Rubber reinforcement cord

A composite cord using aramid and nylon fibers from renewable resources, optimized with specific twist coefficients and coated with a rubber adhesive, addresses the performance decline in rubber reinforcing cords, maintaining high modulus and durability.

JP2024141136AActive Publication Date: 2024-10-10DUPONT TORAY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023052622
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

The use of renewable resource-derived materials in rubber reinforcing cords results in a decrease in glass transition temperature, leading to reduced rubber reinforcing effect due to heat, and adjusting twist structures to enhance the effect compromises bending and compression fatigue properties.

Method used

A composite cord is developed using aramid and nylon fibers derived from renewable resources, with optimized twist coefficients to maintain initial elongation and high modulus characteristics, coated with a rubber adhesive.

Benefits of technology

The composite cord achieves performance equivalent to conventional aramid/nylon cords, with improved moldability and enhanced durability under high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141136000001
    Figure 2024141136000001
  • Figure 2024141136000002
    Figure 2024141136000002
Patent Text Reader

Abstract

To provide a rubber reinforcement fiber cord which contains a raw material derived from renewable resource, is easily molded into a tire and the like, maintains initial elongation, and on the other hand, exhibits high elastic modulus specific to a high elastic modulus fiber in subsequent elongation regions.SOLUTION: A rubber reinforcement cord, in which a surface of an organic fiber cord is coated with a rubber adhesive containing at least one layer of latex, is characterized in that the organic fiber cord is a twisted yarn cord in which a nylon fiber containing a raw material derived from renewable resource and an aramid fiber are twisted.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber reinforcing cord for use in tires and the like. [Background technology]

[0002] Tire cord is the most important material that, together with rubber, forms a tire. The basic performance of a tire is load bearing, braking / driving, shock absorption, and handling stability. Organic fibers used in tire cord include nylon, polyester, rayon, aramid, etc., and are used according to the type of tire, the applicable components, and the performance required of the tire. The performance generally required of tire cord is strength, rigidity (elastic modulus), adhesion to rubber, fatigue resistance, dimensional stability, heat resistance, etc.

[0003] Nylon is characterized by its fatigue resistance, good adhesion, strength, and high elongation, and nylon 6 and nylon 66 are used for tire carcass and breaker materials, etc. Polyester (polyethylene terephthalate) has a higher elastic modulus and good dimensional stability than nylon, but has inferior adhesiveness and strength. Rayon is excellent in that it is easy to achieve both tire handling stability and ride comfort, has very good adhesiveness, and has a low thermal shrinkage rate during vulcanization (heat resistance), but has inferior strength and fatigue resistance. On the other hand, aramid polyparaphenylene terephthalamide fiber has very high strength and elastic modulus, and is used as belt material for passenger car radial tires and motorcycle tires, etc.

[0004] However, for rubber reinforcing cords, it is required to maintain initial elongation for ease of molding process, while at the same time, a high elastic modulus is required in the subsequent elongation range. For this reason, many composite cords made of nylon fiber with good initial elongation and aramid fiber with high elastic modulus have been proposed (for example, see Patent Documents 1 to 3).

[0005] Patent Document 1 discloses that a cord (Example 1) obtained by final twisting one strand of two first-twisted aramid fiber strands and one first-twisted nylon fiber strand has a higher pull-out resistance (i.e., adhesive strength with rubber) and is excellent in high-speed tire durability compared to a cord (Comparative Example 1) in which three first-twisted aramid fiber strands are twisted together.

[0006] Patent Document 2 discloses that when a plurality of first twisted yarns (A) of aramid fibers are doubling and twisting with a first twisted yarn (B) of a single polyester fiber or polyamide fiber, a ratio (B / A) of the first twist coefficient of the first twisted yarn (B) to the first twist coefficient of the first twisted yarn (A) is set to 0.5 to 1.2, thereby achieving both low elongation and resistance to bending fatigue, and that the first twist coefficient is preferably 2 or more from the standpoint of fraying resistance and the like, and is preferably 4 or less from the standpoint of tensile strength and tensile modulus.

[0007] In response to the recent demand to reduce the use of formalin and resorcinol from environmental considerations, Patent Document 3 proposes an environmentally friendly adhesive composition that does not use resorcinol or formalin. The proposal discloses that the organic fiber cord contains fibers whose raw materials can be produced from bio-derived materials, such as polyethylene terephthalate, nylon, rayon, and lyocell, and that the adhesive composition contains at least polyphenols such as resorcinol, 1,4-benzenedicarbaldehyde, and a rubber component. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2020-059464 A (Claims, Table 1, etc.) [Patent Document 2] JP 2021-175844 A (Claims, paragraphs 0042 to 0044, etc.) [Patent Document 3] JP 2021-143436 A (Claims, paragraph 0010, etc.) Summary of the Invention [Problem to be solved by the invention]

[0009] However, when changing from 6,6 nylon, which is commonly used in tire reinforcing cords, to raw materials derived from renewable resources such as 4,10 nylon or 6,10 nylon, problems arise in that the glass transition point of the fiber itself is lowered, resulting in a decrease in the rubber reinforcing effect due to heat. For example, poor running stability is caused by a decrease in elastic modulus due to heat treatment by dipping or the high temperature environment during tire operation. In addition, if the number of twists is reduced in an attempt to increase the rubber reinforcing effect in order to address these issues, the flexural properties and compression fatigue resistance in the tire will decrease.

[0010] On the other hand, the composite cord disclosed in Patent Document 1 adjusts the twist structure and the number of twists so that the length of the nylon strand along the cord circumference relative to the cord circumference of the exposed surface of the composite cord is within a certain range, but since the number of top twists of the composite cord is small relative to the number of first twists of the aramid fiber cord, the high elastic modulus specific to the aramid fiber cannot be fully exhibited. The composite cord disclosed in Patent Document 2 is said to improve the tensile strength of the power transmission belt and achieve both low elongation and bending fatigue resistance only when the fineness of the aramid fiber is 500 to 1500 dtex, but since the twist factor of the composite cord is small, 2 to 4, compared with the aramid first twist factor of 4.0 to 4.5, the strength retention rate after cord fatigue is low. Patent Document 3 discloses an organic fiber cord containing raw materials derived from renewable resources and a formaldehyde-free adhesive, but does not mention a composite cord.

[0011] It is therefore an object of the present invention to provide a composite cord for rubber reinforcement which comprises raw materials derived from renewable resources. Another object of the present invention is to provide a composite cord for reinforcing rubber, which is easily molded into tires and the like, and which maintains its initial elongation while exhibiting the high elastic modulus characteristic of high elastic modulus fibers in the subsequent elongation range. [Means for solving the problem]

[0012] In developing a composite cord for reinforcing rubber, the present inventors conducted extensive research into the fibers to be combined with aramid fiber, which has extremely high strength and elastic modulus, from the standpoints of cord properties and protection of the global environment, and eventually arrived at a composite cord that contains raw materials derived from renewable resources.

[0013] In addition, when raw materials derived from renewable resources are used, the glass transition point of the fibers may be low, and therefore, in composite cords manufactured by the same manufacturing method as in the past, the performance may be degraded due to heat generated during coating with adhesive and during tire running. In order to address the performance degradation, if the number of twists is reduced to enhance the reinforcing effect based on previous knowledge, the flexural fatigue and compressive fatigue in the tire will be degraded. However, it was found that the elongation range used in tire use is not affected by the properties of the nylon, and that there is a relationship of twist coefficient that allows the properties of the nylon to be utilized in the initial elongation. It was also found that by optimizing the twist coefficient of each cord constituting the composite cord, it is possible to achieve the same reinforcing effect as the conventionally used 6,6-nylon, even when raw materials derived from renewable resources are used.

[0014] Specifically, the present invention provides a rubber-reinforcing cord obtained by coating the surface of an organic fiber cord with at least one layer of a rubber adhesive containing latex, the organic fiber cord being a twisted cord obtained by twisting together nylon fiber containing raw materials derived from renewable resources and aramid fiber. The present invention also provides a rubber-reinforcing cord, wherein the organic fiber cord is a composite cord (C) obtained by twisting one or more first twisted cords (A) made of nylon fiber containing raw materials derived from renewable resources and one or more first twisted cords (B) made of aramid fiber in the same direction, and then twisting them together in a direction opposite to the first twist direction. Effect of the Invention

[0015] According to the present invention, an aramid-nylon composite cord that has a low environmental impact can be obtained. Furthermore, by optimizing the twist factor of each cord that constitutes the composite cord, a composite cord having the same performance as a conventional aramid-nylon composite cord can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, the rubber-reinforcing cord of the present invention will be described in detail based on embodiments thereof.

[0017] The rubber-reinforcing cord of the present invention is a rubber-reinforcing cord obtained by coating the surface of an organic fiber cord with at least one layer of a rubber adhesive containing latex, and the organic fiber cord is a twisted cord obtained by twisting together nylon fibers containing raw materials derived from renewable resources and aramid fibers.

[0018] [Nylon fiber] The nylon fiber constituting the rubber reinforcing cord (composite cord) of the present invention contains raw materials derived from renewable resources. Nylon (polyamide) fibers, such as nylon 6 and nylon 66, have been widely used in rubber reinforcing cords, taking advantage of their excellent mechanical properties, excellent abrasion resistance, excellent flexibility, and other properties. The nylon fiber constituting the rubber reinforcing cord of the present invention has dicarboxylic acid units that can be produced from raw materials derived from renewable resources, preferably raw materials derived from plants, and is preferably a nylon (polyamide) fiber obtained by condensation polymerization of the dicarboxylic acid with a diamine.

[0019] Examples of the dicarboxylic acids derived from renewable resources include succinic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, etc. Suberic acid, sebacic acid, and undecanedioic acid are refined from castor oil seeds, and azelaic acid is refined from linseed oil, so they are materials that are excellent for the global environment.

[0020] Among the dicarboxylic acids, nylon fibers having dicarboxylic acid units mainly composed of sebacic acid units are preferred, since the nylon fibers have a high melting point, excellent heat resistance, and excellent tensile strength and tensile elongation. The nylon fibers may be copolymerized with other compounds within the scope of the present invention. Examples of the dicarboxylic acids include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, and adipic acid, alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid, and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid.

[0021] The nylon fiber having dicarboxylic acid units mainly composed of sebacic acid units used in the present invention is preferably a fiber obtained from a condensation polymer of an aliphatic diamine mainly composed of dimethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, nonamethylenediamine, or decamethylenediamine, and a carboxylic acid mainly composed of sebacic acid. Preferred examples include 2,10 nylon fiber, 3,10 nylon fiber, 4,10 nylon fiber, 5,10 nylon fiber, 6,10 nylon fiber, 9,10 nylon fiber, 10,10 nylon fiber, and the like. Among these, 4,10 nylon fiber, 5,10 nylon fiber, and 6,10 nylon fiber are preferred from the viewpoint of their relatively high glass transition points.

[0022] The nylon fibers may contain nylon fibers that do not contain raw materials derived from renewable resources, such as nylon 6 fibers, nylon 6,6 fibers, etc. In the present invention, the ratio of the nylon fibers that do not contain raw materials derived from renewable resources in the first twisted cord (A) can be adjusted depending on the required properties of the rubber reinforcing cord.

[0023] The monofilament fineness of the nylon fiber containing the raw material derived from renewable resources of the present invention can be set arbitrarily according to the required characteristics of the rubber reinforcing fiber cord, but is preferably 0.1 to 20.0 dtex. The finer the monofilament fineness, the lower the bending rigidity of the monofilament, and therefore the lower the bending rigidity of the thread, resulting in better cord formability. On the other hand, by having a monofilament fineness of 0.1 dtex or more, it becomes possible to suppress the generation of fluff in the spinning process and perform high-ratio drawing, resulting in a fiber with high strength. The monofilament fineness is more preferably 0.5 to 15.0 dtex, and even more preferably 1.0 to 10.0 dtex.

[0024] The total fineness of the nylon fiber containing raw materials derived from renewable resources according to the present invention can be set arbitrarily depending on the required properties of the rubber reinforcing fiber cord, but is preferably 200 to 3000 dtex. By setting the total fineness to 3000 dtex or less, the yarn has good workability in the coding process. On the other hand, by setting the total fineness to 200 dtex or more, the yarn is sufficiently durable for practical use. The total fineness is more preferably 500 to 2000 dtex, and even more preferably 800 to 1500 dtex.

[0025] [Aramid fiber] The aramid fiber constituting the rubber reinforcing cord (composite cord) of the present invention is not particularly limited as long as it is a fiber having at least one divalent aromatic group, which may be substituted, in the repeating unit of the polymer forming the fiber and has at least one amide bond. It may be a wholly aromatic polyamide fiber or one called an aramid fiber. The "divalent aromatic group, which may be substituted" means a divalent aromatic group, which may have one or more identical or different substituents. Examples of aramid fibers include para-aramid fibers and meta-aramid fibers, but para-aramid fibers having excellent mechanical properties are preferred. Such aramid fibers are commercially available, and specific examples of para-aramid fibers include polyparaphenylene terephthalamide fibers (manufactured by DuPont USA, Toray DuPont Co., Ltd., trade name "Kevlar" (registered trademark)) and copolyparaphenylene-3,4'-oxydiphenylene terephthalamide fibers (manufactured by Teijin Limited, trade name "Technora" (registered trademark)). Among these para-aramid fibers, polyparaphenylene terephthalamide fibers are particularly preferred because of their excellent mechanical properties.

[0026] The aramid fiber may have an adhesive layer of an epoxy compound on the fiber surface and / or the fiber cord surface. Such an aramid fiber may be obtained by a method of applying an uncured curable epoxy compound to the fiber surface in an oil application step or a subsequent finishing step during the aramid fiber production process. Alternatively, the aramid fiber may be obtained by a method of applying a curable epoxy compound to an existing aramid fiber.

[0027] The curable epoxy compound is preferably one or more selected from aliphatic epoxy compounds and epoxy compounds having aromatic rings. For example, glycerol diglycidyl ether, glycerol triglycidyl ether, polyglycerol polyglycidyl ether, sorbitol polyglycidyl ether, trimethylolpropane polyglycidyl ether, pentaerythritol polyglycidyl ether, etc. Among them, polyfunctional epoxy compounds having two or three glycidyl groups are preferred.

[0028] The single fiber fineness and total fineness of the aramid fiber in the present invention can be set arbitrarily depending on the required properties of the cord. The single fiber fineness is preferably 0.5 to 10 dtex, and within the above range, a rubber reinforcing cord can be produced without technical difficulties. The total fineness is preferably 500 to 3000 dtex, and more preferably 800 to 2000 dtex.

[0029] [Organic fiber cord] In the organic fiber cord of the present invention, the twisting form of the twisted yarn cord is not particularly limited. It is preferable that the twisted yarn cord is a composite cord (C) formed by twisting together one or more first twisted cords (A) made of nylon fiber (hereinafter sometimes referred to as "S-nylon fiber") containing raw materials derived from renewable resources and one or more first twisted cords (B) made of aramid fiber. The number of first twisted cords (A) and (B) may be one, two, or three or more. In addition, the number of first twisted cords (A) and first twisted cords (B) may be the same or different.

[0030] The ratio (mass ratio) of S-nylon fiber to aramid fiber in the composite cord is not particularly limited, and although it varies depending on the purpose and application, the ratio of both fibers is preferably in the range of 20 to 80 mass % of nylon fiber and 20 to 80 mass % of aramid fiber.

[0031] The twist direction of the first twisted cord (A) and the first twisted cord (B) may be either S or Z direction, but they must be twisted in the same direction to properly control the intermediate elongation of the cord. The number of twists varies depending on the purpose and application, and is not particularly limited, but is preferably 20 (t / 10 cm) to 50 (t / 10 cm).

[0032] The first twisted cord (A) and the first twisted cord (B) are twisted together to form an organic fiber cord (composite cord (C)). In this case, it is preferable from the viewpoint of handling of the cord that the first twisted cord (A) and the first twisted cord (B) are twisted together in the opposite direction to the first twisted direction.

[0033] In the composite cord, the Young's modulus (elastic modulus in elongation) at 5% elongation is desirably 2.0 times or more higher than the Young's modulus (elastic modulus in elongation) at 1% elongation. If the ratio is less than 2.0 times, the processability during tire molding is good, but the cord elastic modulus for suppressing the tire from rising up during high-speed tire running is insufficient, which has a significant impact on rolling resistance and tire durability. However, if the ratio is 2.0 times or more, it is possible to achieve both processability during tire molding and tire reinforcement ability. In other words, by increasing the Young's modulus at 5% elongation relative to the Young's modulus at 1% elongation, it is possible to improve tire moldability, which has been a problem when applying conventional aramid fiber cords to tire cords, and to realize high tire reinforcement hardening required of aramid fibers.

[0034] In the present invention, it is preferable that the organic fiber cord (composite cord) satisfies the following relational expressions (I) and (II). That is, in formula (I), TM(A) / TM(B) of 0.5 or more means that the number of ply twists of the S-nylon fiber is half or equal to the number of ply twists of the aramid fiber. This makes it possible to prevent the S-nylon fiber, which has a lower glass transition point than 6,6-nylon, from being stretched too much due to cord fatigue. Also, if the number of twists exceeds the number of ply twists of the aramid fiber, the adhesion between the rubber reinforcing cord and the rubber may decrease.

[0035] In addition, in formula (II), if TM(C) / TM(B) is less than 1.0, the post-fatigue strength retention of the composite cord may decrease significantly, whereas if it exceeds 1.5, the strength of the composite cord may decrease significantly, making it unsuitable as a rubber reinforcing cord.

[0036] 0.5≦TM(A) / TM(B)≦1.0 (I) 1.0≦TM(C) / TM(B)≦1.5 (II) (Where, TM(A): twist factor of the first twisted cord made of nylon fibers containing raw materials derived from recycled resources TM(B): Twist factor of a twisted cord made of aramid fiber TM(C): twist factor of the composite cord

[0037] [Rubber reinforcement cord] The rubber reinforcing cord of the present invention is obtained by covering the surface of the organic fiber cord (composite cord) with at least one layer of a rubber adhesive containing latex. As the latex, for example, vinylpyridine-styrene-butadiene-based, isoprene-based, styrene-butadiene-based, ethylene-propylene-diene-based, acrylonitrile-butadiene-based, chloroprene-based, chlorosulfonated polyethylene-based, acrylate-based, natural rubber-based, and other latexes can be used. These latexes may be used alone or in combination of two or more. The use of latex can improve the adhesion between the organic fiber cord and the rubber member.

[0038] The rubber adhesive may further contain a solvent. In addition, the adhesive may contain a component for enhancing adhesion as appropriate within the scope of the object of the present invention, thereby enabling the rubber and the composite cord to be firmly bonded together. For example, an epoxy compound, an isocyanate compound, etc. EXAMPLES

[0039] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto.

[0040] The evaluation method for rubber reinforcing cords is as follows. (1) Strength retention rate after disk fatigue test The test was evaluated according to JIS L 1017:2002, Appendix 1, 2.2.2, Disc Fatigue Strength (Goodrich Method). Two treated cords were embedded in tire rubber and vulcanized at 150°C for 30 minutes to prepare a rubber compound. The test specimen was subjected to 8% compression, 16% elongation, and fatigue for 300,000 cycles, after which the cords were removed from the rubber and the breaking strength after fatigue was measured, and expressed as the retention rate before and after the fatigue test.

[0041] (Example 1; Reference Example) A single strand of polyparaphenylene terephthalamide fiber (fineness 1110 dtex when converted to 0% moisture content, filament count 1000) was first twisted in the Z direction with a twist number of 40 (t / 10 cm) to obtain an aramid fiber single twist cord. Separately, a nylon fiber single twist cord was obtained by first twisting a single 6,6 nylon fiber multifilament (manufactured by Toray Industries, Inc., single yarn fineness: 6.91 dtex, total fineness: 940 dtex) in the Z direction with a twist number of 20 (t / 10 cm).

[0042] Three of the above single-twisted cords were twisted in the S direction with a twist number of 40 (t / 10 cm) to obtain a twisted yarn cord (aramid-nylon composite cord). The obtained ply-twisted yarn cord was immersed in a first adhesive treatment liquid containing an epoxy compound as a main component, and heat-treated at 140°C for 2 minutes to remove moisture, and then heat-treated at 230°C for 1 minute. The cord was further immersed in a second adhesive treatment liquid containing rubber latex as a main component, and heat-treated at 140°C for 2 minutes to remove moisture, and then heat-treated at 230°C for 1 minute to complete an aramid fiber cord. The results are shown in Table 1.

[0043] The final twist factor (K2) of the ply-twisted cord was calculated using the following formula. JPEG2024141136000001.jpg40137

[0044] Example 2 A single strand of polyparaphenylene terephthalamide fiber (fineness 1110 dtex when converted to 0% moisture content, filament count 1000) was first twisted in the Z direction with a twist number of 40 (t / 10 cm) to obtain an aramid fiber single twist cord. Separately, a nylon fiber single twist cord was obtained by first twisting a single 4,10 nylon fiber multifilament (manufactured by Toray Industries, Inc., single yarn fineness: 6.91 dtex, total fineness: 940 dtex) in the Z direction with a twist number of 20 (t / 10 cm). Three of the above single-twisted cords were used to obtain a ply-twisted twisted yarn cord (aramid-nylon composite cord) by twisting in the S direction in the same manner as in Example 1, except that the twists were 40 (t / 10 cm).

[0045] Example 3 A single strand of polyparaphenylene terephthalamide fiber (fineness 1110 dtex when converted to 0% moisture content, filament count 1000) was first twisted in the Z direction with a twist number of 40 (t / 10 cm) to obtain an aramid fiber single twist cord. Separately, a nylon fiber single twist cord was obtained by first twisting one 4,10 nylon fiber multifilament (manufactured by Toray Industries, Inc., single yarn fineness: 6.91 dtex, total fineness: 940 dtex) in the Z direction with a twist number of 30 (t / 10 cm). A ply-twisted cord (aramid-nylon composite cord) was obtained by twisting three of the above single-twisted cords in the S direction with a twist number of 25 (t / 10 cm) in the same manner as in Example 1, except that a ply-twisted cord was obtained by twisting three of the above single-twisted cords in the S direction with a twist number of 25 (t / 10 cm).

[0046] Example 4 A single strand of polyparaphenylene terephthalamide fiber (fineness 1110 dtex when converted to 0% moisture content, filament count 1000) was first twisted in the Z direction with a twist number of 40 (t / 10 cm) to obtain an aramid fiber single twist cord. Separately, a nylon fiber single twist cord was obtained by first twisting one 4,10 nylon fiber multifilament (manufactured by Toray Industries, Inc., single yarn fineness: 6.91 dtex, total fineness: 940 dtex) in the Z direction with a twist number of 30 (t / 10 cm). A ply-twisted cord (aramid-nylon composite cord) was obtained by twisting the three single-twisted cords in the S direction with a twist number of 50 (t / 10 cm) in the same manner as in Example 1, except that a ply-twisted cord was obtained by twisting the three single-twisted cords in the S direction with a twist number of 50 (t / 10 cm).

[0047] Example 5 A single strand of polyparaphenylene terephthalamide fiber (fineness 1110 dtex when converted to 0% moisture content, filament count 1000) was first twisted in the Z direction with a twist number of 40 (t / 10 cm) to obtain an aramid fiber single twist cord. Separately, a nylon fiber single twist cord was obtained by first twisting one 4,10 nylon fiber multifilament (manufactured by Toray Industries, Inc., single yarn fineness: 6.91 dtex, total fineness: 940 dtex) in the Z direction with a twist number of 30 (t / 10 cm). Three of the above single-twisted cords were used to obtain a ply-twisted twisted yarn cord (aramid-nylon composite cord) by twisting in the S direction in the same manner as in Example 1, except that the twists were 40 (t / 10 cm).

[0048] Example 6 Two polyparaphenylene terephthalamide fibers (fineness 1110 dtex when converted to 0% moisture content, filament count 1000) were first twisted in the Z direction with a twist number of 28 (t / 10 cm) to obtain an aramid fiber single twist cord. Separately, a nylon fiber single twist cord was obtained by first twisting one 4,10 nylon fiber multifilament (manufactured by Toray Industries, Inc., single yarn fineness: 6.91 dtex, total fineness: 940 dtex) in the Z direction with a twist number of 30 (t / 10 cm). Three of the above single-twisted cords were used to obtain a ply-twisted twisted yarn cord (aramid-nylon composite cord) by twisting in the S direction in the same manner as in Example 1, except that the number of twists was 28 (t / 10 cm).

[0049] Example 7 A single strand of polyparaphenylene terephthalamide fiber (fineness 1110 dtex when converted to 0% moisture content, filament count 1000) was first twisted in the Z direction with a twist number of 40 (t / 10 cm) to obtain an aramid fiber single twist cord. Separately, a nylon fiber single twist cord was obtained by first twisting a single 4,10 nylon fiber multifilament (manufactured by Toray Industries, Inc., single yarn fineness: 6.91 dtex, total fineness: 940 dtex) in the Z direction with a twist number of 40 (t / 10 cm). Three of the above single-twisted cords were used to obtain a ply-twisted twisted yarn cord (aramid-nylon composite cord) by twisting in the S direction in the same manner as in Example 1, except that the twists were 40 (t / 10 cm).

[0050] The properties of the twisted cords obtained in the examples are shown in Table 1.

[0051] [Table 1]

[0052] Based on previous findings, when a 4,10 nylon fiber first-twist cord (No. 2) was twisted in the same way as the second-twist cord made of aramid fiber and 6,6 nylon fiber (No. 1), the Young's modulus at 5% elongation decreased and the cord strength decreased.

[0053] Therefore, the number of twists in the 4,10 nylon fiber ply cord was increased and the number of twists in the ply cord was changed (No. 3-4). However, when the number of ply twists was small, the strength retention rate after the cord fatigued decreased, and when the number of ply twists was large, the Young's modulus at 5% elongation became small and the cord strength decreased.

[0054] In addition, the number of twists in the top twist cord was changed while maintaining the same number of twists in the 4,10 nylon fiber first twist cord (No. 5-6). As a result, a cord strength and strength retention after cord fatigue were obtained that were comparable to those of the 6,6-nylon cord (No. 1) (No. 5), and by increasing the number of aramid fiber first twist cords, a composite cord (No. 6) with high cord strength and strength retention after cord fatigue was obtained. Furthermore, by further increasing the number of twists in the 4,10 nylon fiber first twist cord (No. 7), the cord strength and strength retention after cord fatigue were comparable to those of the 6,6-nylon cord (No. 1).

[0055] As shown in Table 1, it can be seen that the twisted cord made by twisting together aramid fiber and nylon fiber containing raw materials derived from renewable resources has properties in cord strength and strength retention after cord fatigue that are equal to or greater than those of the twisted cord made by twisting together aramid fiber and 6,6 nylon fiber.

[0056] The present invention has been specifically described above using examples. However, the above-mentioned embodiment shows one example of a preferred embodiment of the present invention, and the present invention is not limited to the above-mentioned embodiments, and various modifications are possible within the scope of the claims. [Industrial Applicability]

[0057] The rubber reinforcing cord of the present invention can be suitably used as a reinforcing material for tires, and can also be widely used as a reinforcing material for rubber products such as belts and hoses.

Claims

1. A rubber reinforcing cord comprising an organic fiber cord having a surface coated with at least one layer of a rubber adhesive containing latex, A rubber reinforcing cord, wherein the organic fiber cord is a twisted cord obtained by twisting together nylon fiber containing raw materials derived from renewable resources and aramid fiber.

2. 2. The rubber reinforcing cord according to claim 1, wherein the organic fiber cord is a composite cord (C) formed by twisting one or more first twisted cords (A) made of nylon fiber containing raw materials derived from renewable resources and one or more first twisted cords (B) made of aramid fiber in the same direction, and then twisting them together in a direction opposite to the first twist direction.

3. 2. The rubber reinforcing cord according to claim 1, wherein the nylon fibers are obtained by condensation polymerization of an aliphatic diamine and a dicarboxylic acid containing raw materials derived from renewable resources.

4. 4. The rubber reinforcing cord according to claim 1, wherein the organic fiber cord has a Young's modulus at 5% elongation that is at least 2.0 times higher than the Young's modulus at 1% elongation.

5. The rubber reinforcing cord according to any one of claims 1 to 3, wherein the organic fiber cord is characterized in that a twist multiplier TM (A) of a first twisted cord made of nylon fiber containing raw materials derived from recycled resources, a twist multiplier TM (B) of a first twisted cord made of aramid fiber, and a twist multiplier TM (C) of a composite cord obtained by twisting the organic fiber cord satisfy the following relational expressions: 0.5≦TM(A) / TM(B)≦1.0 (I) 1.0≦TM(C) / TM(B)≦1.5 (II)

Citation Information

Patent Citations

  • Pneumatic radial tire for passenger car

    JP1992314604A

  • Hybrid reinforcing material

    JP2016537243A

  • Hybrid cord for use as a reinforcement in a belt band for pneumatic tires for vehicles

    JP2017521574A

  • Strip member and pneumatic tire

    JP2019006279A

  • Reinforcing ply for a pneumatic vehicle tire, preferably for a belt bandage ply of a pneumatic vehicle tire

    JP2019511411A