferably 0.5 mass % or more, and for example, 2.0 mass % or less, preferably 1.5 mass % or less.

[0117] <Additives> The pressure-sensitive adhesive composition may contain additives in an appropriate ratio as necessary, such as antioxidants, ultraviolet absorbers, antistatic agents, silane coupling agents, coating property improvers, leveling agents, defoamers, plasticizers, surfactants, pigments, fillers, antifungals, processing aids, and antiaging agents.

[0118] The additives can be used alone or in combination of two or more kinds.

[0119] <Preparation of adhesive composition> The adhesive composition can be obtained by blending a (meth)acrylic resin, a tackifier, a crosslinking agent which is blended as required, and additives which are blended as required.

[0120] The pressure-sensitive adhesive composition can be diluted with a known solvent. When the (meth)acrylic and / or the polymer is polymerized in the presence of a solvent, the solvent can be used as it is.

[0121] When the pressure-sensitive adhesive composition is diluted, the solid content concentration is, for example, 5 mass % or more, preferably 10 mass % or more, and for example, 70 mass % or less, preferably 60 mass % or less.

[0122] Such an adhesive composition has excellent adhesive strength and holding power in a high temperature range, for example, a range of 70°C or higher and 150°C or lower.

[0123] Furthermore, the adhesive composition has excellent adhesion and holding power, particularly to low-polarity materials, from the viewpoint that the tackifier suppresses the mobility of the acrylic adhesive ((meth)acrylic resin) and makes it less susceptible to shear slippage.

[0124] Examples of low polarity materials include polyolefin resins, such as polyethylene and polypropylene.

[0125] <Action and effect> In the pressure-sensitive adhesive composition, the tackifier is a polymer containing a structural unit derived from isopropenyl toluene. The polymer contains a high molecular weight component. Therefore, the adhesive strength and holding strength are excellent in a high temperature region.

[0126] For more details, see Patent Document 1, and rosin has been conventionally known as a tackifier.

[0127] However, rosin has a drawback in that it has low compatibility with (meth)acrylic resins, resulting in a decrease in holding power.

[0128] On the other hand, in the pressure-sensitive adhesive composition, the tackifier is a polymer containing a structural unit derived from isopropenyl toluene. By using such a tackifier, the compatibility with the (meth)acrylic resin can be improved. As a result, the holding power can be improved.

[0129] The adhesive composition also contains a tackifier, which is a polymer containing a high molecular weight component.

[0130] As shown in Figures 2A and 2B, in an adhesive composition containing a (meth)acrylic resin, the (meth)acrylic polymer chain 1 is flexible, so that molecular mobility tends to be high. In particular, molecular mobility becomes even higher in a high temperature region. When molecular mobility becomes high, adhesive strength and holding power tend to decrease.

[0131] In order to suppress the molecular motion of the (meth)acrylic polymer chain 1, it has been considered to add a tackifier, but as shown in Fig. 2A, if the polymer in the tackifier does not contain a high molecular weight component, the tackifier 2 cannot sufficiently bind the (meth)acrylic polymer chain 1, and cannot sufficiently suppress the molecular motion of the (meth)acrylic polymer chain 1. As a result, the adhesive strength and holding power decrease.

[0132] On the other hand, this adhesive composition contains a tackifier, which is a polymer containing a high molecular weight component. In this case, as shown in Fig. 2B, the tackifier 2 binds the (meth)acrylic polymer chain 1, and can sufficiently suppress the molecular motion of the (meth)acrylic polymer chain 1. As a result, the adhesive strength and holding strength can be improved in a high temperature range. EXAMPLES

[0133] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are based on mass unless otherwise specified. In addition, the specific numerical values ​​of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit value (numerical value defined as "less than or equal to" or "less than") or lower limit value (numerical value defined as "more than or equal to" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".

[0134] <Ingredient details> Details of the abbreviations used in each Example and Comparative Example are given below. IPT: Isopropenyl toluene C5:C5 fraction αMS: α-methylstyrene KE100: Hydrogenated rosin, product name "Pine Crustal KE100", manufactured by Arakawa Chemical Industries Co., Ltd.

[0135] <Production of (meth)acrylic resin> Manufacturing Example 1 A temperature-controllable reactor equipped with a stirrer was charged with 350 parts by mass of ethyl acetate and 40 parts by mass of toluene, purged with nitrogen, and heated. Next, a solution containing 418 parts by mass of butyl acrylate, 2 parts by mass of 2-hydroxyethyl acrylate, and 2 parts by mass of benzoyl peroxide as a polymerization initiator was continuously added to the reactor heated to 75°C, and reacted for 5 hours. After polymerization, the mixture was diluted with 120 parts by mass of toluene to obtain an acrylic resin solution with a solid content concentration of 40%.

[0136] <Production of tackifier (polymer)> Manufacturing Example 2 A mixture of the second polymerization component (isopropenyltoluene and C5 fraction) and dehydrated and purified toluene (second polymerization component / toluene = 1 / 1 (volume ratio)) and a Friedel-Crafts catalyst (boron trifluoride phenolate complex (1.7 times equivalent of phenol) diluted 10 times with dehydrated and purified toluene) were continuously fed to the first stage of a 1270 ml capacity autoclave equipped with a stirring blade, and a polymerization reaction was carried out at 5°C. The mass ratio of isopropenyltoluene to the C5 fraction (isopropenyltoluene / C5 fraction) was 90 / 10, the feed rate of the mixture of the second polymerization component and toluene was 1.0 liter / hour, and the feed rate of the Friedel-Crafts catalyst was 105 milliliters / hour. This resulted in a reaction mixture being obtained.

[0137] The reaction mixture was then transferred to the second autoclave, and the polymerization reaction was continued at 5°C. When the total residence time in the first and second autoclaves reached 2 hours, the reaction mixture was continuously discharged from the autoclave, and when the residence time reached three times, 1 liter of the reaction mixture was collected to terminate the polymerization reaction. After the polymerization was completed, a 1N NaOH aqueous solution was added to the collected reaction mixture to deash the catalyst residue. Furthermore, the reaction mixture was washed five times with a large amount of water, and then the solvent and the unreacted second polymerization component were distilled off under reduced pressure using an evaporator to obtain a polymer (tackifier) ​​that was a copolymer of isopropenyl toluene and a C5 fraction.

[0138] Production Example 3 A polymer (tackifier), which was a copolymer of isopropenyl toluene and a C5 fraction, was obtained according to the same procedure as in Production Example 1. However, the amount of the Friedel-Crafts catalyst supplied was changed to 56 mL / hour.

[0139] Production Example 4 A polymer (tackifier) ​​which was a homopolymer of isopropenyl toluene was obtained according to the same procedure as in Production Example 1. However, the polymerization temperature was changed to 25°C, the second polymerization component was changed to only isopropenyl toluene, and the supply amount of the Friedel-Crafts catalyst was changed to 130 mL / hour.

[0140] Production Example 5 A polymer (tackifier) ​​which was a homopolymer of α-methylstyrene was obtained according to the same procedure as in Production Example 1. However, the second polymerization component was changed to α-methylstyrene alone, and the supply amount of the Friedel-Crafts catalyst was changed to 56 mL / hour.

[0141] <Preparation of adhesive composition> Example 1, Example 2, and Comparative Examples 1 to 3 A (meth)acrylic resin, a tackifier, and a crosslinking agent (isocyanate compound) were mixed together based on the description in Table 2. In this way, a pressure-sensitive adhesive composition was prepared.

[0142] <Evaluation> [Constituent units of each component] The structural units of each component in the polymer of each production example were determined based on the following conditions: 13 The results are shown in Table 1. {conditions} Equipment: Bruker Biospin AVANCEIII cryo-500 nuclear magnetic resonance equipment Measurement nucleus: 13C (125MHz) Measurement mode: Single pulse proton broadband decoupling Pulse width: 45° (5.00μsec) Number of points: 64k Measurement range: 250 ppm (-55 to 195 ppm) Repeat time: 5.5 seconds Number of times accumulated: 128 times Measurement solvent: orthodichlorobenzene / benzene-d6 (4 / 1 (volume ratio)) Sample concentration: 60mg / 0.6mL Measurement temperature: 120℃ Window function: exponential (BF: 1.0Hz) Chemical shift reference: δδ signal 29.73 ppm

[0143] [Softening point] The polymers of each production example and KE100 were measured by the ring and ball method in accordance with JIS K2207. The results are shown in Table 1.

[0144] [Number average molecular weight (Mn), weight average molecular weight (Mw), z-average molecular weight (Mz), Mw / Mn and content of high molecular weight components] For the polymers of each production example and KE100, the number average molecular weight (Mn), weight average molecular weight (Mw), and z-average molecular weight (Mz) in terms of standard polystyrene were measured by gel permeation chromatography (GPC) under the following measurement conditions, and Mw / Mn was calculated. In the obtained chromatogram, the area of ​​the region with a molecular weight of 2000 or more was taken as the content of the high molecular weight component, and the content ratio of the high molecular weight component to the polymer was calculated. The results are shown in Table 1. {Measurement conditions} Equipment: GPC HLC-8320 (Tosoh Corporation) Solvent: Tetrahydrofuran Columns: TSKgel G7000 x 1, TSKgel G4000 x 2, TSKgel G2000 x 1 (all manufactured by Tosoh Corporation) Flow rate: 1.0ml / min Sample: 20mg / mL tetrahydrofuran solution Column temperature: 40℃ Detector: Differential refractive index detector Injection volume: 50μl

[0145] [Preparation of test specimens] The adhesive composition of each Example and Comparative Example was applied to a release paper so that the film thickness after drying was 30 μm, and after drying at 80 ° C for 3 minutes, a PET film of 25 μm was pressed onto the applied surface to prepare an adhesive sheet. It was left at 50 ° C for 7 days. Thereafter, the adhesive sheet was cut to a width of 25 mm and a length of 150 mm. This prepared a test piece.

[0146] [Adhesive strength] The adhesive strength of each test piece was measured. The test piece was pressed onto a polypropylene plate (PP) with a thickness of 5 mm, width of 50 mm, and length of 125 mm at a speed of 300 mm / min using a rubber roll with a mass of 2 kg in an atmosphere of 23°C, and then left for 30 minutes, after which the 180° peel strength was measured at 80°C in accordance with JIS Z0237. The results are shown in Table 2.

[0147] [Holding force] The holding power was measured for each test piece. Specifically, in accordance with JIS Z0237, the test piece was pressed onto a stainless steel plate (SUS304) using a rubber roll of 2 kg mass in an atmosphere of 23°C so that the adhesion area was 25 mm x 25 mm to prepare an adhesion sample. After 30 minutes of pressing, the adhesion sample was hung vertically in an atmosphere of 80°C, a weight of 1 kg was hung on the lower end of the test piece and left to stand, and the slippage width after 1 hour was measured. The results are shown in Table 2.

[0148] [Table 1]

[0149] [Table 2]

Claims

1. Contains a (meth)acrylic resin and a tackifier, The tackifier is a polymer containing a structural unit derived from isopropenyl toluene, The polymer comprises a high molecular weight component having a molecular weight of 2000 or more.

2. The pressure-sensitive adhesive composition according to claim 1 , wherein the content of the high molecular weight component is 10 mass % or more relative to the polymer.

3. The adhesive composition according to claim 1 or 2, wherein the polymer contains structural units derived from a C5 fraction.

4. The polymer contains 90 mol % or more and 99 mol % or less of structural units derived from isopropenyl toluene, The pressure-sensitive adhesive composition according to claim 3 , wherein the polymer contains structural units derived from a C5 fraction in an amount of 1 mol % or more and 10 mol % or less.

Citation Information

Patent Citations

  • Hot-melt adhesive composition

    JP1994184249A

  • (CO)polymer and tackifier

    JP2021004289A

  • Hydrogen sensor element

    JP2021156866A

  • Adhesive composition and adhesive processed product

    JP2023023563A

  • Adhesive composition and adhesive processed product

    JP2023023567A