Polyurethane resin-formable composition for film sealants, film sealant and membrane module
A polyurethane resin-forming composition with polymerized castor oil addresses the issue of low-molecular reactant and solvent elution in membrane sealing materials, enhancing moldability and adhesive strength for membrane modules.
Patent Information
- Application Number
- JP2023052694
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing membrane sealing materials using polyisocyanate and polyol compositions suffer from elution of low-molecular reactants and solvents, which can contaminate the fluid in contact with the membrane, and often compromise the moldability of the cured product.
A polyurethane resin-forming composition comprising a polyisocyanate prepolymer and a polyol component, where the polyol component includes polymerized castor oil with removed hydroxyl groups, is used to form a cured product that suppresses the elution of low-molecular reactants and solvents, while maintaining excellent moldability.
The composition effectively reduces the elution of low-molecular reactants and solvents, ensuring the cured product has improved moldability and adhesive strength, suitable for applications in membrane modules.
Smart Images

Figure 2024141188000005 
Figure 2024141188000001 
Figure 2024141188000002
Abstract
Description
[Technical Field]
[0001] The present invention relates to a polyurethane resin-forming composition for a membrane sealant, a membrane sealant, and a membrane module. [Background technology]
[0002] BACKGROUND ART Membrane seal materials containing polyisocyanate and polyol are widely used to fix and seal membranes such as hollow fiber membranes.
[0003] When a cured product formed from polyisocyanate and polyol is used as a sealing material for a membrane containing glycerin, the polyisocyanate monomer present in the membrane sealing material reacts with glycerin, and low-molecular-weight reactants among the reactants may dissolve into the liquid in contact with the membrane.
[0004] Various proposals have been made to date from the viewpoint of suppressing the elution of low-molecular-weight reaction products. For example, Patent Document 1 discloses a polyurethane resin-forming composition for membrane module sealing materials, which comprises a polyisocyanate component (A) consisting of a prepolymer of partially dehydrated castor oil and / or partially acylated castor oil and an organic polyisocyanate, and a polyol component (B). Patent Document 2 discloses a polyurethane resin-forming composition for membrane sealing materials, which comprises a polyisocyanate prepolymer (A) and a polyol (B), wherein the polyol (B) contains a predetermined amount of a castor oil polymer having a number-average molecular weight of 1,500 or more. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-120043 [Patent Document 2] Patent Publication No. 2021-20135 Summary of the Invention [Problem to be solved by the invention]
[0006] In order to obtain a membrane sealant that can suppress the elution of low-molecular-weight reactants, using partially dehydrated castor oil as a polyol-containing component may increase the elution of solvent from the membrane sealant, while using polymerized castor oil as a polyol-containing component may decrease the moldability of the cured product.
[0007] One aspect of the present disclosure is directed to providing a polyurethane resin-forming composition for a membrane sealant, which is capable of forming a cured product in which elution of low-molecular-weight reactants and solvents is suppressed, and which has excellent moldability. Another aspect of the present invention is directed to providing a membrane sealant and a membrane module using the polyurethane resin-forming composition. [Means for solving the problem]
[0008] According to each aspect of the present disclosure, the following embodiments [1] to
[11] are provided. [1] A polyurethane resin-forming composition for a membrane sealing material, comprising a polyisocyanate prepolymer (A) and a polyol component (B), wherein the polyol component (B) comprises a polymerized castor oil (b1) from which a portion of the hydroxyl groups has been removed by a dehydration reaction. [2] The polyurethane resin-forming composition for a membrane sealing material according to [1], wherein the polymerized castor oil (b1) from which a portion of the hydroxyl groups has been removed by a dehydration reaction has a number average molecular weight of 1,500 or more. [3] The polyurethane resin-forming composition for a membrane sealing material according to [1] or [2], wherein the content of the polymerized castor oil (b1) from which a portion of the hydroxyl groups has been removed by a dehydration reaction is 70.0 mass% or less based on the total mass of the polyurethane resin-forming composition for a membrane sealing material. [4] The polyurethane resin-forming composition for a membrane sealing material according to any one of [1] to [3], wherein the polyisocyanate prepolymer (A) contains a reaction product of at least one (a1) selected from the group consisting of aromatic diisocyanates and modified products thereof, and an active hydrogen-containing compound (a2). [5] The polyurethane resin-forming composition for a membrane sealing material according to [4], wherein the aromatic diisocyanate is diphenylmethane diisocyanate. [6] The polyurethane resin-forming composition for a membrane sealing material according to any one of [1] to [5], wherein the polymerized castor oil (b1) from which a portion of the hydroxyl groups have been removed by a dehydration reaction has a hydroxyl value of 145 mgKOH / g or less. [7] The polyurethane resin-forming composition for a membrane sealing material according to any one of [1] to [6], wherein the polyol component (B) further contains a castor oil-based polyol (b2) other than the polymerized castor oil (b1) in which a portion of the hydroxyl groups has been removed by a dehydration reaction. [8] The polyurethane resin-forming composition for a membrane sealing material according to any one of [1] to [7], wherein the polyol component (B) further contains a hydroxyl group-containing amine compound (b3), and the content of the hydroxyl group-containing amine compound (b3) is 30 parts by mass or less per 100 parts by mass of the total amount of the polyol component (B). [9] A membrane sealing material comprising a cured product of the polyurethane resin-forming composition for a membrane sealing material according to any one of [1] to [8].
[10] A membrane module comprising a main body, a membrane, and the membrane sealing material according to [9] that seals the gap between the main body and the membrane.
[11] The membrane module according to
[10] , wherein the membrane is a plurality of hollow fiber membranes, and the membrane sealing material seals at least a portion of the gap between the main body and at least a portion of the plurality of hollow fiber membranes, and at least a portion of the gap between the plurality of hollow fiber membranes. [Effects of the Invention]
[0009] According to one aspect of the present disclosure, it is possible to provide a polyurethane resin-forming composition for a membrane sealant, which is capable of forming a cured product in which elution of low-molecular-weight reactants and solvents is suppressed, and which has excellent moldability. According to one aspect of the present invention, it is possible to provide a membrane sealant and a membrane module using the polyurethane resin-forming composition. [Brief explanation of the drawings]
[0010] [Figure 1] FIG. 1 is a conceptual diagram illustrating an example of a configuration of a membrane module according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE INVENTION
[0011] Hereinafter, several embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.
[0012] In this specification, numerical ranges indicated using "to" indicate ranges that include the numerical values before and after "to" as the minimum and maximum values, respectively. Unless otherwise specified, the units of the numerical values before and after "to" are the same. In numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range may be replaced with the upper or lower limit of a numerical range of another stage. In numerical ranges described in this specification, the upper or lower limit of that numerical range may be replaced with a value shown in the examples. The upper and lower limits individually described can be combined arbitrarily. Unless otherwise specified, the materials exemplified below may be used alone or in combination of two or more. When multiple substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of those multiple substances present in the composition, unless otherwise specified.
[0013] <Polyurethane resin-forming composition for membrane sealing material> A polyurethane resin-forming composition for a membrane sealant according to one embodiment of the present disclosure includes a polyisocyanate prepolymer (A) and a polyol component (B). The polyol component (B) includes a polymerized castor oil (b1) from which a portion of the hydroxyl groups has been removed by a dehydration reaction.
[0014] The polyurethane resin-forming composition may be a one-component composition in which the polyisocyanate prepolymer (A) and the polyol component (B) are mixed in one liquid, or may be a two-component composition comprising a first liquid containing the polyisocyanate prepolymer (A) and a second liquid containing the polyol component (B).
[0015] <Polyisocyanate prepolymer (A)> The polyisocyanate prepolymer (A) is a prepolymer containing two or more isocyanate groups.
[0016] The content of isocyanate groups in the polyisocyanate prepolymer (A) may be 5.0 mass% or more, 7.0 mass% or more, 8.0 mass% or more, 9.0 mass% or more, 10.0 mass% or more, 13.0 mass% or more, 13.5 mass% or more, 14.0 mass% or more, 15.0 mass% or more, 16.0 mass% or more, 17.0 mass% or more, or 18.0 mass% or more, based on the total mass of the polyisocyanate prepolymer (A). The content of isocyanate groups in the polyisocyanate prepolymer (A) may be 35.0 mass% or less, 30.0 mass% or less, 28.0 mass% or less, 26.0 mass% or less, 24.0 mass% or less, 22.0 mass% or less, 21.0 mass% or less, 20.5 mass% or less, or 20.0 mass% or less, based on the total mass of the polyisocyanate prepolymer (A). The content of isocyanate groups in the polyisocyanate prepolymer (A) is preferably from 13.0 to 21.0 mass%, more preferably from 13.5 to 20.5 mass%, and particularly preferably from 14.0 to 20.0 mass%, based on the total mass of the polyisocyanate prepolymer (A). When the content of isocyanate groups in the polyisocyanate prepolymer (A) is within the above-mentioned range, the polyurethane resin has even better moldability and adhesive strength.
[0017] The content of isocyanate groups in the polyisocyanate prepolymer (A) is measured in accordance with JIS K1603-1:2007.
[0018] The viscosity of the polyisocyanate prepolymer (A) at 25°C may be, for example, 1000 mPa·s or more, 1200 mPa·s or more, 1400 mPa·s or more, or 1600 mPa·s or more, and may be 2600 mPa·s or less, 2400 mPa·s or less, 2200 mPa·s or less, 2000 mPa·s or less, or 1800 mPa·s or less. The viscosity of the polyisocyanate prepolymer (A) at 25°C is the viscosity measured using a rotational viscometer (Type B, No. 3 rotor).
[0019] The crosslinking group density of the polyisocyanate prepolymer (A) may be 0.30 mmol / g or more, 0.35 mmol / g or more, 0.40 mmol / g or more, or 0.45 mmol / g or more, based on the total mass of the polyisocyanate prepolymer (A), and may be 0.60 mmol / g or less, 0.55 mmol / g or less, or 0.50 mmol / g or less. In this specification, the crosslinking group density refers to the total content density of groups capable of forming crosslinks and groups that have already formed crosslinks. The crosslinking group density is measured by the method described in the Examples below.
[0020] The content of the polyisocyanate prepolymer (A) may be 5% by mass or more, 10% by mass or more, 15% by mass or more, 20% by mass or more, 25% by mass or more, or 30% by mass or more, and may be 60% by mass or less, 50% by mass or less, 45% by mass or less, 40% by mass or less, or 35% by mass or less, based on the total mass of the polyisocyanate prepolymer (A) and the polyol component (B).
[0021] The polyisocyanate prepolymer (A) may contain a reaction product of at least one (a1) selected from the group consisting of polyisocyanates and modified products thereof, and an active hydrogen-containing compound (a2).
[0022] <<Polyisocyanates and modified products thereof (a1)>> Polyisocyanate is a compound containing two or more isocyanate groups. The number of isocyanate groups in a polyisocyanate molecule is two or more, and may be 10 or less, 8 or less, 6 or less, 4 or less, or 3 or less, or may be 2.
[0023] The polyisocyanate may include, for example, at least one selected from the group consisting of aromatic polyisocyanates, araliphatic polyisocyanates, aliphatic polyisocyanates, and alicyclic polyisocyanates.
[0024] Aromatic polyisocyanates are compounds containing an aromatic ring and two or more isocyanate groups directly bonded to the aromatic ring in the molecule. Examples of aromatic polyisocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, a 2,4-tolylene diisocyanate / 2,6-tolylene diisocyanate mixture, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, a 2,4'-diphenylmethane diisocyanate / 4,4'-diphenylmethane diisocyanate mixture, m-xylylene diisocyanate, p-xylylene diisocyanate, and 4,4'-diphenylmethane diisocyanate. Examples of suitable diisocyanates include terdiisocyanate, 2-nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane-4,4'-diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, naphthylene-1,4-diisocyanate, naphthylene-1,5-diisocyanate, and 3,3'-dimethoxydiphenyl-4,4'-diisocyanate.
[0025] Aromatic aliphatic polyisocyanates are compounds containing an aliphatic hydrocarbon group, two or more isocyanate groups directly bonded to the aliphatic hydrocarbon group, and an aromatic ring in the molecule. Examples of aromatic aliphatic polyisocyanates include 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, and mixtures thereof; 1,3-bis(1-isocyanato-1-methylethyl)benzene, 1,4-bis(1-isocyanato-1-methylethyl)benzene, and mixtures thereof; ω,ω'-diisocyanato-1,4-diethylbenzene, etc.
[0026] Aliphatic polyisocyanates are compounds that contain an aliphatic hydrocarbon group and two or more isocyanate groups directly bonded to the aliphatic hydrocarbon group in the molecule, but do not contain an aromatic ring. Examples of aliphatic polyisocyanates include hexamethylene diisocyanate, tetramethylene diisocyanate, 2-methylpentane-1,5-diisocyanate, 3-methylpentane-1,5-diisocyanate, lysine diisocyanate, trioxyethylene diisocyanate, ethylene diisocyanate, trimethylene diisocyanate, octamethylene diisocyanate, nonamethylene diisocyanate, 2,2'-dimethylpentane diisocyanate, 2,2,4-trimethylhexane diisocyanate, decamethylene diisocyanate, butene diisocyanate, 1,3-butadiene-1,4-diisocyanate, and 2,4,4-trimethylhexane diisocyanate. Examples of the isocyanate include hexamethylene diisocyanate, 1,6,11-undecane triisocyanate, 1,3,6-hexamethylene triisocyanate, 1,8-diisocyanato-4-(isocyanatomethyl)octane, 2,5,7-trimethyl-1,8-diisocyanato-5-(isocyanatomethyl)octane, bis(isocyanatoethyl)carbonate, bis(isocyanatoethyl)ether, 1,4-butylene glycol dipropyl ether-α,α'-diisocyanate, lysine diisocyanatomethyl ester, 2-isocyanatoethyl-2,6-diisocyanatohexanoate, and 2-isocyanatopropyl-2,6-diisocyanatohexanoate.
[0027] Alicyclic polyisocyanates are compounds containing an alicyclic hydrocarbon group and two or more isocyanate groups directly bonded to the alicyclic hydrocarbon group in the molecule. Examples of alicyclic polyisocyanates include isophorone diisocyanate, cyclohexyl diisocyanate, bis(isocyanatomethyl)cyclohexane, dicyclohexylmethane diisocyanate, methylcyclohexyl diisocyanate, dicyclohexyldimethylmethane diisocyanate, 2,2'-dimethyldicyclohexylmethane diisocyanate, bis(4-isocyanato-n-butylidene)pentaerythritol, and hydrogenated dimer acid diisocyanates. nate, 2-isocyanatomethyl-3-(3-isocyanatopropyl)-5-(isocyanatomethyl)bicyclo[2.2.1]heptane, 2-(isocyanatomethyl)3-(3-isocyanatopropyl)-6-(isocyanatomethyl)-bicyclo[2.2.1]heptane, 2-(isocyanatomethyl)-2-(3-isocyanatopropyl)-5-(isocyanatomethyl)bicyclo[2.2.1]heptane, 2-(isocyanatomethyl)-2-(3-isocyanatopropyl)-5-(isocyanatomethyl)bicyclo[2.2.1]heptane 2-(isocyanatomethyl)-3-(3-isocyanatopropyl)-5-(2-isocyanatoethyl)bicyclo[2.2.1]heptane, 2-(isocyanatomethyl)-3-(3-isocyanatopropyl)-6-(2-isocyanatoethyl)bicyclo[2.2.1]heptane, 2-(isocyanatomethyl)-2-(3-isocyanatopropyl)-5-(2-isocyanatoethyl)bicyclo[2.2.1]heptane Examples include bicyclo[2.2.1]heptane, 2-(isocyanatomethyl)-2-(3-isocyanatopropyl)-6-(2-isocyanatoethyl)bicyclo[2.2.1]heptane, 2,5-bis(isocyanatomethyl)bicyclo[2.2.1]heptane, hydrogenated diphenylmethane diisocyanate, norbornane diisocyanate, hydrogenated tolylene diisocyanate, hydrogenated xylene diisocyanate, and hydrogenated tetramethylxylene diisocyanate.
[0028] Examples of modified polyisocyanates include urethane modified, carbodiimide modified, polymeric, urea modified, allophanate modified, biuret modified, uretonimine modified, and uretdione modified.
[0029] The at least one (a1) selected from the group consisting of polyisocyanates and modified products thereof may include both polyisocyanates and modified products thereof.
[0030] The at least one (a1) selected from the group consisting of polyisocyanates and modified products thereof may be at least one selected from the group consisting of aromatic polyisocyanates and modified products thereof, and may include aromatic polyisocyanates and modified products thereof, since these are suitable for use as membrane sealants.
[0031] The at least one polyisocyanate (a1) selected from the group consisting of polyisocyanates and modified products thereof is suitable for use as a membrane sealant, and may therefore include at least one aromatic diisocyanate selected from the group consisting of diphenylmethane diisocyanate and modified products thereof, or may include at least one diphenylmethane diisocyanate and modified products of diphenylmethane diisocyanate.
[0032] The diphenylmethane diisocyanate may be any commonly available diphenylmethane diisocyanate (hereinafter also referred to as "MDI") monomer. The MDI monomer may include at least one selected from the group consisting of 2,2'-MDI, 2,4'-MDI, and 4,4'-MDI. In the MDI monomer, the content of 2,2'-MDI may be 0% to 5% by mass, the content of 2,4'-MDI may be 0% to 95% by mass, and the content of 4,4'-MDI may be 5% to 100% by mass, based on the total mass of the MDI monomer. MDI is defined as having 4,4'-MDI as the main component, and 2,2'-MDI and 2,4'-MDI as isomeric components.
[0033] The content of the at least one kind (a1) selected from the group consisting of polyisocyanates and modified products thereof may be 50 parts by mass or more, 60 parts by mass or more, or 70 parts by mass or more, and may be 85 parts by mass or less, or 80 parts by mass or less, relative to 100 parts by mass of the total amount of the polyisocyanate prepolymer (A).
[0034] The content of the polyisocyanate monomer in the polyisocyanate prepolymer (A) may be 20% by mass or more, 25% by mass or more, 30% by mass or more, 35% by mass or more, or 40% by mass or more, and may be 60% by mass or less, 55% by mass or less, 50% by mass or less, or 45% by mass or less, based on the total mass of the polyisocyanate prepolymer (A). The content of the polyisocyanate monomer in the polyisocyanate prepolymer (A) is measured by GPC (Gel Permeation Chromatography). Details of the measurement conditions may be as shown in the Examples.
[0035] The content of the polyisocyanate monomer in the polyurethane resin-forming composition is preferably 30.0 mass% or less, 25.0 mass% or less, 20.0 mass% or less, or 18.0 mass% or less, based on the total mass of the polyurethane resin-forming composition, since this further improves the effect of suppressing elution of low-molecular-weight reactants. The content of the polyisocyanate monomer in the polyurethane resin-forming composition may be 5.0 mass% or more, 7.0 mass% or more, 9.0 mass% or more, 11.0 mass% or more, or 13.0 mass% or more, based on the total mass of the polyurethane resin-forming composition. The content of the polyisocyanate monomer may be 5.0 to 30.0 mass%, 7.0 to 25.0 mass%, 9.0 to 20.0 mass% or more, or 11.0 to 18.0 mass%, based on the total mass of the polyurethane resin-forming composition, since this further improves the effect of suppressing elution of low-molecular-weight reactants. The content of the polyisocyanate monomer in the polyurethane resin-forming composition is measured by GPC. The detailed measurement conditions may be as shown in the examples.
[0036] <<Active hydrogen-containing compound (a2)>> The active hydrogen-containing compound (a2) may be a compound having two or more active hydrogen groups, such as a hydroxyl group, an amino group, a carboxyl group, and a thiol group.
[0037] The number of active hydrogen groups in the active hydrogen-containing compound (a2) may be 2 or more, and may be 10 or less, 8 or less, 6 or less, 4 or less, or 3 or less per molecule.
[0038] The active hydrogen-containing compound (a2) may be, for example, a polyol. A polyol is a compound having two or more hydroxyl groups. Examples of polyols include castor oil-based polyols, low-molecular-weight polyols, polyether-based polyols, polyester-based polyols, polylactone-based polyols, and polyolefin-based polyols.
[0039] Examples of castor oil-based polyols include castor oil, partially dehydrated castor oil, polymerized castor oil, diglycerides and monoglycerides of castor oil fatty acids, and reaction products of castor oil or castor oil fatty acids with other polyols. The castor oil may be, for example, refined castor oil. Partially dehydrated castor oil is castor oil from which some of the hydroxyl groups have been removed by dehydration (intramolecular dehydration). Polymerized castor oil is a polymer obtained by homopolymerizing castor oil.
[0040] The castor oil-based polyol may have a linear or branched structure. The main component of castor oil is triglyceride of ricinoleic acid. Castor oil includes hydrogenated castor oil. The main component of castor oil fatty acid is ricinoleic acid, and castor oil fatty acid includes hydrogenated castor oil fatty acid. The other polyol may be, for example, at least one selected from the group consisting of low molecular weight polyols and polyether polyols.
[0041] Examples of reaction products of castor oil or castor oil fatty acid with other polyols include mono-, di-, and triesters of castor oil fatty acid with trimethylolalkane; mono-, di-, and triesters of castor oil fatty acid with polypropylene glycol; and the like.
[0042] Examples of trimethylolalkanes include trimethylolmethane, trimethylolethane, trimethylolpropane, trimethylolbutane, trimethylolpentane, trimethylolhexane, trimethylolheptane, trimethyloloctane, trimethylolnonane, and trimethyloldecane.
[0043] The number average molecular weight of the castor oil-based polyol may be 400 or more, 500 or more, 600 or more, 700 or more, 800 or more, or 900 or more, and may be 3000 or less, 2500 or less, 2000 or less, 1500 or less, or 1000 or less. The number average molecular weight of the castor oil-based polyol is preferably 400 or more and 3000 or less, and more preferably 500 or more and 2500 or less. When the number average molecular weight of the castor oil-based polyol is 400 or more and 3000 or less, a cured resin having even better physical properties, particularly mechanical properties, required for a membrane sealing material can be formed. The number average molecular weight in this specification is the number average molecular weight measured by the method described in the Examples below.
[0044] The hydroxyl value of the castor oil-based polyol may be 20 mg KOH / g or more, 40 mg KOH / g or more, 60 mg KOH / g or more, 80 mg KOH / g or more, 100 mg KOH / g or more, 120 mg KOH / g or more, 140 mg KOH / g or more, or 150 mg KOH / g or more, and 300 mg KOH / g or less, 250 mg KOH / g or less, 200 mg KOH / g or less, or 180 mg KOH / g or less. The hydroxyl value of the castor oil-based polyol is preferably 20 mg KOH / g or more and 300 mg KOH / g or less, more preferably 40 mg KOH / g or more and 250 mg KOH / g or less. When the hydroxyl value is 20 mg KOH / g or more and 300 mg KOH / g or less, it is possible to form a cured resin that is even more excellent in the physical properties, particularly mechanical properties, required for the membrane sealing material. When the hydroxyl value is 20 mgKOH / g or more and 300 mgKOH / g or less, the productivity of the membrane sealing material, and therefore the productivity of the hollow fiber membrane module, can be further improved.
[0045] In this specification, the term "hydroxyl value" refers to the number of milligrams (mg) of potassium hydroxide equivalent to the hydroxyl groups in 1 g of sample, and is measured in accordance with JIS K1557-1.
[0046] Examples of low molecular weight polyols include dihydric polyols such as ethylene glycol, diethylene glycol, propylene glycol, 1,2-, 1,3-, or 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, neopentyl glycol, and hydrogenated bisphenol A, and trihydric to octahydric polyols such as glycerin, trimethylolpropane, hexanetriol, pentaerythritol, sorbitol, and sucrose. The molecular weight or number average molecular weight of the low molecular weight polyol is preferably 50 or more and 200 or less.
[0047] Examples of polyether polyols include alkylene oxide (alkylene oxide having 2 to 8 carbon atoms, such as ethylene oxide, propylene oxide, and butylene oxide) adducts of the above low-molecular-weight polyols, and ring-opening polymerization products of alkylene oxides. Specific examples include polypropylene glycol, polyethylene glycol, polytetramethylene ether glycol, and copolymers of ethylene oxide and propylene oxide.
[0048] The number average molecular weight of the polyether polyol is preferably 200 or more and 7000 or less, and more preferably 500 or more and 5000 or less, from the viewpoint of achieving even better molding processability during production of the membrane sealing material.
[0049] Examples of polyester polyols include polyester polyols obtained by condensation polymerization of polycarboxylic acids and polyols. Examples of polycarboxylic acids used in polyester polyols include adipic acid, azelaic acid, dodecanedioic acid, maleic acid, fumaric acid, itaconic acid, dimerized linoleic acid, phthalic acid, isophthalic acid, terephthalic acid, and other aliphatic saturated and unsaturated polycarboxylic acids, as well as aromatic polycarboxylic acids. Examples of polyols used in polyester polyols include the above-mentioned low-molecular-weight polyols and polyether polyols.
[0050] The number average molecular weight of the polyester polyol is preferably from 200 to 5000, more preferably from 500 to 3000. When the number average molecular weight of the polyester polyol is from 200 to 5000, the molding processability during the formation of the membrane sealing material is particularly excellent.
[0051] The polylactone polyol may be an addition polymerization reaction product of lactone. Examples of lactones include ε-caprolactone, α-methyl-ε-caprolactone, ε-methyl-ε-caprolactone, and β-methyl-δ-valerolactone. The addition polymerization reaction is usually carried out in the presence of a polymerization initiator and a catalyst. Examples of the polymerization initiator include glycols and triols. Examples of the catalyst include organometallic compounds, metal chelate compounds, and fatty acid metal acyl compounds.
[0052] The number average molecular weight of the polylactone polyol is preferably from 200 to 5000, more preferably from 500 to 3000. When the number average molecular weight of the polylactone polyol is from 200 to 5000, the molding processability during formation of the membrane sealing material is particularly excellent.
[0053] Examples of polyolefin polyols include polybutadiene polyols in which hydroxyl groups have been introduced at the terminals of polybutadiene or copolymers of butadiene with styrene or acrylonitrile, and also polyether ester polyols obtained by addition reaction of alkylene oxides, such as ethylene oxide and propylene oxide, with polyesters having terminal carboxyl groups and hydroxyl groups.
[0054] The active hydrogen-containing compound (a2) preferably contains a castor oil-based polyol from the viewpoint of compatibility with the polyol component (B), and more preferably contains partially dehydrated castor oil, since this further improves the effect of suppressing the elution of low-molecular-weight reaction products.
[0055] The content of the active hydrogen-containing compound (a2) may be 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, or 25 parts by mass or more, and may be 35 parts by mass or less, 30 parts by mass or less, or 27 parts by mass or less, relative to 100 parts by mass of the total amount of the polyisocyanate prepolymer (A).
[0056] <<Method for producing polyisocyanate prepolymer (A)>> The polyisocyanate prepolymer (A) can be obtained by a method including a step of reacting at least one (a1) selected from the group consisting of polyisocyanates and modified products thereof with an active hydrogen-containing compound (a2). The reaction conditions may be the same as those used in reactions for forming ordinary polyisocyanate prepolymers. The polyisocyanate prepolymer (A) can be obtained, for example, by heating a reaction mixture containing at least one (a1) selected from the group consisting of polyisocyanates and modified products thereof and the active hydrogen-containing compound (a2). The heating temperature may be, for example, 50 to 90°C or 60 to 80°C, and the heating time may be 1 to 8 hours or 3 to 5 hours. The reaction may be carried out with stirring.
[0057] <Polyol component (B)> The polyol component (B) contains a polymerized castor oil (b1) (hereinafter referred to as "component (b1)") in which some of the hydroxyl groups have been removed by a dehydration reaction. The polyol component (B) may further contain at least one member selected from the group consisting of a castor oil-based polyol (b2) (hereinafter referred to as "component (b2)") other than component (b1), a hydroxyl group-containing amine compound (b3) (hereinafter referred to as "component (b3)"), and an active hydrogen-containing compound (b4) (hereinafter referred to as "component (b4)") that does not fall under any of components (b1), (b2), and (b3).
[0058] The hydroxyl value of the polyol component (B) may be 50 mgKOH / g or more, 75 mgKOH / g or more, 100 mgKOH / g or more, or 110 mgKOH / g or more, and may be 1000 mgKOH / g or less, 750 mgKOH / g or less, 500 mgKOH / g or less, 250 mgKOH / g or less, or 200 mgKOH / g or less. The hydroxyl value of the polyol component (B) is preferably 50 mgKOH / g or more and 1000 mgKOH / g or less, more preferably 75 mgKOH / g or more and 750 mgKOH / g or less from the viewpoint of easy handling of the polyol component (B), and even more preferably 100 mgKOH / g or more and 500 mgKOH / g or less from the viewpoint of excellent molding processability and adhesive strength of the polyurethane resin.
[0059] The crosslinking group density of the polyol component (B), based on the total mass of the polyol component (B), may be 0.80 mmol / g or more, 0.90 mmol / g or more, or 1.00 mmol / g or more, and may be 1.70 mmol / g or less, 1.60 mmol / g or less, 1.50 mmol / g or less, or 1.40 mmol / g or less.
[0060] The ratio of the total number of moles of isocyanate groups in the polyisocyanate prepolymer (A) to the total number of moles of active hydrogen groups in the polyol component (B) (isocyanate groups / active hydrogen groups) may be 0.95 or more, or 1.00 or more, and may be 1.10 or less, or 1.05 or less.
[0061] The polyol component (B) preferably contains the component (b1) and at least one selected from the group consisting of the component (b2) and the component (b3). The polyol component (B) may contain only the component (b1), which will more significantly suppress the elution of low-molecular-weight reactants. The polyol component (B) may contain only the component (b1) and the component (b2), or only the component (b1), the component (b2), and the component (b3), which will further improve the filling property and / or the curing property.
[0062] <<Polymerized castor oil (b1) in which some of the hydroxyl groups have been removed by dehydration reaction>> Component (b1) may be a component obtained by polymerizing partially dehydrated castor oil or by partially dehydrating polymerized castor oil. By including component (b1), it is possible to form a membrane sealing material in which elution of low-molecular-weight reactants and solvents is suppressed, and a polyurethane resin-forming composition with excellent moldability can be obtained.
[0063] The number average molecular weight of component (b1) may be 1500 or more, 1600 or more, 1700 or more, 1800 or more, 1900 or more, or 2000 or more, and may be 3000 or less, 2800 or less, 2600 or less, 2400 or less, or 2200 or less.
[0064] The hydroxyl value of component (b1) is preferably 145 mgKOH / g or less, 140 mgKOH / g or less, 135 mgKOH / g or less, 130 mgKOH / g or less, 125 mgKOH / g or less, or 120 mgKOH / g or less, and is preferably 100 mgKOH / g or more, 105 mgKOH / g or more, or 110 mgKOH / g or more, since this further improves the effect of suppressing the amount of solvent elution.
[0065] The average functionality of component (b1) may be greater than 2.0, 2.5 or more, 3.0 or more, 3.5 or more, or 4.0 or more, and may be less than 5.4, 5.0 or less, or 4.5 or less. The average functionality of component (b1) means the average number of hydroxyl groups in one molecule of component (b1), and is calculated from the number average molecular weight and hydroxyl value of component (b1).
[0066] The crosslinking group density of component (b1) may be 0.80 mmol / g or more, 0.90 mmol / g or more, or 1.00 mmol / g or more, and may be 1.70 mmol / g or less, 1.50 mmol / g or less, 1.30 mmol / g or less, or 1.10 mmol / g or less, based on the total mass of component (b1). The crosslinking group density of component (b1) is measured by the method described in the Examples below.
[0067] The viscosity of component (b1) at 25°C may be 4500 mPa·s or less, 4000 mPa·s or less, 3500 mPa·s or less, 3000 mPa·s or less, 2500 mPa·s or less, 2000 mPa·s or less, or 1500 mPa·s or less, or may be 800 mPa·s or more, 1000 mPa·s or more, 1200 mPa·s or more, or 1400 mPa·s or more. When the viscosity of component (b1) at 25°C is within the above-mentioned range, the filling performance into a mold when forming a molded product is further improved. The viscosity of component (b1) at 25°C is the value measured using a rotational viscometer (Type B, No. 3 rotor).
[0068] The content of the (b1) component may be 80.0 mass% or less, 75.0 mass% or less, or 70.0 mass% or less, based on the total mass of the polyisocyanate prepolymer (A) and the polyol component (B). The content of the (b1) component may be 1.0 mass% or more, 5.0 mass% or more, 10.0 mass% or more, 15.0 mass% or more, 20.0 mass% or more, 25.0 mass% or more, or 30.0 mass% or more, based on the total mass of the polyisocyanate prepolymer (A) and the polyol component (B). In order to further improve the effect of suppressing elution of low-molecular-weight reactants, the content may be 35.0 mass% or more, 40.0 mass% or more, 45.0 mass% or more, 50.0 mass% or more, 55.0 mass% or more, 60.0 mass% or more, or 65.0 mass% or more. The content of component (b1) is preferably from 1.0 to 70.0 mass%, more preferably from 5.0 to 70.0 mass%, and particularly preferably from 10.0 to 70.0 mass%, based on the total mass of the polyisocyanate prepolymer (A) and the polyol component (B). When the content of component (b1) is within these ranges, even more excellent effects are achieved in suppressing the elution of low-molecular-weight reactants and solvents, improving moldability, etc.
[0069] Component (b1) can be obtained, for example, by a method including a polymerization step of polymerizing partially dehydrated castor oil to obtain component (b1). Partially dehydrated castor oil can be obtained by removing some of the hydroxyl groups of castor oil by a dehydration reaction. Commercially available partially dehydrated castor oil may be used as is. The castor oil used to obtain partially dehydrated castor oil by a dehydration reaction may be, for example, refined castor oil. Commercially available refined castor oil may be used as is. Component (b1) can be obtained, for example, by polymerizing partially dehydrated castor oil in the presence of an organic peroxide or the like.
[0070] <<Castor oil-based polyol (b2) other than component (b1)>> The component (b2) is preferably a castor oil-based polyol listed as the active hydrogen-containing compound (a2).
[0071] Component (b2) may contain at least one selected from the group consisting of castor oil, partially dehydrated castor oil, and polymerized castor oil, or may contain at least one selected from the group consisting of castor oil and partially dehydrated castor oil. When polyol component (B) further contains at least one selected from the group consisting of castor oil and partially dehydrated castor oil, the filling ability is further improved. When polyol component (B) further contains castor oil, the effect of suppressing solvent elution is further improved.
[0072] The content of the (b2) component may be 10% by mass or more, 20% by mass or more, or 30% by mass or more, and may be 50% by mass or less, 45% by mass or less, or 40% by mass or less, based on the total mass of the polyisocyanate prepolymer (A) and the polyol component (B).
[0073] <<Hydroxyl group-containing amine compound (b3)>> Component (b3) is a compound containing a hydroxyl group (-OH) and a substituted or unsubstituted amino group. When polyol component (B) contains component (b3), filling properties and curing properties are further improved. The substituted amino group is, for example, a mono-substituted amino group or a di-substituted amino group.
[0074] The number of hydroxyl groups per molecule of the hydroxyl-containing amine compound may be, for example, 1 or more, 2 or more, or 3 or more, and may be 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, or 5 or less. The total number of substituted amino groups and unsubstituted amino groups per molecule of the hydroxyl-containing amine compound may be, for example, 1 or more, or 2 or more, and may be 8 or less, 6 or less, 4 or less, or 3 or less.
[0075] Examples of the component (b3) include linear or branched alkyldiethanolamines such as butyldiethanolamine, hexyldiethanolamine, octyldiethanolamine, lauryldiethanolamine, myristyldiethanolamine, cetyldiethanolamine, and stearyldiethanolamine; low-molecular-weight polyamines having a hydroxyl group; and low-molecular-weight amino alcohols.
[0076] Component (b3) may be, for example, an oxyalkylated derivative of an amine compound, or an amino alcohol or a derivative thereof. The oxyalkylated derivative of an amine compound may be, for example, an adduct of an alkylene oxide with an alkylenediamine. Examples of adducts of an alkylene oxide with an alkylenediamine include N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine and N,N,N',N'-tetrakis[2-hydroxyethyl]ethylenediamine, which are adducts of propylene oxide or ethylene oxide with ethylenediamine. Examples of amino alcohols or derivatives thereof include monoethanolamine, diethanolamine, triethanolamine, and N-methyl-N,N'-diethanolamine.
[0077] Component (b3) is preferably a propylene oxide or ethylene oxide adduct of an amino compound such as ethylenediamine, and more preferably N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine. Use of N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine provides further benefits such as improved processability during molding and reduced elution.
[0078] The content of the (b3) component is preferably 30 parts by mass or less, 25 parts by mass or less, 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less, per 100 parts by mass of the total amount of the polyol component (B). The content of the (b3) component is preferably 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, or 7 parts by mass or more, per 100 parts by mass of the total amount of the polyol component (B). The content of the (b3) component is preferably 5 parts by mass or more and 30 parts by mass or less, and more preferably 5 parts by mass or more and 25 parts by mass or less, per 100 parts by mass of the total amount of the polyol component (B). When the content of the (b3) component is 5 parts by mass or more, per 100 parts by mass of the total amount of the polyol component (B), the (b3) component will exhibit its functions better and will exhibit even more excellent effects. When the content of the (b3) component relative to 100 parts by mass of the total amount of the polyol component (B) is 30 parts by mass or less, the reactivity is further prevented from becoming too high, the workability is further improved, the filling property is ensured, and the hardness of the obtained membrane sealing material is further prevented from becoming too high.
[0079] <<Other active hydrogen-containing compounds (b4)>> The component (b4) is a component that does not fall under either a castor oil-based polyol or a hydroxyl group-containing amine compound. As the component (b4), various polyols other than the castor oil-based polyols exemplified as the active hydrogen-containing compound (a2) can be used. Examples of the component (b4) include low-molecular-weight polyols, polyether polyols, polyester polyols, polylactone polyols, and polyolefin polyols.
[0080] The content of the (b4) component may be 15 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less, or 1 part by mass or more, or 3 parts by mass or more, relative to 100 parts by mass of the total amount of the polyol component (B).
[0081] The content of the polyol component (B) may be 80.0 mass% or less, 75.0 mass% or less, or 70.0 mass% or less, or may be 10.0 mass% or more, 20.0 mass% or more, 30.0 mass% or more, 40.0 mass% or more, 50.0 mass% or more, or 60.0 mass% or more, based on the total mass of the polyisocyanate prepolymer (A) and the polyol component (B).
[0082] The mass ratio (Mb3) / {(Mb1)+(Mb2)} of the content Mb3 of the (b3) component to the total content (Mb1+Mb2) of the (b1) component and the (b2) component is preferably 0 / 100 or more and 30 / 70 or less, and from the viewpoint of curability and filling properties, it is more preferably 5 / 95 or more and 25 / 75 or less.
[0083] The mass ratio (Mb2 / Mb4) of the content Mb2 of the component (b2) to the content Mb4 of the component (b4) is preferably 50 / 50 or more and 100 / 0 or less, and particularly preferably 100 / 0.
[0084] The polyurethane resin-forming composition may further contain a catalyst. When a catalyst is contained, the time required for curing is further shortened, the reaction temperature is lowered, and molding shrinkage of the membrane sealing material can be further suppressed.
[0085] The crosslinking group density of the polyurethane resin-forming composition may be 0.70 mmol / g or more, or 0.75 mmol / g or more, and may be 1.20 mmol / g or less, 1.10 mmol / g or less, or 1.00 mmol / g or less, based on the total mass of the polyisocyanate prepolymer (A) and the polyol component (B). The crosslinking group density of the polyurethane resin-forming composition is preferably 0.70 mmol / g or more, based on the total mass of the polyisocyanate prepolymer (A) and the polyol component (B), in order to further improve the effect of suppressing solvent elution, and more preferably 0.75 mmol / g or more and 1.20 mmol / g or less, in terms of moldability.
[0086] The polyurethane resin-forming composition can form a cured product in which the elution of low-molecular-weight reactants is suppressed. A specific example of the low-molecular-weight reactant is a low-molecular-weight component of a reaction product of glycerin and a polyisocyanate monomer (e.g., MDI monomer). The elution of the low-molecular-weight reactant is evaluated by the low-molecular-weight eluate value measured by the method described in the Examples below. The low-molecular-weight eluate value of the cured product of the polyurethane resin-forming composition may be, for example, 0.060 or less.
[0087] The polyurethane resin-forming composition can form a cured product in which solvent elution is suppressed. Specific examples of the solvent are ethanol and hexane. The solvent elution is evaluated by the ethanol extractability or hexane extractability measured by the method described in the examples below. The ethanol extractability and hexane extractability of the cured product of the polyurethane resin-forming composition may each be less than 2.0%.
[0088] The polyurethane resin-forming composition has excellent defoaming properties, curing properties, and filling properties, and therefore has excellent moldability of the cured product.
[0089] The defoaming property of the polyurethane resin-forming composition is evaluated by the foam breaking time measured by the method described in the examples below. The foam breaking time of the polyurethane resin-forming composition may be 1 minute or less.
[0090] The curability of the polyurethane resin-forming composition is evaluated by the pot life measured by the method described in the Examples below. The pot life of the polyurethane resin-forming composition may be 1700 seconds or less, or 1600 seconds or less.
[0091] The filling property of the polyurethane resin-forming composition is evaluated by the mixed viscosity of the polyurethane resin-forming composition, which is measured by the method described in the Examples below. The mixed viscosity of the polyurethane resin-forming composition refers to the viscosity measured 60 seconds after mixing the polyisocyanate prepolymer (A) and the polyol component (B) after adjusting their temperature to 25°C. The mixed viscosity of the polyurethane resin-forming composition may be 2000 mPa·s or less, 1900 mPa·s or less, 1800 mPa·s or less, or 1700 mPa·s or less, or may be 400 mPa·s or more, 600 mPa·s or more, 800 mPa·s or more, 1000 mPa·s or more, or 1200 mPa·s or more. The mixed viscosity of the polyurethane resin-forming composition is preferably 400 mPa·s or more and 2000 mPa·s or less, and from the viewpoint of excellent molding processability of the polyurethane resin, more preferably 600 mPa·s or more and 2000 mPa·s or less.
[0092] The polyurethane resin-forming composition can form a cured product having an appropriate hardness. The cured product of the polyurethane resin-forming composition has an appropriate hardness, making it easy to cut when used as a membrane sealant. The hardness of the cured product of the polyurethane resin-forming composition is measured by the method described in the examples below. The hardness of the cured product of the polyurethane resin-forming composition may be, for example, 10 to 50, or 12 to 45.
[0093] The polyurethane resin-forming composition is capable of forming a cured product that is suppressed from becoming cloudy and has excellent appearance.
[0094] A cured product of the polyurethane resin-forming composition can be obtained by a method including a step of reacting (urethanization reaction) a polyisocyanate prepolymer (A) and a polyol component (B). The polyisocyanate prepolymer (A) and the polyol component (B) are preferably reacted until a target NCO content is achieved. The reaction temperature may be 0°C to 100°C, 20°C to 80°C, 30°C to 80°C, 40°C to 80°C, 20°C to 60°C, 30°C to 60°C, or 40°C to 60°C. A reaction temperature of 40°C or higher can better suppress the crystallization of compounds (e.g., MDI monomer) that may be contained in each component. A reaction temperature of 80°C or lower can better suppress the generation of by-products.
[0095] <Membrane sealing material> A membrane sealant according to one embodiment of the present disclosure includes a cured product of the polyurethane resin-forming composition described above.
[0096] The membrane sealant can be produced by a method including a curing step of curing a polyurethane resin-forming composition in a mold. The polyurethane resin-forming composition described above has excellent moldability, making it easy to inject into a mold and mold (e.g., centrifugal molding) within the mold. Furthermore, the cured product of the polyurethane resin-forming composition described above also has appropriate hardness, making it easy to perform processes such as cutting after removing the cured product from the mold. Additionally, the membrane sealant containing the cured product of the polyurethane resin-forming composition described above is suitable for use as a medical membrane sealant (potting agent) in plasma separation devices, artificial lungs, artificial kidneys, artificial livers, etc., because elution of low-molecular-weight reactants and solvents is suppressed.
[0097] <Membrane module> A membrane module according to one embodiment of the present disclosure includes a main body, a membrane, and the above-described membrane sealing material. The membrane may be a plurality of hollow fiber membranes. The membrane sealing material seals the gap between the main body and the membrane. It is preferable that the membrane sealing material seals the gap between the main body and at least some of the plurality of hollow fiber membranes, and at least some of the gaps between the plurality of hollow fiber membranes.
[0098] Next, a membrane module according to an embodiment of the present disclosure will be described in more detail with reference to the drawings. Fig. 1 is a conceptual diagram showing an example of the configuration of a membrane module according to an embodiment of the present disclosure. The membrane module (hollow fiber membrane module) 100 shown in Fig. 1 includes a housing (main body) 11, the interior of which is filled with a plurality of hollow fiber membranes (membranes) 13. For example, in the case of a hollow fiber membrane module used as a dialyzer, several thousand to several tens of thousands of hollow fiber membranes are filled.
[0099] The housing 11 has a cylindrical shape. Membrane seals 19 are provided at both ends (both left and right ends in FIG. 1 ) inside the housing 11. The membrane seals fill and seal the gaps between the hollow fiber membranes 13 and the gaps between the hollow fiber membranes 13 and the inner wall of the housing 11, and also bind the multiple hollow fiber membranes 13 together.
[0100] A first fluid inlet 15 and a first fluid outlet 17 are provided on the side of the housing 11. A first fluid (gas or liquid) flows in and out of the housing 11 through the first fluid inlet 15 and the first fluid outlet 17. The first fluid that flows in through the first fluid inlet 15 comes into contact with the plurality of hollow fiber membranes 13 packed in the housing 11, passes through the gaps (outside the hollow fiber membranes) between them, and is discharged through the first fluid outlet 17. Because no membrane sealant 19 is present inside the hollow fiber membranes 13, a second fluid (gas or liquid) flows in and out of the hollow fiber membranes 13 through a second inlet (one end) and a second outlet (the other end) provided in a cap member (not shown). When the first fluid and the second fluid come into contact with each other through the hollow fiber membranes 13, mass transfer occurs from one fluid to the other fluid (or from the other fluid to the first fluid). For example, in the case of a hollow fiber membrane type dialyzer, waste products and excess water in the blood are transferred to the dialysate when the dialysate comes into contact with the blood.
[0101] The membrane module 100 shown in FIG. 1 includes multiple hollow fiber membranes 13, with membrane seals 19 sealing the gaps at both ends of the membranes; however, the membrane module according to this embodiment is not limited to this configuration. For example, the membranes may be single or multiple membranes having various shapes, such as flat membranes or spiral membranes. The membrane seals are not limited to being provided at both ends of the membrane, but may be provided only on a portion of the membrane (one end in the case of a hollow fiber membrane), or on the entire membrane end, for example, the entire outer edge of a flat membrane. The seals may be provided on a portion of the membrane other than the ends to seal it. The housing 11 of the membrane module 100 shown in FIG. 1 has a cylindrical shape, but may have any shape other than a cylindrical shape.
[0102] The membrane module 100 can be manufactured by sealing the gaps between the hollow fiber membranes 13 at the end of a bundle of multiple hollow fiber membranes 13 with the above-mentioned polyurethane resin-forming composition for membrane sealing material, and curing the composition to form the above-mentioned membrane sealing material (the gaps between the hollow fiber membranes are sealed by the membrane sealing material).
[0103] The membrane module according to an embodiment of the present disclosure is suitable for use as a medical module or a water treatment module because it suppresses the elution of low-molecular-weight reactants and solvents. Specific examples of the membrane module include plasma separation devices, artificial lungs, artificial kidneys, artificial livers, and household and industrial water treatment devices. [Example]
[0104] The present invention will be described below based on examples, but the present invention should not be construed as being limited to these examples. In the following, "%" means "% by mass" unless otherwise specified.
[0105] The following components were used in the examples and comparative examples.
[0106] [Polyisocyanate prepolymer (A)] ·a1-1; 4,4'-MDI (manufactured by Tosoh Corporation, product name Millionate MT, Isocyanate group content = 33.6%, Carbodiimide-uretonimine modified substance content: 0%, isomer content: approx. 1%, Crosslinking group density=0mmol / g) ·a1-2; Carbodiimide-modified 4,4'-MDI (Tosoh Corporation, Product name: Millionate MTL-C, isocyanate group content = 28.6%, Carbodiimide-uretonimine modified substance content: 30%, isomer content: approximately 1% Crosslinking group density=0.45mmol / g) a2: Castor oil (manufactured by Ito Oil Mills, product name URIC H-30, Number average molecular weight = 938, Hydroxyl value (OHV) = 160 mg KOH / g, viscosity (25°C) = 690 mPa·s, Crosslinking group density=0.74mmol / g, Average number of functional groups=2.7)
[0107] [Polyol component (B)] ·b1-1; Castor oil (manufactured by Ito Oil Mills, product name URIC H-30) ·b1-2; Partially dehydrated castor oil (manufactured by Ito Oil Mills, Number average molecular weight 950, Hydroxyl value (OHV) = 119 mg KOH / g, viscosity (25°C) = 420 mPa·s, Crosslinking group density=0mmol / g, Average number of functional groups=2) ·b1-3; Polymerized castor oil (manufactured by Ito Oil Mills, product name: Polycaster #30, Number average molecular weight=1991 Hydroxyl value (OHV) = 155 mg KOH / g, viscosity (25°C) = 4800 mPa·s, Crosslinking group density=1.84mmol / g, Average number of functional groups=5.4) ·b1-4; Dehydrated castor oil polymerized polyol (manufactured by Ito Oil Mills, number average molecular weight 2000, Hydroxyl value (OHV) = 115 mg KOH / g, viscosity (25°C) = 1460 mPa·s, Crosslinking group density=1.05mmol / g, Average number of functional groups=4.1) ·b2-1; N,N,N',N'-Tetrakis[2-hydroxypropyl]ethylenediamine (ADEKA, product name EDP-300, hydroxyl value (OHV) = 760 mg KOH / g, Viscosity (25℃) = 50000mPa s, crosslinking group density = 2.63mmol / g)
[0108] <Production of dehydrated castor oil polymerized polyol (b1-4)> A 2-liter four-neck flask equipped with a stirrer, thermometer, heating device, and dropping funnel was charged with 600 parts by mass of castor oil (manufactured by Ito Oil Mills, product name URIC H-30) and 0.9 parts by mass of acidic sodium sulfite, and heated under reduced pressure. The mixture was allowed to react at 230°C for 1 hour, and then clay was added at 150°C, followed by filtration and purification to obtain partially dehydrated castor oil. The hydroxyl value of the resulting partially dehydrated castor oil was 119 mgKOH / g.
[0109] 1,000 parts by mass of partially dehydrated castor oil was added to a 2-liter four-neck flask equipped with a stirrer, thermometer, heating device, and dropping funnel, and the temperature was raised to 140°C under a nitrogen stream. While blowing in nitrogen gas, 160 parts by mass of di-t-butyl peroxide was added dropwise over 30 minutes, and the temperature was raised to 150°C and allowed to react for 4 hours. The decomposition product was then recovered under reduced pressure for 1 hour, and the mixture was filtered and purified at 120°C with the addition of white clay to obtain a polymerized castor oil (b1) in which some of the hydroxyl groups had been removed by a dehydration reaction. The hydroxyl value of the resulting dehydrated castor oil polymerized polyol (b1-4) was 115 mgKOH / g. The dehydrated castor oil polymerized polyol corresponds to the polymerized castor oil (b1) in which some of the hydroxyl groups had been removed by a dehydration reaction.
[0110] <Measurement of number average molecular weight> The number average molecular weight was determined by GPC measurement under the following conditions and method.
[0111] (Measurement conditions for number average molecular weight) (1) Measuring device: "HLC-8120 (product name)" (manufactured by Tosoh Corporation) (2) Column: Four columns packed with two columns of TSKgel G2000HXL and two columns of TSKgel G3000HXL (both trade names, manufactured by Tosoh Corporation) were connected in series. (3) Column temperature: 40°C (4) Detector: RI (refractive index) meter (5) Eluent: tetrahydrofuran (THF) (flow rate: 1 mL / min., 40°C) (6) Calibration curve: A calibration curve was obtained using the following trifunctional polypropylene polyols (all manufactured by Sanyo Chemical Industries, Ltd.). "Sannix GP-250" (number average molecular weight = 250) "Sannix GP-400" (number average molecular weight = 400) "Sannix GP-600" (number average molecular weight = 600) "Sannix GP-1000" (number average molecular weight = 1000) "Sannix GP-3000" (number average molecular weight = 3000) "Sannix GP-4000" (number average molecular weight = 4000) "Sannix GP-5000" (number average molecular weight = 5000) (7) Sample solution: 0.05 g of sample in 10 mL of THF
[0112] <Measurement of hydroxyl value> The hydroxyl value is a value measured by a method using an acetylating reagent in accordance with JIS K1557-1.
[0113] <Calculation of crosslinking group density> The crosslinking group densities shown in Tables 1 to 5 were calculated using the following formula from the number of functional groups and hydroxyl value disclosed by each raw material manufacturer, as well as the number average molecular weight obtained by GPC measurement.
[0114] (Formula 1) Crosslinking group density (mmol / g)={1000×(average number of functional groups-2)} / number average molecular weight (Equation 2) Crosslinking group density (mmol / g) = {Hydroxyl value × (average number of functional groups - 2) / (56.11 × average number of functional groups)}
[0115] <Preparation of Polyisocyanate Prepolymer (A)> The raw materials shown in Table 1 were charged according to the compounding ratio, and reacted by stirring and mixing at 70° C. for 4 hours to obtain a polyisocyanate prepolymer (A-1).
[0116] [Table 1]
[0117] <Preparation of Polyol Component (B)> The raw materials shown in Table 2 were charged according to the blending ratio, and the mixture was stirred and mixed uniformly to obtain polyol-containing components (B-1) to (B-8).
[0118] [Table 2]
[0119] <Preparation and Evaluation of Urethane Resin-Forming Composition> Urethane resin-forming compositions were prepared and molded using the formulations shown in Tables 3 and 4. The values shown in Tables 3 and 4 were calculated from the following test results.
[0120] [NCO content measurement] In the polyisocyanate prepolymer (A-1) shown in Table 1, the NCO content was measured in accordance with JIS K1603-1:2007.
[0121] [Measurement of monomer content in polyisocyanate (MDI)] In the polyisocyanate prepolymer (A-1) shown in Table 1, the content (mass %) of the polyisocyanate (MDI) monomer was determined by GPC measurement under the following conditions and by the following method.
[0122] (Measurement conditions) (1) Measuring device: "HLC-8120 (product name)" (manufactured by Tosoh Corporation) (2) Column temperature: 40°C (3) Detector: RI (refractive index) meter (4) Column: Measurements were performed by connecting columns packed with three types of packing materials, TSKgel G3000HXL, TSKgel G2000HXL, and TSKgel G1000HXL (all trade names, manufactured by Tosoh Corporation), in series. (5) Eluent: tetrahydrofuran (THF) (flow rate: 1 mL / min, 40°C) (6) Calibration curve: A calibration curve was obtained using the following grades of polystyrene (TSK standard POLYSTYRENE). F-2 (molecular weight: 1.81×10 4 ) F-1 (molecular weight: 1.02×10 4 ) A-5000 (molecular weight: 5.97×10 3 ) A-2500 (molecular weight: 2.63×10 3 ) A-500 (molecular weight: 6.82×10 2 , 5.78×10 2 , 4.74×10 2 , 3.70×10 2 , 2.66×10 2 ) Toluene (molecular weight: 92) (7) Sample: 0.05 g of sample in 10 mL of THF solution
[0123] (Measurement method) A calibration curve was prepared from a chart obtained by detecting refractive index difference using polystyrene as a standard substance. Next, for each sample, the mass percentage of the peak near the peak top molecular weight (number average molecular weight) of 230, which indicates polyisocyanate monomer (MDI), was calculated from the chart obtained by detecting refractive index difference based on the same calibration curve.
[0124] [Evaluation of formability] Moldability was evaluated based on defoaming, filling, and curing properties. Filling was evaluated by measuring the mixed viscosity, and curing was evaluated by a pot life test. Moldability was evaluated as good when all of defoaming, filling, and curing properties were good.
[0125] (Defoaming property) In Examples 1 to 3 and Comparative Examples 1 to 5, the defoaming ability of the polyurethane resin-forming compositions was determined by the following method. The polyisocyanate prepolymer (A) and the polyol component (B), whose temperature had been adjusted to 25°C in advance, were weighed out to a total of 100 g in a ratio of isocyanate group / active hydrogen group of 1.00 to 1.05 (molar ratio), mixed with a spatula for 30 seconds, and vacuum degassed at 50 mmHg. The time until the bubbles broke was measured, and if the time taken for the bubbles to break was within 1 minute, the degassing ability was judged to be good.
[0126] (Mixed viscosity and pot life test) In Examples 1 to 3 and Comparative Examples 1 to 5, the mixed viscosity at 25° C. and pot life of the polyisocyanate prepolymer (A) and the polyol component (B) were determined by the following methods. Polyisocyanate prepolymer (A) and polyol component (B), previously adjusted to 25°C, were weighed and mixed to a total of 50 g at a molar ratio of isocyanate group / active hydrogen group of 1.00 to 1.05 to obtain a mixture. The viscosity of the mixture was then measured using a rotational viscometer (Type B, No. 4 rotor) at 25°C. The viscosity measured 60 seconds after the start of mixing polyisocyanate prepolymer (A) and polyol component (B) was defined as the mixed viscosity. The pot life (seconds) was defined as the time from the start of mixing polyisocyanate prepolymer (A) and polyol component (B) until the viscosity of the mixture reached 50,000 mPa·s. A mixed viscosity of 2,000 mPa·s or less at 25°C was considered to have good filling properties. A pot life of 1,700 seconds or less was considered to have good curability.
[0127] [Measurement of low molecular weight extractables] (Preparation of samples for low molecular weight dissolution tests) The polyisocyanate prepolymer (A) and polyol component (B) were blended in the combinations shown in Tables 3 and 4 at a liquid temperature of 45°C, with an isocyanate group / active hydrogen group molar ratio of 1.00 to 1.05 and a total mass of 30 g to obtain a mixed solution. The resulting mixed solution was then stirred for 15 seconds. 10 g of glycerin was then added and stirred for 15 seconds to obtain a cured polyurethane resin-forming composition. The glycerin simulated the glycerin contained in the hollow fibers. The resulting cured product was left to stand in a thermostatic chamber for a primary cure of 50°C for 10 minutes and a secondary cure of 45°C for 2 days. This yielded a sample for a low-molecular-weight elution test.
[0128] (Low molecular weight dissolution test) The low-molecular-weight eluate values of the cured products of the polyurethane resin-forming compositions of Examples 1 to 3 and Comparative Examples 1 to 5 were measured by the following method. First, 20 g of each of the samples for the low-molecular-weight elution test obtained in each Example and Comparative Example was cut into a fan shape and weighed. The samples were immersed in 100 ml of purified water preheated to 40°C and left at 40°C for 2 hours to extract low-molecular-weight reactants into the purified water. Next, 10 ml of the resulting extract was decanted into a 50 ml measuring flask, and the resulting solution was adjusted to 50 ml with purified water to prepare a test solution. The UV absorbance of the test solution was then measured (Shimadzu Corporation, product name UV-1500). The low-molecular-weight elution value was determined to be one-tenth of the maximum absorbance value at 240 to 245 nm. A low-molecular-weight elution value of 0.060 or less indicates that low-molecular-weight reactants (eluates) are present.
[0129] [Solvent extraction rate measurement] (Preparation of samples for solvent extraction tests) The polyisocyanate prepolymer (A) and polyol component (B) were weighed out in the combinations shown in Tables 3 and 4, at a liquid temperature of 25°C, with an isocyanate group / active hydrogen group molar ratio of 1.00 to 1.05, for a total mass of 100 g, and mixed with a spatula for 30 seconds. The mixture was vacuum degassed at 50 mmHg for 60 seconds. After degassing, the mixture was spread on release paper to form a 1 mm thick sheet, which was then left to stand in a thermostatic chamber at 45°C for 2 days. This yielded a sample for solvent extraction testing.
[0130] (Solvent extraction test) The solvent extraction rates of the cured products of the polyurethane resin-forming compositions of Examples 1 to 3 and Comparative Examples 1 to 5 were measured by the following method. First, the solvent extraction test samples obtained in each Example and Comparative Example were cut into 10 mm squares. Next, 10 g of the cut sample and 100 g of ethanol or hexane were placed in a 200 ml sample bottle, sealed, and shaken at 50°C for 48 hours. After shaking, the bottle was further filtered, and the extract was collected in a 300 ml recovery flask and evaporated to dryness. The ethanol extraction rate and hexane extraction rate were then calculated using the following formula. Ethanol extraction rate (%) or hexane extraction rate (%) = {Eggplant flask mass after evaporation (g) - Empty eggplant flask mass (g)} / Sample mass (g) × 100 It is preferable that the ethanol extraction rate and the hexane extraction rate are each less than 2.0%.
[0131] [Hardness (10-second value) evaluation] The polyisocyanate prepolymer (A) and polyol component (B), previously adjusted to a temperature of 25°C, were weighed out to a total of 50 g, with a molar ratio of isocyanate groups to active hydrogen groups of 1.00 to 1.05. The mixture was mixed with a spatula for 30 seconds and then vacuum-degassed at 50 mmHg for 60 seconds. 30 g of the degassed mixture was transferred to a 100 ml plastic cup and cured at 45°C for 48 hours. The cured product was removed from the plastic cup and left in an environment at 25°C for 4 hours, after which the hardness was measured using a Durometer D hardness tester. The reading after 10 seconds of pressing the hardness tester against the sample was recorded as the hardness (10-second value).
[0132] [Appearance evaluation] The appearance of the cured products of the polyurethane resin-forming compositions of Examples 1 to 3 and Comparative Examples 1 to 5 was evaluated as follows. The polyisocyanate prepolymer (A) and polyol component (B), previously adjusted to 25°C, were weighed out to a total of 100 g, with a molar ratio of isocyanate groups to active hydrogen groups of 1.00 to 1.05. The mixture was mixed with a spatula for 30 seconds, degassed under vacuum at 50 mmHg, and then poured into a stainless steel mold. The mixture was left to cure at 45°C for two days and then demolded to obtain a cured product. The appearance of the resulting cured product was visually evaluated; clear materials were rated "A" and cloudy materials were rated "C."
[0133] In Tables 3 and 4, the "crosslinking group density (mmol / g)," "polyisocyanate monomer content (%)," and "dehydrated castor oil polymerized polyol content (%)" are amounts based on the total mass of the polyurethane resin-forming composition.
[0134] [Table 3] [Table 4] [Explanation of symbols]
[0135] 11...Main body portion, 13...Hollow fiber membrane, 15...First fluid inlet, 17...First fluid outlet, 19...Membrane seal material, 100...Membrane module (hollow fiber membrane module)
Claims
1. A polyisocyanate prepolymer (A), A polyol component (B), The polyurethane resin-forming composition for a membrane sealing material, wherein the polyol component (B) contains a polymerized castor oil (b1) in which a portion of the hydroxyl groups has been removed by a dehydration reaction.
2. 2. The polyurethane resin-forming composition for a membrane sealing material according to claim 1, wherein the polymerized castor oil (b1) from which a portion of the hydroxyl groups has been removed by a dehydration reaction has a number average molecular weight of 1,500 or more.
3. The polyurethane resin-forming composition for membrane sealing material according to claim 1 or 2, wherein the content of the polymerized castor oil (b1) from which a part of the hydroxyl groups has been removed by a dehydration reaction is 70.0 mass% or less based on the total mass of the polyurethane resin-forming composition for membrane sealing material.
4. The polyisocyanate prepolymer (A) is At least one (a1) selected from the group consisting of aromatic diisocyanates and modified products thereof; The polyurethane resin-forming composition for a membrane sealant according to claim 1 or 2, comprising a reaction product of an active hydrogen-containing compound (a2) and an active hydrogen-containing compound (a3).
5. The polyurethane resin-forming composition for a membrane sealant according to claim 4, wherein the aromatic diisocyanate is diphenylmethane diisocyanate.
6. 3. The polyurethane resin-forming composition for a membrane sealing material according to claim 1 or 2, wherein the polymerized castor oil (b1) from which a portion of the hydroxyl groups has been removed by a dehydration reaction has a hydroxyl value of 145 mgKOH / g or less.
7. The polyurethane resin-forming composition for membrane sealing material according to claim 1 or 2, wherein the polyol component (B) further comprises a castor oil-based polyol (b2) other than the polymerized castor oil (b1) in which a portion of the hydroxyl groups has been removed by a dehydration reaction.
8. The polyol component (B) further contains a hydroxyl group-containing amine compound (b3), 3. The polyurethane resin-forming composition for a membrane sealing material according to claim 1 or 2, wherein the content of the hydroxyl group-containing amine compound (b3) is 30 parts by mass or less per 100 parts by mass of the total amount of the polyol component (B).
9. A membrane sealant comprising a cured product of the polyurethane resin-forming composition for a membrane sealant according to claim 1 or 2.
10. Main body, Membrane, and A membrane module comprising the membrane seal material according to claim 9 which seals a gap between the main body and the membrane.
11. The membrane is a plurality of hollow fiber membranes, The membrane sealant is A gap between the main body and at least a portion of the plurality of hollow fiber membranes, and The membrane module according to claim 10 , wherein at least a portion of the gaps between the plurality of hollow fiber membranes are sealed.
Citation Information
Patent Citations
Production of polymer of castor oil compound having small number of functional groups
JP1989129097A
Curable resin composition and sealing material
JP2007297532A
Urethane resin-forming composition for sealing material of membrane module
JP2011068886A
Polyurethane resin formative composition for membrane-sealing material, and membrane-sealing material and membrane module using the same
JP2019026837A
Formative composition of polyurethane resin for membrane seal material, and membrane seal material and membrane module using the composition
JP2021020135A