Conductive pattern transfer sheet
The conductive pattern transfer sheet addresses transfer defects by maintaining a specific surface tension difference between the base material and aqueous solution, ensuring accurate and residue-free transfer of conductive patterns using water.
Patent Information
- Application Number
- JP2023053005
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing conductive pattern transfer methods using water as a solvent face challenges in achieving accurate transfer due to variations in adhesive strength between the PVA aqueous solution and the skin, leading to defects such as distorted patterns, particularly for thin lines.
A conductive pattern transfer sheet with a water-insoluble net-like base material and a mesh layer containing a water-soluble resin, where the difference in surface tension between the base material and the aqueous solution is maintained at 20 mN/m or more, ensuring effective peeling and transfer accuracy.
The sheet enables reliable transfer of conductive patterns using water without adhesive residue on the base material, maintaining pattern integrity and accuracy even on sensitive skin surfaces.
Smart Images

Figure 2024141396000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive pattern transfer sheet onto which a conductive pattern such as an electrode or a conductive circuit can be transferred by transfer, and more specifically, to a transfer sheet suitable for transferring a conductive pattern onto the skin surface. [Background technology]
[0002] With the recent development of wearable devices, research is progressing into forming conductive circuits and electrodes directly on the surface of the human skin. For example, International Publication No. 2020 / 241685 (Patent Document 1) proposes a nanomesh laminate that can form a conductive circuit on the skin surface by transfer. This nanomesh laminate uses a mesh substrate made of a hydrophobic thermoplastic resin such as polyethylene or polypropylene, on which a nanomesh composed primarily of PVA nanofibers is formed by electrospinning, and this nanomesh is then coated with a conductive metal or the like to form a conductive circuit.
[0003] When the conductive metal side of such a nanomesh laminate is pressed against the skin surface and water or alcohol is applied from the mesh substrate side in this state, the water or alcohol penetrates the pores of the mesh substrate and reaches the nanomesh layer. The nanomesh layer made of PVA nanofibers dissolves in water or alcohol, and the gel of the PVA solution produced by the dissolution acts as an adhesive, allowing the mesh-shaped conductive metal, i.e., the conductive circuit, to be transferred and fixed onto the skin. After transfer and fixation, when the mesh substrate is peeled off, a conductive circuit fixed by the gel of the PVA solution is formed on the skin surface. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2020 / 241685 Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, some subjects undergoing treatment are hypersensitive to alcohol irritation, and so there is a strong demand to use water rather than alcohol or an alcohol-based aqueous solution as the liquid applied for transfer (transfer solvent).
[0006] Example 3 of Patent Document 1 describes how a PVA nanomesh laminate using a polypropylene mesh substrate was placed on the skin of a subject, and gold wire was transferred by pressing absorbent cotton soaked in water only onto the mesh substrate.
[0007] However, it was found that, depending on the subject, the gold wires may not be transferred properly even when the procedure was performed in the same manner as in Example 3. In particular, when transferring a thin line pattern such as an electric circuit, transfer defects such as the collapse of the transferred pattern tend to occur easily.
[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a sheet for transferring a conductive pattern that can transfer the conductive pattern precisely, even when the conductive pattern is transferred using water. [Means for solving the problem]
[0009] Since the above problem did not occur when alcohol (aqueous solution) was used for transfer, the inventors assumed that the cause of the variation in transfer accuracy was related to the type of liquid used, and conducted various investigations. As a result, they found that the transfer accuracy also varies depending on the subject's skin condition and body temperature, and that in the case of poor transfer, part of the conductive circuit formed on the mesh laminate is not transferred and remains on the mesh base material side of the mesh laminate.
[0010] As a result of further investigation, it was concluded that the difference in adhesive strength between the PVA aqueous solution and the mesh base material, and the adhesive strength between the skin and the PVA aqueous solution, differs depending on the condition of the skin, which is why the transfer accuracy varies from subject to subject. The inventors then reached the conclusion that in the case of a PVA alcohol solution or an alcohol-water solution, the difference in adhesive strength between the skin and the mesh-like substrate is much greater than the variation in adhesive strength between the skin and the PVA alcohol solution or the alcohol-water solution due to individual differences in skin condition, making it less likely that transfer defects will occur due to individual differences in skin condition, and thus arrived at the present invention.
[0011] That is, the conductive pattern transfer sheet of the present invention has the following features. [1] A sheet for transferring a conductive pattern to a surface of an object by using water, comprising: The conductive pattern transfer sheet is a laminate in which a mesh layer containing a water-soluble resin as a main component is laminated on at least a water-insoluble net-like substrate, and a conductive material portion is provided on the mesh layer, The water-insoluble network substrate has an opening ratio of 55 to 70%, A conductive pattern transfer sheet, wherein the difference between the surface tension of the surface constituting material of the water-insoluble network substrate and the surface tension of the aqueous solution of the water-soluble resin is 20 mN / m or more.
[0012] [2] The conductive pattern transfer sheet according to [1], wherein the surface constituent material of the water-insoluble network substrate is a first water-insoluble polymer having a surface tension of 30 mN / m or less.
[0013] [3] The conductive pattern transfer sheet according to [2], wherein the first water-insoluble polymer is a fluorine-based resin or a silicone resin.
[0014] [4] The conductive pattern transfer sheet according to [2] or [3], wherein the water-insoluble mesh substrate is a woven or nonwoven fabric composed of fibers or threads of the first water-insoluble polymer.
[0015] [5] The woven or nonwoven fabric has a fiber diameter of 50 μm to 500 μm and a basis weight of 20 g / cm 2 ~250g / cm 2The conductive pattern transfer sheet according to [4],
[0016] [6] The conductive pattern transfer sheet according to [4], wherein the woven fabric or nonwoven fabric has an opening of 100 μm to 2 mm.
[0017] [7] The conductive pattern transfer sheet according to [2] or [3], wherein the water-insoluble mesh substrate is a mesh base made of a water-insoluble material, the surface of which is coated with the first water-insoluble polymer.
[0018] [8] The conductive pattern transfer sheet according to any one of [1] to [7], wherein the water-soluble resin is a polyvinyl alcohol-based resin.
[0019] [9] The conductive pattern transfer sheet according to [8], wherein the mesh layer is an aggregate of nanofibers of a polyvinyl alcohol-based resin.
[0020]
[10] A method for forming a conductive pattern on a surface of an object, comprising the steps of: a step of placing the sheet for transferring a conductive pattern according to any one of [1] to [9] on a surface of an object so that the conductive material portion is in contact with the object; applying water to the water-insoluble network substrate side of the conductive pattern transfer sheet; and peeling the reticulated substrate after application of water. A method for forming a conductive pattern comprising:
[0021]
[11] A kit for transferring a conductive pattern comprising the sheet for transferring a conductive pattern according to any one of [1] to [9] and a transfer assistant member impregnated with water so as to be releasable by pressure. Effect of the Invention
[0022] In the conductive pattern transfer sheet of the present invention, the aqueous solution of the hydrophilic resin that constitutes the mesh layer has poor wettability with respect to the surface of the mesh substrate, so even if water is used as the transfer solvent, the mesh substrate has good peelability after transfer and the conductive pattern transferability is excellent. [Brief description of the drawings]
[0023] [Figure 1] 1 is a schematic diagram showing a configuration of one embodiment of a transfer sheet of the present invention. [Diagram 2] 1A to 1C are schematic diagrams illustrating a method of using the transfer sheet of one embodiment of the present invention. [Diagram 3] 10A to 10C are schematic diagrams for explaining another example of a method of using the transfer sheet of the embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention will be described in detail below. However, the description of the constituent elements described below is one example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents, and can be implemented in various modifications within the scope of the gist of the present invention.
[0025] [Conductive pattern transfer sheet] The conductive pattern transfer sheet of the present invention is a conductive pattern transfer sheet for transferring a conductive pattern to a surface of an object by using water, and the conductive pattern transfer sheet is a laminate having at least a water-insoluble mesh base material, a mesh layer mainly composed of a water-soluble resin laminated thereon, and a conductive material portion on the mesh layer, The water-insoluble network substrate has an opening ratio of 55 to 70%, In the conductive pattern transfer sheet, the difference between the surface tension of the surface constituent material of the water-insoluble network substrate and the surface tension of the aqueous solution of the water-soluble resin is 20 mN / m or more.
[0026] FIG. 1 is a schematic diagram showing the configuration of one embodiment of the transfer sheet of the present invention. The transfer sheet is a laminate in which a mesh layer 2 containing a water-soluble resin as a main component is laminated on at least a mesh-like substrate 1, and a conductive material portion 3 is provided on the mesh layer 2. Each layer will be described in detail below.
[0027] (1) Mesh base material The net-like substrate 1 is a sheet-like material in which at least the surface is made of a water-insoluble polymer, preferably a hydrophobic resin, and has openings that serve as communicating holes through which water can pass to dissolve the water-soluble resin. It is usually made of a woven or nonwoven fabric made of fibers or threads made of a water-insoluble material. The threads used here may be either monofilament or multifilament. In the case of a woven fabric, the weaving method is not particularly limited. The water-insoluble polymer constituting at least the surface of the network substrate may be referred to as a first water-insoluble polymer (first water-insoluble polymer).
[0028] When the ratio of the openings to the sheet surface, that is, the opening rate, is 55 to 70%, the gaps between the fibers constituting the sheet or the gaps between the threads in the woven fabric become the openings (mesh openings).
[0029] The first water-insoluble polymer has a surface tension that is 20 mN / m or more smaller than the surface tension of the aqueous solution of the water-soluble resin that constitutes the mesh layer 2. As described later, a PVA-based resin is generally used as the water-soluble resin that constitutes the mesh layer 2, and since the concentration of the aqueous solution in which the water-soluble resin is dissolved is about 0.1 to 5%, it is preferable that the surface tension of the surface material is 30 mN / m or less, preferably 25 mN / m or less, and more preferably 23 mN / m or less.
[0030] Examples of the first water-insoluble polymer include fluorine-based resins such as polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), perfluoroethylene-propene copolymer (FEP), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene, and ethylene-chlorotrifluoroethylene copolymer; and silicone resins whose main chains are composed of siloxane bonds. Among these, fluorine-based resins and silicone-based resins, which have particularly low surface tension, are preferred, and polytetrafluoroethylene is more preferred.
[0031] The mesh-like substrate 1 only needs to satisfy the requirement that the surface tension of the surface material of the substrate 1 is smaller than the surface tension of the aqueous solution of the water-soluble resin constituting the mesh layer 2 by 20 mN / m or more. Therefore, in addition to the case where the entire network substrate 1 is made of the first water-insoluble polymer, the surface of a network substrate (main body) made of a water-insoluble material may be coated with the first water-insoluble polymer.
[0032] When the main body and the surface of the net-like substrate are made of different materials, the water-insoluble material constituting the main body does not need to have a small surface tension like the first water-insoluble polymer, so a wide range of water-insoluble materials can be used. For example, in addition to the fluorine-based resin and silicone-based resin exemplified as the first water-insoluble polymer, synthetic resins such as polyolefin resins such as polypropylene and polyethylene, polyamide, polyester, polyurethane, and acrylic resins can be used. Furthermore, natural polymers such as cellulose-based polymers such as cotton and hemp, animal polymers such as wool, and polysaccharides such as chitin, chitosan, and hyaluronic acid can be used. The water-insoluble polymer that can be used here is to be distinguished from the first water-insoluble polymer. Hereinafter, when the main body and the surface of the net-like substrate are made of different materials, the water-insoluble polymer that constitutes the main body will be referred to as the second water-insoluble polymer.
[0033] In addition, when the mesh substrate 1 is a sheet, woven fabric, or nonwoven fabric of the main body portion coated with a first water-insoluble polymer, the main body portion can be a woven fabric or nonwoven fabric composed of fibers or threads made of the second water-insoluble polymer. For example, a woven or nonwoven fabric of the second water-insoluble polymer may be coated with the first water-insoluble polymer.Specific examples include a woven or nonwoven fabric of an olefin resin, polyester, or the like, coated with a fluorine-based resin or silicone resin.
[0034] The ratio of interconnected holes in the mesh substrate 1 (opening ratio) is 50% to 80%, and preferably 55 to 75%. If the opening ratio is too high, the strength of the mesh substrate 1 is too low, the retention of the mesh layer 2 is insufficient, and the sheet-like material becomes weak and difficult to handle. On the other hand, if the opening ratio is too low, the water permeability, permeation amount, and permeation speed are reduced, and it takes a long time to dissolve the mesh layer 2, which in turn takes a long time to transfer and fix the conductive pattern. In particular, since the surface of the mesh substrate 1 is composed of a material (first water-insoluble polymer) with low surface tension as described above, if the opening rate is insufficient or the size of the openings is too small, the applied transfer solvent water will form droplets on the surface of the mesh substrate and will be less likely to pass through the openings.
[0035] The average size of the openings (or mesh size) is not particularly limited, but since the surface of the net-like substrate is formed from a material with low wettability to water, the mesh size is usually 100 μm or more, preferably 200 μm or more. If the size of each individual hole becomes too large, the strength of the net-like substrate decreases and it becomes difficult to uniformly support the nanofibers, so the size of the openings (mesh size) is preferably 2 mm or less, preferably 1 mm or less.
[0036] The size (weight) of the openings and the opening ratio can be adjusted by the diameter of the fibers or the thickness of the threads constituting the woven or nonwoven fabric, the number of meshes, and the like.
[0037] The shape of the openings is not particularly limited, and examples thereof include 60° staggered, square staggered, parallel, oblong hole staggered, oblong hole parallel, square hole staggered, square hole parallel, hexagonal 60° staggered, oblong hole staggered, oblong hole parallel, etc. The square hole parallel type is preferred from the viewpoint of adhesion to the mesh layer 2.
[0038] In this specification, the opening ratio means the area ratio of voids to a unit area when the net-like substrate is viewed in a plane, and when the opening pattern is regular, the opening ratio can be calculated based on the pattern. In the case of woven or nonwoven fabrics, the opening ratio can be calculated from the fiber diameter or thread thickness, basis weight, mesh number, etc.
[0039] In the case where the openings are in an irregular pattern, the opening ratio can be obtained by observing the net-like substrate with a digital microscope and binarizing the pattern of the openings by digital processing. For example, the pattern can be binarized and captured with an optical microscope at a magnification of 10 times, and the ratio of the openings to the total area can be calculated. The size of one grid for binarization can be measured in a range of about 0.1 mm x 0.1 mm. In addition, if the pattern of the openings is particularly irregular, the opening ratio can be obtained by taking an image of a 1 cm x 1 cm range at a magnification of about 10 times, and calculating the ratio of the openings with 0.1 mm x 0.1 mm as one grid. When the pattern of the openings is irregular, the water permeability or water permeation rate may be used as an index instead of the opening ratio.
[0040] In the case of a woven fabric or nonwoven fabric, the preferred lower limit of the fiber diameter of the thread is 50 μm, and the preferred upper limit is 500 μm. If the fiber diameter of the thread is less than 50 μm, the stiffness of the woven fabric or nonwoven fabric is lost, and it tends to be difficult to ensure sufficient strength as a mesh support. On the other hand, if it exceeds 500 μm, it becomes difficult to adjust the size of each opening corresponding to the gap between the fibers or thread within an appropriate range.
[0041] The basis weight of the woven or nonwoven fabric is an amount that can ensure the above-mentioned opening ratio, and varies depending on the type of yarn used and the weaving and knitting methods, but usually, the preferable lower limit is 20 g / m 2 , the preferred upper limit is 250 g / m 2 It is.
[0042] The thickness of the mesh substrate 1 is usually 10 μm or more, preferably 50 μm or more, more preferably 100 μm or more, and usually 500 μm or less, preferably 400 μm or less, more preferably 300 μm or less. If it is too thick, the water passing distance becomes long, which causes a decrease in water permeability. If it is too thin, the strength as a mesh support layer becomes insufficient, and the handling of the transfer sheet decreases.
[0043] (2) Mesh layer The mesh layer 2 is composed of an aggregate of nanofibers 2a made of a water-soluble resin. Examples of the water-soluble resin include synthetic polymers such as polyvinyl alcohol resins, polyethylene glycol, polyethylene oxide, polyacrylic acid, polymethacrylic acid, polyvinylpyrrolidone, and polyacrylamide, as well as natural polymers such as gelatin, pullulan, and water-soluble collagen, and chemically modified polymers thereof (excluding thickening polysaccharides). Of these, polyvinyl alcohol-based resins are preferred, and from the standpoint of ease of production of the nanofibers 2a that constitute the mesh layer, it is preferred that the polyvinyl alcohol-based resin is contained in an amount of more than 50% by weight, preferably 70% by weight or more, and more preferably 90% by weight or more.
[0044] Examples of the PVA-based resin include unmodified PVA, as well as carboxyl group-containing PVA, sulfo group-containing PVA, acetoacetyl group-containing PVA, and modified PVA having a 1,2-diol structure in the side chain, etc. Among them, unmodified PVA is preferred in terms of compatibility with the living body.
[0045] PVA resin is a resin mainly composed of vinyl alcohol structural units, obtained by saponifying vinyl ester resin obtained by polymerizing vinyl ester monomers, and is composed of vinyl alcohol structural units corresponding to the degree of saponification and vinyl ester structural units remaining without saponification. Modified PVA has vinyl alcohol structural units, vinyl ester structural units, and other structural units.
[0046] The average degree of polymerization of the PVA resin is preferably 300 or more, more preferably 350 or more, even more preferably 400 or more, and particularly preferably 500 or more. By setting it in this range, the strength of the mesh is improved. On the other hand, it is preferably 3500 or less, more preferably 3000 or less, even more preferably 2500 or less, and particularly preferably 2300 or less. By setting it in this range, the PVA resin can be easily produced. In this embodiment, the average degree of polymerization of the PVA resin is determined by a method conforming to JIS K 6726.
[0047] From the viewpoint of water solubility, the saponification degree of the PVA resin is preferably 70 to 100 mol%, more preferably 70 to 95 mol%, further preferably 70 to 92 mol%, and particularly preferably 70 to 90 mol%. In the present embodiment, the saponification degree of the PVA resin is a value determined by a method in accordance with JIS K 6726.
[0048] The surface tension of the aqueous solution of the PVA-based resin as described above depends on the molecular weight of the PVA-based resin and the basis weight of the mesh layer, but in relation to the amount of water generally used, the aqueous solution concentration is about 0.1 to 5%, and the surface tension of the aqueous solution is about 40 to 55 mN / m, preferably about 45 to 53 mN / m.
[0049] The fiber diameter of the nanofibers 2a constituting the mesh layer 2 is preferably 50 nm or more, more preferably 100 nm or more, more preferably 200 nm or more, and particularly preferably 300 nm or more. Also, it is usually 1000 nm or less, preferably 900 nm or less, more preferably 800 nm or less, even more preferably 600 nm or less, and particularly preferably 500 nm or less. By setting the fiber diameter to such a value, solubility in a solvent can be ensured, durability as a mesh layer in the transfer sheet can be increased, and the mesh layer can play a role as a support layer for the conductive material portion 3.
[0050] The mesh layer 2 can usually be formed by an electrospinning method (electric field spinning method), a melt blowing method, a sea-island melt spinning method, or the like. The formation of the mesh layer 2 by electrospinning can be carried out by a known method. A solution (spinning solution) in which a water-soluble polymer material is dissolved is filled into a syringe, and a high voltage is applied between the nozzle of the syringe and a conductive collector to spray the solution in a jet form. The solvent volatilizes during the spraying process, and nanofibers are deposited on the collector.
[0051] The mesh layer 2 formed as described above can maintain a sheet-like shape because the nanofibers 2a are bonded at their intersections or the nanofibers 2a are entangled with each other.
[0052] The sheet of nanofibers formed by the electrospinning method may be peeled off from the collector and laminated onto a mesh substrate, or the mesh layer 2 can be laminated directly onto the mesh substrate 1 by setting the mesh substrate 1 on a collector in an electrospinning device.
[0053] In the electrospinning method, the fiber diameter of the nanofibers 2a can be adjusted, for example, by the concentration of the spinning solution used in producing the mesh layer. The fiber diameter becomes thicker as the concentration of the water-soluble resin in the spinning solution increases. In the melt-blowing method, the fiber diameter can be adjusted, for example, by the discharge amount of the spinning solution used in producing the mesh layer. The fiber diameter tends to become thicker as the discharge amount of the spinning solution increases.
[0054] In addition to the water-soluble resin, the components constituting the mesh layer 2 may contain, as necessary, plasticizers such as polyhydric alcohols such as glycerin, sorbitol, and polyethylene glycol, or alkylene oxide adducts thereof, and thickeners such as fermented polysaccharides such as polysaccharides and gums, and glucoses such as starch and dextrin. However, the content of these additives is preferably an amount that does not excessively reduce the surface tension of the aqueous solution of the water-soluble resin constituting the mesh layer 2 and does not affect the water solubility, and specifically, is 10% by weight or less of the mesh layer, preferably 5% by weight or less, and more preferably 2% by weight or less.
[0055] The thickness of the mesh layer 2 may be appropriately set depending on the purpose, and is not particularly limited, but is usually 0.1 μm or more, and may be 1 μm or more, and is usually 100 μm or less, and may be 80 μm or less.
[0056] The mesh layer 2 made of the above-mentioned materials dissolves in water and solidifies when dried, becoming a gel-like substance of a water-soluble resin. The concentration of the water-soluble resin in the gel of the water-soluble resin will vary depending on the amount of water used and the type of water-soluble resin, as described below, but will usually be about 0.1 to 5%. The surface tension of the aqueous solution of the water-soluble resin is usually 40 to 60 mN / m, depending on the type of water-soluble resin and the concentration of the aqueous solution. In the case of PVA-based resin, a 0.1 to 5%, preferably 0.3 to 1% aqueous solution is generally used, and the surface tension of the resulting aqueous solution of PVA-based resin is about 45 mN / m to 50 mN / m. Therefore, the difference in surface tension between the surface of the net-like substrate and the aqueous solution of the water-soluble resin constituting the mesh layer can be 20 mN / m or more, preferably 25 mN / m, and more preferably 28 mN / m.
[0057] (3) Conductive material part The conductive material portion 3 corresponds to a conductive pattern such as an electrode or a conductive circuit formed on the surface of the object. The conductive material used for the conductive material portion 3 is usually a conductive material such as a metal such as platinum, silver, silver chloride, copper, titanium, palladium, chromium, or cobalt, or an alloy thereof, or carbon. Conductive metal oxides such as ITO (indium tin oxide), nickel oxide, tin oxide, indium oxide, indium-zirconium oxide (IZO), titanium oxide, or zinc oxide; PEDOT:PSS in which a polythiophene derivative is doped with polystyrene sulfonic acid, PEDOT:PTS in which a polythiophene derivative is doped with paratoluenesulfonic acid, or conductive polymer materials in which polypyrrole or polyaniline is doped with iodine or the like may be used. Of these, gold, carbon, titanium, PEDOT:PSS, and PEDOT:PTS may also be used in consideration of application to living organisms.
[0058] The method for forming the conductive material portion 3 is not particularly limited, and the conductive material portion 3 is formed by a dry process or a coating method. As the dry process, vapor deposition, sputtering, CVD, etc. are used. Among these, it is easiest to form the conductive material portion (or layer) by vapor deposition. There is no particular limit to the coating method, but specific examples include wire bar coating, blade coating, die coating, slit die coating, reverse roll coating, gravure coating, kiss coating, roll brushing, spray coating, air knife coating, pipe doctor, impregnation coating, curtain coating, flexographic printing, screen printing, inkjet, etc.
[0059] The thickness of the conductive material portion 3 is not particularly limited, but is usually 5 nm or more, and may be 10 nm or more, and is usually 2 μm or less, and may be 1 μm or less, or may be 500 nm or less.
[0060] (4) Other layers The conductive pattern transfer sheet of the present invention may include, as a minimum constituent unit, a laminate in which a mesh layer is laminated on the above-mentioned mesh substrate and a conductive material portion is provided on the mesh. If necessary, a protective layer (not shown) may be further laminated on the surface of the mesh substrate and / or the conductive material portion.
[0061] The protective layer may be a plastic film, paper, woven or nonwoven fabric, etc., which can be easily peeled off before use.
[0062] [How to use] A method for transferring a conductive material portion of the present invention, typically a method for transferring and forming a conductive pattern on the skin of a subject, will now be described.
[0063] FIG. 2 is a process diagram showing a flow of a method for forming conductive pattern 13 on the surface of arm 21, which is an example of an object, using transfer sheet 10 of the embodiment shown in FIG.
[0064] Transfer sheet 10 is placed so that conductive material portion 3 is in contact with the surface (skin) of object 21 (FIG. 2(1)). Next, water, which serves as a transfer solvent, is applied from the side of the reticulated substrate 1. The application method may be to spray the water, or to bring a transfer assistant member containing water into contact with and press it against the reticulated substrate. In Fig. 2(2), water is sprayed from above the reticulated substrate 1. In Fig. 2(2), 23 represents the sprayed water. FIG. 3 shows the application of water using a water-filled transfer assist member 24 .
[0065] The nanofibers 2a of the water-soluble resin that constitutes the mesh layer 2 dissolve, and the gel-like material 12 of the water-soluble resin is fixed onto the skin surface 21. The water-soluble resin gel-like material 12 acts as an adhesive, and the conductive material portion 3 on the mesh layer 2 is fixed and formed as a conductive pattern 13 on the surface of the object 21 (skin surface). Once the solidification of the gel-like material 12 has been confirmed, the mesh base material 1 can be peeled off (FIG. 2(3)). Since the affinity (wettability) of the aqueous solution resin that constitutes the mesh layer 2 with the skin is greater than the affinity of the surface material of the mesh base material 1 with the aqueous solution of the water-soluble resin, the aqueous solution of the water-soluble resin migrates from the surface of the mesh base material to the skin surface and can be peeled off at the interface with the mesh base material 1.
[0066] In this manner, the water-soluble resin gel 12 is transferred onto the skin together with the conductive metal portion 3 and solidifies. That is, a mesh-shaped conductive material portion corresponding to the conductive pattern is formed on the skin surface.
[0067] Although the conductive pattern transfer sheet and its method of use have been described using human skin as an example of an object, the object is not limited to human skin. For example, the conductive pattern transfer sheet of the present invention can be used as a transfer sheet for transferring a conductive pattern such as a conductive circuit or an electrode to an object such as a glass plate or a plastic film. In this case, the above-mentioned method of use can be applied as the transfer method.
[0068] [Conductive pattern transfer kit] The conductive pattern transfer kit of the present invention includes the conductive pattern transfer sheet disclosed in the present specification, and a transfer assistant member impregnated with water as a transfer solvent in such a manner that the water can be repelled by pressure.
[0069] The transfer auxiliary member may be any material that can absorb water in an amount necessary for transfer so as to be water-repellent, and examples of such material include cotton, nylon, polyester woven fabric, and polyester nonwoven fabric.
[0070] The conductive pattern transfer kit is provided to the user in combination with a transfer assistant member that is impregnated with an appropriate amount of water that is necessary and sufficient for a transfer operation using the sheet and is capable of repelling water, and is therefore convenient in that the user does not need to measure the amount of water as a transfer solvent. EXAMPLES
[0071] The present invention will be described in more detail below using examples, but it goes without saying that the scope of the present invention is not limited to the description of the examples. In the examples, "parts" and "%" are by weight unless otherwise specified.
[0072] [Reticulated substrate] As shown below, three types of mesh substrates (3cm x 5cm) with different surface materials were used. The surface tension shown here is the surface tension when the surface is flat (opening ratio 0%). The aperture ratio was calculated from the mesh number (the number of threads per inch) and the fiber diameter (μm), with the distance between the threads being the aperture (mesh size).
[0073] ·Reticulated substrate A: Polytetrafluoroethylene thread (diameter 250μm) square hole parallel mesh sheet (opening 766μm, mesh number 25 / inch), opening rate: 57% Reticulated substrate B: Polypropylene thread (diameter 440μm) mesh sheet with parallel square holes (opening size 710μm, mesh number 23 / inch), opening ratio 63% ·Reticulated substrate C A silicone-based metal release agent (Pando 39D) manufactured by ThreeBond Co., Ltd. was sprayed onto the surface of the mesh-like substrate B (opening ratio 63%). ·Reticulated substrate D: Polypropylene thread (diameter 100μm) mesh sheet with parallel square holes (opening size 106μm, mesh number 119 / inch), aperture ratio 26% ·Reticulated substrate E: A silicone-based metal release agent (Pando 39D) manufactured by ThreeBond Co., Ltd. was sprayed onto the surface of the mesh-like substrate D (opening ratio: 26%).
[0074] [Preparation of transfer sheet and transfer of conductive material portion] (1) Formation of mesh layer 100 parts of PVA (unmodified, saponification degree 88 mol%, 4 wt% aqueous solution viscosity 47.8 mPa·s) and 20 parts of glycerin were dissolved in pure water to prepare an 8 wt% aqueous PVA solution, which was used as the spinning solution. Four milliliters of this spinning solution was placed in the syringe of an electrospinning device, an electrode was attached to the non-beveled 24G 1-pin or 4-pin needle (Terumo Corporation) at the tip of the syringe, a mesh substrate shown in Table 1 was placed on a collector, and a mesh layer (weight per unit area: 1.7 g / m) was produced by electrospinning. 2 The electrospinning apparatus was set as follows:
[0075] <Setting conditions> Target speed: 5m / min Traverse speed: 16cm / min Syringe speed: 0.064mm / min Voltage: 18kV Film forming time: 75min
[0076] (2) Formation of conductive material part (layer) A metal mask with an opening of 0.5 mm x 30 mm was placed on the mesh layer formed above, and a 100 nm-thick gold thin film (conductive material layer) was formed using a ULVAC vacuum deposition machine EX-400.
[0077] (3) Transfer of conductive material Transfer sheets No. 1 to 5 prepared according to the above method were placed so that the conductive material portion (layer) was in contact with the skin surface, and then cotton (transfer assistant member) soaked in sterilized water was pressed against the mesh-like substrate for about 5 minutes in an indoor environment at about 23° C. The cotton, which was the transfer assistant member, was then removed, and the mesh-like substrate was air-dried using a blower for about 30 seconds, after which the mesh-like substrate was peeled off.
[0078] The five subjects each underwent the transfer process twice, and the ease of peeling after transfer, the appearance of the formed conductive pattern, and the adhesive residue on the surface of the net-like substrate after peeling (the remaining state of the PVA-based resin layer and the conductive metal part) were visually observed and evaluated according to the following criteria. The results are shown in Table 1.
[0079] ◯: No adhesive residue remains on the mesh base material, and the transferred conductive pattern is free of any disturbances such as breaks. △: For some subjects, glue residue was found on the mesh base material, and some of the transferred conductive pattern was broken. ×: The mesh layer was insufficiently soluble in water, and there were some subjects who were unable to perform the transfer work. Even if the transfer was possible, the transferred conductive pattern was incomplete, with chips or the like.
[0080] The surface tension of the PVA aqueous solution was calculated based on the surface tension of a 0.5% PVA aqueous solution, which is 49.7 mN / m, and the difference between this and the surface tension of the surface material of the net-like substrate was calculated.
[0081] For the reference example, cotton soaked in a water (20%)-ethanol (80%) mixture was used as a transfer assistant member instead of water, and the mesh layer was dissolved. Note that the surface tension of the water-ethanol mixture of PVA is 28.5 mN / m, and the difference in surface tension in Table 1 shows the difference from the surface tension of the water-ethanol mixture of PVA.
[0082] [Table 1]
[0083] In both transfer sheets No. 3 and 4, the difference in surface tension between the surface material of the mesh substrate and the water-soluble resin aqueous solution (PVA aqueous solution) of the mesh layer was less than 20 mN / m. Perhaps because it had a certain degree of affinity with the mesh substrate surface, residual glue and associated conductive material were found on the mesh substrate after peeling. As a result, the conductive pattern formed on the skin surface was incomplete, with partial chipping.
[0084] On the other hand, in both No. 1 and 2, the difference in surface tension between the surface material of the net-like substrate and the water-soluble resin aqueous solution (PVA aqueous solution) of the mesh layer was 20 mN / m or more. The PVA aqueous solution in which the nanofibers were dissolved transferred from the net-like substrate surface to the skin surface, and the entire conductive material was transferred with it, allowing the intended conductive pattern to be transferred without any defects to the skin surface.
[0085] In No. 5, the surface material of the mesh substrate was the same as in No. 2, and the difference in the surface tension of the water-soluble resin aqueous solution was 20 mN / m or more. However, because the mesh openings in the mesh substrate were small, water used as the transfer solvent could not penetrate sufficiently. As a result, the mesh layer was not sufficiently dissolved, and it was unable to fully function as an adhesive.
[0086] The reference example is a case where a water-ethanol mixture was used as the transfer solvent. The composition of the transfer sheet is the same as No. 4, but the surface tension of the PVA alcohol aqueous solution generated by dissolving the mesh layer was low at 28.5 mN / m, and the surface tension difference was also low at 9 mN / m. Since the PVA alcohol aqueous solution has high wettability with the skin, it is believed that the entire mesh layer peeled off from the net-like substrate, forming a conductive pattern without any chips. [Industrial Applicability]
[0087] The conductive pattern transfer sheet of the present invention can use water as the transfer solvent without impairing the transfer accuracy, and therefore can be used without concern for the usage environment, and even when the object to which the conductive pattern is to be transferred is the human body, there is no need to worry about allergies, etc. [Explanation of symbols]
[0088] 1. Mesh base material 2 Mesh Layer 2a Nanofiber 3 Conductive metal parts 10 Transfer sheet 13 Conductive Pattern 21 Object (skin) 23 Water Spray 24 Transfer auxiliary material
Claims
1. A sheet for transferring a conductive pattern to a surface of an object by using water, comprising: The conductive pattern transfer sheet is a laminate in which a mesh layer containing a water-soluble resin as a main component is laminated on at least a water-insoluble net-like substrate, and a conductive material portion is provided on the mesh layer, The water-insoluble network substrate has an opening ratio of 55 to 70%; The conductive pattern transfer sheet, wherein the difference between the surface tension of the surface constituting material of the water-insoluble network substrate and the surface tension of the aqueous solution of the water-soluble resin is 20 mN / m or more.
2. 2. The conductive pattern transfer sheet according to claim 1, wherein the surface constituting material of the water-insoluble network substrate is a first water-insoluble polymer having a surface tension of 30 mN / m or less.
3. 3. The conductive pattern transfer sheet according to claim 2, wherein the first water-insoluble polymer is a fluorine-based resin or a silicone resin.
4. 3. The conductive pattern transfer sheet according to claim 2, wherein the water-insoluble network substrate is a woven or nonwoven fabric made of fibers or threads of the first water-insoluble polymer.
5. The woven or nonwoven fabric has a fiber diameter of 50 μm to 500 μm and a basis weight of 20 g / cm 2 ~250g / cm 2 The conductive pattern transfer sheet according to claim 4, wherein
6. 5. The conductive pattern transfer sheet according to claim 4, wherein the woven fabric or nonwoven fabric has an opening of 100 μm to 2 mm.
7. 3. The conductive pattern transfer sheet according to claim 2, wherein the water-insoluble network substrate is a network substrate made of a second water-insoluble polymer, the surface of which is coated with the first water-insoluble polymer.
8. 2. The conductive pattern transfer sheet according to claim 1, wherein the water-soluble resin is a polyvinyl alcohol-based resin.
9. 9. The conductive pattern transfer sheet according to claim 8, wherein the mesh layer is an aggregate of nanofibers of a polyvinyl alcohol-based resin.
10. A method for forming a conductive pattern on a surface of an object, comprising the steps of: A step of placing the sheet for transferring a conductive pattern according to any one of claims 1 to 9 on a surface of an object so that the conductive material portion is in contact with the object; applying water to the water-insoluble network substrate side of the conductive pattern transfer sheet; and peeling the reticulated substrate after application of water. A method for forming a conductive pattern comprising:
11. 10. A kit for transferring a conductive pattern comprising the sheet for transferring a conductive pattern according to claim 1 and a transfer assistant member impregnated with water so as to be capable of repelling water by pressure.
Citation Information
Patent Citations
Hologram label
JP2014142546A
Nanomesh multilayer body, method for producing conductive circuit and nanomesh bonding kit
WO2020241685A1