Nonwoven fabric and manufacturing method thereof, filter unit, and air cleaning machine
A nonwoven fabric with controlled fiber diameters and surface irregularities addresses the trade-off between collection efficiency and pressure loss, achieving high efficiency and low loss for fine dust in air and liquid filtration.
Patent Information
- Application Number
- JP2023053080
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing air filters face a trade-off between high collection efficiency for fine dust and low pressure loss, with conventional methods either compromising on one or the other, particularly in applications requiring high efficiency for particles smaller than 0.3 μm.
A nonwoven fabric composed of thermoplastic resin fibers with specific diameter ranges and surface irregularities, along with controlled surface area and height parameters, is developed to achieve both low pressure loss and high collection efficiency for minute dust particles.
The nonwoven fabric exhibits excellent collection efficiency for fine dust while maintaining low pressure loss, suitable for use in air filters, liquid filters, masks, and protective clothing.
Smart Images

Figure 2024141431000001 
Figure 2024141431000002 
Figure 2024141431000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonwoven fabric. [Background technology]
[0002] In recent years, there has been an increasing demand for cleaner spaces, and air filters that remove fine dust particles from the air are used in a wide range of fields, from living environments to industry, to address health problems caused by dust particles with a particle size of 2.5 μm or less, and to eliminate dust in semiconductor and pharmaceutical manufacturing.
[0003] Air filters take in air containing dust and purify the air that passes through by capturing the dust in the filter material. In addition to being able to capture dust efficiently, low pressure loss is also an important feature of air filters, as the lower the pressure loss when gas passes through the filter, the less power consumed by air purifiers and factory filter fan units.
[0004] In order to improve the dust collection efficiency, it is possible to make the filter medium denser by making the fibers that make up the filter medium extremely fine, but this would result in a smaller pore size in the filter medium. This pore size refers to the size of the through holes formed by the fibers that make up the filter medium. As the pore size of the filter medium becomes smaller, the air resistance increases and the pressure loss increases, so collection efficiency and pressure loss are contradictory. In particular, in semiconductor and pharmaceutical manufacturing, dust particles with a particle size of 0.3 μm or less must be collected with high efficiency, and the filter medium must be significantly denser, which increases the pressure loss and increases the power consumption of the filter fan, which is an issue.
[0005] Therefore, various efforts have been made to achieve both high collection efficiency and low pressure loss, which are contradictory properties.
[0006] For example, Patent Document 1 proposes a composite fiber nonwoven fabric produced by a melt-blowing method, in which a number of fiber agglomerates formed by partial aggregation and thermal bonding are present in the nonwoven fabric to form convex portions on the surface of the nonwoven fabric, and the gaps between the constituent fibers are wider around the fiber agglomerates than in areas where no fiber agglomerates are present, resulting in a lower fiber density, and the fabric has a bulkiness within a specific range.The document also describes that, due to the increased bulk, it has become possible to produce an air filter material that can be used without problems in a pleat folding machine, whereas the main raw material used in the past was an air filter made of a polyester resin-bonded nonwoven fabric bonded to a melt-blown nonwoven fabric.
[0007] Patent Document 2 proposes a filter medium having a specific bulk density range, which is made by mixing ultrafine fibers made of polyolefin or polyester with binder fibers in a specific weight ratio. It is described that this provides a filter medium and a filter having low pressure loss, long filter life, and high collection efficiency.
[0008] Furthermore, Patent Document 3 proposes a mixed long fiber nonwoven fabric in which two types of long fibers are made of different thermoplastic resins and the average fiber diameter and specific volume are within specific ranges. It is described that, when used as a filter, the fabric has low pressure loss, high collection efficiency, and can suppress an increase in pressure loss for a long period of time. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2004-3065 A [Patent Document 2] JP 2005-319347 A [Patent Document 3] JP 2013-40412 A Summary of the Invention [Problem to be solved by the invention]
[0010] According to the technology disclosed in Patent Document 1, compared to a normal melt-blown nonwoven fabric, the nonwoven fabric has more fiber agglomerates and is bulkier, so the pressure loss tends to be lower. However, the more fiber agglomerates, the more large voids there are, and as a result, the collection efficiency is also lower. Therefore, it is not suitable for a filter medium for collecting fine dust with high efficiency.
[0011] In addition, according to the technology disclosed in Patent Document 2, the pressure loss tends to be reduced by using binder fibers with a large fiber diameter. However, the collection efficiency is not sufficient, and the effect of reducing the pressure loss is not so great. Therefore, even if the collection efficiency is increased, the pressure loss cannot be sufficiently reduced.
[0012] According to the technology disclosed in Patent Document 3, the pressure loss tends to be low by using two types of long fibers made of different thermoplastic resins and configuring the fiber diameters to be within a specific range. However, the collection efficiency is not high enough as it is, and electret processing is essentially required.
[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a nonwoven fabric which has low pressure loss and exhibits excellent collection efficiency even for fine dust particles. [Means for solving the problem]
[0014] As a result of extensive research into achieving the above-mentioned object, the inventors have discovered that a nonwoven fabric composed of fibers having a fiber diameter within a specific range, having projections and recesses of a specific size on all of its surfaces, and having the sum of the areas of the projections and recesses at a specific ratio to the horizontal projected area, can achieve both low pressure loss and excellent collection efficiency for fine dust particles.
[0015] The present invention has been completed based on these findings, and provides the following inventions.
[0016] [1] A nonwoven fabric composed of fibers whose main component is a thermoplastic resin, The average single fiber diameter of the fibers is 0.10 μm or more and 10.00 μm or less, The minimum single fiber diameter of the fiber is 0.01 μm or more and 1.00 μm or less, The maximum single fiber diameter of the fiber is 2.00 μm or more and 20.00 μm or less, The nonwoven fabric has an arithmetic mean height Sa of 20 μm or more and 500 μm or less on either surface thereof, On either side of the surface of the nonwoven fabric, the sum of the area of the convex portions and the area of the concave portions on the surface is 1.10 times or more and 5.00 times or less the horizontal projected area of the surface. Nonwoven fabric.
[0017] [2] The nonwoven fabric according to [1], wherein the average pore size of the nonwoven fabric is 0.1 μm or more and 9.9 μm or less.
[0018] [3] The nonwoven fabric according to [1] or [2], wherein the root mean square height Sq of the surface on either side of the nonwoven fabric is 50 μm or more and 700 μm or less.
[0019] [4] The nonwoven fabric according to any one of [1] to [3] above, wherein the thickness of the nonwoven fabric is 0.1 mm or more and 2.9 mm or less.
[0020] [5] A filter unit comprising a filter medium containing the nonwoven fabric according to any one of [1] to [4] above, and held by a fixing material.
[0021] [6] An air purifier incorporating the filter unit described in [5] above.
[0022] [7] forming a web composed of fibers primarily made of a thermoplastic resin; adhering a heat shrinkable or stretchable fabric to one surface of the web to form a laminated web; shrinking the laminated web to obtain a shrink laminated web; removing the heat shrinkable or stretchable fabric from said shrinklaminate web; The method for producing a nonwoven fabric according to any one of the above [1] to [4], [8] The method for producing a nonwoven fabric described in [7] above, wherein the step of forming the web and the step of forming the laminated web are carried out in the same step. Effect of the Invention
[0023] According to the present invention, a nonwoven fabric can be obtained that exhibits both low pressure loss and excellent collection efficiency even for fine dust particles. In particular, the nonwoven fabric of the present invention is suitable for use in filter media such as air filters and liquid filters, as well as masks and protective clothing, due to its characteristics of both low pressure loss and high collection efficiency when a fluid passes through it. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The nonwoven fabric of the present invention is a nonwoven fabric composed of fibers mainly composed of a thermoplastic resin, the average single fiber diameter of the fibers is 0.10 μm to 10.00 μm, the minimum single fiber diameter of the fibers is 0.01 μm to 1.00 μm, the maximum single fiber diameter of the fibers is 2.00 μm to 20.00 μm, the arithmetic mean height Sa of the surfaces on either side of the nonwoven fabric is 20 μm to 500 μm, and the sum of the areas of the convex portions and the concave portions on either side of the nonwoven fabric is 1.10 times to 5.00 times the horizontal projection area of the surfaces. The components are described in detail below, but the present invention is not limited to the scope described below as long as it does not deviate from the gist of the invention.
[0025] [Fibers that make up nonwoven fabric] First, the fibers constituting the nonwoven fabric of the present invention are mainly composed of a thermoplastic resin. Here, in the present invention, "fibers mainly composed of a thermoplastic resin" refers to fibers in which the mass ratio of the thermoplastic resin in the fibers is 50 mass% or more.
[0026] Examples of thermoplastic resins include polyesters such as "polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polytrimethylene terephthalate, polylactic acid, etc.", polyolefins such as "polypropylene, polyethylene, etc.", and other melt-moldable polymers such as "polystyrene, polycarbonate, polyacrylate, polyamide, thermoplastic polyurethane, polyphenylene sulfide, etc.", as well as blends and copolymers thereof.
[0027] These thermoplastic resins may contain various additives, such as inorganic substances such as titanium oxide, silica, and barium oxide, colorants such as carbon black, dyes, and pigments, flame retardants, fluorescent brightening agents, antioxidants, light stabilizers, electrostatic stabilizers, water repellents, oil repellents, lubricants, antibacterial agents, antiviral agents, antifungal agents, and ultraviolet absorbing materials, as long as the additives do not impair the object of the present invention.
[0028] In the nonwoven fabric of the present invention, the average single fiber diameter of the fibers is 0.10 μm or more and 10.00 μm or less, the minimum single fiber diameter of the fibers is 0.01 μm or more and 1.00 μm or less, and the maximum single fiber diameter of the fibers is 2.00 μm or more and 20.00 μm or less. By being composed of fibers that satisfy these three conditions, a nonwoven fabric can be obtained that is capable of efficiently collecting fine dust particles while having good handleability and moldability.
[0029] First, the average single fiber diameter of the fibers is 0.10 μm or more and 10.00 μm or less. When the average single fiber diameter is in this range, a nonwoven fabric having a very dense microspace is formed, and the specific surface area effect produced by extremely fine fibers, that is, the effect of increasing the adhesion of fine dust to the fiber surface as the surface area of the fibers constituting the nonwoven fabric increases, can be advantageously exhibited, resulting in a nonwoven fabric exhibiting excellent collection efficiency. When the lower limit of the range of the average single fiber diameter is 0.10 μm or more, preferably 0.15 μm or more, more preferably 0.20 μm or more, the nonwoven fabric is easier to handle during processing and easier to mold. On the other hand, when the upper limit of the range of the average single fiber diameter is 10.00 μm or less, preferably 5.00 μm or less, more preferably 1.00 μm or less, the specific surface area of the fibers is increased, resulting in a nonwoven fabric with higher collection efficiency.
[0030] The average single fiber diameter of the nonwoven fabric referred to here refers to a value obtained by measurement and calculation according to the following method. (1) Randomly cut 2 cm x 2 cm test pieces from the nonwoven fabric. (2) Using a scanning electron microscope (SEM, for example, "S-5500" manufactured by Hitachi High-Technologies Corporation), the cross-sections of the fibers constituting the nonwoven fabric are observed under a microscope, and the diameters of 100 constituent fibers are measured. If the fiber cross-section is not circular but has an irregular shape, the cross-sectional area is measured, and the diameter of a perfect circle having the same cross-sectional area is determined, which is taken as the fiber diameter. (3) Round off the arithmetic mean value (μm) of the diameter obtained in the above measurement to two decimal places.
[0031] Next, the minimum single fiber diameter of the fibers is 0.01 μm or more and 1.00 μm or less. When the minimum single fiber diameter is in this range, a nonwoven fabric having a very dense microspace is formed, and the specific surface area effect of the extremely fine fibers can be advantageously exhibited, resulting in a nonwoven fabric exhibiting excellent collection efficiency. When the lower limit of the range of the minimum single fiber diameter is 0.01 μm or more, preferably 0.05 μm or more, more preferably 0.10 μm or more, the nonwoven fabric is easier to handle during processing and easier to mold. On the other hand, when the upper limit of the range of the minimum single fiber diameter is 1.00 μm or less, preferably 0.90 μm or less, more preferably 0.80 μm or less, the specific surface area of the fibers is increased, resulting in a nonwoven fabric with higher collection efficiency.
[0032] The minimum single fiber diameter of the nonwoven fabric referred to here refers to a value obtained by measurement and calculation according to the following method. (1) Randomly cut 2 cm x 2 cm test pieces from the nonwoven fabric. (2) Using a scanning electron microscope (SEM, for example, "S-5500" manufactured by Hitachi High-Technologies Corporation), the cross-sections of the fibers constituting the nonwoven fabric are observed under a microscope, and the diameters of 100 constituent fibers are measured. If the fiber cross-section is not circular but has an irregular shape, the cross-sectional area is measured, and the diameter of a perfect circle having the same cross-sectional area is determined, which is taken as the fiber diameter. (3) Round off the minimum diameter value (μm) obtained in the above measurement to two decimal places.
[0033] The maximum single fiber diameter of the fibers is 2.00 μm or more and 20.00 μm or less. When the maximum single fiber diameter is in this range, the nonwoven fabric has flexibility and strength that are easy to mold. When the lower limit of the maximum fiber diameter is 2.00 μm or more, preferably 3.00 μm or more, and more preferably 4.00 μm or more, the nonwoven fabric has strength and good handleability. On the other hand, when the upper limit of the range of the maximum single fiber diameter is 20.00 μm or less, preferably 18.00 μm or less, and more preferably 16.00 μm or less, the nonwoven fabric has good moldability.
[0034] The maximum single fiber diameter of the nonwoven fabric referred to here refers to a value obtained by measurement and calculation according to the following method. (1) Randomly cut 2 cm x 2 cm test pieces from the nonwoven fabric. (2) Using a scanning electron microscope (SEM, for example, "S-5500" manufactured by Hitachi High-Technologies Corporation), the cross-sections of the fibers constituting the nonwoven fabric are observed under a microscope, and the diameters of 100 constituent fibers are measured. If the fiber cross-section is not circular but has an irregular shape, the cross-sectional area is measured, and the diameter of a perfect circle having the same cross-sectional area is determined, which is taken as the fiber diameter. (3) Round off the maximum diameter (μm) obtained in the above measurement to two decimal places.
[0035] The cross section of the fibers constituting the nonwoven fabric of the present invention may be not only circular but also irregular as described above, and examples of irregular cross sections include elliptical, flat, Y-shaped, triangular, polygonal, cross, hollow, etc. Also, the fibers may be composite fibers, and examples thereof include core-sheath composite fibers and side-by-side composite fibers. In the case of core-sheath composite fibers, for example, the sheath portion is a low-melting point component, and it is useful to increase the strength of the nonwoven fabric by thermal bonding. In the case of using side-by-side composite fibers, for example, if they are composed of components with different shrinkage properties, they will develop crimps by heat treatment, and the void structure of the nonwoven fabric can be controlled.
[0036] [Nonwoven fabric] The nonwoven fabric of the present invention is made of the above-mentioned fibers. The arithmetic mean height Sa of the surface on either side of the nonwoven fabric is 20 μm or more and 500 μm or less, and the sum of the area of the convex portions and the area of the concave portions on either side of the nonwoven fabric is 1.10 times or more and 5.00 times or less the horizontal projected area of the surface. By satisfying these two conditions simultaneously, the nonwoven fabric has a large surface area while suppressing overlapping of adjacent nonwoven fabrics after pleating, and has low pressure loss when a fluid passes through it.
[0037] First, the nonwoven fabric of the present invention has an arithmetic mean height Sa of 20 μm or more and 500 μm or less on both sides of the surface. When the arithmetic mean height Sa of both sides of the nonwoven fabric is within the range, the nonwoven fabric has good handling properties as a filter medium. In addition, the filter medium is generally pleated when incorporated into a filter unit, and when the arithmetic mean height Sa of both sides of the nonwoven fabric is within the above range, the filter medium overlaps with each other during pleating, resulting in a nonwoven fabric with a surface area that is effective as a filter medium that is not easily reduced. When the lower limit of the range of the arithmetic mean height Sa is 20 μm or more, preferably 30 μm or more, more preferably 40 μm or more, the nonwoven fabric has a large surface area, a low pressure loss, and is easy to increase the surface area of the filter medium. On the other hand, by setting the upper limit of the range of the arithmetic mean height Sa to 500 μm or less, preferably 400 μm or less, and more preferably 350 μm or less, a nonwoven fabric can be obtained in which, after the nonwoven fabrics are laminated and pleated, appropriate gaps can be provided between the nonwoven fabrics in the laminate.
[0038] The arithmetic mean height Sa of the nonwoven fabric referred to here refers to the arithmetic mean height Sa measured based on ISO 25178-2:2012 "Geometric product specification (GPS)-Surface texture-Part 2: Terms, definitions and surface texture parameters." The arithmetic mean height Sa in the present invention refers to a value obtained by measurement and calculation according to the following method. (1) Using a 3D microscope (such as Keyence Corporation's "VR-3050"), capture a height image of the nonwoven fabric surface at a magnification of 12x so that the entire image captures the surface of the nonwoven fabric. At this time, five locations on the nonwoven fabric surface are randomly selected for imaging. (2) Calculate the absolute value of the height from the reference plane for each pixel (x, y) of the captured image, |T(x, y)|. (3) Round off the arithmetic mean value (μm) of |T(x,y)| for all pixels to the nearest integer.
[0039] Furthermore, in order to set the arithmetic mean height Sa of the surface on either side of the nonwoven fabric to be within the above range, this can be achieved, for example, by adjusting the shrinkage rate of the heat-shrinkable fabric or the temperature during the shrinkage treatment, or the elongation rate of the elastic fabric, used when processing the nonwoven fabric surface into irregularities as described below.
[0040] Next, the nonwoven fabric of the present invention has a surface area of convex parts and a surface area of concave parts that is 1.10 times or more and 5.00 times or less than the horizontal projected area of the surface on either side of the surface.The sum of the surface area of convex parts and the surface area of concave parts is within the range of magnification relative to the horizontal projected area of the surface, so that the surface area of the nonwoven fabric is increased, and when used as a filter material, the effect of reducing the pressure loss during fluid passage is fully exerted, while the adjacent nonwoven fabrics can be prevented from overlapping each other due to pleats during pleating processing in filter production, resulting in a nonwoven fabric with excellent processability.The lower limit of the range of the sum of the surface area of convex parts and the surface area of concave parts is 1.10 times or more, preferably 1.15 times or more, more preferably 1.20 times or more on either side of the surface, resulting in a nonwoven fabric with low pressure loss. On the other hand, when the upper limit of the range of the sum of the area of the convex portions and the area of the concave portions on either surface is 5.00 times or less, preferably 4.80 times or less, and more preferably 4.60 times or less, a nonwoven fabric with good processability into a filter can be obtained.
[0041] The convex area, concave area and horizontal projection area referred to here refer to values obtained by measurement and calculation according to the following methods. (1) Using a 3D microscope (such as Keyence Corporation's "VR-3050"), capture a height image of the nonwoven fabric surface at a magnification of 12x so that the entire image captures the surface of the nonwoven fabric. At this time, five locations on the nonwoven fabric surface are randomly selected for imaging. (2) Using the software installed in the 3D microscope, a plane is estimated from the shape of the height image using the least squares method to set a reference plane, and the areas of the convex and concave portions are measured. (3) The area of the photographed region is considered to be the horizontal projection area. (4) Divide the sum of the measured convex and concave areas by the value of the horizontal projection area, and round off to the third decimal place. Furthermore, in order to set the sum of the areas of the convex portions and the concave portions on any surface of the nonwoven fabric to fall within the above-mentioned range, this can be achieved, for example, by adjusting the shrinkage rate of the heat-shrinkable fabric or the temperature during the shrinkage treatment, or the elongation rate of the elastic fabric, used when processing the nonwoven fabric surface into concaves and convexes, as described below.
[0042] The nonwoven fabric of the present invention preferably has an average pore size of 0.1 μm or more and 9.9 μm or less. By having the average pore size in this range, the nonwoven fabric has fine spaces, is excellent in collecting fine dust, and has permeability for fluids such as gas and liquid, has high collection efficiency, and has low pressure loss when the fluid passes through. As the average pore size becomes smaller, the pressure loss increases extremely, but by setting the lower limit of the average pore size to 0.1 μm or more, preferably 0.2 μm or more, and more preferably 0.3 μm or more, a stable fluid flow is ensured, and a nonwoven fabric with low pressure loss is obtained. On the other hand, by setting the upper limit of the average pore size to 9.9 μm or less, preferably 8.5 μm, and more preferably 8.0 μm, a nonwoven fabric with high collection efficiency is obtained.
[0043] The average pore size of the nonwoven fabric referred to here refers to a value obtained by measurement and calculation according to the following method. (1) Randomly cut five 3 cm x 3 cm measurement samples from the nonwoven fabric. (2) Using an automatic porous material pore size measurement system (e.g., PMI CFP-1500A), the pore size distribution is measured according to JIS K3832 (bubble point method) with a measurement sample diameter of 25 mm and a measurement liquid with a known surface tension (e.g., Galwick reagent (PMI), surface tension: 16 mN / m). (3) A WET-UP measurement is performed by applying air pressure to a nonwoven fabric that is completely immersed in the test liquid, and a DRY-UP measurement is performed by applying air pressure to a nonwoven fabric that does not contain liquid. The MEAN FLOW PORE DIAMETER obtained by automatic calculation by this measurement system is the average pore size value of the measurement sample. (4) Repeat (2) and (3) for all measurement samples, and round off the arithmetic mean value (μm) obtained to one decimal place.
[0044] The average pore size of the nonwoven fabric can be adjusted to fall within the above range by adjusting the fiber diameter and / or mixing ratio of the constituent fibers.
[0045] The nonwoven fabric of the present invention preferably has a root mean square height Sq of 50 μm or more and 700 μm or less on either side of the surface. The larger the root mean square height Sq, the greater the variation in surface height. When the root mean square height Sq of the nonwoven fabric surface is within the range, a surface unevenness with small variation is obtained, a fluid passes uniformly, and a nonwoven fabric with low pressure loss is obtained. When the upper limit of the root mean square height Sq of the surface on either side is preferably 700 μm or less, more preferably 650 μm or less, and even more preferably 600 μm or less, the unevenness of the nonwoven fabric surface is small, a fluid passes uniformly, and a nonwoven fabric with low pressure loss is obtained. On the other hand, the lower limit of the root mean square height Sq of the surface on either side of the surface is substantially 50 μm or more due to restrictions on uneven processing of the nonwoven fabric.
[0046] The root mean square height Sq referred to here refers to the root mean square height Sq measured based on ISO 25178-2:2012 "Geometric product specification (GPS)-Surface texture-Part 2: Terms, definitions and surface texture parameters." The root mean square height Sq in the present invention refers to a value obtained by measurement and calculation using the following method. (1) Using a 3D microscope (such as Keyence Corporation's VR-3050), take a height image of the nonwoven fabric surface at a magnification of 12x so that the surface of the nonwoven fabric is visible across the entire image. At this time, five locations on the nonwoven fabric surface are randomly selected for photographing. (2) Using software installed in the 3D microscope, the height T(x, y) from the reference plane for each pixel (x, y) in the image is calculated. (3) From the heights T(x, y) of all pixels, calculate the value (in μm) using the following formula using the software installed in the 3D microscope, and round off the value to the nearest integer.
[0047]
number
[0048] Here, Sq represents the root mean square height (μm) and A represents the total number of pixels.
[0049] Furthermore, in order to bring the root mean square height of any surface of the nonwoven fabric into the above-mentioned range, this can be achieved, for example, by adjusting the processing time when shrinking a heat-shrinkable fabric used in the uneven processing on the nonwoven fabric surface described below, or the time when shrinking an elastic fabric until the stretch is released and the adhesion between the elastic fabric and the nonwoven fabric is released, when shrinking an elastic fabric.
[0050] The nonwoven fabric of the present invention preferably has a thickness of 0.1 mm or more and 2.9 mm or less. When the thickness of the nonwoven fabric is within this range, the nonwoven fabric has low pressure loss when used as a filter medium, but has good handling and molding processability during nonwoven fabric processing. The lower limit of the thickness of the nonwoven fabric is preferably 0.1 mm or more, more preferably 0.2 mm or more, and even more preferably 0.3 mm or more, so that the nonwoven fabric has good handling and molding processability. On the other hand, the upper limit of the thickness of the nonwoven fabric is preferably 2.9 mm or less, more preferably 2.5 mm or less, and even more preferably 2.0 mm or less, so that the contact area between adjacent filter media is reduced after pleating, and the nonwoven fabric has a secured filtration area and suppressed pressure loss.
[0051] The thickness of the nonwoven fabric referred to here refers to a value obtained by measurement and calculation according to the following method. (1) Using a dial thickness gauge (for example, "PEACOCK Model H" manufactured by Ozaki Manufacturing Co., Ltd., measuring probe diameter 10 mm, graduation 0.01 mm, measuring force 1.8 N or less), measure the thickness of the nonwoven fabric at five random locations. (2) Round off the arithmetic mean value (mm) obtained to the third decimal place.
[0052] The basis weight of the nonwoven fabric of the present invention is not particularly limited, but from the viewpoint of handling of the nonwoven fabric, it is preferably 5 g / m 2 More than 500g / m 2 It is preferable that:
[0053] The basis weight of nonwoven fabric is measured in accordance with "6.2 Mass per unit area" of JIS L1913:2010 "General nonwoven fabric test method". In other words, three test pieces of 10 cm x 10 cm are randomly cut out from the nonwoven fabric, and the mass (g) of each piece is measured under standard conditions. The arithmetic mean of the measured values is then subtracted from the mass (g) of 1 m. 2 Mass per unit (g / m 2 ) and rounding it off to the first decimal place shall be the basis weight of the nonwoven fabric.
[0054] The nonwoven fabric of the present invention preferably has a porosity of 70.0% or more from the viewpoint of efficiently passing fluids such as gas and liquid into the microspaces. In particular, from the viewpoint of promoting dust collection in the gas, the porosity of the nonwoven fabric is more preferably 80.0% or more. The practical upper limit of the porosity of the nonwoven fabric is 99.0%.
[0055] The porosity of the nonwoven fabric referred to here refers to a value measured and calculated by the following method. (i) Fiber density (g / cm 3 ) is measured and calculated by the following method. (i-1) The fibers constituting the nonwoven fabric are randomly taken out, cut into pieces having lengths of 0.5 mm to 1.0 mm, and dried in a vacuum desiccator with a vacuum degree of 0.5 kPa or less for 12 hours or more. (i-2) Prepare a NaBr solution (when the specific gravity is 1 or more) or a mixed liquid using water as the heavy liquid and ethyl alcohol as the light liquid (when the specific gravity is 0.789 to 1.4) as the specific gravity measurement liquid, and measure the specific gravity of the fiber according to "8.17.1 Specific Gravity (Floating-Sinking Method)" of JIS L1013:2010 "Test Method for Chemical Fiber Filament Yarn". Specifically, about 8 mL of the adjusted specific gravity measurement liquid is placed in a sedimentation tube, the dried fiber is placed in, and the tube is immersed in a thermostatic bath at 20°C ± 0.1°C and left for 30 minutes. Check the floating and sinking state of the fiber, and repeat the adjustment of the specific gravity of the measurement liquid and leaving it in the thermostatic bath (for 30 minutes) until the floating-sinking equilibrium is reached, and measure the specific gravity of the measurement liquid when the floating-sinking equilibrium is reached. (i-3) The arithmetic mean value of the specific gravity measured for five fibers (g / cm 3 ) to fiber density (g / cm 3 ) (ii) The basis weight (g / m2) of the nonwoven fabric obtained by the above method 2 ), thickness (mm), fiber density (g / cm 3 ) and calculate the filling rate (%) of the nonwoven fabric using the following formula.
[0056] Filling rate (%) = {weight (g / m 2 )} / {Thickness (mm) x Fiber density (g / cm 3 )}×0.1 (iii) Using the obtained filling rate, round off the value obtained by the following formula to one decimal place.
[0057] Porosity (%)=100-Filling rate (%) [Nonwoven fabric manufacturing method] The method for producing the nonwoven fabric of the present invention preferably comprises the steps of: (a) forming a web comprised of fibers primarily composed of a thermoplastic resin; (b) adhering a heat shrinkable or stretchable fabric to one surface of the web to form a laminated web; (c) shrinking the laminated web to obtain a shrink-laminate web; (d) removing the heat shrinkable or stretchable fabric from the shrinklaminate web; Each of the above steps will be described in more detail below.
[0058] (a) forming a web In the method for producing the nonwoven fabric of the present invention, the method for forming a web composed of fibers mainly composed of a thermoplastic resin is not particularly limited. From the viewpoint of productivity, however, preferred examples include a method for obtaining a web composed of long fibers by a melt blowing method or a spunbonding method, and a method for obtaining a web composed of short fibers by a wet method or a dry method using short fibers produced by a melt spinning method or the like.
[0059] (a-1) Formation of web by melt blowing method The melt-blowing method is a method in which a yarn is formed by discharging a reduced amount from a melt-blowing nozzle having a specified hole diameter, hot air is sprayed from a certain angle against the discharge part to thin the yarn, and the thinned yarn is deposited in a collection part to form a web. In order to control the basis weight and thickness, it is possible to stack multiple webs or adjust the line speed by providing multiple discharge parts or depositing the yarn on the web multiple times.
[0060] When two or more kinds of blend polymers are used as raw materials, they may be premixed, dry blended, or separately weighed and then charged into the extruder.
[0061] When using the melt-blowing method, the melt-blowing nozzle preferably has a plurality of nozzle holes. The nozzle holes may be round, triangular, rectangular, Y-shaped, or the like. Among them, round nozzle holes are preferred because they have excellent process stability in the spinning process. In the case of the round nozzle, the diameter is preferably 0.1 mm to 1.0 mm. By setting the diameter of the nozzle to preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less, the resin distribution inside the nozzle is improved, and a uniform web can be formed.
[0062] When the melt-blowing method is used, the spinning temperature is preferably in the range of from 30° C. higher than the melting temperature of the raw material resin to 140° C. higher than the melting point of the raw material resin. By setting the spinning temperature within the above range, the viscosity of the molten resin decreases, and the fibers constituting the web can be easily thinned.
[0063] When the melt-blowing method is used, the distance from the nozzle to the collecting part is preferably 5 cm to 100 cm. By making the distance from the nozzle to the collecting part preferably 5 cm or more, more preferably 10 cm or more, and even more preferably 15 cm or more, the process stability in the spinning process is improved. In addition, by making it preferably 100 cm or less, more preferably 80 cm or less, and even more preferably 60 cm or less, the strength of the web is improved.
[0064] (a-2) Formation of a web by a wet method Next, a method for forming a web from extremely fine short fibers having an average single fiber diameter of 2 μm or less (hereinafter, sometimes simply referred to as "ultrafine short fibers") by a wet method will be described.
[0065] In this wet method, a fiber dispersion is prepared by dispersing short fibers and a particulate or fibrous binder in water, and then diluted to a certain concentration, followed by dehydration on an inclined wire or a cylinder, i.e., by papermaking to form a fiber sheet. Examples of the apparatus used for this papermaking include a cylinder papermaking machine, a Fourdrinier papermaking machine, an inclined short wire papermaking machine, or a papermaking machine that combines these. In the papermaking process, in addition to the dispersibility of the fibers in the papermaking solution, the papermaking speed, the amount of fibers, and the amount of aqueous medium are adjusted to control the accumulation of the fibers during drainage, thereby producing a fiber web that has dense pores due to ultrafine short fibers and is three-dimensionally homogeneous. Here, from the viewpoint of stably forming the web, it is preferable that the fiber length of the constituent fibers is 30 mm or less. In this way, entanglement of the fibers during stirring in water is suppressed, and fiber clumps are less likely to be formed, so that a homogeneous web can be easily obtained.
[0066] In the present invention, when forming a web from ultrafine fibers by a wet method, the raw material may be one in which the easily soluble component (sea component) is dissolved from the sea-island fiber, and the dissolved component may be used as is. Alternatively, the ultrafine fibers may be separated by filtering a dispersion of ultrafine fibers containing a decomposition product of the sea component, and the ultrafine fibers may be washed with water, freeze-dried, and then dispersed again in an aqueous medium to form a web.
[0067] In addition, a dispersant may be included as necessary for the purpose of forming a stable web by suppressing the aggregation of the ultrafine short fibers over time or by increasing the viscosity of the medium. Types of dispersants include natural polymers, synthetic polymers, organic compounds, and inorganic compounds. For example, additives that suppress the aggregation of fibers include cationic compounds, nonionic compounds, and anionic compounds. Among them, when the purpose is to improve dispersibility, it is preferable to use ionic compounds such as cationic and anionic compounds from the viewpoint of electrical repulsion in the aqueous medium.
[0068] The fiber sheet formed by the wet method is subjected to a drying and heat treatment process to remove moisture and to thermally bond the constituent fibers together with the binder in the fiber sheet, and then becomes a web. As a drying method, a method using hot air ventilation (air through) or a method of contacting with a heated rotating roll (heated calendar roll, etc.) is preferable, from the viewpoint of simultaneously drying the sheet and thermally bonding the binder.
[0069] (b) forming a laminated web Next, in this process, a heat-shrinkable fabric or an elastic fabric is bonded to one surface of the web to form a laminated web. Here, in the present invention, the heat-shrinkable fabric refers to a fabric that shrinks by 5% or more in area from its original size when heated, and the elastic fabric refers to a fabric that has elasticity such that it expands by 5% or more from its original area when tensioned and returns to its original size when tension is released. In addition, the "fabric" in the heat-shrinkable fabric and elastic fabric refers to woven fabric, knitted fabric, and nonwoven fabric.
[0070] When a heat-shrinkable fabric is used, the web is placed on the heat-shrinkable fabric and bonded with a heat-melting adhesive, a chemical adhesive, or a fastener such as a clip or a pin to form a laminated web. The heat-shrinkable fabric may be any fabric having heat shrinkability, such as a woven fabric, knitted fabric, or nonwoven fabric, and is not particularly limited. For example, a heat-shrinkable polyester fabric may be preferably used.
[0071] When using an elastic fabric, the elastic fabric is tensioned in the longitudinal and lateral directions at a given elongation rate, and fixed to a fabric fixing substrate with a heat-sealing adhesive, a chemical adhesive, or a fixing device such as a clip or a pin, and the web is placed on top of the fabric and bonded with an adhesive, a fixing device, etc., to form a laminated web. The fabric fixing substrate can be any sheet-like material such as a woven fabric, a nonwoven fabric, a wooden board, or a metal board, and it is preferable to select a material that has a shape retention force greater than the contraction force of the elastic fabric.
[0072] It is also preferable to carry out the above-mentioned (a) web forming step and (b) laminated web forming step in the same process. For example, when forming a web using a melt-blowing method, fibers can be spun and piled directly on the elastic fabric fixed to the fabric fixing base material to form a laminated web in which the web is bonded to the elastic fabric. On the other hand, when forming a web using a papermaking method, the above-mentioned heat-shrinkable fabric can be placed on a papermaking net such as an inclined wire or a cylinder net, and dehydrated by passing a papermaking solution through it from above to form a laminated web in which the web is bonded to the heat-shrinkable fabric.
[0073] (c) Obtaining a shrink-laminated web Further, in this process, the laminate web is shrunk to obtain a shrunk laminate web.
[0074] In the previous step, when a heat-shrinkable fabric is used, the heat-shrinkable fabric is shrunk by heat treatment such as a method using hot air ventilation (air through), a method using dry heat in an oven or the like, or a method of contacting the fabric with a hot rotating roll (a hot calendar roll or the like) to obtain a shrunk laminated web.
[0075] In this case, the shrinkage rate due to the heat treatment can be controlled by the material of the heat-shrinkable fabric, the heat treatment temperature, the heat treatment time, etc., and the heat treatment temperature is preferably set in a range equal to or higher than the softening temperature of the heat-shrinkable fabric and the resin constituting the fibers of the heat-shrinkable fabric and not exceeding the melting point. For example, when a heat-shrinkable polyester fabric is used as the heat-shrinkable fabric, the heat treatment temperature is preferably set to 75°C or higher and 250°C or lower, and the heat treatment time is preferably set to 1 minute or higher and 120 minutes or lower.
[0076] On the other hand, if an elastic fabric is used in the previous step, the tension applied to the elastic fabric is released, causing the contraction force of the elastic fabric to shrink the entire laminated web, thereby obtaining a shrunken laminated web.
[0077] In this case, from the viewpoint of stabilizing the uneven shape formed by shrinkage, it is preferable to hold the elastic fabric and the shrunk web for 1 minute or more before removing the fixed connection, while from the viewpoint of productivity, the upper limit of the holding time is preferably 120 minutes or less.
[0078] (d) removing the heat shrinkable or stretchable fabric from the shrinklaminate web. In this step, the heat shrinkable fabric or the stretchable fabric is removed from the shrink laminated web. Specifically, the heat shrinkable fabric or the stretchable fabric can be removed by peeling it off from the shrink laminated web. The peeling method is not particularly limited, but for example, the heat shrinkable fabric or the stretchable fabric can be removed from the shrink laminated web by fixing the heat shrinkable fabric or the stretchable fabric side of the shrink laminated web with suction or the like, inserting an edge of a knife or the like between the nonwoven fabric and the heat shrinkable fabric or the stretchable fabric, and peeling off the adhesive.
[0079] (e) Other processes Furthermore, in the method for producing a nonwoven fabric of the present invention, the nonwoven fabric can be subjected to post-processing such as antibacterial processing, antiviral processing, antifungal processing, water repellency processing, oil repellency processing, and flame retardancy processing, for example, by a dip-nip method, a pad-dry method, a spray method, a coating method, etc. Also, the nonwoven fabric can be subjected to electret processing by a method such as applying high voltage to the nonwoven fabric using a non-contact type applying electrode, spraying water, or suctioning after water penetration.
[0080] Up to this point, the preferred embodiment of the method for producing the nonwoven fabric of the present invention has been described as an embodiment in which a heat-shrinkable fabric or an elastic fabric is used to shrink the web, but the nonwoven fabric of the present invention can also be obtained by other methods.
[0081] [Filter units, air purifiers] The nonwoven fabric of the present invention is preferably used in a filter unit, because of its characteristics of achieving both low pressure loss during fluid passage and high collection efficiency. In other words, the filter unit of the present invention is preferably formed by holding a filter medium containing the nonwoven fabric by a fixing material. Here, in the present invention, the "filter medium" refers to a sheet that collects dust to be removed in a filter unit. The nonwoven fabric may be used as the filter medium as it is, or may be laminated with a fiber sheet having functionality such as antibacterial, antiviral, antifungal, water repellent, oil repellent, and flame retardant. The form of the fiber sheet is not limited to the nonwoven fabric, and may be woven, knitted, mesh, etc. In addition, the "fixing material" refers to a sheet material provided in the filter unit to stably hold the form of the filter medium.
[0082] Furthermore, the air purifier of the present invention is preferably configured to incorporate the filter unit. Here, in the present invention, the air purifier is not limited to those for home or office use, but also includes those installed in vehicles such as automobiles, trains, and airplanes, those installed in clean rooms in industries that require a clean air environment during the production of semiconductors, precision machinery, pharmaceuticals, and food, and those for industrial use such as those for dust control in factories and workshops, and the air purifier of the present invention can be used for a wide range of applications. EXAMPLES
[0083] The present invention will now be described in detail with reference to examples, although the present invention is not limited to these examples.
[0084] [Measurement method] The evaluation methods and measurement conditions used in the examples are described below. Unless otherwise specified, the measurements of each physical property were performed according to the above-mentioned methods.
[0085] (1) Average single fiber diameter (μm), minimum single fiber diameter (μm), and maximum single fiber diameter (μm) The scanning electron microscope used was an "S-5500" manufactured by Hitachi High-Technologies Corporation, and measurements and calculations were carried out according to the above-mentioned methods.
[0086] (2) Arithmetic mean height Sa (μm) and root mean square height Sq (μm) The 3D microscope used was a "VR-3050" manufactured by Keyence Corporation, and measurements and calculations were performed using the above-mentioned methods.
[0087] (3) Convex area, concave area and horizontal projection area of the nonwoven fabric surface The 3D microscope used was a "VR-3050" manufactured by Keyence Corporation, and measurements and calculations were performed using the above-mentioned methods.
[0088] (4) Average pore size of nonwoven fabric (μm) The porous material automatic pore size measurement system used was the "CFP-1500A" manufactured by PMI, and the measurement liquid with known surface tension was Galwick reagent (manufactured by PMI, surface tension: 16 mN / m), and measurements and calculations were performed using the above-mentioned method.
[0089] (5) Thickness of nonwoven fabric (mm) The thickness of the nonwoven fabric was measured and calculated using a dial thickness gauge "PEACOCK Type H" (measuring probe diameter 10 mm, graduation 0.01 mm, measuring force 1.8 N or less) manufactured by Ozaki Seisakusho Co., Ltd., according to the above-mentioned method.
[0090] (6) Weight of nonwoven fabric (g / m 2 ), fiber density (g / cm 3 ), porosity of nonwoven fabric (%) The basis weight, fiber density and porosity of the nonwoven fabric were measured and calculated by the above-mentioned methods.
[0091] (7) Specific tensile strength (N m / g) The tensile strength index was determined as follows: Specific tensile strength (N·m / g) = Tensile strength (N / m) / Weight per unit area (g / m 2 ) For the measurement, five test pieces of 15mm width x 60mm length were randomly taken from the nonwoven fabric, and a tensile test was carried out using a tensile testing machine "Tensilon UCT-100" manufactured by Orientec Co., Ltd., with a chuck distance of 50mm, in accordance with JIS P8113:2006 "Paper and paperboard - Test methods for tensile properties - Part 2: Constant speed extension method", to measure the tensile strength of the nonwoven fabric. This operation was repeated five times, and the arithmetic mean value of the obtained results, rounded to two decimal places, was determined as the tensile strength of the nonwoven fabric, and the value divided by the basis weight of the nonwoven fabric was determined as the specific tensile strength.
[0092] (8) Collection efficiency of nonwoven fabric (%) To measure the collection efficiency, the nonwoven fabric was placed on a sheet with an effective opening area of 0.01 m. 2 The holder was set to 10,000 static neutralizing polystyrene particles with an average particle size of 0.3 μm per 2.83 × 10 -4 m 3 (0.01ft 3 )~40,000 pieces / 2.83×10 -4 m 3 (0.01ft 3 ) was passed vertically at a surface velocity of 3.3 m / min, and the number of dust particles with a particle size of 0.3 μm was measured upstream and downstream of the nonwoven fabric using a particle counter (KC-01D, manufactured by Rion Co., Ltd.). The collection efficiency was calculated using the following formula: Collection efficiency (%) = 100-{number of particles downstream (pieces) / number of particles upstream (pieces)} x 100 Three samples were used for the measurement, and one randomly selected location was collected for each sample to calculate the collection efficiency. The average value was rounded off to two decimal places to obtain the collection efficiency (%).
[0093] (9) Pressure loss of nonwoven fabric (Pa) When measuring the pressure loss, the nonwoven fabric was placed on a sheet with an effective opening area of 0.01 m 2The filter was placed in a holder and air was passed vertically from the upstream side to the downstream side of the nonwoven fabric at a surface velocity of 3.3 m / min. The pressure difference between the upstream and downstream sides of the filter was measured using a differential pressure gauge "Manostar Gauge WO81 (500 Pa scale)" manufactured by Yamamoto Electric Works, Ltd. Measurements were taken at three randomly selected locations from one sample, and the arithmetic average value was rounded off to the nearest decimal place to obtain the pressure loss (Pa).
[0094] (10) Performance index (QF value (Pa -1 )) The QF value, which is an index of filtration performance, was calculated using the above collection efficiency and pressure loss according to the following formula: QF value (Pa -1 ) = -ln[{1 - collection efficiency (%) / 100} / pressure loss (Pa)] The lower the pressure loss and the higher the collection efficiency, the higher the QF value, indicating better filtration performance.
[0095] [Example 1] (Process of forming web, process of forming laminated web) In the following manner, long fibers produced by a melt spinning method were cut into short fibers, and a web made of the short fibers (hereinafter referred to as a short fiber web) was formed by a wet method (papermaking method) to form a laminated web.
[0096] (1) Preparation of ultrafine fiber dispersion A sea-island composite fiber (number of islands per fiber: 2000, sea / island ratio: 50 / 50, island diameter: 0.20μm) in which the island component is polyethylene terephthalate (PET) and the sea component is polyethylene terephthalate copolymerized with 8.0mol% of 5-sodium sulfoisophthalic acid and 10mass% of polyethylene glycol with a molecular weight of 1000 (referred to as Co-PET) was cut to a fiber length of 0.6mm. The sea-island fiber was treated with a 1mass% aqueous sodium hydroxide solution (bath ratio 1 / 100) heated to 90℃ to obtain an ultrafine fiber dispersion.
[0097] (2) Preparation of PET short fiber dispersion Next, cut fibers (core component fiber diameter 10 μm, fiber length 5.0 mm, hereafter referred to as binder staple fibers) of heat-fusible core-sheath composite fibers (core component: PET, sheath component: polyester with a melting point of 110°C copolymerized at a ratio of 60 mol% terephthalic acid, 40 mol% isophthalic acid, 85 mol% ethylene glycol, and 15 mol% diethylene glycol (referred to as Co-PES in Tables 1 to 3)) and cut fibers of PET (fiber diameter 3 μm, fiber length 3.0 mm, hereafter referred to as PET staple fibers) were weighed out based on the mixing ratio of each fiber set in (3) Formation of wet nonwoven fabric, and the necessary weights were prepared by uniformly mixing and dispersing them with water to prepare a PET staple fiber dispersion.
[0098] (3) Formation of short fiber webs and laminated webs by papermaking The ultrafine fiber dispersion and the PET short fiber dispersion were homogeneously mixed so that the mixture ratio of dispersed fibers was 7.5% by mass for ultrafine fibers, 30.0% by mass for binder short fibers, and 62.5% by mass for PET short fibers, to prepare a papermaking stock solution. This papermaking stock solution was formed on a heat-shrinkable polyester fabric (area shrinkage rate of 30% after heat treatment at 110°C for 30 minutes, indicated as PES fabric A in Tables 1 and 2) placed on a papermaking net using a square sheet machine (250 mm square) manufactured by Kumagai Riki Kogyo Co., Ltd., to form a laminated web in which the heat-shrinkable polyester fabric was bonded to one surface of the short fiber web.
[0099] (Process for obtaining a shrink laminated web) The obtained laminated web was placed in a fan oven and heat-treated at 110° C. for 1 hour to obtain a shrunk laminated web.
[0100] (Step of Removing Heat Shrinkable or Stretchable Fabric from Shrink-Laminated Web) Next, the shrunk polyester fabric was removed from the obtained shrink laminated web to obtain a nonwoven fabric (short fiber nonwoven fabric). The results are shown in Table 1. The obtained nonwoven fabric had fine irregularities on all surfaces. In addition, the filter performance of the obtained nonwoven fabric was evaluated, and the Qf value was 0.040, indicating excellent filter performance.
[0101] [Examples 2 and 3] In (1) Preparation of ultrafine fiber dispersion in (Step of forming a web, Step of forming a laminated web), sea-island composite fibers having 2000 islands per fiber and an island diameter of 0.20 μm were used, but were changed to sea-island composite fibers having an island diameter of 0.15 μm (Example 2) and sea-island composite fibers having 1000 islands per fiber and an island diameter of 0.60 μm (Example 3). Nonwoven fabrics were obtained in the same manner as in Example 1. The evaluation results of the obtained nonwoven fabrics are shown in Table 1.
[0102] The nonwoven fabric of Example 2 had fine irregularities formed on all surfaces, and when its filtering performance was evaluated, it exhibited an excellent filtering performance with a Qf value of 0.047.
[0103] The nonwoven fabric of Example 3 had fine irregularities formed on all surfaces, and when its filtering performance was evaluated, it exhibited an excellent filtering performance with a Qf value of 0.040.
[0104] [Examples 4 and 5] In (2) (Process of forming a web, process of forming a laminated web) preparation of PET short fiber dispersion, binder short fibers having a fiber diameter of 10 μm were used as the core component, but were changed to binder short fibers having a fiber diameter of 3 μm (Example 4) and binder short fibers having a fiber diameter of 20 μm (Example 5), and other than that, nonwoven fabrics were obtained in the same manner as in Example 1. The evaluation results of the obtained nonwoven fabrics are shown in Table 1.
[0105] The nonwoven fabric of Example 4 had fine irregularities formed on all surfaces, and when its filtering performance was evaluated, it exhibited an excellent filtering performance with a Qf value of 0.040.
[0106] The nonwoven fabric of Example 5 had fine irregularities formed on all surfaces, and when its filtering performance was evaluated, it exhibited an excellent filtering performance with a Qf value of 0.040.
[0107] [Examples 6, 7 and 8] In (3) (process of forming a web, process of forming a laminated web) of forming a staple fiber web and forming a laminated web by a papermaking method, a heat-shrinkable polyester fabric (area shrinkage rate of 30% after heat treatment at 110°C for 30 minutes, PES fabric A) was used, and further, in (process of obtaining a shrunk laminated web), the obtained laminated web was placed in a ventilated oven and heat-treated at 110°C for 1 hour. However, the heat-shrinkable polyester fabric was changed to one with an area shrinkage rate of 15% after heat treatment at 110°C for 30 minutes (referred to as PES fabric B in Table 2) and the heat treatment was changed to 110°C for 30 minutes (0.5 hours) (Example 6), the heat-shrinkable polyester fabric was not changed, but the heat treatment was changed to 180°C for 1 hour in a ventilated oven (Example 7), and the heat-shrinkable polyester fabric was not changed, but the heat treatment was changed to 170°C for 1 hour in a ventilated oven (Example 8). The evaluation results of the obtained nonwoven fabric are shown in Table 2.
[0108] The nonwoven fabric of Example 6 had unevenness formed on all surfaces, and when its filtering performance was evaluated, it had a Qf value of 0.030, which was sufficient filtering performance.
[0109] The nonwoven fabric of Example 7 had fine projections and recesses densely formed on all surfaces, and the Qf value evaluated for filter performance was 0.030, which showed sufficient filter performance.
[0110] The nonwoven fabric of Example 8 had fine projections and recesses densely formed on all surfaces, and the Qf value evaluated for filter performance was 0.035, indicating good filter performance.
[0111] [Example 9] In (3) Formation of the short fiber web by the papermaking method and formation of the laminated web in (the process of forming the web and the process of forming the laminated web), the mixture ratios of the dispersed fibers were changed from 7.5% by mass of ultrafine fibers, 30.0% by mass of binder short fibers, and 62.5% by mass of PET short fibers to 10.0% by mass of ultrafine fibers, 30.0% by mass of binder short fibers, and 60.0% by mass of PET short fibers, respectively. A nonwoven fabric was obtained in the same manner as in Example 1. The evaluation results of the obtained nonwoven fabric are shown in Table 2.
[0112] The nonwoven fabric of Example 9 had fine irregularities formed on all surfaces, and when its filtering performance was evaluated, it exhibited an excellent filtering performance with a Qf value of 0.048.
[0113] [Comparative Example 1] A nonwoven fabric was obtained in the same manner as in Example 1, except that the step of obtaining a shrunk laminated web was not carried out. The evaluation results of the obtained nonwoven fabric are shown in Table 3.
[0114] The nonwoven fabric of Comparative Example 1 was smooth with no irregularities observed on any of its surfaces, and when its filtering performance was evaluated, the Qf value was 0.027, which was an insufficient filtering performance.
[0115] [Comparative Example 2] In (3) Formation of the short fiber web and formation of the laminated web by the papermaking method (step of forming a web, step of forming a laminated web), the mixture ratios of the dispersed fibers were changed from 7.5% by mass of ultrafine fibers, 30.0% by mass of binder short fibers, and 62.5% by mass of PET short fibers to 90.0% by mass of binder short fibers and 10.0% by mass of PET short fibers, respectively, to obtain a nonwoven fabric in the same manner as in Example 1. The evaluation results of the obtained nonwoven fabric are shown in Table 3.
[0116] The nonwoven fabric of Comparative Example 2 had rough irregularities on all surfaces, but when the filter performance was evaluated, the Qf value was 0.010, which indicated that the filter performance was insufficient.
[0117] [Comparative Example 3] In the step of obtaining a shrunk laminated web, the obtained laminated web was heat-treated in a ventilated oven at 110° C. for 1 hour, but this was changed to a heat treatment in a ventilated oven at 190° C. for 1 hour. A nonwoven fabric was obtained in the same manner as in Example 1. The evaluation results of the obtained nonwoven fabric are shown in Table 3.
[0118] The nonwoven fabric of Comparative Example 3 shrank significantly and had densely formed fine irregularities on all surfaces. However, when the filtering performance was evaluated, the Qf value was 0.024, which was an insufficient filtering performance.
[0119] [Table 1]
[0120] [Table 2]
[0121] [Table 3]
[0122] [Example 10] (Process of forming web, process of forming laminated web) A web made of long fibers produced by a melt-blowing method (hereinafter referred to as a long-fiber web) was formed, and a laminated web was formed by the following method.
[0123] (1) Formation of long fiber web and layered web Polypropylene (PP) was melted in an extruder and fed to a gear pump. The PP resin measured by the gear pump was fed to a die with 0.12 mm diameter discharge holes arranged in a straight line, and spun by the melt-blowing method under the conditions of a single hole discharge rate of 0.05 g / min, a die temperature of 280°C, and a hot air pressure of 0.16 MPa. A stretchable polyester knitted fabric (referred to as PES knitted fabric C in Table 4) was sewn and fixed to a polyester woven fabric in a stretched state so that the area was 1.3 times the original area. The sheet was placed on a conveyor installed 20 cm below the discharge holes, and the yarn was collected on the sheet to produce a sheet in which the long fiber web, stretchable polyester knitted fabric, and polyester woven fabric were integrated.
[0124] (Process for obtaining a shrink laminated web) The knitted fabric and the woven fabric were released from the obtained integral sheet of the long fiber web, stretchable polyester knitted fabric, and polyester woven fabric, and the long fiber web and the stretchable polyester knitted fabric were allowed to shrink.
[0125] (Step of Removing Heat Shrinkable or Stretchable Fabric from Shrink-Laminated Web) After 30 minutes, the contracted stretchable polyester knit was removed from the filament web to obtain a nonwoven fabric (meltblown nonwoven fabric). The results are shown in Table 4. The nonwoven fabric had fine irregularities on all surfaces. The filter performance of the nonwoven fabric was evaluated, and the Qf value was 0.040, indicating excellent filter performance.
[0126] [Example 11] (1) In the formation of the long fiber web and the laminated web, PP resin measured by a gear pump was supplied to a die having nozzles with a diameter of 0.12 mm arranged in a straight line, and discharged at a single-hole discharge rate of 0.05 g / min. However, the diameter of the nozzle hole was changed to 0.40 mm, and the single-hole discharge rate was changed to 0.10 g / min. A nonwoven fabric was obtained in the same manner as in Example 10. The evaluation results of the obtained nonwoven fabric are shown in Table 4.
[0127] The nonwoven fabric of Example 11 had fine irregularities formed on all surfaces, and when its filtering performance was evaluated, it exhibited an excellent filtering performance with a Qf value of 0.040.
[0128] [Example 12] (1) In the formation of the long fiber web and the laminated web, the single-hole discharge rate was changed from 0.05 g / min to 0.02 g / min, but a nonwoven fabric was obtained in the same manner as in Example 10. The evaluation results of the obtained nonwoven fabric are shown in Table 4.
[0129] The nonwoven fabric of Example 12 had fine irregularities formed on all surfaces, and when its filtering performance was evaluated, it exhibited an excellent filtering performance with a Qf value of 0.040.
[0130] [Example 13] (1) In the formation of the long fiber web and the laminated web, the stretchable polyester knitted fabric was sewn onto the polyester woven fabric in a stretched state so that it had an area 1.3 times larger than the original area, but instead the stretchable polyester knitted fabric was fixed in a stretched state so that it had an area 1.1 times larger than the original area. A nonwoven fabric was obtained in the same manner as in Example 10. The evaluation results of the obtained nonwoven fabric are shown in Table 4.
[0131] The nonwoven fabric of Example 13 had unevenness formed on all surfaces, and when its filtering performance was evaluated, it exhibited a Qf value of 0.031, which was sufficient filtering performance.
[0132] [Comparative Example 4] (1) In the formation of the long fiber web and the laminated web, the stretchable polyester knitted fabric was sewn onto the polyester woven fabric in a stretched state to form a sheet with an area 1.3 times that of the original, but the stretchable polyester knitted fabric was fixed as it was (area magnification: 1.0 times), and other than this, a nonwoven fabric was obtained in the same manner as in Example 10. The evaluation results of the obtained nonwoven fabric are shown in Table 4.
[0133] The nonwoven fabric of Comparative Example 4 was smooth with no irregularities observed on any of its surfaces, and when its filtering performance was evaluated, the Qf value was 0.023, which was an insufficient filtering performance.
[0134] [Table 4]
Claims
1. A nonwoven fabric made of fibers mainly composed of thermoplastic resin, The average single fiber diameter of the fibers is 0.10 μm or more and 10.00 μm or less, The minimum single fiber diameter of the fiber is 0.01 μm or more and 1.00 μm or less, The maximum single fiber diameter of the fiber is 2.00 μm or more and 20.00 μm or less, The nonwoven fabric has an arithmetic mean height Sa of 20 μm or more and 500 μm or less on either surface thereof, On either side of the surface of the nonwoven fabric, the sum of the area of the convex portions and the area of the concave portions on the surface is 1.10 times or more and 5.00 times or less the horizontal projected area of the surface. Nonwoven fabric.
2. 2. The nonwoven fabric according to claim 1, wherein the average pore size of the nonwoven fabric is 0.1 μm or more and 9.9 μm or less.
3. 3. The nonwoven fabric according to claim 1, wherein the root mean square height Sq of the surface on either side of the nonwoven fabric is 50 μm or more and 700 μm or less.
4. 3. The nonwoven fabric according to claim 1, wherein the thickness of the nonwoven fabric is 0.1 mm or more and 2.9 mm or less.
5. A filter unit comprising a filter medium comprising the nonwoven fabric according to claim 1 or 2 and held by a fixing material.
6. An air purifier incorporating the filter unit according to claim 5.
7. forming a web composed of fibers mainly composed of a thermoplastic resin; adhering a heat shrinkable or stretchable fabric to one surface of the web to form a laminated web; shrinking the laminated web to obtain a shrink laminated web; removing the heat shrinkable or stretchable fabric from said shrinklaminate web; The method for producing the nonwoven fabric according to claim 1 or 2,
8. The method for producing a nonwoven fabric according to claim 7 , wherein the step of forming the web and the step of forming the laminated web are carried out in a single step.
Citation Information
Patent Citations
Conjugate fiber nonwoven fabric and composite nonwoven fabric
JP2004003065A
Filter medium for filter and filter
JP2005319347A
Blended filament nonwoven fabric
JP2013040412A