Multilayer structure, packaging material, and vacuum insulation body

A resin composition with specific unsaturated aldehydes and a conjugated polyene compound in EVOH suppresses neck-in and die build-up, addressing issues of uneven thickness and heat-sealing strength in EVOH films, resulting in improved multilayer structures for packaging and vacuum insulation.

JP2024141539AActive Publication Date: 2024-10-10KURARAY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023053256
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Ethylene-vinyl alcohol copolymer (EVOH) resin compositions used in melt molding face issues such as neck-in, die build-up, and uneven thickness leading to poor gas barrier properties and reduced heat-sealing strength due to oxidation and crosslinking reactions, particularly when used in T-die film formation and heat-sealing layers.

Method used

A resin composition containing EVOH with specific ratios of crotonaldehyde, 2,4-hexadienal, and 2,4,6-octatrienal, along with a conjugated polyene compound, is used to form a sealant layer that suppresses neck-in and die build-up, ensuring uniform gas barrier properties and improved heat-sealing strength.

Benefits of technology

The solution provides a multilayer structure with high uniformity and enhanced heat-sealing strength, reducing defects like bumps and streaks, and maintaining gas barrier properties, suitable for packaging materials and vacuum insulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141539000001
    Figure 2024141539000001
  • Figure 2024141539000002
    Figure 2024141539000002
  • Figure 2024141539000003
    Figure 2024141539000003
Patent Text Reader

Abstract

To provide: a multilayer structure increased in the uniformity of a gas barrier property of a sealant layer (α) and improved in the heat seal strength and in the appearance after heat sealing; and a packaging material and a vacuum insulation body that are based on the same.SOLUTION: The multilayer structure comprises a sealant layer (α) comprising a resin composition, and a base material layer (β) comprising a thermoplastic resin having a melting point higher than or equal to 190°C. The sealant layer (α) is the topmost layer. The resin composition comprises: EVOH (A) having an ethylene unit content from 20 mol% to 60 mol% inclusive; crotonaldehyde (B1); and at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3). The resin composition satisfies the formula (1), 2.0≤b1 / (b2+b3)<150.0, and the formula (2), b2+2b3≤0.65.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multi-layer structure, a packaging material, and a vacuum insulator. [Background technology]

[0002] Ethylene-vinyl alcohol copolymer (hereinafter sometimes abbreviated as "EVOH") is excellent in transparency, gas barrier properties, aroma retention, solvent resistance, oil resistance, heat sealability, etc., and by utilizing these properties, it is sometimes used as a heat seal film for food packaging materials, industrial chemical packaging materials, agricultural chemical packaging materials, pharmaceutical packaging materials, vacuum insulators, etc. Such heat seal films are molded into packaging bags and other containers such as bottles. Melt molding is generally used in many cases for molding films. Therefore, a resin composition to be subjected to melt molding is required to have excellent long-run performance, such as no defects such as fish eyes and streaks even after long-term melt molding.

[0003] However, since EVOH has relatively active hydroxyl groups in the molecule, oxidation and crosslinking reactions may proceed in a high-temperature molten state even inside an extrusion molding machine where there is almost no oxygen, and heat degradation products may be generated. In particular, when operated continuously for a long period of time, the above heat degradation products accumulate inside the molding machine, generating gels and particles that cause fish eyes, and the EVOH resin composition may have insufficient long-term run properties.

[0004] In contrast, Patent Document 1 describes that a resin composition containing EVOH and 0.01 to 100 ppm of an unsaturated aldehyde suppresses the occurrence of defects such as fish eyes, gels, and streaks, and has excellent long-run properties. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2013 / 146961 Summary of the Invention [Problem to be solved by the invention]

[0006] It was found that, when the EVOH resin composition of Patent Document 1 is used, neck-in, in which the width of the extruded film is smaller than the effective width of the die, may be a problem in film molding using a T-die. It was also found that the EVOH resin composition prone to such neck-in tends to have uneven gas barrier properties in each part, probably because the thickness of the formed layer in the width direction is likely to be uneven. As a result of intensive research by the present inventors, it was surprisingly found that an EVOH resin composition containing specific types of unsaturated aldehydes in a specific ratio can suppress such neck-in. However, when the content of the multiple types of unsaturated aldehydes is adjusted in an attempt to suppress neck-in, it was found that a new problem occurs in that die build-up (meaning deposits on the outer surface of the die lip) is likely to adhere to the outer surface of the discharge port (die lip) of the molten resin composition, depending on the ratio of the multiple types of unsaturated aldehydes.

[0007] On the other hand, when an EVOH layer is used as a heat seal layer, the EVOH layer has a large area of ​​contact with the die lip, so that when the EVOH layer is co-extruded as the outermost layer of a multilayer structure, or when it is a single-layer film consisting of only an EVOH layer, die build-up can become a significant problem. It has been found that films obtained using EVOH resin compositions prone to die build-up are prone to develop bumps and streaks due to die build-up, which tends to reduce the heat seal strength.

[0008] The present invention has been made under these circumstances, and an object of the present invention is to provide a multilayer structure which has a sealant layer (α) formed using a resin composition which contains EVOH and which is suppressed in necking-in and die build-up during melt molding, and which has high uniformity in the gas barrier properties of the sealant layer (α) and which has improved heat seal strength and appearance after heat sealing, as well as a packaging material and a vacuum insulator which use the same. [Means for solving the problem]

[0009] The above objectives are: [1] A multilayer structure comprising a sealant layer (α) made of a resin composition and a substrate layer (β) containing a thermoplastic resin having a melting point of 190°C or higher, the sealant layer (α) being an outermost layer, the resin composition containing an ethylene-vinyl alcohol copolymer (A) having an ethylene unit content of 20 mol% or more and 60 mol% or less (hereinafter sometimes abbreviated as "EVOH (A)") and crotonaldehyde (B1), and further containing at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3), and the resin composition satisfies the following formulas (1) and (2): 2.0≦b1 / (b2+b3)<150.0 (1) b2+2b3≦0.65 (2) In the above formulas (1) and (2), b1 is the content (ppm) of crotonaldehyde (B1) relative to EVOH (A), b2 is the content (ppm) of 2,4-hexadienal (B2) relative to EVOH (A), and b3 is the content (ppm) of 2,4,6-octatrienal (B3) relative to EVOH (A). [2] The multilayer structure of [1], wherein in the resin composition, the total content (b1+b2+b3) of crotonaldehyde (B1), 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) relative to the EVOH (A) is 0.01 ppm or more and 7.0 ppm or less; [3] The multilayer structure of [1] or [2], wherein in the resin composition, the content b1 of crotonaldehyde (B1) is 0.01 ppm or more and 4.0 ppm or less; [4] The multilayer structure of [1] to [3], wherein in the resin composition, the content b2 of 2,4-hexadienal (B2) is 0.005 ppm or more and 0.65 ppm or less; [5] The multilayer structure of [1] to [4], wherein in the resin composition, the content b3 of 2,4,6-octatrienal (B3) is 0.325 ppm or less; [6] The multilayer structure according to any one of [1] to [5], wherein the resin composition further contains a conjugated polyene compound (C), and the content c of the conjugated polyene compound (C) relative to the EVOH (A) in the resin composition is 1 ppm or more and less than 300 ppm; [7] The multilayer structure of [6], wherein the conjugated polyene compound (C) is sorbic acid; [8] The multilayer structure of [1] to [7], in which a sealant layer (α) and a base layer (β) are laminated via an adhesive layer (γ); [9] The multilayer structure of any one of [1] to [8], which has a multilayer film in which a sealant layer (α), an adhesive layer (γ), and a base layer (β) are directly laminated in this order;

[10] A multilayer structure according to any one of [1] to [9], wherein the EVOH (A) contains EVOH (Aa) and EVOH (Ab), the melting point difference (Aa-Ab) between the EVOH (Aa) and the EVOH (Ab) is 8°C or more, and the mass ratio (Aa / Ab) between the EVOH (Aa) and the EVOH (Ab) is 60 / 40 or more and 95 / 5 or less;

[11] The multilayer structure according to any one of [1] to

[10] , wherein at least a part of the EVOH (A) has at least one structural unit selected from the group consisting of a structural unit represented by the following formula (I) and a structural unit represented by the following formula (II), in an amount of 0.3 mol % to 40 mol % based on the total vinyl alcohol units of the at least a part of the EVOH (A); [ka] [In the above formula (I), R 1 , R 2 and R 3 R each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, or a hydroxyl group.1 , R 2 and R 3 One pair of R 1 , R 2 and R 3 (Except when one pair of these are both hydrogen atoms.) Some or all of the hydrogen atoms in the aliphatic hydrocarbon group having 1 to 10 carbon atoms, the alicyclic hydrocarbon group having 3 to 10 carbon atoms, and the aromatic hydrocarbon group having 6 to 10 carbon atoms may be substituted with a hydroxyl group, an alkoxy group, a carboxyl group, or a halogen atom. In the above formula (II), R 4 , R 5 , R 6 and R 7 R each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, or a hydroxyl group. 4 and R 5 Or R 6 and R 7 may be bonded (provided that R 4 and R 5 Toga or R 6 and R 7 (Except when both are hydrogen atoms.) Some or all of the hydrogen atoms in the aliphatic hydrocarbon group having 1 to 10 carbon atoms, the alicyclic hydrocarbon group having 3 to 10 carbon atoms, and the aromatic hydrocarbon group having 6 to 10 carbon atoms may be substituted with a hydroxyl group, an alkoxy group, a carboxyl group, or a halogen atom.]

[12] The multilayer structure of [1] to

[11] , further comprising a layer (δ) containing a thermoplastic resin having a melting point of less than 190°C;

[13] A multilayer structure according to [1] to

[12] , in which the heat seal strength measured in accordance with JIS Z1707 (2019) when the sealant layers (α) of the multilayer structure are pressed together for 1 second using a hot plate heat sealer at a temperature of 200°C and a pressure of 0.1 MPa is 20 N / 15 mm or more;

[14] [1]~

[13] comprising a multilayer structure;

[15] [1]-

[14] include multilayer structures of vacuum insulators;

[16] The adsorption amount of synthetic pyrethroids in the sealant layer (α) is 10ng / cm2 [1]~

[15] multilayer structures that are less than

[17] The nicotine adsorption capacity of the sealant layer (α) is 1000ng / cm 2 [1]~

[16] multilayer structures that are less than This is achieved by providing Effect of the Invention

[0010] According to the present invention, there can be provided a multilayer structure having a sealant layer (α) formed using a resin composition that contains EVOH and is suppressed in necking-in and die build-up during melt molding, the sealant layer (α) having high uniformity in the gas barrier properties and improved heat seal strength and appearance after heat sealing, as well as a packaging material and a vacuum insulator using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In the present specification, the term "surface (or surface layer)" in a multilayer structure does not mean to distinguish between the front and back, but refers to the exposed surface. In other words, a multilayer structure has two surfaces. Similarly, a multilayer structure has two outermost layers.

[0012] The multilayer structure of the present invention comprises a sealant layer (α) made of a specific resin composition and a substrate layer (β) containing a thermoplastic resin having a melting point of 190° C. or higher. The multilayer structure may comprise an adhesive layer (γ), a thermoplastic resin layer (δ) and other layers in addition to the above-mentioned layers. Each layer will be described below.

[0013] [Sealant layer (α)] The sealant layer (α) is a layer made of a predetermined resin composition, which will be described in detail below.

[0014] (Resin composition) The resin composition contains EVOH (A) and crotonaldehyde (B1), and further contains at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3), and satisfies the following formulas (1) and (2). 2.0≦b1 / (b2+b3)<150.0 (1) b2+2b3≦0.65 (2) In the above formulas (1) and (2), b1 is the content (ppm) of crotonaldehyde (B1) relative to EVOH (A), b2 is the content (ppm) of 2,4-hexadienal (B2) relative to EVOH (A), and b3 is the content (ppm) of 2,4,6-octatrienal (B3) relative to EVOH (A). Note that in this specification, the content expressed in ppm is the content based on mass.

[0015] When the value of b1 / (b2+b3) is 2.0 or more and less than 150.0, the neck-in resistance is good, and the thickness unevenness of the obtained sealant layer (α) is reduced. Therefore, the uniformity of the gas barrier property of the sealant layer (α) is increased, and as a result, the uniformity of the gas barrier property of the multilayer structure tends to be increased. On the other hand, 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) affect the die build-up, and in particular, 2,4,6-octatrienal (B3) has a large effect on the die build-up. Therefore, when the value of b2+2b3 is 0.65 ppm or less, the die build-up is suppressed, and the heat seal strength of the obtained multilayer structure is increased. As a result, the multilayer structure can show a good appearance even after heat sealing. Furthermore, the resin composition is unlikely to cause bumps, streaks, etc. even when repeatedly melt-molded. Therefore, the multilayer structure obtained by using the resin composition is also excellent in recyclability. In this specification, crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3) may be collectively referred to as unsaturated aliphatic aldehyde (B).

[0016] (EVOH(A)) EVOH (A) is a copolymer having ethylene units and vinyl alcohol units, and the ethylene unit content is 20 mol% or more and 60 mol% or less. EVOH (A) is usually obtained by saponification of an ethylene-vinyl ester copolymer. The production and saponification of the ethylene-vinyl ester copolymer can be carried out by a known method. Examples of vinyl esters include vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, vinyl versatate, and other aliphatic carboxylic acid vinyl esters, and vinyl acetate is preferred.

[0017] The ethylene unit content of EVOH (A) is 20 mol% or more, preferably 25 mol% or more, and more preferably 27 mol% or more. The ethylene unit content of EVOH (A) is 60 mol% or less, preferably 55 mol% or less, and more preferably 50 mol% or less. If the ethylene unit content is less than 20 mol%, the thermal stability during melt extrusion decreases, gelation becomes more likely, and streaks, fish eyes, bumps, etc. tend to occur. The occurrence of streaks, fish eyes, bumps, etc. becomes more noticeable when operating for a long time at a higher temperature or higher speed than usual conditions. If the ethylene unit content exceeds 60 mol%, the gas barrier property tends to decrease.

[0018] The saponification degree of EVOH (A) is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 99 mol% or more. When the saponification degree of EVOH (A) is 90 mol% or more, the resulting sealant layer (α) and multilayer structure tend to have good gas barrier properties, heat stability, moisture resistance, etc. The saponification degree may be 100 mol% or less, 99.97 mol% or less, or 99.94 mol% or less.

[0019] In addition, EVOH (A) may have other structural units other than ethylene units, vinyl alcohol units and vinyl ester units, as long as the object of the present invention is not hindered. When EVOH (A) has the other structural units, the content of the other structural units relative to the total structural units of EVOH (A) is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, even more preferably 5 mol% or less, and sometimes particularly preferably 1 mol% or less. In addition, when EVOH (A) has the other structural units, the content may be 0.05 mol% or more, or 0.10 mol% or more. Examples of the other structural units include structural units derived from unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, etc., or their anhydrides, salts, or mono- or dialkyl esters; nitriles such as acrylonitrile, methacrylonitrile, etc.; amides such as acrylamide, methacrylamide, etc.; olefin sulfonic acids such as vinyl sulfonic acid, allyl sulfonic acid, methallylsulfonic acid, etc., or their salts; vinyl silane compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxy-ethoxy)silane, γ-methacryloxypropylmethoxysilane, etc.; alkyl vinyl ethers, vinyl ketones, N-vinylpyrrolidone, vinyl chloride, vinylidene chloride, etc.

[0020] The other structural unit may be at least one of a structural unit (I) represented by the following formula (I), a structural unit (II) represented by the following formula (II), and a structural unit (III) represented by the following formula (III).

[0021] [ka]

[0022] In formula (I), formula (II) and formula (III), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R9 , R 10 and R 11 each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, or a hydroxyl group. 1 , R 2 and R 3 One pair of R 4 and R 5 , R 6 and R 7 may be bonded to form a part of a ring structure. Some or all of the hydrogen atoms in the aliphatic hydrocarbon group having 1 to 10 carbon atoms, the alicyclic hydrocarbon group having 3 to 10 carbon atoms, and the aromatic hydrocarbon group having 6 to 10 carbon atoms may be substituted with a hydroxyl group, an alkoxy group, a carboxyl group, or a halogen atom. In formula (III), R 12 and R 13 each independently represents a hydrogen atom, a formyl group, or an alkanoyl group having 2 to 10 carbon atoms.

[0023] When EVOH (A) has the above structural unit (I), (II) or (III), the flexibility and processability of the resin composition tend to be improved, and the stretchability, thermoformability and the like tend to be good.

[0024] In the structural unit (I), (II) or (III), examples of the aliphatic hydrocarbon group having 1 to 10 carbon atoms include an alkyl group, an alkenyl group, etc., examples of the alicyclic hydrocarbon group having 3 to 10 carbon atoms include a cycloalkyl group, a cycloalkenyl group, etc., and examples of the aromatic hydrocarbon group having 6 to 10 carbon atoms include a phenyl group, etc.

[0025] In the structural unit (I), the R 1 , R 2 and R 3 are preferably each independently a hydrogen atom, a methyl group, an ethyl group, a hydroxyl group, a hydroxymethyl group, or a hydroxyethyl group. Among these, from the viewpoint of further improving the moldability and the like of the resin composition, are more preferably each independently a hydrogen atom, a methyl group, a hydroxyl group, or a hydroxymethyl group.

[0026] The method for incorporating the structural unit (I) in EVOH (A) is not particularly limited, and examples thereof include a method of copolymerizing a monomer derived from the structural unit (I) in the polymerization of ethylene and a vinyl ester. Examples of monomers derived from the structural unit (I) include alkenes such as propylene, butylene, pentene, and hexene; 3-hydroxy-1-propene, 3-acyloxy-1-propene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, 3,4-diacyloxy-1-butene, 3-acyloxy-4-hydroxy-1-butene, 4-acyloxy-3-hydroxy-1-butene, 3-acyloxy-4-methyl-1-butene, 4-acyloxy-2-methyl-1-butene, 4-acyloxy-3-methyl-1-butene, 3,4-diacyloxy-2-methyl-1-butene, 4-hydroxy-1-pentene, 5-hydroxy-1-pentene, 4 Examples of alkenes having a hydroxyl group or an ester group include alkenes having a hydroxyl group or an ester group, such as 5-dihydroxy-1-pentene, 4-acyloxy-1-pentene, 5-acyloxy-1-pentene, 4,5-diacyloxy-1-pentene, 4-hydroxy-3-methyl-1-pentene, 5-hydroxy-3-methyl-1-pentene, 4,5-dihydroxy-3-methyl-1-pentene, 5,6-dihydroxy-1-hexene, 4-hydroxy-1-hexene, 5-hydroxy-1-hexene, 6-hydroxy-1-hexene, 4-acyloxy-1-hexene, 5-acyloxy-1-hexene, 6-acyloxy-1-hexene, and 5,6-diacyloxy-1-hexene. Among them, from the viewpoints of copolymerization reactivity, and processability and gas barrier properties of the resulting sealant layer (α) and multilayer structure, propylene, 3-acyloxy-1-propene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, and 3,4-diacyloxy-1-butene are preferred. Note that "acyloxy" is preferably acetoxy, and specifically, 3-acetoxy-1-propene, 3-acetoxy-1-butene, 4-acetoxy-1-butene, and 3,4-diacetoxy-1-butene are preferred. In the case of an alkene having an ester, it is derived into the above structural unit (I) during the saponification reaction.

[0027] In the above structural unit (II), R 4 and R 5 Preferably, both are hydrogen atoms. 4 and R 5 are both hydrogen atoms, and the above R 6 and R 7 It is more preferable that one of R is an aliphatic hydrocarbon group having 1 to 10 carbon atoms, and the other is a hydrogen atom. The aliphatic hydrocarbon group is preferably an alkyl group or an alkenyl group. From the viewpoint of placing special importance on the gas barrier property of the resulting sealant layer (α) and the multilayer structure, R 6 and R 7 It is more preferable that one of the R 6 and R 7 One of them is (CH2) h It is more preferable that the other of the substituents represented by OH (wherein h is an integer of 1 to 8) is a hydrogen atom. (CH2) h In the substituent represented by OH, h is preferably an integer of 1 to 4, more preferably 1 or 2, and even more preferably 1.

[0028] The method for incorporating the structural unit (II) in EVOH (A) is not particularly limited, and for example, a method of incorporating the structural unit (II) by reacting a monofunctional epoxy compound with EVOH (A) obtained by saponification reaction is used. As the monofunctional epoxy compound, the compounds represented by the following formulae (IV) to (X) are preferably used.

[0029] [ka]

[0030] In the above formulas (IV) to (X), R 14 , R 15 , R 16 , R 17 and R 18each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms (such as an alkyl group or an alkenyl group), an alicyclic hydrocarbon group having 3 to 10 carbon atoms (such as a cycloalkyl group or a cycloalkenyl group), or an aliphatic hydrocarbon group having 6 to 10 carbon atoms (such as a phenyl group). Also, i, j, k, p, and q each independently represent an integer of 1 to 8. However, R 17 is a hydrogen atom, R 18 is a group other than a hydrogen atom.

[0031] Examples of the monofunctional epoxy compound represented by the above formula (IV) include epoxyethane (ethylene oxide), epoxypropane, 1,2-epoxybutane, 2,3-epoxybutane, 3-methyl-1,2-epoxybutane, 1,2-epoxypentane, 3-methyl-1,2-epoxypentane, 1,2-epoxyhexane, 2,3-epoxyhexane, 3,4-epoxyhexane, 3-methyl-1,2-epoxyhexane, 3-methyl-1,2-epoxyheptane, 4-methyl-1,2-epoxyheptane, 1,2-epoxyoctane, 2,3-epoxyoctane, 1,2-epoxynonane, 2,3-epoxynonane, 1,2-epoxydecane, 1,2-epoxydodecane, epoxyethylbenzene, 1-phenyl-1,2-epoxypropane, 3-phenyl-1,2-epoxypropane, etc. Examples of the monofunctional epoxy compound represented by the above formula (V) include various alkyl glycidyl ethers, etc. Examples of the monofunctional epoxy compound represented by the above formula (VI) include various alkylene glycol monoglycidyl ethers. Examples of the monofunctional epoxy compound represented by the above formula (VII) include various alkenyl glycidyl ethers. Examples of the monofunctional epoxy compound represented by the above formula (VIII) include various epoxy alkanols such as glycidol. Examples of the monofunctional epoxy compound represented by the above formula (IX) include various epoxy cycloalkanes. Examples of the monofunctional epoxy compound represented by the above formula (X) include various epoxy cycloalkenes.

[0032] Among the monofunctional epoxy compounds, an epoxy compound having 2 to 8 carbon atoms is preferred. In particular, from the viewpoint of ease of handling of the compound and reactivity, the monofunctional epoxy compound has more preferably 2 to 6 carbon atoms, and further preferably 2 to 4 carbon atoms. In addition, it is particularly preferred that the monofunctional epoxy compound is a compound represented by the above formula (IV) or formula (V). Specifically, from the viewpoint of reactivity with EVOH (A), processability of the resin composition and the resulting sealant layer (α) and multilayer structure, gas barrier properties, etc., 1,2-epoxybutane, 2,3-epoxybutane, epoxypropane, epoxyethane, or glycidol is preferred, and among these, epoxypropane or glycidol is more preferred.

[0033] In the structural unit (III), R 8 , R 9 , R 10 and R 11 is preferably a hydrogen atom or an aliphatic hydrocarbon group having 1 to 5 carbon atoms, and such an aliphatic hydrocarbon group is preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group or an n-pentyl group.

[0034] The method for incorporating the structural unit (III) in EVOH (A) is not particularly limited, and examples thereof include the method described in JP-A-2014-034647.

[0035] The lower limit of the melting point of EVOH (A) is preferably 140°C, more preferably 150°C, and even more preferably 160°C. On the other hand, the upper limit of the melting point is preferably 220°C, more preferably 210°C, and even more preferably 200°C. When the melting point of EVOH (A) is within the above range, the melt moldability is improved, and neck-in and die build-up during melt molding tend to be further suppressed. The melting point of EVOH (A) can be a value measured by the method described in the Examples.

[0036] The EVOH (A) may be used alone or in combination of two or more kinds.

[0037] EVOH (A) may contain two types of EVOH (Aa) and EVOH (Ab) having different melting points. For example, when the melting point of the resin composition is measured by the method described in the examples, peak temperatures corresponding to each EVOH may be confirmed. Furthermore, the resin composition may have a phase-separated structure in which one EVOH is dispersed in the other EVOH, or the two types of EVOH may be completely compatible. EVOH (Aa) and EVOH (Ab) may be two types of EVOH having different ethylene unit contents.

[0038] When EVOH (A) contains two kinds of EVOH (Aa) and EVOH (Ab) having different melting points, the lower limit of the difference in melting points between EVOH (Aa) and EVOH (Ab) (Aa-Ab), i.e., the melting point of EVOH (Aa) minus the melting point of EVOH (Ab), may be, for example, 5°C, but is preferably 8°C. If this melting point difference is 8°C or more, moldability and the like are improved. The lower limit of this melting point difference is more preferably 12°C, more preferably 16°C, even more preferably 20°C, and even more preferably 24°C. The lower limit of this melting point difference may further be 30°C, 40°C, 50°C, or 60°C. The upper limit of the difference in melting points between EVOH (Aa) and EVOH (Ab) may be, for example, 100°C, but is preferably 90°C, and in some cases, 80°C, 70°C, 60°C, 50°C, 40°C, or 30°C may be more preferably. By setting the melting point difference to the lower limit or more, it is possible to improve the moldability, heat stretchability, etc. of the resin composition. Conversely, by setting the melting point difference to the upper limit or less, it is possible to improve the gas barrier property and the effect of suppressing flow marks during long runs (long-term continuous operation) of the resin composition.

[0039] The lower limit of the melting point of EVOH (Aa) is preferably 150° C., more preferably 160° C., and even more preferably 170° C. On the other hand, the upper limit of the melting point is preferably 220° C., more preferably 210° C., and even more preferably 200° C. When the melting point of EVOH (Aa) is within the above range, melt moldability is improved, and neck-in and die build-up during melt molding tend to be further suppressed.

[0040] The lower limit of the ethylene unit content of EVOH (Aa) is preferably 20 mol%, more preferably 23 mol%, and even more preferably 25 mol%. On the other hand, the upper limit of the ethylene unit content of EVOH (Aa) is preferably 50 mol%, more preferably 47 mol%, and even more preferably 43 mol%, 40 mol%, or 35 mol%. By making the ethylene unit content of EVOH (Aa) equal to or higher than the above lower limit, the effects of moldability, flexibility, etc. of the resin composition and the sealant layer (α) obtained therefrom can be sufficiently exhibited. On the other hand, by making the ethylene unit content of EVOH (Aa) equal to or lower than the above upper limit, the gas barrier properties of the resin composition, and the sealant layer (α) and multilayer structure obtained therefrom can be improved.

[0041] The saponification degree of EVOH (Aa) is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 99 mol% or more. When the saponification degree of EVOH (Aa) is 90 mol% or more, the resin composition and the sealant layer (α) and multilayer structure obtained from the resin composition tend to have good gas barrier properties, thermal stability, moisture resistance, etc. Also, the saponification degree of EVOH (Aa) may be 100 mol% or less, 99.97 mol% or less, or 99.94 mol% or less.

[0042] The lower limit of the melting point of EVOH (Ab) is preferably 90° C., more preferably 100° C., and in some cases, more preferably 110° C., 120° C., 130° C., 140° C., or 150° C. On the other hand, the upper limit of the melting point is preferably 220° C., more preferably 210° C., and more preferably 200° C., and in some cases, even more preferably 190° C., 180° C., or 170° C. When the melting point of EVOH (Ab) is within the above range, the melt moldability is improved, and neck-in and die build-up during melt molding tend to be further suppressed.

[0043] The lower limit of the ethylene unit content of EVOH (Ab) is preferably 30 mol%, more preferably 34 mol%, and even more preferably 38 mol%. On the other hand, the upper limit of the ethylene unit content of EVOH (Ab) is preferably 60 mol%, more preferably 55 mol%, and even more preferably 52 mol%. By making the ethylene unit content of EVOH (Ab) equal to or higher than the above lower limit, the effects of moldability, flexibility, etc. of the resin composition and the resulting sealant layer (α) can be sufficiently exhibited. On the other hand, by making the ethylene unit content of EVOH (Ab) equal to or lower than the above upper limit, the gas barrier properties of the resin composition and the resulting sealant layer (α) can be improved.

[0044] The suitable degree of saponification of EVOH (Ab) may be the same as that of EVOH (Aa).

[0045] The lower limit of the difference (Ab-Aa) in the ethylene unit content between EVOH (Ab) and EVOH (Aa), i.e., the value obtained by subtracting the ethylene unit content of EVOH (Aa) from the ethylene unit content of EVOH (Ab), is preferably 4.5 mol%, more preferably 8 mol%, even more preferably 12 mol%, and even more preferably 15 mol%. The upper limit of the difference (Ab-Aa) in the ethylene unit content is preferably 40 mol%, more preferably 30 mol%, and even more preferably 20 mol%. By making the difference in the ethylene unit content between EVOH (Ab) and EVOH (Ab) equal to or greater than the lower limit, the moldability, heat stretchability, etc. of the resin composition and the resulting sealant layer (α) can be improved. Conversely, by making the difference in the ethylene unit content equal to or less than the upper limit, the gas barrier properties of the resin composition can be improved.

[0046] The mass ratio (Aa / Ab) between EVOH (Aa) and EVOH (Ab), i.e., the mass ratio of the content of EVOH (Aa) to the content of EVOH (Ab), may be preferably 60 / 40, more preferably 62 / 38, and even more preferably 65 / 35, 68 / 32, 70 / 30, or 75 / 25. The upper limit of the mass ratio may be preferably 95 / 5, more preferably 93 / 7, more preferably 92 / 8, even more preferably 91 / 9, and even more preferably 85 / 15. When the mass ratio is within the above range, the moldability, flexibility, etc. of the resin composition and the sealant layer (α) obtained are excellent while maintaining the gas barrier properties against various gases. For example, by setting the mass ratio (Aa / Ab) to the above lower limit or more, the gas barrier properties and oil resistance, etc. of the resin composition and the sealant layer (α) obtained can be improved. On the other hand, by setting the mass ratio (Aa / Ab) to the above upper limit or less, the moldability, flexibility, etc. of the resin composition and the resulting sealant layer (α) can be improved.

[0047] From the viewpoint of improving moldability, flexibility, etc. of the resin composition and the resulting sealant layer (α), etc., at least a part of EVOH (A) preferably has at least one structural unit (x) selected from the group consisting of the structural unit represented by the above formula (I) and the structural unit represented by the following formula (II). Of these, it is preferable that EVOH (Ab) has the structural unit (x).

[0048] The lower limit of the content of the structural unit (x) relative to the total vinyl alcohol structural units in the EVOH having the structural unit (x) which is at least a part of the EVOH (A) is preferably 0.3 mol%, more preferably 1 mol%, and even more preferably 3 mol%. By making the content of the structural unit (x) equal to or higher than the lower limit, the moldability, flexibility, etc. of the resin composition and the resulting sealant layer (α) can be sufficiently improved. On the other hand, the upper limit of this content is preferably 40 mol%, more preferably 30 mol%, and even more preferably 20 mol%. By making the content of the structural unit (x) equal to or lower than the upper limit, the gas barrier property, etc. can be improved.

[0049] The content of EVOH (A) in the resin composition is preferably 70% by mass or more, more preferably 80% by mass or more, particularly preferably 90% by mass or more, and may be 95% by mass or more, 99% by mass or more, or 99.9% by mass or more, from the viewpoint of gas barrier properties, etc. The resin constituting the resin composition may be substantially composed of only EVOH (A). On the other hand, the content of EVOH (A) in the resin composition may be, for example, 99.9% by mass or less, or 99% by mass or less.

[0050] (Unsaturated aliphatic aldehyde (B)) The resin composition contains crotonaldehyde (B1), and further contains at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3).

[0051] The lower limit of the content b1 of crotonaldehyde (B1) relative to EVOH (A) in the resin composition is preferably 0.01 ppm, more preferably 0.20 ppm, even more preferably 0.40 ppm, and even more preferably 0.70 ppm or 1.20 ppm. On the other hand, the upper limit of the content b1 is preferably 4.0 ppm, more preferably 3.5 ppm, even more preferably 2.7 ppm, and even more preferably 2.0 ppm or 1.5 ppm. When the content b1 is within the above range, it is easy to adjust the values ​​of b1 / (b2+b3), b1+b2+b3, and b2+2b3 described below to suitable ranges. In addition, when the content b1 is within the above range, coloring tends to be suppressed.

[0052] In one embodiment, the resin composition contains 2,4-hexadienal (B2) at a specific ratio relative to crotonaldehyde (B1), and thus tends to suppress die build-up while exhibiting excellent neck-in resistance. The lower limit of the content b2 of 2,4-hexadienal (B2) relative to EVOH (A) in the resin composition is preferably 0.005 ppm, more preferably 0.01 ppm, and even more preferably 0.02 ppm. On the other hand, the upper limit of the content b2 is preferably 0.65 ppm, more preferably 0.20 ppm, more preferably 0.10 ppm, even more preferably 0.08 ppm, and particularly preferably 0.06 ppm. When the content b2 is within the above range, it is easy to adjust the values ​​of b1 / (b2+b3), b1+b2+b3, and b2+2b3 described below to suitable ranges. In addition, when the content b2 is within the above range, coloring tends to be suppressed.

[0053] In one embodiment, the resin composition contains 2,4,6-octatrienal (B3) at a specific ratio relative to crotonaldehyde (B1), and thus tends to suppress die build-up while exhibiting excellent neck-in resistance. Compared with 2,4-hexadienal (B2), 2,4,6-octatrienal (B3) has a greater effect on die build-up relative to the amount added. Therefore, from the viewpoint of suppressing die build-up while improving neck-in resistance, the resin composition preferably contains 2,4-hexadienal (B2) rather than 2,4,6-octatrienal (B3). The upper limit of the content b3 of 2,4,6-octatrienal (B3) relative to EVOH (A) in the resin composition is preferably 0.325 ppm, more preferably 0.23 ppm, even more preferably 0.07 ppm, and particularly preferably 0.04 ppm. The lower limit of the content B3 may be 0 ppm or 0.005 ppm. When the content b3 is in the above range, the values ​​of b1 / (b2+b3), b1+b2+b3, and b2+2b3 described below can be easily adjusted to a suitable range. In addition, when the content b3 is in the above range, coloring tends to be suppressed.

[0054] In the resin composition, the ratio (b1 / (b2+b3)) of the sum of the content b2 (ppm) of 2,4-hexadienal (B2) and the content b3 (ppm) of 2,4,6-octatrienal (B3) to the content b1 (ppm) of crotonaldehyde (B1) is 2.0 or more and less than 150.0, so that the resin composition has excellent neck-in resistance. Such neck-in resistance is an effect that is not seen when any of the unsaturated aliphatic aldehydes (B) is used alone, and is an effect that is only achieved when b1 / (b2+b3) is in a specific range. The lower limit of b1 / (b2+b3) is preferably 4.0, more preferably 8.0. On the other hand, the upper limit of b1 / (b2+b3) is preferably 60.0, more preferably 25.0, and even more preferably 13.0. By setting b1 / (b2+b3) within the above range, neck-in can be more sufficiently suppressed, and as a result, the uniformity of the thickness of the obtained sealant layer (α) is improved, thereby making it possible to increase the uniformity of the gas barrier property and the heat seal strength of the sealant layer (α) and the multilayer structure.

[0055] In the resin composition, the upper limit of the sum (b2+2b3) of the content b2 (ppm) of 2,4-hexadienal (B2) and twice the content b3 (ppm) of 2,4,6-octatrienal (B3) is 0.65 ppm or less, preferably 0.50 ppm, more preferably 0.30 ppm, and even more preferably 0.10 ppm. When b2+2b3 exceeds the upper limit, the occurrence of die build-up cannot be suppressed. When die build-up occurs, the occurrence of streaks and the like due to die build-up in the resulting sealant layer (α) causes a decrease in heat seal strength and a decrease in gas barrier properties in the multilayer structure. b2+2b3 may be 0.005 ppm or more, or may be 0.01 ppm or more.

[0056] In the resin composition, the upper limit of the total content (b1+b2+b3) of crotonaldehyde (B1), 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) relative to EVOH (A) is preferably 7.0 ppm, more preferably 4.0 ppm, even more preferably 3.5 ppm, even more preferably 3.0 ppm, even more preferably 1.5 ppm, and in some cases, particularly preferably 1.0 ppm. By making b1+b2+b3 equal to or less than the upper limit, coloration of the resin composition can be sufficiently suppressed. On the other hand, the lower limit of b1+b2+b3 is preferably 0.01 ppm, more preferably 0.10 ppm, and even more preferably 0.30 ppm or 0.50 ppm.

[0057] (Conjugated polyene compound (C)) The resin composition preferably further contains a conjugated polyene compound (C). The conjugated polyene compound (C) can suppress the deterioration of color tone due to the oxidative deterioration of the EVOH (A) during melt molding. Here, the conjugated polyene compound (C) is a compound having a structure in which carbon-carbon double bonds and carbon-carbon single bonds are alternately connected and the number of carbon-carbon double bonds is two or more, that is, a compound having a so-called conjugated double bond. However, 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) are not considered to be conjugated polyene compounds (C). The conjugated polyene compound (C) may be a conjugated diene having two conjugated double bonds, a conjugated triene having three conjugated double bonds, or a conjugated polyene having more than two conjugated double bonds. In addition, the structure of the conjugated double bond may have multiple sets in one molecule. For example, a compound having three conjugated triene structures in the same molecule, such as tung oil, is also included in the conjugated polyene compound (C). The upper limit of the number of conjugated double bonds in the conjugated polyene compound (C) is preferably 7. If the resin composition contains a conjugated polyene compound (C) having 8 or more conjugated double bonds, the possibility of coloring of the pellets and thus the molded product increases.

[0058] The conjugated polyene compound (C) may have, in addition to the conjugated double bond, other functional groups such as a carboxy group and a salt thereof, a hydroxyl group, an ester group, an ether group, an amino group, an imino group, an amide group, a cyano group, a diazo group, a nitro group, a sulfone group and a salt thereof, a sulfonyl group, a sulfoxide group, a sulfide group, a thiol group, a phosphate group and a salt thereof, a phenyl group, a halogen atom, a double bond, or a triple bond.

[0059] The lower limit of the carbon number of the conjugated polyene compound (C) is preferably 4. The upper limit of the carbon number of the conjugated polyene compound (C) is preferably 30, and more preferably 10.

[0060] Examples of the conjugated polyene compound (C) include isoprene, 2,3-dimethyl-1,3-butadiene, 2,3-diethyl-1,3-butadiene, 2-t-butyl-1,3-butadiene, 1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2,4-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-pentadiene, and 3-ethyl-1,3-pentadiene. , 2-methyl-1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 2,5-dimethyl-2,4-hexadiene, 1,3-octadiene, 1,3-cyclopentadiene, 1,3-cyclohexadiene, 1-phenyl-1,3-butadiene, 1,4-diphenyl-1,3-butadiene conjugated diene compounds such as ene, 1-methoxy-1,3-butadiene, 2-methoxy-1,3-butadiene, 1-ethoxy-1,3-butadiene, 2-ethoxy-1,3-butadiene, 2-nitro-1,3-butadiene, chloroprene, 1-chloro-1,3-butadiene, 1-bromo-1,3-butadiene, 2-bromo-1,3-butadiene, ocimene, phellandrene, myrcene, farnesene, sorbic acid, sorbic acid esters, and sorbic acid salts; conjugated triene compounds such as 1,3,5-hexatriene, 2,4,6-octatriene-1-carboxylic acid, eleostearic acid, tung oil, cholecalciferol, fulvene, and tropone; cyclooctatetraene, 2,4,6,8-decatetraene-1-carboxylic acid, retinol, and retinoic acid.

[0061] As the conjugated polyene compound (C), sorbic acid, sorbic acid esters, sorbic acid salts, myrcene or a mixture of two or more of these is preferred, and sorbic acid, sorbic acid salts (sodium sorbate, potassium sorbate, etc.) or a mixture of these is more preferred. Sorbic acid, sorbic acid salts or a mixture of these are highly effective in inhibiting oxidative deterioration at high temperatures and are also widely used industrially as food additives, and are therefore preferred from the standpoints of hygiene and availability.

[0062] The molecular weight of the conjugated polyene compound (C) is usually 1,000 or less, preferably 500 or less, more preferably 300 or less. When the molecular weight of the conjugated polyene compound (C) is the above upper limit or less, the dispersion state of the conjugated polyene compound (C) in the resin composition becomes good, and the appearance after melt molding tends to be improved. The lower limit of the molecular weight of the conjugated polyene compound (C) is, for example, 54, and may be 60 or 80.

[0063] The lower limit of the content c of the conjugated polyene compound (C) relative to the EVOH (A) in the resin composition is preferably 1 ppm, more preferably 3 ppm. The content c of the conjugated polyene compound (C) relative to the EVOH (A) in the resin composition is preferably less than 300 ppm, more preferably 100 ppm or less, even more preferably 70 ppm or less, even more preferably 30 ppm or less, and in some cases, particularly preferably 20 ppm or less, 10 ppm or less. When the content c of the conjugated polyene compound (C) is within the above range, the deterioration of the color during melt molding tends to be more suppressed.

[0064] (Other optional ingredients) The resin composition may contain, as optional components other than EVOH (A), unsaturated aliphatic aldehyde (B), and conjugated polyene compound (C), boron compounds, carboxylic acids, phosphorus compounds, metal ions, antioxidants, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, heat stabilizers, other resins other than EVOH (A), metal salts of higher aliphatic carboxylic acids, etc. The resin composition may contain two or more of these components. When the resin composition contains other optional components, the upper limit of the total content is preferably 1 mass%, and in some cases 0.5 mass% is preferable.

[0065] The boron compound suppresses gelation during melt molding and also suppresses torque fluctuations (viscosity changes during heating) in an extrusion molding machine or the like. Examples of the boron compound include boric acids such as orthoboric acid, metaboric acid, and tetraboric acid; boric acid esters such as triethyl borate and trimethyl borate; alkali metal salts or alkaline earth metal salts of the boric acids, borate salts such as borax; and boron hydrides. Among these, boric acids are preferred, and orthoboric acid (hereinafter also referred to as "boric acid") is more preferred. The lower limit of the content of the boron compound relative to EVOH (A) is preferably 100 ppm, more preferably 500 ppm. The upper limit of the content of the boron compound relative to EVOH (A) is preferably 5,000 ppm, more preferably 3,000 ppm, and even more preferably 1,000 ppm. By setting the content of the boron compound to the above lower limit or more, torque fluctuations in an extrusion molding machine or the like can be sufficiently suppressed. On the other hand, by setting the content of the boron compound to the above upper limit or less, gelation is less likely to occur during melt molding, and the appearance of the multilayer structure is improved. The content of the boron compound is the content of the boron compound calculated as orthoboric acid.

[0066] The carboxylic acid prevents the coloring of the sealant layer (α) and suppresses gelation during melt molding. Examples of the carboxylic acid include formic acid, acetic acid, propionic acid, butyric acid, lactic acid, and salts thereof. The carboxylic acid is preferably a carboxylic acid having 4 or less carbon atoms or a saturated carboxylic acid, and more preferably an acetic acid. The acetic acid includes acetic acid and an acetate salt. As the acetic acid, it is preferable to use acetic acid and an acetate salt in combination, and it is more preferable to use acetic acid and sodium acetate in combination. The lower limit of the content of the carboxylic acid relative to the EVOH (A) is preferably 50 ppm, more preferably 100 ppm, and even more preferably 150 ppm. The upper limit of the content of the carboxylic acid relative to the EVOH (A) is preferably 1,000 ppm, more preferably 500 ppm, and even more preferably 400 ppm. By setting the content of the carboxylic acid to be equal to or more than the above lower limit, a sufficient coloring suppression effect can be obtained, and the occurrence of yellowing can be sufficiently suppressed. On the other hand, by setting the content of carboxylic acids to the above upper limit or less, gelation is less likely to occur during melt molding, particularly during long-term melt molding, and the appearance, etc. of the multilayer structure is improved.

[0067] The phosphorus compound suppresses the occurrence of defects such as streaks and fish eyes, and coloring, and improves long-run properties. Examples of the phosphorus compound include phosphates such as phosphoric acid and phosphorous acid. The phosphate may be in the form of primary phosphate, secondary phosphate, or tertiary phosphate. The cationic species of the phosphate is not particularly limited, but is preferably an alkali metal salt or an alkaline earth metal salt, and among these, sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, and dipotassium hydrogen phosphate are more preferred, and sodium dihydrogen phosphate and dipotassium hydrogen phosphate are even more preferred. The lower limit of the content of the phosphorus compound in EVOH (A) is preferably 1 ppm, more preferably 10 ppm, even more preferably 20 ppm, and particularly preferably 30 ppm. The upper limit of the content of the phosphorus compound in EVOH (A) is preferably 200 ppm, more preferably 150 ppm, and even more preferably 100 ppm. By setting the content of the phosphorus compound to be equal to or more than the above lower limit or equal to or less than the above upper limit, the thermal stability is improved, and the generation of gel-like particles, coloration, etc. during long-term melt molding is less likely to occur.

[0068] Examples of the metal ion include monovalent metal ions, divalent metal ions, and other transition metal ions, and these may be composed of one or more kinds. Among them, monovalent metal ions and divalent metal ions are preferred. As the monovalent metal ion, an alkali metal ion is preferred, for example, an ion of lithium, sodium, potassium, rubidium, and cesium, and from the viewpoint of industrial availability, an ion of sodium or potassium is preferred. In addition, examples of the alkali metal salt that gives the alkali metal ion include an aliphatic carboxylate, an aromatic carboxylate, a carbonate, a hydrochloride, a nitrate, a sulfate, a phosphate, and a metal complex. Among them, an aliphatic carboxylate and a phosphate are preferred from the viewpoint of availability, and specifically, sodium acetate, potassium acetate, sodium phosphate, and potassium phosphate are preferred. In some cases, it is preferred to include a divalent metal ion as the metal ion. When the metal ion includes a divalent metal ion, for example, thermal deterioration of EVOH when trim is recovered and reused may be suppressed, and the occurrence of gels and bumps in the obtained molded body may be suppressed. Examples of divalent metal ions include beryllium, magnesium, calcium, strontium, barium, and zinc ions, and magnesium, calcium, or zinc ions are preferred from the viewpoint of industrial availability. Examples of divalent metal salts that provide divalent metal ions include carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, and metal complexes, and carboxylates are preferred. Examples of carboxylic acids that constitute carboxylates are carboxylic acids having 1 to 30 carbon atoms, and specific examples include acetic acid, propionic acid, butyric acid, stearic acid, lauric acid, montanic acid, behenic acid, octanoic acid, sebacic acid, ricinoleic acid, myristic acid, palmitic acid, and the like, and among these, acetic acid and stearic acid are preferred. The lower limit of the content of metal ions in EVOH (A) is preferably 1 ppm, more preferably 100 ppm, and even more preferably 150 ppm. On the other hand, the upper limit of the content of metal ions is preferably 1,000 ppm, more preferably 400 ppm, and even more preferably 350 ppm. When the content of metal ions in EVOH (A) is 1 ppm or more, the interlayer adhesion of the resulting multilayer structure tends to be good.On the other hand, if the metal ion content is 1,000 ppm or less, coloration resistance tends to be good.

[0069] Examples of the antioxidant include 2,5-di-t-butylhydroquinone, 2,6-di-t-butyl-p-cresol, 4,4'-thiobis(6-t-butylphenol), 2,2'-methylene-bis(4-methyl-6-t-butylphenol), octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, etc. Examples of the ultraviolet absorber include ethylene-2-cyano-3,3'-diphenylacrylate, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2-hydroxy-4-oxybenzophenone, etc.

[0070] Examples of the plasticizer include dimethyl phthalate, diethyl phthalate, dioctyl phthalate, wax, liquid paraffin, phosphate ester, etc. Examples of the antistatic agent include pentaerythritol monostearate, sorbitan monopalmitate, sulfated polyolefins, polyethylene oxide, polyethylene glycol (trade name: Carbowax), etc.

[0071] Examples of the lubricant include ethylene bisstearamide and butyl stearate. Examples of the colorant include carbon black, phthalocyanine, quinacridone, indoline, azo pigments, and red iron oxide. Examples of the filler include glass fiber, wollastonite, calcium silicate, talc, and montmorillonite. Examples of the heat stabilizer include hindered phenol compounds and hindered amine compounds.

[0072] Examples of the resin other than EVOH (A) include polyamide, polyolefin, etc. Examples of the metal salt of higher aliphatic carboxylic acid include sodium stearate, potassium stearate, calcium stearate, magnesium stearate, etc.

[0073] In the resin composition, the total content of EVOH (A) and unsaturated aliphatic aldehyde (B) (crotonaldehyde (B1), 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3)) is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and particularly preferably 99% by mass or more. The resin composition may be substantially composed of EVOH (A) and unsaturated aliphatic aldehyde (B), and the resin composition may be composed of EVOH (A) and unsaturated aliphatic aldehyde (B). In this specification, "consists essentially of" means that optional components can be contained within a range that does not affect the effects of the present invention, and "consists only of" means that optional components other than impurities that are inevitably contained are excluded. It is preferable that the sealant layer (α) consists only of the resin composition.

[0074] The lower limit of the melt flow rate (MFR) of the resin composition at 210°C under a load of 2,160 g is preferably 0.5 g / 10 min, more preferably 1 g / 10 min. Meanwhile, the upper limit of this MFR is preferably 30 g / 10 min, more preferably 20 g / 10 min. When the MFR of the resin composition is in the above range, melt moldability and the like can be improved. In addition, when the MFR of the resin composition is in the above range, the neck-in resistance tends to be better.

[0075] <Method for preparing resin composition> The method for producing the resin composition is not particularly limited as long as it is a method capable of blending the unsaturated aliphatic aldehyde (B) into the EVOH (A). (1) copolymerizing ethylene with a vinyl ester; and (2) A step of saponifying the copolymer obtained in the step (1) and a method for producing a resin composition comprising the steps of:

[0076] The method of including the unsaturated aliphatic aldehyde (B) in the resin composition is not particularly limited, and examples thereof include a method of adding the unsaturated aliphatic aldehyde (B) in the above step (1), a method of adding the unsaturated aliphatic aldehyde (B) in the above step (2), and a method of adding the unsaturated aliphatic aldehyde (B) to the EVOH (A) obtained by the above step (2). When adopting the method of adding the unsaturated aliphatic aldehyde (B) in the above step (1) or the method of adding the unsaturated aliphatic aldehyde (B) in the above step (2), in order to include a desired amount of the unsaturated aliphatic aldehyde (B) in the obtained resin composition, it is necessary to increase the amount of the unsaturated aliphatic aldehyde (B) to be added in consideration of the amount consumed in the polymerization reaction in the above step (1) and the saponification reaction in the above step (2). Therefore, when the unsaturated aliphatic aldehyde (B) is added in the polymerization reaction or saponification reaction step, it is preferable to add the amount of the unsaturated aliphatic aldehyde (B) consumed. On the other hand, the method of adding the unsaturated aliphatic aldehyde (B) to the EVOH (A) obtained in the above step (2) is excellent in operability since it can be added without considering consumption in the process.

[0077] Examples of the method for adding the unsaturated aliphatic aldehyde (B) to EVOH (A) include a method of blending the unsaturated aliphatic aldehyde (B) with EVOH (A) in advance and granulating the mixture into pellets, a method of impregnating the strands precipitated in a process of precipitating a paste after saponification of an ethylene-vinyl ester copolymer with the unsaturated aliphatic aldehyde (B), a method of cutting the precipitated strands and then impregnating the unsaturated aliphatic aldehyde (B), a method of adding the unsaturated aliphatic aldehyde (B) to a remelted chip of a dried resin composition, a method of melt-kneading a blend of the components EVOH (A) and the unsaturated aliphatic aldehyde (B), a method of feeding the unsaturated aliphatic aldehyde (B) into a melt of EVOH (A) midway through an extruder to incorporate the unsaturated aliphatic aldehyde (B), and a method of blending the unsaturated aliphatic aldehyde (B) at a high concentration with a part of EVOH (A) to prepare a master batch, which is granulated, dry-blended with EVOH (A), and melt-kneading the master batch.

[0078] Among these, from the viewpoint of being able to disperse a trace amount of unsaturated aliphatic aldehyde (B) in EVOH (A) with high uniformity, a method of blending the unsaturated aliphatic aldehyde (B) with EVOH (A) in advance and pelletizing the mixture is preferred. Specifically, the unsaturated aliphatic aldehyde (B) is added to a solution obtained by dissolving EVOH (A) in a good solvent such as a water / methanol mixed solvent, and the resulting mixed solution is extruded from a nozzle or the like into a poor solvent to precipitate and / or solidify, which is then washed and / or dried to obtain resin composition pellets in which the unsaturated aliphatic aldehyde (B) is mixed with EVOH (A) with high uniformity.

[0079] Examples of methods for incorporating other components other than the unsaturated aliphatic aldehyde (B) in EVOH (A) include a method of mixing the above pellets with the other components and melt-kneading them, a method of mixing the other components together with the unsaturated aliphatic aldehyde (B) when preparing the above pellets, a method of immersing the above pellets in a solution containing the other components, a method of dry-blending the above pellets with the other components, etc. For mixing the other components, a ribbon blender, a high-speed mixer co-kneader, a mixing roll, an extruder, an intensive mixer, etc. can be used.

[0080] The resin composition used for producing the sealant layer (α) is preferably in the form of pellets from the viewpoint of ease of handling. The shape of the pellets of the resin composition is not particularly limited, but may be cylindrical, prismatic, spherical, or approximately spherical (lenticular), and among them, from the viewpoint of pellet transport stability, handling, productivity, etc., cylindrical, spherical, or approximately spherical (lenticular) is preferred. In the case of a cylindrical shape, the diameter is preferably 1 mm or more and 10 mm or less, more preferably 2 mm or more and 8 mm or less, and the height is preferably 1 mm or more and 10 mm or less, more preferably 2 mm or more and 8 mm or less, and even more preferably 3 mm or more and 5 mm or less. In the case of a spherical or approximately spherical (lenticular) shape, the length in the short direction is preferably 1 mm or more and 10 mm or less, more preferably 2 mm or more and 8 mm or less, and the length in the long direction is preferably 1 mm or more and 10 mm or less, and more preferably 2 mm or more and 8 mm or less.

[0081] The average thickness of the sealant layer (α) is not particularly limited, and the lower limit may be, for example, 1 μm, 5 μm, 7 μm, or 10 μm. By making the average thickness of the sealant layer (α) equal to or greater than the above lower limit, it is possible to improve the gas barrier properties. On the other hand, the upper limit of the average thickness may be, for example, 100 μm, 70 μm, 50 μm, or 40 μm. By making the average thickness of the sealant layer (α) equal to or less than the above upper limit, the appearance characteristics tend to be good. The average thickness of the sealant layer (α) and each of the other layers is the average value of thicknesses measured at any 5 or more points, unless otherwise specified.

[0082] The upper limit of oxygen permeability of the sealant layer (α) measured under conditions of 30°C and 65% RH in accordance with ISO14663-2 annex C is 50mL 20μm / m 2 ·day·atm is preferred, 10mL·20μm / m 2 ·day·atm is more preferable, 5mL·20μm / m 2 1 mL 20 μm / m is more preferable. 2 ·day·atm is particularly preferred.

[0083] (single layer film) The sealant layer (α) can be formed, for example, as a single-layer film (substrate film) made of the resin composition. In this case, the forming method is not particularly limited, and for example, the melting method, the solution method, the calendar method, etc. are included, among which the melting method is preferred. As the melting method, the casting method and the inflation method are included, among which the casting method is preferred.

[0084] When the film is formed by the casting method, stretching may be performed. The stretching method is not particularly limited, and may be any of uniaxial stretching, simultaneous biaxial stretching, and sequential biaxial stretching. The lower limit of the stretching ratio in terms of area is preferably 8 times, more preferably 9 times. The upper limit of the stretching ratio is preferably 12 times, more preferably 11 times. By setting the stretching ratio within the above range, the uniformity of the film thickness, gas barrier properties, and mechanical strength can be improved.

[0085] When stretching, it is preferable to previously moisten the raw film (film before stretching). This makes continuous stretching easier. The lower limit of the moisture content of the raw film before stretching is preferably 2% by mass, more preferably 5% by mass, and even more preferably 10% by mass. The upper limit of the moisture content of the raw film before stretching is preferably 30% by mass, more preferably 25% by mass, and even more preferably 20% by mass.

[0086] The stretching temperature varies somewhat depending on the moisture content of the raw sheet before stretching and the stretching method, but is generally set to 50° C. or higher and 130° C. or lower. In order to obtain a biaxially stretched film with little stretching unevenness, the stretching temperature is preferably 70° C. or higher and 100° C. or lower in simultaneous biaxial stretching, and preferably 70° C. or higher and 100° C. or lower in sequential biaxial stretching for longitudinal stretching with rolls and 80° C. or higher and 120° C. or lower in width direction stretching with a tenter.

[0087] The sealant layer (α) may be one layer of a multilayer film (base film) further having other layers. As the multilayer film, for example, a multilayer film (base film) can be prepared in which the sealant layer (α), the adhesive layer (γ) described later, and the thermoplastic resin layer (δ) described later are laminated in this order. The multilayer film is not limited to the above layer structure, and may have the sealant layer (α) as one of the outermost layers and one or more other layers. However, the multilayer film preferably has a thermoplastic resin layer (δ) together with the sealant layer (α), and more preferably has an adhesive layer (γ) provided between the sealant layer (α) and the thermoplastic resin layer (δ).

[0088] The method for producing the multilayer film is not particularly limited, and examples thereof include coextrusion cast molding, coextrusion inflation molding, and coextrusion coating molding.

[0089] The total thickness of the multilayer film can be appropriately set depending on the application. The total thickness is preferably 10 μm or more, more preferably 13 μm or more, and even more preferably 15 μm or more. When the total thickness is 10 μm or more, industrial productivity tends to improve. In addition, the total thickness is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 50 μm or less. When the total thickness is 300 μm or less, industrial productivity tends to improve.

[0090] The multilayer film is preferably stretched. In this case, for example, when the multilayer film has at least a sealant layer (α), an adhesive layer (γ) and a thermoplastic resin layer (δ), the obtained deposition film is preferably one in which at least the sealant layer (α), the adhesive layer (γ) and the thermoplastic resin layer (δ) are stretched together. The degree of stretching is preferably 3 to 12 times, more preferably 4 to 10 times, and even more preferably 5 to 8 times, in terms of area conversion, at least in one axial direction. When the stretching ratio is 3 times or more, the gas barrier property is improved. On the other hand, when the stretching ratio is 12 times or less, the film surface becomes good.

[0091] The multilayer film may be stretched in the biaxial direction at a stretch ratio calculated based on area of ​​9 to 144 times, preferably 16 to 100 times, and more preferably 25 to 64 times. When the stretch ratio is 9 times or more, the gas barrier property is improved. On the other hand, when the stretch ratio is 144 times or less, the film surface is good.

[0092] The stretching method of the multilayer film is not particularly limited, and examples thereof include a tenter stretching method, a tubular stretching method, and a roll stretching method. From the viewpoint of production cost, sequential biaxial stretching or simultaneous biaxial stretching by the tenter stretching method and the tubular stretching method is preferable. From the viewpoint of equipment cost, uniaxial stretching by the roll stretching method is preferable. In addition, when the multilayer film is an inflation molding, the roll stretching method is preferable from the viewpoint of easily stretching the folded cylindrical multilayer film after inflation molding in the uniaxial direction.

[0093] [Base material layer (β)] The base layer (β) is a layer containing a thermoplastic resin having a melting point of 190° C. or higher, and by providing the base layer (β), the appearance after heat sealing can be improved.

[0094] Examples of the thermoplastic resin having a melting point of 190° C. or higher include polyamide, polyester, polystyrene, polyvinyl chloride, poly(meth)acrylic acid ester, polyvinylidene chloride, polyacetal, polycarbonate, polyvinyl acetate, polyurethane, and polyacrylonitrile, with polyester being preferred and polyethylene terephthalate being more preferred.

[0095] The proportion of thermoplastic resin having a melting point of 190°C or higher in the base layer (β) is preferably 60% by mass or higher, more preferably 80% by mass or higher, and even more preferably 90% by mass or higher, and may be 95% by mass or higher, 99% by mass or higher, or may be essentially composed of thermoplastic resin having a melting point of 190°C or higher.

[0096] The average thickness of the base layer (β) is preferably from 2 μm to 200 μm, more preferably from 3 μm to 100 μm, and may be from 5 μm to 50 μm.

[0097] The base material layer (β) may be one layer or two or more layers, and when two or more base material layers (β) are provided, the respective base material layers (β) may be the same or different.

[0098] [Adhesive layer (γ)] In the multilayer structure of the present invention, the sealant layer (α) and the substrate layer (β) are preferably laminated via an adhesive layer (γ). It is more preferable that the adhesive layer (γ) is directly laminated onto the sealant layer (α). That is, it is more preferable that the sealant layer (α), the adhesive layer (γ) and the substrate layer (β) are laminated in this order without any other layers. In addition, when the thermoplastic resin layer (δ) described later is provided, it is preferable to laminate the sealant layer (α) or the substrate layer (β) using the adhesive layer (γ).

[0099] The adhesive layer (γ) is not particularly limited as long as it is a material that enhances the adhesion between layers, but is preferably an adhesive resin layer formed from an adhesive resin or an adhesive layer formed from an adhesive. As the adhesive resin, it is preferable to use a polyolefin having a carboxy group, a carboxylic anhydride group, or an epoxy group. Since such adhesive resins have excellent adhesion to the thermoplastic resin layer (δ) described later, when an adhesive resin layer is suitable as the adhesive layer (γ), the layer structure is sealant layer (α) / adhesive layer (γ) (adhesive resin layer) / thermoplastic resin layer (δ) when the sealant layer (α) and the thermoplastic resin layer (δ) are laminated and " / " means direct lamination.

[0100] Examples of polyolefins containing carboxyl groups include polyolefins copolymerized with acrylic acid or methacrylic acid. In this case, all or part of the carboxyl groups contained in the polyolefin may be present in the form of a metal salt, as typified by ionomers. Examples of polyolefins having carboxylic anhydride groups include polyolefins graft-modified with maleic anhydride or itaconic acid. Examples of polyolefins having epoxy groups include polyolefins copolymerized with glycidyl methacrylate. Among these, polyolefins having carboxylic anhydride groups such as maleic anhydride, particularly polyethylene having carboxylic anhydride groups and polypropylene having carboxylic anhydride groups, are preferred in terms of excellent adhesiveness.

[0101] The adhesive resin preferably has a melt flow rate (MFR) of 0.1 g / 10 min or more and 20.0 g / 10 min or less, more preferably 1.0 g / 10 min or more and 10.0 g / 10 min or less, at 190° C. and 2160 g load, as measured according to JIS K 7210: 2014. When the MFR of the adhesive resin is within the above range, the film formation stability during molding tends to be improved.

[0102] The adhesive may be a known adhesive, preferably a two-liquid reactive polyurethane adhesive in which a polyisocyanate component and a polyol component are mixed and reacted. In addition, the adhesive layer may be further improved in adhesion by adding a small amount of additives such as a known silane coupling agent. The adhesive is preferably used when manufacturing a multilayer structure by a lamination method, and is preferably used when laminating the base layer (β) with other layers.

[0103] From the viewpoints of industrial productivity and quality stability, the average thickness of the adhesive layer (γ) is preferably 0.5 μm or more and 20 μm or less, and more preferably 1 μm or more and 10 μm or less. When the multilayer structure of the present invention has a plurality of sealant layers (α), base material layers (β) and thermoplastic resin layers (δ), or when the multilayer structure of the present invention has an EVOH layer or the like different from the sealant layer (α), the adhesive layer (γ) may be provided between the respective layers, and the number of adhesive layers (γ) in the multilayer structure of the present invention is not particularly limited.

[0104] [Thermoplastic resin layer (δ)] The multilayer structure of the present invention can have increased mechanical strength by including a thermoplastic resin layer (δ) containing a thermoplastic resin having a melting point of less than 190° C. In addition, by forming a multilayer film with the sealant layer (α), the thickness of the sealant layer (α) tends to be thin, and as a result, the multilayer structure of the present invention tends to be easily recycled. In addition, properties such as heat sealability and mechanical strength can be imparted depending on the type of thermoplastic resin constituting the thermoplastic resin layer (δ).

[0105] Examples of thermoplastic resins having a melting point of less than 190° C. include polyethylenes such as linear low-density polyethylene, low-density polyethylene, very low-density polyethylene, medium-density polyethylene, and high-density polyethylene, ethylene-vinyl acetate copolymers, ionomers, ethylene-propylene (block or random) copolymers, ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylic acid ester copolymers, polypropylene, propylene-α-olefin copolymers, polybutene, polypentene, and other olefin homopolymers or copolymers thereof, or polyolefins graft-modified with unsaturated carboxylic acids or their esters; polyesters; polyamides (including copolymerized polyamides); polyvinyl chloride; polyvinylidene chloride; acrylic resins; polystyrene; polyvinyl esters; polyester elastomers; polyurethane elastomers; chlorinated polystyrene; chlorinated polypropylene; aromatic polyketones or aliphatic polyketones, and polyalcohols obtained by reducing these; polyacetals; polycarbonates, etc. Among these, polyolefins are preferred from the viewpoint of excellent heat sealability and recyclability, and polyethylene and polypropylene are more preferred. The polyethylene is preferably at least one selected from the group consisting of linear low-density polyethylene, low-density polyethylene, high-density polyethylene, and other polyethylenes.

[0106] The content of the thermoplastic resin in the thermoplastic resin layer (δ) is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 98% by mass or more. The thermoplastic resin layer (δ) may be substantially composed of a thermoplastic resin alone, or may be composed of a thermoplastic resin alone.

[0107] The melt flow rate (MFR) of the thermoplastic resin constituting the thermoplastic resin layer (δ) measured at 190°C under a load of 2160 g according to JIS K 7210: 2014 is preferably 0.10 g / 10 min to 10.0 g / 10 min, more preferably 0.30 g / 10 min to 5.0 g / 10 min. When the MFR of the thermoplastic resin is within the above range, the film formation stability tends to be improved.

[0108] From the viewpoints of industrial productivity and mechanical properties, the average thickness of the thermoplastic resin layer (δ) is preferably 5 μm or more and 200 μm or less, more preferably 7 μm or more and 100 μm or less, and even more preferably 10 μm or more and 50 μm or less. When the thermoplastic resin layer (δ) has a plurality of layers, it may be preferable that the total thickness of the layers is within the above range.

[0109] In the multilayer structure of the present invention, the thermoplastic resin layer (δ) may be provided in one or more layers.

[0110] [Other layers] Other layers that may be included in the multilayer structure of the present invention include a paper layer, an inorganic vapor deposition layer, a metal foil layer, etc. The multilayer structure of the present invention may also be provided with a vapor deposition layer. Such a vapor deposition layer may be provided on each layer, for example, with the sealant layer (α), the substrate layer (β), and the thermoplastic resin layer (δ) as substrates. As components constituting such a vapor deposition layer, known components used as vapor deposition layers can be appropriately used.

[0111] The inorganic vapor deposition layer can be formed by vapor deposition of an inorganic material. Examples of the inorganic material include metals (e.g., aluminum), metal oxides (e.g., silicon oxide, aluminum oxide), metal nitrides (e.g., silicon nitride), metal nitride oxides (e.g., silicon oxynitride), and metal carbonitrides (e.g., silicon carbonitride). Among these, inorganic vapor deposition layers formed of aluminum, aluminum oxide, silicon oxide, magnesium oxide, or silicon nitride are preferred from the viewpoint of industrial productivity, and aluminum is more preferred.

[0112] Even if the layer is an aluminum vapor deposition layer, oxidation may occur irreversibly and aluminum oxide may be contained in part.

[0113] The lower limit of the average thickness of the inorganic vapor deposition is preferably 15 nm, more preferably 20 nm, even more preferably 30 nm, and particularly preferably 40 nm. The upper limit of the average thickness of the inorganic vapor deposition layer is preferably 150 nm, more preferably 130 nm, and even more preferably 80 nm. By making the average thickness of the inorganic vapor deposition layer equal to or greater than the lower limit, the gas barrier properties can be improved. On the other hand, by making the average thickness of the inorganic vapor deposition layer equal to or less than the upper limit, heat bridging can be suppressed, and the heat insulating effect can be improved.

[0114] The inorganic vapor deposition layer can be provided by a known method.

[0115] [Layer structure, physical properties, etc.] The layer structure of the multilayer structure of the present invention, assuming that " / / " is laminated via an adhesive layer or directly laminated, is, for example, (1) α / / β, (2) α / γ / δ / β, (3) α / / ε / β (4) α / γ / δ / ε / β In addition, α is a sealant layer, β is a base material layer, γ is an adhesive layer, δ is a thermoplastic resin layer, and ε is an inorganic vapor deposition layer.

[0116] For example, the layer structure portion of "α / γ / δ" in the above (2) may be formed as a multilayer film (substrate film) as described above. The multilayer film portion may be stretched or not. When the multilayer film having the above layer structure of "α / γ / δ" is stretched, the layer structure portion of "α / γ / δ" in the deposition film is stretched as a whole. Also, for example, in the above (4), the layer structure portion of "α / γ / δ / / ε / β" may be formed as a multilayer film, or only the layer structure portion of "α / γ / δ" may be formed as a multilayer film, and a thermoplastic resin layer (δ) may be laminated thereon via a separate adhesive layer (γ).

[0117] Specific examples of the layer structure of the multilayer structure of the present invention include a two-layer structure of a resin composition layer (sealant layer (α)) / / polyester layer (substrate layer (β)), and a three-layer structure of a resin composition layer (sealant layer (α)) / / inorganic vapor deposition layer / polyester layer (substrate layer (β)). By providing an inorganic vapor deposition layer as another layer in the multilayer structure, the non-sorption property and gas barrier property can be further improved when used as a packaging bag or the like. Furthermore, other specific examples of the multilayer structure include a resin composition layer (sealant layer (α)) / / polyamide layer (substrate layer (β)) / / polyester layer (substrate layer (β)), a resin composition layer (sealant layer (α)) / / polyamide layer (substrate layer (β)), and the like.

[0118] <Method of manufacturing a multilayer structure> The method for producing the multilayer structure of the present invention is not particularly limited, and known methods for producing single-layer or multilayer films, such as extrusion, coextrusion, dry lamination, extrusion coating, and coextrusion coating, can be adopted. Specifically, when the sealant layer (α) of the multilayer structure is one layer of the multilayer film, examples include a method of coextruding the heat-sealing layer and another layer, a method of extrusion coating the heat-sealing layer on another layer, and a method of dry laminating a film consisting of the heat-sealing layer and a film consisting of another layer. When the sealant layer (α) is one layer of the multilayer film, an adhesive or an adhesive resin can be used as necessary during lamination. The heat-sealing layer or the other layer, when formed from a resin, may be oriented by uniaxial or biaxial stretching.

[0119] The total thickness of the multilayer structure can be appropriately set depending on the application. The total thickness is preferably 10 μm or more, more preferably 13 μm or more, and even more preferably 15 μm or more. When the total thickness is 10 μm or more, industrial productivity tends to improve. In addition, the total thickness is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 50 μm or less. When the total thickness is 300 μm or less, industrial productivity tends to improve.

[0120] The multilayer structure may be stretched. For example, when the multilayer film has at least a sealant layer (α), an adhesive layer (γ) and a thermoplastic resin layer (δ), the obtained multilayer structure may be one in which at least the sealant layer (α), the adhesive layer (γ) and the thermoplastic resin layer (δ) are stretched together. The degree of stretching may be 3 to 12 times, 4 to 10 times, or 5 to 8 times in terms of area-converted stretching ratio at least in one axial direction. When the stretching ratio is 3 times or more, the gas barrier property tends to be improved. On the other hand, when the stretching ratio is 12 times or less, the film surface tends to be good.

[0121] The multilayer film may be stretched in the biaxial direction at a stretch ratio calculated based on area of ​​4 to 144 times, preferably 16 to 100 times, and more preferably 25 to 64 times. When the stretch ratio is 9 times or more, the gas barrier property is improved. On the other hand, when the stretch ratio is 144 times or less, the film surface is good.

[0122] The stretching method of the multilayer film is not particularly limited, and examples thereof include a tenter stretching method, a tubular stretching method, and a roll stretching method. From the viewpoint of production cost, sequential biaxial stretching or simultaneous biaxial stretching by the tenter stretching method and the tubular stretching method is preferable. From the viewpoint of equipment cost, uniaxial stretching by the roll stretching method is preferable. In addition, when the multilayer film is an inflation molding, the roll stretching method is preferable from the viewpoint of easily stretching the folded cylindrical multilayer film after inflation molding in the uniaxial direction.

[0123] The difference in oxygen transmission rate measured at 30°C and 65% RH between the end and center portions in the width direction of the multilayer structure is preferably less than 15%, more preferably less than 10%, even more preferably less than 5%, and even more preferably less than 1%. When the difference in oxygen transmission rate of the multilayer structure is equal to or less than the above upper limit, the period during which the oxygen concentration in the internal space of a bag or the like formed by a packaging material comprising the multilayer structure can be maintained low is extended. Here, oxygen transmission rate (mL / m2 ·day·atm is the amount of oxygen (mL) that permeates the multilayer structure per unit area (m 2 ), divided by the permeation time (days) and the difference (atm) between the oxygen gas pressure on one side and the oxygen gas pressure on the other side. 2 If the oxygen gas pressure difference is 1 atm or less, the film can be heated for 1 m per day. 2 This means that 5 mL of oxygen permeates per unit area. The difference in oxygen permeability in the width direction of the multilayer structure can also be considered to be equivalent to the difference in oxygen permeability in the width direction of the monolayer film of the sealant layer (α).

[0124] The lower limit of the volatile content of the sealant layer (α) is not particularly limited, but is preferably 0.01% by mass, more preferably 0.03% by mass, and even more preferably 0.05% by mass. The upper limit of the volatile content is preferably 1.1% by mass, more preferably 0.5% by mass, and even more preferably 0.3% by mass.

[0125] However, when the multilayer structure is applied to a vacuum insulator, it is preferable that the volatile content in the multilayer structure is as small as possible, because there is a risk that volatile content generated from the multilayer structure will penetrate into the vacuum portion of the vacuum insulator, resulting in a decrease in the degree of vacuum inside the vacuum insulator and a decrease in the insulating performance.

[0126] Here, the content of volatile matter is calculated from the change in mass before and after drying at 105° C. for 3 hours using the following formula. Volatile content (mass%) = [(mass before drying - mass after drying) / mass after drying] x 100

[0127] In the multilayer structure, when the sealant layers (α) of the multilayer structure are pressed together for 1 second using a hot plate heat sealer at a temperature of 200° C. and a pressure of 0.1 MPa, the heat seal strength measured in accordance with JIS Z1707 (2019) is preferably 20 N / 15 mm or more. If the heat seal strength is 20 N / 15 mm or more, the gas barrier properties as a packaging material are good. The heat seal strength is preferably 23 N / 15 mm or more, more preferably 26 N / 15 mm or more. The heat seal strength may be 50 N / 15 mm or less, 40 N / 15 mm or less, or 35 N / 15 mm or less.

[0128] The method for heat-sealing the multilayer structure is not particularly limited as long as the sealant layers (α) are heat-sealed to each other, and known methods can be used, such as a method using a hot plate heat sealer, an impulse sealer, an ultrasonic sealer, a friction heat sealer, a dielectric heating sealer, etc. The temperature during heat sealing is preferably not lower than the melting point of the heat-sealing layer and not higher than the melting point + 30°C in terms of heat seal strength and prevention of defective appearance. The pressure for heat sealing is preferably 0.01 MPa or more and 1.0 MPa or less in terms of heat seal strength and prevention of defective appearance. The time for heat sealing is preferably 0.05 seconds or more and 5 seconds or less in terms of heat seal strength and productivity.

[0129] [Application] The multilayer structure of the present invention has a high uniformity of gas barrier properties of the heat seal layer (α), high heat seal strength, and good appearance after heat sealing. Therefore, the multilayer structure can be applied to various uses. Examples of uses of the multilayer structure include various packaging materials such as food packaging, pharmaceutical packaging, industrial chemical packaging, and agricultural chemical packaging, vacuum insulators, etc.

[0130] <Packaging material> The packaging material of the present invention comprises the multilayer structure of the present invention. The packaging material of the present invention is formed, for example, by secondary processing the multilayer structure of the present invention or a multilayer structure comprising the same. By comprising the multilayer structure, the packaging material has excellent gas barrier properties. In the packaging material of the present invention, the sealant layer (α) of the multilayer structure of the present invention constitutes the inner surface of the packaging material, that is, the packaging material is produced by heat sealing the sealant layers (α) of the multilayer structure together. Since the sealant layer (α) has a property of being unlikely to adsorb compounds and the like (non-adsorbing property), the packaging material of the present invention is unlikely to adsorb the components of the contents, and can be suitably used as a package for, for example, foods, beverages, luxury items, medicines, cosmetics, fragrances, toiletry products, etc., containing aroma components or medicinal components.

[0131] The packaging material of the present invention can be formed into various forms depending on the application, such as a vertical form-fill-seal bag, a vacuum packaging bag, a pouch with a spout, a laminated tube container, a container lid material, and the like.

[0132] [Vertical form fill seal bag] Vertical form fill seal pouches are used for packaging food, beverages, and the like, for example, liquids, viscous materials, powders, bulk solids, and combinations thereof.

[0133] The vertical form fill seal bag is formed by heat sealing the sealant layer (α) of the multilayer structure. When heat sealing is performed, it is usually necessary to place the sealant layer (α) on the layer of the multilayer structure that will be the inner layer of the vertical form fill seal bag.

[0134] The layer structure of the vertical form-fill-seal bag is preferably a base layer (β) / / sealant layer (α).

[0135] As described above, the packaging material of the present invention has excellent gas barrier properties, and therefore, with a vertical form fill seal bag, which is one example of the packaging material, deterioration of the quality of the contents can be suppressed for a long period of time.

[0136] [Vacuum packaging bag] Vacuum packaging bags are used for applications where packaging in a vacuum state is desired, such as the preservation of food, beverages, etc. The layer structure of the vacuum packaging bag is preferably a polyamide layer (substrate layer (β)) / / substrate layer (β) / / sealant layer (α), or a polyamide layer (substrate layer (β)) / / sealant layer (α). Since such a vacuum packaging bag includes the sealant layer (α), it is particularly excellent in gas barrier properties and non-adsorption properties after vacuum packaging.

[0137] [Pouch with spout] Spouted pouches are used for packaging liquid substances, such as liquid beverages such as soft drinks, jelly drinks, yogurt, fruit sauces, seasonings, functional water, liquid foods, etc. The layer structure of this spouted pouch is preferably a polyamide layer (base layer (β)) / / sealant layer (α). Since such a spouted pouch has the multilayer structure, it has excellent gas barrier properties and non-adsorption properties. Therefore, the spouted pouch can prevent deterioration of the contents and retain the aroma even after transportation and long-term storage.

[0138] [Laminated tube container] The laminated tube container is used for packaging cosmetics, medicines, pharmaceuticals, food, toothpaste, etc. The laminated tube container preferably has a layer structure of polyamide layer (base layer (β)) / / sealant layer (α). Such a laminated tube container has excellent gas barrier properties and aroma retention properties due to the multilayer structure.

[0139] [Container lid material] The container lid material is a lid material for containers filled with foods such as processed meat products, processed vegetables, processed seafood products, and fruits. The layer structure of this container lid material is preferably a polyamide layer (base layer (β)) / / sealant layer (α). Since such a container lid material has the multilayer structure, it has excellent gas barrier properties and aroma retention properties, and can suppress quality deterioration of the food contents for a long period of time.

[0140] <Vacuum insulation> The vacuum insulator of the present invention comprises the multilayer structure of the present invention. The vacuum insulator is used for applications requiring cold or warm insulation. For example, this vacuum insulator may be one in which a core material such as glass wool is sealed in a vacuum state within an outer packaging material. The outer packaging material is preferably, for example, the multilayer structure of the present invention that includes at least one inorganic vapor deposition layer, and is formed by heat sealing such a multilayer structure.

[0141] The number of layers and the stacking order in the outer packaging material are not particularly limited, but it is preferable that the outer packaging material contains an inorganic vapor deposition layer. The layer structure of the outer packaging material is preferably polyamide layer (substrate layer (β)) / / substrate layer (β) / inorganic vapor deposition layer / / sealant layer (α) or polyamide layer (substrate layer (β)) / inorganic vapor deposition layer / / substrate layer (β) / / sealant layer (α).

[0142] Such a vacuum insulator has excellent gas barrier properties because the outer packaging material is provided with the multilayer structure of the present invention, and therefore can maintain its insulating effect for a long period of time, and can be used as an insulating material for household appliances such as refrigerators, hot water supply equipment, and rice cookers; as a residential insulating material used in walls, ceilings, attics, floors, and the like; as a vehicle roofing material; and as an insulating panel for vending machines, etc. EXAMPLES

[0143] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0144] [Evaluation method] (1) Measurement of ethylene unit content, degree of saponification, and modification amount of epoxypropane (modification amount relative to total vinyl alcohol units) The crude EVOH obtained in the synthesis example was dried in a vacuum dryer at 120°C for 12 hours. The vacuum-dried EVOH was dissolved in deuterated dimethyl sulfoxide (DMSO-d6) containing tetramethylsilane (TMS) as an internal standard and trifluoroacetic acid (TFA) as an additive, and the solution was analyzed by a 500 MHz spectrometer. 1Measurement was performed at 80°C using H-NMR ("GX-500" manufactured by JEOL Ltd.), and the ethylene unit content and saponification degree were determined from the peak intensity ratio of the ethylene unit, vinyl alcohol unit, and vinyl ester unit. When measuring the EVOH pellets obtained in Synthesis Examples 9 and 10, the measurement was performed without vacuum drying, and the modification amount relative to the total vinyl alcohol units was also calculated from the peak intensity of the epoxypropane-modified vinyl alcohol unit. In the EVOH (A9, A10) obtained in Synthesis Examples 9 and 10, the modification amount of epoxypropane relative to the total vinyl alcohol units is equal to the content of the structural unit (x) relative to the total vinyl alcohol units.

[0145] (2) Sodium ion content, phosphate content, and boric acid content 0.5 g of the dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples, and Comparative Examples was placed in a Teflon (registered trademark) pressure vessel, and 5 mL of concentrated nitric acid was added thereto and decomposed at room temperature for 30 minutes. After 30 minutes, the vessel was closed, and the mixture was decomposed by heating at 150°C for 10 minutes and then at 180°C for 5 minutes using a wet decomposition apparatus (Actac Co., Ltd., "MWS-2"), and then cooled to room temperature. This treatment liquid was transferred to a 50 mL measuring flask (TPX (registered trademark)) and made up to 10 mL with pure water. The metal content of this solution was analyzed using an ICP emission spectrometer (PerkinElmer, Inc., "OPTIMA4300DV"), and the contents of sodium ions (sodium element), phosphoric acid, and boric acid were measured. The phosphoric acid content was calculated as a phosphate root equivalent value, and the boric acid content was calculated as an orthoboric acid equivalent value. In addition, a calibration curve prepared using a commercially available standard solution was used for the quantitative determination.

[0146] (3) Acetic acid content 20 g of the dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples, and Comparative Examples were added to 100 mL of ion-exchanged water and extracted by heating at 95° C. for 6 hours. The extract was neutralized and titrated with 1 / 50 N NaOH using phenolphthalein as an indicator to quantify the acetic acid content.

[0147] (4) Melt flow rate (MFR) The dried resin composition pellets obtained in the Reference Examples and Reference Comparative Examples were filled into a cylinder of Melt Indexer L244 (manufactured by Takara Kogyo Co., Ltd.) with an inner diameter of 9.55 mm and a length of 162 mm, and melted at 210°C. Then, a load was evenly applied to the molten resin composition using a plunger with a mass of 2,160 g and a diameter of 9.48 mm. The amount of resin composition extruded per unit time (g / 10 min) from an orifice with a diameter of 2.1 mm provided in the center of the cylinder was measured, and this was taken as the MFR.

[0148] (5) Determination of crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal 0.50 g of the dried resin composition pellets obtained in the reference example, reference comparative example, examples and comparative examples were frozen and crushed to obtain a sample, which was weighed out to 50.0 mg in a glass tube for a thermal desorption gas chromatograph mass spectrometer to prepare a sample tube. Using the thermal desorption gas chromatograph mass spectrometer described below, the sample was heated under the following conditions to adsorb the entire amount of volatile gas from the sample once into the adsorption tube, and the gas re-emitted from the adsorption tube was separated in a column to detect the peaks of each component. A calibration curve was created from the peak areas of the standard samples of crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal, and each was quantified by the absolute calibration curve method. When measuring the standard sample, the standard sample was impregnated into an adsorption tube (manufactured by Tenax (registered trademark) / Carboxen (registered trademark)), and the adsorption tube impregnated with the standard sample was used instead of the sample tube. The temperature at the time of release after sample adsorption was changed from the sample tube temperature of 170°C to the adsorption tube temperature of 260°C, but the measurement was performed in the same manner as in the measurement of the sample tube. (Heat desorption section) Device: TurboMatrix-ATD (PerkinElmer Japan) Temperature when adsorbing the sample to the adsorption tube: 170℃ (sample tube), -30℃ (adsorption tube), 250℃ (valve), 260℃ (transfer line) Adsorption time in the adsorption tube: 10 minutes Temperature at the time of release after sample adsorption: 170°C (sample tube), 260°C (adsorption tube), 250°C (valve), 260°C (transfer line) Adsorption tube discharge time: 35 minutes Carrier gas: Helium Carrier gas flow rate to column: 1.0 ml / min Pressure: 120kPa (Gas chromatograph mass spectrometry section) Equipment: 7890B GC System, 7977B MSD (Agilent Technologies) Column: DB-WAX UI (length: 30 m, inner diameter: 0.25 mm, film thickness: 0.50 μm) Column oven temperature: 40°C for 5 minutes, then heat up to 240°C at a rate of 10°C / min and hold for 10 minutes (total measurement temperature: 35 minutes) Transfer line (connection) temperature: 240℃ Ionization conditions: EI+ Detected ion mass range: m / z=29-600 Detection method: SCAN (Standard sample) Crotonaldehyde: Aldrich 2,4-Hexadienal: Aldrich 2,4,6-Octatrienal: Produced by NARD Laboratories

[0149] (6) Determination of sorbic acid and myrcene The dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples and Comparative Examples were freeze-pulverized, and 22 g of the pulverized material was loaded into a Soxhlet extractor and extracted with 100 mL of chloroform for 16 hours. The amounts of sorbic acid and myrcene in the obtained chloroform extract were quantitatively analyzed by high performance liquid chromatography to quantify the contents of sorbic acid and myrcene in the resin composition. For the quantification, a calibration curve prepared using sorbic acid and myrcene standards was used.

[0150] (7) Die build-up evaluation The dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples, and Comparative Examples were extruded from an extruder under the following conditions, and after 60 minutes, the die build-up (dye build-up) around the die (die lip) was visually observed and evaluated according to the following criteria. In the cases of A to D, it was determined that the die build-up was suppressed. (Extruder conditions) Equipment: 20mmφ single screw extruder (D2020, manufactured by Toyo Seiki Co., Ltd.) L / D:20 Screw: Full flight Screen mesh: 50 mesh / 100 mesh / 50 mesh Die: φ1mm, 1 hole ·Setting temperature: C1 / C2 / C3 / D=180℃ / 220℃ / 220℃ / 220℃ ·Discharge amount: 1.44kg / h Rotational speed: 100 rpm (Evaluation: Criteria) A (Good): No eye gunk B (fairly good): There is a very small amount of eye mucus. C (Acceptable): A small amount of eye discharge is present D (slightly poor): There is obvious eye discharge E (bad): Large particles of resin are attached around the entire circumference of the die hole.

[0151] (8) Hue evaluation The yellow index (YI) value of the dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples, and Comparative Examples was measured and calculated using a LAB Scan XE manufactured by Hunter Co., Ltd. in accordance with JIS K7373: 2006. It was judged that the smaller the value, the more suppressed the yellowing and the better the hue.

[0152] (9) Evaluation of neck-in resistance during film formation Using the dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples, and Comparative Examples, a resin composition was extruded from a single screw extruder under the following conditions, and the width of the molten resin (melt curtain) discharged from the T-die 10 minutes after the dried resin composition pellets were charged was measured at a position 100 mm from the lip (the discharge port of the T-die). The width of the molten resin was evaluated according to the following criteria. In the cases of A to C, it was determined that neck-in was suppressed. (Extruder conditions) Extruder: L / D=26, 40mmφ single screw extruder Screw: Full flight Screw speed: 50 rpm Screen mesh: 50 mesh / 100 mesh / 50 mesh Die shape: T-type, lip width 550mm, lip spacing 0.7mm ·Setting temperature: C1 / C2 / C3 / D=170℃ / 240℃ / 260℃ / 260℃ (Evaluation: Criteria) A (Good): 85% or more of lip width B (fairly good): 82.5% to less than 85% of the lip width C (slightly poor): 80% or more and less than 82.5% of the lip width D (Poor): Less than 80% of lip width

[0153] (10) Melting point measurement The crude EVOH obtained in Synthesis Example was dried in a vacuum dryer at 120°C for 12 hours. The vacuum-dried EVOH was heated from 30°C to 250°C at a rate of 10°C / min using a TA Instruments differential scanning calorimeter "Q2000", cooled at 50°C / min, and the melting point was determined from the peak temperature measured in the second heating. Note that when measuring the EVOH pellets obtained in Synthesis Examples 9 and 10, they were not vacuum-dried.

[0154] (11) Oxygen transmission rate (OTR) measurement <Single layer film production conditions> The dried resin composition pellets obtained in the Reference Examples and Reference Comparative Examples were subjected to film formation under the following conditions to obtain a single layer film having an average thickness of 30 μm. (Extruder Conditions) · L / D: 26, single screw extruder with a diameter of 40 mm · Screw: Full flight · Screw rotation speed: 30 rpm · Screen mesh: 50 mesh / 100 mesh / 50 mesh · Die shape: T-shaped, lip width 550 mm, lip interval 0.7 mm · Set temperature: C1 / C2 / C3 / D = 170°C / 230°C / 230°C / 230°C · Take-up roll temperature: 80°C · Take-up roll speed: 10 - 11 m / min <OTR (Oxygen Transmission Rate) Measurement> For the obtained single-layer film with a thickness of 30 μm, a sample was cut out in a circle with a diameter of 90 mm centered on the center in the width direction, and after conditioning under the conditions of 30°C and 65% RH, the oxygen transmission rate was measured using an oxygen transmission rate measuring device (「OX-Tran2 / 20」 of ModernControl, detection lower limit 0.01 mL / (m 2 · day·atm)) in accordance with ISO14663-2 annex C at 30°C and 65% RH. Also, the oxygen transmission rate of the single-layer film or multilayer film obtained in the examples and comparative examples was measured in the same manner.

[0155] (12) Width Direction Uniformity of OTR For the single-layer film or multilayer film used in the measurement of (11), a sample was cut out in a circle with a diameter of 90 mm centered on the position 70 mm from the film edge, and the OTR was measured under the same conditions as (11). The difference from the OTR of the sample at the center was taken, and the magnitude of the difference was evaluated in three levels from A to C. (Evaluation: Judgment Criteria) A: The difference is less than 10% B: The difference is 10% or more and less than 15% C: The difference is 15% or more

[0156] (13) Heat Seal Strength and Appearance The heat seal layer (α) of the multilayer structure obtained in the examples and comparative examples was overlapped and pressed for 1 second using a hot plate heat sealer (Hiraishi Shoji Co., Ltd. bag sealer HBS-280) at a temperature of 200 ° C. and a pressure of 0.1 MPa. The heat seal strength (N / 15 mm) per 15 mm width of the heat-sealed film was measured using a tensile tester according to the method described in JIS Z 1707 (2019). The tensile speed during the seal strength measurement was 300 mm / min.

[0157] The appearance of the heat-sealed portion was visually evaluated according to the following criteria: Evaluation C was determined to have failed to suppress deterioration of appearance after heat sealing. A: Excellent appearance B: Slight thinning and foaming, and the appearance is somewhat poor. C: Poor appearance, with noticeable thinning and foaming

[0158] <Synthesis Example 1> A 200L pressurized reactor equipped with a jacket, a stirrer, a nitrogen inlet, an ethylene inlet, and an initiator addition inlet was charged with 75.0 kg of vinyl acetate (hereinafter sometimes referred to as VAc) and 7.2 kg of methanol (hereinafter sometimes referred to as MeOH), and nitrogen bubbling was performed for 30 minutes to replace the atmosphere in the reactor with nitrogen. Next, the temperature in the reactor was adjusted to 65°C, and ethylene was introduced so that the reactor pressure (ethylene pressure) was 4.13 MPa, and 9.4 g of 2,2'-azobis(2,4-dimethylvaleronitrile) ("V-65" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added as a polymerization initiator to start polymerization. During polymerization, the ethylene pressure was maintained at 4.13 MPa and the polymerization temperature at 65°C. After 4 hours, when the conversion rate of VAc (polymerization rate based on VAc) reached 49.7%, the reactor was cooled, and a solution in which 0.2 g of copper acetate was dissolved in 20 kg of methanol was added to the vessel to stop the polymerization. After the reaction vessel was opened to remove ethylene, nitrogen gas was bubbled through to remove ethylene completely. The polymerization liquid was then removed from the vessel and diluted with 20 L of MeOH. This liquid was fed from the top of a tower vessel, and MeOH vapor was fed from the bottom of the vessel to remove the unreacted monomers remaining in the polymerization liquid together with the MeOH vapor, to obtain a MeOH solution of ethylene-vinyl acetate copolymer (hereinafter sometimes referred to as EVAc).

[0159] Next, 150 kg of a 20% by mass MeOH solution of EVAc was charged into a 300 L reaction vessel equipped with a jacket, a stirrer, a nitrogen inlet, a reflux condenser, and a solution addition port. The solution was heated to 60° C. while blowing nitrogen gas into it, and a MeOH solution with a 2N concentration of sodium hydroxide was added at a rate of 450 mL / min for 2 hours. After the addition of the sodium hydroxide MeOH solution was completed, the temperature in the system was kept at 60° C., and the saponification reaction was allowed to proceed for 2 hours while stirring and discharging MeOH and methyl acetate produced by the saponification reaction out of the reaction vessel. Then, 8.7 kg of acetic acid was added to stop the saponification reaction.

[0160] After that, 120L of ion-exchanged water was added while heating and stirring at 80℃, MeOH was discharged from the reaction tank, and EVOH was precipitated. The precipitated EVOH was collected by decantation and crushed in a crusher. The obtained EVOH powder was put into a 1g / L acetic acid aqueous solution (bath ratio 20: 20L of aqueous solution per 1kg of powder) and washed with stirring for 2 hours. This was deliquified, and then put into a 1g / L acetic acid aqueous solution (bath ratio 20) and washed with stirring for 2 hours. The deliquified product was put into ion-exchanged water (bath ratio 20), washed with stirring for 2 hours, and then deliquified. This operation was repeated three times for purification. The electrical conductivity of the washing solution was 3μS / cm (measured with "CM-30ET" by Toa Denpa Kogyo Co., Ltd.). The resulting purified product was then immersed in 250 L of an aqueous solution containing 0.5 g / L of acetic acid and 0.1 g / L of sodium acetate with stirring for 4 hours, then the liquid was removed and the product was dried at 60°C for 16 hours to obtain 16.1 kg of crude dried EVOH.

[0161] The above-mentioned synthesis of EVOH was repeated to obtain 15.9 kg of crude EVOH, and a total of 32.0 kg of crude EVOH (A1) was obtained. The ethylene unit content, saponification degree, and melting point of the crude EVOH (A1) were measured according to the methods described in the above evaluation methods (1) and (10). The results are shown in Table 2.

[0162] <Synthesis Examples 2 to 8> The size of the pressurized reaction vessel, the amount of VAc and MeOH charged, the ethylene pressure, the amount of polymerization initiator added, the temperature inside the reaction vessel (temperature during polymerization), the reaction time, the conversion rate of VAc, the amount of EVAc MeOH solution charged in the saponification step, and the addition rate of sodium hydroxide MeOH solution were set as shown in Table 1, and the crude dried products of EVOH (A2) to EVOH (A8) were obtained in the same manner as in Synthesis Example 1, except that the synthesis was performed only once. The ethylene unit content, saponification degree, and melting point of the crude dried products of EVOH (A2) to EVOH (A8) were measured according to the methods described in the above evaluation methods (1) and (10). The results are shown in Table 2.

[0163] <Synthesis Example 9> EVOH (A9) pellets were produced by the following procedure using the apparatus described in paragraph

[0158] and FIG. 1 of JP 2003-231715 A. Toshiba Machine Co., Ltd.'s TEM-35BS extruder (37 mmφ, L / D=52.5) ​​was used, barrel C1 was water-cooled, barrels C2-C3 were set to 200°C, barrels C4-C15 were set to 240°C, and the screw was operated at a rotation speed of 400 rpm. Dry resin composition pellets obtained in Reference Example 38 described later were fed from the resin feed port of C1 and melted, and then water and oxygen were removed from vent 1, and epoxypropane was fed as modifier 2 from the hydraulic inlet of C9. Thereafter, unreacted epoxypropane was removed from vent 2, pelletized, and then hot air dried at 80°C for 2 hours to obtain EVOH (A9) pellets modified by 8 mol%. The ethylene unit content, saponification degree, epoxypropane modification amount (amount relative to all vinyl alcohol units), and melting point of the obtained EVOH (A9) pellets were measured according to the methods described in the above evaluation methods (1) and (10). The results of the ethylene unit content, saponification degree, and melting point are shown in Table 2. The epoxypropane modification amount (content of structural unit (x) relative to all vinyl alcohol units) was 8 mol%.

[0164] <Synthesis Example 10> Pelletization was carried out in the same manner as in Synthesis Example 9, except that the dry resin composition pellets fed as a raw material were changed to the dry resin composition pellets obtained in Reference Example 43, to obtain 8 mol% modified EVOH (A10) pellets. The ethylene unit content, saponification degree, epoxypropane modification amount (amount relative to all vinyl alcohol units), and melting point of the obtained EVOH (A10) pellets were measured according to the methods described in the above evaluation methods (1) and (10). The results of the ethylene unit content, saponification degree, and melting point are shown in Table 2. The epoxypropane modification amount (content of structural unit (x) relative to all vinyl alcohol units) was 8 mol%.

[0165] [Table 1]

[0166] [Table 2]

[0167] <Reference example 1> In a 60 L stirring tank equipped with a jacket, a stirrer and a reflux condenser, 2 kg of the crude dried EVOH (A1) obtained in Synthesis Example 1, 0.8 kg of water and 2.2 kg of MeOH were charged and stirred at 60°C for 5 hours to completely dissolve. To the obtained solution, sorbic acid, crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal were added. This solution was extruded through a 4 mm diameter gold plate into a mixture of water / MeOH = 90 / 10 cooled to -5°C to precipitate in the form of strands, and the strands were cut into pellets with a strand cutter to obtain hydrous pellets of EVOH. The moisture content of the obtained hydrous pellets of EVOH was measured with a Mettler halogen moisture meter "HR73" and found to be 52% by mass.

[0168] The obtained EVOH hydrous pellets were placed in a 1g / L aqueous acetic acid solution (bath ratio 20) and washed with stirring for 2 hours. The pellets were deliquinated and then placed in a 1g / L aqueous acetic acid solution (bath ratio 20) and washed with stirring for 2 hours. After deliquification, the aqueous acetic acid solution was renewed and the same procedure was carried out. The pellets were washed with the aqueous acetic acid solution, deliquinated, placed in ion-exchanged water (bath ratio 20), washed with stirring for 2 hours, and then deliquinated three times. The procedure was repeated until the electrical conductivity of the washing solution was 3μS / cm or less (measured with Toa Denpa Kogyo Co., Ltd.'s "CM-30ET"), and EVOH hydrous pellets from which the catalyst residue from the saponification reaction had been removed were obtained.

[0169] The obtained hydrous pellets were put into an aqueous solution (bath ratio 20) with a sodium acetate concentration of 0.510 g / L, an acetic acid concentration of 0.8 g / L, and a phosphoric acid concentration of 0.04 g / L, and immersed for 4 hours while stirring periodically for chemical treatment. The pellets were dehydrated and dried at 80°C for 3 hours and at 105°C for 16 hours under a nitrogen stream with an oxygen concentration of 1% by volume or less to obtain cylindrical (average diameter 2.8 mm, average height 3.2 mm) dried resin composition pellets containing EVOH (A1), acetic acid, phosphoric acid, sodium ions (sodium salts), crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal, and sorbic acid. The obtained dried resin composition pellets were evaluated according to the methods described in the above evaluation methods (2) to (9). The sodium ion content in the dried resin composition pellets was 100 ppm, the phosphoric acid content was 40 ppm in terms of phosphate radical, and the acetic acid content was 200 ppm. The contents of each component other than EVOH are based on the EVOH content. Other evaluation results are shown in Table 3. The amount of each component added was adjusted so that the contents of each component, crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal, and sorbic acid, were as shown in Table 3.

[0170] <Reference Examples 2~61, Reference Comparative Examples 1~4, 6~24> Dry resin composition pellets were prepared and evaluated in the same manner as in Reference Example 1, except that the type of EVOH (A), the type and content of the unsaturated aliphatic aldehyde (B), the type and content of the conjugated polyene compound (C), and the content of boric acid were adjusted to be as shown in Tables 3 to 10. When the boric acid was contained at 800 ppm, an aqueous solution containing sodium acetate and the like (bath ratio 20) was used so that the boric acid concentration was 0.25 g / L, and when the boric acid was contained at 1800 ppm, an aqueous solution containing sodium acetate and the like (bath ratio 20) was used so that the boric acid concentration was 0.57 g / L. The sodium ion content of the EVOH in each dry resin composition pellet was 100 ppm, the phosphoric acid content was 40 ppm in terms of phosphate radical, and the acetic acid content was 200 ppm. Other evaluation results are shown in Tables 3 to 10. The contents of each component other than EVOH are all based on the content of EVOH.

[0171] <Reference Comparative Example 5> Crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal were not added, and the hydrous pellets of EVOH from which the catalyst residues during the saponification reaction had been removed were placed in methanol (bath ratio 10), stirred and washed for 2 hours, and deliquored twice. The pellets obtained were placed in ion-exchanged water (bath ratio 20), stirred and washed for 2 hours, and deliquored three times. The dried resin composition pellets were prepared and evaluated in the same manner as in Reference Example 1. The sodium ion content in the dried resin composition pellets was 100 ppm, the phosphoric acid content was 40 ppm in terms of phosphoric acid radical, and the acetic acid content was 200 ppm. The contents of each component other than EVOH are all based on the content of EVOH. Other evaluation results are shown in Table 3. The contents of each component of crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal and sorbic acid were below the detection limit.

[0172] [Table 3]

[0173] [Table 4]

[0174] [Table 5]

[0175] [Table 6]

[0176] [Table 7]

[0177] [Table 8]

[0178] [Table 9]

[0179] [Table 10]

[0180] From the Reference Examples and Reference Comparative Examples, it can be seen that when b1 / (b2+b3) is 2.0 or more and less than 150.0, the neck-in resistance is good, the smaller b1+b2+b3 is, the lower the YI is, the smaller the content c of the conjugated polyene compound (C) is, the lower the YI is, and the smaller the b2+b3 is, the lower the die build-up is.

[0181] A more detailed consideration based on Table 3 is as follows. In Reference Comparative Example 5, which does not contain an unsaturated aliphatic aldehyde (B), and Reference Comparative Examples 1 to 3 and 6 to 9, which contain each type of unsaturated aliphatic aldehyde (B) alone, neck-in is not suppressed. Furthermore, in Reference Comparative Example 10, in which the value of b1 / (b2+b3) is less than 2.0, neck-in is not suppressed. On the other hand, as can be seen from the reference examples, when the value of b1 / (b2+b3) is in the range of 2.0 or more and less than 150.0, neck-in is suppressed, and particularly when the value of b1 / (b2+b3) is around 10 (for example, 8.0 or more and 13.0 or less), as in Reference Examples 4, 5, 13, 14, 21 and 24, neck-in is most suppressed. In addition, in Comparative Example 4, where b2+2b3 exceeds 0.65 ppm, die build-up is not suppressed, whereas in the Reference Examples, when b2+2b3 is 0.65 ppm or less, die build-up is suppressed, and particularly when b2+2b3 is 0.10 ppm or less, die build-up is suppressed. In addition, as can be seen from Comparative Example 4, Reference Examples 1 to 7, 12 to 26, etc., it can be seen that the lower the total content of crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3), the better the hue. Furthermore, it can be seen from Reference Examples 6 and 9 to 11 that the hue is better when the content of the conjugated polyene compound is smaller.

[0182] <Example 1> The dried resin composition pellets (resin composition) obtained in Reference Example 5 were melted at 240°C in a single screw extruder, extruded from a die onto a casting roll, and simultaneously, air was blown at a wind speed of 30 m / sec using an air knife to obtain a monolayer film (sealant layer (α)) having a thickness of 30 μm. The OTR of the obtained monolayer film was measured according to the method described in the above evaluation method (11). The results are shown in Table 12. A PET film (PET12) having a thickness of 12 μm was laminated as a substrate layer (β) on the obtained monolayer film using an adhesive to produce a multilayer structure of sealant layer (α) / adhesive layer (γ) / substrate layer (β). When laminating the substrate layer (β), a two-liquid urethane adhesive ("Takelac A-520" and "Takenate A-50" manufactured by Mitsui Chemicals, Inc.) was applied to a dry thickness of 2 μm to provide an adhesive layer (γ), which was then laminated by a dry lamination method. The heat seal strength and appearance of the obtained multilayer structure were evaluated by the method described in the above evaluation method (13). The results are shown in Table 12. The other evaluation results for the dried resin composition pellets of Reference Example 5 used are shown again in Tables 11 and 12.

[0183] <Examples 2 to 8, Comparative Examples 1 and 2> A single layer film and a multilayer structure were produced and evaluated in the same manner as in Example 1, except that the dried resin composition pellets obtained in Reference Examples 28, 38, 43, 48, 2, 7, Synthesis Example 10, and Reference Comparative Examples 4 and 3 were used. The results are shown in Table 12. The other evaluation results described above for the dried resin composition pellets used in the Reference Examples and Reference Comparative Examples are shown in Tables 11 and 12. The dried EVOH resin composition pellets (A10) obtained in Synthesis Example 10 were evaluated according to the methods described in the above evaluation methods (5) to (12). The evaluation results are shown in Tables 11 and 12.

[0184] <Example 9> The dried resin composition pellets (resin composition) obtained in Reference Example 5 were melted at 240°C in a single screw extruder, extruded from a die onto a casting roll, and simultaneously air was blown at a wind speed of 30 m / sec using an air knife to obtain an unstretched film having a thickness of 170 μm. The obtained unstretched film having a thickness of 170 μm was contacted with 80°C hot water for 10 seconds, stretched 3.2 times in the longitudinal direction and 3.0 times in the transverse direction in a 90°C atmosphere using a tenter-type simultaneous biaxial stretching machine, and further heat-treated for 5 seconds in a tenter set at 170°C, and the film end was cut to obtain a biaxially stretched monolayer film (sealant layer (α)) having a thickness of 12 μm. A multilayer structure was produced and evaluated in the same manner as in Example 1, except that the obtained sealant layer (α) was used. The results are shown in Table 12. The other evaluation results of the dried resin composition pellets used are also shown in Tables 11 and 12.

[0185] [Table 11]

[0186] [Table 12]

[0187] <Example 10> A cylindrical multilayer film was produced under the following conditions using an inflation extrusion molding machine and the dried resin composition pellets (resin composition) obtained in Reference Example 5. The thermoplastic resin layer (δ) was laminated in three layers with a thickness of 30 μm, resulting in one thermoplastic resin layer (δ) with a thickness of 90 μm. (Multilayer film manufacturing conditions) Layer composition of multilayer structure: [Outer surface] Thermoplastic resin layer (δ) / Adhesive layer (γ) / Sealant layer (α) [Inner surface] = 90 μm / 20 μm / 30 μm (total thickness 140 μm) Thermoplastic resin layer (δ): δ-1 (polypropylene Prime Polymer F-704NP) Adhesive layer (γ): γ-1 (modified polypropylene, Mitsui Chemicals QF-500) Sealant layer (α): Resin composition obtained in Reference Example 5 above Equipment: 5-type, 5-layer inflation extrusion molding machine (Dr Collin) Die temperature: 210℃ Blow-up ratio: 2.7 Take-off speed: 4m / min Film folding width: 25cm (Conditions of extruder 1 for thermoplastic resin layer (δ)) Extruder: 30φ single screw extruder (Dr Collin) Rotation speed: 60 rpm Extrusion temperature: feeding section / compression section / metering section=170℃ / 190℃ / 210℃ (Conditions of extruder 2 for thermoplastic resin layer (δ)) Extruder: 20φ single screw extruder (Dr Collin) Rotation speed: 70 rpm Extrusion temperature: feeding section / compression section / metering section=170℃ / 190℃ / 210℃ (Conditions of extruder 3 for thermoplastic resin layer (δ)) Extruder: 20φ single screw extruder (Dr Collin) Rotation speed: 70 rpm Extrusion temperature: feeding section / compression section / metering section=170℃ / 190℃ / 210℃ (Conditions of the adhesive layer (γ) extruder) Extruder: 20φ single screw extruder (Dr Collin) Rotation speed: 70 rpm Extrusion temperature: feeding section / compression section / metering section=170℃ / 190℃ / 210℃ (Conditions of sealant layer (α) extruder) Extruder: 30φ single screw extruder (Dr Collin) Rotation speed: 24 rpm Extrusion temperature: feeding section / compression section / metering section=190℃ / 210℃ / 210℃ The obtained multilayer film was measured for OTR and width direction uniformity of OTR according to the methods described in the above evaluation methods (11) and (12). The results are shown in Table 14.

[0188] A PET film (PET12) having a thickness of 12 μm was laminated as a substrate layer (β) on the obtained multilayer film via an adhesive layer (γ), to produce a multilayer structure having a layer structure of substrate layer (β) / adhesive layer (γ) / thermoplastic resin layer (δ) / adhesive layer (γ) / sealant layer (α). When laminating the substrate layer (β), a two-liquid urethane adhesive ("Takelac A-520" and "Takenate A-50" manufactured by Mitsui Chemicals, Inc.) was applied to a dry thickness of 2 μm to provide an adhesive layer (γ'), which was then laminated by a dry lamination method to obtain a multilayer structure. The heat seal strength and appearance of the obtained multilayer structure were evaluated by the method described in the above evaluation method (13), and the results are shown in Table 12. The other evaluation results for the dried resin composition pellets of Reference Example 5 used are shown again in Tables 13 and 14.

[0189] <Example 11> In a 60 L stirring tank equipped with a jacket, a stirrer and a reflux condenser, 1.6 kg of the crude dried product of EVOH (A1) obtained in Synthesis Example 1, 0.4 kg of the crude dried product of EVOH (A7) obtained in Synthesis Example 7, 0.8 kg of water and 2.2 kg of MeOH were charged and stirred at 60°C for 5 hours to completely dissolve. To the obtained solution, sorbic acid, crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal were added. This solution was extruded through a gold plate with a diameter of 4 mm into a mixture of water / MeOH = 90 / 10 cooled to -5°C to precipitate in the form of strands, and the strands were cut into pellets with a strand cutter to obtain hydrous pellets of EVOH. The moisture content of the obtained hydrous pellets of EVOH was measured with a halogen moisture meter "HR73" manufactured by Mettler and was 52% by mass.

[0190] The obtained EVOH hydrous pellets were placed in a 1g / L aqueous acetic acid solution (bath ratio 20) and washed with stirring for 2 hours. The pellets were deliquinated and then placed in a 1g / L aqueous acetic acid solution (bath ratio 20) and washed with stirring for 2 hours. After deliquification, the aqueous acetic acid solution was renewed and the same procedure was carried out. The pellets were washed with the aqueous acetic acid solution, deliquinated, placed in ion-exchanged water (bath ratio 20), washed with stirring for 2 hours, and then deliquinated three times. The procedure was repeated until the electrical conductivity of the washing solution was 3μS / cm or less (measured with Toa Denpa Kogyo Co., Ltd.'s "CM-30ET"), and EVOH hydrous pellets from which the catalyst residue from the saponification reaction had been removed were obtained.

[0191] The obtained hydrous pellets were put into an aqueous solution (bath ratio 20) with a sodium acetate concentration of 0.510 g / L, an acetic acid concentration of 0.8 g / L, a phosphoric acid concentration of 0.04 g / L, and a boric acid concentration of 0.05 g / L, and immersed for 4 hours while stirring periodically for chemical treatment. The pellets were dehydrated and dried at 80°C for 3 hours and at 105°C for 16 hours under a nitrogen stream with an oxygen concentration of 1% by volume or less to obtain cylindrical (average diameter 2.8 mm, average height 3.2 mm) dried resin composition pellets containing EVOH (A1 and A7), acetic acid, phosphoric acid, sodium ions (sodium salts), crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal, and sorbic acid. The obtained dried resin composition pellets were evaluated according to the methods described in the above evaluation methods (2), (3), and (5) to (9). The sodium ion content in the dry resin composition pellets was 100 ppm, the phosphoric acid content was 40 ppm in terms of phosphate radical, and the acetic acid content was 200 ppm. The contents of each component other than EVOH are all based on the EVOH content. Other evaluation results are shown in Tables 13 and 14. The amount of each component added was adjusted so that the contents of crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal, and sorbic acid were as shown in Table 13.

[0192] Except for using the dried resin composition pellets obtained above, a multilayer film and a multilayer structure were produced and evaluated in the same manner as in Example 10. The results are shown in Table 14.

[0193] <Examples 13, 15, and 16, and Comparative Examples 3 and 4> As shown in Table 13, the type of EVOH (Aa), the type of EVOH (Ab), the mass ratio (Aa) / (Ab), the boric acid content, the content of unsaturated aldehyde (B), and the content of conjugated polyene (C) were changed, and the dried resin composition pellets, multilayer films, and multilayer structures were prepared and evaluated in the same manner as in Example 11. The sodium ion content in the dried resin composition pellets was 100 ppm, the phosphoric acid content was 40 ppm in terms of phosphate radical, and the acetic acid content was 200 ppm. The contents of each component other than EVOH are all amounts based on the content of EVOH. Other evaluation results are shown in Tables 13 and 14. The boric acid concentration of the aqueous solution used for the chemical treatment was appropriately adjusted so that the boric acid content of the obtained dried resin composition pellets was as shown in Table 13.

[0194] <Example 12> 80 parts by mass of the dried resin composition pellets obtained in Reference Example 5 and 20 parts by mass of the dried resin composition pellets obtained in Reference Example 3 were dry-blended to obtain a group of dried resin composition pellets. The obtained group of dried resin composition pellets was extruded using a 30 mmφ twin-screw extruder (manufactured by Japan Steel Works, Ltd., "TEX-30SS-30CRW-2V") under conditions of an extrusion temperature of 200°C, a screw rotation speed of 300 rpm, and an extrusion resin amount of 25 kg / hour, pelletized, and then dried with hot air at 80°C for 2 hours to obtain dried resin composition pellets. The obtained dried resin composition pellets were evaluated according to the methods described in the above evaluation methods (2), (3), (5) to (9), (11), and (12). The results are shown in Tables 13 and 14. A multilayer film and a multilayer structure were produced in the same manner as in Example 10, except that the dried resin composition pellets obtained above were used, and the above evaluations (13) to (15) were performed. The evaluation results are shown in Table 14.

[0195] <Example 14> Dry resin composition pellets were obtained in the same manner as in Example 11, except that 90 parts by mass of the dry resin composition pellets obtained in Reference Example 48 and 10 parts by mass of the EVOH (A9) pellets obtained in Synthesis Example 9 were dry blended. The obtained dry resin composition pellets were evaluated according to the methods described in the above evaluation methods (2), (3), (5) to (9), (11), and (12). The results are shown in Tables 13 and 14. A multilayer structure was produced in the same manner as in Example 10, except that the dry resin composition pellets obtained above were used, and the above evaluations (13) to (15) were performed. The evaluation results are shown in Table 14.

[0196] [Table 13]

[0197] [Table 14]

[0198] As shown in Tables 11 to 14, the multilayer structures prepared in Examples 1 to 15 had good heat seal strength and appearance, while the multilayer structures prepared in Comparative Examples 1 to 4 had poor heat seal strength and appearance. The resin compositions used as the raw material for the heat seal layer (α) in the Examples all had good evaluation results for die build-up and neck-in resistance, and it is presumed that these evaluation results affect the heat seal strength and appearance. In addition, from the results of each reference example, it can be seen that in the resin composition used for the sealant layer (α), when b1 / (b2+b3) is 2.0 or more and less than 150.0, the neck-in resistance is good, and when b2+2b3 is 0.65 ppm or less, the die build-up is suppressed. From this, it can be seen that a multilayer structure having good heat seal strength and appearance can be obtained by using a resin composition used for the sealant layer (α) in which b1 / (b2+b3) is 2.0 or more and less than 150.0, and b2+2b3 is 0.65 ppm or less.

[0199] For the monolayer films obtained in Examples 1 to 9, the adsorption amounts of synthetic pyrethroid and nicotine were evaluated by the following evaluation methods. (Evaluation method) After weighing 40 mg of synthetic pyrethroid or nicotine, 3 The adsorption amount was measured using a film piece of a size appropriate for the amount of adsorption, and a U-shaped SUS net was placed on top of the net so as not to come into contact with the adsorbed material. One film piece of width 1 cm and length 4 cm cut from the above single layer film was placed on the net and left for two weeks in an environment of 20°C and 50% RH. Using a film piece of a size appropriate for the amount of adsorption, the amount of adsorption was measured using the method described below. (Measurement of adsorption amount) The amount of adsorption was measured using a thermal desorption gas chromatograph-mass spectrometer (TCT-GC / MS, TCT: Chrompac "CP-4020", GC / MS: Agilent "5973") according to the following method. (Gas sampling method) The above-mentioned film piece was placed in a glass chamber heated to 80° C. Clean nitrogen was flowed from one side at a flow rate of 100 ml / min, a Tenax collection tube was attached to the other side, and the gas distilled for 3 minutes was collected as a sample. (Gas desorption conditions) The Tenax collection tube was heated to 250°C for desorption. (GC introduction method) The desorbed gas was cold-trapped at -130°C, then heated to 250°C and introduced into the column to measure the amount of adsorption. (Evaluation Criteria) Synthetic pyrethroid adsorption amount A: 1ng / cm 2 less than B: 1ng / cm 2 More than 10ng / cm 2 less than C: 10ng / cm 2 End Nicotine adsorption amount A: 500ng / cm 2 less than B: 500ng / cm 2 More than 1000ng / cm 2 less than C: 1000ng / cm 2 End

[0200] <Comparative Example 5> The adsorption amount of synthetic pyrethroid and the adsorption amount of nicotine were evaluated for the LLDPE film "TUX (trademark) MC-S" (thickness 30 μm) manufactured by Mitsui Chemicals Tocello Co., Ltd. using the above evaluation method.

[0201] The monolayer films obtained in Examples 1 to 9 were all rated "A" for the amount of synthetic pyrethroid and nicotine adsorbed, whereas the LLDPE film used in Comparative Example 5 was all rated "C" for the amount of synthetic pyrethroid and nicotine adsorbed. These evaluation results demonstrated the usefulness of the non-adsorption property of the heat seal layer (α) against such compounds.

Claims

1. The present invention comprises a sealant layer (α) made of a resin composition and a base layer (β) containing a thermoplastic resin having a melting point of 190° C. or more, the sealant layer (α) being an outermost layer, The resin composition includes an ethylene-vinyl alcohol copolymer (A) having an ethylene unit content of 20 mol% or more and 60 mol% or less and crotonaldehyde (B1), and further includes at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3); The above resin composition satisfies the following formulas (1) and (2): 2.0≦b 1 / (b 2 +b 3 )<150.0 ・・・(1) b 2 +2b 3 ≦0.65 ・・・(2) In the above formulas (1) and (2), b 1 is the content (ppm) of crotonaldehyde (B1) relative to the ethylene-vinyl alcohol copolymer (A), and b 2 is the content (ppm) of 2,4-hexadienal (B2) relative to the ethylene-vinyl alcohol copolymer (A), and b 3 is the content (ppm) of 2,4,6-octatrienal (B3) relative to the ethylene-vinyl alcohol copolymer (A).

2. In the above resin composition, the total content of crotonaldehyde (B1), 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) relative to the ethylene-vinyl alcohol copolymer (A) (b 1 +b 2 +b 3 2. The multilayer structure according to claim 1, wherein the content of 0.01 ppm or more and 7.0 ppm or less.

3. In the above resin composition, the content b of crotonaldehyde (B1) 1 The multilayer structure according to claim 1 or 2, wherein the content of the cation exchange resin is 0.01 ppm or more and 4.0 ppm or less.

4. In the above resin composition, the content b of 2,4-hexadienal (B2) 2 The multilayer structure according to claim 1 or 2, wherein the content of the cation exchange resin is 0.005 ppm or more and 0.65 ppm or less.

5. In the above resin composition, the content b of 2,4,6-octatrienal (B3) 3 The multilayer structure according to claim 1 or 2, wherein the Mn content is 0.325 ppm or less.

6. The multilayer structure according to claim 1 or 2, wherein the resin composition further contains a conjugated polyene compound (C), and the content c of the conjugated polyene compound (C) relative to the ethylene-vinyl alcohol copolymer (A) in the resin composition is 1 ppm or more and less than 300 ppm.

7. 7. The multilayer structure of claim 6, wherein the conjugated polyene compound (C) is sorbic acid.

8. 3. The multilayer structure according to claim 1, wherein the sealant layer (α) and the base layer (β) are laminated via an adhesive layer (γ).

9. 3. The multilayer structure according to claim 1, comprising a multilayer film in which a sealant layer (α), an adhesive layer (γ) and a substrate layer (β) are directly laminated in this order.

10. The ethylene-vinyl alcohol copolymer (A) comprises an ethylene-vinyl alcohol copolymer (Aa) and an ethylene-vinyl alcohol copolymer (Ab); the melting point difference (Aa-Ab) between the ethylene-vinyl alcohol copolymer (Aa) and the ethylene-vinyl alcohol copolymer (Ab) is 8°C or more; 3. The multilayer structure according to claim 1, wherein the mass ratio (Aa / Ab) of the ethylene-vinyl alcohol copolymer (Aa) to the ethylene-vinyl alcohol copolymer (Ab) is 60 / 40 or more and 95 / 5 or less.

11. 3. The multilayer structure according to claim 1, wherein at least a part of the ethylene-vinyl alcohol copolymer (A) has at least one structural unit selected from the group consisting of a structural unit represented by the following formula (I) and a structural unit represented by the following formula (II), in an amount of 0.3 mol % to 40 mol % based on all vinyl alcohol units in the at least a part of the ethylene-vinyl alcohol copolymer (A): 【Chemistry 1】 [In the above formula (I), R 1 , R 2 and R 3 R each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, or a hydroxyl group. 1 , R 2 and R 3 may be bonded to one pair (provided that R 1 , R 2 and R 3 (Except when one of the pairs is both hydrogen atoms). A portion or all of the hydrogen atoms in the aliphatic hydrocarbon group having 1 to 10 carbon atoms, the alicyclic hydrocarbon group having 3 to 10 carbon atoms, and the aromatic hydrocarbon group having 6 to 10 carbon atoms may be substituted with a hydroxyl group, an alkoxy group, a carboxyl group, or a halogen atom. In the above formula (II), R 4 , R 5 , R 6 and R 7 R each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, or a hydroxyl group. 4 and R 5 Or R 6 and R 7 may be bonded (provided that R 4 and R 5 Toga or R 6 and R 7 (However, this does not apply when both are hydrogen atoms.) Some or all of the hydrogen atoms in the aliphatic hydrocarbon group having 1 to 10 carbon atoms, the alicyclic hydrocarbon group having 3 to 10 carbon atoms, and the aromatic hydrocarbon group having 6 to 10 carbon atoms may be substituted with a hydroxyl group, an alkoxy group, a carboxyl group, or a halogen atom.]

12. 3. The multilayer structure according to claim 1 or 2, further comprising a layer (δ) containing a thermoplastic resin having a melting point of less than 190°C.

13. 3. The multilayer structure according to claim 1 or 2, wherein the heat seal strength measured in accordance with JIS Z1707 (2019) at a tensile speed of 300 mm / min when the sealant layers (α) of the multilayer structure are pressure-bonded to each other for 1 second using a hot plate heat sealer at a temperature of 200°C and a pressure of 0.1 MPa is 20 N / 15 mm or more.

14. A packaging bag comprising the multilayer structure according to claim 1 or 2.

15. A vacuum insulator comprising the multilayer structure according to claim 1 or 2.

16. The adsorption amount of synthetic pyrethroid in the sealant layer (α) is 10 ng / cm 2 3. The multilayer structure of claim 1 or 2, wherein the thickness is less than 100 nm.

17. The amount of nicotine adsorbed by the sealant layer (α) is 1000 ng / cm 2 3. The multilayer structure of claim 1 or 2, wherein the thickness is less than 100 nm.

Citation Information

Patent Citations

  • Insect-proofing material

    JP2004254599A

  • Heat seal film and wrapper bag

    JP2012041076A

  • Single-layer film, vapor-deposition film, multilayer film and heat seal film

    JP2022032037A

  • Vapor-deposited film, packaging material and vacuum insulation

    JP2023084665A

  • Resin composition containing ethylene-vinyl alcohol copolymer

    WO2013146961A1