Peripheral face light emission type light guide bar having affinity layer
The affinity layer in the circumferential light guide rod enhances adhesion between the core and cladding layers, addressing peeling issues and maintaining brightness under stress or temperature changes, ensuring efficient light guiding and durability.
Patent Information
- Application Number
- JP2023053985
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing circumferential light guide rods face issues with peeling and reduced brightness due to cuts or changes in environmental temperature, particularly at the interface between the core and cladding layers, limiting flexibility and durability.
Incorporating an affinity layer made of non-fluorine resin with adhesive properties between the core and cladding layers, utilizing resins with specific refractive indices and adding a light scattering material to the cladding layer, enhances adhesion and maintains brightness even under bending or temperature changes.
The affinity layer ensures strong bonding between the core and cladding layers, preventing peeling and maintaining high brightness, even in bent or temperature-changed conditions, thus improving light guiding efficiency and durability.
Smart Images

Figure 2024142029000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a peripheral light-emitting type light guide rod that can guide light incident from an end face in the longitudinal direction and emit the guided light from an outer peripheral surface. In particular, the present invention relates to a peripheral light-emitting type light guide rod that has a predetermined affinity layer in order to maintain brightness even if it is cut or the environmental temperature changes. [Background technology]
[0002] There are various types of signs and advertisements for stores and buildings, and neon lights have been used to display letters and figures even at night. However, neon lights made of glass tubes are not flexible, so once they are manufactured in a predetermined shape, they cannot be deformed into another shape. Therefore, they must be individually manufactured according to the desired shape, which is inconvenient in terms of delivery time and economy. Furthermore, when used for external decorative parts of automobiles, neon lights made of fragile glass tubes are not suitable because they lack strength and durability.
[0003] Therefore, light guide rods made of flexible and light-transmitting resin processed into a rod shape are being used in place of neon lines. When light is incident on one end of a light guide rod, it can be guided in the longitudinal direction by repeating total reflection inside the light guide rod. On the other hand, by scattering a part of the light that should be totally reflected, it can be emitted from the outer circumferential surface. In this way, a peripheral light-emitting type light guide rod that guides light in the longitudinal direction and emits light from the outer peripheral surface is flexible and can guide light through total reflection even when bent to a certain extent, so it can be deformed into various shapes for use.
[0004] In order for the light guide rod to efficiently achieve total reflection, the core layer that guides the light and the clad layer that forms the reflective surface must be made of materials with different refractive indices. In this case, it is necessary to ensure that there is no air space between the core layer and the clad layer. If there is an air space in a part of the rod, the difference in refractive index will cause the light scattering property to be non-uniform in that part, resulting in problems such as reduced brightness in a part.
[0005] However, when a peripheral light-emitting type light guide rod is used outdoors, cuts may occur on the surface of the cladding layer due to the collision of a foreign object, etc. In particular, if the depth of the cut reaches the core layer, the core layer and the cladding layer may peel off from the cut area due to a subsequent change in environmental temperature or an external force such as bending. Once peeling occurs, the peeling continues to progress in the longitudinal direction, resulting in the aforementioned inhibition of total reflection and a decrease in luminance of light emitted from the outer circumferential surface.
[0006] The applicant of the present application has previously filed a patent application relating to a peripheral light-emitting type light guide rod in which a light reflecting layer is provided on the outer side of the cladding layer (see Patent Document 1). In this technology, by using a resin for the light reflecting layer that has adhesive properties with respect to the fluorine-based resin cladding layer, it is possible to prevent delamination between the cladding layer and the outermost reflecting layer.
[0007] Patent Document 2 discloses a technique for an optical fiber cable in which the cladding layer has a two-layer structure and the fluororesins used in each layer are a combination of specific resins with good affinity. It is said that the combination of fluororesins with good affinity improves the adhesion between the two cladding layers, resulting in an optical fiber cable with excellent twisting resistance and mechanical durability.
[0008] Furthermore, Patent Document 3 discloses a technology relating to a plastic optical fiber cable consisting of a core layer using an acrylic resin and a cladding layer using a fluorine-based resin with a predetermined Shore D hardness. By using a fluorine-based resin with a Shore D hardness in a predetermined range for the cladding layer, it is said that the cladding layer has appropriate adhesion and softness, and therefore does not easily peel off from the core layer and can be firmly joined. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2015-69808 A [Patent Document 2] Patent Publication No. 2021-156984 [Patent Document 3] JP 2014-215579 A Summary of the Invention [Problem to be solved by the invention]
[0010] However, although the technology of Patent Document 1 can prevent delamination between the clad layer and the light reflecting layer provided on the outside of the clad layer, it does not mention the adhesive strength between the core layer and the clad layer. The same is true of Patent Document 2, which can improve the peel strength of each layer in the multi-layered clad layer, but does not mention the adhesive strength between the core layer and the clad layer.
[0011] On the other hand, Patent Document 3 claims that it is possible to improve not only the adhesion strength between the clad layer and its outer coating layer, but also the adhesion strength between the core layer and the clad layer. However, the technology of Patent Document 3 has a problem in that the hardness of the resin used in the clad layer is limited, which limits flexibility. In addition, although peeling can be prevented by its ability to follow bending, it is difficult to say that it is effective in preventing peeling when cuts are made or when the environmental temperature changes.
[0012] The present invention has been made in consideration of the above-mentioned problems, and has as its object to provide a peripheral light-emitting type light guide rod having an affinity layer that can emit light from the peripheral surface with high brightness even at a location far from the light source, and can maintain high brightness on the outer peripheral surface even if it is cut or used in a bent state in harsh environmental temperatures. [Means for solving the problem]
[0013] The means adopted by the present inventors to solve the above problems will be described below. The peripheral light-emitting type light guide bar with affinity layer (hereinafter referred to as "light guide bar") of the present invention comprises a core layer mainly made of acrylic resin and a cladding layer mainly made of fluororesin, and is configured to guide light incident from the end face in the longitudinal direction and emit light from the peripheral face. It is characterized in that an affinity layer is provided between the core layer and the cladding layer, the affinity layer is mainly made of a non-fluororesin that has adhesive properties with the acrylic resin, and the cladding layer is mainly made of a resin that has adhesive properties with the affinity layer.
[0014] The non-fluorine-based resin used in the affinity layer is mainly made of a resin having adhesive properties with acrylic resin, and therefore has good adhesion with the acrylic resin. The adhesiveness with acrylic resin means, for example, a mechanical bonding property in which the boundary surface of the core layer and the affinity layer melts and solidifies with each other during molding, a bonding property due to a chemical interaction in which the main chains or side chains of both undergo a chemical reaction at the boundary surface to become one, or a bonding property due to a physical interaction in which molecules adjacent to each other at the boundary surface attract each other due to intermolecular forces, and means a bonding strength that is strong enough not to peel off easily in a specified application. This property is not limited to that possessed by the resin itself, but also includes that which is provided by being added by surface modification, etc.
[0015] On the other hand, the fluororesin used in the cladding layer is mainly composed of a resin having adhesive properties with the non-fluororesin in the affinity layer, and therefore good adhesion with the non-fluororesin in the affinity layer can be obtained. The adhesiveness of the affinity layer to the non-fluorinated resin is synonymous with the adhesiveness of the affinity layer to the acrylic resin, and refers to the property of bonding by mechanical bonding, chemical interaction, or physical interaction. This property is not limited to the property that the resin itself has, but also includes the property that is provided by adding the property through surface modification or the like.
[0016] The light guide rod of the present invention can firmly bond the affinity layer and the clad layer by providing an affinity layer having adhesiveness with the core layer as described above. Also, the light guide rod of the present invention can firmly bond the affinity layer and the clad layer by providing a clad layer having adhesiveness with the affinity layer. In this way, since the affinity layer has good adhesion to both the core layer and the cladding layer, even if the cladding layer is cut and subjected to a bending moment such as bending, the interface between the layers does not peel off and the layers can maintain their adhesion. Also, even if the environmental temperature changes and the layers expand and contract in a shearing manner due to differences in the linear expansion coefficients of the layers, the interface between the layers does not peel off and the layers can maintain their adhesion.
[0017] In addition to the above, the means adopted by the present invention to solve the above-mentioned problems may also include making the affinity layer mainly of polyamide resin and making the fluororesin have adhesive functional groups for polyamide resin.
[0018] Acrylic resin and polyamide resin have similar polarity and molecular chains intermingle near the interface, so they have good adhesion. Therefore, by using polyamide resin as the main material for the affinity layer, the core layer and affinity layer can be more strongly adhered to each other. In addition, by using a fluororesin having adhesive functional groups for polyamide resin as the main material for the cladding layer, the functional groups of both materials react near the interface, thereby providing good adhesion to the affinity layer.
[0019] As another means adopted by the present invention to solve the above-mentioned problems, the refractive index of the affinity layer can be made lower than that of the core layer and higher than that of the cladding layer. In particular, it is preferable that the difference in refractive index between the core layer and the affinity layer is 0.05 or more and 0.09 or less, and the difference in refractive index between the affinity layer and the cladding layer is 0.01 or more and 0.05 or less.
[0020] The refractive index of the affinity layer is lower than that of the core layer and higher than that of the cladding layer, so that total reflection can be caused between the core layer and the affinity layer. Even if a part of the light enters the affinity layer, total reflection can be caused between the affinity layer and the cladding layer. This can improve the light guide efficiency. Furthermore, by setting the difference in refractive index between the layers to the above value, the amount of light that is totally reflected within the entire light guiding rod can be increased, thereby further improving the light guiding efficiency.
[0021] In another embodiment of the present invention, the cladding layer may be made mainly of tetrafluoroethylene-perfluoroalkylvinylether copolymer (CPT).
[0022] There are various types of fluororesins, for example, tetrafluoroethylene-ethylene copolymer (ETFE) has been used in the past for the cladding layer, but it is known that ETFE does not have very good adhesion to acrylic resins, especially polymethyl methacrylate (PMMA). Therefore, by using a polyamide resin as the affinity layer and a CPT resin that has good adhesion to the polyamide resin of the affinity layer, the affinity layer and the cladding layer can be bonded more firmly.
[0023] In a configuration using the above-mentioned CPT, it is also possible to configure the cladding layer to have a multilayer structure having at least an inner layer and an outer layer, with the inner layer being made primarily of tetrafluoroethylene-perfluoroalkylvinyl ether copolymer (CPT), and the outer layer being made primarily of tetrafluoroethylene-hexafluoropropylene copolymer (FEP) to which a light scattering material has been added.
[0024] Tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (CPT) and tetrafluoroethylene-hexafluoropropylene copolymer (FEP) have similar polarity and molecular chains intermingle near the interface, making them resins with good adhesion. Therefore, by using CPT resin as the main material for the inner layer and FEP resin as the main material for the outer layer, the inner layer and outer layer can be more strongly adhered to each other. In addition, by making the cladding layer a multi-layer structure and adding a light scattering material to the outermost layer, it is possible to emit light uniformly from the outer surface. The FEP resin used in the outer layer has good adhesion to the CPT resin used in the inner layer, making it less likely to peel off. In addition, because it has a smaller refractive index than CPT resin, some of the light scattered in the inner layer can be totally reflected at the interface between the inner layer and the outer layer and returned to the inner layer, affinity layer, and core layer, improving the efficiency of light guiding. Effect of the Invention
[0025] As described above, the light guide rod of the present invention has an affinity layer between the core layer and the cladding layer, which has adhesive properties with the core layer, and the cladding layer is made mainly of a resin which has adhesive properties with the affinity layer. The above-mentioned structure allows the core layer and the affinity layer, and the affinity layer and the cladding layer to be firmly bonded to each other, so that the high brightness of the outer peripheral surface can be maintained even if the optical fiber is cut or bent in a harsh environmental temperature. [Brief description of the drawings]
[0026] [Figure 1] 1A and 1B are a perspective view and a cross-sectional view showing a light guiding rod of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a light guiding rod according to a first modified example of the present invention. [Diagram 3] 1 is a graph showing the luminance measurement results of the light guiding rod of the present invention. [Figure 4] 1 is a graph showing the chromaticity measurement results of the light guide rod of the present invention. [Diagram 5] FIG. 13 is an explanatory diagram showing the position and size of an incision in brightness measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] An embodiment of the present invention will be described below with reference to FIG. It should be noted that each drawing is drawn diagrammatically for the purpose of explanation, and some dimensions and shapes are shown exaggerated or simplified.
[0028] The peripheral light-emitting type light guide bar having an affinity layer (hereinafter simply referred to as "light guide bar") 100 of the present invention comprises a core layer 1 mainly made of acrylic resin, an affinity layer 2 mainly made of non-fluorine resin, and a cladding layer 3 mainly made of fluorine resin, as shown in Fig. 1. The affinity layer 2 is interposed between the core layer 1 and the cladding layer 3.
[0029] The core layer 1 may have a circular cross-sectional shape as shown in FIG. 1, but may also have other shapes such as a rectangular, elliptical, semicircular, or polygonal shape.
[0030] The material of the core layer 1 may be a thermoplastic resin containing an acrylic resin as a main component. As the acrylic resin, one or more types of hard acrylic resins such as polymethyl methacrylate (PMMA), polyethyl methacrylate, polyisobutyl methacrylate, or polyt-butyl methacrylate can be used. Also usable are one or more types of acrylic elastomers such as a block copolymer of methyl methacrylate-n-butyl acrylate-benzyl acrylate, a block copolymer of methyl methacrylate and butyl acrylate (MMA-BA block copolymer), a block copolymer of methyl acrylate and butyl acrylate, or an acrylic block copolymer composed of methyl methacrylate (methyl acrylate), an acrylic ester, and an aromatic acrylic ester. Furthermore, the above-mentioned hard acrylic resin and acrylic elastomer resin can be mixed and used.
[0031] A bluing agent (blue pigment or purple pigment) can be added to the core layer 1 to suppress yellowing of the luminous color of the light guiding bar 100. The amount of the bluing agent added is preferably 0.1 ppm to 10 ppm by weight relative to the resin material of the core layer 1. The bluing agent can be added not only to the core layer 1 but also to the affinity layer 2 and the cladding layer 3.
[0032] The affinity layer 2 is mainly made of a non-fluorine-based resin that has adhesiveness with acrylic resin. The affinity layer 2 may be formed to have a shape similar to that of the core layer 1 and a uniform thickness, or may be formed to have a shape dissimilar to that of the core layer 1 such that some of the thicknesses differ.
[0033] The material of the affinity layer 2 may be a thermoplastic resin mainly made of a non-fluorinated resin. As the non-fluorine-based resin, one or more of acrylonitrile-styrene copolymer (AS), acrylonitrile-butadiene-styrene (ABS), polycarbonate (PC), polyvinyl chloride (PVC), polyamide 6 (PA6), polyamide 66 (PA66), etc. can be used. In particular, polyamide resins such as PA6 and PA66 are preferable because of their adhesiveness to acrylic resins and their ease of bonding with adhesive functional groups of fluorine-based resins.
[0034] The cladding layer 3 is mainly made of a fluorine-based resin that has adhesiveness with the non-fluorine-based resin of the affinity layer 2 . The cladding layer 3 may be formed to have a shape similar to that of the affinity layer 2 and a uniform thickness, or may be formed to have a shape dissimilar to that of the core layer 1 so that some of the thicknesses differ.
[0035] The material for the cladding layer 3 may be one or more of fluorine-based resins such as ethylene-tetrafluoroethylene copolymer (ETFE), hexafluoropropylene-tetrafluoroethylene-ethylene copolymer (EFEP), polyvinylidene fluoride, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (CPT), or tetrafluoroethylene-hexafluoropropylene copolymer (FEP), with tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (CPT) being particularly preferred due to its ease of bonding with polyamide resin.
[0036] Furthermore, the fluororesin of the cladding layer 3 is generally a polymer in which fluorine atoms are bonded to a chain of carbon atoms, and therefore the fluorine atoms make it difficult to bond with other materials. Therefore, it is preferable to use a material in which some of the fluorine atoms in the main chain or side chain are replaced with adhesive functional groups such as hydroxyl groups, carboxyl groups, and carbonyl groups, and it is particularly preferable to use a special fluororesin that has adhesive functional groups without surface modification such as plasma treatment or corona treatment.
[0037] A light scattering agent can be added to the cladding layer 3 to facilitate the emission of light from the outer peripheral surface. In this case, if the light scattering agent has an ultraviolet absorbing effect, weather resistance can also be improved. Specifically, 0.01 to 5 parts by weight of powdered titanium oxide can be added to 100 parts by weight of the main material of the cladding layer 3 as the light scattering agent. As the light scattering agent, barium sulfate other than titanium oxide can also be used. The light scattering agent can be added not only to the cladding layer 3 but also to the core layer 1 and the affinity layer 2.
[0038] In the embodiment of FIG. 1, when PMMA is used for the core layer 1 and PA resin with a refractive index of 1.42 at the d-line is used for the affinity layer 2, the refractive index of the affinity layer 2 is smaller than that of the core layer 1. Therefore, total reflection occurs at the interface between the core layer 1 and the affinity layer 2. Furthermore, when CPT resin is used for the cladding layer 3, the refractive index of the cladding layer 3 is smaller than that of the affinity layer 2. Therefore, the light incident on the affinity layer 2 can be further totally reflected by the cladding layer 3. This allows the total reflection of light at a wider angle of incidence.
[0039] In this way, by making the refractive indexes of the core layer 1 and the affinity layer 2 similar to each other and making the refractive index of the cladding layer 3 lower than that of the core layer 1, the affinity layer 2 can also be used as a waveguide. Therefore, the aperture ratio can be increased, and the incidence efficiency can be improved.
[0040] The refractive index of the affinity layer 2 may be larger than that of the core layer 1, but a smaller refractive index is preferable, more preferably less than -5%, and further preferably intermediate between the refractive indexes of the core layer 1 and the cladding layer 3. As an example, a PMMA resin with a refractive index of 1.50 can be used for the core layer 1, and a PA resin with a refractive index of 1.42 can be used for the affinity layer 2. If it is greater than +5%, the angle of incidence of the light that enters the affinity layer 2 from the core layer 1 onto the cladding layer 3 becomes too small, and the rate at which total reflection occurs at the boundary with the cladding layer 3 decreases. On the other hand, if it is smaller than -5%, the proportion of total reflection occurring at the boundary surface between the core layer 1 and the affinity layer 2 increases, and the affinity layer 2 becomes a part of the cladding layer 3. In this case, the affinity layer 2 cannot be used as a waveguide, so the aperture ratio cannot be increased and the incidence efficiency cannot be improved.
[0041] 『Variation 1』 The present invention is not limited to the above-mentioned embodiment, and other embodiments may be adopted. For example, as shown in Fig. 2, the cladding layer 3 of the light guide bar 101 may have a multi-layer structure including an inner layer 31 and an outer layer 32. It is also possible to have a structure including a plurality of layers, or to provide a protective layer on the outside of the cladding layer 3, and expose the cladding layer 3 only where display is required (not shown).
[0042] When using a two-layer structure consisting of an inner layer 31 and an outer layer 32, such as light guiding rod 101, it is preferable to use a material mainly made of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (CPT) for the inner layer 31 and a material mainly made of tetrafluoroethylene-hexafluoropropylene copolymer (FEP) for the outer layer 32.
[0043] Among the resins used for the affinity layer 3, the CPT resin having adhesive functional groups has particularly good adhesion to polyamide resins, and can more firmly bond the affinity layer 2 and the cladding layer 3. In addition, the refractive index of the CPT resin at the d line is low at approximately 1.39, so that light over a wider range of incident angles can be totally reflected. Furthermore, by using FEP resin with a refractive index of 1.40 for the outer layer 32, it is possible to firmly bond it to the inner layer 31 using CPT resin. EXAMPLES
[0044] "Evaluation test of luminance decay characteristics" Next, the luminance of the samples of specific Examples 1 to 3 of the light guiding rod of the present invention and the sample of Comparative Example 1, which is a light guiding rod of the prior art, was compared for each distance from the light source. Each sample had a length of 1.0 m and a diameter of 3.5 mm, and the emission luminance was measured at a distance of 100 mm to 900 mm from the light source. In particular, for Examples 2 and 3, measurements were taken at small intervals in the range of 200 mm to 340 mm, and the degree of hot spots where the luminance increased extremely was measured. The measurement was performed by placing a spectroradiometer (Konica Minolta CS-2000) at a position 600 mm vertically away from the measured portion of the sample. The light source used was an LED light source with a drive current of 300 mA and a light output of 28 lm. The "brightness attenuation characteristics" in this specification are based on the emission brightness measured under the test conditions in the table below. [Table 1]
[0045] "Example 1" Example 1 had an overall diameter of 3.5 mm, a core layer with a circular cross section, an affinity layer of uniform thickness around the core layer, and a clad layer of uniform thickness around the affinity layer. The clad layer had a two-layer structure consisting of an inner layer and an outer layer. The core layer is made of transparent polymethylmethacrylate (PMMA) resin that has been improved to have gentle attenuation over distance (hereafter referred to as balanced type), and the affinity layer is made of transparent polyamide (PA) resin. The inner layer of the cladding layer is made of tetrafluoroethylene-perfluoroalkylvinylether copolymer (CPT) resin that has adhesive functional groups for PA resin, and the outer layer of the cladding layer is made of tetrafluoroethylene-hexafluoropropylene copolymer (FEP) resin that has been made milky white by adding titanium oxide, a light scattering agent.
[0046] "Example 2" Example 2 had the same structure as Example 1, but was different in that the amount of light scattering agent added to the outer layer was increased to give it a white color.
[0047] "Comparative Example 1" In Comparative Example 1, similar to Examples 1 and 2, the overall diameter was 3.5 mm, a core layer having a circular cross section was used, and a clad layer of uniform thickness was provided around the core layer. The clad layer had a two-layer structure consisting of an inner layer and an outer layer. The core layer is made of transparent polymethylmethacrylate (PMMA) resin that has been improved to have high brightness (hereafter referred to as high brightness type). The inner layer of the cladding layer is made of tetrafluoroethylene-ethylene copolymer (ETFE) resin, and the outer layer of the cladding layer is made of tetrafluoroethylene-ethylene copolymer (ETFE) resin that has been made milky white by adding titanium oxide, a light scattering agent.
[0048] "Test Results" The test results of the above-mentioned Examples 1 and 2 and Comparative Example 1 are shown in FIGS. 3(a) and (b). As shown in FIG. 3(a), Example 1, which used a balanced core layer and a milky white outer layer, had slightly lower brightness at close distances from the light source than Comparative Example 1, which used a high-brightness core layer, but the brightness at positions farther from the light source was similar, resulting in a smaller rate of attenuation with distance. Similarly, Example 2, which used a balanced core layer and a white outer layer, showed slightly higher brightness at positions close to the light source and also slightly higher brightness at positions farther from the light source than Comparative Example 1, which used a high-brightness core layer.
[0049] On the other hand, as shown in Fig. 3(b), in the range of distance from the light source of 200mm to 340mm, hot spots where brightness extremely increased occurred around 260mm to 270mm in both Example 1 and Example 2. It is considered that these hot spots are caused by the alignment characteristics of the light source and the diameter of the core layer, etc., but compared with Example 2 in which the outer layer was white, Example 1 in which the outer layer was milky white showed a smaller degree of hot spots. In addition, even though the outer layer was white, the hot spots in Comparative Example 1 had the same brightness as Example 2.
[0050] "Evaluation test of chromaticity characteristics" The chromaticity was also evaluated at the same time as the evaluation test of the luminance decay characteristic. The samples and evaluation equipment used in the test were the same as those used in the evaluation test of the luminance decay characteristic described above.
[0051] "Test Results" The test results of the above-mentioned Examples 1 and 2 and Comparative Example 1 are shown in FIG. 4, the chromaticity change of Example 1 having a balanced core layer was not significantly different from that of Comparative Example 1 having a high-brightness core layer. Example 2 having a white outer layer shifted more toward yellow than Example 1, but did not have an extreme chromaticity change that would cause a problem in practical use.
[0052] "Evaluation test of luminance change due to cuts" Next, as shown in Fig. 5, the change in luminance when a cut was made in the light guide rod was evaluated with N=2. Example 2 and Comparative Example 1 were used as samples, and a cut of about 50 mm in length was made in a 500 mm long light guide rod at a position 300 mm from the light source. The cut was deep enough to penetrate the inner and outer layers of the cladding layer and just short of reaching the core layer, and after making the cut, the light guide rod was bent about 4 to 5 times. The luminance was measured using the same equipment as in the evaluation test of the luminance decay characteristics described above, and the luminance of the sample with the cut was compared with that of the sample without the cut. For the sample with the cut, the luminance was measured on the side opposite the cut.
[0053] "Test Results" The test results of Example 2 and Comparative Example 1 are shown in the table below. [Table 2] In Comparative Example 1, which did not have an affinity layer, the core layer and the clad layer peeled off at the location of the cut during folding, and therefore the luminance decreased by 25% or more between the sample with the cut and the sample without the cut. On the other hand, in Example 2 having an affinity layer, the core layer and the clad layer did not peel off even when the sample was bent, and therefore no significant difference in brightness was observed between the sample with and without cuts. [Explanation of symbols]
[0054] 100, 101 Surface-emitting light guide rod with affinity layer 1 Core layer 2 affinity layer 3 Cladding layer 31 Inner layer 32 Outer layer
Claims
1. A peripheral light-emitting type light guide rod that includes a core layer mainly made of an acrylic resin and a clad layer mainly made of a fluorine-based resin, guides light incident from an end face in a longitudinal direction, and emits light from an outer peripheral surface, a compatibility layer between the core layer and the clad layer; The affinity layer is mainly made of a non-fluorine-based resin having adhesive properties with an acrylic resin, A peripheral light-emitting type light guide rod having an affinity layer, characterized in that the cladding layer is mainly made of a resin having adhesive properties with the affinity layer.
2. The affinity layer is mainly made of polyamide resin, 2. The peripheral light-emitting type light guide rod having an affinity layer according to claim 1, wherein the fluorine-based resin has an adhesive functional group for a polyamide resin.
3. 3. The peripheral light-emitting type light guide rod having an affinity layer according to claim 1, wherein the refractive index of the affinity layer is lower than that of the core layer and higher than that of the cladding layer.
4. 3. The peripheral light-emitting type light guide rod having an affinity layer according to claim 1 or 2, wherein the cladding layer is mainly made of a tetrafluoroethylene-perfluoroalkylvinylether copolymer.
5. The cladding layer has a multilayer structure including at least an inner layer and an outer layer, The inner layer is mainly made of tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, The peripheral light-emitting type light guide rod having an affinity layer as described in claim 4, characterized in that the outer layer is made of a tetrafluoroethylene-hexafluoropropylene copolymer as a main material to which a light scattering material is added.
Citation Information
Patent Citations
Plastic optical fiber cable
JP2014215579A
Linear light emitting body
JP2015069808A
Plastic optical fiber, and plastic optical fiber cable
JP2021156984A