Foamed polylactic acid resin sheet and method for producing formed sheet
A polylactic acid resin foam sheet with controlled crystallinity and crystallization temperature is used to enhance heat resistance and manufacturing efficiency, addressing the inefficiencies in conventional thermoforming processes.
Patent Information
- Application Number
- JP2023052796
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional polylactic acid resin foam sheets, particularly those with crystalline resin, face challenges in achieving sufficient heat resistance and efficient production due to the time-consuming process of heat setting to increase crystallinity during thermoforming, which reduces manufacturing efficiency.
A polylactic acid resin foam sheet with crystallinity below 30% and a crystallization temperature of 105°C or less, produced through a method involving primary and secondary heating steps to enhance crystallinity, is used for efficient thermoforming.
This approach enables the production of sheet molded bodies with excellent heat resistance and improved manufacturing efficiency, suitable for applications requiring high thermal stability.
Smart Images

Figure 2024141257000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to a polylactic acid resin foam sheet and a method for producing a sheet molded article using the polylactic acid resin foam sheet. [Background technology]
[0002] Foamed products made from foamed resin compositions have been widely used. These foamed products are lightweight yet strong, offering excellent cushioning and heat insulation. Examples of this type of foamed product include foamed sheets and foamed beads obtained by impregnating non-foamed resin sheets or resin beads with a foaming agent such as acetone or butane and then heating them to foam, as well as foamed molded articles produced by processing these into a three-dimensional shape using a mold. A known example of a resin foamed sheet is an extrusion foaming method, in which a foaming resin composition and a foaming agent are melt-kneaded in an extruder, and the resulting molten mixture is extruded into a sheet through a sheeting die (a flat die or a circular die) attached to the tip of the extruder and foamed at the same time.
[0003] This type of extruded foam sheet is used as a cushioning sheet in its sheet form, or formed into bags and used as packaging material, etc. This type of extruded foam sheet is also used as a base sheet for producing sheet molded articles by thermoforming such as match mold forming and vacuum / pressure forming, and is also widely used as a component of molded articles such as food trays and cups.
[0004] Recently, there has been a growing demand for measures to address the problem of landscape damage caused by illegally dumped packaging materials in places such as mountains, fields, rivers, and coastlines. Against this background, the production of molded articles using polylactic acid resins that can be biodegraded in the natural environment has been studied, and the use of polylactic acid resin foam sheets in various applications has been investigated.
[0005] Many conventional polylactic acid resin foam sheets are made from amorphous polylactic acid resin, which is easily foamable. However, such polylactic acid resin foam sheets and sheet molded articles made from such polylactic acid resin foam sheets are difficult to exhibit sufficient heat resistance. For this reason, crystalline polylactic acid resins are increasingly used, and polylactic acid resin foam sheets are produced from resin compositions containing crystalline polylactic acid resins. When producing sheet molded articles from such polylactic acid resin foam sheets, polylactic acid resin foam sheets produced under conditions that suppress an increase in crystallinity are used, and the crystallinity of the polylactic acid resin foam sheets is increased during thermoforming (see, for example, paragraphs 0059 to 0061 of Patent Document 1 below). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 5517280 Summary of the Invention [Problem to be solved by the invention]
[0007] When producing a sheet molded body using a polylactic acid resin foam sheet containing a crystalline polylactic acid resin, a step called "heat setting" is performed during thermoforming, in which the sheet is held in a heated mold for a certain period of time to increase the crystallinity. If a polylactic acid resin foam sheet with a sufficiently low crystallinity is used to ensure moldability, the heat setting process takes a long time, reducing the production efficiency of the sheet molded body. In view of the above problems, the present invention aims to provide a polylactic acid resin foam sheet suitable for efficiently producing a sheet molded body with excellent heat resistance, thereby improving the production efficiency of the sheet molded body with excellent heat resistance. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention provides: A polylactic acid resin foam sheet made of a polylactic acid resin composition containing a crystalline polylactic acid resin, The crystallinity is 30% or less, Provided is a polylactic acid resin foam sheet that exhibits a crystallization temperature of 105°C or less as observed by heat flux differential scanning calorimetry at a heating rate of 5°C / min.
[0009] In order to solve the above problems, the present invention provides: A method for producing a sheet molded body by thermoforming a resin foam sheet, comprising: The resin foam sheet is The polylactic acid resin composition contains a crystalline polylactic acid resin. The crystallinity is 30% or less, A polylactic acid resin foam sheet that exhibits a crystallization temperature of 105°C or less when measured by heat flux differential scanning calorimetry at a heating rate of 5°C / min. a primary heating step of heating the polylactic acid resin foam sheet; The method for producing a sheet molded body includes a secondary heating step in which the polylactic acid resin foam sheet that has undergone the primary heating step is sandwiched between heated molds to produce a sheet molded body, and the crystallinity of the sheet molded body is increased. [Effects of the Invention]
[0010] According to the present invention, a polylactic acid resin foam sheet suitable for efficiently producing a sheet molding having excellent heat resistance is provided, and the efficiency of producing a sheet molding having excellent heat resistance can be improved. [Brief explanation of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic front view showing an example of a sheet manufacturing apparatus for producing a polylactic acid resin foam sheet. [Figure 2] FIG. 2 is a schematic diagram showing a method for determining the crystallization half time from a DSC curve. [Figure 3] FIG. 3 is a schematic perspective view showing a method for measuring the gel fraction. DETAILED DESCRIPTION OF THE INVENTION
[0012] An embodiment of the present invention will be described below. Hereinafter, the embodiment of the present invention will be described taking as an example a case where the polylactic acid resin foam sheet is an extruded foam sheet obtained by an apparatus such as that shown in FIG. 1. The polylactic acid resin foam sheet of this embodiment can be suitably used to produce a sheet molded product by thermoforming. Examples of such thermoforming include vacuum forming, pressure forming, vacuum-pressure forming, matched mold forming, and press forming.
[0013] The polylactic acid resin foam sheet of this embodiment may be, for example, an extruded foam sheet produced by a sheet manufacturing apparatus 100 illustrated in Fig. 1. The sheet manufacturing apparatus 100 illustrated in Fig. 1 includes a tandem extruder 10 and a circular die CD that extrudes the polylactic acid resin composition melt-kneaded in the tandem extruder 10 into a cylindrical shape. The manufacturing apparatus also includes a cooling device CL that air-cools the polylactic acid resin foam sheet extruded into a cylindrical shape from the circular die CD, and a mandrel MD that expands the cylindrical polylactic acid resin foam sheet into a cylindrical shape of a predetermined size.
[0014] The sheet manufacturing apparatus 100 is equipped with a slitting device that slits the polylactic acid resin foam sheet after it has passed through the mandrel MD and become a cylindrical shape with a predetermined diameter, and divides it into two strip-shaped sheets, and a winding roller 22 that winds up the slit polylactic acid resin foam sheet 1 after passing it through multiple rollers 21.
[0015] The extruder upstream of the tandem extruder 10 (hereinafter also referred to as the "first extruder 10a") is provided with a hopper 11 for feeding a polylactic acid resin composition (hereinafter also simply referred to as the "resin composition"), which is the raw material for the polylactic acid resin foam sheet, and a gas inlet 12 for supplying a foaming agent such as a hydrocarbon into the cylinder.
[0016] The sheet manufacturing apparatus 100 of this embodiment is also provided with an extruder (hereinafter also referred to as "second extruder 10b") downstream of the first extruder 10a. The second extruder 10b melt-mixes a resin composition containing a foaming agent. The polylactic acid resin contained in the polylactic acid resin foam sheet has crystalline properties. The polylactic acid resin is preferably modified by crosslinking or the like so as to exhibit excellent melt tension. The modified polylactic acid resin (hereinafter also referred to as "modified polylactic acid resin") may be incorporated into the polylactic acid resin foam sheet by supplying pre-modified polylactic acid resin to the hopper 11, or by modifying unmodified polylactic acid resin in the extruder used to produce the polylactic acid resin foam sheet.
[0017] The polylactic acid resin foam sheet of this embodiment is produced so that the crystallinity of the polylactic acid resin contained therein is not increased by the cooling device CL or the mandrel MD during production. Specifically, the polylactic acid resin foam sheet of this embodiment is produced so that the crystallinity is 30% or less. A polylactic acid resin foam sheet with a lower crystallinity has better moldability when producing a sheet molded product. Therefore, the crystallinity of the polylactic acid resin foam sheet may be 25% or less, or may be 20% or less. A crystallinity of 30% or less prevents excessive stretching in the mold during thermoforming, making it possible to prevent the resulting sheet molded product from shrinking over time.
[0018] It is advantageous for the polylactic acid resin foam sheet to have a certain degree of crystallinity or higher in order to provide a sheet molding with sufficient crystallinity to exhibit excellent heat resistance. The crystallinity of the polylactic acid resin foam sheet may be 5% or higher, or 10% or higher.
[0019] The polylactic acid resin foam sheet is preferably formed by a process such as heat setting so as to exhibit a higher degree of crystallinity than the polylactic acid resin foam sheet. The polylactic acid resin foam sheet is preferably formed so as to increase the degree of crystallinity by 5% or more, and more preferably so as to increase the degree of crystallinity by 10% or more. The degree of crystallinity that the polylactic acid resin foam sheet can achieve is preferably 25% or more, more preferably 30% or more. The degree of crystallinity that the polylactic acid resin foam sheet can achieve is usually 60% or less. The degree of crystallinity that the polylactic acid resin foam sheet can achieve may be 50% or less.
[0020] The resin composition constituting the polylactic acid resin foam sheet of this embodiment preferably has a half-crystallization time of 30 minutes or less at 80°C. The half-crystallization time is more preferably 25 minutes or less. When the resin composition constituting the polylactic acid resin foam sheet has a half-crystallization time of 30 minutes or less, the crystallinity of the sheet molding can be increased in a shorter molding time during thermoforming, and excellent heat resistance can be imparted to the sheet molding.
[0021] (Crystallization half time) The crystallization half time can be measured using a heat flux differential scanning calorimeter (heat flux DSC) as follows. However, the sampling method and temperature conditions will be as follows: 5.5±0.5 mg of sample was packed tightly at the bottom of an aluminum measurement container (Hitachi High-Tech Science Corporation, product code: GAA-0065), and then an aluminum lid (Hitachi High-Tech Science Corporation, product code: GAA-0064) was placed on the container. Using a differential scanning calorimeter (Hitachi High-Tech Science Corporation, "NEXTA DSC600"), the container was held at 30°C for 2 minutes under a nitrogen gas flow rate of 20 mL / min, and then heated from 30°C to 210°C (first heating) at the maximum capacity of the device, and maintained at this temperature for 10 minutes. Thereafter, the sample is removed from the measuring device, allowed to stand at room temperature for 10 minutes, and then returned to the measuring device at 30°C. Second temperature increase: After increasing the temperature to 70°C at the maximum capacity of the device, increase the temperature to 80°C at a rate of 20°C / min and hold for 30 minutes. Alumina is used as the reference material.
[0022] (How to create a DSC curve) From the start of the second heating cycle until the end of the holding time at the heating end temperature, the heat flow was measured every 0.2 seconds and plotted with time (min) on the horizontal axis and heat flow (mW) on the vertical axis to create a DSC curve (see Figure 2). In Figure 2, the time from the start of measurement to the peak top of the exothermic peak (point x) is defined as the half-crystallization time.
[0023] The resin composition contains a crystalline polylactic acid resin as a main component. The polylactic acid resin refers to a polymer containing 50 mol % or more of lactic acid component units. The polymer includes: (1) Polymers of lactic acid only, (2) copolymers of lactic acid with other aliphatic hydroxycarboxylic acids; (3) a copolymer of lactic acid, an aliphatic polyhydric alcohol, and an aliphatic polycarboxylic acid; (4) Copolymer of lactic acid and aliphatic polycarboxylic acid, (5) copolymers of lactic acid and aliphatic polyhydric alcohols; (6) A mixture of any of the above (1) to (5), etc. Examples include:
[0024] Specific examples of the lactic acid include L-lactic acid, D-lactic acid, DL-lactic acid, or their cyclic dimers, L-lactide, D-lactide, DL-lactide, or a mixture thereof.
[0025] Examples of the aliphatic polycarboxylic acid constituting the copolymer include oxalic acid, succinic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, undecanedioic acid, and dodecanedioic acid. The aliphatic polycarboxylic acid may be an anhydride.
[0026] Examples of the aliphatic polyhydric alcohol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, neopentyl glycol, tetramethylene glycol, and 1,4-cyclohexanedimethanol.
[0027] Examples of the aliphatic hydroxycarboxylic acid other than lactic acid that constitutes the copolymer include glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, and 6-hydroxycaproic acid.
[0028] The polylactic acid resin contained in the resin composition may be a crystalline polylactic acid resin alone, or may contain a crystalline polylactic acid resin and an amorphous polylactic acid resin.
[0029] The polylactic acid resin may have an endothermic capacity (ΔH endo) of, for example, 10 J / g or more as determined by heat flux differential scanning calorimetry. The endothermic capacity (ΔH endo) of the polylactic acid resin is preferably 20 J / g or more, and more preferably 30 J / g or more. The upper limit of the endothermic capacity (ΔH endo) of the polylactic acid resin is not particularly limited, but is generally 60 J / g.
[0030] In this embodiment, the crystalline polylactic acid resin refers to one whose endothermic heat (ΔH endo) determined by heat flux differential scanning calorimetry exceeds 2 J / g. The endothermic heat (ΔH endo) of the crystalline polylactic acid is usually 20 to 65 J / g.
[0031] The polylactic acid resin contained in the resin composition preferably contains a copolymer in which the D- and L-forms of lactic acid are copolymerized. The proportion of the D-form in the copolymer is preferably 0.5 mol % or more and 5 mol % or less. The polylactic acid resin containing the copolymer preferably has a melting point of 130°C or more and 170°C or less. Such a polylactic acid resin has advantages in terms of foamability, moldability, and heat resistance.
[0032] In the present embodiment, the polylactic acid resin foam sheet preferably has a crystallization temperature of 105°C or lower, more preferably 100°C or lower, and even more preferably 98°C or lower, as determined by heat flux differential scanning calorimetry at a heating rate of 5°C / min. When the polylactic acid resin foam sheet has a crystallization temperature below a predetermined temperature, crystallization proceeds more rapidly during thermoforming, improving moldability. Furthermore, to prevent excessive increases in crystallinity during preheating before thermoforming, the crystallization temperature is preferably 70°C or higher, more preferably 75°C or higher, and even more preferably 80°C or higher.
[0033] (melting point, crystallization temperature, degree of crystallinity) The melting point, crystallization temperature, and degree of crystallinity of the polylactic acid resin, the polylactic acid resin foam sheet, and the sheet molding can be determined as follows. The melting point and crystallization temperature of the polylactic acid resin, polylactic acid resin foam sheet, and sheet molding can be measured using a heat flux differential scanning calorimeter (heat flux DSC) as follows. The measurement is carried out according to the methods described in JIS K7122:1987, JIS K7122:2012 "Method for measuring heat of transition of plastics" and JIS K7121:1987, 2012 "Method for measuring transition temperature of plastics". The sampling method and temperature conditions can be as follows: 5.5±0.5 mg of sample was packed tightly at the bottom of an aluminum measurement container (Hitachi High-Tech Science Corporation, product code: GAA-0065), and an aluminum lid (Hitachi High-Tech Science Corporation, product code: GAA-0064) was placed on the container. A DSC curve was then obtained by heating and cooling the sample using a differential scanning calorimeter (Hitachi High-Tech Science Corporation, "NEXTA DSC600") under a nitrogen gas flow rate of 20 mL / min in the following steps: (Step 1) Heat from 30°C to 210°C (first heating) and then hold for 10 minutes. (Step 2) Remove from the measuring device, leave to stand at room temperature for 10 minutes, and then return to the measuring device at 30°C (rapid cooling). (Step 3) Increase the temperature from 30°C to 210°C (second increase). All temperature increases are carried out at a rate of 5°C / min. Alumina is used as the reference material.
[0034] (Melting Point) Using the analysis software attached to the device, the temperature at the top of the melting peak observed during the second heating process is read and taken as the melting temperature (melting point). (crystallization temperature) The crystallization temperature is determined by reading the top temperature of the exothermic peak observed during the second heating process. If multiple exothermic peaks appear, the temperature of the lowest peak is read. (crystallinity) The degree of crystallinity is determined by dividing the difference between the endotherm (heat of fusion (J / g)) obtained from the area of the endothermic peak appearing in the crystalline melting observed in the first heating process and the heat of crystallization (J / g) obtained from the area of the crystallization peak by the theoretical heat of fusion of perfectly crystalline polylactic acid (93 J / g). The heat of fusion and the heat of crystallization are calculated using the analysis software attached to the device. Specifically, the heat of fusion is calculated from the area enclosed by the line connecting the point where the DSC curve departs from the low-temperature baseline and the point where the DSC curve returns to the high-temperature baseline, and the DSC curve. The heat of crystallization is calculated from the area enclosed by the line connecting the point where the DSC curve departs from the low-temperature baseline and the point where the DSC curve returns to the high-temperature side, and the DSC curve. The crystallinity can be calculated using the following formula: Crystallinity (%) = [Heat of fusion (J / g) - Heat of crystallization (J / g)] / 93(J / g) ×100(%)
[0035] The resin composition may contain the polylactic acid resin in a proportion of 100% by mass, or may be a mixture of the polylactic acid resin and a thermoplastic resin other than the polylactic acid resin, containing the polylactic acid resin in a proportion of 50% by mass or more but less than 100% by mass, and containing the thermoplastic resin in a proportion of more than 0% by mass but not more than 50% by mass. That is, the resin composition may contain the thermoplastic resin other than the polylactic acid resin in a proportion of 50% by mass or less.
[0036] When the resin composition contains a thermoplastic resin other than the polylactic acid resin, the proportion of the polylactic acid resin is preferably 60% by mass or more, more preferably 70% by mass or more. Examples of thermoplastic resins other than the polylactic acid resin include polyethylene-based resins, polypropylene-based resins, polystyrene-based resins, and polyester-based resins. The resin composition in this embodiment preferably contains a thermoplastic elastomer or an aliphatic polyester resin, from the viewpoint of improving the impact resistance of a sheet molding made from a polylactic acid resin foam sheet.
[0037] Examples of the thermoplastic elastomer include olefin elastomers, styrene elastomers, acrylic elastomers, and ester elastomers, among which acrylic elastomers, acid-modified styrene elastomers, and ester elastomers are preferred because they have good compatibility with polylactic acid resins.Specifically, commercially available products such as Metablen W-600A manufactured by Mitsubishi Rayon Co., Ltd., Tuftec MP10 manufactured by Asahi Kasei Corporation, and Nofalloy TZ810 manufactured by NOF Corporation can be suitably used.
[0038] The aliphatic polyester resin may be a hydroxy acid polycondensate, a ring-opening polymer of lactone, or a polycondensate of a polyhydric alcohol component and a polycarboxylic acid component. Examples of the hydroxy acid polycondensate include polylactic acid and a polycondensate of hydroxybutyric acid. Examples of the ring-opening polymer of lactone include polycaprolactone and polypropiolactone. Examples of the polycondensate of a polyhydric alcohol component and a polycarboxylic acid component include polyethylene succinate, polybutylene succinate, polybutylene adipate, polybutylene succinate adipate, and polybutylene adipate terephthalate. Among these, polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), or polybutylene adipate terephthalate (PBAT), which have good compatibility with polylactic acid resin, are preferred.
[0039] The polylactic acid resin is preferably suitable for extrusion foaming. It is known that in extrusion foaming, a foamed sheet with a high expansion ratio can generally be obtained by using a resin with a high melt tension. In particular, since crystalline resins generally have a low melt tension, it is known that the melt tension of the resin can be increased by crosslinking the resin using a method such as chemical crosslinking or electron beam crosslinking, or by mixing a high molecular weight component, thereby improving extrusion foamability.
[0040] The polylactic acid resin of this embodiment preferably exhibits a specific characteristic value when its melt tension is measured at 190°C. For example, the polylactic acid resin preferably exhibits a melt tension of 5 cN or more and 80 cN or less when measured at 190°C. The melt tension of the polylactic acid resin may be 75 cN or less, 70 cN or less, or 65 cN or less. The melt tension of the polylactic acid resin may be 8 cN or more or 10 cN or more. Having such a preferable melt tension, the polylactic acid resin can suppress cell breakage during foaming of the resin composition, and is less likely to have a high open cell ratio even when foamed at a high expansion ratio, which can be advantageous for producing a polylactic acid resin foam sheet with a good appearance.
[0041] In this embodiment, it is preferable that the resin composition containing the polylactic acid resin as described above also exhibits the melt tension as described above.
[0042] The polylactic acid resin of this embodiment has a melt mass-flow rate (MFR: temperature 190°C, nominal load 2.16 kg) of, for example, 0.1 g / 10 min or more and 15 g / 10 min or less. The melt mass-flow rate of the resin composition may be 10 g / 10 min or less, 5 g / 10 min or less, 4 g / 10 min or less, or 3 g / 10 min or less.
[0043] In this embodiment, it is preferable that the resin composition containing the polylactic acid resin as described above also exhibits the melt mass flow rate as described above.
[0044] The melt tension and melt mass-flow rate of the polylactic acid resin can be measured by the following method.
[0045] <Melt tension> The melt tension can be measured using a capillary rheometer "Capillograph 1D" (special heating furnace specification) manufactured by Toyo Seiki Seisakusho Co., Ltd., and "Rheotens 71.97" manufactured by Goettfert. The melt tension is measured under the following conditions. The sample is vacuum dried at 90°C for at least 4 hours in advance, and after drying, it is placed in a nylon plastic bag for vacuum packing, vacuum packed, and stored in a desiccator until just before measurement. Install the Rheotens 71.97 so that the distance from the die exit of the Capilograph 1D to the measurement section is 80 mm. (However, if it is not possible to bring the Rheotens close enough to 80 mm due to interference, take measures to avoid interference and set the Rheotens in the specified location.) First, the sample is filled into a barrel heated to a test temperature of 190°C, and then preheated for 5 minutes. The measurement time should not exceed 10 minutes after filling the barrel, including the preheating time. Next, a piston is inserted from the top of the barrel and the molten resin is extruded in a string-like shape. At this time, the piston descending speed (20 mm / min) is kept constant and the extruded string-like material is passed through a Rheotens wheel. Thereafter, the take-up speed is gradually increased and the melt tension of the sample is measured. Regarding the measurement results, the melt tension of the sample is the average of the maximum and minimum tension values just before the point at which the string-like material breaks. If there is only one maximum point on the tension chart, that maximum value is used as the melt tension. Also, if the string-like material becomes thinner and the winding becomes idling, that point is considered to be the break point, and the average of the maximum and minimum tension values just before that point is used as the melt tension of the sample.
[0046] (Capillograph 1D measurement conditions) Die: diameter 2.095 mm, length 8 mm, inlet angle 90 degrees (conical) Barrel diameter: 9.55mm Piston speed: 20mm / min Measurement temperature: 190℃
[0047] (Rheotensile measurement conditions) Wheel spacing: Top 0.7mm, bottom 1.0mm Acceleration: 10mm / s 2 Pulling speed: Initial speed 6.92mm / s
[0048] <Melt mass-flow rate (MFR)> The melt mass flow rate (MFR) of the polylactic acid resin or resin composition can be measured using a "Semi-Auto Melt Indexer 2A" manufactured by Toyo Seiki Seisaku-sho, Ltd. MFR is measured in accordance with the method described in JIS K7210-1:2014 "Plastics - Determination of melt mass-flow rate (MFR) and melt volume-flow rate (MVR) of thermoplastic plastics - Part 1" Method B, which measures the time it takes for a piston to move a specified distance, under the following measurement conditions. The samples to be measured are vacuum dried at 90°C for at least 4 hours, and after drying, they are placed in nylon plastic bags for vacuum packing and vacuum packed until just before measurement, and then stored in a desiccator for measurement.
[0049] (Measurement conditions) Sample: 3 to 8 g Preheat time: 200 seconds Load hold: 30 seconds Test temperature: 190℃ Test load: 21.18N Piston travel distance (interval): 4mm Number of tests: 3 The arithmetic mean of the measured values obtained in each test is taken as the MFR (g / 10 min).
[0050] The above-mentioned heat-melting properties can be exhibited by imparting a bulky molecular structure to the polylactic acid resin. The polylactic acid resin preferably has a mass average molecular weight (Mw) of 100,000 or more and 1,000,000 or less. The mass average molecular weight (Mw) of the polylactic acid resin is more preferably 150,000 or more, and even more preferably 200,000 or more. The mass average molecular weight (Mw) of the polylactic acid resin is more preferably 800,000 or less, even more preferably 600,000 or less, and particularly preferably 400,000 or less.
[0051] The polylactic acid resin of this embodiment preferably has a ratio (Mw / Mn) of the mass average molecular weight (Mw) to the number average molecular weight (Mn) of 2.5 or more, more preferably 2.7 or more, and particularly preferably 2.9 or more. The ratio (Mw / Mn) of the polylactic acid resin is preferably 4.5 or less, more preferably 4.0 or less, and particularly preferably 3.5 or less.
[0052] The number-average molecular weight (Mn) and mass-average molecular weight (Mw) of polylactic acid resin can be measured using gel permeation chromatography (GPC) and calculated as polystyrene (PS) equivalent values. Specifically, the average molecular weight of polylactic acid resin can be determined by the following procedure.
[0053] (Method for determining average molecular weight) Dissolve 20 mg of the sample in 6 mL of chloroform (soaking time: 6 ± 1.0 h), filter through a non-aqueous 0.45 μm syringe filter manufactured by Shimadzu GL Sciences Inc., and then measure using a chromatograph under the following measurement conditions. Determine the mass average molecular weight of the sample from the standard polystyrene calibration curve prepared in advance.
[0054] (Equipment used) Gel permeation chromatograph "HLC-8320GPC EcoSEC" manufactured by Tosoh Corporation (equipped with RI detector and UV detector) (GPC measurement conditions) Guard column = TSK guardcolumn HXL-H (6.0 mm × 4.0 cm) × 1 piece manufactured by Tosoh Corporation Measurement column = TSKgel GMHXL (7.8 mm I.D. × 30 cm) × 2 pieces in series manufactured by Tosoh Corporation Reference side = Resistance tube (inner diameter 0.1 mm × 2 m) × 2 pieces in series Column temperature = 40 °C Mobile phase = Chloroform Mobile phase flow rate: Reference side pump = 0.5 mL / min Sample side pump = 1.0 mL / min Detector = RI detector Injection volume = 50 μL Measurement time = 25 min Sampling pitch = 500 msec
[0055] As the calibration curve standard polystyrene samples, use those with mass average molecular weights of 5,620,000, 3,120,000, 1,250,000, 442,000, 151,000, 53,500, 17,000, 7,660, 2,900, and 1,320, with product names "STANDARD SM-105" and "STANDARD SH-75" manufactured by Showa Denko K.K. The above standard polystyrene for the calibration curve was divided into groups A (5,620,000, 1,250,000, 151,000, 17,000, 2,900) and B (3,120,000, 442,000, 53,500, 7,660, 1,320), and then A (2 mg, 3 mg, 4 mg, 4 mg, 4 mg) was weighed out and dissolved in 30 mL of chloroform, and B (3 mg, 4 mg, 4 mg, 4 mg, 4 mg) was also weighed out and dissolved in 30 mL of chloroform. A standard polystyrene calibration curve is obtained by injecting 50 μL of each of the prepared solutions A and B, measuring the retention times, and creating a calibration curve (cubic equation) from the retention times. The average molecular weight is then calculated using this calibration curve.
[0056] Polylactic acid resins with such melting properties and molecular weight distribution can be obtained by modifying commercially available polylactic acid resins. The modification can involve introducing crosslinked structures or long-chain branched structures into the molecular structure of the polylactic acid resin, or increasing the molecular weight of the polylactic acid resin. Chain extenders such as carbodiimides can be used to increase the molecular weight of the polylactic acid resin. Modification with a chain extender can be carried out using compounds such as acrylic organic compounds, epoxy organic compounds, and isocyanate organic compounds, which have one or more functional groups capable of undergoing a condensation reaction with hydroxyl or carboxyl groups present in the molecular structure of the polylactic acid resin. The modification can be carried out by bonding acrylic organic compounds, epoxy organic compounds, isocyanate organic compounds, or the like to the polylactic acid resin through a reaction.
[0057] Modification of polylactic acid resin through crosslinking or long-chain branching can be achieved, for example, by reacting polylactic acid resins with each other using a radical initiator. Among the above modification methods, reacting polylactic acid resins with each other using a radical initiator is preferred because it can prevent other components from being included in the polylactic acid resin foam sheet. Furthermore, when polylactic acid resins are reacted with each other using a radical initiator with appropriate reactivity, the decomposition starting points of the polylactic acid resin in the extruder are attacked by free radicals generated by the radical initiator, and these points become crosslinking points (branching points) and can be stabilized. Such modification of polylactic acid resin increases its thermal stability and makes it less susceptible to molecular weight degradation when passing through the extruder. Examples of the radical initiator used to modify polylactic acid resin include organic peroxides, azo compounds, and halogen molecules. Among these, organic peroxides are preferred.
[0058] Examples of the organic peroxide used in this embodiment include peroxyesters, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, peroxyketals, and ketone peroxides.
[0059] Examples of the peroxy ester include t-butylperoxy 2-ethylhexyl carbonate, t-hexylperoxy isopropyl monocarbonate, t-hexylperoxybenzoate, t-butylperoxybenzoate, t-butylperoxy laurate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxy acetate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, and t-butylperoxy isopropyl monocarbonate.
[0060] Examples of the hydroperoxide include permethane hydroperoxide, diisopropylbenzene hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide.
[0061] Examples of the dialkyl peroxide include dicumyl peroxide, di-t-butyl peroxide, and 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3.
[0062] Examples of the diacyl peroxide include dibenzoyl peroxide, di(4-methylbenzoyl) peroxide, and di(3-methylbenzoyl) peroxide.
[0063] Examples of the peroxydicarbonate include di(2-ethylhexyl) peroxydicarbonate and diisopropyl peroxydicarbonate.
[0064] Examples of the peroxyketal include 1,1-di-t-butylperoxy-3,3,5-trimethylcyclohexane, 1,1-di-t-butylperoxycyclohexane, 2,2-di(t-butylperoxy)-butane, n-butyl 4,4-di-(t-butylperoxy)valerate, and 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane.
[0065] Examples of the ketone peroxide include methyl ethyl ketone peroxide and acetylacetone peroxide.
[0066] Modification with the organic peroxide may result in the modified polylactic acid resin being contaminated with components having excessively large molecular weights that will gel when thermally melted, or may cause odor problems due to the decomposition residues of the organic peroxide.
[0067] The gel contained in polylactic acid resin can cause the formation of coarse bubbles in the foam layer or tiny protrusions called "lumps." The gel content (gel fraction) of polylactic acid resin or a resin composition is preferably 4% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less. The gel content (gel fraction) of polylactic acid resin or a resin composition can be determined using the apparatus shown in Figure 3 and the following method.
[0068] <Gel content measurement method> The pellet is used as a sample. Prepare approximately 0.5 g of sample and accurately weigh out its initial mass (m0 (g)). Also, prepare a 200-mesh wire mesh (wire diameter φ0.05 mm) to filter the solution in which the sample is dissolved. The initial mass (M0 (g)) of this wire mesh is also accurately weighed. The weighed sample to be measured is placed in a 100 mL beaker (TB in Figure 3). 50 mL of chloroform as a solvent and a stirrer are placed in the beaker, and the beaker is covered with aluminum foil. Stir with a stirrer bar for 2 hours to dissolve at room temperature. After 2 hours, remove the aluminum foil and filter the solution in the beaker through the 200-mesh wire mesh. After filtration, air-dry the wire mesh in a draft for 24 hours. After drying, cool in a desiccator. After cooling, weigh the wire mesh (M1 (g)) to which the insoluble resin adheres, and calculate the gel fraction using the following formula. Gel fraction (mass%) = m1 / m0 × 100 m0: initial mass of the sample m1: Mass of insoluble resin (M1-M0) M0: initial mass of the wire mesh M1: Total mass of insoluble resin and wire mesh
[0069] The organic peroxide is preferably a peroxyester, since it can suppress the risk of gel formation and can easily modify the polylactic acid resin to a state suitable for foaming. Furthermore, among peroxyesters, the organic peroxide used to modify the polylactic acid resin is preferably a peroxycarbonate-based organic peroxide such as peroxymonocarbonate or peroxydicarbonate. In this embodiment, the organic peroxide used to modify the polylactic acid resin is preferably a peroxymonocarbonate-based organic peroxide, and particularly preferably t-butylperoxyisopropylmonocarbonate.
[0070] The organic peroxides described above are typically used in an amount of 0.1 parts by mass or more per 100 parts by mass of the polylactic acid resin to be modified, depending on factors such as the molecular weight. The amount of organic peroxide used is preferably 0.2 parts by mass or more, and particularly preferably 0.3 parts by mass or more. The amount of organic peroxide used is preferably 2.0 parts by mass or less, more preferably 1.5 parts by mass or less, and particularly preferably 1.0 part by mass or less.
[0071] By modifying polylactic acid resin using an organic peroxide in this ratio, the modified polylactic acid resin can be made suitable for foaming. By using an amount of the organic peroxide described above of 0.1 parts by mass or more, the effect of modifying the polylactic acid resin can be more reliably achieved. Furthermore, by using an amount of the organic peroxide of 2.0 parts by mass or less, the presence of gel in the modified polylactic acid resin can be suppressed.
[0072] By using multiple polylactic acid resins with different MFRs as starting materials, the polylactic acid resin of this embodiment can have a gel fraction of, for example, 1.5% by mass or less, preferably 1.0% by mass or less, and particularly preferably 0.8% by mass or less.
[0073] Examples of foaming components used when the polylactic acid resin is extruded into an extruded foam sheet include a foaming agent and a cell regulator.
[0074] As the blowing agent, a common blowing agent can be used, including a volatile blowing agent that becomes a gas at room temperature (23°C) and normal pressure (1 atmosphere) and a decomposition-type blowing agent that generates a gas by thermal decomposition. Examples of the volatile blowing agent that can be used include inert gases, aliphatic hydrocarbons, and alicyclic hydrocarbons. Examples of the inert gas include carbon dioxide and nitrogen. Examples of the aliphatic hydrocarbons include propane, normal butane, isobutane, normal pentane, and isopentane, and examples of the alicyclic hydrocarbons include cyclopentane and cyclohexane. In this embodiment, among the above, normal butane and isobutane are particularly preferred.
[0075] Examples of the decomposition type foaming agent include azodicarbonamide, dinitrosopentamethylenetetramine, sodium bicarbonate, and a mixture of an organic acid such as citric acid or a salt thereof with a bicarbonate.
[0076] Examples of the foam regulator include polytetrafluoroethylene, talc, aluminum hydroxide, silica, etc. The decomposition type foaming agent can be used in combination with a volatile foaming agent to regulate the foam state, and can also be used as a foam regulator.
[0077] Various additives can be added to the resin composition constituting the polylactic acid resin foam sheet as needed. Examples of such additives include resins other than polylactic acid resin, inorganic fillers, and various chemicals. Examples of such chemicals include nucleating agents, lubricants, antioxidants, antistatic agents, flame retardants, UV absorbers, light stabilizers, colorants, and antibacterial agents. The proportion of these additives is preferably 25 parts by weight or less, and more preferably 15 parts by weight or less, per 100 parts by weight of polylactic acid resin.
[0078] The resin composition preferably contains a nucleating agent. The nucleating agent is preferably a substance that functions like a plasticizer and can promote the crystallization of polylactic acid. As such a nucleating agent, a reaction product (A) of (A1) at least one of a polyol and a polyol dehydration condensate, (A2) an alkylene oxide mainly composed of ethylene oxide, and (A3) a fatty acid having 12 to 24 carbon atoms is used.
[0079] Examples of the polyol in (A1) "polyol and polyol dehydration condensate" include glycerin, erythritol, pentaerythritol, xylitol, sorbitol, mannitol, galactitol, and maltitol. These are also advantageous in imparting impact resistance to the polylactic acid resin foam sheet.
[0080] The above (A2) "alkylene oxide mainly composed of ethylene oxide" means that the majority of the alkylene oxide is ethylene oxide, and also includes alkylene oxides in which all of the alkylene oxide is ethylene oxide. When an alkylene oxide other than ethylene oxide is used in combination with ethylene oxide, for example, propylene oxide, butylene oxide, isobutylene oxide, etc. are used in combination.
[0081] Examples of (A3) "fatty acids having 12 to 24 carbon atoms" include saturated fatty acids such as dodecanoic acid (lauric acid), tetradecanoic acid (myristic acid), pentadecanoic acid (pentadecylic acid), hexadecanoic acid (palmitic acid), heptadecanoic acid (margaric acid), octadecanoic acid (stearic acid), icosanoic acid (arachidic acid), heneicosanoic acid (henicosylic acid), docosanoic acid (behenic acid), and tetracosanoic acid (lignoceric acid); and monounsaturated fatty acids such as myristoleic acid, palmitoleic acid, sapienic acid, oleic acid, elaidic acid, vaccenic acid, gadoleic acid, eicosenoic acid, and erucic acid. (A3) "fatty acids having 12 to 24 carbon atoms" may be diunsaturated fatty acids such as linoleic acid, triunsaturated fatty acids such as linolenic acid, or tetraunsaturated fatty acids or pentaunsaturated fatty acids. (A3) "Fatty acid having 12 to 24 carbon atoms" may be a mixture of multiple fatty acids such as coconut oil fatty acid. (A3) "Fatty acid having 12 to 24 carbon atoms" is preferably dodecanoic acid (lauric acid) or octadecanoic acid (stearic acid).
[0082] In order to provide a polylactic acid resin foam sheet with excellent impact resistance, the reaction product (A) preferably has an oxyethylene group content of 20% by mass or more and 95% by mass or less. The oxyethylene group content of the reaction product (A) is more preferably 30% by mass or more and 95% by mass or less. The reaction product (A) may be either a saturated ester in which all of the hydroxyl groups of the polyol and the polyol dehydration condensate are esterified with fatty acids, or a partial ester in which some of the hydroxyl groups are esterified. In order to provide a polylactic acid resin foam sheet with excellent impact resistance, the reaction product (A) preferably has an average number of ester groups per molecule. The average number of ester groups per molecule of the reaction product (A) is preferably more than 2 and not more than 9, more preferably more than 2.5 and not more than 6.
[0083] Examples of methods for producing the reaction product (A) include reacting a polyol with a fatty acid under heating to esterify the polyol, followed by an addition reaction with ethylene oxide in an autoclave under heating to obtain the reaction product (A). Alternatively, a dehydration condensate of a polyol may be reacted with a fatty acid to esterify the polyol, followed by addition of ethylene oxide in the same manner as described above. Alternatively, ethylene oxide may be added to a polyol and a polyol dehydration condensate, followed by reaction with a fatty acid. Another method involves synthesizing a fatty acid ester in advance from a fatty acid and a monohydric alcohol with a short carbon number (methanol, ethanol), then subjecting the ester exchange reaction with a polyol and a polyol dehydration condensate, followed by addition of ethylene oxide in the same manner as described above to obtain the reaction product (A). The reaction products (A) obtained in this manner may be used alone or in combination in the resin composition of this embodiment.
[0084] As the nucleating agent of this embodiment, for example, the following "(B) fatty acid amide" may be used instead of the above "(A) reaction product." As the nucleating agent of this embodiment, one or more of the above (A) reaction products may be used in combination with one or more of the (B) fatty acid amides.
[0085] The (B) fatty acid amide is, for example, at least one fatty acid amide selected from the group consisting of fatty monoamides, fatty acid bisamides, hydroxyl-containing fatty acid monoamides, and hydroxyl-containing fatty acid bisamides, and is preferably a fatty acid amide derived from a fatty acid having 8 to 24 carbon atoms. The (B) fatty acid amide is more preferably a fatty acid bisamide such as N,N'-ethylenebisstearamide, or a hydroxyl-containing fatty acid bisamide such as N,N'-ethylenebis(12-hydroxystearamide) or N,N'-xylylenebis(12-hydroxystearamide). Fatty acid amides are effective in imparting excellent moldability to polylactic acid resin foam sheets. Fatty acid amides are also effective in imparting excellent heat resistance and impact resistance to sheet-molded articles.
[0086] In addition, the crystal nucleating agent may be a hydrocarbon such as liquid paraffin, paraffin wax, or synthetic polyethylene wax; a metal soap such as zinc stearate, calcium stearate, or magnesium stearate; ethylene glycol, diethylene glycol, or higher polyethylene glycols; propylene glycol, dipropylene glycol, or higher polypropylene glycols; 1,3-butylene glycol, 1,4-butylene glycol, or their polymers, polybutylene glycols; or a polyglycerin, diglycerin, or higher polyglycerins.
[0087] The above-exemplified crystal nucleating agents, which function like plasticizers, can migrate to the surface layer of the polylactic acid resin foam sheet and exude from the surface, a phenomenon known as "bleed-out." In particular, fatty acid amides tend to bleed out of the polylactic acid resin foam sheet during thermoforming. While this is typically considered a problem, it can be advantageous in terms of providing adequate slippage between the sheet and the mold, thereby improving the thickness uniformity of the sheet. In other words, if good slippage is not achieved between the mold and the polylactic acid resin foam sheet, the polylactic acid resin foam sheet may be locally stretched, resulting in thin-walled areas in the sheet. However, using fatty acid amides as crystal nucleating agents can avoid this problem. Furthermore, the tendency to bleed out reduces the amount of the agent remaining in the sheet, thereby preventing further crystallization-induced distortion in the case of unintended heating of the sheet.
[0088] The nucleating agent can be used in a proportion of 0.5 to 15 parts by mass per 100 parts by mass of polylactic acid resin. The proportion of the nucleating agent may be 1 part by mass or more, or 1.5 parts by mass or more. The proportion of the nucleating agent per 100 parts by mass of polylactic acid resin may be 10 parts by mass or less, or 5 parts by mass or less.
[0089] The polylactic acid resin foam sheet of this embodiment can be produced by carrying out a process of modifying polylactic acid resin using a twin-screw extruder or the like (modification process), and a process of extrusion-foaming a polylactic acid resin composition containing the modified polylactic acid resin through an extruder equipped with a circular die at its tip (extrusion-foaming process).
[0090] In the modification step, for example, a twin-screw extruder equipped with a granulation die (hot-cut die) may be used to pelletize the modified polylactic acid resin immediately after the modification step. The twin-screw extruder used in the modification step may be equipped with a strand die or T-die, and the modified polylactic acid resin may be formed into strands or sheets in the modification step, followed by a separate step of cutting the strands or sheets and granulating them. Furthermore, as mentioned above, if necessary, a tandem extruder may be used to perform an extrusion-foaming step immediately following the modification step.
[0091] In the extrusion foaming process described above, the resin composition of this embodiment does not easily stretch, and the cell membrane is less likely to become excessively thin. That is, in the polylactic acid resin foam sheet of this embodiment, the cell membrane containing the polylactic acid resin described above exhibits a certain level of resistance when stretched by the foaming force of the foaming agent. Furthermore, in the polylactic acid resin foam sheet of this embodiment, the cell membrane tends to be thin in the center and thick at the periphery. Therefore, the polylactic acid resin foam sheet of this embodiment exhibits excellent mechanical properties because the thick cell membrane is three-dimensionally connected throughout the entire sheet.
[0092] In the polylactic acid resin foam sheet of this embodiment, even if bubbles break during foaming and a hole is created in the bubble film, the bubble film surrounding the hole does not remain as it is but shrinks and increases in thickness in a manner that is effective in exhibiting strength, so that the sheet can exhibit excellent strength even if it has a certain proportion of open bubbles.
[0093] The apparent density of the polylactic acid resin foam sheet is preferably 63 kg / m 3 More than 500kg / m 3More preferably, it is 83 kg / m or less. 3 More than 250kg / m 3 The apparent density of the polylactic acid resin foam sheet is 63 kg / m or less. 3 As a result of the above, the sheet molding of this embodiment has high strength, and further has the advantage that the thermoformability of the polylactic acid resin foam sheet is good, allowing it to be molded into a shape that conforms to the mold.
[0094] The apparent density of the polylactic acid resin foam sheet is 500 kg / m 3 By satisfying the following conditions, there is an advantage that the sheet molding of this embodiment can easily exhibit the characteristics of a foam, such as light weight, heat insulating properties, and shock absorbing properties.
[0095] The thickness of the polylactic acid resin foam sheet is preferably 0.5 mm to 7 mm, more preferably 0.5 mm to 5 mm, and even more preferably 0.7 mm to 3 mm. When the thickness of the polylactic acid resin foam sheet is 0.5 mm or more, the sheet molded article of this embodiment has the advantage of being high in strength. Furthermore, when the thickness of the polylactic acid resin foam sheet is 7 mm or less, the thermoformability is improved, and as a result, the sheet molded article of this embodiment has less thickness unevenness.
[0096] <Apparent density> Apparent density (kg / m) of polylactic acid resin foam sheet 3 ) is the mass of the polylactic acid resin foam sheet per unit area (basis weight: g / m 2 ) by the thickness (mm) of the polylactic acid resin foam sheet. The basis weight can be calculated by arithmetically averaging the measured values of multiple samples cut out from the polylactic acid resin foam sheet. The basis weight of the polylactic acid resin foam sheet is calculated by cutting out a measurement sample from the polylactic acid resin foam sheet so that the dimension in the extrusion direction (MD) is 20 cm and the dimension in the transverse direction (TD) is the full width, and calculating the mass W (g) and area S (cm 2 ) can be calculated using the following formula: Basis weight (g / m 2 )=W / S×10000 The apparent density can be calculated as follows: Apparent density (kg / m 3 ) = basis weight (g / m 2 ) ÷ thickness (mm)
[0097] <Thickness> The thickness of the polylactic acid resin foam sheet can be determined by taking an enlarged photograph of a cross section of the polylactic acid resin foam sheet cut along a plane perpendicular to the polylactic acid resin foam sheet, and is calculated, for example, as the average value of multiple randomly selected locations (e.g., 20 locations).
[0098] The polylactic acid resin foam sheet preferably has a predetermined average cell diameter. The average cell diameter is preferably 0.1 mm to 1 mm, more preferably 0.1 mm to 0.8 mm, and even more preferably 0.1 mm to 0.6 mm. When the average cell diameter of the polylactic acid resin foam sheet is 0.1 mm or more, the open cell ratio tends to be low, resulting in the advantages of a low apparent density of the sheet molded body and improved thermoformability of the polylactic acid resin foam sheet, thereby reducing thickness unevenness of the sheet molded body. Furthermore, when the average cell diameter of the polylactic acid resin foam sheet is 1 mm or less, the sheet molded body of this embodiment exhibits excellent foam characteristics such as heat insulation and cushioning properties. The average cell diameter of the sheet molded body of this embodiment is preferably the same value as the average cell diameter of the polylactic acid resin foam sheet described above.
[0099] (average bubble diameter) The average cell diameter can be measured in accordance with the test method of ASTM D2842-69. Specifically, the polylactic acid resin foam sheet was cut along the extrusion direction (MD) and the transverse direction (TD) perpendicular to the extrusion direction, and the center of each cut surface was magnified using a scanning electron microscope (S-3000N, manufactured by Hitachi, Ltd.) to take two photographs at different locations. Next, the captured image is printed on A4 paper and three 60 mm long straight lines are drawn on the image. For the cut surface cut in the MD direction, a straight line is drawn parallel to the MD, and for the cut surface cut in the TD direction, a straight line is drawn parallel to the TD. Furthermore, for the thickness direction (VD), a straight line is drawn on one image for each of the MD and TD. The magnification of the electron microscope is adjusted so that there are six or more bubbles on each straight line. Then, the average chord length (t) of the bubbles is calculated from the average number of bubbles in each direction on the six lines drawn in each direction using the formula below, and the bubble diameter in each direction (MD, TD, VD) is calculated from this average chord length using the formula below. Average chord length t = 60 (mm) / (number of bubbles x magnification of photo) Bubble diameter D=t / 0.616(mm) When drawing a straight line, the straight line should penetrate as far as possible without making point contact with the air bubbles. If some air bubbles make point contact with the straight line, these air bubbles are also included in the number of bubbles. Furthermore, if both ends of the straight line are located inside the air bubbles without penetrating them, the air bubbles where both ends of the straight line are located are also included in the number of bubbles. The obtained bubble diameter (D MD ) and bubble diameter at TD (D TD ) and bubble diameter at VD (D VD ) is defined as the average cell diameter of the polylactic acid resin foam sheet. That is, the average cell diameter of the polylactic acid resin foam sheet is calculated by the following formula. Average bubble diameter (mm) = (D MD ×D TD ×D VD ) 1 / 3
[0100] The open cell ratio of the polylactic acid resin foam sheet is preferably 50% or less, more preferably 40% or less, and even more preferably 30% or less. Having an open cell ratio of 50% or less in the polylactic acid resin foam sheet has the advantage of providing particularly excellent mechanical strength and secondary foaming properties during thermoforming. Furthermore, a sheet molded product produced from such a polylactic acid resin foam sheet has excellent mechanical strength and also excellent appearance, such as mold reproducibility. In this embodiment, the open cell ratio of the sheet molded product itself is preferably the above-mentioned value. The open cell ratio can be determined as follows.
[0101] (Open cell ratio) The open cell ratio can be determined by the following method. Several sheet-like samples measuring 25 mm long x 25 mm wide are cut out from the polylactic acid resin foam sheet. The cut samples are stacked without leaving any gaps to form test pieces with a thickness of 21 to 23 mm, and three test pieces are prepared. The test pieces are conditioned for 16 hours in a JIS K7100:1999 symbol 23 / 50, class 2 environment, and the thickness (mm) is measured. For example, a "Digimatic Caliper" caliper manufactured by Mitutoyo Corporation can be used to measure the thickness. The thickness is measured to the nearest 1 / 100 mm, and the apparent volume (cm) is calculated from the obtained thickness. 3 ) is found. Next, the volume (cm ) of the test piece was measured under the above environment using a dry automatic density meter (for example, "AccuPic II 1340-100cc" manufactured by Shimadzu Corporation). 3 ) is measured. The measurement conditions are as follows: Gas used: Nitrogen Container used: 35cc Filling pressure: 0.005 psig Pressure equilibrium end rate: 0.005 psig / min Repeat count: 1 time The open cell rate (%) of each test piece is calculated using the following formula, and the average value is taken as the apparent density of the polylactic acid resin foam sheet. Open cell rate (%) = [(apparent volume - volume measured with dry automatic density meter) / apparent volume] x 100 (%)
[0102] Next, a method for manufacturing the sheet molded body of this embodiment will be described. The method for manufacturing a sheet molded body of this embodiment is a method for forming a sheet molded body by carrying out a primary heating step in which the polylactic acid resin foam sheet is heated, and a secondary heating step in which the polylactic acid resin foam sheet that has been subjected to the primary heating step is sandwiched between heated molds to produce a sheet molded body and increase the crystallinity of the sheet molded body.
[0103] In the primary heating step, the polylactic acid resin foam sheet can be heated by a known method, such as sandwiching the polylactic acid resin foam sheet between heating plates or heating the foam sheet with an electric heater. In the method for producing a sheet molded product of this embodiment, the polylactic acid resin foam sheet is heated in the primary heating step so that the surface temperature of the polylactic acid resin foam sheet reaches preferably 60°C or higher, more preferably 70°C or higher, even more preferably 80°C or higher, and particularly preferably 90°C or higher. Heating in the primary heating step is preferably carried out so that the surface temperature of the polylactic acid resin foam sheet reaches 130°C or lower, and more preferably 120°C or lower.
[0104] In the method for producing a sheet molded body of this embodiment, by setting the surface temperature of the polylactic acid resin foam sheet in the primary heating step to the above-mentioned temperature, the transferability of the molding die is improved, and the polylactic acid resin foam sheet is in a favorable softened state, thereby preventing the polylactic acid resin foam sheet from breaking during molding. In addition, in the method for producing a sheet molded body of this embodiment, by setting the surface temperature of the polylactic acid resin foam sheet in the primary heating step to preferably 130°C or less, more preferably 120°C or less, the surface condition of the polylactic acid resin foam sheet is improved, and further, moderate crystallization progresses in the primary heating step, increasing the crystallinity of the formed sheet molded body, which has the advantage of making it easier to obtain a sheet molded body with excellent heat resistance.
[0105] In the secondary heating step, a pair of male and female molds is preferably used as the molding die. In the secondary heating step, the polylactic acid resin foam sheet heated and softened in the primary heating step is sandwiched between the heated male and female molds, shaped, and maintained in this state for a certain period of time, thereby forming a sheet molding and increasing its crystallinity.
[0106] The secondary heating step is carried out by adjusting the temperature of the mold to preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher. The secondary heating step is carried out by adjusting the temperature of the mold to preferably 130°C or lower, more preferably 120°C or lower. By adjusting the temperature of the mold to 50°C or higher in the secondary heating step, there is an advantage that the crystallinity of the sheet-formed body is easily increased, and there is also an advantage that the time required for crystallization is easily shortened, which makes it easier to increase productivity. In addition, by adjusting the heated mold to 130°C or lower in the secondary heating step, there is an advantage that the surface condition of the sheet-formed body is improved.
[0107] In the method for producing a sheet molded body of this embodiment, from the viewpoint of obtaining a polylactic acid resin foam sheet in which the difference between the heat absorption and heat generation is within a preferred range, it is preferable to cool the polylactic acid resin foam sheet obtained by the extrusion foaming method with air or water immediately after extrusion, or to adjust the temperature by keeping the sheet warm with heated air or hot water. The sheet molded body formed by the method for producing a sheet molded body of this embodiment is a molded body with excellent heat resistance. Because of its excellent heat resistance, the sheet molded body of this embodiment can be suitably used as a food packaging container such as a lunch box, a cup noodle container, or a microwaveable container.
[0108] The above examples of the polylactic acid resin foam sheet and sheet molding of this embodiment, and the manufacturing methods thereof, are merely restrictive examples, and the present invention is in no way limited to the above examples, and can be practiced by making appropriate modifications to the above examples. As described above, the present embodiment includes the following disclosures.
[0109] (1) A polylactic acid resin foam sheet made of a polylactic acid resin composition containing a crystalline polylactic acid resin, The crystallinity is 30% or less, A polylactic acid resin foam sheet that exhibits a crystallization temperature of 105°C or less when measured by heat flux differential scanning calorimetry at a heating rate of 5°C / min.
[0110] (2) The polylactic acid resin foam sheet according to (1), wherein the polylactic acid resin composition has a semi-crystallization time of 30 minutes or less at 80°C.
[0111] (3) The polylactic acid resin foam sheet according to (1) or (2), wherein the polylactic acid resin composition contains the polylactic acid resin, which is a copolymer of D- and L-forms of lactic acid, and the D-form content in the copolymer is 0.5 mol % or more and 5 mol % or less, and the melting point of the copolymer is 130°C or more and 170°C or less.
[0112] (4) Apparent density 63kg / m 3 More than 500kg / m 3 A polylactic acid resin foam sheet according to any one of (1) to (3) below:
[0113] (5) The polylactic acid resin foam sheet according to any one of (1) to (4), having a thickness of 0.5 mm or more and 7 mm or less.
[0114] (6) The polylactic acid resin foam sheet according to any one of (1) to (5), having an open cell ratio of 50% or less.
[0115] (7) The polylactic acid resin foam sheet according to any one of (1) to (6), wherein the polylactic acid resin composition contains a modified polylactic acid resin, which is a product modified with an organic peroxide, as the polylactic acid resin.
[0116] (8) The polylactic acid resin foam sheet according to any one of (1) to (7), wherein the polylactic acid resin composition contains a crystal nucleating agent.
[0117] (9) A method for producing a sheet molded body by thermoforming a resin foam sheet, comprising: The resin foam sheet is The polylactic acid resin composition contains a crystalline polylactic acid resin. The crystallinity is 30% or less, A polylactic acid resin foam sheet that exhibits a crystallization temperature of 105°C or less when measured by heat flux differential scanning calorimetry at a heating rate of 5°C / min. a primary heating step of heating the polylactic acid resin foam sheet; The method for producing a sheet molded body includes sandwiching the polylactic acid resin foam sheet that has undergone the primary heating step between heated molds to produce a sheet molded body, and then carrying out a secondary heating step to increase the crystallinity of the sheet molded body.
[0118] (10) In the first heating step, The method for producing a sheet molded body according to (9), wherein the polylactic acid resin foam sheet is heated so that the surface temperature is 60°C or higher and 130°C or lower.
[0119] (11) The method for producing a sheet molded body according to (9) or (10), wherein the temperature of the mold is adjusted to 50° C. or higher and 130° C. or lower in the secondary heating step. [Example]
[0120] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples. (Reference production example 1) (1) Preparation of modified polylactic acid resin Polylactic acid resin (MFR = 10.0 g / 10 min, density = 1240 kg / m 3100 parts by mass of t-butylperoxyisopropyl monocarbonate (1-minute half-life temperature T1: 158.8°C) and 0.5 parts by mass of t-butylperoxyisopropyl monocarbonate (1-minute half-life temperature T1: 158.8°C) were stirred and mixed in a ribbon blender to obtain a mixture. The resulting mixture was fed into a twin-screw extruder (L / D=31.5) with a diameter of 57 mm. The temperature of the feed section was set to 170°C, and the temperatures thereafter to 230°C. The mixture was melt-kneaded in a twin-screw extruder at a rotation speed of 150 rpm, and the kneaded material was extruded in the form of strands at a discharge rate of 50 kg / h from a die with a diameter of 3 mm and 18 holes attached to the tip of the extruder. Next, the extruded strand-like kneaded product was passed through a 2 m long cooling water tank containing water at 30°C to cool it. The cooled strand was cut with a pelletizer to obtain pellets of the modified polylactic acid resin.
[0121] (Reference production examples 2-5) For Reference Manufacturing Examples 2 to 5, modified polylactic acid resins were prepared in the same manner as Reference Manufacturing Example 1, except that the type of polylactic acid resin and the amount of organic peroxide added (amount added (parts by mass) per 100 parts by mass of polylactic acid resin) were changed.
[0122] (Reference examples 1 and 2) Reference Examples 1 and 2 are commercially available polylactic acid resins, which are raw materials before the above-described reactions are carried out. Table 1 shows the types of polylactic acid resins and organic peroxides used in Reference Production Examples 1 to 5, the amounts (parts by mass) of organic peroxides added per 100 parts by mass of polylactic acid resin, and the physical properties of the resulting polylactic acid resins.
[0123] [Table 1]
[0124] (Production of polylactic acid foam sheets) Example 1 A mixture was prepared by dry blending 100 parts by mass of the polylactic acid resin obtained in Reference Production Example 1 and 1.0 part by mass of a cell adjusting agent ("Crown Talc" manufactured by Matsumura Sangyo Co., Ltd.). The mixture was supplied through a hopper to the first extruder (diameter φ50 mm) of a tandem extruder equipped with a first extruder (upstream side) with a diameter of φ50 mm and a second extruder (downstream side) with a diameter of φ65 mm, and was heated and melted in the first extruder. Thereafter, butane (isobutane / normal butane=70 / 30) as a foaming agent was pressure-fed into the first extruder and melt-mixed with the mixture. Next, this molten mixture was transferred to a second extruder with a diameter of 65 mm and uniformly cooled to a temperature suitable for extrusion foaming, and then extrusion foaming was carried out through a circular die with a diameter of 70 mm at a discharge rate of 30 kg / h to obtain a cylindrical foam. The obtained cylindrical foam was placed on a φ206 mm mandrel whose inside was cooled with water at approximately 20°C, and its outer surface was cooled and molded by blowing air onto it using an air ring larger than the diameter of the mandrel.The foam was then cut open at one point on the circumference using a cutter to obtain a strip-shaped polylactic acid resin foam sheet.
[0125] Example 2 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that 10 parts by mass of a nucleating agent (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., trade name "TRIBIO S-920MB") was added per 100 parts by mass of the polylactic acid resin.
[0126] Example 3 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that 2 parts by mass of a nucleating agent (manufactured by Ito Oil Mills, trade name "ITOHWAX J-530" (fatty acid amide)) was added per 100 parts by mass of the polylactic acid resin.
[0127] Example 4 A polylactic acid resin foam sheet was obtained in the same manner as in Example 3, except that the polylactic acid resin used was changed to that obtained in Reference Production Example 2.
[0128] Example 5 A polylactic acid resin foam sheet was obtained in the same manner as in Example 3, except that the amount of the nucleating agent added was changed from 2 parts by mass to 3 parts by mass.
[0129] Example 6 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that 3 parts by mass of polyethylene glycol (PEG-4000P) was added as a nucleating agent relative to 100 parts by mass of the polylactic acid resin.
[0130] Example 7 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that the product names "ITOHWAX J-530" and "PEG-4000P" were used in combination as nucleating agents, and the amount of each added was 3 parts by mass (6 parts by mass in total) per 100 parts by mass of polylactic acid resin.
[0131] Example 8 A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that the polylactic acid resin used was changed to that obtained in Reference Production Example 3.
[0132] Example 9 A polylactic acid resin foam sheet was obtained in the same manner as in Example 3, except that the polylactic acid resin used was changed to that obtained in Reference Production Example 4.
[0133] (Comparative Example 1) A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that a combination of the product names "ITOHWAX J-530" and "PEG-4000P" was used as a nucleating agent, and the amount of "ITOHWAX J-530" added was 1 part by mass and the amount of "PEG-4000P" added was 4 parts by mass per 100 parts by mass of polylactic acid resin.
[0134] (Comparative Example 2) A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that the polylactic acid resin used was changed to that obtained in Reference Production Example 4.
[0135] (Comparative Example 3) A polylactic acid resin foam sheet was obtained in the same manner as in Example 1, except that the polylactic acid resin used was changed to that obtained in Reference Production Example 5.
[0136] (Comparative Examples 4 and 5) An attempt was made to produce a polylactic acid resin foam sheet in the same manner as in Example 1, except that the polylactic acid resins used were those of Reference Example 1 (Comparative Example 4) and Reference Example 2 (Comparative Example 5). However, the melt tension of the resin was low, and a polylactic acid resin foam sheet in good condition could not be obtained.
[0137] <Molding> A flat square test piece measuring 340 mm long x 340 mm wide was cut out from each polylactic acid resin foam sheet. A single-shot molding machine (manufactured by Tosei Sangyo Co., Ltd., product name "FM-3A") was used, and the average temperature of the upper heater of this single-shot molding machine was set to 300°C, and the average temperature of the lower heater was set to 300°C. Next, the test pieces were introduced into a single-shot molding machine and heated for 30 seconds. Then, using a mold heated and maintained at 100°C, five sheet-formed bodies (foamed containers) with openings at the top were produced by thermoforming for each example. Note that the surface temperature of the polylactic acid resin foamed sheet in the first heating step under the above conditions was about 120°C. The containers were in the shape of an inverted truncated pyramid with a square bottom, and the dimensions of each part were as follows: Opening: 140mm x 150mm Bottom: 110mm x 110mm Height: 60mm
[0138] The crystallinity and shrinkage upon heating (hereinafter referred to as heat shrinkage) of each of the obtained containers were measured. The shrinkage upon heating was measured by the following method.
[0139] (heat shrinkage rate) For measuring the heat shrinkage rate, an air circulation oven, for example, a product name "MODEL PSL-2" manufactured by Tabai Espec Co., Ltd., was used. The heat shrinkage rate was calculated from the measured values obtained by placing each of the resulting containers in an air-circulating oven heated to 100°C and heating for 150 seconds, then removing the container from the oven and measuring the length of each side of the container. The heat shrinkage rate of the container is the difference between the length before heating and the length after heating, divided by the length before heating, and multiplied by 100, and is calculated for each of the two sides of the opening of the container. Based on the calculated values, evaluation was carried out according to the following evaluation criteria.
[0140] <Evaluation Criteria> ·〇: Both sides were within 5%. ·△: One side was "within 5%" and the other side was "more than 5%". ·×: Both sides were "over 5%".
[0141] The thickness, weight, expansion ratio, open cell ratio, average cell diameter, degree of crystallinity, crystallization temperature and half-crystallization time of the polylactic acid resin foam sheets of the examples and comparative examples were also measured. The expansion ratio was measured by the following method. The other items were measured by the methods described above.
[0142] (Expansion ratio) Three 10 x 10 cm measurement samples were cut out from the polylactic acid resin foam sheet in the transverse direction (TD), and the thickness and mass of each sample were measured. The arithmetic mean value of the density calculated from the mass and volume of each sample was used as the apparent density of the polylactic acid resin foam sheet. And the density of polylactic acid resin (1240 kg / m 3 ) divided by the apparent density of the polylactic acid resin foam sheet was taken as the expansion ratio. Expansion ratio = 1240 / apparent density of polylactic acid resin foam sheet (kg / m 3 )
[0143] The results are shown in Tables 2 and 3 below.
[0144] [Table 2]
[0145] [Table 3]
[0146] From the above, it can be seen that the present invention can provide a polylactic acid resin foam sheet suitable for efficiently producing a sheet molding having excellent heat resistance. [Explanation of symbols]
[0147] 1: Polylactic acid resin foam sheet, 100: Sheet manufacturing equipment
Claims
1. A polylactic acid resin foam sheet composed of a polylactic acid resin composition containing a crystalline polylactic acid resin, The crystallinity is 30% or less. A polylactic acid resin foam sheet that exhibits a crystallization temperature of 105°C or less when measured by heat flux differential scanning calorimetry at a heating rate of 5°C / min.
2. 2. The polylactic acid resin foam sheet according to claim 1, wherein the polylactic acid resin composition has a semi-crystallization time at 80° C. of 30 minutes or less.
3. 3. The polylactic acid resin foam sheet according to claim 1 or 2, wherein the polylactic acid resin composition contains the polylactic acid resin which is a copolymer in which D- and L-forms of lactic acid are copolymerized, the content of the D-form in the copolymer is 0.5 mol % or more and 5 mol % or less, and the melting point of the copolymer is 130° C. or more and 170° C. or less.
4. Apparent density 63 kg / m 3 More than 500kg / m 3 3. The polylactic acid resin foam sheet according to claim 1, wherein:
5. 3. The polylactic acid resin foam sheet according to claim 1, having a thickness of 0.5 mm or more and 7 mm or less.
6. 3. The polylactic acid resin foam sheet according to claim 1, wherein the open cell ratio is 50% or less.
7. 3. The polylactic acid resin foam sheet according to claim 1, wherein the polylactic acid resin composition contains, as the polylactic acid resin, a modified polylactic acid resin which is a product modified with an organic peroxide.
8. 3. The polylactic acid resin foam sheet according to claim 1, wherein the polylactic acid resin composition contains a crystal nucleating agent.
9. A method for producing a sheet molded body by thermoforming a resin foam sheet, comprising the steps of: The resin foam sheet is The polylactic acid resin composition includes a polylactic acid resin having crystallinity. The crystallinity is 30% or less. A polylactic acid resin foam sheet having a crystallization temperature of 105° C. or less as measured by heat flux differential scanning calorimetry at a heating rate of 5° C. / min. a primary heating step of heating the polylactic acid resin foam sheet; The method for producing a sheet molded body includes a secondary heating step in which the polylactic acid resin foamed sheet subjected to the primary heating step is sandwiched between a heated mold to produce a sheet molded body and to increase the crystallinity of the sheet molded body.
10. In the first heating step, The method for producing a sheet molded article according to claim 9, wherein the polylactic acid resin foam sheet is heated so that the surface temperature is 60° C. or more and 130° C. or less.
11. The method for producing a sheet molded body according to claim 9 or 10, wherein the temperature of the mold is adjusted to 50° C. or higher and 130° C. or lower in the secondary heating step.
Citation Information
Patent Citations
Method of manufacturing polyester based resin foamed molding, and polyester based resin foamed molding
JP2012020444A
Polylactic acid-based resin-foamed sheet molding, and method for producing the same
JP2014139333A
Polylactic resin foam sheet, resin molding, and method for producing polylactic resin foam sheet
JP2020158608A
Excitation circuit for synchronous generator
JP1980017280A