Stretch film

The stretch film with a styrene elastomer layer and olefin resin surface layer addresses stickiness and enhances stretchability, achieving high elasticity and reduced hysteresis loss for improved handling and performance.

JP2024141258AActive Publication Date: 2024-10-10C I TAKIRON CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023052797
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Stretch films with elastomer layers are highly sticky, making them difficult to handle, especially in thin films, and they lack stretchability similar to that of the body.

Method used

A stretch film comprising an elastomer layer with a surface layer made of an olefin resin composition containing an olefin resin and an inorganic filler, characterized by a hysteresis loss of less than 36%, which includes a styrene elastomer in the elastomer layer and optionally an olefin elastomer in the core layer, with specific compositions and thickness ratios to enhance stretchability and reduce stickiness.

Benefits of technology

The film achieves excellent stretchability and reduces stickiness, maintaining high elasticity and dimensional stability, with a hysteresis loss of less than 36%, ensuring effective handling and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141258000001_ABST
    Figure 2024141258000001_ABST
Patent Text Reader

Abstract

To provide a stretch film which has a surface layer laminated to the surface of the elastomer layer, wherein the stretch film has excellent elasticity.SOLUTION: There is provided a stretch film 1 which comprises an elastomer layer 5 and surface layers 6, 7 formed on the surfaces of the elastomer layer 5, wherein the elastomer layer 5 includes a styrene-based elastomer and the surface layers 6, 7 are formed of an olefin-based resin composition comprising an olefin-based resin and an inorganic filler and the stretch film has a hysteresis loss less than 36%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stretch film. [Background technology]

[0002] Stretch films are used in a wide range of fields, including hygiene products, sporting goods, and medical products, to improve handling, wearing comfort (fit), etc. For example, they are used in garments such as underwear, waistbands of disposable diapers, side panels, leg gathers, incontinence products, sanitary napkins, bandages, surgical drapes, tightening bands, hats, swimming trunks, sports supports, medical product supports, bandages, etc.

[0003] Here, stretch films using stretchable elastomers have a strong stickiness due to the properties of the elastomer, and there has been a problem in that they are difficult to handle, particularly in thin films.

[0004] In order to prevent stickiness caused by the elastomer, a stretch film has been proposed that has a surface layer formed of a less sticky resin on the surface of the elastomer. More specifically, for example, a stretch film has been proposed that has an olefin-based resin layer laminated on at least one surface of an elastomer layer (for example, see Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-112878 A Summary of the Invention [Problem to be solved by the invention]

[0006] Generally, the elasticity of a film is evaluated by permanent strain (strain that remains after an external force is applied to the film and then removed), but there is a problem in that it is difficult to obtain an elastic film with elasticity approximating that of an ideal elastic body such as rubber by evaluation based solely on permanent strain.

[0007] Therefore, the present invention has been made in consideration of the above problems, and aims to provide a stretch film having a surface layer laminated on the surface of an elastomer layer, which has excellent stretchability. [Means for solving the problem]

[0008] In order to achieve the above object, the stretch film of the present invention is a stretch film comprising an elastomer layer and a surface layer laminated on at least one side of the elastomer layer, wherein the elastomer layer contains a styrene-based elastomer, and the surface layer is made of an olefin-based resin composition containing an olefin-based resin and an inorganic filler, and is characterized in that the hysteresis loss described below is less than 36%.

[0009] (Hysteresis loss) A rectangular test piece measuring 100 mm in one direction of the film and 25 mm in the direction perpendicular to that direction is cut from the stretch film, and this test piece is fixed to the grips of the testing machine so that the distance between the grips is 25 mm. The test piece is stretched in the longitudinal direction of the test piece at a speed of 254 mm / min so that the strain (elongation) calculated by the following formula (1) becomes 100%. The integral area of ​​the stress-strain curve (SS curve) when this is reached is S1, and immediately after stretching, the test piece is contracted at the same speed until the load (N / 25 mm) of the test piece becomes 0. The integral area of ​​the stress-strain curve (SS curve) when this is reached is S2. Calculate the hysteresis loss [%] from the following formula (2).

[0010] Distortion [%] = (L1-L0) / L0 × 100 (1) Hysteresis loss [%] = S / S1 × 100 (2)

[0011] where L0 is the distance between the grippers before stretching (mm), L1 is the distance between the grippers after stretching (mm), S1 is the integral area in the stress-strain curve when the specimen is stretched from 0% to 100% strain, S2 is the integral area in the stress-strain curve when the specimen is contracted from 100% strain to 0 stress, and S is the integral area (S1-S2) in the stress-strain curve obtained by subtracting the integral area S2 from the integral area S1. Effect of the Invention

[0012] According to the present invention, it is possible to provide a stretch film having excellent stretchability, which has a surface layer laminated on the surface of an elastomer layer. [Brief description of the drawings]

[0013] [Figure 1] 1 is a cross-sectional view showing a stretch film according to a first embodiment of the present invention. [Diagram 2] FIG. 1 is a plan view showing a stretch film according to a first embodiment of the present invention. [Diagram 3] FIG. 1 is a diagram showing the integral area S1 in a stress-strain curve when stretching from 0% to 100% strain. [Figure 4] FIG. 13 is a diagram showing the integral area S2 in a stress-strain curve when contracting from a strain of 100% to a stress of 0. [Diagram 5] FIG. 1 is a diagram showing the integral area in a stress-strain curve obtained by subtracting the integral area S2 from the integral area S1. [Figure 6] FIG. 4 is a cross-sectional view showing a stretch film according to a second embodiment of the present invention. [Figure 7] FIG. 4 is a plan view showing a stretch film according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The stretch film of the present invention will be specifically described below. Note that the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.

[0015] [First embodiment] 1 is a cross-sectional view showing a stretch film according to the present embodiment. As shown in Fig. 1, the stretch film 1 of the present embodiment includes an elastomer layer 5 and surface layers 6 and 7 laminated on the surface of the elastomer layer 5.

[0016] (Elastomer layer) The elastomer layer 5 is a layer that imparts elasticity to the stretch film 1, and this elastomer layer 5 contains a styrene-based elastomer, which is a thermoplastic elastomer.

[0017] <Thermoplastic elastomer> "Thermoplastic elastomer" means a polymer or polymer blend which has properties similar to vulcanized rubber at use temperatures, loses these properties at processing temperatures, is readily processable, and regains its original properties when returned to use temperatures.

[0018] Furthermore, by using a styrene-based elastomer, the film is less likely to stretch, and the dimensional stability during transport is improved.

[0019] Examples of the styrene-based elastomer used in the present invention include styrene-isoprene-styrene copolymer (SIS elastomer), styrene-isoprene block copolymer, styrene-butadiene-styrene block copolymer (SBS elastomer), styrene-butadiene block copolymer, hydrogenated product of styrene-isoprene-styrene block copolymer (styrene-ethylene-propylene-styrene block copolymer (SEPS elastomer)), hydrogenated product of styrene-butadiene-styrene block copolymer (styrene-ethylene-butylene-styrene block copolymer (SEBS elastomer)), styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS elastomer), etc. Among these, SIS elastomer is preferable because of its higher elasticity. The styrene-based elastomer may be used alone or in combination of two or more kinds.

[0020] Thermoplastic elastomers are generally composed of hard segments that govern basic physical properties such as mechanical properties, and soft segments that govern elasticity, which is a rubber-like property. Examples of hard segments of styrene-based elastomers include polystyrene, and examples of soft segments of styrene-based elastomers include polybutadiene, polyisoprene, polyethylene, or hydrogenated products thereof.

[0021] In addition, when an SIS elastomer is used, the content of styrene units relative to the total units of the SIS elastomer is preferably 9% by mass or more and less than 50% by mass, and more preferably 12% by mass or more and less than 30% by mass. If the content of styrene units, which are hard segments, is 9% by mass or more, the stress at 10% elongation [N / mm 2 If the content is less than 50% by mass, the elasticity of the soft segment will result in excellent stretchability in the direction perpendicular to the machine axis direction (hereinafter also referred to as "TD") shown in Figure 2.

[0022] The Shore A hardness of the SIS elastomer is preferably 20 or more and less than 70. If the Shore A hardness is 20 or more, the stress at 10% elongation in the MD [N / mm 2 In addition, if the Shore A hardness is less than 70, the stretchability in TD can be improved.

[0023] The "Shore A hardness" referred to here is that measured using a Type A durometer in accordance with JIS K 6253 at a temperature of 23°C.

[0024] In addition, when the SIS elastomer is used alone, the styrene unit content relative to the total units of the SIS elastomer (i.e., the entire elastomer layer) is preferably 30% by mass or less, more preferably 20% by mass or less. If the styrene unit content of the SIS elastomer is greater than 30% by mass, styrene has poor elasticity, and the hysteresis loss described below increases, which may reduce the elasticity of the elastic film.

[0025] In addition, when the SIS elastomer is blended with other elastomers (for example, when SIS elastomers having different styrene unit contents are blended), the styrene unit content in the entire elastomer layer is preferably 9% by mass or more and 35% by mass or less. If the styrene unit content is 9% by mass or more, the stress at 10% elongation in MD [N / mm 2 When the content is 35% by mass or less, excellent stretchability in TD can be obtained due to the elasticity of the soft segment.

[0026] In addition, when a SIS elastomer is used, the Shore A hardness of the entire elastomer layer is preferably 30 or more and less than 60. If the Shore A hardness is 30 or more, the stress at 10% elongation in the MD [N / mm 2 In addition, if the Shore A hardness is less than 60, the decrease in stretchability in TD can be suppressed.

[0027] In addition, if the Shore A hardness of the entire elastomer layer is 30 or more, the stress at 10% elongation in the MD of the stretch film [N / mm 2 ] is improved, and excellent transportability is obtained, but stretchability in TD is decreased. In other words, since there is a trade-off between transportability in MD and stretchability in TD, the inventors set the Shore A hardness of the entire elastomer layer to 30 or more, and set the stress at 10% elongation in MD [N / mm 2 In order to improve the elasticity in TD and to improve the reduced elasticity in TD, it has been found that the styrene unit content in the entire elastomer layer is set to 35 mass % or less.

[0028] The melt mass flow rate (MFR) of the styrene elastomer is preferably 0.5 to 22 g / 10 min, more preferably 3 to 15 g / 10 min. If the MFR of the styrene elastomer is greater than 22 g / 10 min, the melt viscosity may be too low, making it difficult to control the thickness during film molding. If the MFR of the styrene elastomer is less than 0.5 g / 10 min, melt fracture may occur during film molding, resulting in a rough film surface, or the film may break when extruded at high speed during film molding due to its high melt viscosity.

[0029] The above-mentioned melt mass flow rate can be obtained by measurement in accordance with the JIS K 7210 standard.

[0030] The density of styrene elastomer is 0.99g / cm 3 The density of the styrene elastomer is preferably less than 0.99 g / cm 3 In the above cases, the stretchability of the film may decrease.

[0031] <Other ingredients> The elastomer layer 5 may contain other components in addition to the above-mentioned styrene-based elastomer, so long as the effects of the present invention are not impaired. Examples of other components include resins other than styrene-based elastomers, such as olefin-based resins, amide-based antiblocking agents (e.g., stearic acid amide), plasticizers, UV absorbers, antioxidants, weather stabilizers, antistatic agents, colorants, antifogging agents, metal soaps, waxes, mildew inhibitors, antibacterial agents, nucleating agents, flame retardants, lubricants, etc. The other components may be added to the material for the stretch film in the form of a master batch.

[0032] (Surface layer) The surface layers 6 and 7 are layers for preventing stickiness of the elastomer layer 5 and suppressing the occurrence of blocking in the stretch film 1. The surface layers are provided on at least one or both of the first and second surfaces of the elastomer layer, but from the viewpoint of sufficiently suppressing the occurrence of blocking in the stretch film 1, it is preferable that the surface layers are provided on both the first and second surfaces of the elastomer layer 5 as shown in Fig. 1. The surface layers 6 and 7 may be the same type of surface layer or different types of surface layers.

[0033] Each of the surface layers 6 and 7 is formed of an olefin-based resin composition containing an olefin-based resin and an inorganic filler. The surface layers 6 and 7 may contain the above-mentioned other components as necessary within a range that does not impair the effects of the present invention.

[0034] <Olefin resin> Examples of the olefin resin include polyethylene resin and polypropylene resin. From the viewpoint of improving the elasticity of the surface layers 6, 7, polyethylene resin is preferable, and from the viewpoint of improving the heat resistance of the surface layers 6, 7, polypropylene resin is preferable.

[0035] For example, examples of polyethylene resins include low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE). Among these, from the viewpoint of suppressing stickiness of the elastomer component, low-density polyethylene (density: 0.910 to 0.930 g / cm 3 ) is preferable, and from the viewpoint of improving the elasticity, linear low-density polyethylene (density: 0.910 to 0.920 g / cm 3 ) is preferred.

[0036] Examples of polypropylene-based resins include homopolypropylene (H-PP) obtained by polymerizing propylene alone, random polypropylene (R-PP) obtained by copolymerizing propylene with ethylene, block polypropylene obtained by polymerizing homopolypropylene and then copolymerizing ethylene and propylene in the presence of homopolypropylene (block polypropylene copolymerized with ethylene, B-PP), and propylene-based elastomers such as propylene-ethylene copolymers. Among these, random polypropylene (ethylene unit content: 5% by mass or less, melting point: 135 to 150°C) is preferred from the viewpoint of improving flexibility and improving heat resistance compared to polyethylene resins, since ethylene copolymerization reduces stereoregularity and reduces crystallinity, and propylene-based elastomers (propylene unit content: 70% by mass to 95% by mass, ethylene unit content: 5 to 30% by mass) are preferred from the viewpoint of improving stretchability.

[0037] The olefin resin may be used alone or in combination of two or more. For example, from the viewpoint of improving the elasticity, a random polypropylene may be blended with a linear low-density polyethylene. From the viewpoint of suppressing the occurrence of blocking in the elastomer component, a propylene elastomer may be blended with a low-density polyethylene.

[0038] Furthermore, the content of the olefin resin in the entire surface layer 6 (or surface layer 7) (i.e., the entire olefin resin composition) is preferably 30% by mass or more and 85% by mass or less, assuming that the entire surface layer is 100% by mass. This is because if it is less than 30% by mass, the content of the inorganic filler in the surface layer increases, which may result in a decrease in elasticity, and if it is more than 85% by mass, the content of the inorganic filler in the surface layer decreases, which may result in blocking.

[0039] <Inorganic fillers> The inorganic filler is a component that imparts slipperiness to the surfaces of the surface layers 6 and 7 and further suppresses the occurrence of blocking in the stretch film 1.

[0040] Examples of the inorganic filler include calcium carbonate, zeolite, silica, titanium oxide, calcium oxide, magnesium oxide, zinc oxide, clay, mica, barium sulfate, magnesium hydroxide, etc. The inorganic filler may be used alone or in combination of two or more kinds.

[0041] The content of the inorganic filler in the entire surface layer 6 (or surface layer 7) (i.e., the entire olefin resin composition) is preferably 15% by mass or more and 70% by mass or less, assuming that the entire surface layer is 100% by mass. This is because if it is less than 15% by mass, the content of the inorganic filler in the surface layer decreases, which may cause blocking, and if it is more than 70% by mass, the content of the inorganic filler in the surface layer increases, which may cause a decrease in stretchability.

[0042] The average particle size of the inorganic filler is preferably 0.8 to 10 μm. If the average particle size of the inorganic filler is 0.8 μm or more, secondary aggregation of the inorganic filler is suppressed, dispersibility in the resin is improved, and slipperiness is improved. If the average particle size is 10 μm or less, the feel on the skin is improved.

[0043] <Method of manufacturing stretch film> Next, the method for producing the stretch film of this embodiment will be described in detail.

[0044] The stretch film of the present embodiment is produced by forming a raw material containing the above-mentioned styrene-based elastomer, olefin-based resin, and inorganic filler into a film using an extruder.

[0045] More specifically, first, a styrene-based elastomer and, if necessary, the above-mentioned other components are mixed in a predetermined mixing ratio to obtain a resin mixture for forming the elastomer layer, and then an olefin-based resin, an inorganic filler and, if necessary, other components are mixed in a predetermined mixing ratio, extruded into a strand shape using a co-rotating twin-screw extruder equipped with a strand die, and cut to obtain pellets for forming the surface layer.

[0046] Next, using an extruder equipped with a T-die, the resin mixture for forming the elastomer layer and the pellets for forming the surface layer are extruded at a predetermined temperature, and a cast-fill process is used to obtain an unstretched raw film having an elastomer layer, a first surface layer (e.g., surface layer 6 in Figure 1) provided on a first surface of the elastomer layer, and a second surface layer (e.g., surface layer 7 in Figure 1) provided on a second surface of the elastomer layer.

[0047] The raw film is then stretched by uniaxial stretching to produce the stretch film 1 shown in Figures 1 and 2. The stretching method is not particularly limited, and examples thereof include gear stretching, roll stretching, and tenter stretching.

[0048] For example, gear stretching can be performed using a pair of shaping rolls, including a first shaping roll having multiple ridges extending circumferentially on the peripheral surface of a cylindrical roll body, and a second shaping roll having multiple ridges extending circumferentially on the peripheral surface of the cylindrical roll body, arranged opposite each other with a predetermined clearance provided so that the ridges of the first shaping roll mesh with the grooves between the ridges of the second shaping roll, and so that the grooves between the ridges of the first shaping roll mesh with the ridges of the second shaping roll.

[0049] Then, while rotating the first shaping roll and the second shaping roll, the raw film before the above-mentioned gear stretching is passed between the first shaping roll and the second shaping roll, thereby forming a stretched region and a non-stretched region between the convex ridges of the first shaping roll and the convex ridges of the second shaping roll.

[0050] In the gear stretching, the stretch ratio can be adjusted by adjusting the width W of the top of the convex stripe of the shaping roll, the height H of the convex stripe, the interval P between the tops of adjacent convex stripes, the meshing depth D between the convex stripe of the first shaping roll and the convex stripe of the second shaping roll, etc. In addition, the stretch ratio in the gear stretching can be easily calculated from the stretching principle by Pythagoras' theorem.

[0051] The above-mentioned uniaxial stretching treatment refers to a stretching treatment carried out in either the MD or TD direction shown in Fig. 2. Note that a biaxial stretching treatment in which stretching is carried out in both the MD and TD directions may also be carried out.

[0052] The stretching temperature in the uniaxial stretching process is usually room temperature (23±2°C). This is because stretching at room temperature can remove residual strain that remains during film molding, and has the effect of reducing permanent strain. If stretching is performed at a temperature higher than room temperature, orientation progresses in the stretching direction, which may increase permanent strain.

[0053] The stretching ratio in the uniaxial stretching process is 1.5 times or more and 9 times or less. This is because if the stretching ratio is less than 1.5 times, residual strain that remains during film molding may not be removed. If the stretching ratio is greater than 9 times, the film may break when stretched. The "stretching ratio" here refers to the multiple of the length of the film after stretching to the length of the film before stretching in the stretching direction. In the case of gear stretching, it refers to the multiple of the length of the film in the stretched region to the length of the film before stretching. For example, if the distance between the top of the convex stripe of the first shaping roll and the top of the convex stripe of the second shaping roll adjacent to each other (the width of the stretched part of the film before gear stretching) is 1 mm and the meshing depth is √3 mm, the width of the stretched part of the film is 2 mm, and the stretching ratio is 2 times.

[0054] The stretch film of this embodiment produced by the above-mentioned method has a hysteresis loss of less than 36%, so that in the stretch film 1 having the surface layers 6, 7 laminated on the surface of the elastomer layer 5, it is possible to prevent a decrease in the stretchability of the surface layers 6, 7, and as a result, it is possible to obtain a stretch film 1 with excellent stretchability. The hysteresis loss is preferably less than 30%, and more preferably less than 25%.

[0055] The "hysteresis loss" referred to here is calculated by the following method.

[0056] A rectangular test piece of 100 mm in one direction of the film and 25 mm in the direction perpendicular to the one direction is cut from the stretch film, and this test piece is fixed to the gripper of a testing machine (e.g., Shimadzu Autograph AG-5000A) so that the distance between the grippers is 25 mm. The integral area of ​​the stress-strain curve (SS curve) when the test piece is stretched in the longitudinal direction at a speed of 254 mm / min so that the strain (elongation) calculated by the following formula (1) is 100% is defined as S1, and the integral area of ​​the stress-strain curve (SS curve) when the test piece is immediately contracted at the same speed after stretching until the load (N / 25 mm) of the test piece becomes 0 is defined as S2, and the hysteresis loss [%] is calculated from the following formula (2).

[0057] Distortion [%] = (L1-L0) / L0 × 100 (1) Hysteresis loss [%] = S / S1 × 100 (2)

[0058] where L0 is the distance between the grippers (mm) before stretching, L1 is the distance between the grippers (mm) after stretching, S1 is the integral area in the stress-strain curve when stretching from 0% to 100% strain, S2 is the integral area in the stress-strain curve when shrinking from 100% strain to 0 stress, and S is the integral area in the stress-strain curve obtained by subtracting the integral area S2 from the integral area S1 (i.e., S=S1-S2).

[0059] That is, the integral area in the stress-strain curve obtained by subtracting the integral area S2 in the stress-strain curve shown in FIG. 4 when the strain is contracted from 100% to 0 stress from the integral area S1 in the stress-strain curve shown in FIG. 3 when the strain is extended from 0% to 100% is obtained by dividing the integral area S in the stress-strain curve (i.e., the integral area S shown in FIG. 5) by the integral area S1, and the hysteresis loss can be calculated according to the above formula (2).

[0060] Furthermore, when the stretch film of the present embodiment has a permanent set in the stretching direction of 7% or less, the plastic change is small, and therefore it is possible to obtain excellent stretchability. The permanent set is preferably 6.5% or less.

[0061] The term "permanent set" used herein refers to a value calculated by the following method.

[0062] A rectangular test piece of 100 mm in one direction of the film and 25 mm in the direction perpendicular to the one direction is cut from the stretch film, and the test piece is fixed to the grip of a testing machine (e.g., Shimadzu Autograph AG-5000A) so that the distance between the grips is 25 mm. The test piece is then stretched in the longitudinal direction at a speed of 254 mm / min so that the strain (elongation) calculated by the following formula (1) is 100%, and then the test piece is immediately contracted at the same speed. The permanent set [%] is then calculated from the following formula (3).

[0063] Distortion [%] = (L1-L0) / L0 × 100 (1) Permanent set [%] = (L2-L0) / L0 × 100 (3)

[0064] where L0 is the distance between the grips (mm) before stretching, L1 is the distance between the grips (mm) after stretching, and L2 is the distance between the grips (mm) when the load on the test piece (N / 25 mm) becomes 0 when contracting.

[0065] From the viewpoint of transportability of the stretch film, the stress when stretching the film in the MD so that the strain (elongation) calculated by the above formula (1) is 10% (stress at 10% elongation) is 1.2 N / mm 2 It is preferable that the resistance is 2N / mm or more. 2 More preferably, it is 3N / mm 2 More preferably, it is equal to or greater than this.

[0066] In addition, the stress when elongating the material so that the strain (elongation) calculated by the above formula (1) is 50% in the TD (stress at 50% elongation) is 0.5 to 1.5 N / mm 2It is preferable that the resistance is 0.8 to 1.2 N / mm 2 It is more preferable that the stress at 50% elongation is 0.5 N / mm 2 If the stress is too small, the film must be thickened to obtain adequate elasticity, which may increase costs. 2 In the case of a thickness of 1000 mm or more, the stress is too large, so the film must be thin, and if the film is too thin, handling may become difficult.

[0067] The thickness of the raw film is preferably 20 to 80 μm, more preferably 20 to 60 μm, and even more preferably 30 to 50 μm. If the thickness of the raw film is 20 μm or more, the stretchability is excellent. If the thickness of the raw film is 80 μm or less, the stretch film can be made thin, so that the rigidity is low and the stretchability is excellent.

[0068] The thickness of the elastomer layer 5 in the raw film is preferably 20 to 40 μm, more preferably 25 to 35 μm, and even more preferably 30 to 33 μm. If the thickness of the elastomer layer 5 is 20 μm or more, the stretchability of the stretch film 1 can be sufficiently obtained, and the film can be stably wound up on a roll during film molding. If the thickness of the elastomer layer 5 is 40 μm or less, the stretch film 1 can be made thinner, and the stress of the stretch film can be reduced.

[0069] Furthermore, the thickness of the surface layers 6, 7 in the original film is preferably 1 to 10 μm, more preferably 1 to 5 μm, even more preferably 1 to 3 μm, and most preferably 1.2 to 2.2 μm. If the surface layers 6, 7 have a thickness of 1 μm or more, the occurrence of blocking in the stretch film 1 after stretching can be sufficiently suppressed. If the surface layers 6, 7 have a thickness of 10 μm or less, the stretchability of the stretch film 1 can be sufficiently obtained. Note that the surface layers 6, 7 may have the same thickness or different thicknesses.

[0070] Furthermore, from the viewpoint of improving the elasticity even in an elastic film 1 in which the thickness ratio of the surface layers 6, 7 to the entire elastic film is small, the thickness ratio of the surface layer 7 (or surface layer 8) to the elastomer layer 5 in the original film (surface layer:elastomer layer) is preferably 1:5 to 1:35, more preferably 1:8 to 1:30, and even more preferably 1:15 to 1:27.

[0071] Furthermore, the thickness of the stretchable film 1 after stretching is 85 to 95% of the original film when stretched at room temperature. In the case of gear stretching, the unstretched portion has the same thickness as the original film, and the stretched portion has 85 to 95% of the original film.

[0072] By the above method, in this embodiment, excellent stretchability can be obtained in the stretch film 1 having the surface layers 6, 7 laminated on the surface of the elastomer layer 5.

[0073] In addition, when the stretch film is multi-layered, the composition and thickness of each layer may be the same or different. In addition, when the stretch film is multi-layered, the thickness means the total thickness of the multi-layered film.

[0074] [Second embodiment] Next, a second embodiment of the present invention will be described. Note that the same components as those in the first embodiment are given the same reference numerals and the description thereof will be omitted.

[0075] 6 is a cross-sectional view showing a stretch film according to this embodiment. As shown in Fig. 6, the stretch film 20 of this embodiment includes an elastomer layer 11 and surface layers 6 and 7 laminated on the surface of the elastomer layer 11.

[0076] (Elastomer layer) The elastomer layer 11 is a layer that imparts elasticity to the elastic film 1, and as shown in Figure 6, this elastomer layer 11 has a three-layer structure including a core layer 8 and intermediate layers 9 and 10 laminated on the surface of the core layer 8, with the intermediate layer 9 being provided between the core layer 8 and the surface layer 6, and the intermediate layer 10 being provided between the core layer 8 and the surface layer 7.

[0077] <Core layer> The core layer 8 contains an olefin-based elastomer, which is a thermoplastic elastomer. By using the olefin-based elastomer, it is possible to improve the stress at 50% elongation in TD compared to the case where only the elastomer layer 5 containing a styrene-based elastomer is provided as in the first embodiment described above.

[0078] The olefin-based elastomer used in the present invention includes copolymers containing an olefin having 3 or more carbon atoms as a main component.

[0079] More specifically, for example, α-olefin copolymers such as propylene-ethylene copolymer, propylene-ethylene-1-butene copolymer, 1-butene-ethylene copolymer, 1-butene-propylene copolymer, 4-methylpentene-1-propylene copolymer, 4-methylpentene-1-1-butene copolymer, 4-methylpentene-1-propylene-1-butene copolymer, and propylene-1-butene copolymer may be mentioned. Also, an elastomer in which the above-mentioned elastomer is dispersed in a matrix of crystalline polyolefin may be used. Among these, propylene-based elastomers such as propylene-ethylene copolymers (olefin-based elastomers in which hard segments are made of polypropylene) are preferred because of their higher elasticity. The olefin-based elastomers may be used alone or in combination of two or more kinds.

[0080] Furthermore, examples of the soft segment of the olefin-based elastomer include EPDM, EPM, EBM, IIR, hydrogenated styrene butadiene rubber (HSBR), NBR, and acrylic rubber (ACM).

[0081] In addition, when a propylene-based elastomer is used, the propylene unit content relative to the total units of the propylene-based elastomer is preferably 70% by mass to 95% by mass, more preferably 80% by mass to 90% by mass. For example, in the case of a propylene-ethylene copolymer, the propylene unit content relative to the total units is preferably 70% by mass to 95% by mass (i.e., the ethylene unit content is 5 to 30% by mass). If the propylene unit content, which is the hard segment, is 70% by mass or more, the strength is improved, and therefore excellent moldability is obtained, and if it is 95% by mass or less, excellent stretchability is obtained due to the elasticity of the soft segment.

[0082] The MFR of the propylene-based elastomer is preferably 0.5 to 10 g / 10 min, more preferably 2.0 to 8.0 g / 10 min. If the MFR of the propylene-based elastomer is greater than 10 g / 10 min, the melt viscosity may be too low, making it difficult to control the thickness during film molding. If the MFR of the propylene-based elastomer is less than 0.5 g / 10 min, melt fracture may occur during film molding, resulting in a rough film surface. If the MFR of the propylene-based elastomer is less than 2.0 g / 10 min, the melt viscosity may be high, causing the film to break when extruded at high speed during film molding.

[0083] The density of propylene elastomer is 0.900g / cm 3 The density of the propylene elastomer is preferably less than 0.900 g / cm 3 In the above cases, the stretchability of the film may decrease.

[0084] Furthermore, the core layer 8 may contain other components besides the above-mentioned propylene-based elastomer, so long as the effects of the present invention are not impaired. Examples of other components include resins other than the propylene-based elastomer, such as olefin-based resins, amide-based antiblocking agents (e.g., stearic acid amide), plasticizers, UV absorbers, antioxidants, weather stabilizers, antistatic agents, colorants, antifogging agents, metal soaps, waxes, mildew inhibitors, antibacterial agents, nucleating agents, flame retardants, lubricants, etc. The other components may be added to the material for the stretch film in the form of a master batch.

[0085] <Middle Class> As the intermediate layers 9 and 10, the same elastomer layer 5 described in the first embodiment (that is, the elastomer layer containing the above-mentioned styrene-based elastomer) can be used.

[0086] As described above, when the SIS elastomer is blended with another SIS elastomer (for example, when SIS elastomers with different styrene unit contents are blended), the styrene unit content relative to the total units of the SIS elastomer is preferably 9% by mass or more and 35% by mass or less. However, when a SIS elastomer with a high styrene unit content (i.e., a styrene unit content of more than 30% by mass) is blended with a SIS elastomer with a low styrene unit content (i.e., a styrene unit content of 30% by mass or less), the blend ratio of the SIS elastomer with a high styrene unit content to the SIS elastomer with a low styrene unit content is preferably 20:80 to 50:50 (SIS elastomer with a high styrene unit content: SIS elastomer with a low styrene unit content) from the viewpoint of suppressing a decrease in stretchability in TD while improving the stress in MD. Within this blending ratio range, the stress at 10% elongation in MD [N / mm 2 In order to improve the elasticity in the TD that is sacrificed due to the Shore A hardness, the Shore A hardness can be made 30 or more, and in order to improve the elasticity in the TD that is sacrificed due to the Shore A hardness, the styrene unit content in the entire elastomer layer can be made 35 mass% or less.

[0087] <Method of manufacturing stretch film> Next, the method for producing the stretch film of this embodiment will be described in detail.

[0088] The stretch film of the present invention is produced by forming a raw material containing the above-mentioned olefin-based elastomer, styrene-based elastomer, olefin-based resin, and inorganic filler into a film using an extruder.

[0089] More specifically, first, an olefin-based elastomer and, if necessary, the other components described above are mixed in a predetermined mixing ratio to obtain a resin mixture for forming the core layer. Similarly, a styrene-based elastomer and, if necessary, the other components described above are mixed in a predetermined mixing ratio to obtain a resin mixture for forming the intermediate layer. Also, an olefin-based resin, an inorganic filler and, if necessary, the other components are mixed in a predetermined mixing ratio, extruded into a strand shape using a co-rotating twin-screw extruder equipped with a strand die, and cut to obtain pellets for forming the surface layer.

[0090] Next, using an extruder equipped with a T-die, the resin mixture for forming the core layer, the resin mixture for forming the intermediate layer, and the pellets for forming the surface layer are extruded at a predetermined temperature, and a cast-fill process is used to obtain an unstretched raw film having a core layer, an elastomer layer (e.g., elastomer layer 11 in FIG. 6) having a first intermediate layer (e.g., intermediate layer 9 in FIG. 6) provided on a first surface of the core layer and a second intermediate layer (e.g., intermediate layer 10 in FIG. 6) provided on a second surface of the core layer, a first surface layer (e.g., surface layer 6 in FIG. 6) provided on the first surface of the elastomer layer, and a second surface layer (e.g., surface layer 7 in FIG. 6) provided on the second surface of the elastomer layer.

[0091] The raw film is then stretched by uniaxial stretching in either the MD or TD direction shown in Fig. 7, to produce the stretchable film 20 shown in Figs. 6 to 7. As in the first embodiment, the stretching method is not particularly limited, and examples include gear stretching, roll stretching, and tenter stretching. Biaxial stretching may also be performed in which stretching is performed in both the MD and TD directions.

[0092] Similarly to the first embodiment described above, the stretching temperature in the uniaxial stretching process is usually room temperature (23±2° C.), and the stretch ratio in the uniaxial stretching process is 1.5 times or more and 9 times or less.

[0093] The stretch film of this embodiment produced by the above method has a hysteresis loss of less than 36%, similar to the first embodiment described above, so that in the stretch film 20 having the surface layers 6, 7 laminated on the surface of the elastomer layer 11, it is possible to prevent a decrease in the stretchability of the surface layers 6, 7, and as a result, it is possible to obtain a stretch film 20 with excellent stretchability. The hysteresis loss is preferably less than 30%, and more preferably less than 25%.

[0094] Furthermore, the stretch film of this embodiment, like the first embodiment described above, has a permanent set in the stretching direction of 7% or less, making it possible to obtain excellent stretchability, with the permanent set preferably being 6.5% or less.

[0095] In addition, similarly to the first embodiment described above, from the viewpoint of transportability of the stretch film, the stress when stretching in the MD so that the strain (elongation) calculated by the above formula (1) is 10% (stress at 10% elongation) is 1.2 N / mm 2 It is preferable that the resistance is 2N / mm or more. 2 More preferably, it is 3N / mm 2 More preferably, it is equal to or greater than this.

[0096] In addition, similarly to the first embodiment described above, from the viewpoint of suppressing an increase in costs, the stress (stress at 50% elongation) when elongating the material in the TD so that the strain (elongation) calculated by the above formula (1) becomes 50% is set to 0.5 to 1.5 N / mm 2 It is preferable that the resistance is 0.8 to 1.2 N / mm 2 It is more preferable that:

[0097] Similarly to the first embodiment, the thickness of the raw film is preferably 20 to 80 μm, more preferably 20 to 60 μm, and even more preferably 30 to 50 μm. The thickness of the elastomer layer 11 in the raw film is preferably 20 to 40 μm, more preferably 25 to 35 μm, and even more preferably 30 to 33 μm.

[0098] The thickness of the core layer 8 in the raw film is preferably 5 to 20 μm, more preferably 7 to 18 μm, and even more preferably 9 to 17 μm. The total thickness of the intermediate layers 9 and 10 in the raw film is preferably 10 to 25 μm, more preferably 12 to 22 μm, and even more preferably 14 to 20 μm.

[0099] In particular, in stretch film 20 having a three-layer structure in which elastomer layer 11 is composed of core layer 8 and intermediate layers 9 and 10, from the viewpoint of improving the stress at 50% elongation in TD while suppressing a decrease in stretchability in TD, it is preferable that the thickness ratio of core layer 8 in the original film to the total thickness of intermediate layer 9 and intermediate layer 10 (core layer:total intermediate layer) is 20:80 to 50:50. In other words, there is a trade-off between improving the stress at 50% elongation in TD and improving stretchability in TD, and as long as the thickness ratio of core layer thickness to total intermediate layer thickness is within the above range, it is possible to achieve both an improvement in stress at 50% elongation in TD and an improvement in stretchability in TD.

[0100] Similarly to the above-mentioned first embodiment, the thickness of the surface layers 6, 7 in the raw film is preferably 1 to 10 μm, more preferably 1 to 5 μm, further preferably 1 to 3 μm, and most preferably 1.2 to 2.2 μm.

[0101] Similarly to the first embodiment described above, the thickness ratio of the surface layer 7 (or surface layer 8) to the elastomer layer 11 in the original film (surface layer:elastomer layer) is preferably 1:5 to 1:35, more preferably 1:8 to 1:30, and even more preferably 1:15 to 1:27.

[0102] Similarly to the first embodiment described above, the thickness of the stretchable film 20 after stretching is 85-95% of the original film when stretched at room temperature. In the case of gear stretching, the unstretched portion has the same thickness as the original film, and the stretched portion has 85-95% of the original film.

[0103] By the above method, in this embodiment, excellent stretchability can be obtained in the stretch film 20 in which the surface layers 6, 7 are laminated on the surface of the elastomer layer 11.

[0104] In addition, when the stretch film is multi-layered, the composition and thickness of each layer may be the same or different. In addition, when the stretch film is multi-layered, the thickness means the total thickness of the multi-layered film. EXAMPLES

[0105] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention.

[0106] The materials used to prepare the stretch film are listed below. (1) PP1: Random polypropylene (Prime Polymer Co., Ltd., product name: F227, density: 0.90 g / cm 3 , MFR: 6.7g / 10min (230℃) (2) PP2: Random polypropylene, (Prime Polymer Co., Ltd., product name: F327, density: 0.90 g / cm 3, MFR: 7.0g / 10min (230℃) (3) PP3: Random polypropylene (Prime Polymer Co., Ltd., product name: F-744NP, density: 0.90 g / cm 3 , MFR: 7.0g / 10min (230℃) (4) PP4: Random polypropylene (Prime Polymer Co., Ltd., product name: 730NV, density: 0.90 g / cm 3 , MFR:6.2g / 10min(230℃)) (5) PP5: Random polypropylene (manufactured by Sumitomo Chemical Co., Ltd., product name: FLX86E1, density: 0.89 g / cm 3 , MFR: 7.9g / 10min (230℃) (6) PP6: Random polypropylene (manufactured by SunAllomer Corporation, product name: PF621s, density: 0.90 g / cm 3 , MFR: 6.5g / 10min (230℃) (7) PP7: Random polypropylene (manufactured by SunAllomer Corporation, product name: PC630s, density: 0.90 g / cm 3 , MFR: 7.5g / 10min (230℃) (8) PP8: Random polypropylene (manufactured by SunAllomer, product name: PC630a, density: 0.90 g / cm 3 , MFR: 7.5g / 10min (230℃) (9) Inorganic filler: calcium carbonate, average particle size: 1.8 μm (manufactured by Shiraishi Calcium Co., Ltd., product name: PO-120B-10) (10) SIS elastomer 1 (manufactured by Zeon Corporation, product name: Quintac 3390, styrene unit content: 48 mass%, density: 0.98 g / cm 3 , Shore A hardness: 65, MFR: 14g / 10min (200℃) (11) SIS elastomer 2 (manufactured by Zeon Corporation, product name: Quintac 3290, styrene unit content: 35 mass%, density: 0.93 g / cm 3 , Shore A hardness: 55, MFR: 10g / 10min (200℃) (12) SIS elastomer 3 (manufactured by Zeon Corporation, product name: Quintac 3440, styrene unit content: 18 mass%, density: 0.93 g / cm 3, Shore A hardness: 45, MFR: 10g / 10min (200℃) (13) SIS elastomer 4 (manufactured by Zeon Corporation, product name: Quintac 3620, styrene unit content: 14 mass%, density: 0.93 g / cm 3 , Shore A hardness: 36, MFR: 9g / 10min (200℃)) (14) SIS elastomer 5 (manufactured by Zeon Corporation, product name: Quintac 3433N, styrene unit content: 16 mass%, density: 0.93 g / cm 3 , Shore A hardness: 21, MFR: 12g / 10min (200℃)) (15) SIS elastomer 6 (manufactured by Kaneka Corporation, product name: Sibstar 073T, styrene unit content: 30% by mass, density: 0.954 g / cm 3 , Shore A hardness: 45, MFR: 6g / 10min (230℃) (16) SIS elastomer 7 (manufactured by Kraton Corporation, product name: Kraton D1161, styrene unit content: 15% by mass, density: 0.92 g / cm 3 , Shore A hardness: 32, MFR: 12g / 10min (200℃) (17) SIS elastomer 8 (manufactured by Kraton Corporation, product name: Kraton D1126, styrene unit content: 21 mass%, density: 0.92 g / cm 3 , Shore A hardness: 39, MFR: 22g / 10min (200℃)) (18) Propylene-based elastomer (manufactured by ExxonMobil Corporation, product name: Vistamax (registered trademark) 6102FL, polyethylene content: 16%, density: 0.862 g / cm 3 , Shore A hardness: 67, MFR: 3.0g / 10min (230℃) (19) Ethylene-based elastomer (Dow Chemical, product name: Infuse 9007, ethylene-octene copolymer, density: 0.864 / cm 3 , Shore A hardness: 64, MFR: 0.5g / 10min (190℃) (20) SBS elastomer (manufactured by Asahi Kasei Chemikels Corporation, product name: Tufprene A, styrene unit content: 40 mass%, density: 0.95 g / cm 3, Shore A hardness: 85, MFR: 2.6g / 10min (190℃) (21) SEBS elastomer (manufactured by Asahi Kasei Chemikels Corporation, product name: Tuftec H1221, styrene unit content: 12% by mass, density: 0.89 g / cm 3 , Shore A hardness: 42, MFR: 4.5g / 10min (230℃)

[0107] Example 1 <Preparation of stretchable film> First, the materials shown in Table 1 were mixed to prepare a resin mixture for forming the elastomer layer and a resin mixture for forming the surface layer of Example 1 having the composition (parts by mass) shown in Table 1. Next, the resin mixture for forming the surface layer was extruded in a strand shape using a co-rotating twin-screw extruder (manufactured by JSW Corp., product name: TEX28V-42CW-4V) equipped with a strand die under a condition of 200°C, and cut to obtain pellets for forming the surface layer.

[0108] Next, using an extruder equipped with a T-die (manufactured by Labotec), the resin mixture for forming the elastomer layer and the pellets for forming the surface layer were extruded at 200°C, and a film having an elastomer layer, a first surface layer provided on a first surface of the elastomer layer, and a second surface layer provided on a second surface of the elastomer layer was formed by a cast film process method. The film was then taken up on a take-up roll to obtain an unstretched raw film having the thickness shown in Table 1.

[0109] Then, this raw film was subjected to gear stretching treatment (stretching ratio: 5 times) in the TD at room temperature (23° C.±2° C.) to produce a stretch film.

[0110] <Calculation of styrene unit content (relative to total units of SIS elastomer) in elastomer layer> The styrene unit content [%] of the elastomer layer in the produced stretch film was calculated. More specifically, in Example 1, 100 parts by mass of SIS elastomer 3 (styrene unit content: 18% by mass) was contained per 100 parts by mass of the elastomer layer, so the styrene unit content in the elastomer layer was 18 x (100 / 100) = 18% by mass. The results are shown in Table 1.

[0111] <Measurement of Shore A hardness of elastomer layer> The Shore A hardness of the elastomer layer was measured at a temperature of 23° C. using a type A durometer (spring type rubber hardness tester) in accordance with JIS K 6253. The results are shown in Table 1.

[0112] <Calculation of the styrene elastomer content in the entire stretch film> The content [%] of the styrene-based elastomer in the entire stretch film produced was calculated. More specifically, in Example 1, 100 parts by mass of SIS elastomer 3 (styrene-based elastomer) was contained for 100 parts by mass of the elastomer layer, and the thickness of the elastomer layer was 28 μm for the entire thickness of the stretch film (35 μm), so the content of the styrene-based elastomer in the entire stretch film was (28 / 35) × 100 = 80% by mass. The results are shown in Table 1.

[0113] <Hysteresis loss measurement> From the stretch film thus produced, a rectangular test piece of 100 mm in one direction (TD) of the film and 25 mm in the direction perpendicular to the one direction (MD) was cut, and this test piece was fixed to the gripper of a precision universal testing machine (Shimadzu Corporation, Autograph AG-5000A) so that the distance between the grippers was 25 mm. The integral area in the stress-strain curve (SS curve) when the test piece was stretched in the longitudinal direction at a speed of 254 mm / min so that the strain (elongation) calculated by the above formula (1) was 100% was defined as S1, and the integral area in the stress-strain curve (SS curve) when the test piece was immediately contracted at the same speed after stretching until the load (N / 25 mm) of the test piece became 0 was defined as S2, and the hysteresis loss [%] was calculated from the above formula (2). The results are shown in Table 1.

[0114] <Measurement of permanent deformation> From the stretch film thus produced, a rectangular test piece of 100 mm in one direction (TD) of the film and 25 mm in the direction perpendicular to the one direction (MD) was cut, and this test piece was fixed to the gripper of a precision universal testing machine (Shimadzu Corporation, Autograph AG-5000A) so that the distance between the grippers was 25 mm. Then, the test piece was stretched in the longitudinal direction of the test piece at a speed of 254 mm / min so that the strain (elongation) calculated by the above formula (1) was 100%, and then the test piece was immediately contracted at the same speed. Then, the permanent strain [%] in TD was calculated from the above formula (3). The test was performed at room temperature (23°C ± 2°C). The above results are shown in Table 1.

[0115] <Measurement of stress at 10% elongation> From the stretch film thus produced, a rectangular test piece of 100 mm in one direction (MD) of the film and 25 mm in the direction perpendicular to the one direction (TD) was cut, and this test piece was fixed to the gripping tools of a precision universal testing machine (Shimadzu Corporation, Autograph AG-5000A) so that the distance between the gripping tools was 25 mm. The test piece was then stretched in the longitudinal direction at a speed of 254 mm / min so that the strain (elongation) calculated by the above formula (1) was 10%, and the stress at 10% elongation in MD [N / mm 2 The results are shown in Table 1.

[0116] <Measurement of stress at 50% elongation> From the stretch film thus produced, a rectangular test piece measuring 100 mm in the direction perpendicular to one direction of the film (TD) and 25 mm in one direction (MD) was cut, and this test piece was fixed to the gripping tools of a precision universal testing machine (Shimadzu Corporation, Autograph AG-5000A) so that the distance between the gripping tools was 25 mm. Then, the test piece was stretched in the direction perpendicular to the longitudinal direction of the test piece at a speed of 254 mm / min so that the strain (elongation) calculated by the above formula (1) was 50%, and the stress at 50% elongation in TD [N / mm 2 The results are shown in Table 1.

[0117] (Examples 2 to 9) Except for changing the composition of the surface layer (parts by mass), the composition of the elastomer layer (parts by mass), and the thickness ratio between the surface layer and the elastomer layer to the conditions shown in Table 1, a raw film having the thickness shown in Table 1 was stretched to produce a stretch film in the same manner as in Example 1 described above.

[0118] The styrene unit content in the elastomer layer was calculated, the Shore A hardness of the elastomer layer was measured, the styrene elastomer content in the entire stretch film was calculated, and the hysteresis loss, permanent set, stress at 10% elongation, and stress at 50% elongation were measured in the same manner as in Example 1. The results are shown in Table 1.

[0119] Example 10 <Preparation of stretchable film> First, the materials shown in Table 2 were mixed to prepare a resin mixture for forming an elastomer layer (core layer), a resin mixture for forming an elastomer layer (middle layer), and a resin mixture for forming a surface layer in Example 10 having the composition (parts by mass) shown in Table 2. Next, the resin mixture for forming the surface layer was extruded in a strand shape using a co-rotating twin-screw extruder (manufactured by JSW Corp., product name: TEX28V-42CW-4V) equipped with a strand die under a condition of 200°C, and cut to obtain pellets for forming the surface layer.

[0120] Next, using an extruder (manufactured by Labotec) equipped with a T-die, the resin mixture for forming the elastomer layer (core layer), the resin mixture for forming the elastomer layer (intermediate layer), and pellets for forming the surface layer were extruded at 200°C, and a cast film process was used to form an elastomer layer having a core layer, a first intermediate layer provided on a first surface of the core layer, and a second intermediate layer provided on a second surface of the core layer, a first surface layer provided on the first surface of the elastomer layer, and a second surface layer provided on the second surface of the elastomer layer.The film was then taken up on a take-up roll to obtain a raw film before stretching having the thickness shown in Table 2.

[0121] Then, this raw film was subjected to gear stretching treatment (stretching ratio: 5 times) in the TD at room temperature (23° C.±2° C.) to produce a stretch film.

[0122] The styrene unit content in the elastomer layer was calculated, the Shore A hardness of the elastomer layer was measured, the styrene elastomer content in the entire stretch film was calculated, and the hysteresis loss, permanent set, stress at 10% elongation, and stress at 50% elongation were measured in the same manner as in Example 1. The results are shown in Table 2.

[0123] <Calculation of the content of olefin-based elastomer in the entire stretch film> The content [%] of the olefin-based elastomer in the entire stretch film produced was also calculated. More specifically, in Example 10, 100 parts by mass of the propylene-based elastomer (olefin-based elastomer) was contained for every 100 parts by mass of the core layer, and the thickness of the core layer was 15.54 μm for the entire thickness of the stretch film (35 μm), so the content of the olefin-based elastomer in the entire stretch film was (15.54 / 35)×100=44.4% by mass. The results are shown in Table 2.

[0124] (Examples 11 to 25) Except for changing the composition of the surface layer (parts by mass), the composition of the elastomer layer (core layer) (parts by mass), the composition of the elastomer layer (middle layer) (parts by mass), and the thickness ratio between the surface layer and the elastomer layer to the conditions shown in Tables 2 and 3, a raw film having the thickness shown in Tables 2 and 3 was stretched in the same manner as in Example 10 described above to produce an elastic film.

[0125] The styrene unit content in the elastomer layer was calculated, the Shore A hardness of the elastomer layer was measured, the styrene elastomer content in the entire stretch film was calculated, the hysteresis loss was measured, the permanent set was measured, the stress at 10% elongation was measured, and the stress at 50% elongation was measured in the same manner as in Example 1. The olefin elastomer content in the entire stretch film was calculated in the same manner as in Example 10. The results are shown in Tables 2 and 3.

[0126] (Comparative Examples 1 to 13) Except for changing the composition of the surface layer (parts by mass), the composition of the elastomer layer (parts by mass), and the thickness ratio between the surface layer and the elastomer layer to the conditions shown in Table 4, a raw film having the thickness shown in Table 4 was stretched to produce a stretch film in the same manner as in Example 1 described above.

[0127] The styrene unit content in the elastomer layer was calculated, the Shore A hardness of the elastomer layer was measured, the styrene elastomer content in the entire stretch film was calculated, the hysteresis loss was measured, the permanent set was measured, the stress at 10% elongation was measured, and the stress at 50% elongation was measured in the same manner as in Example 1. In Comparative Examples 1 to 3, the olefin elastomer content in the entire stretch film was calculated in the same manner as in Example 10. The results are shown in Table 4.

[0128] (Comparative Examples 14 to 25) Except for changing the composition of the surface layer (parts by weight), the composition of the elastomer layer (core layer) (parts by weight), the composition of the elastomer layer (middle layer) (parts by weight), and the thickness ratio between the surface layer and the elastomer layer to the conditions shown in Table 5, a raw film having the thickness shown in Table 5 was stretched in the same manner as in Example 10 described above to produce a stretch film.

[0129] The styrene unit content in the elastomer layer was calculated, the Shore A hardness of the elastomer layer was measured, the styrene elastomer content in the entire stretch film was calculated, the hysteresis loss was measured, the permanent set was measured, the stress at 10% elongation was measured, and the stress at 50% elongation was measured in the same manner as in Example 1. In Comparative Examples 20 to 25, the olefin elastomer content in the entire stretch film was calculated in the same manner as in Example 10. The results are shown in Table 5.

[0130] [Table 1]

[0131] [Table 2]

[0132] [Table 3]

[0133] [Table 4]

[0134] [Table 5]

[0135] As shown in Tables 1 to 3, in the stretch films of Examples 1 to 25, the elastomer layer contains a styrene-based elastomer and has a hysteresis loss of less than 36%, and therefore is found to have excellent stretchability.

[0136] On the other hand, as shown in Table 4, the stretch films of Comparative Examples 1 to 3 have a single elastomer layer and contain an olefin-based elastomer (propylene-based elastomer, ethylene-based elastomer) but no SIS elastomer, and therefore have poor stretchability (hysteresis loss of 36% or more). Also, the stretch films of Comparative Examples 1 and 2 have a Shore A hardness of 60 or more, and therefore have poor stretchability (hysteresis loss of 36% or more).

[0137] In addition, in the stretch films of Comparative Examples 4, 7, and 12 to 13, the styrene unit content relative to the entire elastomer layer is greater than 35 mass% and the Shore A hardness is 60 or more, so that the stretchability is poor (the hysteresis loss is 36% or more).

[0138] In addition, in the stretch film of Comparative Example 5, the SIS elastomer and the SEBS elastomer have poor compatibility, and the added SEBS component aggregates, causing a large number of aggregates (foreign matter) to form in the film, resulting in poor stretchability (hysteresis loss of 36% or more).

[0139] In addition, in the stretch film of Comparative Example 6, the elastomer layer contains an SBS elastomer with a very high Shore A hardness, and since the Shore A hardness of the elastomer layer is 60 or more, it is found that the stretchability is poor (the hysteresis loss is 36% or more).

[0140] In the stretch films of Comparative Examples 8 to 10 and 16 to 17, the plastic deformation progresses significantly in the elastomer layers of SIS elastomer 7 and SIS elastomer 8, and the TD permanent set increases, resulting in poor stretchability (hysteresis loss of 36% or more). One of the reasons for this is thought to be the high ratio of diblock components contained in the styrene-based elastomer, which reduces the restoring force after stretching.

[0141] Also, in the stretch films of Comparative Examples 11, 14-15, and 18-19, the styrene unit content in the entire elastomer layer was greater than 35 mass %, and therefore the stretchability was poor (the hysteresis loss was 36% or more).

[0142] In addition, in the stretch films of Comparative Examples 20 to 21, the styrene unit content of SIS elastomer 1 and SIS elastomer 2 contained alone in the core layer of the elastomer layer is greater than 30 mass%, so that the stretchability is poor (hysteresis loss is 36% or more).

[0143] In the stretch films of Comparative Examples 22 to 25, the intermediate layer of the elastomer layer contains SIS elastomer 1 with a styrene unit content of 30% by mass or more and SIS elastomer 2 at 50% or more, and in this case, when the ratio of the total thickness of the intermediate layer to the sum of the thickness of the core layer of the elastomer layer and the total thickness of the intermediate layer (i.e., the total thickness of the elastomer layer, 28 μm) is 50% or less as in Comparative Examples 22 to 25, the stress at 50% elongation in TD is improved, but the decrease in stretchability cannot be suppressed, so the stretchability is poor (hysteresis loss is 36% or more). In addition, the stretch films of Comparative Examples 22 and 25 have Shore A hardness of 60 or more, so the stretchability is poor (hysteresis loss is 36% or more). [Industrial Applicability]

[0144] As described above, the present invention is suitable for stretch films used in, for example, garments such as underwear, waistbands of disposable diapers, side panels, leg gathers, incontinence products, sanitary napkins, bandages, surgical drapes, tightening bands, hats, swimming trunks, sports supports, medical supporters, bandages, etc. [Explanation of symbols]

[0145] 1 Stretch film 5 Elastomer Layer 6,7 Surface layer 8 core layer 9,10 Middle class 11 Elastomer layer 20 Stretch Film

Claims

1. An elastomer layer; a surface layer laminated on at least one surface of the elastomer layer; A stretch film comprising: The elastomer layer contains a styrene-based elastomer, the surface layer is made of an olefin-based resin composition containing an olefin-based resin and an inorganic filler, A stretch film characterized by having a hysteresis loss of less than 36%. (Hysteresis loss) A rectangular test piece measuring 100 mm in one direction of the film and 25 mm in the direction perpendicular to the one direction was cut from the stretch film, and this test piece was fixed to the grips of a testing machine so that the distance between the grips was 25 mm. The test piece was stretched in the longitudinal direction of the test piece at a speed of 254 mm / min so that the strain (elongation) calculated by the following formula (1) was 100%. The integral area in the stress-strain curve (S-S curve) when this was done is defined as S1, and immediately after stretching, the test piece was contracted at the same speed until the load (N / 25 mm) of the test piece became 0. The integral area in the stress-strain curve (S-S curve) when this was done is defined as S2, and the hysteresis loss [%] was calculated using the following formula (2). Distortion [%] = (L1 - L0) / L0 x 100 (1) Hysteresis loss [%] = S / S1 × 100 (2) where L0 is the distance between the grippers (mm) before stretching, L1 is the distance between the grippers (mm) after stretching, S1 is the integrated area in the stress-strain curve when stretching from 0% to 100% strain, S2 is the integrated area in the stress-strain curve when shrinking from 100% strain to 0 stress, and S is the integrated area (S1-S2) in the stress-strain curve obtained by subtracting the integrated area S2 from the integrated area S1.

2. 2. The stretch film according to claim 1, wherein the styrene-based elastomer is a styrene-isoprene-styrene copolymer (SIS elastomer).

3. The elastomer layer includes a core layer and an intermediate layer laminated on at least one surface of the core layer, The stretch film according to claim 2 , wherein the intermediate layer is provided between the core layer and the surface layer.

4. The core layer is made of an olefin-based elastomer, The stretch film according to claim 3, wherein the intermediate layer is made of styrene-isoprene-styrene copolymer (SIS elastomer).

5. 5. The stretch film according to claim 4, wherein the olefin-based elastomer is a propylene-based elastomer.

6. The stretch film according to any one of claims 1 to 5, characterized in that the olefin-based resin is random polypropylene, and the inorganic filler is calcium carbonate.

Citation Information

Patent Citations

  • Elastic laminate and article including the same, and elastic laminate elongation and article including the same

    JP2016112878A

  • Elastic laminate and manufacturing method thereof

    JP2020183119A

  • Stretchable film

    JP2021123677A

  • Stretchable film

    WO2016013577A1

  • Stretching material, stretchable member, and garment product

    WO2017034030A1