Multilayer porous film

A multilayer porous membrane with a polyolefin resin microporous base and inorganic particle layer addresses the challenge of thinner separators by balancing heat resistance, strength, and friction, improving energy density and safety in non-aqueous electrolyte batteries.

JP2024141951APending Publication Date: 2024-10-10ASAHI KASEI KOGYO KABUSHIKI KAISHA

Patent Information

Application Number
JP2023053853
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing non-aqueous electrolyte batteries face challenges in achieving thinner separators with improved heat resistance, strength, and reduced surface friction, which are essential for enhancing energy density and safety.

Method used

A multilayer porous membrane comprising a microporous membrane made of polyolefin resin with a porous layer containing inorganic particles, where the particle size, mass and volume percentage of inorganic particles, and friction coefficients are specified to balance heat resistance, strength, and friction, thereby enabling thinner separators with reduced surface friction.

Benefits of technology

The multilayer porous membrane effectively suppresses overall friction, improves heat resistance and strength, and enhances energy density while ensuring safety and pin removal properties in non-aqueous electrolyte batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141951000001_ABST
    Figure 2024141951000001_ABST
Patent Text Reader

Abstract

To provide a multilayer porous film which can suppress whole friction of a separator surface, and improve heat resistance (namely, thermal contraction suppression ability) and intensity, and also can improve energy density of a non aqueous electrolyte battery, a non aqueous electrolyte battery separator and a non aqueous electrolyte battery including the same.SOLUTION: There is provided a multilayer porous film comprising: a minute porous film which contains, a polyolefin resin as a main component; and a porous layer which includes inorganic particles and is laminated on at least one surface of the minute porous film, where an average particle diameter D50 of the inorganic particles is 0.01 μm or more and less than 0.60 μm, and a mass ratio of the inorganic particles in the porous layer is greater than 80%, a volume ratio of the inorganic particles in the porous layer is greater than 70%. A surface static friction coefficient of the porous layer is 0.01 or more and 0.40 or less, and a surface dynamic friction coefficient of the porous layer is 0.01 or more and 0.35 or less in the multilayer porous film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer porous membrane, and more particularly to a multilayer porous membrane that is suitably used as a separator disposed between a positive electrode and a negative electrode in a nonaqueous electrolyte battery. [Background technology]

[0002] Conventionally, in non-aqueous electrolyte batteries, an electrolytic solution is impregnated into a power generating element in which a separator is interposed between a positive electrode plate and a negative electrode plate. In general, separators are required to have ion permeability and safety such as a shutdown function, and therefore separators having a microporous membrane containing a polyolefin resin are used. Furthermore, from the viewpoints of electrical insulation during thermal runaway, heat resistance, strength, safety of non-aqueous electrolyte batteries, and cycle characteristics, a multilayer porous membrane or a porous film in which a porous layer containing inorganic particles is laminated or coated on a polyolefin microporous membrane is also being considered as a separator (Patent Documents 1 to 9).

[0003] Patent Documents 1 to 4 describe the friction coefficient of a porous layer, a porous film, or a separator.

[0004] Patent Document 1 describes a laminated porous film in which a heat-resistant porous layer containing an inorganic filler and a resin binder is laminated on at least one side of a polyolefin resin porous film, and the heat-resistant porous layer has a surface static friction coefficient of 0.45 or less and an air permeability of 2000 sec / 100 cm 3 The laminated porous film disclosed has a tensile modulus of elasticity of 400 to 1000 MPa at 3% elongation in the longitudinal direction, a proportion of inorganic filler in the total amount of inorganic filler and resin binder of 92 mass % or more, an average particle size of the inorganic filler measured using a scanning electron microscope (SEM) of 0.1 to 3.0 μm, and β-crystal activity.

[0005] Patent Document 2 describes a separator for a non-aqueous secondary battery comprising a polyolefin microporous film and a heat-resistant porous layer containing a heat-resistant resin and an inorganic filler coated on one or both sides of the polyolefin microporous film, the static friction coefficient being 0.3 to 1.0, and the applied load of 36 g / cm is 36 g / cm using a contact type film thickness meter having a circular contact terminal with a diameter of 0.5 cm on the contact bottom surface. 2 and 1.2kg / cm 2 The separator for a nonaqueous secondary battery is disclosed, in which the difference in thickness measured by the above method is 2.0 to 10 μm, the average particle size of the inorganic filler is 0.1 to 1 μm, and the thickness of the heat-resistant porous layer per one side of the polyolefin microporous membrane is 3 to 12 μm.

[0006] Patent Document 3 discloses a porous film obtained by biaxially stretching a non-porous film-like material in which a layer containing a polypropylene resin and a layer containing a polyethylene resin are laminated, the film has a static friction coefficient of 0.5 or more, a static friction coefficient of stainless steel (SUS) is less than 0.9, and has β-crystal activity. The static friction coefficient of the film described in Patent Document 3 means the largest value among the static friction coefficients measured when two porous films to be measured are prepared, the two films are overlapped in a front-to-front, front-to-back, or back-to-back combination, and each is slid, and the static friction coefficient of SUS means the larger value of the front or back among the static friction coefficients measured when the front or back of the porous film to be measured is overlapped with SUS and each is slid.

[0007] Patent Document 4 discloses a separator for a nonaqueous electrolyte battery having a porous substrate and an adhesive porous layer, which is provided on one or both sides of the porous substrate and contains an adhesive resin and an inorganic filler, in which the adhesive porous layer has a surface dynamic friction coefficient of 0.1 to 0.6, a ten-point average roughness (Rz) of 1.0 μm to 8.0 μm, an average particle size of the inorganic filler of 0.1 to 3.0 μm, and the content of the inorganic filler in the adhesive porous layer is 1 to 90 mass % based on the total solid content.

[0008] On the other hand, Patent Documents 5 to 9 do not describe the friction coefficient of the porous layer, the porous film, or the separator.

[0009] In Patent Document 5, a separator for a secondary battery having a heat-resistant porous layer containing barium sulfate particles and a synthetic resin binder provided on at least one side of a polyolefin porous membrane is described. By adjusting the average particle size and volume ratio of the barium sulfate particles, the range of increase in air permeability per 1 μm of the thickness of the heat-resistant porous layer relative to the polyolefin porous membrane, the heat shrinkage rate and hydrogen sulfide concentration of the separator for a secondary battery at 130 ° C., etc., the barium sulfate particles shield X-rays in the same way as the metal foil of the electrode, making it possible to observe the positional deviation with the electrode in the X-ray inspection process in the manufacture of the secondary battery, and since barium sulfate particles with a relatively small average particle size can be filled in the heat-resistant porous layer, it is considered to reduce the moisture content while suppressing heat shrinkage. In the separator for a secondary battery described in Patent Document 5, the synthetic resin binder is not suitable for barium sulfate particles with a small average particle size, and a relatively large amount of synthetic resin binder is required to improve heat resistance, so there is still room for improvement in both improving heat resistance and suppressing the increase in air permeability to the substrate.

[0010] Patent Document 6 proposes a battery separator having a heat-resistant porous layer on at least one side of a polyolefin microporous membrane, which has excellent heat shrinkage resistance even when the heat-resistant porous layer is thin, and has a heat shrinkage rate of 5% or less at 150°C / 1 hour and a shedding amount of the heat-resistant porous layer of 0.6 mg or less, from the viewpoint of reducing shedding of the heat-resistant porous layer. Patent Document 6 describes not only the polyacrylamide contained in the heat-resistant porous layer, but also the BET specific surface area of ​​the barium sulfate particles, but the particle size distribution of the barium sulfate particles is unknown, so there is concern about insufficient heat resistance or deterioration of ion permeability.

[0011] In Patent Document 7, the BET specific surface area is 3.0 m 2 / g or more 6.3m 2It has been considered that a composition for a porous membrane containing barium sulfate particles of 0.1 g or less, a water-soluble polymer such as poly(meth)acrylamide, and water is applied to a separator substrate to reduce the amount of residual water in a non-aqueous secondary battery having a separator, thereby improving the high-temperature cycle characteristics and reducing wear of the coating device. From the upper limit of the BET specific surface area in Patent Document 7, the particle size of the barium sulfate particles becomes relatively large, making it difficult to make the coating layer thin, and since a relatively large amount of water-soluble polymer is required to maintain the strength of the coating layer, it is considered that the increase in air permeability after coating on the substrate is also large.

[0012] Patent Document 8 discloses a separator for a nonaqueous secondary battery comprising a porous substrate and a heat-resistant porous layer containing a binder resin and barium sulfate particles provided on one or both sides of the porous substrate, in which the separator for a nonaqueous secondary battery has a Gurley value (JIS P8117:2009) of 50 to 800 sec / 100 mL, the value obtained by subtracting the Gurley value of the porous substrate from the Gurley value of the separator for a nonaqueous secondary battery is 10 to 300 sec / 100 mL, the volume ratio of barium sulfate particles in the heat-resistant porous layer is 50 to 90 volume %, and the average primary particle size of the barium sulfate particles contained in the heat-resistant porous layer is 0.01 μm or more and less than 0.30 μm.

[0013] In Patent Document 9, from the viewpoint of ensuring the ion permeability of the multilayer porous membrane and reducing the heat shrinkage rate, the median diameter (D 50 ) and the solid mass ratio of the binder polymer to the ionic inorganic filler have been proposed. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] JP 2011-126275 A [Patent Document 2] JP 2010-218749 A [Patent Document 3] International Publication No. 2011 / 108539 [Patent Document 4] International Publication No. 2014 / 021293 [Patent Document 5] International Publication No. 2021 / 029397 [Patent Document 6] JP 2022-089292 A [Patent Document 7] JP 2015-162313 A [Patent Document 8] Patent No. 6526359 [Patent Document 9] JP 2020-116925 A Summary of the Invention [Problem to be solved by the invention]

[0015] In recent years, in order to increase the energy density of nonaqueous electrolyte batteries, there has been a demand for thinner separators for nonaqueous electrolyte batteries. In addition, in order to ensure the safety of nonaqueous electrolyte batteries, a layer containing inorganic particles or inorganic fillers is coated on the surface of a substrate to provide an inorganic porous layer. From the viewpoint of improving the energy density of nonaqueous electrolyte batteries and thinning the separator, thinning the inorganic porous layer is also essential.

[0016] However, in recent years, the strength of separator substrates has been increasing, and such substrates are prone to thermal shrinkage. Therefore, simply thinning the inorganic porous layer reduces the heat shrink resistance and strength of the inorganic porous layer, making it difficult to suppress the thermal shrinkage of the entire separator, i.e., to ensure safety. Therefore, in order to thin the inorganic porous layer while suppressing thermal shrinkage, it is possible to reduce the particle size of the inorganic particles or inorganic filler in the inorganic porous layer, but this may increase the friction of the entire separator surface and deteriorate the pin removal property, etc. Thus, comprehensive thinning of the separator, in which the inorganic porous layer and the inorganic coating layer are also thinned in accordance with the increase in the strength of the separator substrate, has not yet been realized.

[0017] In view of the above circumstances, the present invention aims to provide a multilayer porous membrane that can improve heat resistance (i.e., ability to suppress thermal shrinkage) and strength while suppressing overall friction on the separator surface when making the separator for a nonaqueous electrolyte battery thinner, and can also improve the energy density of the nonaqueous electrolyte battery, as well as a separator for a nonaqueous electrolyte battery and a nonaqueous electrolyte battery including the same. [Means for solving the problem]

[0018] The present inventors have found that the above-mentioned problems can be solved by specifying the particle size and ratio of inorganic particles and the friction coefficient of the porous layer in a multi-layer porous membrane having a microporous membrane containing polyolefin resin as a main component and a porous layer containing inorganic particles laminated on at least one side of the microporous membrane, and have completed the present invention. An example of the embodiment of the present invention is listed below. (1) A multilayer porous membrane having a microporous membrane containing a polyolefin resin as a main component and a porous layer containing inorganic particles laminated on at least one surface of the microporous membrane, The average particle diameter D of the inorganic particles 50 is 0.01 μm or more and less than 0.60 μm, The mass ratio of the inorganic particles in the porous layer is greater than 80%, The volume ratio of the inorganic particles in the porous layer is greater than 70%, The surface static friction coefficient of the porous layer is 0.01 or more and 0.40 or less, and The surface dynamic friction coefficient of the porous layer is 0.01 or more and 0.35 or less. Multilayer porous membrane. (2) The air permeability of the multilayer porous membrane is 400 sec / 100 cm 3 2. The multilayer porous membrane according to item 1, which is: (3) The microporous membrane has a puncture strength calculated based on the basis weight of 0.49 N / (g / m 2 3. The multilayer porous membrane according to item 1 or 2, wherein (4) The multilayer porous membrane according to any one of items 1 to 3, wherein the porous layer has a thickness of 4 μm or less on at least one side of the microporous membrane. (5) The air permeability of the porous layer is 100 sec / 100 cm 3 5. The multilayer porous membrane according to any one of Items 1 to 4, which is: (6) The multilayer porous membrane according to any one of items 1 to 5, wherein a ratio of the surface static friction coefficient to the surface kinetic friction coefficient (surface static friction coefficient / surface kinetic friction coefficient) is 1.07 or less. (7) The multilayer porous membrane according to any one of items 1 to 6, wherein the multilayer porous membrane has a heat shrinkage rate at 150° C. of 10% or less in both MD and TD. (8) The multilayer porous membrane according to any one of items 1 to 7, which is a separator for a non-aqueous electrolyte battery. (9) A nonaqueous electrolyte battery comprising a positive electrode, the multilayer porous membrane according to item 8, a negative electrode, and a nonaqueous electrolyte. Effect of the Invention

[0019] According to the present invention, it is possible to provide a multilayer porous membrane that can improve heat resistance (i.e., ability to suppress thermal shrinkage) and strength while suppressing overall friction on the separator surface in thinning a separator for a nonaqueous electrolyte battery, and can also improve the energy density of the nonaqueous electrolyte battery. By using the membrane, it is possible to provide a separator for a nonaqueous electrolyte battery and a nonaqueous electrolyte battery that can also improve pin removal properties, etc. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a schematic cross-sectional view illustrating a wound state when an electricity storage device separator, a positive electrode, and a negative electrode are wound around a pin to form a wound body. [Diagram 2] FIG. 2 is a schematic diagram showing the overall configuration of the manual winding device (A) and the winding section configuration (B). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, the present invention will be described in detail for the purpose of illustrating the form for carrying out the present invention (hereinafter, abbreviated as "embodiment"), but the present invention is not limited to the following embodiment. In this specification, the upper and lower limits of each numerical range can be arbitrarily combined. In addition, when a certain member contains a specific component as a main component, it means that the content of the specific component is 50 mass% or more based on the mass of the member. Unless otherwise specified, the physical properties or numerical values ​​described in this specification are measured or calculated by the methods described in the examples.

[0022] In this specification, MD refers to the machine direction of the microporous polyolefin membrane, and TD refers to the direction crossing the MD of the microporous polyolefin membrane at an angle of 90°.

[0023] In this specification, the pin removal property refers to a property that can eliminate pin removal failures when a multilayer porous membrane or a separator for a non-aqueous electrolyte battery and an electrode are wound around a pin to produce a wound body and the pin is pulled out of the wound body. Examples of pin removal failures include problems such as the pin periphery of the wound body protruding like a bamboo shoot and losing its shape, the wound body collapsing, step misalignment, and deformation of the end of the wound body.

[0024] <Multilayer porous membrane> The multilayer porous membrane according to this embodiment comprises a porous membrane containing a polyolefin resin as a main component (a microporous PO membrane) and a porous layer containing inorganic particles laminated on at least one side of the microporous PO membrane.

[0025] The multilayer porous membrane according to the present embodiment can be used as a separator for a non-aqueous electrolyte battery (hereinafter, may be abbreviated as a separator). In the porous layer, by specifying the particle size and ratio of inorganic particles and the friction coefficient of the porous layer as described below, it is possible to suppress the overall friction on the separator surface when the separator is thinned while maintaining permeability, and to improve the heat resistance (i.e., ability to suppress thermal shrinkage) and strength, as well as the energy density of the non-aqueous electrolyte battery.

[0026] The structure of the multilayer porous membrane may have a porous layer on one or both sides of the PO microporous membrane, for example, a two-layer structure including a first porous layer containing inorganic particles and a PO microporous membrane, or a three-layer structure including, in order, a first porous layer, a PO microporous membrane, and a second porous layer containing inorganic particles.

[0027] The multilayer structure is not limited to a two-layer structure of a first porous layer-PO microporous membrane, or a three-layer structure of a first porous layer-PO microporous membrane-second porous layer, and may have one or more additional layers formed between the first porous layer and the PO microporous membrane, between the second porous layer and the PO microporous membrane, or on at least one side or the outside of the multilayer porous membrane, as desired. Examples of the additional layer include an additional PO microporous membrane, an additional porous layer containing inorganic particles and a binder polymer, a resin layer containing 50 mass % or more of a resin other than polyolefin (PO), and a thermoplastic polymer-containing layer containing a binder component having an adhesive function such as a thermoplastic polymer.

[0028] The components of the multilayer porous membrane according to this embodiment will be described below.

[0029] <Porous layer> The porous layer is a layer that is laminated on at least one side of the microporous film that contains a polyolefin resin as a main component and contains inorganic particles. The porous layer may contain a resin binder, a dispersant, etc., as desired.

[0030] (Relationship between particle size and ratio of inorganic particles and friction coefficient of porous layer) The porous layer according to this embodiment has an average particle size D 50 is 0.01 μm or more and less than 0.60 μm, the mass ratio of the inorganic particles in the porous layer is greater than 80%, the volume ratio of the inorganic particles in the porous layer is greater than 70%, and the surface static friction coefficient (μ s ) is 0.01 or more and 0.40 or less, and the surface dynamic friction coefficient (μ' s ) is greater than or equal to 0.01 and less than or equal to 0.35.

[0031] In the multilayer porous membrane according to the present embodiment, the average particle diameter D 50 , the mass fraction of inorganic particles in the porous layer (W i ) and volume fraction (V i ), and the surface static friction coefficient of the porous layer (μ s ) and the surface dynamic friction coefficient (μ' s ) is of the following formula: 0.01μm≦D 50 <0.60μm 80% <W i 70% <V i 0.01≦μ s ≦0.40 0.01≦μ' s ≦0.35 When the relationship expressed by the above formula is satisfied, in reducing the thickness of the separator, it is possible to achieve a high degree of heat resistance and rate and cycle performance of the nonaqueous electrolyte battery while suppressing the overall friction on the separator surface, and thus it is possible to improve pin removal properties and safety in nail penetration tests and the like of the nonaqueous electrolyte battery.

[0032] From the relationship represented by the above formula, it has been found that the porous layer arranged on at least one side of the microporous membrane of the multilayer porous membrane realizes dense packing of inorganic particles having a relatively small particle size while suppressing the overall surface friction of the multilayer porous membrane, thereby realizing a thin multilayer porous membrane with high heat resistance, high ion permeability, and high pin removal property.

[0033] Within the range of the relationship represented by the above formula, the multilayer porous membrane can achieve a high degree of low friction, high heat resistance, and low resistance at the same time when the total thickness of the multilayer porous membrane is significantly small, when the thickness (T) of the porous layer is 4 μm or less on at least one side of the PO microporous membrane, when the amount of resin binder in the porous layer is significantly small, and when the ratio T / TB of the thickness (TB) of the PO microporous membrane to the thickness T of the porous layer is 0.10 or more and 0.35 or less.

[0034] Surface static friction coefficient of the porous layer (μ s ) in the MD and / or TD is 0.01≦μ s ≦0.40 and 0.01≦μ in at least MDs It is preferable that the μ of the porous layer satisfies ≦0.40. s In view of suppressing overall friction of the multilayer porous membrane, high heat resistance, high pin removal property and low resistance, in MD and / or TD, the following formula: 0.01≦μ s ≦0.35 It is preferable that the relationship expressed by the following formula is satisfied.

[0035] Surface dynamic friction coefficient of porous layer (μ' s ) in MD and / or TD is 0.01≦μ' s ≦0.35 and 0.01≦μ' in at least MD s It is preferable that μ' of the porous layer satisfies ≦0.35. s In view of suppressing overall friction of the multilayer porous membrane, high heat resistance, high pin removal property and low resistance, in MD and / or TD, the following formula: 0.01≦μ' s ≦0.30 It is preferable that the relationship expressed by the following formula is satisfied.

[0036] In order to achieve a high degree of compatibility between low friction, high heat resistance, and low resistance for the multilayer porous film, the ratio of the surface static friction coefficient to the surface dynamic friction coefficient of the porous layer (μ s / μ' s ) is preferably 1.07 or less and / or 0.09 or more in the MD and / or TD, and the ratio (μ s / μ' s ) is more preferably 1.00 or more and / or 1.04 or less, at least in the MD.

[0037] The relationship of the surface friction coefficient of the porous layer described above can be obtained, for example, by selecting the type of inorganic particle raw material based on the stress relaxation rate in a shear test, adjusting the surface friction coefficient of the porous layer to a microporous membrane or a substrate, or adjusting the surface friction coefficient of the porous layer to a specific mass ratio (W i ) and / or volume fraction (V i This can be achieved by blending inorganic particles in the slurry according to the desired properties, dispersing, stirring, and controlling the particle size of the inorganic particles in the inorganic particle-containing slurry, etc.

[0038] Average particle size D of inorganic particles in the porous layer 50 0.01μm≦D 50 As the average particle diameter of inorganic particles decreases within the range of <0.60 μm, the number of adhesion points between inorganic particles and resin binder, between the porous layer and the microporous PO film, and between inorganic particles increases, improving heat resistance, and the pore size of the porous layer becomes smaller, which makes the current density of the nonaqueous electrolyte battery more uniform, improving cycle performance. 50 From the viewpoint of achieving a high degree of compatibility between low friction, high heat resistance, and low resistance of the multilayer porous film, D is preferably 0.01 μm or more, more preferably 0.10 μm or more, further preferably 0.20 μm or more, and particularly preferably 0.25 μm or more. 50 is preferably 0.50 μm or less, more preferably 0.45 μm or less, further preferably 0.40 μm or less, and particularly preferably 0.35 μm or less.

[0039] The average particle size or particle size distribution of the inorganic particles described above can be achieved, for example, in the process of disposing a porous layer on a microporous membrane or substrate, or in the process of manufacturing a separator, by selecting the type of inorganic particle raw material based on the stress relaxation rate in a shear test, dispersing, stirring, and controlling the particle size of the inorganic particles in a slurry containing the inorganic particles, and the like.

[0040] Specifically, examples of methods for adjusting the particle size distribution of inorganic particles include a method of pulverizing inorganic particles using a ball mill, bead mill, jet mill, etc. to obtain a desired particle size distribution, and a method of preparing inorganic particles with multiple particle size distributions and then blending them.

[0041] The mass ratio of inorganic particles in the porous layer (W i When the W of the inorganic particles in the porous layer is greater than 80%, the proportion of other components, such as resin binders, is relatively small, making it easier to control the friction coefficient or particle size of the inorganic particles described above, and suppressing an increase in the air permeability of the porous membrane to the microporous PO membrane and battery resistance, thereby improving cycle characteristics. iFrom the viewpoint of achieving a high degree of compatibility between low friction, high heat resistance, and low resistance of the multilayer porous film, W is preferably greater than 90%, more preferably 93% or more, even more preferably 95% or more, and particularly preferably 97% or more. i The upper limit is not particularly limited, but may be, for example, 100% or less, less than 100%, or 99% or less.

[0042] The volume fraction of inorganic particles in the porous layer (V i ) is greater than 70% of the volume of the porous layer excluding the voids, which is 100% by volume. i When the V of the inorganic particles in the porous layer is greater than 70%, the ratio of the inorganic particles to other components, such as the resin binder, increases, making it easier to adjust the friction coefficient or particle size of the inorganic particles described above, and suppressing an increase in the air permeability of the microporous PO membrane due to the porous layer, thereby making it possible to reduce the electrical resistance of the multilayer porous membrane. i From the viewpoint of achieving a high degree of compatibility between low friction, high heat resistance, and low resistance of the multilayer porous film, V is preferably greater than 75%, more preferably greater than 80%, even more preferably greater than 85%, and particularly preferably greater than 90%. i is preferably 95% or less, more preferably 93% or less, even more preferably 92% or less, and particularly preferably 91% or less.

[0043] (Inorganic particles) The inorganic particles used in the porous layer are not particularly limited, but may be inorganic fillers for the porous layer, and preferably have high heat resistance and electrical insulation properties, and are electrochemically stable within the range of use of the nonaqueous electrolyte battery.

[0044] Examples of the material of the inorganic particles include oxide ceramics such as alumina, silica, titania, zirconia, magnesia, ceria, yttria, zinc oxide, and iron oxide; nitride ceramics such as silicon nitride, titanium nitride, and boron nitride; ceramics such as silicon carbide, calcium carbonate, magnesium sulfate, aluminum sulfate, barium sulfate, aluminum hydroxide, aluminum oxide hydroxide, or boehmite, potassium titanate, talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand; and glass fibers. Among these, at least one selected from the group consisting of alumina, boehmite, and barium sulfate is preferable from the viewpoint of stability in a nonaqueous electrolyte battery, and from the viewpoint of overall friction reduction of the multilayer porous film, stress relaxation rate in a shear test, and μ of the porous layer. s and / or μ′ s From the viewpoint of easily controlling the stress relaxation rate and the microstructure of the porous layer, barium sulfate is more preferable. Barium sulfate is not limited, but may have a specific gravity of about 4.50, and may be surface-treated or not, and may be used from the viewpoint of the stress relaxation rate and the microstructure of the porous layer. s and / or μ′ s From the viewpoint of easily controlling the amount of the barium sulfate, it is preferable that the barium sulfate is obtained by a sulfuric acid method. In addition, as the boehmite, synthetic boehmite is preferable because it can reduce ionic impurities that adversely affect the characteristics of the non-aqueous electrolyte battery. The inorganic particles may be used alone or in combination.

[0045] The shape of the inorganic particles may be, for example, plate-like, scale-like, polyhedral, needle-like, columnar, granular, spherical, spindle-like, block-like, etc., and a combination of inorganic particles having the above shapes may be used. Among these, from the viewpoint of the balance between permeability and heat resistance, block-like is preferred, and in the case of barium sulfate, it is preferred that the particles are generally granular. A combination of barium sulfate having the above shapes may be used.

[0046] The aspect ratio of the inorganic particles is preferably 1.0 to 3.0, more preferably 1.1 to 2.5. The aspect ratio of 3.0 or less is preferable from the viewpoints of suppressing the amount of water adsorption by the multilayer porous membrane and suppressing capacity deterioration during repeated cycles of the nonaqueous electrolyte battery, and suppressing deformation at a temperature exceeding the melting point of the PO microporous membrane.

[0047] The BET specific surface area of ​​inorganic particles is 5.00m 2 / g or more 50.0m 2 / g or less, and 6.00m 2 / g or more 30.00m 2 / g or less, and more preferably 6.00 to 20.00m 2 More preferably, the range is 15.00m / g. 2 / g or less, and more preferably 6.00 to 12.00 m 2 / g, and more preferably in the range of 6.00 to 10.00 m 2 It is particularly preferable that the range of 6.31 to 6.99 m / g is satisfied. 2 / g, and 2 It is highly preferable that the value is less than 6.31 to 6.49 m / g. 2 It is most preferable that the BET specific surface area of ​​the inorganic particles is in the range of 5.00 m / g. 2 When the BET specific surface area of ​​the inorganic particles is within the above range, it is easy to realize an average particle size suitable for this embodiment.

[0048] The stress relaxation rate in the shear test of the inorganic particles is preferably 17.0% or less, more preferably 15.0% or less, and even more preferably 13.0% or less. When the stress relaxation rate in the shear test of the inorganic particles is in the range of 17.0% or less, the porous layer is formed uniformly and the surface friction of the porous layer is reduced. In addition, the stress relaxation rate in the shear test of the inorganic particles is preferably 1.0% or more, more preferably 5.0% or more, and even more preferably 8.0% or more. When the stress relaxation rate in the shear test of the inorganic particles is in the range of 1.0% or more, the density of the porous layer is not too low, and high permeability can be achieved.

[0049] (Resin binder) The porous layer may contain a resin binder as desired. The resin binder is a material that binds a plurality of inorganic particles together in the porous layer or binds the porous layer to the PO microporous membrane. When the multilayer porous membrane is used as a separator, it is preferable to use a resin binder that is insoluble in the electrolyte of the nonaqueous electrolyte battery and is electrochemically stable within the range of use of the nonaqueous electrolyte battery.

[0050] Specific examples of the resin binder include the following 1) to 7). 1) Polyolefins: for example, polyethylene, polypropylene, ethylene propylene rubber, and modified products thereof; 2) Conjugated diene polymers: for example, styrene-butadiene copolymers and their hydrogenated products, acrylonitrile-butadiene copolymers and their hydrogenated products, acrylonitrile-butadiene-styrene copolymers and their hydrogenated products; 3) Acrylic polymers: for example, methacrylate-acrylate copolymers, styrene-acrylate copolymers, acrylonitrile-acrylate copolymers, poly(meth)acrylamide; 4) Polyvinyl alcohol-based resins: for example, polyvinyl alcohol, polyvinyl acetate; 5) Fluorine-containing resins: for example, polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer; 6) Cellulose derivatives: for example, ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose; 7) Resins having a melting point and / or glass transition temperature of 180°C or higher, or polymers having no melting point but a decomposition temperature of 200°C or higher: for example, polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, polyamide, polyester, and poly(meth)acrylamide.

[0051] From the viewpoint of further improving safety in the event of a short circuit, 3) acrylic polymers, 5) fluorine-containing resins, and 7) polyamides as polymers are preferred. As polyamides, from the viewpoint of durability, aramid resins such as wholly aromatic polyamides, and particularly polymetaphenylene isophthalamide, are preferred.

[0052] From the viewpoint of compatibility between the resin binder and the electrodes, the above 2) conjugated diene polymer is preferred, and from the viewpoint of voltage resistance, the above 3) acrylic polymer and 5) fluorine-containing resin are preferred.

[0053] The above-mentioned 2) conjugated diene polymer is a polymer containing a conjugated diene compound as a monomer unit.

[0054] Examples of the conjugated diene compound include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted linear conjugated pentadiene, substituted and side chain conjugated hexadienes, etc., which may be used alone or in combination of two or more. Among these, 1,3-butadiene is particularly preferred.

[0055] The acrylic polymer 3) is a polymer containing a (meth)acrylic compound or (meth)acrylamide as a monomer unit, and is more preferable than polyvinylidene fluoride (PVDF) or aramid resin from the viewpoint of separator resistance. The (meth)acrylic compound refers to at least one selected from the group consisting of (meth)acrylic acid and (meth)acrylic acid esters.

[0056] Examples of the (meth)acrylic acid used in the above 3) acrylic polymer include acrylic acid and methacrylic acid.

[0057] Examples of the (meth)acrylic acid ester used in the acrylic polymer 3) above include (meth)acrylic acid alkyl esters, such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, and 2-ethylhexyl methacrylate; and epoxy group-containing (meth)acrylic acid esters, such as glycidyl acrylate and glycidyl methacrylate; and these may be used alone or in combination of two or more. Among the above, 2-ethylhexyl acrylate (EHA) and butyl acrylate (BA) are particularly preferred.

[0058] From the viewpoint of safety in a nail penetration test, the acrylic polymer is preferably a polymer containing (meth)acrylamide, EHA or BA as a main structural unit. The main structural unit refers to a polymer portion corresponding to a monomer that accounts for 40 mol % or more of the total raw materials for forming the polymer.

[0059] The above 2) conjugated diene polymer and 3) acrylic polymer may be obtained by copolymerizing other monomers copolymerizable therewith. Examples of the copolymerizable other monomers used include unsaturated carboxylic acid alkyl esters, aromatic vinyl monomers, cyanide vinyl monomers, unsaturated monomers containing hydroxyalkyl groups, unsaturated carboxylic acid amide monomers, crotonic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, etc., which may be used alone or in combination of two or more. Among the above, unsaturated carboxylic acid alkyl ester monomers are particularly preferred. Examples of unsaturated carboxylic acid alkyl ester monomers include dimethyl fumarate, diethyl fumarate, dimethyl maleate, diethyl maleate, dimethyl itaconate, monomethyl fumarate, monoethyl fumarate, etc., which may be used alone or in combination of two or more.

[0060] The above-mentioned 2) conjugated diene polymer may be one obtained by copolymerizing the above-mentioned (meth)acrylic compound as another monomer.

[0061] In the porous layer according to the present embodiment, the resin binder is preferably either or both of a water-soluble polymer and a water-insoluble polymer, more preferably both of which have a poly(meth)acrylamide skeleton, and more preferably in the form of an acrylic polymer latex or containing poly(meth)acrylamide. The latex of the acrylic polymer is preferable from the viewpoint of suppressing thermal shrinkage because the binding force between a plurality of inorganic particles is strong even at high temperatures exceeding room temperature. In general, poly(meth)acrylamide is known to be classified as a water-soluble polymer. In accordance with the reduction in the particle size of the inorganic particles, the porous layer can be made to conform to the mass ratio or volume ratio of the inorganic particles described above.

[0062] The poly(meth)acrylamide may be amphoteric, cationic, anionic, or nonionic, with the anionic type being preferred.

[0063] Since the resin binder may be either a homopolymer or a copolymer, the resin binder containing poly(meth)acrylamide may mean that the resin binder consists of only poly(meth)acrylamide, that the resin binder is a mixture of poly(meth)acrylamide and other polymers, that (meth)acrylamide is copolymerized with other monomers, or that part of the polymer backbone of the resin binder contains repeat units of a component derived from (meth)acrylamide.

[0064] From the viewpoint of the binding strength between multiple inorganic particles and the ability to suppress thermal shrinkage, the weight average molecular weight of the water-soluble polymer is preferably 1,000 or more as the lower limit, more preferably 10,000 or more, even more preferably 100,000 or more, and particularly preferably 150,000 or more as the upper limit, and is preferably 3,000,000 or less, more preferably 2,000,000 or less, even more preferably 1,000,000 or less, and particularly preferably 700,000 or less.

[0065] The mass proportion Wa of the water-soluble polymer contained in the porous layer is preferably greater than 0 mass% from the viewpoints of the binding strength between multiple inorganic particles and the ability to suppress thermal shrinkage, and the upper limit thereof is preferably 5.0 mass% or less, more preferably 2.0 mass% or less, and even more preferably 3.0 mass% or less.

[0066] From the viewpoints of thermal shrinkage suppression ability and transparency, the resin binder used in this embodiment preferably contains a water-insoluble binder. The water-insoluble binder may be composed of one or more water-insoluble binders selected from the above specific examples 1) to 7), and is more preferably in the form of a latex of water-insoluble binder particles, and even more preferably in the form of a latex of water-insoluble acrylic polymer particles.

[0067] Average particle size D of water-insoluble binder particles in latex 50is preferably 0.50 μm or less from the viewpoint that the smaller the particle size, the easier it is to suppress thermal shrinkage, and on the other hand, is preferably 0.01 μm or more from the viewpoint that the larger the particle size, the better the permeability. From the viewpoint of achieving both the ability to suppress thermal shrinkage and permeability, it is more preferable to use two types of water-insoluble binders having different particle size distributions in the latex.

[0068] When two types of water-insoluble binders are used, the first water-insoluble binder with a relatively small particle size is selected from the viewpoint of suppressing thermal shrinkage, and the average particle size D of the first binder is selected from the viewpoint of suppressing thermal shrinkage, and the average particle size D of the second binder is selected from the viewpoint of suppressing thermal shrinkage. 50 and / or an average particle size D of 0.50 μm or less 50 It is preferred that the compound has the formula:

[0069] On the other hand, the second water-insoluble binder having a relatively large particle diameter is selected from the viewpoints of permeability and of forming voids between the separator and the electrodes by protruding from the average thickness of the porous layer, and of alleviating the effects of the expansion and contraction of the electrodes due to the charging and discharging of the nonaqueous electrolyte battery, thereby improving the cycle characteristics, by using the voids. 50 Average particle size D 50 From the same viewpoint as above, it is preferable that the average particle diameter D 50 is preferably 0.3 μm or more, more preferably 0.5 μm or more, and even more preferably 0.50 μm or more, and its upper limit is preferably 5.0 μm or less, more preferably 4.0 μm or less, and even more preferably 3.0 μm or less.

[0070] The mass proportion Wb of the water-insoluble binder contained in the porous layer is preferably 0 mass% or more from the viewpoints of thermal shrinkage suppression ability and permeability, and its upper limit is preferably 5.0 mass% or less, more preferably 2.0 mass% or less, and even more preferably 3.0 mass% or less.

[0071] The mass ratio of the water-soluble polymer in the porous layer is higher than the mass ratio of the water-insoluble binder (i.e., the ratio Wb / Wa of the mass ratio Wa of the water-soluble polymer contained in the porous layer to the mass ratio Wb of the water-insoluble binder) is preferably less than 1.0, more preferably less than 0.5, and even more preferably less than 0.3, and the ratio Wb / Wa is preferably 0.0 or more. The more the water-soluble polymer is contained in the porous layer and the mass ratio of the water-soluble polymer is higher than the mass ratio of the water-insoluble binder, the more the resin binder covers the inorganic particles in a film-like manner, and the more the number of contact points between the two increases, and the heat resistance of the multilayer porous membrane or separator can be further improved.

[0072] (Dispersant) The porous layer may contain a dispersant in addition to the inorganic particles and the resin binder, if desired. Examples of dispersants include polycarboxylates such as polyacrylates, sulfonates, polyoxyethers, etc. The content of the dispersant is preferably 0.0% by mass or more, more preferably more than 0.0% by mass, and even more preferably within the range of 0.3% by mass to 0.7% by mass, based on the solid content of the porous layer. The content of the dispersant is preferably 5.0% by mass or less, more preferably 1.0% by mass or less, and even more preferably 0.7% by mass or less, based on the solid content of the porous layer.

[0073] (Physical properties of porous layers) The volume of the porous layer excluding the voids is 100 volume%, and the ratio of the resin binder is preferably less than 30 volume%, more preferably 20 volume% or less, even more preferably less than 10 volume%, particularly preferably less than 9 volume%, and the lower limit is preferably 0.1 volume% or more. When the volume ratio of the resin binder in the porous layer is within the above range, the ratio of inorganic particles to the resin binder increases, so that the surface friction coefficient of the porous layer described above and the particle size and ratio of inorganic particles can be easily adjusted, and the increase in the air permeability of the microporous film due to the porous layer can be suppressed, and the electrical resistance of the multilayer porous film can be reduced.

[0074] The thickness T of the porous layer is preferably 4 μm or less per at least one side of the PO microporous membrane, more preferably less than 3 μm, even more preferably less than 2.5 μm, even more preferably 2.4 μm or less, particularly preferably 2.0 μm or less, and most preferably 1.5 μm or less, with the lower limit being preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 0.7 μm or more, and particularly preferably 1.0 μm or more. If the thickness T of the porous layer having the above-described surface friction coefficient and particle size and ratio of the inorganic particles is 4 μm or less, the electrical resistance of the multilayer porous membrane or separator is also reduced, and the capacity and cycle characteristics of the nonaqueous electrolyte battery may be improved.

[0075] The thickness T of the porous layer may be formed on at least one side of the PO microporous membrane, or on both sides of the PO microporous membrane. When the porous layer is formed on both sides of the PO microporous membrane, the total thickness of the porous layer is preferably within the above-mentioned range.

[0076] The air permeability of the porous layer is 100sec / 100cm 3 It is preferable that the speed is less than 50 sec / 100 cm. 3 Less than 40sec / 100cm, more preferably 3 More preferably, 30 sec / 100 cm or less 3 More preferably, 25 sec / 100 cm or less 3 Below 20 sec / 100 cm, especially preferred 3 The lower limit is preferably 1 sec / 100 cm or less. 3 More preferably, 3sec / 100cm 3 More preferably, 5 sec / 100 cm 3 More than 10 sec / 100 cm is particularly preferable. 3 The air permeability of the porous layer is 100sec / 100cm 3By keeping the thickness of the porous layer at or below 100 cm, the electrical resistance is reduced, and the capacity and cycle characteristics of the non-aqueous electrolyte battery tend to be improved. From the same viewpoint, the air permeability per unit thickness of the porous layer is preferably 30 (sec / 100 cm 3 ) / μm or less, more preferably 25(sec / 100cm 3 ) / μm or less, more preferably 20 (sec / 100cm 3 ) / μm or less, and particularly preferably 15 (sec / 100 cm 3 ) / μm or less, and the lower limit is preferably 1 (sec / 100 cm 3 ) / μm or more, more preferably 3(sec / 100cm 3 ) / μm or more.

[0077] The layer density in the porous layer has a lower limit of 1.0 g / (m 2 .μm) or more, and more preferably 1.5 g / (m 2 ·μm), and more preferably 2.0 g / (m 2 ·μm) or more, with the upper limit being 5.0g / (m 2 .μm) or less, and more preferably 4.0 g / (m 2 ·μm), and more preferably 3.0 g / (m 2 The layer density in the porous layer is 1.0 g / (m 2 ·μm) or more is preferable from the viewpoint of suppressing deformation at a temperature exceeding the melting point of the microporous PO membrane, and 2 A thickness of 1.0 μm or less is preferable from the viewpoints of maintaining the ion permeability of the porous layer and suppressing capacity deterioration during repeated cycles.

[0078] The lower limit of the 180° peel strength of the porous layer from the multilayer porous membrane or the microporous PO membrane is preferably 100 N / m or more, more preferably 200 N / m or more, even more preferably 250 N / m or more, even more preferably 300 N / m or more, and particularly preferably 400 N / m or more, and the upper limit is preferably 800 N / m or less, more preferably 750 N / m or less, even more preferably 700 N / m or less, even more preferably 600 N / m or less, and particularly preferably 500 N / m or less. The "180° peel strength" is the strength when the coating layer is peeled off so that the surface of the coating layer facing the substrate forms an angle of 180° with the substrate. When the 180° peel strength is 100 N / m or more, the adhesive strength with the electrode is increased and thermal shrinkage is suppressed.

[0079] <Polyolefin microporous membrane> The porous film containing polyolefin as a main component (PO microporous film) contains polyolefin, and is preferably composed of polyolefin. The form of polyolefin may be a microporous body of polyolefin, for example, a polyolefin film, a woven fabric of polyolefin fiber, or a nonwoven fabric of polyolefin fiber. Examples of polyolefin include homopolymers, copolymers, or multi-stage polymers obtained by using ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, or the like as monomers, and these polymers may be used alone or in a mixture of two or more kinds. From the viewpoint of the melt viscosity, shutdown, and meltdown properties of the PO microporous film usable as a separator, the polyolefin is preferably at least one selected from the group consisting of polyethylene, polypropylene, and copolymers thereof, more preferably contains polypropylene, and even more preferably is an ethylene-propylene copolymer or a mixture of polyethylene and polypropylene.

[0080] Specific examples of polyethylene include low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), high molecular weight polyethylene (HMWPE), and ultra-high molecular weight polyethylene (UHMWPE).

[0081] In this specification, high molecular weight polyethylene (HMWPE) means polyethylene with a viscosity average molecular weight (Mv) of 100,000 or more. Generally, ultra-high molecular weight polyethylene (UHMWPE) has an Mv of 1,000,000 or more, so high molecular weight polyethylene (HMWPE) in this specification includes UHMWPE by definition.

[0082] In this specification, high density polyethylene has a density of 0.942 to 0.970 g / cm 3 In the present invention, the density of polyethylene refers to a value measured according to D) density gradient tube method described in JIS K7112 (1999).

[0083] Specific examples of polypropylene include isotactic polypropylene, syndiotactic polypropylene, and atactic polypropylene.

[0084] Specific examples of the copolymer of ethylene and propylene include ethylene-propylene random copolymers and ethylene-propylene rubber.

[0085] When the polyolefin (PO) contained in the PO microporous membrane contains polyethylene (PE), the PE content is from 50% by mass to 100% by mass, based on the total mass of the resin components constituting the PO microporous membrane, and from the viewpoint of fuse characteristics or meltdown characteristics, the PE content is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 93% by mass or more.

[0086] When the PO contained in the PO microporous membrane contains polypropylene (PP), the PP content is more than 0 mass% and less than 50 mass% based on the total mass of the resin components constituting the PO microporous membrane, and from the viewpoints of melt viscosity and fuse characteristics, is preferably 30 mass% or less, more preferably 20 mass% or less, even more preferably 10 mass% or less, and particularly preferably 7 mass% or less.

[0087] The microporous PO membrane may further contain, in addition to the polyolefins listed above, resins such as polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimideamide, polyaramid, polyvinylidene fluoride, nylon, and polytetrafluoroethylene.

[0088] From the viewpoint of suppressing high viscosity of the PO resin composition during film formation and suppressing the occurrence of defective products, the lower limit of the melt index (MI) of the PO microporous film at 190°C is preferably 0.01 g / 10 min or more, more preferably 0.02 g / 10 min or more, even more preferably 0.03 g / 10 min or more, particularly preferably 0.04 g / 10 min or more, and most preferably 0.05 g / 10 min or more, and the upper limit is preferably 0.70 g / 10 min or less, more preferably 0.60 g / 10 min or less, even more preferably 0.40 g / 10 min or less, particularly preferably 0.30 g / 10 min or less, and most preferably 0.20 g / 10 min or less.

[0089] Weight of PO microporous membrane (g / m 2 The puncture strength when converted to 50gf / (g / m 2 ) or more, i.e. 0.49N / (g / m 2 ) or more. 2 A PO microporous membrane having a puncture strength converted into unit weight of 0.54 N / (g / m) or more tends to be resistant to rupture. From the viewpoint of being resistant to rupture, the PO microporous membrane has a puncture strength converted into unit weight of more preferably 0.54 N / (g / m) or more. 2) or more, more preferably 0.59 N / (g / m 2 ) or more, particularly preferably 0.69 N / (g / m 2 From the viewpoint of improving the safety of the nonaqueous electrolyte battery while maintaining the strength of the microporous PO membrane, the puncture strength converted into basis weight is preferably 1.96 N / (g / m 2 ) or less, more preferably 1.47N / (g / m 2 ) or less, more preferably 1.18 N / (g / m 2 ) or less, particularly preferably 1.08 N / (g / m 2 ) or less, most preferably 0.98 N / (g / m 2 ) range.

[0090] The pin puncture strength of the microporous PO membrane not converted into basis weight (hereinafter simply referred to as pin puncture strength) is preferably 0.98 N or more, more preferably 1.47 N or more, and even more preferably 1.96 N or more, from the viewpoint of preventing breakage, and is preferably 9.80 N or less, more preferably 5.88 N or less, and even more preferably 4.90 N or less, from the viewpoint of improving the safety of the nonaqueous electrolyte battery while maintaining the membrane strength.

[0091] The puncture strength or the puncture strength converted into basis weight can be increased by increasing the orientation of the molecular chains due to the shear force or stretching applied to the molded product during extrusion. However, as the strength increases, the thermal stability deteriorates due to an increase in residual stress. Therefore, the puncture strength or the puncture strength converted into basis weight is controlled according to the purpose.

[0092] The thickness (TB) of the microporous PO membrane is preferably 1.0 μm or more, more preferably 2.0 μm or more, even more preferably 3.0 μm or more, still more preferably 4.0 μm or more, and particularly preferably 4.5 μm or more from the viewpoint of ensuring voltage resistance, and is preferably 30.0 μm or less, more preferably 20.0 μm or less, even more preferably 16.0 μm or less, still more preferably 12.0 μm or less, and particularly preferably 9.0 μm or less from the viewpoint of ensuring the capacity of a nonaqueous electrolyte battery. The thickness TB of the microporous PO membrane can be adjusted, for example, by controlling the die lip gap, the stretch ratio in the stretching step, etc.

[0093] The porosity of the PO microporous membrane is preferably 20% or more, more preferably 30% or more, even more preferably 35% or more, and particularly preferably 40% or more from the viewpoint of permeability, and is preferably 80% or less, more preferably 70% or less, even more preferably 60% or less, and particularly preferably 50% or less, from the viewpoint of membrane strength. The porosity of the PO microporous membrane can be adjusted, for example, by controlling the mixing ratio of the polyolefin resin composition and the plasticizer, the stretching temperature, the stretching ratio, the heat setting temperature, the stretching ratio during heat setting, and the relaxation rate during heat setting, or by combining these.

[0094] The air permeability of the microporous PO membrane is preferably 10 sec / 100 cm from the viewpoint of preventing an excessive current from flowing between a plurality of electrodes through the microporous PO membrane. 3 More than 30sec / 100cm, more preferably 30sec / 100cm 3 More preferably, 50 sec / 100 cm 3 More than 70sec / 100cm is especially preferable. 3 From the viewpoint of permeability, it is preferably 300 sec / 100 cm 3 Less than 250sec / 100cm, more preferably 3 Less than 200sec / 100cm is more preferable. 3 Below 150sec / 100cm, particularly preferred 3 It is.

[0095] The lower limit of the viscosity average molecular weight (Mv) of the microporous PO membrane is preferably 400,000 or more, more preferably 450,000 or more, and even more preferably 500,000 or more, and the upper limit is preferably 1,300,000 or less, more preferably 1,200,000 or less, and even more preferably 1,150,000 or less. When the microporous PO membrane has an Mv of 400,000 or more, the melt tension during melt molding is large, the moldability is good, and high membrane strength tends to be obtained due to entanglement of polymers. When the Mv is 1,300,000 or less, the raw material is easily melt-kneaded uniformly, and not only does the sheet moldability, particularly thickness stability, tend to be excellent, but also, when used as a separator for a nonaqueous electrolyte battery, the pores tend to be easily blocked when the temperature rises, and good fuse function tends to be obtained.

[0096] The lower limit of the average pore size of the microporous PO membrane is preferably 0.03 μm or more, more preferably 0.04 μm or more, even more preferably 0.05 μm or more, and even more preferably 0.055 μm or more, and the upper limit is preferably 0.70 μm or less, more preferably 0.20 μm or less, even more preferably 0.10 μm or less, and even more preferably 0.09 μm or less. From the viewpoints of ion conductivity and voltage resistance, the average pore size of the microporous PO membrane is preferably 0.03 μm or more and 0.70 μm or less. The average pore size can be adjusted, for example, by controlling the composition ratio of the polyolefin, the type of polyolefin or plasticizer, the cooling rate of the extruded sheet, the stretching temperature, the stretching ratio, the heat setting temperature, the stretching ratio during heat setting, and the relaxation rate during heat setting, or by combining these.

[0097] The microporous PO membrane preferably has low electronic conductivity, ionic conductivity, high resistance to organic solvents, and fine pores. The microporous PO membrane can be used alone as a separator for a lithium ion secondary battery, and is particularly suitable for use as a laminate-type separator for a lithium ion secondary battery.

[0098] <Thermoplastic polymer-containing layer> At least one side or the outer side of the multi-layer porous membrane according to one embodiment may optionally include a thermoplastic polymer-containing layer. The thermoplastic polymer-containing layer includes a thermoplastic polymer. The thermoplastic polymer layer may optionally include a particulate polymer and / or have a dot pattern.

[0099] (Thermoplastic polymer) The thermoplastic polymer is not particularly limited, but examples thereof include polyolefin resins such as polyethylene, polypropylene, and α-polyolefin; fluorine-containing resins such as polyvinylidene fluoride and polytetrafluoroethylene and copolymers containing these; diene-based polymers containing conjugated dienes such as butadiene and isoprene as monomer units or copolymers containing these and hydrogenated products thereof; acrylic polymers containing acrylic acid esters, methacrylic acid esters, and the like as monomer units or copolymers containing these and hydrogenated products thereof; rubbers such as ethylene propylene rubber, polyvinyl alcohol, and polyvinyl acetate; cellulose derivatives such as ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, and carboxymethyl cellulose; resins having a melting point and / or glass transition temperature of 180° C. or higher, such as polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, polyamide, and polyester, and mixtures thereof. In addition, monomers having a hydroxyl group, sulfonic acid group, carboxyl group, amide group, or cyano group can also be used as monomers used in synthesizing the thermoplastic polymer.

[0100] Among these thermoplastic polymers, diene-based polymers, acrylic-based polymers and fluorine-based polymers are preferred because they have excellent binding properties with the electrode active material, strength and flexibility.

[0101] (Diene Polymer) The diene polymer is not particularly limited, but is a polymer containing a monomer unit obtained by polymerizing a conjugated diene having two conjugated double bonds, such as butadiene or isoprene. The conjugated diene monomer is not particularly limited, but examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-phenyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 4,5-diethyl-1,3-octadiene, and 3-butyl-1,3-octadiene. These may be polymerized alone or copolymerized.

[0102] The proportion of monomer units obtained by polymerizing a conjugated diene in the diene polymer is not particularly limited, but is, for example, 40% by mass or more, preferably 50% by mass or more, and more preferably 60% by mass or more, of the total diene polymer.

[0103] The diene polymer is not particularly limited, but may be, for example, a homopolymer of a conjugated diene such as polybutadiene or polyisoprene, or a copolymer of a conjugated diene and a copolymerizable monomer. The copolymerizable monomer is not particularly limited, but may be, for example, a (meth)acrylate monomer described below or the following monomer (hereinafter also referred to as "other monomer").

[0104] The "other monomer" is not particularly limited, but examples thereof include α,β-unsaturated nitrile compounds such as acrylonitrile and methacrylonitrile; unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, and fumaric acid; styrene-based monomers such as styrene, chlorostyrene, vinyltoluene, t-butylstyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylnaphthalene, chloromethylstyrene, hydroxymethylstyrene, α-methylstyrene, and divinylbenzene; olefins such as ethylene and propylene; halogen atom-containing monomers such as vinyl chloride and vinylidene chloride; vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl benzoate; methyl vinyl ether, and ethyl vinyl ether. vinyl ethers such as butyl vinyl ether; vinyl ketones such as methyl vinyl ketone, ethyl vinyl ketone, butyl vinyl ketone, hexyl vinyl ketone, isopropenyl vinyl ketone; heterocycle-containing vinyl compounds such as N-vinyl pyrrolidone, vinyl pyridine, vinyl imidazole; acrylic acid ester and / or methacrylic acid ester compounds such as methyl acrylate, methyl methacrylate; hydroxyalkyl group-containing compounds such as β-hydroxyethyl acrylate, β-hydroxyethyl methacrylate; amide monomers such as acrylamide, N-methylolacrylamide, acrylamido-2-methylpropanesulfonic acid, etc., and these may be used alone or in combination of two or more.

[0105] (Acrylic polymer) The acrylic polymer is not particularly limited, but is preferably a polymer containing a monomer unit obtained by polymerizing a (meth)acrylate monomer. When the thermoplastic polymer-containing layer contains an acrylic polymer as the thermoplastic polymer, it is preferable that the layer contains a copolymer containing a monomer unit of a (meth)acrylic acid ester monomer. When the thermoplastic polymer of the thermoplastic polymer-containing layer contains a copolymer containing a monomer unit of a (meth)acrylic acid ester monomer, the adhesive strength is improved when the multilayer porous membrane or separator has a low basis weight, which is preferable.

[0106] In this specification, "(meth)acrylic acid" refers to "acrylic acid or methacrylic acid", and "(meth)acrylate" refers to "acrylate or methacrylate".

[0107] The (meth)acrylate monomer is not particularly limited, but examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, and decyl (meth)acrylate. Examples of suitable (meth)acrylates include alkyl (meth)acrylates such as acrylate, lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, and stearyl (meth)acrylate; hydroxy group-containing (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; amino group-containing (meth)acrylates such as aminoethyl (meth)acrylate; and epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate (GMA).

[0108] The proportion of monomer units obtained by polymerizing (meth)acrylate monomers is not particularly limited, but is, for example, 40% by mass or more, preferably 50% by mass or more, and more preferably 60% by mass or more of the total acrylic polymer. Examples of the acrylic polymer include homopolymers of (meth)acrylate monomers and copolymers of the same with monomers copolymerizable therewith. Examples of the copolymerizable monomer include the "other monomers" listed in the section on diene polymers above, and these may be used alone or in combination of two or more.

[0109] (Fluorine-based polymer) The fluorine-based polymer is not particularly limited, but examples thereof include a homopolymer of vinylidene fluoride and a copolymer of the homopolymer and a monomer copolymerizable therewith. The fluorine-based polymer is preferable from the viewpoint of electrochemical stability.

[0110] The proportion of monomer units obtained by polymerization of vinylidene fluoride is not particularly limited, but is, for example, 40 mass % or more, preferably 50 mass % or more, and more preferably 60 mass % or more. The monomer copolymerizable with vinylidene fluoride is not particularly limited, but examples thereof include fluorine-containing ethylenically unsaturated compounds such as vinyl fluoride, tetrafluoroethylene, trifluorochloroethylene, hexafluoropropylene, hexafluoroisobutylene, perfluoroacrylic acid, perfluoromethacrylic acid, and fluoroalkyl esters of acrylic acid or methacrylic acid; fluorine-free ethylenically unsaturated compounds such as cyclohexyl vinyl ether and hydroxyethyl vinyl ether; and fluorine-free diene compounds such as butadiene, isoprene, and chloroprene.

[0111] Among the fluoropolymers, vinylidene fluoride homopolymers, vinylidene fluoride / tetrafluoroethylene copolymers, vinylidene fluoride / tetrafluoroethylene / hexafluoropropylene copolymers, etc. are preferred. A particularly preferred fluoropolymer is vinylidene fluoride / tetrafluoroethylene / hexafluoropropylene copolymer, the monomer composition of which is usually 30-90% by mass of vinylidene fluoride, 50-9% by mass of tetrafluoroethylene, and 20-1% by mass of hexafluoropropylene. These fluororesin particles may be used alone or in combination of two or more kinds.

[0112] Furthermore, as the monomer used in synthesizing the thermoplastic polymer, a monomer having a hydroxyl group, a carboxyl group, an amino group, a sulfonic acid group, an amide group, or a cyano group can also be used.

[0113] The monomer having a hydroxy group is not particularly limited, but examples thereof include vinyl monomers such as penteneol.

[0114] The monomer having a carboxyl group is not particularly limited, but examples thereof include unsaturated carboxylic acids having an ethylenic double bond such as (meth)acrylic acid and itaconic acid, and vinyl monomers such as pentenoic acid.

[0115] The monomer having an amino group is not particularly limited, but examples thereof include 2-aminoethyl methacrylate.

[0116] The monomer having a sulfonic acid group is not particularly limited, but examples thereof include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allylsulfonic acid, styrenesulfonic acid, (meth)acrylic acid-2-ethylsulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid.

[0117] The monomer having an amide group is not particularly limited, but examples thereof include acrylamide (AM), methacrylamide, N-methylol acrylamide, and N-methylol methacrylamide.

[0118] The monomer having a cyano group is not particularly limited, but examples thereof include acrylonitrile (AN), methacrylonitrile, α-chloroacrylonitrile, α-cyanoethyl acrylate, and the like.

[0119] The thermoplastic polymer may be used alone or in a mixture of two or more kinds, but it is preferable to use two or more kinds of polymers. The thermoplastic polymer may be used together with a solvent, and the solvent may be one that can disperse the thermoplastic polymer uniformly and stably, such as N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, water, ethanol, toluene, hot xylene, methylene chloride, hexane, etc., and among them, water-based solvents are preferable. The thermoplastic polymer may be used in the form of a latex.

[0120] (glass transition temperature of thermoplastic polymers) From the viewpoints of being able to secure the distance between the electrodes and the separator in a nonaqueous electrolyte battery while exhibiting adhesion to the substrate, suppressing blocking, and exerting adhesive strength between the separator and the electrodes, and shortening the injection time of the electrolyte, it is preferable for the thermoplastic polymer constituting the thermoplastic polymer-containing layer to have thermal characteristics such that it has at least two glass transition temperatures, at least one of which is in a range of 20°C or less, and at least one of which is in a range of 30°C or more and 120°C or less.

[0121] The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC). In this specification, the glass transition temperature may also be expressed as Tg.

[0122] Specifically, it is determined by the intersection of a straight line extending from the low-temperature side baseline to the high-temperature side in the DSC curve with a tangent to the inflection point of the step-like change in the glass transition. For more details, the method described in the Examples can be referred to.

[0123] Here, "glass transition" refers to a change in heat quantity that occurs on the endothermic side in DSC due to a change in the state of the polymer test piece. Such a change in heat quantity is observed as a step-like change or a combination of a step-like change and a peak in the DSC curve.

[0124] The term "step change" refers to the portion of a DSC curve where the curve leaves the previous baseline and transitions to a new baseline, and includes any combination of a peak and a step change.

[0125] The "inflection point" refers to the point at which the gradient of the step-like change in the DSC curve is maximum, or can be expressed as the point at which the step-like change changes from an upwardly convex curve to a downwardly convex curve.

[0126] The term "peak" refers to the portion of a DSC curve from when the curve leaves the baseline to when it returns to the baseline.

[0127] The term "baseline" refers to a DSC curve in the temperature range where no transition or reaction occurs in the test specimen.

[0128] In one embodiment, at least one of the glass transition temperatures of the thermoplastic polymers used is in the range of 20° C. or less, thereby providing excellent adhesion to the microporous membrane and suppressing blocking, thereby providing the effect of excellent adhesion between the separator and the electrode. From the viewpoints of handleability and blocking resistance, the glass transition temperature is preferably −100° C. or more, more preferably −50° C. or more, even more preferably −40° C. or more, or particularly preferably −6° C. or more, and from the viewpoint of adhesion to the microporous membrane, it is preferably 20° C. or less, more preferably 10° C. or less, or particularly preferably 0° C. or less.

[0129] In one embodiment, at least one of the glass transition temperatures of the thermoplastic polymers used is in the range of 30° C. or higher and 120° C. or lower, so that the adhesiveness and handling between the separator and the electrode are excellent, and further, in a nonaqueous electrolyte battery, the distance between the electrode surface and the separator substrate surface can be maintained, and the injection time of the electrolyte can be shortened. From the viewpoint of handleability and blocking resistance, the glass transition temperature is preferably 30° C. or higher, more preferably 40° C. or higher, even more preferably 70° C. or higher, or particularly preferably 95° C. or higher, and from the viewpoint of adhesive strength, it is preferably 150° C. or lower, more preferably 130° C. or lower, or particularly preferably 120° C. or lower.

[0130] The thermoplastic polymer having two glass transition temperatures can be achieved, for example, by a method such as blending two or more types of thermoplastic polymers, but is not limited to this method.

[0131] In particular, polymer blends can control the glass transition temperature of the entire thermoplastic polymer by combining a polymer with a high glass transition temperature and a polymer with a low glass transition temperature. In addition, multiple functions can be imparted to the entire thermoplastic polymer. For example, in the case of blends, a polymer having a glass transition temperature in the range of 30°C or higher and a polymer having a glass transition temperature in the range of 20°C or lower can be blended to achieve both stickiness resistance and wettability to the polyolefin microporous membrane. The mixing ratio of the polymer having a glass transition temperature in the range of 30°C or higher and the polymer having a glass transition temperature in the range of 20°C or lower is preferably in the range of 0.1:99.9 to 99.9:0.1, more preferably 5:95 to 95:5, even more preferably 50:50 to 95:5, and even more preferably 60:40 to 90:10. In addition, a polymer with high viscosity and a polymer with high elasticity can be combined to control viscoelasticity.

[0132] In one embodiment, the glass transition temperature, i.e., Tg, of the thermoplastic polymer can be adjusted appropriately, for example, by changing the monomer components and the input ratio of each monomer used to produce the thermoplastic polymer. That is, it can be roughly estimated from the Tg of the homopolymer generally shown for each monomer used to produce the thermoplastic polymer (for example, as described in "Polymer Handbook" (A WILEY-INTERSCIENCE PUBLICATION) and the blending ratio of the monomers. For example, a copolymer containing a high ratio of monomers such as styrene, methyl methacrylate, and acrylonitrile, which give a polymer with a Tg of about 100°C, can be obtained with a high Tg, while a copolymer containing a high ratio of monomers such as butadiene, which gives a polymer with a Tg of about -80°C, and n-butyl acrylate and 2-ethylhexyl acrylate, which give a polymer with a Tg of about -50°C, can be obtained with a low Tg.

[0133] The Tg of the polymer can be roughly calculated from the FOX formula (the following formula (1)). Note that the glass transition point of the thermoplastic polymer of the present application is measured by the above-mentioned method using DSC. 1 / Tg=W1 / Tg1+W2 / Tg2+···+W i / Tg i +···W n / Tg n (1) In formula (1), Tg(K) is the Tg of the copolymer, Tg i (K) is the Tg of the homopolymer of each monomer i, W i indicates the mass fraction of each monomer.}

[0134] (Structure of Thermoplastic Polymer-Containing Layer) In the thermoplastic polymer-containing layer, it is preferable that a thermoplastic resin having a glass transition temperature of 30°C or more and 120°C or less is present on the outermost surface side of the multilayer porous membrane, and a thermoplastic resin having a glass transition temperature of 20°C or less is present on the interface side between the polyolefin microporous membrane and the thermoplastic polymer-containing layer. The "outermost surface" refers to the surface of the thermoplastic polymer-containing layer that contacts the electrode when the multilayer porous membrane or separator and the electrode are laminated. The "interface" refers to the surface of the thermoplastic polymer-containing layer that contacts the polyolefin microporous membrane or the porous layer.

[0135] In the thermoplastic polymer-containing layer, the presence of a thermoplastic polymer having a glass transition temperature of 30°C or more and 120°C or less on the outermost surface side of the multilayer porous membrane tends to provide excellent adhesion to the microporous membrane, and as a result, excellent adhesion between the separator and the electrode. In addition, the presence of a thermoplastic polymer having a glass transition temperature of 20°C or less on the interface side between the polyolefin microporous membrane and the thermoplastic polymer-containing layer tends to provide excellent adhesion and handling between the separator and the electrode. The separator has such a thermoplastic polymer-containing layer, which tends to further improve the adhesion and handling between the separator and the electrode.

[0136] The above-mentioned structure can be achieved by (a) the thermoplastic polymer being composed of a particulate thermoplastic polymer and a binder resin that bonds the particulate thermoplastic polymer to the polyolefin microporous membrane with the particulate thermoplastic polymer exposed on the surface, the particulate thermoplastic polymer having a glass transition temperature in the range of 30°C to 120°C, and a thermoplastic polymer having a glass transition temperature of 20°C or less being present on the interface side between the polyolefin microporous membrane and the thermoplastic polymer-containing layer, (b) the thermoplastic polymer having a laminated structure, the glass transition temperature of the thermoplastic polymer in the part that will be the outermost layer when used as a separator being in the range of 30°C to 120°C, and a thermoplastic polymer having a glass transition temperature of 20°C or less being present on the interface side between the polyolefin microporous membrane and the thermoplastic polymer-containing layer, etc. The (b) thermoplastic polymer may have a laminated structure of polymers with different Tg.

[0137] (Average particle size of thermoplastic polymer) The structure of the thermoplastic polymer is not particularly limited, but may be, for example, granular. Such a structure tends to improve the adhesiveness between the separator and the electrode and the handleability of the separator. Here, granular refers to a state in which each thermoplastic polymer has an outline when measured with a scanning electron microscope (SEM), and may be elongated, spherical, polygonal, or the like.

[0138] The particle size distribution and median diameter of the granular thermoplastic polymer can be measured using a laser particle size distribution measuring device (Microtrac MT3300EX, manufactured by Nikkiso Co., Ltd.). If necessary, the particle size distribution of the granular thermoplastic polymer can be adjusted using the particle size distribution of water or the binder polymer as a baseline. The particle size at which the cumulative frequency is 50% is defined as D 50 and D of the granular thermoplastic polymer 50 D P Let us assume that.

[0139] Average particle size D of granular thermoplastic polymer P From the viewpoints of being able to maintain the distance between a plurality of electrodes via the separator while exhibiting adhesive strength between the separator and the electrodes, and of shortening the time required for injecting an electrolyte into a nonaqueous electrolyte battery including the separator, the thickness is preferably 100 nm or more, more preferably 130 nm or more, even more preferably 320 nm or more, and most preferably 400 nm or more, and / or is preferably 1000 nm or less, more preferably 700 nm or less, even more preferably 590 nm or less, and most preferably 550 nm or less.

[0140] (Weight per side of thermoplastic polymer-containing layer) In the separator according to one embodiment, the basis weight per side of the thermoplastic polymer-containing layer is preferably 0.03 g / m from the viewpoint of adhesive strength. 2 More preferably, 0.04 g / m 2More preferably, 0.06 g / m 2 or more, and on the other hand, 0.3 g / m 2 It is preferable that the content is 0.15 g / m or less. 2 More preferably, it is 0.10 g / m or less, and particularly preferably 0.10 g / m 2 The basis weight of the thermoplastic polymer-containing layer can be adjusted by changing the polymer concentration of the coating liquid or the coating amount of the polymer solution. From the viewpoint of improving the cycle characteristics of the battery by suppressing the deformation of the cell shape due to the expansion and contraction of the electrodes within a range that does not impede the effects of this embodiment, the basis weight per side of the thermoplastic polymer-containing layer is 0.08 g / m 2 A range exceeding this is preferred.

[0141] (Mold of thermoplastic polymer-containing layer, coverage rate of substrate surface by thermoplastic polymer-containing layer) The form (pattern) of the thermoplastic polymer-containing layer may be, for example, a state in which the thermoplastic polymer is mutually dispersed over the entire surface of the multilayer porous membrane, or a state in which the thermoplastic polymer is present in a sea-island shape. When the thermoplastic polymer is present in a sea-stripe shape, its arrangement pattern may be, for example, a dot shape, a stripe shape, a lattice shape, a stripe shape, a tortoiseshell shape, a random shape, etc., and combinations thereof. Among them, it is preferable that the thermoplastic polymer-containing layer has a dot shape pattern.

[0142] The dot-like shape indicates that there are parts containing a thermoplastic polymer and parts not containing a thermoplastic polymer on the polyolefin microporous membrane, and the parts containing the thermoplastic polymer are present in islands. Note that, in the thermoplastic polymer-containing layer, the parts containing the thermoplastic polymer may be independent.

[0143] The diameter of the dots in the thermoplastic polymer-containing layer is preferably 20 μm or more, more preferably 30 μm or more, and even more preferably 40 μm or more, from the viewpoints of adhesion to the PO microporous membrane or electrode, improving the strength of the multilayer porous membrane, or suppressing an increase in air permeability to the PO microporous membrane, and on the other hand, is preferably 1,200 μm or less, more preferably 1,100 μm or less, and even more preferably 1,000 μm or less.

[0144] The distance between dots in the thermoplastic polymer-containing layer is preferably 100 μm or more, more preferably 120 μm or more, and even more preferably 140 μm or more, from the viewpoints of improving adhesion to the PO microporous membrane or electrode, improving the strength of the multilayer porous membrane, or suppressing an increase in air permeability to the PO microporous membrane, and on the other hand is preferably 3,500 μm or less, more preferably 3,300 μm or less, and even more preferably 3,000 μm or less.

[0145] In one embodiment, the total coverage area ratio of the thermoplastic polymer-containing layer to the substrate surface is preferably 3% or more, or 4% or more, or 5% or more, or 10% or more, or 20% or more, or 30% or more, or 40% or more, and preferably 90% or less, or 80% or less, or 75% or less, or 70% or less, from the viewpoint of lowering the resistance of the battery while maintaining the adhesive force between the multilayer porous membrane or the separator and the electrode, and shortening the injection time of the electrolyte into the nonaqueous electrolyte battery having the separator. If the coverage area of ​​the thermoplastic polymer-containing layer is small, the distance between the separator and the electrode interface becomes uneven, causing the current distribution to become uneven, and the temperature tends to rise in the (heating) safety test. In addition, if the coverage area of ​​the thermoplastic polymer-containing layer is large, the resistance of the battery increases, leading to deterioration of the rate test. The total coverage area ratio S of the thermoplastic polymer-containing layer present on the substrate surface is calculated from the following formula. S(%)=total coverage area of ​​thermoplastic polymer-containing layer÷surface area of ​​substrate×100

[0146] The total coverage area ratio (%) of the coating pattern of the thermoplastic polymer-containing layer relative to the substrate surface is measured using a microscope (model: VHX-7000, manufactured by Keyence Corporation). After photographing the separator sample at 30x (coaxial epi-illumination), the measurement mode is selected for automatic area measurement, and the total coverage area ratio of the thermoplastic polymer is measured. The coverage area ratio for each sample is calculated as the arithmetic mean value of three measurements.

[0147] The shape or total coverage area ratio of the thermoplastic polymer-containing layer can be adjusted by changing the polymer concentration of the coating liquid, the coating amount of the polymer solution, the coating method, and the coating conditions.

[0148] <Characteristics of multi-layer porous membrane> In the multilayer porous membrane according to the present embodiment, the ratio (T / TB) of the thickness (TB) of the PO microporous membrane to the thickness (T) of the porous layer is preferably 0.05 or more and / or 0.35 or less. A multilayer porous membrane having a thickness ratio (T / TB) within the above range not only enables the separator to be made thinner, thereby contributing to improved productivity, but also contributes to improved energy density and safety when incorporated into a nonaqueous electrolyte battery as a thin-film separator. The thickness ratio (T / TB) may be measured and calculated for either one or both sides of the PO microporous membrane, and from the viewpoint of the action mechanism and thickness measurement principle of the present invention, it is preferable to measure and calculate for both sides of the PO microporous membrane, specifically, the total thickness of the porous layers arranged in the multilayer porous membrane is measured and calculated as T.

[0149] The heat shrinkage rate (150°C heat shrinkage rate) of the multilayer porous membrane when it is left in an atmosphere at a temperature of 150°C for 1 hour is preferably 10% or less, more preferably 5% or less, and the lower limit is preferably 0% or more, in both the MD and TD directions. A multilayer porous membrane with a 150°C heat shrinkage rate of 10% or less not only enables the separator to be made thinner and have high heat resistance, thereby contributing to improved productivity, but also contributes to improved energy density and safety when incorporated into a non-aqueous electrolyte battery as a thin-film separator. The measurement and calculation of the 150°C heat shrinkage rate can be performed in both the MD and TD directions under either a dry condition after the multilayer porous membrane is left in an oven for 1 hour, or under a wet condition after the multilayer porous membrane is immersed in a non-aqueous solvent such as propylene carbonate or a non-aqueous electrolyte containing it and then left in an oven for 1 hour.

[0150] The heat shrinkage rate of the multilayer porous membrane at 140 ° C. (140 ° C. heat shrinkage rate) is preferably 10% or less, more preferably 5% or less, and the lower limit is preferably 0% or more, in both the MD and TD directions. A multilayer porous membrane with a 140 ° C. heat shrinkage rate of 10% or less not only enables the separator to be made thinner and have high heat resistance, thereby contributing to improved productivity, but also contributes to improved energy density and safety when incorporated into a non-aqueous electrolyte battery as a thin-film separator, thereby suppressing membrane rupture and short circuit when an abnormality occurs in the battery. The measurement and calculation of the 140 ° C. heat shrinkage rate can be performed under wet conditions in both the MD and TD directions after immersing the multilayer porous membrane in a non-aqueous solvent such as propylene carbonate or a non-aqueous electrolyte containing it and then leaving it in an oven for 1 hour.

[0151] The heat shrinkage rate of the multilayer porous membrane at 130°C (130°C heat shrinkage rate) is preferably 10% or less as an upper limit in both the MD and TD directions, more preferably 5% or less, and the lower limit is preferably 0% or more. If the 130°C heat shrinkage rate is 10% or less in both the MD and TD directions, it is preferable from the viewpoint of suppressing the rupture of the multilayer porous membrane when an abnormality occurs in the battery and suppressing a short circuit. The measurement and calculation of the 130°C heat shrinkage rate can be performed under dry conditions after leaving the multilayer porous membrane in an oven for 1 hour in both the MD and TD directions.

[0152] The total thickness of the multilayer porous membrane is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more in order to ensure voltage resistance. The total thickness of the multilayer porous membrane is preferably 30 μm or less, since the capacity of the nonaqueous electrolyte battery in which the multilayer porous membrane is mounted is less likely to deteriorate, more preferably 25 μm or less, even more preferably 20 μm or less, and particularly preferably 15 μm or less.

[0153] The air permeability of the multilayer porous membrane is preferably 1 sec / 100 cm from the viewpoint of ensuring the safety of the nonaqueous electrolyte battery by preventing an excessive current from flowing between the electrodes through the multilayer porous membrane. 3 More than 30sec / 100cm, more preferably 30sec / 100cm3 More preferably, 50 sec / 100 cm 3 The air permeability of the multilayer porous membrane is preferably 400 sec / 100 cm from the viewpoint of ion permeability and from the viewpoint of reducing resistance to improve the capacity and cycle characteristics of the nonaqueous electrolyte battery. 3 Less than 300sec / 100cm, more preferably 300sec / 100cm 3 Less than 200sec / 100cm is more preferable. 3 More preferably, 180 sec / 100 cm or less 3 Less than 150sec / 100cm 3 Below 130sec / 100cm, particularly preferred 3 The following is the result.

[0154] In the multilayer porous membrane, the ratio of the air permeability of the porous layer to the air permeability of the polyolefin microporous membrane (air permeability increase rate of the multilayer porous membrane) is preferably such that the air permeability of the polyolefin microporous membrane is not deteriorated, from the viewpoint of ion permeability and from the viewpoint of reducing resistance to improve the capacity and cycle characteristics of the nonaqueous electrolyte battery, and is more preferably 0.01 or more, and from the viewpoint of ensuring the safety of the nonaqueous electrolyte battery by preventing excessive current from flowing between multiple electrodes through the multilayer porous membrane, is preferably 0.40 or less, more preferably 0.30 or less, and even more preferably 0.20 or less.

[0155] From the viewpoint of preventing breakage and improving the safety of the nonaqueous electrolyte battery while maintaining the membrane strength, the puncture strength of the multilayer porous membrane has a lower limit of preferably 0.98 N or more, more preferably 1.47 N or more, and even more preferably 1.96 N or more, and an upper limit of preferably 9.81 N or less, more preferably 5.88 N or less, and even more preferably 4.90 N or less.

[0156] From the viewpoint of suppressing overall friction, high heat resistance, high pin-removal property and low resistance, it is preferable that the multilayer porous membrane does not have β crystal activity.The presence or absence of β crystal activity of the multilayer porous membrane can be measured, for example, by a differential scanning calorimeter (DSC), an X-ray diffractometer (XRD) or the like, as necessary.The multilayer porous membrane without β crystal activity can be obtained, for example, by not using a β crystal nucleating agent or not adding a β crystal nucleating agent to raw materials, intermediates or products in the manufacturing method of the multilayer porous membrane, including the manufacture of a polyolefin microporous membrane, the arrangement of a porous layer, and the formation of a thermoplastic polymer-containing layer.

[0157] <Method of manufacturing multilayer porous membrane> The multilayer porous membrane of this embodiment can be produced by a known method, for example, by forming a microporous PO membrane and then arranging a porous layer on at least one side of the microporous PO membrane.

[0158] If desired, the multilayer porous membrane can be produced, for example, by forming a PO microporous membrane, and then disposing a first porous layer on one side of the PO microporous membrane and a second porous layer on the other side of the PO microporous membrane. Alternatively, the PO microporous membrane and the porous layer can be produced by coextrusion, or the first and second porous layers can be extruded onto both sides of the PO microporous membrane, respectively, or the PO microporous membrane and the porous layer can be bonded together after being separately produced.

[0159] Furthermore, the method for producing a multilayer porous membrane may optionally include a step of obtaining a multilayer porous membrane by arranging a porous layer on at least one side of a microporous PO membrane, and forming a thermoplastic polymer-containing layer on at least one side of the obtained multilayer porous membrane.

[0160] (Method of producing a polyolefin microporous membrane) The method for producing the polyolefin microporous membrane (PO microporous membrane) is not particularly limited, and any known production method can be used.

[0161] In general, the manufacturing method of a polyolefin microporous membrane is roughly divided into a wet method and a dry method. In the wet method, an extractable material is added to and dispersed in a polyolefin, and after molding, the extractable material is extracted with a liquid such as a solvent to make the membrane porous. Examples of the dry method include (a) a method in which an unstretched body having a crystalline lamellar structure is formed during melt extrusion molding, and the body is mainly stretched uniaxially to open the lamellae to make the membrane porous, and (b) a method in which incompatible particles such as inorganic particles are added to a polyolefin and then stretched to peel off the interface between different materials to make the membrane porous.

[0162] Either a wet method or a dry method can be used for producing the microporous PO membrane of this embodiment. From the viewpoints of suppressing overall friction, high heat resistance, high pin removal property, and low resistance of the multilayer porous membrane, it is preferable not to use a β crystal method, in which β crystals with low crystal density are produced in a melt-extruded resin molded product and then stretched to cause crystal transition to α crystals with high crystal density, resulting in porosity due to the difference in crystal density between the two, as the dry method. It is more preferable not to use a β crystal nucleating agent, not to add a β crystal nucleating agent to the raw materials, intermediates, or products, or to prevent or remove the inclusion of a β crystal nucleating agent by observing the production line in the PO microporous membrane production process.

[0163] The method for producing the microporous PO membrane according to the present embodiment can be, for example: (1) A method in which a polyolefin resin composition and a pore-forming material are melt-kneaded to form a sheet, which is then stretched as necessary, and the pore-forming material is extracted to make the sheet porous; (2) A method in which a polyolefin resin composition is melt-kneaded and extruded at a high draw ratio, and then heat-treated and stretched to peel off the polyolefin crystal interface, thereby making the composition porous; (3) A method in which a polyolefin resin composition and an inorganic filler are melt-kneaded and formed into a sheet, and then the interface between the polyolefin and the inorganic filler is peeled off by stretching to make the sheet porous; (4) A method in which a polyolefin resin composition is dissolved and then immersed in a poor solvent for polyolefin to coagulate the polyolefin and simultaneously remove the solvent to make the composition porous; etc.

[0164] As an example of a method for producing a microporous PO membrane, a method in which a polyolefin resin composition and a pore-forming material are melt-kneaded and formed into a sheet, and then the pore-forming material is extracted will be described below.

[0165] First, the polyolefin resin composition and the pore-forming material are melt-kneaded. For example, the melt-kneading method may include a method in which the polyolefin resin and other additives, if necessary, are put into a resin kneading device such as an extruder, a feeder, a lab plastomill, a kneading roll, or a Banbury mixer, and the pore-forming material is introduced at an arbitrary ratio while the resin components are heated and melted, and kneaded.

[0166] Examples of the pore-forming material include plasticizers, inorganic materials, and combinations thereof. Examples of the plasticizer include, but are not limited to, non-volatile solvents capable of forming a homogeneous solution at or above the melting point of the polyolefin, such as hydrocarbons such as liquid paraffin and paraffin wax; esters such as dioctyl phthalate and dibutyl phthalate; and higher alcohols such as oleyl alcohol and stearyl alcohol. Among the plasticizers, liquid paraffin is preferred because, when the polyolefin resin is polyethylene and / or polypropylene, it is highly compatible with these, and even when the molten kneaded product is stretched, the interfacial peeling between the resin and the plasticizer is unlikely to occur, and uniform stretching tends to be easily performed. The inorganic material is not particularly limited, and examples thereof include oxide ceramics such as alumina, silica (silicon oxide), titania, zirconia, magnesia, ceria, yttria, zinc oxide, and iron oxide; nitride ceramics such as silicon nitride, titanium nitride, and boron nitride; ceramics such as silicon carbide, calcium carbonate, aluminum sulfate, aluminum hydroxide, potassium titanate, talc, kaolin clay, kaolinite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand; and glass fiber. These may be used alone or in combination of two or more. Among these inorganic materials, silica, alumina, and titania are preferred from the viewpoint of electrochemical stability, and silica is particularly preferred from the viewpoint of ease of extraction.

[0167] Next, the molten kneaded product is molded into a sheet. Examples of methods for producing a sheet-shaped molded product include a method in which the molten kneaded product is extruded into a sheet through a T-die or the like, and then brought into contact with a thermal conductor to a temperature sufficiently lower than the crystallization temperature of the resin component to solidify. Examples of thermal conductors used for cooling and solidifying include metal, water, air, and plasticizers. Among these, it is preferable to use a metal roll because of its high thermal conduction efficiency. In addition, when the extruded kneaded product is brought into contact with a metal roll, it is more preferable to sandwich the product between the rolls because this further increases the thermal conduction efficiency, and the sheet is oriented to increase the film strength and improve the surface smoothness of the sheet. The die lip interval when the molten kneaded product is extruded into a sheet from a T-die is preferably 200 μm or more, more preferably 500 μm or more or less, and also preferably 3,000 μm or less, and more preferably 2,500 μm or less. When the die lip distance is 200 μm or more, the occurrence of scum is reduced, and the impact on the film quality such as streaks and defects is small, and the risk of film breakage in the subsequent stretching process can be reduced. On the other hand, when the die lip distance is 3,000 μm or less, the cooling speed is fast, preventing uneven cooling and maintaining the thickness stability of the sheet.

[0168] The sheet-shaped molded body may also be rolled. Rolling can be performed, for example, by a pressing method using a double belt press or the like. By performing rolling, the orientation of the surface layer portion in particular can be increased. The rolling area ratio is preferably more than 1 time and not more than 3 times, and more preferably more than 1 time and not more than 2 times. When the rolling ratio exceeds 1 time, the surface orientation increases, and the membrane strength of the finally obtained porous membrane tends to increase. On the other hand, when the rolling ratio is 3 times or less, the orientation difference between the surface layer portion and the central interior is small, and a uniform porous structure tends to be formed in the thickness direction of the membrane.

[0169] Next, the pore-forming material is removed from the sheet-like molded body to obtain a porous membrane. For example, a method for removing the pore-forming material may be a method in which the sheet-like molded body is immersed in an extraction solvent to extract the pore-forming material and then thoroughly dried. The method for extracting the pore-forming material may be either a batch method or a continuous method. In order to suppress the shrinkage of the porous membrane, it is preferable to restrain the end of the sheet-like molded body during a series of steps of immersion and drying. In addition, it is preferable that the amount of the pore-forming material remaining in the porous membrane is less than 1% by mass with respect to the mass of the entire porous membrane.

[0170] The extraction solvent used when extracting the pore-forming material is preferably a poor solvent for the polyolefin resin and a good solvent for the pore-forming material, and has a boiling point lower than the melting point of the polyolefin resin. Examples of such extraction solvents include hydrocarbons such as n-hexane and cyclohexane; halogenated hydrocarbons such as methylene chloride and 1,1,1-trichloroethane; non-chlorine halogenated solvents such as hydrofluoroethers and hydrofluorocarbons; alcohols such as ethanol and isopropanol; ethers such as diethyl ether and tetrahydrofuran; and ketones such as acetone and methyl ethyl ketone. These extraction solvents may be recovered and reused by operations such as distillation. In addition, when an inorganic material is used as the pore-forming material, an aqueous solution of sodium hydroxide, potassium hydroxide, or the like can be used as the extraction solvent.

[0171] It is also preferable to stretch the sheet-like molded body or the porous membrane. The stretching may be performed before the pore-forming material is extracted from the sheet-like molded body. The stretching may also be performed on the porous membrane from which the pore-forming material has been extracted from the sheet-like molded body. Furthermore, the stretching may be performed before and after the pore-forming material is extracted from the sheet-like molded body.

[0172] As the stretching treatment, either uniaxial stretching or biaxial stretching can be suitably used, but biaxial stretching is preferred from the viewpoint of improving the strength, etc., of the resulting microporous PO membrane. When a sheet-like molded product is stretched biaxially at a high ratio, the molecules are oriented in the planar direction, and the finally obtained microporous membrane is less likely to tear and has high pin puncture strength.

[0173] Examples of the stretching method include simultaneous biaxial stretching, sequential biaxial stretching, multi-stage stretching, multiple stretching, etc. From the viewpoints of improving the puncture strength, uniformity of stretching, and shut-down property, simultaneous biaxial stretching is preferred. Also, from the viewpoint of ease of control of the plane orientation, sequential biaxial stretching is preferred.

[0174] Here, the simultaneous biaxial stretching refers to a stretching method in which MD stretching and TD stretching are performed simultaneously, and the stretching ratios in each direction may be different. The sequential biaxial stretching refers to a stretching method in which MD and TD stretching are performed independently, and while stretching is performed in MD or TD, the other direction is in an unconstrained state or fixed at a fixed length.

[0175] The areal stretching ratio is preferably 20 times or more, more preferably 25 times or more, and is preferably 100 times or less, more preferably 70 times or less. The areal stretching ratios in each axial direction are preferably 4 times or more in MD and 4 times or more in TD, more preferably 5 times or more in MD and 5 times or more in TD, and preferably 10 times or less in MD and 10 times or less in TD, and more preferably 8 times or less in MD and 8 times or less in TD. A total areal stretching ratio of 20 times or more tends to impart sufficient strength to the resulting microporous PO membrane, while a total areal stretching ratio of 100 times or less tends to prevent membrane breakage in the stretching step and achieve high productivity.

[0176] In order to suppress shrinkage of the PO microporous membrane, a heat treatment for heat setting can be performed after the stretching step or after the formation of the PO microporous membrane. The PO microporous membrane may also be subjected to post-treatment such as hydrophilization treatment with a surfactant or crosslinking treatment with ionizing radiation or the like.

[0177] The microporous PO membrane is preferably heat-treated for the purpose of heat setting in order to suppress shrinkage. Examples of the heat treatment method include a stretching operation carried out in a predetermined temperature atmosphere at a predetermined stretch ratio for the purpose of adjusting physical properties, and / or a relaxation operation carried out in a predetermined temperature atmosphere at a predetermined relaxation ratio for the purpose of reducing stretching stress. The relaxation operation may be carried out after the stretching operation. These heat treatments can be carried out using a tenter or roll stretching machine.

[0178] The stretching operation is preferably performed by stretching the membrane in MD and / or TD by 1.1 times or more, more preferably 1.2 times or more, from the viewpoint of obtaining a microporous PO membrane with even higher strength and higher porosity.

[0179] The relaxation operation is a shrinking operation in the MD and / or TD of the membrane. The relaxation rate is a value obtained by dividing the dimensions of the membrane after the relaxation operation by the dimensions of the membrane before the relaxation operation. When both MD and TD are relaxed, the relaxation rate is a value obtained by multiplying the relaxation rate in MD and the relaxation rate in TD. The relaxation rate is preferably 1.0 or less, more preferably 0.97 or less, and even more preferably 0.95 or less. From the viewpoint of membrane quality, the relaxation rate is preferably 0.5 or more. The relaxation operation may be performed in both MD and TD, or may be performed in only one of MD or TD.

[0180] The stretching and relaxation operation after the plasticizer extraction is preferably performed in TD from the viewpoint of process control and from the viewpoint of controlling the hole area in a 400° C. solder test. The temperature in the stretching and relaxation operation is preferably lower than the melting point (hereinafter also referred to as "Tm") of the polyolefin resin, and more preferably in the range of 1° C. to 25° C. lower than Tm. The above-mentioned range of temperature in the stretching and relaxation operation is preferable from the viewpoint of the balance between the reduction of the thermal shrinkage rate and the porosity.

[0181] (Porous layer arrangement method) The method for disposing a porous layer on at least one surface of the microporous PO membrane can be a known disposing method, coating method, lamination method, extrusion method, etc. For example, a method can be used in which a coating liquid or slurry containing the inorganic particles described above and, if desired, a resin binder and / or a dispersant is applied to a microporous PO membrane to form a porous layer.

[0182] The method for disposing a first porous layer on one side of the PO microporous membrane and a second porous layer on the other side of the PO microporous membrane can be a known disposing method, coating method, lamination method, extrusion method, etc. For example, there is a method in which a coating liquid or slurry containing the inorganic particles described above and, if desired, the resin binder and / or dispersant described above is applied to both sides of the PO microporous membrane to form a porous layer.

[0183] From the viewpoint of the relationship of the surface friction coefficient of the porous layer described above, in the process of arranging the porous layer, it is preferable to select the type of inorganic particle raw material based on the stress relaxation rate in the shear test, and the μ s and / or μ′ s From the viewpoint of easily controlling the above, it is more preferable to use barium sulfate, and it is even more preferable to use barium sulfate obtained by a sulfuric acid method.

[0184] The total of inorganic particles, resin binder and dispersant contained in the coating liquid or slurry is 100 volume %, and the ratio of inorganic particles is preferably more than 70 volume %, more preferably more than 75 volume %, even more preferably more than 80 volume %, even more preferably more than 85 volume %, and particularly preferably more than 90 volume %, and the upper limit is preferably 95 volume % or less, more preferably 93 volume % or less, even more preferably 92 volume % or less, and particularly preferably 91 volume % or less. When the volume ratio of inorganic particles in the coating liquid is within the above range, the ratio of inorganic particles to other components such as resin binder increases, making it easier to adjust the surface friction coefficient of the porous layer described above, and suppressing the increase in air permeability of the PO microporous membrane due to the porous layer, reducing the electrical resistance of the multilayer porous membrane, and contributing to the high compatibility of low friction, high heat resistance and low resistance of the multilayer porous membrane.

[0185] From the same viewpoint as the volume ratio, the mass ratio of the inorganic particles in the coating liquid or slurry is preferably more than 80 mass%, more preferably more than 90 mass%, even more preferably 93 mass% or more, even more preferably 95 mass% or more, and particularly preferably 97 mass% or more, based on 100 mass% of the total of the inorganic particles, the resin binder, and the dispersant. The upper limit of the mass ratio of the inorganic particles in the coating liquid or slurry is not particularly limited, and may be, for example, 100 mass% or less, less than 100 mass%, or 99 mass% or less.

[0186] From the viewpoint of the relationship of the surface friction coefficient of the porous layer described above and the viewpoint of enhancing the interaction between the inorganic particles and other contained components to further improve the thermal shrinkage suppression ability and strength of the multilayer porous film as well as the capacity and cycle characteristics of the nonaqueous electrolyte battery, it is preferable that the particle size distribution of the inorganic particle-containing coating liquid or slurry satisfies at least one of the following relationships: ·Average particle size D 50 About 0.01μm≦D 50 <0.60μm, 0.01μm≦D 50 ≦0.50μm, 0.10μm≦D 50 ≦0.45μm, 0.20μm≦D 50 ≦0.40μm, 0.25μm≦D 50 ≦0.35μm.

[0187] Methods for adjusting the particle size distribution of the inorganic particle-containing coating liquid or slurry as described above include, for example, a method in which barium sulfate is pulverized using a ball mill, bead mill, jet mill, etc. to obtain the desired particle size distribution, a method in which barium sulfate with multiple particle size distributions is prepared as an inorganic filler and then blended, and the like.

[0188] In forming an inorganic particle-containing slurry or coating liquid, from the viewpoints of the interaction between a water-soluble polymer such as poly(meth)acrylamide and barium sulfate, an increase in the number of contact points between the two, and the heat resistance of the multilayer porous membrane or separator, the ratio (Wb' / Wa') of the mass fraction Wa' of the water-soluble binder to the mass fraction Wb' of the water-insoluble binder contained in the slurry or coating liquid is preferably 1.0 or less, more preferably 0.5 or less, and even more preferably 0.3 or less, and the lower limit thereof is preferably 0 or more or exceeds 0.

[0189] A dispersant such as a surfactant may be added to the inorganic particle-containing coating liquid or slurry to stabilize the dispersion or improve the coating property. The dispersant is adsorbed to the surface of the inorganic particles in the slurry and stabilizes the inorganic particles by electrostatic repulsion, and is, for example, a polycarboxylate, a sulfonate, or a polyoxyether. The amount of the dispersant added is preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, in terms of solid content, and is preferably 5.0 parts by mass or less, more preferably 1.0 parts by mass or less, in terms of solid content.

[0190] In order to stabilize the dispersion or improve the coatability, and further to adjust the contact angle on the surface of the porous layer, various additives such as thickeners, wetting agents, antifoaming agents, and pH adjusters containing acids and alkalis may be added to the coating liquid. The total amount of these additives added is preferably 20 parts by mass or less of the active ingredient (the mass of the dissolved additive ingredient when the additive is dissolved in a solvent) per 100 parts by mass of inorganic particles, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less.

[0191] As for additives, anionic surfactants include, for example, higher fatty acid salts, alkyl sulfonates, alpha olefin sulfonates, alkanesulfonates, alkylbenzene sulfonates, sulfosuccinates, alkyl sulfates, alkyl ether sulfates, alkyl phosphates, alkyl ether phosphates, alkyl ether carboxylates, alpha sulfo fatty acid methyl esters, and methyl taurates. Nonionic surfactants include, for example, glycerin fatty acid esters, polyglycerin fatty acid esters, sucrose fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, polyoxyethylene fatty acid esters, fatty acid alkanolamides, and alkyl glucosides. Amphoteric surfactants include, for example, alkyl betaines, fatty acid amidopropyl betaines, and alkyl amine oxides. Cationic surfactants include, for example, alkyl trimethyl ammonium salts, dialkyl dimethyl ammonium salts, alkyl dimethyl benzyl ammonium salts, and alkyl pyridinium salts. Other examples include polymer surfactants such as fluorosurfactants, cellulose derivatives, polycarboxylates, and polystyrene sulfonates.

[0192] The medium for the coating liquid is preferably one in which the inorganic particles or resin binder can be uniformly and stably dispersed or dissolved, and examples thereof include N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, water, ethanol, toluene, hot xylene, methylene chloride, and hexane.

[0193] The method for dispersing or dissolving the inorganic particles and the resin binder in the medium of the coating liquid is not particularly limited as long as it can realize the dispersion characteristics of the coating liquid required for the coating process. For example, a ball mill, a bead mill, a planetary ball mill, a vibrating ball mill, a sand mill, a colloid mill, an attritor, a roll mill, high-speed impeller dispersion, a disperser, a homogenizer, a high-speed impact mill, ultrasonic dispersion, mechanical stirring with a stirring blade, etc. can be mentioned.

[0194] The method for applying the barium sulfate-containing coating liquid or barium sulfate-containing slurry to the PO microporous membrane is not particularly limited as long as it is a method that can realize the required layer thickness or coating area, and examples of the method include a gravure coater method, a small-diameter gravure coater method, a reverse roll coater method, a transfer roll coater method, a kiss coater method, a dip coater method, a knife coater method, an air doctor coater method, a blade coater method, a rod coater method, a squeeze coater method, a cast coater method, a die coater method, a screen printing method, a spray coating method, and the like.

[0195] In one embodiment, the barium sulfate-containing coating liquid or barium sulfate-containing slurry is applied to a PO microporous membrane so that the coating thickness of the porous layer on at least one side of the PO microporous membrane is preferably 4 μm or less, more preferably less than 3 μm, even more preferably less than 2.5 μm, still more preferably 2.4 μm or less, particularly preferably 2.0 μm or less, and most preferably 1.5 μm or less, with the lower limit being preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 0.7 μm or more, and particularly preferably 1.0 μm or more, from the viewpoints of suppressing an increase in air permeability of the PO microporous membrane, forming a strong porous layer, reducing the thickness of the resulting multilayer porous membrane or separator, and heat resistance (i.e., ability to suppress thermal shrinkage).

[0196] In one embodiment, the inorganic particle-containing coating liquid or slurry is applied to the microporous PO membrane so that the coating weight of the porous layer is preferably 1.0 g / m from the viewpoint of the action mechanism of the present invention. 2More preferably, 1.5 g / m 2 The concentration is preferably 5.0 g / m or more. 2 Less than 4.0 g / m 2 This is done so that:

[0197] If desired, the PO microporous membrane may be subjected to a surface treatment prior to application of the inorganic particle-containing coating liquid or slurry. Surface treatment of the PO microporous membrane may facilitate application of the coating liquid or slurry and may improve adhesion between the barium sulfate-containing porous layer and the PO microporous membrane surface after application. The method of surface treatment is not particularly limited as long as it does not significantly impair the porous structure of the PO microporous membrane, and examples of the method include corona discharge treatment, plasma discharge treatment, mechanical roughening, solvent treatment, acid treatment, and ultraviolet oxidation.

[0198] The method for removing the medium from the coating film after coating is not particularly limited as long as it does not adversely affect the PO microporous membrane, and examples thereof include a method of drying the PO microporous membrane at a temperature below its melting point while fixing it, a method of drying under reduced pressure at a low temperature, and extraction drying. In addition, a part of the solvent may be left as long as it does not significantly affect the properties of the nonaqueous electrolyte battery. For a multilayer porous membrane formed by laminating a PO microporous membrane and a porous layer, it is preferable to appropriately adjust the drying temperature, winding tension, etc., from the viewpoint of controlling the shrinkage stress in the MD direction.

[0199] From the viewpoints of overall friction suppression, high heat resistance, high pin removal property and low resistance of the multilayer porous membrane throughout the process of arranging the porous layers, it is preferable not to use a β-crystal nucleating agent, not to add a β-crystal nucleating agent to the raw materials, intermediates or products, or to prevent or remove the inclusion of a β-crystal nucleating agent by observing the production line.

[0200] (Method of forming thermoplastic polymer-containing layer) The method for forming a thermoplastic polymer-containing layer on a microporous PO membrane or porous layer as a substrate is not particularly limited, and examples thereof include a method in which a coating liquid containing a thermoplastic polymer is applied to the microporous PO membrane or porous layer.

[0201] The method of applying the coating solution containing a thermoplastic polymer to the PO microporous membrane or porous layer is not particularly limited as long as it can achieve the required layer thickness and coating area. For example, gravure coater method, small diameter gravure coater method, reverse roll coater method, transfer roll coater method, kiss coater method, dip coater method, knife coater method, air doctor coater method, blade coater method, rod coater method, squeeze coater method, cast coater method, die coater method, screen printing method, spray coating method, spray coater coating method, inkjet coating method, etc. can be mentioned. Among these, gravure coater method or spray coating method is preferred from the viewpoint of high degree of freedom of the coating shape of the thermoplastic polymer and easy obtaining of a preferred area ratio. For the formation of a dot-shaped pattern of the thermoplastic polymer-containing layer, gravure coater method, inkjet coating, and coating method that is easy to adjust the printing plate are preferred.

[0202] When a thermoplastic polymer is coated onto a PO microporous membrane, if the coating solution penetrates into the microporous membrane or the porous layer, the adhesive resin fills the surfaces and interiors of the pores, reducing permeability, and therefore the medium for the coating solution is preferably a poor solvent for the thermoplastic polymer.

[0203] When a poor solvent for the thermoplastic polymer is used as the medium for the coating liquid, the coating liquid does not penetrate into the microporous membrane or the porous layer, and the adhesive polymer is mainly present on the surface of the microporous membrane, which is preferable from the viewpoint of suppressing the decrease in permeability. Such a medium is preferably water. In addition, the medium that can be used in combination with water is not particularly limited, but may include ethanol, methanol, etc. If desired, a defoamer may be added to the coating liquid containing the thermoplastic polymer.

[0204] With regard to the thermoplastic polymer-containing coating liquid (hereinafter also simply referred to as paint), from the viewpoint of adhesion to the separator electrode, and from the viewpoint of compatibility with high-temperature storage tests while simultaneously achieving resistance to the separator temperature rise and resistance to cycle deterioration, the paint viscosity is preferably 30 cP or more, more preferably 50 cP or more, and preferably 100 cP or less, more preferably 80 cP or less. From the same viewpoint, the pH of the paint is preferably 5 or more, more preferably 5.5 or more, and preferably 7.9 or less, more preferably 7.7 or less.

[0205] Furthermore, it is preferable to subject the microporous membrane as the separator substrate to a surface treatment prior to coating, since this makes it easier to apply the coating liquid and improves the adhesion between the microporous membrane or porous layer and the adhesive polymer. The method of surface treatment is not particularly limited as long as it does not significantly impair the porous structure of the microporous membrane, and examples of the method include corona discharge treatment, plasma treatment, mechanical roughening, solvent treatment, acid treatment, and ultraviolet oxidation.

[0206] In the case of the corona discharge treatment method, the corona treatment intensity on the substrate surface is 1 W / (m 2 / min) or more, and 3W / (m 2 / min) or more is more preferable, and 5 W / (m 2 / min) or more, and 40 W / (m 2 / min) or less, and 32 W / (m 2 / min) or less, and 25 W / (m 2 / min) or less is even more preferable.

[0207] The method for removing the solvent from the coating film after coating is not particularly limited as long as it does not adversely affect the microporous membrane or the porous layer, for example, a method of drying the microporous membrane and / or the porous layer at a temperature below their melting point while fixing them, a method of drying under reduced pressure at a low temperature, a method of immersing in a poor solvent for the adhesive polymer to coagulate the adhesive polymer and simultaneously extract the solvent, etc.

[0208] The drying rate of the coating is 0.03 g / (m 2 s) or more, and 0.05 g / (m 2 s) or more, and 0.08g / (m 2 s) or more, and more preferably 4.0 g / (m 2 s) or less, and 3.5 g / (m 2 s) or less, and 3.0 g / (m 2 In drying the coating film, it is also preferable to raise the temperature by warming or heating to an extent that does not damage the particle shape of the thermoplastic polymer-containing layer.

[0209] <Separator for non-aqueous electrolyte battery, and non-aqueous electrolyte battery> The multilayer porous membrane according to the present embodiment can be used as a separator for a nonaqueous electrolyte battery. The nonaqueous electrolyte battery includes a positive electrode, a separator, a negative electrode, and a nonaqueous electrolyte, and specifically includes a lithium battery, a lithium secondary battery, a lithium ion secondary battery, a sodium secondary battery, a sodium ion secondary battery, a magnesium secondary battery, a magnesium ion secondary battery, a calcium secondary battery, a calcium ion secondary battery, an aluminum secondary battery, an aluminum ion secondary battery, a nickel hydrogen battery, a nickel cadmium battery, an electric double layer capacitor, a lithium ion capacitor, a redox flow battery, and a lithium sulfur battery. Among these, from the viewpoint of practicality, a lithium battery, a lithium secondary battery, a lithium ion secondary battery, a nickel hydrogen battery, or a lithium ion capacitor is preferable, and a lithium ion secondary battery is more preferable.

[0210] A nonaqueous electrolyte battery can be produced, for example, by stacking a positive electrode and a negative electrode with a separator made of the multilayer porous membrane described above between them, and, as necessary, winding or zigzag forming a laminated electrode body or a wound electrode body or a zigzag folded body, which is then loaded into an exterior body, connecting the positive and negative electrodes to the positive and negative electrode terminals of the exterior body via lead bodies or the like, and further injecting a nonaqueous electrolyte containing a nonaqueous solvent such as a chain or cyclic carbonate and an electrolyte such as a lithium salt into the exterior body, and then sealing the exterior body.

[0211] The nonaqueous electrolyte battery includes the above-described laminate, a wound laminate, or a zigzag laminate, together with a nonaqueous electrolyte, in an exterior body such as a cylindrical can, a pouch-type case, a laminate case, etc. The nonaqueous electrolyte battery using the multilayer porous membrane according to the present embodiment as a separator may not only be excellent in safety, but also in energy density and cycle characteristics.

[0212] When the nonaqueous electrolyte battery is a secondary battery, a positive electrode terminal is welded to an end of a positive electrode laminate consisting of a positive electrode current collector and a positive electrode active material layer, and a negative electrode terminal is welded to an end of a negative electrode laminate consisting of a negative electrode current collector and a negative electrode active material layer, whereby charging and discharging of the secondary battery including the positive electrode laminate with terminals and the negative electrode laminate with terminals can be performed.

[0213] Furthermore, the positive electrode laminate with terminals and the negative electrode laminate with terminals are laminated via a separator, and wound or folded as desired, and the resulting laminate, wound body, or folded body is housed in an outer casing, a nonaqueous electrolyte solution is injected into the outer casing, and the outer casing is sealed to obtain a secondary battery.

[0214] When a non-aqueous electrolyte secondary battery is manufactured using the multilayer porous membrane according to this embodiment as a separator, a known positive electrode, negative electrode, and non-aqueous electrolyte may be used.

[0215] The positive electrode material is not particularly limited, but examples thereof include lithium-containing composite oxides such as LiCoO2, LiNiO2, spinel-type LiMnO4, and olivine-type LiFePO4.

[0216] The negative electrode material is not particularly limited, but examples thereof include carbon materials such as graphite, non-graphitizable carbon, easily graphitizable carbon, and composite carbon bodies; silicon, tin, metallic lithium, and various alloy materials.

[0217] The non-aqueous electrolyte is not particularly limited, but an electrolyte solution obtained by dissolving an electrolyte in an organic solvent can be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. Examples of the electrolyte include lithium salts such as LiClO4, LiBF4, and LiPF6. EXAMPLES

[0218] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples and comparative examples.

[0219] Testing and Evaluation Methods

[0220] <Viscosity average molecular weight (Mv)> The intrinsic viscosity [η] (dl / g) at 135°C in decalin solvent was determined based on ASTM-D4020. The Mv of the polyethylene and polyolefin microporous membranes was calculated by the following formula. [η]=6.77×10 -4 Mv 0.67 The Mv of polypropylene was calculated using the following formula. [η]=1.10×10 -4 Mv 0.80

[0221] <Thickness of polyolefin microporous membrane, multilayer porous membrane, and porous layer (μm)> The thickness of the polyolefin microporous membrane and the multilayer porous membrane were measured at room temperature (23±2° C.) using a micro thickness gauge "KBM (trademark)" manufactured by Toyo Seiki Co., Ltd., and the coating thickness of the porous layer was calculated from each thickness. In addition, from the viewpoint of detection from the multilayer porous membrane, it is also possible to measure the thickness of each layer using a cross-sectional SEM image.

[0222] <Melt index (MI) of microporous polyolefin membrane (g / 10 min)> The melt index (MI) of a polyolefin microporous membrane (PO microporous membrane) was measured according to JIS K7210:1999 (Melt mass flow rate (MFR) and melt volume flow rate (MVR) of plastics-thermoplastics). A load of 21.6 kgf was applied to the membrane at 190°C, and the amount of resin (g) flowing out from an orifice with a diameter of 1 mm and a length of 10 mm in 10 minutes was measured, and the value rounded off to the first decimal place was taken as the MI.

[0223] <Average particle size and particle size distribution of inorganic particles> The particle size distribution and median diameter (μm) of the inorganic particle dispersion or slurry coating liquid were measured using a laser particle size distribution measuring device (Microtrac MT3300EX, manufactured by Nikkiso Co., Ltd.). If necessary, the particle size distribution of the inorganic particle dispersion or slurry coating liquid was adjusted using the particle size distribution of water or resin binder as a baseline. The particle size at which the cumulative frequency is 50% was defined as D 50 It was decided.

[0224] <BET specific surface area of ​​inorganic particles (m 2 / g)> The specific surface area of ​​the inorganic particles was measured by the nitrogen adsorption BET method.

[0225] <Stress relaxation rate of inorganic particles> The measurements were carried out at room temperature using a powder bed shear force measuring device NS-S500 (manufactured by Nano Seeds). The device is broadly composed of the measuring device body and a control box. The measuring device body is composed of a powder bed shear cell, a pressure unit, a linear actuator, etc., and the control box is composed of various instrument amplifiers and a control computer. The substrate used was carbide (surface polished, material G5). The sample was filled into a shear cell, the top surface of the powder layer was flattened, and then a pressing load of 40 N was applied, and the stress relaxation rate was calculated from the following formula. Stress relaxation rate = ((indentation load) - (load 100 seconds after reaching the indentation load)) / (indentation load) x 100

[0226] <Air permeability (sec / 100cm 3 ), and the air permeability ratio of the multilayer porous membrane to the polyolefin microporous membrane> The air permeability of the multilayer porous membrane and the polyolefin microporous membrane, where the air permeability was determined as the air permeability resistance in accordance with JIS P-8117, was measured in accordance with JIS P-8117 by measuring the air permeability resistance of the multilayer porous membrane and the polyolefin microporous membrane in an atmosphere at a temperature of 23°C and a humidity of 40% using a Gurley air permeability meter "G-B2 (trademark)" manufactured by Toyo Seiki Co., Ltd. The air permeability of the porous layer was calculated by subtracting the air permeability of the polyolefin microporous membrane from the air permeability of the multilayer porous membrane. Air permeability increase rate = Air permeability of porous layer / Air permeability of polyolefin microporous membrane The air permeability increase rate was calculated according to the following formula: Furthermore, the air permeability per unit thickness of the porous layer was also calculated.

[0227] <Content of inorganic particles in the porous layer (mass % and volume %)> The content of inorganic particles in the porous layer can be calculated from the blending ratio of the constituent materials when preparing the coating liquid. From the viewpoint of detection from the multilayer porous membrane, it is also possible to use TG-DTA to measure the weight change of each of the organic matter and the inorganic particles. Specifically, the porous layer part is scraped off from the multilayer porous membrane with a glass plate, and 8 mg to 10 mg is collected. The sample of the collected porous layer is set in the device, and the temperature is raised from room temperature to 600°C at a heating rate of 10°C / min in an air atmosphere, and the weight change is measured and calculated. Note that the mass content and volume content of the inorganic particles are interchangeable based on the specific gravity of the inorganic particles.

[0228] <Porosity (%)> A 10 cm x 10 cm square sample was cut from the microporous membrane and its volume (cm 3 ) and mass (g), and compare them with the film density (g / cm 3 ) the porosity was calculated using the following equation. Porosity (%) = (volume-mass / density) / volume x 100

[0229] <Measurement of the surface friction coefficient of porous layer> (Friction test) For the surface of the separator sample on which the porous layer was formed, a MH-3 friction tester manufactured by Toyo Seiki Seisakusho was used, and under conditions of sled mass 200g, load range 2N, contact area 63mm x 63mm (felt material), contact feed speed 100mm / min, temperature 23°C, and humidity 50%, the maximum value within a measurement distance of 5mm was determined as the static friction coefficient, and the value at a measurement distance of 300mm was determined as the kinetic friction coefficient. Measurements were made three times in MD or TD, and the average values ​​were calculated to determine the respective friction coefficients. The SUS plate used for the measurement was a SUS304 6F processed product (pre-process: plate milling, special #200 buff + nitriding + finishing, buff finishing: uniform processing direction (width direction processing), polished with special #200 (tolerance of about #200 to #230)) on the table.

[0230] <Piercing strength (N) and area weight conversion piercing strength (N / (g / m 2 ))> Using a Kato Tech handy compression tester "KES-G5 (trademark)", the microporous membrane or multilayer porous membrane was fixed with a sample holder with an opening diameter of 11.3 mm. Next, a puncture test was performed on the center of the fixed microporous membrane or multilayer porous membrane in an atmosphere of temperature 23°C and humidity 40% with a needle tip curvature radius of 0.5 mm and a puncture speed of 2 mm / sec, to obtain the raw puncture strength (gf) as the maximum puncture load. The obtained puncture strength (N) was converted to basis weight (N / (g / m 2 )) was also calculated.

[0231] <Dry heat shrinkage rate (%) at 130℃ and 150℃> As a sample, the multilayer porous membrane was cut into a size of 100 mm in the MD direction and 100 mm in the TD direction, and left to stand in an oven at 130°C or 150°C for 1 hour. At this time, the sample was sandwiched between 10 sheets of paper so that the hot air would not directly hit the sample. After removing the sample from the oven and cooling, the length (mm) was measured and the thermal shrinkage was calculated using the following formula. The measurement was performed in the MD direction and the TD direction, and the average of both values ​​was displayed as the thermal shrinkage. Heat shrinkage rate (%) = {(100 - length after heating) / 100} x 100

[0232] <Wet heat shrinkage rate at 140℃ (%)> The multilayer porous membrane was cut into 50 mm in the MD direction and 50 mm in the TD direction, and sandwiched between Teflon (registered trademark) sheets (thickness 100 μm, 60 mm square). This laminate was stored in a package (thickness 35 μm, 100 mm square) made of aluminum laminate film, 0.5 mL of propylene carbonate was poured, the multilayer porous membrane was immersed in propylene carbonate, and the remaining piece was sealed to obtain a sample. The sample was left to stand for 24 hours, and then left to stand in an oven at 140 ° C. for 1 hour. The sample was taken out of the oven and cooled, and the length (mm) of the multilayer porous membrane in each direction was measured, and the heat shrinkage was calculated by the following formula. Measurements were performed in the MD direction and the TD direction, and the average of both values ​​was displayed as the heat shrinkage. Heat shrinkage rate (%) = {(50 - length after heating) / 50} x 100.

[0233] <180° peel strength (N / m)> The surface of the multilayer porous membrane cut into 2 mm x 7 mm was attached to a glass plate with double-sided tape on the side opposite to the coating layer to be measured, and tape (product name "Mending Tape MP-12", manufactured by 3M) was attached to the coating layer. 5 mm of the tip of the tape was peeled off, and the tip of the tape was clamped with a chuck in a tensile tester (model "AG-IS, SLBL-1kN, manufactured by Shimadzu Corporation) so that the tape was peeled off at an angle of 180° to the surface direction of the multilayer porous membrane. A tensile test was performed at a pulling speed of 50 mm / s, a temperature of 25 degrees, and a relative humidity of 40%, and the tensile strength (N / m) was measured.

[0234] <Glass transition temperature of thermoplastic polymer (℃)> An appropriate amount of the thermoplastic polymer coating solution (non-volatile content = 30%) was placed on an aluminum dish and dried for 30 minutes in a hot air dryer at 130 ° C. Approximately 17 mg of the dried film was packed into an aluminum container for measurement, and a DSC curve and a DDSC curve were obtained under a nitrogen atmosphere using a DSC measurement device (Shimadzu Corporation, DSC6220). The measurement conditions were as follows. (1st stage heating program) Start at 70℃, increase temperature at a rate of 15℃ per minute. After reaching 110℃, maintain temperature for 5 minutes. (2nd stage cooling program) Decrease temperature from 110℃ at a rate of 40℃ per minute. After reaching -50℃, maintain for 5 minutes. (Third stage heating program) The temperature was increased from -50°C to 130°C at a rate of 15°C per minute. DSC and DDSC data were obtained during this third temperature increase. The glass transition temperature (Tg) was determined as the intersection point between the baseline (a straight line extending the baseline of the obtained DSC curve toward the higher temperature side) and the tangent at the inflection point (the point where the upward convex curve changes to a downward convex curve).

[0235] <Dot diameter and distance between dots> For the thermoplastic polymer-containing coating liquid, the dot diameter of the coating pattern was measured using a microscope (model: VHX-7000, manufactured by Keyence Corporation). The separator sample was photographed at 100x (coaxial epi-illumination), and the diameters of multiple dots (5 points) were measured in measurement mode, and the average value was calculated as the dot diameter. In addition, the distance from the outer edge of a dot to the outer edge of the nearest other dot was measured in measurement mode for five observation points, and the average value was calculated as the dot distance.

[0236] <Adhesion to electrodes> The multilayer porous membrane or separator obtained in each Example and Comparative Example and the negative electrode (manufactured by Enertech, negative electrode material: graphite, conductive additive: acetylene black, L / W: 20 mg / cm on both sides) as an adherend 2 , Cu current collector thickness: 10 μm, negative electrode thickness after pressing: 140 μm) were cut into rectangular shapes with a width of 15 mm and a length of 60 mm, and these were overlapped so that the thermoplastic polymer-containing layer of the multilayer porous membrane or the separator and the negative electrode active material faced each other to obtain a laminate, and then the laminate was pressed under the following conditions. Press pressure: 1MPa Temperature: 90℃ Press time: 1 minute The laminate after pressing was subjected to a 90° peel test at a peel speed of 50 mm / min by fixing the electrode and gripping and pulling the multilayer porous membrane or separator using Imada Co., Ltd. force gauges ZP5N and MX2-500N (product name), and the peel strength was measured. At this time, the average value of the peel strength in the peel test for a length of 40 mm performed under the above conditions was adopted as the adhesive strength with the electrode. The adhesive strength was measured before and after the laminate was immersed in propylene carbonate (PC), and the adhesive strength before the PC impregnation was expressed as dry adhesive strength, and the adhesive strength after the PC impregnation was expressed as wet adhesive strength. When a separator that achieves an adhesive strength of preferably 1.0 N / m or more, more preferably 1.8 N / m or more as the adhesive strength obtained by this method is used in a non-aqueous electrolyte battery, the adhesive strength with the opposing positive and negative electrodes is good. From the viewpoint of ionic resistance, the adhesive strength is preferably 100.0 N / m or less.

[0237] <Pin removal after winding the battery> Using a manual winding machine manufactured by Kaito Seisakusho Co., Ltd., a winding sample (12) with a length of 3 m and a width of 60 mm was prepared as shown in FIG. 2(A), which shows the overall configuration of the device. As shown in FIG. 1, two separators and a positive electrode (manufactured by Enertech, positive electrode material: LiCoO2, conductive additive: carbon black (Super-P Li), binder: PVDF, L / W: 36 mg / cm on both sides) were wound. 2 , thickness of Al collector: 15μm, 5.47mAh / cm 2 ) and a negative electrode (Enertech, negative electrode material: graphite, conductive additive: carbon black (Super-P Li), binder: PVDF, L / W: 20 mg / cm on both sides 2 , Cu collector thickness: 10μm, 5.75mAh / cm 2 ) and one sheet of the winding section 1, totaling four sheets, were wound around pin (9) under a load of 400 g. In the winding section configuration shown in FIG. 2(B), pin I (10) was removed, and the wound sample (12) was pulled by hand to remove it from pin II (11). After removal, the pin removal properties were evaluated based on the wound appearance of the sample according to the following criteria. A (Good): The percentage of items that are pulled by the pin and have a displacement of 2 mm or more from the area in contact with the pin before the pin is removed is 1 item / 100 or less B (defective): The percentage of items that are pulled by the pin and the contact part of the pin is shifted by 2 mm or more from before the pin was removed. 2-4 items / 100 items C (severely defective): The percentage of parts that are pulled by the pin and have shifted 2 mm or more from the part in contact with the pin before the pin was removed: 5 / 100 or more

[0238] <Nail penetration test> (Preparation of positive electrode) The positive electrode active material is lithium nickel manganese cobalt composite oxide powder (LiNi 1 / 3 Mn 1 / 3 Co 1 / 3A mixture of 85 parts by mass of a mixed positive electrode active material obtained by mechanically mixing lithium manganese oxide powder (LiMn2O4) and lithium manganese composite oxide powder (LiMn2O4) in a mass ratio of 70:30, 6 parts by mass of acetylene black as a conductive assistant, and 9 parts by mass of PVdF as a binder were mixed uniformly using N-methyl-2-pyrrolidone (NMP) as a solvent to prepare a positive electrode mixture paste. This positive electrode mixture paste was uniformly applied to both sides of a 20 μm thick current collector made of aluminum foil, dried, and then compression molded with a roll press machine to adjust the thickness of the positive electrode mixture layer so that the total thickness was 130 μm. A positive electrode was prepared by using a rectangular sheet with a short side of 95 mm and a long side of 120 mm, with an aluminum foil with a length of 20 mm that was not coated with the active material as a lead tab on the upper part of the short side.

[0239] (Preparation of negative electrode) A negative electrode mixture-containing paste was prepared by mixing 91 parts by mass of graphite, which is a negative electrode active material, and 9 parts by mass of PVdF, which is a binder, uniformly using NMP as a solvent. This negative electrode mixture-containing paste was uniformly applied to both sides of a 15 μm-thick current collector made of copper foil, dried, and then compression-molded with a roll press machine to adjust the thickness of the negative electrode mixture layer so that the total thickness was 130 μm. A negative electrode was prepared on a rectangular sheet with a short side of 95 mm and a long side of 120 mm, with a 20 mm-long copper foil without active material coating as a lead tab on the upper part of the short side.

[0240] (Preparation of non-aqueous electrolyte) The non-aqueous electrolyte was prepared by dissolving LiPF6 as a solute in a mixed solvent of ethylene carbonate: ethyl methyl carbonate: dimethyl carbonate = 1: 1: 1 (volume ratio) to a concentration of 1.0 mol / L.

[0241] (Cell preparation) The electrode plate laminate was produced by stacking 27 positive electrode sheets and 28 negative electrode sheets alternately and isolating each sheet with a multilayer porous film as a separator. The separator was a strip-shaped separator with a width of 125 mm, which was folded alternately in a zigzag pattern to produce an electrode plate laminate. After pressing the electrode plate laminate into a flat plate, it was housed in an aluminum laminate film and three sides were heat-sealed. The positive electrode lead tab and the negative electrode lead tab were each led out from one side of the laminate film. After drying, the nonaqueous electrolyte was injected into the laminate film with the three sides sealed, and the remaining side was sealed. The laminated lithium ion secondary battery produced in this way was designed to have a capacity of 10 Ah.

[0242] (Nail penetration rating) The laminated lithium-ion secondary battery was placed on an iron plate in a temperature-controllable explosion-proof booth. The temperature in the explosion-proof booth was set to 40°C, and an iron nail with a diameter of 3.0 mm was inserted into the center of the laminated lithium-ion secondary battery at a speed of 2 mm / sec. The nail was maintained in the penetrated state. The temperature of a thermocouple installed inside the nail so that the temperature inside the laminated battery could be measured after the nail penetrated was measured, and the presence or absence of ignition and the maximum temperature reached were evaluated as follows. A: No fire, maximum temperature is less than 300℃ B: No ignition, maximum temperature reached is 300℃ or more C: Ignition occurs 15 seconds after the start of the test D: Ignition occurs within 15 seconds of starting the test

[0243] <Battery evaluation> (a. Preparation of Positive Electrode) Lithium nickel manganese cobalt composite oxide (Li[Ni 1 / 3 Mn 1 / 3 Co 1 / 391.2 parts by mass of ]O2), 2.3 parts by mass each of flake graphite and acetylene black as conductive materials, and 4.2 parts by mass of polyvinylidene fluoride (PVDF) as a resin binder were prepared, and these were dispersed in N-methylpyrrolidone (NMP) to prepare a slurry. This slurry was applied to one side of an aluminum foil with a thickness of 20 μm to serve as the positive electrode using a die coater, with the positive electrode active material coating amount being 120 g / m 2 After drying at 130°C for 3 minutes, the positive electrode active material was pressed using a roll press so that the bulk density of the positive electrode active material was 2.90 g / cm 3 The positive electrode was compressed and molded to have an area of ​​2.00 cm. 2 It was punched into a circular shape.

[0244] (b. Preparation of the negative electrode) As the negative electrode active material, 96.6 parts by mass of artificial graphite, 1.4 parts by mass of ammonium salt of carboxymethyl cellulose and 1.7 parts by mass of styrene-butadiene copolymer latex were prepared as the resin binder, and these were dispersed in purified water to prepare a slurry. This slurry was applied to one side of a 16 μm-thick copper foil serving as a negative electrode current collector using a die coater so that the negative electrode active material was 53 g / m 2 After drying at 120°C for 3 minutes, the negative electrode active material was pressed using a roll press so that the bulk density of the negative electrode active material was 1.35 g / cm 3 This was compression molded to obtain a negative electrode with an area of ​​2.05 cm. 2 It was punched into a circular shape.

[0245] (c. Preparation of non-aqueous electrolyte) A non-aqueous electrolyte solution was prepared by dissolving LiPF6 as a solute in a mixed solvent of ethylene carbonate:ethyl carbonate = 1:2 (volume ratio) to a concentration of 1.0 ml / L.

[0246] (d. Battery Assembly) The negative electrode, the multilayer porous membrane, and the positive electrode were stacked in this order from the bottom so that the active material surfaces of the positive and negative electrodes faced each other. This laminate was placed in a lidded stainless steel metal container insulated from the container body and the lid so that the copper foil of the negative electrode and the aluminum foil of the positive electrode were in contact with the container body and the lid, respectively, to obtain a cell. This cell was dried at 70°C under reduced pressure for 10 hours. Thereafter, a nonaqueous electrolyte was poured into the container in an argon box and the container was sealed to obtain an evaluation battery.

[0247] (e. Cycle Test) The battery assembled in (d. Battery Assembly) above was charged at a temperature of 25°C with a current value of 3 mA (approximately 0.5 C) up to a battery voltage of 4.2 V, and then the current value was tapered from 3 mA to maintain 4.2 V. In this manner, the initial charging after battery fabrication was performed for a total of approximately 6 hours, and then the battery was discharged at a current value of 3 mA down to a battery voltage of 3.0 V. Next, at 25°C, the battery was charged to a battery voltage of 4.2 V at a current value of 6 mA (approximately 1.0 C), and then the current was tapered from 6 mA to maintain the battery voltage at 4.2 V. In this manner, the battery was charged for a total of approximately 3 hours, and then discharged to a battery voltage of 3.0 V at a current value of 6 mA, and the discharge capacity at that point was recorded as the 1C discharge capacity (mAh). Next, at 25°C, the battery was charged to a battery voltage of 4.2 V at a current value of 6 mA (approximately 1.0 C), and then the current value was tapered from 6 mA to maintain the battery voltage at 4.2 V for a total of approximately 3 hours. After that, the battery was discharged to a battery voltage of 3.0 V at a current value of 60 mA (approximately 10 C), and the discharge capacity at that time was recorded as the 10 C discharge capacity (mAh). The battery was then discharged at a discharge current of 1 C to a discharge cut-off voltage of 3 V at a temperature of 25° C., and then charged at a charge current of 1 C to a charge cut-off voltage of 4.2 V. This constitutes one cycle, and charging and discharging were repeated. The cycle characteristics were evaluated according to the following criteria, using the capacity retention rate after 300 cycles relative to the initial capacity (capacity in the first cycle). A: Capacity retention rate of 83% or more B: Capacity retention rate of 80% or more but less than 83% C: Capacity retention rate of 75% or more but less than 80% D: Capacity retention rate of less than 75%

[0248] [Example 1] Using a tumbler blender, a polymer mixture was formed of 46.5% by mass of polyethylene (PE) homopolymer with a viscosity average molecular weight (Mv) of 700,000, 46.5% by mass of PE homopolymer with a Mv of 250,000, and 7% by mass of polypropylene (PP) homopolymer with a Mv of 400,000. 1 part by mass of pentaerythrityl-tetrakis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] was added as an antioxidant to 99 parts by mass of the polymer mixture, and the mixture was dry-blended again using a tumbler blender to obtain a polymer mixture. The obtained polymer mixture was replaced with nitrogen and then fed to a twin-screw extruder under a nitrogen atmosphere using a feeder. Liquid paraffin (dynamic viscosity at 37.78°C 7.59×10 -5 m 2 / s) was pumped into the extruder cylinder by a plunger pump.

[0249] The mixture was melt-kneaded, and the feeder and pump were adjusted so that the ratio of liquid paraffin in the total mixture extruded was 68% by mass (resin composition concentration was 32% by mass). The melt-kneading conditions were a set temperature of 200°C, a screw rotation speed of 70 rpm, and a discharge rate of 145 kg / h.

[0250] Next, the molten mixture was extruded through a T-die onto a cooling roll whose surface temperature was controlled at 25° C., and cast to obtain a gel sheet having a thickness of 1,350 μm.

[0251] Next, the gel sheet was introduced into a simultaneous biaxial tenter stretching machine and biaxially stretched. The stretching conditions were MD magnification 7.0 times, TD magnification 6.38 times, and set temperature 122 ° C. Next, the gel sheet was introduced into a methylene chloride tank and thoroughly immersed in methylene chloride to extract and remove liquid paraffin, and then the methylene chloride was dried and removed to obtain a porous body.

[0252] The porous body was then introduced into a TD tenter and heat-set. The heat-setting temperature was 132°C, the TD maximum magnification was 1.85 times, and the relaxation rate was 0.784, to obtain a polyolefin microporous membrane (PO microporous membrane A) having a thickness of 12.0 μm. The resin composition of the obtained polyolefin microporous membrane and the above measurement results are shown in Table 1.

[0253] Next, using inorganic particles having the average particle size (D50), BET specific surface area, and stress relaxation rate shown in Table 2, a dispersant, a water-soluble binder, and a water-insoluble binder resin binder were mixed with the inorganic particles as shown in Table 3, and then an appropriate amount of water and sodium polycarboxylate (solid content equivalent) were mixed and stirred and dispersed. At this time, a bead mill treatment was performed under conditions of a bead diameter of 0.1 mm and a mill rotation speed of 2000 rpm, as necessary. Xantham gum was added as a thickener to the mixed solution after the treatment as necessary to prepare a coating solution.

[0254] After carrying out corona discharge treatment on the surface of the polyolefin microporous membrane, a coating liquid was applied to the treated surface using a gravure coater.Then, the coating liquid on the polyolefin microporous membrane was dried at 60°C to remove water, and a porous layer having a thickness of 1.5 μm and containing 97.5 mass % (90.6 volume %) of inorganic particles was formed on one side of the polyolefin microporous membrane to obtain a multilayer porous membrane.The membrane properties of the obtained multilayer porous membrane and the evaluation results of a battery equipped with the multilayer porous membrane as a separator are also shown in Table 3.

[0255] [Examples 2 to 13 and Comparative Examples 1 to 6] A multilayer porous membrane was formed in the same manner as in Example 1, except that the production conditions and physical properties of the polyolefin microporous membrane, the type of inorganic particles, the type of components of the porous layer, the coating solution composition, and the coating conditions were set as shown in Tables 1 to 3. The various properties of the obtained multilayer porous membrane and the battery including the same as a separator were evaluated by the above-mentioned methods. The evaluation results are shown in Table 3.

[0256] In Examples 12 and 13, 80 parts by mass of adhesive resin (acrylic polymer, glass transition temperature 90°C, average particle size 380nm, electrolyte swelling degree 2.8) and 20 parts by mass of adhesive resin having a different glass transition temperature (acrylic polymer, glass transition temperature -6°C, average particle size 132nm, electrolyte swelling degree 2.5) were mixed, and ion-exchanged water was added to prepare an adhesive resin-containing coating liquid (adhesive resin concentration 3% by mass). The adhesive resin-containing coating liquid was applied in dots on one side of a polyolefin microporous membrane having a porous layer or on the porous layer with a gravure coater to form a dot pattern having the dot diameter and dot distance shown in Table 3. Then, the mixture was dried at 60°C to remove water.

[0257] [Table 1]

[0258] [Table 2]

[0259] [Table 3-1]

[0260] [Table 3-2]

[0261] [Table 3-3]

[0262] [Table 3-4]

[0263] [Table 3-5]

[0264] [Table 3-6]

[0265] [Table 3-7]

[0266] [Table 3-8] [Explanation of symbols]

[0267] Solid line Separator Dotted line Positive electrode One-dot chain line: negative electrode 1 Flat Pin 9-pin 10 Pin I 11 Pin II 12 Winding sample

Claims

1. A multi-layer porous membrane having a microporous membrane containing a polyolefin resin as a main component and a porous layer containing inorganic particles laminated on at least one surface of the microporous membrane, The average particle diameter D of the inorganic particles 50 is 0.01 μm or more and less than 0.60 μm, The mass ratio of the inorganic particles in the porous layer is greater than 80%, The volume ratio of the inorganic particles in the porous layer is greater than 70%, The surface static friction coefficient of the porous layer is 0.01 or more and 0.40 or less, and The surface dynamic friction coefficient of the porous layer is 0.01 or more and 0.35 or less. Multilayer porous membrane.

2. The air permeability of the multilayer porous membrane is 400 sec / 100 cm 3 2. The multilayer porous membrane according to claim 1, wherein:

3. The microporous membrane has a puncture strength calculated based on the basis weight of 0.49 N / (g / m 2 3. The multilayer porous membrane according to claim 1 or 2, wherein the porous membrane has a molecular weight of 100 or more.

4. The multilayer porous membrane according to claim 1 or 2, wherein the porous layer has a thickness of 4 μm or less on at least one side of the microporous membrane.

5. The air permeability of the porous layer is 100 sec / 100 cm 3 The multilayer porous membrane according to claim 1 or 2, wherein:

6. 3. The multilayer porous membrane according to claim 1, wherein the ratio of the surface static friction coefficient to the surface kinetic friction coefficient (surface static friction coefficient / surface kinetic friction coefficient) is 1.07 or less.

7. The multilayer porous membrane according to claim 1 or 2, wherein the multilayer porous membrane has a heat shrinkage rate at 150°C of 10% or less in both the MD and TD directions.

8. The multilayer porous membrane according to claim 1 or 2, which is a separator for a non-aqueous electrolyte battery.

9. A non-aqueous electrolyte battery comprising a positive electrode, the multilayer porous membrane according to claim 8, a negative electrode, and a non-aqueous electrolyte.

Citation Information

Patent Citations

  • Separator for nonaqueous secondary battery, and nonaqueous secondary battery

    JP2010218749A

  • Laminated porous film, battery separator, and battery

    JP2011126275A

  • Composition for nonaqueous secondary battery porous films, porous film for nonaqueous secondary batteries, and secondary battery

    JP2015162313A

  • Multilayer porous film having polyolefin microporous film

    JP2020116925A

  • Cell separator

    JP2022089292A

Cited By

  • A battery cell and battery

    KR102983986B1

  • Separator for electrochemical device and electrochemical device comprising same

    WO2026173368A1