Polycarbonate resin composition
The polycarbonate resin composition with a graft copolymer and arylphosphine oxide/phosphine improves weather resistance and impact resistance, addressing hue deterioration and outdoor discoloration issues.
Patent Information
- Application Number
- JP2023052716
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Polycarbonate resin lacks sufficient weather resistance, which limits its use due to discoloration and strength loss under outdoor or fluorescent light conditions, and incorporating ultraviolet absorbers worsens hue deterioration during processing.
A polycarbonate resin composition containing 55 to 90% polycarbonate resin with specific molecular weights, combined with a graft copolymer, arylphosphine oxide, and arylphosphine in precise ratios, enhances weather resistance, impact resistance, and fluidity.
The composition achieves high weather resistance, impact resistance, and moldability, suitable for various applications.
Smart Images

Figure 2024141202000001 
Figure 2024141202000002 
Figure 2024141202000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polycarbonate resin composition, and more particularly to a polycarbonate resin composition having excellent weather resistance and a molded article thereof. [Background technology]
[0002] Polycarbonate resin has excellent mechanical properties such as impact resistance, as well as excellent heat resistance and transparency, and is therefore widely used in a wide range of applications, including various optical components, electrical and electronic equipment components, automotive interior and exterior parts, office equipment components, sheets, machine parts, and building materials. However, polycarbonate resins do not have sufficient weather resistance, and for example, when used outdoors or indoors under fluorescent light, discoloration or loss of strength of the product is observed, so that their use is somewhat limited.
[0003] For this reason, various light stabilizers have been used either alone or in combination, and it is known to incorporate ultraviolet absorbers such as benzotriazoles. However, when such ultraviolet absorbers are incorporated into polycarbonate resin, there is a problem that the color of the polycarbonate resin composition deteriorates due to thermal degradation during melt kneading and molding processing. Various additives have also been incorporated to enhance functionality. For example, Patent Document 1 describes that a fiber-reinforced polycarbonate resin composition having excellent dimensional stability, mechanical strength, and fluidity can be obtained by mixing 5 to 15 mass% of triphenyl phosphate with 85 to 95 mass% of polycarbonate resin.
[0004] In recent years, with the rapid progress in improving the functionality and performance of various devices, there is a strong demand for polycarbonate resins, particularly for improved weather resistance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 3308657 Summary of the Invention [Problem to be solved by the invention]
[0006] An object (object) of the present invention is to provide a polycarbonate resin composition having excellent weather resistance, good impact resistance, heat resistance and fluidity (moldability). [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors have conducted intensive research to achieve the above object, and as a result have found that a polycarbonate resin composition containing small amounts of an arylphosphine oxide and an arylphosphine in a specific quantitative ratio in a resin alloy with a graft polymer such as ABS resin has excellent weather resistance while having good impact resistance and heat resistance, and have thus completed the present invention. The present invention relates to the following polycarbonate resin composition and molded article.
[0008] 1. For a total of 100 parts by mass of (A) and (B) containing 55 to 90% by mass of a polycarbonate resin (A) having a viscosity average molecular weight of 17,500 to 30,000 and 10 to 45% by mass of a graft copolymer (B) containing an aromatic vinyl monomer component (b1), a vinyl cyanide monomer component (b2) and a diene rubber polymer component (b3), A polycarbonate resin composition comprising 0.001 to 0.3 parts by mass of an arylphosphine oxide (C) and 0.001 to 0.3 parts by mass of an arylphosphine (D), wherein the mass ratio (D) / (C) of the contents of the arylphosphine (D) to the arylphosphine oxide (C) is 0.003 or more and 4 or less. 2. The polycarbonate resin composition according to the above 1, wherein the arylphosphine oxide (C) is triphenylphosphine oxide. 3. The polycarbonate resin composition according to the above 1, wherein the arylphosphine (D) is triphenylphosphine. 4. Pellets of the polycarbonate resin composition according to any one of 1 to 3 above. 5. A molded article made of the polycarbonate resin composition according to any one of 1 to 3 above. 6. A molded article comprising pellets of the polycarbonate resin composition described in 4 above. Effect of the Invention
[0009] The polycarbonate resin composition of the present invention has a high degree of weather resistance, and is excellent in impact resistance, heat resistance, and fluidity (moldability). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the present invention will be described in detail with reference to embodiments and examples. In this specification, unless otherwise specified, the symbol "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit.
[0011] The polycarbonate resin composition of the present invention contains 55 to 90 mass% of a polycarbonate resin (A) having a viscosity average molecular weight of 17,500 to 30,000, and 10 to 45 mass% of a graft copolymer (B) containing an aromatic vinyl monomer component (b1), a vinyl cyanide monomer component (b2), and a diene rubber polymer component (b3), and the composition comprises, per 100 parts by mass of the total of (A) and (B), The composition is characterized in that it contains 0.001 to 0.3 parts by mass of arylphosphine oxide (C) and 0.001 to 0.3 parts by mass of arylphosphine (D), and the mass ratio (D) / (C) of the content of the arylphosphine (D) to the arylphosphine oxide (C) is 0.003 or more and 4 or less.
[0012] [Polycarbonate resin (A)] The polycarbonate resin (A) used in the present invention is not limited in type, and may be used alone or in any combination of two or more kinds in any ratio. Polycarbonate resins can be classified into aromatic polycarbonate resins in which the carbons directly bonded to the carbonate bonds are aromatic carbons, and aliphatic polycarbonate resins in which the carbons directly bonded to the carbonate bonds are aliphatic carbons, and either of these can be used. Among these, aromatic polycarbonate resins are preferred as the polycarbonate resin (A) from the viewpoints of heat resistance, mechanical properties, electrical properties, etc.
[0013] Among the monomers that are raw materials for aromatic polycarbonate resins, examples of aromatic dihydroxy compounds include: Dihydroxybenzenes such as 1,2-dihydroxybenzene, 1,3-dihydroxybenzene (i.e., resorcinol), and 1,4-dihydroxybenzene; Dihydroxybiphenyls such as 2,5-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl, and 4,4'-dihydroxybiphenyl;
[0014] dihydroxynaphthalenes such as 2,2'-dihydroxy-1,1'-binaphthyl, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, and 2,7-dihydroxynaphthalene;
[0015] dihydroxydiaryl ethers such as 2,2'-dihydroxydiphenyl ether, 3,3'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 1,4-bis(3-hydroxyphenoxy)benzene, and 1,3-bis(4-hydroxyphenoxy)benzene;
[0016] 2,2-bis(4-hydroxyphenyl)propane (i.e., bisphenol A), 1,1-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane (i.e., bisphenol C), 2,2-bis(3-methoxy-4-hydroxyphenyl)propane, 2-(4-hydroxyphenyl)-2-(3-methoxy-4-hydroxyphenyl)propane, 1,1-bis(3-t-butyl-4-hydroxyphenyl)propane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 2,2-bis(3-cyclohexyl-4-hydroxyphenyl)propane, 2-(4-hydroxyphenyl)-2-(3-cyclohexyl-4-hydroxyphenyl)propane, α,α'-bis(4-hydroxyphenyl)-1,4-diisopropylbenzene, 1,3-bis[2-(4-hydroxyphenyl)-2-propyl]benzene, bis(4-hydroxyphenyl)methane, Bis(4-hydroxyphenyl)cyclohexylmethane, Bis(4-hydroxyphenyl)phenylmethane, Bis(4-hydroxyphenyl)(4-propenylphenyl)methane, Bis(4-hydroxyphenyl)diphenylmethane, Bis(4-hydroxyphenyl)naphthylmethane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)-1-naphthylethan, 1,1-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis(4-hydroxyphenyl)hexane, 2,2-bis(4-hydroxyphenyl)hexane, 1,1-bis(4-hydroxyphenyl)octane, 2,2-bis(4-hydroxyphenyl)octane, 4,4-bis(4-hydroxyphenyl)heptane, 2,2-bis(4-hydroxyphenyl)nonane, 1,1-bis(4-hydroxyphenyl)decane, 1,1-bis(4-hydroxyphenyl)dodecane, Bis(hydroxyaryl)alkanes such as;
[0017] 1,1-bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3-dimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,4-dimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,5-dimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxy-3,5-dimethylphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3-propyl-5-methylcyclohexane, 1,1-bis(4-hydroxyphenyl)-3-t-butyl-cyclohexane, 1,1-bis(4-hydroxyphenyl)-4-t-butyl-cyclohexane, 1,1-bis(4-hydroxyphenyl)-3-phenylcyclohexane, 1,1-bis(4-hydroxyphenyl)-4-phenylcyclohexane, Bis(hydroxyaryl)cycloalkanes such as;
[0018] 9,9-bis(4-hydroxyphenyl)fluorene, Cardo structure-containing bisphenols such as 9,9-bis(4-hydroxy-3-methylphenyl)fluorene;
[0019] 4,4'-dihydroxydiphenyl sulfide, Dihydroxydiaryl sulfides such as 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfide; Dihydroxydiaryl sulfoxides such as 4,4'-dihydroxydiphenyl sulfoxide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide; 4,4'-dihydroxydiphenyl sulfone, dihydroxydiarylsulfones such as 4,4'-dihydroxy-3,3'-dimethyldiphenylsulfone; etc.
[0020] Of these, bis(hydroxyaryl)alkanes are preferred, and bis(4-hydroxyphenyl)alkanes are particularly preferred. In particular, from the standpoint of impact resistance and heat resistance, 2,2-bis(4-hydroxyphenyl)propane (i.e., bisphenol A) and 2,2-bis(3-methyl-4-hydroxyphenyl)propane (i.e., bisphenol C) are preferred. The aromatic dihydroxy compounds may be used alone or in any combination of two or more in any ratio.
[0021] Among the monomers that are raw materials for polycarbonate resins, examples of carbonate precursors include carbonyl halides, carbonate esters, etc. The carbonate precursors may be used alone or in any combination and ratio of two or more.
[0022] Specific examples of carbonyl halides include phosgene; haloformates such as bischloroformates of dihydroxy compounds and monochloroformates of dihydroxy compounds; and the like.
[0023] Specific examples of carbonate esters include diaryl carbonates such as diphenyl carbonate and ditolyl carbonate; dialkyl carbonates such as dimethyl carbonate and diethyl carbonate; biscarbonates of dihydroxy compounds, monocarbonates of dihydroxy compounds, and carbonates of dihydroxy compounds such as cyclic carbonates.
[0024] The method for producing the polycarbonate resin (A) is not particularly limited, and any method can be adopted. Examples of the method include interfacial polymerization, melt transesterification, pyridine method, ring-opening polymerization of cyclic carbonate compounds, and solid-phase transesterification of prepolymers. Among these, the interfacial polymerization and melt transesterification methods are preferred because they have a higher effect of improving resistance to moist heat, and the interfacial polymerization method is particularly preferred.
[0025] The polycarbonate resin (A) used has a viscosity average molecular weight (Mv) in the range of 17500 to 30000. By using a polycarbonate resin having a viscosity average molecular weight (Mv) in such a range and containing an arylphosphine oxide (C) and an arylphosphine (D), a polycarbonate resin composition having good impact resistance, heat resistance, and fluidity (moldability) and excellent weather resistance can be obtained. When a polycarbonate resin having an Mv of less than 17500 is used, the impact resistance is insufficient, the weather resistance is deteriorated, and the heat resistance is likely to decrease. When a polycarbonate resin having an Mv of more than 30000 is used, the fluidity is likely to decrease, and high-temperature molding at 300°C or higher is required, which causes thermal degradation of the graft copolymer (B) and tends to deteriorate the impact resistance. The viscosity average molecular weight (Mv) is preferably 18,000 or more, particularly 18,500 or more, 19,000 or more, or 19,500 or more, and particularly preferably 20,000 or more, and is preferably 29,000 or less, and more preferably 26,000 or less. Two or more polycarbonate resins having different viscosity average molecular weights may be mixed and used. In this case, a polycarbonate resin having a viscosity average molecular weight outside the above range may be mixed to adjust the viscosity average molecular weight within the above range.
[0026] The viscosity average molecular weight Mv of the polycarbonate resin (A) is calculated by measuring the intrinsic viscosity [η] (unit: dl / g) at 25°C using methylene chloride as a solvent and an Ubbelohde viscometer, and then calculating the viscosity average molecular weight Mv using the Schnell viscosity formula, i.e., η = 1.23 × 10 -4 Mv 0.83 The intrinsic viscosity [η] is the value calculated from the specific viscosity [η sp ] was measured and the value was calculated according to the following formula.
number
[0027] In order to improve the appearance and flowability of the molded article, the polycarbonate resin (A) may contain a polycarbonate oligomer. The viscosity average molecular weight [Mv] of this polycarbonate oligomer is usually 1500 or more, preferably 2000 or more, and usually 9500 or less, preferably 9000 or less. Furthermore, the amount of the polycarbonate oligomer contained is preferably 30% by mass or less of the polycarbonate resin (including the polycarbonate oligomer).
[0028] Furthermore, the polycarbonate resin (A) may be not only a virgin raw material but also a polycarbonate resin regenerated from a used product (so-called material recycled polycarbonate resin), and it is preferable to contain both a virgin raw material and a recycled resin, or it may be made of a recycled polycarbonate resin. The proportion of the recycled polycarbonate resin in the polycarbonate resin (A) is preferably 40% or more, 50% or more, 60% or more, or 80% or more, and particularly preferably 100%.
[0029] [Graft copolymer (B)] The graft copolymer (B) contained in the polycarbonate resin composition of the present invention is a graft copolymer containing an aromatic vinyl monomer component (b1), a vinyl cyanide monomer component (b2), and a diene rubber polymer component (b3). The graft copolymer (B) preferably comprises 40-80% by mass of the aromatic vinyl monomer component (b1), 10-30% by mass of the vinyl cyanide monomer component (b2), and 10-50% by mass of the diene rubber polymer component (b3), and may further contain 0-30% by mass of other monomer components (b4).
[0030] Examples of the aromatic vinyl monomer component (b1) in the graft copolymer (B) include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, vinylxylene, ethylstyrene, dimethylstyrene, pt-butylstyrene, vinylnaphthalene, methoxystyrene, monobromostyrene, dibromostyrene, fluorostyrene, and tribromostyrene, with styrene being particularly preferred. The proportion of the aromatic vinyl monomer component (b1) in the graft copolymer (B) is preferably in the range of 40 to 80 mass%, more preferably 45 mass% or more, even more preferably 50 mass% or more, particularly preferably 55 mass% or more, and more preferably 75 mass% or less, even more preferably 70 mass% or less, particularly preferably 65 mass% or less, based on 100 mass% of the graft copolymer (B).
[0031] Examples of the vinyl cyanide monomer component (b2) in the graft copolymer (B) include acrylonitrile and methacrylonitrile, with acrylonitrile being particularly preferred. The proportion of the vinyl cyanide monomer component (b2) in the graft copolymer (B) is preferably in the range of 10 to 30 mass%, more preferably 12 mass% or more, even more preferably 14 mass% or more, particularly preferably 15 mass% or more, and more preferably 28 mass% or less, even more preferably 26 mass% or less, particularly preferably 25 mass% or less, based on 100 mass% of the graft copolymer (B).
[0032] As the diene rubbery polymer component (b3) of the graft copolymer (B), for example, a rubber component such as polybutadiene, polyisoprene, or styrene-butadiene copolymer is used. The proportion of the diene rubbery polymer component (b3) in the graft copolymer (B) is preferably in the range of 10 to 50 mass%, more preferably 13 mass% or more, even more preferably 14 mass% or more, particularly preferably 15 mass% or more, and more preferably 45 mass% or less, in 100 mass% of the graft copolymer (B).
[0033] Furthermore, it may be a copolymer of other monomer components (b4) copolymerizable with these. In this case, examples of the other copolymerizable vinyl monomers include maleimide-based monomers such as maleimide, N-methylmaleimide, N-cyclohexylmaleimide, and N-phenylmaleimide, acrylamide-based monomers such as acrylamide and N-methylacrylamide, unsaturated acid anhydrides such as maleic anhydride and itaconic anhydride, unsaturated acids such as acrylic acid and methacrylic acid, glycidyl acrylate, glycidyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, methoxypolyethylene glycol methacrylate, and the like. The proportion of the other monomer component (b4) in the graft copolymer (B) is preferably in the range of 0 to 30 mass%, more preferably 20 mass% or less, even more preferably 10 mass% or less, even more preferably 5 mass% or less, particularly preferably 3 mass% or less, and even more preferably 2 mass% or less, based on 100 mass% of the graft copolymer (B).
[0034] Specific preferred examples of the graft copolymer (B) include acrylonitrile-butadiene-styrene graft copolymer, acrylonitrile-butadiene-styrene-α-methylstyrene graft copolymer, acrylonitrile-ethylene-propylene-diene-styrene copolymer, etc., and among these, acrylonitrile-butadiene-styrene graft copolymer (ABS resin) is particularly preferred.
[0035] The graft copolymer (B) is usually produced by a method such as bulk polymerization, solution polymerization, suspension polymerization, or emulsion polymerization, and any of these methods can be used.
[0036] The content of the graft copolymer (B) is 10 to 45% by mass, preferably 12% by mass or more, more preferably 15% by mass or more, preferably 42% by mass or less, and more preferably 40% by mass or less, based on 100% by mass of the total of the polycarbonate resin (A) and the graft copolymer (B). When the content is within such a range, the resin composition can have excellent heat resistance and fluidity. If the amount of the graft copolymer (B) exceeds 45% by mass, the heat resistance decreases, and if it is less than 10% by mass, the fluidity decreases.
[0037] [Arylphosphine oxide (C)] The polycarbonate resin composition of the present invention contains an arylphosphine oxide (C). Here, the aryl group means a group containing a monocyclic or polycyclic aromatic group which may have a substituent, and particularly preferably means a phenyl group which may have a substituent. Preferred examples of the arylphosphine oxide (C) include triphenylphosphine oxide, diphenylbutylphosphine oxide, diphenyloctadecylphosphine oxide, tris(p-tolyl)phosphine oxide, tris(p-nonylphenyl)phosphine oxide, tris(naphthyl)phosphine oxide, diphenyl(hydroxymethyl)phosphine oxide, diphenyl(acetoxymethyl)phosphine oxide, diphenyl(β-ethylcarboxyethyl)phosphine oxide, tris(p-chlorophenyl)phosphine oxide, tris(p-fluorophenyl)phosphine oxide, diphenylbenzylphosphine oxide, diphenyl-β-cyanoethylphosphine oxide, diphenyl(p-hydroxyphenyl)phosphine oxide, diphenyl-1,4-dihydroxyphenyl-2-phosphine oxide, and phenylnaphthylbenzylphosphine oxide. Triarylphosphine oxide is preferred, and triphenylphosphine oxide is particularly preferred.
[0038] The content of the arylphosphine oxide (C) is 0.001 to 0.3 parts by mass relative to 100 parts by mass of the total of the polycarbonate resin (A) and the graft copolymer (B). With such an amount, a resin composition containing a combination of a predetermined amount of the arylphosphine (D) and a specific content ratio can achieve excellent weather resistance. The content of the arylphosphine oxide (C) is preferably 0.002 parts by mass or more, more preferably 0.003 parts by mass or more, particularly preferably 0.004 parts by mass or more, and also preferably 0.25 parts by mass or less, particularly preferably 0.2 parts by mass or less, 0.15 parts by mass or less, 0.13 parts by mass or less, particularly preferably 0.1 parts by mass or less.
[0039] [Arylphosphine (D)] The polycarbonate resin composition of the present invention preferably further contains an arylphosphine (D). Here, the aryl group means a group containing a monocyclic or polycyclic aromatic group which may have a substituent, and particularly preferably means a phenyl group which may have a substituent. Preferred examples of the arylphosphine (D) include triphenylphosphine, diphenylbutylphosphine, diphenyloctadecylphosphine, tris(p-tolyl)phosphine, tris(p-nonylphenyl)phosphine, tris(naphthyl)phosphine, diphenyl(hydroxymethyl)phosphine, diphenyl(acetoxymethyl), diphenyl(β-ethylcarboxyethyl)phosphine, tris(p-chlorophenyl)phosphine, tris(p-fluorophenyl)phosphine, diphenylbenzylphosphine, diphenyl-β-cyanoethylphosphine, diphenyl(p-hydroxyphenyl)phosphine, diphenyl-1,4-dihydroxyphenyl-2-phosphine, phenylnaphthylbenzylphosphine, and the like. Triarylphosphines are preferred, and triphenylphosphine and tritolylphosphine are preferred, with triphenylphosphine being particularly preferred.
[0040] The content of the arylphosphine (D) when contained is preferably 0.001 to 0.3 parts by mass relative to 100 parts by mass in total of the polycarbonate resin (A) and the graft copolymer (B). With such an amount, the resin composition containing the arylphosphine oxide (C) together can further improve the weather resistance. The content of the arylphosphine (D) is more preferably 0.005 parts by mass or more, of which 0.008 parts by mass or more, particularly preferably 0.01 parts by mass or more, and more preferably 0.25 parts by mass or less, of which 0.2 parts by mass or less, 0.15 parts by mass or less, 0.1 parts by mass or less, 0.05 parts by mass or less, particularly preferably 0.04 parts by mass or less. The mass ratio (D) / (C) of the contents of the arylphosphine (D) and the arylphosphine oxide (C) is from 0.003 to 4, and by setting it in such a range, it is possible to improve the weather resistance. The mass ratio (D) / (C) is preferably 0.005 or more, more preferably 0.01 or more, and particularly preferably 0.03 or more, and is preferably 3.5 or less, more preferably 3 or less, 2.5 or less, 2.0 or less, 1.5 or less, 1.2 or less, 1.1 or less, and particularly preferably 1.0 or less.
[0041] [Triaryl phosphite] The polycarbonate resin composition of the present invention preferably further contains a triaryl phosphite. Here, the aryl group means a group containing a monocyclic or polycyclic aromatic group which may have a substituent, and particularly preferably means a phenyl group which may have a substituent.
[0042] Preferred examples of the triaryl phosphite include triphenyl phosphite, tris(p-tolyl)phosphite, tris(p-nonylphenyl)phosphite, tris(mononyl / dinonyl phenyl)phosphite, tris(2,4-di-t-butylphenyl)phosphite, tris(naphthyl)phosphite, tris(p-chlorophenyl)phosphite, tris(p-fluorophenyl)phosphite, diphenylbenzylphosphine, diphenyl(p-hydroxyphenyl)phosphite, diphenyl-1,4-dihydroxyphenyl-2-phosphite, and phenylnaphthylbenzylphosphine, with triphenyl phosphite and tris(2,4-di-t-butylphenyl)phosphite being particularly preferred.
[0043] The content of triaryl phosphite when it is contained is preferably 0.001 to 0.3 parts by mass relative to 100 parts by mass of the total of the polycarbonate resin (A) and the graft copolymer (B). By containing such an amount in combination with the aryl phosphine oxide (C) and the aryl phosphine (D), the residence heat stability can be further improved. The content of the aryl phosphine is more preferably 0.005 parts by mass or more, particularly preferably 0.008 parts by mass or more, particularly preferably 0.01 parts by mass or more, and more preferably 0.25 parts by mass or less, particularly preferably 0.2 parts by mass or less, 0.15 parts by mass or less, 0.1 parts by mass or less, 0.05 parts by mass or less, and particularly preferably 0.04 parts by mass or less.
[0044] [Compounds with phenol structure] The polycarbonate resin composition of the present invention also preferably contains a compound having a phenol structure. A compound having a phenol structure is a compound in which a hydroxy group is directly bonded to a benzene ring, and specifically, 4-t-butylphenol, 2,4-di-t-butylphenol, 4-α-cumylphenol, and bisphenol A are preferred. Among these, 4-t-butylphenol, 4-α-cumylphenol, and 4-t-butylphenol are more preferred. The compound having a phenol structure may contain one kind alone or two or more kinds. The compound having a phenol structure does not include a phenol-based antioxidant, which will be described later.
[0045] When the compound having a phenol structure is contained, the content is preferably 0.001 to 0.3 parts by mass per 100 parts by mass of the total of the polycarbonate resin (A) and the graft copolymer (B). When two or more kinds of compounds having a phenol structure are contained, the content is the total amount thereof. A resin composition containing the polycarbonate resin (A) and the graft copolymer (B) together with the arylphosphine oxide (C) and the arylphosphine (D) in such amounts is further excellent in highly weather resistance, impact resistance, heat resistance, and fluidity (moldability).
[0046] When a compound having a phenol structure is contained, the content is more preferably 0.0015 parts by mass or more, even more preferably 0.002 parts by mass or more, and more preferably 0.25 parts by mass or less, particularly preferably 0.2 parts by mass or less, 0.1 parts by mass or less, 0.05 parts by mass or less, 0.01 parts by mass or less, and particularly preferably 0.005 parts by mass or less, per 100 parts by mass of the polycarbonate resin (A) and the graft copolymer (B) in total.
[0047] When 4-t-butylphenol is contained as the compound having a phenol structure, the content is preferably 0.0012 to 0.01 parts by mass, and more preferably 0.0015 to 0.005 parts by mass, relative to 100 parts by mass of the total of (A) and (B). When 2,4-di-t-butylphenol is contained as a compound having a phenol structure, the content is preferably 0.0012 to 0.01 parts by mass, and more preferably 0.0015 to 0.005 parts by mass, relative to 100 parts by mass of the total of (A) and (B). When 4-α-cumylphenol is contained, the content is preferably 0.0012 to 0.01 parts by mass, and more preferably 0.0015 to 0.005 parts by mass, per 100 parts by mass of the total of (A) and (B). When bisphenol A is contained as the compound having a phenol structure, the content is preferably 0.002 to 0.03 parts by mass, and more preferably 0.004 to 0.01 parts by mass, per 100 parts by mass of the total of (A) and (B).
[0048] 4-t-butylphenol, 2,4-di-t-butylphenol, 4-α-cumylphenol, or bisphenol A may be present in a free state either as a by-product or used during the production of the polycarbonate resin (A), or derived from recycled polycarbonate resin, and the amounts of these are also included in the amount of the compound having a phenol structure.
[0049] [Phenol-based antioxidants] The polycarbonate resin composition of the present invention preferably further contains a phenol-based antioxidant. Preferred examples of the phenol-based antioxidant include hindered phenol-based antioxidants. Specific examples thereof include pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, thiodiethylene bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 3,3',3",5,5',5"-hexa-t-butyl-a,a',a"-(mesitylene-2,4, 6-triyl)tri-p-cresol, 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene)bis[3-(5-t-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-t-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-t-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, 2-[1-(2-hydroxy-3,5-di-t-pentylphenyl)ethyl]-4,6-di-t-pentylphenyl acrylate, and the like.
[0050] Among these, pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate are particularly preferred. The phenol-based antioxidant may be contained alone or in any combination and ratio of two or more kinds.
[0051] The content of the phenol-based antioxidant, when contained, is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, and preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, based on 100 parts by mass of the total of the polycarbonate resin (A) and the graft copolymer (B). By making the content of the phenol-based antioxidant equal to or more than the lower limit of the above range, the effect of the phenol-based antioxidant can be sufficiently obtained. In addition, by making the content of the phenol-based antioxidant equal to or less than the upper limit of the above range, the effect does not plateau, and it is economical.
[0052] [Release agent] The resin composition of the present invention also preferably contains a release agent. Examples of the release agent include aliphatic carboxylic acids, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds having a number average molecular weight of 200 to 15,000, and polysiloxane-based silicone oils.
[0053] Examples of the aliphatic carboxylic acid include saturated or unsaturated aliphatic mono-, di- or tri-carboxylic acids. Here, the aliphatic carboxylic acid also includes alicyclic carboxylic acids. Among these, preferred aliphatic carboxylic acids are mono- or di-carboxylic acids having 6 to 36 carbon atoms, and more preferred are saturated aliphatic mono-carboxylic acids having 6 to 36 carbon atoms. Specific examples of such aliphatic carboxylic acids include palmitic acid, stearic acid, caproic acid, capric acid, lauric acid, arachic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tetralinic acid, montanic acid, adipic acid, and azelaic acid.
[0054] The aliphatic carboxylic acid in the ester of aliphatic carboxylic acid and alcohol can be, for example, the same as the aliphatic carboxylic acid. On the other hand, the alcohol can be, for example, a saturated or unsaturated monohydric or polyhydric alcohol. These alcohols may have a substituent such as a fluorine atom or an aryl group. Among these, a monohydric or polyhydric saturated alcohol having 30 or less carbon atoms is preferred, and an aliphatic saturated monohydric alcohol or an aliphatic saturated polyhydric alcohol having 30 or less carbon atoms is more preferred. Here, the term aliphatic is used to include alicyclic compounds.
[0055] Specific examples of such alcohols include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentylene glycol, ditrimethylolpropane, and dipentaerythritol.
[0056] The above ester may contain an aliphatic carboxylic acid and / or alcohol as an impurity. The above ester may be a pure substance, or may be a mixture of a plurality of compounds. The aliphatic carboxylic acid and alcohol that are combined to form an ester may each be used alone or in any combination and ratio of two or more.
[0057] Specific examples of esters of aliphatic carboxylic acids and alcohols include beeswax (a mixture mainly composed of myricyl palmitate), stearyl stearate, behenyl behenate, stearyl behenate, glycerin monopalmitate, glycerin monostearate, glycerin distearate, glycerin tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, and pentaerythritol tetrastearate.
[0058] Examples of aliphatic hydrocarbons having a number average molecular weight of 200 to 15,000 include liquid paraffin, paraffin wax, microwax, polyethylene wax, Fischer-Tropsch wax, and α-olefin oligomers having 3 to 12 carbon atoms. The aliphatic hydrocarbons also include alicyclic hydrocarbons. These hydrocarbons may be partially oxidized. Among these, paraffin wax, polyethylene wax, or a partial oxide of polyethylene wax is preferred, and paraffin wax and polyethylene wax are more preferred. The number average molecular weight of the aliphatic hydrocarbon is preferably 5,000 or less. The aliphatic hydrocarbon may be a single substance, but a mixture of substances having various constituent components and molecular weights can also be used as long as the main component is within the above range.
[0059] Examples of polysiloxane-based silicone oils include dimethyl silicone oil, methylphenyl silicone oil, diphenyl silicone oil, and fluorinated alkyl silicone.
[0060] The above-mentioned release agents may be contained alone or in any combination and ratio of two or more kinds.
[0061] The content of the release agent is usually 0.001 parts by mass or more, preferably 0.01 parts by mass or more, and usually 2 parts by mass or less, preferably 1 part by mass or less, and more preferably 0.5 parts by mass or less, based on 100 parts by mass in total of the polycarbonate resin (A) and the graft copolymer (B). If the content of the release agent is less than the lower limit of the above range, the effect of releasability may be insufficient, whereas if the content of the release agent is more than the upper limit of the above range, there is a possibility that a decrease in hydrolysis resistance and mold contamination during injection molding may occur.
[0062] [Ultraviolet absorber] The polycarbonate resin composition of the present invention also preferably contains an ultraviolet absorber. Examples of the ultraviolet absorber include inorganic ultraviolet absorbers such as cerium oxide and zinc oxide; and organic ultraviolet absorbers such as benzotriazole compounds, benzophenone compounds, salicylate compounds, cyanoacrylate compounds, triazine compounds, oxanilide compounds, malonic acid ester compounds, and hindered amine compounds. Among these, organic ultraviolet absorbers are preferred, and benzotriazole compounds are more preferred. By selecting an organic ultraviolet absorber, the transparency and mechanical properties of the resin composition of the present invention can be improved.
[0063] Specific examples of the benzotriazole compound include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-[2'-hydroxy-3',5'-bis(α,α-dimethylbenzyl)phenyl]-benzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole, and 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole. myl)-benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol] and the like. Among these, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole and 2,2'-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)phenol] are preferred, and 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole is particularly preferred.
[0064] Specific examples of the benzophenone compound include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid, 2-hydroxy-4-n-octoxybenzophenone, 2-hydroxy-n-dodecyloxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2,2'-dihydroxy-4-methoxybenzophenone, and 2,2'-dihydroxy-4,4'-dimethoxybenzophenone.
[0065] Specific examples of the salicylate compound include phenyl salicylate, 4-t-butylphenyl salicylate, and the like. Specific examples of the cyanoacrylate compound include ethyl-2-cyano-3,3-diphenylacrylate, 2-ethylhexyl-2-cyano-3,3-diphenylacrylate, and the like. Specific examples of the oxanilide compound include 2-ethoxy-2'-ethyloxalic acid bis-anilide. As the malonic acid ester compound, 2-(alkylidene)malonic acid esters are preferred, and 2-(1-arylalkylidene)malonic acid esters are more preferred.
[0066] The content of the ultraviolet absorber, when contained, is usually 0.05 parts by mass or more, preferably 0.1 parts by mass or more, and usually 1 part by mass or less, preferably 0.5 parts by mass or less, based on 100 parts by mass of the total of the polycarbonate resin (A) and the graft copolymer (B). If the content of the ultraviolet absorber is less than the lower limit of the above range, the effect of improving weather resistance and light resistance may be insufficient, and if the content of the ultraviolet absorber is more than the upper limit of the above range, mold deposits or the like may occur, causing mold contamination. The ultraviolet absorbing agent may be contained alone or in any combination and ratio of two or more kinds.
[0067] [Additives, etc.] The polycarbonate resin composition of the present invention may contain additives other than those described above, such as fluorescent whitening agents, pigments (including titanium oxide, etc.), dyes, flame retardants, impact resistance improvers, plasticizers, compatibilizers, etc. These additives may be contained alone or in combination of two or more.
[0068] The polycarbonate resin (A) and the graft copolymer (B) may contain other resins. Examples of the other resins include thermoplastic polyester resins such as polyethylene terephthalate, polytrimethylene terephthalate, and polybutylene terephthalate; styrene-based resins such as polystyrene resin (GPPS), high-impact polystyrene resin (HIPS), and acrylonitrile-styrene copolymer (AS resin); polyolefin resins such as polyethylene resin and polypropylene resin; polyamide resin; polyimide resin; polyetherimide resin; polyurethane resin; polyphenylene ether resin; polyphenylene sulfide resin; polysulfone resin; and polymethacrylate resin. When other resins than the polycarbonate resin (A) and the graft copolymer (B) are contained, the content thereof is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, even more preferably 5 parts by mass or less, and particularly preferably 3 parts by mass or less, per 100 parts by mass of the total of the polycarbonate resin (A) and the graft copolymer (B). EXAMPLES
[0069] In order to confirm the effects of the polycarbonate resin composition of the present invention, polycarbonate resin compositions were prepared as follows, but the present invention should not be construed as being limited to the following examples. The components used are as shown in Table 1 below.
[0070] [Table 1]
[0071] (Examples 1 to 9, Comparative Examples 1 to 13) The above-mentioned components were mixed in the ratios (parts by mass) shown in Table 2 below, fed to a twin-screw extruder (Toshiba Machine Co., Ltd., "TEM26SX"), kneaded under conditions of a screw rotation speed of 150 rpm, a discharge rate of 25 kg / hour, and a barrel temperature of 260°C, and extruded in the form of strands from the tip of the extrusion nozzle. The strands were quenched in a water tank and cut and pelletized using a pelletizer to obtain pellets of a polycarbonate resin composition.
[0072] <mvr> The pellets obtained by the above method were dried at 100° C. for 5 hours, and then the MVR (melt volume rate, unit: g / 10 min) was measured in accordance with ISO1133 at a measurement temperature of 250° C. and a load of 2.16 kgf.
[0073] <Charpy notched strength> The pellets obtained by the above method were dried at 100°C for 5 hours, and then injection molded using an injection molding machine (Nissei Plastic Industrial Co., Ltd., "NEX80III") at a cylinder temperature of 260°C and a mold temperature of 60°C to produce ISO multipurpose test pieces (4 mmt). Using the obtained ISO multipurpose test piece (4 mmt), the notched Charpy strength (unit: kJ / m) was measured at a temperature of 23°C based on ISO standard 179. 2 ) was measured.
[0074] <Heat resistance DTUL (temperature deflection under load)> Based on ISO75-1 and ISO75-2, a constant bending load (1.80 MPa) was applied in the flatwise direction to the centre of a 4 mm x 10 mm ISO multipurpose test piece (4 mmt), the temperature was raised at a constant rate, and the temperature (unit: °C) was measured when the strain at the centre reached 0.34 mm.
[0075] <Weather resistance (ΔE)> The obtained pellets were injection molded using a Toshiba Machine Co., Ltd. injection molding machine "EC50SXII" at a cylinder temperature of 260°C and a mold temperature of 60°C to obtain a plate-shaped molded product with a length of 90 mm, a width of 60 mm, and a thickness of 2 mm. The obtained plate-shaped molded product was subjected to a xenon weather test using a xenon weather tester (ATLAS, "Ci4000") with light of wavelength 300-400 nm at a temperature of 89°C and an irradiation intensity of approximately 55 W / m 2 The lightfastness treatment was carried out under the conditions of a treatment time of 100 hours (200 hours for carbon black added systems), and the hue before and after the lightfastness treatment was measured using a Nippon Denshoku Industries Co., Ltd. "SE6000" under D65, 10° field of view, and reflective conditions, and the color difference ΔE was calculated to evaluate the lightfastness. ΔE is preferably 7.5 or less, and in the case of a carbon black-added system, it is preferably 3.0 or less.
[0076] The above evaluation results are shown in Table 2 below.
[0077] [Table 2]
[0078] [Table 3]
[0079] [Table 4] [Industrial Applicability]
[0080] INDUSTRIAL APPLICABILITY The polycarbonate resin composition of the present invention has high weather resistance, and is excellent in impact resistance, heat resistance and fluidity (moldability), and can therefore be suitably used for various molded articles.< / mvr>
Claims
1. The composition contains 55 to 90 mass% of a polycarbonate resin (A) having a viscosity average molecular weight of 17,500 to 30,000, and 10 to 45 mass% of a graft copolymer (B) containing an aromatic vinyl monomer component (b1), a vinyl cyanide monomer component (b2), and a diene rubber polymer component (b3), per 100 mass parts of the total of (A) and (B), A polycarbonate resin composition comprising 0.001 to 0.3 parts by mass of an arylphosphine oxide (C) and 0.001 to 0.3 parts by mass of an arylphosphine (D), wherein the mass ratio (D) / (C) of the contents of the arylphosphine (D) to the arylphosphine oxide (C) is 0.003 or more and 4 or less.
2. 2. The polycarbonate resin composition according to claim 1, wherein the arylphosphine oxide (C) is triphenylphosphine oxide.
3. 2. The polycarbonate resin composition according to claim 1, wherein the arylphosphine (D) is triphenylphosphine.
4. A pellet of the polycarbonate resin composition according to any one of claims 1 to 3.
5. A molded article comprising the polycarbonate resin composition according to any one of claims 1 to 3.
6. A molded article comprising pellets of the polycarbonate resin composition according to claim 4.
Citation Information
Patent Citations
Polycarbonate composition with improved optical properties
JP2013506719A
Resin composition, production method of resin composition, and molded body
JP2014031459A
Resin composition and molding
JP2023025384A
Polycarbonate resin composition for molding
JP3308657B2