Molded product

A resin molded article with a thermoplastic base and decorative layers achieves enhanced decorative properties and heat resistance by omitting ink components, ensuring durability and recyclability.

JP2024141813AInactive Publication Date: 2024-10-10YUPO CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023053655
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Ink compositions used for decorating resin molded articles contain additives with low heat resistance, leading to deterioration and discoloration under high temperatures, and hinder recycling through heating and melting.

Method used

A molded article with a base layer made of a thermoplastic resin and a decorative layer composed of a second thermoplastic resin, devoid of ink components, achieving opacity and whiteness values that enhance decorative properties and heat resistance.

Benefits of technology

The solution provides a molded article with excellent decorative properties and heat resistance, maintaining appearance and recyclability without ink components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141813000003
    Figure 2024141813000003
  • Figure 2024141813000004
    Figure 2024141813000004
  • Figure 2024141813000005
    Figure 2024141813000005
Patent Text Reader

Abstract

To provide a molded product with superior decorative properties and heat resistance.SOLUTION: A molded product includes a base layer and a decorative layer provided on part or all of the base layer. The base layer includes a first thermoplastic resin. The decorative layer includes a second thermoplastic resin and is substantially free of ink components. The decorative layer has an opacity of 30% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molded article having a decorative portion. [Background technology]

[0002] 2. Description of the Related Art Conventionally, plastic containers made of polyolefins such as polypropylene or polyethylene terephthalate (PET) have been widely used as beverage bottles, food storage containers, and the like.

[0003] Among such resin molded articles, there are some that have a decorative portion that is decorated with an ink composition for the purpose of improving design or the like. For example, Patent Document 1 describes a resin molded article that is decorated with an ink composition. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-220151 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the ink composition usually contains additives such as auxiliaries and adhesives in addition to coloring components such as dyes and pigments, and some of these additives have low heat resistance. For example, acrylic adhesives, which are general-purpose adhesives, deteriorate and become discolored when exposed to heat. Therefore, resin molded products having decorative parts decorated with the ink composition have poor suitability for use in high-temperature environments and poor suitability for resin recycling by heat melting.

[0006] The present invention has been made in consideration of the above-mentioned conventional circumstances, and has an object to provide a resin molded article that is excellent in both decorativeness and heat resistance. [Means for solving the problem]

[0007] As a result of intensive research into solving the above-mentioned problems, the inventors have found that in a molded body having a base layer and a decorative layer, the above-mentioned problems can be solved by making the decorative layer contain a thermoplastic resin, substantially contain no ink components, and have an opacity of a predetermined value or less, thereby solving the present invention.

[0008] That is, the present invention solves the problems by the following means. [1] A molded body having a base layer and a decorative layer provided on a part or the whole of the base layer, the base layer comprises a first thermoplastic resin; the decorative layer contains a second thermoplastic resin and is substantially free of an ink component; The opacity (Haze) of the decorative layer is 30% or more. Molded body. [2] The molded article according to [1] above, wherein the whiteness (W) of the decorative layer is 80% or more. [3] The decorative layer is provided on a part of the base layer, The difference in opacity (ΔHaze) between the base layer and the decorative layer is 3% or more. The molded article according to the above [1] or [2]. [4] The decorative layer is provided on a part of the base layer, The difference in whiteness (ΔW) between the base layer and the decorative layer is 3% or more; The molded article according to the above [1] or [2]. [5] The molded article according to the above [1] or [2], wherein the void ratio of the decorative layer is 10% or more. [6] The molded article according to [1] or [2] above, wherein the decorative layer contains a filler. [7] The molded article according to [1] or [2] above, wherein the decorative layer has a thickness of 5 μm or less. [8] The molded body according to [1] or [2] above, wherein the first thermoplastic resin and the second thermoplastic resin contain the same resin. Effect of the Invention

[0009] According to the present invention, a molded article having excellent decoratability and heat resistance can be provided. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of one aspect of a molded article according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of another aspect of the molded article according to the embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view of a film for forming a decorative layer used in the production of a molded article according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The molded body of the present invention will be described in detail below. The following description of the constituent elements may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In the present invention, "to" means a range including the numerical values ​​before and after it as the minimum and maximum values, respectively. In the present invention, "parts by weight" and "parts by mass", "% by weight" and "% by mass" each have the same meaning. In addition, the embodiments shown in the drawings are schematic in order to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the actual provided object.

[0012] [Molded body] The molded body according to the embodiment of the present invention is a molded body having a base layer and a decorative layer provided on a part or the entirety of the base layer, the base layer comprises a first thermoplastic resin; the decorative layer contains a second thermoplastic resin and is substantially free of an ink component; The decorative layer has an opacity (haze) of 30% or more.

[0013] [Base layer] In an embodiment of the present invention, the base layer is a layer that constitutes a main body of the molded article. The base layer includes a first thermoplastic resin.

[0014] (1st thermoplastic resin) The type of the first thermoplastic resin used in the base layer is not particularly limited, and can be selected from a wide variety of thermoplastic resins. For example, olefin-based resins; polyamide-based resins such as nylon-6,6; thermoplastic polyester-based resins such as polyethylene terephthalate or its copolymer, polybutylene succinate, polylactic acid, and other aliphatic polyesters; polycarbonate; styrene-based resins, etc., are listed, and olefin-based resins are preferred. These may be used alone or in combination.

[0015] Olefin resin Specific examples of the olefin resin include polypropylene, polyethylene such as high density polyethylene, medium density polyethylene, linear low density polyethylene, etc. Among these, polypropylene is preferable.

[0016] ··polypropylene The polypropylene is not particularly limited as long as propylene is used as the main monomer. For example, propylene homopolymer, propylene-α-olefin copolymer, which is a copolymer of propylene as the main component and α-olefin such as ethylene or 1-butene, and the like, can be mentioned. Among them, propylene homopolymer is preferable. The copolymer may be a multi-component system, and may be a random copolymer or a block copolymer. Furthermore, propylene homopolymer and propylene copolymer may be used in combination.

[0017] As the polypropylene, a graft-modified product thereof may be used as necessary from the viewpoint of improving the adhesion between the base layer and the adjacent layer or the moldability.

[0018] (Other Ingredients) If necessary, the base layer may contain fillers, heat stabilizers (antioxidants), light stabilizers, dispersants, lubricants, nucleating agents, and the like, as long as the effects of the present invention are not impaired. Examples of the filler include inorganic fillers and organic fillers that can be contained in the decorative layer described below.

[0019] The opacity (haze) of the base layer is not particularly limited, but may be, for example, 20 to 90%, and preferably 50 to 85%. The whiteness (W) of the base layer is not particularly limited, but may be, for example, 20 to 95%, and preferably 50 to 90%. The opacity and whiteness of the base layer can be measured in the same manner as the measurement of the opacity and whiteness of the decorative layer described below, except that the opacity and whiteness of the base layer are measured only for the base layer.

[0020] The thickness of the base layer is not particularly limited and can be appropriately selected depending on the application of the molded article, but is, for example, in the range of 20 to 200 μm, preferably 40 to 100 μm.

[0021] [Decorative layer] The molded article according to the embodiment of the present invention has a decorative layer provided on a part or the whole of the base layer. The decorative layer constitutes a decorative part that decorates the main body of the molded article of the present invention. The decorative layer contains a second thermoplastic resin, is substantially free of ink components, and has an opacity (haze) of 30% or more.

[0022] In this embodiment, the decorative layer does not substantially contain ink components. The ink components refer to coloring components such as dyes and pigments, as well as components typically contained in ink compositions such as auxiliaries and adhesives. Here, the decorative layer does not substantially contain ink components means that the decorative layer does not contain ink components to the extent that it has the function of improving the visibility of the pattern, and for example, the content of the ink components per decorative layer is 5% by mass or less. Additives that are typically added to ink compositions include compounds with low heat resistance. However, in an embodiment of the present invention, the ink composition is substantially free of ink components, and therefore, thermal degradation caused by these compounds does not occur.

[0023] In this embodiment, the opacity (haze) of the decorative layer is 30% or more. By setting the opacity to 30% or more, it is possible to obtain visibility similar to that of a decorative layer using ink, and it is possible to function as a decorative layer. The opacity may be 30% or more, and is preferably 50% or more, more preferably 80% or more, even more preferably 90% or more, and particularly preferably 95% or more. The upper limit is 100%.

[0024] The opacity (haze) of the decorative layer can be measured in accordance with JIS-K-7136:2000, not by cutting out just the decorative layer and measuring it, but with the base layer also present (i.e., when it is a molded body with a decorative layer).

[0025] In addition, in this embodiment, the whiteness (W) of the decorative layer is preferably 80% or more. By making the whiteness 80% or more, it is possible to obtain visibility close to that of a decorative layer using ink, and the decorative layer is excellent. The whiteness is more preferably 85% or more, and even more preferably 90% or more. From the viewpoint of feasibility, the upper limit is preferably 99% or less, and more preferably 95% or less.

[0026] The whiteness (W) of the decorative layer can be measured in accordance with JIS-L1015:2021, not by cutting out only the decorative layer, but also with the base layer (i.e., in the state where it is a molded body having a decorative layer).

[0027] Specific means for achieving the opacity of the decorative layer within the above range without substantially using ink components include, for example, a method of forming a brittle and weak decorative precursor layer and destroying the decorative precursor layer to obtain a decorative layer with an opacity of 30% or more; a method of increasing the opacity to 30% or more by adding a filler; and a method of increasing the opacity to 30% or more by embossing. Of these, the method of forming a brittle and weak decorative precursor layer and destroying the decorative precursor layer to obtain a decorative layer with an opacity of 30% or more is preferred. The decorative layer in each case will be described in detail below.

[0028] <<First Aspect>> A first preferred embodiment is a embodiment in which a decorative precursor layer which is brittle and has low strength is formed on a base layer, and then the decorative precursor layer is destroyed to form a decorative layer having an opacity of 30% or more. Specifically, first, a film 3 for forming a decorative layer shown in FIG. 3 is prepared. The film 3 for forming a decorative layer is a film obtained by laminating a base layer 13 and a decorative precursor layer 12', and preferably further stretching the film, and in the film, the decorative precursor layer is a layer that is more brittle and weaker in strength than the base layer. When the film for forming a decorative layer is peeled off from a laminate in which such a film for forming a decorative layer and a base layer are laminated by in-mold molding so that the base layer and the decorative precursor layer are in contact with each other, the base layer can be easily peeled off from the laminate with the base layer due to the destruction of the decorative precursor layer, and the decorative precursor layer remaining on the surface of the base layer side after peeling becomes the decorative layer. The first embodiment is an embodiment in which the opacity of the decorative layer is 30% or more by the peeling operation. That is, the composition of each component contained in the decorative precursor layer and the decorative layer is the same. In the first embodiment, in order to facilitate the destruction of the decorative precursor layer, the decorative layer may be formed by blending a filler and stretching the layer to make it porous, by blending at least two mutually incompatible resins to form an interface between the incompatible resins, or by combining the above two methods. Among these, the method of blending a filler and stretching the layer to make it porous is preferred.

[0029] <Aspect 1A> First, a preferred embodiment in which the whiteness (W) of the decorative layer is within the above-mentioned preferred range will be described.

[0030] (Second thermoplastic resin) As the second thermoplastic resin, the same resins as those listed as the first thermoplastic resin can be used.

[0031] In the present invention, the term "incompatible" between two resins means that when a blend of the resins is observed under an electron microscope, it has a morphology of an island-sea structure, and the dimensions of the structure are 0.3 to 10 μm.

[0032] (Filler) The decorative layer preferably contains a filler in addition to the second thermoplastic resin. By stretching the decorative layer while containing the filler, a large number of voids (holes) are formed in the decorative layer, which makes it more susceptible to cohesive failure and exhibits fracturing suitability. The filler may be an inorganic filler or an organic filler, or a combination of these may be used. Examples of the inorganic filler include heavy calcium carbonate, light calcium carbonate, calcined clay, talc, titanium oxide, and other inorganic fillers, composite inorganic fillers having aluminum oxide or hydroxide around the core of the inorganic filler, hollow glass beads, etc. In the embodiment 1A, heavy calcium carbonate is preferred among them because it is inexpensive and can form many voids during stretching. If there are many voids, the molten resin will enter the openings on the surface of the decorative precursor layer due to the resin pressure during molding of the laminate of the base layer and the film for forming the decorative layer, and the film's adhesion to the base layer will be improved due to the anchoring effect. In addition, the void ratio of the decorative layer obtained by peeling off the film for forming the decorative layer will be improved, and not only will the desired whiteness be easily obtained, but cohesive failure will be easily caused, making it easier to function as a decorative part.

[0033] As the organic filler, it is preferable to select a resin different from the polypropylene resin used as the second thermoplastic resin. For example, a polymer such as polyethylene terephthalate, polycarbonate, polystyrene, polymethacrylate, etc., which has a melting point (e.g., 170 to 300°C) or a glass transition temperature (e.g., 170 to 280°C) higher than the melting point of the polypropylene resin and is incompatible with the polypropylene resin, can be used.

[0034] In an embodiment of the present invention, the void ratio of the decorative layer is preferably 10% or more. If the void ratio of the decorative layer is 10% or more, the light incident on the decorative layer is easily diffused, and the desired whiteness is easily obtained, which is preferable. From the same viewpoint, the void ratio of the decorative layer is more preferably 15% or more, and further preferably 20% or more. From the viewpoint of molding stability, the void ratio is preferably 50% or less, and more preferably 40% or less.

[0035] The void ratio of the decorative layer can be determined as the ratio of the area occupied by voids by observing the decorative layer with an electron microscope and analyzing the observed image. A specific measuring method will be described in the Examples section.

[0036] As the filler, it is preferable to use at least one of the above-exemplified inorganic fillers whose surface has been hydrophilized with a surface treatment agent. The surface treatment agent includes water-soluble anionic surfactants, water-soluble cationic surfactants, and water-soluble nonionic surfactants.

[0037] In the embodiment 1A, the decorative layer contains 40 to 70% by mass, preferably 50 to 65% by mass, of a filler, and the decorative layer is preferably stretched in at least one axial direction. By making the content of the filler in the decorative layer 40% by mass or more, sufficient peelability can be obtained when peeling off the film for forming the decorative layer. Also, by making the content of the filler in the decorative layer 70% by mass or less, molding stability can be obtained.

[0038] (Resin incompatible with the second thermoplastic resin) In the embodiment 1A, the decorative layer preferably contains a resin that is incompatible with the second thermoplastic resin. The presence of at least two mutually incompatible resins allows interfacial peeling to occur between the incompatible resins during the preparation of the stretched film, improving the peelability. In the present invention, the term "incompatible" between two resins means that when a blend of the resins is observed under an electron microscope, it has a morphology of a sea-island structure, and the dimensions of the structure are 0.3 to 10 μm.

[0039] The decorative layer may further contain the additives listed as (other components) of the base layer within the range that does not impair the effects of the present invention.

[0040] (Method of Manufacturing Molded Product) The molded body of embodiment 1A can be obtained by laminating a base layer and a decorative precursor layer, stretching the resulting film for forming a decorative layer, and laminating the resulting film and base layer by in-mold molding, and then peeling off the film for forming a decorative layer.

[0041] ·Manufacture of films for decorative layer formation The film for forming a decorative layer has a base layer and a decoration precursor layer. The base layer includes a third thermoplastic resin, which may be any of the thermoplastic resins listed above as the first thermoplastic resin. The base layer may contain the additives listed in the (other components) of the base layer within the range that does not impair the effects of the present invention. The base layer may be of a single layer structure or of a multi-layer structure having two or more layers. The thickness of the base layer is not particularly limited, but is, for example, in the range of 10 to 500 μm.

[0042] The components contained in the decorative precursor layer are the same as the components contained in the decorative layer described above. The thickness of the decorative precursor layer is, for example, in the range of 0.1 to 20 μm. In the first embodiment, since the decorative layer is obtained by destroying the decorative precursor layer, the thickness of the decorative layer is equal to or less than the thickness of the decorative precursor layer.

[0043] Various known methods can be used to laminate the base layer and the decorative precursor layer, and specific examples include a multi-layer die method using multiple extruders and feed blocks, a multi-manifold, and a multi-layer die, and an extrusion lamination method using multiple extruders and dies, etc. It is also possible to use a combination of the multi-layer die method and the extrusion lamination method.

[0044] Various known methods can be used for stretching. The stretching temperature can be within a known temperature range suitable for the thermoplastic resin, which is from the glass transition temperature of the thermoplastic resin mainly used in the base layer to the melting point of the crystalline portion. The stretching ratio is not particularly limited, but when the number of stretching axes is uniaxial, the stretching ratio is usually 2 to 11, and preferably 3 to 10. When the number of stretching axes is biaxial, the area ratio is usually 2 to 80, preferably 3 to 60, and more preferably 4 to 50.

[0045] It is preferable to subject the laminated resin film after stretching to a heat treatment, which reduces the thermal shrinkage rate in the stretching direction and reduces waviness due to shrinkage during in-mold molding.

[0046] In-mold molding Next, the film for forming a decorative layer and the base layer are laminated by in-mold molding, so that the film for forming a decorative layer and the base layer are in contact with each other. The molding method is preferably direct blow molding, in which a molten resin parison is pressed against the inner wall of a mold using compressed air, or stretch blow molding using a preform, but it may also be injection molding, in which molten resin is injected into a mold using an injection device and cooled and solidified, or differential pressure molding using a differential pressure molding mold.

[0047] ·Removal of film for decorative layer formation The film for forming a decorative layer is peeled off from the resulting laminate of the film for forming a decorative layer and the base layer. The decorative precursor layer is destroyed by the peeling, and the decorative precursor layer remaining on the base layer side becomes the decorative layer.

[0048] <Aspect 1B> Next, a preferred embodiment of a decorative layer with reduced whiteness will be described.

[0049] (Second thermoplastic resin) As the second thermoplastic resin, the same resins as those listed as the first thermoplastic resin can be used.

[0050] (Resin incompatible with the second thermoplastic resin) In the embodiment of 1B, the decorative layer preferably contains a resin that is incompatible with the second thermoplastic resin. The presence of at least two mutually incompatible resins can improve the peelability by causing interfacial peeling between the incompatible resins during the preparation of the stretched film. Examples of incompatible resins include styrene-based resins, polycarbonate resins, and ester-based resins. Among them, styrene-based resins are preferred.

[0051] The resin incompatible with the second thermoplastic resin is blended in an amount of 50 to 200 parts by mass, preferably 80 to 120 parts by mass, per 100 parts by mass of the second thermoplastic resin.

[0052] (Filler) The decorative layer may contain a filler in addition to the second thermoplastic resin to the extent that the whiteness is not excessively increased. As the filler, the fillers described in the first embodiment A above can be used.

[0053] The decorative layer may contain the additives listed in the (other components) of the base layer within the range that does not impair the effects of the present invention.

[0054] (Method of Manufacturing Molded Product) The molded article of the embodiment 1B, like the embodiment 1A described above, can be obtained by peeling off the film for forming a decorative layer from a laminate in which a film for forming a decorative layer and a base layer are laminated by in-mold molding.

[0055] ·Manufacture of films for decorative layer formation The film for forming a decorative layer has a base layer and a decoration precursor layer. The base layer may be the same as the base layer described in embodiment 1A.

[0056] The components contained in the decorative precursor layer are the same as the components contained in the decorative layer described above. The thickness of the decorative precursor layer is, for example, in the range of 0.1 to 20 μm.

[0057] In the embodiment 1B, the film for forming a decorative layer preferably has a heat seal layer on the surface of the decorative precursor layer opposite to the base layer, from the viewpoint of improving adhesion to the base layer.

[0058] The main component of the heat seal layer is not particularly limited as long as it can provide heat sealability, but it is preferable to use a low-melting-point resin that has a lower melting point than the olefin-based resins contained in the base layer and the decoration precursor layer and that facilitates heat sealing. The low-melting-point resin is a thermoplastic resin having a melting point of 135° C. or less. Specific examples include homopolymers of olefins such as ethylene and propylene, and copolymers of two or more of these olefins.

[0059] The heat seal layer preferably contains an olefin-based elastomer from the viewpoints of interlayer adhesion with the decoration precursor layer and of imparting strength. The heat seal layer may further contain the additives listed in the (other components) of the base layer within the range that does not impair the effects of the present invention.

[0060] The thickness of the heat seal layer is preferably 1 μm or more and 50 μm or less.

[0061] With regard to the lamination method of each layer and the stretching of the film, the description of the embodiment 1A may be cited.

[0062] The description of the embodiment 1A may also be applied to the in-mold molding and peeling off of the film for forming a decorative layer. When the film for forming a decorative layer has a heat seal layer, the film for forming a decorative layer and the base layer are laminated together so that the heat seal layer and the base layer are in contact with each other during in-mold molding.

[0063] <<Second aspect>> A second preferred embodiment is a decorative layer in which the opacity (haze) is increased to 30% or more by adding a filler.

[0064] (Second thermoplastic resin) In the second embodiment, the second thermoplastic resin in the decorative layer may be, for example, the thermoplastic resin listed as the first thermoplastic resin, and from the viewpoint of mono-material, it is preferable to use the same resin as the resin used in the base layer.

[0065] (Filler) In the second embodiment, the decorative layer contains a filler in addition to the second thermoplastic resin. As the filler, the fillers described in the first embodiment A above can be used.

[0066] From the viewpoint of the whiteness (W) of the decorative layer, calcium carbonate is preferred as the filler.

[0067] In the second embodiment, the filler is preferably contained in an amount of 10 to 50% by mass, more preferably 15 to 30% by mass, based on 100 parts by mass of the second thermoplastic resin. By making the amount 10% by mass or more, it is easy to obtain the desired opacity and whiteness. Also, by making the amount 50% by mass or less, molding stability is obtained.

[0068] In the second embodiment, the decorative layer may contain the additives listed in the (other components) of the base layer within the range that does not impair the effects of the present invention.

[0069] The method for producing the molded body of the second embodiment is not particularly limited, but for example, a film for forming a decorative layer may be prepared in the same manner as in the first embodiment, and the film and the base layer may be laminated by in-mold molding. In the second embodiment, the film for forming a decorative layer does not need to be peeled off, and the decoration precursor layer becomes the decorative layer as it is. In addition, for example, a decorative layer film having an opacity of 30% or more by adding a separately prepared filler may be attached via an adhesive layer to the surface of a base layer formed by a known resin molding method such as injection molding.

[0070] <<Third Aspect>> A third preferred embodiment is a decorative layer having an opacity of 30% or more by performing a surface treatment such as embossing.

[0071] (Second thermoplastic resin) In the third embodiment, the second thermoplastic resin contained in the decorative layer may be, for example, the thermoplastic resin listed as the first thermoplastic resin, and from the viewpoint of mono-material, it is preferable to use the same resin as the resin used in the base layer.

[0072] In the third embodiment, the decorative layer may contain the additives listed in the (other components) of the base layer within the range that does not impair the effects of the present invention.

[0073] The manufacturing method of the molded body of the third embodiment is not particularly limited, but for example, a base layer may be molded by a known resin molding method such as injection molding, and a decorative layer that has been embossed on the surface of the molded base layer may be attached by a known method.

[0074] In the molded body according to the embodiment of the present invention, the thickness of the decorative layer is not particularly limited, and may be, for example, 20 μm or less, but from the viewpoint of improving the recyclability of the molded body, it is preferable that it is 5 μm or less. By making it 5 μm or less, the mass ratio of the decorative layer in the molded body can be reduced. That is, the ratio of the second thermoplastic resin to the first thermoplastic resin in the molded body is reduced, and impurities can be reduced when the molded body is melted and reused. More preferably, it is 3 μm or less. From the viewpoints of uniformity and visibility of the decoration, the thickness of the decorative layer is preferably 0.1 μm or more.

[0075] Furthermore, from the viewpoint of recyclability, in the molded body according to the embodiment of the present invention, it is preferable that the first thermoplastic resin and the second thermoplastic resin contain the same resin, and it is more preferable that the same resin is the main component. Specifically, it is preferable that both the first thermoplastic resin and the second thermoplastic resin contain an olefin resin, and it is more preferable that both contain polypropylene.

[0076] [Shape of Molded Product] The shape of the molded body according to the embodiment of the present invention is not particularly limited, and as long as it is a molded body having the above-mentioned base layer and the above-mentioned decorative layer provided on a part or the entirety of the base layer, it may be a three-dimensional molded body or a planar (sheet-like) molded body. FIG. 1 is a schematic cross-sectional view of one aspect of a molded article according to an embodiment of the present invention, which is a molded article having a decorative layer provided over the entirety of a base layer. Fig. 2 is a schematic cross-sectional view of another embodiment of the molded body according to the present invention, which is a molded body having a decorative layer provided on a part of a base layer. Fig. 2 is a schematic cross-sectional view of a molded body produced by laminating a film for forming a decorative layer and a base layer by in-mold molding and peeling off the film for forming a decorative layer.

[0077] In this specification, "the decorative layer is provided over the entire base layer" means that the decorative layer is provided over one entire main surface of the base layer. That is, as shown in FIG. 1, the decorative layer 12 may be provided over the entire surface of one side of the base layer 11 in the molded body 1, and may not be provided over the other surface. In addition, the decorative layer may not be provided on the side surface of the base layer, i.e., in the thickness direction of the base layer.

[0078] A preferred embodiment of the molded article of the present invention is a molded article in which a decorative layer is provided on a part of a base layer, and the difference in opacity (ΔHaze) between the base layer and the decorative layer is 3% or more. The ΔHaze is more preferably 5% or more, even more preferably 10% or more, particularly preferably 15% or more, and may be 80% or less. In such a molded article, contrast is generated in the molded article, and the decorative layer has excellent visibility and decorativeness.

[0079] A preferred embodiment of the molded article of the present invention is a molded article in which a decorative layer is provided on a part of a base layer, and the difference in whiteness (ΔW) between the base layer and the decorative layer is 3% or more. The ΔW is more preferably 4% or more, further preferably 10% or more, and may be 80% or less. In such a molded article, contrast is generated in the molded article, and the decorative layer has excellent visibility and decorativeness.

[0080] When the molded article is a three-dimensional molded article, the molded article is preferably a container. When the molded article is a container, the decorative layer is preferably provided on a part or the whole of the outer surface of the base layer, i.e., the layer forming the container body.

[0081] The molded article of the present invention can be used, for example, as a bottle, a container, a squeeze container, etc. for medicines or foods. It can also be used as stationery such as writing pads and clear files. EXAMPLES

[0082] The present invention will be described in more detail below with reference to examples and test examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. may be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. The raw materials used in each Example and Comparative Example are listed in Table 1. Table 2 lists the types (symbols) and amounts (weight%) of the thermoplastic resin and filler materials used in producing the molded bodies (decorative layer, base layer) of each Example and Comparative Example, as well as the evaluation results. The material symbols listed in Table 2 correspond to the material symbols listed in Table 1.

[0083] [Table 1]

[0084] [Table 2]

[0085] [Example 1] <Preparation of Molded Body> (Preparation of film for forming decorative layer) The compound [A1] described in Table 2 was melt-kneaded in an extruder set at 250 ° C, extruded into a sheet through a die, and cooled to 70 ° C in a cooling device to obtain a single-layer unstretched sheet. After reheating this unstretched sheet to 145 ° C, it was stretched 5 times in the longitudinal direction using the peripheral speed difference between many rolls to obtain a longitudinal uniaxially stretched film. Next, the compound [A2] and compound [B] described in Table 2 were melt-kneaded in an extruder set at 250 ° C individually, extruded into a sheet through a die, and compound [A2] was laminated on one side of the longitudinal uniaxially stretched film and compound [B] was laminated on the other side, respectively, to obtain a laminate having a three-layer structure of [A2] / [A1] / [B]. Next, the laminate was reheated to 158 ° C using an oven, and then stretched 9 times in the transverse direction using a tenter stretching machine to obtain a three-layer laminated resin film with a uniaxial stretching / biaxial stretching / uniaxial stretching structure, which was used as a film for forming a decorative layer. [A2] and [A1] correspond to the base layer, and [B] corresponds to the decoration precursor layer.

[0086] (Preparation of Molded Body) [Injection molding] Using an injection molding machine (Niigata Iron Works Co., Ltd., model: NV50ST, clamping force: 50 tons, vertical arrangement) and a split mold for injection molding that would produce a resin molded product with a flat plate size of 130 mm wide, 150 mm long, and 1 mm thick, the decorative layer forming film obtained above was cut into a size of 100 mm wide and 130 mm long, and the film was fixed to the surface of the female mold attached to the lower fixed platen side so that the base layer side was in contact with the mold. Then, the split mold was clamped, and molten polystyrene (PS Japan Co., Ltd., product name: HIPS 433, MFR: 21 g / 10 min (200 °C, 5 kg load), melting start temperature: approximately 95 °C) was injected at 745 kgf / cm from an injection unit set at 200 °C. 2 The molten resin was injected into the mold from the gate at a pressure of 1000 MPa, and the molten resin was cooled and solidified while the film was adhered. The mold was then opened to obtain a flat PS injection-molded product with the film adhered thereto, which was designated as film-attached resin molded product 1. The film for forming a decorative layer was then peeled off from the obtained resin molded article 1 with a film at a peeling speed of 300 mm / min to obtain a molded article 1 which was a laminate of the base layer and the decorative layer.

[0087] [Comparative Example 1] <Preparation of Molded Body> Except for not using the film for forming the decorative layer, a resin molded product was produced by injection molding in the same manner as in Example 1. Next, ink (Bestcure UV161 (white), manufactured by T&K Toka Co., Ltd.) was applied to the resin molded product at a rate of 1.5 g / m using a printing machine (RI-3 type printability tester, manufactured by Kokubo Seimitsu Co., Ltd.). 2 After printing, the resin film was irradiated with 100 mJ / cm 2 of ultraviolet light using a UV irradiator. 2 The ultraviolet-curable ink was dried under the above conditions using ultraviolet light (ECS-401GX, manufactured by iGraphics Co., Ltd.), to obtain a molded body 2 which is a laminate of a base layer and an ink-decorated layer.

[0088] [evaluation] The opacity (Haze) of the decorative layer, the difference in opacity between the decorative layer and the base layer (ΔHaze), the whiteness (W) of the decorative layer, the difference in whiteness (ΔW) between the decorative layer and the base layer, the void ratio of the decorative layer, and the thickness of the decorative layer were measured by the following methods. The heat resistance of the obtained molded body was also evaluated by the following methods. The evaluation results are shown in Table 2 above.

[0089] <Opacity (Haze)> (Decorative layer opacity (Haze)) The opacity of the decorative layer was measured in accordance with JIS-K-7136:2000 using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name: NDH2000). In the examples and comparative examples, a test piece measuring 3 cm×3 cm was cut out with a cutter from the portion of the obtained molded article where the decorative layer was provided, and used as a test sample.

[0090] (Opacity difference (ΔHaze)) In the examples and comparative examples, a 3 cm x 3 cm test piece was cut out with a cutter from a part of the obtained molded product where no decorative layer was provided, and used as a test sample. The opacity of the base layer was measured in the same manner as described above, and the difference in opacity between the decorative layer and the base layer was calculated.

[0091] <Heat resistance> The molded products obtained in the examples and comparative examples were melt-kneaded again in an extruder set at 250°C and pelletized to obtain remelted pellets. Meanwhile, the blend used to manufacture the base layer ([A2] / [A1]) was made into virgin pellets. The color and MFR were measured for both the remelted pellets and the virgin pellets, and the heat resistance of the resin composition was evaluated from the amount of change. (color difference ΔE) About 5 g each of the remelted pellets and the virgin pellets was hydraulically pressed at 230° C. using a compression molding machine (Mini Test Press MP-WC, manufactured by Toyo Seiki Seisakusho Co., Ltd.) to obtain a disk-shaped resin sheet for evaluation having a diameter of about 50 mm and a thickness of about 2 mm. Next, the lightness L* value and color coordinate a* value and b* value of the obtained resin sheet for evaluation before and after heating were measured using a color meter (touch panel type color computer SM-T, manufactured by Suga Test Instruments Co., Ltd.), and the color difference ΔE*ab in the L*a*b* display system was calculated, and this was defined as the color difference ΔE. (ΔMFR) The MFR of the remelted pellets and the virgin pellets was measured according to JIS-K7210: 1999. Next, the difference in MFR value before and after heating (MFR value after heating - MFR value before heating) was calculated and this was taken as ΔMFR. (evaluation) ○(Acceptable): ΔE is 5 or less and ΔMFR is 5g / 10min or less × (Not acceptable): ΔE is greater than 5 or ΔMFR is greater than 5g / 10min

[0092] <Whiteness> (Whiteness of decorative layer (W)) The whiteness of the decorative layer was measured in accordance with JIS-L1015:2021. In the examples and comparative examples, a test piece measuring 3 cm×3 cm was cut out with a cutter from the portion of the obtained molded article where the decorative layer was provided, and used as a test sample.

[0093] (Whiteness difference (ΔW)) In the examples and comparative examples, a 3 cm x 3 cm test piece was cut out with a cutter from a portion of the obtained molded product where no decorative layer was provided, and used as a test sample. The whiteness of the base layer was measured in the same manner as described above, and the difference in whiteness between the decorative layer and the base layer was calculated.

[0094] <Void ratio of decorative layer> A test sample similar to the test sample for the opacity of the decorative layer was embedded in epoxy resin and solidified, and then a cut surface parallel to the thickness direction of the test sample (i.e. perpendicular to the surface direction) was prepared using a microtome. This cut surface was metallized by deposition, and then observed at 3000 times magnification using an electron microscope (Hitachi, Ltd., scanning microscope S-2400). The voids in the decorative layer were traced on a tracing film and filled in, and the image was processed using an image analyzer (Nireco Corporation: Luzex IID model), and the area ratio (%) of the voids occupying the measurement range was calculated to determine the void ratio (%) of the decorative layer.

[0095] <Thickness of decorative layer> Using the same test sample as the test sample for the opacity of the decorative layer, a cut surface parallel to the thickness direction of the test sample (i.e. perpendicular to the surface direction) was prepared using a microtome. This cut surface was observed at 3000 times magnification using an electron microscope (S-2400 scanning microscope, manufactured by Hitachi, Ltd.), and the thickness of the decorative layer laminated on the base layer was determined as the thickness of the decorative layer.

[0096] As is clear from the results in Table 2, an opaque decorative layer was obtained without using ink, and a molded product with excellent heat resistance was obtained in Example 1. The decorative layer of the molded product in Example 1 was obtained by peeling off the decorative layer-forming film, and thus had a unique texture like Japanese paper. On the other hand, in Comparative Example 1, since the decorative layer contained an ink component, the heat resistance was poor. [Explanation of symbols]

[0097] 1, 2 Molded body 3 Film for forming decorative layer 11 Base Layer 12 Decorative layer 12' Pre-decoration layer 13 Base layer

Claims

1. A molded body having a base layer and a decorative layer provided on a part or the entirety of the base layer, the base layer comprises a first thermoplastic resin; the decorative layer contains a second thermoplastic resin and is substantially free of an ink component; The opacity (haze) of the decorative layer is 30% or more. Molded body.

2. The molded article according to claim 1 , wherein the decorative layer has a whiteness (W) of 80% or more.

3. The decorative layer is provided on a part of the base layer, The difference in opacity (ΔHaze) between the base layer and the decorative layer is 3% or more. The molded article according to claim 1 or 2.

4. The decorative layer is provided on a part of the base layer, The difference (ΔW) in whiteness between the base layer and the decorative layer is 3% or more; The molded article according to claim 1 or 2.

5. The molded article according to claim 1 , wherein the decorative layer has a void ratio of 10% or more.

6. The molded article according to claim 1 , wherein the decorative layer contains a filler.

7. The molded article according to claim 1 or 2, wherein the decorative layer has a thickness of 5 μm or less.

8. The molded article according to claim 1 , wherein the first thermoplastic resin and the second thermoplastic resin contain the same resin.

Citation Information

Patent Citations

  • Joining method and device made by this method, joining apparatus, and substrate joined by this method

    JP2009220151A